Method for manufacturing hot-rolled and annealed sheets for non-oriented electrical steel sheets, and method for manufacturing non-oriented electrical steel sheets.

A hot-rolled and annealed sheet for non-oriented electrical steel sheets with controlled compositions and processes addresses the challenge of fracture during cold rolling by effectively removing Fe-Al oxides, ensuring both magnetic properties and stability in the rolling process.

JP7948330B2Active Publication Date: 2026-11-11JFE STEEL CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024552680
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-08-30
Filing Date
2024-05-24
Publication Date
2026-11-11
Estimated Expiration
2044-05-24

AI Technical Summary

Technical Problem

Existing methods for manufacturing non-oriented electrical steel sheets fail to adequately prevent fracture during cold rolling while maintaining good magnetic properties, despite the addition of elements like Si and Al to improve iron loss characteristics.

Method used

A hot-rolled and annealed sheet for non-oriented electrical steel sheets with specific chemical compositions and manufacturing processes, including controlled heating and annealing temperatures, shot blasting, pickling with hydrochloric acid, and optional brush grinding, to effectively remove Fe-Al oxides and enhance fracture resistance.

Benefits of technology

The method enables the production of non-oriented electrical steel sheets with excellent magnetic properties and reduced fracture risk during cold rolling by thoroughly removing Fe-Al oxides, thereby stabilizing the rolling process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007948330000001
    Figure 0007948330000001
  • Figure 0007948330000002
    Figure 0007948330000002
  • Figure 0007948330000003
    Figure 0007948330000003
Patent Text Reader

Abstract

According to the present invention, a steel slab containing a predetermined amount of C, Si, Mn, P, S, Al, N, O, Sn, and Sb is heated under a predetermined condition, hot rolled, hot annealed, shot blasted and pickled, or the steel slab is heated under a predetermined condition, hot rolled, hot annealed, brush ground and pickled such that the average grain size in a cross section in the rolling direction of a steel sheet after the pickling is 40-250 μm and the integrated intensity of Fe-Al-based oxides in the surface layer of the steel sheet measured by X-ray diffraction is 200 cps∙degree or less, thereby obtaining a hot-rolled annealed sheet for a non-oriented electromagnetic steel sheet, which enables the prevention of sheet breakage during cold rolling and exhibits excellent magnetic properties after cold-rolled sheet annealing. In addition, a non-oriented electromagnetic steel sheet is manufactured using the hot-rolled annealed sheet.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to a hot-rolled annealed sheet for non-oriented electrical steel sheets that has excellent fracture resistance in cold rolling, a method for manufacturing the same, and a method for manufacturing non-oriented electrical steel sheets using the above-mentioned hot-rolled annealed sheet. [Background technology]

[0002] In recent years, with growing awareness of environmental issues, there has been a strong need to reduce CO2 emissions and conserve energy, and there is a strong demand for higher efficiency in electrical equipment, including electric vehicles. Therefore, there is a strong demand for improved iron loss characteristics in non-oriented electrical steel sheets, which are widely used as core materials for motors used in electrical equipment. To this end, iron loss has been improved by adding large amounts of elements that increase resistivity, such as Si and Al, or by reducing the thickness of the sheet. On the other hand, adding large amounts of Si or Al, or reducing the final sheet thickness, increases the manufacturing load during cold rolling. Therefore, in addition to improving magnetic properties, it is becoming increasingly important to prevent problems such as steel sheet fracture during cold rolling.

[0003] Therefore, to solve this problem, technologies have been proposed to suppress sheet fracture during cold rolling by controlling the annealing temperature of the hot-rolled sheet and improving its toughness.

[0004] For example, Patent Document 1 discloses a non-oriented electrical steel sheet containing, by mass%, C: 0.0010~0.0050%, Si: 2.5~4.0%, Al: 0.2~2.0%, Mn: 0.05~2.0%, P: 0.005~0.15%, S: 0.0001~0.0030%, Ti: 0.0005~0.0030%, and N: 0.0010~0.0030%, with the remainder being Fe and unavoidable impurities, with a base metal thickness of 0.10 mm to 0.35 mm, and satisfying the relationship shown in the following formula (1) regarding the Al concentration in the depth direction from the base metal surface. According to this explanation, if the soaking temperature during hot-rolled sheet annealing exceeds 1100°C, or if the soaking time exceeds 300 seconds, there is a possibility that the base metal may fracture during the subsequent cold rolling process. 0.1≦Al(x≦2μm) / Al(x=10μm)<1.0 (1) Here, in equation (1) above, x is the depth from the base metal surface [μm], Al(x≦2μm) is the average value of the Al concentration from the base metal surface to a depth of 2μm, and Al(x=10μm) is the Al concentration at a depth of 10μm. [Prior art documents] [Patent Documents]

[0005] [Patent Document 1] Japanese Patent Publication No. 2018-021241 [Overview of the project] [Problems that the invention aims to solve]

[0006] However, the prior art disclosed in the above-mentioned patent document has the following problems.

[0007] According to the inventors' investigation, it was found that controlling the hot-rolled sheet annealing conditions described in Patent Document 1 above is not necessarily sufficient to suppress fracture occurrence, and that it is difficult to achieve both fracture resistance during cold rolling and good magnetic properties after cold-rolled sheet annealing.

[0008] This invention has been made in view of the above problems, and aims to provide a hot-rolled annealed sheet for non-oriented electrical steel sheets that prevents fracture during cold rolling after hot-rolled sheet annealing and has excellent magnetic properties after cold-rolled sheet annealing, as well as to propose a method for manufacturing the same and a method for manufacturing non-oriented electrical steel sheets using the above hot-rolled annealed sheet. [Means for solving the problem]

[0009] The hot-rolled and annealed sheet for non-oriented electrical steel sheets according to the present invention, which advantageously solves the above problems, is constructed as follows. [1] A hot-rolled and annealed sheet for non-oriented electrical steel, having a composition by mass% of C: 0.0050% or less, Si: 2.0~5.0%, Mn: 0.2~2.0%, P: 0.030% or less, S: 0.0050% or less, Al: 0.25~2.50%, N: 0.0050% or less, O: 0.0050% or less, and Sn and Sb: 0.01~0.20% in total, with the remainder being Fe and unavoidable impurities, an average grain size of the cross-section in the rolling direction of the steel sheet of 40~250 μm, and an integrated intensity of Fe-Al oxide on the surface layer of the steel sheet measured by X-ray diffraction of 200 cps· degrees or less. [2] In addition to the above component composition in [1], the hot-rolled and annealed sheet for non-oriented electrical steel sheet further contains, by mass%, one or more components selected from groups A to D below. Group A: One or more elements selected from Ca, Mg, and REM, totaling 0.0010-0.0080% Group B: One or more elements selected from Cr, Mo, Cu, and Ni, totaling 0.01-0.60% • Group C: One or more elements selected from Ti, Nb, and V, totaling 0.0005-0.0030% ·Group D; B:0.0001~0.0020% [3] The hot-rolled and annealed sheet for non-oriented electrical steel sheets, characterized in that, in addition to the above component composition, it further contains, by mass%, one or more components selected from the following groups E to J. Group E; Zn: 0.001~0.010% Group F: One or more elements selected from Zr, Ta, W, and Se, totaling 0.001-0.010% • Group G: One or more species selected from Ga and Ge, totaling 0.0001 to 0.0200% • Group H: One or more selected from Pb and Bi, totaling 0.00005-0.0020% Group I; Co: 0.001~0.100% Group J; As: 0.0005~0.020%

