Gallium nitride film manufacturing method

The described sputtering process addresses the challenge of forming high-quality gallium nitride films at low temperatures, enabling reliable micro-LEDs on glass substrates by utilizing controlled plasma generation and metastable gas reactions.

JP7595740B2Active Publication Date: 2024-12-06JAPAN DISPLAY INC
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023500606
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-02-19
Filing Date
2022-01-06
Publication Date
2024-12-06
Estimated Expiration
2042-01-06

AI Technical Summary

Technical Problem

Existing methods for forming gallium nitride films at low temperatures result in films of insufficient quality, hindering the direct deposition of micro-LEDs on glass substrates.

Method used

A method involving a sputtering process where a substrate is placed facing a target containing nitrogen and gallium in a vacuum chamber, with nitrogen radicals and voltage application to generate plasma, followed by controlled voltage cessation to facilitate the deposition of gallium nitride using nitrogen anions and gallium ions, leveraging metastable sputtering gas for high-quality film formation at low temperatures.

Benefits of technology

This method enables the production of high-quality gallium nitride films at low temperatures, suitable for direct deposition on glass substrates, enhancing the reliability and performance of micro-LED display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595740000001
    Figure 0007595740000001
  • Figure 0007595740000002
    Figure 0007595740000002
  • Figure 0007595740000003
    Figure 0007595740000003
Patent Text Reader

Abstract

Provided is a method for producing a gallium nitride film in which a substrate is arranged so as to face a target including nitrogen and gallium within a vacuum chamber, a sputtering gas is supplied within the vacuum chamber, nitrogen radicals are supplied within the vacuum chamber, plasma of the sputtering gas is generated by applying voltage to the target, ions of the sputtering gas are made to collide with the target and gallium ions are generated, application of the voltage to the target is stopped, and gallium nitride resulting from reaction of the gallium ions and nitrogen anions that are the result of electrons and nitrogen radicals reacting within the vacuum chamber is deposited on the substrate.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] One embodiment of the present invention relates to a method for producing a gallium nitride film. [Background technology]

[0002] For small and medium-sized display devices such as smartphones, display devices using liquid crystal or OLED (Organic Light Emitting Diode) have already been commercialized. In particular, OLED display devices using OLED, which is a self-luminous element, have the advantage of high contrast and no need for backlight compared to liquid crystal display devices. However, because OLED is composed of organic compounds, it is difficult to ensure high reliability of OLED display devices due to the deterioration of the organic compounds.

[0003] In recent years, so-called micro LED display devices or mini LED display devices, which are equipped with tiny LED chips in the pixels of a circuit board, have been developed as next-generation display devices. LEDs are self-emitting elements similar to OLEDs, but unlike OLEDs, they are composed of stable inorganic compounds containing gallium (Ga) or indium (In), making it easier to ensure high reliability in micro LED display devices compared to OLED display devices. Furthermore, LED chips have high luminous efficiency and can achieve high brightness. Therefore, micro LED display devices or mini LED display devices are expected to be next-generation display devices with high reliability, high brightness, and high contrast.

[0004] Incidentally, gallium nitride films used in micro LEDs and the like are generally formed on sapphire substrates using MOCVD (Metal Organic Chemical Vapor Deposition) or HVPE (Hydride Vapor Phase Epitaxy) at high temperatures of 800° C. to 1000° C. However, in recent years, a method for forming gallium nitride films by sputtering, which allows film formation at relatively low temperatures, has been developed (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2020-164927 A Summary of the Invention [Problem to be solved by the invention]

[0006] If gallium nitride films could be deposited at low temperatures, it would be possible to form micro-LEDs directly on glass substrates. However, gallium nitride films produced by sputtering have not been of sufficient quality.

[0007] In view of the above problems, one object of one embodiment of the present invention is to provide a method for producing a high-quality gallium nitride film that can be formed at a low temperature. [Means for solving the problem]

[0008] A method for producing a gallium nitride film according to one embodiment of the present invention includes placing a substrate facing a target containing nitrogen and gallium in a vacuum chamber, supplying a sputtering gas into the vacuum chamber, supplying nitrogen radicals into the vacuum chamber, generating a plasma of the sputtering gas by applying a voltage to the target, causing ions of the sputtering gas to collide with the target to generate gallium ions, stopping the application of voltage to the target, and depositing gallium nitride formed by reaction between gallium ions and nitrogen anions formed by reaction between electrons and nitrogen radicals in the vacuum chamber, on the substrate.

