High-performance asphalt composition, asphalt mixture containing same, and method for producing asphalt mixture
The asphalt composition addresses high-temperature production issues by using penetration regulators and anti-peeling agents to improve compaction and moisture resistance, achieving lower production temperatures and enhanced performance.
Patent Information
- Application Number
- JP2021214575
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-01-04
- Filing Date
- 2021-12-28
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2041-12-28
AI Technical Summary
Existing asphalt mixtures require high-temperature production, leading to energy consumption, harmful emissions, and oxidative aging, while Warm Mix Asphalt (WMA) faces challenges with water removal and aggregate adhesion due to high viscosity, resulting in premature pavement cracking and reduced performance.
An asphalt composition incorporating penetration regulators and anti-peeling agents, such as specific chemical compounds, to improve penetration and moisture resistance while maintaining viscosity, allowing for lower production temperatures and enhanced aggregate adhesion.
The asphalt composition enhances road paving performance by improving compaction and moisture resistance, reducing production temperatures by 20-50°C, and increasing productivity, while maintaining plastic deformation resistance.
Smart Images

Figure 0007594997000001 
Figure 0007594997000002 
Figure 0007594997000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an asphalt composition having improved penetration as well as improved moisture resistance and compactibility, an asphalt mixture containing the same, and a method for producing an asphalt mixture. [Background technology]
[0002] Asphalt mixture, commonly called ascon, is produced by putting asphalt, aggregate, filler, etc. into an asphalt mixing plant, heating these materials to a high temperature of 160~180℃, and mixing them together, and then used as a road paving material.
[0003] Therefore, in the process of producing an asphalt mixture, not only is a lot of energy required for high temperature heating, but harmful gases such as carbon dioxide, sulfur oxides, and nitrogen oxides are also emitted during construction, which can have a negative impact on the environment and the health of workers. In addition, when paving roads, it takes a long time to cool the asphalt mixture produced at a high temperature of 160-180°C to room temperature, which causes problems such as delays in opening the road to traffic and exposure of workers to safety accidents. Furthermore, producing asphalt at high temperatures causes oxidation aging of the asphalt to progress relatively quickly, which leads to early cracks in the pavement, thereby shortening the lifespan of the pavement.
[0004] Meanwhile, warm mix asphalt (WMA) has advantages such as energy consumption, cost savings, reduced harmful gas emissions, and earlier traffic reopening due to the lower production and compaction temperatures compared to heated asphalt mixtures. However, since the aggregate is heated at a lower temperature than heated asphalt mixtures, there is a limit to how much moisture can be removed from the aggregate, and the relatively high viscosity of asphalt makes it difficult to coat the aggregate. Therefore, in the case of warm mix asphalt mixtures, water that flows into the asphalt pavement weakens the adhesive or bonding strength between the aggregate and asphalt, which can lead to detachment of the aggregate from the asphalt.
[0005] For this reason, in addition to asphalt stripping inhibitors and softeners, by-products of petroleum vacuum distillation processes, by-products of heavy oil fluidized bed catalytic cracking processes, by-products of deasphaltenization processes, lubricating oil-based and animal and plant-based fractions are used as asphalt penetration adjusters. In this case, however, a decrease in performance representative of the plastic deformation resistance of asphalt, such as viscosity, occurs, which severely limits the production of the desired high quality asphalt.
[0006] Therefore, there is a need to develop a technology that can improve the road pavement performance of asphalt by increasing only the penetration while maintaining the viscosity of asphalt and maintaining the plastic deformation resistance, while also improving the moisture resistance and compaction properties of asphalt. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Korean Patent No. 10-1439294 (2014.09.02) Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention has been devised to solve the above problems, and an object of the present invention is to provide an asphalt composition having an improved penetration, moisture resistance and compactibility.
[0009] Another object of the present invention is to provide a high-quality asphalt composition that improves the penetration of asphalt while maintaining the viscosity of the asphalt and preventing a decrease in plastic deformation resistance. [Means for solving the problem]
[0010] In order to achieve the above-mentioned object, the present invention provides an asphalt composition comprising a penetration modifier represented by the following chemical formula 1, one or more anti-stripping agents selected from the group consisting of a compound represented by the following chemical formula 2 and a compound represented by the following chemical formula 3, and asphalt.
