Method for forming cesium tungsten oxide film

JPWO2022249591A5Active Publication Date: 2024-12-03
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023523993
Authority / Receiving Office
JP · JP
Patent Type
Applications
Priority Date
2022-02-21
Filing Date
2022-02-21
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Cesium tungsten oxide films formed by sputtering often deviate from the desired atomic ratio, leading to decreased transparency in the visible wavelength range and absorption in the near-infrared wavelength range, which affects their heat ray shielding and radio wave transparency properties.

Method used

A sputtering target with a specific composition and configuration, where the distance between the target and the object, and atmospheric pressure are adjusted to maintain a cesium to tungsten atomic ratio within 0.3 to 0.36, using a sputtering method that involves cesium and tungsten sources, ensuring high transparency and absorption characteristics.

Benefits of technology

The method effectively forms cesium tungsten oxide films with high transparency in the visible wavelength range, absorption in the near-infrared range, and radio wave transparency, suitable for energy-efficient window applications.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

[Problem] To provide a sputtering target of which the nCs / nW, which is the ratio of the number of atoms of Cs to the number of atoms of W in a cesium tungsten oxide film formed by a sputtering method, is set to a desired range (0.3-0.36) in which high transmissivity in a visible wavelength range and absorption properties in a near-infrared wavelength range can be exhibited. [Solution] This target contains Cs and W, and is characterized in that when the distance between the target and an object to be film-formed during film formation is defined as [T-S distance], the pressure of the atmosphere is defined as P, the number of atoms of W contained in the target is defined as nW, and the number of atoms of Cs is defined as nCs, nCs / nW (T), which is the ratio of the numbers of atoms of W and Cs in the target, satisfies (expression 1) for [T-S distance] and P. 0.09 / {(-000161×[T-S distance]+0.00559)×P+0.346}≤nCs / nW (T)≤0.13 / {(-000161×[T-S distance]+0.00559)×P+0.346} (Expression 1)
Need to check novelty before this filing date? Find Prior Art

Description

Sputtering target and method for forming cesium tungsten oxide film

[0001] The present invention relates to a sputtering target used in forming a cesium tungsten oxide film by a sputtering method, which has high transmittance in the visible wavelength range, absorbance in the near-infrared wavelength range, and radio wave transmittance, and a method for forming the cesium tungsten oxide film. In particular, the present invention relates to a sputtering target used in forming a cesium tungsten oxide film by a sputtering method, which has high transmittance in the visible wavelength range, absorbance in the near-infrared wavelength range, and radio wave transmittance, and a method for forming the cesium tungsten oxide film. Cs / n W (However, n W is the number of W atoms in the cesium tungsten oxide film, n Cs The present invention relates to a sputtering target in which the number of Cs atoms in the cesium tungsten oxide film is set within a desired range, and a method for forming the cesium tungsten oxide film.

[0002] In recent years, in order to reduce the energy consumption of air conditioners indoors and in vehicles such as cars during the summer, progress has been made in the development of heat-shielding technologies for windows that let in natural light. These technological means include attaching to windows colored films with heat-shielding effects or films with optical thin films (light-shielding materials), coating windows with substances with heat-shielding effects, and using windows on which optical thin films with heat-shielding effects have been formed by vapor deposition, sputtering, etc. The latter method does not allow the application of optical thin films to existing windows, but it does allow the formation of highly durable optical thin films.

[0003] For example, Patent Document 1 describes a film (light-shielding member) having a mirror-like finish, formed by vapor deposition of a metal film such as aluminum, as the light-shielding member for window materials, etc. However, when such a light-shielding member is used, the appearance becomes half-mirror-like, which causes dazzling reflections when used outdoors, resulting in a problem in terms of appearance. In addition, metal films such as aluminum have high conductivity, which reflect radio waves, making it difficult for devices that use radio waves, such as mobile phones, smartphones, and devices using GPS (Global Positioning System), to connect.

[0004] As a method for applying a heat-shielding substance, the present applicant has proposed an infrared-shielding microparticle dispersion containing composite tungsten oxide microparticles represented by the general formula MxWyOz (where M is one or more elements selected from alkali metals, etc., W is tungsten, O is oxygen, and 0.001≦x / y≦1, 2.2≦z / y≦3.0), as described in Patent Document 2. The composite tungsten oxide microparticles efficiently absorb sunlight, particularly light in the near-infrared region, and also have high transparency to visible light. The infrared-shielding microparticle dispersion is prepared by dispersing composite tungsten oxide microparticles in an appropriate solvent to form a dispersion, adding a medium resin to the resulting dispersion, and then coating the substrate surface with the dispersion to form a thin film, which possesses both heat-shielding properties and radio wave transmittance. However, the method described in Patent Document 2 involves forming a thin film by a coating method, which requires advanced coating techniques to control the film thickness and ensure uniformity and flatness over a large area.

