Separators and their applications

The hydrolyzed resin film separator with non-hydrolyzable and hydrolyzable polymers addresses low conductivity and safety issues, providing enhanced ionic conductivity and preventing ion permeability for improved battery performance and safety.

JP7595686B2Active Publication Date: 2024-12-06MICROCOSM TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023001213
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-01-14
Filing Date
2023-01-06
Publication Date
2024-12-06
Estimated Expiration
2043-01-06

AI Technical Summary

Technical Problem

Existing separators in energy storage devices face challenges with low ionic conductivity, safety issues such as rupture, liquid leakage, and combustion, and inadequate prevention of electron and gas passage, which affect battery performance and safety.

Method used

A separator is formed by hydrolyzing a resin film composed of non-hydrolyzable organic polymers like polybenzimidazole and hydrolyzable organic polymers, with specific functional groups, to enhance ionic conductivity and prevent vanadium ion and hydrogen permeability.

Benefits of technology

The separator achieves high ionic conductivity, low swelling, and improved mechanical properties, effectively preventing vanadium ion and hydrogen permeability, enhancing battery safety and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595686000020
    Figure 0007595686000020
  • Figure 0007595686000021
    Figure 0007595686000021
  • Figure 0007595686000022
    Figure 0007595686000022
Patent Text Reader

Abstract

To provide a separator with good ion conductivity and thus, is extremely suitable for use in various types of batteries.SOLUTION: The present invention provides a separator formed by hydrolysis of a resin film. The resin film comprises a non-hydrolyzable organic polymer; and a hydrolyzable organic polymer being hydrolyzable by treatment with at least one of an acid aqueous solution, an alkaline aqueous solution and pure water. The content of the hydrolyzable organic polymer ranges from 10 parts by weight to 70 parts by weight relative to 100 parts by weight of the resin film.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a separator and its application, in particular to an ion-conductivity separator and its application. [Background technology]

[0002] Energy storage devices commonly used around the world include hydrogen fuel cells, all-vanadium flow batteries, lithium-ion and other chemical energy storage. Energy storage systems are one of the key factors that affect the success of renewable energy development. Energy storage has a regulating effect, reserve load capacity and instantaneous power supply capability, which can delay the impact of instantaneous changes on the power grid, thus becoming an essential and important part of the power supply system.

[0003] Various energy storage methods have their own advantages and disadvantages, and separators play an important role in batteries. As market demands for battery safety and performance increase, separators are required to have high ionic conductivity, prevent the passage of positive and negative electrons, prevent leakage due to the passage of solids, liquids or gases that would cause a decrease in capacitance, and prevent safety issues such as bursting, liquid leakage, air leakage, and combustion. Summary of the Invention [Problem to be solved by the invention]

[0004] In view of the above problems, an object of the present invention is to provide a separator having high ionic conductivity. [Means for solving the problem]

[0005] In order to achieve the above object, the present invention provides a separator formed by hydrolysis of a resin film, the resin film comprising: A non-hydrolyzable organic polymer; and a hydrolyzable organic polymer that can be hydrolyzed by treatment with at least one of an acid aqueous solution, an alkaline aqueous solution, and pure water; The content of the hydrolyzable organic polymer is 10 to 70 parts by weight based on 100 parts by weight of the resin film.

[0006] Preferably, the non-hydrolyzable organic polymer comprises polybenzimidazole, polybenzoxazole, polybenzothiazole, polyetherketone, polyphenylene ether, polyethersulfone, polysulfone, polyphenylene sulfide, polypropylene, polyethylene, polystyrene, or a combination thereof. More preferably, the non-hydrolyzable organic polymer has a hydrophilic functional group in a side chain. Particularly preferably, the hydrophilic functional group comprises a sulfonic acid group, a phosphoric acid group, a carboxylic acid group, an amide group, or a hydroxyl group.

[0007] Preferably, the hydrolyzable organic polymer comprises a repeat unit represented by formula (1): [ka] Here, X1 is a tetravalent group containing at least one aromatic group or alicyclic group, Y1 is a divalent group containing at least one aromatic group or alicyclic group, and at least one of X1 and Y1 contains at least one functional group structure selected from the group consisting of an ester bond, an amide bond, a sulfonic acid group, a phosphoric acid group, a carboxylic acid group, a hydroxyl group, and a nitro group.

[0008] X1 is more preferably selected from tetravalent groups represented by formula (2), formula (3), formula (4), formula (5) or formula (6), [ka] where R1 is independently -H, -F, or -CF 3 , -SO 3 H, -PO 3 H 2, -COOH, -OH, a straight or branched chain alkyl group having 1 to 6 carbon atoms, or a phenyl; R2 each independently represents a straight or branched chain hydrocarbon group having 2 to 36 carbon atoms or a cyclic hydrocarbon group having 3 to 20 carbon atoms; R3 each independently represents -H, -F, -CF 3 ,-SO 3 H,-PO 3 H 2 , -COOH, -OH, or a straight or branched chain hydrocarbon group having 1 to 6 carbon atoms; each L1 is independently -O-, -S-, -SO 2 -, single bond, -NH-, -C(=O)-, -CH=CH-, -C≡C-, -CH 2 -, -(CH 2 ) 2 -, -C(CH 3 ) 2 -, -C(CF 3 ) 2 each n independently represents an integer from 0 to 5; and m represents an integer from 1 to 5.

[0009] Y1 is more preferably a divalent group represented by formula (7), formula (8) or formula (9), [ka] Here, each L2 is independently -O-, -S-, or -SO 2 -, single bond, -NH-, -C(=O)-, -CH=CH-, -C≡C-, -CH 2 -, -(CH 2 ) 2 -, -C(CH 3 ) 2 -, -C(CF 3 ) 2 R4 represents -, -C(=O)O-, -OC(=O)-, -C(=O)NH-, or -NHC(=O)-; each R4 is independently -H, -F, -CF 3 , -SO 3 H, -PO 3 H 2, -COOH, -OH, a straight or branched chain hydrocarbon having 1 to 6 carbon atoms, or phenyl; R5 is each independently -H, -F, -CF 3 , -SO 3 H, -PO 3 H 2 , -COOH, -OH, a linear or branched chain hydrocarbon group having 1 to 6 carbon atoms, or phenyl; R6 and R7 each independently represent a linear or branched chain hydrocarbon group having 1 to 9 carbon atoms; and n represents an integer from 0 to 5.

[0010] The separator preferably has an ionic conductivity improved by 10% or more after hydrolysis.

[0011] The separator preferably has an elongation at break of more than 10%.

[0012] The thickness of the separator is preferably from 0.1 μm to 100 μm.