[0009] A substrate is placed facing a target containing nitrogen and gallium in a vacuum chamber, a sputtering gas is supplied into the vacuum chamber, nitrogen radicals are supplied into the vacuum chamber, a voltage is applied to the target to generate a plasma of the sputtering gas, ions of the sputtering gas are collided with the target to generate gallium ions, the application of the voltage to the target is stopped, nitrogen atoms are generated using the sputtering gas in a metastable state in the vacuum chamber, and gallium nitride formed by reaction between nitrogen anions formed by reaction between electrons and nitrogen atoms in the vacuum chamber and gallium ions is deposited on the substrate. [Brief description of the drawings]

[0010] [Figure 1] 1 is a schematic diagram showing the configuration of a film formation apparatus used in a method for producing a gallium nitride film according to one embodiment of the present invention. [Diagram 2] FIG. 1 is a flow chart showing a method for manufacturing a gallium nitride film according to an embodiment of the present invention. [Diagram 3] FIG. 2 is a sequence diagram showing the on / off timing of a sputtering power supply and a nitrogen radical supply source in a gallium nitride film manufacturing method according to an embodiment of the present invention. [Figure 4] FIG. 2 is a sequence diagram showing the on / off timing of a sputtering power supply and a nitrogen radical supply source in a gallium nitride film manufacturing method according to an embodiment of the present invention. [Diagram 5] FIG. 1 is a flow chart showing a method for manufacturing a gallium nitride film according to an embodiment of the present invention. [Figure 6] FIG. 2 is a sequence diagram showing the on / off timing of a sputtering power supply and a nitrogen radical supply source in a gallium nitride film manufacturing method according to an embodiment of the present invention. [Figure 7] FIG. 2 is a sequence diagram showing the on / off timing of a sputtering power supply and a nitrogen radical supply source in a gallium nitride film manufacturing method according to an embodiment of the present invention. [Figure 8] 1 is a schematic diagram showing a configuration of a light-emitting element according to one embodiment of the present invention. [Figure 9] 1 is a schematic diagram showing a configuration of a semiconductor element according to an embodiment of the present invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, each embodiment of the present invention will be described with reference to the drawings. Note that each embodiment is merely an example, and those that a person skilled in the art can easily come up with by appropriately modifying the invention while keeping the gist of the invention are naturally included in the scope of the present invention. In addition, in order to make the explanation clearer, the width, thickness, shape, etc. of each part may be shown diagrammatically compared to the actual embodiment. However, the illustrated shapes are merely examples and do not limit the interpretation of the present invention.

[0012] In this specification, unless otherwise specified, expressions such as "α includes A, B, or C," "α includes any one of A, B, and C," and "α includes one selected from the group consisting of A, B, and C" do not exclude cases where α includes multiple combinations of A to C. Furthermore, these expressions do not exclude cases where α includes other elements.

[0013] In this specification, for convenience of explanation, the terms "up" or "upper" or "lower" or "lower" are used for explanation, but in principle, the substrate on which the structure is formed is used as the reference, and the direction from the substrate to the structure is referred to as "up" or "upper". Conversely, the direction from the structure to the substrate is referred to as "lower" or "lower". Therefore, in the expression "structure on substrate", the surface of the structure facing the substrate is the lower surface of the structure, and the surface on the opposite side is the upper surface of the structure. In addition, in the expression "structure on substrate", the upper and lower relationship between the substrate and the structure is merely described, and other members may be disposed between the substrate and the structure. Furthermore, the terms "up" or "upper" or "lower" or "lower" refer to the order of stacking in a structure in which multiple layers are stacked, and do not necessarily have to be in a positional relationship of overlapping in a planar view.

[0014] In this specification, the letters "first," "second," or "third" attached to each component are convenient labels used to distinguish each component, and have no other meaning unless otherwise specified.