[0010] The method for manufacturing a hot-rolled and annealed sheet for non-oriented electrical steel sheets according to the present invention, which advantageously solves the above problems, is configured as follows. [4] A hot rolling process in which a steel slab having a composition in mass%, C: 0.0050% or less, Si: 2.0~5.0%, Mn: 0.2~2.0%, P: 0.030% or less, S: 0.0050% or less, Al: 0.25~2.50%, N: 0.0050% or less, O: 0.0050% or less, Sn and Sb: 0.01~0.20% in total, with the remainder being Fe and unavoidable impurities, is heated and hot-rolled to produce a hot-rolled steel sheet, and the hot-rolled steel sheet is annealed. The process includes a hot-rolled sheet annealing process to produce a hot-rolled annealed sheet, a shot-blasting process to apply shot blasting to the hot-rolled annealed sheet, and a pickling process to pickle the shot-blasted hot-rolled annealed sheet. In the hot-rolling process, the heating temperature of the steel slab is set to 1150°C or lower, the finish rolling temperature to 960°C or lower, and the coiling temperature to 700°C or lower. In the hot-rolled sheet annealing process, the annealing temperature is set to 800°C or higher and 1100°C or lower. In the shot-blasting process, the projection density is set to 10-40 kg / m². 2 This is a method for manufacturing a hot-rolled annealed sheet for non-oriented electrical steel sheets, comprising applying shot blasting to the hot-rolled annealed sheet, and then pickling the shot-blasted steel sheet in the pickling process using hydrochloric acid with a concentration of 5% or more, a pickling temperature of 70°C or more, and a pickling time of 10 s to 120 s. [5] The method for producing a hot-rolled and annealed sheet for non-oriented electrical steel sheets is characterized in that, in addition to the above component composition, the steel slab further contains, by mass%, one or more components selected from groups A to D below. Group A: One or more elements selected from Ca, Mg, and REM, totaling 0.0010-0.0080% ·Group B; the total content of one or more elements selected from Cr, Mo, Cu and Ni is 0.01 to 0.60% ·Group C; the total content of one or more elements selected from Ti, Nb and V is 0.0005 to 0.0030% ·Group D; B: 0.0001 to 0.0020%, in the manufacturing method. [6] The method for manufacturing a hot-rolled annealed sheet for non-oriented electrical steel sheets according to the above [4] or [5], characterized in that the steel slab further contains, in mass%, one or more groups of components selected from the following Groups E to J in addition to the above component composition. ·Group E; Zn: 0.001 to 0.010% ·Group F; the total content of one or more elements selected from Zr, Ta, W and Se is 0.001 to 0.010% ·Group G; the total content of one or more elements selected from Ga and Ge is 0.0001 to 0.0200% ·Group H; the total content of one or more elements selected from Pb and Bi is 0.00005 to 0.0020% ·Group I; Co: 0.001 to 0.100% ·Group J; As: 0.0005 to 0.020% [7] The method for manufacturing a hot-rolled annealed sheet for non-oriented electrical steel sheets according to any one of the above [4] to [6], characterized in that before annealing the hot-rolled steel sheet, the hot-rolled steel sheet is subjected to rolling and / or tension bending working with an elongation rate of 0.1 to 10.0%. [8] The method for manufacturing a hot-rolled annealed sheet for non-oriented electrical steel sheets according to any one of the above [4] to [7], characterized in that after the pickling step, brush grinding is performed on the front and back surfaces of the pickled steel sheet.

[0011] The method for manufacturing a non-oriented electrical steel sheet according to the present invention, which advantageously solves the above problems, is configured as follows. [9] A method for manufacturing a non-oriented electrical steel sheet, wherein the hot-rolled annealed sheet obtained in any one of the above [4] to [8] is subjected to one cold rolling pass or two or more cold rolling passes including intermediate annealing to obtain a cold-rolled sheet of final thickness, and the cold-rolled sheet is annealed at a soaking temperature of 700 to 1100°C to obtain a cold-rolled annealed sheet.

[0012] Another method for manufacturing hot-rolled and annealed sheets for non-oriented electrical steel sheets according to the present invention, which advantageously solves the above problems, is configured as follows.

[10] A hot rolling process is performed to obtain a hot-rolled steel sheet by heating a steel slab having a composition in mass%, where C: 0.0050% or less, Si: 2.0~5.0%, Mn: 0.2~2.0%, P: 0.030% or less, S: 0.0050% or less, Al: 0.25~2.50%, N: 0.0050% or less, O: 0.0050% or less, Sn and Sb: 0.01~0.20% in total, with the remainder being Fe and unavoidable impurities; a hot rolling process is performed to obtain a hot-rolled steel sheet by annealing the hot-rolled steel sheet; and a hot-rolled sheet annealing process is performed to obtain a hot-rolled annealed sheet. The method for manufacturing a hot-rolled annealed sheet for non-oriented electrical steel includes a brush grinding step in which a blunt sheet is brush-ground, and a pickling step in which the brush-ground hot-rolled annealed sheet is pickled, wherein in the hot-rolling step the heating temperature of the steel slab is 1150°C or less, the finish rolling temperature is 960°C or less, and the winding temperature is 700°C or less; in the hot-rolled sheet annealing step the annealing temperature is 800°C or more and 1100°C or less; and in the pickling step the brush-ground steel sheet is pickled with hydrochloric acid concentration of 5% or more, pickling temperature of 70°C or more, and pickling time of 10 s to 120 s or less.

[11] In the above

[10] , the steel slab further contains, in addition to the above component composition, one or more components selected from groups A to D below in mass%, in a method for manufacturing a hot-rolled and annealed sheet for non-oriented electrical steel sheets. Group A: One or more elements selected from Ca, Mg, and REM, totaling 0.0010-0.0080% Group B: One or more elements selected from Cr, Mo, Cu, and Ni, totaling 0.01-0.60% • Group C: One or more elements selected from Ti, Nb, and V, totaling 0.0005-0.0030% • Group D; B: This is a manufacturing method with a yield of 0.0001 to 0.0020%.

[12] The method for producing a hot-rolled and annealed sheet for non-oriented electrical steel sheets, characterized in that the steel slab further contains, in addition to the above component composition, one or more components selected from the following groups E to J in mass percent. Group E; Zn: 0.001~0.010% Group F: One or more elements selected from Zr, Ta, W, and Se, totaling 0.001-0.010% • Group G: One or more species selected from Ga and Ge, totaling 0.0001 to 0.0200% • Group H: One or more selected from Pb and Bi, totaling 0.00005-0.0020% Group I; Co: 0.001~0.100% Group J; As: 0.0005~0.020%

[13] A method for manufacturing a hot-rolled annealed sheet for non-oriented electrical steel sheets, characterized in that, in any one of

[10] to

[12] above, the hot-rolled steel sheet is subjected to rolling and / or tensile bending with an elongation ratio of 0.1 to 10.0% before annealing.