[0013] The resin film preferably further contains a filler in an amount of more than 0 to 60 parts by weight per 100 parts by weight of the resin film. The filler is preferably selected from a flame retardant, a hydrophilic material consisting of an acidic substance and an alkaline substance, a ceramic oxide, a lithium salt, an organic acid, an ionic liquid, or a combination thereof.

[0014] The resin film is preferably formed from a composition including a non-hydrolyzable organic polymer, a hydrolyzable organic polymer, and an optional organic solvent.

[0015] The present invention also provides a composite film including the separator described above.

[0016] The present invention also provides a battery, the battery comprising: an anode layer; A cathode layer; and and the separator described above disposed between the anode layer and the cathode layer.

[0017] The battery is suitable for use in a fuel cell, a flow battery, or a lithium battery.

[0018] The separator of the present invention has high ionic conductivity and low swelling due to the design of the hydrolyzable polymer and dosage, and can effectively prevent the passage of vanadium ions in the electrolyte of a flow battery and hydrogen in a fuel cell. As a result, the separator has low vanadium ion permeability and low hydrogen permeability, which contributes to improving the safety of the battery. [Brief description of the drawings]

[0019] [Figure 1] FIG. 2 is a diagram showing an FTIR spectrum of the separator according to Example 1 of the present invention before hydrolysis.

[0020] [Diagram 2] FIG. 2 is a diagram showing an FTIR spectrum of the separator (after hydrolysis) according to Example 1 of the present invention.

[0021] [Diagram 3] FIG. 13 is a diagram showing an FTIR spectrum of a separator according to Example 9 of the present invention before hydrolysis.

[0022] [Figure 4] FIG. 13 is a diagram showing the FTIR spectrum of the separator (after hydrolysis) according to Example 9 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] The separator provided by the present invention is different from conventional separators in that it has high ionic conductivity, low swelling, high volume stability, excellent mechanical properties, low vanadium ion permeability, and low hydrogen permeability.

[0024] The separator of the present invention is formed by hydrolyzing a resin film, and the resin film contains a non-hydrolyzable organic polymer and a hydrolyzable organic polymer that can be hydrolyzed by treatment with at least one (e.g., two or three) of an acid aqueous solution, an alkali aqueous solution, and pure water, and the content of the hydrolyzable organic polymer is 10 to 70 parts by weight (preferably 20 to 70 parts by weight, more preferably 30 to 70 parts by weight, and particularly preferably 40 to 70 parts by weight) per 100 parts by weight of the resin film.

[0025] The non-hydrolyzable organic polymer has a non-hydrolyzable covalent bond, such as an imidazole bond, an oxazole bond, a carbon-carbon bond, a sulfone bond, a biphenyl, a fluorine group, a ketone group, an ether group, etc., and therefore the structure is not affected even if the polymer is hydrolyzed. Examples of the non-hydrolyzable organic polymer include, but are not limited to, polybenzimidazole (PBI), polybenzoxazole (PBO), polybenzothiazole (PBT), polyetherketone (PEEK), polyphenylene oxide (PPO), polyethersulfone (PES), polysulfone, polyphenylene sulfide (PPS), polypropylene (PP), polyethylene (PE), and polystyrene (PS). The non-hydrolyzable organic polymers can be used alone or in combination of two or more (eg, three or four).

[0026] In the present invention, the non-hydrolyzable organic polymer preferably has a hydrophilic functional group in a side chain thereof that assists the hydrolysis reaction of the hydrolyzable polymer of the present invention. Preferred examples of the hydrophilic functional group include a sulfonic acid group, a phosphoric acid group, a carboxylic acid group, an amide group, and a hydroxyl group.

[0027] In the present invention, the content of the non-hydrolyzable organic polymer may be in the range of 30 to 90 parts by weight (preferably 30 to 80 parts by weight, more preferably 30 to 70 parts by weight, and particularly preferably 30 to 60 parts by weight) per 100 parts by weight of the resin film.

[0028] In the present invention, the hydrolyzable organic polymer preferably contains a repeating unit represented by formula (1). [ka]

[0029] In formula (1), X1 is a tetravalent group containing at least one aromatic group or alicyclic group, Y1 is a divalent group containing at least one aromatic group or alicyclic group, and at least one of X1 and Y1 contains at least one functional group structure of an ester bond, an amide bond, a sulfonic acid group, a phosphoric acid group, a carboxylic acid group, a hydroxyl group, and a nitro group. For example, X1 contains at least one functional group structure of an ester bond, an amide bond, a sulfonic acid group, a phosphoric acid group, a carboxylic acid group, a hydroxyl group, and a nitro group, and Y1 does not contain any functional group structure of an ester bond, an amide bond, a sulfonic acid group, a phosphoric acid group, a carboxylic acid group, a hydroxyl group, and a nitro group. Alternatively, Y1 contains at least one functional group structure of an ester bond, an amide bond, a sulfonic acid group, a phosphoric acid group, a carboxylic acid group, a hydroxyl group, and a nitro group, and X1 does not contain any functional group structure of an ester bond, an amide bond, a sulfonic acid group, a phosphoric acid group, a carboxylic acid group, a hydroxyl group, and a nitro group. Alternatively, both X1 and Y1 contain at least one functional group structure selected from the group consisting of an ester bond, an amide bond, a sulfonic acid group, a phosphoric acid group, a carboxylic acid group, a hydroxyl group, and a nitro group.More specifically, the hydrolyzable organic polymer may contain at least one (e.g., at least two, at least three, at least four, or at least five) repeating units represented by formula (1).

[0030] In the present invention, at least one of X1 and Y1 contains at least one (e.g., two or three) functional group structures of an ester bond, an amide bond, a sulfonic acid group, a phosphoric acid group, a carboxylic acid group, a hydroxyl group, and a nitro group. For example, at least one of X1 and Y1 contains both an ester bond and a hydroxyl group, or at least one of X1 and Y1 contains both an ester bond and a sulfonic acid group, or at least one of X1 and Y1 contains both an ester bond and a phosphoric acid group, or at least one of X1 and Y1 contains both an ester bond and a carboxylic acid group.

