Member for inkjet head, method for manufacturing member for inkjet head, and inkjet head
Patent Information
- Application Number
- JP2024508114
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-22
AI Technical Summary
Inkjet head members face challenges with durability and adhesion between the base material and functional layers, leading to issues with ink resistance, scratch resistance, and continuous ejection performance due to the peeling of layers during the manufacturing process and exposure to ink.
A base material adhesion layer containing group 4 or 5 elements, nitrogen, and oxygen is used, with a higher atomic concentration of oxygen on the surface than within, along with a liquid-repellent layer containing a fluorine-based coupling agent, to enhance adhesion and durability, and a method involving reactive sputtering and oxygen plasma treatment is employed.
The solution ensures long-term durability against ink, improved scratch resistance, and continuous ejection performance by enhancing the adhesion between the base material and functional layers, preventing peeling and maintaining inkjet head performance over time.
Abstract
Description
Inkjet head member, method of manufacturing inkjet head member, and inkjet head
[0001] The present invention relates to an inkjet head component, a method for manufacturing an inkjet head component, and an inkjet head, and in particular to an inkjet head component that can achieve both durability in the manufacturing process and adhesion between the substrate and the functional layer, thereby ensuring long-term durability against ink and abrasion resistance, and also having excellent continuous ejection properties.
[0002] Inkjet recording devices that are currently in widespread use hold an inkjet head equipped with a nozzle plate in which multiple nozzle holes are arranged in a row by attaching it to a frame or the like, and form an image on the recording medium by ejecting each color ink in the form of tiny droplets from each of the multiple nozzles toward the recording medium.
[0003] Typical ink ejection methods for inkjet heads include a method in which the water in the ink is vaporized and expanded by the heat generated by passing an electric current through an electrical resistor placed in a pressure chamber, thereby applying pressure to the ink and ejecting it, and a method in which part of the flow path member that makes up the pressure chamber is made of a piezoelectric material, or a piezoelectric material is installed in the flow path member, and the piezoelectric materials that correspond to multiple nozzle holes are selectively driven, thereby deforming the pressure chamber based on the dynamic pressure of each piezoelectric material and ejecting liquid from the nozzle.
[0004] In order to achieve good ink droplet ejection performance in an inkjet head, the surface characteristics of the surface on which the nozzles are provided are extremely important.
[0005] If ink liquid or dust adheres to the vicinity of the nozzle holes of the inkjet head, the ejection direction of the ejected ink droplets may be curved or the ejection angle of the ink droplets from the nozzle holes may widen, causing satellites.
[0006] In order to eject ink droplets stably, it is of course necessary to optimize the design of the ink flow path and the method of applying pressure to the ink, but this alone is not enough; it is also necessary to always maintain a stable surface condition around the nozzle holes that eject the ink. To achieve this, methods are being considered for applying a liquid-repellent layer with liquid-repellent properties to the areas around the nozzle holes on the ink ejection surface of the nozzle plate to prevent unwanted ink from adhering to or remaining on them.
[0007] Generally, a silicone compound or a fluorine-containing organic compound, such as a silane coupling agent, is used for the liquid-repellent layer formed on the nozzle surface of a nozzle plate provided in an inkjet head. It is known that the use of a silane coupling agent in forming the liquid-repellent layer makes it possible to form a liquid-repellent layer with excellent adhesion.
[0008] It is also known that abrasion resistance and chemical resistance can be improved by forming a substrate adhesion layer containing TaSiOx on the substrate of the nozzle plate before forming the liquid-repellent layer (see, for example, Patent Document 1). However, such materials have a problem in that they tend to peel off at the interface near the nozzle due to heat in the manufacturing process, such as during nozzle processing after forming the substrate adhesion layer and the liquid-repellent layer, or during plasma treatment used to improve the adhesion of the liquid-repellent layer.
[0009] On the other hand, Patent Document 2 discloses that the adhesion of a liquid-repellent layer or a bonding film can be improved by using a metal nitride film as a base layer underlying the liquid-repellent layer of a nozzle plate, and Patent Document 3 discloses that the adhesion of a liquid-repellent layer or a bonding film can be improved by using a metal nitride film as an intermediate layer for increasing the bonding strength between the nozzle plate and a bonding film containing organosiloxane. However, it has been found that metal nitride films that do not contain oxygen atoms cannot ensure adhesion with the liquid-repellent layer or the bonding film. It is also known that substrates such as nozzle plates are provided with, in addition to the liquid-repellent layer and the base layer, a protective layer to protect the substrate from corrosion or an adhesive layer to bond the substrate to another substrate. There is a demand for improving the adhesion between functional layers such as these liquid-repellent layers, base layers, protective layers, and adhesive layers and the substrate.
[0010] Furthermore, when pigment ink is used, it has been confirmed that the liquid-repellent layer surface gradually wears away due to rubbing between the wipe material used during maintenance and the pigment ink containing pigment particles. It has been found that repeating such an operation over a long period of time poses a problem in that the durability (abrasion resistance) of the above layer structure cannot be ensured.
[0011] Patent No. 6217170 European Patent No. 2484526 Patent No. 4900457
[0012] The present invention has been made in consideration of the above problems and circumstances, and the problem to be solved is to provide an inkjet head component, a manufacturing method for an inkjet head component, and an inkjet head that can achieve both durability in the manufacturing process and adhesion between the substrate and the functional layer, thereby ensuring long-term durability and abrasion resistance against ink and having excellent continuous ejection properties.
[0013] In the course of investigating the causes of the above problems in order to solve them, the present inventors discovered that by incorporating a Group 4 or 5 element, a nitrogen element, and an oxygen element into a substrate adhesion layer between the substrate and the functional layer, and by making the atomic concentration (atm %) of the oxygen element on the surface of the substrate adhesion layer facing the functional layer higher than that inside the substrate adhesion layer, it is possible to achieve both durability in the manufacturing process and adhesion between the substrate and the functional layer, ensure long-term durability to ink and abrasion resistance, and achieve excellent continuous ejection properties, thereby arriving at the present invention. That is, the above problems according to the present invention are solved by the following means.
[0014] 1. An inkjet head member having at least a substrate, a substrate adhesion layer, and a functional layer in this order, wherein the substrate adhesion layer contains a Group 4 or Group 5 element, a nitrogen element, and an oxygen element, and the atomic concentration (atm %) of the oxygen element on the surface of the substrate adhesion layer facing the functional layer is higher than that inside the substrate adhesion layer.
[0015] 2. The inkjet head member according to item 1, wherein the Group 5 element contained in the substrate adhesion layer is tantalum (Ta).
[0016] 3. The inkjet head member according to item 1 or 2, wherein the ratio of the atomic concentration (atm %) of nitrogen element to the atomic concentration (atm %) of Group 4 or Group 5 element within the substrate adhesion layer satisfies the following formula (I): 0.3≦atomic concentration of nitrogen element / atomic concentration of Group 4 or Group 5 element≦1
[0017] 4. The substrate adhesion layer is found to contain Ta in an X-ray diffraction (XRD) measurement. 2 4. The ink jet head member according to any one of items 1 to 3, having a peak derived from N.
[0018] 5. The inkjet head member according to any one of items 1 to 3, wherein the thickness of the substrate adhesion layer is within the range of 1 to 1500 nm.
[0019] 6. The inkjet head member according to any one of items 1 to 5, wherein the functional layer includes a liquid-repellent layer containing a coupling agent containing fluorine (F).
[0020] 7. The inkjet head member according to any one of items 1 to 6, wherein the functional layer includes a liquid-repellent layer containing a coupling agent containing fluorine (F) and an underlayer that serves as a base for the liquid-repellent layer.
[0021] 8. The ink jet head member according to item 7, wherein the underlayer is a layer containing at least an inorganic oxide or an oxide containing carbon (C).
[0022] 9. The ink jet head member according to item 8, wherein the underlayer contains an oxide composed of at least carbon (C), silicon (Si), and oxygen (O).
[0023] 10. The ink jet head member according to item 8 or 9, wherein the underlayer is a layer made of a silane coupling agent containing at least carbon (C) and oxygen (O).
[0024] 11. The inkjet head member according to item 10, wherein the silane coupling agent contained in the underlayer has reactive functional groups at both ends and a molecular structure containing a hydrocarbon chain and a benzene ring in the middle.
[0025] 12. The inkjet head member according to any one of items 1 to 11, wherein the substrate is made of stainless steel.
[0026] 13. A method for manufacturing an inkjet head member according to any one of items 1 to 12, comprising forming the substrate adhesion layer on the substrate, forming the functional layer on the substrate adhesion layer, and then forming nozzles by laser processing.
[0027] 14. The method for producing an inkjet head member according to item 13, wherein the substrate adhesion layer is formed by a reactive sputtering method using a dry process.
[0028] 15. The method for producing an inkjet head member according to item 13 or 14, wherein the surface treatment of the substrate adhesion layer is performed by oxygen plasma treatment.
[0029] 16. An inkjet head comprising the inkjet head member according to any one of items 1 to 12.
[0030] The above-mentioned means of the present invention make it possible to achieve both durability in the manufacturing process and adhesion between the substrate and the functional layer, thereby ensuring long-term durability and abrasion resistance against ink, and providing an inkjet head component, a manufacturing method for an inkjet head component, and an inkjet head that are excellent in continuous ejection properties.
[0031] Although the mechanism of action or manifestation of the effects of the present invention is not clear, it is speculated as follows. In the present invention, the substrate adhesion layer contains a Group 4 or 5 element, nitrogen, and oxygen. Therefore, by using a nitride film of a Group 4 or 5 element with a high melting point, heat resistance and adhesion can be improved. As a result, heat resistance during the manufacturing process of an inkjet head component and adhesion durability at the interface between the substrate and the functional film can be improved. Furthermore, by increasing the atomic concentration (atm %) of oxygen on the surface of the substrate adhesion layer facing the functional layer compared to the interior of the substrate adhesion layer, chemical bonds such as covalent bonds and hydrogen bonds, which exhibit greater bond energy, are more likely to occur, thereby improving adhesion between the substrate and the functional film. In particular, even when printing for long periods using real ink (sublimation / disperse dye ink), ink penetration into the interface between the substrate and the functional film can be prevented, ensuring long-term durability and abrasion resistance. Furthermore, by imparting conductivity to the substrate adhesion layer by containing a Group 4 or 5 element, adhesion of ink mist during ejection can be prevented, improving continuous ejection performance.
