Resin composition, its manufacturing method, and manufacturing method of pattern-forming composition
By adding antioxidants to resin compositions containing polyimide or polybenzoxazole precursors and controlling solvent content, the resin compositions achieve enhanced filterability and pattern formation, addressing the challenges of polymerization-induced issues in existing technologies.
Patent Information
- Application Number
- JP2022528888
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-06-05
- Filing Date
- 2021-06-03
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2041-06-03
AI Technical Summary
Existing resin compositions containing polymerizable groups face challenges in filterability when redissolved in solvents and the ability to form fine patterns, particularly in powder, granule, or pellet forms, due to polymerization issues that hinder effective pattern formation.
Incorporating an antioxidant with a content of 0.1 mass ppm to 10,000 mass ppm in resin compositions comprising polyimide or polybenzoxazole precursors, along with a controlled amount of organic solvent, to suppress polymerization and enhance filterability and pattern formation properties.
The resin composition exhibits excellent filterability and pattern forming capabilities when redissolved in solvents, enabling the formation of finer patterns by preventing excessive polymerization, thus improving the quality and efficiency of pattern formation processes.
Smart Images

Figure 0007595076000001 
Figure 0007595076000002 
Figure 0007595076000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition, a method for producing the same, and a method for producing a pattern-forming composition. [Background technology]
[0002] 2. Description of the Related Art Conventionally, a resin having a polymerizable group has been synthesized in an organic solvent to obtain a synthesis reaction liquid containing the resin having a polymerizable group. The resin may be used in the form of a powdery, granular or pellet-like resin composition containing the resin and the organic solvent, obtained by removing a portion of the organic solvent from the synthesis reaction liquid by drying. For example, when preparing a composition such as a pattern-forming composition containing the above-mentioned resin, a method of redissolving the above-mentioned resin composition in a solvent may be used.
[0003] For example, Patent Document 1 describes a light emitting device comprising a reflector and a lead frame embedded in the reflector, a base having a recess with a part of the lead frame exposed at the bottom of the recess, a light emitting element mounted in the recess of the base, and a sealant filled in the recess of the base and sealing the light emitting element, wherein a region of the surface of the lead frame in contact with the reflector has a roughened surface with an Ra in the range of 0.5 to 1.5 μm, and the reflector is a molded body of a resin composition containing silica powder with an average particle size of 9 to 25 μm and a proportion of particles with a particle size of 6 μm or less of 25 to 40 volume %. Patent Document 2 describes a thermosensitive color-changing resin composition obtained by incorporating microcapsules encapsulating a reversible thermochromic coloring material, an ultraviolet absorbing agent, and an antioxidant into a resin. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2018-107360 A [Patent Document 2] Japanese Patent Application Publication No. 7-331090 Summary of the Invention [Problem to be solved by the invention]
[0005] There is a demand for improved filterability of a powder, granule or pellet-like resin composition containing a resin having a polymerizable group when redissolved in a solvent. Furthermore, in a pattern-forming composition prepared by redissolving the above-mentioned resin composition, it is required that a finer pattern can be formed. In the present invention, the ability of the pattern-forming composition to form a finer pattern is also referred to as "having excellent pattern-forming ability."
[0006] The present invention aims to provide a resin composition that is excellent in filterability when redissolved in a solvent and in pattern formability when a pattern-forming composition is prepared by redissolving the resin composition, and a method for producing the resin composition and a method for producing a pattern-forming composition. [Means for solving the problem]
[0007] Examples of typical embodiments of the present invention are given below. <1> At least one resin selected from the group consisting of polyimide precursors and polybenzoxazole precursors, the resin containing a polymerizable group, an antioxidant, and an organic solvent. the content of the antioxidant is 0.1 ppm by mass to 10,000 ppm by mass relative to the content of the resin, In powder, granule or pellet form Resin composition. <2> The content of the organic solvent is more than 0 and 10 mass% or less with respect to the total mass of the resin composition. <1> The resin composition according to claim 1. <3> The total content of the resin, the antioxidant, and the organic solvent is 95% by mass or more based on the total mass of the resin composition. <1> or <2> The resin composition according to claim 1. <4> The resin includes a polyimide precursor. <1> ~ <3> 10. The resin composition according to claim 9 . <5> The resin contains a repeating unit represented by the following formula (2) or (3): <1> ~ <4> 10. The resin composition according to claim 9 . Formula (2) [ka] Formula (3) [ka] In formula (2), A 1 and A 2 each independently represents an oxygen atom or NH; R 111 represents a divalent organic group, R 115 represents a tetravalent organic group, R 113 and R 114 each independently represents a hydrogen atom or a monovalent organic group, In formula (3), R 121 represents a divalent organic group, R 122 represents a tetravalent organic group, R 123 and R 124 each independently represents a hydrogen atom or a monovalent organic group. <6> The polymerizable group is a radical polymerizable group. <1> ~ <5> 10. The resin composition according to claim 9 . <7> The oxidation-reduction potential of the antioxidant is 0.91 V or less. <1> ~ <6> 10. The resin composition according to claim 9 . <8> The antioxidant contains at least one compound selected from the group consisting of a phenol-based compound, an alcohol-based compound, an aldehyde-based compound, an amine-based compound, a nitroso-based compound, a phosphorus-based compound, a sulfur-based compound, and a ketone-based compound. <1> ~ <7> 10. The resin composition according to claim 9 . <9> The antioxidant is a phenolic compound having an unsaturation degree of 1 or more, or an alcoholic compound having an unsaturation degree of 1 or more. <1> ~ <8> 10. The resin composition according to claim 9 . <10> The organic solvent contains at least one selected from the group consisting of hydrocarbon compounds, alcohol compounds, carboxylic acids, ketone compounds, ester compounds, ether compounds, nitrile compounds, amide compounds, amine compounds, sulfone compounds, and sulfoxide compounds. <1> ~ <9> 10. The resin composition according to claim 9 . <11> <1> ~ <10> A method for producing the resin composition according to any one of the above, A method for producing a resin composition, comprising: adding the antioxidant to a production composition containing the organic solvent and the resin. <12> A synthesis step of reacting raw materials in a solvent to obtain a reaction solution containing the resin; and a reprecipitation / redissolution step of reprecipitating the resin in the reaction solution and redissolving the reprecipitated resin in the organic solvent to obtain a resin solution, The resin solution is used as the manufacturing composition to carry out the adding step. <11> A method for producing the resin composition according to claim 1. <13> A reprecipitation step of reprecipitating the resin after the adding step is included. <11> or <12> A method for producing the resin composition according to claim 1. <14> After the reprecipitation step, a drying step is performed to remove the organic solvent. <13> A method for producing the resin composition according to claim 1. <15> <1> ~ <10> The method includes a mixing step of mixing the resin composition according to any one of the above with a solvent. A method for producing a pattern-forming composition. <16> In the mixing step, a photosensitizer is further mixed. <15> A method for producing the pattern-forming composition according to claim 1. Effect of the Invention
[0008] According to the present invention, there are provided a resin composition which is excellent in filterability when redissolved in a solvent and in pattern formability when a pattern-forming composition is prepared by redissolving the resin composition, a method for producing the resin composition, and a method for producing a pattern-forming composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The main embodiments of the present invention will be described below, however, the present invention is not limited to the embodiments explicitly described. In this specification, a numerical range expressed using the symbol "to" means a range that includes the numerical values before and after "to" as the lower limit and upper limit, respectively. In this specification, the term "process" includes not only an independent process but also a process that cannot be clearly distinguished from other processes, so long as the process can achieve its intended effect. In the description of groups (atomic groups) in this specification, when there is no indication of whether they are substituted or unsubstituted, the term encompasses both groups (atomic groups) that have no substituents and groups (atomic groups) that have a substituent. For example, the term "alkyl group" encompasses not only alkyl groups that have no substituents (unsubstituted alkyl groups) but also alkyl groups that have a substituent (substituted alkyl groups). In this specification, unless otherwise specified, the term "exposure" includes not only exposure using light but also exposure using particle beams such as electron beams and ion beams. Examples of light used for exposure include the bright line spectrum of a mercury lamp, far ultraviolet light represented by an excimer laser, extreme ultraviolet light (EUV light), X-rays, electron beams, and other actinic rays or radiation. In this specification, "(meth)acrylate" means both or either of "acrylate" and "methacrylate", "(meth)acrylic" means both or either of "acrylic" and "methacrylic", and "(meth)acryloyl" means both or either of "acryloyl" and "methacryloyl". In this specification, Me in the structural formulae represents a methyl group, Et represents an ethyl group, Bu represents a butyl group, and Ph represents a phenyl group. In this specification, the total solid content refers to the total mass of all components of the composition excluding the solvent, and in this specification, the solid content concentration refers to the mass percentage of the other components excluding the solvent with respect to the total mass of the composition. In this specification, the weight average molecular weight (Mw) and the number average molecular weight (Mn) are defined as polystyrene equivalent values according to gel permeation chromatography (GPC measurement) unless otherwise specified. In this specification, the weight average molecular weight (Mw) and the number average molecular weight (Mn) can be determined, for example, by using HLC-8220GPC (manufactured by Tosoh Corporation) and guard columns HZ-L, TSKgel Super HZM-M, TSKgel Super HZ4000, TSKgel Super HZ3000, and TSKgel Super HZ2000 (manufactured by Tosoh Corporation). Unless otherwise specified, these molecular weights are measured using THF (tetrahydrofuran) as an eluent. In addition, detection in GPC measurement is performed using a UV ray (ultraviolet ray) detector at a wavelength of 254 nm unless otherwise specified. In this specification, when the positional relationship of each layer constituting the laminate is described as "upper" or "lower", it is sufficient that there is another layer above or below the reference layer among the multiple layers being noted. In other words, a third layer or element may be interposed between the reference layer and the other layer, and the reference layer does not need to be in contact with the other layer. In addition, unless otherwise specified, the direction in which the layers are stacked on the substrate is referred to as "upper", or, in the case of a photosensitive layer, the direction from the substrate to the photosensitive layer is referred to as "upper", and the opposite direction is referred to as "lower". Note that such a vertical direction is set for the convenience of this specification, and in an actual embodiment, the "upper" direction in this specification may be different from the vertical upward direction. In this specification, unless otherwise specified, the composition may contain, as each component contained in the composition, two or more compounds corresponding to that component. Furthermore, unless otherwise specified, the content of each component in the composition means the total content of all compounds corresponding to that component. In this specification, unless otherwise specified, the temperature is 23° C., the atmospheric pressure is 101,325 Pa (1 atm), and the relative humidity is 50% RH. As used herein, combinations of preferred aspects are more preferred aspects.
[0010] (Resin composition) The resin composition of the present invention is at least one resin selected from the group consisting of polyimide precursors and polybenzoxazole precursors, and contains a resin having a polymerizable group (hereinafter also referred to as a "specific resin"), an antioxidant, and an organic solvent, the content of the antioxidant being 0.1 ppm by mass to 10,000 ppm by mass relative to the content of the resin, and is in the form of a powder, granules, or pellets.
[0011] The resin composition of the present invention is excellent in filterability when redissolved in a solvent, and in pattern formability when a pattern-forming composition is prepared. The mechanism by which the above effects are obtained is unclear, but is speculated to be as follows.
[0012] In a powdery, granular, or pellet-like composition containing a resin having a polymerizable group and an organic solvent, polymerization of the polymerizable group contained in the resin having a polymerizable group may proceed due to peroxides contained in the organic solvent, or peroxides generated from the powder or pellets during production or storage of the powder, granules, or pellets. In this way, since polymerization proceeds in the powdery, granular, or pellet-like composition, when the powdery, granular, or pellet-like composition is redissolved in a solvent, the filterability may be reduced in some cases. In particular, polyimide precursors or polybenzoxazole precursors (particularly polyimide precursors) have low solubility in solvents, and if the polymerization of the resin proceeds as described above, the filterability of the composition after redissolution may be significantly reduced. Therefore, the present inventors conducted extensive research and found that the filterability can be improved by adding an antioxidant to the composition in an amount of 0.1 ppm by mass or more relative to the content of the specific resin. This is presumably because when the antioxidant is present at 0.1 ppm by mass or more, the polymerization of the above-mentioned polymerizable groups is suppressed. In addition, it has been found that, by setting the content of the antioxidant to 10,000 ppm by mass or less relative to the content of the resin, excellent pattern formability is achieved even in the case where the powdery, granular or pellet-like composition is dissolved in a solvent to prepare a pattern-forming composition. This is presumably because, by setting the content of the antioxidant within the above range, polymerization in the pattern-forming composition is prevented from being excessively suppressed.
[0013] Here, Patent Documents 1 and 2 do not describe or suggest that a powdery, granular, or pellet-like resin composition contains an antioxidant at a specific content.
[0014] In the present invention, the resin composition being in a powder form means that the resin composition is in the form of fine solid particles, the average length in the major axis direction of which is less than 30 μm. In the present invention, the resin composition being in the form of particles means that the resin composition is in the form of fine solid particles, the average length in the major axis direction of which is 30 μm or more and 1 mm or less. Furthermore, the particulate resin may come into contact with each other and aggregate to form larger particles, or an aggregate that is a mass containing the particulate resin may be formed. The resin composition being in the form of pellets means that the resin composition is molded into a lump. The size of the pellets is not particularly limited, and may be determined depending on the application of the resin composition. The components contained in the curable resin composition of the present invention will be described in detail below.
[0015] <Specific resin> The resin composition of the present invention contains at least one resin (specific resin) having a polymerizable group, which is selected from the group consisting of polyimide precursors and polybenzoxazole precursors. The polyimide precursor and the polybenzoxazole precursor are cyclized, for example, by heating or chemical treatment, to form polyimide and polybenzoxazole, respectively. Since polyimide or polybenzoxazole has excellent heat resistance, insulating properties, and the like, when the resin composition of the present invention contains a specific resin, the pattern-forming composition obtained by redissolving the resin composition of the present invention in a solvent can be applied to various applications. The above-mentioned uses are not particularly limited, but in the case of semiconductor devices for mounting, the use thereof can be, for example, as an insulating film, a sealing material, or a protective film, and can also be used as a base film or coverlay for flexible substrates.
[0016] Examples of the polymerizable group include known polymerizable groups such as a radical polymerizable group, an epoxy group, an oxetanyl group, a methylol group, and an alkoxymethyl group, and the radical polymerizable group is preferred. The radically polymerizable group is preferably a group having an ethylenically unsaturated bond. Examples of the group having an ethylenically unsaturated bond include a group having an optionally substituted vinyl group directly bonded to an aromatic ring, such as a vinyl group, an allyl group, or a vinylphenyl group, a (meth)acrylamide group, or a (meth)acryloyloxy group, with a (meth)acryloyloxy group being preferred.
[0017] The resin composition of the present invention more preferably contains a polyimide precursor as the specific resin. Moreover, the resin of the present invention preferably contains a repeating unit represented by formula (2) or formula (3) described below, and more preferably contains a repeating unit represented by formula (2).
[0018] [Polyimide precursor] The polyimide precursor used in the present invention is not particularly limited in terms of its type, but it preferably contains a repeating unit represented by the following formula (2). The polyimide precursor used in the present invention has a polymerizable group. The polymerizable group may be contained in a repeating unit represented by the following formula (2), may be contained in another repeating unit, or may be contained at the end of a polyimide precursor. One of the preferred embodiments of the present invention is an embodiment in which the polymerizable group is contained in a repeating unit represented by the following formula (2). 111 , R 113 or R 114 In a preferred embodiment, at least one of R 113 or R 114 It is more preferable that at least one of R 113 and R 114 is a polymerizable group. Formula (2) [ka] In formula (2), A 1 and A 2 each independently represents an oxygen atom or NH; R 111 represents a divalent organic group, R 115 represents a tetravalent organic group, R 113 and R 114 each independently represents a hydrogen atom or a monovalent organic group.
[0019] A in Equation (2) 1 and A 2 each independently represents an oxygen atom or NH, and an oxygen atom is preferred. R in Equation (2) 111 represents a divalent organic group. Examples of the divalent organic group include a linear or branched aliphatic group, a cyclic aliphatic group, and a group containing an aromatic group. A linear or branched aliphatic group having 2 to 20 carbon atoms, a cyclic aliphatic group having 6 to 20 carbon atoms, an aromatic group having 6 to 20 carbon atoms, or a group consisting of a combination thereof is preferred, and a group containing an aromatic group having 6 to 20 carbon atoms is more preferred. A particularly preferred embodiment of the present invention is a group represented by -Ar-L-Ar-, where each Ar is independently an aromatic group, and L is an aliphatic hydrocarbon group having 1 to 10 carbon atoms which may be substituted with a fluorine atom, -O-, -CO-, -S-, -SO 2 - or NHCO-, or a group consisting of a combination of two or more of the above. The preferred ranges of these are as described above.
[0020] R 111 is preferably derived from a diamine. Examples of diamines used in the production of the polyimide precursor include linear or branched aliphatic, cyclic aliphatic or aromatic diamines. Only one type of diamine may be used, or two or more types may be used. Specifically, it is preferable that the diamine contains a linear or branched aliphatic group having 2 to 20 carbon atoms, a cyclic aliphatic group having 6 to 20 carbon atoms, an aromatic group having 6 to 20 carbon atoms, or a group consisting of a combination thereof, and it is more preferable that the diamine contains a group consisting of an aromatic group having 6 to 20 carbon atoms. Examples of the aromatic group include the following.
[0021] [ka] In the formula, A is a single bond, an aliphatic hydrocarbon group having 1 to 10 carbon atoms which may be substituted with a fluorine atom, -O-, -C(=O)-, -S-, -SO 2 -, NHCO-, or a combination thereof, and is preferably a single bond, an alkylene group having 1 to 3 carbon atoms which may be substituted with a fluorine atom, -O-, -C(=O)-, -S-, or -SO 2 -, more preferably a group selected from -CH 2 -, -O-, -S-, -SO 2 -, -C(CF 3 ) 2 - or -C(CH 3 ) 2 It is even more preferable that In the formula, * represents a bonding site with another structure.
[0022] Specific examples of diamines include 1,2-diaminoethane, 1,2-diaminopropane, 1,3-diaminopropane, 1,4-diaminobutane, and 1,6-diaminohexane; 1,2- or 1,3-diaminocyclopentane, 1,2-, 1,3-, or 1,4-diaminocyclohexane, 1,2-, 1,3-, or 1,4-bis(aminomethyl)cyclohexane, bis-(4-aminocyclohexyl)methane, bis-(3-aminocyclohexyl)methane, 4,4'-diamino-3,3'-dimethylcyclohexylmethane, and isophoronediamine; m- or p-phenylenediamine, diaminotoluene, 4,4'- or 3,3'-diaminobiphenyl, 4,4'-diaminodiphenyl ether, 3,3-diaminodiphenyl ether, 4,4'- and 3,3'-diaminodiphenylmethane, 4,4'- and 3,3'-diaminodiphenyl sulfone, 4,4'- and 3,3'-diaminodiphenyl sulfide, 4,4'- or 3,3'-diaminobenzophenone, 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dimethoxy-4,4'- Diaminobiphenyl, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-aminophenyl)hexafluoropropane, 2,2-bis(3-hydroxy-4-aminophenyl)propane, 2,2-bis(3-hydroxy-4-aminophenyl)hexafluoropropane, 2,2-bis(3-amino-4-hydroxyphenyl)propane, 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, bis(3-amino-4-hydroxyphenyl)sulfone, bis(4-amino-3-hydroxyphenyl)sulfone, 4 ,4'-Diaminoparaterphenyl, 4,4'-bis(4-aminophenoxy)biphenyl, bis[4-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(2-aminophenoxy)phenyl]sulfone, 1,4-bis(4-aminophenoxy)benzene, 9,10-bis(4-aminophenyl)anthracene, 3,3'-dimethyl-4,4'-diaminodiphenylsulfone, 1,3-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene, 1,3-Bis(4-aminophenyl)benzene, 3,3'-diethyl-4,4'-diaminodiphenylmethane, 3,3'-dimethyl-4,4'-diaminodiphenylmethane, 4,4'-diaminooctafluorobiphenyl, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 9,9-bis(4-aminophenyl)-10-hydroanthracene, 3,3',4,4'-tetraaminobiphenyl, 3,3',4,4'-tetraaminodiphenyl ether, 1 ,4-diaminoanthraquinone, 1,5-diaminoanthraquinone, 3,3-dihydroxy-4,4'-diaminobiphenyl, 9,9'-bis(4-aminophenyl)fluorene, 4,4'-dimethyl-3,3'-diaminodiphenyl sulfone, 3,3',5,5'-tetramethyl-4,4'-diaminodiphenylmethane, 2,4- and 2,5-diaminocumene, 2,5-dimethyl-p-phenylenediamine, acetoguanamine, 2,3,5,6-tetramethyl-p-phenylenediamine, 2,4,6-trimethyl-m-phenylenediamine, bis( 3-aminopropyl)tetramethyldisiloxane, 2,7-diaminofluorene, 2,5-diaminopyridine, 1,2-bis(4-aminophenyl)ethane, diaminobenzanilide, esters of diaminobenzoic acid, 1,5-diaminonaphthalene, diaminobenzotrifluoride, 1,3-bis(4-aminophenyl)hexafluoropropane, 1,4-bis(4-aminophenyl)octafluorobutane, 1,5-bis(4-aminophenyl)decafluoropentane, 1,7-bis(4-aminophenyl)tetradecafluoroheptane, 2,2- Bis[4-(3-aminophenoxy)phenyl]hexafluoropropane, 2,2-bis[4-(2-aminophenoxy)phenyl]hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)-3,5-dimethylphenyl]hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)-3,5-bis(trifluoromethyl)phenyl]hexafluoropropane, p-bis(4-amino-2-trifluoromethylphenoxy)benzene, 4,4'-bis(4-amino-2-trifluoromethylphenoxy)biphenyl, 4,At least one diamine selected from 4'-bis(4-amino-3-trifluoromethylphenoxy)biphenyl, 4,4'-bis(4-amino-2-trifluoromethylphenoxy)diphenyl sulfone, 4,4'-bis(3-amino-5-trifluoromethylphenoxy)diphenyl sulfone, 2,2-bis[4-(4-amino-3-trifluoromethylphenoxy)phenyl]hexafluoropropane, 3,3',5,5'-tetramethyl-4,4'-diaminobiphenyl, 4,4'-diamino-2,2'-bis(trifluoromethyl)biphenyl, 2,2',5,5',6,6'-hexafluorotolidine, and 4,4'-diaminoquaterphenyl can be mentioned.
[0023] Also preferred are the diamines (DA-1) to (DA-18) described in paragraphs 0030 to 0031 of WO 2017 / 038598.
[0024] In addition, the following diamines can also be suitably used. [ka]
[0025] In addition, diamines having two or more alkylene glycol units in the main chain described in paragraphs 0032 to 0034 of WO 2017 / 038598 are also preferably used.
[0026] R 111 From the viewpoint of flexibility of the obtained organic film, it is preferably represented by -Ar-L-Ar-, where each Ar is independently an aromatic group, and L is an aliphatic hydrocarbon group having 1 to 10 carbon atoms which may be substituted with a fluorine atom, -O-, -CO-, -S-, -SO 2 Ar is preferably a phenylene group, and L is preferably an aliphatic hydrocarbon group having 1 or 2 carbon atoms which may be substituted with a fluorine atom, -O-, -CO-, -S- or SO 2 The aliphatic hydrocarbon group here is preferably an alkylene group.
[0027] Also, R 111 From the viewpoint of i-line transmittance, it is preferable that the divalent organic group represented by the following formula (51) or formula (61) is used. In particular, from the viewpoint of i-line transmittance and ease of availability, it is more preferable that the divalent organic group represented by the formula (61) is used. Formula (51) [ka] In formula (51), R 50 ~R 57 are each independently a hydrogen atom, a fluorine atom, or a monovalent organic group; R 50 ~R 57 At least one of is a fluorine atom, a methyl group, or a trifluoromethyl group. R 50 ~R 57 Examples of the monovalent organic group include an unsubstituted alkyl group having 1 to 10 carbon atoms (preferably 1 to 6 carbon atoms) and a fluorinated alkyl group having 1 to 10 carbon atoms (preferably 1 to 6 carbon atoms). [ka] In formula (61), R 58 and R 59 are each independently a fluorine atom or a trifluoromethyl group. Examples of the diamine compound giving the structure of formula (51) or (61) include 2,2'-dimethylbenzidine, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 2,2'-bis(fluoro)-4,4'-diaminobiphenyl, 4,4'-diaminooctafluorobiphenyl, etc. These may be used alone or in combination of two or more.
[0028] Also, R 111 may be a structure containing a polymerizable group. For example, R 111 can also be a structure derived from a diamine compound having a polymerizable group. The diamine compound having a polymerizable group is not particularly limited, but is preferably a compound containing an aromatic ring structure, and more preferably a compound having a structure in which a structure containing an amino group and a polymerizable group is directly bonded to the aromatic ring structure. As the polymerizable group, a group having an ethylenically unsaturated bond, a cyclic ether group, a group containing a methylol group or an alkoxymethyl group is preferred, a vinyl group, a (meth)allyl group, a (meth)acrylamide group, a (meth)acryloxy group, a maleimide group, a vinylphenyl group, an epoxy group, an oxetanyl group, a methylol group or an alkoxymethyl group is more preferred, and a (meth)acryloxy group, a (meth)acrylamide group, an epoxy group, a methylol group or an alkoxymethyl group is even more preferred.
[0029] R in Equation (2) 115 represents a tetravalent organic group. As the tetravalent organic group, a tetravalent organic group containing an aromatic ring is preferable, and a group represented by the following formula (5) or formula (6) is more preferable. In formula (5) or formula (6), each * independently represents a bonding site to another structure. [ka] In formula (5), R 112 represents a single bond, an aliphatic hydrocarbon group having 1 to 10 carbon atoms which may be substituted with a fluorine atom, -O-, -CO-, -S-, -SO 2 -, NHCO-, and combinations thereof are preferred, and examples thereof include a single bond, an alkylene group having 1 to 3 carbon atoms which may be substituted with a fluorine atom, -O-, -CO-, -S-, and SO 2 -, more preferably a group selected from -CH 2 -, -C(CF 3 ) 2 -, -C(CH 3 ) 2 -, -O-, -CO-, -S- and SO 2 It is more preferably a divalent group selected from the group consisting of -.
[0030] R 115Specifically, the tetracarboxylic acid residue remaining after removal of the anhydride group from the tetracarboxylic acid dianhydride can be mentioned. Only one type of tetracarboxylic acid dianhydride may be used, or two or more types of tetracarboxylic acid dianhydrides may be used. The tetracarboxylic dianhydride is preferably represented by the following formula (O). [ka] In formula (O), R 115 R represents a tetravalent organic group. 115 The preferred range of R in formula (2) is 115 The same definition and preferred range are also the same.
[0031] Specific examples of tetracarboxylic dianhydrides include pyromellitic dianhydride (PMDA), 3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-diphenylsulfide tetracarboxylic dianhydride, 3,3',4,4'-diphenylsulfone tetracarboxylic dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 3,3',4,4'-diphenylmethane tetracarboxylic dianhydride, 2,2 ',3,3'-Diphenylmethanetetracarboxylic dianhydride, 2,3,3',4'-Biphenyltetracarboxylic dianhydride, 2,3,3',4'-Benzophenonetetracarboxylic dianhydride, 4,4'-oxydiphthalic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 1,4,5,7-naphthalenetetracarboxylic dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, 2,2-bis(2, 1,3-diphenylhexafluoropropane-3,3,4,4-tetracarboxylic dianhydride, 1,4,5,6-naphthalenetetracarboxylic dianhydride, 2,2',3,3'-diphenyltetracarboxylic dianhydride, 3,4,9,10-perylenetetracarboxylic dianhydride, 1,2,4,5-naphthalenetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, 1,8,9,10-phenanthrenetetracarboxylic dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride, 1,1-bis(3,4-dicarboxyphenyl)ethane dianhydride, 1,2,3,4-benzenetetracarboxylic dianhydride, and their alkyl and alkoxy derivatives having 1 to 6 carbon atoms.
