Method for producing branched conjugated diene polymer, method for producing rubber composition, method for producing tire, branched conjugated diene polymer, and branched conjugated diene polymer composition

By polymerizing conjugated diene compounds with a styrene derivative and silane sulfide compound, the method addresses the limitations of existing branching methods, resulting in polymers with enhanced performance characteristics for tire applications.

JP7595446B2Active Publication Date: 2024-12-06ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020202847
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-03-18
Filing Date
2020-12-07
Publication Date
2024-12-06
Estimated Expiration
2040-12-07

AI Technical Summary

Technical Problem

Existing methods for introducing branched structures into conjugated diene polymers face limitations in the degree of branching due to the number of reactive groups available, restricting the molecular design and processability of rubber materials used in tire treads.

Method used

A method involving the polymerization of conjugated diene compounds with an alkali metal compound, followed by reacting a styrene derivative as a branching agent and a silane sulfide compound to introduce branch points into the main chain, allowing for higher degrees of branching and adjustable polymer lengths.

Benefits of technology

This approach produces branched conjugated diene polymers with improved fuel efficiency, abrasion resistance, wet skid resistance, and fracture strength, enhancing the performance of tire materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595446000001
    Figure 0007595446000001
  • Figure 0007595446000002
    Figure 0007595446000002
  • Figure 0007595446000003
    Figure 0007595446000003
Patent Text Reader

Abstract

To provide a method for producing a branched conjugated diene-based polymer excellent in low fuel consumption, wear resistance, wet skid resistance and breaking strength.SOLUTION: There is provided a method for producing a branched conjugated diene-based polymer which comprises: a polymerization step of polymerizing or copolymerizing a conjugated diene compound or a conjugated diene compound and an aromatic vinyl compound using an alkali metal compound or an alkaline-earth metal compound as a polymerization initiator to obtain a conjugated diene-based polymer having an active terminal; and a branching step of reacting a styrene derivative as a branching agent to introduce a branched structure into the active terminal of the conjugated diene-based polymer.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a branched conjugated diene polymer, a method for producing a rubber composition, a method for producing a tire, a branched conjugated diene polymer, and a branched conjugated diene polymer composition. [Background technology]

[0002] From the viewpoint of environmental load, there has been an increasing demand for automobiles to have lower fuel consumption. In particular, there is a demand for improved fuel consumption in the materials used for the tread portion of automobile tires, which is in direct contact with the ground. In recent years, there has been a demand for the development of materials having low rolling resistance, i.e., low hysteresis loss. At the same time, there is a trend to reduce the weight of tires, which requires a reduction in the thickness of the tire tread, and at the same time, materials with high abrasion resistance are required for the tire tread. On the other hand, from the viewpoint of safety, materials used in the tire tread portion are required to have excellent wet skid resistance and sufficient fracture properties for practical use.

[0003] Materials that meet the various requirements as described above include rubber materials that contain a rubber-like polymer and a reinforcing filler such as carbon black or silica. The use of rubber materials containing silica can improve the balance between low hysteresis loss (an index of fuel economy) and wet skid resistance. Also, by introducing a functional group having affinity or reactivity with silica to the molecular end of a rubber-like polymer with high mobility, the dispersibility of silica in the rubber material can be improved, and further, the mobility of the molecular end of the rubber-like polymer can be reduced by bonding with silica particles, thereby reducing hysteresis loss. On the other hand, one method for improving the abrasion resistance is to increase the molecular weight of the rubber-like polymer, but increasing the molecular weight of the rubber-like polymer tends to deteriorate the processability when the rubber-like polymer is kneaded with a reinforcing filler. In view of these circumstances, attempts have been made to introduce a branched structure into rubber-like polymers in order to increase the molecular weight without impairing processability.

[0004] For example, a resin composition has been proposed in the past that contains silica and a modified conjugated diene polymer obtained by reacting an alkoxysilane containing an amino group with an active terminal of a conjugated diene polymer. In addition, modified conjugated diene polymers have been proposed that have a branched structure obtained by subjecting an active terminal of a polymer to a coupling reaction with a polyfunctional silane compound (see, for example, Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2007 / 114203 Brochure [Patent Document 2] International Publication No. 2016 / 133154 Brochure Summary of the Invention [Problem to be solved by the invention]

[0006] However, in the method of introducing a branched structure into a conjugated diene polymer by coupling reaction of an active end of a polymer with a polyfunctional silane compound, the degree of branching of the modified conjugated diene polymer obtained by the method is largely dependent on the number of groups capable of reacting with the active end of the polymer possessed by the polyfunctional silane compound, and does not exceed the number of reactive groups. From the viewpoint of synthesis feasibility, there is a limit to the number of reactive groups that can be imparted to one polyfunctional silane, and therefore there is a problem in that the degree of branching of the modified conjugated diene polymer obtained is also limited.

[0007] Therefore, the present invention provides a method for producing a branched conjugated diene polymer that can produce a conjugated diene polymer with a higher degree of branching by introducing a branch point into the main chain compared to a case in which a branched structure is introduced into a conjugated diene polymer using only a modifier or a coupling agent, and that allows the lengths of the main chain and side chains to be adjusted, thereby providing a method for producing a branched conjugated diene polymer with a high degree of freedom in polymer design, and thereby aims to provide a method for producing a branched conjugated diene polymer that is excellent in fuel economy, abrasion resistance, wet skid resistance, and breaking strength. [Means for solving the problem]

[0008] Means for Solving the Problems of the Prior Art As a result of intensive research and investigation, the present inventors have found a method for producing a branched conjugated diene polymer, which can introduce a branch point into the main chain by reacting a conjugated diene polymer having an active terminal with a specific styrene derivative as a branching agent, and have thus completed the present invention. That is, the present invention is as follows.

[0009] [1] a polymerization step of polymerizing or copolymerizing a conjugated diene compound, or a conjugated diene compound and an aromatic vinyl compound, using an alkali metal compound or an alkaline earth metal compound as a polymerization initiator to obtain a conjugated diene polymer having an active terminal; a branching step of reacting an active terminal of the conjugated diene polymer with a styrene derivative as a branching agent to introduce a branched structure; The present invention relates to a method for producing a branched conjugated diene polymer comprising the steps of: [2] The method for producing a branched conjugated diene polymer according to [1] above, further comprising a step of adding a conjugated diene compound and / or an aromatic vinyl compound to the reaction system during and / or after the branching step. [3] The method for producing a branched conjugated diene polymer according to [1] or [2] above, further comprising a reaction step of reacting an active terminal of the conjugated diene polymer obtained in the branching step with a coupling agent or a polymerization terminator. [4] In the reaction step, The method for producing a branched conjugated diene polymer according to the above item [3], wherein the coupling agent is a silane sulfide compound represented by the following formula (3):

[0010] [ka]

[0011] (In formula (3), Si represents a silicon atom, O represents an oxygen atom, and S represents a sulfur atom. x is an integer of 1 to 3, y is 0 or an integer of 1 to 2, and x+y is 3. R 1 , R 2 , R 4 may be the same or different and represent an alkyl group having 1 to 16 carbon atoms; R 3 represents an aryl group having 6 to 16 carbon atoms, an alkylene group having 1 to 16 carbon atoms, or an alkyl chain having 1 to 16 carbon atoms.

[0012] [5] The styrene derivative is The method for producing the branched conjugated diene-based polymer according to any one of [1] to [4] above, which is a compound represented by the following formula (1) and / or the following formula (2):

[0013] [ka]

[0014] [ka]

[0015] (In formulas (1) and (2), R 1 represents any one selected from the group consisting of a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, and an aryl group having 6 to 20 carbon atoms, which may partially have a branched structure. X 1 , X 2 , X 3is a single bond or an organic group containing any one selected from the group consisting of carbon, hydrogen, nitrogen, sulfur, and oxygen. Y 1 , Y 2 , Y 3 represents any one selected from the group consisting of an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, and a halogen atom. Each may be independent and the same or different.

[0016] [6] A step of obtaining a branched conjugated diene polymer by the production method according to any one of [1] to [5] above; obtaining a rubber component containing 10% by mass or more of the branched conjugated diene polymer; and adding a filler in an amount of 5.0 parts by mass or more and 150 parts by mass or less to 100 parts by mass of the rubber component to obtain a rubber composition. [7] Obtaining a rubber composition by the method for producing a rubber composition according to [6] above; molding the rubber composition to obtain a tire; A tire manufacturing method comprising the steps of: [8] having one or more side chains in the polymer chain, A branched conjugated diene polymer having a branching degree (Bn) of 1 or more as measured by a viscosity detector-equipped GPC-light scattering method, the branched conjugated diene polymer contains sulfur atoms and silicon atoms, and the molar ratio of the silicon atoms to the sulfur atoms is 1.05 or more and less than 10; The Mooney viscosity measured at 100°C is 40 or more and 170 or less. Branched conjugated diene polymers. [9] The branched conjugated diene polymer according to [8] above, which has a branching degree (Bn) of 2 or more and 25 or less, as measured by a GPC-light scattering method with a viscosity detector.

[10] The polymer chain has a portion derived from a vinyl monomer containing an alkoxysilyl group or a halosilyl group, The moiety derived from the vinyl monomer containing an alkoxysilyl group or a halosilyl group has a side chain. The branched conjugated diene polymer according to [8] or [9] above.

[11] The portion derived from the vinyl monomer containing an alkoxysilyl group or a halosilyl group is A monomer unit based on a compound represented by the following formula (4) or (5): The branched conjugated diene polymer according to

[10] above, having a polymer chain branching point due to a monomer unit based on a compound represented by the following formula (4) or (5):

[0017] [ka]

[0018] [ka]

[0019] (In formula (4), R 1 represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, or an aryl group having 6 to 20 carbon atoms, which may partially have a branched structure. R 2 ~R 3 each independently represents an alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 20 carbon atoms, which may partially have a branched structure. R when multiple exist 1 ~R 3 are each independent. X 1 represents an independent halogen atom. m represents an integer of 0 to 2, n represents an integer of 0 to 3, and l represents an integer of 0 to 3. (m+n+l) represents 3.) (In formula (5), R 2 ~R 5 Each of R independently represents an alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 20 carbon atoms, and may partially have a branched structure. 2 ~R5 are each independent. X 2 ~X 3 represents an independent halogen atom. m represents an integer of 0 to 2, n represents an integer of 0 to 3, and l represents an integer of 0 to 3. (m+n+l) represents 3. a represents an integer of 0 to 2, b represents an integer of 0 to 3, and c represents an integer of 0 to 3. (a+b+c) represents 3.)

[0020]

[12] The branched conjugated diene polymer according to any one of [8] to

[11] above, wherein at least one end of the branched conjugated diene polymer is modified with a silane sulfide compound represented by the following formula (3):

[0021] [ka]

[0022] (In formula (3), Si represents a silicon atom, O represents an oxygen atom, and S represents a sulfur atom. x is an integer of 1 to 3, y is 0 or an integer of 1 to 2, and x+y is 3. R 1 , R 2 , R 4 may be the same or different and represent an alkyl group having 1 to 16 carbon atoms; R 3 represents an aryl group having 6 to 16 carbon atoms, an alkylene group having 1 to 16 carbon atoms, or an alkyl chain having 1 to 16 carbon atoms.

[0023]

[13] A branched conjugated diene polymer composition comprising 10% by mass or more and less than 100% by mass of a branched conjugated diene polymer having one or more side chains in the polymer chain and a branching degree (Bn) of 1 or more as measured by a GPC-light scattering method with a viscosity detector, the conjugated diene polymer containing sulfur atoms and silicon atoms, a molar ratio of the silicon atoms to the sulfur atoms being 1.05 or more and less than 10, and a Mooney viscosity measured at 100°C being 40 or more and 170 or less.

[14] The branched conjugated diene polymer comprises The branched conjugated diene polymer composition according to

[13] above, which contains a branched conjugated diene polymer coupled with at least one compound selected from the group consisting of tin halides, tin alkoxides, silicon halides, and alkoxysilanes. Effect of the Invention

[0024] According to the present invention, by introducing a branch point into the main chain, a branched conjugated diene-based polymer having a higher degree of branching than when only a coupling agent is used can be produced, and a method for producing a branched conjugated diene-based polymer with a high degree of freedom in polymer design, which allows the lengths of the main chain and side chains to be adjusted, can be provided. As a result, a method for producing a branched conjugated diene-based polymer having excellent fuel economy, abrasion resistance, wet skid resistance, and breaking strength can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] Hereinafter, an embodiment of the present invention (hereinafter, referred to as "the present embodiment") will be described in detail. It should be noted that the following embodiment is merely an example for explaining the present invention, and the present invention is not limited to the following embodiment. The present invention can be practiced with appropriate modifications within the scope of the gist of the present invention.

[0026] [Method for producing branched conjugated diene polymer] The method for producing a branched conjugated diene polymer according to the present embodiment includes the steps of: The method includes a polymerization step of polymerizing or copolymerizing a conjugated diene compound, or a conjugated diene compound and an aromatic vinyl compound, using an alkali metal compound or an alkaline earth metal compound as a polymerization initiator to obtain a conjugated diene polymer having an active end, and a branching step of reacting a styrene derivative as a branching agent with the active end of the conjugated diene polymer to introduce a branched structure. The conjugated diene polymer constituting the branched conjugated diene polymer may be any of a homopolymer of a single conjugated diene compound, a polymer or copolymer of different types of conjugated diene compounds, and a copolymer of a conjugated diene compound and an aromatic vinyl compound. According to the method for producing a branched conjugated diene polymer of the present embodiment, by introducing a branch point into the main chain, it is possible to produce a conjugated diene polymer having a higher degree of branching than when a branched structure is introduced into a conjugated diene polymer using only a coupling agent, and it is also possible to adjust the length of the main chain and / or side chains.

[0027] (Polymerization process) In the polymerization step in the method for producing a branched conjugated diene polymer of the present embodiment, an alkali metal compound or an alkaline earth metal compound is used as a polymerization initiator to polymerize or copolymerize a conjugated diene compound, or a conjugated diene compound and an aromatic vinyl compound, to obtain a conjugated diene polymer having an active end. In the polymerization step, it is preferable to carry out polymerization by a propagation reaction through a living anionic polymerization reaction, whereby a conjugated diene polymer having an active terminal can be obtained.

[0028] <Polymerization initiator> As the polymerization initiator, an alkali metal compound or an alkaline earth metal compound is used. As the polymerization initiator, an organolithium compound is preferably used, and an organomonolithium compound is more preferably used. The organomonolithium compound is not limited to the following, but examples thereof include organomonolithium compounds of low molecular weight compounds and solubilized oligomeric organomonolithium compounds. In addition, the organomonolithium compound can be any of compounds having a carbon-lithium bond, a nitrogen-lithium bond, and a tin-lithium bond in terms of the bonding mode between the organic group and the lithium.

[0029] The amount of the polymerization initiator used is preferably determined depending on the targeted molecular weight of the conjugated diene polymer. The amount of a monomer such as a conjugated diene compound used relative to the amount of a polymerization initiator used relates to the degree of polymerization of a target conjugated diene polymer, i.e., tends to relate to the number average molecular weight and / or weight average molecular weight. Therefore, in order to increase the molecular weight of the conjugated diene polymer, the amount of the polymerization initiator should be adjusted to decrease, and in order to decrease the molecular weight, the amount of the polymerization initiator should be adjusted to increase.

[0030] From the viewpoint that the organomonolithium compound is used as one method for introducing nitrogen atoms into the conjugated diene polymer, it is preferably an alkyllithium compound having a substituted amino group or a dialkylaminolithium. In this case, a conjugated diene polymer having a nitrogen atom consisting of an amino group at the polymerization initiation terminal is obtained.

[0031] The substituted amino group is an amino group that does not have an active hydrogen or has a structure in which the active hydrogen is protected. Examples of alkyllithium compounds having an amino group that does not have an active hydrogen include, but are not limited to, 3-dimethylaminopropyllithium, 3-diethylaminopropyllithium, 4-(methylpropylamino)butyllithium, and 4-hexamethyleneiminobutyllithium. Examples of alkyllithium compounds having an amino group with an active hydrogen protected structure include, but are not limited to, 3-bistrimethylsilylaminopropyllithium and 4-trimethylsilylmethylaminobutyllithium.

[0032] Examples of dialkylaminolithium include, but are not limited to, lithium dimethylamide, lithium diethylamide, lithium dipropylamide, lithium dibutylamide, lithium di-n-hexylamide, lithium diheptylamide, lithium diisopropylamide, lithium dioctylamide, lithium-di-2-ethylhexylamide, lithium didecylamide, lithium ethylpropylamide, lithium ethylbutylamide, lithium ethylbenzylamide, lithium methylphenethylamide, lithium hexamethyleneimide, lithium pyrrolidide, lithium piperidide, lithium heptamethyleneimide, lithium morpholide, 1-lithioazacyclooctane, 6-lithio-1,3,3-trimethyl-6-azabicyclo[3.2.1]octane, and 1-lithio-1,2,3,6-tetrahydropyridine.

[0033] These organomonolithium compounds having a substituted amino group can also be used as oligomeric organomonolithium compounds solubilized in normal hexane or cyclohexane by reacting them with a small amount of a polymerizable monomer, such as 1,3-butadiene, isoprene, or styrene.

[0034] The organomonolithium compound is preferably an alkyllithium compound from the viewpoints of industrial availability and ease of control of the polymerization reaction, in which case a conjugated diene-based polymer having an alkyl group at the polymerization initiation terminal can be obtained. Examples of the alkyl lithium compound include, but are not limited to, n-butyl lithium, sec-butyl lithium, tert-butyl lithium, n-hexyl lithium, benzyl lithium, phenyl lithium, and stilbene lithium. As the alkyllithium compound, n-butyllithium and sec-butyllithium are preferred from the viewpoints of industrial availability and ease of control of the polymerization reaction.

[0035] These organomonolithium compounds may be used alone or in combination of two or more, and may also be used in combination with other organometallic compounds. Examples of the other organometallic compounds include alkaline earth metal compounds, other alkali metal compounds, and other organometallic compounds. Alkaline earth metal compounds include, but are not limited to, organomagnesium compounds, organocalcium compounds, and organostrontium compounds, as well as alkaline earth metal alkoxides, sulfonates, carbonates, and amides. Organomagnesium compounds include, for example, dibutylmagnesium and ethylbutylmagnesium. Other examples of organometallic compounds include organoaluminum compounds.

[0036] In the polymerization step, the polymerization reaction mode is not limited to the following modes, but examples thereof include batch and continuous polymerization reaction modes. In the continuous system, one or more connected reactors can be used. The continuous reactor is, for example, a tank type or a tube type equipped with an agitator. In the continuous system, preferably, the monomer, the inert solvent, and the polymerization initiator are continuously fed to the reactor, a polymer solution containing a polymer is obtained in the reactor, and the polymer solution is continuously discharged. The batch reactor may be, for example, a tank-type reactor equipped with a stirrer. In the batch reactor, preferably, a monomer, an inert solvent, and a polymerization initiator are fed, and if necessary, a monomer is added continuously or intermittently during polymerization to obtain a polymer solution in the reactor, and the polymer solution is discharged after the polymerization is completed. In the method for producing a branched conjugated diene polymer of this embodiment, in order to obtain a conjugated diene polymer having a high proportion of active ends in the polymerization step, a continuous system is preferred, which allows the polymer to be continuously discharged and subjected to the next reaction in a short time. In the continuous system, the number of reactors is not particularly limited, and one or two or more connected reactors can be used. The reactor is preferably one that can sufficiently contact the monomer and the polymerization initiator in a solution, and a tank type or a tube type with a stirrer is used. The number of reactors can be appropriately selected, but one is preferred from the viewpoint of space saving of the production equipment, and two or more are preferred from the viewpoint of improving productivity. When two or more reactors are used, it is more preferable to add the branching agent described later to the second or subsequent reactors.

[0037] In the polymerization step of the conjugated diene polymer, the polymerization is preferably carried out in an inert solvent. Examples of the inert solvent include hydrocarbon solvents such as saturated hydrocarbons and aromatic hydrocarbons. Examples of the hydrocarbon solvent include, but are not limited to, aliphatic hydrocarbons such as butane, pentane, hexane, and heptane; alicyclic hydrocarbons such as cyclopentane, cyclohexane, methylcyclopentane, and methylcyclohexane; aromatic hydrocarbons such as benzene, toluene, and xylene, and hydrocarbons consisting of mixtures thereof. By treating the impurities, that is, allenes and acetylenes, with an organometallic compound before subjecting the polymer to the polymerization reaction, a conjugated diene-based polymer having a high concentration of active ends tends to be obtained, which is preferable since a modified conjugated diene-based polymer having a high modification rate tends to be obtained.

[0038] In the polymerization step, a polar compound (polar substance) may be added. This allows the aromatic vinyl compound to be randomly copolymerized with the conjugated diene compound. In addition, polar compounds tend to be usable as vinylating agents for controlling the microstructure of the conjugated diene portion. Furthermore, they tend to be effective in promoting the polymerization reaction.

[0039] Examples of polar compounds that can be used include, but are not limited to, ethers such as tetrahydrofuran, diethyl ether, dioxane, ethylene glycol dimethyl ether, ethylene glycol dibutyl ether, diethylene glycol dimethyl ether, diethylene glycol dibutyl ether, dimethoxybenzene, and 2,2-bis(2-oxolanyl)propane; tertiary amine compounds such as tetramethylethylenediamine, dipiperidinoethane, trimethylamine, triethylamine, pyridine, and quinuclidine; alkali metal alkoxide compounds such as potassium tert-amylate, potassium tert-butylate, sodium tert-butylate, and sodium amylate; and phosphine compounds such as triphenylphosphine. These polar compounds may be used alone or in combination of two or more.

[0040] The amount of the polar compound used is not particularly limited and can be selected depending on the purpose, but is preferably 0.01 moles or more and 100 moles or less per mole of the polymerization initiator. Such polar compounds (vinylating agents) can be used in an appropriate amount according to the desired vinyl bond amount as regulators for the microstructure of the conjugated diene portion of the conjugated diene polymer. Many polar compounds simultaneously have an effective randomizing effect in the copolymerization of a conjugated diene compound and an aromatic vinyl compound, and tend to be usable as an adjuster for the distribution of the aromatic vinyl compound and as an adjuster for the amount of styrene blocks. As a method for randomizing the conjugated diene compound and the aromatic vinyl compound, for example, as described in JP-A-59-140211, a copolymerization reaction may be initiated with the total amount of styrene and a portion of 1,3-butadiene, and the remaining 1,3-butadiene may be intermittently added during the copolymerization reaction.

[0041] The polymerization temperature in the polymerization step is preferably a temperature at which living anionic polymerization proceeds, and from the viewpoint of productivity, is more preferably 0° C. or higher and 120° C. or lower. By setting the temperature within this range, it is possible to ensure a sufficient amount of the branching agent and coupling agent to react with the active terminals after the polymerization is completed.

[0042] (Branching process) In the method for producing a branched conjugated diene polymer of the present embodiment, a branching step is carried out in which a styrene derivative is reacted as a branching agent with the active terminal of the conjugated diene polymer obtained in the polymerization step. While the branching agent maintains its polymerization activity and polymerizes with the monomer, the functional group of the branching agent reacts with the active end of another polymer chain, forming a branched structure in the polymer. It is also possible to form a further branched structure by polymerizing and reacting the branched conjugated diene polymer into which the branched structure has been introduced with a monomer and a branching agent, or to react the branched conjugated diene polymer with a functional group to form a modified conjugated diene polymer, or to further extend the polymer chain by a coupling reaction. In this way, a branched conjugated diene polymer can be obtained by continuing the polymerization reaction as an aromatic vinyl compound and using a styrene derivative whose functional group reacts with the active end of the polymer as a branching agent.

[0043] <Branching agent> From the viewpoints of polymerization continuity and gelation prevention, the styrene derivative used as a branching agent in the branching step must have a main skeleton that leaves only one active end at the branch site after the branching reaction, and further, the styrene derivative portion formed after the branching reaction must have sufficient reactivity to react with other polymer active ends. More specifically, the styrene derivative as the branching agent is preferably a compound having a vinyl group on the benzene ring and a functional group that quantitatively reacts with the polymer active end of living anionic polymerization. The functional group of the styrene derivative reacts one-to-one with the polymer active end, and the functional group is eliminated to form a single bond, while the vinyl group is polymerized with other monomers in the reactor, forming a branched structure in the polymer. The functional group other than the vinyl group of the styrene derivative is a group that is eliminated by nucleophilic substitution reaction with the polymer active end of living anionic polymerization, and examples of such functional groups include alkoxy groups, halogens, ester groups, formyl groups, ketone groups, amide groups, acid chloride groups, acid anhydride groups, and epoxy groups. By having the above-mentioned structure, the styrene derivative is incorporated into the main chain while maintaining its polymerization activity as styrene, and another monomer is polymerized to the terminal that maintains its activity, thereby further extending the polymer chain. In addition, the functional group of the incorporated styrene derivative reacts with the active terminal of another polymer chain to form a bond, resulting in a branched structure. By repeating this reaction, the number of branches in the polymer chain increases, the polymer structure becomes more complex, and the molecular weight becomes larger. From the viewpoint of the continuity of polymerization and the controllability of the polymer structure, it is also necessary that the functional group which is eliminated after the styrene derivative portion reacts with the active end of another polymer chain has little inhibitory effect on the polymerization. Here, "low polymerization inhibition effect" means that, for example, side reactions of anionic polymerization such as chain transfer reaction, deactivation during polymerization, and decrease in activity due to an increase in the degree of polymer association are low. The functional group of the styrene derivative as the branching agent must not excessively improve the polymerization activity, and must not deactivate the polymerization activity. When polymerizing a polymer by living anionic polymerization, it is important that the functional group does not have a hydrogen atom as a functional group that does not deactivate the active terminal, and is a hard base as defined based on Pearson's HASB rule, and more specifically, an alkoxy group or a halogen group can be mentioned. From these, the structure of the styrene derivative as the branching agent used in the production method of this embodiment can be selected from the viewpoints of reactivity with the active terminal and that the eliminated functional group does not inhibit polymerization. More specifically, it is preferable to use a branching agent represented by the following formula (1) having a styrene skeleton as the main skeleton, or a branching agent represented by the following formula (2) having a diphenylethylene skeleton as the main skeleton, from the viewpoints of suppressing chain transfer reactions, suppressing deactivation of active terminals, and preventing gelation.

[0044] [ka]

[0045] [ka]

[0046] (In formulas (1) and (2), R 1 represents any one selected from the group consisting of a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, and an aryl group having 6 to 20 carbon atoms, which may partially have a branched structure. X 1 , X 2 , X 3 is a single bond or an organic group containing any one selected from the group consisting of carbon, hydrogen, nitrogen, sulfur, and oxygen. Y 1 , Y 2 , Y 3 represents any one selected from the group consisting of an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, and a halogen atom. Each may be independent and the same or different.

[0047] The styrene derivative used as a branching agent in the branching step is represented by the formula (1) R 1 is a hydrogen atom, and Y 1 is preferably any one selected from the group consisting of an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, and a halogen atom.

[0048] In the present embodiment, the styrene derivative used as the branching agent in the branching step is, from the viewpoint of improving the degree of branching, 2 is preferably any one selected from the group consisting of an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, and a halogen atom.

[0049] In the present embodiment, the branching agent used in the branching step is a styrene derivative represented by the formula (1), R 1 is a hydrogen atom, and Y 1 is more preferably an alkoxy group having 1 to 20 carbon atoms or a halogen atom.

[0050] In the present embodiment, the branching agent used in the branching step is a styrene derivative represented by the formula (2), Y 2 is an alkoxy group or a halogen atom, Y 3 is more preferably an alkoxy group having 1 to 20 carbon atoms or a halogen atom.

[0051] In the present embodiment, the branching agent used in the branching step is a styrene derivative represented by the formula (1) R 1 is a hydrogen atom, and Y 1 is more preferably an alkoxy group having 1 to 20 carbon atoms.

[0052] In the present embodiment, the branching agent used in the branching step is a styrene derivative represented by the formula (1) R 1 is a hydrogen atom, and X 1 is a single bond, and Y 1 is even more preferably an alkoxy group having 1 to 20 carbon atoms.

[0053] In the present embodiment, the branching agent used in the branching step is a styrene derivative represented by the formula (2) X 2 is a single bond, and Y 2 is an alkoxy group having 1 to 20 carbon atoms or a halogen atom, and X 3 is a single bond, and Y 3 is even more preferably an alkoxy group having 1 to 20 carbon atoms or a halogen atom.

[0054] Examples of the branching agent represented by the formula (1) include, but are not limited to, trimethoxy(4-vinylphenyl)silane, triethoxy(4-vinylphenyl)silane, tripropoxy(4-vinylphenyl)silane, tributoxy(4-vinylphenyl)silane, triisopropoxy(4-vinylphenyl)silane, trimethoxy(3-vinylphenyl)silane, triethoxy(3-vinylphenyl)silane, tripropoxy(3-vinylphenyl)silane, tributoxy(3-vinylphenyl)silane, triisopropoxy(3-vinylphenyl)silane, (2-vinylphenyl)silane, trimethoxy(2-vinylphenyl)silane, triethoxy(2-vinylphenyl)silane, tripropoxy(2-vinylphenyl)silane, tributoxy(2-vinylphenyl)silane, triisopropoxy(2-vinylphenyl)silane, dimethoxymethyl(4-vinylphenyl)silane, diethoxymethyl(4-vinylphenyl)silane, dipropoxymethyl(4-vinylphenyl)silane, dibutoxymethyl(4-vinylphenyl)silane, diisopropoxymethyl(4-vinylphenyl)silane, dimethoxymethyl methyl(3-vinylphenyl)silane, diethoxymethyl(3-vinylphenyl)silane, dipropoxymethyl(3-vinylphenyl)silane, dibutoxymethyl(3-vinylphenyl)silane, diisopropoxymethyl(3-vinylphenyl)silane, dimethoxymethyl(2-vinylphenyl)silane, diethoxymethyl(2-vinylphenyl)silane, dipropoxymethyl(2-vinylphenyl)silane, dibutoxymethyl(2-vinylphenyl)silane, diisopropoxymethyl(2-vinylphenyl)silane, dimethylmethoxy(4-vinylphenyl)silane, phenyl)silane, dimethylethoxy(4-vinylphenyl)silane, dimethylpropoxy(4-vinylphenyl)silane, dimethylbutoxy(4-vinylphenyl)silane, dimethylisopropoxy(4-vinylphenyl)silane, dimethylmethoxy(3-vinylphenyl)silane, dimethylethoxy(3-vinylphenyl)silane, dimethylpropoxy(3-vinylphenyl)silane, dimethylbutoxy(3-vinylphenyl)silane, dimethylisopropoxy(3-vinylphenyl)silane, dimethylmethoxy(2-vinylphenyl)silane,Dimethylethoxy(2-vinylphenyl)silane, dimethylpropoxy(2-vinylphenyl)silane, dimethylbutoxy(2-vinylphenyl)silane, dimethylisopropoxy(2-vinylphenyl)silane, trimethoxy(4-isopropenylphenyl)silane, triethoxy(4-isopropenylphenyl)silane, tripropoxy(4-isopropenylphenyl)silane, tributoxy(4-isopropenylphenyl)silane, triisopropoxy(4-isopropenylphenyl)silane, trimethoxy(3-isopropenylphenyl)silane )silane, triethoxy(3-isopropenylphenyl)silane, tripropoxy(3-isopropenylphenyl)silane, tributoxy(3-isopropenylphenyl)silane, triisopropoxy(3-isopropenylphenyl)silane, trimethoxy(2-isopropenylphenyl)silane, triethoxy(2-isopropenylphenyl)silane, tripropoxy(2-isopropenylphenyl)silane, tributoxy(2-isopropenylphenyl)silane, triisopropoxy(2-isopropenylphenyl)silane, dimethoxymethyl (4-isopropenylphenyl)silane, diethoxymethyl(4-isopropenylphenyl)silane, dipropoxymethyl(4-isopropenylphenyl)silane, dibutoxymethyl(4-isopropenylphenyl)silane, diisopropoxymethyl(4-isopropenylphenyl)silane, dimethoxymethyl(3-isopropenylphenyl)silane, diethoxymethyl(3-isopropenylphenyl)silane, dipropoxymethyl(3-isopropenylphenyl)silane, dibutoxymethyl(3-isopropenylphenyl)silane, diisoprop methoxymethyl(3-isopropenylphenyl)silane, dimethoxymethyl(2-isopropenylphenyl)silane, diethoxymethyl(2-isopropenylphenyl)silane, dipropoxymethyl(2-isopropenylphenyl)silane, dibutoxymethyl(2-isopropenylphenyl)silane, diisopropoxymethyl(2-isopropenylphenyl)silane, dimethylmethoxy(4-isopropenylphenyl)silane, dimethylethoxy(4-isopropenylphenyl)silane, dimethylpropoxy(4-isopropenylphenyl)silane,Dimethylbutoxy(4-isopropenylphenyl)silane, Dimethylisopropoxy(4-isopropenylphenyl)silane, Dimethylmethoxy(3-isopropenylphenyl)silane, Dimethylethoxy(3-isopropenylphenyl)silane, Dimethylpropoxy(3-isopropenylphenyl)silane, Dimethylbutoxy(3-isopropenylphenyl)silane, Dimethylisopropoxy(3-isopropenylphenyl)silane, Dimethylmethoxy(2-isopropenylphenyl)silane, Dimethylethoxy(2-isopropenylphenyl)silane, Dimethylpropoxy(2-isopropenylphenyl)silane, Dimethylbutoxy(2-isopropenylphenyl)silane, Dimethylisopropoxy(2-isopropenylphenyl)silane, Trichloro(4-vinylphenyl)silane, Trichloro(3-vinylphenyl)silane, Trichloro(2-vinylphenyl)silane, Examples of the silane include tribromo(4-vinylphenyl)silane, tribromo(3-vinylphenyl)silane, tribromo(2-vinylphenyl)silane, dichloromethyl(4-vinylphenyl)silane, dichloromethyl(3-vinylphenyl)silane, dichloromethyl(2-vinylphenyl)silane, dibromomethyl(4-vinylphenyl)silane, dibromomethyl(3-vinylphenyl)silane, dibromomethyl(2-vinylphenyl)silane, dimethylchloro(4-vinylphenyl)silane, dimethylchloro(3-vinylphenyl)silane, dimethylchloro(2-vinylphenyl)silane, dimethylbromo(4-vinylphenyl)silane, dimethylbromo(3-vinylphenyl)silane, dimethylbromo(2-vinylphenyl)silane, trimethoxy(4-vinylbenzyl)silane, triethoxy(4-vinylbenzyl)silane, and tripropoxy(4-vinylbenzyl)silane. Among these, trimethoxy(4-vinylphenyl)silane, triethoxy(4-vinylphenyl)silane, tripropoxy(4-vinylphenyl)silane, tributoxy(4-vinylphenyl)silane, triisopropoxy(4-vinylphenyl)silane, trimethoxy(3-vinylphenyl)silane, triethoxy(3-vinylphenyl)silane, tripropoxy(3-vinylphenyl)silane, tributoxy(3-vinylphenyl)silane, triisopropoxy(3 ... tributoxy(3-vinylphenyl)silane, triisopropoxy(3-vinylphenyl)silane, trimethoxy(3-vinylphenyl)silane, triethoxy(3-vinylphenyl)silane, tripropoxy(3-vinylphenyl)silane, tributoxy(3-vinylphenyl)silane, triisopropoxy(3-vinylphenyl)silane, trimethoxy(3-vinylphenyl)silane, triethoxy(3-vinylphenyl)silane, tripropoxy(3-vinylphenyl)silane, tripeptoxy(3-vinylphenyl)silane, triisopropoxy(3-vinylphenyl)silane, trimethoxy(3-vinylphenyl)silane, triethoxy(3-vinylphenyl)silane, tripeptoxy(3-vinylphenyl)silane, tripeptoxy(3-vinylphenyl)sil Preferred is trimethoxy(4-vinylphenyl)silane, triethoxy(4-vinylphenyl)silane, tripropoxy(4-vinylphenyl)silane, tributoxy(4-vinylphenyl)silane, triisopropoxy(4-vinylphenyl)silane, trimethoxy(4-vinylbenzyl)silane, and triethoxy(4-vinylbenzyl)silane, and further preferred are trimethoxy(4-vinylphenyl)silane and triethoxy(4-vinylphenyl)silane.