[0032] Schematic cross-sectional view showing an example of a nozzle plate. Schematic cross-sectional view showing another example of the configuration of the nozzle plate. Schematic cross-sectional view showing an example of a partial configuration in which nozzle holes are formed in the nozzle plate. Graph showing an example of an element concentration distribution curve (depth profile) in the thickness direction of the substrate and the substrate adhesion layer. Graph showing an example of the results of XRD diffraction measurement of the substrate adhesion layer. Schematic view showing an example of a high-frequency plasma device in RIE mode used to form the substrate adhesion layer. Schematic perspective view showing an example of the structure of an inkjet head to which the nozzle plate of the present invention can be applied. Bottom view showing an example of a nozzle plate constituting the inkjet head shown in FIG. 7.
[0033] The inkjet head member of the present invention comprises at least a substrate, a substrate adhesion layer, and a functional layer in this order, wherein the substrate adhesion layer contains a Group 4 or Group 5 element, a nitrogen element, and an oxygen element, and the atomic concentration (atm %) of the oxygen element is higher on the surface of the substrate adhesion layer facing the functional layer than in the interior of the substrate adhesion layer. This feature is a technical feature common to or corresponding to each of the following embodiments.
[0034] In an embodiment of the present invention, the Group 5 element contained in the substrate adhesion layer is preferably tantalum (Ta), from the viewpoint of imparting electrical conductivity and improving ink ejection properties. Furthermore, it is preferable that the ratio of the atomic concentrations (atm %) of nitrogen element and Group 4 or Group 5 element in the substrate adhesion layer satisfies formula (I) (0.3≦atomic concentration of nitrogen element / atomic concentration of Group 4 or Group 5 element≦1), from the viewpoint of imparting electrical conductivity and preventing mist adhesion during ink ejection. Furthermore, it is preferable that the substrate adhesion layer is such that, in X-ray diffraction (XRD) measurement, Ta 2 Having a peak derived from N is preferable in terms of imparting conductivity and preventing mist adhesion when ink is ejected.
[0035] The thickness of the substrate adhesion layer is preferably within the range of 1 to 1500 nm from the viewpoint of nozzle processing and uniform nozzle shape due to the distribution of the substrate adhesion layer deposition.
[0036] The functional layer preferably includes a liquid-repellent layer containing a coupling agent containing fluorine (F) from the viewpoints of improving adhesion to the substrate adhesion layer and abrasion resistance to ink.
[0037] It is preferable that the functional layer includes a liquid-repellent layer containing a coupling agent containing fluorine (F) and an underlayer that serves as a base for the liquid-repellent layer, in that the adhesion of the liquid-repellent layer can be improved.
[0038] The underlayer is a layer containing at least an inorganic oxide or an oxide containing carbon (C), and preferably the underlayer contains an oxide composed of at least carbon (C), silicon (Si), and oxygen (O) as the oxide containing carbon (C), which is preferable in that it exhibits the effect of retaining the coupling agent containing fluorine (F) contained in the liquid-repellent layer as the upper layer, and further improves the adhesion between the liquid-repellent layer and the substrate adhesion layer.
[0039] Furthermore, it is preferable that the underlayer is a layer made of a silane coupling agent containing at least carbon (C) and oxygen (O), and further that the silane coupling agent has reactive functional groups at both ends and a molecular structure containing a hydrocarbon chain and a benzene ring in the middle, because the silane coupling agent polymerizes at a high density and generates stacking interactions with each other, thereby improving the adhesion between the substrate and the constituent layers provided thereon when the substrate is subjected to stress, particularly in the thickness direction, and when the substrate is a nozzle plate, it can also improve the resistance when the surface is subjected to stress in the width direction by a wipe material used for maintenance, etc.
[0040] The substrate is preferably made of stainless steel, as this allows for better durability to be achieved.
[0041] In the method for manufacturing an inkjet head member of the present invention, the substrate adhesion layer is formed on the substrate, the functional layer is formed on the substrate adhesion layer, and then a nozzle is formed by laser processing. By using the substrate adhesion layer of the present invention, an inkjet head member can be manufactured without problems such as thermal deterioration of substrate adhesion or film peeling, even when laser processing is performed after the formation of the substrate adhesion layer and the functional layer.
[0042] The substrate adhesion layer is preferably formed by a reactive sputtering method using a dry process in terms of productivity and safety. Also, the surface treatment of the substrate adhesion layer is preferably performed by oxygen plasma treatment, since the atomic concentration of oxygen element on the surface of the substrate adhesion layer on the functional layer side can be easily increased.
[0043] The inkjet head member of the present invention is suitably used in inkjet heads.
[0044] The present invention, its components, and embodiments and modes for carrying out the present invention will be described below. In this application, the symbol "to" is used to mean that the numerical values before and after it are included as the lower limit and upper limit.
[0045] [Inkjet head member] The inkjet head member of the present invention is an inkjet head member having at least a substrate, a substrate adhesion layer, and a functional layer in this order, wherein the substrate adhesion layer contains a Group 4 or Group 5 element, a nitrogen element, and an oxygen element, and the atomic concentration (atm %) of the oxygen element on the surface of the substrate adhesion layer facing the functional layer is higher than that inside the substrate adhesion layer.
[0046] The inkjet head member of the present invention is a member that constitutes an inkjet head, and examples thereof include members that constitute a nozzle plate, a nozzle substrate, an ink flow path, an ink chamber, or an exterior part.
[0047] The following description will take a nozzle plate as an example of an inkjet head component. FIG. 1 is a schematic cross-sectional view showing an example of a nozzle plate. As shown in FIG. 1, the nozzle plate 1 basically comprises a substrate 2, a substrate adhesion layer 3 containing a group 4 or 5 element, a nitrogen element, and an oxygen element, and a functional layer 4 formed thereon. The atomic concentration (atm %) of the oxygen element on the surface of the substrate adhesion layer 3 facing the functional layer 4 is higher than that inside the substrate adhesion layer 3. The functional layer 4 may be, for example, a single liquid-repellent layer, a liquid-repellent layer and an underlying layer that forms an underlying layer for the liquid-repellent layer, a protective layer that protects the substrate, or an adhesive layer that bonds the nozzle plate substrate to another substrate. Examples of the other substrates include substrates for pressure chambers, flow path substrates, wiring substrates, common flow paths, cap receivers, exteriors, etc. Materials include stainless steel, metals such as nickel (Ni), gold (Au), aluminum (Al), and copper (Cu), silicon, metal oxides, metal nitrides, resins such as polyimide, liquid crystal polymer, PPS, and epoxy.
[0048] Fig. 2 is a schematic cross-sectional view showing another example of the configuration of a nozzle plate. The nozzle plate shown in Fig. 2 differs from the nozzle plate 1 shown in Fig. 1 in that the functional layer 4 is composed of an underlayer 41 and a liquid-repellent layer 42, and the underlayer 41 is further composed of two layers, a first underlayer 41a and a second underlayer 41b.
[0049] For example, the first underlayer 41a may be configured to contain a silane coupling agent having reactive functional groups at both ends and including a hydrocarbon chain and a benzene ring in the middle, and the second underlayer 41b may be configured to contain an oxide composed mainly of carbon (C), silicon (Si), and oxygen (O), such as a low-molecular-weight silane compound or a silane compound.
[0050] 3 is a schematic cross-sectional view showing an example of a partial configuration in which nozzle holes are formed in the nozzle plate described above. As shown in Fig. 3, a substrate adhesion layer 3 containing a Group 4 or Group 5 element, a nitrogen element, and an oxygen element is provided between the substrate 2 and the functional layer 4 (underlying layer 41 and liquid-repellent layer 42). By making the atomic concentration of the oxygen element on the surface of the substrate adhesion layer 3 facing the functional layer 4 higher than that in the interior, it is possible to improve adhesion between the substrate 2 and the functional film 4.
[0051] [Constituent Materials of Nozzle Plate] As an example of a nozzle plate according to the present invention, the constituent materials of a nozzle plate comprising a substrate, a substrate adhesion layer, an underlayer, and a liquid-repellent layer will be described in detail. In the present invention, the substrate adhesion layer contains a Group 4 or Group 5 element, a nitrogen element, and an oxygen element, and the atomic concentration (atm %) of the oxygen element on the surface of the substrate adhesion layer facing the functional layer is higher than that inside the substrate adhesion layer. In the present invention, the "surface of the substrate adhesion layer facing the functional layer" refers to a region within a depth of 5 nm from the outermost surface on the side of the substrate adhesion layer that contacts the functional layer. Furthermore, the "inside of the substrate adhesion layer" refers to a region excluding the surface of the substrate adhesion layer facing the functional layer and the surface on the substrate side, i.e., a region deeper than 5 nm from the outermost surface on each side of the substrate adhesion layer that contacts the functional layer and the side that contacts the substrate.
[0052] The atomic concentration (atm %) of oxygen element on the surface of the substrate adhesion layer on the functional layer side is preferably in the range of 20 to 75 atm %, more preferably in the range of 25 to 65 atm %, and the atomic concentration (atm %) of oxygen element inside the substrate adhesion layer is preferably in the range of 0 to 50 atm %, more preferably in the range of 0 to 35 atm %.
[0053] <Substrate> The substrate constituting the nozzle plate can be selected from materials that have high mechanical strength, ink resistance, and excellent dimensional stability. For example, various materials such as inorganic materials, metal materials, and resin films can be used. Among these, inorganic materials and metal materials are preferred, and metal materials such as silicon wafers, iron (for example, stainless steel (SUS)), aluminum, nickel, and stainless steel are more preferred, and stainless steel (SUS) is particularly preferred.
[0054] The thickness of the substrate constituting the nozzle plate is not particularly limited, but is in the range of 10 to 500 μm, and preferably in the range of 30 to 150 μm.
[0055] <Substrate Adhesion Layer> The substrate adhesion layer according to the present invention contains a Group 4 or Group 5 element, a nitrogen element, and an oxygen element, and the atomic concentration (atm %) of the oxygen element on the surface of the substrate adhesion layer facing the functional layer is higher than that in the interior of the substrate adhesion layer. As described above, the surface of the substrate adhesion layer facing the functional layer is the surface on the functional layer side that contacts the substrate, and generally refers to a region up to 5 nm deep from the outermost surface of the substrate adhesion layer toward the substrate.
[0056] Examples of the Group 4 elements include titanium (Ti), zirconium (Zr), and hafnium (Hf), and examples of the Group 5 elements include vanadium (V), niobium (Nb), and tantalum (Ta). Among these, tantalum (Ta), titanium (Ti), and zirconium (Zr) are preferred, and tantalum (Ta) is particularly preferred.
