Thermoplastic elastomer composition, vibration damping material, gear, and composite molded body

A thermoplastic elastomer composition combining polyester and hydrogenated aromatic vinyl compounds addresses bonding and damping issues, enhancing adhesion and vibration damping in composite molded bodies and gears.

JP7596307B2Active Publication Date: 2024-12-09KURARAY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2021567202
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-27
Filing Date
2020-12-10
Publication Date
2024-12-09
Estimated Expiration
2040-12-10

AI Technical Summary

Technical Problem

The existing thermoplastic elastomer compositions used in composite molded bodies face issues with poor bonding strength and complex manufacturing processes due to the combination of non-heat-sealable resins, and they also suffer from insufficient vibration damping properties.

Method used

A thermoplastic elastomer composition is developed by combining a polyester thermoplastic elastomer with a hydrogenated aromatic vinyl compound elastomer, which includes a polymer block derived from an aromatic vinyl compound and a conjugated diene compound, with a specific glass transition temperature range, to enhance adhesion and vibration damping properties.

Benefits of technology

The composition improves vibration damping properties while maintaining the properties of the polyester thermoplastic elastomer, offering better bonding strength and simplifying the manufacturing process, suitable for various applications including gears and composite molded articles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007596307000001
    Figure 0007596307000001
  • Figure 0007596307000002
    Figure 0007596307000002
  • Figure 0007596307000003
    Figure 0007596307000003
Patent Text Reader

Abstract

Provided is a thermoplastic elastomer composition which can have improved vibration-damping properties while retaining properties inherent in the thermoplastic elastomer, which is based on a polyester. The thermoplastic elastomer composition comprises a polyester-based thermoplastic elastomer (A) and an elastomer (B) based on a hydrogenated aromatic vinyl compound and having a glass transition temperature Tg of -10 to 40°C, wherein the elastomer (B) based on a hydrogenated aromatic vinyl compound is a product of hydrogenation of a block copolymer comprising a polymer block (a) having a structural unit derived from an aromatic vinyl compound and a polymer block (b) having a structural unit derived from a conjugated diene compound, the mass ratio of the polyester-based thermoplastic elastomer (A) to the elastomer (B) based on a hydrogenated aromatic vinyl compound, A / B, being 99 / 1 to 1 / 99.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermoplastic elastomer composition, a vibration damping material, a gear, and a composite molded article. [Background technology]

[0002] When manufacturing a composite molded product by combining resins that do not thermally bond, the composite part of the two resins is provided with uneven parts, the core material is partially covered with a surface layer material, holes are drilled in the core material and the surface layer material is extended to the back side, adhesive is applied to the joint parts, etc. As a result, the obtained composite molded product has problems such as poor bonding strength between the two layers, a complicated structure, and an increase in the number of steps in the manufacturing stage.

[0003] Under such circumstances, in order to solve the above problems, a thermoplastic elastomer composition having excellent heat fusion properties to the material to be fused was obtained by adding a styrene-based elastomer to a polyester-based thermoplastic elastomer (TPEE) (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 3381488 Summary of the Invention [Problem to be solved by the invention]

[0005] However, the above thermoplastic elastomer composition has a new problem in that the vibration damping properties are insufficient.

[0006] Therefore, an object of the present invention is to provide a thermoplastic elastomer composition that can improve vibration damping while maintaining the properties of a polyester-based thermoplastic elastomer, a vibration damping material containing the thermoplastic elastomer composition, a gear containing the thermoplastic elastomer composition, and a composite molded product having a thermoplastic elastomer composition layer that contains the thermoplastic elastomer composition. [Means for solving the problem]

[0007] Means for Solving the Problems The present inventors have conducted extensive research to solve the above problems, and as a result have found that by adding a hydrogenated aromatic vinyl compound-based elastomer (B) having a glass transition temperature within a predetermined range to a polyester-based thermoplastic elastomer (A), it is possible to improve vibration damping properties while maintaining the properties of the polyester-based thermoplastic elastomer (A), thereby solving the above problems and completing the present invention. That is, the present invention is as follows. A thermoplastic elastomer composition comprising a polyester-based thermoplastic elastomer (A) and a hydrogenated aromatic vinyl compound-based elastomer (B) having a glass transition temperature Tg of −10 to 40° C., The hydrogenated aromatic vinyl compound-based elastomer (B) is a hydrogenated product of a block copolymer containing a polymer block (a) having a structural unit derived from an aromatic vinyl compound and a polymer block (b) having a structural unit derived from a conjugated diene compound, A thermoplastic elastomer composition, wherein the mass ratio (A / B) of the polyester-based thermoplastic elastomer (A) to the hydrogenated aromatic vinyl compound-based elastomer (B) is 99 / 1 to 1 / 99. Effect of the Invention

[0008] According to the present invention, it is possible to provide a thermoplastic elastomer composition that can improve vibration damping while maintaining the properties of a polyester-based thermoplastic elastomer, a vibration damping material containing the thermoplastic elastomer composition, a gear containing the thermoplastic elastomer composition, and a composite molded product having a thermoplastic elastomer composition layer that contains the thermoplastic elastomer composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] In this specification, preferred definitions may be selected arbitrarily, and combinations of preferred definitions may be considered more preferred. In this specification, the expression "XX to YY" means "at least XX and at most YY." In this specification, the lower limit and upper limit described in stages for the preferred numerical range (e.g., range of content, etc.) can be independently combined. For example, the description "preferably 10 to 90, more preferably 30 to 60" can be combined with the "preferable lower limit (10)" and the "more preferable upper limit (60)" to form "10 to 60." In this specification, the term "unit" (where "" indicates a monomer) means "a structural unit derived from", for example, "propylene unit" means "a structural unit derived from propylene". In this specification, for example, "(meth)acrylic acid" refers to both "acrylic acid" and "methacrylic acid", and similar terms. In this specification, the weight average molecular weight is a weight average molecular weight calculated in terms of standard polystyrene by gel permeation chromatography (GPC).

[0010] (Thermoplastic elastomer composition) The thermoplastic elastomer composition of the present invention contains a polyester-based thermoplastic elastomer (A) and a hydrogenated aromatic vinyl compound-based elastomer (B), and further contains additives as required.

[0011] The mass ratio (A / B) of the polyester-based thermoplastic elastomer (A) to the hydrogenated aromatic vinyl compound-based elastomer (B) is not particularly limited as long as it is 99 / 1 to 1 / 99. From the viewpoint of the balance between oil resistance, solvent resistance and vibration damping properties, however, it is preferably 75 / 25 to 95 / 5, and more preferably 80 / 20 to 90 / 10. Here, if the amount of hydrogenated aromatic vinyl compound-based elastomer (B) added is too small (the mass ratio (A / B) exceeds 99 / 1), there is a risk that vibration damping properties cannot be exhibited. On the other hand, if the amount of hydrogenated aromatic vinyl compound-based elastomer (B) added is too large (the mass ratio (A / B) is less than 1 / 99), the properties of the thermoplastic polyester-based elastomer (TPEE) may be lost.

[0012] <Polyester-based thermoplastic elastomer (A)> The polyester-based thermoplastic elastomer (A) can be obtained, for example, by subjecting (i) an aliphatic and / or alicyclic diol having 2 to 12 carbon atoms, (ii) an aromatic dicarboxylic acid or an alkyl ester thereof, and (iii) a polyalkylene ether glycol as raw materials to an esterification reaction or a transesterification reaction, and then subjecting the resulting oligomer to a polycondensation reaction.

[0013] <<(i) Aliphatic and / or alicyclic diol having 2 to 12 carbon atoms>> As the aliphatic and / or alicyclic diol having 2 to 12 carbon atoms, those known as raw materials for polyesters, particularly raw materials for polyester elastomers, can be used, such as ethylene glycol, propylene glycol, trimethylene glycol, 1,4-butanediol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, etc. These aliphatic and / or alicyclic diols may be used alone or in combination of two or more. Among these, 1,4-butanediol and ethylene glycol are preferred, and 1,4-butanediol is more preferred.

[0014] <<(ii) Aromatic dicarboxylic acid or its alkyl ester>> As the aromatic dicarboxylic acid, those known as raw materials for polyesters, particularly raw materials for polyester elastomers, can be used, for example, terephthalic acid, isophthalic acid, phthalic acid, 2,6-naphthalenedicarboxylic acid, etc. These aromatic dicarboxylic acids may be used alone or in combination of two or more. Among these, terephthalic acid and 2,6-naphthalenedicarboxylic acid are preferred, and terephthalic acid is more preferred. Examples of the alkyl ester of aromatic dicarboxylic acid include dimethyl esters such as dimethyl terephthalate, dimethyl isophthalate, dimethyl phthalate, and 2,6-dimethyl naphthalate. These alkyl esters of aromatic dicarboxylic acid may be used alone or in combination of two or more. Among these, dimethyl terephthalate and 2,6-dimethyl naphthalate are preferred, and dimethyl terephthalate is more preferred. In addition to the above, a small amount of a trifunctional diol, other diols, other dicarboxylic acids and their esters may be copolymerized. Furthermore, an aliphatic or alicyclic dicarboxylic acid such as adipic acid or an alkyl ester thereof may also be used as a copolymerization component.

[0015] <<(iii) Polyalkylene ether glycol>> Examples of polyalkylene ether glycols include polyethylene glycol, poly(1,2 and 1,3 propylene ether) glycol, polytetramethylene ether glycol, polyhexamethylene ether glycol, block or random copolymers of ethylene oxide and propylene oxide, block or random copolymers of ethylene oxide and tetrahydrofuran, etc. These polyalkylene ether glycols may be used alone or in combination of two or more. Among these, polytetramethylene ether glycol is preferred. The weight-average molecular weight of the polyalkylene ether glycol is preferably 400 to 6,000, more preferably 500 to 4,000, and particularly preferably 600 to 3,000. When the weight-average molecular weight of the polyalkylene ether glycol is within the above range, the block property of the copolymer can be improved, and a decrease in the physical properties of the polymer due to phase separation in the system can be suppressed.

[0016] The content of polyalkylene ether glycol is preferably 5 to 95 mass %, more preferably 10 to 85 mass %, and particularly preferably 20 to 80 mass %, based on the produced block copolymer. By reducing the content of polyalkylene ether glycol to less than 95 mass %, it becomes possible to obtain a polymer by condensation polymerization.

[0017] Instead of the polyalkylene ether glycol, (iv) a polyester oligomer obtained by condensing an aliphatic or alicyclic dicarboxylic acid with an aliphatic diol, or (v) a polyester oligomer synthesized from an aliphatic lactone or an aliphatic monool carboxylic acid may be used.

[0018] <<(iv) Polyester oligomers condensed with aliphatic or alicyclic dicarboxylic acids and aliphatic diols>> Examples of polyester oligomers obtained by condensing an aliphatic or alicyclic dicarboxylic acid with an aliphatic diol include polyester oligomers having a structure obtained by condensing (a) one or more of alicyclic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid, 1,2-cyclohexanedicarboxylic acid, dicyclohexyl-4,4'-dicarboxylic acid, etc., or aliphatic or alicyclic dicarboxylic acids such as succinic acid, oxalic acid, adipic acid, sebacic acid, etc., with (b) one or more of aliphatic diols such as ethylene glycol, propylene glycol, tetramethylene glycol, pentamethylene glycol, etc.

[0019] <<(v) Polyester oligomers synthesized from aliphatic lactones or aliphatic monool carboxylic acids>> Examples of polyester oligomers synthesized from aliphatic lactones or aliphatic monool carboxylic acids include polycaprolactone-based polyester oligomers synthesized from ε-caprolactone, ω-oxycaproic acid, and the like.

[0020] <<Esterification reaction, transesterification reaction, polycondensation reaction>> The above-mentioned esterification reaction, ester exchange reaction, and polycondensation reaction can be carried out according to a conventional method.

[0021] As the catalyst for these reactions, one or more of known catalysts such as alcoholates, chlorides, and oxides of tin, titanium, zinc, manganese, etc. can be used. It is preferable to use an organic titanium catalyst, and it is more preferable to use tetrabutyl titanate.