[0055] The branching agent represented by the formula (2) is not limited to the following, but may be, for example, 1-bis(4-trimethoxysilylphenyl)ethylene, 1,1-bis(4-triethoxysilylphenyl)ethylene, 1,1-bis(4-tripropoxysilylphenyl)ethylene, 1,1-bis(4-tripentoxysilylphenyl)ethylene, 1,1-bis(4-triisopropoxysilylphenyl)ethylene, 1,1-bis(3-trimethoxysilylphenyl)ethylene, 1,1-bis(3-triethoxysilylphenyl)ethylene, 1,1-bis(3-tripentoxysilylphenyl)ethylene, 1,1-bis(3-triisopropoxysilylphenyl)ethylene, 1,1-bis(2-trimethoxysilylphenyl)ethylene, 1,1-bis(2-triethoxysilylphenyl)ethylene, 1,1-bis(3-tripentoxysilylphenyl)ethylene, Examples of the ethylene include 1,1-bis(2-tripentoxysilylphenyl)ethylene, 1,1-bis(2-triisopropoxysilylphenyl)ethylene, 1,1-bis(4-(dimethylmethoxysilyl)phenyl)ethylene, 1,1-bis(4-(diethylmethoxysilyl)phenyl)ethylene, 1,1-bis(4-(dipropylmethoxysilyl)phenyl)ethylene, 1,1-bis(4-(dimethylethoxysilyl)phenyl)ethylene, 1,1-bis(4-(diethylethoxysilyl)phenyl)ethylene, 1,1-bis(4-(dipropylethoxysilyl)phenyl)ethylene, 1,1-bis(4-trimethoxysilylbenzyl)ethylene, 1,1-bis(4-triethoxysilylbenzyl)ethylene, 1,1-bis(4-trippropoxysilylbenzyl)ethylene, and 1,1-bis(4-tripentoxysilylbenzyl)ethylene. Among these, 1,1-bis(4-trimethoxysilylphenyl)ethylene, 1,1-bis(4-triethoxysilylphenyl)ethylene, 1,1-bis(4-tripropoxysilylphenyl)ethylene, 1,1-bis(4-tripentoxysilylphenyl)ethylene, and 1,1-bis(4-triisopropoxysilylphenyl)ethylene are preferred, with 1,1-bis(4-trimethoxysilylphenyl)ethylene being more preferred. By using the branching agents represented by the above formulas (1) and (2), the number of branches is increased, and the effects of improving the wear resistance and processability can be obtained.

[0056] The timing of adding the branching agent is not particularly limited and can be selected depending on the purpose, etc., but from the viewpoint of improving the absolute molecular weight of the branched conjugated diene-based polymer and improving the coupling rate, the timing is preferably when the raw material conversion rate after addition of the polymerization initiator is 20% or more, more preferably 40% or more, even more preferably 50% or more, even more preferably 65% ​​or more, and even more preferably 75% or more. During and / or after the branching step, a monomer as a desired raw material may be further added to the reaction system, and the polymerization step may be continued after the branching step, or the above-described contents may be repeated. Incidentally, "after the branching step" refers to after the branching agent is added. The monomer to be added is not particularly limited, but is preferably a conjugated diene compound and / or an aromatic vinyl compound. In particular, when a monomer is added during the branching step, from the viewpoint of improving the modification rate by alleviating steric hindrance at the branching point of the conjugated diene polymer, the monomer is preferably 5% or more of the total amount of conjugated diene monomers used in the polymerization step, for example, the total amount of butadiene, more preferably 10% or more, even more preferably 15% or more, even more preferably 20% or more, and even more preferably 25% or more. In this case, it is particularly preferable to add a monomer using a continuous polymerization process at the branching step, in an amount of 5% or more of the total amount of conjugated diene monomers used in the polymerization step, for example, the total amount of butadiene, from the viewpoint of improving the modification rate. The length of the main chain and side chains can be adjusted by changing the timing of adding the branching agent and the amount of monomer added, allowing for a high degree of freedom in polymer design.

[0057] The branched structure of the branched conjugated diene polymer obtained in the branching step in the method for producing a branched conjugated diene polymer of the present embodiment preferably has 3 or more and 24 or less branches, more preferably has 4 or more and 20 or less branches, and further preferably has 5 or more and 18 or less branches. By restricting the number of branches to 24 or less, it tends to be easier to react with a modifier having a functional group to form a modified conjugated diene polymer or to further extend the polymer chain by a coupling reaction, and by restricting the number of branches to 3 or more, the obtained branched conjugated diene polymer tends to have excellent processability and abrasion resistance.

[0058] The amount of branching agent added is not particularly limited, and can be selected depending on the purpose, etc.; however, from the viewpoints of improving the terminal termination reaction rate of the conjugated diene polymer, improving the coupling rate, and continuity of polymerization after branching, the molar ratio of the branching agent to the amount of active polymerization initiator is preferably 1 / 2 or less and 1 / 100 or more, more preferably 1 / 3 or less and 1 / 50 or more, even more preferably 1 / 4 or less and 1 / 30 or more, even more preferably 1 / 6 or less and 1 / 25 or more, and even more preferably 1 / 8 or less and 1 / 12 or more.

[0059] As mentioned above, further monomer may be added during and / or after the branching step and the polymerization step may be continued after branching, or further branching agent may be added after the further addition of monomer and the addition of further monomer may be repeated. By adding monomers, the steric hindrance around the branching points is alleviated, and the continuity of the polymerization is improved, and the coupling rate and modification rate are improved, so that the molecular weight of the polymer can be increased while a branched structure can be formed at a desired position. The monomer to be added may be an aromatic vinyl compound such as styrene, a conjugated diene compound such as butadiene, or a mixture thereof, and may be the same as or different from the type and ratio of the monomer to be polymerized initially, but from the viewpoint of continuity of polymerization, a conjugated diene compound is preferred. From the viewpoint of improving the heat resistance of the polymer, it is preferable to add an aromatic vinyl compound.

[0060] The branched conjugated diene polymer obtained in the branching step in the production method of the present embodiment has a Mooney viscosity measured at 110°C of preferably 10 or more and 150 or less, more preferably 15 or more and 140 or less, even more preferably 20 or more and 130 or less, and still more preferably 30 or more and 100 or less. When the Mooney viscosity is within the above range, the branched conjugated diene polymer obtained by the production method of the present embodiment tends to have excellent processability and abrasion resistance.

[0061] The weight average molecular weight of the branched conjugated diene polymer obtained in the branching step in the production method of this embodiment is preferably 10,000 or more and 1,500,000 or less, more preferably 100,000 or more and 1,000,000 or less, and even more preferably 200,000 or more and 900,000 or less. When the weight average molecular weight is within the above range, the branched conjugated diene polymer obtained by the production method of the present embodiment tends to be excellent in processability, abrasion resistance, and a balance of these properties. When producing an unmodified branched conjugated diene polymer, in order to reach a weight average molecular weight range of 100,000 to 1,000,000, it is necessary to control the amount of branching agent added to be within a range of 1 / 3 or less and 1 / 5 or more in molar ratio to the polymerization initiator, thereby preventing the polymerization initiator from being completely consumed before the coupling step while forming branches, and to make the number of functional groups of the coupling agent 2 or more. In order to reach a weight average molecular weight range of 200,000 to 900,000, it is necessary to control the amount of branching agent added to be within a range of 1 / 3 or less and 1 / 50 or more in molar ratio to the polymerization initiator, while making the number of functional groups of the coupling agent 3 or more. When producing a modified branched conjugated diene polymer, in order to reach a weight-average molecular weight in the range of 100,000 or more and 1,000,000 or less, it is necessary to control the amount of branching agent added to be in the range of 1 / 3 or less and 1 / 50 or more in molar ratio to the polymerization initiator, thereby preventing the polymerization initiator from being completely consumed before the coupling step while forming branches, and to make the number of functional groups of the coupling agent two or more. In order to reach a weight-average molecular weight in the range of 200,000 or more and 900,000 or less, it is necessary to control the amount of branching agent added to be in the range of 1 / 3 or less and 1 / 50 or more in molar ratio to the polymerization initiator, and to make the number of functional groups of the coupling agent three or more.

[0062] The branched conjugated diene-based polymer obtained by the production method of the present embodiment may be a polymer of a conjugated diene monomer and a branching agent, or may be a copolymer of a conjugated diene monomer, a branching agent, and a monomer other than these. For example, when the conjugated diene monomer is butadiene or isoprene and is polymerized with a branching agent containing an aromatic vinyl moiety, the polymer chain is a so-called polybutadiene or polyisoprene, and the branched portion contains a structure derived from aromatic vinyl. By having such a structure, it is possible to improve the linearity of each polymer chain and improve the crosslinking density after vulcanization, and the effect of improving the abrasion resistance of the polymer is achieved. Therefore, it is suitable for applications such as tires, resin modification, interior and exterior parts of automobiles, anti-vibration rubber, and footwear. When the conjugated diene polymer is used for tire tread applications, a copolymer of a conjugated diene monomer, an aromatic vinyl monomer, and a branching agent is suitable, and in the copolymer for this application, the bound conjugated diene content is preferably 40% by mass or more and 100% by mass or less, and more preferably 55% by mass or more and 80% by mass or less. Furthermore, the amount of bound aromatic vinyl in the branched conjugated diene polymer obtained by the production method of this embodiment is not particularly limited, but is preferably from 0% by mass to 60% by mass, and more preferably from 20% by mass to 45% by mass. When the bound conjugated diene amount and bound aromatic vinyl amount are within the above ranges, the balance between low hysteresis loss and wet skid resistance, abrasion resistance, and fracture properties tend to be excellent when made into a vulcanizate. The amount of bound aromatic vinyl can be measured by ultraviolet absorption of the phenyl group, and the amount of bound conjugated diene can also be calculated from the amount. Specifically, the amount can be measured according to the method described in the examples below.

[0063] In the branched conjugated diene polymer obtained by the production method of the present embodiment, the amount of vinyl bonds in the conjugated diene bond units is not particularly limited, but is preferably 10 mol % or more and 75 mol % or less, and more preferably 20 mol % or more and 65 mol % or less. When the vinyl bond amount is within the above range, the balance between low hysteresis loss and wet skid resistance, abrasion resistance, and breaking strength tend to be excellent when made into a vulcanizate. Here, when the branched conjugated diene polymer is a copolymer of butadiene and styrene, the vinyl bond amount (1,2-bond amount) in the butadiene bond unit can be determined by the Hampton method (RR Hampton, Analytical Chemistry, 21, 923 (1949)). Specifically, it can be measured by the method described in the examples below.

[0064] Regarding the microstructure of the branched conjugated diene polymer, when the bond amounts in the branched conjugated diene polymer obtained by the production method of the present embodiment are within the above-mentioned numerical ranges, and further, when the glass transition temperature of the branched conjugated diene polymer is within the range of -80°C or higher and -15°C or lower, a vulcanizate having an even better balance between low hysteresis loss and wet skid resistance tends to be obtained. The glass transition temperature is measured in accordance with ISO 22768:2006 by recording a DSC curve while increasing the temperature within a specified temperature range, and the peak top (inflection point) of the DSC differential curve is taken as the glass transition temperature.

[0065] When the branched conjugated diene polymer obtained by the production method of the present embodiment is a conjugated diene-aromatic vinyl copolymer, the branched conjugated diene polymer preferably has a small number of blocks in which 30 or more aromatic vinyl units are linked, or has no blocks. More specifically, when the branched conjugated diene polymer obtained by the production method of the present embodiment is a butadiene-styrene copolymer, the block in which 30 or more aromatic vinyl units are linked is preferably 5.0% by mass or less, more preferably 3.0% by mass or less, based on the total amount of the branched conjugated diene polymer, in a known method in which the polymer is decomposed by the Kolthoff method (the method described in I.M.Kolthoff, et al., J.Polym.Sci.1,429(1946)) and the amount of polystyrene insoluble in methanol is analyzed.

[0066] When the branched conjugated diene polymer obtained by the production method of the present embodiment is a conjugated diene-aromatic vinyl copolymer, it is preferable that the proportion of aromatic vinyl units present alone is high from the viewpoint of improving fuel saving performance. Specifically, when the branched conjugated diene polymer obtained by the production method of the present embodiment is a butadiene-styrene copolymer, when the branched conjugated diene polymer is decomposed by an ozonolysis method known as the Tanaka et al. method (Polymer, 22, 1721 (1981)) and the styrene chain distribution is analyzed by GPC, it is preferable that the amount of isolated styrene is 40% by mass or more and the amount of chain styrene structures having 8 or more styrene chains is 5.0% by mass or less relative to the total bound styrene amount. In this case, the resulting vulcanized rubber tends to have excellent performance, particularly low hysteresis loss.

[0067] (Reaction process) In the method for producing a branched conjugated diene polymer of the present embodiment, it is preferable to carry out a step of performing a coupling reaction on the active terminal of the conjugated diene polymer obtained through the above-mentioned polymerization step and branching step using a coupling agent, for example, a reactive compound having three or more functionalities, for example, a step of performing a coupling reaction using a coupling agent consisting of a silane sulfide compound represented by the following formula (3), or a step of performing a polymerization termination reaction on the active terminal of the conjugated diene polymer using a polymerization terminator, for example, a reactive compound having two or less functionalities. Hereinafter, the step of reacting a coupling agent (coupling step) or the step of reacting a polymerization terminator (polymerization terminator step) will be collectively referred to as a reaction step. In the reaction step, one of the active terminals of the conjugated diene polymer is reacted with a coupling agent or a polymerization terminator.

[0068] <Coupling process> In the method for producing a branched conjugated diene polymer of the present embodiment, it is preferable that the reaction step involves subjecting the conjugated diene polymer obtained through the above-mentioned polymerization step and branching step to a coupling reaction using a coupling agent. The coupling reaction can efficiently lengthen the molecular chain, and can also introduce branches into the polymer by using a coupling agent with three or more functionalities. Although the function of forming branches is common to the process using a branching agent, it is preferable to perform the coupling process in terms of forming branches while introducing desired elements such as nitrogen, sulfur, and silicon using a known coupling agent. In the coupling step, for example, a trifunctional or higher reactive compound, a coupling agent having a nitrogen atom-containing group, or a coupling agent consisting of a silane sulfide compound represented by the following formula (3) (hereinafter, these may be collectively referred to as "coupling agent") is preferably used for the active terminal of the conjugated diene polymer.

[0069] In the reaction step, for example, a branched conjugated diene polymer can be obtained by coupling reaction with a reactive compound having three or more functionalities, a coupling agent having a nitrogen atom-containing group, or a silane sulfide compound represented by the following formula (3), which is a modifying agent containing silicon and sulfur atoms, at one active end of the conjugated diene polymer.

[0070] [Reactive compounds with three or more functional groups] In the method for producing a branched conjugated diene-based polymer of this embodiment, the tri- or higher functional reactive compound used in the coupling step is preferably a tri- or higher functional reactive compound having a silicon atom.

[0071] Examples of the tri- or higher functional reactive compound having a silicon atom include, but are not limited to, halogenated silane compounds, epoxy silane compounds, vinylated silane compounds, alkoxy silane compounds, and the like.

[0072] Examples of halogenated silane compounds that are coupling agents include, but are not limited to, methyltrichlorosilane, tetrachlorosilane, tris(trimethylsiloxy)chlorosilane, tris(dimethylamino)chlorosilane, hexachlorodisilane, bis(trichlorosilyl)methane, 1,2-bis(trichlorosilyl)ethane, 1,2-bis(methyldichlorosilyl)ethane, 1,4-bis(trichlorosilyl)butane, and 1,4-bis(methyldichlorosilyl)butane.

[0073] Examples of the epoxidized silane compound that is a coupling agent include, but are not limited to, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and epoxy-modified silicone.

[0074] Examples of the alkoxysilane compound that is a coupling agent include, but are not limited to, tetramethoxysilane, tetraethoxysilane, triphenoxymethylsilane, 1,2-bis(triethoxysilyl)ethane, and methoxy-substituted polyorganosiloxane.

[0075] [Coupling Agent Having Nitrogen Atom-Containing Group] Examples of coupling agents having a nitrogen atom-containing group include, but are not limited to, isocyanate compounds, isothiocyanate compounds, isocyanuric acid derivatives, carbonyl compounds having a nitrogen atom-containing group, vinyl compounds having a nitrogen atom-containing group, epoxy compounds having a nitrogen atom-containing group, alkoxysilane compounds having a nitrogen atom-containing group, and protected amine compounds having a nitrogen atom-containing group and capable of forming a primary or secondary amine.

[0076] In the coupling agent having a nitrogen atom-containing group, the nitrogen atom-containing functional group can preferably be a functional group derived from an amine compound that does not have active hydrogen, and the amine compound can be, for example, a tertiary amine compound, or a protected amine compound in which the above-mentioned active hydrogen is replaced with a protective group.Other compounds that can form a nitrogen atom-containing functional group can be, for example, an imine compound represented by the general formula -N=C, and an alkoxysilane compound that is bonded to the above-mentioned nitrogen atom-containing group.

[0077] Examples of isocyanate compounds that are coupling agents having a nitrogen atom-containing group include, but are not limited to, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, diphenylmethane diisocyanate, polymeric diphenylmethane diisocyanate (C-MDI), phenyl isocyanate, isophorone diisocyanate, hexamethylene diisocyanate, butyl isocyanate, and 1,3,5-benzene triisocyanate.

[0078] Examples of isocyanuric acid derivatives that are coupling agents having a nitrogen atom-containing group include, but are not limited to, 1,3,5-tris(3-trimethoxysilylpropyl)isocyanurate, 1,3,5-tris(3-triethoxysilylpropyl)isocyanurate, 1,3,5-tris(oxiran-2-yl)-1,3,5-triazinane-2,4,6-trione, 1,3,5-tris(isocyanatomethyl)-1,3,5-triazinane-2,4,6-trione, and 1,3,5-trivinyl-1,3,5-triazinane-2,4,6-trione.

[0079] Examples of carbonyl compounds that are coupling agents having a nitrogen atom-containing group include, but are not limited to, 1,3-dimethyl-2-imidazolidinone, 1-methyl-3-ethyl-2-imidazolidinone, 1-methyl-3-(2-methoxyethyl)-2-imidazolidinone, N-methyl-2-pyrrolidone, N-methyl-2-piperidone, N-methyl-2-quinolone, 4,4'-bis(diethylamino)benzophenone, 4,4'-bis(dimethylamino)benzophenone, and the like. Examples of such amines include methyl-2-pyridyl ketone, methyl-4-pyridyl ketone, propyl-2-pyridyl ketone, di-4-pyridyl ketone, 2-benzoylpyridine, N,N,N',N'-tetramethylurea, N,N-dimethyl-N',N'-diphenylurea, N,N-diethylmethylcarbamate, N,N-diethylacetamide, N,N-dimethyl-N',N'-dimethylaminoacetamide, N,N-dimethylpicolinic acid amide, and N,N-dimethylisonicotinic acid amide.

[0080] Examples of vinyl compounds that are coupling agents having a nitrogen atom-containing group include, but are not limited to, N,N-dimethylacrylamide, N,N-dimethylmethacrylamide, N-methylmaleimide, N-methylphthalimide, N,N-bistrimethylsilylacrylamide, morpholinoacrylamide, 3-(2-dimethylaminoethyl)styrene, (dimethylamino)dimethyl-4-vinylphenylsilane, 4,4'-vinylidenebis(N,N-dimethylaniline), 4,4'-vinylidenebis(N,N-diethylaniline), 1,1-bis(4-morpholinophenyl)ethylene, and 1-phenyl-1-(4-N,N-dimethylaminophenyl)ethylene.

[0081] The epoxy compound, which is a coupling agent having a nitrogen atom-containing group, includes, but is not limited to, for example, an epoxy group-containing hydrocarbon compound bonded to an amino group, and further includes an epoxy group-containing hydrocarbon compound bonded to an ether group. Such an epoxy compound includes, but is not limited to, for example, an epoxy compound represented by the general formula (i):

[0082] [ka]

[0083] In the formula (i), R is a divalent or higher organic group having at least one polar group selected from the group consisting of a divalent or higher hydrocarbon group, or an oxygen-containing polar group such as an ether, epoxy, or ketone, a sulfur-containing polar group such as a thioether or thioketone, and a nitrogen-containing polar group such as a tertiary amino group or an imino group.

[0084] The divalent or higher hydrocarbon group is a saturated or unsaturated, linear, branched or cyclic hydrocarbon group, and includes an alkylene group, an alkenylene group, a phenylene group, etc. A hydrocarbon group having 1 to 20 carbon atoms is preferable. Examples thereof include methylene, ethylene, butylene, cyclohexylene, 1,3-bis(methylene)-cyclohexane, 1,3-bis(ethylene)-cyclohexane, o-, m-, p-phenylene, m-, p-xylene, and bis(phenylene)-methane.

[0085] In the formula (i), R 1 , R 4 is a hydrocarbon group having 1 to 10 carbon atoms, R 1 , R 4 may be the same or different from each other. In the formula (i), R 2 , R 5 is hydrogen or a hydrocarbon group having 1 to 10 carbon atoms, R 2 , R 5 may be the same or different from each other. In the formula (i), R 3 is a hydrocarbon group having 1 to 10 carbon atoms, or a structure represented by the following formula (ii): R 1 , R 2 , R 3 may be bonded to each other to form a cyclic structure. Also, R 3 When R is a hydrocarbon group, R may be bonded to R to form a cyclic structure. 3 The N bonded to R may be directly bonded to the N bonded to R. In the above formula (i), n is an integer of 1 or more, and m is 0 or a natural number of 1 or more.

[0086] [ka]

[0087] In the formula (ii), R 1 , R 2 is R in the formula (i). 1 , R 2is defined similarly to R 1 , R 2 may be the same or different from each other.

[0088] The epoxy compound, which is a coupling agent having a nitrogen atom-containing group, is preferably one having an epoxy group-containing hydrocarbon group, more preferably one having a glycidyl group-containing hydrocarbon group.

[0089] The epoxy group-containing hydrocarbon group bonded to the amino group or ether group is not particularly limited, but may be, for example, a glycidylamino group, a diglycidylamino group, or a glycidoxy group. More preferred molecular structures are epoxy group-containing compounds each having a glycidylamino group or a diglycidylamino group, and a glycidoxy group, and examples thereof include compounds represented by the following general formula (iii).

[0090] [ka]

[0091] In the formula (iii), R is defined as R in the formula (i), 6 is a hydrocarbon group having 1 to 10 carbon atoms or a structure represented by the following formula (iv): R 6 When R is a hydrocarbon group, R may be bonded to R to form a cyclic structure. In this case, R 6 The N bonded to R may be directly bonded to the N bonded to R. In formula (iii), n is an integer of 1 or more, and m is 0 or an integer of 1 or more.

[0092] [ka]

[0093] As the epoxy compound which is a coupling agent having a nitrogen atom-containing group, a compound having one or more diglycidylamino groups and one or more glycidoxy groups in the molecule is particularly preferred.

[0094] The epoxy compound used as the coupling agent having a nitrogen atom-containing group is not limited to the following, but examples thereof include N,N-diglycidyl-4-glycidoxyaniline, 1-N,N-diglycidylaminomethyl-4-glycidoxy-cyclohexane, 4-(4-glycidoxyphenyl)-(N,N-diglycidyl)aniline, 4-(4-glycidoxyphenoxy)-(N,N-diglycidyl)aniline, 4-(4-glycidoxybenzyl)-(N,N-diglycidyl)aniline, 4-(N,N'-diglycidyl-2-piperazinyl)-glycidoxybenzene, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, N,N,N',N'-tetraglycidyl -m-xylylenediamine, 4,4-methylene-bis(N,N-diglycidylaniline), 1,4-bis(N,N-diglycidylamino)cyclohexane, N,N,N',N'-tetraglycidyl-p-phenylenediamine, 4,4'-bis(diglycidylamino)benzophenone, 4-(4-glycidylpiperazinyl)-(N,N-diglycidyl)aniline, 2-[2-(N,N-diglycidylamino)ethyl]-1-glycidylpyrrolidine, N,N-diglycidylaniline, 4,4'-diglycidyl-dibenzylmethylamine, N,N-diglycidylaniline, N,N-diglycidylorthotoluidine, and N,N-diglycidylaminomethylcyclohexane are examples thereof. Among these, particularly preferred ones include N,N-diglycidyl-4-glycidoxyaniline and 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane.

[0095] Examples of the alkoxysilane compound, which is a coupling agent having a nitrogen atom-containing group, include, but are not limited to, 3-dimethylaminopropyltrimethoxysilane, 3-dimethylaminopropylmethyldimethoxysilane, 3-diethylaminopropyltriethoxysilane, 3-morpholinopropyltrimethoxysilane, 3-piperidinopropyltriethoxysilane, 3-hexamethyleneiminopropylmethyldiethoxysilane, 3-(4-methyl-1-piperazino)propyltriethoxysilane, 1-[3-(triethoxysilyl)-propyl] ... pyl]-3-methylhexahydropyrimidine, 3-(4-trimethylsilyl-1-piperazino)propyltriethoxysilane, 3-(3-triethylsilyl-1-imidazolidinyl)propylmethyldiethoxysilane, 3-(3-trimethylsilyl-1-hexahydropyrimidinyl)propyltrimethoxysilane, 3-dimethylamino-2-(dimethylaminomethyl)propyltrimethoxysilane, bis(3-dimethoxymethylsilylpropyl)-N-methylamine, bis(3-trimethoxysilylpropyl)-N-methylamine, bis(3-triethylsilylpropyl)-N-methylamine, (trimethoxysilylpropyl)methylamine, tris(trimethoxysilyl)amine, tris(3-trimethoxysilylpropyl)amine, N,N,N',N'-tetra(3-trimethoxysilylpropyl)ethylenediamine, 3-isocyanatopropyltrimethoxysilane, 3-cyanopropyltrimethoxysilane, 2,2-dimethoxy-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(3-triethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-( 4-trimethoxysilylbutyl)-1-aza-2-silacyclohexane, 2,2-dimethoxy-1-(3-dimethoxymethylsilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-phenyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-butyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-methyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-8-(4-methylpiperazinyl)methyl-1,6-dioxa-2-silacyclooctane, 2,2-dimethoxy-8-(N,N-diethylamino)methyl-1,6-dioxa-2-silacyclooctane, etc.

[0096] Examples of protected amine compounds that are coupling agents having a nitrogen atom-containing group and can form primary or secondary amines include compounds having an unsaturated bond and a protected amine in the molecule, but are not limited to the following: 4,4'-vinylidenebis[N,N-bis(trimethylsilyl)aniline], 4,4'-vinylidenebis[N,N-bis(triethylsilyl)aniline], 4,4'-vinylidenebis[N,N-bis(t-butyldimethylsilyl)aniline], 4,4'-vinylidenebis[N-methyl-N-(trimethylsilyl)aniline], 4,4'-vinylidenebis[N-ethyl-N-(trimethylsilyl)aniline], 4, Examples thereof include 4'-vinylidenebis[N-methyl-N-(triethylsilyl)aniline], 4,4'-vinylidenebis[N-ethyl-N-(triethylsilyl)aniline], 4,4'-vinylidenebis[N-methyl-N-(t-butyldimethylsilyl)aniline], 4,4'-vinylidenebis[N-ethyl-N-(t-butyldimethylsilyl)aniline], 1-[4-N,N-bis(trimethylsilyl)aminophenyl]-1-[4-N-methyl-N-(trimethylsilyl)aminophenyl]ethylene, and 1-[4-N,N-bis(trimethylsilyl)aminophenyl]-1-[4-N,N-dimethylaminophenyl]ethylene.

[0097] Coupling agents having a nitrogen atom-containing group, which are protected amine compounds capable of forming primary or secondary amines, and which have an alkoxysilane and a protected amine in the molecule, include, but are not limited to, N,N-bis(trimethylsilyl)aminopropyltrimethoxysilane, N,N-bis(trimethylsilyl)aminopropylmethyldimethoxysilane, N,N-bis(trimethylsilyl)aminopropyltriethoxysilane, N,N-bis(trimethylsilyl)aminopropylmethyldiethoxysilane, N ,N-Bis(trimethylsilyl)aminoethyltrimethoxysilane, N,N-Bis(trimethylsilyl)aminoethylmethyldiethoxysilane, N,N-Bis(triethylsilyl)aminopropylmethyldiethoxysilane, 3-(4-trimethylsilyl-1-piperazino)propyltriethoxysilane, 3-(3-triethylsilyl-1-imidazolidinyl)propylmethyldiethoxysilane, 3-(3-trimethylsilyl-1-hexahydropyrimidinyl)propyltrimethoxysilane, 2,2-dimethoxy-1-(3-trimethylsilyl-1-hexahydropyrimidinyl)propyltrimethoxysilane, 2,2-diethoxy-1-(3-triethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(4-trimethoxysilylbutyl)-1-aza-2-silacyclohexane, 2,2-dimethoxy-1-(3-dimethoxymethylsilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-phenyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-butyl-1-aza-2-silacyclopentane, 2,2-Dimethoxy-1-methyl-1-aza-2-silacyclopentane, N-(1,3-dimethylbutylidene)-3-(triethoxysilyl)-1-propanamine, N-(1-methylethylidene)-3-(triethoxysilyl)-1-propanamine, N-ethylidene-3-(triethoxysilyl)-1-propanamine, N-(1-methylpropylidene)-3-(triethoxysilyl)-1-propanamine, N-(4-N,N-dimethylaminobenzylidene)-3-(triethoxysilyl)-1-propanamine, N-(1,Examples of the silane include 3-dimethylbutylidene)-3-(triethoxysilyl)-1-propanamine, 3-(benzylideneamino)propyltrimethoxysilane, 3-(benzylideneamino)propyltriethoxysilane, and 3-(benzylideneamino)propyltripropylsilane.

[0098] Particularly preferred alkoxysilane compounds that are coupling agents having a nitrogen atom-containing group include, but are not limited to, tris(3-trimethoxysilylpropyl)amine, tris(3-triethoxysilylpropyl)amine, tris(3-tripropoxysilylpropyl)amine, bis(3-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]amine, tetrakis(3-trimethoxysilylpropyl)-1,3-propanediamine, tris(3-trimethoxysilylpropyl)-1,3-propanediamine, tris(3-trimethoxysilylpropyl)-[3-(1-methoxy-2-methyl-1-sila-2-azacyclopentane)propyl]-1,3-propanediamine, bis(3-triethoxysilylpropyl)-[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-[3-(1-ethoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-propanediamine, Tetrakis(3-trimethoxysilylpropyl)-1,3-bisaminomethylcyclohexane, tris(3-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-1,3-bisaminomethylcyclohexane, tetrakis(3-trimethoxysilylpropyl)-1,6-hexamethylenediamine, pentakis(3-trimethoxysilylpropyl)-diethylenetriamine, tris(3-trimethoxysilylpropyl)-methyl-1,3-propanediamine, tetrakis[3-(2,2-dimethoxysilylpropyl)-methyl-1,3-propanediamine silane, bis(3-trimethoxysilylpropyl)-bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]silane, tris[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-(3-trimethoxysilylpropyl)silane, tris[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]silane, 3-tris[2-(2,2-dimethoxy-1-aza-2-silacyclopentane)ethoxy]silyl-1-trimethoxysilylpropane, 1-[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-3,4,5-tris(3-trimethoxysilylpropyl)-cyclohexane, 1-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-3,4,5-tris(3-trimethoxysilylpropyl)-cyclohexane, 3,4,5-tris(3-trimethoxysilylpropyl)-cyclohexyl-[3 -(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]ether, (3-trimethoxysilylpropyl)phosphate, bis(3-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]phosphate, bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-(3-trimethoxysilylpropyl)phosphate, and tris[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]phosphate.

[0099] The coupling agent used in the reaction step is preferably a silane sulfide compound represented by the following formula (3).

[0100] [ka]

[0101] (In formula (3), Si represents a silicon atom, O represents an oxygen atom, and S represents a sulfur atom. x is an integer of 1 to 3, y is 0 or an integer of 1 to 2, and x+y is 3. R 1 , R 2 , R 4 may be the same or different and represent an alkyl group having 1 to 16 carbon atoms; R 3 represents an aryl group having 6 to 16 carbon atoms, an alkylene group having 1 to 16 carbon atoms, or an alkyl chain having 1 to 16 carbon atoms.