[0057] (Specific composition analysis method of substrate adhesion layer) <Measurement of composition ratio of constituent elements of substrate adhesion layer> In the present invention, the method for measuring the composition ratio of the elements constituting the substrate adhesion layer is not particularly limited. In the present invention, for example, a method of scraping a 10 nm region from the surface of the substrate adhesion layer using a trimming glass knife or the like and quantitatively analyzing the composition of the material constituting the sliced portion, a method of quantifying the mass of compounds in the thickness direction of the substrate adhesion layer using infrared spectroscopy (IR) or atomic absorption spectroscopy, or the like, and even if the substrate adhesion layer is an extremely thin film of 10 nm or less, it can be quantified by XPS (X-ray photoelectron spectroscopy) analysis. Among these, the use of XPS analysis is a preferred method from the viewpoint that elemental analysis can be performed even on an extremely thin film, and the composition distribution profile in the layer thickness direction of the entire substrate adhesion layer can be measured by the depth profile measurement described below.
[0058] X-ray photoelectron spectroscopy, also known as XPS (X-ray Photoelectron Spectroscopy) or ESCA (Electron Spectroscopy for Chemical Analysis), is a type of photoelectron spectroscopy that analyzes the constituent elements present in the surface region up to a depth of 5 nm from the sample surface and their electronic states.
[0059] As described above, in the substrate adhesion layer according to the present invention, the atomic concentration (atm %) of oxygen element on the surface facing the functional layer is preferably within the range of 20 to 75 atm %, and the atomic concentration (atm %) of oxygen element inside the substrate adhesion layer is preferably within the range of 25 to 65 atm %. The ratio (S / I) of the atomic concentration (S) of oxygen element on the surface facing the functional layer of the substrate adhesion layer to the atomic concentration (I) of oxygen element inside the substrate adhesion layer is preferably 1.01 or more. Furthermore, the ratio of the atomic concentrations (atm %) of nitrogen element to Group 4 or Group 5 element inside the substrate adhesion layer preferably satisfies the following formula (I): Formula (I): 0.3≦atomic concentration of nitrogen element / atomic concentration of Group 4 or Group 5 element≦1. It is more preferable that the ratio value is within the range of 0.33 to 0.67.
[0060] In the present invention, in order to measure the atomic concentration of the oxygen element, or the atomic concentration of the nitrogen element, or the group 4 or 5 element on the functional layer side and inside of the substrate adhesion layer, it is preferable to measure the atomic concentration distribution in the layer thickness direction.
[0061] <Analysis Method: Measurement of Atomic Concentration Distribution in Layer Thickness Direction> In the present invention, the atomic concentration distribution curve (hereinafter referred to as "depth profile") in the thickness direction of the substrate from the substrate adhesion layer according to the present invention can be measured by combining X-ray photoelectron spectroscopy measurement and ion sputtering using a rare gas or the like to measure the concentration (atm %) of metal oxide or nitride, the concentration (atm %) of silicon oxide or nitride, the concentration (atm %) of carbon (C), nitrogen (N), oxygen (O), Group 4 or Group 5 element, etc., by exposing the surface of the substrate adhesion layer from the surface on the functional layer side toward the substrate side and sequentially performing surface composition analysis from the surface on the functional layer side of the substrate adhesion layer toward the substrate side.
[0062] The distribution curve obtained by such XPS depth profile measurement can be created, for example, with the concentration of each element (unit: atm%) on the vertical axis and the etching time (sputtering time) on the horizontal axis. In such an atomic concentration distribution curve with the etching time on the horizontal axis, the etching time roughly correlates with the distance from the surface of the substrate adhesion layer in the layer thickness direction. Therefore, the "distance from the surface of the substrate adhesion layer in the thickness direction of the substrate adhesion layer" can be used as the distance from the surface of the substrate adhesion layer calculated from the relationship between the etching rate and etching time used in the XPS depth profile measurement. Furthermore, the sputtering method used in such XPS depth profile measurement can be a rare gas ion sputtering method using argon (Ar) as the etching ion species. The etching rate (etching rate) can be calculated by using a SiO 2 film with a known thickness. 2 The etching depth can be measured using a thermal oxide film. 2 It is often expressed as a thermal oxide film equivalent value.
[0063] An example of specific conditions for XPS analysis applicable to the composition analysis of the substrate adhesion layer according to the present invention is shown below.
[0064] Analysis equipment: QUANTERA SXM manufactured by ULVAC-PHI, Inc. X-ray source: Monochromated Al-Kα 15 kV 25 W Sputter ions: Ar (1 keV) Depth profile: SiO 2 Measurements were repeated at predetermined thickness intervals using the converted sputtering thickness to obtain a depth profile in the depth direction. The thickness interval was 2.6 nm (data was obtained every 2.6 nm in the depth direction). Quantitation: The background was determined using the Shirley method, and quantitation was performed using the relative sensitivity factor method from the obtained peak area. Data processing was performed using a MultiPak manufactured by ULVAC-PHI, Inc.
[0065] An example of the measurement results is shown below: Fig. 4 shows an example of the atomic concentration distribution curve (Death profile) measured by XPS for a nozzle plate composed of a substrate (SUS) / substrate adhesion layer (TaN) / first underlayer (SiOC) / second underlayer (SiOC) / liquid-repellent layer (fluorine-containing coupling agent).
[0066] The atomic concentration distribution curve (Death profile) shown in Figure 4 shows an example of a substrate adhesion layer formed on the surface of a SUS substrate by sputtering deposition, and shows that the oxygen concentration in the surface portion of the substrate adhesion layer is higher than the oxygen (O) concentration inside the substrate adhesion layer.
[0067] The point where the concentration of carbon (C) derived from the underlayer among the constituent atoms from the liquid-repellent layer to the substrate becomes half of the peak concentration can be understood as the surface portion of the substrate adhesion layer (the interface between the first underlayer and the substrate adhesion layer). In other words, when the etching time is 60 minutes, the location about 94 nm from the surface of the liquid-repellent layer can be considered to be the interface between the first underlayer and the substrate adhesion layer.
[0068] On the other hand, the point where the oxygen concentration levels off can be understood as the inside of the substrate adhesion layer. That is, in this case, the etching time is 74 (min), and the location approximately 116 nm from the surface of the liquid-repellent layer can be considered to be the interface between the substrate adhesion layer and the substrate. It can be seen that there is a layer where the oxygen concentration in the surface part of the substrate adhesion layer is higher than the oxygen concentration inside the substrate.
[0069] (X-ray diffraction measurement of substrate adhesion layer) The substrate adhesion layer according to the present invention is measured by X-ray diffraction (XRD). 2 Having a peak derived from N is preferable in terms of imparting conductivity and preventing mist adhesion when ink is ejected.
[0070] X-ray diffraction measurement of the substrate adhesion layer can be performed by the following procedure. Using a 6-inch silicon wafer as the substrate, a Ta target was used to perform sputtering film formation on the substrate in an atmosphere of argon gas and nitrogen gas to form a substrate adhesion layer. Specifically, under vacuum conditions, a Ta target that had been set in advance on the electrode of a DC sputtering film formation device was sputtered under the following conditions: Sputtering conditions Target: Ta DC power density: 1.1 W / cm 2 Power: 200 W Temperature: 25°C Pressure: 0.3 Pa Introduced gas: argon gas + nitrogen gas Film formation time: 10 min
[0071] The substrate adhesion layer formed on the silicon wafer was measured using an X-ray diffractometer (Rigaku Corporation, Ultima III multipurpose X-ray diffractometer) under the following conditions to obtain an X-ray diffraction pattern. Apparatus: Rigaku Corporation, Ultima III multipurpose X-ray diffractometer; X-ray source: Cu-kα 40 kV-30 mA; Scan axis: θ / 2θ; Scan range: 25° to 85° (sampling width: 0.02°); Scan speed: 10° / min
[0072] 5 is an example showing the results of XRD diffraction measurement of the substrate adhesion layer. As shown in FIG. 5, in the measured X-ray diffraction spectrum, Ta is detected at 2θ of 32.6°. 2 The peak was attributed to N.
[0073] (Resistivity of Substrate Adhesion Layer) The resistivity of the substrate adhesion layer according to the present invention is 1×10 -8 ~1 x 10 16 For example, as described in Japanese Patent Application Laid-Open No. 50-35698, the resistivity of TaN contained in the substrate adhesion layer according to the present invention is low, within the range of 100 to 350 μΩcm. 2 O 5The resistivity of the material indicates high insulating properties and high resistivity. Known methods for measuring the resistivity include the two-terminal method, the four-terminal method, and the four-probe method.
[0074] (Method of Forming Substrate Adhesion Layer) The method of forming the substrate adhesion layer according to the present invention is not particularly limited, but the following methods can be applied.
[0075] Examples of methods for forming a substrate adhesion layer that can be applied to the present invention include dry film formation methods such as physical vapor deposition (PVD) and chemical vapor deposition (CVD), and wet film formation methods such as electrolytic plating and electroless plating. In the present invention, however, formation by a dry film formation method is preferred because it allows the formation of a thin, dense film.
[0076] In the present invention, examples of dry film formation methods include sputtering, vacuum deposition, laser ablation, ion plating, electron beam epitaxy (MBE), metal organic chemical vapor deposition (MOCVD), plasma CVD, and plasma etching mode using oxygen gas (O 2 PE mode), reactive ion etching using oxygen gas (O 2 However, from the viewpoint of being able to form a thin, dense film with a high metal element concentration, a sputtering method or a plasma etching mode method using oxygen gas (O 2 PE mode) is preferred.
[0077] In the present invention, among the above-described methods, the method of forming a film by sputtering and then performing a surface treatment by plasma treatment is preferred in that it allows the formation of a desired substrate adhesion layer.
[0078] (Specific Film Forming Method of Substrate Adhesion Layer) Typical film forming methods for the substrate adhesion layer include the following methods. 1. Film formation method: A metal layer (content of 30 to 70 atomic %) consisting of a Group 4 or Group 5 element is formed on a substrate by a sputtering method targeting a Group 4 or Group 5 element, and then the metal layer is subjected to a plasma treatment described below to form a substrate adhesion layer. Note that the following description will be given taking Ta (tantalum) as an example of a metal consisting of a Group 4 or Group 5 element.