[14] A method for manufacturing a hot-rolled annealed sheet for non-oriented electrical steel sheet, characterized in that, in any one of the above

[10] to

[13] , brush grinding is performed on the front and back surfaces of the pickled steel sheet after the pickling step.

[0013] Another method for manufacturing non-oriented electrical steel sheets according to the present invention, which advantageously solves the above problems, is configured as follows.

[15] A method for manufacturing non-oriented electrical steel sheets, in which a hot-rolled annealed sheet obtained in any one of

[10] to

[14] above is subjected to one cold-rolling or two or more cold-rolling including intermediate annealing to obtain a cold-rolled sheet of the final thickness, and the cold-rolled sheet is annealed at a soaking temperature of 700 to 1100°C to obtain a cold-rolled annealed sheet. [Effects of the Invention]

[0014] According to the present invention, it is possible to efficiently manufacture non-oriented electrical steel sheets with excellent magnetic properties while suppressing fracture of steel sheets during cold rolling. [Modes for carrying out the invention]

[0015] The inventors diligently investigated the causes of sheet fracture during cold rolling. As a result, they found that in steel sheets with large amounts of Si and Al added, as in the present invention, not only iron oxides but also Si and Al oxides are formed on the surface of the steel sheet during hot rolling or hot-rolled sheet annealing. In particular, Fe-Al scale is densely formed near the interface between the base metal and the oxide layer. Since this Fe-Al scale is poorly soluble in acid, they found that if it cannot be completely removed in the pickling process, it accelerates the wear of the rolling rolls during cold rolling, making the steel sheet more prone to fracture. To solve this problem, they investigated the mechanical and chemical conditions related to scale removal and found appropriate conditions that can stably remove scale including Fe-Al scale, leading to the development of the present invention.

[0016] The following describes the hot-rolled and annealed sheet for non-oriented electrical steel sheets according to this embodiment. First, the component composition of the hot-rolled and annealed sheet for non-oriented electrical steel sheets according to this embodiment and the reasons for its limitation will be explained. In the following description, unless otherwise specified, the notation "%" means "mass%". <Hot-rolled and annealed sheet for non-oriented electrical steel sheets> The hot-rolled and annealed sheet for non-oriented electrical steel sheets according to this embodiment has a composition by mass% containing C: 0.0050% or less, Si: 2.0~5.0%, Mn: 0.2~2.0% or less, P: 0.030% or less, S: 0.0050% or less, Al: 0.25~2.50% or less, N: 0.0050% or less, O: 0.0050% or less, and Sn and Sb: one or more types totaling 0.01~0.20%, with the remainder being Fe and unavoidable impurities.

[0017] C: 0.0050% or less Carbon (C) is an element that forms carbides, degrading iron loss after finish annealing. Furthermore, C increases the hardness of hot-rolled annealed sheets, inducing sheet fracture during cold rolling. Therefore, the C content should be 0.0050% or less. A preferred C content is 0.0030% or less. While there is no specific lower limit for the C content, it is preferable to have a C content of 0.0010% or more from the viewpoint of improving the toughness of hot-rolled annealed sheets and preventing sheet fracture during cold rolling.

[0018] Si: 2.0~5.0% Si has the effect of increasing the resistivity of steel and reducing iron loss after finish annealing, so its content should be 2.0% or more. Preferably, it should be 2.7% or more. On the other hand, if the Si content exceeds 5.0%, the hot-rolled and annealed sheet becomes excessively hardened and brittle, making it prone to fracture during cold rolling, so the upper limit should be 5.0%. Preferably, it should be 4.5% or less.

[0019] Mn: 0.2~2.0% Like Si, manganese (Mn) is a useful element for reducing iron loss and also improves the toughness of the base metal, suppressing plate fracture during cold rolling. Therefore, the Mn content should be 0.2% or higher, preferably 0.35% or higher. On the other hand, if the Mn content exceeds 2.0%, the hot-rolled and annealed plate becomes excessively hardened and prone to fracture during cold rolling, so it should be kept below 2.0%.

[0020] P:0.030% or less P has the effect of increasing the strength of steel and can be used for strength adjustment. On the other hand, if the P content exceeds 0.030%, the steel becomes brittle, leading to a decrease in manufacturability. Therefore, the P content should be 0.030% or less. From the viewpoint of preventing brittleness, a preferable P content is 0.015% or less. Although there is no specific lower limit for the P content, from the viewpoint of reducing the load of P removal, it is preferable to set it at around 0.004%.

[0021] S: 0.0050% or less S segregates at grain boundaries, embrittles hot-rolled and annealed sheets, making them more prone to fracture during cold rolling. Furthermore, it forms fine sulfides, degrading iron loss after finish annealing. Therefore, the upper limit of S content should be 0.0050%. A preferred S content is 0.0025% or less. While there is no specific lower limit for S content, a lower limit of around 0.001% is preferable from the viewpoint of reducing the desulfurization load.

[0022] Al: 0.25~2.50% Al, like Si, increases the resistivity of steel sheets and reduces iron loss after finish annealing; therefore, the Al content should be 0.25% or more. In addition, Al forms AlN, which reduces the average grain size of hot-rolled and annealed sheets through a pinning effect, improving fracture resistance during cold rolling. For this reason, it is preferable that the Al content be 0.50% or more, and more preferably 0.70% or more. On the other hand, if the Al content exceeds 2.50%, a large amount of Fe-Al oxides will be produced in the scale generated during hot rolling and hot-rolled sheet annealing, and these cannot be completely removed in the pickling process, becoming a cause of sheet fracture during cold rolling. For this reason, the upper limit of Al is 2.50%, preferably 2.30% or less.

[0023] N: 0.0050% or less Since nitrogen (N) can form nitrides, which can be the starting point for sheet fracture during cold rolling, the upper limit for N content should be 0.0050%. Furthermore, because fine nitrides inhibit grain growth and degrade iron loss after finish annealing, a preferable N content is 0.0035% or less.

[0024] O: 0.0050% or less Since oxygen (O) can form oxides that can become the starting point for plate fracture during cold rolling, the upper limit for O content should be 0.0050%. Furthermore, because the formed oxides inhibit grain growth in the ferrite structure and degrade iron loss after finish annealing, the preferred O content is 0.0025% or less.

[0025] Sn and Sb: One or more types totaling 0.01-0.20% In addition to improving magnetic properties by improving the texture after cold rolling and finish annealing, Sn and Sb also have the effect of improving fracture resistance during cold rolling by suppressing the formation of Fe-Al oxides through surface segregation. For this reason, the total content of Sn and Sb should be 0.01% or more, preferably 0.02% or more. On the other hand, excessive addition not only saturates the effect but also deteriorates the toughness of the hot-rolled and annealed sheet, making it more prone to fracture during cold rolling. Therefore, the upper limit for the total content of Sn and Sb should be 0.20%.