[0102] The coupling agent represented by the formula (3) is not limited to the following, for example, S-trimethylsilylmercaptopropyltrimethoxysilane, S-trimethylsilylmercaptopropyltriethoxysilane, S-trimethylsilylmercaptopropyltripropoxysilane, S-trimethylsilylmercaptopropyltributoxysilane, S-trimethylsilylmercaptoethyltrimethoxysilane, S-trimethylsilylmercaptoethyltriethoxysilane, S-trimethylsilylmercaptoethyltripropoxysilane, S-trimethylsilylmercaptoethyltributoxysilane, S-trimethylsilylmercaptomethyltrimethoxysilane, S-trimethylsilylmercaptomethyltriethoxysilane, S-trimethylsilylmercaptomethyltriethoxysilane, Examples of the silane include methyl tripropoxysilane, S-trimethylsilyl mercapto methyl tributoxy silane, S-trimethylsilyl mercapto-2,2-dimethylpropyl trimethoxy silane, S-trimethylsilyl mercapto-2,2-dimethylpropyl triethoxy silane, S-trimethylsilyl mercapto-2,2-dimethylpropyl tripropoxy silane, S-trimethylsilyl mercapto-2,2-dimethylpropyl tributoxy silane, S-trimethylsilyl mercapto-2-methylpropyl trimethoxy silane, S-trimethylsilyl mercapto-2-methylpropyl triethoxy silane, S-trimethylsilyl mercapto-2-methylpropyl tripropoxy silane, and S-trimethylsilyl mercapto-2-methylpropyl tributoxy silane.

[0103] Also, S-trimethylsilylmercaptopropylmethyldimethoxysilane, S-trimethylsilylmercaptopropylmethyldiethoxysilane, S-trimethylsilylmercaptopropylmethyldipropoxysilane, S-trimethylsilylmercaptopropylmethyldibutoxysilane, S-trimethylsilylmercaptoethylmethyldimethoxysilane, S-trimethylsilylmercaptoethylmethyldiethoxysilane, S-trimethylsilylmercaptoethylmethyldipropoxysilane, S-trimethylsilylmercaptoethylmethyldibutoxysilane, S-trimethylsilylmercaptomethylmethyldimethoxysilane, S-trimethylsilylmercaptomethylmethyldiethoxysilane, S-trimethylsilylmercapto Examples of the silane include methyl methyl dipropoxy silane, S-trimethylsilyl mercapto methyl methyl dibutoxy silane, S-trimethylsilyl mercapto-2,2-dimethyl propyl methyl dimethoxy silane, S-trimethylsilyl mercapto-2,2-dimethyl propyl methyl diethoxy silane, S-trimethylsilyl mercapto-2,2-dimethyl propyl methyl dipropoxy silane, S-trimethylsilyl mercapto-2,2-dimethyl propyl methyl dibutoxy silane, S-trimethylsilyl mercapto-2-methyl propyl methyl dimethoxy silane, S-trimethylsilyl mercapto-2-methyl propyl methyl diethoxy silane, and S-trimethylsilyl mercapto-2-methyl propyl methyl dipropoxy silane.

[0104] Also, S-trimethylsilylmercapto-2-methylpropylmethyldibutoxysilane, S-trimethylsilylmercaptopropyldimethylmethoxysilane, S-trimethylsilylmercaptopropyldimethylethoxysilane, S-trimethylsilylmercaptopropyldimethylpropoxysilane, S-trimethylsilylmercaptopropyldimethylbutoxysilane, S-trimethylsilylmercaptoethyldimethylmethoxysilane, S-trimethylsilylmercaptoethyldimethylethoxysilane, S-trimethylsilylmercaptoethyldimethylpropoxysilane, S-trimethylsilylmercaptoethyldimethylbutoxysilane, S-trimethylsilylmercaptomethyldimethylmethoxysilane, Examples of the silane include S-trimethylsilylmercaptomethyldimethylethoxysilane, S-trimethylsilylmercaptomethyldimethylpropoxysilane, S-trimethylsilylmercaptomethyldimethylbutoxysilane, S-trimethylsilylmercapto-2,2-dimethylpropyldimethylmethoxysilane, S-trimethylsilylmercapto-2,2-dimethylpropyldimethylethoxysilane, S-trimethylsilylmercapto-2,2-dimethylpropyldimethylpropoxysilane, S-trimethylsilylmercapto-2,2-dimethylpropyldimethylbutoxysilane, S-trimethylsilylmercapto-2-methylpropyldimethylmethoxysilane, and S-trimethylsilylmercapto-2-methylpropyldimethylethoxysilane.

[0105] Also, S-trimethylsilylmercapto-2-methylpropyldimethylpropoxysilane, S-trimethylsilylmercapto-2-methylpropyldimethylbutoxysilane, S-triethylsilylmercaptopropyltrimethoxysilane, S-triethylsilylmercaptopropyltriethoxysilane, S-triethylsilylmercaptopropyltripropoxysilane, S-triethylsilylmercaptopropyltributoxysilane, S-triethylsilylmercaptoethyltrimethoxysilane, S-triethylsilylmercaptoethyltriethoxysilane, S-triethylsilylmercaptoethyltripropoxysilane, S-triethylsilylmercaptoethyltributoxysilane, S-triethylsilylmercaptomethyltrimethoxysilane, S-triethyl Examples of the silylmercaptomethyltriethoxysilane include S-triethylsilylmercaptomethyltripropoxysilane, S-triethylsilylmercaptomethyltributoxysilane, S-triethylsilylmercapto-2,2-dimethylpropyltrimethoxysilane, S-triethylsilylmercapto-2,2-dimethylpropyltriethoxysilane, S-triethylsilylmercapto-2,2-dimethylpropyltripropoxysilane, S-triethylsilylmercapto-2,2-dimethylpropyltributoxysilane, S-triethylsilylmercapto-2-methylpropyltrimethoxysilane, S-triethylsilylmercapto-2-methylpropyltriethoxysilane, and S-triethylsilylmercapto-2-methylpropyltripropoxysilane.

[0106] Also, S-triethylsilylmercapto-2-methylpropyltributoxysilane, S-triethylsilylmercaptopropylmethyldimethoxysilane, S-triethylsilylmercaptopropylmethyldiethoxysilane, S-triethylsilylmercaptopropylmethyldipropoxysilane, S-triethylsilylmercaptopropylmethyldibutoxysilane, S-triethylsilylmercaptoethylmethyldimethoxysilane, S-triethylsilylmercaptoethylmethyldiethoxysilane, S-triethylsilylmercaptoethylmethyldipropoxysilane, S-triethylsilylmercaptoethylmethyldibutoxysilane, S-triethylsilylmercaptomethylmethyl Examples of suitable silanes include S-triethylsilylmercaptomethylmethyldiethoxysilane, S-triethylsilylmercaptomethylmethyldipropoxysilane, S-triethylsilylmercaptomethylmethyldibutoxysilane, S-triethylsilylmercapto-2,2-dimethylpropylmethyldimethoxysilane, S-triethylsilylmercapto-2,2-dimethylpropylmethyldiethoxysilane, S-triethylsilylmercapto-2,2-dimethylpropylmethyldipropoxysilane, S-triethylsilylmercapto-2,2-dimethylpropylmethyldibutoxysilane, and S-triethylsilylmercapto-2-methylpropylmethyldimethoxysilane.

[0107] Also, S-triethylsilylmercapto-2-methylpropylmethyldiethoxysilane, S-triethylsilylmercapto2-methylpropylmethyldipropoxysilane, S-triethylsilylmercapto2-methylpropylmethyldibutoxysilane, S-triethylsilylmercaptopropyldimethylmethoxysilane, S-triethylsilylmercaptopropyldimethylethoxysilane, S-triethylsilylmercaptopropyldimethylpropoxysilane, S-triethylsilylmercaptopropyldimethylbutoxysilane, S-triethylsilylmercaptoethyldimethylmethoxysilane, S-triethylsilylmercaptoethyldimethylethoxysilane, S-triethylsilylmercaptoethyldimethylpropoxysilane Examples of the silane include dimethylsilane, S-triethylsilylmercaptoethyldimethylbutoxysilane, S-triethylsilylmercaptomethyldimethylmethoxysilane, S-triethylsilylmercaptomethyldimethylethoxysilane, S-triethylsilylmercaptomethyldimethylpropoxysilane, S-triethylsilylmercaptomethyldimethylbutoxysilane, S-triethylsilylmercapto-2,2-dimethylpropyldimethylmethoxysilane, S-triethylsilylmercapto-2,2-dimethylpropyldimethylethoxysilane, S-triethylsilylmercapto-2,2-dimethylpropyldimethylpropoxysilane, and S-triethylsilylmercapto-2,2-dimethylpropyldimethylbutoxysilane.

[0108] Also, S-dimethyl tertbutylsilyl mercaptopropyl trimethoxysilane, S-dimethyl tertbutylsilyl mercaptopropyl triethoxysilane, S-dimethyl tertbutylsilyl mercaptopropyl tripropoxysilane, S-dimethyl tertbutylsilyl mercaptopropyl tributoxysilane, S-dimethyl tertbutylsilyl mercaptoethyl trimethoxysilane, S-dimethyl tertbutylsilyl mercaptoethyl triethoxysilane, S-dimethyl tertbutylsilyl mercaptoethyl Examples of the silane include S-dimethyl tertbutylsilylmercaptomethyltripropoxysilane, S-dimethyl tertbutylsilylmercaptoethyltributoxysilane, S-dimethyl tertbutylsilylmercaptomethyltrimethoxysilane, S-dimethyl tertbutylsilylmercaptomethyltriethoxysilane, S-dimethyl tertbutylsilylmercaptomethyltripropoxysilane, S-dimethyl tertbutylsilylmercaptomethyltributoxysilane, and S-dimethyl tertbutylsilylmercapto-2,2-dimethylpropyltrimethoxysilane.

[0109] Also, S-dimethyl tertbutylsilylmercapto-2,2-dimethylpropyltriethoxysilane, S-dimethyl tertbutylsilylmercapto-2,2-dimethylpropyltripropoxysilane, S-dimethyl tertbutylsilylmercapto-2,2-dimethylpropyltributoxysilane, S-dimethyl tertbutylsilylmercapto-2-methylpropyltrimethoxysilane, S-dimethyl tertbutylsilylmercapto-2-methylpropyltriethoxysilane, S-dimethyl tertbutylsilylmercapto-2-methylpropyltripropoxysilane, S-dimethyl tertbutylsilylmercapto- Examples of the silane include 2-methylpropyl tributoxy silane, S-dimethyl tertbutylsilyl mercaptopropyl methyl dimethoxy silane, S-dimethyl tertbutylsilyl mercaptopropyl methyl diethoxy silane, S-dimethyl tertbutylsilyl mercaptopropyl methyl dipropoxy silane, S-dimethyl tertbutylsilyl mercaptopropyl methyl dibutoxy silane, S-dimethyl tertbutylsilyl mercaptoethyl methyl dimethoxy silane, S-dimethyl tertbutylsilyl mercaptoethyl methyl diethoxy silane, and S-dimethyl tertbutylsilyl mercaptoethyl methyl dipropoxy silane.

[0110] Also, S-dimethyl tertbutylsilyl mercaptoethyl methyl dibutoxysilane, S-dimethyl tertbutylsilyl mercaptomethyl methyl dimethoxysilane, S-dimethyl tertbutylsilyl mercaptomethyl methyl diethoxysilane, S-dimethyl tertbutylsilyl mercaptomethyl methyl dipropoxysilane, S-dimethyl tertbutylsilyl mercaptomethyl methyl dibutoxysilane, S-dimethyl tertbutylsilyl mercapto-2,2-dimethylpropyl methyl dimethoxysilane, S-dimethyl tertbutylsilyl mercapto-2,2-dimethylpropyl methyl diethoxysilane, S-dimethyl tertbutylsilyl Mercapto-2,2-dimethylpropylmethyldipropoxysilane, S-dimethyltertbutylsilylmercapto-2,2-dimethylpropylmethyldibutoxysilane, S-dimethyltertbutylsilylmercapto-2-methylpropylmethyldimethoxysilane, S-dimethyltertbutylsilylmercapto-2-methylpropylmethyldiethoxysilane, S-dimethyltertbutylsilylmercapto-2-methylpropylmethyldipropoxysilane, S-dimethyltertbutylsilylmercapto-2-methylpropylmethyldibutoxysilane, S-dimethyltertbutylsilylmercaptopropyldimethylmethoxysilane.

[0111] Further examples thereof include S-dimethyl tertbutylsilyl mercaptopropyl dimethylethoxysilane, S-dimethyl tertbutylsilyl mercaptopropyl dimethylpropoxysilane, S-dimethyl tertbutylsilyl mercaptopropyl dimethylbutoxysilane, S-dimethyl tertbutylsilyl mercaptoethyl dimethylmethoxysilane, S-dimethyl tertbutylsilyl mercaptoethyl dimethylethoxysilane, S-dimethyl tertbutylsilyl mercaptoethyl dimethylpropoxysilane, S-dimethyl tertbutylsilyl mercaptoethyl dimethylbutoxysilane, S-dimethyl tertbutylsilyl mercaptomethyl dimethylmethoxysilane, S-dimethyl tertbutylsilyl mercaptomethyl dimethylethoxysilane, S-dimethyl tertbutylsilyl mercaptomethyl dimethylpropoxysilane, and S-dimethyl tertbutylsilyl mercaptomethyl dimethylbutoxysilane.

[0112] Further examples thereof include S-dimethyl tertbutylsilylmercapto-2,2-dimethylpropyldimethylmethoxysilane, S-dimethyl tertbutylsilylmercapto-2,2-dimethylpropyldimethylethoxysilane, S-dimethyl tertbutylsilylmercapto-2,2-dimethylpropyldimethylpropoxysilane, S-dimethyl tertbutylsilylmercapto-2,2-dimethylpropyldimethylbutoxysilane, S-dimethyl tertbutylsilylmercapto-2-methylpropyldimethylmethoxysilane, S-dimethyl tertbutylsilylmercapto-2-methylpropyldimethylethoxysilane, S-dimethyl tertbutylsilylmercapto-2-methylpropyldimethylpropoxysilane, and S-dimethyl tertbutylsilylmercapto-2-methylpropyldimethylbutoxysilane.

[0113] <Branched conjugated diene polymer obtained through polymerization process, branching process, and reaction process> In the method for producing a branched conjugated diene polymer of the present embodiment, the branched conjugated diene polymer obtained through the above-mentioned reaction step, particularly the step of reacting a coupling agent, preferably contains a structure derived from a compound having a nitrogen atom-containing group represented by the following general formula (i) or any of the general formulae (A) to (C).

[0114] [ka]

[0115] In the formula (i), R is a divalent or higher organic group having at least one polar group selected from a divalent or higher hydrocarbon group, or a polar group having oxygen such as ether, epoxy, or ketone, a polar group having sulfur such as thioether or thioketone, or a polar group having nitrogen such as a tertiary amino group or imino group.

[0116] The divalent or higher hydrocarbon group is a saturated or unsaturated, linear, branched or cyclic hydrocarbon group, and includes an alkylene group, an alkenylene group, a phenylene group, etc. A hydrocarbon group having 1 to 20 carbon atoms is preferable. Examples thereof include methylene, ethylene, butylene, cyclohexylene, 1,3-bis(methylene)-cyclohexane, 1,3-bis(ethylene)-cyclohexane, o-, m-, p-phenylene, m-, p-xylene, and bis(phenylene)-methane.

[0117] In the formula (i), R 1 , R 4 is a hydrocarbon group having 1 to 10 carbon atoms, R 1 , R 4 may be the same or different from each other. In the formula (i), R 2 , R 5 is hydrogen or a hydrocarbon group having 1 to 10 carbon atoms, R 2 , R 5 may be the same or different from each other. In the formula (i), R 3 is a hydrocarbon group having 1 to 10 carbon atoms, or a structure represented by the following formula (ii): R1 , R 2 , R 3 may be bonded to each other to form a cyclic structure. Also, R 3 When R is a hydrocarbon group, R may be bonded to R to form a cyclic structure. 3 The N bonded to R may be directly bonded to the N bonded to R. In the above formula (i), n is an integer of 1 or more, and m is 0 or an integer of 1 or more.

[0118] [ka]

[0119] In the formula (ii), R 1 , R 2 is R in the formula (i). 1 , R 2 is defined similarly to R 1 , R 2 may be the same or different from each other.

[0120] [ka]

[0121] (In formula (A), R 1 ~R 4 each independently represents an alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 20 carbon atoms; R 5 represents an alkylene group having 1 to 10 carbon atoms; R 6 represents an alkylene group having 1 to 20 carbon atoms. m represents an integer of 1 or 2, n represents an integer of 2 or 3, and (m+n) represents an integer of 4 or more. 1 ~R 4 are independent of each other.)

[0122] [ka]

[0123] (In formula (B), R 1 ~R 6 each independently represents an alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 20 carbon atoms; R 7 ~R 9 each independently represents an alkylene group having 1 to 20 carbon atoms. m, n, and l each independently represent an integer of 1 to 3, and (m+n+l) represents an integer of 4 or more. 1 ~R 6 are independent of each other.)

[0124] [ka]

[0125] (In formula (C), R 12 ~R 14 each independently represents a single bond or an alkylene group having 1 to 20 carbon atoms; R 15 ~R 18 , and R 20 each independently represents an alkyl group having 1 to 20 carbon atoms; R 19 and R 22 each independently represents an alkylene group having 1 to 20 carbon atoms; R 21 represents an alkyl group having 1 to 20 carbon atoms or a trialkylsilyl group. m represents an integer of 1 to 3; p represents 1 or 2. R when there are multiple of each 12 ~R 22 , m, and p are each independent and may be the same or different. i represents an integer of 0 to 6, j represents an integer of 0 to 6, k represents an integer of 0 to 6, and (i+j+k) is an integer of 4 to 10. A represents a hydrocarbon group having 1 to 20 carbon atoms, or an organic group having at least one atom selected from the group consisting of an oxygen atom, a nitrogen atom, a silicon atom, a sulfur atom, and a phosphorus atom and having no active hydrogen.

[0126] The coupling agent having a nitrogen atom-containing group represented by the formula (A) is not limited to the following, but examples thereof include 2,2-dimethoxy-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(3-triethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(4-trimethoxysilylbutyl)-1-aza-2-silacyclohexane, 2,2-dimethoxy-1-(5-trimethoxysilylpentyl)-1-aza-2-silacycloheptane, 2,2-dimethoxy-1-(3-dimethoxymethylsilylpropyl)-1-aza-2-silacyclopentane, Examples of such silacyclopentane include 2,2-diethoxy-1-(3-diethoxyethylsilylpropyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-ethoxy,2-ethyl-1-(3-triethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(3-dimethoxymethylsilylpropyl)-1-aza-2-silacyclopentane, and 2-ethoxy-2-ethyl-1-(3-diethoxyethylsilylpropyl)-1-aza-2-silacyclopentane.

[0127] Among these, from the viewpoints of reactivity and interaction between the functional group of the coupling agent having a nitrogen atom-containing group and an inorganic filler such as silica, and from the viewpoint of processability, those in which m is 2 and n is 3 are preferred. Specifically, 2,2-dimethoxy-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane and 2,2-diethoxy-1-(3-triethoxysilylpropyl)-1-aza-2-silacyclopentane are preferred.

[0128] The reaction temperature, reaction time, and the like when reacting the coupling agent having the nitrogen atom-containing group represented by the formula (A) with the polymerization active terminal are not particularly limited, but it is preferable to react at 0° C. or higher and 120° C. or lower for 30 seconds or longer.

[0129] The total number of moles of alkoxy groups bonded to silyl groups in the coupling agent compound having a nitrogen atom-containing group represented by formula (A) is preferably in the range of 0.6 to 3.0 times the number of moles of the alkali metal compound and / or alkaline earth metal compound added as the polymerization initiator, more preferably in the range of 0.8 to 2.5 times, and even more preferably in the range of 0.8 to 2.0 times. From the viewpoint of obtaining a sufficient modification rate, molecular weight, and branched structure of the obtained branched conjugated diene polymer, it is preferable to set it to 0.6 times or more, and from the viewpoint of the cost of the coupling agent, it is preferable to couple the polymer terminals with each other to obtain a branched conjugated diene polymer component in order to improve processability, and it is preferable to set it to 3.0 times or less.

[0130] The number of moles of the polymerization initiator is preferably 3.0 times or more, more preferably 4.0 times or more, by mole relative to the number of moles of the coupling agent having a nitrogen atom-containing group represented by the formula (A).

[0131] Coupling agents having a nitrogen atom-containing group represented by formula (B) include, but are not limited to, tris(3-trimethoxysilylpropyl)amine, tris(3-methyldimethoxysilylpropyl)amine, tris(3-triethoxysilylpropyl)amine, tris(3-methyldiethoxysilylpropyl)amine, tris(trimethoxysilylmethyl)amine, tris(2-trimethoxysilylethyl)amine, and tris(4-trimethoxysilylbutyl)amine.

[0132] Among these, from the viewpoint of reactivity and interaction between the functional group of the coupling agent and an inorganic filler such as silica, and from the viewpoint of processability, it is preferable that n, m, and 1 in the formula (B) all represent 3. Preferable specific examples include tris(3-trimethoxysilylpropyl)amine and tris(3-triethoxysilylpropyl)amine.

[0133] The reaction temperature, reaction time, and the like when reacting the coupling agent having the nitrogen atom-containing group represented by the formula (B) with the active terminal of the conjugated diene polymer obtained in the branching step are not particularly limited, but it is preferable to react at 0° C. or higher and 120° C. or lower for 30 seconds or longer.

[0134] The total number of moles of alkoxy groups bonded to silyl groups in the coupling agent compound represented by formula (B) is preferably in the range of 0.6 to 3.0 times the number of moles of lithium constituting the above-mentioned polymerization initiator, more preferably in the range of 0.8 to 2.5 times, and even more preferably in the range of 0.8 to 2.0 times. In order to obtain a sufficient modification rate, molecular weight, and branched structure in the branched conjugated diene polymer obtained by the production method of this embodiment, it is preferably 0.6 times or more, and in order to improve processability, it is preferable to couple the polymer terminals to each other to obtain a branched conjugated diene polymer component, and in terms of the cost of the coupling agent, it is preferably 3.0 times or less.

[0135] The number of moles of the polymerization initiator is preferably 4.0 times or more, more preferably 5.0 times or more, by mole relative to the number of moles of the coupling agent having a nitrogen atom-containing group represented by the formula (B) above.

[0136] In the above formula (C), A is preferably represented by any one of the following general formulae (II) to (V).

[0137] [ka]

[0138] (In formula (II), B 1 represents a single bond or a hydrocarbon group having 1 to 20 carbon atoms, and a represents an integer of 1 to 10. When a plurality of B1's are present, each is independent.

[0139] [ka]

[0140] (In formula (III), B 2 represents a single bond or a hydrocarbon group having 1 to 20 carbon atoms; B 3 represents an alkyl group having 1 to 20 carbon atoms, and a represents an integer of 1 to 10. 2 and B. 3 are independent of each other.)

[0141] [ka]

[0142] (In formula (IV), B 4 represents a single bond or a hydrocarbon group having 1 to 20 carbon atoms, and a represents an integer of 1 to 10. 4 are independent of each other.)

[0143] [ka]

[0144] (In formula (V), B 5 represents a single bond or a hydrocarbon group having 1 to 20 carbon atoms, and a represents an integer of 1 to 10. 5 are independent of each other.)

[0145] In the formula (C), when A is represented by formula (II), examples of the coupling agent having a nitrogen atom-containing group include, but are not limited to, tris(3-trimethoxysilylpropyl)amine, bis(3-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]amine, bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-(3-trimethoxysilylpropyl)amine, tris[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-(3-trimethoxysilylpropyl)amine, bis(3-triethoxysilylpropyl)-[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]amine, bis[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-(3-triethoxysilylpropyl)amine, tris[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]amine, tetrakis(3-trimethoxysilylpropyl)-1,3-propanediamine , tris(3-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-1,3-propanediamine, bis(3-trimethoxysilylpropyl)-bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-1,3-propanediamine, tris[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-(3-trimethoxysilylpropyl)-1,3-propanediamine, tetrakis[3-(2,2-dimethoxy-1 -aza-2-silacyclopentane)propyl]-1,3-propanediamine, tris(3-trimethoxysilylpropyl)-[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-propanediamine, bis(3-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-propanediamine, bis[3-(2,2-Dimethoxy-1-aza-2-silacyclopentane)propyl]-(3-trimethoxysilylpropyl)-[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-propanediamine, tris[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-propanediamine, tetrakis(3-triethoxysilylpropyl)-1,3-propanediamine, tris(3 -triethoxysilylpropyl)-[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-1,3-propanediamine, bis(3-triethoxysilylpropyl)-bis[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-1,3-propanediamine, tris[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-(3-triethoxysilylpropyl)-1,3-propanediamine, tetrakis[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl pyl]-1,3-propanediamine, tris(3-triethoxysilylpropyl)-[3-(1-ethoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-propanediamine, bis(3-triethoxysilylpropyl)-[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-[3-(1-ethoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-propanediamine, bis[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl yl]-(3-triethoxysilylpropyl)-[3-(1-ethoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-propanediamine, tris[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-[3-(1-ethoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-propanediamine, tetrakis(3-trimethoxysilylpropyl)-1,3-bisaminomethylcyclohexane, tris(3-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-1,3-bisaminomethylcyclohexane, bis(3-trimethoxysilylpropyl)-bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-1,3-bisaminomethylcyclohexane, tris[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-(3-trimethoxysilylpropyl)-1,3-bisaminomethylcyclohexane, tetrakis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane )propyl]-1,3-propanediamine, tris(3-trimethoxysilylpropyl)-[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-bisaminomethylcyclohexane, bis(3-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-bisaminomethylcyclohexane, bis[3-(2,2-dimethoxy -1-aza-2-silacyclopentane)propyl]-(3-trimethoxysilylpropyl)-[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-bisaminomethylcyclohexane, tris[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-bisaminomethylcyclohexane, tetrakis(3-triethoxysilylpropyl)-1,3-propane Diamine, tris(3-triethoxysilylpropyl)-[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-1,3-bisaminomethylcyclohexane, bis(3-triethoxysilylpropyl)-bis[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-1,3-bisaminomethylcyclohexane, tris[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-(3-triethoxysilylpropyl)-1,3-propanediamine, tetrakis[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-1,3-propanediamine, tris(3-triethoxysilylpropyl)-[3-(1-ethoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-bisaminomethylcyclohexane, bis(3-triethoxysilylpropyl)-[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-[3-(1-ethoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-bisaminomethylcyclohexane, bis[3-(2,2-diethoxy-1-aza-2-silacyclo pentane)propyl]-(3-triethoxysilylpropyl)-[3-(1-ethoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-bisaminomethylcyclohexane, tris[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-[3-(1-ethoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-bisaminomethylcyclohexane, tetrakis(3-trimethoxysilylpropyl)-1,6-hexamethylenediamine, and pentakis(3-trimethoxysilylpropyl)-diethylenetriamine.

[0146] In the formula (C), when A is represented by formula (III), examples of the coupling agent having a nitrogen atom-containing group include, but are not limited to, tris(3-trimethoxysilylpropyl)-methyl-1,3-propanediamine, bis(2-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-methyl-1,3-propanediamine, bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-(3-trimethoxysilylpropyl)-methyl-1,3-propanediamine, tris(3-triethoxysilylpropyl)-methyl-1,3-propanediamine, bis(2-triethoxysilylpropyl)-[3-(2,2- diethoxy-1-aza-2-silacyclopentane)propyl]-methyl-1,3-propanediamine, bis[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-(3-triethoxysilylpropyl)-methyl-1,3-propanediamine, N1,N1'-(propane-1,3-diyl)bis(N1-methyl-N3,N3-bis(3-(trimethoxysilyl)propyl)-1,3-propanediamine), and N1-(3-(bis(3-(trimethoxysilyl)propyl)amino)propyl)-N1-methyl-N3-(3-(methyl(3-(trimethoxysilyl)propyl)amino)propyl)-N3-(3-(trimethoxysilyl)propyl)-1,3-propanediamine.

[0147] In the formula (C), when A is represented by formula (IV), examples of the coupling agent having a nitrogen atom-containing group include, but are not limited to, tetrakis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]silane, tris[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-(3-trimethoxysilylpropyl)silane, tris[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-(3-trimethoxysilylpropyl)silane, silane, bis(3-trimethoxysilylpropyl)-bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]silane, (3-trimethoxysilyl)-[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)-bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]silane silane, bis[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)-bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]silane, tris(3-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]silane, bis(3-trimethoxysilylpropyl)-[3-(1-methoxy-2-trimethylsilyl-1-silane bis[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-bis(3-trimethoxysilylpropyl)silane, and bis(3-trimethoxysilylpropyl)-bis[3-(1-methoxy-2-methyl-1-sila-2-azacyclopentane)propyl]silane.

[0148] In the formula (C) above, when A is represented by formula (V), examples of the coupling agent having a nitrogen atom-containing group include, but are not limited to, 3-tris[2-(2,2-dimethoxy-1-aza-2-silacyclopentane)ethoxy]silyl-1-(2,2-dimethoxy-1-aza-2-silacyclopentane)propane and 3-tris[2-(2,2-dimethoxy-1-aza-2-silacyclopentane)ethoxy]silyl-1-trimethoxysilylpropane.

[0149] In the formula (C), A is preferably represented by formula (II) or formula (III), and k is 0.

[0150] Coupling agents having such a nitrogen atom-containing group tend to be easily available, and when the branched conjugated diene polymer obtained by the production method of this embodiment is vulcanized, the abrasion resistance and low hysteresis loss performance tend to be superior. Coupling agents having such a nitrogen atom-containing group include, but are not limited to, bis(3-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]amine, tris(3-trimethoxysilylpropyl)amine, tris(3-triethoxysilylpropyl)amine, tris(3-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-1,3-propanediamine, tetrakis ... tetrakis(3-trimethoxysilylpropyl)-1,3-propanediamine, tetrakis(3-trimethoxysilylpropyl)-1,3-propanediamine, tetrakis(3-trimethoxysilylpropyl)-1,3-bisaminomethylcyclohexane, tris(3-trimethoxysilylpropyl)-methyl-1,3-propanediamine, and bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-(3-trismethoxysilylpropyl)-methyl-1,3-propanediamine.

[0151] In the formula (C), it is more preferable that A is represented by formula (II) or formula (III), k is 0, and a is an integer of 2 to 10 in formula (II) or formula (III). This tends to result in better abrasion resistance and low hysteresis loss performance when vulcanized. Examples of coupling agents having such a nitrogen atom-containing group include, but are not limited to, tetrakis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-1,3-propanediamine, tetrakis(3-trimethoxysilylpropyl)-1,3-propanediamine, tetrakis(3-trimethoxysilylpropyl)-1,3-bisaminomethylcyclohexane, and N1-(3-(bis(3-(trimethoxysilyl)propyl)amino)propyl)-N1-methyl-N3-(3-(methyl(3-(trimethoxysilyl)propyl)amino)propyl)-N3-(3-(trimethoxysilyl)propyl)-1,3-propanediamine.

[0152] The amount of the compound represented by formula (C) added as a coupling agent having a nitrogen atom-containing group can be adjusted so that the moles of the conjugated diene polymer to the moles of the coupling agent react in a desired stoichiometric ratio, which tends to achieve a desired highly branched star structure.

[0153] The number of moles of the polymerization initiator is preferably 5.0 times or more, more preferably 6.0 times or more, by mole relative to the number of moles of the coupling agent having a nitrogen atom-containing group represented by the above formula (C).

[0154] In this case, in formula (C), the number of functional groups of the coupling agent ((m-1)xi+pxj+k) is preferably an integer of 5-10, and more preferably an integer of 6-10.

[0155] In the branched conjugated diene polymer obtained by the production method of this embodiment, the proportion of the polymer having a nitrogen atom-containing group in the polymer is represented by a modification rate. The modification rate is preferably 60% by mass or more, more preferably 65% ​​by mass or more, even more preferably 70% by mass or more, still more preferably 75% by mass or more, still more preferably 80% by mass or more, and particularly preferably 82% by mass or more. By setting the modification rate to 60% by mass or more, the processability when vulcanized is excellent, and the vulcanized product tends to have better abrasion resistance and low hysteresis loss performance.

[0156] <Polymerization termination step> In the method for producing a branched conjugated diene polymer of the present embodiment, a reaction step can be carried out in which the above-mentioned coupling agent or polymerization terminator is reacted with the active terminal of the conjugated diene polymer obtained through the above-mentioned polymerization step and branching step. As the polymerization terminating step, for example, a polymerization terminating step performed using a bifunctional reactive compound on the active terminal of the conjugated diene polymer, or a polymerization terminating step performed using a polymerization terminating agent having a nitrogen atom-containing group (hereinafter, these may be collectively referred to as "polymerization terminating agent") is preferable.

[0157] In the polymerization terminating step, for example, the active terminal of the polymer obtained in the branching step described above is subjected to a polymerization terminating reaction with a bifunctional reactive compound or a polymerization terminator having a nitrogen atom-containing group, to obtain the target branched conjugated diene-based polymer.

[0158] [Bifunctional reactive compounds] In the method for producing a branched conjugated diene-based polymer of the present embodiment, the bifunctional reactive compound used in the polymerization termination step may have any structure, but is preferably a bifunctional reactive compound having a silicon atom.

[0159] [Polymerization terminator having nitrogen atom-containing group] In the method for producing a branched conjugated diene polymer of the present embodiment, the polymerization terminator having a nitrogen atom-containing group used in the polymerization termination step may have any structure, but preferably has a functional group that reacts with the conjugated diene polymer.

[0160] As the polymerization terminator having a nitrogen atom-containing group, from the viewpoint of improving fuel efficiency performance, an alkoxy compound having a nitrogen atom-containing group is preferred. Examples of the polymerization terminator having a nitrogen atom-containing group include 3-(N,N-dimethylaminopropyl)dimethoxymethylsilane, 3-(N,N-diethylaminopropyl)dimethoxymethylsilane, 3-(N,N-dipropylaminopropyl)dimethoxymethylsilane, 3-(N,N-dimethylaminopropyl)diethoxymethylsilane, 3-(N,N-diethylaminopropyl)diethoxymethylsilane, 3-(N,N-dipropylaminopropyl)diethoxymethylsilane, 3-(N,N-dimethylaminopropyl)dimethoxyethylsilane, 3-(N,N-diethylaminopropyl)dimethoxyethylsilane, 3-(N,N-dipropylaminopropyl)dimethoxyethylsilane, 3-(N,N-dimethylaminopropyl)diethoxyethylsilane, 3-(N,N-diethylaminopropyl)diethoxyethylsilane, 3-(N,N-dipropylaminopropyl)diethoxyethylsilane, and the like.