[0079] (1) Formation of a substrate adhesion layer by sputtering In the sputtering method, a metal of Group 4 or Group 5 element (e.g., Ta) is used as a target and sputtering is performed in an atmosphere of argon gas, oxygen gas, nitrogen gas, methane, etc. to form a substrate adhesion layer. To form a nitrogen-containing film (nitride film) on a nozzle plate as in the present invention, a method of sputtering using a metal target of Group 4 or Group 5 element in a nitrogen gas atmosphere (reactive sputtering) or a method of sputtering using a metal nitride target of Group 4 or Group 5 element in an argon gas atmosphere can be used. The former (reactive sputtering) is preferred because it is easier to control the film composition to an optimum value.
[0080] A specific example of a film formation method using sputtering is shown below. Under vacuum conditions, a Ta target that had been set in advance on the electrode of a DC sputtering film formation device was sputtered under the following conditions. In this case, not only DC sputtering but also other plasma sources may be used.
[0081] Target: Ta DC power density: 1.1 W / cm 2 Power: 200 W Temperature: 25°C Pressure: 0.3 Pa Introduced gas: argon gas + nitrogen gas Film formation time: 10 min
[0082] (2) Plasma Treatment after Sputtering Plasma etching modes applicable to the present invention include RIE mode and PE mode. The "RIE" (Reactive Ion Etching) mode referred to in the present invention is a method in which a substrate constituting a nozzle plate as a plasma treatment target, such as SUS304, is placed on the power supply electrode side of a pair of opposing flat-plate electrodes, and plasma treatment is performed on the surface of the plasma treatment target. On the other hand, the "PE" (Plasma Etching) mode is a method in which a plasma treatment target is placed on the ground electrode side of a pair of opposing flat-plate electrodes, and plasma treatment is performed on the surface of the plasma treatment target.
[0083] Further details regarding the plasma etching mode will be explained with reference to the accompanying drawings. <RIE Mode Plasma Processing Apparatus> FIG. 6 is a schematic diagram showing an example of a high-frequency plasma processing apparatus in RIE mode (reactive ion etching mode) used to form a substrate adhesion layer. The RIE mode is suitable for physical, high-speed surface processing using ion bombardment. In FIG. 6, the RIE mode high-frequency plasma processing apparatus 20A (hereinafter also referred to as "plasma processing apparatus 20A") includes a reaction chamber 21, a high-frequency power supply 22 (RF (Radio Frequency) power supply), a capacitor 23, a planar electrode 24 (cathode, also referred to as "power supply electrode"), a counter electrode 25 (anode, also referred to as "ground electrode"), a grounding portion 26, and the like. The reaction chamber 21 includes a gas inlet 27 and outlet 28. The planar electrode 24 and the counter electrode 25 are disposed within the reaction chamber 21.
[0084] A pair of electrodes, consisting of a flat electrode 24 connected to a high-frequency power supply 22 via a capacitor 23 and an opposing electrode 25 facing the flat electrode 24 and grounded by a grounding portion 26, is disposed in a sealable reaction chamber 21. A nozzle plate substrate 30 serving as an object to be subjected to plasma processing is disposed on the flat electrode 24.
[0085] First, air is sufficiently removed from the reaction chamber 21 through the gas outlet 28. In this state, a reaction gas G (Ar, O 2 When the high frequency power supply 22 is started while supplying a high frequency power of 3 MHz or more and 100 MHz or less (typically 13.56 MHz) to the high frequency power supply 22, a discharge D occurs between the flat electrode 24 and the counter electrode 25, forming a discharge space 31 in which low temperature plasma (cations and electrons) of the reactive gas G and radical species are generated. At this time, the high frequency power density is preferably set within the range of 0.01 to 3 W / cm.
[0086] In the above configuration, due to the difference in mobility between ions and electrons, electrons are captured by the flat electrode 24, causing the flat electrode 24 to become relatively negatively charged (self-biased). The electrons from the flat electrode 24 travel via the power supply line 33 and are stopped at the capacitor 23. The electrons from the counter electrode 25 flow to the ground 26 via the power supply line 32.
[0087] On the other hand, radical species and positive ions move within the plasma without being easily captured by the electrodes. When a nozzle plate substrate 30 serving as an object to be treated is placed on the planar electrode 24 in this plasma, an ion sheath is generated with a strong electric field on the opposing electrode 25 side of the nozzle plate substrate 30, and an electric field of 400 to 1000 V is generated by cathode fall, causing the positive ions moving within the nozzle plate substrate 30 to collide with or come into contact with the surface of the nozzle plate substrate 30. In this way, surface treatment (etching in this case) of the object to be treated is performed.
[0088] Examples of reactive gases G used in etching include rare gases (e.g., helium gas, neon gas, argon gas, krypton gas, and xenon gas), oxygen gas, and hydrogen gas. In the present invention, an RIE mode plasma processing method using argon gas as the reactive gas G is referred to as "Ar-RIE mode plasma processing," and an RIE mode plasma processing method using oxygen gas as the reactive gas is referred to as "O2-RIE mode plasma processing."
[0089] (Thickness of Substrate Adhesion Layer) In the nozzle plate of the present invention, the thickness of the substrate adhesion layer is generally in the range of 1 to 20,000 nm, but from the viewpoint of nozzle processing and uniformity of the nozzle shape due to the distribution of the substrate adhesion layer deposition, it is preferably in the range of 1 to 5,000 nm, and further from the viewpoint of productivity, it is more preferably in the range of 1 to 1,500 nm.
[0090] <Underlayer> The underlayer according to the present invention is preferably a layer formed between the substrate adhesion layer according to the present invention and the liquid-repellent layer, and contains at least an inorganic oxide or an oxide containing carbon (C).
[0091] The inorganic oxide applicable to the formation of the underlayer according to the present invention is not particularly limited, and examples thereof include oxides and composite oxides of metals such as transition metals, noble metals, alkali metals, alkaline earth metals, etc. More specifically, the inorganic oxide fine particles are preferably oxides or composite oxides containing one or more metal elements selected from silicon, aluminum, titanium, magnesium, zirconium, antimony, iron, and tungsten.
[0092] The oxide or composite oxide may further contain one or more elements selected from phosphorus, boron, cerium, alkali metals, and alkaline earth metals.
[0093] Common inorganic oxides include, for example, aluminum oxide, silica (silicon dioxide), magnesium oxide, zinc oxide, lead oxide, tin oxide, tantalum oxide, indium oxide, bismuth oxide, yttrium oxide, cobalt oxide, copper oxide, manganese oxide, selenium oxide, iron oxide, zirconium oxide, germanium oxide, tin oxide, titanium oxide, niobium oxide, molybdenum oxide, and vanadium oxide.
[0094] In the present invention, the inorganic oxide contained in the underlayer is preferably a layer composed mainly of silicon dioxide, and the inorganic oxide may contain organic substances such as organic groups and resins as secondary components.
[0095] The underlayer is preferably an organic oxide containing at least carbon (C).
[0096] Examples of organic oxides containing carbon (C) include silicon compounds such as silane, tetramethoxysilane, tetraethoxysilane (TEOS), tetra-n-propoxysilane, tetraisopropoxysilane, tetra-n-butoxysilane, tetra-t-butoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, diethyldimethoxysilane, diphenyldimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, phenyltriethoxysilane, (3,3,3-trifluoropropyl)trimethoxysilane, hexamethyldisiloxane, bis-(dimethylamino)dimethylsilane, bis-(dimethylamino)methylvinylsilane, bis-(ethylamino)dimethylsilane, N,O-bis-(trimethylsilyl)acetamide, and bis-(trimethylsilyl). Examples of the titanium compound include titanium methoxide, titanium ethoxide, titanium isopropoxide, titanium tetraisopropoxide, titanium n-butoxide, titanium diisopropoxide (bis-2,4-pentanedionate), titanium diisopropoxide (bis-2,4-ethylacetoacetate), titanium di-n-butoxide (bis-2,4-pentanedionate), titanium acetylacetonate, and butyl titanate dimer. Examples of zirconium compounds include zirconium n-propoxide, zirconium n-butoxide, zirconium t-butoxide, zirconium tri-n-butoxide acetylacetonate, zirconium di-n-butoxide bis-acetylacetonate, zirconium acetylacetonate, zirconium acetate, and zirconium hexafluoropentanedionate.Examples of aluminum compounds include aluminum ethoxide, aluminum triisopropoxide, aluminum isopropoxide, aluminum n-butoxide, aluminum s-butoxide, aluminum t-butoxide, aluminum acetylacetonate, and triethyldialuminum tri-s-butoxide.
[0097] Among the above-mentioned organic oxides containing carbon (C), it is more preferable that the layer containing carbon (C), silicon (Si), and oxygen (O) as main components is formed using a silane compound (e.g., alkoxysilane, silazane, etc.) having a molecular weight of 300 or less or a silane coupling agent.
[0098] The underlayer according to the present invention is preferably a layer formed using a silane coupling agent, and more preferably, the silane coupling agent contained in the underlayer has reactive functional groups at both ends and contains a hydrocarbon chain and a benzene ring in the middle.
[0099] As a specific configuration of the underlayer, for example, as an inorganic oxide applicable to the underlayer of the present invention, a preferred embodiment (first underlayer) is one in which the underlayer has reactive functional groups at both ends and forms a high-density polymer film by a dehydration condensation reaction of a silane coupling agent A containing a hydrocarbon chain and a benzene ring in the middle, and another preferred embodiment (second underlayer) is one in which the underlayer is composed of an oxide mainly composed of an inorganic oxide or an organic oxide containing at least Si.
[0100] (Formation of base layer using silane coupling agent A: first base layer) In the present invention, it is preferable to use, as the silane coupling agent used to form the base layer by a dehydration condensation reaction, a silane coupling agent A having reactive functional groups at both ends and containing a hydrocarbon chain and a benzene ring in the middle.
[0101] There are no particular restrictions on the silane coupling agent A that can be used in the underlayer, and any conventionally known compound that satisfies the above requirements can be appropriately selected and used. However, from the viewpoint of fully achieving the intended effects of the present invention, it is preferable that the silane coupling agent A be a compound represented by the following general formula (1), which has an alkoxy group, chlorine, an acyloxy group, or an amino group as reactive functional groups at both ends, and has a structure containing a hydrocarbon chain and a benzene ring (phenylene group) in the middle.
[0102] <Compound having a structure represented by general formula (1)> General formula (1): XsQ 3 -sSi(CH 2 ) tC 6 H 4 (CH 2 ) uSiR 3 -mXm In the above general formula (1), Q and R each represent a methyl group or an ethyl group. t and u each represent a natural number from 1 to 10. s and m each represent a natural number from 1 to 3. When s is 1 and m is 1, there are two Qs and two Rs, and the two Qs and Rs may have the same structure or different structures. C 6 H 4 is a phenylene group, and X represents an alkoxy group, chlorine, an acyloxy group, or an amino group.