[0015] In this specification and drawings, the same reference numerals are used to collectively represent multiple identical or similar components, and lowercase or uppercase alphabets may be added to each of these components to distinguish them from one another. In addition, hyphens and natural numbers may be used to distinguish between multiple parts of one component.

[0016] The following embodiments can be combined with each other as long as no technical contradiction occurs.

[0017] First Embodiment A method for producing a gallium nitride film according to one embodiment of the present invention will be described with reference to FIGS.

[0018] [1. Configuration of the film forming apparatus 10] FIG. 1 is a schematic diagram showing the configuration of a film formation apparatus 10 used in a method for producing a gallium nitride film according to one embodiment of the present invention.

[0019] 1, the film forming apparatus 10 includes a vacuum chamber 100, a substrate support 110, a heating unit 120, a target 130, a target support 140, a pump 150, a sputtering power supply 160, a sputtering gas supply source 170, and a nitrogen radical supply source 180. The film forming apparatus 10 is a so-called sputtering apparatus.

[0020] A substrate support 110, a heating unit 120, a target 130, and a target support 140 are provided in the vacuum chamber 100. The substrate support 110 and the heating unit 120 are provided at a lower part in the vacuum chamber 100. A substrate is disposed on the substrate support 110. The heating unit 120 is provided in the substrate support 110 and is capable of heating the substrate on the substrate support 110. The target 130 and the target support 140 are provided at an upper part in the vacuum chamber 100. The target 130 is supported by the target support 140 and is provided to face the substrate support 110.

[0021] In addition, while FIG. 1 shows an example in which the substrate support part 110 and the heating part 120 are provided at the bottom within the vacuum chamber 100, and the target 130 and the target support part 140 are provided at the top within the vacuum chamber 100, these may be reversed.

[0022] The target 130 is gallium nitride containing nitrogen and gallium. The composition ratio of the gallium nitride of the target 130 is preferably 0.7 or more and 2 or less of gallium to nitrogen. In addition, since the nitrogen of the gallium nitride film formed on the substrate can be supplied from a nitrogen radical source, while the gallium of the gallium nitride film is supplied from the target 130, it is more preferable that the composition ratio of the gallium nitride of the target 130 is higher in gallium than in nitrogen.

[0023] Outside the vacuum chamber 100, a pump 150, a sputtering power supply 160, a sputtering gas supply 170, and a nitrogen radical supply 180 are provided.

[0024] The pump 150 is connected to the vacuum chamber 100 through a pipe 151. The pump 150 can exhaust gas from within the vacuum chamber 100 through the pipe 151. In addition, the pressure within the vacuum chamber 100 can be kept constant by opening and closing a valve 152 connected to the pipe 151. For example, a turbo molecular pump or a cryopump can be used as the pump 150.

[0025] The sputtering power supply 160 is electrically connected to the target 130 via wiring 161. The sputtering power supply 160 can generate a direct current voltage (DC voltage) or an alternating current voltage (AC voltage) and apply the generated voltage to the target 130. The AC voltage is 13.56 (MHz). The sputtering power supply 160 can also apply a bias voltage to the target 130 and further apply a DC voltage or an AC voltage.

[0026] The sputtering power supply 160 can periodically stop the voltage applied to the target 130. The time for stopping the application of the voltage to the target 130 is 2 (msec) or more and 10 (msec) or less. The voltage applied by the sputtering power supply 160 to the target 130 may be a pulsed voltage having a predetermined frequency. In this case, the predetermined frequency is 100 (kHz) or more and 500 (kHz) or less.

[0027] The sputtering gas supply source 170 is connected to the vacuum chamber 100 through a pipe 171. The sputtering gas supply source 170 can supply a sputtering gas into the vacuum chamber 100 through the pipe 171. In addition, the flow rate of the sputtering gas can be controlled by a mass flow controller 172 connected to the pipe 171. The sputtering gas supplied from the sputtering gas supply source 170 can be argon (Ar) or krypton (Kr).

[0028] The nitrogen radical supply source 180 is connected to a pipe 181 provided in the vacuum chamber 100, and can irradiate nitrogen radicals from the pipe 181 toward the substrate placed on the substrate support 110. The nitrogen radical supply source 180 can generate nitrogen radicals by converting nitrogen gas into plasma.