[0161] The branched conjugated diene polymer obtained by the production method of this embodiment through the above-mentioned polymerization step, branching step, and reaction step has a branched structure of preferably 8 to 36 branches, more preferably 10 to 24 branches, and even more preferably 12 to 20 branches. The total number of branching points in the branched conjugated diene polymer obtained by the production method of this embodiment is preferably 2 or more, more preferably 3 or more, even more preferably 4 or more, and even more preferably 5 or more. When the branched structure and the total number of branching points are within the above ranges, the processability, fuel economy, and abrasion resistance tend to be excellent. In order to construct a branched conjugated diene polymer having a branched structure with 8 to 36 branches and, in the case of a modified polymer, a total number of branching points of 2 to 15, it is necessary to use a branching agent with a molar ratio of 1 / 2 or less and 1 / 100 or more of that of the polymerization initiator, and a coupling agent with 3 or more functional groups. In the case of a polymer that does not require modification, the branching point may be 1 or more. In order to construct a branched structure having 8 to 36 branches and a total number of branching points of 3 to 12, it is preferable to use a branching agent having a molar ratio of 1 / 3 or less and 1 / 50 or more of the polymerization initiator and a coupling agent having 4 or more functional groups. In order to construct a branched structure having 10 to 24 branches and a total number of branching points of 4 to 10, it is preferable to use a branching agent having a molar ratio of 1 / 6 or less and 1 / 25 or more of the polymerization initiator and a coupling agent having 5 or more functional groups. In order to construct a branched structure having 12 to 20 branches and a total number of branching points of 5 to 9, it is preferable to use a branching agent having a molar ratio of 1 / 8 or less and 1 / 12 or more of that of the polymerization initiator and a coupling agent having 6 or more functional groups.

[0162] (Condensation reaction process) In the method for producing a branched conjugated diene polymer of the present embodiment, a condensation reaction step of carrying out a condensation reaction in the presence of a condensation promoter may be carried out after the above-mentioned coupling step or before the coupling step.

[0163] (Hydrogenation process) In the method for producing a branched conjugated diene polymer of the present embodiment, a hydrogenation step of hydrogenating the conjugated diene portion may be carried out. The method for hydrogenating the conjugated diene portion of the conjugated diene polymer is not particularly limited, and any known method can be used. A suitable hydrogenation method is to blow gaseous hydrogen into a polymer solution in the presence of a catalyst. The catalyst is not particularly limited, but examples thereof include heterogeneous catalysts such as catalysts in which precious metals are supported on porous inorganic materials; catalysts in which salts of nickel, cobalt, etc. are solubilized and reacted with organoaluminum, etc.; and homogeneous catalysts such as catalysts using metallocenes such as titanocene. Among these, titanocene catalysts are preferred from the viewpoint of being able to select mild hydrogenation conditions. Hydrogenation of aromatic groups can also be carried out by using a catalyst supported on a precious metal.

[0164] Examples of the hydrogenation catalyst include, but are not limited to, (1) supported heterogeneous hydrogenation catalysts in which metals such as Ni, Pt, Pd, Ru, etc. are supported on carbon, silica, alumina, diatomaceous earth, etc., (2) so-called Ziegler-type hydrogenation catalysts that use transition metal salts such as organic acid salts or acetylacetone salts of Ni, Co, Fe, Cr, etc. and reducing agents such as organoaluminum, and (3) so-called organometallic complexes such as organometallic compounds of Ti, Ru, Rh, Zr, etc. Furthermore, examples of the hydrogenation catalyst include, but are not limited to, known hydrogenation catalysts described in JP-B-42-8704, JP-B-43-6636, JP-B-63-4841, JP-B-1-37970, JP-B-1-53851, JP-B-2-9041, and JP-A-8-109219. Preferred hydrogenation catalysts include a reaction mixture of a titanocene compound and a reducing organometallic compound.

[0165] (Deactivator and neutralizer addition process) In the method for producing a branched conjugated diene polymer of this embodiment, after the above-mentioned coupling step, a deactivator, a neutralizer, and the like may be added to the polymer solution, if necessary. The quenching agent is not limited to the following, but examples thereof include water; alcohols such as methanol, ethanol, isopropanol, and the like; and the like. Examples of neutralizing agents include, but are not limited to, carboxylic acids such as stearic acid, oleic acid, and versatic acid (a highly branched carboxylic acid mixture having 9 to 11 carbon atoms, with the majority having 10 carbon atoms); aqueous solutions of inorganic acids, and carbon dioxide gas.

[0166] (rubber stabilizer addition process) In the method for producing a branched conjugated diene-based polymer of the present embodiment, it is preferable to add a rubber stabilizer from the viewpoint of preventing gel formation after polymerization and improving stability during processing. The rubber stabilizer is not limited to the following ones, and known ones can be used. For example, antioxidants such as 2,6-di-tert-butyl-4-hydroxytoluene (hereinafter also referred to as "BHT"), n-octadecyl-3-(4'-hydroxy-3',5'-di-tert-butylphenol)propionate, and 2-methyl-4,6-bis[(octylthio)methyl]phenol are preferred.

[0167] (rubber softener addition process) In the method for producing a branched conjugated diene polymer of the present embodiment, from the viewpoint of further improving the productivity of the branched conjugated diene polymer and the processability when a filler or the like is blended to form a resin composition, a rubber softener can be added as necessary. The rubber softener is not particularly limited, but examples thereof include extender oil, liquid rubber, and resin. The method of adding a rubber softener to a branched conjugated diene polymer is not limited to the following, but a preferred method is to add a rubber softener to a branched conjugated diene polymer solution, mix, and remove the solvent from the resulting polymer solution containing the rubber softener.

[0168] Examples of preferred extender oils include aromatic oils, naphthenic oils, and paraffinic oils. Among these, aromatic substitute oils having a polycyclic aromatic (PCA) content of 3% by mass or less according to the IP346 method are preferred from the viewpoints of environmental safety, oil bleeding prevention, and wet grip properties. Examples of aromatic substitute oils include TDAE (Treated Distillate Aromatic Extracts), MES (Mild Extraction Solvate), and RAE (Residual Aromatic Extracts) as shown in Kautschuk Gummi Kunststoffe 52(12)799(1999). Preferred liquid rubbers include, but are not limited to, liquid polybutadiene, liquid styrene-butadiene rubber, and the like. The effects of adding liquid rubber include the ability to improve the processability of a resin composition containing a branched conjugated diene polymer and a filler, etc., and the ability to shift the glass transition temperature of the resin composition to a lower temperature, which tends to improve the abrasion resistance, low hysteresis loss, and low-temperature properties of a vulcanized product. Resins as rubber softeners include, but are not limited to, aromatic petroleum resins, coumarone-indene resins, terpene resins, rosin derivatives (including paulownia oil resins), tall oil, tall oil derivatives, rosin ester resins, natural and synthetic terpene resins, aliphatic hydrocarbon resins, aromatic hydrocarbon resins, mixed aliphatic / aromatic hydrocarbon resins, coumarin-indene resins, phenolic resins, p-tert-butylphenol-acetylene resins, phenol-formaldehyde resins, xylene-formaldehyde resins, monoolefin oligomers, diolefin oligomers, hydrogenated aromatic hydrocarbon resins, cyclic aliphatic hydrocarbon resins, hydrogenated hydrocarbon resins, hydrocarbon resins, hydrogenated paulownia oil resins, hydrogenated oil resins, esters of hydrogenated oil resins and monofunctional or polyfunctional alcohols, etc. These resins may be used alone or in combination of two or more. When hydrogenating, all unsaturated groups may be hydrogenated, or some may be left. Effects of adding a resin as a rubber softener include improving the processability of a resin composition obtained by blending a branched conjugated diene polymer with a filler or the like, tending to improve the breaking strength of a vulcanized product, and tending to improve wet skid resistance by shifting the glass transition temperature of the resin composition to a higher temperature.

[0169] The amount of the rubber softener, such as an extender oil, liquid rubber, or resin, added is not particularly limited, but is preferably 1 part by mass or more and 60 parts by mass or less, more preferably 5 parts by mass or more and 50 parts by mass or less, and even more preferably 10 parts by mass or more and 37.5 parts by mass or less, relative to 100 parts by mass of the branched conjugated diene-based polymer obtained by the production method of the present embodiment. When the rubber softener is added within the above range, the processability of a resin composition obtained by blending the branched conjugated diene-based polymer obtained by the production method of the present embodiment with a filler or the like becomes good, and the breaking strength and abrasion resistance of a vulcanizate tend to be good.

[0170] (Desolvation process) In the method for producing a branched conjugated diene polymer of the present embodiment, a known method can be used to obtain the obtained branched conjugated diene polymer from the polymer solution. The method is not particularly limited, but examples thereof include a method of separating the solvent by steam stripping or the like, filtering the polymer, and then dehydrating and drying it to obtain the polymer, a method of concentrating the polymer in a flashing tank and further devolatilizing the polymer with a vent extruder or the like, and a method of directly devolatilizing the polymer with a drum dryer or the like.

[0171] [Branched conjugated diene polymer] Hereinafter, a preferred embodiment of the branched conjugated diene polymer obtained by the method for producing a branched conjugated diene polymer of the present embodiment will be described. In a preferred embodiment of the branched conjugated diene polymer of the present embodiment, the branched conjugated diene polymer has one or more side chains in the polymer chain and has a branching degree (Bn) of 1 or more as measured by a GPC-light scattering method with a viscosity detector, the branched conjugated diene polymer contains sulfur atoms and silicon atoms, the molar ratio of the silicon atoms to the sulfur atoms is 1.05 or more and less than 10, and the Mooney viscosity measured at 100°C is 40 or more and 170 or less. The branched conjugated diene-based polymer of the present embodiment, particularly due to having the above-mentioned structure, has excellent processability when vulcanized, and when vulcanized, exhibits particularly excellent abrasion resistance and breaking strength.

[0172] A branching degree (Bn) of 1 or more as measured by GPC-light scattering method with a viscosity detector means that the polymer chain has one or more side chains. After specifying the polymer chain structure, the Mooney viscosity and the number of moles of silicon atoms relative to sulfur atoms are specified within specific ranges, and further the amount of vinyl bonds in the conjugated diene bond units and the amount of aromatic vinyl compounds are adjusted arbitrarily, whereby the glass transition temperature (hereinafter also referred to as "Tg") can be adjusted arbitrarily while maintaining processability when made into a vulcanizate. For example, by setting the amount of vinyl bonds in the conjugated diene bond units and the amount of aromatic vinyl compounds low, the Tg of the branched conjugated diene polymer decreases, and the abrasion resistance and rupture strength of the vulcanized product improve, and a rubber composition having excellent low hysteresis loss tends to be obtained. In addition, by setting the vinyl bond amount in the conjugated diene bond unit and the aromatic vinyl compound amount high, the Tg of the branched conjugated diene polymer increases, the processability when vulcanized improves, and a rubber composition having excellent wet skid resistance tends to be obtained.

[0173] (Mooney viscosity) The branched conjugated diene polymer of the present embodiment described above has one or more side chains in the polymer, has a branching degree (Bn) of 1 or more as measured by a GPC-light scattering method with a viscosity detector, and may have a branched structure in the side chain as described later. Generally, polymers with branched structures tend to have smaller molecular size compared to linear polymers with the same molecular weight. Therefore, the molecular weight of a polymer with branched structures tends to be underestimated when it is screened by molecular size and measured in terms of polystyrene using gel permeation chromatography (hereinafter also referred to as "GPC"), which is a relative comparison method with a standard polystyrene sample. In addition, the absolute molecular weight measured by the GPC-light scattering method with a viscosity detector tends to be able to accurately measure the molecular weight without being influenced by the polymer structure or interactions with the column packing material, and without being influenced by the polymer structure such as the branched structure of the conjugated diene polymer, because the molecular size is directly observed by the light scattering method and the molecular weight (absolute molecular weight) is measured, compared with the polystyrene-equivalent molecular weight determined by gel permeation chromatography (GPC). However, it is easily influenced by the detection method of the light scattering detector, and although it is effective for relative comparison under specific measurement conditions, it is difficult to identify the true structure of the conjugated diene polymer.

[0174] On the other hand, Mooney viscosity is an index showing the overall characteristics of a branched conjugated diene polymer, including information on the molecular weight, molecular weight distribution, degree of branching, and content of softener. The method for measuring Mooney viscosity is specified in ISO289, and the measurement error due to the difference in the instrument is small, so that Mooney viscosity is extremely effective in controlling the performance of the branched conjugated diene polymer. Generally, viscosity can be regarded as an alternative index to molecular weight. However, since it is difficult to accurately grasp the molecular weight of a polymer having a branched structure, the present inventors set Mooney viscosity as one of the requirements for the branched conjugated diene-based polymer of the present embodiment. The branched conjugated diene polymer of this embodiment preferably has a Mooney viscosity (hereinafter also referred to as "ML") measured at 100°C of 40 or more and 170 or less. Normally, when the ML is adjusted to a low value by decreasing the molecular weight or by adding a softener (oil, etc.), the abrasion resistance and breaking strength of the vulcanized product tend to be impaired. That is, in order to obtain a branched conjugated diene-based polymer exhibiting desired performance, it is insufficient to only control the molecular weight or the Mooney viscosity. Therefore, in this embodiment, from the viewpoint of increasing the elastic modulus of the rubber composition, the structure of the side chain of the polymer, the degree of branching, and the molar ratio of silicon atoms to sulfur atoms in the polymer are specified in addition to the Mooney viscosity, and the abrasion resistance and breaking strength of the vulcanizate are improved without impairing the processability of the rubber composition.

[0175] The branched conjugated diene polymer of the present embodiment has a Mooney viscosity measured at 100°C of preferably 40 or more and 170 or less, more preferably 50 or more and 150 or less, and even more preferably 55 or more and 130 or less, from the viewpoints of productivity of the branched conjugated diene polymer, processability when the polymer is made into a rubber composition containing a filler or the like, and abrasion resistance and breaking strength when the rubber composition is made into a vulcanizate. When the Mooney viscosity measured at 100°C is 40 or more, the abrasion resistance and breaking strength of the vulcanized product tend to be improved. On the other hand, when the Mooney viscosity measured at 100°C is 170 or less, problems in the production of the branched conjugated diene polymer are prevented, and the processability of the rubber composition containing a filler or the like tends to be good.

[0176] In the branched conjugated diene polymer of this embodiment, the Mooney viscosity can be controlled by adjusting the molecular weight as described above or by adding a predetermined amount of a rubber softener. Specifically, the above numerical range can be controlled by adding 1 part by mass or more and 60 parts by mass or less of a rubber softener described later to 100 parts by mass of the branched conjugated diene polymer. When the branched conjugated diene polymer of the present embodiment is produced by continuous polymerization, it is common to extend the branched conjugated diene polymer with oil or the like within a range that does not impair the performance of the branched conjugated diene polymer from the viewpoint of productivity in the solvent removal step. The present inventors have focused on the fact that the processability of the polymer can be appropriately controlled by specifying the physical properties in the extended and finished state rather than in the state of the polymer alone, and have considered that when a softener is added to finish the polymer, the Mooney viscosity should be specified in the state containing the softener, and have defined it as above. In measuring the Mooney viscosity, a sample of a branched conjugated diene polymer formed into a plate shape by a pressure press is set in the device, and the sample is first preheated at 100°C for 1 minute, then the rotor is rotated at 2 rpm, and the torque is measured after 4 minutes, and the measured value is regarded as the Mooney viscosity (ML (1+4) More specifically, it can be measured by the method described in the Examples below.

[0177] (Side Chain) The branched conjugated diene-based polymer of the present embodiment in the above-mentioned preferred embodiment has a branching degree (Bn) measured by a GPC-light scattering method with a viscosity detector of at least 1. This means that the polymer has a structure having one or more side chains in the polymer chain. The side chain in the branched conjugated diene polymer of the present embodiment means that there is one or more polymer chains branched from the longest polymer chain. Specifically, the side chains can be formed by a method of introducing a polymer chain into the longest polymer chain via a branching agent, which will be described later. The number of side chains in the polymer chain can be controlled to a desired value by selecting the structure and amount of the branching agent to be added, as well as the structure of the modifying agent to be described later.

[0178] The branched conjugated diene polymer of the present embodiment has one or more side chains, preferably two or more, more preferably four or more, and further preferably five or more. A branched conjugated diene polymer having the number of side chains within the above range tends to have excellent processability when vulcanized, and tends to have excellent abrasion resistance and fracture properties when vulcanized. The upper limit of the number of side chains in the branched conjugated diene polymer of the present embodiment is not particularly limited, but in terms of industrial production, it is practically 25 or less, more preferably 23 or less, and even more preferably 20 or less. For example, when the number of side chains in the polymer chain of the branched conjugated diene polymer of the present embodiment is 25 or less, a compound having an excellent balance of processability when vulcanized, abrasion resistance when vulcanized, and fracture properties, which are mutually contradictory properties, tends to be obtained. In addition, when the number of side chains in the polymer chain is one or more, the processability when vulcanized is good, and a compound having an excellent balance between fuel efficiency and wet skid resistance, which are mutually contradictory properties, when vulcanized tends to be obtained.

[0179] A structure having one or more side chains in a polymer chain has generally been formed by carrying out a coupling reaction at the end of the polymer chain to introduce a branched structure, and forming a structure in which uniform polymer chains are bonded in a star shape, starting from a coupling agent. However, when a branching agent is used to form side chains, the polymer chain length bonded to the side chain, the number of polymer chains, and the polymer chain length of the main chain can be freely adjusted by adjusting the timing of adding the branching agent, the structure of the branching agent, and the amount added, which allows for a high degree of freedom in designing the polymer structure and tends to make it easier to obtain a polymer with the desired balance of physical properties, which is preferable. The number of side chains of the branched conjugated diene polymer is the sum of the branches due to the coupling reaction at the terminals and the branches due to the branching agent, and can be appropriately set depending on the structure of the branched conjugated diene polymer to be produced, such as the Mooney viscosity, the ratio of silicon atoms to sulfur atoms, the molecular weight, the vinyl content, the aromatic vinyl content, and the like, and the production process, such as the setting of the polymerization initiator and the presence or absence of a branching process or a modification process. In this embodiment, the number of side chains theoretically determined from the type and amount of coupling agent and the type and amount of branching agent can be determined as the degree of branching (Bn) measured by a GPC-light scattering method with a viscosity detector described later.

[0180] (Conjugated diene polymer containing silicon and sulfur atoms) The branched conjugated diene-based polymer of the present embodiment in the above-mentioned preferred embodiment contains a silicon atom and a sulfur atom. The branched conjugated diene polymer of the present embodiment has a branching degree of 1 or more and contains silicon atoms and sulfur atoms, and therefore has excellent processability when vulcanized, and when vulcanized, has excellent abrasion resistance and fracture properties. From the viewpoint of the effect of making the processability excellent when vulcanized, the molar ratio of silicon atoms to sulfur atoms tends to contribute greatly. Specifically, when the molar ratio of silicon atoms to sulfur atoms (silicon atoms / sulfur atoms) is large, the amount of branching agent added is large, and the number of side chains in the polymer chain tends to be large. In this case, the processability when vulcanized tends to be excellent.

[0181] In the branched conjugated diene polymer of the above-mentioned preferred embodiment, the positions at which the silicon atoms and sulfur atoms are introduced have little effect on the properties, so that the silicon atoms and sulfur atoms may be introduced in any position. Silicon atoms can be introduced into the branched conjugated diene polymer as a branching agent residue while increasing the number of branches in the polymer by main chain branching, for example, by reacting the conjugated diene polymer with a branching agent having a silicon atom. Also, silicon atoms can be introduced into the branched conjugated diene polymer as a modifier residue by reacting the branched conjugated diene polymer with a modifier having a silicon atom. The sulfur atom can be introduced into the conjugated diene polymer as a modifier residue, for example, by reacting the conjugated diene polymer with a modifier having a sulfur atom. When a modifier having a sulfur atom is reacted with the active end of a conjugated diene polymer, a sulfur atom can be placed at the end of the polymer chain, and vulcanization can be performed at the end of the polymer chain. This reduces the number of free polymer ends from the crosslinking points, improves crosslinking efficiency, and strengthens the interface between the surface of the silica as a filler and the polymer, tending to provide a rubber composition with excellent fuel saving performance.

[0182] (molar ratio of silicon atoms to sulfur atoms) The branched conjugated diene-based polymer of the present embodiment in the above-mentioned preferred embodiment has a degree of branching of 1 or more and a structure containing silicon atoms and sulfur atoms, and the molar ratio of silicon atoms to sulfur atoms (silicon atoms / sulfur atoms) is 1.05 or more and less than 10, preferably 1.07 or more and less than 8, more preferably 1.1 or more and less than 7, and even more preferably 1.12 or more and less than 6. A branched conjugated diene polymer having a molar ratio of silicon atoms to sulfur atoms within this range tends to exhibit excellent abrasion resistance and fracture properties when vulcanized. In the case where the branching agent forming the main chain branch contains a silicon atom and the terminal modifier contains a sulfur atom, the silicon atom is derived from the total amount of the branching agent residue and the modifier residue, and the sulfur atom is derived from the modifier residue. When the molar number of silicon atoms relative to the sulfur atom is large, it indicates that the amount of the branching agent added is large, and the processability when the vulcanizate is made tends to be excellent. When the molar number of silicon atoms relative to the sulfur atom is small, it indicates that the amount of the branching agent added is small, and the wear resistance and fracture properties when the vulcanizate is made tend to be excellent. The molar ratio of silicon atoms to sulfur atoms can be controlled within the above numerical range by adjusting the types and amounts of the branching agent and the modifying agent added.

[0183] (Branching degree (Bn)) The number of side chains in the branched conjugated diene polymer of this embodiment can be expressed as the branching degree (Bn) measured by a GPC-light scattering method with a viscosity detector (hereinafter, also simply referred to as the branching degree (Bn)). In a preferred embodiment of the branched conjugated diene polymer of the present invention, that is, a branched conjugated diene polymer having the above-mentioned configuration, i.e., having one or more side chains in the polymer chain and having a branching degree (Bn) of 1 or more as measured by a GPC-light scattering method with a viscosity detector, the branched conjugated diene polymer contains sulfur atoms and silicon atoms, the molar ratio of the silicon atoms to the sulfur atoms is 1.05 or more and less than 10, and the Mooney viscosity measured at 100°C is 40 or more and 170 or less, the branching degree (Bn) as measured by a GPC-light scattering method with a viscosity detector is 1 or more, preferably 2 or more and 25 or less, and more preferably 3 or more and 20 or less, from the viewpoints of processability, abrasion resistance, and breaking strength.

[0184] For example, the degree of branching (Bn) being 4 or more means that the branched conjugated diene-based polymer of the present embodiment has substantially 4 or more side polymer chains relative to the longest polymer main chain. The branching degree (Bn) of the branched conjugated diene polymer is defined as g'=6Bn / [(Bn+1)(Bn+2)], where g' is a shrinkage factor measured by a GPC-light scattering method with a viscometer. In general, a polymer having branches tends to have a smaller molecular size when compared to a linear polymer having the same absolute molecular weight. The shrinkage factor (g') is a measure of the ratio of the molecular size to that of a linear polymer of the same assumed absolute molecular weight. In other words, the greater the degree of branching of a polymer, the smaller the shrinkage factor (g') tends to be. In this embodiment, the intrinsic viscosity is used as an index of molecular size for this shrinkage factor. For linear polymers, the intrinsic viscosity [η] is −3.883M 0.771 In the above formula, M is the absolute molecular weight. However, the shrinkage factor represents the rate of reduction in molecular size and does not accurately represent the branched structure of a polymer. Therefore, the branching degree (Bn) of the branched conjugated diene polymer is calculated using the value of the shrinkage factor (g') at each absolute molecular weight of the branched conjugated diene polymer. The calculated "branching degree (Bn)" accurately represents the number of polymers that are directly or indirectly bonded to each other with respect to the longest main chain structure. The calculated branching degree (Bn) is an index that expresses the branching structure of a branched conjugated diene polymer. For example, in the case of a typical four-branched star polymer (four polymer chains connected to the center), two polymer chain arms are bonded to the longest highly branched main chain structure, and the branching degree (Bn) is evaluated as 2.

[0185] The branched conjugated diene-based polymer of the present embodiment in the above-mentioned preferred embodiment has a branching degree (Bn) of 1 or more, preferably 2 or more and 25 or less. In such a case, it means that the modified conjugated diene-based polymer has a star polymer structure having 3 to 27 branches similar to a star polymer structure. Here, "branch" refers to a structure formed by direct or indirect bonding of one polymer to another polymer, and "degree of branching (Bn)" refers to the number of polymers that are directly or indirectly bonded to each other in the longest main chain structure. Since the branching degree (Bn) is 1 or more, preferably 2 or more and 25 or less, the branched conjugated diene-based polymer of the present embodiment has extremely excellent processability when vulcanized, and when vulcanized, has excellent abrasion resistance and breaking strength.

[0186] In general, an increase in absolute molecular weight tends to deteriorate processability. When the absolute molecular weight is increased in a linear polymer structure, the viscosity of the vulcanizate increases significantly, and processability deteriorates significantly. Therefore, even if a large number of functional groups are introduced into the polymer to improve the affinity and / or reactivity with silica blended as a filler, the silica cannot be sufficiently dispersed in the polymer during the kneading process, which causes a problem that the function of the introduced functional groups is not exerted, and the effects of low hysteresis loss and improved wet skid resistance that should be expected by the introduction of functional groups tend not to be exerted. On the other hand, the branched conjugated diene polymer of the present embodiment is specified to have a branching degree (Bn) of 1 or more, preferably 2 to 25, and thus the increase in viscosity during vulcanization associated with an increase in absolute molecular weight is significantly suppressed, and the polymer is thoroughly mixed with silica or the like in the kneading step, making it possible to disperse silica around the branched conjugated diene polymer. As a result, by setting the molecular weight of the branched conjugated diene polymer to be large, it becomes possible to improve abrasion resistance and fracture strength, and by thoroughly kneading the polymer, it becomes possible to disperse silica around the polymer and allow the functional groups to act and / or react, making it possible to provide a polymer with low hysteresis loss and wet skid resistance sufficient for practical use. The absolute molecular weight of the branched conjugated diene polymer can be measured by the method described in the examples below. The degree of branching (Bn) of the branched conjugated diene polymer of the present embodiment can be controlled to a desired value by adjusting the type and amount of the branching agent described below.

[0187] (Side chain structure) The branched conjugated diene polymer of the present embodiment preferably has a portion derived from a vinyl monomer containing an alkoxysilyl group or a halosilyl group in a part of the polymer chain, and the portion derived from the vinyl monomer containing an alkoxysilyl group or a halosilyl group preferably has a side chain. The side chain has one or more branching points, preferably three or more branching points, and more preferably four or more branching points, at a branching point derived from a vinyl monomer containing an alkoxysilyl group or a halosilyl group. In addition, the branch point forming the side chain preferably has at least one polymer chain, more preferably has two or more polymer chains that are not the main chain, and even more preferably has four or more polymer chains that are not the main chain. In particular, in the case of a main chain branched structure consisting of a vinyl monomer containing an alkoxysilyl group or a halosilyl group, when signal detection is performed by 29Si-NMR, a peak derived from the main chain branched structure is detected in the range of -45 ppm to -65 ppm, more specifically in the range of -50 ppm to -60 ppm.

[0188] A preferred embodiment of the branched conjugated diene polymer of the present embodiment is a structure in which a terminal of a polymer chain is modified with a modifying agent containing a sulfur atom, a part of the polymer chain has a portion derived from a vinyl monomer containing an alkoxysilyl group or a halosilyl group, and the portion derived from the vinyl monomer containing an alkoxysilyl group or a halosilyl group has a further main chain branched structure. A method for obtaining a branched conjugated diene polymer having the above-mentioned structure includes, for example, a method in which an organolithium compound is used as a polymerization initiator to carry out polymerization, a branching agent that provides a specific branching point is added during or after polymerization, and the polymerization is continued, followed by modification with a sulfur atom-containing modifier that provides a specific branching rate. In this case, the modifying group can be controlled by adjusting the number of functional groups and the amount added of the sulfur-containing modifier, and the main chain branched structure can be controlled by adjusting the number of functional groups, the amount added, and the timing of addition of the branching agent. Such means for controlling the polymerization conditions will be described in the production method in the examples given below.

[0189] (Details of side chain structure) In the branched conjugated diene polymer of the present embodiment, the portion derived from the vinyl monomer containing an alkoxysilyl group or a halosilyl group is preferably a monomer unit based on a compound represented by the following formula (4) or (5), and the polymer chain preferably has a branching point due to the monomer unit based on a compound represented by the following formula (4) or (5). Moreover, the branched conjugated diene polymer of the present embodiment is more preferably a branched conjugated diene polymer obtained by using a coupling agent, and further preferably a modified conjugated diene polymer in which at least one end of the conjugated diene polymer is modified with a sulfur atom-containing group.

[0190] [ka]

[0191] [ka]

[0192] (In formula (4), R 1 represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, or an aryl group having 6 to 20 carbon atoms, which may partially have a branched structure. R 2 ~R 3 each independently represents an alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 20 carbon atoms, which may partially have a branched structure. R when multiple exist 1 ~R 3 are each independent. X 1 represents an independent halogen atom. m represents an integer of 0 to 2, n represents an integer of 0 to 3, and l represents an integer of 0 to 3. (m+n+l) represents 3.) (In formula (5), R 2 ~R 5 Each of R independently represents an alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 20 carbon atoms, and may partially have a branched structure. 2 ~R 5 are each independent. X 2 ~X 3 represents an independent halogen atom. m represents an integer of 0 to 2, n represents an integer of 0 to 3, and l represents an integer of 0 to 3. (m+n+l) represents 3. a represents an integer of 0 to 2, b represents an integer of 0 to 3, and c represents an integer of 0 to 3. (a+b+c) represents 3.)

[0193] The branched conjugated diene polymer of the present embodiment is represented by the formula (4) above, R 1 is a hydrogen atom and m = 0. This increases the number of branches, and provides the effect of improving abrasion resistance and processability.

[0194] In addition, the branched conjugated diene polymer of the present embodiment is preferably a branched conjugated diene polymer having a monomer unit based on the compound represented by formula (5), in which m = 0 and b = 0. This provides an effect of improving abrasion resistance and processability.

[0195] In addition, the branched conjugated diene polymer of the present embodiment is preferably a branched conjugated diene polymer having monomer units based on the compound represented by formula (5), in which m = 0, l = 0, n = 3, a = 0, b = 0, and c = 3. This provides the effect of improving abrasion resistance and processability.

[0196] In addition, the branched conjugated diene polymer of the present embodiment is a polymer represented by the formula (4), 1 It is more preferable that the polymer is a branched conjugated diene-based polymer having monomer units based on the compound represented by formula (4) in which m is a hydrogen atom, m is 0, l is 0, and n is 3. This improves the modification rate and the degree of branching, and provides the effects of improving fuel saving performance, abrasion resistance, and processability.

[0197] (Branching Agent) In the branched conjugated diene polymer of the present embodiment, when constructing a main chain branched structure, it is preferable to use a branching agent represented by the following formula (4) or formula (5) as a branching agent. The portion derived from the vinyl monomer containing an alkoxysilyl group or a halosilyl group is a monomer unit based on a compound represented by the following formula (4) or (5), and the branched conjugated diene polymer of the present embodiment preferably has a structure having a polymer chain branching point due to a monomer unit based on a compound represented by the following formula (4) or (5).

[0198] [ka]

[0199] [ka]

[0200] (In formula (4), R 1 represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, or an aryl group having 6 to 20 carbon atoms, which may partially have a branched structure. R 2 ~R 3 each independently represents an alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 20 carbon atoms, which may partially have a branched structure. R when multiple exist 1 ~R 3 are each independent. X 1 represents an independent halogen atom. m represents an integer of 0 to 2, n represents an integer of 0 to 3, and l represents an integer of 0 to 3. (m+n+l) represents 3.) (In formula (5), R 2 ~R 5 Each of R independently represents an alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 20 carbon atoms, and may partially have a branched structure. 2 ~R 5 are each independent. X 2 ~X 3 represents an independent halogen atom. m represents an integer of 0 to 2, n represents an integer of 0 to 3, and l represents an integer of 0 to 3. (m+n+l) represents 3. a represents an integer of 0 to 2, b represents an integer of 0 to 3, and c represents an integer of 0 to 3. (a+b+c) represents 3.)

[0201] The branching agent used in constructing the main chain branched structure of the branched conjugated diene polymer of the present embodiment is preferably a branching agent represented by formula (4) R 1 is a hydrogen atom and m=0.

[0202] In the present embodiment, the branching agent used in constructing the main chain branched structure of the branched conjugated diene polymer is preferably a compound in which m=0 and b=0 in formula (5), from the viewpoint of improving the degree of branching.

[0203] In the present embodiment, the branching agent used in constructing the main chain branched structure of the branched conjugated diene polymer is, from the viewpoints of continuity of polymerization and improvement of the modification rate and the branching degree, R 1 is a hydrogen atom, m=0, l=0, and n=3.

[0204] In the present embodiment, the branching agent used in constructing the main chain branched structure of the branched conjugated diene polymer is preferably a compound in which m=0, l=0, n=3, a=0, b=0, and c=3 in the above formula (5), from the viewpoint of improving the modification rate and the degree of branching.