[0103] Examples of the alkoxy group include alkoxy groups having 1 to 12 carbon atoms, such as methoxy, ethoxy, propoxy, and butoxy groups, preferably alkoxy groups having 1 to 8 carbon atoms, and more preferably alkoxy groups having 1 to 6 carbon atoms.
[0104] Examples of the acyloxy group include linear or branched acyloxy groups having 2 to 19 carbon atoms (acetoxy, ethylcarbonyloxy, propylcarbonyloxy, isopropylcarbonyloxy, butylcarbonyloxy, isobutylcarbonyloxy, sec-butylcarbonyloxy, tert-butylcarbonyloxy, octylcarbonyloxy, tetradecylcarbonyloxy, and octadecylcarbonyloxy).
[0105] The amino group is an amino group (-NH 2) and substituted amino groups having 1 to 15 carbon atoms (for example, methylamino, dimethylamino, ethylamino, methylethylamino, diethylamino, n-propylamino, methyl-n-propylamino, ethyl-n-propylamino, n-propylamino, isopropylamino, isopropylmethylamino, isopropylethylamino, diisopropylamino, phenylamino, diphenylamino, methylphenylamino, ethylphenylamino, n-propylphenylamino, and isopropylphenylamino).
[0106] Exemplary compounds having a structure represented by general formula (1) according to the present invention are listed below, but the present invention is not limited to these exemplary compounds.
[0107] 1) 1,4-bis(trimethoxysilylethyl)benzene 2) 1,4-bis(triethoxysilylethyl)benzene 3) 1,4-bis(trimethoxysilylbutyl)benzene 4) 1,4-bis(triethoxysilylbutyl)benzene 5) 1,4-bis(trimethylaminosilylethyl)benzene 6) 1,4-bis(triethylaminosilylethyl)benzene 7) 1,4-bis(trimethylaminosilylbutyl)benzene 7) 1,4-bis(triacetoxysilylethyl)benzene 8) 1,4-bis(trichloromethylsilylethyl)benzene 9) 1,4-bis(trichloroethylsilylethyl)benzene The compound having a structure represented by general formula (1) according to the present invention can be synthesized according to a conventionally known synthesis method. It is also available as a commercially available product.
[0108] <Method for forming an underlayer using silane coupling agent A> The underlayer according to the present invention is formed by dissolving the silane coupling agent A according to the present invention, which has reactive functional groups at both ends and contains a hydrocarbon chain and a benzene ring in the middle, to a desired concentration in an organic solvent such as ethanol, propanol, butanol, or 2,2,2-trifluoroethanol to prepare a coating liquid for forming an underlayer, and then applying and drying the resulting solution on a substrate by a wet coating method.
[0109] The concentration of the silane coupling agent A in the coating liquid for forming the undercoat layer is not particularly limited, but is generally in the range of 0.5 to 50% by mass, and preferably in the range of 1.0 to 30% by mass.
[0110] The thickness of the first underlayer according to the present invention is not particularly limited, but is preferably in the range of about 1 to 500 nm, and more preferably in the range of 5 to 200 nm.
[0111] (Formation of Underlayer Composed of Oxide Containing Si-Containing Organic Oxide as Main Component: Second Underlayer) In the underlayer according to the present invention, a preferred embodiment is a second underlayer composed of an oxide composed of Si-containing organic oxide as a main component.
[0112] Preferably, as shown in Figure 2, the base layer 41 is composed of two layers, a first base layer 41a and a second base layer 41b, where the first base layer 41a is composed of a first base layer having reactive functional groups at both ends as described above and containing silane coupling agent A containing a hydrocarbon chain and a benzene ring in the middle, and the second base layer 41b is composed of a second base layer composed of an organic oxide containing Si as described below.
[0113] Examples of alkoxysilanes, silazanes, or silane coupling agents having a molecular weight of 300 or less that can be used in the present invention are shown below, but the present invention is not limited to these examples. The numerical value in parentheses after each compound is the molecular weight (Mw).
[0114] Examples of alkoxysilanes include tetraethoxysilane (Si(OCH) , Mw: 208.3), methyltriethoxysilane (CHSi(OCH) , Mw: 178.3), methyltrimethoxysilane (CHSi(OCH) , Mw: 136.2), dimethyldiethoxysilane ((CH)Si(OCH) , Mw: 148.3), and dimethyldimethoxysilane ((CH)Si(OCH) , Mw: 120.2).
[0115] Examples of silazanes include 1,1,1,3,3,3-hexamethyldisilazane ((CH)SiNHSi(CH), 161.4), 1,1,1,3,3,3-hexaethyldisilazane ((CH)SiNHSi(CH)), 245.4), and others such as 1,3-bis(chloromethyl)tetramethyldisilazane and 1,3-divinyl-1,1,3,3-tetramethyldisilazane.
[0116] Examples of silane coupling agents include 1) vinyl silane coupling agents: vinyltrimethoxysilane (CH2=CHSi(OCH3)3, Mw: 148.2), vinyltriethoxysilane (CH2=CHSi(OC2H5)3, Mw: 190.3), and others such as CH2=CHSi(CH3)(OCH3)2, CH2=CHCOO(CH2)2Si(OCH3)3, CH2=CHCOO(CH2)2Si(CH3)Cl2, CH2=CHCOO(CH2)3SiCl3, CH2=C(CH3)Si(OC2H5)3, etc.
[0117] 2) Amino-based silane coupling agents: Examples include 3-aminopropyltrimethoxysilane (HNCHCHCHSi(OCH) , mW: 179.3), 3-(2-aminoethylamino)propyltrimethoxysilane (HNCHCHNHCHCHCHSi(OCH) , Mw: 222.4), and 3-(2-aminoethylamino)propylmethyldimethoxysilane (HNCHCHNHCHCHCHSi(CH)(OCH) , Mw: 206.4).
[0118] 3) Epoxy-based silane coupling agents: Examples include 3-glycidoxypropyltrimethoxysilane (Mw: 236.3) and 3-glycidoxypropyltriethoxysilane (Mw: 278.4).
[0119] <Method for forming second underlayer> The second underlayer according to the present invention is formed by dissolving a silane compound according to the present invention having a molecular weight of 300 or less, such as a conventionally known alkoxysilane, silazane, or silane coupling agent, to a desired concentration in an organic solvent, such as ethanol, propanol, butanol, or 2,2,2-trifluoroethanol, to prepare a coating solution for forming an intermediate layer, and then coating and drying the coating solution on the underlayer by a wet coating method.
[0120] The concentration of the inorganic oxide forming material in the second underlayer forming coating liquid is not particularly limited, but is generally in the range of 0.5 to 50% by mass, and preferably in the range of 1.0 to 30% by mass.
[0121] The thickness of the second underlayer according to the present invention is in the range of 0.5 to 500 nm, preferably in the range of 1 to 300 nm, and more preferably in the range of 5 to 100 nm.
[0122] <Liquid-Repellent Layer> In the present invention, the liquid-repellent layer (also referred to as "water-repellent layer") preferably contains a coupling agent containing fluorine (F) (hereinafter also referred to as coupling agent B).
[0123] The coupling agent B having fluorine (F) that can be used in the liquid-repellent layer according to the present invention is not particularly limited, but preferably contains a fluorine-based compound, and the fluorine-based compound is (1) a compound having a perfluoroalkyl group that contains at least an alkoxysilyl group, a phosphonic acid group, or a hydroxy group, or a compound having a perfluoropolyether group that contains an alkoxysilyl group, a phosphonic acid group, or a hydroxy group, or (2) a mixture containing a compound having a perfluoroalkyl group, or a mixture containing a compound having a perfluoropolyether group.
[0124] Specific compounds of the coupling agent B having fluorine (F) that can be used in the liquid-repellent layer according to the present invention include chlorodimethyl[3-(2,3,4,5,6-pentafluorophenyl)propyl]silane, pentafluorophenyldimethylchlorosilane, pentafluorophenylethoxydimethylsilane, pentafluorophenylethoxydimethylsilane, trichloro(1H,1H,2H,2H-tridecafluoro-n-octyl)silane, trichloro(1H,1H,2H,2H-heptadecafluorodecyl)silane, trimethoxy(3,3,3-trifluoropropyl)silane, triethoxy(1H,1H,2H,2H-nonafluorohexyl)silane, and silane, triethoxy-1H,1H,2H,2H-heptadecafluorodecylsilane, trimethoxy(1H,1H,2H,2H-heptadecafluorodecyl)silane, trimethoxy(1H,1H,2H,2H-nonafluorohexyl)silane, trichloro[3-(pentafluorophenyl)propyl]silane, trimethoxy(11-pentafluorophenoxyundecyl)silane, triethoxy[5,5,6,6,7,7,7-heptafluoro-4,4-bis(trifluoromethyl)heptyl]silane, trimethoxy(pentafluorophenyl)silane, triethoxy(1H,1H,2H,2H-nonafluorohexyl)silane, and the like.
[0125] Furthermore, fluorine (F)-containing silane coupling agents are also available as commercially available products, and are marketed by, for example, Dow Corning Toray Silicone Co., Ltd., Shin-Etsu Chemical Co., Ltd., Daikin Industries, Ltd. (e.g., Optool DSX), Asahi Glass Co., Ltd. (e.g., Cytop), Seco Corporation (e.g., TopCleanSafe (registered trademark)), Fluorotechnology Co., Ltd. (e.g., Fluorosurf), Gelest Inc. Solvay Solexis K.K. (e.g., Fluorolink S10), and the like, and can be easily obtained. In addition, for example, they are described in J. Fluorine Chem., 79(1), 87(1996), Materials Technology, 16(5), 209(1998), Collect. Czech. Chem. Commun., Vol. 44, pp. 750-755, J. Examples of such compounds include those described in Amer. Chem. Soc., 1990, Vol. 112, pp. 2341-2348, Inorg. Chem., Vol. 10, pp. 889-892, 1971, and U.S. Pat. No. 3,668,233. Furthermore, the compounds can be produced by the synthesis methods described in JP-A-58-122979, JP-A-7-242675, JP-A-9-61605, JP-A-11-29585, JP-A-2000-64348, JP-A-2000-144097, or synthetic methods similar thereto.
