All-solid-state electrochemical elements and sulfur-carbon composites

The all-solid-state electrochemical element with a sulfur-carbon composite and sulfide solid electrolyte addresses polarization issues, enhancing electron and ion conduction to improve performance and energy density.

JP7948181B2Active Publication Date: 2026-11-11GS YUASA CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023527882
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-06-09
Filing Date
2022-06-08
Publication Date
2026-11-11
Estimated Expiration
2042-06-08

AI Technical Summary

Technical Problem

Lithium-ion rechargeable batteries using sulfur as a positive electrode active material experience significant polarization, which hinders their performance.

Method used

An all-solid-state electrochemical element with a sulfur-carbon composite where the carbon has an average pore diameter of 0.5 nm to 3.0 nm and an average particle size of 0.1 μm to 30.0 μm, along with a sulfide solid electrolyte, to enhance electron and ion conduction paths.

Benefits of technology

The sulfur-carbon composite reduces polarization, improving the charge-discharge characteristics and energy density of the all-solid-state electrochemical element.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007948181000002
    Figure 0007948181000002
  • Figure 0007948181000003
    Figure 0007948181000003
  • Figure 0007948181000004
    Figure 0007948181000004
Patent Text Reader

Abstract

An all-solid-state electrochemical element according to one aspect of the present invention comprises a positive electrode active material layer, an isolation layer, and a negative electrode active material layer. The positive electrode active material layer contains a sulfur-carbon complex, the sulfur-carbon complex contains sulfur and porous carbon, the average pore diameter of the carbon is 0.5-3.0 nm, inclusive, and the average particle diameter of the carbon is 0.1-30.0 μm, inclusive.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to an all-solid-state electrochemical element and a sulfur-carbon composite. [Background technology]

[0002] Lithium-ion rechargeable batteries are widely used in electronic devices such as personal computers and communication terminals, as well as in automobiles, due to their high energy density. Generally, these lithium-ion rechargeable batteries consist of a pair of electrodes electrically isolated by a separator, and a non-aqueous electrolyte interposed between these electrodes. They are configured to charge and discharge by transferring lithium ions between the two electrodes. In addition to lithium-ion rechargeable batteries, capacitors such as lithium-ion capacitors are also widely used as energy storage elements.

[0003] In recent years, there has been a demand for positive electrode active materials with high energy density to increase the capacity of energy storage devices. Sulfur is known as such a positive electrode active material. As an energy storage device using sulfur as a positive electrode active material, for example, Patent Document 1 proposes a sulfur-carbon composite material for use as an electrode in a non-aqueous electrolyte type secondary battery, in which 5% or more of sulfur by total weight is contained in the mesopores of mesoporous carbon with an average pore diameter of 1 to 40 nm (see Patent Document 1). [Prior art documents] [Patent Documents]

[0004] [Patent Document 1] Re-tabled publication 2016 / 075916 [Overview of the Initiative] [Problems that the invention aims to solve]

[0005] However, the inventors have found that when sulfur is used as the positive electrode active material in an all-solid-state electrochemical element, the polarization is large.

[0006] The present invention has been made based on the circumstances described above, and aims to provide an all-solid-state electrochemical element that can reduce polarization when sulfur is used as the positive electrode active material, and to provide a sulfur-carbon composite that can reduce polarization when used as the positive electrode active material of an all-solid-state electrochemical element. [Means for solving the problem]

[0007] An all-solid-state electrochemical element according to one aspect of the present invention comprises a positive electrode active material layer, an isolation layer, and a negative electrode active material layer, wherein the positive electrode active material layer contains a sulfur-carbon composite, the sulfur-carbon composite contains sulfur and porous carbon, the average pore diameter of the carbon is 0.5 nm to 3.0 nm, and the average particle size is 0.1 μm to 30.0 μm.

[0008] Another aspect of the present invention relates to a sulfur-carbon composite comprising sulfur and porous carbon, wherein the average pore size of the carbon is 0.5 nm or more and 3.0 nm or less, and the average particle size is 0.1 μm or more and 30.0 μm or less. [Effects of the Invention]

[0009] An all-solid-state electrochemical element according to one aspect of the present invention can reduce the polarization that occurs when sulfur is used as the positive electrode active material.

[0010] Another aspect of the present invention relates to a sulfur-carbon composite that can reduce polarization when used as a positive electrode active material in an all-solid-state electrochemical device. [Brief explanation of the drawing]

[0011] [Figure 1] Figure 1 is a schematic cross-sectional view of an all-solid-state battery, which is one embodiment of the all-solid-state electrochemical element of the present invention. [Figure 2] Figure 2 is a schematic diagram showing one embodiment of an energy storage device constructed by assembling multiple all-solid-state electrochemical elements. [Figure 3] Figure 3 shows the charge and discharge curves of the examples and comparative examples. [Figure 4]Figure 4 is a diagram showing charge curves of Examples and Comparative Examples. [Figure 5] Figure 5 is a diagram showing discharge curves of Examples and Comparative Examples. [Figure 6] Figure 6 is a diagram showing charge-discharge curves of Examples and Comparative Examples. [Figure 7] Figure 7 is a diagram showing a charge-discharge curve of a Reference Example. [Mode for Carrying Out the Invention]

[0012] As will be understood from the following description and Examples, the matters disclosed by the present specification include the following.

[0013] [1]: An all-solid-state electrochemical element comprising a positive electrode active material layer, a separator layer, and a negative electrode active material layer, the positive electrode active material layer containing a sulfur-carbon composite, the sulfur-carbon composite containing sulfur and porous carbon, wherein the carbon has an average pore diameter of 0.5 nm or more and 3.0 nm or less, and an average particle diameter of 0.1 μm or more and 30.0 μm or less.

[0014] [2]: The all-solid-state electrochemical element according to the above [1], wherein the positive electrode active material layer contains a sulfide solid electrolyte.

[0015] [3]: A sulfur-carbon composite containing sulfur and porous carbon, wherein the carbon has an average pore diameter of 0.5 nm or more and 3.0 nm or less, and an average particle diameter of 0.1 μm or more and 30.0 μm or less.