[0205] Examples of the branching agent represented by the formula (4) include, but are not limited to, trimethoxy(4-vinylphenyl)silane, triethoxy(4-vinylphenyl)silane, tripropoxy(4-vinylphenyl)silane, tributoxy(4-vinylphenyl)silane, triisopropoxy(4-vinylphenyl)silane, trimethoxy(3-vinylphenyl)silane, triethoxy(3-vinylphenyl)silane, tripropoxy(3-vinylphenyl)silane, tributoxy(3-vinylphenyl)silane, triisopropoxy(3-vinylphenyl)silane, (2-vinylphenyl)silane, trimethoxy(2-vinylphenyl)silane, triethoxy(2-vinylphenyl)silane, tripropoxy(2-vinylphenyl)silane, tributoxy(2-vinylphenyl)silane, triisopropoxy(2-vinylphenyl)silane, dimethoxymethyl(4-vinylphenyl)silane, diethoxymethyl(4-vinylphenyl)silane, dipropoxymethyl(4-vinylphenyl)silane, dibutoxymethyl(4-vinylphenyl)silane, diisopropoxymethyl(4-vinylphenyl)silane, dimethoxymethyl methyl(3-vinylphenyl)silane, diethoxymethyl(3-vinylphenyl)silane, dipropoxymethyl(3-vinylphenyl)silane, dibutoxymethyl(3-vinylphenyl)silane, diisopropoxymethyl(3-vinylphenyl)silane, dimethoxymethyl(2-vinylphenyl)silane, diethoxymethyl(2-vinylphenyl)silane, dipropoxymethyl(2-vinylphenyl)silane, dibutoxymethyl(2-vinylphenyl)silane, diisopropoxymethyl(2-vinylphenyl)silane, dimethylmethoxy(4-vinylphenyl)silane, phenyl)silane, dimethylethoxy(4-vinylphenyl)silane, dimethylpropoxy(4-vinylphenyl)silane, dimethylbutoxy(4-vinylphenyl)silane, dimethylisopropoxy(4-vinylphenyl)silane, dimethylmethoxy(3-vinylphenyl)silane, dimethylethoxy(3-vinylphenyl)silane, dimethylpropoxy(3-vinylphenyl)silane, dimethylbutoxy(3-vinylphenyl)silane, dimethylisopropoxy(3-vinylphenyl)silane, dimethylmethoxy(2-vinylphenyl)silane,Dimethylethoxy(2-vinylphenyl)silane, dimethylpropoxy(2-vinylphenyl)silane, dimethylbutoxy(2-vinylphenyl)silane, dimethylisopropoxy(2-vinylphenyl)silane, trimethoxy(4-isopropenylphenyl)silane, triethoxy(4-isopropenylphenyl)silane, tripropoxy(4-isopropenylphenyl)silane, tributoxy(4-isopropenylphenyl)silane, triisopropoxy(4-isopropenylphenyl)silane, trimethoxy(3-isopropenylphenyl)silane )silane, triethoxy(3-isopropenylphenyl)silane, tripropoxy(3-isopropenylphenyl)silane, tributoxy(3-isopropenylphenyl)silane, triisopropoxy(3-isopropenylphenyl)silane, trimethoxy(2-isopropenylphenyl)silane, triethoxy(2-isopropenylphenyl)silane, tripropoxy(2-isopropenylphenyl)silane, tributoxy(2-isopropenylphenyl)silane, triisopropoxy(2-isopropenylphenyl)silane, dimethoxymethyl (4-isopropenylphenyl)silane, diethoxymethyl(4-isopropenylphenyl)silane, dipropoxymethyl(4-isopropenylphenyl)silane, dibutoxymethyl(4-isopropenylphenyl)silane, diisopropoxymethyl(4-isopropenylphenyl)silane, dimethoxymethyl(3-isopropenylphenyl)silane, diethoxymethyl(3-isopropenylphenyl)silane, dipropoxymethyl(3-isopropenylphenyl)silane, dibutoxymethyl(3-isopropenylphenyl)silane, diisoprop methoxymethyl(3-isopropenylphenyl)silane, dimethoxymethyl(2-isopropenylphenyl)silane, diethoxymethyl(2-isopropenylphenyl)silane, dipropoxymethyl(2-isopropenylphenyl)silane, dibutoxymethyl(2-isopropenylphenyl)silane, diisopropoxymethyl(2-isopropenylphenyl)silane, dimethylmethoxy(4-isopropenylphenyl)silane, dimethylethoxy(4-isopropenylphenyl)silane, dimethylpropoxy(4-isopropenylphenyl)silane,Dimethylbutoxy(4-isopropenylphenyl)silane, Dimethylisopropoxy(4-isopropenylphenyl)silane, Dimethylmethoxy(3-isopropenylphenyl)silane, Dimethylethoxy(3-isopropenylphenyl)silane, Dimethylpropoxy(3-isopropenylphenyl)silane, Dimethylbutoxy(3-isopropenylphenyl)silane, Dimethylisopropoxy(3-isopropenylphenyl)silane, Dimethylmethoxy(2-isopropenylphenyl)silane, Dimethylethoxy(2-isopropenylphenyl)silane, Dimethylpropoxy(2-isopropenylphenyl)silane, Dimethylbutoxy(2-isopropenylphenyl)silane, Dimethylisopropoxy(2-isopropenylphenyl)silane, Trichloro(4-vinylphenyl)silane, Trichloro(3 -vinylphenyl)silane, trichloro(2-vinylphenyl)silane, tribromo(4-vinylphenyl)silane, tribromo(3-vinylphenyl)silane, tribromo(2-vinylphenyl)silane, dichloromethyl(4-vinylphenyl)silane, dichloromethyl(3-vinylphenyl)silane, dichloromethyl(2-vinylphenyl)silane, dibromomethyl(4-vinylphenyl)silane, dibromomethyl(3-vinylphenyl)silane, dibromomethyl(2-vinylphenyl)silane, dimethylchloro(4-vinylphenyl)silane, dimethylchloro(3-vinylphenyl)silane, dimethylchloro(2-vinylphenyl)silane, dimethylbromo(4-vinylphenyl)silane, dimethylbromo(3-vinylphenyl)silane, and dimethylbromo(2-vinylphenyl)silane.

[0206] Among these, trimethoxy(4-vinylphenyl)silane, triethoxy(4-vinylphenyl)silane, tripropoxy(4-vinylphenyl)silane, tributoxy(4-vinylphenyl)silane, triisopropoxy(4-vinylphenyl)silane, trimethoxy(3-vinylphenyl)silane, triethoxy(3-vinylphenyl)silane, tripropoxy(3-vinylphenyl)silane, tributoxy(3-vinylphenyl)silane, triisopropoxy(3-vinylphenyl)silane, and trichloro(4-vinylphenyl)silane are preferred, and trimethoxy(4-vinylphenyl)silane, triethoxy(4-vinylphenyl)silane, tripropoxy(4-vinylphenyl)silane, tributoxy(4-vinylphenyl)silane, and triisopropoxy(4-vinylphenyl)silane are more preferred.

[0207] The branching agent represented by the formula (5) is not limited to the following, but examples thereof include 1,1-bis(4-trimethoxysilylphenyl)ethylene, 1,1-bis(4-triethoxysilylphenyl)ethylene, 1,1-bis(4-tripropoxysilylphenyl)ethylene, 1,1-bis(4-tripentoxysilylphenyl)ethylene, 1,1-bis(4-triisopropoxysilylphenyl)ethylene, 1,1-bis(3-trimethoxysilylphenyl)ethylene, 1,1-bis(3-triethoxysilylphenyl)ethylene, 1,1-bis(3-tripoxysilylphenyl)ethylene, 1,1-bis(3-tripentoxysilylphenyl)ethylene, 1,1-bis(3-triisopropoxysilylphenyl)ethylene, 1,1-bis(2 -trimethoxysilylphenyl)ethylene, 1,1-bis(2-triethoxysilylphenyl)ethylene, 1,1-bis(3-tripropoxysilylphenyl)ethylene, 1,1-bis(2-tripentoxysilylphenyl)ethylene, 1,1-bis(2-triisopropoxysilylphenyl)ethylene, 1,1-bis(4-(dimethylmethoxysilyl)phenyl)ethylene, 1,1-bis(4-(diethylmethoxysilyl)phenyl)ethylene, 1,1-bis(4-(dipropylmethoxysilyl)phenyl)ethylene, 1,1-bis(4-(dimethylethoxysilyl)phenyl)ethylene, 1,1-bis(4-(diethylethoxysilyl)phenyl)ethylene, and 1,1-bis(4-(dipropylethoxysilyl)phenyl)ethylene.

[0208] Among these, 1,1-bis(4-trimethoxysilylphenyl)ethylene, 1,1-bis(4-triethoxysilylphenyl)ethylene, 1,1-bis(4-tripropoxysilylphenyl)ethylene, 1,1-bis(4-tripentoxysilylphenyl)ethylene, and 1,1-bis(4-triisopropoxysilylphenyl)ethylene are preferred, with 1,1-bis(4-trimethoxysilylphenyl)ethylene being more preferred.

[0209] (Modifier) In the branched conjugated diene polymer of the present embodiment, as a preferred embodiment, the branched conjugated diene polymer contains a sulfur atom and a silicon atom. The branched conjugated diene-based polymer of the present embodiment is preferably modified with a predetermined modifying agent, and the modifying agent used in the modification step is preferably a compound having a sulfur atom, more preferably a compound having a silicon atom and a sulfur atom. The branched conjugated diene polymer containing silicon atoms and sulfur atoms of the present embodiment can be obtained, for example, by reacting a branched conjugated diene polymer with a modifier containing silicon atoms and sulfur atoms described below. The branched conjugated diene polymer of the present embodiment is more preferably a branched conjugated diene polymer obtained by subjecting an active terminal of a branched conjugated diene polymer obtained through a polymerization and branching step to a modification reaction using a reactive compound containing a silicon atom and a sulfur atom.

[0210] A branched conjugated diene polymer modified with a modifier containing silicon atoms and sulfur atoms is made into a rubber composition blended with a filler such as silica, and when the rubber composition is vulcanized, the number of free polymer ends from the crosslinking points decreases, crosslinking efficiency improves, and the interface between the silica surface as a filler and the polymer becomes strong, which tends to result in excellent fuel economy performance. That is, the branched conjugated diene-based polymer modified with the above-mentioned modifier has good dispersibility of silica, and the rubber composition containing a filler or the like has good processability, and when the rubber composition is vulcanized, the abrasion resistance and breaking strength tend to be good.

[0211] The modifying agent containing silicon atoms and sulfur atoms is not limited, but is preferably, for example, a sulfide group-containing alkoxysilane compound, and more preferably, a compound having a silane sulfide structure in which the sulfide group is substituted with an alkylsilane compound. In the silane sulfide structure in which the sulfide group is replaced by an alkylsilane compound, the alkoxysilane is eliminated to form a thiol group in the solvent removal step described below. When a rubber composition is made by compounding a filler such as silica, the generated thiol group has an increased interaction with the silica, which improves the dispersion of the silica in the polymer, improving the fuel saving performance and improving the processability. In addition, when the rubber composition is vulcanized, the ends of the polymer chains are crosslinked by the sulfur atoms introduced at the ends of the polymer chains, which reduces the number of free polymer ends from the crosslinking points and improves crosslinking efficiency, which tends to result in excellent abrasion resistance and fracture properties when the rubber composition is vulcanized.

[0212] The modifying agent containing a silicon atom and a sulfur atom is preferably a silane sulfide compound represented by the following formula (3), and the branched conjugated diene-based polymer of the present embodiment is preferably modified with the silane sulfide compound represented by the following formula (3).

[0213] [ka]

[0214] (In formula (3), Si represents a silicon atom, O represents an oxygen atom, and S represents a sulfur atom. x is an integer of 1 to 3, y is 0 or an integer of 1 to 2, and x+y is 3. R 1 , R 2 , R 4 may be the same or different and represent an alkyl group having 1 to 16 carbon atoms; R 3 represents an aryl group having 6 to 16 carbon atoms, an alkylene group having 1 to 16 carbon atoms, or an alkyl chain having 1 to 16 carbon atoms.

[0215] Specific examples of the silane sulfide compound represented by the formula (3) are as described above.

[0216] (Coupling Agent) In the above-mentioned preferred embodiment, the branched conjugated diene-based polymer of the present embodiment is preferably coupled with a coupling agent comprising at least one compound selected from the group consisting of tin halides, tin alkoxides, silicon halides, and alkoxysilanes. The branched conjugated diene-based polymer of the present embodiment may be in the form of a branched conjugated diene-based polymer composition partially containing the above-mentioned coupled polymer, or may be entirely coupled.

[0217] The coupling agent may have only a coupling function, or may also have a modifying function of introducing sulfur and / or silicon into the polymer. When the coupling agent does not contain silicon and / or sulfur, from the viewpoint of controlling the physical properties of a rubber composition containing a filler such as silica, it is preferable to modify a part of the polymer with the above-mentioned modifier and further add a coupling agent to adjust the molecular weight and / or branching degree of the remaining unmodified conjugated diene polymer. A branched conjugated diene polymer to which a coupling agent has been added has a high ratio of high molecular weight components, and tends to have excellent abrasion resistance and fracture properties when vulcanized.

[0218] The coupling agent is selected from the group consisting of tin halides, tin alkoxides, silicon halides, and alkoxysilanes. These coupling agents may be used alone or in combination of two or more. In the present embodiment, the preferred amount of the coupling agent to be added is, in terms of the number of moles of the functional group of the coupling agent relative to the number of moles of the polymerization initiator involved in the polymerization (hereinafter referred to as the number of equivalents), 0 or more and 0.6 or less equivalents, more preferably 0.1 or more and 0.5 or less equivalents, and even more preferably 0.2 or more and 0.4 or less equivalents. In the case of a coupling agent that is a tin halide compound or a silicon halide compound, the number of functional groups is the number of moles of halogen. In the case of tin alkoxide compounds and alkoxysilane compounds, generally, all alkoxy groups bonded to tin atoms and silicon atoms tend not to react, and one alkoxy group remains per tin atom or silicon atom. Therefore, the number of functional groups of tin alkoxide compounds and alkoxysilane compounds is the number of alkoxy groups bonded to the same tin atom or silicon atom minus 1. More specifically, the number of functional groups of the coupling agent is calculated by assuming that tetraalkoxytin (silyl) compounds are trifunctional, trialkoxytin (silyl) compounds are bifunctional, dialkoxytin (silyl) compounds are monofunctional, and monoalkoxysilyl groups are 0 functional.

[0219] Examples of the tin halide compound that is a coupling agent include, but are not limited to, tin tetrachloride, tin tetrabromide, tin tetrafluoride, methyltrichlorostannane, tris(trimethylsiloxy)chlorostannane, tris(dimethylamino)chlorostannane, hexachlorodistannane, bis(trichlorostannane)methane, 1,2-bis(trichlorostannane)ethane, 1,2-bis(methyldichlorostannane)ethane, 1,4-bis(trichlorostannane)butane, and 1,4 bis(methyldichlorostannane)butane. Examples of halogenated silicon compounds that are coupling agents include, but are not limited to, methyltrichlorosilane, tetrachlorosilane, tris(trimethylsiloxy)chlorosilane, tris(dimethylamino)chlorosilane, hexachlorodisilane, bis(trichlorosilyl)methane, 1,2-bis(trichlorosilyl)ethane, 1,2-bis(methyldichlorosilyl)ethane, 1,4-bis(trichlorosilyl)butane, and 1,4 bis(methyldichlorosilyl)butane. Examples of tin alkoxide compounds that are coupling agents include, but are not limited to, tetramethoxystannane, tetraethoxystannane, triphenoxymethylstannane, and 1,2-bis(triethoxystannane)ethane. Examples of the alkoxysilane compound that is a coupling agent include, but are not limited to, tetramethoxysilane, tetraethoxysilane, triphenoxymethylsilane, 1,2-bis(triethoxysilyl)ethane, and methoxy-substituted polyorganosiloxane.

[0220] [Branched conjugated diene polymer composition] The branched conjugated diene polymer composition of the present embodiment contains a branched conjugated diene polymer produced by the method for producing a branched conjugated diene polymer of the present embodiment described above, or a branched conjugated diene polymer having the preferred embodiment described above. That is, the branched conjugated diene polymer composition preferably contains 10% by mass or more and less than 100% by mass of a branched conjugated diene polymer which has one or more side chains in the polymer chain and has a branching degree (Bn) of 1 or more as measured by a GPC-light scattering method equipped with a viscosity detector, the branched conjugated diene polymer contains sulfur atoms and silicon atoms, the molar ratio of the silicon atoms to the sulfur atoms is 1.05 or more and less than 10, and the Mooney viscosity as measured at 100°C is 40 or more and 170 or less. By having the content of the branched conjugated diene polymer of the present embodiment in the branched conjugated diene polymer composition of the present embodiment be 10% by mass or more, the effect of excellent wear resistance and fracture properties can be obtained when the composition is made into a vulcanizate. From this viewpoint, the content of the branched conjugated diene polymer is preferably 20% by mass or more, more preferably 30% by mass or more.

[0221] The branched conjugated diene polymer composition of the present embodiment may contain, in the branched conjugated diene polymer, a coupled conjugated diene polymer obtained by the above-mentioned coupling step. Preferably, the polymer may contain a branched conjugated diene polymer coupled with at least one compound selected from the group consisting of tin halides, tin alkoxides, silicon halides, and alkoxysilanes.

[0222] The branched conjugated diene polymer composition of the present embodiment may be in an embodiment containing the branched conjugated diene polymer of the present embodiment described above and a rubber softener. In such a configuration, the rubber softener is preferably 1 to 60 parts by mass, more preferably 5 to 55 parts by mass, and even more preferably 10 to 50 parts by mass, per 100 parts by mass of the branched conjugated diene polymer, from the viewpoint of productivity in producing the branched conjugated diene polymer.

[0223] [Rubber composition and method for producing rubber composition] The rubber composition of the present embodiment contains a rubber component containing 10% by mass or more of the branched conjugated diene-based polymer produced by the production method of the present embodiment described above, and 5.0 parts by mass or more and 150 parts by mass or less of a filler per 100 parts by mass of the rubber component. The method for producing the rubber composition of the present embodiment includes the steps of obtaining a branched conjugated diene polymer by the above-described production method, obtaining a rubber component containing 10% by mass or more of the branched conjugated diene polymer, and incorporating 5.0 parts by mass or more and 150 parts by mass or less of a filler per 100 parts by mass of the rubber component. Furthermore, by containing 10% by mass or more of the branched conjugated diene polymer obtained by the production method of this embodiment in the rubber component, it is possible to improve fuel economy performance, processability, and abrasion resistance.

[0224] The filler preferably includes a silica-based inorganic filler. By dispersing a silica-based inorganic filler as a filler, the rubber composition tends to have excellent processability when vulcanized, and the vulcanized product tends to have an excellent balance between abrasion resistance, breaking strength, and low hysteresis loss and wet skid resistance. The rubber composition preferably contains a silica-based inorganic filler even when it is used for vulcanized rubber applications such as automobile parts such as tires and anti-vibration rubbers, and shoes.

[0225] The rubber composition of the present embodiment is obtained by mixing a rubber component containing 10% by mass or more of the branched conjugated diene-based polymer obtained by the above-mentioned production method with the filler. The rubber component may contain a rubber-like polymer (hereinafter simply referred to as a "rubber-like polymer") other than the above-mentioned branched conjugated diene-based polymer. Examples of such rubber-like polymers include, but are not limited to, conjugated diene polymers or hydrogenated products thereof, random copolymers of conjugated diene compounds and vinyl aromatic compounds or hydrogenated products thereof, block copolymers of conjugated diene compounds and vinyl aromatic compounds or hydrogenated products thereof, and others include non-diene polymers and natural rubber.

[0226] Examples of rubber-like polymers include styrene-based elastomers such as butadiene rubber or hydrogenated products thereof, isoprene rubber or hydrogenated products thereof, styrene-butadiene rubber or hydrogenated products thereof, styrene-butadiene block copolymer or hydrogenated products thereof, and styrene-isoprene block copolymer or hydrogenated products thereof; and acrylonitrile-butadiene rubber or hydrogenated products thereof.

[0227] Examples of non-diene polymers include, but are not limited to, olefin elastomers such as ethylene-propylene rubber, ethylene-propylene-diene rubber, ethylene-butene-diene rubber, ethylene-butene rubber, ethylene-hexene rubber, and ethylene-octene rubber, butyl rubber, brominated butyl rubber, acrylic rubber, fluororubber, silicone rubber, chlorinated polyethylene rubber, epichlorohydrin rubber, α,β-unsaturated nitrile-acrylate-conjugated diene copolymer rubber, urethane rubber, and polysulfide rubber.

[0228] Examples of natural rubber include, but are not limited to, smoked sheets such as RSS3 to 5, SMR, and epoxidized natural rubber.

[0229] The above-mentioned various rubber-like polymers may be modified rubbers to which a polar functional group such as a hydroxyl group, an amino group, etc. When used for tires, butadiene rubber, isoprene rubber, styrene-butadiene rubber, natural rubber, and butyl rubber are preferably used.

[0230] From the viewpoint of the balance between various performances and processing characteristics of the rubber composition, the weight average molecular weight of the rubber polymer is preferably from 2000 to 2,000,000, and more preferably from 5000 to 1,500,000. Also, a low molecular weight rubber polymer, so-called liquid rubber, can be used. These rubber-like polymers may be used alone or in combination of two or more.

[0231] When the rubber composition using the branched conjugated diene polymer obtained by the production method of this embodiment is used as a rubber composition containing the above-mentioned rubbery polymer, the content ratio (mass ratio) of the above-mentioned branched conjugated diene polymer to the rubbery polymer (above-mentioned branched conjugated diene polymer / rubbery polymer) is preferably 10 / 90 or more and 100 / 0 or less, more preferably 20 / 80 or more and 90 / 10 or less, and even more preferably 50 / 50 or more and 80 / 20 or less. Therefore, the rubber component contains the above-mentioned branched conjugated diene polymer in an amount of preferably 10% by mass or more and 100% by mass or less, more preferably 20% by mass or more and 90% by mass or less, and even more preferably 50% by mass or more and 80% by mass or less, based on the total amount (100% by mass) of the rubber component.

[0232] By setting the content ratio of (branched conjugated diene polymer / rubber-like polymer) within the above range, the abrasion resistance and breaking strength of the vulcanized product tend to be excellent, and the balance between low hysteresis loss and wet skid resistance also tends to be good.

[0233] The filler contained in the rubber composition is not limited to the following, but examples thereof include, in addition to the silica-based inorganic filler, carbon black, metal oxides, and metal hydroxides. Among these, silica-based inorganic fillers are preferred. The fillers may be used alone or in combination of two or more. The content of the filler in the rubber composition is 5.0 parts by mass or more and 150 parts by mass or less, preferably 20 parts by mass or more and 100 parts by mass or less, and more preferably 30 parts by mass or more and 90 parts by mass or less, based on 100 parts by mass of the rubber component containing the branched conjugated diene-based polymer. In the rubber composition, the content of the filler is 5.0 parts by mass or more per 100 parts by mass of the rubber component from the viewpoint of expressing the effect of adding the filler, and is 150 parts by mass or less per 100 parts by mass of the rubber component from the viewpoint of sufficiently dispersing the filler and making the processability and mechanical strength of the rubber composition practically sufficient.

[0234] The silica-based inorganic filler is not particularly limited and may be any known one, but solid particles containing SiO2 or Si3Al as a structural unit are preferred, and solid particles containing SiO2 or Si3Al as a main component of the structural unit are more preferred. Here, the main component refers to a component contained in the silica-based inorganic filler in an amount of 50% by mass or more, preferably 70% by mass or more, and more preferably 80% by mass or more.

[0235] Examples of silica-based inorganic fillers include, but are not limited to, inorganic fibrous substances such as silica, clay, talc, mica, diatomaceous earth, wollastonite, montmorillonite, zeolite, glass fiber, etc. Other examples include silica-based inorganic fillers whose surfaces have been hydrophobized, and mixtures of silica-based inorganic fillers and inorganic fillers other than silica-based fillers. Among these, silica and glass fiber are preferred from the viewpoints of strength, abrasion resistance, and the like, and silica is more preferred. Examples of silica include dry silica, wet silica, and synthetic silicate silica. Among these silicas, wet silica is preferred from the viewpoint of excellent balance between the effect of improving fracture strength and wet skid resistance.

[0236] From the viewpoint of obtaining practically satisfactory abrasion resistance and breaking strength in a rubber composition, the nitrogen adsorption specific surface area of ​​the silica-based inorganic filler determined by the BET adsorption method is 100 m2 / g or more 300m 2 / g or less, and 2 / g or more 250m 2 It is more preferable that the molecular weight is not more than 1 / g. If necessary, a relatively small specific surface area (e.g., a specific surface area of ​​200 m 2 / g) and silica-based inorganic fillers with a relatively large specific surface area (e.g., 200 m 2 / g or more) in combination with a silica-based inorganic filler. In particular, those with a relatively large specific surface area (e.g., 200 m 2 In the case where a silica-based inorganic filler (having a molecular weight of 100 or more per 1000 parts by weight and a molecular weight of 100 or more per 1000 parts by ... silica-based inorganic filler) is used, the rubber composition containing the branched conjugated diene polymer described above improves the dispersibility of silica, and is particularly effective in improving abrasion resistance, and tends to be able to achieve a high level of balance between good fracture strength and low hysteresis loss.

[0237] The content of the silica-based inorganic filler in the rubber composition is preferably 5.0 parts by mass or more and 150 parts by mass or less, and more preferably 20 parts by mass or more and 100 parts by mass or less, per 100 parts by mass of the rubber component containing the branched conjugated diene polymer obtained by the production method of this embodiment. The content of the silica-based inorganic filler in the rubber composition is preferably 5.0 parts by mass or more per 100 parts by mass of the rubber component from the viewpoint of exhibiting the effect of adding the silica-based inorganic filler, and is preferably 150 parts by mass or less per 100 parts by mass of the rubber component from the viewpoint of sufficiently dispersing the silica-based inorganic filler and making the processability and mechanical strength of the rubber composition practically sufficient.

[0238] The carbon black is not limited to the following, but examples thereof include carbon blacks of various classes such as SRF, FEF, HAF, ISAF, and SAF. Among these, carbon blacks having a nitrogen adsorption specific surface area of ​​50 m 2 / g or more and a dibutyl phthalate (DBP) oil absorption of 80 mL / 100 g or less is preferred.

[0239] The content of carbon black in the rubber composition is preferably 0.5 parts by mass or more and 100 parts by mass or less, more preferably 3.0 parts by mass or more and 100 parts by mass or less, and even more preferably 5.0 parts by mass or more and 50 parts by mass or less, per 100 parts by mass of the rubber component containing the branched conjugated diene polymer obtained by the production method of this embodiment. In the rubber composition, the content of carbon black is preferably 0.5 parts by mass or more per 100 parts by mass of the rubber component from the viewpoint of expressing performance required for applications such as tires, such as dry grip performance and electrical conductivity, and is preferably 100 parts by mass or less per 100 parts by mass of the rubber component from the viewpoint of dispersibility.

[0240] Metal oxide refers to solid particles whose main component is a structural unit represented by the chemical formula MxOy (M represents a metal atom, and x and y each independently represent an integer of 1 to 6).

[0241] Examples of metal oxides include, but are not limited to, alumina, titanium oxide, magnesium oxide, and zinc oxide.

[0242] Examples of metal hydroxides include, but are not limited to, aluminum hydroxide, magnesium hydroxide, and zirconium hydroxide.

[0243] In the method for producing the rubber composition of the present embodiment, a step of incorporating a silane coupling agent may be carried out. The silane coupling agent has a function of strengthening the interaction between the rubber component and the inorganic filler. Specifically, it has a group having affinity or binding properties for both the rubber component and the silica-based inorganic filler, and is preferably a compound having a sulfur bond portion and an alkoxysilyl group or silanol group portion in one molecule. Examples of such compounds include, but are not limited to, bis-[3-(triethoxysilyl)-propyl]-tetrasulfide, bis-[3-(triethoxysilyl)-propyl]-disulfide, and bis-[2-(triethoxysilyl)-ethyl]-tetrasulfide.

[0244] In the rubber composition, the content of the silane coupling agent is preferably 0.1 parts by mass or more and 30 parts by mass or less, more preferably 0.5 parts by mass or more and 20 parts by mass or less, and even more preferably 1.0 parts by mass or more and 15 parts by mass or less, relative to 100 parts by mass of the inorganic filler. When the content of the silane coupling agent is within the above range, the above-mentioned addition effect of the silane coupling agent tends to be more remarkable.

[0245] The rubber composition may contain a rubber softener from the viewpoint of improving the processability thereof. The amount of rubber softener added is expressed as the total amount including the amount of rubber softener previously contained in the branched conjugated diene polymer or other rubber-like polymers and the amount of rubber softener added when producing the rubber composition, per 100 parts by mass of the rubber component containing the branched conjugated diene polymer obtained by the production method of the present embodiment. As the rubber softener, mineral oil or liquid or low molecular weight synthetic softener is preferable. Mineral oil-based rubber softeners, called process oils or extender oils, which are used to soften rubber, increase its volume, and improve its processability, are mixtures of aromatic rings, naphthene rings, and paraffin chains, and those in which the carbon number of the paraffin chain is 50% or more of the total carbon are called paraffin-based, those in which the carbon number of the naphthene ring is 30% to 45% of the total carbon are called naphthene-based, and those in which the aromatic carbon number is more than 30% of the total carbon are called aromatic. When the branched conjugated diene polymer of this embodiment is a copolymer of a conjugated diene compound and a vinyl aromatic compound, it is preferable to use a rubber softener having a moderate aromatic content, since it tends to be compatible with the branched conjugated diene polymer. In the rubber composition, the content of the rubber softener is preferably 0 to 100 parts by mass, more preferably 10 to 90 parts by mass, and even more preferably 30 to 90 parts by mass, per 100 parts by mass of the rubber component. By making the content of the rubber softener 100 parts by mass or less per 100 parts by mass of the rubber component, bleeding out is suppressed, and stickiness of the surface of the rubber composition tends to be suppressed.

[0246] The method for mixing the branched conjugated diene polymer obtained by the production method of the present embodiment with additives such as other rubber-like polymers, silica-based inorganic fillers, carbon black and other fillers, silane coupling agents, and rubber softeners is not limited to the following, but examples thereof include a melt-kneading method using a general mixer such as an open roll, a Banbury mixer, a kneader, a single-screw extruder, a twin-screw extruder, or a multi-screw extruder, and a method in which the components are dissolved and mixed and then the solvent is removed by heating. Among these, the melt kneading method using a roll, a Banbury mixer, a kneader, or an extruder is preferred from the viewpoints of productivity and good kneading properties. In addition, either a method of kneading the rubber component, other fillers, a silane coupling agent, and additives at once, or a method of mixing them in several batches can be applied.

[0247] The rubber composition may be a vulcanized composition that has been vulcanized with a vulcanizing agent. Examples of the vulcanizing agent include, but are not limited to, radical generators such as organic peroxides and azo compounds, oxime compounds, nitroso compounds, polyamine compounds, sulfur, and sulfur compounds. Examples of the sulfur compounds include sulfur monochloride, sulfur dichloride, disulfide compounds, and polymeric polysulfur compounds. In the rubber composition, the content of the vulcanizing agent is preferably 0.01 parts by mass to 20 parts by mass, more preferably 0.1 parts by mass to 15 parts by mass, based on 100 parts by mass of the rubber component. As the vulcanization method, a conventionally known method can be applied, and the vulcanization temperature is preferably 120°C to 200°C, more preferably 140°C to 180°C.

[0248] In vulcanization, a vulcanization accelerator and a vulcanization aid may be used, if necessary. As the vulcanization accelerator, a conventionally known material can be used, and examples thereof include, but are not limited to, sulfenamide-based, guanidine-based, thiuram-based, aldehyde-amine-based, aldehyde-ammonia-based, thiazole-based, thiourea-based, and dithiocarbamate-based vulcanization accelerators. Furthermore, the vulcanization aid may include, but is not limited to, zinc oxide and stearic acid. The amount of the vulcanization accelerator is preferably 0.01 parts by mass or more and 20 parts by mass or less, and more preferably 0.1 parts by mass or more and 15 parts by mass or less, based on 100 parts by mass of the rubber component.

[0249] The rubber composition may contain various additives such as other softeners, other fillers, heat stabilizers, antistatic agents, weather stabilizers, antioxidants, colorants, and lubricants, in addition to those described above, within the scope of the present embodiment. As the other softening agents, known softening agents can be used. Other fillers include, but are not limited to, calcium carbonate, magnesium carbonate, aluminum sulfate, and barium sulfate. As the heat resistance stabilizer, antistatic agent, weather resistance stabilizer, antioxidant, colorant, and lubricant, known materials can be used.

[0250] [Tire and tire manufacturing method] The tire of the present embodiment contains the rubber composition of the present embodiment described above. The method for producing a tire according to the present embodiment includes a step of obtaining a branched conjugated diene polymer by the production method according to the present embodiment, a step of obtaining a rubber composition containing the branched conjugated diene polymer, and a step of molding the rubber composition. The rubber composition containing the branched conjugated diene polymer obtained by the production method of the present embodiment described above is suitably used as a rubber composition for tires.

[0251] The rubber composition for tires can be used in various tire parts such as treads, carcasses, sidewalls, and beads of various tires such as fuel-efficient tires, all-season tires, high-performance tires, and studless tires, although the tire rubber composition is not limited thereto. The rubber composition for tires containing the branched conjugated diene-based polymer of the present embodiment has an excellent balance between abrasion resistance, breaking strength, low hysteresis loss and wet skid resistance when vulcanized, and is therefore suitably used for the treads of fuel-saving tires and high-performance tires. EXAMPLES

[0252] Hereinafter, the present embodiment will be described in more detail with reference to specific examples and comparative examples, but the present embodiment is not limited in any way to the following examples and comparative examples. [First embodiment] As a first example, the present embodiment will be described in detail by giving a specific example and a comparative example. Hereinafter, a conjugated diene polymer coupled with a nitrogen atom-containing modifier will be referred to as a "coupled conjugated diene polymer". Moreover, the conjugated diene polymer in an unmodified state is referred to as an "unmodified conjugated diene polymer." In the tables, it is simply referred to as a "conjugated diene polymer." Furthermore, a conjugated diene polymer having a branched structure is referred to as a "branched conjugated diene polymer." Various physical properties in the examples and comparative examples were measured by the methods shown below.

[0253] (Physical Properties 1) Polymer Mooney Viscosity An unmodified conjugated diene polymer or a conjugated diene polymer coupled with a nitrogen atom-containing modifier (hereinafter also referred to as a "coupled conjugated diene polymer") was used as a sample, and the Mooney viscosity was measured using a Mooney viscometer (manufactured by Ueshima Seisakusho Co., Ltd., product name "VR1132") using an L-type rotor in accordance with ISO 289. The measurement temperature was 110°C when an unmodified conjugated diene polymer (simply referred to as conjugated diene polymer in the table) was used as the sample, and 100°C when a coupled conjugated diene polymer was used as the sample. First, the sample was preheated at the test temperature for 1 minute, and then the rotor was rotated at 2 rpm. The torque was measured after 4 minutes to determine the Mooney viscosity (ML (1+4) ) was decided.