[0126] Specifically, examples of compounds having a silane group-terminated perfluoropolyether group include the above-mentioned "Optool DSX" manufactured by Daikin Industries, Ltd., examples of compounds having a silane group-terminated fluoroalkyl group include, for example, "FG-5010Z130-0.2" manufactured by Fluorosurf Corporation, examples of polymers having a perfluoroalkyl group include, for example, the "SF Coat Series" manufactured by AGC Seimi Chemical Co., Ltd., and examples of polymers having a fluorine-containing heterocyclic structure in the main chain include, for example, "Cytop" manufactured by Asahi Glass Co., Ltd. Also included are mixtures of FEP (tetrafluoroethylene-hexafluoropropylene copolymer) dispersions and polyamideimide resins.
[0127] Furthermore, as a coupling agent having fluorine (F) at a position other than the silane group terminal, a phosphonic acid derivative having a fluorinated alkyl chain (for example, FOPA) manufactured by Dojindo Laboratories, Inc. can also be used.
[0128] In a method for forming a liquid-repellent layer by PVD, a fluoroalkylsilane mixed oxide, Evaporation Substance WR1 or WR4, manufactured by Merck Japan, is used as a fluorine-based compound, and it is preferable to form a silicon oxide layer in advance as a base layer when forming a liquid-repellent layer using WR1 on a silicon substrate. The liquid-repellent layer formed using WR1 or WR4 exhibits liquid-repellent properties against organic solvents such as alcohols such as ethanol, ethylene glycol (including polyethylene glycol), thinners, and paints in addition to water.
[0129] The thickness of the liquid-repellent layer according to the present invention is generally within the range of 1 to 500 nm, preferably within the range of 1 to 400 nm, and more preferably within the range of 2 to 200 nm.
[0130] [Method for manufacturing an inkjet head member] In the method for manufacturing an inkjet head member of the present invention, the substrate adhesion layer is formed on the substrate, the functional layer is formed on the substrate adhesion layer, and then a nozzle is formed by laser processing. In particular, it is preferable that the substrate adhesion layer is formed by a reactive sputtering method using a dry process, and it is preferable that the surface of the substrate adhesion layer is treated by oxygen plasma.
[0131] As an example of a method for manufacturing an inkjet head component, a method for manufacturing a nozzle plate using the above-mentioned underlayer and liquid-repellent layer as functional layers will be described below. The method for manufacturing the nozzle plate, as detailed above, includes: 1) forming a substrate adhesion layer on the substrate; 2) configuring the surface of the substrate adhesion layer on the functional layer side so that the atomic concentration of oxygen elements is higher than that inside the substrate adhesion layer; 3) then forming a substrate adhesion layer on the substrate adhesion layer using an inorganic oxide or an oxide containing carbon (C); 4) then forming a liquid-repellent layer on the substrate adhesion layer using a coupling agent containing fluorine (F); and 5) then forming a nozzle by laser processing the substrate, substrate adhesion layer, underlayer, and liquid-repellent layer.
[0132] The above-mentioned FIG. 2 is a schematic cross-sectional view showing an example of the configuration of the nozzle hole portion of the nozzle plate according to the present invention.
[0133] As shown in FIG. 2, a nozzle portion N having a desired shape as an ink ejection portion is formed in the substrate 2, the substrate adhesion layer 3, the underlayer 41, and the liquid-repellent layer .
[0134] Regarding specific methods for forming the nozzle holes and the like, for example, JP-A-005-533662, JP-A-2007-152871, JP-A-2007-313701, JP-A-2009-255341, JP-A-2009-274415, JP-A-2009-286036, JP-A-2010-023446, JP-A-2011-011425, JP-A-2013-202886, JP-A-2014-144485, JP-A-2018-083316, JP-A-2018-111208, etc. Methods described therein can be referenced, and detailed description thereof will be omitted here.
[0135] The nozzle plate manufactured as described above can achieve both durability in the manufacturing process and adhesion between the substrate and the undercoat layer and liquid-repellent layer, and can also ensure long-term durability against ink and abrasion resistance.
[0136] In the nozzle plate of the present invention, the nozzle holes are preferably formed by laser processing.
[0137] In the manufacturing method of the nozzle plate according to the present invention, it is preferable to use a laser for processing the outer shape of the nozzle holes, and it is further preferable that the laser is a pulsed laser or a CW laser.
[0138] As a laser that can be used in the manufacture of the nozzle plate according to the present invention, it is preferable to use a continuous wave laser beam (CW laser beam) or a pulsed wave laser beam (pulse laser beam).
[0139] The laser beams that can be used here include gas lasers such as Ar lasers, Kr lasers, and excimer lasers, and single crystal YAG and YVO 4 , forsterite (Mg 2 SiO 4 ), YAlO 3 , GdVO 4 , YLF, or polycrystalline (ceramic) YAG, Y 2 O 3 , Y.V.O. 4 , YAlO 3 , GdVO 4 Examples of lasers include lasers that use a medium containing one or more of Nd, Yb, Cr, Ti, Ho, Er, Tm, and Ta as a dopant, and lasers that oscillate from one or more of a glass laser, a ruby laser, an alexandrite laser, a Ti:sapphire laser, a copper vapor laser, and a gold vapor laser.
[0140] Among these, the laser used emits ultraviolet laser light with a wavelength of about 266 nm, for example, YAG-UV (yttrium aluminum garnet crystal: wavelength 266 nm) or YVO 4 (Wavelength: 355 nm) is preferred. In particular, when a laser with a wavelength of about 266 nm is used, if the object to be processed is an organic material, it is possible to dissociate molecular bonds such as C-H bonds and C-C bonds by thermal action.
[0141] As an example of irradiation conditions, for example, for YAG-UV (wavelength 266 nm), the pulse width is 12 nsec and the output is 1.6 W, and for YVO4 (wavelength: 355 nm), the pulse width is 18 nsec and the output is 2.4 W.
[0142] Furthermore, the duration is approximately 10 -11 Seconds (10 psec) to 10 -14 Ultrafast lasers produce intense laser pulses of about 10 fsec (10 fs) in duration, and pulses of about 10-10 sec (100 psec) to 10 -11 Short pulse lasers are also available that produce intense laser pulses on the order of 10 psec. These pulsed lasers are also useful for cutting or drilling a wide range of materials.
[0143] [Inkjet head] Fig. 7 is a schematic external view showing an example of the structure of an inkjet head to which the nozzle plate according to the present invention can be applied, and Fig. 8 is a bottom view of an inkjet head equipped with the nozzle plate according to the present invention.
[0144] 7, an inkjet head 100 equipped with a nozzle plate according to the present invention is mounted on an inkjet printer (not shown), and includes a head chip that ejects ink from nozzles, a wiring substrate on which the head chip is disposed, a drive circuit substrate connected to the wiring substrate via a flexible substrate, a manifold that introduces ink into channels of the head chip via a filter, a housing 56 inside which the manifold is housed, a cap receiving plate attached to cover an opening in the bottom surface of the housing 56, first and second joints 81a and 81b attached to first and second ink ports of the manifold, a third joint 82 attached to a third ink port of the manifold, and a cover member 59 attached to the housing 56. Also, mounting holes 68 are formed in each housing 56 for mounting the housing 56 to the printer main body.
[0145] 8 is formed as a generally rectangular plate having an outer shape that is elongated in the left-right direction in accordance with the shape of the cap receiving plate attachment portion 62, and is provided with a nozzle opening 71 that is elongated in the left-right direction in the approximate center thereof to expose the nozzle plate 61 in which the plurality of nozzles N are arranged. Furthermore, for the specific structure inside the inkjet head shown in FIG. 7, reference can be made to, for example, FIG. 2 described in JP-A-2012-140017.
[0146] 7 and 8 show representative examples of inkjet heads, but other inkjet heads having configurations described in, for example, JP 2012-140017 A, JP 2013-010227 A, JP 2014-058171 A, JP 2014-097644 A, JP 2015-142979 A, JP 2015-142980 A, JP 2016-002675 A, JP 2016-002682 A, JP 2016-107401 A, JP 2017-109476 A, JP 2017-177626 A, etc. can also be appropriately selected and applied.
[0147] [Inkjet Ink] There are no particular limitations on the inkjet ink that can be applied to the inkjet recording method using the inkjet head of the present invention, and various types of inkjet inks are available, such as water-based inkjet inks that contain water as the main solvent, oil-based inkjet inks that contain mainly a non-volatile solvent that does not volatilize at room temperature and are substantially free of water, organic solvent-based inkjet inks that contain mainly a solvent that volatilizes at room temperature and are substantially free of water, hot-melt inks that are printed by heating and melting ink that is solid at room temperature, and actinic ray-curable inkjet inks that are cured by actinic rays such as ultraviolet light after printing. However, in the present invention, the application of an alkaline ink is a preferred embodiment from the viewpoint of being able to exert the effects of the present invention.
[0148] Inks include, for example, alkaline inks and acidic inks. In particular, alkaline inks may cause chemical deterioration of the substrate, the liquid-repellent layer, and the nozzle formation surface. In inkjet recording methods using such alkaline inks, it is particularly effective to apply an inkjet head equipped with the nozzle plate of the present invention.
[0149] Specifically, inks applicable to the present invention include coloring materials such as dyes and pigments, water, water-soluble organic solvents, pH adjusters, etc. Examples of water-soluble organic solvents that can be used include ethylene glycol, propylene glycol, diethylene glycol, dipropylene glycol, glycerin, triethylene glycol, ethanol, and propanol. Examples of pH adjusters that can be used include sodium hydroxide, potassium hydroxide, sodium acetate, sodium carbonate, sodium bicarbonate, alkanolamines, hydrochloric acid, and acetic acid.
[0150] When sodium hydroxide, potassium hydroxide, sodium acetate, sodium carbonate, sodium bicarbonate, alkanolamine, or the like is used as a pH adjuster, the ink becomes alkaline and becomes an alkaline ink (liquid) that may cause chemical damage (chemical deterioration) to the liquid-repellent layer and the nozzle formation surface. Alkaline ink has a pH of 8.0 or higher.
[0151] As described above, the liquid-repellent layer is formed from a fluorine-containing silane coupling agent or the like. The liquid-repellent layer has a structure in which a partial structure containing silicon and a partial structure containing fluorine are bonded by a substituent such as a methylene group (CH). The bond energy between carbon (C) and carbon (C) is smaller than the bond energy between silicon (Si) and oxygen (O) and the bond energy between carbon (C) and fluorine (F). Therefore, the bond between carbon (C) and carbon (C) is weaker than the bond between silicon (Si) and oxygen (O) and the bond between carbon (C) and fluorine (F), and is therefore more susceptible to mechanical and chemical damage.
[0152] In ink jet recording methods using alkaline inks that are prone to such phenomena, it is effective to apply a nozzle plate having the structure specified in the present invention in terms of improving durability.