[0016] First, an overview of the all-solid-state electrochemical element and the sulfur-carbon composite disclosed by the present specification will be described.

[0017] An all-solid-state electrochemical element according to one aspect of the present invention comprises a positive electrode active material layer, an isolation layer, and a negative electrode active material layer, wherein the positive electrode active material layer contains a sulfur-carbon composite, the sulfur-carbon composite contains sulfur and porous carbon, the average pore diameter of the carbon is 0.5 nm to 3.0 nm, and the average particle size is 0.1 μm to 30.0 μm.

[0018] The all-solid-state electrochemical element in question can reduce the polarization that occurs when sulfur is used as the positive electrode active material. The reason for this is not entirely clear, but the following reasons are speculated: The average pore size of the carbon in the sulfur-carbon composite is between 0.5 nm and 3.0 nm, which ensures that the electron conduction paths between sulfur and carbon are well maintained. As a result, the polarization that occurs when sulfur is used as the positive electrode in the all-solid-state electrochemical element can be reduced. Furthermore, the average particle size of the carbon is between 0.1 μm and 30.0 μm, which reduces the voids in the positive electrode active material layer of the all-solid-state electrochemical element, making it easier to construct ion and electron conduction paths within this positive electrode active material layer. Therefore, it is speculated that the all-solid-state electrochemical element can reduce the polarization that occurs when sulfur is used as the positive electrode active material.

[0019] In the all-solid-state electrochemical element, the positive electrode active material layer preferably contains a sulfide solid electrolyte. This can improve the performance of the all-solid-state electrochemical element.

[0020] Another aspect of the present invention relates to a sulfur-carbon composite comprising sulfur and porous carbon, wherein the average pore size of the carbon is 0.5 nm or more and 3.0 nm or less, and the average particle size is 0.1 μm or more and 30.0 μm or less.

[0021] The sulfur-carbon composite in question contains sulfur and porous carbon, and because the average pore size and average particle size of the carbon are within a specific range, it can reduce polarization when used as the positive electrode active material in an all-solid-state electrochemical element. The reason for this is not entirely clear, but it is thought to be the same reason why polarization is reduced when sulfur is used as the positive electrode active material in the same all-solid-state electrochemical element.

[0022] The configuration of an all-solid-state electrochemical element, the configuration of an energy storage device, a method for manufacturing an all-solid-state electrochemical element, and other embodiments according to one embodiment of the present invention will be described in detail. Note that the names of the components (parts) used in each embodiment may differ from the names of the components (parts) used in the background art.

[0023] <All-solid-state electrochemical elements> As one embodiment of the all-solid-state electrochemical element of the present invention, an all-solid-state battery will be described below as a specific example. The all-solid-state battery 10 shown in Figure 1 is a secondary battery in which a positive electrode 1 and a negative electrode 2 are arranged with an isolation layer 3 in between. The positive electrode 1 has a positive electrode substrate 4 and a positive electrode active material layer 5, with the positive electrode substrate 4 being the outermost layer of the positive electrode 1. The positive electrode active material layer 5 contains the sulfur-carbon composite. The negative electrode 2 has a negative electrode substrate 7 and a negative electrode active material layer 6, with the negative electrode substrate 7 being the outermost layer of the negative electrode 2. In the all-solid-state battery 10 shown in Figure 1, the negative electrode active material layer 6, isolation layer 3, positive electrode active material layer 5, and positive electrode substrate 4 are stacked on the negative electrode substrate 7 in this order.

[0024] [Positive electrode] The positive electrode 1 comprises a positive electrode substrate 4 and a positive electrode active material layer 5 that is laminated directly onto the surface of the positive electrode substrate 4 or via an intermediate layer.

[0025] (Positive electrode substrate) The positive electrode substrate 4 is conductive. Whether or not it is conductive is determined by the volume resistivity measured in accordance with JIS-H-0505 (1975) when it is 10 7The determination is made using Ω·cm as the threshold. The positive electrode substrate material can be a metal such as aluminum, titanium, tantalum, or stainless steel, or an alloy thereof. Among these, aluminum or an aluminum alloy is preferred from the viewpoint of high potential resistance, high conductivity, and cost. Examples of positive electrode substrates include foil, vapor-deposited film, mesh, and porous material, with foil being preferred from the viewpoint of cost. Therefore, aluminum foil or aluminum alloy foil is preferred as the positive electrode substrate. Examples of aluminum or aluminum alloys include A1085, A3003, and A1N30 as specified in JIS-H-4000 (2014) or JIS-H-4160 (2006).

[0026] The average thickness of the positive electrode substrate 4 is preferably 3 μm to 50 μm, more preferably 5 μm to 40 μm, even more preferably 8 μm to 30 μm, and particularly preferably 10 μm to 25 μm. By setting the average thickness of the positive electrode substrate 4 within the above range, the strength of the positive electrode substrate 4 can be increased while increasing the energy density per unit volume of the all-solid-state battery.

[0027] (Middle class) The intermediate layer is a layer placed between the positive electrode substrate 4 and the positive electrode active material layer 5. The intermediate layer contains a conductive agent such as carbon particles to reduce the contact resistance between the positive electrode substrate and the positive electrode active material layer. The composition of the intermediate layer is not particularly limited and may include, for example, a binder and a conductive agent.

[0028] (Cathode active material layer) The positive electrode active material layer 5 contains a positive electrode active material. The positive electrode active material layer 5 usually further contains a solid electrolyte. The positive electrode active material layer 5 may contain a mixture or composite containing the positive electrode active material and the solid electrolyte. The positive electrode active material layer 5 may optionally contain optional components such as a conductive agent, binder, thickener, or filler.

[0029] The above-mentioned positive electrode active material contains the sulfur-carbon composite. The sulfur-carbon composite contains sulfur and porous carbon. When used as the positive electrode active material of an all-solid-state electrochemical element, the sulfur-carbon composite can reduce polarization. The above-mentioned sulfur-carbon composite means a composite in which at least a portion of sulfur is filled into the pores of porous carbon.