[0254] (Physical property 2) Mooney relaxation rate A coupling conjugated diene polymer was used as a sample, and the Mooney viscosity was measured using a Mooney viscometer (manufactured by Ueshima Seisakusho Co., Ltd. under the trade name "VR1132") with an L-shaped rotor in accordance with ISO 289. The rotation of the rotor was then immediately stopped, and the torque was recorded in Mooney units every 0.1 seconds for 1.6 to 5 seconds after the rotor was stopped. The slope of the straight line obtained by plotting the torque versus time (seconds) on a double logarithmic scale was determined, and the absolute value of the slope was taken as the Mooney relaxation rate (MSR).

[0255] (Physical property 3) Branching degree (Bn) The branching degree (Bn) of the coupling conjugated diene polymer was measured by a GPC-light scattering method equipped with a viscosity detector as follows. A coupling conjugated diene polymer was used as a sample, and measurements were performed using a gel permeation chromatography (GPC) measuring device (manufactured by Malvern under the trade name "GPCmax VE-2001") in which three columns packed with polystyrene gel were connected together, and three detectors were connected in that order: a light scattering detector, an RI detector, and a viscosity detector (manufactured by Malvern under the trade name "TDA305"). Based on standard polystyrene, the absolute molecular weight was calculated from the measurement results of the light scattering detector and the RI detector, and the intrinsic viscosity was calculated from the measurement results of the RI detector and the viscosity detector. Linear polymer has an intrinsic viscosity [η] = -3.883M 0.771 The shrinkage factor (g') was calculated as the ratio of the intrinsic viscosity corresponding to each molecular weight, where M represents the absolute molecular weight. The obtained shrinkage factor (g') was then used to calculate the branching degree (Bn), defined as g' = 6Bn / [(Bn+1)(Bn+2)]. The eluent used was tetrahydrofuran (hereinafter also referred to as "THF") containing 5 mmol / L triethylamine. The columns used were "TSKgel G4000HXL", "TSKgel G5000HXL", and "TSKgel G6000HXL" manufactured by Tosoh Corporation. 20 mg of the measurement sample was dissolved in 10 mL of THF to prepare a measurement solution, and 100 μL of the measurement solution was injected into a GPC measurement device and measured under conditions of an oven temperature of 40° C. and a THF flow rate of 1 mL / min.

[0256] (Physical property 4) Molecular weight <Measurement condition 1>: Using an unmodified conjugated diene polymer or a coupled conjugated diene polymer as a sample, a chromatogram was measured using a GPC measuring device (manufactured by Tosoh Corporation under the trade name "HLC-8320GPC") in which three columns packed with polystyrene gel were connected together, and an RI detector (manufactured by Tosoh Corporation under the trade name "HLC8020") was used. Based on a calibration curve obtained using standard polystyrene, the weight average molecular weight (Mw), number average molecular weight (Mn), and molecular weight distribution (Mw / Mn) were determined. The eluent used was tetrahydrofuran (THF) containing 5 mmol / L triethylamine. Three columns, Tosoh Corporation's "TSKgel SuperMultiporeHZ-H" (trade name), were connected, and a Tosoh Corporation's "TSKguardcolumn SuperMP(HZ)-H" (trade name) was connected in front of them as a guard column. 10 mg of the measurement sample was dissolved in 10 mL of THF to prepare a measurement solution, and 10 μL of the measurement solution was injected into a GPC measurement device and measured under conditions of an oven temperature of 40° C. and a THF flow rate of 0.35 mL / min. Among the various samples measured under the above measurement condition 1, samples whose molecular weight distribution (Mw / Mn) was less than 1.6 were measured again under the following measurement condition 2. For samples whose molecular weight distribution was 1.6 or more when measured under measurement condition 1, the measured value under measurement condition 1 was used. <Measurement condition 2>: Using an unmodified conjugated diene polymer or a coupled conjugated diene polymer as a sample, a chromatogram was measured using a GPC measuring device having three columns connected together, each column using a polystyrene gel as a packing material, and the weight average molecular weight (Mw) and number average molecular weight (Mn) were determined based on a calibration curve using standard polystyrene. The eluent used was THF containing 5 mmol / L triethylamine. The columns used were the following: guard column: Tosoh Corporation's product name "TSKguardcolumn SuperH-H"; columns: Tosoh Corporation's product names "TSKgel SuperH5000", "TSKgel SuperH6000", and "TSKgel SuperH7000". An RI detector (manufactured by Tosoh Corporation under the trade name "HLC8020") was used under the conditions of an oven temperature of 40° C. and a THF flow rate of 0.6 mL / min. 10 mg of a sample to be measured was dissolved in 20 mL of THF to prepare a measurement solution, and 20 μL of the measurement solution was injected into a GPC measurement device for measurement. For samples that were measured under measurement condition 1 and had a molecular weight distribution value of less than 1.6, measurement was performed under measurement condition 2, and the measured value was adopted.

[0257] (Physical property 5) Modification rate The modification rate of the coupling conjugated diene polymer was measured by a column adsorption GPC method as follows. The coupling conjugated diene polymer was used as a sample, and the measurement was carried out by utilizing the adsorption property of the modified basic polymer component in a GPC column packed with silica gel. The amount of a sample solution containing a sample and low molecular weight internal standard polystyrene was adsorbed onto the silica-based column by measuring the difference between the chromatogram measured using a polystyrene-based column and the chromatogram measured using a silica-based column, and the modification rate was calculated. Specifically, it is as follows: Furthermore, for samples that were measured under the above (Physical Property 4) Measurement Condition 1 and had a molecular weight distribution value of 1.6 or more, they were measured under the following Measurement Condition 3, and the measured value was adopted. For samples that were measured under the above (Physical Property 4) Measurement Condition 1 and had a molecular weight distribution value of less than 1.6, they were measured under the following Measurement Condition 4, and the measured value was adopted.

[0258] <Preparation of sample solution>: 10 mg of the sample and 5 mg of standard polystyrene were dissolved in 20 mL of THF to prepare a sample solution. <Measurement condition 3>: GPC measurement conditions using polystyrene columns: A Tosoh Corporation product name "HLC-8320GPC" was used, and 10 μL of the sample solution was injected into the device using THF containing 5 mmol / L triethylamine as the eluent. A chromatogram was obtained using an RI detector under the following conditions: column oven temperature 40°C, THF flow rate 0.35 mL / min. The columns used were three Tosoh Corporation products (TSKgel SuperMultiporeHZ-H) connected together, with a Tosoh Corporation product (TSKguardcolumn SuperMP(HZ)-H) connected in front of them as a guard column.

[0259] <Measurement condition 4>: THF containing 5 mmol / L triethylamine was used as the eluent, and 20 μL of the sample solution was injected into the device for measurement. The columns used were a guard column manufactured by Tosoh Corporation under the trade name "TSKguardcolumn SuperH-H" and columns manufactured by Tosoh Corporation under the trade names "TSKgel SuperH5000", "TSKgel SuperH6000", and "TSKgel SuperH7000". Measurement was performed using an RI detector (manufactured by Tosoh Corporation, HLC8020) under conditions of a column oven temperature of 40°C and a THF flow rate of 0.6 mL / min, to obtain a chromatogram.

[0260] GPC measurement conditions using a silica column: A Tosoh Corporation product name "HLC-8320GPC" was used, THF was used as the eluent, 50 μL of the sample solution was injected into the device, and a chromatogram was obtained using an RI detector under the conditions of a column oven temperature of 40°C and a THF flow rate of 0.5 ml / min. The columns used were Zorbax PSM-1000S, PSM-300S, and PSM-60S, and a guard column "DIOL 4.6 × 12.5 mm 5 micron" was connected to the front of the columns.

[0261] How to calculate the denaturation rate: The total peak area of ​​the chromatogram using the polystyrene column was set as 100, the peak area of ​​the sample was set as P1, the peak area of ​​the standard polystyrene was set as P2, the total peak area of ​​the chromatogram using the silica column was set as 100, the peak area of ​​the sample was set as P3, and the peak area of ​​the standard polystyrene was set as P4, and the modification rate (%) was calculated using the following formula. Denaturation rate (%) = [1-(P2 x P3) / (P1 x P4)] x 100 (where P1+P2=P3+P4=100)

[0262] (Physical property 6) Bound styrene content A coupling conjugated diene polymer not containing a rubber softener was used as a sample, and 100 mg of the sample was dissolved in chloroform up to 100 mL to prepare a measurement sample. The amount of bound styrene (mass%) relative to 100 mass% of the sample coupled conjugated diene polymer was measured based on the amount of absorption of ultraviolet light (around 254 nm) by the phenyl group of styrene (measuring device: Shimadzu Corporation spectrophotometer "UV-2450").

[0263] (Physical property 7) Microstructure of butadiene part (1,2-vinyl bond amount) A coupling conjugated diene polymer not containing a rubber softener was used as a sample, and 50 mg of the sample was dissolved in 10 mL of carbon disulfide to prepare a measurement sample. Using a solution cell, infrared spectra are recorded from 600 to 1000 cm -1 The absorbance at a predetermined wave number was measured in the range of 100 nm to 150 nm, and the microstructure of the butadiene portion, i.e., the amount of 1,2-vinyl bonds (mol%) was calculated according to the formula of Hampton's method (method described in R.R. Hampton, Analytical Chemistry 21, 923 (1949)) (measuring device: Fourier transform infrared spectrophotometer "FT-IR230" manufactured by JASCO Corporation).

[0264] (Physical Property 8) Molecular weight (absolute molecular weight) measured by GPC-light scattering method The coupling conjugated diene polymer was used as a sample, and a chromatogram was measured using a GPC-light scattering measuring device in which three columns packed with polystyrene gel were connected, and the weight average molecular weight (Mw-i) was calculated based on the solution viscosity and the light scattering method (also referred to as "absolute molecular weight"). The eluent used was a mixed solution of tetrahydrofuran and triethylamine (THF in TEA: prepared by mixing 5 mL of triethylamine in 1 L of tetrahydrofuran). The columns used were a guard column (manufactured by Tosoh Corporation under the trade name "TSKguardcolumn HHR-H") and columns (manufactured by Tosoh Corporation under the trade names "TSKgel G6000HHR", "TSKgel G5000HHR", and "TSKgel G4000HHR"). A GPC-light scattering measuring device (trade name "Viscotek TDAmax" manufactured by Malvern Instruments) was used under conditions of an oven temperature of 40° C. and a THF flow rate of 1.0 mL / min. 10 mg of the sample to be measured was dissolved in 20 mL of THF to prepare a measurement solution, and 200 μL of the measurement solution was injected into the GPC measurement device and measured.

[0265] [Branched conjugated diene polymer] ( Reference example 1-1) Coupling conjugated diene polymer (sample 1-1) The internal volume is 10 L, and the ratio of internal height (L) to diameter (D) (L / D) is 4.0. The reactor is a tank type reactor with an agitator, an inlet at the bottom and an outlet at the top, and has a jar for temperature control. Two tank-type pressure vessels with a tank cap were connected together as polymerization reactors. 1,3-butadiene, which had been previously dehydrated, was fed at 18.6 g / min, and styrene at 10.0 g / min. The mixture was fed to the inlet of the reactor. In the static mixer installed in the piping that supplies the gas, a gas for inactivating remaining impurities is used. -Butyllithium was added at 0.103mmol / min and mixed, then continuously poured into the bottom of the reactor. In addition, 2,2-bis(2-oxolanyl)propane was added as a polar substance at 0.0 At a rate of 81 mmol / min, 0.143 mmol of n-butyllithium was used as a polymerization initiator. The mixture was fed to the bottom of the first reactor, which was vigorously mixed with an agitator, at a rate of 1 / min. The temperature inside the reactor was kept at 67°C. The temperature was kept at .degree. The polymer solution was continuously withdrawn from the top of the first reactor and continuously poured into the bottom of the second reactor. The reaction was continued at 70°C, and then the mixture was fed to the static mixer from the top of the second unit. When the polymerization is sufficiently stable, 1,3-butadiene and styrene are copolymerized. From the bottom of the second reactive group, trimethoxy(4-vinylphenyl)silane ( In the table, this is abbreviated as "BS-1.") was added at a rate of 0.0190 mmol / min to form a main chain branch structure. The polymerization reaction and branching reaction were carried out to obtain a conjugated diene polymer having the above structure. After the polymerization reaction and the branching reaction were stabilized, the conjugated diene before the addition of the coupling agent was A small amount of the polymer solution was taken out, and the antioxidant (BHT) was adjusted to 0.2 g per 100 g of polymer. After the solvent was removed, the Mooney viscosity at 110°C and various molecular weights were measured. The physical properties are shown in Table 1. Next, the polymer solution discharged from the outlet of the reactor was mixed with tetraethoxysilane as a coupling agent. Silane (abbreviated as "A" in the table) was added continuously at a rate of 0.0480 mmol / min. The mixture was mixed using a static mixer and subjected to a coupling reaction. The time it took for the coupling agent to be added to the polymer solution flowing out of the nozzle was 4.8 minutes, and the temperature was The difference between the temperature during the polymerization process and the temperature before adding the coupling agent is 68°C. After the coupling reaction, a small amount of the conjugated diene polymer solution was taken out and added with an antioxidant. (BHT) was added in an amount of 0.2 g per 100 g of polymer, and the solvent was then removed to give a The amount of styrene in the mixture (Physical Properties 6) and the microstructure of the butadiene part (1,2-vinyl bond amount: The results are shown in Table 1. Next, add an antioxidant (BHT) to the polymer solution after the coupling reaction for 100 g of polymer. The amount of n-hexane solution was continuously added at 0.055 g / min so that the amount was 0.2 g per unit time. The coupling reaction was completed. In contrast, SRAE oil (JOMO Process NC140 manufactured by JX Nippon Oil & Energy Corporation) The mixture was added continuously to a total of 25.0 g and mixed with a static mixer. The solvent is removed by stripping, and a compound represented by the following formula (1) is added to a part of the main chain. It has a four-branched structure derived from a branching agent (hereinafter also referred to as "branching agent structure (1)"), and is coupled A coupling conjugated diene polymer (sample 1) with a three-branched star polymer structure derived from a coupling agent -1). The physical properties of Sample 1-1 are shown in Table 1. The polymer before the addition of the branching agent, the polymer after the addition of the branching agent, and the polymer after the addition of the coupling agent are The molecular weight of the polymer in each process was measured by GPC and the molecular weight was measured by GPC with a viscometer. The structure of the coupling conjugated diene polymer was identified by comparing with the branching degree by the method described below. The structure of each sample was identified in the same manner.

[0266] [ka]

[0267] (In formula (1), R 1represents any one selected from the group consisting of a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, and an aryl group having 6 to 20 carbon atoms, which may partially have a branched structure. X 1 is a single bond or an organic group containing any one selected from the group consisting of carbon, hydrogen, nitrogen, sulfur, and oxygen. Y 1 represents any one selected from the group consisting of an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, and a halogen atom. Each may be independent and the same or different.

[0268] ( Reference example 1-2) Coupling conjugated diene polymer (sample 1-2) The coupling agent was converted from tetraethoxysilane to 1,2-bis(triethoxysilyl)ethene. (abbreviated as "B" in the table) and the amount added was changed to 0.0360 mmol / min. Outside, Reference example In the same manner as in 1-1, a coupling conjugated diene polymer (sample 1-2) was obtained, which has a 4-branch structure derived from the branching agent structure (1) in a part of the main chain and a 4-branch star polymer structure derived from the coupling agent. The physical properties of sample 1-2 are shown in Table 1.

[0269] ( Reference example 1-3) Coupling conjugated diene polymer (sample 1-3) Coupling agent was prepared from tetraethoxysilane to 1,3-bis(N,N-diglycidyl amine) (C)cyclohexane (abbreviated as "C" in the table), and the amount added was 0.0360 Except for changing to mmol / min. Reference example In the same manner as in 1-1, a coupling conjugated diene polymer (sample 1-3) was obtained, which has a 4-branch structure derived from the branching agent structure (1) in a part of the main chain and a 4-branch star polymer structure derived from the coupling agent. The physical properties of sample 1-3 are shown in Table 1.

[0270] ( Reference example1-4) Coupling conjugated diene polymer (sample 1-4) Coupling agent was prepared from tetraethoxysilane to 2,2-dimethoxy-1-(3-trimethoxysilane) (xysilylpropyl)-1-aza-2-silacyclopentane (abbreviated as "D" in the table). The addition rate was changed to 0.0360 mmol / min. Reference example In the same manner as in 1-1, a coupling conjugated diene polymer (sample 1-4) was obtained, which has a 4-branched structure derived from the branching agent structure (1) in a part of the main chain and a 4-branched star polymer structure derived from the coupling agent. The physical properties of sample 1-4 are shown in Table 1.

[0271] ( Reference example 1-5) Coupling conjugated diene polymer (sample 1-5) Coupling agent was changed from tetraethoxysilane to tris(3-trimethoxysilylpropyl ) amine (abbreviated as "E" in the table) and its addition rate was changed to 0.0250 mmol / min. Other than that, Reference example In the same manner as in 1-1, a coupling conjugated diene polymer (sample 1-5) was obtained, which has a 4-branch structure derived from the branching agent structure (1) in a part of the main chain and a 6-branch star polymer structure derived from the coupling agent. The physical properties of sample 1-5 are shown in Table 1.

[0272] ( Reference example 1-6) Coupling conjugated diene polymer (sample 1-6) Coupling agent was converted from tetraethoxysilane to tetrakis(3-trimethoxysilylpropane) (Pyryl)-1,3-propanediamine (abbreviated as "F" in the table), and the amount added was 0. Except for changing to 0190mmol / min, Reference example In the same manner as in 1-1, a coupling conjugated diene polymer (sample 1-6) was obtained, which has a 4-branch structure derived from the branching agent structure (1) in a part of the main chain and an 8-branch star polymer structure derived from the coupling agent. The physical properties of sample 1-6 are shown in Table 1.

[0273] ( Reference example 1-7) Coupling conjugated diene polymer (sample 1-7) Coupling agent was converted from tetraethoxysilane to tetrakis(3-trimethoxysilylpropane) (Pyryl)-1,3-propanediamine (abbreviated as "F" in the table), and the amount added was 0. Except for changing to 0160mmol / min, Reference example In the same manner as in 1-1, a coupling conjugated diene polymer (sample 1-7) was obtained, which has a 4-branch structure derived from the branching agent structure (1) in a part of the main chain and an 8-branch star polymer structure derived from the coupling agent. The physical properties of sample 1-7 are shown in Table 1.

[0274] ( Reference example 1-8) Coupling conjugated diene polymer (sample 1-8) The addition rate of 1,3-butadiene was increased from 18.6 g / min to 24.3 g / min, and that of styrene was increased from 18.6 g / min to 24.3 g / min. The flow rate was changed from 10.0 g / min to 4.3 g / min, and 2,2-bis( The addition rate of 2-oxolanylpropane was changed from 0.081 mmol / min to 0.044 mmol / min. l / min, and the coupling agent was changed from tetraethoxysilane to tetrakis(3-trimethysilane). (xysilylpropyl)-1,3-propanediamine (abbreviated as "F" in the table), and Except for changing the amount of added to 0.0160mmol / min, Reference example In the same manner as in 1-1, a coupling conjugated diene polymer (sample 1-8) was obtained, which has a 4-branch structure derived from the branching agent structure (1) in a part of the main chain and an 8-branch star polymer structure derived from the coupling agent. The physical properties of sample 1-8 are shown in Table 1.

[0275] ( Reference example 1-9) Coupling conjugated diene polymer (sample 1-9) The addition rate of 1,3-butadiene was increased from 18.6 g / min to 17.1 g / min, and that of styrene was increased from 18.6 g / min to 17.1 g / min. The speed was changed from 10.0 g / min to 11.5 g / min, and 2,2-bis(2,2-diphenyl ether) was added as a polar substance. The addition rate of (2-oxolanyl)propane was increased from 0.081 mmol / min to 0.089 mmol / min. ol / min, and the coupling agent was changed from tetraethoxysilane to tetrakis(3-trimethylsilane). (trimethoxysilylpropyl)-1,3-propanediamine (abbreviated as "F" in the table), Except for changing the amount of addition to 0.0160mmol / min, Reference example In the same manner as in 1-1, a coupling conjugated diene polymer (sample 1-9) was obtained, which has a 4-branch structure derived from the branching agent structure (1) in a part of the main chain and an 8-branch star polymer structure derived from the coupling agent. The physical properties of sample 1-9 are shown in Table 2.

[0276] ( Reference example 1-10) Coupling conjugated diene polymer (sample 1-10) The addition rate of the polar substance 2,2-bis(2-oxolanyl)propane was set at 0.081mmol. The flow rate was changed from 1 l / min to 0.200 mmol / min, and the coupling agent was changed from tetraethoxysilane to Tetrakis(3-trimethoxysilylpropyl)-1,3-propanediamine (in the table, (abbreviated as "F").) and its addition amount was changed to 0.0160 mmol / min. Reference example In the same manner as in 1-1, a coupling conjugated diene polymer (sample 1-10) was obtained, which has a 4-branch structure derived from the branching agent structure (1) in a part of the main chain and an 8-branch star polymer structure derived from the coupling agent. The physical properties of sample 1-10 are shown in Table 2.

[0277] ( Reference example 1-11) Coupling conjugated diene polymer (sample 1-11) The branching agent was converted from trimethoxy(4-vinylphenyl)silane to dimethylmethoxy(4-vinyl (BS-2) in the table, and the amount added was 0.0350m mol / min, and the coupling agent was changed from tetraethoxysilane to 1,2-bis(triethoxysilane) (xysilyl)ethane (abbreviated as "B" in the table), and the amount added was 0.0360mmol Except for changing to l / min. Reference example In the same manner as in 1-1, a coupling conjugated diene polymer (sample 1-11) was obtained, which has a two-branch structure derived from the branching agent structure (1) in a part of the main chain and a four-branch star polymer structure derived from the coupling agent. The physical properties of sample 1-11 are shown in Table 2.

[0278] ( Reference example 1-12) Coupling conjugated diene polymer (sample 1-12) The branching agent was converted from trimethoxy(4-vinylphenyl)silane to dimethylmethoxy(4-vinyl (BS-2) in the table, and the amount added was 0.0350m mol / min, and the coupling agent was changed from tetraethoxysilane to 2,2-dimethoxy-1 -(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane (see " D" and its addition rate was changed to 0.0360 mmol / min. Reference example In the same manner as in 1-1, a coupling conjugated diene polymer (sample 1-12) having a two-branch structure derived from the branching agent structure (1) in a part of the main chain and a four-branch star polymer structure derived from the coupling agent was obtained. The physical properties of sample 1-12 are shown in Table 2.

[0279] ( Reference example 1-13) Coupling conjugated diene polymer (sample 1-13) The branching agent was converted from trimethoxy(4-vinylphenyl)silane to dimethylmethoxy(4-vinyl (BS-2) in the table, and the amount added was 0.0350m mol / min, and the coupling agent was changed from tetraethoxysilane to tetrakis(3-trimethylsilane). (trimethoxysilylpropyl)-1,3-propanediamine (abbreviated as "F" in the table), Except for changing the amount of addition to 0.0160mmol / min, Reference example In the same manner as in 1-1, a coupling conjugated diene polymer (sample 1-13) was obtained, which has a two-branch structure derived from the branching agent structure (1) in a part of the main chain and an eight-branch star polymer structure derived from the coupling agent. The physical properties of sample 1-13 are shown in Table 2.

[0280] ( Reference example 1-14) Coupling conjugated diene polymer (sample 1-14) Branching agents were prepared from trimethoxy(4-vinylphenyl)silane to 1,1-bis(4-(dimethylphenyl)silane) (phenylmethoxysilyl)phenyl)ethylene (abbreviated as "BS-3" in the table) and its addition The amount was changed to 0.0120 mmol / min, and the coupling agent was changed from tetraethoxysilane to 1, The amount of 2-bis(triethoxysilyl)ethane (abbreviated as "B" in the table) was changed to Except for changing to 0.0360mmol / min, Reference example In the same manner as in 1-1, a branching agent represented by the following formula (2) (hereinafter also referred to as "branching agent structure (2)") is added to a part of the main chain. Coupling agent having a three-branched structure derived from the coupling agent and a four-branched star polymer structure derived from the coupling agent. A ring-conjugated diene polymer (sample 1-14) was obtained. The physical properties of sample 1-14 are shown in Table 2.

[0281] [ka]

[0282] (In formula (2), X 2 , X 3 is a single bond or an organic group containing any one selected from the group consisting of carbon, hydrogen, nitrogen, sulfur, and oxygen. Y 2 , Y 3represents any one selected from the group consisting of an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, and a halogen atom. Each may be independent and the same or different.

[0283] ( Reference example 1-15) Coupling conjugated diene polymer (sample 1-15) Branching agents were prepared from trimethoxy(4-vinylphenyl)silane to 1,1-bis(4-(dimethylphenyl)silane) (phenylmethoxysilyl)phenyl)ethylene (abbreviated as "BS-3" in the table) and its addition The amount was changed to 0.0120 mmol / min, and the coupling agent was changed from tetraethoxysilane to 2, 2-Dimethoxy-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclo Change to pentane (abbreviated as "D" in the table) and change the amount added to 0.0360 mmol / min. Other than that, Reference example In the same manner as in 1-1, a coupling conjugated diene polymer (sample 1-15) was obtained, which has a three-branched structure derived from the branching agent structure (2) in part of the main chain and a four-branched star polymer structure derived from the coupling agent. The physical properties of sample 1-15 are shown in Table 2.

[0284] ( Reference example 1-16) Coupling conjugated diene polymer (sample 1-16) Branching agents were prepared from trimethoxy(4-vinylphenyl)silane to 1,1-bis(4-(dimethylphenyl)silane) (phenylmethoxysilyl)phenyl)ethylene (abbreviated as "BS-3" in the table) and its addition The amount was changed to 0.0120 mmol / min, and the coupling agent was changed from tetraethoxysilane to tetra Rakis(3-trimethoxysilylpropyl)-1,3-propanediamine (in the table, "F" ) and the amount added was changed to 0.0160 mmol / min. Reference exampleIn the same manner as in 1-1, a coupling conjugated diene polymer (sample 1-16) was obtained, which has a three-branched structure derived from the branching agent structure (2) in a part of the main chain and an eight-branched star polymer structure derived from the coupling agent. The physical properties of sample 1-16 are shown in Table 2.

[0285] ( Reference example 1-17) Coupling conjugated diene polymer (sample 1-17) Branching agents were synthesized from trimethoxy(4-vinylphenyl)silane to 1,1-bis(4-trimethoxy (xysilylphenyl)ethylene (abbreviated as "BS-4" in the table), and the amount added was 0. The coupling agent was changed from tetraethoxysilane to 1,2-bis(1,2-diphenylsilane). (triethoxysilyl)ethane (abbreviated as "B" in the table), and the amount added was 0.03 Except for changing to 60mmol / min, Reference example In the same manner as in 1-1, a coupling conjugated diene polymer (sample 1-17) was obtained, which has a 7-branch structure derived from the branching agent structure (2) in a part of the main chain and a 4-branch star polymer structure derived from the coupling agent. The physical properties of sample 1-17 are shown in Table 3.

[0286] ( Reference example 1-18) Coupling conjugated diene polymer (sample 1-18) Branching agents were synthesized from trimethoxy(4-vinylphenyl)silane to 1,1-bis(4-trimethoxy (xysilylphenyl)ethylene (abbreviated as "BS-4" in the table), and the amount added was 0. The coupling agent was changed from tetraethoxysilane to 2,2-dimethylsilane. Toxo-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane (abbreviated as "D" in the table) and the amount added was changed to 0.0360 mmol / min. teeth, Reference exampleIn the same manner as in 1-1, a coupling conjugated diene polymer (sample 1-18) was obtained, which has a 7-branch structure derived from the branching agent structure (2) in a part of the main chain and a 4-branch star polymer structure derived from the coupling agent. The physical properties of sample 1-18 are shown in Table 3.

[0287] ( Reference example 1-19) Coupling conjugated diene polymer (sample 1-19) Branching agents were synthesized from trimethoxy(4-vinylphenyl)silane to 1,1-bis(4-trimethoxy (xysilylphenyl)ethylene (abbreviated as "BS-4" in the table), and the amount added was 0. 0210mmol / min, and the coupling agent was changed from tetraethoxysilane to tetrakis( 3-trimethoxysilylpropyl)-1,3-propanediamine (abbreviated as "F" in the table. ) and the amount added was changed to 0.0160mmol / min. Reference example In the same manner as in 1-1, a coupling conjugated diene polymer (sample 1-19) was obtained, which has a 7-branch structure derived from the branching agent structure (2) in a part of the main chain and an 8-branch star polymer structure derived from the coupling agent. The physical properties of sample 1-19 are shown in Table 3.

[0288] ( Reference example 1-20) Coupling conjugated diene polymer (sample 1-20) The branching agent was converted from trimethoxy(4-vinylphenyl)silane to trichloro(4-vinylphenyl)silane. (BS-5) in the table, and the amount added was 0.0190 mmol. / min, and the coupling agent was changed from tetraethoxysilane to 1,2-bis(triethoxysilane) (aryl)ethane (abbreviated as "B" in the table), and the amount added was 0.0360 mmol / min. Other than changing it to Reference exampleIn the same manner as in 1-1, a coupling conjugated diene polymer (sample 1-20) was obtained, which has a 4-branch structure derived from the branching agent structure (1) in a part of the main chain and an 8-branch star polymer structure derived from the coupling agent. The physical properties of sample 1-20 are shown in Table 3.

[0289] ( Reference example 1-21) Coupling conjugated diene polymer (sample 1-21) The branching agent was converted from trimethoxy(4-vinylphenyl)silane to trichloro(4-vinylphenyl)silane. (BS-5) in the table, and the amount added was 0.0190 mmol. / min, and the coupling agent was changed from tetraethoxysilane to 2,2-dimethoxy-1-(3 -trimethoxysilylpropyl)-1-aza-2-silacyclopentane (represented by "D" in the table). (abbreviated as "0.0360 mmol / min") and the amount added was changed to 0.0360 mmol / min. Reference example In the same manner as in 1-1, a coupling conjugated diene polymer (sample 1-21) was obtained, which has a 4-branch structure derived from the branching agent structure (1) in a part of the main chain and an 8-branch star polymer structure derived from the coupling agent. The physical properties of sample 1-21 are shown in Table 3.

[0290] ( Reference example 1-22) Coupling conjugated diene polymer (sample 1-22) The branching agent was converted from trimethoxy(4-vinylphenyl)silane to trichloro(4-vinylphenyl)silane. (BS-5) in the table, and the amount added was 0.0190 mmol. / min, and the coupling agent was changed from tetraethoxysilane to tetrakis(3-trimethoxysilane). silylpropyl)-1,3-propanediamine (abbreviated as "F" in the table), and its addition Except for changing the dosage to 0.0160mmol / min, Reference exampleIn the same manner as in 1-1, a coupling conjugated diene polymer (sample 1-22) was obtained, which has a 4-branch structure derived from the branching agent structure (1) in a part of the main chain and an 8-branch star polymer structure derived from the coupling agent. The physical properties of sample 1-22 are shown in Table 3.

[0291] ( Reference example 1-23) Coupling conjugated diene polymer (sample 1-23) The branching agent trimethoxy(4-vinylphenyl)silane (abbreviated as "BS-1" in the table) The amount of addition was changed from 0.0190mmol / min to 0.0100mmol / min, and the coupling The agent was converted from tetraethoxysilane to tetrakis(3-trimethoxysilylpropyl)-1,3 - Propanediamine (abbreviated as "F" in the table) was added in an amount of 0.0190mmol Except for changing to l / min. Reference example In the same manner as in 1-1, a coupling conjugated diene polymer (sample 1-23) was obtained, which has a 4-branch structure derived from the branching agent structure (1) in a part of the main chain and an 8-branch star polymer structure derived from the coupling agent. The physical properties of sample 1-23 are shown in Table 3.

[0292] ( Reference example 1-24) Coupling conjugated diene polymer (sample 1-24) The branching agent trimethoxy(4-vinylphenyl)silane (abbreviated as "BS-1" in the table) The amount of addition was changed from 0.0190mmol / min to 0.0250mmol / min, and the coupling The agent was converted from tetraethoxysilane to tetrakis(3-trimethoxysilylpropyl)-1,3 - Propanediamine (abbreviated as "F" in the table) was added in an amount of 0.0190mmol Except for changing to l / min. Reference example In the same manner as in 1-1, a coupling conjugated diene polymer (sample 1-24) was obtained, which has a 4-branch structure derived from the branching agent structure (1) in a part of the main chain and an 8-branch star polymer structure derived from the coupling agent. The physical properties of sample 1-24 are shown in Table 4.

[0293] ( Reference example 1-25) Coupling conjugated diene polymer (sample 1-25) The branching agent trimethoxy(4-vinylphenyl)silane (abbreviated as "BS-1" in the table) The amount of addition was changed from 0.0190mmol / min to 0.0350mmol / min, and the coupling The agent was converted from tetraethoxysilane to tetrakis(3-trimethoxysilylpropyl)-1,3 - Propanediamine (abbreviated as "F" in the table) was added in an amount of 0.0190mmol Except for changing to l / min. Reference example In the same manner as in 1-1, a coupling conjugated diene polymer (sample 1-25) was obtained, which has a 4-branch structure derived from the branching agent structure (1) in a part of the main chain and an 8-branch star polymer structure derived from the coupling agent. The physical properties of sample 1-25 are shown in Table 4.

[0294] ( Reference example 1-26) Coupling conjugated diene polymer (sample 1-26) Coupling agent was converted from tetraethoxysilane to tetrakis(3-trimethoxysilylpropane) (Pyryl)-1,3-propanediamine (abbreviated as "F" in the table), and the amount added was 0. 0190mmol / min, and changed to SRAE oil added as a rubber softener, and liquid Except for the addition of rubber (Kuraray Co., Ltd. liquid polybutadiene LBR-302), Reference example In the same manner as in 1-1, a coupling conjugated diene polymer (sample 1-26) was obtained, which has a 4-branch structure derived from the branching agent structure (1) in a part of the main chain and an 8-branch star polymer structure derived from the coupling agent. The physical properties of sample 1-26 are shown in Table 4.