[0031] X1 may be a tetravalent group derived from a dianhydride monomer. X1 may be the same or different in each occurrence. X1 may be selected from tetravalent groups represented by formula (2), formula (3), formula (4), formula (5) or formula (6). [ka]

[0032] In formula (2) to formula (4), R1 may be the same or different at each occurrence, and each occurrence is independently -H, -F, -CF 3 , -SO 3 H, -PO 3 H 2 , -COOH, -OH, a straight or branched chain alkyl group having 1 to 6 carbon atoms, or phenyl. R2 may be the same or different at each occurrence and each independently represent a straight or branched chain hydrocarbon group having 2 to 36 carbon atoms or a cyclic hydrocarbon group having 3 to 20 carbon atoms. R3 may be the same or different at each occurrence and each independently represent -H, -F, -CF 3 , -SO 3 H, -PO 3 H 2 L1 may represent -COOH, -OH, or a straight or branched chain hydrocarbon group having 1 to 6 carbon atoms. Each occurrence of L1 may be the same or different, and each occurrence independently represents -O-, -S-, -SO 2 -, single bond, -NH-, -C(=O)-, -CH=CH-, -C≡C-, -CH 2-, -(CH 2 ) 2 -, -C(CH 3 ) 2 -, -C(CF 3 ) 2 "n" may be the same or different at each occurrence and each independently represents any integer from 0 to 5 (e.g., 1, 2, 3, or 4). "m" represents any integer from 1 to 5 (e.g., 1, 2, 3, or 4).

[0033] Here are some examples of X1:

[0034] For example, when n is 0, X1 may be a tetravalent group such as: [ka]

[0035] X1 may be a tetravalent group such as those exemplified below. [ka]

[0036] The hydrolyzable organic polymer may have one or more (3, 4, 5, etc.) tetravalent groups as described above.

[0037] In formula (1), Y1 is a divalent group represented by formula (7), formula (8), or formula (9). [ka]

[0038] L2 may be the same or different for each occurrence, -O-, -S-, -SO 2 -, single bond, -NH-, -C(=O)-, -CH=CH-, -C≡C-, -CH 2 -, -(CH 2 ) 2 -, -C(CH 3) 2 -, -C(CF 3 ) 2 R4 may independently represent -, -C(=O)O-, -OC(=O)-, -C(=O)NH-, or -NHC(=O)-, and each occurrence of R4 may be the same or different and each independently represent -H, -F, -CF 3 , -SO 3 H, -PO 3 H 2 , -COOH, -OH, a straight or branched chain hydrocarbon group having 1 to 6 carbon atoms, or phenyl; R5 may be the same or different at each occurrence and each independently represents -H, -F, -CF 3 , -SO 3 H, -PO 3 H 2 , -COOH, -OH, a linear or branched chain hydrocarbon group having 1 to 6 carbon atoms, or phenyl; R6 may be the same or different in each occurrence and each independently may represent a linear or branched chain hydrocarbon group having 1 to 9 carbon atoms; R7 may be the same or different in each occurrence and each independently may represent a linear or branched chain hydrocarbon group having 1 to 9 carbon atoms; and n represents any integer from 0 to 5 (such as 1, 2, 3, or 4).

[0039] Some examples of Y1 are given below:

[0040] For example, when n is 0, Y1 may be a divalent group such as: [ka]

[0041] For example, when n is 1, Y1 may be a divalent group such as: [ka]

[0042] Y1 may be a divalent group such as those exemplified below. [ka]

[0043] The hydrolyzable organic polymer may have one or more (three, four, five, etc.) divalent groups as described above.

[0044] In the present invention, the hydrolyzable organic polymer is preferably always hydrolyzable in any of an acid aqueous solution, an alkaline aqueous solution, and pure water, and is preferably hydrolyzable in all three conditions of an acid aqueous solution, an alkaline aqueous solution, and pure water.

[0045] Considering ionic conductivity, it is preferable that the hydrolyzable polymer has an imide bond in the structure. Compared with an amide bond that generates one carboxylic acid group and one hydroxyl group after hydrolysis or an ester bond that generates one carboxylic acid group and one hydroxyl group, an imide bond that generates two carboxylic acid groups and one amine group generates more hydrophilic functional groups than an amide bond or an ester bond, and therefore has excellent ionic conductivity.

[0046] In some embodiments of the present invention, the equilibrium swelling ratio of the separator after immersion in water, an acid solution, or an alkaline solution is less than 1.1.

[0047] In the present invention, the resin film may be formed from a composition including a non-hydrolyzable organic polymer, a hydrolyzable organic polymer, and an optional organic solvent. The preparation process of the resin film preferably includes an organic solvent. The resin film (separator precursor) may be formed by applying the composition and then heat treating to remove the organic solvent. In some embodiments, the content of the hydrolyzable organic polymer in the composition is 10 to 70 parts by weight per 400 parts by weight of the organic solvent. In some embodiments, the content of the non-hydrolyzable organic polymer in the composition is 30 to 90 parts by weight per 400 parts by weight of the organic solvent. In some embodiments, the content of the hydrolyzable organic polymer is 10 to 70 parts by weight per 500 parts by weight of the composition. In some embodiments, the content of the non-hydrolyzable organic polymer is 30 to 90 parts by weight per 500 parts by weight of the composition.

[0048] The method for preparing the separator precursor of the present invention may include the steps of mixing a non-hydrolyzable organic polymer, a hydrolyzable organic polymer, and an organic solvent to obtain a mixture (composition), forming a coating film of the mixture on a substrate, and subjecting the coating film to a heat treatment.

[0049] The method for preparing the separator of the present invention may include the steps of mixing a non-hydrolyzable organic polymer, a hydrolyzable organic polymer, and an organic solvent to obtain a mixture (composition), forming a coating of the mixture on a substrate, subjecting the coating to a heat treatment, and performing hydrolysis on the heat-treated coating. In the present invention, the hydrolysis can be performed in an acidic aqueous solution, an alkaline aqueous solution, or pure water. In some embodiments, the hydrolysis is first performed in an alkaline aqueous solution and then in an acidic aqueous solution. In some embodiments, the hydrolysis is first performed in an acidic aqueous solution and then in an alkaline aqueous solution.

[0050] The conditions of the mixing process (such as temperature and time) are adjusted depending on the types of the non-hydrolyzable organic polymer, the hydrolyzable organic polymer, and the organic solvent. In some embodiments of the present invention, the temperature range of the mixing process is 60°C to 100°C, and the time range is 2 hours to 4 hours. The organic solvent can be used alone or in combination of two or more (for example, three or four). The organic solvent includes, but is not limited to, N-methylpyrrolidone, 2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, γ-butyrolactone, dichlorobenzene, dioxane, toluene, xylene, chloroform, acetone, butanone, ethanol, and methanol. When the total amount of the organic solvent is 100 parts by weight, the total amount of the non-hydrolyzable organic polymer and the hydrolyzable organic polymer is preferably in the range of 2 parts by weight to 55 parts by weight.

[0051] The coating may be formed by blade coating, spin coating, or spray coating. In some embodiments of the present invention, the coating is formed by coating the mixture on a substrate. The purpose of the heat treatment is to remove the organic solvent and densify the separator precursor. The heat treatment temperature is adjusted according to the components of the mixture. In some embodiments of the present invention, the heat treatment temperature is in the range of 60°C to 250°C, for example, 80°C, 100°C, 120°C, 150°C, 180°C, 210°C, or 230°C.