[0153] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these. In the following examples, unless otherwise specified, operations were carried out at room temperature (25°C). Furthermore, unless otherwise specified, "%" and "parts" mean "% by mass" and "parts by mass", respectively.
[0154] Example 1 [Preparation of Nozzle Plate 1] A nozzle plate 1 composed of the substrate 2 / substrate adhesion layer 3 / first underlayer 41a / second underlayer 41b / liquid-repellent layer 42 shown in FIG. 2 was prepared according to the following method.
[0155] (1) Preparation of Substrate As the substrate, a stainless steel substrate (SUS304) having a length of 3 cm, a width of 8 cm and a thickness of 50 μm and having not been subjected to any surface treatment was used.
[0156] (2) Formation of TaN Layer (Substrate Adhesion Layer X) by Sputtering Method In the sputtering method, Ta was used as a target and sputtering film formation was carried out on the substrate in an atmosphere of argon gas and nitrogen gas to form a metal nitride film layer.
[0157] Specifically, under vacuum conditions, a Ta target that had been set in advance on an electrode of a DC sputtering film-forming apparatus was sputtered under the following conditions.
[0158] Target: Ta DC power density: 1.1 W / cm 2 Power: 200 W Temperature: 25°C Pressure: 0.3 Pa Introduced gas: argon gas + nitrogen gas Film formation time: 10 min Layer thickness: 20 nm
[0159] (3) Formation of First Underlayer (Preparation of Coating Liquid for Forming First Underlayer) <Preparation of Liquid A-1> The following constituent materials were mixed to prepare Liquid A-1. A mixed solution of ethanol and 2,2,2-trifluoroethanol (volume ratio 8:2) 30 mL Silane coupling agent a: 1,4-bis(trimethoxysilylethyl)benzene ((CH 3 O) 3 Si(CH 2 ) 2 (C 6 H 4 ) (CH 2 ) 2 Si(OCH 3 ) 3 ) (see below) 2 mL <Preparation of A-2 solution> Mixture of ethanol and 2,2,2-trifluoroethanol (volume ratio 8:2) 19.5 mL Pure water 30 mL Hydrochloric acid (36% by volume) 0.5 mL
[0160] (Formation of First Underlayer) While stirring the prepared A-1 solution with a stirrer, 5 mL of A-2 solution was added dropwise. After stirring for about 1 hour after the addition, this mixed solution was applied onto the substrate adhesion layer by spin coating under conditions such that the thickness of the first underlayer after drying would be 100 nm. The spin coating conditions were 5000 rpm for 20 seconds. Thereafter, the substrate was dried at room temperature for 1 hour and then baked at 200°C for 30 minutes.
[0161] (4) Formation of Second Underlayer (Preparation of Coating Solution for Forming Second Underlayer) The following constituent materials were mixed to prepare a coating solution for forming a second underlayer. Mixed solution of ethanol and 2,2,2-trifluoroethanol (volume ratio 8:2) 69 mL Pure water 30 mL Silane coupling agent c: 3-aminopropyltriethoxysilane ((C 2 H 5 O) 3 SiC 3 H6 NH 2 ), Shin-Etsu Chemical Co., Ltd. KBE-903) (see below) 1 mL
[0162] (Formation of Second Underlayer) The second underlayer-forming coating solution (KBE-903 concentration: 1.0% by volume) prepared above was applied onto the first underlayer of the substrate by spin coating under conditions such that the thickness of the second underlayer after drying would be 20 nm. The spin coating conditions were 3000 rpm and 20 seconds. The substrate was then dried at room temperature for 1 hour and then heat-treated at 90°C and 80% RH for 1 hour.
[0163] (5) Formation of Liquid-Repellent Layer (Preparation of Coating Liquid for Forming Liquid-Repellent Layer) The following constituent materials were mixed to prepare a coating liquid for forming a liquid-repellent layer.
[0164] Mixture of ethanol and 2,2,2-trifluoroethanol (volume ratio 8:2) 69.8 mL Pure water 30 mL Fluorine-containing coupling agent b: (2-perfluorooctyl)ethyltrimethoxysilane (CF 3 (CF 2 ) 7 C 2 H 4 Si(OCH 3 ) 3 ) 0.2mL
[0165] (Formation of Liquid-Repellent Layer) The liquid-repellent layer-forming coating solution containing 0.2 volume % of the fluorine-containing coupling agent b (see below) prepared above was applied to the second underlayer formed above by spin coating under conditions such that the liquid-repellent layer would have a thickness of 10 nm after drying. The spin coating conditions were 1000 rpm and 20 seconds. The substrate was then dried at room temperature for 1 hour, and then heat-treated at 90°C and 80% RH for 1 hour to produce a nozzle plate 1.
[0166]
[0167] [Production of Nozzle Plate 2] In the production of the nozzle plate 1, after forming the substrate adhesion layer, O 2 Nozzle plate 2 was produced in the same manner except that the treatment was carried out in the RIE plasma mode.
[0168] The plasma treatment conditions were as follows: Plasma treatment apparatus: RIE mode high frequency plasma apparatus; Reactive gas G: oxygen gas; Gas flow rate: 30 sccm; Gas pressure: 10 Pa; High frequency power: 13.56 MHz; High frequency power density: 0.10 W / cm 2 Inter-electrode voltage: 450 W Treatment time: 5 min
[0169] [Preparation of Nozzle Plate 3] Nozzle plate 3 was prepared in the same manner as in the preparation of nozzle plate 1, except that after forming the substrate adhesion layer, a treatment in Ar-RIE plasma mode was carried out using a high-frequency plasma device by the following method.
[0170] The plasma treatment conditions were as follows: Plasma treatment apparatus: RIE mode high frequency plasma apparatus; Reactive gas G: Argon gas; Gas flow rate: 50 sccm; Gas pressure: 10 Pa; High frequency power: 13.56 MHz; High frequency power density: 0.10 W / cm 2 Inter-electrode voltage: 450 W Treatment time: 5 min
[0171] [Preparation of Nozzle Plate 4] Nozzle plate 4 was prepared in the same manner as in the preparation of nozzle plate 1, except that a Ti target was used to form the substrate adhesion layer by the following method.
[0172] Target: Ti DC power density: 1.1 W / cm 2 Power: 200 W Temperature: 25°C Pressure: 0.3 Pa Introduced gas: argon gas + nitrogen gas Film formation time: 6 min
[0173] [Preparation of Nozzle Plate 5] Nozzle plate 5 was prepared in the same manner as in the preparation of nozzle plate 1, except that a Ta target was used to form the substrate adhesion layer by the following method.
[0174] Target: Ta DC power density: 1.1 W / cm 2 Power: 200 W Temperature: 25°C Pressure: 0.3 Pa Introduced gas: argon gas Film formation time: 2 min 30 sec
[0175] [Preparation of Nozzle Plate 6] Nozzle plate 5 was prepared in the same manner as in the preparation of nozzle plate 1, except that a Ti target was used to form the substrate adhesion layer by the following method.
[0176] Target: Ti DC power density: 1.1 W / cm 2 Power: 200 W Temperature: 25°C Pressure: 0.3 Pa Introduced gas: argon gas Film formation time: 1 min 30 sec
[0177] For each of the produced nozzle plates, the composition of the substrate adhesion layer in the thickness direction was analyzed by the above-mentioned XPS analysis, and the elemental composition of the surface and inside of the substrate adhesion layer is shown in the table below. Specific conditions are as follows: Analysis device: QUANTERA SXM manufactured by ULVAC-PHI, Inc. X-ray source: Monochromated Al-Kα 15 kV 25 W Sputter ions: Ar (1 keV) Depth profile: SiO 2 Measurements were repeated at predetermined thickness intervals using the converted sputtering thickness to obtain a depth profile in the depth direction. The thickness interval was 2.6 nm (data was obtained every 2.6 nm in the depth direction). Quantitation: The background was determined using the Shirley method, and quantitation was performed using the relative sensitivity factor method from the obtained peak area. Data processing was performed using a MultiPak manufactured by ULVAC-PHI, Inc.
[0178] [Evaluation] (1) Evaluation of ink durability (Formation of nozzle holes) A plurality of nozzle holes having a diameter of 25 μm and having the configuration shown in FIG. 1 or 2 were formed in the nozzle plates 1 to 6 prepared above using a laser processing machine.
[0179] (Preparation of Actual Ink for Evaluation: Disperse Dye Ink) <Preparation of Dispersion> Disperse dye: C.I. Disperse Yellow 160 24.0% by mass, diethylene glycol 30.6% by mass, styrene-maleic anhydride copolymer (dispersant) 12.0% by mass, water 33.4% by mass. The above mixture was dispersed using ceramic beads having a diameter of 0.5 mm in a sand grinder manufactured by Imex Co., Ltd. at a rotation speed of 2500 rpm for 5 hours. This dispersion was diluted with water / diethylene glycol = 1:4 so that the dye concentration was 5% to prepare Dispersion 1.
[0180] <Preparation of Experimental Ink> Each composition was added to the above-mentioned Dispersion 1 and stirred to prepare an experimental ink (disperse dye ink) for evaluation. Dispersion 1 20.0 mass% Ethylene glycol 10.0 mass% Glycerin 8.0 mass% Emulgen 911 (manufactured by Kao Corporation) 0.05 mass% Ion-exchanged water was added to make up to 100 mass%. The liquid property of the ink thus prepared was investigated, and it was confirmed to be alkaline (pH 8.0 or higher).
[0181] (Evaluation of Nozzle Plate) The nozzle plate having each nozzle hole formed therein was immersed in the actual ink at 65° C. for 40 days.
[0182] After the immersion treatment, the sample was washed with pure water and dried, and then the presence or absence of peeling between the substrate and the substrate adhesive layer inside the nozzle hole as shown in Figure 1 or Figure 2 was observed with a 100x magnifying glass, and the adhesion durability of the nozzle hole to actual ink was evaluated according to the following criteria: AAA: No peeling was observed in any of the nozzles AA: Very weak peeling was observed in less than 5% of the nozzles, but this is not a problem in practical use A: Weak separation was observed in 5% or more but less than 10% of the nozzles, and the quality is acceptable in practical use B: Clear peeling was observed in some nozzles, and the quality is problematic in practical use
[0183] (2) Scratch Resistance (Wiping Resistance) (Preparation of Black Ink) A black ink for evaluation was prepared consisting of the following components. <Preparation of Black Pigment Dispersion> C.I. Pigment Black 6 12 g, PB822 (Ajinomoto Fine-Tech Co., Ltd.) 5 g, methyl isopropyl sulfone 5 g, triethylene glycol monobutyl ether 68 g, ethylene glycol diacetate 10 g. The above ingredients were mixed and dispersed in a horizontal bead mill filled with 0.3 mm zirconia beads at a volume ratio of 60%, to obtain a black pigment dispersion. The average particle size was 125 nm.