[0011] [Chemical formula 1] [ka] [Chemical formula 2] [ka] [Chemical formula 3] [ka]
[0012] In the above Chemical Formulas 1 to 3, R is a C1-C30 hydrocarbyl or a C1-C30 heterohydrocarbyl; R 1 is C1-C30 alkyl, C1-C30 alkenyl, or C1-C30 alkynyl; R 2 ~R 4 are each independently hydrogen, C1-C30 alkyl, C1-C30 alkenyl, or C1-C30 alkynyl; R 5 or R 6are independently hydrogen, C1-C30 alkyl, C1-C30 alkenyl, or C1-C30 alkynyl; R 5 and R 6 at least one of is C1-C30 alkyl, C1-C30 alkenyl, or C1-C30 alkynyl; m is an integer from 1 to 10; n is an integer from 0 to 20; The hydrocarbyl or heterohydrocarbyl of R and R 1 ~R 4 The alkyl, alkenyl or alkynyl may be further substituted with one or more substituents selected from hydroxy, C1-C20 alkoxy, C1-C20 alkyl, carbonyl, halogen and amino groups.
[0013] In the asphalt composition according to one embodiment of the present invention, the penetration modifier represented by Chemical Formula 1 may be a compound represented by Chemical Formula 4 below.
[0014] [Chemical formula 4] [ka]
[0015] In the above Chemical Formula 4, R' is a C1-C30 alkyl, a C1-C30 alkenyl, or a C1-C30 alkynyl, and the alkyl, alkenyl, or alkynyl of R' may be further substituted with one or more substituents selected from a hydroxy group, a carbonyl group, an alkoxy group, and a carboxy group, and q is 0 or 1.
[0016] In the asphalt composition according to one embodiment of the present invention, the penetration modifier represented by Chemical Formula 1 may be a compound represented by Chemical Formula 5 below.
[0017] [Chemical formula 5] [ka]
[0018] In the above Chemical Formula 5, R″ is a C1-C30 alkyl, a C1-C30 alkenyl, or a C1-C30 alkynyl, and A is a C1-C5 alkylene, and the alkyl, alkenyl, or alkynyl of R″ and the alkylene of A may be further substituted with one or more substituents selected from a hydroxy group, a carbonyl group, an alkoxy group, and a carboxy group.
[0019] According to one embodiment of the present invention, the compound represented by the formula 2 is R 1 is C1-C30 alkyl or C1-30 alkenyl, R 2 ~R 4 are each independently hydrogen or C1-C3 alkyl, which may be substituted with a hydroxy group.
[0020] According to one embodiment of the present invention, the compound represented by Chemical Formula 3 may be a mixture of monophosphate and diphosphate. The penetration modifier represented by Chemical Formula 1 according to one embodiment of the present invention may be included in an amount of 0.05 to 10 parts by weight based on 100 parts by weight of asphalt.
[0021] According to one embodiment of the present invention, one or more anti-stripping agents selected from the compound represented by Chemical Formula 2 and the compound represented by Chemical Formula 3 may be included in an amount of 0.1 to 10 parts by weight per 100 parts by weight of asphalt.
[0022] According to one embodiment of the present invention, the monophosphate ester and diphosphate ester may be included in an amount of 0.1 to 5 parts by weight based on 100 parts by weight of asphalt. According to one embodiment of the present invention, the asphalt may be any one or more selected from the group consisting of natural asphalt, petroleum asphalt, petroleum pitch, reclaimed asphalt, and modified asphalt.
[0023] The present invention provides an asphalt mixture comprising the above-described asphalt composition, aggregate and filler. The present invention also provides a method for producing an asphalt mixture, the method including: a premixing step of producing an asphalt composition containing asphalt, a penetration modifier represented by the following chemical formula 1, and one or more anti-stripping agents selected from the group consisting of a compound represented by the following chemical formula 2 and a compound represented by the following chemical formula 3; and a step of mixing the asphalt composition, aggregate, and filler.
[0024] [Chemical formula 1] [ka] [Chemical formula 2] [ka] [Chemical formula 3] [ka]
[0025] In the above Chemical Formulas 1 to 3, R is a C1-C30 hydrocarbyl or a C1-C30 heterohydrocarbyl; R 1 is C1-C30 alkyl, C1-C30 alkenyl, or C1-C30 alkynyl; R 2 ~R 4 are each independently hydrogen, C1-C30 alkyl, C1-C30 alkenyl, or C1-C30 alkynyl; R 5 or R 6 are independently hydrogen, C1-C30 alkyl, C1-C30 alkenyl, or C1-C30 alkynyl; R 5 and R 6 at least one of is C1-C30 alkyl, C1-C30 alkenyl, or C1-C30 alkynyl; m is an integer from 1 to 10; n is an integer from 0 to 20; The hydrocarbyl or heterohydrocarbyl of R and R 1 ~R4 The alkyl, alkenyl or alkynyl may be further substituted with one or more substituents selected from hydroxy, C1-C20 alkoxy, C1-C20 alkyl, carbonyl, halogen and amino groups.
[0026] According to one aspect of the present invention, the premixing step may include a step of preparing an additive by mixing a penetration modifier and an anti-stripping agent, and a step of preparing an asphalt composition by adding asphalt to the additive and stirring the mixture.