[0032] Further, preferred examples include the tetracarboxylic dianhydrides (DAA-1) to (DAA-5) described in paragraph 0038 of WO 2017 / 038598.
[0033] R 111 and R 115 It is also preferable that at least one of R111 Examples of the residue include residues of bisaminophenol derivatives.
[0034] R 113 and R 114 each independently represents a hydrogen atom or a monovalent organic group; R 113 and R 114 It is preferable that at least one of the above contains a polymerizable group, and it is more preferable that both of the above contain a polymerizable group. The polymerizable group is a group capable of undergoing a crosslinking reaction by the action of heat, radicals, etc., and is preferably a radically polymerizable group. Specific examples of the polymerizable group in the specific resin include a group having an ethylenically unsaturated bond, an alkoxymethyl group, a hydroxymethyl group, an acyloxymethyl group, an epoxy group, an oxetanyl group, a benzoxazolyl group, a blocked isocyanate group, a methylol group, and an amino group. As the radically polymerizable group possessed by the polyimide precursor or the like, a group having an ethylenically unsaturated bond is preferable. Examples of the group having an ethylenically unsaturated bond include a vinyl group, a (meth)allyl group, and a group represented by the following formula (III), with the group represented by the following formula (III) being preferred.
[0035] [ka]
[0036] In formula (III), R 200 represents a hydrogen atom or a methyl group, and is preferably a hydrogen atom. In formula (III), * represents a bonding site to another structure. In formula (III), R 201 is an alkylene group having 2 to 12 carbon atoms, -CH 2 CH(OH)CH 2 - or a polyalkyleneoxy group. Suitable R 201 Examples of the alkyl group include ethylene, propylene, trimethylene, tetramethylene, 1,2-butanediyl, 1,3-butanediyl, pentamethylene, hexamethylene, octamethylene, dodecamethylene, -CH 2CH(OH)CH 2 -, and polyalkyleneoxy groups, such as an ethylene group, a propylene group, a trimethylene group, -CH 2 CH(OH)CH 2 A polyalkyleneoxy group is more preferable, and a polyalkyleneoxy group is even more preferable. In the present invention, the polyalkyleneoxy group refers to a group in which two or more alkyleneoxy groups are directly bonded. The alkylene groups in the multiple alkyleneoxy groups contained in the polyalkyleneoxy group may be the same or different. When the polyalkyleneoxy group contains multiple types of alkyleneoxy groups having different alkylene groups, the arrangement of the alkyleneoxy groups in the polyalkyleneoxy group may be a random arrangement, an arrangement having blocks, or an arrangement having a pattern such as alternating. The number of carbon atoms in the alkylene group (including the number of carbon atoms in the substituent when the alkylene group has a substituent) is preferably 2 or more, more preferably 2 to 10, more preferably 2 to 6, even more preferably 2 to 5, still more preferably 2 to 4, particularly preferably 2 or 3, and most preferably 2. The alkylene group may have a substituent, and preferred examples of the substituent include an alkyl group, an aryl group, and a halogen atom. The number of alkyleneoxy groups contained in the polyalkyleneoxy group (the number of repeating polyalkyleneoxy groups) is preferably 2-20, more preferably 2-10, and even more preferably 2-6. From the viewpoint of solvent solubility and solvent resistance, the polyalkyleneoxy group is preferably a polyethyleneoxy group, a polypropyleneoxy group, a polytrimethyleneoxy group, a polytetramethyleneoxy group, or a group in which multiple ethyleneoxy groups and multiple propyleneoxy groups are bonded, more preferably a polyethyleneoxy group or a polypropyleneoxy group, and even more preferably a polyethyleneoxy group.In the group in which multiple ethyleneoxy groups and multiple propyleneoxy groups are bonded, the ethyleneoxy groups and the propyleneoxy groups may be arranged randomly, may be arranged in blocks, or may be arranged in a pattern such as alternating.The preferred embodiment of the number of repetitions of the ethyleneoxy groups in these groups is as described above.
[0037] R 113 and R 114 are each independently a hydrogen atom or a monovalent organic group. Examples of the monovalent organic group include aromatic groups and aralkyl groups in which an acidic group is bonded to one, two or three, preferably one, of the carbon atoms constituting the aryl group. Specific examples include aromatic groups having 6 to 20 carbon atoms and having an acidic group, and aralkyl groups having 7 to 25 carbon atoms and having an acidic group. More specific examples include a phenyl group having an acidic group and a benzyl group having an acidic group. The acidic group is preferably an OH group. R 113 or R 114 It is also more preferable that is a hydrogen atom, 2-hydroxybenzyl, 3-hydroxybenzyl, or 4-hydroxybenzyl.
[0038] From the viewpoint of solubility in organic solvents, R 113 or R 114 is preferably a monovalent organic group. The monovalent organic group preferably contains a linear or branched alkyl group, a cyclic alkyl group, or an aromatic group, and more preferably an alkyl group substituted with an aromatic group. The number of carbon atoms of the alkyl group is preferably 1 to 30. The alkyl group may be linear, branched, or cyclic. Examples of the linear or branched alkyl group include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, a dodecyl group, a tetradecyl group, an octadecyl group, an isopropyl group, an isobutyl group, a sec-butyl group, a t-butyl group, a 1-ethylpentyl group, a 2-ethylhexyl group, a 2-(2-(2-methoxyethoxy)ethoxy)ethoxy group, a 2-(2-(2-ethoxyethoxy)ethoxy)ethoxy group, a 2-(2-(2-(2-methoxyethoxy)ethoxy)ethoxy)ethoxy group, and a 2-(2-(2-(2-ethoxyethoxy)ethoxy)ethoxy)ethoxy group. The cyclic alkyl group may be a monocyclic cyclic alkyl group or a polycyclic cyclic alkyl group. Examples of the monocyclic cyclic alkyl group include a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, and a cyclooctyl group. Examples of the polycyclic cyclic alkyl group include an adamantyl group, a norbornyl group, a bornyl group, a camphenyl group, a decahydronaphthyl group, a tricyclodecanyl group, a tetracyclodecanyl group, a campholoyl group, a dicyclohexyl group, and a pinenyl group. Among them, the cyclohexyl group is the most preferable from the viewpoint of compatibility with high sensitivity. In addition, the alkyl group substituted with an aromatic group is preferably a linear alkyl group substituted with an aromatic group as described below. Specific examples of the aromatic group include a substituted or unsubstituted benzene ring, a naphthalene ring, a pentalene ring, an indene ring, an azulene ring, a heptalene ring, an indacene ring, a perylene ring, a pentacene ring, an acenaphthene ring, a phenanthrene ring, an anthracene ring, a naphthacene ring, a chrysene ring, a triphenylene ring, a fluorene ring, a biphenyl ring, a pyrrole ring, a furan ring, a thiophene ring, an imidazole ring, an oxazole ring, a thiazole ring, a pyridine ring, a pyrazine ring, A pyrimidine ring, a pyridazine ring, an indolizine ring, an indole ring, a benzofuran ring, a benzothiophene ring, an isobenzofuran ring, a quinolizine ring, a quinoline ring, a phthalazine ring, a naphthyridine ring, a quinoxaline ring, a quinoxazoline ring, an isoquinoline ring, a carbazole ring, a phenanthridine ring, an acridine ring, a phenanthroline ring, a thianthrene ring, a chromene ring, a xanthene ring, a phenoxathiin ring, a phenothiazine ring, or a phenazine ring. A benzene ring is most preferred.
[0039] In formula (2), R 113 is a hydrogen atom, or R 114 When is a hydrogen atom, the polyimide precursor may form a counter salt with a tertiary amine compound having an ethylenically unsaturated bond. An example of such a tertiary amine compound having an ethylenically unsaturated bond is N,N-dimethylaminopropyl methacrylate.
[0040] It is also preferable that the polyimide precursor has a fluorine atom in the structural unit. The fluorine atom content in the polyimide precursor is preferably 10% by mass or more and 20% by mass or less.
[0041] In order to improve adhesion to the substrate, the polyimide precursor may be copolymerized with an aliphatic group having a siloxane structure.Specific examples of the diamine component include bis(3-aminopropyl)tetramethyldisiloxane and bis(p-aminophenyl)octamethylpentasiloxane.
[0042] The repeating unit represented by formula (2) is preferably a repeating unit represented by formula (2-A). That is, at least one of the polyimide precursors used in the present invention is preferably a precursor having a repeating unit represented by formula (2-A). By adopting such a structure, it is possible to further expand the width of the exposure latitude. Formula (2-A) [ka] In formula (2-A), A 1 and A 2 represents an oxygen atom, R 111 and R 112 each independently represents a divalent organic group; R 113 and R 114 each independently represents a hydrogen atom or a monovalent organic group; R 113 and R 114 At least one of the groups is a group containing a polymerizable group, and it is preferable that both of the groups are polymerizable groups.
[0043] A 1 , A 2 , R 111 , R 113 and R 114 Each independently represents A in formula (2). 1 , A 2 , R 111 , R 113 and R 114 The same definition and preferred range are also the same. R 112 is R in Eq. (5). 112 The same definition and preferred range are also the same.
[0044] The polyimide precursor may contain one type of repeating structural unit represented by formula (2), or may contain two or more types. In addition, it may contain a structural isomer of the repeating unit represented by formula (2). It goes without saying that the polyimide precursor may contain other types of repeating structural units in addition to the repeating unit of formula (2).
[0045] One embodiment of the polyimide precursor in the present invention is a polyimide precursor in which 50 mol % or more, further 70 mol % or more, and particularly 90 mol % or more of all repeating units are repeating units represented by formula (2).
[0046] The weight average molecular weight (Mw) of the polyimide precursor is preferably 18,000 to 30,000, more preferably 20,000 to 27,000, and even more preferably 22,000 to 25,000.The number average molecular weight (Mn) of the polyimide precursor is preferably 7,200 to 14,000, more preferably 8,000 to 12,000, and even more preferably 9,200 to 11,200. The polyimide precursor has a molecular weight dispersity of preferably 2.5 or more, more preferably 2.7 or more, and even more preferably 2.8 or more. The upper limit of the molecular weight dispersity of the polyimide precursor is not particularly specified, but is, for example, preferably 4.5 or less, more preferably 4.0 or less, even more preferably 3.8 or less, even more preferably 3.2 or less, even more preferably 3.1 or less, even more preferably 3.0 or less, and particularly preferably 2.95 or less. In this specification, the dispersity of molecular weight is a value calculated by weight average molecular weight / number average molecular weight.
[0047] [Polybenzoxazole precursor] The polybenzoxazole precursor used in the present invention is not particularly limited with respect to its structure, but preferably contains a repeating unit represented by the following formula (3). The polybenzoxazole precursor used in the present invention has a polymerizable group. The polymerizable group may be contained in a repeating unit represented by the following formula (3), may be contained in another repeating unit, or may be contained at the end of a polybenzoxazole precursor. One of the preferred embodiments of the present invention is an embodiment in which the polymerizable group is contained in a repeating unit represented by the following formula (3). 123 or R 124 It is more preferable that at least one of R123 and R 124 is a polymerizable group. Formula (3) [ka] In formula (3), R 121 represents a divalent organic group, R 122 represents a tetravalent organic group, R 123 and R 124 each independently represents a hydrogen atom or a monovalent organic group.
[0048] In formula (3), R 123 and R 124 are R in Eq. (2), 113 In other words, it is preferable that at least one of them is a polymerizable group. In formula (3), R 121 R represents a divalent organic group. The divalent organic group is preferably a group containing at least one of an aliphatic group and an aromatic group. The aliphatic group is preferably a linear aliphatic group. 121 The dicarboxylic acid residue is preferably a dicarboxylic acid residue. Only one type of dicarboxylic acid residue may be used, or two or more types of dicarboxylic acid residues may be used.
[0049] As the dicarboxylic acid residue, a dicarboxylic acid residue containing an aliphatic group and a dicarboxylic acid residue containing an aromatic group are preferred, and a dicarboxylic acid residue containing an aromatic group is more preferred. The dicarboxylic acid containing an aliphatic group is preferably a dicarboxylic acid containing a linear or branched (preferably linear) aliphatic group, and more preferably a dicarboxylic acid consisting of a linear or branched (preferably linear) aliphatic group and two -COOH. The number of carbon atoms in the linear or branched (preferably linear) aliphatic group is preferably 2 to 30, more preferably 2 to 25, even more preferably 3 to 20, even more preferably 4 to 15, and particularly preferably 5 to 10. The linear aliphatic group is preferably an alkylene group. Dicarboxylic acids containing a linear aliphatic group include malonic acid, dimethylmalonic acid, ethylmalonic acid, isopropylmalonic acid, di-n-butylmalonic acid, succinic acid, tetrafluorosuccinic acid, methylsuccinic acid, 2,2-dimethylsuccinic acid, 2,3-dimethylsuccinic acid, dimethylmethylsuccinic acid, glutaric acid, hexafluoroglutaric acid, 2-methylglutaric acid, 3-methylglutaric acid, 2,2-dimethylglutaric acid, 3,3-dimethylglutaric acid, 3-ethyl-3-methylglutaric acid, adipic acid, octafluoroadipic acid, 3-methyladipic acid, pimelic acid, and 2,2,6,6-tetramethylpimelic acid. , suberic acid, dodecafluorosuberic acid, azelaic acid, sebacic acid, hexadecafluorosebacic acid, 1,9-nonanedioic acid, dodecanedioic acid, tridecanedioic acid, tetradecanedioic acid, pentadecanedioic acid, hexadecanedioic acid, heptadecanedioic acid, octadecanedioic acid, nonadecanedioic acid, eicosanediacid, heneicosanediacid, docosanediacid, tricosanediacid, tetracosanediacid, pentacosanediacid, hexacosanediacid, heptacosanediacid, octacosanediacid, nonacosanediacid, triacontanedioic acid, hentriacontanedioic acid, dotriacontanedioic acid, diglycolic acid, and further dicarboxylic acids represented by the following formula.
[0050] [ka] (In the formula, Z is a hydrocarbon group having 1 to 6 carbon atoms, and n is an integer of 1 to 6.)
[0051] As the dicarboxylic acid containing an aromatic group, the following dicarboxylic acids having an aromatic group are preferred, and the following dicarboxylic acids consisting of only an aromatic group and two -COOH groups are more preferred.
[0052] [ka] In the formula, A is -CH 2 -, -O-, -S-, -SO 2 -, -CO-, -NHCO-, -C(CF 3 )2 - and -C(CH 3 ) 2 -, and each * independently represents a bonding site to another structure.
[0053] Specific examples of dicarboxylic acids containing an aromatic group include 4,4'-carbonyldibenzoic acid and 4,4'-dicarboxydiphenyl ether, and terephthalic acid.
[0054] In formula (3), R 122 represents a tetravalent organic group. The tetravalent organic group is R 115 The same definition and preferred range are also the same. R 122 is also preferably a group derived from a bisaminophenol derivative, and examples of the group derived from a bisaminophenol derivative include 3,3'-diamino-4,4'-dihydroxybiphenyl, 4,4'-diamino-3,3'-dihydroxybiphenyl, 3,3'-diamino-4,4'-dihydroxydiphenyl sulfone, 4,4'-diamino-3,3'-dihydroxydiphenyl sulfone, bis-(3-amino-4-hydroxyphenyl)methane, 2,2-bis(3-amino-4-hydroxyphenyl)propane, 2,2-bis-(3-amino-4-hydroxyphenyl)hexafluoropropane, 2,2-bis-(4-amino bis-(4-amino-3-hydroxyphenyl)hexafluoropropane, bis-(4-amino-3-hydroxyphenyl)methane, 2,2-bis-(4-amino-3-hydroxyphenyl)propane, 4,4'-diamino-3,3'-dihydroxybenzophenone, 3,3'-diamino-4,4'-dihydroxybenzophenone, 4,4'-diamino-3,3'-dihydroxydiphenyl ether, 3,3'-diamino-4,4'-dihydroxydiphenyl ether, 1,4-diamino-2,5-dihydroxybenzene, 1,3-diamino-2,4-dihydroxybenzene, 1,3-diamino-4,6-dihydroxybenzene, etc. These bisaminophenols may be used alone or in combination.
[0055] Among the bisaminophenol derivatives, the following bisaminophenol derivatives having an aromatic group are preferred.
[0056] [ka] In the formula, X 1 -O-, -S-, -C(CF 3 ) 2 -, -CH 2 -, -SO 2 R represents a hydrogen atom or a monovalent substituent, preferably a hydrogen atom or a hydrocarbon group, and more preferably a hydrogen atom or an alkyl group. 122 It is also preferable that R is a structure represented by the above formula. 122 is a structure represented by the above formula, any two of the four * and # are R 122 is a bonding site with the nitrogen atom to which it is bonded, and the other two are R 122 is preferably a bonding site with the oxygen atom to which the bond is bonded, and the two * are preferably R 122 is a bonding site with the oxygen atom to which it is bonded, and the two #'s are R 122 is a bonding site with the nitrogen atom to which the bond is bonded, or two * are R 122 is a bonding site with the nitrogen atom to which it is bonded, and the two #'s are R 122 is more preferably a bonding site with the oxygen atom to which the bond is bonded, and two * are 122 is a bonding site with the oxygen atom to which it is bonded, and the two #'s are R 122 It is more preferable that the nitrogen atom to which the group is bonded is the bonding site.
[0057] [ka]
[0058] In formula (As), R 1is a hydrogen atom, alkylene, substituted alkylene, -O-, -S-, -SO 2 R is -, -CO-, -NHCO-, a single bond, or an organic group selected from the group represented by the following formula (A-sc). 2 R is a hydrogen atom, an alkyl group, an alkoxy group, an acyloxy group, or a cyclic alkyl group, and may be the same or different. 3 are either a hydrogen atom, a linear or branched alkyl group, an alkoxy group, an acyloxy group, or a cyclic alkyl group, and may be the same or different.
[0059] [ka] (In formula (A-sc), * indicates bonding to the aromatic ring of the aminophenol group of the bisaminophenol derivative represented by the above formula (As).)
[0060] In the above formula (As), the ortho position of the phenolic hydroxy group, i.e., R 3 It is believed that the distance between the carbonyl carbon of the amide bond and the hydroxy group is made shorter, which is particularly preferable since it further enhances the effect of achieving a high cyclization rate when cured at low temperature.
[0061] In addition, in the above formula (As), R 2 is an alkyl group, and R 3 It is preferable that the alkyl group is used since the effects of high transparency to i-line and a high cyclization rate when cured at a low temperature can be maintained.
[0062] In addition, in the above formula (As), R 1 It is more preferred that R is alkylene or substituted alkylene. 1 Specific examples of the alkylene and substituted alkylene include linear or branched alkyl groups having 1 to 8 carbon atoms. 2 -, -CH(CH 3 )-, -C(CH 3 ) 2is more preferable in that it is possible to obtain a polybenzoxazole precursor having a good balance between high transparency to i-line and a high cyclization rate when cured at a low temperature and sufficient solubility in a solvent.
[0063] For the production method of the bisaminophenol derivative represented by the above formula (As), reference can be made to, for example, paragraphs 0085 to 0094 and Example 1 (paragraphs 0189 to 0190) of JP 2013-256506 A, the contents of which are incorporated herein by reference.
[0064] Specific examples of the structure of the bisaminophenol derivative represented by the above formula (As) include those described in paragraphs 0070 to 0080 of JP 2013-256506 A, the contents of which are incorporated herein by reference. Of course, it goes without saying that the present invention is not limited to these.
[0065] The polybenzoxazole precursor may contain other types of repeating structural units in addition to the repeating unit of formula (3) above. In terms of being able to suppress the occurrence of warping due to ring closure, it is preferable that the resin contains a diamine residue represented by the following formula (SL) as another type of repeating structural unit.
[0066] [ka] In formula (SL), Z has an a structure and a b structure, and R 1s is a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms, R 2s is a hydrocarbon group having 1 to 10 carbon atoms, and R 3s , R 4s , R 5s , R 6s At least one of them is an aromatic group, and the rest are hydrogen atoms or organic groups having 1 to 30 carbon atoms, which may be the same or different. The polymerization of the a structure and the b structure may be block polymerization or random polymerization. The molar percentage of the Z portion is 5 to 95 mol % for the a structure, 95 to 5 mol % for the b structure, and a+b is 100 mol %.
[0067] In formula (SL), preferred Z is R in the b structure. 5s and R 6s is a phenyl group. The molecular weight of the structure represented by formula (SL) is preferably 400 to 4,000, more preferably 500 to 3,000. By setting the molecular weight within the above range, it is possible to more effectively reduce the elastic modulus of the polybenzoxazole precursor after dehydration ring closure, and to simultaneously achieve the effect of suppressing warpage and the effect of improving solvent solubility.
[0068] When the diamine residue represented by formula (SL) is contained as another type of repeating structural unit, it is also preferable that the diamine residue represented by formula (SL) further contains, as a repeating structural unit, a tetracarboxylic acid residue remaining after removal of the anhydride group from the tetracarboxylic dianhydride. 115 Examples include:
[0069] When used in a composition described later, the polybenzoxazole precursor has a weight average molecular weight (Mw) of preferably 18,000 to 30,000, more preferably 20,000 to 29,000, and even more preferably 22,000 to 28,000. Also, the number average molecular weight (Mn) is preferably 7,200 to 14,000, more preferably 8,000 to 12,000, and even more preferably 9,200 to 11,200. The polybenzoxazole precursor has a molecular weight dispersity of preferably 1.4 or more, more preferably 1.5 or more, and even more preferably 1.6 or more. The upper limit of the molecular weight dispersity of the polybenzoxazole precursor is not particularly specified, but is preferably 2.6 or less, more preferably 2.5 or less, even more preferably 2.4 or less, even more preferably 2.3 or less, and even more preferably 2.2 or less.
[0070] -End capping agent- In the method for producing a polyimide precursor or the like, in order to further improve the storage stability of the composition, it is preferable to cap the ends of the polyimide precursor or the like with an end-capping agent such as an acid anhydride, a monocarboxylic acid, a monoacid chloride compound, a monoactive ester compound, etc. As the end-capping agent, it is more preferable to use a monoamine, and preferred monoamine compounds include aniline, 2-ethynylaniline, 3-ethynylaniline, 4-ethynylaniline, 5-amino-8-hydroxyquinoline, 1-hydroxy-7-aminonaphthalene, 1-hydroxy-6-aminonaphthalene, 1-hydroxy-5-aminonaphthalene, 1-hydroxy-4-aminonaphthalene, 2-hydroxy-7-aminonaphthalene, 2-hydroxy-6-aminonaphthalene, 2-hydroxy-5-aminonaphthalene, 1-carboxy-7-aminonaphthalene, 1-carboxy-6-aminonaphthalene, 1-carboxy-5-aminonaphthalene, 1-carboxy-5-aminonaphthalene, 1-carboxy-6-aminonaphthalene, 1-carboxy-5-aminonaphthalene, 1-carboxy-5-aminonaphthalene, 1-carboxy-5-aminonaphthalene, 1-hydroxy ... aminonaphthalene, 2-carboxy-7-aminonaphthalene, 2-carboxy-6-aminonaphthalene, 2-carboxy-5-aminonaphthalene, 2-aminobenzoic acid, 3-aminobenzoic acid, 4-aminobenzoic acid, 4-aminosalicylic acid, 5-aminosalicylic acid, 6-aminosalicylic acid, 2-aminobenzenesulfonic acid, 3-aminobenzenesulfonic acid, 4-aminobenzenesulfonic acid, 3-amino-4,6-dihydroxypyrimidine, 2-aminophenol, 3-aminophenol, 4-aminophenol, 2-aminothiophenol, 3-aminothiophenol, 4-aminothiophenol, 4-aminostyrene, etc. Two or more of these may be used, and multiple different terminal groups may be introduced by reacting multiple terminal blocking agents.
[0071] [Content] The content of the specific resin in the resin composition of the present invention is preferably 80% by mass or more, more preferably 85% by mass or more, and even more preferably 90% by mass or more, based on the total solid content of the resin composition. The content of the resin in the resin composition of the present invention is preferably 99.5% by mass or less, more preferably 99% by mass or less, even more preferably 98% by mass or less, and even more preferably 97% by mass or less, based on the total solid content of the resin composition. The composition of the present invention may contain only one type of specific resin, or may contain two or more types. When two or more types are contained, the total amount is preferably within the above range.
[0072] <Antioxidants> The resin composition of the present invention contains an antioxidant. The content of the antioxidant is from 0.1 ppm by mass to 10,000 ppm by mass, preferably from 10 to 1,000 ppm by mass, and more preferably from 50 to 500 ppm by mass, relative to the content of the resin. The resin composition of the present invention may contain one type of antioxidant alone or two or more types. When two or more types are contained, the total amount thereof is preferably within the above range.
[0073] From the viewpoint of filterability when redissolved in a solvent, the oxidation-reduction potential of the antioxidant is preferably 0.91 V or less, more preferably 0.65 V or less, and even more preferably 0.45 V or less. The lower limit of the oxidation-reduction potential is not particularly limited, but is preferably −2.00 V or higher. The above-mentioned oxidation-reduction potential is measured by the method described in the Examples below. If the oxidation-reduction potential is within the above range, it is believed that the reduction ability of the above-mentioned peroxide is excellent, and the filterability when redissolved in a solvent is improved.
[0074] The antioxidant is preferably at least one compound selected from the group consisting of phenol-based compounds, alcohol-based compounds, aldehyde-based compounds, amine-based compounds, nitroso-based compounds, phosphorus-based compounds, sulfur-based compounds, and ketone-based compounds.
[0075] Examples of the phenolic compounds include hydroquinone, o-methoxyphenol, p-methoxyphenol, 2,6-dimethoxyphenol, and pyrogallol.
[0076] Examples of the alcohol-based compound include ascorbic acid and glucose.
[0077] Examples of the aldehyde compounds include formaldehyde, acetaldehyde, benzaldehyde, and p-methoxybenzaldehyde.
[0078] Examples of the amine compounds include 2-methoxyaniline, 4-methoxyaniline, 4-hydroxyaniline, and p-phenylenediamine.
[0079] Examples of the nitroso compounds include 4-nitrosoanisole and 4-nitrosodimethylaniline.
[0080] Examples of the phosphorus-based compounds include triethylphosphine and triphenylphosphine.
[0081] Examples of sulfur-based compounds include thiophenol, 4-hydroxythiophenol, and cysteine.
[0082] An example of the ketone compound is 3-bromo-β-lapachone.
[0083] Among these, from the viewpoint of filterability when redissolved in a solvent, phenol-based compounds having an unsaturation degree of 1 or more, or alcohol-based compounds having an unsaturation degree of 1 or more are preferred. The degree of unsaturation is a number expressed as (2C+2-H-X+N) / 2, where C is the number of carbon atoms, H is the number of hydrogen atoms, X is the number of halogen atoms, and N is the number of nitrogen atoms. The degree of unsaturation is preferably 1-5, and more preferably 2-4.
[0084] <Organic solvent> The resin composition of the present invention contains an organic solvent. The content of the organic solvent is not particularly limited, but is preferably more than 0 and 10 mass% or less, more preferably 0.1 to 8 mass% or less, and even more preferably 1 to 6 mass% or less, relative to the total mass of the resin composition. When the organic solvent is 10% by mass or less (preferably 8% by mass or less, and more preferably 6% by mass or less), it is considered that uneven distribution of the antioxidant between parts where the organic solvent is present and parts where it is not present in the resin composition is suppressed, and filterability after redissolution is more likely to be improved. The resin composition of the present invention may contain one kind of organic solvent alone or two or more kinds. When two or more kinds are contained, the total amount thereof is preferably within the above range.
[0085] The organic solvent preferably contains at least one selected from the group consisting of hydrocarbon compounds, alcohol compounds, carboxylic acids, ketone compounds, ester compounds, ether compounds, nitrile compounds, amide compounds, amine compounds, sulfone compounds, and sulfoxide compounds.
[0086] Examples of the hydrocarbon compound include aromatic hydrocarbons such as toluene, xylene, and anisole, and cyclic terpenes such as limonene.
[0087] Examples of the alcohol-based compound include methanol, ethanol, propanol, isopropanol, and butanol.