[0030] The lower limit of the sulfur content in the sulfur-carbon composite (the ratio of the mass of sulfur atoms to the mass of the sulfur-carbon composite) is preferably 50% by mass, and more preferably 55% by mass. On the other hand, the upper limit of this content is preferably 90% by mass, and more preferably 80% by mass. By setting the sulfur content in the sulfur-carbon composite to be above or below the above lower limit or upper limit, the energy density as an all-solid-state electrochemical element can be increased, and good cathode characteristics can be achieved.

[0031] The average pore size of the carbon in the sulfur-carbon composite is 0.5 nm to 3.0 nm, preferably 0.7 nm to 2.7 nm, more preferably 0.8 nm to 2.6 nm, even more preferably 0.9 nm to 2.5 nm, and even more preferably 1.0 nm to 2.4 nm. By keeping the average pore size below the upper limit, the electron conduction path between sulfur and carbon is well maintained, thereby reducing polarization in the all-solid-state electrochemical element. On the other hand, by keeping the average pore size above the lower limit, a surface area suitable for intercalation and deintercalation of the charge carrier is secured, improving charge-discharge characteristics.

[0032] The average pore size of the carbon in the sulfur-carbon composite was measured by the following method. First, 1.00 g of carbon powder, which is to be measured, is placed in a sample tube for measurement, and the moisture in the sample is thoroughly removed by vacuum drying at 120°C for 6 hours and then at 180°C for 6 hours. Next, the average pore size of the carbon is calculated by measuring the isotherms on the adsorption and desorption sides within a relative pressure P / P0 (P0 = approximately 770 mmHg) range of 0 to 1 using the nitrogen gas adsorption method with liquid nitrogen. The measurement device and control / analysis software are not particularly limited as long as they are capable of the above measurement. For example, "autosorb iQ" manufactured by Quantachrome can be used as the measurement device, and "ASiQwin" can be used as the control / analysis software.

[0033] Here, when the carbon powder sample to be measured is taken from the positive electrode mixture extracted by disassembling an all-solid-state electrochemical element, the sample is prepared by the following method: Before disassembling the all-solid-state electrochemical element, the element is discharged at a constant current of 0.05C in a 25°C environment until it reaches the lower limit voltage of normal use. The all-solid-state electrochemical element is disassembled and the positive electrode mixture is extracted. The sulfur-carbon composite is collected from the extracted positive electrode mixture. Next, the collected sulfur-carbon composite is heated to 500°C in an argon flow to vaporize the sulfur. Then, the remaining carbon residue is collected and subjected to measurement.

[0034] The average particle size of carbon in the sulfur-carbon composite is 0.1 μm to 30.0 μm, preferably 1.0 μm to 25.0 μm, more preferably 3.0 μm to 20.0 μm, even more preferably 4.0 μm to 17.0 μm, and even more preferably 4.5 μm to 15.4 μm. Having the average particle size of carbon below the upper limit reduces the voids in the positive electrode active material layer, making it easier to construct ion and electron conduction paths within the positive electrode active material layer. Furthermore, the number of pores per unit surface area of ​​the carbon increases, resulting in a more uniform current distribution, thus reducing polarization in the all-solid-state electrochemical element. Having the average particle size of carbon above the lower limit makes the sulfur-carbon composite easier to handle.

[0035] The average carbon particle size in the sulfur-carbon composite refers to the value at which the volume-based integrated distribution, calculated in accordance with JIS-Z-8819-2 (2001), becomes 50%, based on the particle size distribution measured by laser diffraction / scattering on a dilution obtained by diluting the particles with a solvent, in accordance with JIS-Z-8825 (2013). The measuring device and measurement control software are not particularly limited as long as they are capable of the above measurement. For example, Nikkiso's "Microtrac (model number: MT3000)" can be used as the measuring device, and "Microtrac DHS for Win98 (MT3000)" can be used as the measurement control software.

[0036] The porous carbon in the sulfur-carbon composite has a specific surface area of ​​2000 m². 2 / g or more 3000m 2 It is preferable that the amount is less than or equal to / g. When the specific surface area of ​​the porous carbon is within the above range, the sulfur and the porous carbon come into good contact, increasing conductivity, and thus improving the sulfur utilization rate in all-solid-state batteries.

[0037] The content of the sulfur-carbon composite in the positive electrode active material layer 5 (the ratio of the mass of the sulfur-carbon composite to the mass of the positive electrode active material layer) is preferably 40% by mass or more and 77% by mass or less, and more preferably 48% by mass or more and 72% by mass or less. By setting the sulfur-carbon composite content within the above range, it is possible to achieve both a large electrical capacity and good conductivity, thereby increasing the energy density of the all-solid-state battery.

[0038] The positive electrode active material may contain other positive electrode active materials besides the sulfur-carbon composite. Examples of other positive electrode active materials besides the sulfur-carbon composite include polymers, metals, oxides, etc. However, the lower limit of the sulfur-carbon composite content in the total positive electrode active material is preferably 80% by mass, more preferably 85% by mass, and even more preferably 88% by mass. The upper limit of the sulfur-carbon composite content in the total positive electrode active material may be 100% by mass, 99% by mass, or 98% by mass. In other words, the sulfur-carbon composite content in the total positive electrode active material may be 80% by mass or more and 100% by mass or less, 85% by mass or more and 99% by mass or less, or 88% by mass or more and 98% by mass or less.

[0039] The positive electrode active material layer 5 typically contains a solid electrolyte. Examples of solid electrolytes include sulfide solid electrolytes, oxide solid electrolytes, fluoride solid electrolytes, nitride solid electrolytes, dry polymer electrolytes, and gel polymer electrolytes. Among these, sulfide solid electrolytes are preferred. Furthermore, the positive electrode active material layer 5 may contain multiple different types of solid electrolytes.