[0026] The above describes the basic components of the hot-rolled and annealed sheet for non-oriented electrical steel sheets according to this embodiment. Furthermore, in order to improve various properties, it is preferable to include at least one group of components selected from groups A to D below.

[0027] Group A: One or more elements selected from Ca, Mg, and REM, totaling 0.0010-0.0080% Ca, Mg, and REM have the effect of fixing S as sulfides and improving iron loss. For this reason, it is preferable that the total content of one or more of Ca, Mg, and REM be 0.0010% or more. More preferably, it is 0.0020% or more. On the other hand, if the total content of Ca, Mg, and REM exceeds 0.0080%, inclusions are excessively generated and the manufacturability decreases, so the upper limit is set at 0.0080%. The preferred total content of Ca, Mg, and REM is 0.0060% or less.

[0028] Group B: One or more elements selected from Cr, Mo, Cu, and Ni, totaling 0.01-0.60% Cr, Mo, Cu, and Ni have the effect of increasing the resistivity of steel and improving iron loss. For this reason, it is preferable that the total content of one or more of Cr, Mo, Cu, and Ni be 0.01% or more. On the other hand, if added in excess, it hardens the hot-rolled and annealed sheet, making it more prone to fracture during cold rolling, so it is preferable that the upper limit of the total content be 0.40%.

[0029] Group C; one or more elements selected from Ti, Nb, and V, totaling 0.0005-0.0030% Ti, Nb, and V have the effect of refining the microstructure of hot-rolled and annealed sheets, improving toughness, and suppressing sheet fracture during cold rolling. For this reason, the total content of Ti, Nb, and V is preferably 0.0005% or more. On the other hand, if added in excess, a large amount of fine precipitates will be generated, significantly inhibiting grain growth, so the upper limit of the total content of Ti, Nb, and V is preferably 0.0030%.

[0030] Group D; B:0.0001~0.0020% B segregates at grain boundaries, improving toughness and suppressing plate fracture during cold rolling. For this reason, the B content is preferably 0.0001% or more, and more preferably 0.0003% or more. On the other hand, if the B content exceeds 0.0020%, iron borides are formed, eliminating the toughness-improving effect, so the upper limit is preferably 0.0020%.

[0031] Furthermore, in order to improve various properties, it is preferable to include at least one component selected from groups E to J below.

[0032] Group E; Zn: 0.001~0.010% Zn has the effect of improving iron loss in finish annealed plates by coarsening inclusions and promoting grain growth during finish annealing. For this reason, it is preferable that the Zn content be 0.001% or more. On the other hand, even if the Zn content exceeds 0.010%, the above effect saturates, so it is preferable that the upper limit be 0.010%.

[0033] Group F: One or more elements selected from Zr, Ta, W, and Se, totaling 0.001-0.010% Zr, Ta, W, and Se form precipitates that reduce the grain size of the hot-rolled and annealed sheet, thereby contributing to improved cold-rollability. For this reason, it is preferable to contain at least 0.001% in total of one or more elements selected from Zr, Ta, W, and Se. On the other hand, if the total content exceeds 0.010%, the iron loss of the finish-annealed sheet may deteriorate, so it is preferable to set the upper limit at 0.010%.

[0034] Group G; one or more elements selected from Ga and Ge, totaling 0.0001 to 0.0200% Ga and Ge have the effect of improving the texture of the finished annealed sheet and thereby enhancing its magnetic properties. For this reason, it is preferable to contain at least 0.0001% in total of one or more of Ga and Ge. On the other hand, the above effect saturates if the content exceeds 0.0200%, so it is preferable to set the upper limit to 0.0200%.

[0035] Group H; one or more selected from Pb and Bi, totaling 0.00005-0.0020% Pb and Bi are effective in improving the cold-rollability of hot-rolled and annealed sheets by reducing the grain size. For this reason, it is preferable to contain at least 0.00005% in total of one or more elements selected from Pb and Bi. On the other hand, if the content exceeds 0.0020%, the iron loss of the finish-annealed sheet deteriorates, so it is preferable to set the upper limit at 0.0020%.

[0036] Group I; Co: 0.001~0.100% Co has the effect of improving magnetic flux density. For this reason, it is preferable to contain 0.001% or more. On the other hand, if the content exceeds 0.100%, precipitates will form and the iron loss of the finished annealed plate will deteriorate, so it is preferable to set the upper limit to 0.100%.

[0037] Group J; As: 0.0005~0.020% As segregates at grain boundaries, reducing the grain size of hot-rolled and annealed sheets, which is effective in improving cold-rollability. For this reason, it is preferable to contain 0.0005% or more. On the other hand, if the content exceeds 0.020%, it promotes grain boundary fracture and actually reduces cold-rollability, so it is preferable to set the upper limit at 0.020%.

[0038] The chemical composition of the hot-rolled and annealed sheet for non-oriented electrical steel sheets according to this embodiment is, with the remainder being Fe and unavoidable impurities, in addition to the elements mentioned above.

[0039] <Steel structure of hot-rolled and annealed sheets for non-oriented electrical steel sheets> Next, the microstructure of the hot-rolled and annealed sheet for non-oriented electrical steel sheets according to this embodiment will be described. Average grain size of steel sheet in the rolling direction cross-section: 40-250 μm If the microstructure of the hot-rolled and annealed sheet is coarse, the sheet becomes brittle and prone to fracture during cold rolling. Therefore, the average grain size should be 250 μm or less. From the viewpoint of suppressing fracture, it is preferably 180 μm or less, and more preferably 120 μm or less. On the other hand, if the average grain size is less than 40 μm, the hot-rolled and annealed sheet hardens, increasing the load during cold rolling and making the sheet more prone to fracture. Therefore, it is necessary to have an average grain size of 40 μm or more. A preferred average grain size is 60 μm or more.

[0040] Integrated intensity of Fe-Al oxides on the surface of steel plate: 200 cps·° or less Fe-Al oxides are hard and have poor wettability with lubricating oil. If they remain on the surface of steel sheets, they can damage the rolling rolls during cold rolling, increasing the coefficient of friction and rolling load, making rolling unstable and potentially leading to sheet fracture. Therefore, Fe-Al oxides must be thoroughly removed during the pickling process. As an indicator, the integrated intensity of Fe-Al oxides on the surface of hot-rolled and annealed steel sheets measured by X-ray diffraction after pickling should be 200 cps·° or less.

[0041] <Method for manufacturing hot-rolled and annealed sheets for non-oriented electrical steel sheets> Next, a method for manufacturing a hot-rolled and annealed sheet for non-oriented electrical steel sheets according to this embodiment will be described.