[0029] The nitrogen radical source 180 may be provided within the vacuum chamber 100 to generate nitrogen radicals within the vacuum chamber 100 .

[0030] [2. Gallium nitride film manufacturing method] A method for producing a gallium nitride film according to one embodiment of the present invention will be described with reference to Figures 2 to 4. Since the gallium nitride film is produced using a film formation apparatus 10, the following description may refer to the reference symbols shown in Figure 1 for convenience.

[0031] FIG. 2 is a flow chart showing a method for producing a gallium nitride film according to one embodiment of the present invention.

[0032] In step S100, the substrate is placed on the substrate support 110 so as to face the target 130. As the substrate, for example, a quartz substrate or a glass substrate can be used. Alternatively, as the substrate, a quartz substrate or a glass substrate on which an aluminum nitride film is formed can be used.

[0033] In step S110, the substrate is heated to a predetermined temperature by the heating unit 120. The predetermined temperature is, for example, 400° C. or higher and lower than 600° C.

[0034] In step S120, the pump 150 exhausts the gas in the vacuum chamber 100 to a predetermined vacuum level or less. The predetermined vacuum level is, for example, 10 -6 (Pa).

[0035] In step S130, the sputtering gas supply source 170 supplies a sputtering gas into the vacuum chamber 100. For example, argon or krypton can be used as the sputtering gas. The flow rate of the sputtering gas is adjusted by the mass flow controller 172 so that the pressure inside the vacuum chamber 100 becomes a predetermined pressure. The predetermined pressure is, for example, 0.1 (Pa) or more and 10 (Pa) or less.

[0036] In step S140, the nitrogen radical source 180 supplies nitrogen radicals into the vacuum chamber 100.

[0037] In step S150, the sputtering power supply 160 applies a predetermined voltage to the target 130 so that the target 130 serves as a cathode with respect to the substrate. This causes the sputtering gas in the vacuum chamber 100 to be turned into plasma, generating ions (specifically, positive ions) of the sputtering gas and electrons. The ions of the sputtering gas are accelerated by the potential difference between the substrate and the target 130, and collide with the target 130. As a result, gallium ions (e.g., gallium positive ions) are released from the target 130.

[0038] In step S160, the sputtering power supply 160 stops applying a voltage to the target 130. At this time, the gallium nitride produced by the reaction can be deposited on the substrate. Here, the production of gallium nitride will be described.

[0039] In step S160, nitrogen radicals are supplied from the nitrogen radical source 180. Nitrogen atoms or nitrogen radicals have a large electronegativity and easily attract electrons. Therefore, the nitrogen radicals react with electrons in the vacuum chamber 100 to generate nitrogen anions. In addition, the generated nitrogen anions undergo a recombination reaction with gallium ions (specifically, gallium cations) present near the substrate to generate gallium nitride. The generated gallium nitride is deposited on the substrate. Since the recombination reaction of cations and anions releases a large amount of energy, the gallium nitride film formed on the substrate is a high-quality film even when the temperature of the substrate is low. In this way, in step S160, even when the application of voltage to the target 130 is stopped and sputtering is not performed, gallium nitride can be generated by utilizing the nitrogen radicals supplied from the nitrogen radical source 180.

[0040] It should be noted that cations and anions may be referred to as positive ions and negative ions, respectively.

[0041] In step S160, gallium nitride can be produced by utilizing the metastable state of a rare gas.

[0042] It is known that rare gas atoms in a metastable state with a long life exist in a rare gas plasma. For example, the metastable energy of argon atoms and krypton atoms is 11.61 (eV) and 9.91 (eV), respectively. Such metastable argon or krypton atoms are generated in the sputtering plasma, and can exist even after the plasma has disappeared due to their long life. That is, the metastable argon or krypton atoms can exist even after the application of a voltage to the target 130 is stopped.