[0005] Furthermore, as a method using sputtering or the like, Patent Document 3 discloses a vehicle window glass and a manufacturing method thereof, and proposes a vehicle window glass formed by sequentially depositing, for example, a first metal oxide film (ITO) / a first Ag film / a second metal oxide film (ITO) / a second Ag film / a third metal oxide film (ITO) using a large in-line sputtering device capable of processing a large-area substrate for the vehicle window glass. Patent Document 4 proposes a composite tungsten oxide film (a composite tungsten oxide film represented by the above general formula MxWyOz) derived from sputtering deposition.

[0006] Japanese Patent Application Laid-Open No. 5-113085 Japanese Patent No. 4096205 Japanese Patent Application Laid-Open No. 2002-020142 Japanese Patent No. 6540859

[0007] Incidentally, when a cesium tungsten oxide film, which is a type of composite tungsten oxide represented by the general formula MxWyOz (a cesium tungsten oxide film in which M in the general formula MxWyOz is composed of the alkali metal cesium), is formed by the sputtering method described in Patent Document 4, the chemical composition of the cesium tungsten oxide constituting the sputtering target and the chemical composition of the formed cesium tungsten oxide film sometimes do not match.

[0008] Specifically, n represents the ratio of the number of tungsten (W) and cesium (Cs) atoms in the formed cesium tungsten oxide film. Cs / n W (n W is the number of W atoms in the cesium tungsten oxide film, n Cs is the number of Cs atoms), which indicates the ratio of the number of W and Cs atoms in the cesium tungsten oxide that constitutes the sputtering target. Cs / n W The n of the cesium tungsten oxide film does not match Cs / n W As a result of deviation from the desired range (0.3 or more and 0.36 or less), there was a problem that the high transmittance in the visible wavelength range and the absorbance in the near-infrared wavelength range, which are the characteristics of the cesium tungsten oxide film, were reduced.

[0009] The present invention has been made in view of such problems, and the object of the present invention is to improve the ratio of the number of W atoms to the number of Cs atoms in the cesium tungsten oxide film, n Cs / n W The present invention provides a sputtering target in which the refractive index is set to a desired range (0.3 to 0.36) that can exhibit high transmittance in the visible wavelength range and absorbance in the near-infrared wavelength range, and a method for forming a cesium tungsten oxide film that has high transmittance in the visible wavelength range, absorbance in the near-infrared wavelength range, and radio wave transmittance.

[0010] Therefore, the present inventors have conducted extensive research to solve the above problems, and have found that the ratio of the number of W atoms to the number of Cs atoms in a cesium tungsten oxide film formed on a substrate by sputtering is n Cs / n WRegarding n, which indicates the ratio of the number of atoms of W and Cs in the sputtering target, which is the film formation material, Cs / n W In addition to the above condition, it has been found that the distance between the sputtering target and the object to be coated during sputtering deposition and the pressure conditions of the atmosphere during sputtering deposition also play a role. Cs / n W In order to set the value of n, which represents the ratio of the number of W atoms to the number of Cs atoms in the sputtering target, to the desired range (0.3 or more and 0.36 or less), Cs / n W It was confirmed that it was necessary to adjust the above conditions, the distance between the sputtering target and the object to be coated during sputtering deposition, and the pressure conditions of the atmosphere during sputtering deposition.

[0011] The above n, which indicates the ratio of the number of W and Cs atoms in the cesium tungsten oxide film, Cs / n W Regarding Cs / n W (film), and the n represents the ratio of the number of W and Cs atoms in the cesium tungsten oxide constituting the sputtering target. Cs / n W Regarding Cs / n W It may be abbreviated as (T).

[0012] As a result of repeated experiments, the inventors have found that the above n of the sputtering target is related to the distance between the sputtering target and the object to be coated (hereinafter abbreviated as "TS distance") during sputtering deposition and the atmospheric pressure P during sputtering deposition. Cs / n W When (T) satisfies the condition of the following (formula 1), the above n of the cesium tungsten oxide film Cs / n W It was found that the (film) can be set within the desired range (0.3 or more and 0.36 or less). 0.09 / {(-000161 × [T-S distance] + 0.00559) × P + 0.346} ≦n Cs / n W(T)≦0.13 / {(-000161×[TS distance]+0.00559)×P+0.346} (Formula 1)

[0013] The present invention has been completed based on experiments and technical analysis by the inventors.

[0014] That is, the first invention according to the present invention is a sputtering target used when forming a cesium tungsten oxide film on a substrate by sputtering, which contains cesium (Cs) and tungsten (W), wherein the distance between the sputtering target and the substrate during sputtering is [T-S distance], the pressure of the atmosphere is P, and the number of W atoms contained in the sputtering target is n. W , the number of Cs atoms is n Cs When this is the case, n, which indicates the ratio of the number of W and Cs atoms in the sputtering target, Cs / n W (T) is characterized in that it satisfies the following (Equation 1) with respect to the [T-S distance] and P: 0.09 / {(-000161 × [T-S distance] + 0.00559) × P + 0.346} ≦n Cs / n W (T)≦0.13 / {(-000161×[TS distance]+0.00559)×P+0.346} (Formula 1)

[0015] A second invention according to the present invention is characterized in that the sputtering target according to the first invention is composed of a cesium tungsten oxide sintered body produced from cesium tungsten oxide powder. A third invention is characterized in that the sputtering target according to the first invention is composed of a thermally sprayed film of cesium tungsten oxide powder. A fourth invention is characterized in that the sputtering target according to the second or third invention is made from a cesium source metal or compound and a tungsten source metal or compound as raw materials. A fifth invention is characterized in that the sputtering target according to the fourth invention is made from the cesium source compound composed of an oxide, carbonate or chloride. A sixth invention is characterized in that the sputtering target according to the fourth invention is made from the tungsten source compound composed of an oxide or carbide.