[0088] Examples of the carboxylic acid include formic acid, acetic acid, propionic acid, and lactic acid.
[0089] Examples of the ketone compounds include methyl ethyl ketone, cyclohexanone, cyclopentanone, 2-heptanone, and 3-heptanone.
[0090] Examples of the ester compounds include ethyl acetate, n-butyl acetate, isobutyl acetate, amyl formate, isoamyl acetate, butyl propionate, isopropyl butyrate, ethyl butyrate, butyl butyrate, methyl lactate, ethyl lactate, γ-butyrolactone, ε-caprolactone, δ-valerolactone, alkyl alkyloxyacetates (e.g., methyl alkyloxyacetate, ethyl alkyloxyacetate, butyl alkyloxyacetate (e.g., methyl methoxyacetate, ethyl methoxyacetate, butyl methoxyacetate, methyl ethoxyacetate, ethyl ethoxyacetate, etc.)), 3-alkyloxypropionic acid alkyl esters (e.g., methyl 3-alkyloxypropionate, ethyl 3-alkyloxypropionate, etc. (e.g., methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, etc.)), ethyl pyruvate, etc.), 2-alkyloxypropionic acid alkyl esters (for example, methyl 2-alkyloxypropionate, ethyl 2-alkyloxypropionate, propyl 2-alkyloxypropionate, etc. (for example, methyl 2-methoxypropionate, ethyl 2-methoxypropionate, propyl 2-methoxypropionate, methyl 2-ethoxypropionate, ethyl 2-ethoxypropionate)), methyl 2-alkyloxy-2-methylpropionate and ethyl 2-alkyloxy-2-methylpropionate (for example, methyl 2-methoxy-2-methylpropionate, ethyl 2-ethoxy-2-methylpropionate, etc.), methyl pyruvate, ethyl pyruvate, propyl pyruvate, methyl acetoacetate, ethyl acetoacetate, methyl 2-oxobutanoate, ethyl 2-oxobutanoate, etc.
[0091] Examples of the ether compounds include diethylene glycol dimethyl ether, tetrahydrofuran, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, and propylene glycol monopropyl ether acetate.
[0092] Examples of the nitrile compounds include acetonitrile, propionitrile, and benzonitrile.
[0093] Examples of the amide compounds include N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N,N-dimethylacetamide, and N,N-dimethylformamide.
[0094] Examples of the amine compounds include monomethanolamine, dimethanolamine, trimethanolamine, monoethanolamine, diethanolamine, triethanolamine, and dimethylamine.
[0095] The sulfone-based compounds include sulfolane and the like.
[0096] The sulfoxide compounds include dimethyl sulfoxide and the like.
[0097] Of these, the resin composition of the present invention preferably contains an amide-based compound, an ether-based compound, a ketone-based compound, or an ester-based compound, and more preferably contains a lactam-based compound, a cyclic ether-based compound, a cyclic ketone-based compound, or a lactone-based solvent.
[0098] <Other ingredients> The resin composition of the present invention may further contain other components in addition to the specific resin, the antioxidant, and the organic solvent. The resin composition of the present invention may also be in an embodiment that does not substantially contain other components. Specifically, the total content of the specific resin, the antioxidant, and the organic solvent is preferably 90% by mass or more, and more preferably 95% by mass or more, based on the total mass of the resin composition.
[0099] Examples of other components include nitrogen-containing compounds and compounds having a polymerizable group.
[0100] [Nitrogen-containing compounds] Preferred examples of the nitrogen-containing compound include a compound containing a urea structure, a compound containing a carbodiimide structure, and a compound containing an isourea structure. Specifically, examples of the nitrogen-containing compound include a compound represented by the following formula (1-1), a compound represented by the following formula (1-2), and a compound represented by the following formula (1-3). [ka] In the formula (1-1), the formula (1-2) or the formula (1-3), R 11 and R 12 each independently represents an aliphatic hydrocarbon group having 1 to 7 carbon atoms which may have a substituent; R 21 and R 22 each independently represents an aliphatic hydrocarbon group having 1 to 7 carbon atoms which may have a substituent; R 31 and R 32 each independently represents an aliphatic hydrocarbon group having 1 to 7 carbon atoms which may have a substituent; R 33 represents an aliphatic hydrocarbon group having 1 to 7 carbon atoms which may have a substituent. In formula (1-1), R 11 and R 12are each independently preferably an unsubstituted aliphatic hydrocarbon group having 1 to 7 carbon atoms, or an aliphatic hydrocarbon group having 1 to 7 carbon atoms and having, as a substituent, at least one substituent selected from the group consisting of a primary amine salt structure, a secondary amine salt structure, a tertiary amino group, a tertiary amine salt structure, and a quaternary ammonium group, and more preferably an unsubstituted aliphatic hydrocarbon group having 1 to 7 carbon atoms. R 11 and R 12 The unsubstituted aliphatic hydrocarbon group having 1 to 7 carbon atoms in the formula (I) is preferably an unsubstituted saturated aliphatic hydrocarbon group having 1 to 7 carbon atoms, more preferably an unsubstituted saturated aliphatic hydrocarbon group having 2 to 7 carbon atoms, and more preferably an ethyl group, an isopropyl group, a t-butyl group or a cyclohexyl group.
[0101] In formula (1-1), R 11 and R 12 may each independently be an aliphatic hydrocarbon group having 2 to 7 carbon atoms having at least one substituent selected from the group consisting of a hydroxy group, an alkoxy group, a thiol group, and an alkylthio group. The aliphatic hydrocarbon group having 2 to 7 carbon atoms may have two or more of the above-mentioned substituents, but an embodiment having only one of the above-mentioned substituents is also one of the preferred embodiments of the present invention.
[0102] In formula (1-2), R 21 and R 22 each independently represents an aliphatic hydrocarbon group having 1 to 7 carbon atoms which may have a substituent. In formula (1-2), R 21 and R 22 is preferably an unsubstituted aliphatic hydrocarbon group having 1 to 7 carbon atoms, or an aliphatic hydrocarbon group having 1 to 7 carbon atoms and having an amino group or a quaternary ammonium group as a substituent, and more preferably an unsubstituted aliphatic hydrocarbon group having 1 to 7 carbon atoms. In formula (1-2), R 21 and R 22 Preferred embodiments of the unsubstituted aliphatic hydrocarbon group having 1 to 7 carbon atoms or the substituted aliphatic hydrocarbon group having 1 to 7 carbon atoms in the above formula are respectively represented by the following formula: 11 and R 12This is similar to that shown in the explanation of .
[0103] In formula (1-3), R 31 and R 32 is preferably an unsubstituted aliphatic hydrocarbon group having 1 to 7 carbon atoms, or an aliphatic hydrocarbon group having 1 to 7 carbon atoms and having an amino group or a quaternary ammonium group as a substituent, and more preferably an unsubstituted aliphatic hydrocarbon group having 1 to 7 carbon atoms. In formula (1-3), R 31 and R 32 Preferred embodiments of the unsubstituted aliphatic hydrocarbon group having 1 to 7 carbon atoms or the substituted aliphatic hydrocarbon group having 1 to 7 carbon atoms in the above formula are respectively represented by the following formula: 11 and R 12 This is similar to that shown in the explanation of .
[0104] In formula (1-3), R 33 represents an aliphatic hydrocarbon group having 1 to 7 carbon atoms which may have a substituent, is preferably an unsubstituted aliphatic hydrocarbon group having 1 to 7 carbon atoms, is more preferably an unsubstituted saturated aliphatic hydrocarbon group having 1 to 7 carbon atoms, and is more preferably a saturated aliphatic hydrocarbon group having 1 to 4 carbon atoms. In formula (1-3), R 33 As the alkyl group, a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group or a t-butyl group is preferable, and an ethyl group is more preferable.
[0105] [Compound having a polymerizable group] The resin composition of the present invention may contain a compound having a polymerizable group as another component. Examples of the polymerizable group include the same groups as the polymerizable groups in the specific resin described above, and preferred embodiments are also the same. The compound having a polymerizable group may be contained as an unreacted component among the raw materials used for introducing a polymerizable group into the above-mentioned polyimide or polybenzoxazole, for example. As the compound having a polymerizable group, a compound having a polymerizable group and a hydroxy group is preferable, and examples thereof include hydroxymethyl(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, and glycerin di(meth)acrylate.
[0106] [Content] The content of other components is not particularly limited, but is preferably 10% by mass or less, and more preferably 5% by mass or less. The lower limit is not particularly limited, and may be 0 mass %. The resin composition of the present invention may contain one type of other component alone, or two or more types may be used in combination. When two or more types are used in combination, the total amount is preferably within the above range.
[0107] (Method of producing resin composition) The method for producing a resin composition of the present invention includes an adding step of adding the antioxidant to a production composition containing the organic solvent and the specific resin. The amount of the antioxidant added may be any amount so long as the content of the antioxidant in the resin composition falls within the above-mentioned range.
[0108] The method for producing a resin composition of the present invention preferably includes a synthesis step of reacting raw materials in a solvent to obtain a reaction liquid containing a specific resin. The synthesis step may be carried out by a known method. For example, when the specific resin is a polyimide precursor or a polybenzoxazole precursor, the process is preferably a step of reacting a dicarboxylic acid or a dicarboxylic acid derivative with a diamine to obtain the specific resin. The synthesis conditions and the like can be those of known methods without any particular limitations. For example, a method can be mentioned in which a dicarboxylic acid or a dicarboxylic acid derivative is halogenated with a halogenating agent, and then reacted with a diamine to obtain the specific resin. It is also preferable to synthesize using a non-halogen catalyst without using the halogenating agent. As the non-halogen catalyst, a known amidation catalyst that does not contain a halogen atom can be used without any particular limitation, and examples thereof include boroxine compounds, N-hydroxy compounds, tertiary amines, phosphoric acid esters, amine salts, urea compounds, and carbodiimide compounds. As the carbodiimide compounds, N,N'-diisopropylcarbodiimide, N,N'-dicyclohexylcarbodiimide, and the like can be mentioned. The solvent used in the synthesis step can be appropriately determined depending on the raw materials, and examples thereof include pyridine, diethylene glycol dimethyl ether (diglyme), N-methylpyrrolidone, and N-ethylpyrrolidone. The organic solvent in the resin composition described above may also be used. In the synthesis step, it is also preferable to remove the precipitate generated in the reaction solution by filtration. In the method for producing a resin composition of the present invention, the above reaction liquid may be used as the above-mentioned production composition, but it is preferable to use the specific resin solution after the reprecipitation / redissolution step described below as the above-mentioned production composition. That is, one preferred embodiment of the method for producing a resin composition of the present invention includes a synthesis step and a reprecipitation / redissolution step, and the adding step is carried out using the specific resin solution obtained in the reprecipitation / redissolution step as the production composition.
[0109] The method for producing a resin composition of the present invention preferably includes a reprecipitation / redissolution step of reprecipitating the specific resin in the reaction liquid and redissolving the reprecipitated specific resin in the organic solvent to obtain a specific resin solution. Specifically, the reprecipitation method can involve supplying a reaction liquid containing a specific resin such as a polyimide precursor and the above-mentioned solvent to a poor solvent (a solvent in which the specific resin has low solubility) such as water or alcohol, thereby causing reprecipitation. The reprecipitated specific resin can be obtained, for example, by a method such as filtration. The organic solvent used for redissolution may be any good solvent for the resin (a solvent that has high solubility for the specific resin), and is preferably an organic solvent described above in relation to the resin composition. The conditions such as temperature during reprecipitation or redissolution are not particularly limited, and may be those according to known methods.
[0110] In addition, it is preferable to include a reprecipitation step of reprecipitating the specific resin after the adding step. The reprecipitation step can be carried out in the same manner as in the reprecipitation / redissolution step described above. In the reprecipitation step, the reprecipitated specific resin can be obtained by, for example, a method such as filtration, etc. That is, the reprecipitation step results in the specific resin being obtained in a form containing a small amount of the organic solvent.
[0111] In addition, it is preferable to include a drying step of removing the organic solvent after the reprecipitation step. The drying conditions are not particularly limited, but for example, drying can be performed under reduced pressure at 25 to 45° C. for 1 hour to 7 days. The drying means is not particularly limited, and for example, a known reduced pressure dryer can be used. The degree of drying is not particularly limited as long as at least a portion of the organic solvent is removed, and it is preferable to dry so that the content of the organic solvent is within the above-mentioned range relative to the total mass of the resin composition.
[0112] (Method of manufacturing a pattern-forming composition) The method for producing the pattern-forming composition of the present invention preferably includes a mixing step of mixing the resin composition of the present invention with a solvent. The mixing method is not particularly limited, and may be a conventionally known method. In the method for producing a pattern-forming composition of the present invention, it is preferable that a photosensitizer is further mixed in the mixing step. In the method for producing a pattern-forming composition of the present invention, other components may be further mixed in the mixing step. The content of the specific resin in the pattern-forming composition of the present invention is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, and even more preferably 50% by mass or more, based on the total solid content of the resin composition. The content of the resin in the composition of the present invention is preferably 99.5% by mass or less, more preferably 99% by mass or less, even more preferably 98% by mass or less, even more preferably 97% by mass or less, and even more preferably 95% by mass or less, based on the total solid content of the composition. The pattern-forming composition of the present invention may contain only one specific resin, or may contain two or more specific resins. When two or more specific resins are contained, the total amount is preferably within the above range. In addition, when the pattern-forming composition contains two or more specific resins, a resin composition containing two or more specific resins may be used, or a resin composition containing a certain specific resin may be used in combination with a resin composition containing another specific resin.
[0113] In addition, it is preferable to perform filtration using a filter in order to remove foreign matter such as dust and fine particles from the pattern-forming composition. The filter pore size is preferably 1 μm or less, more preferably 0.5 μm or less, and even more preferably 0.1 μm or less. On the other hand, from the viewpoint of productivity, it is preferably 5 μm or less, more preferably 3 μm or less, and even more preferably 1 μm or less. The material of the filter is preferably polytetrafluoroethylene, polyethylene, or nylon. The filter may be used after being washed in advance with an organic solvent. In the filter filtration process, multiple types of filters may be connected in series or parallel. When multiple types of filters are used, filters with different pore sizes or materials may be used in combination. In addition, various materials may be filtered multiple times. When filtering multiple times, circulation filtration may be performed. In addition, filtration may be performed under pressure. When filtering under pressure, the pressure applied is preferably 0.05 MPa or more and 0.3 MPa or less. On the other hand, from the viewpoint of productivity, the pressure is preferably 0.01 MPa or more and 1.0 MPa or less, more preferably 0.03 MPa or more and 0.9 MPa or less, and even more preferably 0.05 MPa or more and 0.7 MPa or less. In addition to filtration using a filter, impurity removal treatment using an adsorbent may be performed. Filter filtration and impurity removal treatment using an adsorbent may be combined. As the adsorbent, a known adsorbent may be used. For example, inorganic adsorbents such as silica gel and zeolite, and organic adsorbents such as activated carbon may be used. Hereinafter, the solvent, photosensitizer, and other components contained in the pattern-forming composition obtained by the method for producing a pattern-forming composition of the present invention will be described as components contained in the pattern-forming composition. In the method for producing a pattern-forming composition of the present invention, these components are mixed as necessary to obtain a pattern-forming composition.
[0114] <Solvent> The pattern-forming composition of the present invention preferably contains a solvent. Any known solvent can be used as the solvent. The solvent is preferably an organic solvent. Examples of the organic solvent include compounds such as esters, ethers, ketones, cyclic hydrocarbons, sulfoxides, amides, ureas, and alcohols.
[0115] Examples of esters include ethyl acetate, n-butyl acetate, isobutyl acetate, hexyl acetate, amyl formate, isoamyl acetate, butyl propionate, isopropyl butyrate, ethyl butyrate, butyl butyrate, methyl lactate, ethyl lactate, γ-butyrolactone, ε-caprolactone, δ-valerolactone, alkyl alkyloxyacetates (e.g., methyl alkyloxyacetate, ethyl alkyloxyacetate, butyl alkyloxyacetate (e.g., methyl methoxyacetate, ethyl methoxyacetate, butyl methoxyacetate, methyl ethoxyacetate, ethyl ethoxyacetate, etc.)), 3-alkyloxypropionic acid alkyl esters (e.g., methyl 3-alkyloxypropionate, ethyl 3-alkyloxypropionate, etc. (e.g., methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, etc.)), 2-alkyloxypropionic acid alkyl esters (e.g., methyl 3-alkyloxypropionate, ethyl 3-alkyloxypropionate, etc. (e.g., methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, etc.)), 3-alkyloxypropionic acid alkyl esters (e.g., methyl 3-alkyloxypropionate, ethyl 3-alkyloxypropionate, etc. (e.g., methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, etc.)), 2-alkyloxypropionic acid alkyl esters (e.g., methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-eth Preferred examples of the cypropionic acid alkyl esters include methyl 2-alkyloxypropionate, ethyl 2-alkyloxypropionate, and propyl 2-alkyloxypropionate (e.g., methyl 2-methoxypropionate, ethyl 2-methoxypropionate, propyl 2-methoxypropionate, methyl 2-ethoxypropionate, and ethyl 2-ethoxypropionate), methyl 2-alkyloxy-2-methylpropionate and ethyl 2-alkyloxy-2-methylpropionate (e.g., methyl 2-methoxy-2-methylpropionate, ethyl 2-ethoxy-2-methylpropionate), methyl pyruvate, ethyl pyruvate, propyl pyruvate, methyl acetoacetate, ethyl acetoacetate, methyl 2-oxobutanoate, ethyl 2-oxobutanoate, ethyl hexanoate, ethyl heptanoate, dimethyl malonate, and diethyl malonate.
[0116] Suitable examples of the ethers include diethylene glycol dimethyl ether, tetrahydrofuran, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether, ethylene glycol monobutyl ether acetate, diethylene glycol ethyl methyl ether, and propylene glycol monopropyl ether acetate.
[0117] Suitable examples of ketones include methyl ethyl ketone, cyclohexanone, cyclopentanone, 2-heptanone, 3-heptanone, 3-methylcyclohexanone, levoglucosenone, and dihydrolevoglucosenone.
[0118] Suitable examples of cyclic hydrocarbons include aromatic hydrocarbons such as toluene, xylene, and anisole, and cyclic terpenes such as limonene.
[0119] A preferred example of the sulfoxides is dimethyl sulfoxide.
[0120] Preferred examples of the amides include N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, N,N-dimethylisobutyramide, 3-methoxy-N,N-dimethylpropionamide, 3-butoxy-N,N-dimethylpropionamide, N-formylmorpholine, and N-acetylmorpholine.
[0121] Preferred examples of the ureas include N,N,N',N'-tetramethylurea and 1,3-dimethyl-2-imidazolidinone.
[0122] Examples of alcohols include methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 1-pentanol, 1-hexanol, benzyl alcohol, ethylene glycol monomethyl ether, 1-methoxy-2-propanol, 2-ethoxyethanol, diethylene glycol monoethyl ether, diethylene glycol monohexyl ether, triethylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monomethyl ether, polyethylene glycol monomethyl ether, polypropylene glycol, tetraethylene glycol, ethylene glycol monobutyl ether, ethylene glycol monobenzyl ether, ethylene glycol monophenyl ether, methylphenyl carbinol, n-amyl alcohol, methylamyl alcohol, and diacetone alcohol.
[0123] From the viewpoint of improving the properties of the coated surface, it is also preferable to mix two or more kinds of solvents.
[0124] In the present invention, one solvent selected from methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, ethyl cellosolve acetate, ethyl lactate, diethylene glycol dimethyl ether, butyl acetate, methyl 3-methoxypropionate, 2-heptanone, cyclohexanone, cyclopentanone, γ-butyrolactone, dimethyl sulfoxide, ethyl carbitol acetate, butyl carbitol acetate, N-methyl-2-pyrrolidone, propylene glycol methyl ether, and propylene glycol methyl ether acetate, or a mixed solvent composed of two or more of them, is preferred. The combined use of dimethyl sulfoxide and γ-butyrolactone is particularly preferred. Also preferred are combinations of N-methyl-2-pyrrolidone and ethyl lactate, N-methyl-2-pyrrolidone and ethyl lactate, diacetone alcohol and ethyl lactate, and cyclopentanone and γ-butyrolactone.
[0125] From the viewpoint of coatability, the content of the solvent is preferably an amount that makes the total solid concentration of the pattern-forming composition 5 to 80 mass %, more preferably an amount that makes the total solid concentration of the pattern-forming composition 5 to 75 mass %, even more preferably an amount that makes the total solid concentration of the pattern-forming composition 10 to 70 mass %, and even more preferably an amount that makes the total solid concentration of the pattern-forming composition 40 to 70 mass %. The content of the solvent may be adjusted according to the desired thickness of the coating film and the coating method.
[0126] The composition may contain one solvent or two or more solvents. When two or more solvents are contained, the total amount of the solvents is preferably within the above range.
[0127] <Photosensitizer> The pattern forming composition preferably contains a photosensitizer. The photosensitizer is preferably a photopolymerization initiator.
[0128] [Photopolymerization initiator] The pattern-forming composition preferably contains a photopolymerization initiator as a photosensitizer. The photopolymerization initiator is preferably a photoradical polymerization initiator. The photoradical polymerization initiator is not particularly limited and can be appropriately selected from known photoradical polymerization initiators. For example, a photoradical polymerization initiator having photosensitivity to light rays in the ultraviolet to visible regions is preferable. Alternatively, it may be an activator that generates active radicals by reacting with a photoexcited sensitizer. As the photoradical polymerization initiator, an oxime compound described below is preferable.
[0129] The photoradical polymerization initiator has a wavelength of about 300 to 800 nm (preferably 330 to 500 nm) and a concentration of at least about 50 L mol -1 ·cm -1 It is preferable that the composition contains at least one compound having a molar absorption coefficient of 0.01 g / L. The molar absorption coefficient of the compound can be measured using a known method. For example, it is preferable to measure the molar absorption coefficient at a concentration of 0.01 g / L using an ultraviolet-visible spectrophotometer (Varian Cary-5 spectrophotometer) using ethyl acetate as a solvent.
[0130] Any known compound can be used as the photoradical polymerization initiator. For example, halogenated hydrocarbon derivatives (e.g., compounds having a triazine skeleton, compounds having an oxadiazole skeleton, compounds having a trihalomethyl group, etc.), acylphosphine compounds such as acylphosphine oxides, hexaarylbiimidazoles, oxime compounds such as oxime derivatives, organic peroxides, thio compounds, ketone compounds, aromatic onium salts, ketoxime ethers, aminoacetophenone compounds, hydroxyacetophenones, azo compounds, azide compounds, metallocene compounds, organic boron compounds, iron arene complexes, etc. For details of these, refer to the descriptions in paragraphs 0165 to 0182 of JP 2016-027357 A and paragraphs 0138 to 0151 of WO 2015 / 199219 A, the contents of which are incorporated herein by reference.
[0131] Examples of the ketone compound include the compounds described in paragraph 0087 of JP2015-087611A, the contents of which are incorporated herein by reference. As a commercially available product, Kayacure DETX (manufactured by Nippon Kayaku Co., Ltd.) is also preferably used.
[0132] In one embodiment of the present invention, as the photoradical polymerization initiator, a hydroxyacetophenone compound, an aminoacetophenone compound, and an acylphosphine compound can be suitably used. More specifically, for example, an aminoacetophenone-based initiator described in JP-A-10-291969 and an acylphosphine oxide-based initiator described in JP-A-4225898 can be used.
[0133] As the hydroxyacetophenone-based initiator, IRGACURE 184 (IRGACURE is a registered trademark), DAROCUR 1173, IRGACURE 500, IRGACURE-2959, and IRGACURE 127 (trade names: all manufactured by BASF) can be used.
[0134] As the aminoacetophenone initiator, commercially available products such as IRGACURE 907, IRGACURE 369, and IRGACURE 379 (product names: all manufactured by BASF) can be used.
[0135] As the aminoacetophenone-based initiator, the compounds described in JP-A-2009-191179, which have an absorption maximum wavelength matching a light source with a wavelength of 365 nm or 405 nm, can also be used.
[0136] Examples of the acylphosphine initiator include 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, etc. In addition, commercially available products such as IRGACURE-819 and IRGACURE-TPO (trade names: both manufactured by BASF) can be used.
[0137] Examples of the metallocene compound include IRGACURE-784 and IRGACURE-784EG (both manufactured by BASF).
[0138] As the photoradical polymerization initiator, more preferably, an oxime compound is used. By using an oxime compound, it is possible to more effectively improve the exposure latitude. The oxime compound is particularly preferred because it has a wide exposure latitude (exposure margin) and also functions as a photocuring accelerator.
[0139] Specific examples of the oxime compound that can be used include the compounds described in JP-A-2001-233842, JP-A-2000-080068, and JP-A-2006-342166.
[0140] Examples of preferred oxime compounds include compounds having the following structure, 3-benzoyloxyiminobutan-2-one, 3-acetoxyiminobutan-2-one, 3-propionyloxyiminobutan-2-one, 2-acetoxyiminopentan-3-one, 2-acetoxyimino-1-phenylpropan-1-one, 2-benzoyloxyimino-1-phenylpropan-1-one, 3-(4-toluenesulfonyloxy)iminobutan-2-one, and 2-ethoxycarbonyloxyimino-1-phenylpropan-1-one. In the pattern-forming composition, it is particularly preferred to use an oxime compound (oxime-based photopolymerization initiator) as a photoradical polymerization initiator. The oxime-based photopolymerization initiator has a linking group of >C=NOC(=O)- in the molecule.
[0141] [ka]
[0142] Commercially available products include IRGACURE OXE 01, IRGACURE OXE 02, IRGACURE OXE 03, and IRGACURE OXE 04 (manufactured by BASF), and Adeka Optomer N-1919 (manufactured by ADEKA Corporation, photoradical polymerization initiator 2 described in JP 2012-014052 A). TR-PBG-304 (manufactured by Changzhou Strong Electronic New Materials Co., Ltd.), Adeka Arcles NCI-831, and Adeka Arcles NCI-930 (manufactured by ADEKA Corporation) can also be used. DFI-091 (manufactured by Daito Chemistry Co., Ltd.) can also be used. Oxime compounds having the following structure can also be used. [ka]
[0143] As the photopolymerization initiator, an oxime compound having a fluorene ring can also be used. Specific examples of the oxime compound having a fluorene ring include the compounds described in JP-A-2014-137466 and the compounds described in JP-A-06636081.
[0144] As the photopolymerization initiator, an oxime compound having a skeleton in which at least one benzene ring of a carbazole ring is replaced with a naphthalene ring can also be used. Specific examples of such oxime compounds include the compounds described in WO 2013 / 083505.
[0145] In addition, it is also possible to use an oxime compound having a fluorine atom. Specific examples of such oxime compounds include the compounds described in JP-A-2010-262028, compounds 24, 36 to 40 described in JP-A-2014-500852, paragraph 0345, and compound (C-3) described in JP-A-2013-164471, paragraph 0101.
[0146] Most preferred examples of the oxime compound include oxime compounds having specific substituents as disclosed in JP-A-2007-269779 and oxime compounds having a thioaryl group as disclosed in JP-A-2009-191061.
[0147] From the viewpoint of exposure sensitivity, the photoradical polymerization initiator is preferably a compound selected from the group consisting of trihalomethyltriazine compounds, benzyl dimethyl ketal compounds, α-hydroxyketone compounds, α-aminoketone compounds, acylphosphine compounds, phosphine oxide compounds, metallocene compounds, oxime compounds, triarylimidazole dimers, onium salt compounds, benzothiazole compounds, benzophenone compounds, acetophenone compounds and derivatives thereof, cyclopentadiene-benzene-iron complexes and salts thereof, halomethyloxadiazole compounds, and 3-aryl substituted coumarin compounds.
[0148] More preferred photoradical polymerization initiators are trihalomethyltriazine compounds, α-aminoketone compounds, acylphosphine compounds, phosphine oxide compounds, metallocene compounds, oxime compounds, triarylimidazole dimers, onium salt compounds, benzophenone compounds, and acetophenone compounds. At least one compound selected from the group consisting of trihalomethyltriazine compounds, α-aminoketone compounds, oxime compounds, triarylimidazole dimers, and benzophenone compounds is even more preferred. It is even more preferred to use a metallocene compound or an oxime compound, and even more preferred is an oxime compound.