[0022] As an auxiliary, phosphoric acid, phosphorous acid, hypophosphorous acid, or metal salts thereof may be added. Among these, it is preferable to add an alkali metal hypophosphite in terms of improving hydrolysis resistance.

[0023] [Alkaline metal hypophosphite] Examples of the alkali metal hypophosphite include sodium hypophosphite, potassium hypophosphite, lithium hypophosphite, etc. Among these, sodium hypophosphite is preferred. The amount of the alkali metal hypophosphite added is not particularly limited, but is preferably 1 to 1,000 ppm by mass, more preferably 3 to 200 ppm by mass, and particularly preferably 5 to 80 ppm by mass, based on the produced polymer. By setting the amount of the alkali metal hypophosphite to be added within the above range, the effect of the addition can be fully obtained and inhibition of the polycondensation reaction can be suppressed. The method of adding the alkali metal hypophosphite is not particularly limited, and the alkali metal hypophosphite may be added to the molten polymer in any state of solution, slurry, or solid, but is preferably added in the form of a slurry. The timing of addition of the alkali metal hypophosphite is not particularly limited, and it may be added at any time at least before the end of the polycondensation reaction, i.e., before the esterification reaction or the ester exchange reaction, and before the end of the polycondensation reaction. However, it is preferable to add it immediately before the start of polycondensation in order to minimize the decrease in polymerizability.

[0024] In the reaction steps of the esterification reaction, the ester exchange reaction, and the polycondensation reaction, additives other than the above-mentioned catalysts and auxiliaries may be present. Examples of additives other than the catalyst and auxiliary include hindered phenol-based oxidation stabilizers, hindered amine-based oxidation stabilizers, phosphorus-based oxidation stabilizers, sulfur-based oxidation stabilizers, triazole-based light stabilizers, and other known additives. Among these, the hindered phenol-based oxidation stabilizers are preferred, and it is more preferable in terms of effectiveness to add the hindered phenol-based oxidation stabilizer in an amount of 0.01 to 1% by mass based on the polymer.

[0025] The esterification reaction or the ester exchange reaction is usually carried out at 120 to 250° C., and preferably at 150 to 230° C. The melt polycondensation reaction, which is a type of polycondensation reaction, is usually carried out at 200 to 280° C. for 2 to 6 hours under a reduced pressure of 10 torr or less.

[0026] Usually, the polymer obtained by melt polycondensation is kept at a temperature above the melting point, and is sequentially discharged from the reactor and pelletized. The pellets obtained here may be further solid-phase polymerized as necessary. Examples of such polyester-based thermoplastic elastomers (A) include commercially available polymers such as "Pelprene P" or "Pelprene S" (product name of Toyobo Co., Ltd.), "Hytrel" (product name of Toray-DuPont Co., Ltd.), "Lowmod" (product name of Japan GE Plastics Co., Ltd.), "Nichigo Polyester" (product name of Nippon Synthetic Chemical Industry Co., Ltd.), and "Teijin Polyester Elastomer" (product name of Teijin Limited).

[0027] <<Content of polyester-based thermoplastic elastomer (A)>> The content of the polyester-based thermoplastic elastomer (A) in the thermoplastic elastomer composition is not particularly limited as long as it is 1% by mass or more and 99% by mass or less based on 100% by mass of the total amount of the thermoplastic elastomer composition, and can be appropriately adjusted depending on the type of the polyester-based thermoplastic elastomer (A) and the use of the thermoplastic elastomer composition. The content of the polyester-based thermoplastic elastomer (A) is not particularly limited, and may be, for example, 90% by mass or less, 75% by mass or less, 60% by mass or less, or 50% by mass or less based on 100% by mass of the total amount of the thermoplastic elastomer composition, or 10% by mass or more, 25% by mass or more, 40% by mass or more, or 50% by mass or more.

[0028] <<Structure of polyester-based thermoplastic elastomer (A)>> The structure of the polyester-based thermoplastic elastomer (A) is not particularly limited, but examples thereof include a structure consisting of a hard segment (crystalline phase) made of a polyester portion and a soft segment (amorphous phase) made of a polyether portion or a polyester portion. Examples of the polyester portion of the hard segment include a polybutylene terephthalate (PBT) portion, a polyethylene terephthalate portion, and a polyethylene naphthalate portion. Examples of the polyether moiety of the soft segment include an aliphatic polyether moiety such as a polytetramethylene ether moiety. The polyester moiety of the soft segment may, for example, be an aliphatic polyester moiety such as a poly-ε-caprolactone moiety.

[0029] <<Maximum tan δ strength of polyester thermoplastic elastomer (A) at 0 to 40°C>> The maximum value of the tan δ strength of the polyester-based thermoplastic elastomer (A) at 0 to 40° C. is not particularly limited, but is preferably 0.05 or more, more preferably 0.055 or more, and particularly preferably 0.06 or more. If the maximum value of the tan δ strength of the polyester-based thermoplastic elastomer (A) is within the above range, the vibration damping property can be further improved. The maximum value of the tan δ strength of the polyester-based thermoplastic elastomer (A) is a value measured according to the measurement method described in the examples. In addition, when the thermoplastic elastomer composition contains multiple types of polyester-based thermoplastic elastomers (A), the maximum value of the tan δ strength of the thermoplastic elastomer composition consisting only of multiple polyester-based thermoplastic elastomers (A) is defined as the maximum value of the tan δ strength of the polyester-based thermoplastic elastomer (A) at 0 to 40°C.

[0030] <<Characteristics of polyester-based thermoplastic elastomer (A)>> The properties of the polyester-based thermoplastic elastomer (A) include oil resistance, heat resistance, sliding properties, good moldability, mechanical strength resistance, chemical resistance, and aging resistance due to the hard segment (crystalline phase), and sound deadening properties, low-temperature flexibility, and high impact absorption due to the soft segment (amorphous phase).

[0031] <Hydrogenated aromatic vinyl compound elastomer (B)> The hydrogenated aromatic vinyl compound-based elastomer (B) is a hydrogenated product obtained by hydrogenating a block copolymer containing a polymer block (a) having a structural unit derived from an aromatic vinyl compound and a polymer block (b) having a structural unit derived from a conjugated diene compound.

[0032] <<Polymer block (a)>> The polymer block (a) constituting the block copolymer is a polymer block having a structural unit derived from an aromatic vinyl compound used as a monomer. When the polymer block (a) is a polymer block having a structural unit derived from an aromatic vinyl compound, vibration-damping properties and mechanical properties can be improved. The polymer block (a) preferably contains structural units derived from an aromatic vinyl compound (hereinafter, may be abbreviated as "aromatic vinyl compound units") in more than 70 mol % of the polymer block (a), and from the viewpoint of mechanical properties, the content is preferably 80 mol % or more, more preferably 90 mol % or more, particularly preferably 95 mol % or more, and particularly preferably substantially 100 mol %.

[0033] [Aromatic vinyl compounds] Examples of aromatic vinyl compounds include styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, α-methylstyrene, β-methylstyrene, 2,6-dimethylstyrene, 2,4-dimethylstyrene, α-methyl-o-methylstyrene, α-methyl-m-methylstyrene, α-methyl-p-methylstyrene, β-methyl-o-methylstyrene, β-methyl-m-methylstyrene, β-methyl-p-methylstyrene, 2,4,6-trimethylstyrene, α-methyl-2,6-dimethylstyrene, α-methyl-2,4-dimethylstyrene, β-methyl-2,6-dimethylstyrene, β-methyl-2,4-dimethylstyrene, o-chlorostyrene, m-chlorostyrene, p-chlorostyrene, 2,6-dichlorostyrene, 2,4-dichlorostyrene, α-chloro-o-chlorostyrene, α-chlorostyrene, Examples of the aromatic vinyl compounds include 2-m-chlorostyrene, α-chloro-p-chlorostyrene, β-chloro-o-chlorostyrene, β-chloro-m-chlorostyrene, β-chloro-p-chlorostyrene, 2,4,6-trichlorostyrene, α-chloro-2,6-dichlorostyrene, α-chloro-2,4-dichlorostyrene, β-chloro-2,6-dichlorostyrene, β-chloro-2,4-dichlorostyrene, ot-butylstyrene, mt-butylstyrene, pt-butylstyrene, o-methoxystyrene, m-methoxystyrene, p-methoxystyrene, o-chloromethylstyrene, m-chloromethylstyrene, p-chloromethylstyrene, o-bromomethylstyrene, m-bromomethylstyrene, p-bromomethylstyrene, styrene derivatives substituted with silyl groups, indene, vinylnaphthalene, and N-vinylcarbazole. These aromatic vinyl compounds may be used alone or in combination of two or more. Among these, from the viewpoint of the balance between production costs and physical properties, styrene, α-methylstyrene, p-methylstyrene, and mixtures thereof are preferred, and styrene is more preferred.

[0034] As long as the object and effect of the present invention are not hindered, the polymer block (a) may contain structural units derived from unsaturated monomers other than aromatic vinyl compounds (hereinafter, sometimes abbreviated as "other unsaturated monomer units"), but the amount of such units in the polymer block (a) is preferably 30 mol % or less, more preferably less than 20 mol %, even more preferably less than 15 mol %, still more preferably less than 10 mol %, even more preferably less than 5 mol %, and particularly preferably 0 mol %. Examples of the other unsaturated monomer include at least one selected from the group consisting of butadiene, isoprene, 2,3-dimethylbutadiene, 1,3-pentadiene, 1,3-hexadiene, isobutylene, methyl methacrylate, methyl vinyl ether, β-pinene, 8,9-p-menthene, dipentene, methylenenorbornene, 2-methylenetetrahydrofuran, etc. When the polymer block (a) contains the other unsaturated monomer unit, the bonding form is not particularly limited and may be either random or tapered.

[0035] The block copolymer may have at least one polymer block (a). When the block copolymer has two or more polymer blocks (a), the polymer blocks (a) may be the same or different. In this specification, "polymer blocks are different" means that at least one of the monomer units constituting the polymer blocks, the weight average molecular weight, the stereoregularity, and, when a plurality of monomer units are present, the ratio of each monomer unit and the form of copolymerization (random, gradient, block) is different.

[0036] [Weight average molecular weight] The weight average molecular weight (Mw) of the polymer block (a) is not particularly limited, but among the polymer blocks (a) contained in the block copolymer, at least one polymer block (a) preferably has a weight average molecular weight of 3,000 to 60,000, and more preferably 4,000 to 50,000. When the block copolymer has at least one polymer block (a) having a weight average molecular weight within the above range, the mechanical strength is further improved and the moldability is also excellent. The weight average molecular weight is a weight average molecular weight calculated in terms of standard polystyrene by gel permeation chromatography (GPC).

[0037] [Content of polymer block (a)] The content of the polymer block (a) in the block copolymer is preferably 30% by mass or less, more preferably 16% by mass or less, and particularly preferably 14% by mass or less. If the content of the polymer block (a) in the block copolymer is 30% by mass or less, the hydrogenated block copolymer can have appropriate flexibility and excellent vibration damping properties without decreasing the peak top intensity of tan δ. The lower limit is preferably 1% by mass or more, more preferably 3% by mass or more, and particularly preferably 6% by mass or more. If the content is 1% by mass or more, the hydrogenated block copolymer can have mechanical properties and moldability suitable for various applications. The content of the polymer block (a) in the block copolymer is 1 The value was determined by H-NMR measurement, and more specifically, the value was measured according to the method described in the Examples.

[0038] <<Polymer block (b)>> The polymer block (b) constituting the block copolymer is a polymer block having a structural unit derived from a conjugated diene compound, and preferably has a structural unit containing one or more alicyclic skeletons (X) represented by the following formula (X) in the main chain (hereinafter sometimes abbreviated as "alicyclic skeleton-containing unit"). Furthermore, the polymer block (b) may contain a structural unit derived from a conjugated diene compound that does not contain an alicyclic skeleton (X) (hereinafter, sometimes abbreviated as "conjugated diene unit"). The total amount of the conjugated diene units in the polymer block (b) is not particularly limited, but is preferably 50 mol % or more, more preferably 70 mol % or more, even more preferably 90 mol % or more, and particularly preferably substantially 100 mol %. The total of the alicyclic skeleton-containing units and the conjugated diene units in the polymer block (b) is not particularly limited, but from the viewpoint of exhibiting excellent vibration damping properties, it is preferably 50 mol % or more, more preferably 70 mol % or more, even more preferably 90 mol % or more, and particularly preferably substantially 100 mol %.

