Molded article
Patent Information
- Application Number
- JP2023524554
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Priority Date
- 2023-03-27
- Filing Date
- 2023-03-27
- Publication Date
- 2024-12-05
AI Technical Summary
Molded products using hollow particles often suffer from surface irregularities and whitening issues, leading to poor appearance, despite their potential for high strength and light-shielding properties.
Incorporating hollow particles with a black material in their shells, such as carbon black, to enhance strength, light-shielding, and appearance, while controlling the particle diameter and content of the black material to achieve uniform dispersion and improved heat retention.
The solution results in a molded article with improved strength, reduced surface irregularities, and enhanced appearance quality, maintaining high light-shielding properties and uniform black color.
Abstract
Description
Molded body
[0001] The present invention relates to a molded article.
[0002] Hollow particles having voids inside the particle are used in an extremely wide range of fields, such as various molded products such as injection molded products, injection compression molded products, extrusion molded products, and hollow molded products, as well as wallpaper, paints, sealants, pressure-sensitive adhesives, and diffusion materials, for the purposes of weight reduction, light diffusion, pore formation, imparting heat insulation properties, sound insulation properties, low dielectric properties, imparting impact resistance, improving rigidity, improving texture, preventing sink marks, improving coatability, and the like.
[0003] Known examples of such hollow particles include hollow resin particles obtained by using a special surfactant, as described in Patent Document 1. Such thermoplastic hollow resin particles have superior light diffusing properties compared to spherical resin particles that do not have a hollow structure, and are therefore said to provide excellent effects when used as a light diffusing material, such as in a light diffusion plate.
[0004] Japanese Patent Application Laid-Open No. 2020-045399
[0005] However, when a molded body is produced using the hollow particles and resin described in Patent Document 1, problems arise in that white spots originating from the hollow particles appear on the surface of the molded body, or surface irregularities occur, impairing the appearance of the molded body.
[0006] An object of the present invention is to provide a molded article that is less likely to suffer from poor appearance due to surface irregularities or whitening and that has high strength.
[0007] Disclosure (1) is a molded article comprising hollow particles containing a resin and a black material in a shell, the hollow particles having an average particle size of 3 to 200 μm. Disclosure (2) is the molded article according to Disclosure (1), in which the black material is a black pigment or a black dye. Disclosure (3) is the molded article according to Disclosure (2), in which the black pigment is at least one selected from the group consisting of carbon-based black pigments and oxide-based black pigments. Disclosure (4) is the molded article according to Disclosure (2), in which the black dye is an organic black dye. Disclosure (5) is the molded article according to any one of Disclosures (1) to (4), in which the content of the black material is 0.01 to 30 wt % relative to the total weight of the hollow particles. Disclosure (6) is the molded article according to any one of Disclosures (1) to (5), in which the molded article further contains a colorant. The present invention will be described in detail below.
[0008] A molded article according to one embodiment of the present invention includes hollow particles containing a resin and a black material in the shell. The hollow particles may have a void core or may contain a liquid or the like, but preferably have a void core. This void structure has the advantages of being less likely to change dimensions when heat is applied to the molded article and of reducing volatiles from the liquid. Furthermore, when expanded particles or the like are used, the presence of unexpanded particles can result in insufficient reduction in specific gravity. However, when hollow particles are used, all particles can contribute to reducing the specific gravity, allowing the specific gravity of the molded article to be efficiently reduced.
[0009] The hollow particles constituting the molded body according to one embodiment of the present invention contain a black material in the shell. The inclusion of the black material can increase the strength of the molded body and further improve the light-blocking properties and appearance of the molded body. The black material exhibits a black color by absorbing all light rays, including those in the visible light range of sunlight. While typical black pigments exhibit a black color by absorbing light in the visible light range (approximately 380 to 780 nm), they also absorb light in the near-infrared range, including the wavelength range of 800 to 1,400 nm, which contributes significantly to heat generation. Furthermore, the inclusion of the black material improves the dispersibility of the hollow particles in the molded body, making white spots on the surface of the molded body less noticeable. Furthermore, the inclusion of the black material increases the heat retention of the molded body and reduces temperature changes in the molded body. Additionally, the inclusion of the black material increases the shell strength of the hollow particles, making them less susceptible to fracture during kneading.