[0042] The method for manufacturing a hot-rolled annealed sheet for non-oriented electrical steel sheets according to this embodiment includes a hot-rolling step of heating and hot-rolling a steel slab having the above-mentioned component composition to form a hot-rolled steel sheet, a hot-rolled sheet annealing step of annealing the hot-rolled steel sheet to form a hot-rolled annealed sheet, a shot-blasting step of applying shot blasting to the hot-rolled annealed sheet, and a pickling step of pickling the shot-blasted hot-rolled annealed sheet. In the hot-rolling step, the heating temperature of the steel slab is 1150°C or less, the finish rolling temperature is 960°C or less, and the coiling temperature is 700°C or less. In the hot-rolled sheet annealing step, the annealing temperature is 800°C or more and 1100°C or less, and in the shot-blasting step, the projection density is 10 to 40 kg / m 2 Shot blasting is applied to the hot-rolled annealed sheet metal. Next, in the pickling process, the shot-blasted steel sheet metal is pickled with hydrochloric acid at a concentration of 5% or more, a pickling temperature of 70°C or more, and a pickling time of 10 s to 120 s. I will explain this in detail below.

[0043] [Hot rolling process] Steel slab The composition of the steel slab used in the production of the hot-rolled and annealed sheet for non-oriented electrical steel sheets in this embodiment is adjusted to the range described above. The method of melting the steel can be any known refining process such as a converter, electric furnace, or vacuum degassing device, and is not particularly limited. Furthermore, continuous casting is preferred as the manufacturing method for the steel slab. Iron scrap or directly reduced iron may also be used as raw materials. Iron scrap is particularly preferable because it allows for the inexpensive incorporation of elements useful for reducing iron loss, such as Cu and Ni.

[0044] Heating temperature: 1150℃ or less Hot rolling is a process in which, after manufacturing a steel slab having the above components, it is immediately hot-rolled, or cooled and then heated to a predetermined temperature before hot-rolling, to obtain a hot-rolled sheet of a predetermined thickness. If the heating temperature of the slab is too high, AlN and MnS will remelt and precipitate finely in subsequent processes, degrading grain growth and iron loss; therefore, the upper limit is set at 1150°C. To coarseen the AlN and MnS in the steel slab and improve grain growth and iron loss, it is preferable to heat it to 1000°C or higher. Furthermore, from the viewpoint of stable manufacturing by reducing the hot rolling load, 1050°C or higher is even more preferable.

[0045] Finishing rolling temperature: 960℃ or less If the finish rolling temperature in hot rolling exceeds 960°C, the scale on the hot-rolled sheet becomes thicker, reducing its pickling properties. Therefore, the finish rolling temperature should be 960°C or lower. A preferred finish rolling temperature is 920°C or lower. On the other hand, if the finish rolling temperature is too low, the rolling load increases and the rolling pressure becomes larger. Therefore, the lower limit is preferably 750°C. More preferably, it is 780°C or higher.

[0046] Winding temperature: 700℃ or less If the winding temperature exceeds 700°C, the scale increases, and in particular the Fe-Al oxide becomes thicker, reducing pickling properties, so the upper limit should be 700°C. Preferably, it should be 620°C or lower. On the other hand, if the winding temperature is too low, the rapid cooling between the completion of hot rolling and winding will cause large temperature variations, so it is preferable to set the lower limit at 450°C. From the viewpoint of reducing iron loss by coarsening the precipitates during winding, a preferred winding temperature is 480°C or higher.

[0047] [Hot-rolled sheet annealing process] Hot-rolled sheet annealing temperature: 800~1100℃ Hot-rolled sheet annealing is performed to improve fracture resistance during cold rolling and to improve magnetic properties after cold rolling and finish annealing, by homogenizing the microstructure and controlling the ferrite grain size within a predetermined range. If the annealing temperature of the hot-rolled sheet is higher than 1100°C, the microstructure becomes too coarse, reducing toughness and making the sheet more prone to fracture during cold rolling. Therefore, it is necessary to keep the temperature below 1100°C. A preferred annealing temperature for hot-rolled sheets is 1030°C or lower. Furthermore, from the viewpoint of suppressing scale growth during hot-rolled sheet annealing, it is preferable to keep the temperature below 960°C. On the other hand, if the hot-rolled sheet annealing temperature is lower than 800°C, the grain size will not increase sufficiently, and the magnetic properties after finish annealing will deteriorate; therefore, it is necessary to set the temperature at 800°C or higher. The preferred hot-rolled sheet annealing temperature is 900°C or higher. There is no specific annealing time, but from the viewpoint of ensuring uniformity, it is preferable to set it to 10 seconds or more.

[0048] [Shot blasting process] Shot blast projection density: 10-40 kg / m 2 Shot blasting the hot-rolled annealed sheet metal before pickling introduces cracks in the scale, which accelerates scale removal during pickling. Fe-Al scale, in particular, is poorly soluble in acid, so it is necessary to introduce cracks to expose the base metal, allowing the acid to penetrate and dissolve it from the base metal side of the base metal interface. The required shot blasting density for this purpose is 10 kg / m³. 2 That is all. Preferably 15 kg / m 2 That's all. On the other hand, 40 kg / m 2 If it exceeds this, not only will cracks be introduced into the scale, but the area near the surface of the base metal will also be deformed, becoming the starting point for plate fracture during cold rolling. Therefore, the projection density should be 40 kg / m³. 2 The following applies: The preferred projection density is 35 kg / m³. 2 The following applies:

[0049] If the particle size of the shot blast particles is large, the number of impacts per unit area decreases even at the same projection density, meaning the number of cracks introduced into the scale decreases and the pickling effect deteriorates. Therefore, the average particle size of the shot blast particles is preferably 0.50 mm or less. From the viewpoint of promoting pickling effect, 0.30 mm or less is more preferable. Conversely, if the particle size is too small, the crack introduction effect weakens, so the average particle size of the shot blast particles is preferably 0.15 mm or more. The average particle size of the shot blast particles can be measured, for example, by particle size analysis - laser diffraction and scattering method described in JIS Z 8825:2013. Also, if the shot blast particles are soft, the shot blast particles themselves deform when they collide with the steel plate, making it impossible to efficiently introduce cracks into the scale. Therefore, the Vickers hardness of the shot blast particles is preferably 400 HV or higher.

[0050] [Brush grinding process (before pickling)] Instead of shot blasting, brush grinding can be performed on hot-rolled, annealed plates before pickling to introduce cracks into the scale, thereby accelerating scale removal during pickling. To grind the steel plate surface evenly, it is preferable to use a brush roll for brush grinding. The brush material and grinding conditions can be selected as appropriate, but from the viewpoint of even grinding that follows the shape of the steel plate, it is preferable to use synthetic fibers that are softer than metal for the brush bristles. Furthermore, from the viewpoint of efficiently introducing cracks into the scale, it is preferable that the brush contains abrasive grains such as alumina, silicon carbide, or diamond. During brush grinding, it is preferable to spray cooling water to remove grinding powder and prevent overheating of the brush.