[0027] The asphalt composition according to one embodiment of the present invention may contain 0.05 to 10 parts by weight of a penetration modifier and 0.1 to 10 parts by weight of an anti-stripping agent relative to 100 parts by weight of asphalt. According to one aspect of the present invention, the mixing step may be carried out at 80 to 180°C. Effect of the Invention
[0028] The asphalt composition according to the present invention can simultaneously improve the moisture resistance and compactibility of the asphalt and aggregate, and can improve the productivity and workability of the asphalt mixture.
[0029] The asphalt composition according to the present invention uses an additive that increases only the penetration while maintaining the viscosity of the asphalt, thereby maintaining the resistance to plastic deformation and improving the road paving performance of the asphalt while satisfying the standards for asphalt for road paving.
[0030] When using the asphalt composition of the present invention, application can be performed at temperatures 20 to 50°C lower than the application temperatures of existing asphalt, which allows for faster work and therefore economical and environmentally friendly application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0031] The asphalt composition, asphalt mixture and its manufacturing method according to the present invention will be described in detail below. In this regard, unless otherwise defined, all technical and scientific terms have the meanings that are commonly understood by those having ordinary knowledge in the technical field to which the present invention belongs, and the terms used in the description of the present invention are merely for the purpose of effectively describing specific embodiments and are not intended to limit the present invention.
[0032] In the following description, the description of known effects and configurations that may unnecessarily obscure the gist of the present invention will be omitted. In the following description, units used without special mention are based on weight, and as an example, the unit of % or ratio means % by weight or weight ratio.
[0033] In addition, in describing components of the present invention, terms such as first, second, A, B(a), (b), etc. may be used. Such terms are merely used to distinguish the components from other components, and do not limit the essence, order, or sequence of the components.
[0034] Furthermore, as used herein, the singular forms "a," "an," and "the" are intended to include the plural forms as well, unless the context clearly indicates otherwise. In addition, "alkyl", "alkenyl" and "alkynyl" used in the present specification may include either a straight chain or a branched chain, and "alkenyl" and "alkynyl" are meant to include one or more unsaturated bonds, such as double bonds or triple bonds.
[0035] The present invention provides an asphalt composition comprising a penetration modifier represented by the following chemical formula 1, one or more anti-stripping agents selected from a compound represented by the following chemical formula 2 and a compound represented by the following chemical formula 3, and asphalt.
[0036] [Chemical formula 1] [ka] [Chemical formula 2] [ka] [Chemical formula 3] [ka]
[0037] In the above Chemical Formulas 1 to 3, R is C1-C30 hydrocarbyl or C1-C30 heterohydrocarbyl, R 1 is C1-C30 alkyl, C1-C30 alkenyl, or C1-C30 alkynyl; R 2 ~R 4 are each independently hydrogen, C1-C30 alkyl, C1-C30 alkenyl, or C1-C30 alkynyl; R 5 or R 6 are independently hydrogen, C1-C30 alkyl, C1-C30 alkenyl, or C1-C30 alkynyl; R 5 and R 6 at least one of R is C1-C30 alkyl, C1-C30 alkenyl, or C1-C30 alkynyl, m is an integer of 1 to 10, and n is an integer of 0 to 20; 1 ~R 4 The alkyl, alkenyl or alkynyl may be further substituted with one or more substituents selected from hydroxy, C1-C20 alkoxy, C1-C20 alkyl, carbonyl, halogen and amino groups.
[0038] Preferably, the R 2 ~R 4 is a C1-C7 alkyl, a C1-C7 alkenyl, or a C1-C7 alkynyl, wherein said alkyl, alkenyl, or alkynyl may be further substituted with one or more substituents selected from hydroxy, C1-C15 alkoxy, and carbonyl groups.
[0039] In a preferred embodiment of the present invention, the penetration modifier represented by Formula 1 may be a compound represented by Formula 4 below.
[0040] [Chemical formula 4] [ka]
[0041] In the above Chemical Formula 4, R' is a C1-C30 alkyl, a C1-C30 alkenyl, or a C1-C30 alkynyl, and the alkyl, alkenyl, or alkynyl of R' may be further substituted with one or more substituents selected from a hydroxy group, a carbonyl group, an alkoxy group, and a carboxy group, and q is 0 or 1.
[0042] Alternatively, in a preferred embodiment of the present invention, the penetration modifier represented by Formula 1 may be represented by Formula 5 below.
[0043] [Chemical formula 5] [ka]
[0044] In the above Chemical Formula 5, R″ is a C1-C30 alkyl, a C1-C30 alkenyl, or a C1-C30 alkynyl, and A is a C1-C5 alkylene, and the alkyl, alkenyl, or alkynyl of R″ and the alkylene of A may be further substituted with one or more substituents selected from a hydroxy group, a carbonyl group, an alkoxy group, and a carboxy group.