[0010] The preferred lower limit of the OD value of the black material is 1.5, and the preferred upper limit is 5.0. By setting it within the above range, a molded product can be obtained that has both high light-blocking properties and jet blackness. That is, the OD value of the black material is preferably 1.5 to 5.0. The OD value of the black material refers to the OD value measured when an acrylic resin (coating thickness 1 μm) containing 50% by weight of the black material is used. In this specification, the optical density (OD value) is the intensity of light incident on an optical density variable element, expressed as I 0 , the transmitted light intensity is I T When X = -log(I T / I 0 The optical density (OD value) can be measured using a color difference meter, a Macbeth densitometer, or the like.
[0011] Examples of the black material include black pigments, black dyes, and black conductive polymers. It is particularly preferable to use at least one material selected from the group consisting of black pigments, black dyes, and black conductive polymers. Among these, black pigments are preferred. Examples of the black pigment include inorganic black pigments such as carbonaceous black pigments and oxide-based black pigments, as well as organic black pigments. Among these, at least one material selected from the group consisting of carbonaceous black pigments and oxide-based black pigments is preferred. Examples of the carbonaceous black pigment include carbon black, graphite, activated carbon, and graphene. Examples of the carbon black include furnace black, channel black, acetylene black, thermal black, lamp black, and bone black. Carbon nanotubes, carbon nanofibers, fullerenes, and graphite may also be used. Examples of the oxide-based black pigment include titanium black, iron oxide, magnetite, and cuprous oxide (cuprous oxide), as well as composite oxide black pigments containing copper and chromium, copper and manganese, copper, iron, and manganese, or cobalt, chromium, and iron as main metal components. Furthermore, as the inorganic black pigment, metal oxides, composite oxides, metal sulfides, metal sulfates, metal carbonates, etc. of titanium black, copper, iron, manganese, cobalt, chromium, nickel, zinc, calcium, silver, etc. can also be used. As the organic black pigment, aniline black (C.I. Pigment Black 1) can be mentioned. Among them, carbon black is more preferred because it has excellent heat resistance, excellent dispersibility in resins, and can impart a uniform black color.
[0012] Examples of the black dye include inorganic black dyes and organic black dyes. Of these, organic black dyes are preferred. Examples of the inorganic black dye include metal complex azo black dyes. Examples of the metal complex azo black dye include Neo Super Black C-832 (product name Solvent Black 27, manufactured by Chuo Synthetic Chemical Industry Co., Ltd.).
[0013] Examples of the organic black dye include disazo black dyes, azine black dyes, phthalocyanine black dyes, anthraquinone black dyes, and indigoid black dyes. Examples of the disazo black dye include OIL BLACK 860 (product name: Solvent Black 3, manufactured by Orient Chemical Co., Ltd.). Examples of the azine black dye include NUBIAN BLACK TH-807 (product name: Solvent Black 7, manufactured by Orient Chemical Co., Ltd.).
[0014] Examples of the black conductive polymer include polythiophene, polydopamine, polypyrrole, polyaniline, polyphenylene vinylene, polyphenylene, polyacetylene, polyquinoxaline, polyoxadiazole, polybenzothiadiazole, etc., and polymers having a plurality of these conductive skeletons, etc. Among these, polythiophene and its derivatives are preferred, and poly(3,4-ethylenedioxythiophene) [PEDOT], poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonate) [PEDOT / PSS], and polythienothiophene are particularly preferred.
[0015] Among the black materials, particulate black materials (black particulates) are preferred. The black particulates preferably have an average particle diameter of 1 μm or less, more preferably 10 to 500 nm. By setting the average particle diameter within the above range, the black particulates are dispersed in the resin, resulting in a uniform hue (black). The average particle diameter can be measured, for example, by observation using a particle size distribution measuring device (ELSZ-2000ZS, manufactured by Otsuka Electronics Co., Ltd.) or by observation using a transmission electron microscope or the like after preparing a thin film so as to pass through the vicinity of the center of the hollow particles dispersed in the embedding resin.