[0043] After the application of the voltage to the target 130 is stopped, nitrogen molecules are present in the vacuum chamber 100 in addition to the nitrogen radicals from the nitrogen radical source 180. The dissociation energy from nitrogen molecules to nitrogen atoms due to the collision of electrons is 9.756 (eV), which is close to the metastable energy of argon atoms or krypton atoms. Therefore, when a nitrogen molecule collides with an argon atom or krypton atom in a metastable state, a dissociation reaction of the nitrogen molecule occurs, and nitrogen radicals and nitrogen atoms are generated. That is, even after the application of the voltage to the target 130 is stopped, nitrogen radicals and nitrogen atoms are generated by the argon atom or krypton atom in the metastable state. As described above, since the electronegativity of the nitrogen radical and the nitrogen atom is large, the nitrogen radical and the nitrogen atom react with the electrons in the vacuum chamber 100, and nitrogen anions are generated. In addition, the generated nitrogen anions recombine and react with gallium ions present near the substrate, and gallium nitride is generated.

[0044] As described above, in step S160, gallium nitride can be produced by utilizing not only nitrogen radicals but also argon atoms or krypton atoms in a metastable state.

[0045] In the method for producing a gallium nitride film according to this embodiment, a gallium nitride film is formed on a substrate by repeating steps S150 and S160. Here, the timing of turning on or off the sputtering power supply 160 will be illustrated with reference to FIGS. 3 and 4.

[0046] 3 and 4 are sequence diagrams showing the on / off timing of the sputtering power supply and the nitrogen radical supply source in a gallium nitride film manufacturing method according to one embodiment of the present invention.

[0047] In FIG. 3, the voltage applied to the target 130 is periodically stopped. That is, the sputtering power supply 160 controls in a pulsed manner so as to periodically repeat a first period in which a voltage is applied to the target 130 and a second period in which no voltage is applied to the target 130. The first period and the second period may be the same or different. The first period is not particularly limited, and may be determined by the time it takes for the plasma to stabilize. The second period may be determined by the lifetime of the sputtering gas in a metastable state or the lifetime of metastable excited nitrogen molecules. The second period is, for example, 2 (μsec) or more and 10 (msec). The frequency of the pulse is, for example, 90 (Hz) or more and 400 (kHz) or less.

[0048] In Fig. 4, the sputtering power supply 160 controls the voltage applied to the target 130 by a pulsed voltage in which the first period and the second period are the same. In this case, if a predetermined frequency is determined, the first period and the second period are equally divided. Therefore, the sputtering power supply can control the voltage applied to the target 130 based on one parameter, the frequency. The frequency is, for example, 90 (Hz) or more and 400 (kHz) or less.

[0049] As described above, according to the method for producing a gallium nitride film according to this embodiment, by utilizing nitrogen radicals and a metastable sputtering gas when the application of voltage to the target 130 is stopped, a high-quality gallium nitride film can be formed even at a low substrate temperature.

[0050] <Second embodiment> 5 to 7, a method for producing a gallium nitride film according to one embodiment of the present invention, which is different from the first embodiment, will be described. Note that, in the following, description of the configuration described in the first embodiment may be omitted.

[0051] FIG. 5 is a flow chart showing a method for producing a gallium nitride film according to one embodiment of the present invention.

[0052] In the method for manufacturing a gallium nitride film according to this embodiment, step S170 is performed after step S160 is performed.

[0053] In step S170, the nitrogen radical supply source 180 stops supplying nitrogen radicals into the vacuum chamber 100. Since the supply of nitrogen radicals is stopped in step S170, generation of gallium nitride using the metastable sputtering gas described in the first embodiment becomes dominant.

[0054] In the method for producing a gallium nitride film according to this embodiment, a gallium nitride film is formed on a substrate by repeating steps S140 to S170. Here, the timing of turning on or off the sputtering power supply 160 will be illustrated with reference to Figs. 6 and 7.

[0055] 6 and 7 are sequence diagrams showing the on / off timing of the sputtering power supply and the nitrogen radical supply source in a method for producing a gallium nitride film according to one embodiment of the present invention.

[0056] In FIG. 6, the voltage applied to the target 130 is periodically stopped. That is, the sputtering power supply 160 is controlled in a pulsed manner so as to periodically repeat a first period in which a voltage is applied to the target 130 and a second period in which no voltage is applied to the target 130. Also, the nitrogen radical supply source 180 stops the supply of nitrogen radicals into the vacuum chamber 100 during the second period. The period during which the supply of nitrogen radicals is stopped is equal to or shorter than the second period. That is, the period during which the supply of nitrogen radicals is stopped is, for example, 2 (μsec) or more and 10 (msec). The frequency of the pulse is, for example, 90 (Hz) or more and 400 (kHz) or less.