[0052] The method for producing a separator of the present invention includes a hydrolysis step, which can improve the properties of the resulting separator and can provide a higher ionic conductivity. In some embodiments, the hydrolysis step is carried out in an acid or alkaline aqueous solution. Specifically, the hydrolysis step is carried out in the following manner. First, the high-concentration separator precursor (resin film) is immersed in a 4M aqueous sodium hydroxide solution (alkali) at 25°C to 70°C for 24 hours, or in a 4M aqueous lithium hydroxide solution for 24 hours, or in a 4M aqueous sulfuric acid solution (acid) for 24 hours. Next, it is washed three times with deionized water. Next, it is dried at 120°C for 1 hour to obtain a separator. In a preferred embodiment, the separator precursor is hydrolyzed in pure water.

[0053] In a preferred embodiment, the separator has an ion conductivity improved by 10% or more compared to a non-hydrolyzed separator (resin film). In another preferred embodiment, the separator has a breaking elongation of more than 10%.

[0054] In the present invention, the thickness of the separator is not particularly limited and may be adjusted depending on the actual application, but is preferably in the range of 0.1 μm to 100 μm.

[0055] In the present invention, the resin film may further contain a filler, and the content of the filler is more than 0 parts by weight and not more than 60 parts by weight, preferably 10 parts by weight to 60 parts by weight, and more preferably 20 parts by weight to 60 parts by weight, per 100 parts by weight of the resin film.

[0056] In the present invention, the composition may further contain a filler, and the content of the filler is more than 0 part by weight and not more than 60 parts by weight, preferably in the range of 10 parts by weight to 60 parts by weight, and more preferably in the range of 20 parts by weight to 60 parts by weight, relative to 500 parts by weight of the composition.

[0057] The filler in the present invention may be a flame retardant, a hydrophilic material consisting of an acidic substance and an alkaline substance, a ceramic oxide, a lithium salt, an organic acid, an ionic liquid, or any combination thereof. The hydrophilic substance may be composed of an acidic substance (such as a Lewis acid) and an alkaline substance (such as a Lewis base). Examples of hydrophilic materials include, but are not limited to, melamine sulfate, melamine hydrochloride, melamine polyphosphate, melamine pyrophosphate, melamine cyanurate, melamine oxalate, metal orthophosphate, or any combination thereof.

[0058] The present invention also provides a composite film including the separator described above.

[0059] The present invention also provides a battery, including, but not limited to, a fuel cell, a flow battery, or a lithium battery, comprising an anode layer and the above-described separator disposed between the anode layer and the cathode layer.

[0060] The present invention will be further described with reference to the following examples, which are for illustrative purposes only and are not intended to limit the practice of the present invention.

[0061] Sources and preparation of materials in the examples:

[0062] Preparation Example 1: Preparation of polybenzimidazole

[0063] A 500 mL four-necked reaction flask was prepared, and dry nitrogen gas was passed through the reaction flask. Then, 2 g of 2,2-bis(4-carboxyphenyl)-hexafluoropropane (purchased from TCI), 6 g of monosodium 2-sulfoterephthalate (purchased from TCI), 6 g of 3,3'-diaminobenzidine (purchased from TCI), 30 g of P 2 O 5 (purchased from Sigma-Aldrich) and 460 g of polyphosphoric acid (purchased from ARCOS) were added in sequence. This was stirred uniformly with a mechanical motor, and the temperature was raised to 200°C and reacted for 24 hours. A large amount of deionized water was poured into the resulting reaction solution to precipitate a solid. The solid was alkaline washed with a 10 wt% NaOH aqueous solution, then repeatedly washed with large amounts of deionized water until it became neutral, and dried in an oven at 140°C for 24 hours to obtain a polybenzimidazole powder.

[0064] Preparation Example 2: Preparation of polybenzoxazole

[0065] A 500 mL four-necked reaction flask was prepared, and dry nitrogen gas was passed through the reaction flask. Then, 9.1 g of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (purchased from TCI), 9.8 g of 2,2-bis(4-carboxyphenyl)-hexafluoropropane (purchased from TCI), 30 g of P 2 O5 (purchased from Sigma-Aldrich), and 460 g of polyphosphoric acid (purchased from ARCOS) were added in sequence. This was stirred uniformly with a mechanical motor, and the temperature was raised to 200°C and reacted for 24 hours. A large amount of deionized water was poured into the resulting reaction solution to precipitate a solid. The solid was alkaline washed with a 10 wt% NaOH aqueous solution, then repeatedly washed with a large amount of deionized water until it became neutral, and dried in an oven at 140°C for 24 hours to obtain a polybenzothiazole powder.

[0066] Preparation Example 3: Preparation of polyamide-imide

[0067] A 500 mL four-necked reaction flask was prepared, and dry nitrogen gas was passed through the reaction flask. Then, 24 g of 4,4'-(hexafluoroisopropylidene)diphthalic anhydride (6FDA) (purchased from TCI), 12 g of 4,4'-diaminobenzanilide (DABA) (purchased from TCI), and 140 g of N-methylpyrrolidone (purchased from Shiny Chemical Industrial Co., Ltd.) were added in sequence. The mixture was stirred uniformly with a mechanical motor and reacted for 24 hours, and the temperature was raised to 180°C and maintained for 4 hours to carry out a thermal ring closing reaction. A large amount of methanol was poured into the resulting reaction solution to precipitate a solid. The solid was washed with methanol and then dried in an oven at 140°C for 24 hours to obtain a polyamide-polyimide powder.

[0068] Preparation Example 4: Preparation of polyesterimide

[0069] A 500 mL four-necked reaction flask was prepared, and after passing dry nitrogen gas through the reaction flask, 22 g of ethylene glycol bis(trimellitic anhydride) (TMEG) (purchased from TCI), 11 g of 4,4'-oxydianiline (ODA) (purchased from TCI), and 140 g of N-methylpyrrolidone (purchased from Shiny Chemical Industrial) were added in sequence. This was uniformly stirred with a mechanical motor and reacted for 24 hours, and the temperature was raised to 180°C and maintained for 4 hours to carry out a thermal ring-closing reaction. A large amount of methanol was poured into the resulting reaction solution to precipitate a solid. The solid was washed with methanol and then dried in an oven at 140°C for 24 hours to obtain a polyester-polyamideimide powder.