[0051] [Pickling process] Pickling: Hydrochloric acid concentration 5% or more, pickling temperature 70℃ or more, pickling time 10s or more, 120s or less The pickling process removes scale from hot-rolled and annealed sheets that have undergone the shot-blasting or brush grinding described above. By thoroughly removing not only iron oxides but also Fe-Al-based scale, sheet fracture during cold rolling can be suppressed. For this reason, the hydrochloric acid concentration should be 5% or higher, preferably 8% or higher. There is no particular upper limit, but since over-pickling may occur, it is preferable to keep the hydrochloric acid concentration at 20% or lower. To promote pickling, the temperature of the pickling solution (pickling temperature) should be 70°C or higher, preferably 75°C or higher. If the pickling temperature is too high, over-pickling is more likely to occur, and the amount of evaporation of the pickling solution increases, increasing manufacturing costs, so it is preferable to keep it at 96°C or lower. To ensure sufficient pickling, the pickling time should be 10 seconds or longer, preferably 15 seconds or longer. If it exceeds 120 seconds, the amount of hydrogen generated increases, and hydrogen embrittlement makes the sheet more prone to fracture during cold rolling, so the upper limit of the pickling time should be 120 seconds. As mentioned above, the pickling properties change depending on the Al content, hot rolling temperature, and winding temperature, so the pickling solution may be adjusted by adding pickling accelerators or pickling inhibitors as needed.

[0052] Furthermore, in the present invention, from the viewpoint of completely removing Fe-Al-based scale, it is preferable to add the following steps to the descaling process described above. Rolling and / or tensile bending process with an elongation rate of 0.1-10.0% before the hot-rolled sheet annealing process. By introducing cracks into the scale, particularly the Fe-Al scale, at the hot-rolled sheet stage, and exposing the base metal, the oxidation behavior during annealing of the hot-rolled sheet changes. Specifically, iron oxides that are relatively easily soluble in acid are formed in the areas where the base metal is exposed. During pickling, these iron oxides dissolve, which then become the starting point for the dissolution of the base metal, allowing the Fe-Al scale to be removed. Therefore, it is preferable to stretch the hot-rolled sheet by light rolling and / or tensile bending. It is preferable to perform a process on the hot-rolled sheet before hot-rolling and annealing that elongates it to an elongation rate of 0.1% or more using a skin pass rolling mill or tension leveler. Preferably, the elongation rate is 0.3% or more. If it exceeds 10.0%, not only will the above effects saturate, but the average grain size of the hot-rolled and annealed sheet will become too large due to strain-induced grain growth, so it is preferable to keep the elongation rate at 10.0% or less. More preferably, it is 6.0% or less. When rolling and / or tensile bending with an elongation rate of 0.1 to 10.0% is performed before annealing the hot-rolled sheet, it is preferable to perform the above process so that the integrated strength of the hot-rolled and annealed sheet after pickling is 150 cps·degree or less.

[0053] [Brush grinding process (after pickling)] It is preferable to brush grind the front and back surfaces of the steel plate after pickling to mechanically remove any Fe-Al scale that remained during pickling. To remove all scale, including Fe-Al scale, by brush grinding alone would require a large-scale device, resulting in high initial and maintenance costs. Therefore, by removing most of the scale through pickling and then removing only the remaining Fe-Al scale with brush grinding, equipment costs can be reduced. To grind the steel plate surface evenly, it is preferable to use a brush roll for brush grinding. The brush material and grinding conditions can be selected as appropriate, but from the viewpoint of grinding evenly while following the shape of the steel plate, it is preferable to use synthetic fibers that are softer than metal for the brush bristles, and from the viewpoint of efficiently removing Fe-Al scale, it is preferable that the brush contains abrasive grains such as alumina, silicon carbide, or diamond. During brush grinding, it is preferable to spray cooling water to remove grinding powder and prevent overheating of the brush. Furthermore, when brush grinding is performed on both the front and back surfaces of the steel plate after pickling, it is preferable to perform the brush grinding so that the integrated strength of the hot-rolled and annealed plate after brush grinding is 60 cps· degrees or less.

[0054] Next, a method for producing non-oriented electrical steel sheets from hot-rolled and annealed sheets obtained by the manufacturing method of the present invention described above will be explained. [Cold rolling process] The above-mentioned pickled, hot-rolled, annealed sheet is preferably cold-rolled once or twice or more, including intermediate annealing, to obtain a cold-rolled sheet of the final thickness. From the viewpoint of production efficiency, it is preferable to use a tandem rolling mill, but a reverse rolling mill may also be used, and rolling should be done by conventional methods.

[0055] [Finishing annealing process] Finish annealing temperature: 700~1100℃ The finish annealing process after cold rolling described above is a process to recrystallize and grow grains in the cold-rolled sheet to obtain good magnetic properties. The soaking temperature in the finish annealing is preferably 700°C or higher. More preferably 800°C or higher. On the other hand, if the soaking temperature in the finish annealing is too high, nitriding may occur during annealing, or the crystal grains may become too coarse, leading to deterioration of iron loss. Therefore, it is preferable to set the temperature at 1100°C or lower. More preferably 1050°C or lower. [Examples]

[0056] Embodiments of the present invention will be further described by reference to examples. However, the present invention is not limited to the manufacturing conditions and product performance shown in the following examples. Within the scope of the present invention, the desired performance can be achieved in the embodiments.

[0057] (Example 1) Steel containing the various components shown in Table 1, with the remainder being Fe and unavoidable impurities, was melted using a conventional refining process and then cast into slabs using a continuous casting method. Next, these slabs were heated in a gas furnace under the conditions shown in Tables 2-1 and 2-2, and then hot-rolled, consisting of rough rolling and finish rolling, to obtain hot-rolled sheets with a thickness of 1.8 mm and a width of 1200 mm. Subsequently, the hot-rolled sheets were annealed and then pickled to obtain hot-rolled annealed sheets. In this process, some of the hot-rolled sheets were subjected to either light rolling before hot-rolled annealing using a skin-pass rolling mill, or brush grinding after pickling, or both. For brush grinding, a silicon carbide-based brush roll was used, with nylon bristles and silicon carbide-based abrasive grains. The elongation rate (%) during light rolling before hot rolling and annealing, and the torque (N·m) and rotational speed (rpm) during grinding with brush rolls after pickling are shown in Tables 2-1 and 2-2.

[0058] steel plate structure A sample was cut from the obtained hot-rolled and annealed sheet so that the thickness cross-section in the rolling direction could be observed. The sample was then embedded, polished, and etched to reveal the microstructure, and the steel sheet microstructure was observed. The average grain size was calculated from the captured microstructure photographs using image analysis. Here, the average grain size was defined as the equivalent diameter of a circle.

[0059] Integrated intensity of oxides A sample measuring 25 x 30 mm (thickness) was cut from the obtained hot-rolled and annealed sheet, and the amount of remaining scale on the steel sheet surface was measured by X-ray diffraction. The measurement was performed with an incident X-ray angle of 1 degree, and the integrated intensity of the (311) plane peak of Fe-Al oxide (hersinite, FeAl2O4) appearing at 2θ = approximately 36.4 degrees was calculated.