[0016] Next, a seventh aspect of the present invention is a method for depositing a cesium tungsten oxide film on a substrate using the sputtering target according to any one of the first to sixth aspects, characterized in that the distance [T-S distance] between the sputtering target and the substrate during sputtering deposition is 60 mm or more and 140 mm or less, and an eighth aspect of the present invention is the method for depositing a cesium tungsten oxide film according to the seventh aspect, characterized in that the atmospheric pressure P during sputtering deposition is 0.2 Pa or more and 0.8 Pa or less.

[0017] The sputtering target according to the present invention contains Cs and W, and n represents the ratio of the number of W atoms to the number of Cs atoms. Cs / n W Since (T) satisfies the following (Equation 1) with respect to the [T-S distance] and the atmospheric pressure P during sputtering deposition, 0.09 / {(-000161 × [T-S distance] + 0.00559) × P + 0.346} ≦n Cs / n W(T)≦0.13 / {(−000161×[T−S distance]+0.00559)×P+0.346} (Formula 1) n represents the ratio of the number of W and Cs atoms in the cesium tungsten oxide film formed using this sputtering target. Cs / n W The refractive index is set in a desired range (0.3 to 0.36) so that the film can exhibit high transmittance in the visible wavelength range and absorbency in the near-infrared wavelength range.

[0018] Therefore, by using the sputtering target according to the present invention, it is possible to form a cesium tungsten oxide film on a substrate, which has high transmittance in the visible wavelength range, absorbance in the near-infrared wavelength range, and radio wave transmittance.

[0019] Schematic diagram showing the crystal structure of a composite tungsten oxide having a hexagonal crystal structure. 0.33 The sputtering target was prepared by sintering WO3 fine particle powder, and the distance between the sputtering target and the substrate to be coated [T-S distance] was set to 66 mm, 100 mm, and 134 mm, and the sputtering gas pressure P was set to 0.2 (Pa), 0.6 (Pa), and 0.8 (Pa). The n represents the ratio of the number of W and Cs atoms in the sputtering film (cesium tungsten oxide film). Cs / n W Graph showing the relationship between the thickness of the film and the T-S distance and the pressure P (Pa) of the sputtering gas. 0.33 The sputtering target was prepared by sintering WO3 fine particle powder, and the distance between the sputtering target and the substrate (T-S distance) was set to 66 mm, 100 mm, and 134 mm. The sputtering gas pressure P was set to 0.6 (Pa). The ratio of the number of W atoms to the number of Cs atoms in the sputtering film (cesium tungsten oxide film) was n. Cs / n W Graph showing the relationship between the pressure P (Pa) of the sputtering gas and the n of the sputtering film (cesium tungsten oxide film) and the T-S distance and the oxygen concentration (%) of the sputtering gas. Cs / n W The regression equation in Figure 2 showing the relationship between (film) [n Cs / n WGraph showing the relationship between the slope (a) of the equation [(film)=aP+0.346] and [T-S distance]. Graph showing the relationship between the wavelength (nm) and transmittance (%) of the heat ray-shielding film according to the example.

[0020] Hereinafter, embodiments of the present invention will be described in detail.

[0021] 1. Composite Tungsten Oxide Film The cesium tungsten oxide film according to the present invention is a type of composite tungsten oxide represented by the general formula MxWyOz (M is one or more elements selected from alkali metals and the like, W is tungsten, O is oxygen, 0.001≦x / y≦1, 2.2≦z / y≦3.0), and contains cesium (Cs), tungsten (W), and oxygen (O).

[0022] The applicant's technology for infrared shielding using composite tungsten oxide microparticles is disclosed in detail in Patent Document 2, as mentioned above, and it is necessary to use a composite tungsten oxide in the above-mentioned composition range as the main component in order to obtain a composite tungsten oxide film that has high transmittance in the visible wavelength range and absorbency in the near-infrared wavelength range. The basic optical properties of the composite tungsten oxide film are derived from the theoretically calculated atomic arrangement of element M (M is one or more elements selected from H, He, alkali metals, alkaline earth metals, rare earth elements, Mg, Zr, Cr, Mn, Fe, Ru, Co, Rh, Ir, Ni, Pd, Pt, Cu, Ag, Au, Zn, Cd, Al, Ga, In, Tl, Si, Ge, Sn, Pb, Sb, B, F, P, S, Se, Br, Te, Ti, Nb, V, Mo, Ta, Re, Be, Hf, Os, Bi, and I), tungsten (W), and oxygen (O). Specifically, when the composite tungsten oxide microparticles have a hexagonal crystal structure, the transmittance of the microparticles in the visible light region is improved, and the absorption in the near-infrared region is improved. The composite tungsten oxide fine particles may be crystalline or amorphous.