[0070] Preparation Example 5: Preparation of polybenzosulfonate-imide

[0071] A 500 mL four-necked reaction flask was prepared, and after passing dry nitrogen gas through the reaction flask, 24 g of 4,4'-(hexafluoroisopropylidene)diphthalic anhydride (6FDA) (purchased from TCI), 19 g of 4,4'-diaminobenzidine-2,2'-disulfonic acid (BDSA) (purchased from TCI), and 140 g of N-methylpyrrolidone (purchased from Shiny Chemical Industrial) were added in sequence. This was uniformly stirred with a mechanical motor and reacted for 24 hours, and the temperature was raised to 180 ° C and maintained for 4 hours to carry out a thermal ring-closing reaction. A large amount of methanol was poured into the resulting reaction solution to precipitate a solid. The solid was washed with methanol and then dried in an oven at 140 ° C for 24 hours to obtain a hexafluoropolyimide powder.

[0072] Preparation Example 6: Preparation of polybenzoate-imide

[0073] A 500 mL four-necked reaction flask was prepared, and after passing dry nitrogen gas through the reaction flask, 24 g of 4,4'-(hexafluoroisopropylidene)diphthalic anhydride (6FDA) (purchased from TCI), 15 g of 6,6'-bisamino-3,3'-methylidenedibenzoic acid (MBAA) (purchased from TCI), and 140 g of N-methylpyrrolidone (purchased from Shiny Chemical Industrial) were added in sequence. This was uniformly stirred with a mechanical motor and reacted for 24 hours, and the temperature was raised to 180 ° C and maintained for 4 hours to carry out a thermal ring-closing reaction. A large amount of methanol was poured into the resulting reaction solution to precipitate a solid. The solid was washed with methanol and then dried in an oven at 140 ° C for 24 hours to obtain a transparent polyimide powder.

[0074] Preparation of fillers

[0075] Flame retardant: Melamine cyanurate (purchased from Haiwang Chemical)

[0076] Lithium salt: HQ-115 (purchased from 3M)

[0077] Ionic liquid: imidazolium 1-hexyl-3-methyl tetrafluoromethanesulfonate (purchased from Sigma-Aldrich)

[0078] Ceramic oxide: Lithium lanthanum zirconium oxide Li 7 La 3 Zr 2 O 12 Preparation of (LLZO)

[0079] In the experiment, Li 7 La 3 Zr 2 O 12 (LLZO) was prepared by the conventional solid-phase method. The specific steps were as follows: 2 O(95%, alpha), ZrO 2 (99%, Alpha), La 2 O 3(99.95%, Alpha) was accurately weighed on an electronic balance according to the stoichiometric ratio, where LiOH H was added to compensate for the loss of Li element during high-temperature sintering. 2 O was weighed out in 10% excess. After the materials were prepared, ball milling and discharging were performed. The prepared raw materials were placed in a ball mill tank at once, and then a certain amount of anhydrous ethanol was added. The ball mill tank was sealed and then placed in a planetary ball mill for 12 hours of ball milling. After ball milling was completed, the uniformly mixed slurry was poured into a clean mortar and placed under a baking lamp to dry. The dried powder was placed in a crucible, which was then placed in a high-temperature furnace and sintered at 1100 °C for 12 hours to obtain a precursor with a predetermined crystal structure. After sintering was completed, the obtained powder was ball milled for a second time for 12 hours, and then sieved to obtain lithium lanthanum zirconium oxide Li 7 La 3 Zr 2 O 12 (LLZO) powder was obtained.

[0080] Example 1

[0081] 7g (70 parts by weight) of polybenzimidazole, 3g (30 parts by weight) of polyamide-polyimide, and 40g (400 parts by weight) of N-methylpyrrolidone were mixed in a mixer at 120°C and 1 atm for 2 hours to prepare a colloidal mixture. The colloidal mixture was applied onto a glass substrate to form a coating film having a thickness of 200μm on the glass substrate. The coating film was heat-treated and dried at 90°C to 150°C for 5 minutes. The temperature was then raised to 250°C and aged at this temperature for 1 hour to obtain a separator precursor (i.e., a resin film) having a thickness of 20μm.

[0082] Examples 2 to 7 and Comparative Examples 1 to 4

[0083] Separator precursors (i.e., non-hydrolyzed separators) of Examples 2 to 7 and Comparative Examples 1 to 4 were obtained in the same manner as in Example 1, except that the types and amounts of each component were changed as shown in Table 1.

[0084] Example 8

[0085] 4g (40 parts by weight) of polybenzimidazole, 4g (40 parts by weight) of polyamide-polyimide, 2g (20 parts by weight) of melamine cyanurate, and 40g (400 parts by weight) of N-methylpyrrolidone (purchased from Shiny Chemical Industrial) were mixed in a mixer at 120°C and 1 atm for 2 hours to prepare a colloidal mixture, which was then crushed and dispersed three times in three drums. The colloidal mixture was applied onto a glass substrate to form a coating film having a thickness of 200 μm on the glass substrate. The coating film was heat-treated by drying at 150°C to 250°C for 30 minutes to form a heat-treated coating film, and a separator precursor (resin film) having a thickness of 20 μm was obtained.

[0086] Examples 9 to 11 and Comparative Examples 5 to 7

[0087] The separator precursors of Examples 9 to 11 and Comparative Examples 5 to 7 (i.e., non-hydrolyzed separators) were obtained in the same manner as in Example 8, except that the types and amounts of each component were changed as shown in Table 2.

[0088] Example 12

[0089] 4g (40 parts by weight) of polybenzimidazole, 4g (40 parts by weight) of polyamide-polyimide, 2g (20 parts by weight) of lithium salt, and 40g (400 parts by weight) of N-methylpyrrolidone (purchased from Shiny Chemical Industrial) were mixed using a mixer at 120°C and 1 atm for 2 hours to prepare a colloidal mixture. The colloidal mixture was applied onto a glass substrate to form a coating film having a thickness of 200 μm on the glass substrate. The coating film was heat-treated by drying at 150°C to 250°C for 30 minutes under a nitrogen atmosphere to form a heat-treated coating film, and a separator precursor (resin film) having a thickness of 20 μm was obtained.

[0090] Example 13 and Comparative Examples 8 to 9

[0091] Separator precursors (i.e., non-hydrolyzed separators) of Example 13 and Comparative Examples 8 to 9 were obtained in the same manner as in Example 12, except that the types and amounts of each component were changed as shown in Table 2.

[0092] The hydrolysis method for the separator precursors of the above examples and comparative examples was to immerse them in a 4M aqueous sulfuric acid solution at 25°C for 24 hours, wash them with deionized water three times, and dry them at 120°C for 1 hour to complete the hydrolysis of the separator.