[0039] [ka] (In the above formula (X), R 1 ~R 3 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 11 carbon atoms, 1 ~R 3 may be the same or different.)

[0040] In the above formula (X), R 1 ~R 3 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 11 carbon atoms, 1 ~R 3 may be the same or different. The number of carbon atoms in the hydrocarbon group is preferably 1 to 5, more preferably 1 to 3, and particularly preferably 1 (i.e., a methyl group). The hydrocarbon group may be a straight chain or branched chain, and may be a saturated or unsaturated hydrocarbon group. From the viewpoint of physical properties and the formation of an alicyclic skeleton (X), R 1 ~R 3 are preferably each independently a hydrogen atom or a methyl group. When the block copolymer is hydrogenated, the vinyl group in the above formula (X) can be hydrogenated, and therefore the alicyclic skeleton (X) in the hydrogenated product contains a skeleton in which the vinyl group in the above formula (X) has been hydrogenated.

[0041] The polymer block (b) is a structural unit derived from a conjugated diene compound, and the alicyclic skeleton (X) is derived from the conjugated diene compound. The alicyclic skeleton (X) is produced by anionic polymerization of a conjugated diene compound by the method described below, and it is preferable that the alicyclic skeleton (X) is contained in the main chain of the alicyclic skeleton-containing unit depending on the conjugated diene compound used. By incorporating the alicyclic skeleton (X) in the main chain of the structural unit contained in the polymer block (b), molecular motion is reduced, so that the glass transition temperature is increased, and the peak top intensity of tan δ around room temperature is improved, thereby enabling the development of excellent vibration damping properties.

[0042] [Conjugated diene compounds] Examples of the conjugated diene compound include butadiene, isoprene, hexadiene, 2,3-dimethyl-1,3-butadiene, 2-phenyl-1,3-butadiene, 1,3-pentadiene, 2-methyl-1,3-pentadiene, 1,3-hexadiene, 1,3-octadiene, 1,3-cyclohexadiene, 2-methyl-1,3-octadiene, 1,3,7-octatriene, farnesene, myrcene, and chloroprene. These conjugated diene compounds may be used alone or in combination of two or more. Among these, isoprene is preferably used.

[0043] When isoprene and butadiene are used in combination, there is no particular limitation on the blending ratio [isoprene / butadiene] (mass ratio), but it is preferably 5 / 95 to 95 / 5, more preferably 10 / 90 to 90 / 10, even more preferably 40 / 60 to 70 / 30, and particularly preferably 45 / 55 to 65 / 35. The blending ratio [isoprene / butadiene] in molar ratio is preferably 5 / 95 to 95 / 5, more preferably 10 / 90 to 90 / 10, even more preferably 40 / 60 to 70 / 30, and particularly preferably 45 / 55 to 55 / 45.

[0044] As a specific example, an alicyclic skeleton (X) that can be mainly produced when butadiene, isoprene, or a combination of butadiene and isoprene is used as the conjugated diene compound will be described. When butadiene is used alone as the conjugated diene compound, an alicyclic skeleton (X) having a combination of the following substituents (i) can be produced. In this case, the alicyclic skeleton (X) is R 1 ~R 3 and R are simultaneously hydrogen atoms. Therefore, as a preferred embodiment of the block copolymer or its hydrogenated product, the polymer block (b) is 1 ~R 3 and (X) are both hydrogen atoms.

[0045] When isoprene is used alone as the conjugated diene compound, two types of alicyclic skeletons (X) having the following combinations of substituents (v) and (vi) can be mainly produced. When butadiene and isoprene are used in combination as the conjugated diene compound, six types of alicyclic skeletons (X) having the following combinations of substituents (i) to (vi) can be mainly produced. (i):R 1 = hydrogen atom, R 2 = hydrogen atom, R 3 = Hydrogen atom (ii):R 1 = hydrogen atom, R 2 = methyl group, R 3 = Hydrogen atom (iii):R 1 = hydrogen atom, R 2 = hydrogen atom, R 3 = Methyl group (iv):R 1 = methyl group, R 2 = hydrogen atom, R 3 = Hydrogen atom (v):R 1 = methyl group, R 2 = methyl group, R 3 = Hydrogen atom (vi):R 1 = methyl group, R 2 = hydrogen atom, R 3 = Methyl group

[0046] In the above formula (X), from the viewpoint of further improving vibration damping properties by making molecular motion smaller by having a substituent which is a hydrocarbon group, at least one alicyclic skeleton (X) in the polymer block (b) is 1 ~R 3 It is preferable that at least one of the above is an alicyclic skeleton (X') which is a hydrocarbon group having 1 to 11 carbon atoms. Among these, it is more preferable that the hydrocarbon group in the alicyclic skeleton (X') is a methyl group, from the viewpoints of efficiently producing the alicyclic skeleton from the conjugated diene compound and of the balance between vibration damping properties and mechanical properties. Especially R 1 ~R 3 each independently represents a hydrogen atom or a methyl group, and R 1 ~R 3 is preferably an alicyclic skeleton not simultaneously containing a hydrogen atom. In other words, the polymer block (b) preferably has a constitutional unit containing in the main chain at least one of the alicyclic skeletons having the combinations of the above substituents (ii) to (vi).

[0047] [Amount of vinyl bonds in polymer block (b)] When the structural units constituting the polymer block (b) are any of an isoprene unit, a butadiene unit, and a mixed unit of isoprene and butadiene, the respective bonding forms of isoprene and butadiene other than the bonding form forming the alicyclic skeleton (X) can be 1,2-bonds and 1,4-bonds in the case of butadiene, and 1,2-bonds, 3,4-bonds and 1,4-bonds in the case of isoprene.

[0048] The total content of 3,4-bond units and 1,2-bond units in the polymer block (b) (hereinafter sometimes simply referred to as "vinyl bond content") is not particularly limited, but is preferably 65 to 90 mol%, more preferably 70 to 87 mol%, and particularly preferably 75 to 85 mol%. If it is within the above range, excellent vibration damping properties can be exhibited. Here, the vinyl bond amount is measured according to the method described in the Examples. 1 This value was calculated by H-NMR measurement. When the polymer block (b) is composed only of butadiene, the above-mentioned "content of 3,4-bond units and 1,2-bond units" is to be read as "content of 1,2-bond units".

[0049] [Alicyclic skeleton (X) content in polymer block (b)] In the polymer block (b), from the viewpoint of exhibiting a more excellent vibration-damping effect and easily suppressing a decrease in adhesive strength even at high temperatures, the polymer block (b) preferably contains 1 mol% or more of an alicyclic skeleton (X), more preferably contains 1.1 mol% or more, even more preferably contains 1.4 mol% or more, even more preferably contains 1.8 mol% or more, even more preferably contains 4 mol% or more, even more preferably contains 10 mol% or more, and particularly preferably contains 13 mol% or more. The upper limit of the content of the alicyclic skeleton (X) in the polymer block (b) is not particularly limited as long as it is within a range that does not impair the effects of the present invention, but from the viewpoint of productivity, it is preferably 40 mol% or less, may be 30 mol% or less, may be 20 mol% or less, or may be 18 mol% or less. From the viewpoint of further improving vibration-damping properties, the polymer block (b) preferably contains the alicyclic skeleton (X') at 1 mol % or more, more preferably at 1.3 mol % or more, and particularly preferably at 1.6 mol % or more. The upper limit of the content of the alicyclic skeleton (X') is the same as the upper limit of the content of the alicyclic skeleton (X).

[0050] More specifically, when isoprene is used as the conjugated diene compound, when butadiene is used, or when butadiene and isoprene are used in combination, the alicyclic skeleton content in each case is as follows. When isoprene is used as the conjugated diene compound, when there is one or more alicyclic skeletons (X') having a combination of the substituents (v) and (vi) in the polymer block (b), their total content is not particularly limited, but from the viewpoint of exhibiting a better vibration-damping effect and making it easier to suppress the decrease in adhesive strength even at high temperatures, it is preferably 1 mol% or more, more preferably 1.5 mol% or more, and from the viewpoint of obtaining a better vibration-damping effect in a wide temperature range, it is even more preferably 2 mol% or more, even more preferably 3 mol% or more, and particularly preferably 4 mol% or more. In addition, the upper limit of the above total content when isoprene is used is the same as the upper limit of the content of the alicyclic skeleton (X).

[0051] When butadiene is used as the conjugated diene compound, the content of the alicyclic skeleton (X) in the polymer block (b) is preferably 5 mol% or more, more preferably 10 mol% or more, even more preferably 15 mol% or more, even more preferably 20 mol% or more, even more preferably 25 mol% or more, and particularly preferably 30 mol% or more, from the viewpoint of exhibiting a more excellent vibration-damping effect and easily suppressing a decrease in adhesive strength even at high temperatures. The upper limit of the content when butadiene is used is the same as the upper limit of the content of the alicyclic skeleton (X).

[0052] In the case where butadiene and isoprene are used in combination as the conjugated diene compound, when one or more alicyclic skeletons (X') having a combination of the substituents (ii), (iii), (v), and (vi) are present in the polymer block (b), the total content thereof is preferably 1 mol% or more, more preferably 2 mol% or more, even more preferably 5 mol% or more, even more preferably 8 mol% or more, and particularly preferably 13 mol% or more, from the viewpoint of exhibiting a more excellent vibration-damping effect and making it easier to suppress a decrease in adhesive strength even at high temperatures. The upper limit of the above total content when butadiene and isoprene are used in combination is the same as the upper limit of the content of the alicyclic skeleton (X). In addition, when butadiene and isoprene are used in combination as the conjugated diene compound, when one or more alicyclic skeletons (X) having a combination of the substituents (i) to (vi) are present in the polymer block (b), the total content thereof is preferably 1 mol% or more, and more preferably 5 mol% or more, from the viewpoint of exhibiting a more excellent vibration-damping effect and making it easier to suppress a decrease in adhesive strength even at high temperatures. The upper limit of the above-mentioned total content when butadiene and isoprene are used in combination is the same as the upper limit of the content of the alicyclic skeleton (X).

[0053] The content of the alicyclic skeleton (X) (including (X')) in the block copolymer or its hydrogenated product is 13 It is a value determined from the integral value derived from the alicyclic skeleton (X) in the polymer block (b) by C-NMR measurement, and more specifically, it is a value measured according to the method described in the Examples.

[0054] For hydrogenated products, 13 In the C-NMR measurement, almost no peaks due to the carbon atoms on the alicyclic skeleton (X) are observed, but the substituent R 3 is a hydrocarbon group having 1 to 11 carbon atoms, 3 A peak derived from a carbon atom on the alicyclic skeleton (X) bonded to a branched alkyl group derived from a vinyl group having the formula: In this way, when the hydrogenation rate of the polymer block (b) in the hydrogenated product is 85 to 99 mol%, the above R 3 It is also possible to specify the molar ratio of the carbon atom on the alicyclic skeleton (X) bonded to the branched alkyl group derived from the vinyl group and the carbon atom on the main chain bonded to the branched alkyl group derived from the vinyl group.

[0055] For example, in the alicyclic skeleton (X) having a combination of the substituents (iii) and (vi) described above, the carbon atom (c) in the alicyclic skeleton (X) bonded to the isoprene group is 13 The chemical shift in C-NMR appears in the vicinity of 50.0 to 52.0 ppm, which corresponds to the carbon atom on the main chain that bonds to the isoprene group ((d) in the chemical formula below). 13 The chemical shift in C-NMR appears at around 43.0 to 45.0 ppm. When the hydrogenation rate is 40 to 99 mol%, 13 The peak area ratio [peak area at chemical shift values ​​of 50.0 to 52.0 ppm] / [peak area at chemical shift values ​​of 43.0 to 45.0 ppm] measured by C-NMR is usually in the range of 0.01 to 3.00, and from the viewpoint of exhibiting better vibration damping properties, the area ratio is preferably in the range of 0.01 to 1.50, more preferably in the range of 0.01 to 1.00, even more preferably in the range of 0.01 to 0.50, and particularly preferably in the range of 0.01 to 0.25. More specifically, the peak area ratio can be measured according to the method described in the Examples.