[0040] The sulfide solid electrolyte may be any material that contains sulfur and exhibits ion conductivity to carrier ions. The sulfide solid electrolyte typically contains elemental lithium and elemental sulfur and has lithium ion conductivity. The sulfide solid electrolyte preferably contains elemental lithium, elemental sulfur and elemental phosphorus as main components, and more preferably contains elemental lithium, elemental sulfur, elemental phosphorus and elemental halogen as main components. The sulfide solid electrolyte may further contain typical nonmetallic elements such as B, N, O, C and Si, typical metallic elements such as Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr and Ba, and transition metal elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Nb and W. The sulfide solid electrolyte may be any of a crystalline material, glass ceramics and glass. Specific examples of the sulfide solid electrolyte include Li2S-P2S5 system, Li2S-P2S5-LiI system, Li2S-P2S5-LiCl system, Li2S-P2S5-LiBr system, Li2S-P2S5-Li2O system, Li2S-P2S5-Li2O-LiI system, Li2S-P2S5-Li3N system, Li2S-SiS2 system, Li2S-SiS2-LiI system, Li2S-SiS2-LiBr system, Li2S-SiS2-LiCl system, Li2S-SiS2-B2S3-LiI system, Li2S-SiS2-P2S5-LiI system, Li2S-B2S3 system, Li2S-P2S5-Z m S 2n system (wherein m and n are positive numbers, and Z is any one of Ge, Zn and Ga), Li2S-GeS2 system, Li2S-SiS2-Li3PO4 system, Li2S-SiS2-Li x MO y system (wherein x and y are positive numbers, and M is any one of P, Si, Ge, B, Al, Ga and In), Li 10 GeP2S 12 system and the like can be mentioned.

[0041] When the positive electrode active material layer 5 contains a solid electrolyte, the content of the solid electrolyte is preferably 1 mass% or more and 50 mass% or less, and more preferably 1 mass% or more and 45 mass% or less. By setting the content of the solid electrolyte within the above range, the electric capacity of the all-solid-state battery 10 can be increased.

[0042] The conductive agent is not particularly limited as long as it is a conductive material. Examples of such conductive agents include carbonaceous materials, metals, and conductive ceramics. Examples of carbonaceous materials include graphite, non-graphitic carbon, and graphene-based carbon. Examples of non-graphitic carbon include carbon nanofibers, pitch-based carbon fibers, and carbon black. Examples of carbon black include furnace black, acetylene black, and Ketjen black. Examples of graphene-based carbon include graphene, carbon nanotubes (CNTs), and fullerenes. The conductive agent can take the form of powder or fiber. One of these materials may be used alone as the conductive agent, or two or more may be used in mixture form. These materials may also be used in composite form. For example, a composite material of carbon black and CNTs may be used. Among these, carbon black is preferred from the viewpoint of electronic conductivity and coating properties, and acetylene black is particularly preferred.

[0043] The content of the conductive agent in the positive electrode active material layer 5 is preferably 1% by mass or more and 10% by mass or less, and more preferably 3% by mass or more and 9% by mass or less. By setting the content of the conductive agent within the above range, the energy density of the all-solid-state battery 10 can be increased.

[0044] Examples of binders include thermoplastic resins such as fluororesins (polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), etc.), polyethylene, polypropylene, polyacrylic, and polyimide; elastomers such as ethylene-propylene-diene rubber (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), and fluororubber; and polysaccharide polymers.

[0045] The binder content in the positive electrode active material layer 5 is preferably 1% by mass or more and 10% by mass or less, and more preferably 3% by mass or more and 9% by mass or less. By keeping the binder content within the above range, the active material can be stably retained.

[0046] Examples of thickening agents include polysaccharide polymers such as carboxymethylcellulose (CMC) and methylcellulose. If the thickening agent has a functional group that reacts with lithium or the like, this functional group may be deactivated beforehand by methylation or the like.

[0047] The filler is not particularly limited. Examples of fillers include polyolefins such as polypropylene and polyethylene, inorganic oxides such as silicon dioxide, alumina, titanium dioxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, and aluminosilicates, hydroxides such as magnesium hydroxide, calcium hydroxide, and aluminum hydroxide, carbonates such as calcium carbonate, sparingly soluble ionic crystals such as calcium fluoride, barium fluoride, and barium sulfate, nitrides such as aluminum nitride and silicon nitride, mineral resource-derived materials such as talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, and mica, or artificial products thereof.

[0048] The positive electrode active material layer 5 may contain typical nonmetallic elements such as B, N, P, F, Cl, Br, and I, typical metallic elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, and Ba, and transition metal elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Nb, and W as components other than the positive electrode active material, solid electrolyte, conductive agent, binder, thickener, and filler.

[0049] [Negative electrode] The negative electrode 2 comprises a negative electrode substrate 7 and a negative electrode active material layer 6 disposed directly on the negative electrode substrate 7 or via an intermediate layer. The configuration of the intermediate layer is not particularly limited and can be selected from, for example, the configurations exemplified in the positive electrode 1.

[0050] (Negative electrode substrate) The negative electrode substrate 7 is electrically conductive. The negative electrode substrate 7 can be made from metals such as copper, nickel, stainless steel, nickel-plated steel, or aluminum, or alloys thereof, or carbonaceous materials. Among these, copper or copper alloys are preferred. Examples of negative electrode substrate 7 include foil, vapor-deposited film, mesh, and porous materials, with foil being preferred from a cost standpoint. Therefore, copper foil or copper alloy foil is preferred as the negative electrode substrate. Examples of copper foil include rolled copper foil and electrolytic copper foil.

[0051] The average thickness of the negative electrode substrate 7 is preferably 2 μm to 35 μm, more preferably 3 μm to 30 μm, even more preferably 4 μm to 25 μm, and particularly preferably 5 μm to 20 μm. By setting the average thickness of the negative electrode substrate 7 within the above range, the strength of the negative electrode substrate 7 can be increased while increasing the energy density per unit volume of the all-solid-state battery 10.