[0023] When the composite tungsten oxide fine particles having a hexagonal crystal structure have a uniform crystal structure, the amount of element M added is preferably 0.2 or more and 0.5 or less, more preferably 0.33, relative to 1 of tungsten (W). 0.33By forming WO3, it is thought that the added element M is arranged in all of the hexagonal voids in the unit structure of the composite tungsten oxide shown in FIG. 1 (a structure in which six octahedra formed by one WO6 unit are assembled to form hexagonal voids, and the element M2 is arranged in the voids).

[0024] In the case of the cesium tungsten oxide film according to the present invention, the ratio of cesium (Cs) to tungsten (W) is preferably about 0.33, more preferably 0.22 to 0.37, and even more preferably 0.3 to 0.36. Cs / n W When the refractive index (R) of the cesium tungsten oxide film is in the range of 0.22 or more and 0.37 or less, preferably 0.3 or more and 0.36 or less, the cesium tungsten oxide film has a hexagonal crystal structure and has high transmittance in the visible wavelength range and absorbency in the near-infrared wavelength range.

[0025] 2. Issues during sputtering deposition of cesium tungsten oxide film Cs 0.33 A sputtering target prepared by sintering WO3 fine particle powder [i.e., n, which indicates the ratio of the number of W and Cs atoms] Cs / n W The inventors conducted repeated sputtering tests using a sputtering target with a T-S distance of 0.33, and found that the n value, which indicates the ratio of the number of W atoms to the number of Cs atoms in the cesium tungsten oxide film formed, was determined by the distance [T-S distance] between the sputtering target and the glass substrate on which the film was to be formed, and the pressure P of the sputtering gas. Cs / n W It was confirmed that (film) was significantly smaller than 0.33.

[0026] That is, Cs 0.33 A sputtering target made by sintering WO3 fine particle powder [n indicates the ratio of the number of W and Cs atoms] Cs / n W (T) is 0.33], and the n of the cesium tungsten oxide film formed by sputtering was measured by changing the [T-S distance] condition and the sputtering gas pressure P condition during sputtering. Cs / nW The relationship between the thickness of the film and the T-S distance and the pressure P (Pa) of the sputtering gas is shown in Figure 2. The T-S distance conditions were 66 mm, 100 mm, and 134 mm, and the pressure P conditions were 0.2 (Pa), 0.6 (Pa), and 0.8 (Pa). As the T-S distance increased and as the sputtering gas pressure P (Pa) increased, the n of the cesium tungsten oxide film increased, as shown in Figure 2. Cs / n W It is confirmed that the film thickness is significantly smaller than 0.33. The sputtering method for the cesium tungsten oxide film was reactive sputtering (a method in which the oxygen contained in the sputtering gas reacts with the film during deposition) in which argon and oxygen were mixed into the sputtering gas, and the sputtering gas was a mixed gas of 5% oxygen and the remainder argon.

[0027] The sputtering target used in the test was obtained as follows.

[0028] First, Cs manufactured by Sumitomo Metal Mining Co., Ltd. 0.33 The WO3 fine particle powder was placed in a hot press and sintered under vacuum conditions at a temperature of 950°C and a pressure of 25 MPa to produce a cesium tungsten oxide sintered body. Chemical analysis of the sintered body composition revealed that the ratio of Cs / W, i.e., tungsten (W) to cesium (Cs) was 0.33 [n, which indicates the ratio of the number of W and Cs atoms]. Cs / n W was 0.33].

[0029] The oxide sintered body was then ground by machining to a diameter of 4 inches and a thickness of 5 mm, and bonded to a stainless steel backing plate using a metallic indium brazing material to obtain a sputtering target.

[0030] It is known that the composition ratio of metal elements contained in a sputtered film is generally the same as the composition ratio of metal elements contained in the sputtering target used. For example, when a sputtering film is formed using a sputtering target composed of a Ni-Cr alloy of 80 atomic % Ni and 20 atomic % Cr, the resulting sputtered film will be 80 atomic % Ni-20 atomic % Cr.

[0031] However, in the case of cesium tungsten oxide, the composition ratio of the cesium tungsten oxide constituting the sputtering target [n Cs / n W (T)] and the composition ratio of the formed cesium tungsten oxide film [n Cs / n W (membrane)] will not be identical as mentioned above.