[0057] In Fig. 7, the sputtering power supply 160 controls the voltage applied to the target 130 by a pulsed voltage having the same first and second periods. When no voltage is applied to the target 130, the supply of nitrogen radicals into the vacuum chamber 100 is also stopped. That is, the sputtering power supply 160 and the nitrogen radical supply source are controlled to be synchronized at a predetermined frequency. The predetermined frequency is, for example, 90 (Hz) or more and 400 (kHz) or less.

[0058] As described above, according to the method for producing a gallium nitride film according to this embodiment, by utilizing nitrogen radicals or a metastable sputtering gas when the application of voltage to the target 130 is stopped, a high-quality gallium nitride film can be formed even at a low substrate temperature.

[0059] <Third embodiment> FIG. 8 is a schematic diagram showing the configuration of a light-emitting device 1000 according to one embodiment of the present invention.

[0060] 8, the light emitting element 1000 includes a substrate 1010, a barrier layer 1020, a buffer layer 1030, an n-type semiconductor layer 1040, a light emitting layer 1050, a p-type semiconductor layer 1060, an n-type electrode 1070, and a p-type electrode 1080. The light emitting element 1000 is a so-called LED (Light Emitting Diode), but is not limited to this.

[0061] The substrate 1010 may be, for example, a quartz substrate or a glass substrate. The barrier layer 1020 may be, for example, a silicon nitride film. The buffer layer 1030 may be, for example, an aluminum nitride film. The n-type semiconductor layer 1040 may be, for example, a gallium nitride film doped with silicon. The light-emitting layer 1050 may be, for example, a laminate in which an indium gallium nitride film and a gallium nitride film are alternately stacked. The p-type semiconductor layer 1060 may be, for example, a gallium nitride film doped with magnesium. The n-type electrode 1070 may be, for example, a metal such as indium. The p-type electrode 1080 may be, for example, a metal such as palladium or gold.

[0062] The manufacturing method of the light emitting device 1000 is as follows. A silicon nitride film and an aluminum nitride film are sequentially formed on the substrate 1010 to form a barrier layer 1020 and a buffer layer 1030. A silicon-doped gallium nitride film is formed on the buffer layer 1030. An indium gallium nitride film and a gallium nitride film are alternately formed on the buffer layer 1030 to form a laminate. A magnesium-doped gallium nitride film is formed on the laminate. Next, the magnesium-doped gallium film, the laminate, and the silicon-doped gallium nitride film are etched using photolithography to form a p-type semiconductor layer 1060, a light emitting layer 1050, and an n-type semiconductor layer 1040. At this time, etching is performed so as to expose a part of the surface of the silicon-doped gallium nitride film. An n-type electrode 1070 and a p-type electrode 1080 are formed on the n-type semiconductor layer 1040 and the p-type semiconductor layer 1060, respectively.

[0063] The method for manufacturing the gallium nitride film described in the first or second embodiment can be applied not only to the gallium nitride film of the light emitting layer 1050 but also to the formation of the aluminum nitride film of the light emitting layer 1050. When forming an aluminum gallium nitride film, aluminum gallium nitride containing nitrogen, aluminum, and gallium can be used as the target 130 of the film forming apparatus 10. In addition, two vacuum chambers may be connected via a substrate transfer unit, a gallium nitride film may be formed in one vacuum chamber, and aluminum gallium nitride may be formed in the other vacuum chamber without breaking the vacuum.

[0064] The method for manufacturing a gallium nitride film described in the first or second embodiment can also be applied to forming an aluminum nitride film for the buffer layer 1030, a silicon-doped gallium nitride film for the n-type semiconductor layer 1040, or a magnesium-doped gallium nitride film for the p-type semiconductor layer 1060.

[0065] As described above, the light-emitting device 1000 according to this embodiment can form a gallium nitride film or the like by applying the gallium nitride film manufacturing method described in the first or second embodiment, and therefore can be fabricated using a substrate with low heat resistance, for example a glass substrate.

[0066] <Fourth embodiment> FIG. 9 is a schematic diagram showing the configuration of a semiconductor device 2000 according to one embodiment of the present invention.