[0149] In addition, the photoradical polymerization initiator may be benzophenone, N,N'-tetraalkyl-4,4'-diaminobenzophenone such as N,N'-tetramethyl-4,4'-diaminobenzophenone (Michler's ketone), aromatic ketone such as 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1,2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propanone-1, quinones condensed with aromatic rings such as alkylanthraquinones, benzoin ether compounds such as benzoin alkyl ethers, benzoin compounds such as benzoin and alkylbenzoins, benzyl derivatives such as benzyl dimethyl ketal, etc. In addition, a compound represented by the following formula (I) may be used.
[0150] [ka]
[0151] In formula (I), R I00is an alkyl group having 1 to 20 carbon atoms, an alkyl group having 2 to 20 carbon atoms interrupted by one or more oxygen atoms, an alkoxy group having 1 to 12 carbon atoms, a phenyl group, an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, a halogen atom, a cyclopentyl group, a cyclohexyl group, an alkenyl group having 2 to 12 carbon atoms, an alkyl group having 2 to 18 carbon atoms interrupted by one or more oxygen atoms, and a phenyl group substituted with at least one of an alkyl group having 1 to 4 carbon atoms, or a biphenyl; R I01 is a group represented by formula (II), or R I00 is the same group as R I02 ~R I04 each independently represents an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, or a halogen.
[0152] [ka]
[0153] In the formula, R I05 ~R I07 is R in the above formula (I). I02 ~R I04 is the same as:
[0154] In addition, the compounds described in paragraphs 0048 to 0055 of WO 2015 / 125469 can also be used as the photoradical polymerization initiator.
[0155] When a photopolymerization initiator is contained, the content thereof is preferably 0.1 to 30 mass% based on the total solid content of the pattern-forming composition, more preferably 0.1 to 20 mass%, further preferably 0.5 to 15 mass%, and even more preferably 1.0 to 10 mass%. Only one type of photopolymerization initiator may be contained, or two or more types may be contained. When two or more types of photopolymerization initiators are contained, the total amount is preferably within the above range.
[0156] [Photoacid generator] The pattern-forming composition also preferably contains a photoacid generator as a photosensitizer. By including a photoacid generator, for example, acid is generated in exposed areas of the photosensitive film, increasing the solubility of the exposed areas in a developer (e.g., an alkaline aqueous solution), and a positive pattern can be obtained in which the exposed areas are removed by the developer. In addition, by containing a photoacid generator and a crosslinking agent other than the radical crosslinking agent described later, the composition for pattern formation can be configured such that, for example, the acid generated in the exposed area promotes the crosslinking reaction of the crosslinking agent, making the exposed area more difficult to remove by a developer than the non-exposed area. According to such an embodiment, a negative pattern can be obtained.
[0157] The photoacid generator is not particularly limited as long as it generates an acid upon exposure to light, and examples of the photoacid generator include quinone diazide compounds, onium salt compounds such as diazonium salts, phosphonium salts, sulfonium salts, and iodonium salts, and sulfonate compounds such as imide sulfonates, oxime sulfonates, diazodisulfones, disulfones, and o-nitrobenzyl sulfonate.
[0158] Examples of the quinone diazide compound include a polyhydroxy compound to which a sulfonic acid of quinone diazide is bonded via an ester bond, a polyamino compound to which a sulfonic acid of quinone diazide is bonded via a sulfonamide bond, a polyhydroxypolyamino compound to which a sulfonic acid of quinone diazide is bonded via at least one of an ester bond and a sulfonamide bond, etc. In the present invention, for example, it is preferable that 50 mol % or more of the total functional groups of these polyhydroxy compounds or polyamino compounds are substituted with quinone diazide.
[0159] In the present invention, either 5-naphthoquinone diazide sulfonyl group or 4-naphthoquinone diazide sulfonyl group is preferably used as the quinone diazide. 4-naphthoquinone diazide sulfonyl ester compound has absorption in the i-line region of a mercury lamp and is suitable for i-line exposure. 5-naphthoquinone diazide sulfonyl ester compound has absorption extending to the g-line region of a mercury lamp and is suitable for g-line exposure. In the present invention, it is preferable to select a 4-naphthoquinone diazide sulfonyl ester compound or a 5-naphthoquinone diazide sulfonyl ester compound depending on the wavelength of exposure. In addition, naphthoquinone diazide sulfonyl ester compound having a 4-naphthoquinone diazide sulfonyl group and a 5-naphthoquinone diazide sulfonyl group in the same molecule may be contained, or a 4-naphthoquinone diazide sulfonyl ester compound and a 5-naphthoquinone diazide sulfonyl ester compound may be contained.
[0160] The naphthoquinone diazide compound can be synthesized by an esterification reaction between a compound having a phenolic hydroxyl group and a quinone diazide sulfonic acid compound, and can be synthesized by a known method. The use of these naphthoquinone diazide compounds improves the resolution, sensitivity, and film remaining rate. Examples of the naphthoquinone diazide compound include 1,2-naphthoquinone-2-diazide-5-sulfonic acid, 1,2-naphthoquinone-2-diazide-4-sulfonic acid, salts or esters of these compounds.
[0161] Examples of the onium salt compound or sulfonate compound include the compounds described in paragraphs 0064 to 0122 of JP-A No. 2008-013646.
[0162] It is also preferable that the photoacid generator is a compound containing an oxime sulfonate group (hereinafter, also simply referred to as an "oxime sulfonate compound"). The oxime sulfonate compound is not particularly limited as long as it has an oxime sulfonate group, but is preferably an oxime sulfonate compound represented by the following formula (OS-1), or the below-described formula (OS-103), formula (OS-104), or formula (OS-105).
[0163] [ka]
[0164] In formula (OS-1), X 3 represents an alkyl group, an alkoxyl group, or a halogen atom. 3 When there are a plurality of X's, they may be the same or different. 3 The alkyl group and alkoxy group in the above formula (X) may have a substituent. 3 The alkyl group in the above formula (X) is preferably a linear or branched alkyl group having 1 to 4 carbon atoms. 3 The alkoxyl group in X is preferably a linear or branched alkoxyl group having 1 to 4 carbon atoms. 3 The halogen atom in is preferably a chlorine atom or a fluorine atom. In formula (OS-1), m3 represents an integer of 0 to 3, preferably 0 or 1. When m3 is 2 or 3, a plurality of X 3 may be the same or different. In formula (OS-1), R 34 represents an alkyl group or an aryl group, and is preferably an alkyl group having 1 to 10 carbon atoms, an alkoxyl group having 1 to 10 carbon atoms, a halogenated alkyl group having 1 to 5 carbon atoms, a halogenated alkoxyl group having 1 to 5 carbon atoms, a phenyl group which may be substituted with W, a naphthyl group which may be substituted with W, or an anthranyl group which may be substituted with W. W represents a halogen atom, a cyano group, a nitro group, an alkyl group having 1 to 10 carbon atoms, an alkoxyl group having 1 to 10 carbon atoms, a halogenated alkyl group having 1 to 5 carbon atoms or a halogenated alkoxyl group having 1 to 5 carbon atoms, an aryl group having 6 to 20 carbon atoms, or a halogenated aryl group having 6 to 20 carbon atoms.
[0165] In formula (OS-1), m3 is 3, and X 3 is a methyl group, and X 3 The substitution position of is the ortho position, and R 34 Particularly preferred are compounds in which R is a linear alkyl group having 1 to 10 carbon atoms, a 7,7-dimethyl-2-oxonorbornylmethyl group, or a p-tolyl group.
[0166] Specific examples of the oxime sulfonate compound represented by formula (OS-1) include the following compounds described in paragraphs 0064 to 0068 of JP2011-209692A and paragraphs 0158 to 0167 of JP2015-194674A, the contents of which are incorporated herein by reference.
[0167] [ka]
[0168] In formula (OS-103) ~ formula (OS-105), R s1 R represents an alkyl group, an aryl group, or a heteroaryl group, and may be present in plural. s2 R each independently represents a hydrogen atom, an alkyl group, an aryl group, or a halogen atom, and may be present in plurality. s6 each independently represents a halogen atom, an alkyl group, an alkyloxy group, a sulfonic acid group, an aminosulfonyl group or an alkoxysulfonyl group; Xs represents O or S; ns represents 1 or 2; and ms represents an integer of 0 to 6. In formula (OS-103) ~ formula (OS-105), R s1 The alkyl group (preferably having 1 to 30 carbon atoms), aryl group (preferably having 6 to 30 carbon atoms) or heteroaryl group (preferably having 4 to 30 carbon atoms) represented by the following formula may have a substituent T.
[0169] In formula (OS-103) ~ formula (OS-105), R s2is preferably a hydrogen atom, an alkyl group (preferably having 1 to 12 carbon atoms) or an aryl group (preferably having 6 to 30 carbon atoms), and more preferably a hydrogen atom or an alkyl group. s2 Among R, it is preferable that one or two of them are an alkyl group, an aryl group, or a halogen atom, it is more preferable that one of them is an alkyl group, an aryl group, or a halogen atom, and it is particularly preferable that one of them is an alkyl group and the remaining one is a hydrogen atom. s2 The alkyl group or aryl group represented by the following formula (I) may have a substituent T. In formula (OS-103), formula (OS-104), or formula (OS-105), Xs represents O or S, and is preferably O. In the above formulae (OS-103) to (OS-105), the ring containing Xs as a ring member is a 5-membered or 6-membered ring.
[0170] In formulae (OS-103) to (OS-105), ns represents 1 or 2. When Xs is O, ns is preferably 1; and when Xs is S, ns is preferably 2. In formula (OS-103) ~ formula (OS-105), R s6 The alkyl group (preferably having 1 to 30 carbon atoms) and alkyloxy group (preferably having 1 to 30 carbon atoms) represented by the following formula may have a substituent. In formulae (OS-103) to (OS-105), ms represents an integer of 0 to 6, is preferably an integer of 0 to 2, more preferably 0 or 1, and particularly preferably 0.
[0171] Furthermore, the compound represented by formula (OS-103) above is particularly preferably a compound represented by formula (OS-106), formula (OS-110) or formula (OS-111) below; the compound represented by formula (OS-104) above is particularly preferably a compound represented by formula (OS-107) below; and the compound represented by formula (OS-105) above is particularly preferably a compound represented by formula (OS-108) or formula (OS-109) below. [ka]
[0172] In formula (OS-106) ~ formula (OS-111), R t1 represents an alkyl group, an aryl group, or a heteroaryl group; R t7 represents a hydrogen atom or a bromine atom, R t8 represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, a halogen atom, a chloromethyl group, a bromomethyl group, a bromoethyl group, a methoxymethyl group, a phenyl group, or a chlorophenyl group; R t9 represents a hydrogen atom, a halogen atom, a methyl group, or a methoxy group; R t2 represents a hydrogen atom or a methyl group. In formula (OS-106) ~ formula (OS-111), R t7 represents a hydrogen atom or a bromine atom, and is preferably a hydrogen atom.
[0173] In formula (OS-106) ~ formula (OS-111), R t8 represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, a halogen atom, a chloromethyl group, a bromomethyl group, a bromoethyl group, a methoxymethyl group, a phenyl group, or a chlorophenyl group, and is preferably an alkyl group having 1 to 8 carbon atoms, a halogen atom, or a phenyl group, more preferably an alkyl group having 1 to 8 carbon atoms, even more preferably an alkyl group having 1 to 6 carbon atoms, and particularly preferably a methyl group.
[0174] In formula (OS-106) ~ formula (OS-111), R t9 represents a hydrogen atom, a halogen atom, a methyl group or a methoxy group, and is preferably a hydrogen atom. R t2 represents a hydrogen atom or a methyl group, and is preferably a hydrogen atom. In the above oxime sulfonate compound, the stereochemical structure (E, Z) of the oxime may be either one or a mixture. Specific examples of the oxime sulfonate compounds represented by the above formulas (OS-103) to (OS-105) include the compounds described in paragraphs 0088 to 0095 of JP-A No. 2011-209692 and paragraphs 0168 to 0194 of JP-A No. 2015-194674, the contents of which are incorporated herein by reference.
[0175] Other preferable embodiments of the oxime sulfonate compound containing at least one oxime sulfonate group include compounds represented by the following formula (OS-101) and formula (OS-102).
[0176] [ka]
[0177] In formula (OS-101) or formula (OS-102), R u9 R represents a hydrogen atom, an alkyl group, an alkenyl group, an alkoxyl group, an alkoxycarbonyl group, an acyl group, a carbamoyl group, a sulfamoyl group, a sulfo group, a cyano group, an aryl group, or a heteroaryl group. u9 is more preferably a cyano group or an aryl group, u9 More preferably, is a cyano group, a phenyl group, or a naphthyl group. In formula (OS-101) or formula (OS-102), R u2a represents an alkyl group or an aryl group. In formula (OS-101) or formula (OS-102), Xu is -O-, -S-, -NH-, -NR u5 -, -CH 2 -, -CR u6 H- or CR u6 R u7 - represents R u5 ~R u7 each independently represents an alkyl group or an aryl group.
[0178] In formula (OS-101) or formula (OS-102), R u1 ~R u4R each independently represents a hydrogen atom, a halogen atom, an alkyl group, an alkenyl group, an alkoxyl group, an amino group, an alkoxycarbonyl group, an alkylcarbonyl group, an arylcarbonyl group, an amido group, a sulfo group, a cyano group, or an aryl group. u1 ~R u4 Two of the rings may be bonded to each other to form a ring. In this case, the rings may be condensed to form a condensed ring together with the benzene ring. u1 ~R u4 is preferably a hydrogen atom, a halogen atom or an alkyl group, and R u1 ~R u4 It is also preferable that at least two of R are bonded to each other to form an aryl group. u1 ~R u4 is preferably a hydrogen atom. Any of the above-mentioned substituents may further have a substituent.
[0179] The compound represented by the above formula (OS-101) is more preferably a compound represented by the formula (OS-102). In the above oxime sulfonate compound, the stereostructures (E, Z, etc.) of the oxime and benzothiazole rings may each be either one or a mixture. Specific examples of the compound represented by formula (OS-101) include the compounds described in paragraphs 0102 to 0106 of JP-A No. 2011-209692 and paragraphs 0195 to 0207 of JP-A No. 2015-194674, the contents of which are incorporated herein by reference. Among the above compounds, b-9, b-16, b-31 and b-33 are preferred.
[0180] In addition, commercially available photoacid generators may be used. Commercially available products include WPAG-145, WPAG-149, WPAG-170, WPAG-199, WPAG-336, WPAG-367, WPAG-370, WPAG-443, WPAG-469, WPAG-638, and WPAG-699 (all manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), Omnicat 250 and Omnicat 270 (all manufactured by IGM Resins BV), Irgacure 250, Irgacure 270, and Irgacure 290 (all manufactured by BASF), and MBZ-101 (manufactured by Midori Chemical Industry Co., Ltd.).
[0181] Further, compounds represented by the following structural formulas are also preferred examples. [ka]
[0182] As the photoacid generator, an organic halogenated compound can also be used. Specific examples of the organic halogenated compounds include those described in Wakabayashi et al., Bull Chem. Soc Japan, vol. 42, p. 2924 (1969), U.S. Pat. No. 3,905,815, JP-B-4605, JP-A-48-36281, JP-A-55-32070, JP-A-60-239736, JP-A-61-169835, JP-A-61-169837, JP-A-62-58241, JP-A-62-212401, JP-A-63-70243, JP-A-63-298339, and M.P. Hutt, Journal of Heterocyclic Chemistry, Vol. 1 (No. 3), (1970), and in particular, oxazole compounds substituted with a trihalomethyl group: S-triazine compounds. More preferably, an s-triazine derivative having at least one mono-, di-, or trihalogen-substituted methyl group bonded to the s-triazine ring, specifically, for example, 2,4,6-tris(monochloromethyl)-s-triazine, 2,4,6-tris(dichloromethyl)-s-triazine, 2,4,6-tris(trichloromethyl)-s-triazine, 2-methyl-4,6-bis(trichloromethyl)-s-triazine, 2-n-propyl-4,6-bis(trichloromethyl)-s-triazine, riazine, 2-(α,α,β-trichloroethyl)-4,6-bis(trichloromethyl)-s-triazine, 2-phenyl-4,6-bis(trichloromethyl)-s-triazine, 2-(p-methoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(3,4-epoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(p-chlorophenyl)-4,6-bis(trichloromethyl)-s-triazine, 2-[1-(p-methoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine, phenyl)-2,4-butadienyl]-4,6-bis(trichloromethyl)-s-triazine, 2-styryl-4,6-bis(trichloromethyl)-s-triazine, 2-(p-methoxystyryl)-4,6-bis(trichloromethyl)-s-triazine, 2-(pi-propyloxystyryl)-4,6-bis(trichloromethyl)-s-triazine, 2-(p-tolyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(4-nathoxynaphthyl)-4,6- Examples of the bis(trichloromethyl)-s-triazine include bis(trichloromethyl)-s-triazine, 2-phenylthio-4,6-bis(trichloromethyl)-s-triazine, 2-benzylthio-4,6-bis(trichloromethyl)-s-triazine, 2,4,6-tris(dibromomethyl)-s-triazine, 2,4,6-tris(tribromomethyl)-s-triazine, 2-methyl-4,6-bis(tribromomethyl)-s-triazine, and 2-methoxy-4,6-bis(tribromomethyl)-s-triazine.
[0183] As the photoacid generator, an organic borate compound can also be used. Examples of the organic borate compound include those described in JP-A-62-143044, JP-A-62-150242, JP-A-9-188685, JP-A-9-188686, JP-A-9-188710, JP-A-2000-131837, JP-A-2002-107916, Japanese Patent No. 2764769, and Japanese Patent Application No. 2000-310808, and those described in Kunz, Martin, "Rad Tech'98. Proceedings of April 1999, Vol. 1, No. 2, pp. 1111-1115, 1999. 19-22, 1998, Chicago", etc.; organoboron sulfonium complexes or organoboron oxosulfonium complexes described in JP-A-6-157623, JP-A-6-175564, and JP-A-6-175561; organoboron iodonium complexes described in JP-A-6-175554 and JP-A-6-175553; organoboron phosphonium complexes described in JP-A-9-188710; and organoboron transition metal coordination complexes described in JP-A-6-348011, JP-A-7-128785, JP-A-7-140589, JP-A-7-306527, JP-A-7-292014, etc., are specifically exemplified.
[0184] As the photoacid generator, a disulfone compound can also be used. Examples of the disulfone compound include compounds described in JP-A-61-166544 and JP-A-2001-132318, and diazodisulfone compounds.
[0185] Examples of the onium salt compound include diazonium salts described in SI Schlesinger, Photogr. Sci. Eng., 18, 387 (1974) and TSBal et al., Polymer, 21, 423 (1980); ammonium salts described in U.S. Pat. No. 4,069,055 and JP-A-4-365049; phosphonium salts described in U.S. Pat. Nos. 4,069,055 and 4,069,056; and iodonium salts described in European Patent Nos. 104 and 143, U.S. Pat. Nos. 339,049 and 410,201, JP-A-2-150848 and JP-A-2-296514. sulfonium salts described in the specifications of European Patent Nos. 370,693, 390,214, 233,567, 297,443, and 297,442, U.S. Patent Nos. 4,933,377, 161,811, 410,201, 339,049, 4,760,013, 4,734,444, and 2,833,827, German Patent Nos. 2,904,626, 3,604,580, and 3,604,581; selenonium salts described in JV Crivello et al., J. Polymer Sci., Polymer Chem. Ed., 17, 1047(1979); arsonium salts described in C.S. Wen et al., Teh., Proc. Conf. Rad. Curing ASIA, p478, Tokyo, Oct. (1988); and onium salts such as pyridinium salts.
[0186] The onium salt includes onium salts represented by the following general formulas (RI-I) to (RI-III). [ka] In formula (RI-I), Ar11 represents an aryl group having 20 or less carbon atoms which may have 1 to 6 substituents, and preferred substituents include an alkyl group having 1 to 12 carbon atoms, an alkenyl group having 1 to 12 carbon atoms, an alkynyl group having 1 to 12 carbon atoms, an aryl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryloxy group having 1 to 12 carbon atoms, a halogen atom, an alkylamino group having 1 to 12 carbon atoms, a dialkylamino group having 1 to 12 carbon atoms, an alkylamide group or an arylamide group having 1 to 12 carbon atoms, a carbonyl group, a carboxyl group, a cyano group, a sulfonyl group, a thioalkyl group having 1 to 12 carbon atoms, and a thioaryl group having 1 to 12 carbon atoms. Z11 - represents a monovalent anion, such as a halogen ion, a perchlorate ion, a hexafluorophosphate ion, a tetrafluoroborate ion, a sulfonate ion, a sulfinate ion, a thiosulfonate ion, or a sulfate ion, with the perchlorate ion, hexafluorophosphate ion, tetrafluoroborate ion, sulfonate ion, and sulfinate ion being preferred from the standpoint of stability. In formula (RI-II), Ar21 and Ar22 each independently represent an aryl group having 20 or less carbon atoms which may have 1 to 6 substituents, and preferred substituents include an alkyl group having 1 to 12 carbon atoms, an alkenyl group having 1 to 12 carbon atoms, an alkynyl group having 1 to 12 carbon atoms, an aryl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryloxy group having 1 to 12 carbon atoms, a halogen atom, an alkylamino group having 1 to 12 carbon atoms, a dialkylamino group having 1 to 12 carbon atoms, an alkylamide group or an arylamide group having 1 to 12 carbon atoms, a carbonyl group, a carboxyl group, a cyano group, a sulfonyl group, a thioalkyl group having 1 to 12 carbon atoms, and a thioaryl group having 1 to 12 carbon atoms. Z21 -represents a monovalent anion, such as a halogen ion, a perchlorate ion, a hexafluorophosphate ion, a tetrafluoroborate ion, a sulfonate ion, a sulfinate ion, a thiosulfonate ion, or a sulfate ion, and from the standpoint of stability and reactivity, a perchlorate ion, a hexafluorophosphate ion, a tetrafluoroborate ion, a sulfonate ion, a sulfinate ion, or a carboxylate ion is preferred. In formula (RI-III), R31, R32, and R33 each independently represent an aryl group, an alkyl group, an alkenyl group, or an alkynyl group having 20 or less carbon atoms, which may have 1 to 6 substituents, and are preferably aryl groups from the standpoint of reactivity and stability. Preferred substituents include an alkyl group having 1 to 12 carbon atoms, an alkenyl group having 1 to 12 carbon atoms, an alkynyl group having 1 to 12 carbon atoms, an aryl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryloxy group having 1 to 12 carbon atoms, a halogen atom, an alkylamino group having 1 to 12 carbon atoms, a dialkylamino group having 1 to 12 carbon atoms, an alkylamide group or an arylamide group having 1 to 12 carbon atoms, a carbonyl group, a carboxyl group, a cyano group, a sulfonyl group, a thioalkyl group having 1 to 12 carbon atoms, and a thioaryl group having 1 to 12 carbon atoms. - represents a monovalent anion, such as a halogen ion, a perchlorate ion, a hexafluorophosphate ion, a tetrafluoroborate ion, a sulfonate ion, a sulfinate ion, a thiosulfonate ion, or a sulfate ion, and from the standpoint of stability and reactivity, a perchlorate ion, a hexafluorophosphate ion, a tetrafluoroborate ion, a sulfonate ion, a sulfinate ion, or a carboxylate ion is preferred.
[0187] Specific examples include the following: [ka] [ka] [ka] [ka]
[0188] When a photoacid generator is contained, its content is preferably 0.1 to 30 mass % based on the total solid content of the pattern-forming composition, more preferably 0.1 to 20 mass %, and even more preferably 2 to 15 mass %. Only one type of photoacid generator may be contained, or two or more types may be contained. When two or more types of photoacid generators are contained, the total content is preferably within the above range.
[0189] [Photobase Generator] The pattern-forming composition may contain a photobase generator as a photosensitizer. By containing a photobase generator and a crosslinking agent described later, the pattern-forming composition can be configured such that, for example, the base generated in the exposed area promotes cyclization of a specific resin, the crosslinking reaction of the crosslinking agent is promoted, etc., so that the exposed area is more difficult to remove by a developer than the non-exposed area. According to such an embodiment, a negative relief pattern can be obtained.
[0190] The photobase generator is not particularly limited as long as it generates a base upon exposure to light, and any known photobase generator can be used. For example, M. Shirai, and M. Tsunooka, Prog. Polym. Sci., 21, 1 (1996); Masahiro Kadooka, Polymer Processing, 46, 2 (1997); C. Kutal, Coord. Chem. Rev., 211, 353 (2001); Y. Kaneko, A. Sarker, and D. Neckers, Chem. Mater., 11, 170 (1999); H. Tachi, M. Shirai, and M. Tsunooka, J. Photopolym. Sci. Technol., 13, 153 (2000); M. Winkle, and K. Graziano, J. Photopolym. Sci. Technol., 3, 419 (1990); M. Tsunooka, H. Tachi, and As described in S. Yoshitaka, J. Photopolym. Sci. Technol., 9, 13 (1996); K. Suyama, H. Araki, M. Shirai, J. Photopolym. Sci. Technol., 19, 81 (2006), examples of the compound include ionic compounds in which the base component is neutralized by forming a salt, such as transition metal compound complexes, compounds having an ammonium salt structure, and compounds in which the amidine moiety is rendered latent by forming a salt with a carboxylic acid, and nonionic compounds in which the base component is rendered latent by a urethane bond or oxime bond, such as carbamate derivatives, oxime ester derivatives, and acyl compounds. In the present invention, preferred examples of the photobase generator include carbamate derivatives, amide derivatives, imide derivatives, α-cobalt complexes, imidazole derivatives, cinnamic acid amide derivatives, and oxime derivatives.
[0191] The basic substance generated from the photobase generator is not particularly limited, but examples thereof include compounds having an amino group, particularly monoamines, polyamines such as diamines, and amidines. From the viewpoint of the imidization rate, the basic substance preferably has a large pKa in DMSO (dimethyl sulfoxide) of the conjugate acid. The pKa is preferably 1 or more, more preferably 3 or more. The upper limit of the pKa is not particularly limited, but is preferably 20 or less. Here, the pKa refers to the logarithm of the reciprocal of the first dissociation constant of an acid, and can be found in Determination of Organic Structures by Physical Methods (authors: Brown, HC, McDaniel, DH, Hafliger, O., Nachod, FC; editors: Braude, EA, Nachod, FC; Academic Press, New York, 1955) and Data for Biochemical Research (authors: Dawson, RMC et al; Oxford, Clarendon Press, 1959). For compounds not described in these documents, the value calculated from the structural formula using ACD / pKa (ACD / Labs) software is used as the pKa.
[0192] From the viewpoint of storage stability of the pattern forming composition, the photobase generator is preferably a photobase generator that does not contain a salt in its structure, and it is preferable that there is no charge on the nitrogen atom of the base portion generated in the photobase generator. The photobase generator is preferably one in which the base generated is made latent using a covalent bond, and the base generation mechanism is preferably one in which the covalent bond between the nitrogen atom of the base portion generated and the adjacent atom is broken to generate the base. If the photobase generator does not contain a salt in its structure, the photobase generator can be neutralized, so that the solvent solubility is better and the pot life is improved. For these reasons, the amine generated from the photobase generator used in the present invention is preferably a primary amine or a secondary amine. From the viewpoint of the chemical resistance of the pattern, the photobase generator is preferably a photobase generator containing a salt in its structure.
[0193] For the reasons mentioned above, it is preferable that the photobase generator generates a base in a latent form using a covalent bond as described above, and it is preferable that the generated base is latent using an amide bond, a carbamate bond, or an oxime bond. Examples of the photobase generator according to the present invention include photobase generators having a cinnamic acid amide structure as disclosed in JP 2009-080452 A and WO 2009 / 123122 A, photobase generators having a carbamate structure as disclosed in JP 2006-189591 A and JP 2008-247747 A, photobase generators having an oxime structure or a carbamoyloxime structure as disclosed in JP 2007-249013 A and JP 2008-003581 A, but are not limited to these, and other known photobase generator structures can also be used.