[0093] Evaluation items

[0094] Porosity measurement (%): The separators of Examples 1 to 13 and Comparative Examples 1 to 9 were measured using a mercury porosimeter (brand: Micromeritics, model: AutoPore (trademark) IV9520).

[0095] Measurement of tensile strength (MPa) and elongation at break (%): The separators of Examples 1 to 13 and Comparative Examples 1 to 9 were measured using a tensile tester (brand: LLOYD, model LRX) at a pulling speed of 100 mm / min.

[0096] Measurement of acid content (%): The separators of Examples 1 to 13 and Comparative Examples 1 to 9 were weighed (W1, in grams) and immersed in an aqueous sulfuric acid solution (containing sulfuric acid and water, with a sulfuric acid concentration of 3M) at 25±3°C for 7 days. After that, the separator was taken out, the aqueous sulfuric acid solution attached to the surface was wiped off, and the weight was measured (W2, in grams). The acid content (%) was calculated as [(W2-W1) / W1]×100%.

[0097] Measurement of moisture content (%): The separators of Examples 1 to 13 and Comparative Examples 1 to 9 were weighed (W1, in grams) and immersed in an aqueous solution at 80°C for one day. The separators were then taken out, and the aqueous solution adhering to the surface was wiped off to form water-absorbed separators, which were then weighed (W2, in grams). The moisture content (%) was calculated as [(W2-W1) / W1] x 100%.

[0098] Measurement of ionic conductivity (mS / cm): For the separators of Examples 1 to 13 and Comparative Examples 1 to 9, impedance values ​​were measured at 25° C. or less using a quadrupole column conductivity measuring instrument manufactured by BekkTECH LLC, USA, and an AC impedance analysis method using an impedance analyzer Autolab. Ionic conductivity (S / cm) is 1 / [(impedance value×separator width×separator thickness) / reference electrode spacing], and the units of separator width, separator thickness, and reference electrode spacing are cm.

[0099] Vanadium ion diffusion rate (%): VOSO sulfuric acid solution with a concentration of 2.5M 4 Mixed with VOSO 4 A first mixed solution was prepared in which the concentration of MgSO was 1 M and the concentration of sulfuric acid was 2.5 M. The 2.5 M sulfuric acid aqueous solution was dissolved in MgSO 4 Mix with MgSO 4 A second mixed solution was prepared with a concentration of 1M of sulfuric acid and a concentration of 2.5M of sulfuric acid. The temperature of the experimental environment was 25±3°C. The separators of Examples 1 to 13 and Comparative Examples 1 to 9 were placed in a container having a storage space divided into a first storage space portion (left side) and a second storage space portion (right side). The first mixed solution was placed in the first storage space portion, and the second mixed solution was placed in the second storage space portion. The first mixed solution and the second mixed solution were irradiated with light having a wavelength of 766 nm, and the absorbance (A V ) and the absorbance of the second mixed solution (A Mg After that, the vanadium ions started to pass through the separator, and the above steps were repeated at different measurement times (t), and the absorbance (A V ) and the absorbance of the second mixed solution (A Mg ) was calculated as ln(A V -2A Mg) was plotted to obtain the first equation, which was used to calculate the mass transfer coefficient (ks). The mass transfer coefficient was then substituted into the second equation to calculate the vanadium ion diffusivity (D). The first equation is expressed as ln(A V -2A Mg )=lnA V -(2×ks×A×t) / V A The second equation is D = ks × d, where A is the contact area of ​​the separator (unit: cm 2 ), t is the measurement time, V A is the volume of the second storage space (unit: cm 3 ), and d is the thickness of the separator (unit: cm).

[0100] Gas permeability (%): In this test, oxygen gas permeability test was carried out based on the principle of differential pressure method. The pretreated test specimen was placed between the upper and lower test chambers and clamped. First, the low pressure chamber (lower chamber) was vacuum treated, and then the whole system was evacuated. When the specified vacuum level was reached, the lower test chamber was closed, and the high pressure chamber (upper chamber) was filled with test gas at a certain pressure to create a certain pressure difference on both sides of the test specimen, so that the gas would permeate from the high pressure side to the low pressure side under the action of the pressure difference gradient. By monitoring the internal pressure on the low pressure side, various barrier parameters of the test specimen were obtained. The oxygen transmission rate (OTR) of the relevant samples was mainly measured using a trace oxygen permeation analyzer, product model: 8001, model 8001 oxygen permeation analyzer. At room temperature, under the condition of evacuating one side of the separator and supplying oxygen to the other side of the separator, the amount of oxygen permeating the sample per unit area in unit time was obtained by the trace oxygen permeation analyzer device. Q=K A Δp, where Q is the permeability of the gas passing through the separator, K is the permeability coefficient of a certain gas when it passes through the separator, A is the area of ​​the separator, and Δp is the gas pressure difference on both sides of the separator.

[0101] [Table 1]

[0102] [Table 2]

[0103] The FTIR spectrum of the separator of Example 1 before hydrolysis is shown in FIG. -1 and 1722cm -1 Two characteristic peaks, which are the C=O bond absorption peaks of the symmetric imide and asymmetric amide, respectively, can be observed. The FTIR spectrum after hydrolysis of the separator of Example 1 is shown in FIG. 2. After hydrolysis by acid treatment, the FTIR spectrum at a wavelength of 1771 cm -1 and 1714cm -1 The two characteristic peaks of α- and β-imide bonds were obviously decreased, indicating that the content of amide-imide bonds was decreased and the separator was hydrolyzed.

[0104] The FTIR spectrum of the separator of Example 9 before hydrolysis is shown in FIG. -1 and 1739cm -1 Two characteristic peaks, which are the C=O bond absorption peaks of the symmetric imide and asymmetric amide, respectively, can be observed. The FTIR spectrum after hydrolysis of the separator of Example 9 is shown in FIG. 4. After hydrolysis by acid treatment, the FTIR spectrum at a wavelength of 1774 cm -1 and 1715cm -1 The two characteristic peaks of α- and β-imide bonds were obviously decreased, indicating that the content of amide-imide bonds was decreased and the separator was hydrolyzed.

[0105] As shown in Tables 1 and 2, the separators of Examples 1 and 7 after hydrolysis treatment by immersion in a 4M sulfuric acid solution have high ionic conductivity, large breaking elongation, low vanadium ion diffusion rate, and low gas permeability. This effectively prevents the passage of vanadium ions in the electrolyte of the vanadium redox flow battery and the fuel gas in the fuel cell, effectively improving the safety and life of the battery, thereby achieving the object of the present invention. The separators of Examples 8 and 13 contain a filler and have high ionic conductivity after hydrolysis by immersion in a 4M sulfuric acid solution, but the vanadium ion diffusion rate and gas permeability are slightly higher than those of the separators of Examples 1 and 7.