[0045] The asphalt composition according to the present invention has the effect of dramatically improving the mixability of asphalt and aggregate, compactibility and moisture resistance, thereby improving the productivity of asphalt mixtures and enhancing workability during construction.
[0046] In one embodiment of the present invention, the compound represented by Formula 2 is 1 is C1-C20 alkyl or C1-C20 alkenyl, R 2 ~R 4are each independently hydrogen or C1-C20 alkyl, and said alkyl or alkenyl may be further substituted with one or more selected from a hydroxy group, a C1-C15 alkoxy, a carbonyl, and an amino group.
[0047] In one embodiment of the present invention, the compound represented by Formula 2 is 1 is C1-C30 alkyl or C1-C30 alkenyl, R 2 ~R 4 are each independently hydrogen or C1-C3 alkyl, which may be substituted with a hydroxy group.
[0048] In one embodiment of the present invention, the compound represented by Chemical Formula 3 may be an organic phosphate mixture. The organic phosphate mixture refers to a mixture of two or more compounds having the same or different alkyl, alkenyl or alkynyl bonded to the oxygen atom of the ester functional group, and contains a phosphate group to exhibit acidity. Specific examples include a mixture of two different monophosphates, a mixture of two different diphosphates, a mixture of one monophosphate and one diphosphate, or a mixture of three or more different monophosphates and / or diphosphates.
[0049] In a preferred embodiment of the present invention, the compound represented by the chemical formula 3 may be a mixture of monophosphate ester and diphosphate ester having the same alkyl, alkenyl or alkynyl, and the molar ratio of the monophosphate ester and diphosphate ester may be 1:1 to 4:1. In this case, the adhesion between asphalt and aggregate and the effect of reducing peeling are excellent.
[0050] In one embodiment of the present invention, the asphalt composition may contain 0.05 to 10 parts by weight, preferably 0.1 to 8 parts by weight, more preferably 0.2 to 5 parts by weight of the penetration modifier relative to 100 parts by weight of asphalt. The anti-stripping agent may be contained in an amount of 0.1 to 10 parts by weight, preferably 0.2 to 8 parts by weight, more preferably 0.3 to 5 parts by weight relative to 100 parts by weight of asphalt. When the penetration modifier and anti-stripping agent are used as asphalt additives within the above ranges, they can economically increase the penetration while exhibiting excellent anti-stripping effects.
[0051] The asphalt may be any one or more selected from the group consisting of natural asphalt, petroleum asphalt, petroleum pitch, reclaimed asphalt, and modified asphalt, but is not particularly limited thereto.
[0052] The present invention provides an asphalt mixture including an asphalt composition, aggregate, and filler, which includes the above-mentioned technical concept. The aggregate may be a mixture of coarse aggregate, fine aggregate, etc., depending on the type of pavement to be constructed. Here, coarse aggregate refers to aggregate that passes through a 2.5 mm sieve, and means crushed stone (crushed stone), slag, or crushed gravel. Fine aggregate refers to aggregate that passes through a 2.5 mm sieve and passes through a 0.08 mm sieve, and means natural sand, crushed sand, or a mixture of both.
[0053] The filler may be any one or a mixture of two or more selected from the group consisting of stone powder, limestone powder, blast furnace slag powder, cellulose fiber, glass fiber, carbon black, fly ash, clay powder, light coal powder, hydrated lime, quicklime, cement, and steel dust, but is not particularly limited thereto, and other fillers may be included depending on the application of the asphalt mixture.
[0054] The asphalt composition according to one embodiment of the present invention may further contain additional additives in addition to the asphalt additive containing the penetration modifier and anti-stripping agent of the present invention, as long as the effects of the present invention are not impaired. Specific examples include asphalt modifiers, softeners, regenerators, penetration modifiers, antioxidants, heat stabilizers, antistatic agents, lubricants, and surfactants. If necessary, any one or more of these may be further contained.
[0055] The additional additives may be used without limitation as long as they are components commonly used in the industry, and may be used in an amount of 0.05 to 20 parts by weight, preferably 0.1 to 15 parts by weight, and more preferably 0.3 to 12 parts by weight, per 100 parts by weight of asphalt. The above ranges are sufficient to achieve the desired effects and are also economically preferable, but are not particularly limited thereto.
[0056] The asphalt modifier may be any one or a mixture of two or more selected from the group consisting of polymer-based modifiers and hydrocarbon-based modifiers. A specific example of the polymer modifier may be any one or a mixture of two or more selected from natural rubber, styrene-butadiene rubber copolymer, styrene-butadiene-styrene copolymer, polyethylene, polypropylene, nylon, vinyl chloride, ethylene methacrylate, ethylene propylene rubber, ethylene vinyl acetate copolymer, polybutadiene, polyisoprene, butyl rubber, styrene-butadiene rubber, polychloroprene rubber, recycled rubber from waste tires, etc., but is not limited thereto. The polymer modifier is not limited, but may have a weight average molecular weight of 20,000 to 600,000 g / mol.