[0056] [ka]

[0057] [Other structural units] The polymer block (b) may contain a structural unit derived from a polymerizable monomer other than the conjugated diene compound, so long as it does not impede the object and effect of the present invention. In this case, the content of the structural unit derived from a polymerizable monomer other than the conjugated diene compound in the polymer block (b) is preferably less than 50 mol%, more preferably less than 30 mol%, even more preferably less than 20 mol%, still more preferably less than 10 mol%, and particularly preferably 0 mol%. Preferred examples of the other polymerizable monomer include aromatic vinyl compounds such as styrene, α-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, pt-butylstyrene, 2,4-dimethylstyrene, N-vinylcarbazole, vinylnaphthalene, and vinylanthracene, as well as at least one compound selected from the group consisting of methyl methacrylate, methyl vinyl ether, β-pinene, 8,9-p-menthene, dipentene, methylenenorbornene, 2-methylenetetrahydrofuran, 1,3-cyclopentadiene, 1,3-cyclohexadiene, 1,3-cycloheptadiene, and 1,3-cyclooctadiene.

[0058] The block copolymer may have at least one polymer block (b). When the block copolymer has two or more polymer blocks (b), the polymer blocks (b) may be the same or different.

[0059] [Weight average molecular weight] From the viewpoints of vibration damping properties, molding processability, and the like, the total weight average molecular weight of the polymer blocks (b) in the block copolymer before hydrogenation is preferably 15,000 to 800,000, more preferably 50,000 to 700,000, even more preferably 70,000 to 600,000, particularly preferably 90,000 to 500,000, and most preferably 130,000 to 450,000.

[0060] [Content of polymer block (b)] The content of the polymer block (b) in the block copolymer is preferably 70% by mass or more, more preferably 84% by mass or more, and particularly preferably 86% by mass or more. If the content of the polymer block (b) in the block copolymer is 70% by mass or more, the hydrogenated block copolymer can have appropriate flexibility and excellent vibration damping properties without decreasing the peak top intensity of tan δ. The upper limit is preferably 99% by mass or less, more preferably 97% by mass or less, and particularly preferably 94% by mass or less. If the content is 99% by mass or less, the hydrogenated block copolymer can have mechanical properties and moldability suitable for various applications. The content of the polymer block (b) in the block copolymer is 1 The value was determined by H-NMR measurement, and more specifically, the value was measured according to the method described in the Examples.

[0061] <<Method of manufacturing block copolymer>> As a method for producing a block copolymer, for example, one or more kinds of conjugated diene compounds are polymerized by an anionic polymerization method as monomers to form a polymer block (b) having a structural unit containing the alicyclic skeleton (X) in the main chain. Then, a monomer of the polymer block (a) is added, and if necessary, a monomer of the polymer block (a) and a conjugated diene compound are further added successively to obtain a block copolymer. The above-mentioned anionic polymerization method can be used to generate an alicyclic skeleton by known techniques (see, for example, U.S. Pat. No. 3,966,691). An alicyclic skeleton is formed at the end of a polymer due to the depletion of monomers, and polymerization can be started again from the alicyclic skeleton by successively adding monomers to the polymer. Therefore, the presence or absence of the generation of the alicyclic skeleton and its content can be controlled by the time of successive addition of monomers, the polymerization temperature, the type and amount of catalyst, the combination of monomer and catalyst, and the like. In addition, an anionic polymerization method can use an anionic polymerization initiator, a solvent, and, if necessary, a Lewis base.

[0062] In the above method, examples of organolithium compounds that can be used as polymerization initiators for anionic polymerization include methyllithium, ethyllithium, n-butyllithium, sec-butyllithium, tert-butyllithium, pentyllithium, etc. Examples of dilithium compounds that can be used as polymerization initiators include naphthalenedilithium, dilithiohexylbenzene, etc. Examples of the coupling agent include dichloromethane, dibromomethane, dichloroethane, dibromoethane, dibromobenzene, and phenyl benzoate. The amount of these polymerization initiators and coupling agents used is appropriately determined according to the desired weight average molecular weight of the block copolymer and its hydrogenated product. Usually, initiators such as alkyl lithium compounds and dilithium compounds are preferably used in a ratio of 0.01 to 0.2 parts by mass per 100 parts by mass of the total of the monomers of the polymer block (a) and the monomers such as conjugated diene compounds used in polymerization, and when a coupling agent is used, it is preferably used in a ratio of 0.001 to 0.8 parts by mass per 100 parts by mass of the total of the monomers.

[0063] The solvent is not particularly limited as long as it does not adversely affect the anionic polymerization reaction, and examples thereof include aliphatic hydrocarbons such as cyclohexane, methylcyclohexane, n-hexane, and n-pentane, and aromatic hydrocarbons such as benzene, toluene, and xylene. The polymerization reaction is usually carried out at a temperature of 0 to 100° C., preferably 10 to 70° C., for 0.5 to 50 hours, preferably 1 to 30 hours.

[0064] Furthermore, by adding a Lewis base as a co-catalyst during polymerization of the conjugated diene compound, the content of the alicyclic skeleton (X) and the contents of 3,4-bonds and 1,2-bonds in the polymer block (b) can be increased. Examples of Lewis bases include ethers such as dimethyl ether, diethyl ether, tetrahydrofuran, and 2,2-di(2-tetrahydrofuryl)propane (DTHFP); glycol ethers such as ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, and tetraethylene glycol dimethyl ether; amines such as triethylamine, N,N,N',N'-tetramethylenediamine, N,N,N',N'-tetramethylethylenediamine (TMEDA), and N-methylmorpholine; metal salts such as sodium or potassium salts of aliphatic alcohols such as sodium t-butylate, sodium t-amylate, or sodium isopentylate, or sodium or potassium salts of alicyclic alcohols such as dialkyl sodium cyclohexanolate, for example, sodium mentholate; and the like. These Lewis bases can be used alone or in combination of two or more.

[0065] The amount of Lewis base added is determined by the extent to which the content of the alicyclic skeleton (X) is controlled, and when the polymer block (b) contains a structural unit derived from isoprene and / or butadiene, the vinyl bond amount of the isoprene unit and / or butadiene unit constituting the polymer block (b) is controlled. Therefore, the amount of Lewis base added is not strictly limited, but is preferably used within the range of 0.1 to 1,000 mol, more preferably within the range of 1 to 100 mol, per gram atom of lithium contained in the alkyllithium compound or dilithium compound used as a polymerization initiator.

[0066] The average feed rate of the conjugated diene compound (hereinafter, sometimes referred to as "average diene feed rate") is not particularly limited, but from the viewpoint of increasing the content of the alicyclic skeleton (X), it is preferably 150 kg / h or less, more preferably 110 kg / h or less, particularly preferably 55 kg / h or less, and may be 45 kg / h or less, 30 kg / h or less, or may be 22 kg / h or less per mole of active terminal. The lower limit of the average feed rate of the conjugated diene compound is not particularly limited, but from the viewpoint of increasing productivity, it is preferably 1 kg / h or more, more preferably 3 kg / h or more, particularly preferably 5 kg / h or more, and may be 7 kg / h or more, 10 kg / h or more, or may be 15 kg / h or more per mole of active terminal.

[0067] After polymerization has been carried out by the above-mentioned method, an active hydrogen compound such as an alcohol, a carboxylic acid, or water is added to terminate the polymerization reaction, thereby obtaining a block copolymer.

[0068] <<Hydrogenation>> By subjecting the block copolymer obtained by the above-mentioned production method to a hydrogenation reaction (hydrogenation reaction), the carbon-carbon double bond derived from the conjugated diene compound in the polymer block (b) in the block copolymer is hydrogenated, and a hydrogenated product of the block copolymer can be obtained. The hydrogenation reaction (hydrogenation reaction) is carried out, for example, in an inert organic solvent in the presence of a hydrogenation catalyst. The hydrogenation reaction can be carried out under a hydrogen pressure of about 0.1 to 20 MPa, preferably 0.5 to 15 MPa, and more preferably 0.5 to 5 MPa, at a reaction temperature of about 20 to 250° C., preferably 50 to 180° C., and more preferably 70 to 180° C., for a reaction time of usually about 0.1 to 100 hours, and preferably 1 to 50 hours. Examples of the hydrogenation catalyst include Raney nickel; heterogeneous catalysts in which a metal such as Pt, Pd, Ru, Rh, or Ni is supported on a substrate such as carbon, alumina, or diatomaceous earth; Ziegler catalysts comprising a combination of a transition metal compound with an alkylaluminum compound, an alkyllithium compound, or the like; and metallocene catalysts.

[0069] The hydrogenated product thus obtained can be obtained by pouring the polymerization reaction liquid into methanol or the like to coagulate it, and then drying it under heating or reduced pressure, or by pouring the polymerization reaction liquid together with steam into hot water to remove the solvent by azeotropy (so-called steam stripping), and then drying it under heating or reduced pressure.

[0070] The hydrogenation rate of the polymer block (b) is not particularly limited, but is preferably 85 to 99 mol%, more preferably 87 to 98 mol%, and particularly preferably 88 to 97 mol%. The higher the hydrogenation rate of the polymer block (b), the more improved the heat resistance and weather resistance of the hydrogenated product can be. The hydrogenation rate is determined by measuring the content of carbon-carbon double bonds in the structural units derived from the conjugated diene compound and the alicyclic skeleton (X) in the polymer block (b) after hydrogenation. 1 The value was determined by H-NMR measurement, and more specifically, the value was measured according to the method described in the Examples.

[0071] <<Bonding Mode of Polymer Block (a) and Polymer Block (b) in Block Copolymer>> The block copolymer is not limited in the bonding form as long as the polymer block (a) and the polymer block (b) are bonded, and may be linear, branched, radial, or a combination of two or more of these. Among these, the bonding form between the polymer block (a) and the polymer block (b) is preferably linear, and examples thereof include a diblock copolymer represented by AB, a triblock copolymer represented by ABA or BAB, a tetrablock copolymer represented by ABAB, a pentablock copolymer represented by ABABA or BABAB, and an (AB)nZ type copolymer (Z represents a coupling agent residue, and n represents an integer of 3 or more), when the polymer block (a) is represented by A and the polymer block (b) is represented by B. Among these, a linear triblock copolymer or diblock copolymer is preferred, and an ABA type triblock copolymer is more preferred from the viewpoints of flexibility, ease of production, and the like. A specific example of the ABA triblock copolymer is a styrene-hydrogenated butadiene / isoprene-styrene copolymer. That is, the block copolymer preferably contains at least a styrene-hydrogenated butadiene / isoprene-styrene copolymer.

[0072] Here, in this specification, when the same type of polymer blocks are linearly bonded via a bifunctional coupling agent or the like, the entirety of the bonded polymer blocks is treated as one polymer block. Accordingly, including the above examples, polymer blocks that should strictly be expressed as YZY (Z represents a coupling residue) are expressed as Y as a whole, except when it is necessary to distinguish them from a single polymer block Y. In this specification, since this type of polymer block containing a coupling agent residue is treated as above, for example, a block copolymer containing a coupling agent residue and that should strictly be expressed as ABZBA (Z represents a coupling agent residue) is expressed as ABA and is treated as an example of a triblock copolymer.

[0073] <<Total content of polymer block (a) and polymer block (b) in block copolymer>> The block copolymer may contain a polymerization block composed of a monomer other than the polymerization blocks (a) and (b) as long as it does not impede the object and effect of the present invention, but the total content of the polymer blocks (a) and (b) is preferably 90% by mass or more, more preferably 95% by mass or more, and particularly preferably substantially 100% by mass. If it is 90% by mass or more, it is possible to obtain a hydrogenated block copolymer that is excellent in vibration damping property and moldability and is easy to suppress a decrease in adhesive strength even at high temperatures.