[0194] Other examples of the photobase generator include the compounds described in JP2012-093746A, paragraphs
[0185] to
[0188] ,
[0199] to
[0200] , and
[0202] , the compounds described in JP2013-194205A, paragraphs
[0022] to
[0069] , the compounds described in JP2013-204019A, paragraphs
[0026] to
[0074] , and the compound described in WO2010 / 064631A, paragraph
[0052] .
[0195] In addition, commercially available products may be used as the photobase generator. Commercially available products include WPBG-266, WPBG-300, WPGB-345, WPGB-140, WPBG-165, WPBG-027, WPBG-018, WPGB-015, WPBG-041, WPGB-172, WPGB-174, WPBG-166, WPGB-158, WPGB-025, WPGB-168, WPGB-167, and WPBG-082 (all manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), A2502, B5085, N0528, N1052, O0396, O0447, and O0448 (manufactured by Tokyo Chemical Industry Co., Ltd.).
[0196] When a photobase generator is contained, its content is preferably 0.1 to 30 mass% based on the total solid content of the pattern-forming composition, more preferably 0.1 to 20 mass%, and even more preferably 2 to 15 mass%. Only one type of photobase generator may be contained, or two or more types may be contained. When two or more types of photobase generators are contained, the total content is preferably within the above range.
[0197] <Thermal polymerization initiator> The pattern-forming composition may contain a thermal polymerization initiator, and in particular may contain a thermal radical polymerization initiator. The thermal radical polymerization initiator is a compound that generates radicals by thermal energy and initiates or promotes the polymerization reaction of a polymerizable compound. By adding the thermal radical polymerization initiator, the polymerization reaction of the resin and the crosslinking agent can be promoted in the heating step for obtaining a cured product, so that the solvent resistance can be further improved.
[0198] Specific examples of the thermal radical polymerization initiator include the compounds described in paragraphs 0074 to 0118 of JP-A No. 2008-063554.
[0199] When a thermal polymerization initiator is contained, its content is preferably 0.1 to 30 mass% based on the total solid content of the pattern-forming composition, more preferably 0.1 to 20 mass%, and even more preferably 5 to 15 mass%. Only one type of thermal polymerization initiator may be contained, or two or more types may be contained. When two or more types of thermal polymerization initiators are contained, the total amount is preferably within the above range.
[0200] <Thermal acid generator> The pattern-forming composition may contain a thermal acid generator. The thermal acid generator generates an acid upon heating, and has the effect of promoting the crosslinking reaction of at least one compound selected from a compound having a hydroxymethyl group, an alkoxymethyl group, or an acyloxymethyl group, an epoxy compound, an oxetane compound, and a benzoxazine compound.
[0201] The thermal decomposition starting temperature of the thermal acid generator is preferably 50° C. to 270° C., more preferably 50° C. to 250° C. In addition, it is preferable to select as the thermal acid generator a material that does not generate acid during drying (pre-baking: about 70 to 140° C.) after the pattern-forming composition is applied to the substrate, but generates acid during final heating (cure: about 100 to 400° C.) after patterning by subsequent exposure and development, because this can suppress a decrease in sensitivity during development. The thermal decomposition onset temperature is determined as the lowest exothermic peak temperature when the thermal acid generator is heated to 500° C. at 5° C. / min in a pressure-resistant capsule. An example of an instrument used to measure the thermal decomposition onset temperature is Q2000 (manufactured by TA Instruments).
[0202] The acid generated from the thermal acid generator is preferably a strong acid, for example, an arylsulfonic acid such as p-toluenesulfonic acid or benzenesulfonic acid, an alkylsulfonic acid such as methanesulfonic acid, ethanesulfonic acid or butanesulfonic acid, or a haloalkylsulfonic acid such as trifluoromethanesulfonic acid, etc. Examples of such thermal acid generators include those described in paragraph 0055 of JP2013-072935A.
[0203] Among these, from the viewpoint of being less likely to remain in the organic film and being less likely to deteriorate the physical properties of the organic film, those which generate alkylsulfonic acids having 1 to 4 carbon atoms or haloalkylsulfonic acids having 1 to 4 carbon atoms are more preferred, and examples thereof include (4-hydroxyphenyl)dimethylsulfonium methanesulfonate, (4-((methoxycarbonyl)oxy)phenyl)dimethylsulfonium methanesulfonate, benzyl(4-hydroxyphenyl)methylsulfonium methanesulfonate, benzyl(4-((methoxycarbonyl)oxy)phenyl)methylsulfonium methanesulfonate, (4-hydroxyphenyl)methyl((2-methylphenyl)methyl)sulfonium methanesulfonate, (4-hydroxyphenyl)dimethylsulfonium trifluoromethanesulfonate, and the like. As the thermal acid generator, preferred are fluorine, (4-((methoxycarbonyl)oxy)phenyl)dimethylsulfonium trifluoromethanesulfonate, benzyl(4-hydroxyphenyl)methylsulfonium trifluoromethanesulfonate, benzyl(4-((methoxycarbonyl)oxy)phenyl)methylsulfonium trifluoromethanesulfonate, (4-hydroxyphenyl)methyl((2-methylphenyl)methyl)sulfonium trifluoromethanesulfonate, 3-(5-(((propylsulfonyl)oxy)imino)thiophene-2(5H)-ylidene)-2-(o-tolyl)propanenitrile, and 2,2-bis(3-(methanesulfonylamino)-4-hydroxyphenyl)hexafluoropropane.
[0204] In addition, the compounds described in paragraph 0059 of JP-A-2013-167742 are also preferred as thermal acid generators.
[0205] The content of the thermal acid generator is preferably 0.01 parts by mass or more, more preferably 0.1 parts by mass or more, relative to 100 parts by mass of the specific resin. By containing 0.01 parts by mass or more, the crosslinking reaction is promoted, so that the mechanical properties and solvent resistance of the organic film can be further improved. In addition, from the viewpoint of the electrical insulation of the organic film, the content is preferably 20 parts by mass or less, more preferably 15 parts by mass or less, and even more preferably 10 parts by mass or less.
[0206] <Onium salt> The pattern forming composition may further contain an onium salt. In particular, when the pattern-forming composition contains a polyimide precursor or a polybenzoxazole precursor as the specific resin, it preferably contains an onium salt. The type of onium salt is not particularly limited, but preferred examples include ammonium salts, iminium salts, sulfonium salts, iodonium salts and phosphonium salts. Among these, ammonium salts or iminium salts are preferred from the viewpoint of high thermal stability, and sulfonium salts, iodonium salts or phosphonium salts are preferred from the viewpoint of compatibility with the polymer.
[0207] Furthermore, an onium salt is a salt of a cation and an anion having an onium structure, and the cation and anion may or may not be bonded via a covalent bond. That is, the onium salt may be an intramolecular salt having a cationic moiety and an anionic moiety in the same molecular structure, or an intermolecular salt in which a cationic molecule and an anionic molecule, which are separate molecules, are ionic-bonded, but is preferably an intermolecular salt. In addition, in the pattern-forming composition, the cationic moiety or cationic molecule and the anionic moiety or anionic molecule may be ionic-bonded or dissociated. The cation in the onium salt is preferably an ammonium cation, a pyridinium cation, a sulfonium cation, an iodonium cation or a phosphonium cation, and more preferably at least one cation selected from the group consisting of a tetraalkylammonium cation, a sulfonium cation and an iodonium cation.
[0208] The onium salt used in the present invention may be a thermal base generator, which will be described later. The thermal base generator refers to a compound that generates a base when heated, and examples thereof include compounds that generate a base when heated to 40° C. or higher. Examples of the onium salt include the onium salts described in paragraphs 0122 to 0138 of WO 2018 / 043262. In addition, onium salts used in the field of polyimide precursors can be used without particular limitation.
[0209] When the pattern-forming composition contains an onium salt, the content of the onium salt is preferably 0.1 to 50% by mass based on the total solid content of the pattern-forming composition. The lower limit is more preferably 0.5% by mass or more, even more preferably 0.85% by mass or more, and even more preferably 1% by mass or more. The upper limit is more preferably 30% by mass or less, even more preferably 20% by mass or less, and even more preferably 10% by mass or less, and may be 5% by mass or less, or may be 4% by mass or less. The onium salt may be used alone or in combination of two or more. When two or more types are used, the total amount is preferably within the above range.
[0210] <Thermal base generator> The pattern-forming composition may further contain a thermal base generator. In particular, when the pattern-forming composition contains a polyimide precursor or a polybenzoxazole precursor as the specific resin, it is preferable that the composition contains a thermal base generator. The other thermal base generator may be a compound corresponding to the above-mentioned onium salt, or may be a thermal base generator other than the above-mentioned onium salt. Examples of thermal base generators other than the above-mentioned onium salts include nonionic thermal base generators. Examples of the nonionic thermal base generator include compounds represented by formula (B1) or formula (B2). [ka]
[0211] In formula (B1) and formula (B2), Rb 1 , Rb 2 and Rb 3 are each independently an organic group not having a tertiary amine structure, a halogen atom, or a hydrogen atom. 1 and Rb2 cannot be hydrogen atoms at the same time. 1 , Rb 2 and Rb 3 None of the above has a carboxy group. In this specification, the term "tertiary amine structure" refers to a structure in which all three bonds of a trivalent nitrogen atom are covalently bonded to a hydrocarbon carbon atom. Therefore, this does not apply to cases in which the bonded carbon atom is a carbon atom that forms a carbonyl group, that is, when the bonded carbon atom forms an amide group together with the nitrogen atom.
[0212] In formulas (B1) and (B2), Rb 1 , Rb 2 and Rb 3 At least one of these preferably contains a cyclic structure, and more preferably at least two of them contain a cyclic structure. The cyclic structure may be either a monocyclic ring or a condensed ring, and is preferably a monocyclic ring or a condensed ring in which two monocyclic rings are condensed. The monocyclic ring is preferably a 5-membered or 6-membered ring, and more preferably a 6-membered ring. The monocyclic ring is preferably a cyclohexane ring or a benzene ring, and more preferably a cyclohexane ring.
[0213] More specifically, Rb 1 and Rb 2 is preferably a hydrogen atom, an alkyl group (preferably having 1 to 24 carbon atoms, more preferably having 2 to 18 carbon atoms, and even more preferably having 3 to 12 carbon atoms), an alkenyl group (preferably having 2 to 24 carbon atoms, more preferably having 2 to 18 carbon atoms, and even more preferably having 3 to 12 carbon atoms), an aryl group (preferably having 6 to 22 carbon atoms, more preferably having 6 to 18 carbon atoms, and even more preferably having 6 to 10 carbon atoms), or an arylalkyl group (preferably having 7 to 25 carbon atoms, more preferably having 7 to 19 carbon atoms, and even more preferably having 7 to 12 carbon atoms). These groups may have a substituent within the range in which the effects of the present invention are exhibited. Rb 1 and Rb 2 Rb may be bonded to each other to form a ring. The ring formed is preferably a 4- to 7-membered nitrogen-containing heterocycle. 1 and Rb 2is particularly preferably a linear, branched or cyclic alkyl group (preferably having 1 to 24 carbon atoms, more preferably having 2 to 18 carbon atoms, and even more preferably having 3 to 12 carbon atoms) which may have a substituent, more preferably a cycloalkyl group (preferably having 3 to 24 carbon atoms, more preferably having 3 to 18 carbon atoms, and even more preferably having 3 to 12 carbon atoms) which may have a substituent, and even more preferably a cyclohexyl group which may have a substituent.
[0214] Rb 3 Examples of the group include an alkyl group (preferably having 1 to 24 carbon atoms, more preferably having 2 to 18 carbon atoms, and more preferably having 3 to 12 carbon atoms), an aryl group (preferably having 6 to 22 carbon atoms, more preferably having 6 to 18 carbon atoms, and more preferably having 6 to 10 carbon atoms), an alkenyl group (preferably having 2 to 24 carbon atoms, more preferably having 2 to 12 carbon atoms, and more preferably having 2 to 6 carbon atoms), an arylalkyl group (preferably having 7 to 23 carbon atoms, more preferably having 7 to 19 carbon atoms, and more preferably having 7 to 12 carbon atoms), an arylalkenyl group (preferably having 8 to 24 carbon atoms, more preferably having 8 to 20 carbon atoms, and more preferably having 8 to 16 carbon atoms), an alkoxy group (preferably having 1 to 24 carbon atoms, more preferably having 2 to 18 carbon atoms, and more preferably having 3 to 12 carbon atoms), an aryloxy group (preferably having 6 to 22 carbon atoms, more preferably having 6 to 18 carbon atoms, and more preferably having 6 to 12 carbon atoms), and an arylalkyloxy group (preferably having 7 to 23 carbon atoms, more preferably having 7 to 19 carbon atoms, and more preferably having 7 to 12 carbon atoms). Among these, a cycloalkyl group (preferably having 3 to 24 carbon atoms, more preferably having 3 to 18 carbon atoms, and even more preferably having 3 to 12 carbon atoms), an arylalkenyl group, and an arylalkyloxy group are preferable. 3 may further have a substituent within the range in which the effects of the present invention are exhibited.
[0215] The compound represented by formula (B1) is preferably a compound represented by the following formula (B1-1) or (B1-2). [ka]
[0216] In the formula, Rb 11 and Rb 12 , and Rb 31 and Rb32 respectively represent Rb in formula (B1). 1 and Rb 2 is the same as: Rb 13 is an alkyl group (preferably having 1 to 24 carbon atoms, more preferably having 2 to 18 carbon atoms, and even more preferably having 3 to 12 carbon atoms), an alkenyl group (preferably having 2 to 24 carbon atoms, more preferably having 2 to 18 carbon atoms, and even more preferably having 3 to 12 carbon atoms), an aryl group (preferably having 6 to 22 carbon atoms, more preferably having 6 to 18 carbon atoms, and even more preferably having 6 to 12 carbon atoms), or an arylalkyl group (preferably having 7 to 23 carbon atoms, more preferably having 7 to 19 carbon atoms, and even more preferably having 7 to 12 carbon atoms), and may have a substituent within the range in which the effects of the present invention can be achieved. 13 is preferably an arylalkyl group.
[0217] Rb 33 and Rb 34 each independently represents a hydrogen atom, an alkyl group (preferably having 1 to 12 carbon atoms, more preferably having 1 to 8 carbon atoms, and more preferably having 1 to 3 carbon atoms), an alkenyl group (preferably having 2 to 12 carbon atoms, more preferably having 2 to 8 carbon atoms, and more preferably having 2 to 3 carbon atoms), an aryl group (preferably having 6 to 22 carbon atoms, more preferably having 6 to 18 carbon atoms, and more preferably having 6 to 10 carbon atoms), or an arylalkyl group (preferably having 7 to 23 carbon atoms, more preferably having 7 to 19 carbon atoms, and more preferably having 7 to 11 carbon atoms), and a hydrogen atom is preferable.
[0218] Rb 35 is an alkyl group (preferably having 1 to 24 carbon atoms, more preferably having 1 to 12 carbon atoms, and more preferably having 3 to 8 carbon atoms), an alkenyl group (preferably having 2 to 12 carbon atoms, more preferably having 2 to 10 carbon atoms, and more preferably having 3 to 8 carbon atoms), an aryl group (preferably having 6 to 22 carbon atoms, more preferably having 6 to 18 carbon atoms, and more preferably having 6 to 12 carbon atoms), or an arylalkyl group (preferably having 7 to 23 carbon atoms, more preferably having 7 to 19 carbon atoms, and more preferably having 7 to 12 carbon atoms), and an aryl group is preferable.
[0219] The compound represented by formula (B1-1) is also preferably a compound represented by formula (B1-1a). [ka]
[0220] Rb 11 and Rb 12 is Rb in formula (B1-1). 11 and Rb 12 is synonymous with. Rb 15 and Rb 16 represents a hydrogen atom, an alkyl group (preferably having 1 to 12 carbon atoms, more preferably having 1 to 6 carbon atoms, and more preferably having 1 to 3 carbon atoms), an alkenyl group (preferably having 2 to 12 carbon atoms, more preferably having 2 to 6 carbon atoms, and more preferably having 2 to 3 carbon atoms), an aryl group (preferably having 6 to 22 carbon atoms, more preferably having 6 to 18 carbon atoms, and more preferably having 6 to 10 carbon atoms), or an arylalkyl group (preferably having 7 to 23 carbon atoms, more preferably having 7 to 19 carbon atoms, and more preferably having 7 to 11 carbon atoms), and preferably a hydrogen atom or a methyl group. Rb 17 is an alkyl group (preferably having 1 to 24 carbon atoms, more preferably having 1 to 12 carbon atoms, and more preferably having 3 to 8 carbon atoms), an alkenyl group (preferably having 2 to 12 carbon atoms, more preferably having 2 to 10 carbon atoms, and more preferably having 3 to 8 carbon atoms), an aryl group (preferably having 6 to 22 carbon atoms, more preferably having 6 to 18 carbon atoms, and more preferably having 6 to 12 carbon atoms), or an arylalkyl group (preferably having 7 to 23 carbon atoms, more preferably having 7 to 19 carbon atoms, and more preferably having 7 to 12 carbon atoms), and among these, an aryl group is preferable.
[0221] The molecular weight of the nonionic thermal base generator is preferably 800 or less, more preferably 600 or less, and even more preferably 500 or less. The lower limit is preferably 100 or more, more preferably 200 or more, and even more preferably 300 or more.
[0222] Among the above-mentioned onium salts, specific examples of compounds that are thermal base generators, or specific examples of thermal base generators other than the above-mentioned onium salts, include the following compounds.
[0223] [ka]
[0224] [ka]
[0225] [ka]
[0226] The content of the other thermal base generator is preferably 0.1 to 50% by mass based on the total solid content of the pattern-forming composition. The lower limit is more preferably 0.5% by mass or more, and even more preferably 1% by mass or more. The upper limit is more preferably 30% by mass or less, and even more preferably 20% by mass or less. One or more types of thermal base generators can be used. When two or more types are used, the total amount is preferably within the above range.
[0227] <Crosslinking agent> The pattern-forming composition preferably contains a crosslinking agent. The crosslinking agent may be a radical crosslinking agent or other crosslinking agent.
[0228] <Radical crosslinking agent> The pattern-forming composition preferably further contains a radical crosslinking agent. The radical crosslinking agent is a compound having a radical polymerizable group. The radical polymerizable group is preferably a group having an ethylenically unsaturated bond. The group having an ethylenically unsaturated bond includes a group having an ethylenically unsaturated bond such as a vinyl group, an allyl group, a vinylphenyl group, and a (meth)acryloyl group. Among these, the group containing an ethylenically unsaturated bond is preferably a (meth)acryloyl group, and from the viewpoint of reactivity, a (meth)acryloxy group is more preferable.
[0229] The radical crosslinking agent may be a compound having one or more ethylenically unsaturated bonds, and more preferably a compound having two or more ethylenically unsaturated bonds. The compound having two ethylenically unsaturated bonds is preferably a compound having two of the above groups containing an ethylenically unsaturated bond. From the viewpoint of the film strength of the obtained pattern, the pattern-forming composition preferably contains a compound having 3 or more ethylenically unsaturated bonds as a radical crosslinking agent. The compound having 3 or more ethylenically unsaturated bonds is preferably a compound having 3 to 15 ethylenically unsaturated bonds, more preferably a compound having 3 to 10 ethylenically unsaturated bonds, and even more preferably a compound having 3 to 6 ethylenically unsaturated bonds. Furthermore, the compound having three or more ethylenically unsaturated bonds is preferably a compound having three or more groups containing the ethylenically unsaturated bonds, more preferably a compound having 3 to 15 such bonds, even more preferably a compound having 3 to 10 such bonds, and particularly preferably a compound having 3 to 6 such bonds. From the viewpoint of the film strength of the obtained pattern, it is also preferable that the pattern-forming composition contains a compound having two ethylenically unsaturated bonds and the above-mentioned compound having three or more ethylenically unsaturated bonds.
[0230] The molecular weight of the radical crosslinking agent is preferably 2,000 or less, more preferably 1,500 or less, and even more preferably 900 or less. The lower limit of the molecular weight of the radical crosslinking agent is preferably 100 or more.
[0231] Specific examples of the radical crosslinking agent include unsaturated carboxylic acids (e.g., acrylic acid, methacrylic acid, itaconic acid, crotonic acid, isocrotonic acid, maleic acid, etc.) and their esters and amides, preferably esters of unsaturated carboxylic acids and polyhydric alcohol compounds, and amides of unsaturated carboxylic acids and polyvalent amine compounds. In addition, addition reaction products of unsaturated carboxylic acid esters or amides having nucleophilic substituents such as hydroxyl groups, amino groups, and sulfanyl groups with monofunctional or polyfunctional isocyanates or epoxies, and dehydration condensation reaction products of monofunctional or polyfunctional carboxylic acids are also preferably used. In addition, addition reaction products of unsaturated carboxylic acid esters or amides having electrophilic substituents such as isocyanate groups and epoxy groups with monofunctional or polyfunctional alcohols, amines, and thiols, and substitution reaction products of unsaturated carboxylic acid esters or amides having eliminable substituents such as halogeno groups and tosyloxy groups with monofunctional or polyfunctional alcohols, amines, and thiols are also suitable. As another example, it is also possible to use a compound group in which the above unsaturated carboxylic acid is replaced with an unsaturated phosphonic acid, a vinylbenzene derivative such as styrene, a vinyl ether, an allyl ether, etc. As specific examples, the description in paragraphs 0113 to 0122 of JP2016-027357A can be referred to, and the contents of these are incorporated herein by reference.
[0232] In addition, the radical crosslinking agent is preferably a compound having a boiling point of 100° C. or more under normal pressure. Examples of such a compound include polyethylene glycol di(meth)acrylate, trimethylolethane tri(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, hexanediol (meth)acrylate, trimethylolpropane tri(acryloyloxypropyl)ether, tri(acryloyloxyethyl)isocyanurate, glycerin, trimethylolethane, and many other compounds. Examples of the compound include polyfunctional acrylates and methacrylates such as compounds obtained by adding ethylene oxide or propylene oxide to a functional alcohol and then (meth)acrylating the compound, urethane (meth)acrylates as described in JP-B-48-041708, JP-B-50-006034, and JP-A-51-037193, polyester acrylates as described in JP-A-48-064183, JP-B-49-043191, and JP-A-52-030490, and epoxy acrylates which are reaction products of epoxy resins and (meth)acrylic acid, and mixtures thereof. Compounds described in paragraphs 0254 to 0257 of JP-A-2008-292970 are also suitable. Further, there can be mentioned polyfunctional (meth)acrylates obtained by reacting a polyfunctional carboxylic acid with a compound having a cyclic ether group and an ethylenically unsaturated bond, such as glycidyl (meth)acrylate.
[0233] In addition, as preferred radical crosslinking agents other than those described above, compounds having a fluorene ring and two or more groups having an ethylenically unsaturated bond, as described in JP-A-2010-160418, JP-A-2010-129825, Japanese Patent No. 4364216, etc., and cardo resins can also be used.
[0234] Other examples include specific unsaturated compounds described in JP-B-46-043946, JP-B-01-040337, and JP-B-01-040336, and vinylphosphonic acid compounds described in JP-A-02-025493. Compounds containing perfluoroalkyl groups described in JP-A-61-022048 can also be used. Furthermore, those introduced as photopolymerizable monomers and oligomers in the Journal of the Japan Adhesion Association, Vol. 20, No. 7, pages 300-308 (1984) can also be used.
[0235] In addition to the above, the compounds described in paragraphs 0048 to 0051 of JP 2015-034964 A and the compounds described in paragraphs 0087 to 0131 of WO 2015 / 199219 A can also be preferably used, the contents of which are incorporated herein by reference.
[0236] In addition, compounds obtained by adding ethylene oxide or propylene oxide to a polyfunctional alcohol and then (meth)acrylating the resulting compound, which are described in JP-A-10-062986 as formula (1) and formula (2) together with specific examples thereof, can also be used as radical crosslinking agents.
[0237] Furthermore, the compounds described in paragraphs 0104 to 0131 of JP-A-2015-187211 can also be used as radical crosslinking agents, the contents of which are incorporated herein by reference.
[0238] As the radical crosslinking agent, dipentaerythritol triacrylate (commercially available products include KAYARAD D-330, manufactured by Nippon Kayaku Co., Ltd.), dipentaerythritol tetraacrylate (commercially available products include KAYARAD D-320, manufactured by Nippon Kayaku Co., Ltd., and A-TMMT, manufactured by Shin-Nakamura Chemical Co., Ltd.), dipentaerythritol penta(meth)acrylate (commercially available products include KAYARAD D-310, manufactured by Nippon Kayaku Co., Ltd.), dipentaerythritol hexa(meth)acrylate (commercially available products include KAYARAD DPHA, manufactured by Nippon Kayaku Co., Ltd., and A-DPH, manufactured by Shin-Nakamura Chemical Co., Ltd.), and structures in which these (meth)acryloyl groups are bonded via ethylene glycol residues or propylene glycol residues are preferred. Oligomer types of these may also be used.
[0239] Commercially available radical crosslinking agents include, for example, SR-494, a tetrafunctional acrylate having four ethyleneoxy chains, manufactured by Sartomer Corporation; SR-209, 231, and 239, difunctional methacrylates having four ethyleneoxy chains, manufactured by Sartomer Corporation; DPCA-60, a hexafunctional acrylate having six pentyleneoxy chains, TPA-330, a trifunctional acrylate having three isobutyleneoxy chains, manufactured by Nippon Kayaku Co., Ltd.; and urethane Examples of such oligomers include UAS-10 and UAB-140 (manufactured by Nippon Paper Industries Co., Ltd.), NK Ester M-40G, NK Ester 4G, NK Ester M-9300, NK Ester A-9300, and UA-7200 (manufactured by Shin-Nakamura Chemical Co., Ltd.), DPHA-40H (manufactured by Nippon Kayaku Co., Ltd.), UA-306H, UA-306T, UA-306I, AH-600, T-600, and AI-600 (manufactured by Kyoeisha Chemical Co., Ltd.), and Blenmer PME400 (manufactured by NOF Corporation).
[0240] As the radical crosslinking agent, urethane acrylates as described in JP-B-48-041708, JP-A-51-037193, JP-B-02-032293, and JP-B-02-016765, and urethane compounds having an ethylene oxide skeleton as described in JP-B-58-049860, JP-B-56-017654, JP-B-62-039417, and JP-B-62-039418 are also suitable. Furthermore, as the radical crosslinking agent, compounds having an amino structure or a sulfide structure in the molecule as described in JP-A-63-277653, JP-A-63-260909, and JP-A-01-105238 can also be used.
[0241] The radical crosslinking agent may be a radical crosslinking agent having an acid group such as a carboxy group or a phosphoric acid group. The radical crosslinking agent having an acid group is preferably an ester of an aliphatic polyhydroxy compound and an unsaturated carboxylic acid, and more preferably a radical crosslinking agent in which an acid group is provided by reacting a non-aromatic carboxylic anhydride with an unreacted hydroxy group of an aliphatic polyhydroxy compound. Particularly preferred is a compound in which the aliphatic polyhydroxy compound is pentaerythritol or dipentaerythritol in a radical crosslinking agent in which an acid group is provided by reacting a non-aromatic carboxylic anhydride with an unreacted hydroxy group of an aliphatic polyhydroxy compound. Examples of commercially available products include M-510, M-520, etc., as polybasic acid modified acrylic oligomers manufactured by Toagosei Co., Ltd.
[0242] The acid value of the radical crosslinking agent having an acid group is preferably 0.1 to 40 mgKOH / g, and particularly preferably 5 to 30 mgKOH / g. If the acid value of the radical crosslinking agent is within the above range, the handling property during production is excellent, and furthermore, the developability is excellent. Also, the polymerizability is good. On the other hand, from the viewpoint of the development speed in the case of alkali development, the acid value of the radical crosslinking agent having an acid group is preferably 0.1 to 300 mgKOH / g, and particularly preferably 1 to 100 mgKOH / g. The acid value is measured in accordance with the description of JIS K 0070:1992.