[0060] Fracture resistance in cold rolling The obtained hot-rolled and annealed sheets were rolled in a tandem cold-rolling mill to a finished thickness of 0.25 mm, with a feed speed of 600 m / min at the exit of the final stand, excluding the transient section near the weld, for a total length of 8000 m. Sheets that fractured once or more were marked with ×, those that did not fracture were marked with ○, and those that did not fracture and showed small load fluctuations at the first stand were marked with ◎. Here, the small load variation means that the average value of the rolling load at #1stand when rolling at 600m / min with a tandem rolling mill is defined as L ave , and when the difference between the maximum value and the minimum value of the above rolling load is defined as ΔL, the ratio ΔL / L between the average value L of the above rolling load ave and the difference ΔL between the maximum value and the minimum value ave ×100 is 10% or less.

[0061] Iron loss W of the finish-annealed sheet 10 / 400 The above cold-rolled sheet was subjected to finish annealing under the conditions shown in Table 2-1 and Table 2-2. The soaking time was set to 10s. From the obtained finish-annealed sheet, test pieces with a width of 30mm and a length of 280mm were taken from the L direction (rolling direction) and the C direction (direction perpendicular to the rolling direction), and the iron loss W was measured in accordance with JIS C2550-1 10 / 400 .

[0062] The above measurement results are also shown in Table 2-1 and Table 2-2. From these results, it is understood that by controlling the manufacturing conditions of the steel sheet within the scope of the present invention, a hot-rolled annealed sheet for non-oriented electrical steel sheets that achieves both prevention of fracture during cold rolling after hot-rolled sheet annealing and excellent magnetic properties after cold-rolled sheet annealing can be obtained.

[0063] [Table 1]

[0064] [Table 2-1]

[0065] [Table 2-2]

[0066] (Example 2) The slab produced in Example 1, having a composition consisting of various components shown in Table 1, with the remainder being Fe and unavoidable impurities, was heated in a gas furnace under the conditions shown in Tables 3-1 and 3-2. After heating, it was hot-rolled, consisting of rough rolling and finish rolling, to obtain a hot-rolled sheet with a thickness of 1.8 mm and a width of 1200 mm. Subsequently, the hot-rolled sheet was annealed, brush-ground, and then pickled to obtain a hot-rolled annealed sheet. In this process, some of the hot-rolled sheets were subjected to either light rolling before hot-rolling annealing using a skin-pass rolling mill, or brush grinding after pickling, or both. For brush grinding, a silicon carbide-based brush roll with nylon bristles and silicon carbide-based abrasive grains was used. The elongation rate (%) of lightly rolled material before hot rolling and annealing, the torque (N·m) and rotational speed (rpm) during grinding with brush rolls before pickling, and the torque (N·m) and rotational speed (rpm) during grinding with brush rolls after pickling are shown in Tables 3-1 and 3-2.

[0067] steel plate structure A sample was cut from the obtained hot-rolled and annealed sheet so that the thickness cross-section in the rolling direction could be observed. The sample was then embedded, polished, and etched to reveal the microstructure, and the steel sheet microstructure was observed. The average grain size was calculated from the captured microstructure photographs using image analysis. Here, the average grain size was defined as the equivalent diameter of a circle.

[0068] Integrated intensity of oxides A sample measuring 25 x 30 mm (thickness) was cut from the obtained hot-rolled and annealed sheet, and the amount of remaining scale on the steel sheet surface was measured by X-ray diffraction. The measurement was performed with an incident X-ray angle of 1 degree, and the integrated intensity of the (311) plane peak of Fe-Al oxide (hersinite, FeAl2O4) appearing at 2θ = approximately 36.4 degrees was calculated.

[0069] Fracture resistance in cold rolling The obtained hot-rolled and annealed sheets were rolled in a tandem cold-rolling mill to a finished thickness of 0.25 mm, with a feed speed of 600 m / min at the exit of the final stand, excluding the transient section near the weld, for a total length of 8000 m. Sheets that fractured once or more were marked with ×, those that did not fracture were marked with ○, and those that did not fracture and showed small load fluctuations at the first stand were marked with ◎. Here, "small load fluctuation" means that the average value of the rolling load of #1std when rolling at 600 m / min in a tandem rolling mill is L. ave When the difference between the maximum and minimum values ​​of the above rolling load is ΔL, the average value L of the above rolling load ave The ratio of the difference between the maximum and minimum values ​​ΔL to ΔL / L ave This means that the result of multiplying by 100 is 10% or less.

[0070] Iron loss W of finished annealed plate 10 / 400 The cold-rolled sheets described above were subjected to finish annealing under the conditions shown in Tables 3-1 and 3-2. The soaking time was 10 s. From the resulting finish-annealed sheets, test specimens measuring 30 mm in width and 280 mm in length were taken from the L direction (rolling direction) and the C direction (direction perpendicular to the rolling direction), and the iron loss W was measured in accordance with JIS C2550-1. 10 / 400 We measured it.

[0071] The above measurement results are shown together in Tables 3-1 and 3-2. From these results, it can be seen that by controlling the steel sheet manufacturing conditions within the scope of the present invention, a hot-rolled annealed sheet for non-oriented electrical steel can be obtained that achieves both prevention of fracture during cold rolling after hot-rolled sheet annealing and excellent magnetic properties after cold-rolled sheet annealing.

[0072] [Table 3-1]

[0073] [Table 3-2]

Claims

1. In mass%, C: 0.0050% or less, Si: 2.0 to 5.0%, Mn: 0.2-2.0%, P: 0.030% or less, S: 0.0050% or less, Al: 0.25-2.50%, N: 0.0050% or less, O: 0.0050% or less, and It contains 0.01 to 0.20% in total of one or both selected from Sn and Sb. It contains at least one component selected from groups A to J below, A hot rolling process involves heating a steel slab having a composition consisting of Fe and unavoidable impurities, and hot rolling it to produce a hot-rolled steel sheet. The process involves annealing the aforementioned hot-rolled steel sheet to obtain a hot-rolled annealed sheet, A shot blasting process in which the hot-rolled annealed plate is subjected to shot blasting, The process includes a pickling step of pickling the shot-blasted hot-rolled annealed sheet, In the hot rolling process, the heating temperature of the steel slab is set to 1150°C or lower, the finish rolling temperature to 960°C or lower, and the winding temperature to 700°C or lower. In the aforementioned hot-rolled sheet annealing process, the annealing temperature is set to 800°C or higher and 1100°C or lower. In the aforementioned shot blasting process, the projection density is 10 to 40 kg / m³. 2 Shot blasting is performed on the hot-rolled annealed plate, the average particle size of the shot blast particles is set to 0.15 mm or more and 0.50 mm or less, and the Vickers hardness of the shot blast particles is set to 400 HV or more. In the aforementioned pickling process, the shot-blasted steel plate is pickled with hydrochloric acid at a concentration of 5% or more, a pickling temperature of 70°C or more, and a pickling time of 10 s to 120 s. The average grain size of the steel sheet in the rolling direction cross-section is set to be in the range of 40 to 250 μm. The integrated intensity of Fe-Al oxides on the surface of the steel plate, as measured by X-ray diffraction, is set to 200 cps·degrees or less. Herein, the integrated intensity of Fe-Al oxides on the surface of the steel sheet measured by X-ray diffraction is calculated by taking the X-ray incident angle of 1 degree with respect to the steel sheet surface and determining the integrated intensity of the (311) plane peak of Fe-Al oxides (Hershinite, FeAl₂O₄) that appears around 2θ = 36.4 degrees, in a method for manufacturing hot-rolled and annealed sheets for non-oriented electrical steel sheets. Group A: At least one selected from Ca, Mg, and REM in total amount of 0.0010 to 0.0080%. Group B: At least one element selected from Cr, Mo, Cu, and Ni, totaling 0.01 to 0.60%. Group C: At least one selected from Ti, Nb, and V, totaling 0.0005 to 0.0030%. ・Group D; B: 0.0001-0.0020%, ・Group E; Zn: 0.001-0.010%, Group F: At least one selected from Zr, Ta, W, and Se, totaling 0.001 to 0.010% Group G: One or two types selected from Ga and Ge, in total, 0.0001 to 0.0200% Group H: One or two selected from Pb and Bi, totaling 0.00005 to 0.0020% Group I; Co: 0.001–0.100%, and - Group J; As: 0.0005-0.020%.