[0052] (Negative electrode active material layer) The negative electrode active material layer 6 contains a negative electrode active material. The negative electrode active material layer 6 may be formed from a negative electrode mixture containing the negative electrode active material, and may optionally contain conductive agents, binders, thickeners, fillers, etc. The conductive agents, binders, thickeners, fillers, etc., can be selected from the materials exemplified in the positive electrode 1 above. When the negative electrode active material layer 6 is formed from a negative electrode mixture, the negative electrode active material layer 6 usually further contains a solid electrolyte.

[0053] In the all-solid-state electrochemical element, a negative electrode active material containing the element lithium, such as metallic lithium or lithium compounds, is preferably used. Among these, metallic lithium is preferred as the negative electrode active material. The metallic lithium may be pure metallic lithium consisting substantially only of the element lithium, or it may be a lithium alloy containing other metallic elements. Examples of lithium alloys include lithium silver alloy, lithium zinc alloy, lithium calcium alloy, lithium aluminum alloy, lithium magnesium alloy, and lithium indium alloy. The lithium alloy may contain multiple metallic elements other than the element lithium. An example of a lithium compound is Li4Ti5O 12 Examples include LiTiO2.

[0054] The content of the lithium-containing negative electrode active material in the negative electrode active material layer 6 is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 99% by mass or more.

[0055] The negative electrode active material layer 6 may be a non-porous layer (solid layer) containing lithium. The negative electrode active material layer 6 may be a porous layer having particles containing lithium. The negative electrode active material layer 6 may be a layer consisting substantially only of negative electrode active material containing lithium. The negative electrode active material layer 6 may be pure metallic lithium foil or lithium alloy foil. When the negative electrode active material layer 6 contains negative electrode active material containing lithium, the average thickness of the negative electrode active material layer 6 is preferably 5 μm or more and 1,000 μm or less, more preferably 10 μm or more and 500 μm or less, and even more preferably 30 μm or more and 300 μm or less. The "average thickness" of the negative electrode active material layer refers to the average value of the thickness measured at any five locations in the negative electrode active material layer.

[0056] The negative electrode active material layer 6 may further contain other negative electrode active materials other than the negative electrode active material containing lithium element. However, the content of the negative electrode active material containing lithium element relative to all negative electrode active materials in the negative electrode active material layer 6 is preferably 90% by mass or more, more preferably 99% by mass or more, and even more preferably 100% by mass.

[0057] Other negative electrode active materials besides those containing lithium can be appropriately selected from known negative electrode active materials. Examples of such negative electrode active materials include metals or metalloids such as Si and Sn; metal oxides or metalloid oxides such as Si oxide, Ti oxide, and Sn oxide; titanium-containing oxides such as TiNb2O7; polyphosphate compounds; silicon carbide; and carbon materials such as graphite and non-graphitizable carbon (easily graphitizable carbon or poorly graphitizable carbon). In the negative electrode active material layer 6, one of these materials may be used alone, or two or more may be used in combination. Furthermore, these materials may be used in combination with negative electrode active materials containing lithium.

[0058] When the negative electrode active material layer 6 is formed from a negative electrode mixture, the negative electrode active material layer 6 usually contains a solid electrolyte. The same type of solid electrolyte as those listed for the positive electrode can be used, and among these, a sulfide solid electrolyte is preferred. When the negative electrode active material layer 6 contains a solid electrolyte, the solid electrolyte content is preferably 1% by mass or more and 50% by mass or less, and more preferably 1% by mass or more and 45% by mass or less. By setting the solid electrolyte content within the above range, the electrical capacity of the all-solid-state battery 10 can be increased.

[0059] When the negative electrode active material layer 6 is formed from a negative electrode mixture, the content of the negative electrode active material in the negative electrode active material layer 6 is preferably 60% by mass or more and 99% by mass or less, and more preferably 90% by mass or more and 98% by mass or less. By setting the content of the negative electrode active material within the above range, it is possible to achieve both high energy density and manufacturability of the negative electrode active material layer 6.

[0060] When the negative electrode active material layer 6 is formed from a negative electrode mixture, the average thickness of the negative electrode active material layer 6 is preferably 30 μm or more and 1,000 μm or less, and more preferably 60 μm or more and 500 μm or less. By setting the average thickness of the negative electrode active material layer 6 to be above the lower limit, an all-solid-state battery 10 with a high energy density can be obtained. By setting the average thickness of the negative electrode active material layer 6 to be below the upper limit, it is possible to miniaturize the all-solid-state battery 10.

[0061] The negative electrode active material layer 6 may contain typical nonmetallic elements such as B, N, P, F, Cl, Br, and I, typical metallic elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, and Ba, and transition metallic elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Ta, Hf, Nb, and W as components other than the negative electrode active material, solid electrolyte, conductive agent, binder, thickener, and filler.

[0062] [Isolation layer] The isolation layer 3 contains a solid electrolyte. Various solid electrolytes as exemplified in the positive electrode 1 can be used as the solid electrolyte contained in the isolation layer 3, and among these, a sulfide solid electrolyte is preferred. The solid electrolyte content in the isolation layer 3 is preferably 70% by mass or more, more preferably 90% by mass or more, even more preferably 99% by mass or more, and even more preferably substantially 100% by mass.

[0063] The isolation layer 3 may contain optional components such as binders, thickeners, and fillers. These optional components can be selected from the materials exemplified in the positive electrode 1.

[0064] The average thickness of the isolation layer 3 is preferably 1 μm to 50 μm, and more preferably 3 μm to 20 μm. By setting the average thickness of the isolation layer 3 to above the lower limit, it becomes possible to reliably insulate the positive electrode 1 and the negative electrode 2. By setting the average thickness of the isolation layer 3 to below the upper limit, it becomes possible to increase the energy density of the all-solid-state battery 10.

[0065] The all-solid-state battery 10 of this embodiment can be installed as an energy storage device in which multiple all-solid-state batteries 10 are assembled, such as in power supplies for automobiles such as electric vehicles (EVs), hybrid electric vehicles (HEVs), and plug-in hybrid electric vehicles (PHEVs), power supplies for electronic devices such as personal computers and communication terminals, or power storage devices. In this case, it is sufficient that the technology of the present invention is applied to at least one of the all-solid-state batteries 10 included in the energy storage device.