[0032] Here, the sputtering deposition of the cesium tungsten oxide film uses a mixed gas of argon and oxygen as the sputtering gas as described above, and therefore the composition ratio [n Cs / n W Although the influence of the oxygen content on the film was considered, the influence of the oxygen content was not confirmed. 0.33 A sputtering target prepared by sintering WO3 fine particle powder [the above n Cs / n W The n of the sputtered film (cesium tungsten oxide film) formed using a sputtering target with a T-S distance of 66 mm, 100 mm, and 134 mm was measured. The sputtering gas pressure P was set to 0.6 (Pa). Cs / n W The graph in FIG. 3 shows the relationship between the T-S distance and the oxygen concentration (%) of the sputtering gas. The oxygen content of the sputtering gas is related to the composition ratio [n Cs / n W It was confirmed that this does not affect the membrane.

[0033] 2 and 3, which show the ratio of the number of W atoms to the number of Cs atoms in the sputtering film (cesium tungsten oxide film), Cs / n W (Film) was determined by identifying the sputtered film (cesium tungsten oxide film) by ICP emission spectrometry.

[0034] 3. Composition ratio of cesium tungsten oxide film [n Cs / n W Causes of fluctuations in the thickness of the film: Films are formed by sputtering when ions from the sputtering gas collide with the sputtering target, ejecting atoms from the target surface, which then reach the substrate (e.g., a glass substrate).

[0035] The mean free path of atoms ejected from the sputtering target is important in sputtering film formation. The mean free path is the average distance an ejected atom travels before colliding with another atom. The mean free path is proportional to temperature, inversely proportional to the square of the atomic diameter, and inversely proportional to pressure. The atomic diameter of cesium is 476 Å, and the atomic diameter of tungsten is 300 Å. In terms of these atomic diameters, the mean free path of cesium is much smaller than that of tungsten. Furthermore, the higher the pressure, the shorter the mean free path. Therefore, when the atmospheric pressure during sputtering film formation is low, there is no difference in the ease with which cesium and tungsten can reach the substrate, but as the atmospheric pressure increases, cesium, with its short mean free path, has difficulty reaching the substrate. Similarly, as the distance between the sputtering target and the substrate (TS distance) increases, it becomes more difficult for cesium, which has a short mean free path, to reach the substrate. This is shown in the graph in Figure 2.

[0036] 4. Composition ratio [n Cs / n WIn sputtering, in order to optimize the sputtering film formed on the substrate, the atmospheric pressure during film formation and the distance between the sputtering target and the substrate [T-S distance] may be adjusted. As a result, the n Cs / n W (film) may become lower than about 0.33, and the high transmittance in the visible wavelength range and the absorption in the near-infrared wavelength range, which are the characteristics of the sputtering film (cesium tungsten oxide film), may be reduced. In this case, the above n Cs / n W In order to make the film thickness near 0.33, the amount of cesium contained in the sputtering target should be increased. However, the amount of cesium added [i.e., the number of tungsten atoms contained in the sputtering target is increased by n W , the number of cesium atoms is n Cs When this is done, the ratio of the number of tungsten and cesium atoms, n Cs / n W (T)] needs to be clearly defined.

[0037] As a result of repeated sputtering experiments, the inventors have found that n Cs / n W For the film, the following formula (1) has been found to be related to a sputtering target that can be set to the desired range (0.3 or more and 0.36 or less): 0.09 / {(-000161 x [T-S distance] + 0.00559) x P + 0.346} ≦n Cs / n W (T)≦0.13 / {(-000161×[TS distance]+0.00559)×P+0.346} (Formula 1)

[0038] The following explanation is given: (1) The graph in Figure 2 shows the Cs 0.33 A sputtering target made by sintering WO3 fine particle powder [n indicates the ratio of the number of W and Cs atoms] Cs / n W(T) is 0.33], and the ratio of the number of W and Cs atoms in the cesium tungsten oxide film (sputtered film) formed by sputtering was determined by changing the [T-S distance] condition and the sputtering gas pressure P condition during sputtering film formation. Cs / n W The relationship between the thickness of the film and the T-S distance and the sputtering gas pressure P (Pa) is shown. The T-S distance conditions are 66 mm, 100 mm, and 134 mm, and the pressure P conditions are 0.2 (Pa), 0.6 (Pa), and 0.8 (Pa).

[0039] The relationship between the "pressure P (Pa) of the sputtering gas" and the "n (Pa) of the sputtering film" in FIG. Cs / n W The regression equation (regression equation) showing the relationship between "(membrane)" is the following (first equation): Cs / n W (Membrane)=aP+0.346 (first formula)

[0040] Here, a is the slope of the regression equation shown in (first equation).

[0041] Then, when the straight line with the T-S distance of 66 mm is calculated using the least squares method, Cs / n W (membrane) = -0.0981P + 0.346 (first equation 1) Multiple correlation coefficient 0.995, slope (a) = -0.0981 Similarly, when the line where [T-S distance] is 100 mm is calculated using the least squares method, n Cs / n W (Membrane) = -0.1596P + 0.346 (Equation 2) Multiple correlation coefficient 0.999, slope (a) = -0.1596 When the line with [T-S distance] of 134 mm is calculated using the least squares method, Cs / n W (membrane) = -0.2073P + 0.346 (Equation 3) The multiple correlation coefficient is 0.994 and the slope (a) is -0.2073.