[0106] As shown in Tables 1 and 2, the separators of Comparative Example 1 and Comparative Example 2 use only organic polymer components with a non-hydrolyzable structure, and the ionic conductivity after immersion in a 4M sulfuric acid solution at room temperature cannot be measured due to the hydrolysis treatment. The separator of Comparative Example 3 contained 80% (weight ratio) of an organic polymer having a hydrolyzable structure. After hydrolysis with a 4M sulfuric acid solution at room temperature, the separator was damaged and unusable, and a membrane for detection could not be formed. The separator of Comparative Example 5 contained 70% filler by weight. After hydrolysis with a 4M sulfuric acid solution at room temperature, the separator was damaged and unusable. The separators of Comparative Example 4 and Comparative Examples 6 to 9 were not subjected to hydrolysis treatment by immersion in a 4M sulfuric acid solution at room temperature, and the ionic conductivity could not be measured.

[0107] The separators of Comparative Example 4 and Comparative Examples 6 to 9 used the non-hydrolyzable organic polymer and hydrolyzable organic polymer components of the present invention, but were not immersed in a 4M sulfuric acid solution for hydrolysis, so the ionic conductivity of these separators could not be measured and these separators could not be used in batteries. On the other hand, the separators of Examples 1 to 7 of the present invention contained the non-hydrolyzable organic polymer and hydrolyzable organic polymer components of the present invention. After being immersed in a 4M sulfuric acid solution at room temperature for hydrolysis, the hydrophilicity of the separator increased and the ionic conductivity improved, so this separator is useful for applications such as flow batteries, fuel cells, and lithium batteries.

[0108] Application example 1 and application example 2

[0109] Flow battery production and testing:

[0110] Measurement of coulombic efficiency (%), voltage efficiency (%), and energy efficiency (%) of the flow battery: The separators of Example 2 and Example 3, graphite felt electrodes, bipolar plates, and 100 ml of electrolyte were assembled using a polyvinyl chloride plate and a frame to form a single battery with an effective area of ​​5 cm x 5 cm. The electrolyte was VOSO 4 The powder was mixed with 456 grams of powder and 1000 milliliters of aqueous sulfuric acid, the concentration of which was 3 M. The single battery was charged and discharged using a battery charge-discharge tester [brand: Chroma, model: 17011] to measure the power and the current density was 100 mA / cm 2 The coulombic efficiency, energy efficiency, and voltage efficiency were calculated based on the power when the cutoff voltage was 0.7 V to 1.6 V and the flow rate was 50 mL / min. The electrical test results for Application Example 1 and Application Example 2 are shown in Table 3.

[0111] [Table 3]

[0112] As shown in Tables 1, 2, and 3, the separators of Examples 2 and 3 have high Coulombic efficiency and low vanadium ion diffusion rate, and therefore can prevent vanadium ions in a flow battery from interdiffusing through the separator. As shown by the test results of Application Examples 1 and 2 in Table 3, the separators containing hydrolyzable organic polymers exhibit excellent electrical properties after hydrolysis when applied to a flow battery.

[0113] Application Example 3 and Application Example 4

[0114] Preparation of membrane electrode assemblies for fuel cells:

[0115] The separator precursors (resin films) of Examples 2 and 13 were immersed in a 4M sulfuric acid solution for hydrolysis, and then immersed in 10M phosphoric acid at 60° C. for 1 hour to produce 6×6 cm 2 The gas diffusion electrodes of the membrane electrode element were cathode and anode gas diffusion layers each measuring 5 × 5 cm. 2 The carbon paper used was 280 microns thick. The cathode gas diffusion layer and the anode gas diffusion layer were then coated with a commercially available Pt / C catalyst slurry and dried at 160°C to form an electrocatalyst layer in the gas diffusion electrode. The electrocatalyst layers were formed on the cathode gas diffusion layer and the anode gas diffusion layer, respectively. The cathode gas diffusion layer with the electrocatalyst layer is the cathode gas diffusion electrode here, and the anode gas diffusion layer with the electrocatalyst layer is the anode gas diffusion electrode here, with a total Pt content of about 1 mg / cm. 2 Next, an electrode catalyst layer of a cathode gas diffusion electrode and an electrode catalyst layer of an anode gas diffusion electrode were arranged on both sides of the phosphorylated separator (phosphorylated PBI electrolyte membrane) described above, and then a hot press treatment was performed at a temperature of, for example, 130 to 160°C and a pressure of, for example, 20 to 30 MPa to form a membrane electrode element. The results of the electrical test of the fuel cell are shown in Application Example 3 and Application Example 4 in Table 4.

[0116] Fuel cell power density test: First, the prepared cell was activated by the following process: (1) In the open circuit voltage (OCV) state, hydrogen was supplied to the anode terminal at 200cc / min, and air was supplied to the cathode terminal at 500cc / min, and the cell was heated to 120°C. (2) When the cell temperature reached 120°C, 200mA / cm 2 A constant current of 10 ...

[0117] [Table 4]

[0118] As shown in Tables 1, 2, and 4, the separators of Examples 2 and 13 are hydrolyzed, and therefore have high ionic conductivity and low gas permeability, and can effectively prevent fuel gas in a fuel cell from interdiffusing within the separator. As shown by the electrical test results of Application Examples 3 and 4 to a fuel cell, the hydrolyzed separator of Application Example 3 had a higher current density when applied to a fuel cell.

[0119] Application Example 5 and Application Example 6

[0120] Lithium Battery Preparation:

[0121] A solid polymer electrolyte (SPE) was prepared by mixing PEO (MW = 300,000, Sigma-Aldrich) with LiTFSI (HQ-115, 3M) (PEO:LiTFSi = 10:1) and acetonitrile (anhydrous, Sigma-Aldrich) using a high-speed mixer. 4 (LFP) powder (purchased from MTI), PEO / LiTFSI, and carbon black (w:w:w = 60:25:15) were mixed with acetonitrile using a high-speed mixer. The LFP active material loading was 1.5 mg / cm. 2The slurry was then cast onto aluminum foil with a doctor blade. The electrodes were then dried in a vacuum oven at 60°C for at least 48 hours. The separator precursors of Examples 3 and 11 were hydrolyzed by immersing in a 4M sulfuric acid solution, then immersing in a 4MLiOH aqueous solution (Sigma-Aldrich) for 24 hours, washing with deionized water three times, and vacuum baking at 200°C for 1 hour. The lithium foil / SPE / separator / SPE / LFP was then pressed into a button battery (lithium foil, Sigma-Aldrich). The electrical test results of the lithium batteries of Application Examples 5 and 6 are shown in Table 5. At a temperature of 60°C, a single cell was charged and discharged at different rates C / 10, C / 5, C / 2, and 1C using a battery charge-discharge tester [brand: Chroma, model: 17011], and the average power of 10 cycles was measured.