[0074] <<Content of hydrogenated aromatic vinyl compound elastomer (B)>> The content of the hydrogenated aromatic vinyl compound-based elastomer (B) in the thermoplastic elastomer composition is not particularly limited as long as it is 1% by mass or more and 99% by mass or less based on 100% by mass of the total amount of the thermoplastic elastomer composition, and can be appropriately adjusted depending on the type of the hydrogenated aromatic vinyl compound-based elastomer (B) and the use of the thermoplastic elastomer composition. The content of the hydrogenated aromatic vinyl compound-based elastomer (B) may be, for example, 90% by mass or less, 75% by mass or less, 60% by mass or less, or 50% by mass or less, or 10% by mass or more, 25% by mass or more, 40% by mass or more, or 50% by mass or more based on 100% by mass of the total amount of the thermoplastic elastomer composition.

[0075] <<Weight average molecular weight of hydrogenated aromatic vinyl compound elastomer (B)>> The weight average molecular weight (Mw) of the hydrogenated aromatic vinyl compound-based elastomer (B) determined by gel permeation chromatography in terms of standard polystyrene is not particularly limited, but is preferably 30,000 to 300,000, more preferably 50,000 to 250,000, and particularly preferably 100,000 to 200,000. If the weight average molecular weight of the hydrogenated aromatic vinyl compound-based elastomer (B) is 30,000 or more, the heat resistance is high, and if it is 300,000 or less, the moldability and processability are good.

[0076] <<Glass transition temperature Tg of hydrogenated aromatic vinyl compound elastomer (B)>> The glass transition temperature Tg of the hydrogenated aromatic vinyl compound-based elastomer (B) is not particularly limited as long as it is -10 to 40°C, but is preferably -7 to 35°C, more preferably -5 to 30°C, and particularly preferably -5 to 25°C. If the glass transition temperature Tg of the hydrogenated aromatic vinyl compound-based elastomer (B) is lower than -10°C or exceeds 40°C, the vibration damping property in the practical temperature range will be reduced. When the glass transition temperature Tg of the hydrogenated aromatic vinyl compound-based elastomer (B) is within the above preferred range, it can exhibit high vibration damping properties in the practical temperature range.

[0077] <<Storage modulus G' of hydrogenated aromatic vinyl compound elastomer (B)>> The ratio of the storage modulus G'(0°C) at 0°C to the storage modulus G'(50°C) at 50°C (G'(0°C) / G'(50°C)) of the hydrogenated aromatic vinyl compound-based elastomer (B) is not particularly limited, but is preferably greater than 10, more preferably 50 or more, and particularly preferably 100 or more. When the ratio of the storage modulus G'(0°C) at 0°C to the storage modulus G'(50°C) at 50°C (G'(0°C) / G'(50°C)) of the hydrogenated aromatic vinyl compound-based elastomer (B) is within the above range, high vibration damping properties can be exhibited.

[0078] <<Tan δ of hydrogenated aromatic vinyl compound elastomer (B)>> -Tan δ peak top intensity and peak top temperature- Tan δ (loss tangent) is the ratio of loss modulus / storage modulus at a frequency of 1 Hz in dynamic viscoelasticity measurement, and the peak top strength and peak top temperature of tan δ contribute greatly to vibration damping and other physical properties. Here, the peak top strength of tan δ refers to the value of tan δ when the peak of tan δ is maximum. Also, the peak top temperature of tan δ refers to the temperature when the peak of tan δ is maximum.

[0079] In this specification, the peak top strength and peak top temperature of tan δ of the hydrogenated aromatic vinyl compound elastomer (B) are measured by preparing a single layer sheet with a thickness of 1.0 mm by pressing the hydrogenated aromatic vinyl compound elastomer (B) at a temperature of 230°C and a pressure of 10 MPa for 3 minutes, cutting the single layer sheet into a disk shape, and measuring the test piece. The measurement conditions are in accordance with JIS K 7244-10 (2005), with a strain of 0.1%, a frequency of 1 Hz, a measurement temperature of -70 to 100°C, and a heating rate of 3°C / min. More specifically, the peak top intensity and peak top temperature of the hydrogenated aromatic vinyl compound-based elastomer (B) are values ​​measured according to the method described in the Examples.

[0080] The hydrogenated aromatic vinyl compound elastomer (B) preferably has a peak top intensity of tan δ of 1.0 or more as measured above. In some cases, it is 1.5 or more, or even 1.9 or more. The higher the peak top intensity of tan δ, the better the physical properties such as vibration damping at that temperature. If it is 1.0 or more, sufficient vibration damping can be obtained in the actual usage environment. The peak top temperature of tan δ of the hydrogenated aromatic vinyl compound-based elastomer (B) is not particularly limited, but is preferably -50°C or higher, more preferably -40°C or higher, even more preferably -30°C or higher, particularly preferably -25°C or higher, and may be 0°C or higher. The upper limit of the peak top temperature of tan δ may be within a range that does not impair the effects of the present invention, and may be 50°C or lower, 40°C or lower, or 35°C or lower. The range of the peak top temperature of tan δ of the hydrogenated aromatic vinyl compound-based elastomer (B) is not particularly limited, but is preferably -50 to 50°C, more preferably -40 to 40°C, even more preferably -30 to 30°C, and particularly preferably -25 to 25°C. If the peak top temperature of tan δ is -50°C or higher, sufficient vibration damping properties can be obtained under practical use conditions, and if it is 50°C or lower, desirable adhesion can be exhibited when used in an adhesive layer.

[0081] [Maximum width of temperature range where tan δ is 1.0 or more] The hydrogenated aromatic vinyl compound-based elastomer (B) has a temperature range in which tan δ measured under the above-mentioned measurement conditions is 1.0 or more at −70 to 100° C. There is no particular limitation on the maximum width of the temperature range, but it is preferably 12° C. or more, more preferably 13° C. or more, even more preferably 15° C. or more, and particularly preferably 17° C. or more. When the alicyclic skeleton (X) is incorporated in the main chain in the structural unit of the polymer block (b), it can have a higher vinyl bond content, and the molecular motion is reduced, so the glass transition temperature rises and the glass transition becomes gentler with respect to temperature changes. This broadens the temperature range in which the hydrogenated product of the block copolymer (hydrogenated aromatic vinyl compound-based elastomer (B)) exhibits tan δ of 1 or more, making it possible to exhibit vibration damping properties over a wide temperature range. If the maximum width of the temperature range in which tan δ is 1.0 or more is 12°C or more, or even 13°C or more, it is possible to obtain better vibration damping properties in the actual usage environment.

[0082] -Maximum value of tan δ intensity of hydrogenated aromatic vinyl compound elastomer (B) at 0 to 40°C- The maximum value of the tan δ strength of the hydrogenated aromatic vinyl compound elastomer (B) at 0 to 40° C. is not particularly limited, but is preferably 1.0 or more, more preferably 1.5 or more, and particularly preferably 2.0 or more. When the maximum value of the tan δ strength of the hydrogenated aromatic vinyl compound-based elastomer (B) is within the above range, the vibration damping property can be further improved. The maximum value of the tan δ strength of the hydrogenated aromatic vinyl compound-based elastomer (B) is a value measured according to the measurement method described in the Examples. In addition, when the thermoplastic elastomer composition contains multiple types of hydrogenated aromatic vinyl compound-based elastomers (B), the maximum value of the tan δ strength of the thermoplastic elastomer composition consisting only of multiple hydrogenated aromatic vinyl compound-based elastomers (B) is defined as the maximum value of the tan δ strength of the hydrogenated aromatic vinyl compound-based elastomer (B) at 0 to 40°C. For example, as shown in Reference Example 1 described later, when the thermoplastic elastomer composition contains 50 parts by mass of B-1 and 50 parts by mass of B-3, the maximum value of tan δ strength of the hydrogenated aromatic vinyl compound-based elastomer (B) at 0 to 40°C is 1.03.

[0083] <<Total content of polyester-based thermoplastic elastomer (A) and hydrogenated aromatic vinyl compound-based elastomer (B)>> In the thermoplastic elastomer composition of the present invention, additives other than the polyester thermoplastic elastomer (A) and the hydrogenated aromatic vinyl compound elastomer (B) may be contained as described below, as long as they do not interfere with the objects and effects of the present invention, but the total content of the polyester thermoplastic elastomer (A) and the hydrogenated aromatic vinyl compound elastomer (B) is preferably 90% by mass or more, more preferably 95% by mass or more, and particularly preferably substantially 100% by mass. If it is 90% by mass or more, it is possible to obtain a thermoplastic elastomer composition that can improve vibration damping while maintaining the characteristics of the polyester thermoplastic elastomer.

[0084] <Additives> Optional additives include, for example, compatibilizers, other resins, other components, and the like.

[0085] <<Content>> When the thermoplastic elastomer composition contains the above-mentioned additives, the content of the additives is not particularly limited and can be appropriately adjusted depending on the type of additive and the use of the thermoplastic elastomer composition, and may be, for example, 50 mass% or less, 45 mass% or less, 30 mass% or less, 20 mass% or less, 10 mass% or less, or may be 0.01 mass% or more, 0.1 mass% or more, 1 mass% or more, 5 mass% or more, relative to the total amount (100 mass%) of the thermoplastic elastomer composition.

[0086] <<Compatibilizer>> The compatibilizer has the effect of compatibilizing the polyester-based thermoplastic elastomer (A) and the hydrogenated aromatic vinyl compound-based elastomer (B). This compatibilizing effect is obtained, for example, by the reaction of a terminal functional group of the polyester-based thermoplastic elastomer (A) with a terminal functional group of the hydrogenated aromatic vinyl compound-based elastomer (B) with a functional group (e.g., an epoxy group) in the compatibilizer.

[0087] Suitable examples of the compatibilizer include epoxy group-containing resins such as epoxy group-containing ethylene copolymers and epoxidized diene polymers. When an epoxy group-containing resin is used as a compatibilizer, a polar resin can be easily dispersed in a polyester thermoplastic elastomer (A) with a small amount of use compared to other compatibilizers. When a compatibilizer other than an epoxy group-containing resin is used, the amount of use tends to be large, but the compatibilizer can be easily uniformly dispersed in the resin composition, and the feed amount can be easily stabilized when performing continuous production such as extrusion molding.

[0088] [Epoxy Group-Containing Ethylene-Based Copolymer] The epoxy group-containing ethylene copolymer is a copolymer containing structural units derived from ethylene and structural units derived from glycidyl methacrylate. The content of structural units derived from glycidyl methacrylate in this epoxy group-containing ethylene copolymer is not particularly limited, but from the viewpoint of compatibilization effect, when the mass of the copolymer is 100 mass%, it is preferably 3 to 30 mass%, more preferably 5 to 25 mass%, and particularly preferably 10 to 20 mass%. The content of structural units derived from glycidyl methacrylate is measured by infrared spectroscopy.

[0089] The epoxy group-containing ethylene-based copolymer may be an epoxy group-containing ethylene-based copolymer consisting only of structural units derived from ethylene and structural units derived from glycidyl methacrylate, or may be an epoxy group-containing ethylene-based copolymer further containing structural units derived from ethylene, structural units derived from glycidyl methacrylate, and structural units derived from one or more compounds selected from the group consisting of compounds represented by the following formula (1) and compounds represented by the following formula (2). CH2=CR 4 R 5 (1) CHR 6 =CHR 7 (2) During the ceremony, R 4 represents a hydrogen atom or an alkyl group having 1 to 8 carbon atoms, R 5 is a halogen atom or -COOR 8 A group represented by R 8 represents an alkyl group having 1 to 8 carbon atoms; R 6 is a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, or -COOR 9 A group represented by R 9 represents an alkyl group having 1 to 8 carbon atoms; R 7 is an alkylnitrile having 1 to 8 carbon atoms, an alkyl ether group, an alkylamide, a halogen atom, a phenyl group, or -COOR 10A group represented by R 10 represents an alkyl group having 1 to 8 carbon atoms, or R 7 Ha-OCOR 11 A group represented by R 11 represents an alkyl group having 1 to 8 carbon atoms. Examples of the compound represented by formula (1) include propylene, 1-butene, vinyl acetate, acrylic acid, methacrylic acid, methyl acrylate, ethyl acrylate, methyl methacrylate, ethyl methacrylate, vinyl chloride, vinylidene chloride, styrene, acrylonitrile, isobutyl vinyl ether, and acrylamide. These may be used alone or in combination of two or more. Among these, vinyl acetate, methyl acrylate, and methyl methacrylate are preferred. Examples of the compound represented by formula (2) include dimethyl maleate, diethyl maleate, dimethyl fumarate, and diethyl fumarate. When the epoxy group-containing ethylene copolymer is composed of a structural unit derived from ethylene, a structural unit derived from glycidyl methacrylate, and a structural unit derived from a compound represented by formula (1) or formula (2), the content of the monomer unit derived from the compound represented by formula (1) or formula (2) is not particularly limited, but is preferably 40% by mass or less, more preferably 30% by mass or less, when the mass of the copolymer is 100% by mass. In the above case, the content of the monomer unit derived from glycidyl methacrylate is not particularly limited, but is preferably 2-20% by mass, more preferably 3-10% by mass, and particularly preferably 5-7% by mass, when the mass of the copolymer is 100% by mass.