[0057] In addition, examples of the hydrocarbon-based modifier may be any one or a mixture of two or more selected from the group consisting of wax-based asphalt additives, natural asphalt, petroleum pitch, and Gilsonite, but are not limited thereto.
[0058] The softener is a liquid or solid substance added to give flexibility to a product. In general, softeners can be classified into fatty oil-based, pine oil-based, tall oil, factice, petroleum-based, coal tar-based, synthetic resin-based, etc. The asphalt softener reinforces the aromatic component that acts as a dispersant for asphaltene among the components of asphalt, and improves the brittleness and low-temperature flexibility of aged asphalt.
[0059] The asphalt softener includes at least one of aromatic process oil having a high aromatic content and a low saturate content, vacuum residue (VR) of crude oil, and a product of a deasphaltene process of vacuum residue.
[0060] Similarly, the regenerative additive and the additionally added penetration modifier may comprise one or more selected from petroleum-based vacuum distillation process by-products, heavy oil fluidized bed catalytic cracking process by-products, deasphaltenization process by-products, lubricating oil-based and animal and plant-based fractions.
[0061] The surfactant may be a cationic, anionic, or amphoteric surfactant. Specific examples of the cationic surfactant include linear alkyl amine, linear alkyl ammonium, linear diamine, n-dodecyl pyridinium chloride, imidazole, and morpholine compound. Specific examples of the nonionic surfactant include ethoxylated alcohol, alkyl phenol, fatty acid ester, and nitrogenated nonionic surfactant. Specific examples of the anionic surfactant include sulfate, sulfonate, organo phosphorous surfactant, sarcoside, and alkyl amino acid. Examples of amphoteric surfactants include amino propionic acid, imido propionic acid, quaternized compounds, etc. The surfactant according to one embodiment of the present invention can also be used in the form of a mixture of two or more surfactants.
[0062] The asphalt mixture according to one embodiment of the present invention may be used in any one or more selected from the surface layer, intermediate layer, and base layer of asphalt concrete, but is not limited thereto.
[0063] The asphalt mixture according to one embodiment of the present invention may be used for asphalt concrete pavement selected from dense-graded asphalt concrete pavement, flow-resistant asphalt concrete pavement, coarse-graded asphalt concrete pavement, open-graded asphalt concrete pavement, drainage asphalt concrete pavement, and crushed stone mastic asphalt concrete pavement, but is not limited thereto.
[0064] The present invention also provides a method for producing an asphalt mixture, the method including: a premixing step of producing an asphalt composition containing asphalt, a penetration modifier represented by the following chemical formula 1, and one or more anti-stripping agents selected from the group consisting of a compound represented by the following chemical formula 2 and a compound represented by the following chemical formula 3; and a step of mixing the asphalt composition, aggregate, and filler.
[0065] [Chemical formula 1] [ka] [Chemical formula 2] [ka] [Chemical formula 3] [ka]
[0066] In the above Chemical Formulas 1 to 3, R is a C1-C30 hydrocarbyl or a C1-C30 heterohydrocarbyl; R 1 is C1-C30 alkyl, C1-C30 alkenyl, or C1-C30 alkynyl; R 2 ~R 4 are each independently hydrogen, C1-C30 alkyl, C1-C30 alkenyl, or C1-C30 alkynyl; R 5 or R 6are independently hydrogen, C1-C30 alkyl, C1-C30 alkenyl, or C1-C30 alkynyl; R 5 and R 6 at least one of is C1-C30 alkyl, C1-C30 alkenyl, or C1-C30 alkynyl; m is an integer from 1 to 10; n is an integer from 0 to 20; The hydrocarbyl or heterohydrocarbyl of R and R 1 ~R 4 The alkyl, alkenyl or alkynyl may be further substituted with one or more substituents selected from hydroxy, C1-C20 alkoxy, C1-C20 alkyl, carbonyl, halogen and amino groups.
[0067] The premixing step may include a step of preparing an additive by mixing a penetration modifier and an anti-stripping agent, and a step of preparing an asphalt composition by adding asphalt to the additive and stirring the mixture.
[0068] The asphalt composition may contain 0.05 to 10 parts by weight of a penetration regulator and 0.1 to 10 parts by weight of an anti-stripping agent relative to 100 parts by weight of asphalt. The step of mixing the asphalt composition, aggregate and filler may be carried out at 80 to 180°C.