[0066] Figure 2 shows an example of a power storage device 30 which is formed by further assembling power storage units 20, each of which is a collection of two or more electrically connected solid-state batteries 10. The power storage device 30 may include busbars (not shown) that electrically connect two or more solid-state batteries 10, busbars (not shown) that electrically connect two or more power storage units 20, etc. The power storage unit 20 or the power storage device 30 may include a condition monitoring device (not shown) that monitors the state of one or more solid-state batteries 10.

[0067] [Manufacturing method for all-solid-state electrochemical elements] A method for manufacturing an all-solid-state electrochemical element according to one embodiment of the present invention can be carried out by a commonly known method, except that the sulfur-carbon composite is used to manufacture the positive electrode. Specifically, this manufacturing method comprises, for example, (1) manufacturing a sulfur-carbon composite, (2) preparing a positive electrode, (3) preparing a material for the isolation layer, (4) preparing a negative electrode, and (5) laminating the positive electrode, isolation layer, and negative electrode. Each step will be described in detail below.

[0068] (1) Sulfur-carbon composite fabrication process In this process, a sulfur-carbon composite is produced by compounding a mixture of porous carbon and sulfur. This compounding is carried out by heat-treating the mixture in a sealed container. Examples of this heat treatment include performing the first and second heating steps described later, or slowly raising the temperature without dividing it into the first and second heating steps.

[0069] An example of a heat treatment that performs the above-mentioned first and second heating steps is as follows: By performing the first and second heating steps, sulfur particles are supported not only on the surface of the porous carbon but also in the pores with high dispersion, thereby increasing the utilization rate of sulfur. (1-1) First heating step The first heating step involves heating to the temperature at which sulfur melts. Specifically, the mixture is heated from room temperature to a range of 112°C to 159°C, and then held at that temperature range. The holding time is preferably 5 hours or more. This step uniformly coats the porous carbon surface with sulfur. (1-2) Second heating step The second heating step involves heating to a temperature at which sulfur vaporizes. In the second heating step, it is preferable to raise the temperature to 250°C or higher and maintain it there. In the second heating step, the sulfur, which has been uniformly supported on the surface of the porous carbon by the first heating step, can be vaporized near the pores of the porous carbon.

[0070] The heating rate in the first and second heating steps is not particularly limited, but is preferably 1°C / min to 5°C / min for work efficiency. Furthermore, a step of cooling to 95°C or below may be included between the first and second heating steps to promote the immobilization of the sulfur coated on the porous carbon surface.

[0071] (2) Positive electrode preparation process In this process, a positive electrode mixture is typically prepared to form a positive electrode active material layer using the sulfur-carbon composite as the positive electrode active material. There are no particular restrictions on the method of preparing the positive electrode mixture, and it can be appropriately selected depending on the purpose. Examples include processing the positive electrode mixture material by mechanical milling, and compression molding of the positive electrode active material. If the positive electrode mixture contains a positive electrode active material and a solid electrolyte, this process may include mixing the positive electrode active material and the solid electrolyte using, for example, mechanical milling, to prepare a mixture or composite of the positive electrode active material and the solid electrolyte.

[0072] Preparing a positive electrode containing a positive electrode active material may be equivalent to manufacturing a positive electrode containing a positive electrode active material. The positive electrode can be manufactured, for example, by applying a positive electrode mixture paste directly to a positive electrode substrate or via an intermediate layer, and then drying it. The positive electrode mixture paste contains a sulfur-carbon composite and optional components such as a conductive agent and a binder, which constitute the positive electrode mixture. The positive electrode mixture paste may further contain a dispersion medium. Specific examples and preferred examples of the prepared positive electrode are the same as those provided in the all-solid-state battery according to the above-described embodiment of the present invention. Alternatively, the positive electrode can also be manufactured by forming it by pressure molding the positive electrode mixture directly to a positive electrode substrate or via an intermediate layer.

[0073] (3) Preparation of materials for the isolation layer In this process, materials for forming the isolation layer are typically produced. The main component of the isolation layer material in all-solid-state batteries is usually a solid electrolyte. The solid electrolyte used as the isolation layer material can be produced by conventionally known methods. For example, it can be obtained by processing a predetermined material by mechanical milling. Alternatively, the isolation layer material may be produced by heating a predetermined material above its melting temperature using a melt-and-cooling method, melting and mixing the two in a predetermined ratio, and then rapidly cooling. Other methods for synthesizing the isolation layer material include, for example, a solid-phase method involving encapsulation under reduced pressure and calcination, a liquid-phase method such as dissolution extraction, a gas-phase method (PLD), and calcination under an argon atmosphere after mechanical milling.

[0074] (4) Negative electrode preparation process In this process, a negative electrode mixture is typically prepared to form a negative electrode active material layer. The specific method for preparing the negative electrode mixture is the same as that for the positive electrode mixture. If the negative electrode mixture contains a negative electrode active material and a solid electrolyte, this process may include mixing the negative electrode active material and the solid electrolyte using, for example, a mechanical milling method, to prepare a mixture or composite of the negative electrode active material and the solid electrolyte. Preparing a negative electrode containing a negative electrode active material may be equivalent to manufacturing a negative electrode containing a negative electrode active material. The manufacturing of the negative electrode can be carried out in the same way as the manufacturing of the positive electrode. Furthermore, if the negative electrode active material is a metal such as metallic lithium, the negative electrode can be manufactured, for example, by laminating foil-shaped negative electrode active material directly onto a negative electrode substrate or via an intermediate layer.