[0122] [Table 5]

[0123] As shown in Tables 1, 2, and 5, the separator precursors of Examples 3 and 11 were immersed in a 4M lithium hydroxide aqueous solution (alkaline) for hydrolysis, and then batteries were fabricated. The prepared batteries were applied to lithium batteries. As shown by the electrical test results of Application Examples 5 and 6, the lithium batteries can both be charged and discharged.

[0124] In summary, the separator provided by the present invention has high ionic conductivity, high breaking elongation, low vanadium ion diffusivity, and low gas permeability through the use of non-hydrolyzable polymer, hydrolyzable polymer, and dosage design, and therefore can effectively prevent the passage of vanadium ions in the electrolyte, as well as reduce the permeability of vanadium ions. When applied to a flow battery, the Coulomb efficiency is increased, and when applied to a fuel cell or lithium battery, the electrical properties are good, and the safety and life of the battery are effectively improved. Therefore, the separator of the present invention can be used in an all-vanadium flow battery, a fuel cell, or a lithium battery.

[0125] The above is merely a preferred embodiment of the present invention, and does not limit the scope of the present invention; that is, all simple and equivalent changes and modifications made based on the claims and the contents of the specification of the present invention are included in the claims of the present invention.

Claims

1. A separator formed by hydrolysis of a resin film, The resin film is A non-hydrolyzable organic polymer; and a hydrolyzable organic polymer that can be hydrolyzed by treatment with at least one of an acid aqueous solution, an alkaline aqueous solution, and pure water; the content of the hydrolyzable organic polymer is 10 parts by weight to 70 parts by weight based on 100 parts by weight of the resin film, The separator has a breaking elongation of more than 10%, The hydrolyzable organic polymer comprises a repeating unit represented by formula (1), [Case 1] Here, X1 is a tetravalent group containing at least one aromatic group or alicyclic group, Y1 is a divalent group containing at least one aromatic group or alicyclic group, and at least one of X1 and Y1 contains at least one functional group structure selected from the group consisting of an ester bond, an amide bond, a sulfonic acid group, a phosphoric acid group, a carboxylic acid group, a hydroxyl group, and a nitro group. The separator.

2. 2. The separator of claim 1, wherein the non-hydrolyzable organic polymer comprises polybenzimidazole, polybenzoxazole, polybenzothiazole, polyetherketone, polyphenylene ether, polyethersulfone, polysulfone, polyphenylene sulfide, polypropylene, polyethylene, polystyrene, or a combination thereof.

3. The separator according to claim 2 , wherein the non-hydrolyzable organic polymer has a hydrophilic functional group in a side chain.

4. The separator according to claim 3 , wherein the hydrophilic functional group includes a sulfonic acid group, a phosphoric acid group, a carboxylic acid group, an amide group, or a hydroxyl group.

5. X1 is selected from a tetravalent group represented by formula (2), formula (3), formula (4), formula (5), or formula (6), [Case 2] Here, each R1 is independently -H, -F, or -CF 3 , -SO 3 H, -PO 3 H 2 , -COOH, -OH, a linear or branched alkyl group having 1 to 6 carbon atoms, or a phenyl group; R2 each independently represents a linear or branched hydrocarbon group having 2 to 36 carbon atoms or a cyclic hydrocarbon group having 3 to 20 carbon atoms; R3 each independently represents -H, -F, -CF 3 , -SO 3 H, -PO 3 H 2 , —COOH, —OH, or a linear or branched hydrocarbon group having 1 to 6 carbon atoms; each L1 independently represents —O—, —S—, or —SO 2 -, single bond, -NH-, -C(=O)-, -CH=CH-, -C≡C-, -CH 2 -, -(CH 2 ) 2 -, -C(CH 3 ) 2 -, -C(CF 3 ) 2 -, -C(=O)O-, -OC(=O)-, -C(=O)NH-, or -NHC(=O)-; each n is independently an integer from 0 to 5; and m is an integer from 1 to 5. The separator according to claim 1 .

6. In the separator according to claim 1, Y1 is a divalent group represented by formula (7), formula (8), or formula (9), [C3] Here, each L2 is independently -O-, -S-, or -SO 2 -, single bond, -NH-, -C(=O)-, -CH=CH-, -C≡C-, -CH 2 -, -(CH 2 ) 2 -, -C(CH 3 ) 2 -, -C(CF 3 ) 2R4 represents -, -C(=O)O-, -OC(=O)-, -C(=O)NH-, or -NHC(=O)-; each R4 is independently -H, -F, or -CF 3 , -SO 3 H, -PO 3 H 2 , -COOH, -OH, a straight or branched chain hydrocarbon having 1 to 6 carbon atoms, or phenyl; R5 is independently -H, -F, -CF 3 , -SO 3 H, -PO 3 H 2 , -COOH, -OH, a linear or branched chain hydrocarbon group having 1 to 6 carbon atoms, or phenyl; R6 and R7 each independently represent a linear or branched chain hydrocarbon group having 1 to 9 carbon atoms; n represents an integer from 0 to 5; The separator according to claim 5 .

7. 10. The separator of claim 1 having a thickness of 0.1 μm to 100 μm.

8. The separator according to claim 1 , wherein the resin film further contains a filler whose content is more than 0 part by weight and not more than 60 parts by weight per 100 parts by weight of the resin film.

9. 9. The separator of claim 8, wherein the filler is selected from a flame retardant, a hydrophilic material composed of an acidic substance and an alkaline substance, a ceramic oxide, a lithium salt, an organic acid, an ionic liquid, or a combination thereof.

10. The separator according to claim 1 , wherein the resin film is formed from a composition including the non-hydrolyzable organic polymer, the hydrolyzable organic polymer, and an optional organic solvent.

11. A composite film comprising the separator of claim 1.

12. an anode layer; A cathode layer; and a separator according to claim 1 disposed between the anode layer and the cathode layer; A battery comprising:

13. 13. The battery of claim 12, wherein the battery is selected from a fuel cell, a flow battery, or a lithium battery.

Citation Information

Patent Citations

  • Method for preparing high-conductivity proton exchange membrane for direct methanol fuel cells

    CN102188913A

  • Isolating plate for alkaline battery

    JP1981022044A

  • Phosphoric acid-doped electrolyte membrane, method for producing the same, and fuel cell including the same

    JP2011068872A

  • Electrochemical separation membrane and the manufacturing method thereof

    US20130327704A1

  • Varnish, porous polyimide film produced using said varnish, and method for producing said film

    WO2014196435A1