[0090] Examples of epoxy group-containing ethylene copolymers include ethylene-glycidyl methacrylate copolymers, ethylene-propylene-glycidyl methacrylate copolymers, ethylene-butene-1-glycidyl methacrylate copolymers, ethylene-vinyl acetate-glycidyl methacrylate copolymers, ethylene-acrylic acid-glycidyl methacrylate copolymers, ethylene-methacrylic acid-glycidyl methacrylate copolymers, ethylene-methyl acrylate-glycidyl methacrylate copolymers, ethylene-ethyl acrylate-glycidyl methacrylate copolymers, ethylene-methyl methacrylate-glycidyl methacrylate copolymers, ethylene-ethyl methacrylate-glycidyl methacrylate copolymers, Examples of such copolymers include ethylene-methyl maleate-glycidyl methacrylate copolymer, ethylene-ethyl maleate-glycidyl methacrylate copolymer, ethylene-methyl fumarate-glycidyl methacrylate copolymer, ethylene-ethyl fumarate-glycidyl methacrylate copolymer, ethylene-vinyl chloride-glycidyl methacrylate copolymer, ethylene-vinylidene chloride-glycidyl methacrylate copolymer, ethylene-styrene-glycidyl methacrylate copolymer, ethylene-acrylonitrile-glycidyl methacrylate copolymer, ethylene-isobutyl vinyl ether-glycidyl methacrylate copolymer, ethylene-acrylamide-glycidyl methacrylate copolymer, etc. These may be used alone or in combination of two or more. Among these, ethylene-glycidyl methacrylate copolymers (e.g., Bondfast BF-E, manufactured by Sumitomo Chemical Co., Ltd., ethylene units: 88 mass%, glycidyl methacrylate units: 12 mass%) and ethylene-methyl acrylate-glycidyl methacrylate copolymers (e.g., Bondfast BF-7M, manufactured by Sumitomo Chemical Co., Ltd., ethylene units: 67 mass%, glycidyl methacrylate units: 6 mass%, methyl acrylate units: 27 mass%) are preferred.

[0091] The epoxy group-containing ethylene copolymer can be synthesized by various methods, such as bulk polymerization, emulsion polymerization, and solution polymerization using a free radical initiator. Representative polymerization methods include those described in JP-A-48-11388 and JP-A-61-127709, and those using a polymerization initiator that generates free radicals and is heated at a pressure of 500 kg / cm 2 As described above, the copolymerization can be carried out at a temperature of 40 to 300°C.

[0092] Other examples include a method in which an unsaturated epoxy compound and a radical generator are mixed with a polymer containing a structural unit derived from ethylene and, optionally, a structural unit derived from a compound represented by formula (1) or formula (2), and melt-graft copolymerized in an extruder; and a method in which ethylene, an unsaturated epoxy compound, and, optionally, a compound represented by formula (1) or formula (2) are copolymerized in an inert medium such as water or an organic solvent in the presence of a radical generator.

[0093] [Epoxidized Diene Polymer] The epoxidized diene polymer is a polymer in which an epoxy group is introduced into the molecule by epoxidizing the diene polymer with an epoxidizing agent. Examples of the diene polymer used in the epoxidized diene polymer include butadiene polymer, styrene-butadiene copolymer, isoprene polymer, styrene-isoprene copolymer, and acrylonitrile-butadiene copolymer. These may be used alone or in combination of two or more. Among these, the epoxidized styrene-butadiene block copolymer using the styrene-butadiene copolymer is particularly preferred from the viewpoint of improving compatibility. Examples of the epoxidized styrene-butadiene block copolymer include epoxidized styrene-butadiene block copolymers represented by the following general formula (3) or (4).

[0094] [ka]

[0095] Commercially available epoxidized styrene-butadiene block copolymers include Epofriend AT501 and Epofriend CT310 manufactured by Daicel Corporation.

[0096] [Amount of Compatibilizer Added] The amount of the compatibilizer to be added is not particularly limited, but is preferably 0.1 to 20 parts by mass, more preferably 0.5 to 10 parts by mass, and particularly preferably 1 to 5 parts by mass, per 100 parts by mass of the total of the polyester-based thermoplastic elastomer (A) and the hydrogenated aromatic vinyl compound-based elastomer (B).

[0097] <<Other resins>> Examples of other resins include olefin resins; polyisoprene; polybutadiene; ethylene-propylene-diene copolymer vulcanizates; styrene-butadiene rubber; styrene-isoprene rubber; nitrile rubber, butyl rubber; natural rubber; ethylene-vinyl acetate copolymers; ethylene-(meth)acrylate copolymers; ethylene-ethyl(meth)acrylate copolymers; ethylene-(meth)acrylic acid copolymers and other metal ion crosslinked resins (ionomers); styrene-based resins such as polystyrene, AS resin, and ABS resin; polyphenylene ether-based resins; polyamide resins such as nylon 6 and nylon 66; polyester-based resins such as polyethylene terephthalate and polybutylene terephthalate; polyurethane-based resins; acetal-based resins such as polyoxymethylene homopolymers and polyoxymethylene copolymers; acrylic resins such as polymethyl methacrylate-based resins; polyvinyl chloride; vinyl chloride-vinyl acetate copolymers; ethylene-vinyl chloride-vinyl acetate copolymers; and the like.

[0098] <<Other Ingredients>> Examples of other components include crosslinking agents (isocyanate-based crosslinking agents, epoxy-based crosslinking agents, metal chelate-based crosslinking agents, aziridine-based crosslinking agents, amine resins, etc.), heat stabilizers, light stabilizers, ultraviolet absorbers, infrared absorbers, antioxidants, lubricants, colorants, antistatic agents, flame retardants, water repellents, waterproofing agents, hydrophilicity-imparting agents, electrical conductivity-imparting agents, thermal conductivity-imparting agents, electromagnetic wave shielding agents, light transmittance adjusting agents, fluorescent agents, sliding properties-imparting agents, transparency-imparting agents, antiblocking agents, metal deactivators, antibacterial agents, crystal nucleating agents, crack prevention agents, ozone deterioration inhibitors, rodent repellents, dispersants, thickeners, light resistance agents, weather resistance agents, copper damage inhibitors, reinforcing agents, antifungal agents, macrocyclic molecules (cyclodextrin, calixarene, cucurbituril, etc.), and adhesives other than the tackifying resins (acrylic adhesives, etc.). One or more of these may be used.

[0099] <Tan δ strength of thermoplastic elastomer composition> The maximum value of the tan δ strength of the thermoplastic elastomer composition of the present invention is not particularly limited, and is preferably 0.1 or more, more preferably 0.13 or more, and particularly preferably 0.15 or more at 0 to 40°C. If the tan δ strength of the thermoplastic elastomer composition is within the above range, the vibration damping property can be further improved. More specifically, the tan δ intensity is a value measured according to the method described in the Examples.

[0100] The ratio of the maximum tan δ strength of the hydrogenated aromatic vinyl compound-based elastomer (B) at 0 to 40°C to the maximum tan δ strength of the polyester-based thermoplastic elastomer (A) at 0 to 40°C (tan δ(B)max / tan δ(A)max) is not particularly limited, but is preferably 10 to 80, more preferably 12 to 40, and particularly preferably 14 to 35. When the ratio (tan δ(B)max / tan δ(A)max) is within the above range, the vibration damping property of the thermoplastic elastomer composition can be further improved.

[0101] (vibration damping material) The vibration damping material of the present invention is characterized by comprising the thermoplastic elastomer composition of the present invention. It should be noted that vibration-damping materials are used to prevent vibration and noise in various structures and maintain quietness. For example, they are widely used not only under the floors of automobile interiors, but also in railway vehicles, ships, aircraft, electrical equipment, building structures, construction equipment, and the like.

[0102] <Content> The content of the thermoplastic elastomer composition in the vibration-damping material is not particularly limited, but from the viewpoint of performance as a vibration-damping material, it is preferably 10% by mass or more, more preferably 30% by mass or more, and particularly preferably 50% by mass or more. The upper limit of the content of the thermoplastic elastomer composition in the vibration-damping material is not particularly limited within a range that does not impair the effects of the present invention, and may be 100% by mass, but from the viewpoint of economic efficiency, it is preferably 90% by mass or less, more preferably 80% by mass or less, and particularly preferably 70% by mass or less.

[0103] (Gear) The gear of the present invention is characterized by comprising the thermoplastic elastomer composition of the present invention. The type of gear of the present invention is not particularly limited, and examples thereof include noiseless gears, headlamp actuator gears, and HVAC gears.

[0104] <Content> The content of the thermoplastic elastomer composition in the gear is not particularly limited, but from the viewpoint of the performance of the gear, it is preferably 10% by mass or more, more preferably 30% by mass or more, and particularly preferably 50% by mass or more. The upper limit of the content of the thermoplastic elastomer composition in the gear is not particularly limited within a range that does not impair the effects of the present invention, and may be 100% by mass, but from the viewpoint of economy, it is preferably 90% by mass or less, more preferably 80% by mass or less, and particularly preferably 70% by mass or less.

[0105] (composite molded body) The composite molded product of the present invention is characterized in that a thermoplastic elastomer composition layer containing a thermoplastic elastomer composition is fused to a polar resin layer containing a polar resin.

[0106] <Thermoplastic elastomer composition layer> The thermoplastic elastomer composition layer is a layer containing the thermoplastic elastomer composition of the present invention. The content of the thermoplastic elastomer composition in the thermoplastic elastomer composition layer is not particularly limited, but from the viewpoint of the performance of the thermoplastic elastomer composition layer, it is preferably 50% by mass or more, more preferably 70% by mass or more, and particularly preferably 75% by mass or more. The upper limit of the content of the thermoplastic elastomer composition in the thermoplastic elastomer composition layer is not particularly limited within a range that does not impair the effects of the present invention, and may be 100% by mass, but from the viewpoint of economy, it is preferably 90% by mass or less, more preferably 85% by mass or less, and particularly preferably 80% by mass or less.

[0107] <Polar resin layer> The polar resin layer is a layer containing a polar resin. The content of the polar resin in the polar resin layer is not particularly limited, but from the viewpoint of performance as a polar resin layer, it is preferably 50% by mass or more, more preferably 70% by mass or more, and particularly preferably 80% by mass or more.