[0067] 9, the semiconductor device 2000 includes a substrate 2010, a barrier layer 2020, a buffer layer 2030, a gallium nitride layer 2040, a first aluminum gallium nitride layer 2050, a second aluminum gallium nitride layer 2060, a third aluminum gallium nitride layer 2070, a source electrode 2080, a drain electrode 2090, a gate electrode 2100, a first insulating layer 2110, a second insulating layer 2120, and a shield electrode 2130. The semiconductor device 2000 is a so-called HEMT (High Electron Mobility Transistor), but is not limited thereto.

[0068] The substrate 2010 may be, for example, a quartz substrate or a glass substrate. The barrier layer 2020 may be, for example, a silicon nitride film. The buffer layer 2030 may be, for example, an aluminum nitride film. The gallium nitride layer 2040 may be, for example, a gallium nitride film. The first aluminum gallium nitride layer 2050 may be, for example, an aluminum gallium nitride film. The second aluminum gallium nitride layer 2060 may be, for example, a silicon-doped gallium nitride film. The third aluminum gallium nitride layer 2070 may be, for example, an aluminum gallium nitride film. The source electrode 2080 and the drain electrode 2090 may be, for example, a metal such as titanium or aluminum. The gate electrode 2100 may be, for example, a metal such as nickel or gold. The first insulating layer 2110 may be, for example, a silicon nitride film. The second insulating layer 2120 may be, for example, a silicon oxide film. The shield electrode 2130 may be made of a laminated metal such as aluminum / titanium (Al / Ti).

[0069] The manufacturing method of the semiconductor device 2000 is as follows. On the substrate 2010, a silicon nitride film, an aluminum nitride film, a gallium nitride film, and an aluminum gallium nitride film are formed to form a barrier layer 2020, a buffer layer 2030, a gallium nitride layer 2040, and a first aluminum gallium nitride layer 2050. Also, on the first aluminum gallium nitride layer 2050, a silicon-doped aluminum gallium nitride film and an aluminum gallium nitride film are formed. Next, the aluminum gallium nitride film and the silicon-doped aluminum gallium nitride film are etched using photolithography to form a third aluminum gallium nitride layer 2070 and a second aluminum gallium nitride layer 2060. At this time, etching is performed so as to expose a part of the surface of the silicon-doped aluminum gallium nitride film. On the second aluminum gallium nitride layer 2060, a source electrode 2080 and a drain electrode 2090 are formed. Furthermore, a gate electrode 2100 is formed on the third aluminum gallium nitride layer 2070. A silicon nitride film and a silicon oxide film are deposited in this order to cover the source electrode 2080, the drain electrode 2090, and the gate electrode 2100, thereby forming a first insulating layer 2110 and a second insulating layer 2120. A shield electrode 2130 is formed on the second insulating layer 2120.

[0070] The method for manufacturing a gallium nitride film described in the first or second embodiment can be applied to forming not only the gallium nitride film of the gallium nitride layer 2040, but also the aluminum nitride film of the buffer layer 2030, the aluminum nitride film of the first aluminum gallium nitride layer 2050, the silicon-doped aluminum gallium nitride film of the second aluminum gallium nitride layer 2060, and the aluminum gallium nitride film of the third aluminum gallium nitride layer 2070.

[0071] As described above, the semiconductor device 2000 according to this embodiment can form a gallium nitride film or the like by applying the gallium nitride film manufacturing method described in the first or second embodiment, and therefore can be fabricated using a substrate with low heat resistance, for example, a glass substrate.

[0072] The above-described embodiments of the present invention may be combined as appropriate as long as they are not mutually inconsistent. Furthermore, those in which a person skilled in the art appropriately adds or removes components or modifies designs, or adds or omits steps or modifies conditions, based on the embodiments, are also included in the scope of the present invention as long as they include the gist of the present invention.