[0243] From the viewpoints of pattern resolution and film elasticity, the pattern-forming composition preferably uses a bifunctional methacrylate or acrylate. Specific compounds include triethylene glycol diacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, tetraethylene glycol diacrylate, PEG200 diacrylate, PEG200 dimethacrylate, PEG600 diacrylate, PEG600 dimethacrylate, polytetraethylene glycol diacrylate, polytetraethylene glycol dimethacrylate, neopentyl glycol diacrylate, neopentyl glycol dimethacrylate, 3-methyl-1,5-pentanediol diacrylate, and 1,6-hexanediol diacrylate. , 1,6-hexanediol dimethacrylate, dimethylol-tricyclodecane diacrylate, dimethylol-tricyclodecane dimethacrylate, EO adduct diacrylate of bisphenol A, EO adduct dimethacrylate of bisphenol A, PO adduct diacrylate of bisphenol A, PO adduct dimethacrylate of bisphenol A, 2-hydroxy-3-acryloyloxypropyl methacrylate, isocyanuric acid EO modified diacrylate, isocyanuric acid modified dimethacrylate, other bifunctional acrylates having urethane bonds, and bifunctional methacrylates having urethane bonds can be used. Two or more of these can be mixed and used as necessary. In addition, from the viewpoint of suppressing warpage associated with controlling the elastic modulus of the pattern, a monofunctional radical crosslinking agent can be preferably used as the radical crosslinking agent.As the monofunctional radical crosslinking agent, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, butoxyethyl (meth)acrylate, carbitol (meth)acrylate, cyclohexyl (meth)acrylate, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, N-methylol (meth)acrylamide, glycidyl (meth)acrylate, polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, and other (meth)acrylic acid derivatives, N-vinyl compounds such as N-vinylpyrrolidone and N-vinylcaprolactam, and allyl compounds such as allyl glycidyl ether, diallyl phthalate, and triallyl trimellitate are preferably used. As the monofunctional radical crosslinking agent, a compound having a boiling point of 100° C. or more under normal pressure is also preferred in order to suppress volatilization before exposure.
[0244] When the radical crosslinking agent is contained, the content thereof is preferably more than 0% by mass and not more than 60% by mass based on the total solid content of the pattern-forming composition. The lower limit is more preferably 5% by mass or more. The upper limit is more preferably 50% by mass or less, and even more preferably 30% by mass or less.
[0245] The radical crosslinking agent may be used alone or in combination of two or more. When two or more types are used in combination, the total amount is preferably within the above range.
[0246] <Other crosslinking agents> The pattern-forming composition preferably contains a crosslinking agent other than the above-mentioned radical crosslinking agent. In the present invention, the other crosslinking agent refers to a crosslinking agent other than the above-mentioned radical crosslinking agent, and is preferably a compound having in its molecule a plurality of groups that promote a reaction to form a covalent bond with another compound in the pattern-forming composition or a reaction product thereof upon exposure to light by the above-mentioned photosensitizer, and is preferably a compound having in its molecule a plurality of groups that promote a reaction to form a covalent bond with another compound in the pattern-forming composition or a reaction product thereof under the action of an acid or a base. The acid or base is preferably an acid or base generated from a photoacid generator or photobase generator, which is a photosensitizer, in the exposure step. As the other crosslinking agent, a compound having at least one group selected from the group consisting of a methylol group and an alkoxymethyl group is preferred, and a compound having a structure in which at least one group selected from the group consisting of a methylol group and an alkoxymethyl group is directly bonded to a nitrogen atom is more preferred. Other crosslinking agents include compounds having a structure in which an amino group-containing compound such as melamine, glycoluril, urea, alkylene urea, or benzoguanamine is reacted with formaldehyde or formaldehyde and alcohol, and the hydrogen atom of the amino group is replaced with a methylol group or an alkoxymethyl group.The method for producing these compounds is not particularly limited, and they may be compounds having the same structure as the compounds produced by the above method.In addition, they may be oligomers formed by self-condensation of the methylol groups of these compounds. As the above amino group-containing compound, a crosslinking agent using melamine is called a melamine-based crosslinking agent, a crosslinking agent using glycoluril, urea or alkylene urea is called a urea-based crosslinking agent, a crosslinking agent using alkylene urea is called an alkylene urea-based crosslinking agent, and a crosslinking agent using benzoguanamine is called a benzoguanamine-based crosslinking agent. Among these, the pattern-forming composition preferably contains at least one compound selected from the group consisting of urea-based crosslinking agents and melamine-based crosslinking agents, and more preferably contains at least one compound selected from the group consisting of glycoluril-based crosslinking agents and melamine-based crosslinking agents described below.
[0247] Specific examples of the melamine-based crosslinking agent include hexamethoxymethylmelamine, hexaethoxymethylmelamine, hexapropoxymethylmelamine, and hexabutoxybutylmelamine.
[0248] Specific examples of urea-based crosslinking agents include glycoluril-based crosslinking agents such as monohydroxymethylated glycoluril, dihydroxymethylated glycoluril, trihydroxymethylated glycoluril, tetrahydroxymethylated glycoluril, monomethoxymethylated glycoluril, dimethoxymethylated glycoluril, trimethoxymethylated glycoluril, tetramethoxymethylated glycoluril, monomethoxymethylated glycoluril, dimethoxymethylated glycoluril, trimethoxymethylated glycoluril, tetraethoxymethylated glycoluril, monopropoxymethylated glycoluril, dipropoxymethylated glycoluril, tripropoxymethylated glycoluril, tetrapropoxymethylated glycoluril, monobutoxymethylated glycoluril, dibutoxymethylated glycoluril, tributoxymethylated glycoluril, and tetrabutoxymethylated glycoluril; Urea-based crosslinking agents such as bismethoxymethylurea, bisethoxymethylurea, bispropoxymethylurea, and bisbutoxymethylurea; ethyleneurea-based crosslinking agents such as monohydroxymethylated ethyleneurea or dihydroxymethylated ethyleneurea, monomethoxymethylated ethyleneurea, dimethoxymethylated ethyleneurea, monoethoxymethylated ethyleneurea, diethoxymethylated ethyleneurea, monopropoxymethylated ethyleneurea, dipropoxymethylated ethyleneurea, monobutoxymethylated ethyleneurea, or dibutoxymethylated ethyleneurea; propylene urea-based crosslinking agents such as monohydroxymethylated propylene urea, dihydroxymethylated propylene urea, monomethoxymethylated propylene urea, dimethoxymethylated propylene urea, monodiethoxymethylated propylene urea, diethoxymethylated propylene urea, monopropoxymethylated propylene urea, dipropoxymethylated propylene urea, monobutoxymethylated propylene urea, or dibutoxymethylated propylene urea; Examples include 1,3-di(methoxymethyl)-4,5-dihydroxy-2-imidazolidinone and 1,3-di(methoxymethyl)-4,5-dimethoxy-2-imidazolidinone.
[0249] Specific examples of benzoguanamine-based crosslinking agents include monohydroxymethylated benzoguanamine, dihydroxymethylated benzoguanamine, trihydroxymethylated benzoguanamine, tetrahydroxymethylated benzoguanamine, monomethoxymethylated benzoguanamine, dimethoxymethylated benzoguanamine, trimethoxymethylated benzoguanamine, tetramethoxymethylated benzoguanamine, monomethoxymethylated benzoguanamine, dimethoxymethylated benzoguanamine, trimethoxymethylated benzoguanamine, tetraethoxymethylated benzoguanamine, monopropoxymethylated benzoguanamine, dipropoxymethylated benzoguanamine, tripropoxymethylated benzoguanamine, tetrapropoxymethylated benzoguanamine, monobutoxymethylated benzoguanamine, dibutoxymethylated benzoguanamine, tributoxymethylated benzoguanamine, and tetrabutoxymethylated benzoguanamine.
[0250] In addition, as the compound having at least one group selected from the group consisting of a methylol group and an alkoxymethyl group, a compound in which at least one group selected from the group consisting of a methylol group and an alkoxymethyl group is directly bonded to an aromatic ring (preferably a benzene ring) is also preferably used. Specific examples of such compounds include benzenedimethanol, bis(hydroxymethyl)cresol, bis(hydroxymethyl)dimethoxybenzene, bis(hydroxymethyl)diphenyl ether, bis(hydroxymethyl)benzophenone, hydroxymethylphenyl hydroxymethylbenzoate, bis(hydroxymethyl)biphenyl, dimethylbis(hydroxymethyl)biphenyl, bis(methoxymethyl)benzene, bis(methoxymethyl)cresol, bis(methoxymethyl)dimethoxybenzene, bis(methoxymethyl)diphenyl ether, bis(methoxymethyl)benzophenone, methoxymethylphenyl methoxymethylbenzoate, bis(methoxymethyl)biphenyl, dimethylbis(methoxymethyl)biphenyl, 4,4',4''-ethylidene tris[2,6-bis(methoxymethyl)phenol], 5,5'-[2,2,2-trifluoro-1-(trifluoromethyl)ethylidene]bis[2-hydroxy-1,3-benzenedimethanol], and 3,3',5,5'-tetrakis(methoxymethyl)-1,1'-biphenyl-4,4'-diol.
[0251] As the other crosslinking agent, commercially available products may be used, and suitable commercially available products include 46DMOC, 46DMOEP (both manufactured by Asahi Organic Chemicals Co., Ltd.), DML-PC, DML-PEP, DML-OC, DML-OEP, DML-34X, DML-PTBP, DML-PCHP, DML-OCHP, DML-PFP, DML-PSBP, DML-POP, DML-MBOC, DML-MBPC, DML-MTrisPC, DML-BisOC-Z, DML-BisOCHP-Z, DML-BPC, DMLBisOC-P, DMOM-PC, DMOM-PTBP, DMOM-MBPC, TriML-P, and TriML-35XL. , TML-HQ, TML-BP, TML-pp-BPF, TML-BPE, TML-BPA, TML-BPAF, TML-BPAP, TMOM-BP, TMOM-BPE, TMOM-BPA, TMOM-BPAF, TMOM-BPAP, HML-TPPHBA, HML-TPHAP, HMOM-TPPHBA, HMOM-TPHAP (all manufactured by Honshu Chemical Industry Co., Ltd.), Nikalac (registered trademark, the same applies below) MX-290, Nikalac MX-280, Nikalac MX-270, Nikalac MX-279, Nikalac MW-100LM, Nikalac MX-750LM (all manufactured by Sanwa Chemical Co., Ltd.), and the like.
[0252] The pattern-forming composition also preferably contains, as another crosslinking agent, at least one compound selected from the group consisting of epoxy compounds, oxetane compounds, and benzoxazine compounds.
[0253] [Epoxy compounds (compounds having an epoxy group)] The epoxy compound is preferably a compound having two or more epoxy groups in one molecule. The epoxy group undergoes a crosslinking reaction at 200°C or less, and does not undergo a dehydration reaction due to crosslinking, so film shrinkage is unlikely to occur. Therefore, the inclusion of an epoxy compound is effective in curing the pattern-forming composition at a low temperature and suppressing warpage.
[0254] The epoxy compound preferably contains a polyethylene oxide group. This further reduces the elastic modulus and suppresses warping. The polyethylene oxide group refers to a group having 2 or more repeating ethylene oxide units, and the number of repeating units is preferably 2 to 15.
[0255] Examples of epoxy compounds include, but are not limited to, bisphenol A type epoxy resins; bisphenol F type epoxy resins; alkylene glycol type epoxy resins or polyhydric alcohol hydrocarbon type epoxy resins such as propylene glycol diglycidyl ether, neopentyl glycol diglycidyl ether, ethylene glycol diglycidyl ether, butylene glycol diglycidyl ether, hexamethylene glycol diglycidyl ether, and trimethylolpropane triglycidyl ether; polyalkylene glycol type epoxy resins such as polypropylene glycol diglycidyl ether; and epoxy group-containing silicones such as polymethyl(glycidyloxypropyl)siloxane.Specifically, Epicron (registered trademark) 850-S, Epicron (registered trademark) HP-4032, Epicron (registered trademark) HP-7200, Epicron (registered trademark) HP-820, Epicron (registered trademark) HP-4700, Epicron (registered trademark) EXA-4710, Epicron (registered trademark) HP-4770, Epicron (registered trademark) EXA-859CRP, Epicron (registered trademark) EXA-1514, Epicron (registered trademark) EXA-4880, Epicron (registered trademark) EXA-4850-15 0, Epicron EXA-4850-1000, Epicron (registered trademark) EXA-4816, Epicron (registered trademark) EXA-4822, Epicron (registered trademark) EXA-830LVP, Epicron (registered trademark) EXA-8183, Epicron (registered trademark) EXA-8169, Epicron (registered trademark) N-660, Epicron (registered trademark) N-665-EXP-S, Epicron (registered trademark) N-740, Likaresin (registered trademark) BEO-20E (all trade names, manufactured by DIC Corporation), Likaresin (registered trademark) (registered trademark) BEO-60E, Likaresin (registered trademark) HBE-100, Likaresin (registered trademark) DME-100, Likaresin (registered trademark) L-200 (product name, New Japan Chemical Co., Ltd.), EP-4003S, EP-4000S, EP-4088S, EP-3950S (all product names, manufactured by ADEKA Corporation), Celoxide 2021P, 2081, 2000, 3000, EHPE3150, Epolead GT400, Cellvinars B0134, B0177 (all product names, manufactured by Daicel Corporation), NC-300 0, NC-3000-L, NC-3000-H, NC-3000-FH-75M, NC-3100, CER-3000-L, NC-2000-L, XD-1000, NC-7000L, NC-7300L, EPPN-501H, EPPN-501HY, EPPN-502H, EOCN-1020, EOCN-102S, EOCN-103S, EOCN-104S, CER-1020, EPPN-201, BREN-S, BREN-10S (all trade names, manufactured by Nippon Kayaku Co., Ltd.).
[0256] [Oxetane compounds (compounds having an oxetanyl group)] Examples of the oxetane compound include compounds having two or more oxetane rings in one molecule, 3-ethyl-3-hydroxymethyloxetane, 1,4-bis{[(3-ethyl-3-oxetanyl)methoxy]methyl}benzene, 3-ethyl-3-(2-ethylhexylmethyl)oxetane, 1,4-benzenedicarboxylic acid-bis[(3-ethyl-3-oxetanyl)methyl]ester, etc. Specific examples include the Aron Oxetane series (e.g., OXT-121, OXT-221, OXT-191, OXT-223) manufactured by Toagosei Co., Ltd., which may be used alone or in combination of two or more kinds.
[0257] [Benzoxazine compounds (compounds having a benzoxazolyl group)] Benzoxazine compounds are preferred because they undergo a crosslinking reaction derived from a ring-opening addition reaction, so that degassing does not occur during curing, and further, they reduce thermal shrinkage and suppress the occurrence of warping.
[0258] Preferred examples of benzoxazine compounds include Ba-type benzoxazine, Bm-type benzoxazine, Pd-type benzoxazine, Fa-type benzoxazine (all trade names, manufactured by Shikoku Chemical Industry Co., Ltd.), benzoxazine adducts of polyhydroxystyrene resins, and phenol novolac-type dihydrobenzoxazine compounds. These may be used alone or in combination of two or more.
[0259] The content of the other crosslinking agent is preferably 0.1 to 30% by mass, more preferably 0.1 to 20% by mass, further preferably 0.5 to 15% by mass, and particularly preferably 1.0 to 10% by mass, based on the total solid content of the pattern-forming composition. Only one type of other crosslinking agent may be contained, or two or more types may be contained. When two or more types of other crosslinking agents are contained, the total amount is preferably within the above range.
[0260] <Compounds having a sulfonamide structure, compounds having a thiourea structure> From the viewpoint of improving the adhesion of the resulting pattern to the substrate, it is preferable that the pattern-forming composition further contains at least one compound selected from the group consisting of compounds having a sulfonamide structure and compounds having a thiourea structure.
[0261] [Compounds having a sulfonamide structure] The sulfonamide structure is a structure represented by the following formula (S-1). [ka] In formula (S-1), R represents a hydrogen atom or an organic group, R may bond to another structure to form a ring structure, and each * independently represents a bonding site to another structure. The above R is R in the following formula (S-2): 2 It is preferable that the group is the same as the following group. The compound having a sulfonamide structure may be a compound having two or more sulfonamide structures, but is preferably a compound having one sulfonamide structure.
[0262] The compound having a sulfonamide structure is preferably a compound represented by the following formula (S-2). [ka] In formula (S-2), R 1 , R 2 and R 3 each independently represents a hydrogen atom or a monovalent organic group; R 1 , R 2 and R 3 Two or more of these may be bonded to each other to form a ring structure. R 1 , R 2 and R 3 is preferably each independently a monovalent organic group. R 1 , R 2 and R 3Examples of the alkyl group include a hydrogen atom, an alkyl group, a cycloalkyl group, an alkoxy group, an alkyl ether group, an alkylsilyl group, an alkoxysilyl group, an aryl group, an aryl ether group, a carboxy group, a carbonyl group, an allyl group, a vinyl group, a heterocyclic group, or a combination of two or more of these groups. The alkyl group is preferably an alkyl group having 1 to 10 carbon atoms, and more preferably an alkyl group having 1 to 6 carbon atoms. Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, an isopropyl group, and a 2-ethylhexyl group. The above cycloalkyl group is preferably a cycloalkyl group having 5 to 10 carbon atoms, more preferably a cycloalkyl group having 6 to 10 carbon atoms. Examples of the above cycloalkyl group include a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, and a cyclohexyl group. The above alkoxy group is preferably an alkoxy group having 1 to 10 carbon atoms, and more preferably an alkoxy group having 1 to 5 carbon atoms. Examples of the above alkoxy group include a methoxy group, an ethoxy group, a propoxy group, a butoxy group, and a pentoxy group. The above alkoxysilyl group is preferably an alkoxysilyl group having 1 to 10 carbon atoms, and more preferably an alkoxysilyl group having 1 to 4 carbon atoms. Examples of the above alkoxysilyl group include a methoxysilyl group, an ethoxysilyl group, a propoxysilyl group, and a butoxysilyl group. The aryl group is preferably an aryl group having 6 to 20 carbon atoms, more preferably an aryl group having 6 to 12 carbon atoms. The aryl group may have a substituent such as an alkyl group. Examples of the aryl group include a phenyl group, a tolyl group, a xylyl group, and a naphthyl group. Examples of the heterocyclic group include a triazole ring, a pyrrole ring, a furan ring, a thiophene ring, an imidazole ring, an oxazole ring, a thiazole ring, a pyrazole ring, an isoxazole ring, an isothiazole ring, a tetrazole ring, a pyridine ring, a pyridazine ring, a pyrimididine ring, a pyrazine ring, a piperidine ring, a piperazine ring, a morpholine ring, a dihydropyran ring, a tetrahydropyran group, and a group in which one hydrogen atom has been removed from a heterocyclic structure such as a triazine ring.
[0263] Among these, R 1 is an aryl group, and R 2 and R 3 are each independently a hydrogen atom or an alkyl group.
[0264] Examples of compounds having a sulfonamide structure include benzenesulfonamide, dimethylbenzenesulfonamide, N-butylbenzenesulfonamide, sulfanilamide, o-toluenesulfonamide, p-toluenesulfonamide, hydroxynaphthalenesulfonamide, naphthalene-1-sulfonamide, naphthalene-2-sulfonamide, m-nitrobenzenesulfonamide, p-chlorobenzenesulfonamide, methanesulfonamide, N,N-dimethylmethanesulfonamide, N,N-dimethylethanesulfonamide, N,N-diethylmethanesulfonamide, N-methoxymethanesulfonamide, N-dodecylmethanesulfonamide, N-cyclohexyl-1-butanesulfonamide, and 2-aminoethanesulfonamide.
[0265] [Compounds having a thiourea structure] The thiourea structure is a structure represented by the following formula (T-1). [ka] In formula (T-1), R 4 and R 5 each independently represents a hydrogen atom or a monovalent organic group; R 4 and R 5may be bonded to form a ring structure, R 4 may combine with another structure to which * is bonded to form a ring structure, R 5 may bond to another structure to which the * is bonded to form a ring structure, and each * independently represents a bonding site to another structure.
[0266] R 4 and R 5 are each preferably independently a hydrogen atom. R 4 and R 5 Examples of the alkyl group include a hydrogen atom, an alkyl group, a cycloalkyl group, an alkoxy group, an alkyl ether group, an alkylsilyl group, an alkoxysilyl group, an aryl group, an aryl ether group, a carboxy group, a carbonyl group, an allyl group, a vinyl group, a heterocyclic group, or a combination of two or more of these groups. The alkyl group is preferably an alkyl group having 1 to 10 carbon atoms, and more preferably an alkyl group having 1 to 6 carbon atoms. Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, an isopropyl group, and a 2-ethylhexyl group. The above cycloalkyl group is preferably a cycloalkyl group having 5 to 10 carbon atoms, more preferably a cycloalkyl group having 6 to 10 carbon atoms. Examples of the above cycloalkyl group include a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, and a cyclohexyl group. The above alkoxy group is preferably an alkoxy group having 1 to 10 carbon atoms, and more preferably an alkoxy group having 1 to 5 carbon atoms. Examples of the above alkoxy group include a methoxy group, an ethoxy group, a propoxy group, a butoxy group, and a pentoxy group. The above alkoxysilyl group is preferably an alkoxysilyl group having 1 to 10 carbon atoms, and more preferably an alkoxysilyl group having 1 to 4 carbon atoms. Examples of the above alkoxysilyl group include a methoxysilyl group, an ethoxysilyl group, a propoxysilyl group, and a butoxysilyl group. The aryl group is preferably an aryl group having 6 to 20 carbon atoms, more preferably an aryl group having 6 to 12 carbon atoms. The aryl group may have a substituent such as an alkyl group. Examples of the aryl group include a phenyl group, a tolyl group, a xylyl group, and a naphthyl group. Examples of the heterocyclic group include a triazole ring, a pyrrole ring, a furan ring, a thiophene ring, an imidazole ring, an oxazole ring, a thiazole ring, a pyrazole ring, an isoxazole ring, an isothiazole ring, a tetrazole ring, a pyridine ring, a pyridazine ring, a pyrimididine ring, a pyrazine ring, a piperidine ring, a piperazine ring, a morpholine ring, a dihydropyran ring, a tetrahydropyran group, and a group in which one hydrogen atom has been removed from a heterocyclic structure such as a triazine ring. The compound having a thiourea structure may be a compound having two or more thiourea structures, but is preferably a compound having one thiourea structure.
[0267] The compound having a thiourea structure is preferably a compound represented by the following formula (T-2). [ka] In formula (T-2), R 4 ~R 7 each independently represents a hydrogen atom or a monovalent organic group; R 4 ~R 7 At least two of these may be bonded to each other to form a ring structure.
[0268] In formula (T-2), R 4 and R 5 is R in formula (T-1) 4 and R 5 The same applies to the preferred embodiments. In formula (T-2), R 6 and R 7 is preferably each independently a monovalent organic group. In formula (T-2), R 6 and R 7 A preferred embodiment of the monovalent organic group in formula (T-1) is4 and R 5 The preferred embodiments are the same as those of the monovalent organic group in the above.
[0269] Examples of compounds having a thiourea structure include N-acetylthiourea, N-allylthiourea, N-allyl-N'-(2-hydroxyethyl)thiourea, 1-adamantylthiourea, N-benzoylthiourea, N,N'-diphenylthiourea, 1-benzyl-phenylthiourea, 1,3-dibutylthiourea, 1,3-diisopropylthiourea, 1,3-dicyclohexylthiourea, 1-(3-(trimethoxysilyl)propyl)-3-methylthiourea, trimethylthiourea, tetramethylthiourea, N,N-diphenylthiourea, ethylenethiourea (2-imidazolinethione), carbimazole, and 1,3-dimethyl-2-thiohydantoin.
[0270] [Content] The total content of the compound having a sulfonamide structure and the compound having a thiourea structure relative to the total mass of the composition for pattern formation is preferably 0.05 to 10 mass%, more preferably 0.1 to 5 mass%, and even more preferably 0.2 to 3 mass%. The composition for pattern formation may contain only one compound selected from the group consisting of compounds having a sulfonamide structure and compounds having a thiourea structure, or may contain two or more compounds. When only one compound is contained, the content of the compound is preferably within the above range, and when two or more compounds are contained, the total amount is preferably within the above range.
[0271] <Migration inhibitor> The pattern-forming composition preferably further contains a migration inhibitor, which makes it possible to effectively inhibit migration of metal ions originating from the metal layer (metal wiring) into the photosensitive film.
[0272] The migration inhibitor is not particularly limited, but includes compounds having a heterocycle (pyrrole ring, furan ring, thiophene ring, imidazole ring, triazole ring, oxazole ring, thiazole ring, pyrazole ring, isoxazole ring, isothiazole ring, tetrazole ring, pyridine ring, pyridazine ring, pyrimidine ring, pyrazine ring, piperidine ring, piperazine ring, morpholine ring, 2H-pyran ring and 6H-pyran ring, triazine ring), compounds having thioureas and sulfanyl groups, hindered phenol compounds, salicylic acid derivative compounds, and hydrazide derivative compounds. In particular, triazole compounds such as 1,2,4-triazole and benzotriazole, and tetrazole compounds such as 1H-tetrazole and 5-phenyltetrazole can be preferably used.
[0273] Alternatively, an ion trapping agent that traps anions such as halogen ions can be used.
[0274] Other examples of the migration inhibitor include the rust inhibitor described in paragraph 0094 of JP-A-2013-015701, the compounds described in paragraphs 0073 to 0076 of JP-A-2009-283711, the compounds described in paragraph 0052 of JP-A-2011-059656, the compounds described in paragraphs 0114, 0116 and 0118 of JP-A-2012-194520, and the compounds described in paragraph 0166 of WO 2015 / 199219.
[0275] Specific examples of the migration inhibitor include the following compounds.
[0276] [ka]
[0277] When the pattern-forming composition contains a migration inhibitor, the content of the migration inhibitor is preferably 0.01 to 5.0 mass %, more preferably 0.05 to 2.0 mass %, and even more preferably 0.1 to 1.0 mass %, based on the total solid content of the pattern-forming composition.
[0278] The migration inhibitor may be one type or two or more types. When two or more types of migration inhibitors are used, the total amount is preferably within the above range.
[0279] <Polymerization inhibitor> The pattern-forming composition preferably contains a polymerization inhibitor.
[0280] Examples of the polymerization inhibitor include hydroquinone, o-methoxyphenol, methoxyhydroquinone, p-methoxyphenol, di-tert-butyl-p-cresol, pyrogallol, p-tert-butylcatechol (t-butylcatechol), 1,4-benzoquinone, diphenyl-p-benzoquinone, 4,4'-thiobis(3-methyl-6-tert-butylphenol), 2,2'-methylenebis(4-methyl-6-tert-butylphenol), N-nitrophenyl-p-benzoquinone, and the like. Nitroso-N-phenylhydroxyamine aluminum salt, phenothiazine, N-nitrosodiphenylamine, N-phenylnaphthylamine, ethylenediaminetetraacetic acid, 1,2-cyclohexanediaminetetraacetic acid, glycol ether diaminetetraacetic acid, 2,6-di-tert-butyl-4-methylphenol, 5-nitroso-8-hydroxyquinoline, 1-nitroso-2-naphthol, 2-nitroso-1-naphthol, 2-nitroso-5-(N-ethyl-N-sulfopropionate), p-phenylamino)phenol, N-nitrosophenylhydroxyamine cerium salt, N-nitroso-N-(1-naphthyl)hydroxyamine ammonium salt, bis(4-hydroxy-3,5-tert-butyl)phenylmethane, N,N'-diphenyl-p-phenylenediamine, 2,4-di-tert-butylphenol, di-t-butylhydroxytoluene, 1,4-naphthoquinone, 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethyl Benzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 4-hydroxy-2,2,6,6-tetramethylpiperidine 1-oxyl free radical, phenothiazine, 1,1-diphenyl-2-picrylhydrazyl, dibutyldithiocarbamate copper (II), nitrobenzene, N-nitroso-N-phenylhydroxylamine aluminum salt, N-nitroso-N-phenylhydroxylamine ammonium salt, etc. can be suitably used. In addition, the polymerization inhibitor described in paragraph 0060 of JP-A-2015-127817 and the compounds described in paragraphs 0031 to 0046 of WO2015 / 125469 can also be used.