[0108] <<Polar resin>> Polar resins refer to, for example, (i) resins having polar groups such as carboxy groups, sulfonic acid groups, hydroxyl groups, and cyano groups; (ii) resins having ether bonds, ester bonds, amide bonds, sulfide bonds, and the like in the resin; and (iii) resins containing at least one of oxygen, nitrogen, sulfur, and halogen in the molecule, and are resins in which electronic polarization occurs within the molecule and which have thermoplastic properties. Specific examples of polar resins include polyamide resins such as nylon 6, nylon 66, nylon 610, nylon 9, nylon 6 / 66, nylon 66 / 610, nylon 6 / 11, nylon 6 / 12, nylon 12, nylon 46, and amorphous nylon; polyester resins such as polyethylene terephthalate, polyethylene naphthalate, and polybutylene terephthalate; polyacetal resins such as polyoxymethylene homopolymers and polyoxymethylene copolymers; polyphenylene sulfide resins, polyurethane resins, polyvinyl alcohol resins, polycarbonate resins, ethylene-vinyl acetate copolymers, ethylene-methacrylic acid copolymers, polyether ketones, polyether ether ketones, polyvinyl chloride, polyvinylidene chloride, polyacrylonitrile, vinylon, triacetyl cellulose, ABS resins, AS resins, ACS resins, xylene resins, and acrylic resins. These polar resins may be used alone or in combination of two or more. Among these, polyamide resins, polyester resins, polyacetal resins, polyphenylene sulfide resins, polyurethane resins, polyvinyl alcohol resins, and polycarbonate resins are preferable. At least one of the glass transition temperature and the melting point of the polar resin is preferably 80° C. or higher, more preferably 100° C. or higher, and particularly preferably 150° C. or higher. Here, the melting point is measured with a DSC measuring device. When at least one of the glass transition temperature and the melting point is within the above range, the mechanical properties of the polar resin become good.

[0109] <Method of manufacturing composite molded body> As a method for producing a composite molded body, various molding methods can be used, such as insert injection molding, two-color injection molding, T-die laminate molding, co-extrusion molding, blow molding, core-back injection molding, sandwich injection molding, and injection press molding.

[0110] <<Insert injection molding method>> The insert injection molding method is a molding method in which a core material (polar resin) is molded in advance by injection molding, extrusion molding, sheet molding, film molding, etc., the shaped molded product is inserted into a mold, and then a surface material (thermoplastic elastomer composition) is injection molded into the gap between the molded product and the mold; alternatively, a thermoplastic elastomer composition is molded in advance by injection molding, extrusion molding, sheet molding, film molding, etc., the shaped molded product is inserted into a mold, and then a polar resin is injection molded into the gap between the molded product and the mold.

[0111] <<Two-color injection molding method, core-back injection molding method>> The two-color injection molding method is a molding method in which a polar resin is injection-molded using two or more injection molding machines, the molds are rotated or moved to exchange the mold cavities, a gap is formed between the molded product and the mold, and a thermoplastic elastomer composition is injection-molded into the gap. The core-back injection molding method is a molding method in which a polar resin is injection-molded using one injection molding machine and one mold, the mold cavity volume is expanded, and a thermoplastic elastomer composition is injection-molded into the gap between the molded product and the mold.

[0112] The polar resin may be molded by a normal injection molding method or by gas injection molding. The injection molding temperature for the polar resin is not particularly limited, but is preferably from 100 to 300°C, and more preferably from 150 to 280°C. There is no particular restriction on the injection molding pressure for polar resins, but it is generally between 50 and 1,000 kg / cm 2 is preferably 100 to 800 kg / cm 2 It is more preferable that:

[0113] The average thickness of the polar resin layer in this injection molded article is not particularly limited, but is preferably 0.5 to 6 mm. By being in the above range, it is possible to prevent the occurrence of sink marks in the polar resin layer and improve the smoothness of the molded article surface, and also to satisfy the mechanical properties such as rigidity and strength, heat resistance, and durability required for use in, for example, automotive interior parts. The average thickness of the thermoplastic elastomer composition layer is not particularly limited, but is preferably 1 to 5 mm. By keeping it within the above range, the soft feel can be improved and the adhesion between the polar resin and the thermoplastic elastomer composition can be improved.

[0114] The injection molding temperature for the thermoplastic elastomer composition layer is not particularly limited, but is preferably from 150 to 300°C, more preferably from 200 to 290°C, and particularly preferably from 220 to 280°C. The injection molding pressure for the thermoplastic elastomer composition layer is not particularly limited, but is preferably 50 to 1,000 kg / cm. 2 is preferably 100 to 800 kg / cm 2 It is more preferable that:

[0115] The composite molded article thus obtained can be used as various industrial parts. Specifically, it can be used for automobile interior parts such as instrument panels, center panels, center console boxes, door trims, pillars, assist grips, handles, and airbag covers, automobile exterior parts such as moldings, automobile functional parts such as rack and pinion boots, suspension boots, and constant velocity joint boots, home appliance parts such as vacuum cleaner bumpers, remote control switches, and various key tops of office automation equipment, underwater products such as underwater goggles and underwater camera covers, various cover parts, industrial parts with various packings for the purpose of sealing, waterproofing, soundproofing, vibration prevention, and the like, electrical and electronic parts such as curl cord electric wire coatings, belts, hoses, tubes, and soundproofing gears, and sports goods, etc. EXAMPLES

[0116] Hereinafter, the present invention will be specifically described with reference to Examples and Comparative Examples, but the present invention is not limited thereto.

[0117] <Hydrogenated aromatic vinyl compound-based elastomer (B)> The method for evaluating the physical properties of the hydrogenated aromatic vinyl compound-based elastomer (B) obtained in the production examples described below is shown below. (1) Content of polymer block (a) The block copolymer before hydrogenation was dissolved in CDCl3 1 1H-NMR measurement [apparatus: "ADVANCE 400 Nano bay" (manufactured by Bruker), measurement temperature: 30 ° C] was performed, and the content of the polymer block (a) was calculated from the ratio of the peak intensity derived from styrene as an aromatic vinyl compound to the peak intensity derived from diene.

[0118] (2) Weight-average molecular weight (Mw) The weight-average molecular weight (Mw) in terms of polystyrene of the hydrogenated aromatic vinyl compound-based elastomer (B) was determined by gel permeation chromatography (GPC) measurement under the following conditions. <<GPC measurement apparatus and measurement conditions>> · Apparatus: GPC apparatus "HLC-8020" (manufactured by Tosoh Corporation) · Separation column: "TSKgel GMHXL", "G4000HXL" and "G5000HXL" manufactured by Tosoh Corporation were connected in series. · Eluent: Tetrahydrofuran · Eluent flow rate: 0.7 mL / min · Sample concentration: 5 mg / 10 mL · Column temperature: 40 ° C · Detector: Differential refractive index (RI) detector · Calibration curve: Prepared using standard polystyrene

[0119] (3) Hydrogenation rate in polymer block (b) 1It was calculated from the ratio of the peak area derived from the residual olefins of isoprene and / or butadiene to the peak area derived from ethylene, propylene and / or butylene by H-NMR measurement. Equipment: Nuclear magnetic resonance equipment "ADVANCE 400 Nano bay" (Bruker) Solvent: CDCl3

[0120] (4) Amount of vinyl bonds in polymer block (b) The block copolymer before hydrogenation was dissolved in CDCl3. 1 H-NMR measurement was performed [apparatus: "ADVANCE 400 Nano bay" (manufactured by Bruker), measurement temperature: 30°C]. The vinyl bond amount (total content of 3,4-bond units and 1,2-bond units) was calculated from the ratio of the total peak area of ​​structural units derived from isoprene and / or butadiene to the peak area corresponding to the 3,4-bond units and 1,2-bond units in the isoprene structural unit, the 1,2-bond units in the butadiene structural unit, or, in the case of structural units derived from a mixture of isoprene and butadiene, the vinyl bond amount (total content of 3,4-bond units and 1,2-bond units) was calculated from the ratio of the peak area corresponding to each of the above bond units.

[0121] (5) Content of alicyclic skeleton (X) in polymer block (b) 600 mg of block copolymer before hydrogenation and 340 mg of Cr(acac) were dissolved in 34 mL of CDCl and quantitatively analyzed using a 10 mm NMR tube. 13 C-NMR measurement (pulse program: zgig, inverse gated 1H decoupling method) [apparatus: "ADVANCE 400 Nano bay" (Bruker), measurement temperature: 30°C] was performed using the following method. Polymer block (b) The contents of the alicyclic skeletons X, X1, and X2 in the polymer were calculated. In addition, Table 1-1, Table 1-2, and In Table 3, X, X1, and X2 represent the following alicyclic skeletons. X: an alicyclic skeleton having a combination of the following substituents (i) to (vi): X1: an alicyclic skeleton having a combination of the following substituents (i) and (iv): X2: Below (ii), (iii), (v), (vi)An alicyclic skeleton having a combination of the following substituents: (i):R 1 = hydrogen atom, R 2 = hydrogen atom, R 3 = Hydrogen atom; (1,2Bd+Bd) (ii):R 1 = hydrogen atom, R 2 = methyl group, R 3 = Hydrogen atom; (1,2Bd+1,2Ip) (iii):R 1 = hydrogen atom, R 2 = hydrogen atom, R 3 = Methyl group; (1,2Bd + 3,4Ip) (iv):R 1 = methyl group, R 2 = hydrogen atom, R 3 = Hydrogen atom; (1,2Ip+Bd) (v):R 1 = methyl group, R 2 = methyl group, R 3 = Hydrogen atom; (1,2Ip+1,2Ip) (vi):R 1 = methyl group, R 2 = hydrogen atom, R 3 = Methyl group; (1,2Ip + 3,4Ip)

[0122] [Calculation method] Table 1-1 shows each peak and the structure it is derived from. If the integral values ​​of each peak are a to g, the integral values ​​of each structure are as shown in Table 1-2, and the contents of X, X1, and X2 can be calculated as (a+gc) / (a+b+c-d+e / 2+2f), (gc) / (a+b+c-d+e / 2+2f), and a / (a+b+c-d+e / 2+2f), respectively.

[0123] [Table 1]

[0124] (6) Glass transition temperature Tg (℃) For the hydrogenated aromatic vinyl compound-based elastomers (B) of Production Examples 1 to 3, the glass transition temperature Tg was measured by the following method. [Glass transition temperature (Tg) measurement] The measurement was performed in accordance with JIS K7121:2012. A differential scanning calorimetry (DSC) device (DSC250 manufactured by TA) was used for the measurement. The measurement conditions for the DSC curve were as follows: the sample was heated once to 230°C, then cooled to -90°C, and then heated from -90°C to 230°C at a rate of 10°C / min. The midpoint glass transition temperature was determined from the DSC curve measured during the second heating, and the midpoint glass transition temperature was taken as the glass transition temperature (Tg).

[0125] (7) Peak top temperature of tan δ, peak top intensity, and maximum width of the temperature range where tan δ is 1.0 or more For the following measurements, a single-layer sheet having a thickness of 1.0 mm was prepared by pressing the hydrogenated aromatic vinyl compound-based elastomer (B) at a temperature of 230° C. and a pressure of 10 MPa for 3 minutes. The single-layer sheet was cut into a disk shape to be used as a test sheet. For the measurements, a distortion-controlled dynamic viscoelasticity device "ARES-G2" (manufactured by TA Instruments Japan) with a disk diameter of 8 mm was used as a parallel plate oscillatory rheometer based on JIS K 7244-10 (2005). The gap between the two flat plates was completely filled with the test sheet, and the test sheet was subjected to vibration at a frequency of 1 Hz with a distortion of 0.1%, and the temperature was raised from -70°C to 100°C at a constant rate of 3°C / min to determine the maximum value of the peak strength of tan δ (peak top strength) and the temperature (°C) at which the maximum value was obtained (peak top temperature (°C)). In addition, the maximum value of the tan δ strength of the hydrogenated aromatic vinyl compound-based elastomer (B) at 0 to 40°C was determined. Furthermore, the maximum width (°C) of the temperature region where tan δ was 1.0 or more was determined. The larger this value, the better the vibration damping property. (8) G' ratio of hydrogenated aromatic vinyl compound elastomer (B) (G'(0℃) / G'(50℃)) The G' ratio (G'(0℃) / G'(50℃)) of the hydrogenated aromatic vinyl compound elastomer (B) in Production Examples 1 to 3 was measured using a test sheet cut into a disk shape from a single layer sheet having a thickness of 1.0 mm, which was prepared by pressing the hydrogenated aromatic vinyl compound elastomer (B) at a temperature of 230℃ and a pressure of 10 MPa for 3 minutes, according to JIS K 7244-10 (2005), using a distortion-controlled dynamic viscoelasticity device "ARES-G2" (manufactured by TA Instruments Japan) with a disk diameter of 8 mm as a parallel plate vibration rheometer.