[0069] In the case of general heated asphalt, aggregate is heated to 160-180°C and mixed with asphalt heated to 160-180°C as a binder, while warm-temperature asphalt is produced by lowering the temperature of aggregate and asphalt to 110-150°C. Since the asphalt composition according to the present invention contains the asphalt additive, the production temperature of the asphalt mixture can be lowered by 30-50°C compared to the existing temperature, and it is possible to provide a warm-temperature asphalt mixture that can be applied at 110-150°C in particular. In addition, it can be applied to asphalt for reducing potholes and asphalt for recycling waste asphalt.
[0070] In the case of the asphalt mixture of the present invention, the production temperature can be reduced, which significantly reduces CO2 emissions, making it environmentally friendly, and it has the advantage of allowing the pavement to be opened to traffic sooner by shortening the cooling time after construction.
[0071] When producing the asphalt mixture according to the present invention, the asphalt composition may contain 0.05 to 10 parts by weight, preferably 0.1 to 8 parts by weight, more preferably 0.2 to 5 parts by weight of the penetration modifier relative to 100 parts by weight of asphalt. The anti-stripping agent may be contained in an amount of 0.1 to 10 parts by weight, preferably 0.2 to 8 parts by weight, more preferably 0.3 to 5 parts by weight relative to 100 parts by weight of asphalt. When the penetration modifier and anti-stripping agent are used as asphalt additives within the above ranges, they can economically increase the penetration while exhibiting excellent anti-stripping effects.
[0072] The present invention will be described in more detail below with reference to the following examples. However, the following examples are merely a reference for explaining the present invention in detail, and the present invention is not limited thereto and may be realized in various forms.
[0073] [Production Example 1] Production of anti-stripping agent 1 1.30 g (21.63 mmol) of ethylenediamine and 10.50 g (43.32 mmol) of glycidyl lauryl ether were placed in a round-bottom flask and reacted at an internal temperature of 100° C. for 16 hours to produce the product.
[0074] [ka] 1 H NMR (500 MHz, CDCl3) δ 3.89-3.81 (m, 2H), 3.44-3.36 (m, 8H), 2.81-2.54 (m, 8H), 1.56-1.55 (m, 4H), 1.28-1.25 (m, 36H), 0.87 (t, J= 7.0 Hz, 6H).
[0075] [Production Example 2] Production of anti-stripping agent 2 The anti-stripping agent 2, N,N-bis(2-hydroxyethyl)oleylamine, was purchased from Zhangjiagang Halberdo Chemical Co., Ltd. and used. [ka]
[0076] [Production Example 3] Production of Anti-stripping Agent 3 Under a nitrogen atmosphere, 16.45g (107.28mmol) of phosphoryl chloride was placed in a round-bottom flask, and then 10.00g (53.67mmol) of 1-dodecanol was added at an internal temperature of 10°C or less, and the mixture was reacted for 3 hours at an internal temperature of 50°C. After cooling to room temperature, the reactant was poured into ice water, and diethyl ether was further added and thoroughly stirred. The layers were separated, the aqueous layer was removed, and the remaining organic layer was concentrated.
[0077] [ka] 1 H NMR (500 MHz, CDCl3) δ 10.63 (br, 2H), 4.07-4.05 (m, 2H), 1.70-1.65 (m, 2H), 1.36-1.26 (m, 18H), 0.88 (t, J= 6.8 Hz, 3H).
[0078] [Example 1] Production of Asphalt Composition 1 and Asphalt Mixture 1 1-1. Production of asphalt composition 1 0.3 parts by weight of oleyl alcohol and 0.5 parts by weight of anti-stripping agent 1 produced in Production Example 1 were added to 100 parts by weight of petroleum-based asphalt having a penetration index of 72 at 25°C, and the mixture was stirred at 140 to 150°C for 20 minutes at a speed of 500 rpm to produce asphalt composition 1. The penetration index and viscosity of the asphalt composition were measured and are shown in Table 1 below. Oleyl alcohol was purchased from Sigma-Aldrich Corporation.
[0079] 1-2. Preparation of asphalt mixture 1 and test specimens 5.0 wt% of the prepared asphalt composition and 95.0 wt% of granite gneiss aggregate (WC-2 grain size) were mixed at 130°C to prepare asphalt mixture 1. The asphalt mixture was compacted at 115°C to prepare test pieces, and the degree of compaction was measured and shown in Table 2 below.
[0080] [Example 2] Production of asphalt composition 2 and asphalt mixture 2 2-1. Production of asphalt composition 2 The same preparation as in Example 1-1 was carried out, except that antistripping agent 2 of Preparation Example 2 was used instead of antistripping agent 1 of Preparation Example 1 in Example 1-1.
[0081] 2-2. Preparation of asphalt mixture 2 and test specimens The same procedure as in Example 1-2 was repeated, except that the asphalt composition 2 of Example 2-1 was used instead of the asphalt composition 1 in Example 1-2.