[0281] In addition, the following compounds can be used.
[0282] [ka]
[0283] When the pattern-forming composition contains a polymerization inhibitor, the content of the polymerization inhibitor is, for example, 0.01 to 20.0 mass % relative to the total solid content of the pattern-forming composition, preferably 0.01 to 5 mass %, more preferably 0.02 to 3 mass %, and even more preferably 0.05 to 2.5 mass %.
[0284] The polymerization inhibitor may be one type or two or more types. When two or more types of polymerization inhibitors are used, the total amount thereof is preferably within the above range.
[0285] <Metal adhesion improver> The pattern-forming composition preferably contains a metal adhesion improver for improving adhesion to metal materials used for electrodes, wiring, etc. Examples of metal adhesion improvers include silane coupling agents, aluminum-based adhesion aids, titanium-based adhesion aids, compounds having a sulfonamide structure, compounds having a thiourea structure, phosphoric acid derivative compounds, β-ketoester compounds, amino compounds, and the like.
[0286] Examples of the silane coupling agent include the compounds described in paragraph 0167 of WO 2015 / 199219, the compounds described in paragraphs 0062-0073 of JP 2014-191002 A, the compounds described in paragraphs 0063-0071 of WO 2011 / 080992 A, the compounds described in paragraphs 0060-0061 of JP 2014-191252 A, the compounds described in paragraphs 0045-0052 of JP 2014-041264 A, and the compounds described in paragraph 0055 of WO 2014 / 097594 A. It is also preferable to use two or more different silane coupling agents as described in paragraphs 0050-0058 of JP 2011-128358 A. It is also preferable to use the following compounds as the silane coupling agent. In the following formula, Et represents an ethyl group.
[0287] [ka] Other silane coupling agents include, for example, vinyltrimethoxysilane, vinyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, N-2 -(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, tris-(trimethoxysilylpropyl)isocyanurate, 3-ureidopropyltrialkoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-isocyanatepropyltriethoxysilane, 3-trimethoxysilylpropylsuccinic anhydride. These can be used alone or in combination of two or more.
[0288] [Aluminum-based adhesion promoter] Examples of aluminum-based adhesion promoters include aluminum tris(ethylacetoacetate), aluminum tris(acetylacetonate), and ethylacetoacetate aluminum diisopropylate.
[0289] Furthermore, as the metal adhesion improver, the compounds described in paragraphs 0046 to 0049 of JP-A No. 2014-186186 and the sulfide-based compounds described in paragraphs 0032 to 0043 of JP-A No. 2013-072935 can also be used.
[0290] The content of the metal adhesion improver is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 15 parts by mass, and even more preferably 0.5 to 5 parts by mass, relative to 100 parts by mass of the specific resin. By making it equal to or more than the lower limit, the adhesion between the pattern and the metal layer becomes good, and by making it equal to or less than the upper limit, the heat resistance and mechanical properties of the pattern become good. The metal adhesion improver may be of only one type, or of two or more types. When two or more types are used, the total is preferably within the above range.
[0291] <Metal adhesion improver> The pattern-forming composition preferably contains a metal adhesion improver for improving adhesion to metal materials used for electrodes, wiring, etc. As the metal adhesion improver, the compounds described in paragraphs 0046 to 0049 of JP2014-186186A and the sulfide-based compounds described in paragraphs 0032 to 0043 of JP2013-072935A can also be used.
[0292] The content of the metal adhesion improver is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 15 parts by mass, and even more preferably 0.5 to 5 parts by mass, relative to 100 parts by mass of the heterocycle-containing polymer precursor. By making it equal to or more than the lower limit, the adhesion between the pattern and the metal layer after the heating step is improved, and by making it equal to or less than the upper limit, the heat resistance and mechanical properties of the cured product after the heating step are improved. The metal adhesion improver may be one type or two or more types. When two or more types are used, the total is preferably within the above range.
[0293] <Other additives> The pattern-forming composition may contain various additives, such as sensitizers, chain transfer agents, surfactants, higher fatty acid derivatives, inorganic particles, curing agents, curing catalysts, fillers, antioxidants, ultraviolet absorbers, anti-aggregation agents, etc., as necessary, within the range in which the effects of the present invention can be obtained. When these additives are added, the total amount of the additives is preferably 3% by mass or less of the solid content of the pattern-forming composition.
[0294] [Sensitizer] The pattern forming composition may contain a sensitizer. The sensitizer absorbs specific active radiation and becomes electronically excited. The sensitizer in the electronically excited state comes into contact with a thermal curing accelerator, a thermal radical polymerization initiator, a photoradical polymerization initiator, or the like, and effects such as electron transfer, energy transfer, and heat generation occur. As a result, the thermal curing accelerator, the thermal radical polymerization initiator, and the photoradical polymerization initiator undergo a chemical change and decompose, generating a radical, an acid, or a base. Examples of the sensitizer include Michler's ketone, 4,4'-bis(diethylamino)benzophenone, 2,5-bis(4'-diethylaminobenzal)cyclopentane, 2,6-bis(4'-diethylaminobenzal)cyclohexanone, 2,6-bis(4'-diethylaminobenzal)-4-methylcyclohexanone, 4,4'-bis(dimethylamino)chalcone, 4,4'-bis(diethylamino)chalcone, p-dimethylaminocinnamylideneindanone, p-dimethylaminobenzylamine ... Dilidene indanone, 2-(p-dimethylaminophenylbiphenylene)-benzothiazole, 2-(p-dimethylaminophenylvinylene)benzothiazole, 2-(p-dimethylaminophenylvinylene)isonaphthothiazole, 1,3-bis(4'-dimethylaminobenzal)acetone, 1,3-bis(4'-diethylaminobenzal)acetone, 3,3'-carbonyl-bis(7-diethylaminocoumarin), 3-acetyl-7-dimethylaminocoumarin, 3-ethoxycarbo N-phenyl-7-dimethylaminocoumarin, 3-benzyloxycarbonyl-7-dimethylaminocoumarin, 3-methoxycarbonyl-7-diethylaminocoumarin, 3-ethoxycarbonyl-7-diethylaminocoumarin, N-phenyl-N'-ethylethanolamine, N-phenyldiethanolamine, Np-tolyldiethanolamine, N-phenylethanolamine, 4-morpholinobenzophenone, isoamyl dimethylaminobenzoate, isoamyl diethylaminobenzoate, 2-methylaminobenzoate, Examples of the mercaptobenzoimidazole include mercaptobenzimidazole, 1-phenyl-5-mercaptotetrazole, 2-mercaptobenzothiazole, 2-(p-dimethylaminostyryl)benzoxazole, 2-(p-dimethylaminostyryl)benzthiazole, 2-(p-dimethylaminostyryl)naphtho(1,2-d)thiazole, 2-(p-dimethylaminobenzoyl)styrene, diphenylacetamide, benzanilide, N-methylacetanilide, and 3',4'-dimethylacetanilide. As the sensitizer, a sensitizing dye may be used. For details about the sensitizing dye, reference can be made to paragraphs 0161 to 0163 of JP2016-027357A, the contents of which are incorporated herein by reference.
[0295] When the composition for pattern formation contains a sensitizer, the content of the sensitizer is preferably 0.01 to 20 mass %, more preferably 0.1 to 15 mass %, and further preferably 0.5 to 10 mass %, based on the total solid content of the composition for pattern formation. The sensitizer may be used alone or in combination of two or more kinds.
[0296] [Chain transfer agent] The pattern forming composition may contain a chain transfer agent. The chain transfer agent is defined, for example, in the Third Edition of the Polymer Dictionary (edited by the Society of Polymer Science, 2005), pages 683-684. As the chain transfer agent, for example, a group of compounds having SH, PH, SiH, and GeH in the molecule is used. These can donate hydrogen to a low activity radical to generate a radical, or can generate a radical by being oxidized and then deprotonated. In particular, a thiol compound can be preferably used.
[0297] In addition, as the chain transfer agent, the compounds described in paragraphs 0152 to 0153 of WO 2015 / 199219 can also be used.
[0298] When the composition for pattern formation contains a chain transfer agent, the content of the chain transfer agent is preferably 0.01 to 20 parts by mass, more preferably 1 to 10 parts by mass, and even more preferably 1 to 5 parts by mass, based on 100 parts by mass of the total solid content of the composition for pattern formation. The chain transfer agent may be one type or two or more types. When two or more types of chain transfer agents are used, the total amount is preferably within the above range.
[0299] [Surfactant] A surfactant may be added to the pattern-forming composition from the viewpoint of further improving the coating property. As the surfactant, various types of surfactants such as fluorine-based surfactants, nonionic surfactants, cationic surfactants, anionic surfactants, and silicone-based surfactants can be used. The following surfactants are also preferred. In the following formula, the parentheses indicating the repeating unit of the main chain indicate the content (mol %) of each repeating unit, and the parentheses indicating the repeating unit of the side chain indicate the number of repetitions of each repeating unit. [ka] In addition, the compounds described in paragraphs 0159 to 0165 of WO 2015 / 199219 can also be used as the surfactant. The fluorine-containing surfactant may be a fluorine-containing polymer having an ethylenically unsaturated group in the side chain. Specific examples include the compounds described in paragraphs 0050-0090 and 0289-0295 of JP2010-164965A, such as Megafac RS-101, RS-102, and RS-718K manufactured by DIC Corporation.
[0300] The fluorine content in the fluorosurfactant is preferably 3 to 40 mass%, more preferably 5 to 30 mass%, and particularly preferably 7 to 25 mass%. A fluorosurfactant having a fluorine content within this range is effective in terms of uniformity of the coating film thickness and liquid saving properties, and also has good solubility in the composition.
[0301] Examples of silicone surfactants include Toray Silicone DC3PA, Toray Silicone SH7PA, Toray Silicone DC11PA, Toray Silicone SH21PA, Toray Silicone SH28PA, Toray Silicone SH29PA, Toray Silicone SH30PA, Toray Silicone SH8400 (all manufactured by Toray Dow Corning Co., Ltd.), TSF-4440, TSF-4300, TSF-4445, TSF-4460, TSF-4452 (all manufactured by Momentive Performance Materials, Inc.), KP341, KF6001, KF6002 (all manufactured by Shin-Etsu Silicone Co., Ltd.), BYK307, BYK323, BYK330 (all manufactured by BYK-Chemie Co., Ltd.), and the like.
[0302] Examples of hydrocarbon surfactants include Paionin A-76, Newkalgen FS-3PG, Paionin B-709, Paionin B-811-N, Paionin D-1004, Paionin D-3104, Paionin D-3605, Paionin D-6112, Paionin D-2104-D, Paionin D-212, Paionin D-931, Paionin D-941, Paionin D-951, Paionin E-5310, Paionin P-1050-B, Paionin P-1028-P, Paionin P-4050-T, and the like (all manufactured by Takemoto Oil Co., Ltd.).
[0303] Examples of nonionic surfactants include glycerol, trimethylolpropane, trimethylolethane, and their ethoxylates and propoxylates (e.g., glycerol propoxylate, glycerol ethoxylate, etc.), polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene oleyl ether, polyoxyethylene octylphenyl ether, polyoxyethylene nonylphenyl ether, polyethylene glycol dilaurate, polyethylene glycol distearate, sorbitan fatty acid ether, and the like. Examples of such compounds include Stel, Pluronic (registered trademark) L10, L31, L61, L62, 10R5, 17R2, and 25R2 (manufactured by BASF), Tetronic 304, 701, 704, 901, 904, and 150R1 (manufactured by BASF), Solsperse 20000 (manufactured by Lubrizol Japan Co., Ltd.), NCW-101, NCW-1001, and NCW-1002 (manufactured by Wako Pure Chemical Industries, Ltd.), Paionin D-6112, D-6112-W, and D-6315 (manufactured by Takemoto Oil Co., Ltd.), Olfin E1010, and Surfynol 104, 400, and 440 (manufactured by Nissin Chemical Industry Co., Ltd.).
[0304] Specific examples of cationic surfactants include organosiloxane polymer KP341 (manufactured by Shin-Etsu Chemical Co., Ltd.), (meth)acrylic acid-based (co)polymer Polyflow No. 75, No. 77, No. 90, No. 95 (manufactured by Kyoeisha Chemical Co., Ltd.), and W001 (manufactured by Yusho Co., Ltd.).
[0305] Specific examples of the anionic surfactant include W004, W005, W017 (manufactured by Yusho Co., Ltd.), Sandet BL (manufactured by Sanyo Chemical Industries, Ltd.), and the like.
[0306] When the pattern-forming composition contains a surfactant, the content of the surfactant is preferably 0.001 to 2.0% by mass, more preferably 0.005 to 1.0% by mass, based on the total solid content of the pattern-forming composition. The surfactant may be one type or two or more types. When the surfactant is two or more types, the total is preferably within the above range.
[0307] [Higher fatty acid derivative] In order to prevent polymerization inhibition caused by oxygen, a higher fatty acid derivative such as behenic acid or behenic acid amide may be added to the pattern-forming composition, and the higher fatty acid derivative may be unevenly distributed on the surface of the pattern-forming composition during drying after application.
[0308] In addition, the higher fatty acid derivative may be a compound described in paragraph 0155 of WO 2015 / 199219.
[0309] When the composition for pattern formation contains a higher fatty acid derivative, the content of the higher fatty acid derivative is preferably 0.1 to 10 mass % based on the total solid content of the composition for pattern formation. The higher fatty acid derivative may be one type or two or more types. When the composition for pattern formation contains two or more types of higher fatty acid derivatives, the total is preferably within the above range.
[0310] [Inorganic particles] The resin composition of the present invention may contain inorganic particles, specifically, calcium carbonate, calcium phosphate, silica, kaolin, talc, titanium dioxide, alumina, barium sulfate, calcium fluoride, lithium fluoride, zeolite, molybdenum sulfide, glass, etc.
[0311] The average particle size of the inorganic particles is preferably from 0.01 to 2.0 μm, more preferably from 0.02 to 1.5 μm, further preferably from 0.03 to 1.0 μm, and particularly preferably from 0.04 to 0.5 μm. By incorporating inorganic particles having the above average particle size, it is possible to achieve both good mechanical properties of the cured film and suppression of scattering of exposure light.
[0312] [Ultraviolet absorber] The composition of the present invention may contain an ultraviolet absorbing agent. Examples of the ultraviolet absorbing agent that can be used include salicylate-based, benzophenone-based, benzotriazole-based, substituted acrylonitrile-based, and triazine-based ultraviolet absorbing agents. Examples of salicylate-based ultraviolet absorbers include phenyl salicylate, p-octylphenyl salicylate, and pt-butylphenyl salicylate. Examples of benzophenone-based ultraviolet absorbers include 2,2'-dihydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2,4-dihydroxybenzophenone, and 2-hydroxy-4-octoxybenzophenone. Examples of benzotriazole-based ultraviolet absorbers include 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-tert-amyl-5'-isobutylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-isobutyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-isobutyl-5'-propylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)benzotriazole, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, and 2-[2'-hydroxy-5'-(1,1,3,3-tetramethyl)phenyl]benzotriazole.
[0313] Examples of the substituted acrylonitrile ultraviolet absorber include ethyl 2-cyano-3,3-diphenylacrylate and 2-ethylhexyl 2-cyano-3,3-diphenylacrylate. Further, examples of triazine-based ultraviolet absorbers include mono(hydroxyphenyl)triazine compounds such as 2-[4-[(2-hydroxy-3-dodecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-tridecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, and 2-(2,4-dihydroxyphenyl)-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine; 2,4-bis(2-hydroxy-4-propyloxyphenyl)-6-(2,4-dimethylphenyl)-1,3,5-triazine; bis(hydroxyphenyl)triazine compounds such as 2,4-bis(2-hydroxy-3-methyl-4-propyloxyphenyl)-6-(4-methylphenyl)-1,3,5-triazine and 2,4-bis(2-hydroxy-3-methyl-4-hexyloxyphenyl)-6-(2,4-dimethylphenyl)-1,3,5-triazine; and tris(hydroxyphenyl)triazine compounds such as 2,4-bis(2-hydroxy-4-butoxyphenyl)-6-(2,4-dibutoxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-4-octyloxyphenyl)-1,3,5-triazine and 2,4,6-tris[2-hydroxy-4-(3-butoxy-2-hydroxypropyloxy)phenyl]-1,3,5-triazine.
[0314] In the present invention, the above-mentioned various ultraviolet absorbents may be used alone or in combination of two or more. The composition of the present invention may or may not contain an ultraviolet absorber. When the composition of the present invention contains an ultraviolet absorber, the content of the ultraviolet absorber is preferably from 0.001% by mass to 1% by mass, and more preferably from 0.01% by mass to 0.1% by mass, relative to the total solid mass of the composition of the present invention.
[0315] [Organotitanium Compounds] The resin composition of the present embodiment may contain an organotitanium compound. By containing an organotitanium compound in the resin composition, a resin layer having excellent chemical resistance can be formed even when cured at a low temperature.
[0316] Usable organic titanium compounds include those in which an organic group is bonded to a titanium atom via a covalent bond or an ionic bond. Specific examples of the organotitanium compound are shown below in I) to VII): I) Titanium chelate compounds: Among these, titanium chelate compounds having two or more alkoxy groups are more preferred because they provide good storage stability for the negative photosensitive resin composition and provide a good cured pattern. Specific examples include titanium bis(triethanolamine) diisopropoxide, titanium di(n-butoxide) bis(2,4-pentanedionate), titanium diisopropoxide bis(2,4-pentanedionate), titanium diisopropoxide bis(tetramethylheptanedionate), titanium diisopropoxide bis(ethylacetoacetate), and the like. II) Tetraalkoxytitanium compounds: For example, titanium tetra(n-butoxide), titanium tetraethoxide, titanium tetra(2-ethylhexoxide), titanium tetraisobutoxide, titanium tetraisopropoxide, titanium tetramethoxide, titanium tetramethoxypropoxide, titanium tetramethylphenoxide, titanium tetra(n-nonyloxide), titanium tetra(n-propoxide), titanium tetrastearyloxide, titanium tetrakis[bis{2,2-(allyloxymethyl)butoxide}], and the like. III) Titanocene compounds: For example, pentamethylcyclopentadienyltitanium trimethoxide, bis(η5-2,4-cyclopentadiene-1-yl)bis(2,6-difluorophenyl)titanium, bis(η5-2,4-cyclopentadiene-1-yl)bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium, and the like. IV) Monoalkoxytitanium compounds: For example, titanium tris(dioctylphosphate) isopropoxide, titanium tris(dodecylbenzenesulfonate) isopropoxide, etc. V) Titanium oxide compounds: For example, titanium oxide bis(pentanedionate), titanium oxide bis(tetramethylheptanedionate), phthalocyanine titanium oxide, and the like. VI) Titanium tetraacetylacetonate compounds: For example, titanium tetraacetylacetonate. VII) Titanate coupling agents: For example, isopropyl tridodecylbenzenesulfonyl titanate.
[0317] Among them, the organic titanium compound is preferably at least one compound selected from the group consisting of I) titanium chelate compounds, II) tetraalkoxytitanium compounds, and III) titanocene compounds, from the viewpoint of exhibiting better chemical resistance. In particular, titanium diisopropoxide bis(ethylacetoacetate), titanium tetra(n-butoxide), and bis(η5-2,4-cyclopentadiene-1-yl)bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium are preferred.
[0318] When an organic titanium compound is blended, the blending amount is preferably 0.05 to 10 parts by mass, more preferably 0.1 to 2 parts by mass, based on 100 parts by mass of the cyclized resin precursor. When the blending amount is 0.05 parts by mass or more, the obtained cured pattern exhibits good heat resistance and chemical resistance, while when it is 10 parts by mass or less, the composition has excellent storage stability.
[0319] [Antioxidants] The composition of the present invention may contain an antioxidant. By containing an antioxidant as an additive, it is possible to improve the elongation properties of the film after curing and the adhesion to metal materials. Examples of the antioxidant include phenolic compounds, phosphite compounds, and thioether compounds. As the phenolic compound, any phenolic compound known as a phenolic antioxidant can be used. As a preferred phenolic compound, a hindered phenolic compound can be mentioned. A compound having a substituent at the site (ortho position) adjacent to the phenolic hydroxyl group is preferred. As the aforementioned substituent, a substituted or unsubstituted alkyl group having 1 to 22 carbon atoms is preferred. In addition, as the antioxidant, a compound having a phenolic group and a phosphite group in the same molecule is also preferred. In addition, as the antioxidant, a phosphorus-based antioxidant can also be suitably used. Examples of phosphorus-based antioxidants include tris[2-[[2,4,8,10-tetrakis(1,1-dimethylethyl)dibenzo[d,f][1,3,2]dioxaphosphepin-6-yl]oxy]ethyl]amine, tris[2-[(4,6,9,11-tetra-tert-butyldibenzo[d,f][1,3,2]dioxaphosphepin-2-yl)oxy]ethyl]amine, and ethyl bis(2,4-di-tert-butyl-6-methylphenyl)phosphite. Examples of commercially available antioxidants include ADK STAB AO-20, ADK STAB AO-30, ADK STAB AO-40, ADK STAB AO-50, ADK STAB AO-50F, ADK STAB AO-60, ADK STAB AO-60G, ADK STAB AO-80, and ADK STAB AO-330 (all manufactured by ADEKA CORPORATION). In addition, the compounds described in paragraphs 0023 to 0048 of Japanese Patent No. 6268967 can also be used as the antioxidant. In addition, the composition of the present invention may contain a latent antioxidant as necessary. Examples of latent antioxidants include compounds in which the site functioning as an antioxidant is protected with a protecting group, and which function as an antioxidant when heated at 100 to 250° C. or heated at 80 to 200° C. in the presence of an acid / base catalyst, causing the protecting group to be eliminated.Examples of latent antioxidants include compounds described in International Publication No. 2014 / 021023, International Publication No. 2017 / 030005, and JP-A-2017-008219. Examples of commercially available latent antioxidants include Adeka Arcles GPA-5001 (manufactured by ADEKA Corporation). Examples of preferred antioxidants include 2,2-thiobis(4-methyl-6-t-butylphenol), 2,6-di-t-butylphenol, and a compound represented by the general formula (3).
[0320] [ka]
[0321] In general formula (3), R5 represents a hydrogen atom or an alkyl group having 2 or more carbon atoms, R6 represents an alkylene group having 2 or more carbon atoms, R7 represents a monovalent to tetravalent organic group containing at least one of an alkylene group having 2 or more carbon atoms, an O atom, and an N atom, and k represents an integer of 1 to 4.
[0322] The compound represented by the general formula (3) suppresses the oxidative deterioration of the aliphatic groups and phenolic hydroxyl groups of the resin, and also suppresses the oxidation of metals by its rust-preventing effect on metal materials.
[0323] Since it can act simultaneously on resin and metal materials, k is more preferably an integer of 2 to 4. Examples of R7 include an alkyl group, a cycloalkyl group, an alkoxy group, an alkyl ether group, an alkyl silyl group, an alkoxy silyl group, an aryl group, an aryl ether group, a carboxyl group, a carbonyl group, an allyl group, a vinyl group, a heterocyclic group, -O-, -NH-, -NHNH-, and combinations thereof, and may further have a substituent. Among these, it is preferable to have an alkyl ether or -NH- from the viewpoint of solubility in a developer and metal adhesion, and -NH- is more preferable from the viewpoint of interaction with a resin and metal adhesion due to metal complex formation.
[0324] Examples of the compound represented by the following general formula (3) include, but are not limited to, the following structures.
[0325] [ka]
[0326] [ka]
[0327] [ka]
[0328] [ka]
[0329] The amount of the antioxidant added is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 5 parts by mass, relative to the resin. If the amount added is less than 0.1 part by mass, it is difficult to obtain the effect of improving the elongation characteristics after reliability and the adhesion to metal materials, and if it is more than 10 parts by mass, there is a risk of causing a decrease in the sensitivity of the resin composition due to interaction with the photosensitizer. Only one type of antioxidant may be used, or two or more types may be used. When two or more types are used, it is preferable that the total amount thereof is within the above range.
[0330] <Restrictions on other substances> The water content of the pattern-forming composition is preferably less than 5% by mass, more preferably less than 1% by mass, and even more preferably less than 0.6% by mass, from the viewpoint of the properties of the coated surface. Methods for maintaining the water content include adjusting the humidity under storage conditions and reducing the porosity of the storage container.
[0331] The metal content of the pattern forming composition is preferably less than 5 mass ppm (parts per million), more preferably less than 1 mass ppm, and even more preferably less than 0.5 mass ppm, from the viewpoint of insulation. Examples of metals include sodium, potassium, magnesium, calcium, iron, chromium, and nickel. When a plurality of metals are contained, the total of these metals is preferably within the above range.
[0332] In addition, examples of methods for reducing metal impurities unintentionally contained in the pattern-forming composition include selecting raw materials having a low metal content as raw materials constituting the pattern-forming composition, filtering the raw materials constituting the pattern-forming composition, lining the inside of an apparatus with polytetrafluoroethylene or the like and performing distillation under conditions that suppress contamination as much as possible, and the like.
[0333] Considering the use of the pattern forming composition as a semiconductor material, the content of halogen atoms is preferably less than 500 mass ppm, more preferably less than 300 mass ppm, and even more preferably less than 200 mass ppm from the viewpoint of wiring corrosion. Among them, those existing in the form of halogen ions are preferably less than 5 mass ppm, more preferably less than 1 mass ppm, and even more preferably less than 0.5 mass ppm. Examples of halogen atoms include chlorine atoms and bromine atoms. It is preferable that the total of chlorine atoms and bromine atoms, or chlorine ions and bromine ions, is within the above range. A preferred method for adjusting the content of halogen atoms is ion exchange treatment.
[0334] A container for storing the pattern-forming composition may be a container known in the art. In addition, in order to prevent impurities from being mixed into the raw materials or the pattern-forming composition, it is also preferable to use a multi-layer bottle whose inner wall is made of six types of six-layer resin or a bottle with a seven-layer structure made of six types of resin. Examples of such containers include the container described in JP-A-2015-123351.
[0335] <Uses of the pattern forming composition> The pattern-forming composition is preferably used for forming an interlayer insulating film for a redistribution layer. Furthermore, the present invention can also be used for forming an insulating film for a semiconductor device, a stress buffer film, or the like. EXAMPLES
[0336] The present invention will be described in more detail below with reference to examples. The materials, amounts used, ratios, processing contents, processing procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention is not limited to the specific examples shown below. "Parts" and "%" are by weight unless otherwise specified.
[0337] (Production of resin composition) In each of the Examples and Comparative Examples, a resin composition or a comparative composition was produced according to the following production method. The types and contents of the specific resin, the antioxidant, and other ingredients (other components) contained in the obtained resin composition or the comparative composition, as well as the oxidation-reduction potential of the antioxidant, are shown in the table below. The oxidation-reduction potential of the antioxidant was measured by the following method. Cyclic voltammetry measurements were performed using a WaveNano potentiostat (Pine Research Instrumentation). The following materials were used for the reference electrode, counter electrode, and working electrode. Reference electrode: silver / silver nitrate (silver wire immersed in a freshly prepared solution of 5 mmol / L silver nitrate in anhydrous acetonitrile using 0.1 mol / L tetraalkylammonium tetrafluoroborate in acetonitrile as electrolyte); Counter electrode: platinum wire Working electrode: platinum disk (diameter 1.6 mm) The oxidation potential of each antioxidant was measured using a tetrahydrofuran (THF) solution (5 mmol / L) of each antioxidant, with 1 mol / L tetrabutylammonium perchlorate (TBAP) used as the supporting electrolyte. The reduction scan was measured using a 0.1 mol / L solution of TBAP in acetonitrile versus a THF solution (5 mmol / L) of each antioxidant. Typically, 3 cycles (6 segments) were performed at a sweep rate of 20 mV / s. The energy levels were corrected by an offset of 4.7 V to convert to the vacuum level. Voltammograms were measured for a tetrahydrofuran (THF) solution (5 mmol / L) of each antioxidant using the above method, and the redox potential was calculated as the half-wave potential obtained from the voltammograms. In the table, "-" means that the corresponding component is not contained.