2. A method for manufacturing a hot-rolled and annealed sheet for non-oriented electrical steel sheets according to claim 1, characterized in that, before annealing the hot-rolled steel sheet, the hot-rolled steel sheet is subjected to at least one of rolling and tensile bending with an elongation ratio of 0.1 to 10.0%.

3. The method for manufacturing a hot-rolled annealed sheet for non-oriented electrical steel sheets according to claim 1, characterized in that, after the pickling step, the front and back surfaces of the pickled steel sheet are brush-ground using a chemical fiber brush containing abrasive particles.

4. The method for manufacturing a hot-rolled annealed sheet for non-oriented electrical steel sheets according to claim 2, characterized in that, after the pickling step, the front and back surfaces of the pickled steel sheet are brush-ground using a brush made of chemical fibers containing abrasive grains.

5. A method for producing a non-oriented electrical steel sheet, comprising: obtaining a hot-rolled and annealed sheet by the manufacturing method described in any one of claims 1 to 4; performing one cold-rolling or two or more cold-rolling processes including intermediate annealing to obtain a cold-rolled sheet of the final thickness; and annealing the cold-rolled sheet at a soaking temperature of 700 to 1100°C to obtain a cold-rolled and annealed sheet.

6. In mass%, C: 0.0050% or less, Si: 2.0 to 5.0%, Mn: 0.2-2.0%, P: 0.030% or less, S: 0.0050% or less, Al: 0.25-2.50%, N: 0.0050% or less, O: 0.0050% or less, and It contains 0.01 to 0.20% in total of one or both selected from Sn and Sb. It contains at least one component selected from groups A to J below, A hot rolling process involves heating a steel slab having a composition consisting of Fe and unavoidable impurities, and hot rolling it to produce a hot-rolled steel sheet. The process involves annealing the aforementioned hot-rolled steel sheet to obtain a hot-rolled annealed sheet, A brush grinding step is performed on the hot-rolled annealed plate using a brush made of chemical fibers containing abrasive grains. The process includes an acid pickling step of pickling the brush-ground hot-rolled annealed sheet, In the hot rolling process, the heating temperature of the steel slab is set to 1150°C or lower, the finish rolling temperature to 960°C or lower, and the winding temperature to 700°C or lower. In the aforementioned hot-rolled sheet annealing process, the annealing temperature is set to 800°C or higher and 1100°C or lower. In the aforementioned pickling process, the brush-ground steel plate is pickled with hydrochloric acid at a concentration of 5% or more, a pickling temperature of 70°C or more, and a pickling time of 10 s to 120 s. The average grain size of the steel sheet in the rolling direction cross-section is set to be in the range of 40 to 250 μm. The integrated intensity of Fe-Al oxides on the surface of the steel plate, as measured by X-ray diffraction, is set to 200 cps·degrees or less. Herein, the integrated intensity of Fe-Al oxides on the surface of the steel sheet measured by X-ray diffraction is calculated by taking the X-ray incident angle of 1 degree with respect to the steel sheet surface and determining the integrated intensity of the (311) plane peak of Fe-Al oxides (Hershinite, FeAl₂O₄) that appears around 2θ = 36.4 degrees, in a method for manufacturing hot-rolled and annealed sheets for non-oriented electrical steel sheets. Group A: At least one selected from Ca, Mg, and REM in total amount of 0.0010 to 0.0080%. Group B: At least one element selected from Cr, Mo, Cu, and Ni, totaling 0.01 to 0.60%. Group C: At least one selected from Ti, Nb, and V, totaling 0.0005 to 0.0030%. ・Group D; B: 0.0001-0.0020%, ・Group E; Zn: 0.001-0.010% - Group F: At least one selected from Zr, Ta, W, and Se, totaling 0.001 to 0.010%. Group G: One or two types selected from Ga and Ge, in total, 0.0001 to 0.0200%. Group H: One or two selected from Pb and Bi, totaling 0.00005 to 0.0020%. Group I; Co: 0.001–0.100%, and ・Group J; As: 0.0005-0.020%

7. The method for manufacturing a hot-rolled and annealed sheet for non-oriented electrical steel sheets according to claim 6, characterized in that, before annealing the hot-rolled steel sheet, the hot-rolled steel sheet is subjected to at least one of rolling and tensile bending with an elongation ratio of 0.1 to 10.0%.

8. The method for manufacturing a hot-rolled annealed sheet for non-oriented electrical steel sheets according to claim 6, characterized in that, after the pickling step, the front and back surfaces of the pickled steel sheet are brush-ground using a chemical fiber brush containing abrasive particles.

9. The method for manufacturing a hot-rolled annealed sheet for non-oriented electrical steel sheets according to claim 7, characterized in that, after the pickling step, the front and back surfaces of the pickled steel sheet are brush-ground using a chemical fiber brush containing abrasive grains.

10. A method for manufacturing a non-oriented electrical steel sheet, comprising: obtaining a hot-rolled and annealed sheet by the manufacturing method described in any one of claims 6 to 9; performing one cold-rolling or two or more cold-rolling processes including intermediate annealing to obtain a cold-rolled sheet of the final thickness; and annealing the cold-rolled sheet at a soaking temperature of 700 to 1100°C to obtain a cold-rolled and annealed sheet.

Citation Information

Patent Citations

  • Production of electromagnetic steel plate

    JP2000054025A

  • Method for manufacturing high-grade non-oriented electromagnetic steel sheet

    JP2006161094A

  • Nonoriented electromagnetic steel sheet, manufacturing method of nonoriented electromagnetic steel sheet and manufacturing method of motor core

    JP2018021241A

  • Non-oriented electromagnetic steel sheet and method for producing the same

    JP2021038458A

  • Non-oriented electrical steel sheet and motor core comprising the same

    KR1020230096879A