[0126] [Production Example 1] Production of hydrogenated aromatic vinyl compound elastomer (B) A nitrogen-purged, dried pressure vessel was charged with 50 kg of cyclohexane as a solvent and 87 g of a 10.5 mass % cyclohexane solution of sec-butyllithium as an anionic polymerization initiator (effective amount of sec-butyllithium added: 9.1 g). After the temperature inside the pressure vessel was raised to 50°C, 1.0 kg of styrene (1) was added and polymerized for 1 hour. At a vessel temperature of 50°C, 63 g of 2,2-di(2-tetrahydrofuryl)propane (DTHFP) was added as a Lewis base, and a mixed solution of 8.16 kg of isoprene and 6.48 kg of butadiene was added over 5 hours at the average diene feed rate shown in Table 2, followed by polymerization for 2 hours. Further, 1.0 kg of styrene (2) was added and polymerized for 1 hour, thereby obtaining a reaction liquid containing a polystyrene-poly(isoprene / butadiene)-polystyrene triblock copolymer. A Ziegler-based hydrogenation catalyst formed from nickel octylate and trimethylaluminum was added to the reaction liquid under a hydrogen atmosphere, and the reaction was carried out for 5 hours under conditions of a hydrogen pressure of 1 MPa and 80° C. After the reaction liquid was allowed to cool and the pressure was released, the catalyst was removed by washing with water, and the reaction liquid was dried in a vacuum to obtain a hydrogenated product of polystyrene-poly(isoprene / butadiene)-polystyrene triblock copolymer (hydrogenated aromatic vinyl compound-based elastomer (B)). Each raw material and its amount (kg) used are shown in Table 2. The results of the physical property evaluation are shown in Table 3.

[0127] [Manufacturing Examples 2-3] Production of hydrogenated aromatic vinyl compound elastomer (B) A hydrogenated block copolymer (hydrogenated aromatic vinyl compound-based elastomer (B)) was produced in the same manner as in Production Example 1, except that the components and their amounts used, and the reaction conditions were changed as shown in Table 2. The results of the physical property evaluation are shown in Table 3.

[0128] [Table 2]

[0129] [Table 3]

[0130] [Examples 1 to 10, Comparative Examples 1 and 2, and Reference Examples] The hydrogenated aromatic vinyl compound-based elastomers (B) of Production Examples 1 and 2 exhibit a peak top intensity of tan δ of 1.0 or more and a peak top temperature of tan δ over a wide temperature range, and therefore can be said to be suitable for a wide range of applications as vibration damping materials.

[0131] The thermoplastic elastomer compositions shown in Tables 4 and 5 (parts by mass) were added to a Brabender (Brabender's "Plastograph EC: 50cc mixer") and melt-kneaded for 3 minutes at a cylinder temperature of 240°C and a screw rotation speed of 100 rpm. The resulting compositions were then press-molded (240°C, 2 minutes) to produce sheets (thickness 1 mm). The tan δ strength of the sheets (thickness 1 mm) produced above was measured by the following method. The dispersion diameter (μm) of the test pieces used to measure the tan δ strength was also measured by the following method.

[0132] [Dispersion diameter measurement] The above test piece used for measuring tan δ was freeze-fractured using liquid nitrogen, the cross section was etched with xylene, and then platinum was evaporated to prepare a sample, which was then observed with a SEM. In the obtained image, the average diameter of 50 pores removed by etching was taken as the volume average dispersion diameter. The results are shown in Table 5.

[0133] [Tan δ strength measurement (shear, 1Hz)] The measurement was carried out according to JIS K 7244-10 (2005). Specifically, the obtained sheet was cut into a diameter of 8 mm and used as a sample. Using a strain-controlled dynamic viscoelasticity device "ARES-G2" (manufactured by TA Instruments Japan), vibration was applied at a frequency of 1 Hz with a strain of 0.1%, and the temperature was raised from -70°C to 100°C at a constant rate of 3°C / min to measure the tan δ strength of the sheet at 0°C, 10°C, 20°C, 30°C, and 40°C, and the maximum value of the tan δ strength from 0°C to 40°C was obtained. The higher the tan δ strength, the better the vibration damping properties. The results are shown in Tables 4 and 5.

[0134] [Table 4] [Table 5]

[0135] The components shown in Tables 4 and 5 are as follows. A-1: Hytrel 3046 manufactured by Toray DuPont Co., Ltd. (polyester-based thermoplastic elastomer (A): TPEE) The maximum value of tan δ intensity of A-1 at 0 to 40° C. was measured in the same manner as in the hydrogenated aromatic vinyl compound-based elastomer (B) and was found to be 0.07. B-1: Hydrogenated aromatic vinyl compound-based elastomer (B) prepared according to Production Example 1 B-2: Hydrogenated aromatic vinyl compound elastomer (B) prepared according to Production Example 2 B-3: Hydrogenated aromatic vinyl compound elastomer (B) prepared according to Production Example 3 C-1: Compatibilizer: Ethylene-glycidyl methacrylate copolymer Bondfast BF-7M manufactured by Sumitomo Chemical Co., Ltd. C-2: Compatibilizer: Ethylene-glycidyl methacrylate copolymer Bondfast BF-E manufactured by Sumitomo Chemical Co., Ltd. C-3: Compatibilizer: Epofriend AT501, an epoxy-based styrene-butadiene block copolymer manufactured by Daicel Corporation

[0136] From Tables 4 and 5, it can be seen that by containing a polyester-based thermoplastic elastomer (A) and a hydrogenated aromatic vinyl compound-based elastomer (B) which is a hydrogenated product of a block copolymer containing a polymer block (a) having a structural unit derived from an aromatic vinyl compound (styrene) and a polymer block (b) having a structural unit derived from a conjugated diene (isoprene, or isoprene and butadiene) and has a glass transition temperature of -10 to 40°C, in a mass ratio (A / B) of 99 / 1 to 1 / 99, it is possible to improve vibration damping while maintaining the properties of the polyester-based thermoplastic elastomer (A). From Table 4, in Examples 1 to 3 including the hydrogenated aromatic vinyl compound-based elastomer (B-1) obtained by using isoprene and butadiene in combination, Isoprene It was found that a higher tan δ was obtained at 0°C to 20°C than in Examples 4 to 5 containing the hydrogenated aromatic vinyl compound-based elastomer (B-2) obtained by using only Isoprene It can be seen that Examples 4 to 5 containing the hydrogenated aromatic vinyl compound-based elastomer (B-2) obtained by using only isoprene and butadiene have a higher tan δ at 30°C to 40°C than Examples 1 to 3 containing the hydrogenated aromatic vinyl compound-based elastomer (B-1) obtained by using isoprene and butadiene in combination. From Table 5, it can be seen that when a compatibilizer is added, the value of tan δ does not change significantly even if the amount of compatibilizer added is changed within the range of 1 part by mass to 3 parts by mass per 100 parts by mass of the total of the polyester-based thermoplastic elastomer (A) and the hydrogenated aromatic vinyl compound-based elastomer (B) (Examples 6 to 8).It can also be seen that when a compatibilizer is added, the value of tan δ does not change significantly even if the type of compatibilizer is changed between C-1 and C-3 (Examples 7, 9, and 10). [Industrial Applicability]

[0137] The thermoplastic elastomer composition of the present invention can improve vibration damping properties while maintaining the properties of the polyester-based thermoplastic elastomer (A), and therefore can be suitably used, for example, in vibration damping materials, gears, composite moldings, etc.

Claims

1. A thermoplastic elastomer composition comprising a polyester-based thermoplastic elastomer (A), a hydrogenated aromatic vinyl compound-based elastomer (B) having a glass transition temperature Tg of −10 to 40° C., and a compatibilizer, The hydrogenated aromatic vinyl compound-based elastomer (B) is a hydrogenated product of a block copolymer containing a polymer block (a) having a structural unit derived from an aromatic vinyl compound and a polymer block (b) having a structural unit derived from a conjugated diene compound, a mass ratio (A / B) of the polyester-based thermoplastic elastomer (A) to the hydrogenated aromatic vinyl compound-based elastomer (B) is 99 / 1 to 1 / 99; The thermoplastic elastomer composition, wherein the compatibilizer is an epoxy group-containing resin.

2. The thermoplastic elastomer composition according to claim 1, wherein the ratio (G'(0°C) / G'(50°C)) of the storage modulus G'(0°C) at 0°C to the storage modulus G'(50°C) at 50°C of the hydrogenated aromatic vinyl compound-based elastomer (B) is greater than 10.

3. The thermoplastic elastomer composition according to claim 1 or 2, wherein a mass ratio (A / B) of the polyester-based thermoplastic elastomer (A) to the hydrogenated aromatic vinyl compound-based elastomer (B) is 75 / 25 to 95 / 5.

4. The thermoplastic elastomer composition according to any one of claims 1 to 3, wherein the content of the polymer block (a) in the block copolymer is 30 mass% or less.

5. The thermoplastic elastomer composition according to claim 4 , wherein the content of the polymer block (a) in the block copolymer is 16% by mass or less.

6. The thermoplastic elastomer composition according to any one of claims 1 to 5, wherein the conjugated diene compound comprises isoprene.

7. The thermoplastic elastomer composition according to any one of claims 1 to 6, wherein the polymer block (b) has a structural unit containing, in a main chain, one or more alicyclic skeletons (X) represented by the following formula (X): 【Chemistry 1】 (In the above formula (X), R 1 ~R 3 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 11 carbon atoms, 1 ~R 3 may be the same or different.)

8. At least one of the alicyclic skeletons (X) is 1 ~R 3 The thermoplastic elastomer composition according to claim 7, wherein at least one of the above is an alicyclic skeleton (X') which is a hydrocarbon group having 1 to 11 carbon atoms.

9. The thermoplastic elastomer composition according to any one of claims 1 to 8, wherein the hydrogenation rate of the polymer block (b) is 85 to 99 mol %.

10. The thermoplastic elastomer composition according to any one of claims 1 to 9, wherein the vinyl bond content of the polymer block (b) is 65 to 90 mol %.

11. The thermoplastic elastomer composition according to any one of claims 1 to 10, wherein the hydrogenated aromatic vinyl compound-based elastomer (B) has a weight average molecular weight of 30,000 to 300,000.

12. The thermoplastic elastomer composition according to any one of claims 1 to 11, wherein the hydrogenated aromatic vinyl compound-based elastomer (B) has a peak top intensity of tan δ of 1.0 or more.

13. The thermoplastic elastomer composition according to any one of claims 1 to 12, wherein the maximum value of tan δ strength of the thermoplastic elastomer composition at 0 to 40°C is 0.1 or more.

14. The thermoplastic elastomer composition according to claim 13, wherein the maximum value of tan δ strength of the thermoplastic elastomer composition at 0 to 40° C. is 0.15 or more.

15. The thermoplastic elastomer composition according to any one of claims 1 to 13, wherein the maximum value of tan δ strength of the polyester-based thermoplastic elastomer (A) at 0 to 40°C is 0.05 or more.

16. The thermoplastic elastomer composition according to any one of claims 1 to 15, wherein the ratio (tan δ(B)max / tan δ(A)max) of the maximum tan δ strength of the hydrogenated aromatic vinyl compound-based elastomer (B) at 0 to 40 ° C. to the maximum tan δ strength of the polyester-based thermoplastic elastomer (A) at 0 to 40 ° C. is 10 to 80.

17. A vibration damping material comprising the thermoplastic elastomer composition according to any one of claims 1 to 16.

18. A gear comprising the thermoplastic elastomer composition according to any one of claims 1 to 16.

19. A composite molded article comprising a thermoplastic elastomer composition layer containing the thermoplastic elastomer composition according to any one of claims 1 to 16 fused to a polar resin layer containing a polar resin.

Citation Information

Patent Citations

  • THERMOPLASTIC ELASTOMER COMPOSITION AND COMPOSITE MOLDED PRODUCT

    JP3381488B2

  • Block copolymer or hydrogenated product of same

    WO2019103048A1