[0082] [Example 3] Production of Asphalt Composition 3 and Asphalt Mixture 3 3-1. Production of asphalt composition 3 The same preparation as in Example 1-1 was carried out, except that oleic acid and anti-stripping agent 3 of Preparation Example 3 were used instead of oleyl alcohol and anti-stripping agent 1 of Preparation Example 1. Oleic acid was purchased from Sigma-Aldrich Corporation.
[0083] 3-2. Preparation of asphalt mixture 3 and test specimens The same procedure as in Example 1-2 was repeated, except that the asphalt composition 3 of Example 3-1 was used instead of the asphalt composition 1 of Example 1-2.
[0084] [Comparative Example 1] Manufacture of General Asphalt Mixture 4 (without additives) The same procedures as in Examples 1-2 to 3-2 were carried out except that, instead of the asphalt compositions 1 to 3 in Examples 1 to 3, general asphalt not containing the penetration regulators oleyl alcohol and oleic acid and the anti-stripping agents 1 to 3 and aggregate were mixed at 160°C to prepare asphalt mixture 4, and the asphalt mixture was compacted at 145°C.
[0085] [Comparative Examples 2 and 3] Preparation of Asphalt Compositions 5 and 6 and Asphalt Mixtures 5 and 6 without Penetration Adjuster The asphalt composition was prepared in the same manner as in Examples 1 and 2, except that oleyl alcohol was not added during the preparation of the asphalt composition.
[0086] [Comparative Example 4] Preparation of Asphalt Composition 7 and Asphalt Mixture 7 without Penetration Adjuster The asphalt composition was prepared in the same manner as in Example 3, except that oleic acid was not added during the preparation of the asphalt composition.
[0087] [Comparative Example 5] Preparation of Asphalt Composition 8 and Asphalt Mixture 8 without Antistripping Agent The asphalt composition was prepared in the same manner as in Example 1, except that the antistripping agent 1 was not added during the preparation of the asphalt composition.
[0088] [Comparative Example 6] Preparation of Asphalt Composition 9 and Asphalt Mixture 9 without Antistripping Agent The asphalt composition was prepared in the same manner as in Example 3, except that the antistripping agent 3 was not added during the preparation of the asphalt composition.
[0089] [Experimental Example 1] Evaluation of the penetration of asphalt composition According to the KS M 2252 bitumen material penetration test method, the penetration of the asphalt compositions of Examples 1-1 to 3-1 and Comparative Examples 1 to 4 was evaluated. The evaluation results are shown in Table 1 below.
[0090] It can be seen from Table 1 that in the case of the asphalt compositions of Examples 1-1 to 3-1, the penetration was improved by about 10% in comparison with the asphalt compositions of Comparative Examples 1 to 4.
[0091] [Experimental Example 2] Evaluation of viscosity of asphalt composition According to the absolute viscosity test method of asphalt KS M 2247, the viscosity of the asphalt compositions of Examples 1-1 to 3-1 and Comparative Examples 1 to 4 was evaluated. The evaluation results are shown in Table 1 below.
[0092] As can be seen from Table 1, there is almost no difference in viscosity between the asphalt compositions of Examples 1-1 to 3-1 and the asphalt compositions of Comparative Examples 1 to 4. This confirms that, in the case of the asphalt composition of the present invention, it is possible to provide a plastic deformation resistance maintenance effect by increasing only the penetration while maintaining the viscosity.
[0093] [Experimental Example 3] Evaluation of moisture resistance performance of asphalt mixture Based on the EN-12697-11 Determination of the Affinity between Aggregate and Bitumen experimental method, the coverage rate (%) after dynamic water immersion was evaluated. 510 g of 8-11.2 mm aggregate and 16 g of the asphalt composition of Examples 1 to 3 and Comparative Examples 1 to 6 were mixed for 2 minutes at the mixing temperature described in the Examples and Comparative Examples, and cooled at room temperature. Of these, 150 g of sample was taken and placed in a test glass bottle containing water, and rotated at a speed of 60 times per minute for 24 hours, after which the amount of asphalt coated on the aggregate was evaluated with the naked eye. The results are shown in Table 2 below.
[0094] As shown in Table 2, in the cases of Examples 1-2 to 3-2, the coverage rate after dynamic water immersion was about 5 times higher than that of Comparative Example 1, which did not use any of the penetration modifier and anti-stripping agent according to the present invention, and the coverage rate after dynamic water immersion was more than 5 times higher than that of Comparative Examples 5 and 6, which did not use any anti-stripping agent. From this, it can be confirmed that the moisture resistance performance was significantly improved in the case of the asphalt mixture containing all of the penetration modifier and anti-stripping agent according to the present invention.