[0075] (5)Lamination process In this process, for example, a positive electrode having a positive electrode substrate and a positive electrode active material layer, an isolation layer, and a negative electrode having a negative electrode substrate and a negative electrode active material layer are laminated. In this process, the positive electrode, isolation layer, and negative electrode may be formed sequentially in this order, or in reverse order, and the order of formation of each layer is not particularly limited. The positive electrode is formed, for example, by pressure molding a positive electrode substrate and a positive electrode mixture, the isolation layer is formed by pressure molding an isolation layer material, and the negative electrode is formed by pressure molding a negative electrode substrate and a negative electrode mixture. The positive electrode, isolation layer, and negative electrode may also be laminated by pressure molding the positive electrode substrate, positive electrode mixture, isolation layer material, negative electrode mixture, and negative electrode substrate at the same time. The positive electrode and negative electrode may be pre-molded and then laminated by pressure molding with the isolation layer.

[0076] [Other embodiments] The present invention is not limited to the embodiments described above, and can be implemented in various modified and improved forms in addition to those described above. For example, the all-solid-state battery may include other layers besides the positive electrode, isolation layer, and negative electrode, such as an intermediate layer or an adhesive layer. The all-solid-state electrochemical element according to the present invention may be a bipolar all-solid-state battery. The all-solid-state electrochemical element according to the present invention may be a capacitor or the like, or a primary battery, in addition to an all-solid-state battery which is an energy storage element. [Examples]

[0077] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0078] (Preparation of solid electrolytes) Li2S (0.478g) and P2S5 (0.772g) were mixed in an agate mortar. The mixture was placed in a sealed 80mL zirconia pot containing 160g of 4mm diameter zirconia balls. These steps were carried out under an argon atmosphere with a dew point of -50°C or lower. Next, the mixture was mechanically milled for 45 hours at a rotational speed of 510rpm using a planetary ball mill (FRITSCH, model number Premium line P-7) to obtain the sulfide solid electrolyte 75Li2S·25P2S5(LPS).

[0079] [Example 1] (Preparation of positive electrode mixture) Sulfur and a specific surface area of ​​2100 m 2 Porous carbon at a density of / g was mixed in a mass ratio of 65:35. The average pore size and average particle size of the porous carbon are shown in Table 1. This mixture was placed in a sealed electric furnace. After 1 hour of argon flow, the temperature was increased to 150°C at a heating rate of 5°C / min and held for 2 hours. Then, it was allowed to cool to 80°C, the temperature at which sulfur solidifies, and then the temperature was increased again to 300°C at a heating rate of 5°C / min and held for 2 hours. After cooling to room temperature, a sulfur-carbon composite was prepared. Subsequently, the sulfur-carbon composite and a sulfide solid electrolyte were mixed in a mass ratio of 60:40. Next, under an argon atmosphere, the mixture was placed in a sealed 80 mL zirconia pot containing 160 g of 4 mm diameter zirconia balls and compounded by mechanical milling at a rotational speed of 300 rpm for 15 minutes using a planetary ball mill to obtain a cathode composite.

[0080] (Fabrication of all-solid-state batteries) 80 mg of sulfide solid electrolyte was placed in a powder molding machine with an inner diameter of 10 mm as the material for the isolation layer, and then press-molded using a hydraulic press to create the isolation layer. After the pressure was released, 5 mg of positive electrode mixture was placed on one side of the isolation layer and press-molded at 360 MPa for 5 minutes to create the positive electrode active material layer. After the pressure was released, the negative electrode, which was the negative electrode active material layer consisting of a metallic lithium foil and an indium foil that had been pre-bonded, was placed opposite the isolation layer and press-molded at 45 MPa. This resulted in a 10 mm diameter laminate having a positive electrode active material layer, an isolation layer, and a negative electrode active material layer. A rectangular polytetrafluoroethylene plate, approximately 30 mm square, with a through-hole of approximately 10 mm in diameter in the center, was prepared, the obtained laminate was placed in this through-hole, and the center of the polytetrafluoroethylene plate was sandwiched between two stainless steel foils. This was then vacuum-sealed in an outer casing made of a metal-resin composite film. At this time, each end of the lead terminal, which is made of nickel foil and pre-attached to each stainless steel foil, was led out from the sealing portion of the outer casing. Both sides of this outer casing were sandwiched between two sheets of polytetrafluoroethylene, each approximately 40 mm square, and these two sides were further sandwiched between two stainless steel plates, each approximately 60 mm square. The stainless steel plates were then fastened together with screws under the condition that a pressure of 50 MPa was applied to the laminate. In this way, the all-solid-state battery of Example 1 was obtained.

[0081] [Examples 2 to 5 and Comparative Examples 1 to 4] All-solid-state batteries were obtained in the same manner as in Example 1, except that the average pore size and average particle size of the porous carbon in the sulfur-carbon composite, which is the positive electrode active material, were as shown in Table 1.

[0082] [Reference example 1] (Fabrication of the positive electrode) As the positive electrode active material, a sulfur-carbon composite containing porous carbon with the average pore size and average particle size shown in Table 1 was used. Next, a positive electrode paste was prepared using water as the dispersion medium, containing the above positive electrode active material, acetylene black (AB) as a conductive agent, carboxymethylcellulose (CMC) as a thickener, and styrene-butadiene rubber (SBR) as a binder in a mass ratio of 80:10:3.6:6.4. The above positive electrode paste was coated onto one side of an aluminum foil, which served as the positive electrode substrate, dried, and pressed to produce a positive electrode with a layer of positive electrode active material.

[0083] (Fabrication of the negative electrode) A lithium metal plate measuring 30 mm in width, 40 mm in length, and 500 μm in thickness was used as the negative electrode.

[0084] (Preparation of non-aqueous electrolyte) A mixed solvent consisting of fluoroethylene carbonate and methyl-2,2,2-trifluoroethyl carbonate in a 50:50 volume ratio is mixed with lithium bis(trifluoromethanesulfonyl)imide as the electrolyte salt at a concentration of 1 mol / dm³. 3 A solution was prepared by dissolving the substance at the specified concentration, and this was used as a non-aqueous electrolyte.

[0085] (Construction of non-aqueous electrolyte batteries) A bag-shaped separator with two pockets was fabricated using a 25 μm thick polypropylene microporous membrane. The negative electrode was inserted into one of the pockets of the bag-shaped separator, and the positive electrode was inserted into the other pocket so that the side with the positive electrode active material layer faced the negative electrode. In this way, an electrode body was fabricated.