[0295] ( Reference example 1-27) Coupling conjugated diene polymer (sample 1-27) Coupling agent was converted from tetraethoxysilane to tetrakis(3-trimethoxysilylpropane) (Pyryl)-1,3-propanediamine (abbreviated as "F" in the table), and the amount added was 0. 0190mmol / min, and SRAE oil was added as a rubber softener. Except for the addition of terpene resin YS Resin PX1250 manufactured by Yasuhara Chemical Co., Ltd. , Reference example In the same manner as in 1-1, a coupling conjugated diene polymer (sample 1-27) was obtained, which has a 4-branch structure derived from the branching agent structure (1) in a part of the main chain and an 8-branch star polymer structure derived from the coupling agent. The physical properties of sample 1-27 are shown in Table 4.

[0296] ( Reference example 1-28) Coupling conjugated diene polymer (sample 1-28) Coupling agent was converted from tetraethoxysilane to tetrakis(3-trimethoxysilylpropane) (Pyryl)-1,3-propanediamine (abbreviated as "F" in the table), and the amount added was 0. 0190mmol / min, and SRAE oil added as a rubber softener, and naphtha Except for the addition of naphthenic oil (Nytex810, naphthenic oil manufactured by Nynas), Reference example In the same manner as in 1-1, a coupling conjugated diene polymer (sample 1-28) was obtained, which has a 4-branch structure derived from the branching agent structure (1) in a part of the main chain and an 8-branch star polymer structure derived from the coupling agent. The physical properties of sample 1-28 are shown in Table 4.

[0297] ( Reference example 1-29) Coupling conjugated diene polymer (sample 1-29) Coupling agent was converted from tetraethoxysilane to tetrakis(3-trimethoxysilylpropane) (Pyryl)-1,3-propanediamine (abbreviated as "F" in the table), and the amount added was 0. The flow rate was changed to 0.190 mmol / min, and no rubber softener was added. Reference example In the same manner as in 1-1, a coupling conjugated diene polymer (sample 1-29) was obtained, which has a 4-branch structure derived from the branching agent structure (1) in a part of the main chain and an 8-branch star polymer structure derived from the coupling agent. The physical properties of sample 1-29 are shown in Table 4.

[0298] ( Reference example 1-30) Coupling conjugated diene polymer (sample 1-30) Coupling agent was converted from tetraethoxysilane to tetrakis(3-trimethoxysilylpropane) (Pyryl)-1,3-propanediamine (abbreviated as "F" in the table), and the amount added was 0. The amount of SRAE oil added as a rubber softener was increased by 0.190 mmol / min. Other than changing the amount from 25.0g to 37.5g per 100g of combined weight, Reference example In the same manner as in 1-1, a coupling conjugated diene polymer (sample 1-30) was obtained, which has a 4-branch structure derived from the branching agent structure (1) in a part of the main chain and an 8-branch star polymer structure derived from the coupling agent. The physical properties of sample 1-30 are shown in Table 4.

[0299] ( Reference example 1-31) Conjugated diene polymer (sample 1-31) When the polymerization is sufficiently stable, trimethoprim is added as a branching agent to the bottom of the second reactive group. 0.0190mmol bis(4-vinylphenyl)silane (abbreviated as "BS-1" in the table). 1 / min, except that no coupling agent was added. Reference example In the same manner as in 1-1, a conjugated diene polymer (sample 1-31) was obtained, which has a 4-branch structure derived from the branching agent structure (1) in a part of the main chain and does not show a star-shaped coupling structure derived from the coupling agent. The physical properties of sample 1-31 are shown in Table 5.

[0300] ( Reference example1-32) Coupling conjugated diene polymer (sample 1-32) When the polymerization is sufficiently stable, trimethoprim is added as a branching agent to the bottom of the second reactive group. 0.0190mmol bis(4-vinylphenyl)silane (abbreviated as "BS-1" in the table). The coupling agent was tetraethoxysilane (represented as "A" in the table) at a rate of 1 / min. The amount of added 100 mmol / min was changed from 0.0480 mmol / min to 0.0120 mmol / min. Outside, Reference example In the same manner as in 1-1, a coupling conjugated diene polymer (sample 1-32) was obtained, which has a 4-branch structure derived from the branching agent structure (1) in a part of the main chain and a 3-branch star polymer structure derived from the coupling agent. The physical properties of sample 1-32 are shown in Table 5.

[0301] ( Reference example 1-33) Coupling conjugated diene polymer (sample 1-33) When the polymerization is sufficiently stable, trimethoprim is added as a branching agent to the bottom of the second reactive group. 0.0190mmol bis(4-vinylphenyl)silane (abbreviated as "BS-1" in the table). The coupling agent was tetraethoxysilane to tetrakis( 3-trimethoxysilylpropyl)-1,3-propanediamine (abbreviated as "F" in the table. ) and the amount added was changed to 0.0038mmol / min. Reference example In the same manner as in 1-1, a coupling conjugated diene polymer (sample 1-33) was obtained, which has a 4-branch structure derived from the branching agent structure (1) in a part of the main chain and an 8-branch star polymer structure derived from the coupling agent. The physical properties of sample 1-33 are shown in Table 5.

[0302] ( Reference example 1-34) Coupling conjugated diene polymer (sample 1-34) When the polymerization is sufficiently stable, dimethyl ether is added as a branching agent to the bottom of the second reactive group. Methoxy(4-vinylphenyl)silane (abbreviated as "BS-2" in the table) at 0.0350 The coupling agent tetraethoxysilane was added at a rate of 0.0 mmol / min. Except for changing from 480mmol / min to 0.0120mmol / min, Reference example In the same manner as in 1-1, a coupling conjugated diene polymer (sample 1-34) was obtained, which has a bi-branched structure derived from the branching agent structure (1) in a part of the main chain and a tri-branched star polymer structure derived from the coupling agent. The physical properties of sample 1-34 are shown in Table 5.

[0303] ( Reference example 1-35) Coupling conjugated diene polymer (sample 1-35) When the polymerization is sufficiently stable, the 1,1- Bis(4-(dimethylmethoxysilyl)phenyl)ethylene (abbreviated as "BS-3" in the table) ) was added at a rate of 0.0120 mmol / min, and the coupling agent tetraethoxysilane Except for changing the amount of added water from 0.0480mmol / min to 0.0120mmol / min, Reference example In the same manner as in 1-1, a coupling conjugated diene polymer (sample 1-35) was obtained, which has a three-branched structure derived from the branching agent structure (2) in a part of the main chain and a three-branched star polymer structure derived from the coupling agent. The physical properties of sample 1-35 are shown in Table 5.

[0304] ( Reference example 1-36) Coupling conjugated diene polymer (sample 1-36) The coupling agent was prepared by converting tetraethoxysilane to 3-(benzylideneamino)propyl trimethylsilane. Ethoxysilane (abbreviated as "G" in the table) was added in an amount of 0.0620 mmol / Other than changing it to minutes, Reference exampleIn the same manner as in 1-1, a coupling conjugated diene polymer (sample 1-36) was obtained, which has a 4-branch structure derived from the branching agent structure (1) in a part of the main chain and a 2-branch star polymer structure derived from the coupling agent. The physical properties of sample 1-36 are shown in Table 5.

[0305] ( Reference example 1-37) Coupling conjugated diene polymer (sample 1-37) 1,3-butadiene added to the first reactor from 18.6g / min to 13.95g / min The branching agent and 1,3-butadiene were added at 4.65g from the bottom of the second reaction unit. g / min. Reference example In the same manner as in 1-1, a coupling conjugated diene polymer (sample 1-37) was obtained, which has a 4-branch structure derived from the branching agent structure (1) in a part of the main chain and a 4-branch star polymer structure derived from the coupling agent. The physical properties of sample 1-37 are shown in Table 5.

[0306] ( Reference example A-1) Coupling conjugated diene polymer (sample A-1) The internal volume is 10 L, and the ratio of internal height (L) to diameter (D) (L / D) is 4.0. The reactor is a tank type reactor with an agitator, an inlet at the bottom and an outlet at the top, and has a jar for temperature control. Two tank-type pressure vessels with a tank cap were connected together as polymerization reactors. 1,3-butadiene, which had been previously dehydrated, was fed at 14 g / min and styrene at 10.0 g / min. n-Hexane was mixed at 175.2 g / min. The mixture was mixed in a static mixer provided in the pipe that supplied the mixture to the inlet of the reactor. n-Butyllithium was added at 0.103mmol / min to inactivate the remaining impurities. After mixing, the mixture was continuously fed to the bottom of the reactor. n-Butylpropane was used as a polymerization initiator at a rate of 0.081 mmol / min. The first reactor is vigorously mixed with a stirrer at a rate of 0.143 mmol / min. The internal temperature of the reactor was maintained at 67°C. The polymer solution was continuously withdrawn from the top of the first reactor and continuously poured into the bottom of the second reactor. The reaction was continued at 70°C, and then the mixture was fed to the static mixer from the top of the second unit. When the polymerization is sufficiently stable, 1,3-butadiene and styrene are copolymerized. From the bottom of the second reactive group, the branching agent trimethoxy(4-vinylphenyl)silane ( In the table, this is abbreviated as "BS-1.") was administered at a rate of 0.0190 mmol / min, and in parallel, 1, 3-Butadiene was added at a rate of 4.6 g / min to obtain a conjugated diene polymer having a main chain branched structure. Polymerization and branching reactions were carried out using the above-mentioned copolymer. After the polymerization reaction and the branching reaction were stabilized, the conjugated diene before the addition of the coupling agent was A small amount of the polymer solution was taken out, and the antioxidant (BHT) was adjusted to 0.2 g per 100 g of polymer. After the solvent was removed, the Mooney viscosity at 110°C and various molecular weights were measured. The physical properties are shown in Table 7. Next, the polymer solution discharged from the outlet of the reactor was mixed with a coupling agent of 2,2-dimethoxyphenyl -1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane (see table (abbreviated as "D"), and the amount added was 0.0360 mmol / min. The mixture was mixed using a static mixer and subjected to a coupling reaction. At this time, the time until the coupling agent is added to the polymer solution flowing out from the outlet of the reactor The time was 4.8 minutes and the temperature was 68°C. The temperature in the polymerization process and the addition of the coupling agent were The difference in temperature between the time of the test and the time of the test was 2°C. After the coupling reaction, a small amount of the conjugated diene polymer solution was extracted and an antioxidant (BHT) was added. After adding 0.2 g per 100 g of polymer, the solvent was removed and the amount of bound styrene was measured. (Physical property 6), and the microstructure of the butadiene portion (1,2-vinyl bond amount: Physical property 7) were measured. The measurement results are shown in Table 7. Next, add an antioxidant (BHT) to the polymer solution after the coupling reaction for 100 g of polymer. The amount of n-hexane solution was continuously added at 0.055 g / min so that the amount was 0.2 g per unit time. The coupling reaction was terminated. At the same time as an antioxidant, SRAE oil (J) was used as a rubber softener for 100 g of polymer. X Nippon Oil & Energy Corporation JOMO Process NC140) was added to make 25.0 g. The ingredients were added continuously and mixed with a static mixer. The solvent is removed by steam stripping, and the main chain is partially substituted with the compound represented by the above formula (1). The branching agent (hereinafter also referred to as "branching agent structure (1)") is a compound having a four-branched structure. Coupling conjugated diene based copolymer with a four-branch star polymer structure derived from the coupling agent. A polymer (sample A-1) was obtained. The physical properties of sample A-1 are shown in Table 7. The polymer before the addition of the branching agent, the polymer after the addition of the branching agent, and the polymer after the addition of the coupling agent are The molecular weight of the polymer in each process was measured by GPC and the molecular weight was measured by GPC with a viscometer. The structure of the coupling conjugated diene polymer was identified by comparing with the branching degree by the method described above.

[0307] ( Reference example A-2) Coupling conjugated diene polymer (sample A-2) The internal volume is 10 L, and the ratio of internal height (L) to diameter (D) (L / D) is 4.0. The reactor is a tank type reactor with an agitator, an inlet at the bottom and an outlet at the top, and has a jar for temperature control. Two tank-type pressure vessels with a tank cap were connected together as polymerization reactors. The water was removed in advance, and the 1,3-butadiene was fed at 14 g / min, styrene at 8.0 g / min, and n -Hexane was mixed at 175.2 g / min. The mixture was mixed in a static mixer provided in the pipe that supplied the mixture to the inlet of the reactor. n-Butyllithium was added at 0.103mmol / min to inactivate the remaining impurities. After mixing, the mixture was continuously fed to the bottom of the reactor. n-Butylpropane was used as a polymerization initiator at a rate of 0.081 mmol / min. The first reactor is vigorously mixed with a stirrer at a rate of 0.143 mmol / min. The internal temperature of the reactor was maintained at 67°C. The polymer solution was continuously withdrawn from the top of the first reactor and continuously poured into the bottom of the second reactor. The reaction was continued at 70°C, and then the mixture was fed to the static mixer from the top of the second unit. When the polymerization is sufficiently stable, 1,3-butadiene and styrene are copolymerized. From the bottom of the second reactive group, the branching agent trimethoxy(4-vinylphenyl)silane ( In the table, this is abbreviated as "BS-1.") was administered at a rate of 0.0190 mmol / min, and in parallel, 1, 3-Butadiene was added at 4.6 g / min and styrene at 2.0 g / min to obtain a polymer with a branched main chain structure. The polymerization reaction and branching reaction were carried out to obtain a conjugated diene polymer. After the polymerization reaction and the branching reaction were stabilized, the conjugated diene before the addition of the coupling agent was A small amount of the polymer solution was taken out, and the antioxidant (BHT) was adjusted to 0.2 g per 100 g of polymer. After the solvent was removed, the Mooney viscosity at 110°C and various molecular weights were measured. The physical properties are shown in Table 7. Next, a coupling agent was added to the polymer solution discharged from the outlet of the reactor. 1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane (Table (abbreviated as "D"), and the amount added was 0.0360 mmol / min. The mixture was mixed using a static mixer and subjected to a coupling reaction. At this time, the time until the coupling agent is added to the polymer solution flowing out from the outlet of the reactor The time was 4.8 minutes and the temperature was 68°C. The temperature in the polymerization process and the addition of the coupling agent were The difference in temperature between the time when the coupling reaction was completed and the time when the coupling reaction was completed was 2°C. A small amount was taken out and an antioxidant (BHT) was added so that the amount was 0.2 g per 100 g of polymer. After that, the solvent was removed, and the amount of bound styrene (physical property 6) and the microstructure of the butadiene portion (1 The physical properties7) of the 2-vinyl bond content were measured. The results are shown in Table 7. Next, add an antioxidant (BHT) to the polymer solution after the coupling reaction for 100 g of polymer. The amount of n-hexane solution was continuously added at 0.055 g / min so that the amount was 0.2 g per unit time. The coupling reaction was terminated. At the same time as an antioxidant, SRAE oil (J) was used as a rubber softener for 100 g of polymer. X Nippon Oil & Energy Corporation JOMO Process NC140) was added to make 25.0 g. The ingredients were added continuously and mixed with a static mixer. The solvent is removed by steam stripping, and the main chain is partially substituted with the compound represented by the above formula (1). The branching agent (hereinafter also referred to as "branching agent structure (1)") is a compound having a four-branched structure. Coupling conjugated diene based copolymer with a four-branch star polymer structure derived from the coupling agent. A polymer (sample A-2) was obtained. The physical properties of sample A-2 are shown in Table 7. The polymer before the addition of the branching agent, the polymer after the addition of the branching agent, and the polymer after the addition of the coupling agent are The molecular weight of the polymer in each process was measured by GPC and the molecular weight was measured by GPC with a viscometer. The structure of the coupling conjugated diene polymer was identified by comparing with the branching degree by the method described above.

[0308] [Coupling Conjugated Diene Polymer] (Comparative Example 1-1) Coupling conjugated diene polymer (Sample 1-38) Two tank-type pressure vessels having an internal volume of 10 L, an internal height (L) to diameter (D) ratio (L / D) of 4.0, an inlet at the bottom and an outlet at the top, and an agitator as a tank-type reactor and a jacket for temperature control were connected together as polymerization reactors. 1,3-butadiene, which had been previously dehydrated, was mixed at 18.6 g / min, styrene at 10.0 g / min, and n-hexane at 175.2 g / min. In a static mixer installed in the middle of the pipe supplying this mixed solution to the inlet of the reactor, n-butyllithium for inactivating remaining impurities was added at 0.103 mmol / min, mixed, and then continuously supplied to the bottom of the reactor. Furthermore, 2,2-bis(2-oxolanyl)propane as a polar substance was supplied at a rate of 0.081 mmol / min, and n-butyllithium as a polymerization initiator was supplied at a rate of 0.143 mmol / min to the bottom of the first reactor, which was vigorously mixed with a stirrer, and the temperature inside the reactor was maintained at 67°C. The polymer solution was continuously withdrawn from the top of the first reactor and continuously fed to the bottom of the second reactor to continue the reaction at 70°C, and then fed to a static mixer from the top of the second reactor. When the polymerization was sufficiently stable, a small amount of the polymer solution before the addition of the coupling agent was withdrawn, and an antioxidant (BHT) was added so that the amount was 0.2 g per 100 g of polymer, after which the solvent was removed and the Mooney viscosity at 110°C and various molecular weights were measured. The physical properties are shown in Table 6. Next, tetraethoxysilane (abbreviated as "A" in the table) was continuously added as a coupling agent to the polymer solution flowing out from the outlet of the reactor at a rate of 0.0480 mmol / min, and mixed using a static mixer to carry out a coupling reaction. At this time, the time until the coupling agent was added to the polymer solution flowing out from the outlet of the reactor was 4.8 minutes, the temperature was 68°C, and the difference between the temperature in the polymerization process and the temperature before the coupling agent was added was 2°C. A small amount of the conjugated diene polymer solution after the coupling reaction was extracted, and an antioxidant (BHT) was added so that the amount was 0.2 g per 100 g of polymer, and then the solvent was removed, and the amount of bound styrene (physical property 6) and the microstructure of the butadiene portion (1,2-vinyl bond amount: physical property 7) were measured. The measurement results are shown in Table 6. Next, an antioxidant (BHT) was continuously added to the polymer solution after the coupling reaction at 0.055 g / min (n-hexane solution) so that the amount was 0.2 g per 100 g of polymer, and the coupling reaction was terminated. Simultaneously with the antioxidant, SRAE oil (JOMO Process NC140 manufactured by JX Nippon Oil & Energy Corporation) was continuously added as a rubber softener so that the amount was 25.0 g per 100 g of polymer, and mixed with a static mixer. The solvent was removed by steam stripping to obtain a coupling conjugated diene polymer (sample 1-38) having no main chain branching derived from the branching agent and having a three-branched star polymer structure derived from the coupling agent. The physical properties of sample 1-38 are shown in Table 6.

[0309] (Comparative Example 1-2) Coupling conjugated diene polymer (Sample 1-39) The coupling agent was changed from tetraethoxysilane to 2,2-dimethoxy-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane (abbreviated as "D" in the table), and the amount of the coupling agent was changed to 0.0360mmol / min. In the same manner as in Comparative Example 1-1, a coupling conjugated diene polymer (sample 1-39) was obtained that has no main chain branching derived from the branching agent and has a four-branch star polymer structure derived from the coupling agent. The physical properties of sample 1-39 are shown in Table 6.

[0310] (Comparative Example 1-3) Coupling conjugated diene polymer (Sample 1-40) The coupling agent was changed from tetraethoxysilane to tetrakis(3-trimethoxysilylpropyl)-1,3-propanediamine (abbreviated as "F" in the table), and the amount of the coupling agent was changed to 0.0190mmol / min. In the same manner as in Comparative Example 1-1, a coupling conjugated diene polymer (sample 1-40) was obtained that has no main chain branching derived from the branching agent and has an 8-branch star polymer structure derived from the coupling agent. The physical properties of sample 1-40 are shown in Table 6.

[0311] (Comparative Example B-1) Coupling Conjugated Diene Polymer (Sample B-1) Two tank-type pressure vessels having an internal volume of 10 L, an internal height (L) to diameter (D) ratio (L / D) of 4.0, an inlet at the bottom and an outlet at the top, and an agitator as a tank-type reactor and a jacket for temperature control were connected together as polymerization reactors. 1,3-butadiene, from which moisture had been removed in advance, was mixed at a flow rate of 18.6 g / min, styrene at 10.0 g / min, and n-hexane at 175.2 g / min. In a static mixer installed in the middle of the pipe supplying this mixed solution to the inlet of the reactor, n-butyllithium for inactivating remaining impurities was added at 0.103 mmol / min, mixed, and then continuously supplied to the bottom of the reactor. Furthermore, 2,2-bis(2-oxolanyl)propane as a polar substance at a rate of 0.081 mmol / min and n-butyllithium as a polymerization initiator at a rate of 0.143 mmol / min were supplied to the bottom of the first reactor, which was vigorously mixed with a stirrer, and the temperature inside the reactor was maintained at 67°C. The polymer solution was continuously withdrawn from the top of the first reactor and continuously fed to the bottom of the second reactor to continue the reaction at 70°C, and then fed to the static mixer from the top of the second reactor. When the polymerization was sufficiently stabilized, a small amount of the polymer solution before the addition of the coupling agent was withdrawn, and an antioxidant (BHT) was added so that the amount was 0.2 g per 100 g of polymer, after which the solvent was removed and the Mooney viscosity at 110°C and various molecular weights were measured. The physical properties are shown in Table 7. Next, trimethoxy(4-vinylphenyl)silane (abbreviated as "BS-1" in the table) was added to the polymer solution discharged from the outlet of the reactor at a rate of 0.0190 mmol / min, and at the same time, tetraethoxysilane (abbreviated as "A" in the table) was continuously added at a rate of 0.0480 mmol / min. The mixture was mixed using a static mixer to carry out a coupling reaction. At this time, the time until the coupling agent was added to the polymer solution flowing out from the outlet of the reactor was 4.8 minutes, the temperature was 68 ° C, and the difference between the temperature in the polymerization process and the temperature before the coupling agent was added was 2 ° C. A small amount of the conjugated diene polymer solution after the coupling reaction was withdrawn, and an antioxidant (BHT) was added so that the amount was 0.2 g per 100 g of polymer, and then the solvent was removed, and the bound styrene amount (physical property 6) and the microstructure of the butadiene portion (1,2-vinyl bond amount: physical property 7) were measured. The measurement results are shown in Table 7. Next, an antioxidant (BHT) was continuously added to the polymer solution after the coupling reaction at 0.055 g / min (n-hexane solution) so that the amount was 0.2 g per 100 g of polymer, and the coupling reaction was terminated. Simultaneously with the antioxidant, SRAE oil (JOMO Process NC140 manufactured by JX Nippon Oil & Energy Corporation) was continuously added as a rubber softener so that the amount was 25.0 g per 100 g of polymer, and mixed with a static mixer. The solvent was removed by steam stripping to obtain a coupling conjugated diene polymer (sample B-1). The physical properties of sample B-1 are shown in Table 7. In Comparative Example B-1 of Table 7 below, "BS-1" is listed in the column for branching agent. However, in the addition method in which "BS-1" and "A" were added simultaneously as in this example, a main chain branch point could not be formed, and thus the branching agent did not function. The structure of the coupled conjugated diene polymer was identified by comparing the molecular weight measured by GPC and the branching degree measured by GPC equipped with a viscometer for the polymer before the addition of "BS-1", the polymer after the addition of "BS-1", and the polymer in each step after the addition of "A".

[0312] (Comparative Example B-2) Coupling conjugated diene polymer (sample B-2) No branching agent was used. In addition, the coupling agent used was the coupling agent shown in (Z-1) below (abbreviated as "Z-1" in the table), and the amount added was 0.0360 mmol / min. Otherwise, in the same manner as in Comparative Example B-1, a coupling conjugated diene polymer (sample B-2) was obtained that had no main chain branching derived from the branching agent and had a 10-branch star polymer structure derived from the coupling agent. The physical properties of sample B-2 are shown in Table 7.

[0313] [ka]

[0314] [Table 1]

[0315] [Table 2]

[0316] [Table 3]

[0317] [Table 4]

[0318] [Table 5]

[0319] [Table 6]

[0320] [Table 7]

[0321] ( Reference example 1-38~1-74, Reference example a-1 to 2, and Comparative Examples 1-4 to 1-6, and Comparative Examples b-1 to 2) Samples 1-1 to 1-40 shown in Tables 1 to 6 and samples (A-1 to 2, B-1 to 2) is used as the raw rubber, and the rubber composition containing each raw rubber is prepared according to the formula shown below. I got something.

[0322] (Rubber component) Branched conjugated diene polymers and coupled conjugated diene polymers (samples 1-1 to 1-40, A-1 to 2, B-1 to 2) : 80 parts by weight (excluding rubber softener) High cis polybutadiene (product name "UBEPOL BR150" manufactured by Ube Industries) :20 parts by mass

[0323] (Combination conditions) The amount of each compounding ingredient added is shown in parts by mass per 100 parts by mass of the rubber component not including the rubber softener. Silica 1 (product name "Ultrasil 7000GR" manufactured by Evonik Degussa) Nitrogen adsorption specific surface area 170m2 / g): 50.0 parts by mass Silica 2 (Rhodia product name "Zeosil Premium 200MP") Nitrogen adsorption specific surface area 220m2 / g): 25.0 parts by mass Carbon black (product name "Seast KH (N339)" manufactured by Tokai Carbon Co., Ltd.) :5.0 parts by mass Silane coupling agent (product name "Si75" manufactured by Evonik Degussa, bis(triethoxysilylpropyl) disulfide): 6.0 parts by mass SRAE oil (product name "Process NC140" manufactured by JX Nippon Oil & Energy Corporation) :42.0 parts by mass (This includes the amount previously added as a rubber softener in Samples 1-1 to 1-40, A-1 to 2, and B-1 to 2.) ·Zinc white: 2.5 parts by mass Stearic acid: 1.0 parts by weight Anti-aging agent (N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine): 2.0 parts by mass ·Sulfur: 2.2 parts by mass Vulcanization accelerator 1 (N-cyclohexyl-2-benzothiazylsulfinamide) :1.7 parts by mass Vulcanization accelerator 2 (diphenyl guanidine): 2.0 parts by mass ·Total: 239.4 parts by mass

[0324] (Mixing method) The above materials were kneaded by the following method to obtain a rubber composition. Using an internal kneader (capacity 0.3 L) equipped with a temperature control device, the raw rubber (samples 1-1 to 1-40, samples A-1 to 2, samples B-1 to 2), fillers (silica 1, silica 2, carbon black), silane coupling agent, SRAE oil, zinc oxide, and stearic acid were kneaded under the conditions of a filling rate of 65% and a rotor rotation speed of 30 to 50 rpm in the first stage of kneading. At this time, the temperature of the internal kneader was controlled, and each rubber composition (compound) was obtained at a discharge temperature of 155 to 160°C. Next, as the second stage of kneading, the mixture obtained above was cooled to room temperature, and then the antioxidant was added and kneaded again to improve the dispersion of the silica. In this case, the discharge temperature of the mixture was adjusted to 155 to 160°C by controlling the temperature of the kneader. After cooling, in the third stage of kneading, sulfur and vulcanization accelerators 1 and 2 were added and kneaded using an open roll set at 70°C. Thereafter, the product was molded and vulcanized in a vulcanization press at 160°C for 20 minutes. The rubber compositions before and after vulcanization were evaluated. Specifically, the evaluation was performed by the following methods. The results are shown in Tables 8 to 14.

[0325] [Evaluation of characteristics] (Evaluation 1) Compound Mooney Viscosity The compound obtained above after the second mixing step and before the third mixing step was used as a sample, and the viscosity was measured using a Mooney viscometer in accordance with ISO 289 after preheating at 130°C for 1 minute and rotating the rotor at 2 revolutions per minute for 4 minutes. The results of Comparative Examples 1-4 were indexed to 100. The smaller the index, the better the processability.

[0326] (Evaluation 2) Tensile strength and tensile elongation The tensile strength and tensile elongation were measured according to the tensile test method of JIS K6251, and indexed with the results of Comparative Examples 1-4 set at 100. A larger index indicates better tensile strength and tensile elongation (breaking strength).

[0327] (Rating 3) Abrasion resistance Using an Acron abrasion tester (manufactured by Yasuda Seiki Seisakusho Co., Ltd.), the amount of wear was measured at a load of 44.4 N and 1000 revolutions in accordance with JIS K6264-2, and indexed with the results of Comparative Examples 1-4 set at 100. A higher index indicates better abrasion resistance.

[0328] (Evaluation 4) Viscoelastic parameters Viscoelastic parameters were measured in torsion mode using a viscoelasticity tester "ARES" manufactured by Rheometrics Scientific Co., Ltd. Each measured value was indexed with the result for the rubber composition of Comparative Example 1-4 set at 100. Tan δ measured at 0°C, a frequency of 10 Hz, and a strain of 1% was used as an index of wet skid resistance. A higher index value indicates better wet skid resistance. In addition, tan δ measured at 50°C, a frequency of 10 Hz, and a strain of 3% was used as an index of fuel economy. The smaller the index, the better the fuel economy. Furthermore, the elastic modulus (G') measured at 50°C, a frequency of 10 Hz, and a strain of 3% was used as an index of steering stability. A higher index value indicates better steering stability.

[0329] [Table 8]

[0330] [Table 9]

[0331] [Table 10]

[0332] [Table 11]

[0333] [Table 12]

[0334] [Table 13]

[0335] [Table 14]

[0336] As shown in Tables 8 to 13, compared with Comparative Examples 1-4 to 1-6, Examples 1-38 to 1-74 showed low compound Mooney viscosity when vulcanized and good processability, and were confirmed to have excellent abrasion resistance, handling stability, and rupture strength when vulcanized, as well as an excellent balance between low hysteresis loss and wet skid resistance. As shown in Table 14, it was confirmed that, compared with Comparative Examples b-1 and b-2, Examples a-1 and a-2 had low Mooney viscosity of the compound when vulcanized and showed good processability, and when vulcanized, had excellent abrasion resistance, handling stability and fracture strength, and also had an excellent balance between low hysteresis loss and wet skid resistance.

[0337] Second Example Hereinafter, as a second embodiment, the present embodiment will be described in more detail by giving specific examples and comparative examples, but the present embodiment is not limited in any way by the following examples and comparative examples. Hereinafter, a conjugated diene polymer modified with a modifying agent will be referred to as a "modified conjugated diene polymer", and a conjugated diene polymer coupled with a coupling agent will be referred to as a "coupled conjugated diene polymer". Moreover, the conjugated diene polymer in an unmodified state is referred to as an "unmodified conjugated diene polymer." In the tables, it is simply referred to as a "conjugated diene polymer." Furthermore, a conjugated diene polymer having a branched structure is referred to as a "branched conjugated diene polymer." Various physical properties in the examples and comparative examples were measured by the methods shown below.

[0338] (Physical Properties 1) Polymer Mooney Viscosity The conjugated diene polymer before the modification reaction, the conjugated diene polymer modified with a silicon- and sulfur-containing modifier (modified conjugated diene polymer), and the conjugated diene polymer modified with a silicon- and sulfur-containing modifier and further coupled with a coupling agent (coupled conjugated diene polymer) were used as samples, and the Mooney viscosity was measured using a Mooney viscometer (manufactured by Ueshima Seisakusho Co., Ltd., product name "VR1132") using an L-type rotor in accordance with ISO 289. The measurement temperature was 110°C when the sample was a conjugated diene polymer before the modification reaction, and 100°C when the sample was a conjugated diene polymer modified with a silicon atom- and sulfur atom-containing modifier, or a polymer modified with a silicon atom- and sulfur atom-containing modifier and further coupled with a coupling agent. First, the sample was preheated at the test temperature for 1 minute, and then the rotor was rotated at 2 rpm. The torque was measured after 4 minutes to determine the Mooney viscosity (ML (1+4) ) was decided.

[0339] (Physical property 2) Branching degree (Bn) The branching degree (Bn) of the conjugated diene polymer was measured by a GPC-light scattering method equipped with a viscosity detector as follows. The modified conjugated diene polymer and the coupled conjugated diene polymer were used as samples, and measurements were performed using a gel permeation chromatography (GPC) measuring device (manufactured by Malvern under the trade name "GPCmax VE-2001") in which three columns packed with polystyrene gel were connected together, and three detectors were connected in this order: a light scattering detector, an RI detector, and a viscosity detector (manufactured by Malvern under the trade name "TDA305"). Based on standard polystyrene, the absolute molecular weight was determined from the results of the light scattering detector and the RI detector, and the intrinsic viscosity was determined from the results of the RI detector and the viscosity detector. Linear polymer has an intrinsic viscosity [η] = -3.883M 0.771 The shrinkage factor (g') was calculated as the ratio of the intrinsic viscosity corresponding to each molecular weight, where M represents the absolute molecular weight. The obtained shrinkage factor (g') was then used to calculate the branching degree (Bn), defined as g' = 6Bn / [(Bn+1)(Bn+2)]. The eluent used was tetrahydrofuran (hereinafter also referred to as "THF") containing 5 mmol / L triethylamine. The columns used were "TSKgel G4000HXL", "TSKgel G5000HXL", and "TSKgel G6000HXL" manufactured by Tosoh Corporation. 20 mg of the measurement sample was dissolved in 10 mL of THF to prepare a measurement solution, and 100 μL of the measurement solution was injected into a GPC measurement device and measured under conditions of an oven temperature of 40° C. and a THF flow rate of 1 mL / min.

[0340] (Physical property 3) Silicon atom content Sample purification: The modified conjugated diene polymer and the coupled conjugated diene polymer were used as samples. The samples were dissolved in toluene, and then a poor solvent, which was a mixture of ethanol and acetone in a volume ratio of 7:3, was added to the toluene solution of the sample to precipitate the polymer, and the rubber softener and stabilizer contained in the sample were removed. The recovered polymer was dissolved again in toluene, and the poor solvent was added to precipitate the polymer. After repeating this operation five times, the sample was dried for five hours in a vacuum dryer adjusted to 40°C to obtain a purified sample from which the rubber softener and stabilizer contained in the sample had been completely removed (hereinafter referred to as the purified sample). Sample digestion: After weighing the purified sample, 5 mL of 96% sulfuric acid (for atomic absorption spectrometry) and 3 mL of 60% nitric acid (for atomic absorption spectrometry) were added, and the purified sample was decomposed with acid using a microwave decomposition device (Milestone General ETHOS-1). After acid decomposition, the sample was diluted to 50 mL with pure water to prepare a sample for ICP analysis. Determination of silicon atomic weight: The amount of silicon in the purified sample prepared by the above method was measured using an inductively coupled plasma emission spectrometer (iCAP 7400 Duo, manufactured by Thermo Fisher Scientific). A calibration curve was prepared using an ICP silicon standard solution (Agilent) to quantify the amount of silicon in the purified sample.