[0095] [Experimental Example 4] Evaluation of warm-temperature performance of asphalt mixture (degree of compaction) The asphalt mixture specimens were manufactured based on the ASTM D6925 Standard Test Method for Preparation and Determination of the Relative Density of Asphalt Mix Specimens by Means of the Superpave Gyratory Compactor test method. The mixture was compacted based on the compaction method and density calculation method for asphalt mixtures using the KS F 2377 gyratory compaction tester, and the porosity of the mixture was calculated. The compaction degree was calculated as the ratio of the porosity of the heated asphalt mixture, which was mixed at 160°C using ordinary asphalt without additives and compacted at 145°C, to the porosity of the warm asphalt mixture, which was mixed at 130°C using asphalt with additives and compacted at 115°C.
number
[0096] The compaction degree is a standard for evaluating the compaction effect of warm-mix asphalt proposed by the Ministry of Land, Infrastructure and Transport of the Republic of Korea, and in order to meet the W64 standard for warm-mix asphalt mixtures, the compaction degree must be 1 or less. The results are shown in Table 2 below.
[0097] [Experimental Example 5] Evaluation of plastic deformation resistance of asphalt mixture The wheel tracking test method for asphalt mixtures was used as the standard. Specifically, asphalt and aggregate were mixed at 125°C for 2 minutes, then placed in a mold measuring 300×300×50mm in width×length×height, and compacted at 115°C to a pore size of 4±1% to prepare a test specimen. The number of wheel passes required to deform 1mm after 45 minutes at a temperature of 60°C was evaluated. The results are shown in Table 2 below.
[0098] In the case of Examples 1-2 to 3-2 according to the present invention, it can be confirmed that the viscosity is maintained while the penetration is improved and the plastic deformation resistance is improved.
[0099] [Table 1]
[0100] [Table 2]
[0101] Although the preferred embodiment of the present invention has been described above, the present invention is not limited thereto, and can be embodied in various modified forms within the scope of the claims, the description of the invention, and the accompanying drawings, which also fall within the scope of the present invention.
Claims
1. An asphalt composition comprising: a penetration modifier including oleyl alcohol or oleic acid; one or more anti-stripping agents selected from the group consisting of a compound represented by the following chemical formula 2A, a compound represented by the following chemical formula 2, and a compound represented by the following chemical formula 3A; and asphalt. [Chemical formula 2A] [Case 1] [Chemical formula 2] [chemical 2] In the above Chemical Formula 2, R 1 is C1-C30 alkyl or C2-C30 alkenyl, R 3 and R 4 are each independently selected from C1-C30 alkyl, 3 and R 4 wherein the alkyl is further substituted with hydroxy; The n is 0. [Chemical formula 3A] [C3]
2. The compound represented by Chemical Formula 2 is a compound represented by Chemical Formula 2B below. The asphalt composition according to claim 1. [Chemical formula 2B] [C4]
3. The asphalt composition according to claim 1, wherein the penetration modifier is contained in an amount of 0.05 to 10 parts by weight per 100 parts by weight of asphalt.
4. The asphalt composition according to claim 1, wherein the anti-stripping agent is contained in an amount of 0.1 to 10 parts by weight per 100 parts by weight of asphalt.
5. The asphalt composition according to claim 1, wherein the asphalt is any one or more selected from the group consisting of natural asphalt, petroleum asphalt, petroleum pitch, reclaimed asphalt, and modified asphalt.
6. An asphalt mixture comprising the asphalt composition of any one of claims 1 to 5, aggregate and filler.
7. A pre-mixing step of preparing an asphalt composition including asphalt, a penetration modifier including oleyl alcohol or oleic acid, and at least one anti-stripping agent selected from the group consisting of a compound represented by the following formula 2A, a compound represented by the following formula 2, and a compound represented by the following formula 3A; and mixing the asphalt composition, aggregate, and filler. [Chemical formula 2A] [C5] [Chemical formula 2] [C6] In the above Chemical Formula 2, R 1 is C1-C30 alkyl or C2-C30 alkenyl, R 3 and R 4 are each independently selected from C1-C30 alkyl, 3 and R 4 wherein the alkyl is further substituted with hydroxy; The n is 0. [Chemical formula 3A] [C7]
8. The premixing step includes a step of preparing an additive by mixing a penetration regulator and an anti-stripping agent, and a step of preparing an asphalt composition by adding asphalt to the additive and stirring the mixture. The method for preparing an asphalt mixture according to claim 7.
9. The method for producing an asphalt mixture according to claim 7, wherein the asphalt composition contains 0.05 to 10 parts by weight of a penetration regulator and 0.1 to 10 parts by weight of an anti-stripping agent relative to 100 parts by weight of asphalt.
10. The method for producing an asphalt mixture according to claim 7, wherein the mixing step is carried out at 80 to 180°C.
Citation Information
Patent Citations
JP1974006174A
Asphalt emulsion
JP1982042763A
Additive composition for asphalt
JP2000143993A
Additive for heated asphalt