[0042] (2) Next, the graph in FIG. 4 shows the relationship between the pressure P (Pa) of the sputtering gas and the n of the sputtering film (cesium tungsten oxide film). Cs / n W The regression equation (regression equation) showing the relationship between the slope (a) of the regression equation in Figure 2, which shows the relationship between the [T-S distance] and the [T-S distance], is given by the following (second equation): a = -000161 [T-S distance] + 0.00559 (second equation)

[0043] (3) Then, by substituting (Equation 2) into (Equation 1), the following relational expression (Equation 3) is derived. Cs / n W (Membrane) = (-000161 [TS distance] + 0.00559) x P + 0.346 (3rd formula)

[0044] The third equation derived from the graphs in Figures 2 and 4 is 0.33 A sputtering target made by sintering WO3 fine particle powder [n indicates the ratio of the number of W and Cs atoms] Cs / n W (T) is 0.33]. Cs / n W The relationship between the experimental value of (film), the [TS distance] during sputtering film formation, and the pressure P of the sputtering gas is expressed by a mathematical formula.

[0045] (4) Incidentally, the n of the sputtering film (cesium tungsten oxide film) Cs / n W (film) and the above n of the sputtering target Cs / n W (T) is the n related to the target sputtering film (cesium tungsten oxide film). Cs / n W If (membrane) is α, the following (fourth formula) holds: [n Cs / n W (T)] / α = α / [n Cs / n W (Membrane) ] (Fourth formula)

[0046] The left side of (Equation 4) indicates the compositional deviation between the "composition ratio of the target sputtering target" and the "composition ratio α of the target sputtering film," and the right side of (Equation 4) indicates the compositional deviation between the "composition ratio α of the sputtering target set to be the same as the composition ratio of the target sputtering film" and the "composition ratio of the experimental sputtering film (experimental value)." The reason why the left and right sides are equivalent is that, taking into consideration the compositional deviation between the "composition ratio α of the sputtering target" on the right side and the "composition ratio of the experimental sputtering film (experimental value)," the "composition ratio of the target sputtering target" on the left side, i.e., the composition ratio [n Cs / n W This is because it determines the

[0047] And if we rewrite (fourth formula), we get (fifth formula). Cs / n W (T) = α 2 / [n Cs / n W (Membrane)] (Fifth formula)

[0048] (5) Next, (Equation 3) is substituted into (Equation 5) to derive (Equation 6). Cs / n W (T) = α 2 / {(-000161×[TS distance]+0.00559)×P+0.346} (6th equation)

[0049] (6) Furthermore, α [n of the target cesium tungsten oxide film] Cs / n W (film)] must be set in the desired range (0.3 or more and 0.36 or less) so that the cesium tungsten oxide film can exhibit high transmittance in the visible wavelength range and absorbency in the near-infrared wavelength range. Therefore, by substituting "0.3" for α in (6-1) (sixth formula), n Cs / n W The lower limit of (T) is found, and n Cs / n W (T) = (0.3) 2 / [(-000161 × [T-S distance] + 0.00559) × P + 0.346] = 0.09 / [(-000161 × [T-S distance] + 0.00559) × P + 0.346] (6-2) Substitute "0.36" for α in (6th formula) to get n Cs / n W The upper limit of (T) is found. Cs / n W (T) = (0.36) 2 / [(-000161×[TS distance]+0.00559)×P+0.346] =0.13 / [(-000161×[TS distance]+0.00559)×P+0.346]

[0050] (7) That is, the above n of the cesium tungsten oxide film Cs / n W For the film, the following formula (1) is derived for a sputtering target that can be set to the desired range (0.3 or more and 0.36 or less): 0.09 / {(-000161 x [T-S distance] + 0.00559) x P + 0.346} ≦n Cs / n W (T)≦0.13 / {(-000161×[TS distance]+0.00559)×P+0.346} (Formula 1)

[0051] In the formula (1), [TS distance] is the distance between the sputtering target and the object to be coated during sputtering deposition, P is the atmospheric pressure, and n Cs / n W n Cs is the number of Cs atoms contained in the sputtering target, n W means the number of W atoms contained in the sputtering target.

[0052] 5. Method for Manufacturing a Sputtering Target The sputtering target according to the present invention is made from a metal or compound serving as a cesium source and a metal or compound serving as a tungsten source, and is a target having n which represents the ratio of the number of tungsten and cesium atoms. Cs / n W It can be produced using cesium tungsten oxide powder in which (T) is set to a composition ratio that satisfies the condition of the above (Equation 1).

[0053] (1) Production of Cesium Tungsten Oxide Powder A cesium source and a tungsten source are mixed so as to have a composition ratio that satisfies the condition of the above (formula 1), and the mixture is heated and fired to produce a cesium tungsten oxide powder.