[0086] The electrode assembly was housed in a metal-resin composite film, which served as the outer casing, such that the open ends of the lead terminals pre-connected to the positive and negative electrodes were exposed to the outside. The assembly was then sealed except for the portion that would serve as the electrolyte injection hole. After the non-aqueous electrolyte solution was injected, the injection hole was hermetically sealed. In this way, a non-aqueous electrolyte battery was manufactured.

[0087] [Reference example 2] A non-aqueous electrolyte battery of Reference Example 2 was obtained in the same manner as Reference Example 1, except that a sulfur-carbon composite containing porous carbon with the average pore size and average particle size shown in Table 1 was used as the positive electrode active material.

[0088] [evaluation] (Charge / Discharge Test) Charge-discharge tests were conducted in an environment of 25°C. In the charge-discharge tests, an initial charge-discharge cycle of two cycles starting with discharge was performed under the following conditions. For Examples 1 to 5 and Comparative Examples 1 to 4, the discharge current was 0.4 mA / cm. 2 The discharge termination voltage is 0.7V, constant current (CC) discharge is performed, and charging is performed with a charging current of 0.4mA / cm². 2 The charging termination voltage was 2.4V, and constant current (CC) charging was performed. Furthermore, the discharge in Reference Example 1 and Reference Example 2 was performed with a discharge current of 0.4mA / cm². 2 The discharge termination voltage is 1.0V, constant current (CC) discharge is performed, and charging is performed with a charging current of 0.4mA / cm². 2 The charging was performed using constant current (CC) charging with a charging termination voltage of 3.0V. The rest period between these discharge and charging cycles was set to 10 minutes.

[0089] Figure 3 shows the second charge-discharge curves for Examples 1 to 3, Comparative Example 1, and Comparative Example 2, Figure 4 shows the second charge curves for these, and Figure 5 shows the second discharge curves for these. Figure 6 shows the second charge-discharge curves for Example 2 and Comparative Example 3, and Figure 7 shows the second charge-discharge curves for Reference Example 1 and Reference Example 2. Table 1 shows the voltage difference (operating voltage difference) between the cell voltage at 50% DOD (Depth Of Discharge) during the second discharge and the cell voltage at 50% SOC (State Of Charge) during the second charge.

[0090] [Table 1]

[0091] As shown in Table 1 and Figures 3 to 6, Examples 1 to 5, in which the positive electrode active material layer contained a sulfur-carbon composite with an average pore diameter of 3.0 nm or less and an average particle size of 30.0 μm or less, showed lower cell voltages in the charging curve, higher cell voltages in the discharge curve, and smaller operating voltage differences compared to Comparative Examples 1 to 4, in which the average pore diameter of the carbon was greater than 3.0 nm or the average particle size was greater than 30.0 μm. From this, it can be seen that polarization is reduced when the positive electrode active material layer of an all-solid-state battery contains a sulfur-carbon composite with an average pore diameter of 3.0 nm or less and an average particle size of 30.0 μm or less. Furthermore, when compared with the charge-discharge curve of the all-solid-state battery shown in Figure 6, as shown in Figure 7, the difference in cell voltage between the charge-discharge curves of Reference Example 1, in which the average particle size of carbon in the sulfur-carbon composite contained in the positive electrode active material layer is 30.0 μm or less, and Reference Example 2, in which the average particle size of the carbon is greater than 30.0 μm, was found to be very small in the non-aqueous electrolyte battery. Also, as shown in Table 1, a comparison between Example 2, in which the average particle size of carbon in the sulfur-carbon composite contained in the positive electrode active material layer is 30.0 μm or less, and Reference Example 1, showed that Example 2, an all-solid-state battery, had a smaller operating voltage difference than Reference Example 1, a non-aqueous electrolyte battery. Therefore, it is considered that the sulfur-carbon composite can more fully exert its effect of reducing polarization in the form of a positive electrode active material in an all-solid-state battery.

[0092] The results above demonstrate that the all-solid-state electrochemical element exhibits excellent polarization reduction capabilities. [Explanation of symbols]

[0093] 1 positive electrode 2 negative electrode 3 isolation layer 4. Positive electrode substrate 5 Cathode active material layer 6 Negative electrode active material layer 7. Negative electrode substrate 10. All-solid-state electrochemical devices (all-solid-state batteries) 20 Energy storage units 30 Energy storage devices

Claims

1. It comprises a positive electrode active material layer, an isolation layer, and a negative electrode active material layer. The above positive electrode active material layer contains a sulfur-carbon composite, The above sulfur-carbon composite contains sulfur and porous carbon. The average pore size in the above carbon is 0.5 nm or more and 3.0 nm or less. An all-solid-state electrochemical element having an average particle size of 0.1 μm or more and 30.0 μm or less.

2. The all-solid-state electrochemical element according to claim 1, wherein the positive electrode active material layer comprises a sulfide solid electrolyte.

3. Containing sulfur and porous carbon, The average pore size in the above carbon is 0.5 nm or more and 3.0 nm or less. The average particle size is 0.1 μm or more and 30.0 μm or less. A sulfur-carbon composite material for use as a positive electrode active material in the positive electrode active material layer of an all-solid-state electrochemical device.

Citation Information

Patent Citations

  • Radiation position detector

    JP1988085486A

  • SOLID ELECTROLYTE FOR ALL-SOLID-STATE LITHIUM-SULFUR BATTERY INCLUDING Li2S-P2S5-SeS2 SERIES GLASS CERAMIC, POSITIVE ELECTRODE MATERIAL SUITABLE FOR SOLID ELECTROLYTE, MANUFACTURING METHOD THEREOF, AND ALL-SOLID-STATE LITHIUM-SULFUR BATTERY INCLUDING THESE

    JP2020031027A

  • Electrode material, lithium-sulfur battery electrode, lithium-sulfur battery and battery material production method

    WO2016009936A1