[0184] <Preparation of Black Ink> Black pigment dispersion 33 g Ethylene glycol monobutyl ether 57 g Triethylene glycol monomethyl ether acetate 6.7 g N-methyl-2-pyrrolidone 3.3 g
[0185] (Wiping test) Each nozzle plate, in which a plurality of nozzle holes had been formed by the above-mentioned method using fixed metallurgy, was fixed with the liquid-repellent layer facing up in a container containing the black ink prepared above at 25°C, and the surface of the liquid-repellent layer of the nozzle plate was subjected to multiple wiping operations using a wiper blade made of ethylene propylene diene rubber, and the abrasion durability was evaluated according to the following criteria. AAA: Even after 5,000 or more wiping operations, no peeling of the liquid-repellent layer was observed near the nozzles for any of the nozzles. AA: After fewer than 5,000 wiping operations, no peeling of the liquid-repellent layer was observed near the nozzles for any of the nozzles, but after 5,000 or more wiping operations, very weak peeling was observed for less than 5% of the nozzles. A: After fewer than 1,000 wiping operations, no peeling of the liquid-repellent layer was observed near the nozzles for any of the nozzles, but after 1,000 to 5,000 wiping operations, very weak peeling was observed for less than 5% of the nozzles. B: After 1,000 wiping operations, it was confirmed that nozzles had obvious peeling of the liquid-repellent layer, which would be a problem in practical use,
[0186] (3) Evaluation of continuous jetting property An ink consisting of a black pigment dispersion and triethylene glycol monomethyl ether acetate was introduced into an inkjet head to which nozzles made with Example Nozzle Plates 1 to 4 and Comparative Example Nozzle Plates 5 and 6 were joined, and continuous jetting was carried out from all nozzles with a gap to the media of about 6 mm. The jetting (continuous jetting property) after 30 minutes of continuous jetting was evaluated according to the following criteria: A: No noticeable adhesion of droplets to the nozzle surface was observed even after 30 minutes of continuous jetting, and normal jetting was maintained. B: Clear adhesion of droplets was observed to the nozzle surface after 30 minutes of continuous jetting, and partial jetting defects were confirmed.
[0187]
[0188] As shown by the above results, the nozzle plate having the configuration specified in the present invention, compared to the comparative example, has a substrate adhesion layer containing nitrogen and a higher oxygen concentration at the surface than inside, which means that the bond between the substrate adhesion layer and the underlayer is strong and the ink resistance is excellent, even in an environment where it is exposed to ink components for a long period of time. Furthermore, evaluation of continuous ejection properties showed that there was little adhesion of droplets to the nozzle surface having a substrate adhesion layer containing nitrogen. This phenomenon is thought to be due to the low surface resistance of the substrate adhesion layer containing nitrogen (when a UA probe (2-pin type) was attached to a Hiresta-UX manufactured by Nitto Seiko Analytech to check, the resistance value was below the measurement limit, so the nozzle surface was not charged and mist adhesion due to ejection was suppressed).
[0189] Example 2: Nozzle plates 7 to 10 were produced by forming a liquid-repellent layer (fluorine-containing coupling agent) directly on the substrate adhesion layer without providing the first and second underlayers in the production of nozzle plates 1 to 4 in Example 1. In this case, Optool DSX (manufactured by Daikin Industries, Ltd.) was used as the fluorine-containing coupling agent instead of the fluorine-containing coupling agent b. Furthermore, in the production of nozzle plates 1 to 4 in Example 1, nozzle holes were formed in a stainless steel substrate (SUS304) by laser processing, and then a substrate adhesion layer was formed by sputtering, and a liquid-repellent layer (fluorine-containing coupling agent) was directly formed on the substrate adhesion layer to produce nozzle plates 11 to 14. In this case, Optool DSX (manufactured by Daikin Industries, Ltd.) was used as the fluorine-containing coupling agent instead of the fluorine-containing coupling agent b. Furthermore, nozzle plates 15 and 16 were produced in the same manner as plate 12, except that the thickness of the substrate adhesion layer was changed as shown in Table III below by changing the film formation time. The film formation conditions for nozzle plates 15 and 16 are shown below.
[0190] (Nozzle plate 15) Target: Ta DC power density: 1.1 W / cm 2 Power: 200 W Temperature: 25°C Pressure: 0.3 Pa Introduced gas: argon gas + nitrogen gas Film formation time: 100 min Layer thickness: 200 nm
[0191] (Nozzle plate 16) Target: Ta DC power density: 1.1 W / cm 2 Power: 200 W Temperature: 25°C Pressure: 0.3 Pa Introduced gas: argon gas + nitrogen gas Film formation time: 500 min Layer thickness: 1000 nm
[0192] These nozzle plates 11 to 16 were evaluated for ink resistance, abrasion durability, and continuous ejection stability in the same manner as in Example 1. The results are shown in Tables II and III below. As with the results of Example 1, excellent effects were confirmed in ink durability, abrasion durability, and continuous ejection stability.
[0193] Example 3: A substrate adhesion layer was formed on a silicon wafer plate having nozzle holes formed thereon by Deep-RIE, in the same manner as nozzle plate 1 in Example 1, and a hydrogen-repellent layer (a fluorine-containing coupling agent) was then formed directly thereon to produce nozzle plate 17. In this case, Optool DSX (manufactured by Daikin Industries, Ltd.) was used as the fluorine-containing coupling agent instead of the fluorine-containing coupling agent b. This nozzle plate 17 was evaluated for ink durability, abrasion durability, and continuous ejection stability in the same manner as in Example 1. The results are shown in Table III below. Similar to the results of Example 1, excellent effects were confirmed in terms of ink durability, abrasion durability, and continuous ejection stability.
[0194]
[0195]
[0196] Furthermore, for nozzle plates 1 to 17, measurements were performed under the following conditions using an X-ray diffractometer (Rigaku Corporation, Ultima III multipurpose X-ray diffractometer) to obtain X-ray diffraction patterns of the substrate adhesion layers. Apparatus: Rigaku Corporation, Ultima III multipurpose X-ray diffractometer X-ray source: Cu-kα 40 kV-30 mA Scan axis: θ / 2θ Scan range: 25° to 85° (sampling width: 0.02°) Scan speed: 10° / min
[0197] In the obtained X-ray diffraction spectrum, a peak at 2θ of 32.6° was confirmed for nozzle plates 1 to 4 and 7 to 17.
[0198] The present invention can be used for an inkjet head member, a manufacturing method for an inkjet head member, and an inkjet head that can ensure long-term durability and abrasion resistance to ink and have excellent continuous ejection properties.
[0199] REFERENCE SIGNS LIST 1 nozzle plate 2 substrate 3 substrate adhesion layer 4 functional layer 41 foundation layer 41a first foundation layer 41b second foundation layer 42 liquid-repellent layer 20A RIE plasma processing apparatus 21 reaction chamber 22 high-frequency power supply 23 capacitor 24 flat electrode (power supply electrode) 25 counter electrode (ground electrode) 26 earth 27 gas inlet 28 gas outlet 30 nozzle plate substrate 31 discharge space 32, 33 power supply line 56 housing 57 cap receiving plate 59 cover member 61 nozzle plate 62 cap receiving plate mounting portion 68 mounting hole 71 nozzle opening 81a first joint 81b second joint 82 third joint 100 inkjet head D discharge G reactive gas N nozzle P pump In ink
Claims
1. An inkjet head member having at least a substrate, a substrate adhesion layer, and a functional layer in this order, The substrate adhesion layer contains a Group 4 or Group 5 element, a nitrogen element, and an oxygen element, An inkjet head member, characterized in that the atomic concentration (atm %) of oxygen element is higher on the surface of the substrate adhesion layer on the side of the functional layer than in the interior of the substrate adhesion layer.
2. 2. The inkjet head member according to claim 1, wherein the Group 5 element contained in the substrate adhesion layer is tantalum (Ta).
3. 2. The member for an inkjet head according to claim 1, wherein a ratio of atomic concentrations (atm %) of nitrogen element to group 4 or group 5 element inside the substrate adhesion layer satisfies the following formula (I): Formula (I): 0.3≦atomic concentration of nitrogen element / atomic concentration of Group 4 or Group 5 element≦1
4. The substrate adhesion layer is characterized by the following in terms of Ta 2 2. The ink jet head member according to claim 1, further comprising a peak derived from N.
5. 2. The inkjet head member according to claim 1, wherein the thickness of the substrate adhesion layer is within a range of 1 to 1500 nm.
6. 2. The inkjet head member according to claim 1, wherein the functional layer includes a liquid-repellent layer containing a coupling agent containing fluorine (F).
7. 2. The inkjet head member according to claim 1, wherein the functional layer includes a liquid-repellent layer containing a coupling agent containing fluorine (F) and a base layer serving as a base for the liquid-repellent layer.
8. 8. The inkjet head member according to claim 7, wherein the undercoat layer is a layer containing at least an inorganic oxide or an oxide containing carbon (C).
9. 9. The ink jet head member according to claim 8, wherein the undercoat layer contains an oxide composed of at least carbon (C), silicon (Si), and oxygen (O).
10. 9. The inkjet head member according to claim 8, wherein the undercoat layer is a layer made of a silane coupling agent containing at least carbon (C) and oxygen (O).
11. 11. The inkjet head member according to claim 10, wherein the silane coupling agent contained in the undercoat layer has reactive functional groups at both ends and a molecular structure including a hydrocarbon chain and a benzene ring in the middle.
12. 2. The ink jet head member according to claim 1, wherein the base material is made of stainless steel.
13. A method for producing an inkjet head member according to any one of claims 1 to 12, comprising the steps of: The substrate adhesion layer is formed on the substrate, A method for manufacturing an inkjet head member, comprising forming the functional layer on the substrate adhesion layer, and then forming a nozzle by laser processing.
14. 14. The method for producing an inkjet head member according to claim 13, wherein the substrate adhesion layer is formed by a reactive sputtering method using a dry process.
15. The method for producing an inkjet head member according to claim 13, characterized in that the surface treatment of the substrate adhesion layer is an oxygen plasma treatment.
16. An ink-jet head comprising the ink-jet head member according to any one of claims 1 to 12.