[0341] (Physical property 4) Sulfur atom content Sample purification: The modified conjugated diene polymer and the coupled conjugated diene polymer were used as samples. The samples were dissolved in toluene, and then a poor solvent, which was a mixture of ethanol and acetone in a volume ratio of 7:3, was added to the toluene solution of the sample to precipitate the polymer, and the rubber softener and stabilizer contained in the sample were removed. The recovered polymer was dissolved again in toluene, and the poor solvent was added to precipitate the polymer. After repeating this operation five times, the sample was dried for five hours in a vacuum dryer adjusted to 40°C to obtain a purified sample from which the rubber softener and stabilizer contained in the sample had been completely removed (hereinafter referred to as the purified sample). Determination of sulfur atomic weight: The amount of sulfur in the refined sample was measured by oxidative decomposition-ultraviolet fluorescence method using a trace sulfur analyzer (Mitsubishi Chemical Analytech Co., Ltd. TS-2100H). A calibration curve was prepared using a toluene solution of dibutyl disulfide to quantify the amount of sulfur in the purified sample.

[0342] (Physical property 5) Molecular weight Measurement condition 1: The conjugated diene polymer before modification, the modified conjugated diene polymer, and the coupled conjugated diene polymer were used as samples, and chromatograms were measured using a GPC measurement device (manufactured by Tosoh Corporation under the trade name "HLC-8320GPC") in which three columns packed with polystyrene gel were connected together, and an RI detector (manufactured by Tosoh Corporation under the trade name "HLC8020"), and the weight average molecular weight (Mw), number average molecular weight (Mn), and molecular weight distribution (Mw / Mn) were determined based on a calibration curve obtained using standard polystyrene. The eluent used was tetrahydrofuran (THF) containing 5 mmol / L triethylamine. Three columns, Tosoh Corporation's "TSKgel SuperMultiporeHZ-H" (trade name), were connected, and a Tosoh Corporation's "TSKguardcolumn SuperMP(HZ)-H" (trade name) was connected in front of them as a guard column. 10 mg of the measurement sample was dissolved in 10 mL of THF to prepare a measurement solution, and 10 μL of the measurement solution was injected into a GPC measurement device and measured under conditions of an oven temperature of 40° C. and a THF flow rate of 0.35 mL / min. Among the various samples measured under the above measurement condition 1, samples whose molecular weight distribution (Mw / Mn) was less than 1.6 were measured again under the following measurement condition 2. For samples that were measured under measurement condition 1 and had a molecular weight distribution value of 1.6 or more, measurement was performed under measurement condition 1. Measurement condition 2: The conjugated diene polymer before modification, the modified conjugated diene polymer, and the coupled conjugated diene polymer were used as samples, and chromatograms were measured using a GPC measurement device in which three columns packed with polystyrene gel were connected, and the weight average molecular weight (Mw) and number average molecular weight (Mn) were determined based on a calibration curve using standard polystyrene. The eluent used was THF containing 5 mmol / L triethylamine. The columns used were the following: guard column: Tosoh Corporation's product name "TSKguardcolumn SuperH-H"; columns: Tosoh Corporation's product names "TSKgel SuperH5000", "TSKgel SuperH6000", and "TSKgel SuperH7000". An RI detector (manufactured by Tosoh Corporation under the trade name "HLC8020") was used under the conditions of an oven temperature of 40° C. and a THF flow rate of 0.6 mL / min. 10 mg of a sample to be measured was dissolved in 20 mL of THF to prepare a measurement solution, and 20 μL of the measurement solution was injected into a GPC measurement device for measurement. For samples that were measured under measurement condition 1 and had a molecular weight distribution value of less than 1.6, measurement was performed under measurement condition 2.

[0343] (Physical property 6) Bound styrene content A modified conjugated diene polymer not containing a rubber softener and a coupled conjugated diene polymer were used as samples, and 100 mg of the sample was dissolved in chloroform up to 100 mL to prepare a measurement sample. The amount of bound styrene (mass%) relative to 100 mass% of the sample modified conjugated diene polymer or coupled conjugated diene polymer was measured based on the amount of absorption of ultraviolet light by the phenyl group of styrene (near 254 nm) (measuring device: Shimadzu Corporation spectrophotometer "UV-2450").

[0344] (Physical property 7) Microstructure of butadiene part (1,2-vinyl bond amount) The modified conjugated diene polymer not containing a rubber softener and the coupled conjugated diene polymer were used as samples, and 50 mg of each sample was dissolved in 10 mL of carbon disulfide to prepare a measurement sample. Using a solution cell, infrared spectra are recorded from 600 to 1000 cm -1The absorbance at a predetermined wave number was measured in the range of 100 nm to 150 nm, and the microstructure of the butadiene portion, i.e., the amount of 1,2-vinyl bonds (mol%) was calculated according to the formula of Hampton's method (method described in R.R. Hampton, Analytical Chemistry 21, 923 (1949)) (measuring device: Fourier transform infrared spectrophotometer "FT-IR230" manufactured by JASCO Corporation).

[0345] [Branched conjugated diene polymer] (Example 2-1) Modified conjugated diene polymer (sample 2-1) Two tank-type pressure vessels having an internal volume of 10 L, an internal height (L) to diameter (D) ratio (L / D) of 4.0, an inlet at the bottom and an outlet at the top, and an agitator as a tank-type reactor and a jacket for temperature control were connected together as polymerization reactors. 1,3-butadiene, which had been previously dehydrated, was mixed at 18.6 g / min, styrene at 10.0 g / min, and n-hexane at 175.2 g / min to obtain a mixed solution. In a static mixer installed in the middle of the pipe supplying this mixed solution to the inlet of the reactor, n-butyllithium for inactivating remaining impurities was added at 0.103 mmol / min, mixed, and then continuously supplied to the bottom of the reactor. Furthermore, 2,2-bis(2-oxolanyl)propane as a polar substance was supplied at a rate of 0.081 mmol / min, and n-butyllithium as a polymerization initiator was supplied at a rate of 0.143 mmol / min to the bottom of the first reactor, which was vigorously mixed with a stirrer, and the temperature inside the reactor was maintained at 67°C. The polymer solution was continuously withdrawn from the top of the first reactor, continuously fed to the bottom of the second reactor, and the reaction was continued at 70°C, and further fed to a static mixer from the top of the second reactor. When the polymerization was sufficiently stabilized, trimethoxy(4-vinylphenyl)silane (abbreviated as "BS-1" in the table) was added as a branching agent from the bottom of the second reactor at a rate of 0.0191 mmol / min, and when the polymerization reaction and branching reaction were further stabilized, a small amount of the conjugated diene polymer solution before the addition of the modifier was withdrawn, an antioxidant (BHT) was added so that it was 0.2 g per 100 g of polymer, and then the solvent was removed, and the Mooney viscosity at 110°C and various molecular weights were measured. The physical properties are shown in Table 15. Next, S-trimethylsilylmercaptopropyltrimethoxysilane (abbreviated as "T-1" in the table) was continuously added as a modifier to the polymer solution flowing out from the outlet of the reactor at a rate of 0.073 mmol / min, and the mixture was mixed using a static mixer to carry out a modification reaction. At this time, the time until the modifier was added to the polymer solution flowing out from the outlet of the reactor was 4.8 minutes, the temperature was 68°C, and the difference between the temperature in the polymerization process and the temperature before the modifier was added was 2°C. An antioxidant (BHT) was continuously added to the modified polymer solution at 0.055 g / min (n-hexane solution) so that the amount was 0.2 g per 100 g of polymer, and the modification reaction was terminated. Simultaneously with the antioxidant, SRAE oil (JOMO Process NC140 manufactured by JX Nippon Oil & Energy Corporation) was continuously added as a rubber softener so that the amount was 25.0 g per 100 g of polymer, and the mixture was mixed using a static mixer. The solvent was removed by steam stripping to obtain a modified conjugated diene polymer (sample 2-1). The physical properties of sample 2-1 are shown in Table 15.

[0346] (Example 2-2) Modified conjugated diene polymer (sample 2-2) The modified conjugated diene polymer (sample 2-2) was obtained in the same manner as in Example 2-1, except that the modifying agent was changed from S-trimethylsilylmercaptopropyltrimethoxysilane to S-trimethylsilylmercaptopropylmethyldimethoxysilane (abbreviated as "T-2" in the table) and the amount of the modified agent was changed to 0.145 mmol / min. The physical properties of sample 2-2 are shown in Table 15.

[0347] (Example 2-3) Coupling conjugated diene polymer (sample 2-3) Before the addition of the modifying agent, tin tetrachloride was added continuously as a coupling agent at a rate of 0.011 mmol / min, and mixed using a static mixer to carry out a coupling reaction. Thereafter, S-trimethylsilylmercaptopropyltrimethoxysilane (abbreviated as "T-1" in the table) was added continuously at a rate of 0.045 mmol / min as a modifying agent, and the mixture was mixed using a static mixer in the latter stage to carry out a modification reaction. In the same manner as in Example 2-1, a coupling conjugated diene polymer (sample 2-3) was obtained. The physical properties of sample 2-3 are shown in Table 15.

[0348] (Example 2-4) Coupling conjugated diene polymer (sample 2-4) Before the addition of the modifying agent, tin tetrachloride was added continuously as a coupling agent at a rate of 0.011 mmol / min, and mixed using a static mixer to carry out a coupling reaction. Thereafter, the modifying agent was changed from S-trimethylsilylmercaptopropyltrimethoxysilane to S-trimethylsilylmercaptopropylmethyldimethoxysilane (abbreviated as "T-2" in the table), the amount of the modifying agent was changed to 0.099 mmol / min and added continuously, and the modified reaction was carried out by mixing using a static mixer in the latter stage. The procedure was the same as in Example 2-1, except that a coupling conjugated diene polymer (sample 2-4) was obtained. The physical properties of sample 2-4 are shown in Table 15.

[0349] (Example 2-5) Modified conjugated diene polymer (sample 2-5) The addition rate of 1,3-butadiene was changed from 18.6 g / min to 24.3 g / min, the addition rate of styrene was changed from 10.0 g / min to 4.3 g / min, and the addition amount of the polar substance 2,2-bis(2-oxolanyl)propane was changed from 0.081 mmol / min to 0.022 mmol / min, and the temperature of the second reactor was set to 80°C. At this time, the difference between the temperature in the polymerization step and the temperature before the modifier was added was 3°C, and the temperature at which the modifier was added was 77°C. Otherwise, a modified conjugated diene polymer (sample 2-5) was obtained in the same manner as in Example 2-1. The physical properties of sample 2-5 are shown in Table 15.

[0350] (Example 2-6) Modified conjugated diene polymer (sample 2-6) The addition rate of 1,3-butadiene was changed from 18.6 g / min to 17.2 g / min, the addition rate of styrene was changed from 10.0 g / min to 11.4 g / min, and the addition amount of the polar substance 2,2-bis(2-oxolanyl)propane was changed from 0.081 mmol / min to 0.283 mmol / min, and the temperature of the second reactor was set to 65°C. At this time, the difference between the temperature in the polymerization step and the temperature before the modifier was added was 2°C, and the temperature at which the modifier was added was 63°C. Otherwise, a modified conjugated diene polymer (sample 2-6) was obtained in the same manner as in Example 2-1. The physical properties of sample 2-6 are shown in Table 15.

[0351] (Example 2-7) Modified conjugated diene polymer (sample 2-7) The amount of n-butyllithium, which is a polymerization initiator, added was changed from 0.143mmol / min to 0.101mmol / min, and the amount of 2,2-bis(2-oxolanyl)propane, which is a polar substance, added was changed from 0.081mmol / min to 0.059mmol / min, but the same procedure as in Example 2-1 was followed to obtain a modified conjugated diene polymer (sample 2-7). The physical properties of sample 2-7 are shown in Table 15.

[0352] (Example 2-8) Modified conjugated diene polymer (sample 2-8) The amount of n-butyllithium, which is a polymerization initiator, added was changed from 0.143mmol / min to 0.152mmol / min, and the amount of 2,2-bis(2-oxolanyl)propane, which is a polar substance, added was changed from 0.081mmol / min to 0.086mmol / min, but the same procedure as in Example 2-1 was followed to obtain a modified conjugated diene polymer (sample 2-8). The physical properties of sample 2-8 are shown in Table 15.

[0353] (Example 2-9) Modified conjugated diene polymer (sample 2-9) A modified conjugated diene polymer (sample 2-9) was obtained in the same manner as in Example 2-1, except that the branching agent was changed from trimethoxy(4-vinylphenyl)silane to dimethylmethoxy(4-vinylphenyl)silane (abbreviated as "BS-2" in the table) and the amount of the branching agent was changed to 0.0383 mmol / min. The physical properties of sample 2-9 are shown in Table 15.

[0354] (Example 2-10) Modified conjugated diene polymer (sample 2-10) The branching agent was changed from trimethoxy(4-vinylphenyl)silane to dimethylmethoxy(4-vinylphenyl)silane (abbreviated as "BS-2" in the table), and the amount added was changed to 0.0383mmol / min, and the modifying agent was changed from S-trimethylsilylmercaptopropyltrimethoxysilane to S-trimethylsilylmercaptopropylmethyldimethoxysilane (abbreviated as "T-2" in the table), and the amount added was changed to 0.145mmol / min, but the same procedure as in Example 2-1 was used to obtain a modified conjugated diene polymer (sample 2-10). The physical properties of sample 2-10 are shown in Table 15.

[0355] (Example 2-11) Modified conjugated diene polymer (sample 2-11) A modified conjugated diene polymer (sample 2-11) was obtained in the same manner as in Example 2-1, except that the branching agent was changed from trimethoxy(4-vinylphenyl)silane to 1,1-bis(4-(dimethylmethoxysilyl)phenyl)ethylene (abbreviated as "BS-3" in the table) and the amount of the branching agent was changed to 0.0255 mmol / min. The physical properties of sample 2-11 are shown in Table 16.

[0356] (Example 2-12) Modified conjugated diene polymer (sample 2-12) A modified conjugated diene polymer (sample 2-12) was obtained in the same manner as in Example 2-1, except that the branching agent was changed from trimethoxy(4-vinylphenyl)silane to 1,1-bis(4-(dimethylmethoxysilyl)phenyl)ethylene (abbreviated as "BS-3" in the table) and the amount added was changed to 0.0255 mmol / min, and the modifying agent was changed from S-trimethylsilylmercaptopropyltrimethoxysilane to S-trimethylsilylmercaptopropylmethyldimethoxysilane (abbreviated as "T-2" in the table) and the amount added was changed to 0.145 mmol / min. The physical properties of sample 2-12 are shown in Table 16.

[0357] (Example 2-13) Modified conjugated diene polymer (sample 2-13) A modified conjugated diene polymer (sample 2-13) was obtained in the same manner as in Example 2-1, except that the branching agent was changed from trimethoxy(4-vinylphenyl)silane to 1,1-bis(4-trimethoxysilylphenyl)ethylene (abbreviated as "BS-4" in the table) and the amount of the branching agent was changed to 0.0109 mmol / min. The physical properties of sample 2-13 are shown in Table 16.

[0358] (Example 2-14) Modified conjugated diene polymer (sample 2-14) A modified conjugated diene polymer (sample 2-14) was obtained in the same manner as in Example 2-1, except that the branching agent was changed from trimethoxy(4-vinylphenyl)silane to 1,1-bis(4-trimethoxysilylphenyl)ethylene (abbreviated as "BS-4" in the table), and the amount added was changed to 0.0109mmol / min, and the modifying agent was changed from S-trimethylsilylmercaptopropyltrimethoxysilane to S-trimethylsilylmercaptopropylmethyldimethoxysilane (abbreviated as "T-2" in the table), and the amount added was changed to 0.145mmol / min. The physical properties of sample 2-14 are shown in Table 16.

[0359] (Example 2-15) Modified conjugated diene polymer (sample 2-15) A modified conjugated diene polymer (sample 2-15) was obtained in the same manner as in Example 2-1, except that the branching agent was changed from trimethoxy(4-vinylphenyl)silane to trichloro(4-vinylphenyl)silane (abbreviated as "BS-5" in the table). The physical properties of sample 2-15 are shown in Table 16.

[0360] (Example 2-16) Modified conjugated diene polymer (sample 2-16) A modified conjugated diene polymer (sample 2-16) was obtained in the same manner as in Example 2-1, except that the branching agent was changed from trimethoxy(4-vinylphenyl)silane to trichloro(4-vinylphenyl)silane (abbreviated as "BS-5" in the table), the modifying agent was changed from S-trimethylsilylmercaptopropyltrimethoxysilane to S-trimethylsilylmercaptopropylmethyldimethoxysilane (abbreviated as "T-2" in the table), and the amount of the modified agent was changed to 0.145 mmol / min. The physical properties of sample 2-16 are shown in Table 16.

[0361] (Example 2-17) Modified conjugated diene polymer (sample 2-17) A modified conjugated diene polymer (sample 2-17) was obtained in the same manner as in Example 2-1, except that SRAE oil, a rubber softener, was not added. The physical properties of sample 2-17 are shown in Table 16.

[0362] (Example 2-18) Modified conjugated diene polymer (sample 2-18) A modified conjugated diene polymer (sample 2-18) was obtained in the same manner as in Example 2-1, except that the amount of SRAE oil added as a rubber softener was changed from 25.0 g to 37.5 g per 100 g of polymer. The physical properties of sample 2-18 are shown in Table 16.

[0363] (Example 2-19) Modified conjugated diene polymer (sample 2-19) A modified conjugated diene polymer (sample 2-19) was obtained in the same manner as in Example 2-1, except that naphthenic oil (Nytex810 naphthenic oil manufactured by Nynas) was used instead of SRAE oil added as a rubber softener. The physical properties of sample 2-19 are shown in Table 16.

[0364] (Example 2-20) Modified conjugated diene polymer (sample 2-20) A modified conjugated diene polymer (sample 2-20) was obtained in the same manner as in Example 2-1, except that the SRAE oil added as a rubber softener was replaced with liquid rubber (liquid polybutadiene LBR-302 manufactured by Kuraray Co., Ltd.). The physical properties of sample 2-20 are shown in Table 16.

[0365] (Example 2-21) Modified conjugated diene polymer (sample 2-21) A modified conjugated diene polymer (sample 2-21) was obtained in the same manner as in Example 2-1, except that the SRAE oil added as a rubber softener was replaced with a resin (Yasuhara Chemical Co., Ltd., terpene resin YS Resin PX1250). The physical properties of sample 2-21 are shown in Table 16.

[0366] (Example 2-22) Coupling conjugated diene polymer (sample 2-22) A tank-type pressure vessel having an internal volume of 10 L and an internal height (L) to diameter (D) ratio (L / D) of 4.0, which is a tank-type reactor equipped with a stirrer and a jacket for temperature control, was used as the polymerization reactor. 5,000 g of n-hexane and n-butyllithium for neutralizing impurities present in the reactor that may hinder the polymerization reaction were placed in the reactor and stirred at 70°C for 5 minutes, and then cooled to room temperature, the solution was removed, and the reactor was emptied. Next, 5022 g of n-hexane, 286.2 g of styrene, 478.3 g of 1,3-butadiene, 1.83 mmol of 2,2-bis(2-oxolanyl)propane as a polar substance, and 0.546 mmol of trimethoxy(4-vinylphenyl)silane (abbreviated as "BS-1" in the table) as a branching agent, which had been previously removed of impurities, were placed in a reactor, and the internal temperature of the reactor was controlled at 40° C. After the internal temperature of the reactor stabilized, 4.402 mmol of n-butyllithium was added as a polymerization initiator to start polymerization. Immediately after the polymerization started, the temperature inside the reactor rose and reached a peak temperature of 76°C. Immediately after the peak temperature was reached, 53.1g of 1,3-butadiene was added and stirred for 5 minutes, after which a small amount of the polymer solution was sampled and an antioxidant (BHT) was added in an amount of 0.2g per 100g of polymer. The solvent was removed by vacuum drying, and the Mooney viscosity at 110°C and various molecular weights were measured. The physical properties are shown in Table 18. Next, 0.314 mmol of tin tetrachloride as a coupling agent was added and stirred for 5 minutes, and then 1.286 mmol of S-trimethylsilylmercaptopropyltrimethoxysilane (abbreviated as "T-1" in the table) as a modifying agent was added and stirred for 5 minutes. As a polymerization terminator, 0.15 mmol of ethanol was added to terminate the reaction, thereby obtaining a conjugated diene polymer. To the obtained polymer solution, an antioxidant (BHT) was added in an amount of 0.2 g per 100 g of polymer, and the solvent was removed by steam stripping to obtain a coupling conjugated diene polymer (sample 2-22). The physical properties of sample 2-22 are shown in Table 18.

[0367] (Example 2-23) Coupling conjugated diene polymer (sample 2-23) The modifier was changed from S-trimethylsilylmercaptopropyltrimethoxysilane (abbreviated as "T-1" in the table) to S-trimethylsilylmercaptopropylmethyldimethoxysilane (abbreviated as "T-2" in the table), and the amount of the modifier was changed to 2.572 mmol. The same procedure as in Example 2-22 was followed to obtain a coupling conjugated diene polymer (sample 2-23). ​​The physical properties of sample 2-23 are shown in Table 18.

[0368] [Coupling or modified conjugated diene polymer] (Comparative Example 2-1) Modified conjugated diene polymer (sample 2-24) Two tank-type pressure vessels having an internal volume of 10 L, an internal height (L) to diameter (D) ratio (L / D) of 4.0, an inlet at the bottom and an outlet at the top, and an agitator as a tank-type reactor and a jacket for temperature control were connected together as polymerization reactors. 1,3-butadiene, which had been previously dehydrated, was mixed at 18.6 g / min, styrene at 10.0 g / min, and n-hexane at 175.2 g / min. In a static mixer installed in the middle of the pipe supplying this mixed solution to the inlet of the reactor, n-butyllithium for inactivating remaining impurities was added at 0.103 mmol / min, mixed, and then continuously supplied to the bottom of the reactor. Furthermore, 2,2-bis(2-oxolanyl)propane as a polar substance was supplied at a rate of 0.081 mmol / min, and n-butyllithium as a polymerization initiator was supplied at a rate of 0.143 mmol / min to the bottom of the first reactor, which was vigorously mixed with a stirrer, and the temperature inside the reactor was maintained at 67°C. The polymer solution was continuously withdrawn from the top of the first reactor and continuously fed to the bottom of the second reactor to continue the reaction at 70°C, and then fed to the static mixer from the top of the second reactor. When the polymerization reaction was stabilized, a small amount of the conjugated diene polymer solution before the addition of the modifier was withdrawn, and an antioxidant (BHT) was added so that the amount was 0.2 g per 100 g of polymer, after which the solvent was removed and the Mooney viscosity at 110°C and various molecular weights were measured. The physical properties are shown in Table 17. Next, S-trimethylsilylmercaptopropyltrimethoxysilane (abbreviated as "T-1" in the table) was continuously added as a modifier to the polymer solution flowing out from the outlet of the reactor at a rate of 0.073 mmol / min, and the mixture was mixed using a static mixer to carry out a modification reaction. At this time, the time until the modifier was added to the polymer solution flowing out from the outlet of the reactor was 4.8 minutes, the temperature was 68°C, and the difference between the temperature in the polymerization process and the temperature before the modifier was added was 2°C. An antioxidant (BHT) was continuously added to the modified polymer solution at 0.055 g / min (n-hexane solution) so that the amount was 0.2 g per 100 g of polymer, and the modification reaction was terminated. Simultaneously with the antioxidant, SRAE oil (JOMO Process NC140 manufactured by JX Nippon Oil & Energy Corporation) was continuously added as a rubber softener so that the amount was 25.0 g per 100 g of polymer, and the mixture was mixed using a static mixer. The solvent was removed by steam stripping to obtain a modified conjugated diene polymer (Sample 2-24). The physical properties of Sample 2-24 are shown in Table 17.

[0369] (Comparative Example 2-2) Modified conjugated diene polymer (sample 2-25) A modified conjugated diene polymer (sample 2-25) was obtained in the same manner as in Comparative Example 2-1, except that the modifying agent was changed from S-trimethylsilylmercaptopropyltrimethoxysilane to S-trimethylsilylmercaptopropylmethyldimethoxysilane (abbreviated as "T-2" in the table) and the amount of the modified agent was changed to 0.145 mmol / min. The physical properties of sample 2-25 are shown in Table 17.

[0370] (Comparative Example 2-3) Coupling conjugated diene polymer (Sample 2-26) Before the addition of the modifier, tin tetrachloride was added continuously as a coupling agent at a rate of 0.011 mmol / min, and the mixture was mixed using a static mixer to carry out a coupling reaction. After that, S-trimethylsilylmercaptopropyltrimethoxysilane (abbreviated as "T-1" in the table) was added continuously as a modifier at a rate of 0.045 mmol / min, and the mixture was mixed using a static mixer in the latter stage to carry out a modification reaction. A coupling conjugated diene polymer (sample 2-26) was obtained in the same manner as in Comparative Example 2-1. The physical properties of sample 2-26 are shown in Table 17.

[0371] (Comparative Example 2-4) Coupling conjugated diene polymer (Sample 2-27) Before the addition of the modifier, tin tetrachloride was added continuously as a coupling agent at a rate of 0.011 mmol / min, mixed using a static mixer, and a coupling reaction was carried out. After that, the modifier was changed from S-trimethylsilylmercaptopropyltrimethoxysilane to S-trimethylsilylmercaptopropylmethyldimethoxysilane (abbreviated as "T-2" in the table), and the amount added was changed to 0.099 mmol / min and added continuously, mixed using a static mixer in the latter stage, and a modification reaction was carried out. A coupling conjugated diene polymer (sample 2-27) was obtained in the same manner as in Comparative Example 2-1. The physical properties of sample 2-27 are shown in Table 17.

[0372] (Comparative Example 2-5) Conjugated diene polymer (Sample 2-28) A tank-type pressure vessel having an internal volume of 10 L and an internal height (L) to diameter (D) ratio (L / D) of 4.0, which is a tank-type reactor equipped with a stirrer and a jacket for temperature control, was used as the polymerization reactor. 5,000 g of n-hexane and n-butyllithium for neutralizing impurities present in the reactor that may hinder the polymerization reaction were placed in the reactor and stirred at 70°C for 5 minutes, and then cooled to room temperature, the solution was removed, and the reactor was emptied. Next, 5022 g of n-hexane, 286.2 g of styrene, 478.3 g of 1,3-butadiene, and 1.83 mmol of 2,2-bis(2-oxolanyl)propane as a polar substance, from which impurities had been removed in advance, were placed in a reactor, and the internal temperature of the reactor was controlled at 40° C. After the internal temperature of the reactor became stable, 4.402 mmol of n-butyllithium was added as a polymerization initiator to initiate polymerization. Immediately after the polymerization started, the temperature inside the reactor rose and reached a peak temperature of 76°C. Immediately after the peak temperature was reached, 53.1g of 1,3-butadiene was added and stirred for 5 minutes, after which a small amount of the polymer solution was sampled and an antioxidant (BHT) was added in an amount of 0.2g per 100g of polymer. The solvent was removed by vacuum drying, and the Mooney viscosity at 110°C and various molecular weights were measured. The physical properties are shown in Table 18. Next, 0.314 mmol of tin tetrachloride as a coupling agent was added and stirred for 5 minutes, and then 1.286 mmol of S-trimethylsilylmercaptopropyltrimethoxysilane as a modifying agent was added and stirred for 5 minutes. As a polymerization terminator, 0.15 mmol of e...

Claims

1. a polymerization step of polymerizing or copolymerizing a conjugated diene compound, or a conjugated diene compound and an aromatic vinyl compound, using an alkali metal compound or an alkaline earth metal compound as a polymerization initiator to obtain a conjugated diene polymer having an active terminal; a branching step of reacting an active terminal of the conjugated diene polymer with a styrene derivative as a branching agent to introduce a branched structure; having a reaction step of reacting a coupling agent with the active terminal of the conjugated diene polymer obtained in the branching step, Furthermore, In the reaction step, The coupling agent is a silane sulfide compound represented by the following formula (3): A method for producing a branched conjugated diene polymer. [Formula 1] (In formula (3), Si represents a silicon atom, O represents an oxygen atom, and S represents a sulfur atom. x is an integer of 1 to 3, y is 0 or an integer of 1 to 2, and x+y is 3. R 1 , R 2 , and R 4 may be the same or different and each represents an alkyl group having 1 to 16 carbon atoms, and R 3 represents an aryl group having 6 to 16 carbon atoms, an alkylene group having 1 to 16 carbon atoms, or an alkyl chain having 1 to 16 carbon atoms.

2. The method further comprises a step of adding a conjugated diene compound and / or an aromatic vinyl compound to the reaction system during and / or after the branching step. A method for producing the branched conjugated diene polymer according to claim 1.

3. The styrene derivative is A compound represented by the following formula (1) and / or the following formula (2): A method for producing the branched conjugated diene polymer according to claim 1 or 2. [chemical 2] [C3] (In formulas (1) and (2), R 1 represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, or a group having 6 aryl group having a branched structure in a portion thereof. It is okay to do so. X 1 , X 2 , X 3 is a single bond or a group consisting of carbon, hydrogen, nitrogen, sulfur, and oxygen. It is an organic group containing any of the following: Y 1 , Y 2 , Y 3 represents an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, and and halogen atoms. may be the same or different.)

4. A step of obtaining a branched conjugated diene polymer by the production method according to any one of claims 1 to 3; obtaining a rubber component containing 10% by mass or more of the branched conjugated diene polymer; a step of obtaining a rubber composition by adding a filler in an amount of 5.0 parts by mass or more and 150 parts by mass or less to 100 parts by mass of the rubber component; The method for producing a rubber composition comprising the steps of:

5. Obtaining a rubber composition by the method for producing a rubber composition according to claim 4; molding the rubber composition to obtain a tire; A tire manufacturing method comprising the steps of:

6. having one or more side chains in the polymer chain, The branching degree (Bn) measured by a GPC-light scattering method with a viscosity detector is 1 or more. A conjugated diene polymer, The branched conjugated diene polymer contains a sulfur atom and a silicon atom, and the sulfur atom is the molar ratio of silicon atoms to silicon is 1.05 or more and less than 10, The Mooney viscosity measured at 100° C. is 40 or more and 170 or less, A polymer or copolymer of a conjugated diene compound, or a conjugated diene compound and an aromatic vinyl compound, The branched conjugated diene polymer has a branched structure based on a styrene derivative at a terminal thereof, At least one end of the branched conjugated diene polymer is modified with a silane sulfide compound represented by the following formula (3): Branched conjugated diene polymers. [C6] (In formula (3), Si represents a silicon atom, O represents an oxygen atom, and S represents a sulfur atom. x is an integer of 1 to 3, y is 0 or an integer of 1 to 2, and x+y is 3. R 1 , R 2 , and R 4 may be the same or different and each represents an alkyl group having 1 to 16 carbon atoms, and R 3 represents an aryl group having 6 to 16 carbon atoms, an alkylene group having 1 to 16 carbon atoms, or an alkyl chain having 1 to 16 carbon atoms.

7. The branching degree (Bn) measured by a GPC-light scattering method with a viscosity detector is 2 to 25. The branched conjugated diene-based polymer according to claim 6 .

8. The polymer chain is derived from a vinyl monomer containing an alkoxysilyl group or a halosilyl group. and In the portion derived from the vinyl monomer containing the alkoxysilyl group or halosilyl group, and having a side chain, The branched conjugated diene polymer according to claim 6 or 7.

9. The portion derived from the vinyl monomer containing an alkoxysilyl group or a halosilyl group is A monomer unit based on a compound represented by the following formula (4) or (5): A branching point of a polymer chain due to a monomer unit based on a compound represented by the following formula (4) or (5): The branched conjugated diene-based polymer according to claim 8, having the formula: [C4] [C5] (In formula (4), R 1 is a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, or an alkyl group having 6 to 20 carbon atoms. It represents an aryl group, part of which may have a branched structure. R 2 ~R 3 each independently represents an alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 20 carbon atoms; It represents a aryl group, part of which may have a branched structure. R when there are multiple 1 ~R 3 are each independent. X 1 represents an independent halogen atom. m is an integer of 0 to 2, n is an integer of 0 to 3, and 1 is an integer of 0 to 3. (m+n+l) represents 3.) (In formula (5), R 2 ~R 5 each independently represents an alkyl group having 1 to 20 carbon atoms or It represents an aryl group having a molecular weight of 20, and may have a branched structure in part. R 2 ~R 5 are each independent. X 2 ~X 3 represents an independent halogen atom. m is an integer of 0 to 2, n is an integer of 0 to 3, and 1 is an integer of 0 to 3. (m+n+l) represents 3. a represents an integer of 0 to 2, b represents an integer of 0 to 3, and c represents an integer of 0 to 3. (a+b+c) represents 3.

10. A branched conjugated diene polymer composition comprising the branched conjugated diene polymer according to any one of claims 6 to 9, The branched conjugated diene polymer is contained in an amount of 10% by mass or more and less than 100% by mass. A branched conjugated diene-based polymer composition.

11. The branched conjugated diene polymer comprises Tin halides, tin alkoxides, silicon halides, and alkoxysilanes Polymerization of a branched conjugated diene system coupled with at least one compound selected from the group consisting of Including the body, The branched conjugated diene-based polymer composition according to claim 10.

Citation Information

Patent Citations

  • Elastomeric polymers chain-end modified with silane-sulfides

    JP2009512762A

  • Method for producing modified conjugated diene polymer, and modified conjugated diene polymer produced using the same

    JP2019515073A

  • Method for producing branched conjugated diene-based polymer, rubber composition, method for producing rubber composition, and method for manufacturing tire

    JP2021155701A

  • Method for producing branched conjugated diene-based polymer, branched conjugated diene-based polymer, method for producing rubber composition, and method for manufacturing tire

    JP2021155702A

  • Styrene copolymer

    US20040059075A1