[0054] The cesium source can be a metal, oxide, carbonate, or chloride. Cesium oxides include CsO, CsO, CsO, CsO, CsO, Cs 11 O3, Cs4O, and Cs7O can be mentioned.

[0055] The tungsten source can be a metal, oxide, or carbide. Tungsten oxides include WO, WO, and W. 20 O 58 , WO3 can be used.

[0056] Hydrates of the oxides of the cesium source and the tungsten source can also be used.

[0057] For example, cesium tungsten oxide powder can be produced by mixing an aqueous solution of ammonium metatungstate and cesium chloride in a composition ratio that satisfies the conditions of the above formula (1), drying at 100°C or higher to remove water, and then calcining this precursor at 500°C or higher. Alternatively, the precursor can be prepared by drying an aqueous solution of tungstic acid and cesium carbonate. The atmosphere in which the precursor is calcined may be a reducing atmosphere of a mixture of argon and hydrogen, or air.

[0058] (2) Manufacturing of the sputtering target according to the present invention The cesium tungsten oxide powder is filled into a mold, molded into the shape of a sputtering target, and then sintered by hot pressing or hot isostatic pressing to obtain a sintered body.

[0059] The conditions for sintering the mold filled with cesium tungsten oxide powder by hot pressing or hot isostatic pressing are as follows: in a vacuum or inert atmosphere, at a sintering temperature of 700°C or higher but lower than 1300°C, and at a pressure of 20 MPa or higher.

[0060] The resulting sintered body is ground by mechanical processing to obtain the sputtering target according to the present invention.

[0061] The pressure sintering sputtering target manufacturing procedure can be applied to both flat and cylindrical targets. Flat targets are fixed to a backing plate, while cylindrical targets are fixed to a backing tube for sputtering deposition.

[0062] Alternatively, a cylindrical target can be prepared by forming a base layer selected from a nickel-aluminum alloy, a nickel-chromium alloy, a copper-aluminum alloy, a copper-zinc alloy, or the like by thermal spraying on a backing tube whose surface has been roughened by blasting, and then directly spraying cesium tungsten oxide powder to form a sprayed film (target film) having a thickness of 5 mm to 20 mm, and then polishing the sprayed film (target film) to form a rotary target.

[0063] If the sputtering target is a conductor having a resistivity of 1 Ω·cm or less, a highly productive DC sputtering device can be used.

[0064] 6. Sputtering Film Formation The obtained sputtering target is mounted in a sputtering film formation device, and a cesium tungsten oxide film can be produced by sputtering a film onto a substrate such as a glass substrate.

[0065] The sputtering conditions were as follows: composition ratio n of the sputtering target Cs / n W It is natural to set the pressure P of the sputtering gas and the [TS distance] when (T) is determined.

[0066] The pressure P of the sputtering gas is preferably 0.2 Pa or more and 0.8 Pa or less. If the pressure P is less than 0.2 Pa, the amount of argon that is ionized decreases, resulting in a lower sputtering rate (efficiency). On the other hand, if the pressure P exceeds 0.8 Pa, the plasma during sputtering may become unstable.

[0067] Furthermore, the [TS distance] is preferably 60 mm or more and 140 mm or less. In sputtering deposition of a large substrate, the [TS distance] is about 100 mm.

[0068] After the film formation, a heat treatment is performed to obtain a glass substrate having an infrared shielding film made of a cesium tungsten oxide film. The atmospheric conditions for the heat treatment must be changed depending on the proportion of oxygen gas contained in the sputtering gas, and an oxidizing atmosphere, an inert gas atmosphere, or a reducing atmosphere containing a reducing gas such as hydrogen is selected. For example, when the oxygen content of the sputtering gas is 0% or more but less than 1%, the heat treatment is performed in an oxidizing atmosphere, and the oxidizing atmosphere may be air, a mixed gas of 5% to 20% oxygen and nitrogen, or the like. Furthermore, when the oxygen content of the sputtering gas is 1% or more, the heat treatment is performed in a reducing atmosphere such as nitrogen gas.

[0069] Examples of the present invention will be specifically described below.

[0070] The sputtering device used was an apparatus equipped with a DC magnetron sputtering cathode and a substrate holder in a film formation chamber.

[0071] The distance between the sputtering target and the substrate [TS distance] was 100 mm, an argon mixed gas containing 5% oxygen was used as the sputtering gas, and the pressure P of the sputtering gas during sputtering film formation was adjusted to 0.6 Pa.

[0072] Furthermore, the n in the cesium tungsten oxide film Cs / n W The target value of (film) is set to 0.33, and the n of the sputtering target Cs / n W (T) was calculated as 0.431 by substituting [T-S distance] = 100 mm, P = 0.6 Pa, and α = 0.33 into (Equation 6). Cs / n W (T) = α 2 / {(-000161×[TS distance]+0.00559)×P+0.346} (6th equation)

[0073] [Example 1] (1) Preparation of Cesium Tungsten Oxide Powder 9.70 kg of cesium carbonate (CsCO) was dissolved in 6.70 kg of water to obtain a cesium carbonate solution. This solution was added to 34.57 kg of tungstic acid (HWO), thoroughly mixed, and then dried with stirring to obtain a dried product. Note that n, which indicates the ratio of the number of W and Cs atoms contained in the dried product, is used. Cs / n W is equivalent to 0.431.