[0338] <Example 1> 21.2 g of 4,4'-oxydiphthalic dianhydride (ODPA), 18.0 g of 2-hydroxyethyl methacrylate (HEMA), 23.9 g of pyridine, 0.10 g of water, and 250 ml of diglyme were mixed and stirred at a temperature of 60°C for 4 hours to produce a diester of ODPA and HEMA. The reaction mixture was then cooled to -10°C, and 17.0 g of SOCl was added while maintaining the temperature at -10±5°C. 2was added over 60 minutes. After dilution with 50 ml of N-methylpyrrolidone, a solution of 12.6 g of 4,4'-diaminodiphenyl ether dissolved in 100 ml of N-methylpyrrolidone was added dropwise to the reaction mixture over 60 minutes at -10±5°C, and the mixture was stirred for 2 hours. Next, the crude polymer was precipitated in 3 liters of water, and the water-polymer mixture was stirred at a speed of 5000 rpm for 15 minutes. The solid crude polymer was filtered off and dissolved in 380 ml of N-methylpyrrolidone, and 0.05 g of hydroquinone was mixed. The resulting solution was added to 3 liters of water to precipitate the polymer, and the water-polymer mixture was stirred at a speed of 5000 rpm for 15 minutes. The polymer was again filtered off and dried under reduced pressure at 45°C for 3 days to obtain a powdered resin composition. This polymer A-1 had a weight average molecular weight of 26,000. The structure of the obtained polymer A-1 is presumed to be a structure represented by the following formula (A-1). [ka]
[0339] <Example 2> 155.1 g of 4,4'-oxydiphthalic dianhydride (ODPA) was placed in a 2-liter separable flask, and 134.0 g of 2-hydroxyethyl methacrylate (HEMA) and 400 ml of γ-butyrolactone were added. 79.1 g of pyridine was added while stirring at room temperature to obtain a reaction mixture. After the end of the heat generation due to the reaction, the mixture was allowed to cool to room temperature and left to stand for another 16 hours. Next, under ice cooling, a solution in which 206.3 g of dicyclohexylcarbodiimide (DCC) was dissolved in 180 ml of γ-butyrolactone was added to the reaction mixture over 40 minutes while stirring. Subsequently, a suspension in which 148.7 g of 2,2'-bis(trifluoromethyl)benzidine was suspended in 350 ml of γ-butyrolactone was added over 60 minutes while stirring. After further stirring at room temperature for 2 hours, 30 ml of ethyl alcohol was added and stirred for 1 hour. Then, 400 ml of γ-butyrolactone was added. The precipitate formed in the reaction mixture was removed by filtration to obtain a reaction solution. The obtained reaction solution was added to 3 liters of ethyl alcohol to produce a crude polymer. The crude polymer was filtered and dissolved in 1.5 liters of tetrahydrofuran, and then 0.3 g of p-methoxyphenol was mixed to obtain a crude polymer solution. The obtained crude polymer solution was dropped into 28 liters of water to precipitate the polymer, and the water-polymer mixture was stirred at a speed of 5000 rpm for 15 minutes. The polymer was again filtered and dried under reduced pressure at 45°C for 3 days to obtain a powdered resin composition. This polymer A-2 had a weight average molecular weight (Mw) of 20,000. The structure of the obtained polymer A-2 is presumed to be a structure represented by the following formula (A-2). [ka]
[0340] <Example 3> 14.9 g of pyromellitic anhydride, 18.0 g of 2-hydroxyethyl methacrylate (HEMA), 23.9 g of pyridine, 0.10 g of water, and 250 ml of diglyme were mixed and stirred at a temperature of 60° C. for 4 hours to produce a diester of pyromellitic anhydride and HEMA. The reaction mixture was then cooled to −10° C., and 17.0 g of SOCl was added while maintaining the temperature at −10±5° C.2 was added over 60 minutes. After dilution with 50 ml of N-methylpyrrolidone, a solution of 20.2 g of 2,2'-bis(trifluoromethyl)benzidine dissolved in 100 ml of N-methylpyrrolidone was added dropwise to the reaction mixture over 60 minutes at -10±5°C, and the mixture was stirred for 2 hours. The crude polymer was then precipitated in 3 liters of water, and the water-polymer mixture was stirred at a speed of 5000 rpm for 15 minutes. The solid crude polymer was filtered off, dissolved in 380 ml of cyclohexanone, and mixed with 0.1 g of 4-methoxyaniline. The resulting solution was added to 3 liters of water to precipitate the polymer, and the water-polymer mixture was stirred at a speed of 5000 rpm for 15 minutes. The polymer was again filtered off and dried under reduced pressure at 45°C for 3 days to obtain a powdered resin composition. This polymer A-3 had a weight average molecular weight of 21,000. The structure of the obtained polymer A-3 is presumed to be a structure represented by the following formula (A-3). [ka]
[0341] <Example 4> 147.1 g of 2,2'-biphthalic anhydride was placed in a 2-liter separable flask, and 134.0 g of 2-hydroxyethyl methacrylate (HEMA) and 400 ml of γ-butyrolactone were added. 79.1 g of pyridine was added while stirring at room temperature to obtain a reaction mixture. After the end of the heat generation due to the reaction, the mixture was allowed to cool to room temperature and left to stand for another 16 hours. Next, under ice cooling, a solution in which 206.3 g of dicyclohexylcarbodiimide (DCC) was dissolved in 180 ml of γ-butyrolactone was added to the reaction mixture over 40 minutes while stirring. Subsequently, a suspension in which 93.0 g of 4,4'-diaminodiphenyl ether was suspended in 350 ml of γ-butyrolactone was added over 60 minutes while stirring. After further stirring at room temperature for 2 hours, 30 ml of ethyl alcohol was added and stirred for 1 hour. Then, 400 ml of γ-butyrolactone was added. The precipitate formed in the reaction mixture was removed by filtration to obtain a reaction solution. The obtained reaction solution was added to 3 liters of ethyl alcohol to produce a crude polymer. The crude polymer was filtered and dissolved in 1.5 liters of tetrahydrofuran, and then 0.3 g of p-methoxyphenol was mixed to obtain a crude polymer solution. The obtained crude polymer solution was dropped into 28 liters of water to precipitate the polymer, and the water-polymer mixture was stirred at a speed of 5000 rpm for 15 minutes. The polymer was again filtered and dried under reduced pressure at 45°C for 3 days to obtain a powdered resin composition. This polymer A-4 had a weight average molecular weight (Mw) of 20,500. The structure of the obtained polymer A-4 is presumed to be a structure represented by the following formula (A-4). [ka]
[0342] <Example 5> 22.0 g of 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 18.0 g of 2-hydroxyethyl methacrylate (HEMA), 23.9 g of pyridine, 0.10 g of water, and 250 ml of diglyme were mixed and stirred at a temperature of 60°C for 4 hours to produce a diester of 3,3',4,4'-benzophenonetetracarboxylic dianhydride and HEMA. The reaction mixture was then cooled to -10°C, and 17.0 g of SOCl was added while maintaining the temperature at -10±5°C. 2 was added over 60 minutes. After dilution with 50 ml of N-methylpyrrolidone, a solution of 12.6 g of 4,4'-diaminodiphenyl ether dissolved in 100 ml of N-methylpyrrolidone was added dropwise to the reaction mixture over 60 minutes at -10±5°C, and the mixture was stirred for 2 hours. Next, the crude polymer was precipitated in 3 liters of water, and the water-polymer mixture was stirred at a speed of 5000 rpm for 15 minutes. The solid crude polymer was filtered off and dissolved in 380 ml of dimethylacetamide, and 0.05 g of triphenylphosphine was mixed. The resulting solution was added to 3 liters of water to precipitate the polymer, and the water-polymer mixture was stirred at a speed of 5000 rpm for 15 minutes. The polymer was again filtered off and dried under reduced pressure at 45°C for 3 days to obtain a powdered resin composition. This polymer A-5 had a weight average molecular weight of 22,000. The structure of the obtained polymer A-5 is presumed to be a structure represented by the following formula (A-5). [ka]
[0343] <Example 6> 21.2 g of 4,4'-oxydiphthalic dianhydride (ODPA), 18.0 g of 2-hydroxyethyl methacrylate (HEMA), 23.9 g of pyridine, 0.10 g of water, and 250 ml of diglyme were mixed and stirred at a temperature of 60°C for 4 hours to produce a diester of ODPA and HEMA. The reaction mixture was then cooled to -10°C, and 17.0 g of SOCl was added while maintaining the temperature at -10±5°C. 2was added over 60 minutes. After dilution with 50 ml of N-methylpyrrolidone, a solution of 6.8 g of 1,4-phenylenediamine dissolved in 100 ml of N-methylpyrrolidone was dropped into the reaction mixture over 60 minutes at -10±5°C, and the mixture was stirred for 2 hours. Next, the crude polymer was precipitated in 3 liters of water, and the water-polymer mixture was stirred at a speed of 5000 rpm for 15 minutes. The solid crude polymer was filtered off and dissolved in 380 ml of tetrahydrofuran, and 0.3 g of cysteine was mixed. The resulting solution was added to 3 liters of water to precipitate the polymer, and the water-polymer mixture was stirred at a speed of 5000 rpm for 15 minutes. The polymer was again filtered off, and the obtained powder was put into a dry pellet molding machine and molded into pellets by crushing and extrusion to obtain a pellet-shaped resin composition. This polymer A-6 had a weight average molecular weight of 20,000. The structure of the obtained polymer A-6 is presumed to be a structure represented by the following formula (A-6). [ka]
[0344] <Example 7> 30.4 g of 4,4'-(hexafluoroisopropylidene)diphthalic anhydride, 18.0 g of 2-hydroxyethyl methacrylate (HEMA), 23.9 g of pyridine, 0.10 g of water, and 250 ml of diglyme were mixed and stirred at a temperature of 60°C for 4 hours to produce a diester of 4,4'-(hexafluoroisopropylidene)diphthalic anhydride and HEMA. The reaction mixture was then cooled to -10°C, and 17.0 g of SOCl was added while maintaining the temperature at -10±5°C. 2was added over 60 minutes. After dilution with 50 ml of N-methylpyrrolidone, a solution of 12.6 g of 4,4'-diaminodiphenyl ether dissolved in 100 ml of N-methylpyrrolidone was dropped into the reaction mixture over 60 minutes at -10±5°C, and the mixture was stirred for 2 hours. Then, the crude polymer was precipitated in 3 liters of water, and the water-polymer mixture was stirred at a speed of 5000 rpm for 15 minutes. The solid crude polymer was filtered off and dissolved in 380 ml of γ-butyrolactone, and 0.05 g of 4-nitrosoanisole was mixed. The resulting solution was added to 3 liters of water to precipitate the polymer, and the water-polymer mixture was stirred at a speed of 5000 rpm for 15 minutes. The polymer was again filtered off, and the obtained powder was put into a dry pellet molding machine and molded into pellets by crushing and extrusion to obtain a pellet-shaped resin composition. This polymer A-7 had a weight average molecular weight of 20,000. The structure of the obtained polymer A-7 is presumed to be a structure represented by the following formula (A-7). [ka]
[0345] <Example 8> 21.2 g of 4,4'-oxydiphthalic dianhydride (ODPA), 18.0 g of 2-hydroxyethyl methacrylate (HEMA), 23.9 g of pyridine, 0.10 g of water, and 250 ml of diglyme were mixed and stirred at a temperature of 60°C for 4 hours to produce a diester of ODPA and HEMA. The reaction mixture was then cooled to -10°C, and 17.0 g of SOCl was added while maintaining the temperature at -10±5°C. 2was added over 60 minutes. After dilution with 50 ml of N-methylpyrrolidone, a solution of 15.6 g of 4,4'-diaminodiphenylsulfone dissolved in 100 ml of N-methylpyrrolidone was added dropwise to the reaction mixture over 60 minutes at -10±5°C, and the mixture was stirred for 2 hours. The crude polymer was then precipitated in 3 liters of water, and the water-polymer mixture was stirred at a speed of 5000 rpm for 15 minutes. The solid crude polymer was filtered off, dissolved in 380 ml of N-methylpyrrolidone, and mixed with 1.0 g of 3-bromo-β-lapachone. The resulting solution was added to 3 liters of water to precipitate the polymer, and the water-polymer mixture was stirred at a speed of 5000 rpm for 15 minutes. The polymer was again filtered off and dried under reduced pressure at 45°C for 3 days to obtain a powdered resin composition. This polymer A-8 had a weight average molecular weight of 25,000. The structure of the obtained polymer A-8 is presumed to be a structure represented by the following formula (A-8). [ka]
[0346] <Example 9> 21.2 g of 4,4'-oxydiphthalic dianhydride (ODPA), 18.0 g of 2-hydroxyethyl methacrylate (HEMA), 23.9 g of pyridine, 0.10 g of water, and 250 ml of diglyme were mixed and stirred at a temperature of 60°C for 4 hours to produce a diester of ODPA and HEMA. The reaction mixture was then cooled to -10°C, and 17.0 g of SOCl was added while maintaining the temperature at -10±5°C. 2was added over 60 minutes. After dilution with 50 ml of N-methylpyrrolidone, a solution of 21.0 g of 2,2'-bis(4-aminophenyl)hexafluoropropane dissolved in 100 ml of N-methylpyrrolidone was added dropwise to the reaction mixture over 60 minutes at -10±5°C, and the mixture was stirred for 2 hours. Next, the crude polymer was precipitated in 3 liters of water, and the water-polymer mixture was stirred at a speed of 5000 rpm for 15 minutes. The solid crude polymer was filtered off and dissolved in 380 ml of cyclohexanone, and 0.5 g of ascorbic acid was mixed. The resulting solution was added to 3 liters of water to precipitate the polymer, and the water-polymer mixture was stirred at a speed of 5000 rpm for 15 minutes. The polymer was again filtered off, and the obtained powder was put into a dry pellet molding machine and molded into pellets by crushing and extrusion to obtain a pellet-shaped resin composition. This polymer A-9 had a weight average molecular weight of 20,000. The structure of the obtained polymer A-9 is presumed to be a structure represented by the following formula (A-9). [ka]
[0347] <Example 10> 14.9 g of pyromellitic anhydride, 18.0 g of 2-hydroxyethyl methacrylate (HEMA), 23.9 g of pyridine, 0.10 g of water, and 250 ml of diglyme were mixed and stirred at a temperature of 60° C. for 4 hours to produce a diester of pyromellitic anhydride and HEMA. The reaction mixture was then cooled to −10° C., and 17.0 g of SOCl was added while maintaining the temperature at −10±5° C. 2was added over 60 minutes. After dilution with 50 ml of N-methylpyrrolidone, a solution of 12.6 g of 4,4'-diaminodiphenyl ether dissolved in 100 ml of N-methylpyrrolidone was added dropwise to the reaction mixture over 60 minutes at -10±5°C, and the mixture was stirred for 2 hours. The crude polymer was then precipitated in 3 liters of water, and the water-polymer mixture was stirred at a speed of 5000 rpm for 15 minutes. The solid crude polymer was filtered off, dissolved in 380 ml of cyclopentanone, and mixed with 0.03 g of p-methoxybenzaldehyde. The resulting solution was added to 3 liters of water to precipitate the polymer, and the water-polymer mixture was stirred at a speed of 5000 rpm for 15 minutes. The polymer was again filtered off and dried under reduced pressure at 45°C for 3 days to obtain a granular resin composition. This polymer A-10 had a weight average molecular weight of 22,000. The structure of the obtained polymer A-10 is presumed to be a structure represented by the following formula (A-10). [ka]
[0348] <Example 11> The powdered resin compositions synthesized in Examples 2 and 4 were mixed in equal amounts to obtain a powdered resin composition containing two types of resins, an antioxidant, and a solvent.
[0349] <Example 12> A crude polymer was obtained by the same procedure as in Example 8. The crude polymer was dissolved in 380 ml of N-methylpyrrolidone, and 0.5 g of p-methoxyphenol and 0.5 g of ascorbic acid were mixed. The obtained solution was added to 3 liters of water to precipitate the polymer, and the water-polymer mixture was stirred at a speed of 5000 rpm for 15 minutes. The polymer was again filtered and dried under reduced pressure at 45°C for 3 days to obtain a powdered resin composition. This polymer A-8 had a weight average molecular weight of 25,000. The structure of the obtained polymer A-8 is presumed to be the structure represented by the above formula (A-8).
[0350] <Example 13> A crude polymer was obtained by the same procedure as in Example 2. The crude polymer was dissolved in 1.5 liters of tetrahydrofuran, and then mixed with 0.3 g of p-methoxyphenol and 7.5 g of diethanolamine to obtain a crude polymer solution. The obtained crude polymer solution was dropped into 28 liters of water to precipitate the polymer, and the water-polymer mixture was stirred at a speed of 5000 rpm for 15 minutes. The polymer was again filtered and dried under reduced pressure at 45°C for 3 days to obtain a powdered resin composition. This polymer A-2 had a weight average molecular weight (Mw) of 20,000. The structure of the obtained polymer A-2 is presumed to be the structure represented by the above formula (A-2).
[0351] <Example 14> A crude polymer was synthesized in the same manner as in Example 1. The crude polymer was dissolved in 380 ml of tetrahydrofuran and mixed with 0.1 g of 2,6-di-tert-butyl-p-cresol. The resulting solution was added to 3 liters of water to precipitate the polymer, and the water-polymer mixture was stirred at a speed of 5000 rpm for 15 minutes. The polymer was again filtered and dried under reduced pressure at 45°C for 3 days to obtain a powdery resin composition.
[0352] <Example 15> A crude polymer was synthesized in the same manner as in Example 1. The crude polymer was dissolved in 500 ml of N-methylpyrrolidone and mixed with 0.05 g of p-methoxyphenol. The resulting solution was added to 2 liters of water to precipitate the polymer, and the water-polymer mixture was stirred at a speed of 5000 rpm for 15 minutes. The polymer was again filtered and dried under reduced pressure at 45° C. for 3 days to obtain a powdered comparative composition.
[0353] <Comparative Example 1> A crude polymer was synthesized in the same manner as in Example 1. The crude polymer was dissolved in 380 ml of tetrahydrofuran. The resulting solution was added to 3 liters of water to precipitate the polymer, and the water-polymer mixture was stirred at a speed of 5000 rpm for 15 minutes. The polymer was again filtered and dried under reduced pressure at 45° C. for 3 days to obtain a powdered comparative composition.
[0354] <Comparative Example 2> A crude polymer was synthesized in the same manner as in Example 1. The crude polymer was dissolved in 380 ml of tetrahydrofuran and mixed with 5.0 g of hydroquinone. The resulting solution was added to 3 liters of water to precipitate the polymer, and the water-polymer mixture was stirred at a speed of 5000 rpm for 15 minutes. The polymer was again filtered and dried under reduced pressure at 45° C. for 3 days to obtain a powdered comparative composition.
[0355] (Evaluation method) <Preparation of Photosensitive Resin Composition> In each of the Examples and Comparative Examples, the components described below were mixed to prepare a homogeneous solution to prepare a photosensitive resin composition (coating liquid).
[0356] [Composition of photosensitive resin composition] Resin composition prepared in each Example or Comparative Example or Comparative composition: 32 parts by mass Photoradical polymerization initiator: IRGACURE OXE 01 (BASF) 1.2 parts by mass Radical polymerizable compound: 5.6 parts by mass of the following compound (the subscripts in parentheses indicate the number of repetitions): [ka] Polymerization inhibitor: 0.08 parts by mass of p-benzoquinone (Tokyo Chemical Industry Co., Ltd.) Migration inhibitor: 0.12 parts by mass of the following compound [ka] Metal adhesion improver: 0.6 parts by mass of the following compound (Et represents an ethyl group): [ka] Base generator: 0.4 parts by mass of the following compound (Et represents an ethyl group): [ka] Solvent: 45 parts by mass of γ-butyrolactone (manufactured by Sanwa Yuka Kogyo Co., Ltd.) and 15 parts by mass of dimethyl sulfoxide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.)
[0357] <Evaluation of filterability> Each photosensitive resin composition was filtered through a polytetrafluoroethylene filter with a pore width of 0.8 μm at a pressure of 0.3 MPa for 90 minutes. The filtration rate (min / g) was calculated from the composition mass at the end of the filtration and the measurement time, and evaluated according to the following evaluation criteria. The evaluation results are shown in the "Filterability" column in the table. It can be said that the smaller the value, the more favorable the filterability. [Evaluation Criteria] A: 4.0 min / g or more and less than 5.0 min / g. B: 5.0 min / g or more and less than 6.0 min / g. C: 6.0 min / g or more and less than 7.0 min / g. D: 7.0 min / g or more and less than 8.0 min / g. E: 8.0 min / g or more.
[0358] <Evaluation of pattern formability> Each photosensitive resin composition was filtered under pressure at a pressure of 0.3 MPa through a filter with a pore width of 0.8 μm, and then coated on a silicon wafer by spin coating. The silicon wafer coated with the photosensitive resin composition layer was dried on a hot plate at 100° C. for 5 minutes to form a photosensitive resin composition layer with a uniform thickness of 10 μm on the silicon wafer. The photosensitive resin composition layer on the silicon wafer was exposed using a stepper (Nikon NSR 2005 i9C). Exposure was performed with i-line at a wavelength of 365 nm, with 200, 300, 400, 500, 600, 700, and 800 mJ / cm. 2 At each exposure energy, a resin layer was obtained by exposure using a photomask on which a 1:1 line and space pattern was formed in 1 μm increments from 5 μm to 25 μm. The resin layer obtained above was negatively developed with cyclopentanone for 60 seconds and rinsed with propylene glycol monomethyl ether acetate (PGMEA). The minimum line width at which a 1:1 line and space pattern of the patterned resin layer was formed was measured using a scanning electron microscope for each of the seven types of exposure energy. The smallest line width among the seven minimum line widths was used as the index value. Using the above index values, evaluation was performed according to the following evaluation criteria, and the evaluation results are shown in the "Pattern Formability" column in the table. The smaller the line width of the resulting resin layer (pattern), the greater the difference in solubility in the developer between the irradiated and non-irradiated areas, which is favorable. The measurement limit is 5 μm. [Evaluation Criteria] A: The above index value was 5 μm or more and less than 6 μm. B: The above index value was 6 μm or more and less than 7.5 μm. C: The above index value was 7.5 μm or more and less than 10 μm. D: The above index value exceeded 10 μm.
[0359] [Table 1]
[0360] From the above results, it is understood that the resin composition of the present invention is excellent in filterability when redissolved in a solvent, and in pattern formability when a pattern-forming composition is prepared by redissolving the composition. The comparative composition according to Comparative Example 1 does not contain an antioxidant. It is clear that such a composition has poor filterability after being dissolved in a solvent. The comparative composition according to Comparative Example 2 contains an antioxidant in an amount exceeding 10,000 ppm by mass relative to the content of the specific resin. When a pattern-forming composition (photosensitive resin composition) is prepared using such a composition, it is found that the pattern formability is reduced.
[0361] <Example 101> The photosensitive resin composition used in Example 1 was applied in a layer form by spin coating on the surface of the thin copper layer of the resin substrate on which the thin copper layer was formed, and dried at 100°C for 4 minutes to form a curable resin composition layer with a thickness of 20 μm, and then exposed using a stepper (Nikon Corporation, NSR1505 i6). Exposure was performed at a wavelength of 365 nm through a mask (a binary mask with a 1:1 line and space pattern and a line width of 10 μm). After exposure, the substrate was heated at 100°C for 4 minutes. After the above heating, the substrate was developed with cyclohexanone for 2 minutes and rinsed with PGMEA for 30 seconds to obtain a layer pattern. Next, the temperature was increased at a rate of 10° C. / min in a nitrogen atmosphere, and after reaching 230° C., the temperature was maintained at 230° C. for 3 hours to form an interlayer insulating film for a redistribution layer. This interlayer insulating film for a redistribution layer had excellent insulating properties. Furthermore, when semiconductor devices were manufactured using these interlayer insulating films for redistribution layers, it was confirmed that they operated without any problems.
Claims
1. At least one resin selected from the group consisting of a polyimide precursor and a polybenzoxazole precursor, the resin containing a polymerizable group, an antioxidant, and an organic solvent. The content of the antioxidant is 50 ppm by mass to 500 ppm by mass relative to the content of the resin, The oxidation-reduction potential of the antioxidant is 0.65 V or less; The content of the organic solvent is more than 0 and 10 mass% or less with respect to the total mass of the resin composition, In powder, granule or pellet form Resin composition.
2. The resin composition according to claim 1 , wherein a total content of the resin, the antioxidant, and the organic solvent is 90 mass% or more with respect to a total mass of the resin composition.
3. The resin composition according to claim 1 , wherein a total content of the resin, the antioxidant, and the organic solvent is 95 mass% or more with respect to a total mass of the resin composition.
4. The resin composition according to any one of claims 1 to 3, wherein the resin comprises a polyimide precursor.
5. The resin composition according to any one of claims 1 to 4, wherein the resin contains a repeating unit represented by the following formula (2) or (3): Formula (2) [Formula 1] Formula (3) [Case 2] In formula (2), A 1 and A 2 each independently represents an oxygen atom or NH; R 111 represents a divalent organic group; R 115 represents a tetravalent organic group; R 113 and R 114 each independently represents a hydrogen atom or a monovalent organic group, In formula (3), R 121represents a divalent organic group; R 122 represents a tetravalent organic group; R 123 and R 124 each independently represents a hydrogen atom or a monovalent organic group.
6. The resin composition according to any one of claims 1 to 5, wherein the polymerizable group is a radically polymerizable group.
7. The resin composition according to any one of claims 1 to 6, wherein the antioxidant comprises at least one compound selected from the group consisting of phenol-based compounds, alcohol-based compounds, aldehyde-based compounds, amine-based compounds, nitroso-based compounds, phosphorus-based compounds, sulfur-based compounds, and ketone-based compounds.
8. The resin composition according to any one of claims 1 to 7, wherein the antioxidant is a phenol-based compound having an unsaturation degree of 1 or more, or an alcohol-based compound having an unsaturation degree of 1 or more.
9. The resin composition according to any one of claims 1 to 8, wherein the organic solvent comprises at least one selected from the group consisting of hydrocarbon compounds, alcohol compounds, carboxylic acids, ketone compounds, ester compounds, ether compounds, nitrile compounds, amide compounds, amine compounds, sulfone compounds, and sulfoxide compounds.
10. A method for producing the resin composition according to any one of claims 1 to 9, comprising the steps of: A method for producing a resin composition, comprising: adding the antioxidant to a production composition containing the organic solvent and the resin.
11. A synthesis step of reacting raw materials in a solvent to obtain a reaction liquid containing the resin; and a reprecipitation / redissolution step of reprecipitating the resin in the reaction solution and redissolving the reprecipitated resin in the organic solvent to obtain a resin solution, The method for producing a resin composition according to claim 10, wherein the adding step is carried out using the resin solution as the production composition.
12. The method for producing a resin composition according to claim 10 or 11, further comprising a reprecipitation step of reprecipitating the resin after the adding step.
13. The method for producing a resin composition according to claim 12 , further comprising the step of: performing a drying step for removing the organic solvent after the reprecipitation step.
14. The method includes a mixing step of mixing the resin composition according to any one of claims 1 to 9 with a solvent. A method for producing a pattern-forming composition.
15. The method for producing a pattern-forming composition according to claim 14 , wherein a photosensitizer is further mixed in the mixing step.
Citation Information
Patent Citations
Radiation sensitive precursor of high heat- resistant polymer
JP1982025329A
Temperature-sensitive color-changeable resin composition and construction member using the same
JP1995331090A
Photosensitive resin composition, formation of pattern, and electronic part
JP2001075280A
Semiconductor device and its material
JP2003209104A
Light-emitting device
JP2018107360A