[0073] Even if there are other effects and advantages different from those brought about by the respective embodiments described above, those which are clear from the description in this specification or which can be easily predicted by a person skilled in the art are naturally understood to be brought about by the present invention. [Explanation of symbols]

[0074] 10: film forming apparatus, 100: vacuum chamber, 110: substrate support, 120: heating unit, 130: target, 140: target support, 150: pump, 151: piping, 152: valve, 160: sputtering power supply, 161: wiring, 170: sputtering gas supply source, 171: piping, 172: mass flow controller, 180: nitrogen radical supply source, 181: piping, 1000: light emitting element, 1010: substrate, 1020: barrier layer, 1030: buffer layer, 1040: n-type semiconductor layer, 1050: light emitting layer, 1060: p-type semiconductor layer, 1070: n-type electrode, 1080: p-type electrode, 2000: semiconductor element, 2010: substrate, 2020: barrier layer, 2030: buffer layer, 2040: gallium nitride layer, 2050: first aluminum gallium nitride layer, 2060: second aluminum gallium nitride layer, 2070: third aluminum gallium nitride layer, 2080: source electrode, 2090: drain electrode, 2100: gate electrode, 2110: first insulating layer, 2120: second insulating layer, 2130: shield electrode

Claims

1. Positioning the substrate facing a target containing nitrogen and gallium in a vacuum chamber; Supplying a sputtering gas into the vacuum chamber; Supplying nitrogen radicals into the vacuum chamber; generating a plasma of the sputtering gas by applying a voltage to the target; bombarding the target with ions of the sputtering gas to generate gallium ions; stopping the application of the voltage to the target, and depositing gallium nitride formed by reaction of the gallium ions with nitrogen anions formed by reaction of the electrons in the vacuum chamber with the nitrogen radicals on the substrate; The method for producing a gallium nitride film, wherein the supply of the nitrogen radicals is stopped when the voltage to the target is stopped.

2. Positioning the substrate facing a target containing nitrogen and gallium in a vacuum chamber; Supplying a sputtering gas into the vacuum chamber; Supplying nitrogen radicals into the vacuum chamber; generating a plasma of the sputtering gas by applying a voltage to the target; bombarding the target with ions of the sputtering gas to generate gallium ions; stopping the application of the voltage to the target, generating nitrogen atoms using a metastable sputtering gas in the vacuum chamber, and depositing gallium nitride on the substrate, the nitrogen atoms reacting with electrons in the vacuum chamber to form nitrogen anions, which react with the gallium ions; The method for producing a gallium nitride film, wherein the supply of the nitrogen radicals is stopped when the voltage to the target is stopped.

3. 3. The method for producing a gallium nitride film according to claim 1, wherein the voltage application is stopped for a period of time ranging from 2 (μsec) to 10 (msec).

4. The method for producing a gallium nitride film according to claim 3 , wherein the voltage applied to the target is in the form of a pulse having a predetermined frequency.

5. The method for producing a gallium nitride film according to claim 4 , wherein the predetermined frequency is equal to or greater than 90 (Hz) and equal to or less than 400 (kHz).

6. 6. The method for producing a gallium nitride film according to claim 1, wherein the target is gallium nitride having a composition ratio of the gallium to the nitrogen of 0.7 or more and 2 or less.

7. 6. The method for producing a gallium nitride film according to claim 1, wherein the target is gallium nitride having a composition in which the gallium is more abundant than the nitrogen.

8. The method for producing a gallium nitride film according to claim 1 , wherein the sputtering gas is argon or krypton.

9. The method for producing a gallium nitride film according to claim 1 , wherein the substrate is a quartz substrate.

10. The method for producing a gallium nitride film according to claim 1 , wherein the substrate is a glass substrate.

11. The method for producing a gallium nitride film according to claim 1 , wherein the substrate is provided with an aluminum nitride film.

12. The method for producing a gallium nitride film according to claim 1 , further comprising heating the substrate.

13. The method for producing a gallium nitride film according to claim 12 , wherein the substrate is heated to a temperature of 400° C. or more and 600° C. or less.

Citation Information

Patent Citations

  • Method for forming epitaxial thin film, method for manufacturing semiconductor substrate, semiconductor element, light emitting element and electronic element

    JP2008270749A

  • Film forming apparatus and film formation method

    JP2013125851A

  • Gallium nitride-based film and production method thereof

    JP2016204748A

  • Semiconductor substrate and manufacturing method of the same

    JP2019192697A

  • Film deposition apparatus

    JP2020164927A