[0074] Next, the dried product was heated while supplying 5% by volume of H gas with N gas as a carrier, and calcined at a temperature of 800°C for 5.5 hours. Thereafter, the gas supply was switched to N gas only, and the temperature was lowered to room temperature, yielding a cesium tungsten oxide powder.

[0075] (2) Production of sputtering target The obtained cesium tungsten oxide powder was placed in a hot press and sintered in a vacuum atmosphere at a temperature of 950°C and a pressure of 25 MPa to produce a cesium tungsten oxide sintered body. Chemical analysis of the composition of the produced sintered body revealed that n, which indicates the ratio of the number of W and Cs atoms contained in the sintered body, Cs / n W was 0.43.

[0076] The obtained cesium tungsten oxide sintered body was then machined to a diameter of 4 inches and a thickness of 5 mm, and bonded to a stainless steel backing plate using a metallic indium brazing material to obtain a sputtering target according to the example.

[0077] (3) Production of Infrared Shielding Film Made of Cesium Tungsten Oxide Film A 4-inch quartz wafer was used as the substrate, and the quartz wafer was heated to 300° C. by a near-infrared heater.

[0078] The deposition chamber and substrate stocker chamber of the sputtering device were then 5×10 -4The chamber was evacuated to a vacuum of 0.6 Pa or less, and argon gas (sputtering gas) mixed with 5% oxygen was introduced into the film formation chamber at 200 sccm. The pressure of the sputtering gas was adjusted to 0.6 Pa, and then a cesium tungsten oxide film was formed on the quartz wafer by reactive sputtering.

[0079] When the formed cesium tungsten oxide film was analyzed by ICP, n Cs / n W The film thickness of the cesium tungsten oxide film was 400 nm.

[0080] Next, the cesium tungsten oxide film was subjected to annealing treatment at 600° C. for 10 minutes in a nitrogen gas reducing atmosphere to obtain an infrared shielding film made of a cesium tungsten oxide film.

[0081] (4) Transmittance of Infrared Shielding Film The transmittance of the obtained infrared shielding film was measured using a spectrophotometer (Hitachi, Model No. V-670), and the spectral optical characteristics shown in the graph of FIG. 5 were obtained.

[0082] From the graph in FIG. 5, it was confirmed that this infrared shielding film has high transmittance in the visible wavelength range and absorbance in the near-infrared wavelength range, and furthermore, due to its material composition, it also has radio wave transmittance.

[0083] n represents the ratio of the number of W and Cs atoms in the cesium tungsten oxide film formed using the sputtering target of the present invention. Cs / n W The film has industrial applicability for use in, for example, vehicle window glass that reduces the energy consumption of air conditioners in the summer, because the film is set in a desired range (0.3 or more and 0.36 or less) that allows the film to exhibit high transmittance in the visible wavelength range and absorbency in the near-infrared wavelength range.

[0084] 1 WO6 unit 2 element M

Claims

1. A method for forming a cesium tungsten oxide film on a substrate using a sputtering target containing cesium (Cs) and tungsten (W), comprising: The distance between the sputtering target and the object to be coated during sputtering is [T-S distance], the pressure of the atmosphere is P, and the number of W atoms contained in the sputtering target is n W , the number of Cs atoms is n Cs When n indicates the ratio of the number of W and Cs atoms in the sputtering target. Cs / n W A method for forming a cesium tungsten oxide film, characterized in that (T) satisfies the following (Formula 1) with respect to the above [T-S distance] and P.

2. 2. The method for forming a cesium tungsten oxide film according to claim 1, wherein the sputtering target is made of a cesium tungsten oxide sintered body produced from cesium tungsten oxide powder.

3. 2. The method for forming a cesium tungsten oxide film according to claim 1, wherein the sputtering target is a thermally sprayed film of cesium tungsten oxide powder.

4. 4. The method for forming a cesium tungsten oxide film according to claim 2, wherein the cesium tungsten oxide powder is made from a metal or compound of a cesium source and a metal or compound of a tungsten source.

5. 5. The method for forming a cesium tungsten oxide film according to claim 4, wherein the cesium source compound is composed of an oxide, a carbonate or a chloride.

6. 5. The method for forming a cesium tungsten oxide film according to claim 4, wherein the compound of the tungsten source is composed of an oxide or a carbide.

7. 7. The method for forming a cesium tungsten oxide film according to claim 1, wherein the distance [T-S distance] between the sputtering target and the object to be coated during sputtering is 60 mm or more and 140 mm or less.

8. 8. The method for forming a cesium tungsten oxide film according to claim 7, wherein the pressure P of the atmosphere during sputtering is 0.2 Pa or more and 0.8 Pa or less.