[0016] The preferred lower limit of the content of the black material is 0.01 wt % relative to the total hollow particle content, and the preferred upper limit is 30 wt %. By setting the content at 0.01 wt % or more, fusion of hollow particles in the resin during molding can be suppressed. By setting the content at 30 wt % or less, the strength of the shell against melt-kneading during molding can be increased, and the appearance performance can be further improved. A more preferred lower limit is 0.3 wt %, a more preferred upper limit is 15 wt %, an even more preferred upper limit is 10 wt %, and an even more preferred upper limit is 7 wt %. That is, the content of the black material is preferably 0.01 to 30 wt %, more preferably 0.3 to 15 wt %, even more preferably 0.3 to 10 wt %, and particularly preferably 0.3 to 7 wt %. The content of the black material can be determined, for example, by increasing the temperature of hollow particles in a nitrogen atmosphere to 600°C at 10°C / min, maintaining this temperature for 10 minutes, then decreasing the temperature to 400°C at 10°C / min and maintaining this temperature for 10 minutes, switching the atmosphere to air, increasing the temperature to 1000°C in air, and maintaining this temperature for 10 minutes. The content of the black material can also be determined from the weight loss between 400°C and 1000°C. The content of the black material can also be calculated from the amounts of the black material and other components added in the manufacturing process.
[0017] The black material has a specific surface area of 500 m 2 / g or less, and more preferably 5 to 300m 2 / g. By setting the specific surface area within the above range, the black material is dispersed in the resin, and the hue (black) becomes uniform. The specific surface area can be measured by measuring a nitrogen adsorption isotherm using a surface area / pore size analyzer (NOVA4200e, manufactured by Quantachrome Instruments) and calculating the specific surface area of the black material from the measurement results in accordance with the BET method.
[0018] The black material has a DBP (dibutyl phthalate) oil absorption of 30 cm 3 / 100g or more, 140cm 3 When the DBP oil absorption is within the above range, the structure becomes appropriate and the blackness can be improved. A more preferable lower limit of the DBP oil absorption is 45 cm 3 / 100g, more preferably the upper limit is 110cm 3 The DBP oil absorption can be measured in accordance with JIS K 6221.
[0019] In the present invention, the black material may be present on the shell surface of the hollow particle, inside the shell, or on the inner surface of the shell. It is preferable that the black material be present on the shell surface of the hollow particle. When the black material is present on the shell surface, the appearance of the molded body can be improved. Furthermore, it is preferable that the hollow particle has an outermost layer, and that the outermost layer contains the black material. This configuration further enhances dispersibility in the resin during molding. The black material may be present both on the shell surface and inside the shell, i.e., part of the black material may be exposed and part may be present inside. In such a case, poor appearance due to surface irregularities and whitening can be further suppressed. The location of the black material can be confirmed using a transmission electron microscope or the like after forming a thin film that passes through the vicinity of the center of the hollow particle dispersed in the embedded resin.
[0020] The shell constituting the hollow particles contains a resin. The resin is preferably a polymer of a monomer composition such as an unsaturated carboxylic acid monomer, a nitrile monomer, a polyfunctional monomer, a conjugated diene monomer, or a vinyl monomer. Two or more of these may be used in combination as a copolymer. It is particularly preferred to use a polyfunctional monomer alone or to use an unsaturated carboxylic acid monomer and a nitrile monomer in combination.
[0021] The unsaturated carboxylic acid monomer is preferably a (meth)acrylic acid ester or an unsaturated carboxylic acid. The (meth)acrylic acid ester is preferably an alkyl methacrylate such as methyl methacrylate, ethyl methacrylate, or n-butyl methacrylate, or an alicyclic, aromatic, or heterocyclic methacrylate such as cyclohexyl methacrylate, benzyl methacrylate, or isobornyl methacrylate.
[0022] Examples of the unsaturated carboxylic acid include unsaturated monocarboxylic acids such as acrylic acid, methacrylic acid, ethacrylic acid, crotonic acid, and cinnamic acid, as well as maleic acid, itaconic acid, fumaric acid, citraconic acid, and chloromaleic acid. Monoesters of the unsaturated dicarboxylic acids may also be used. Examples of the monoesters of the unsaturated dicarboxylic acids include monomethyl maleate, monoethyl maleate, monobutyl maleate, monomethyl fumarate, monoethyl fumarate, monomethyl itaconate, monoethyl itaconate, and monobutyl itaconate. Of these, acrylic acid, methacrylic acid, maleic acid, maleic anhydride, and itaconic acid are particularly preferred.
[0023] The nitrile monomer is not particularly limited, and examples thereof include acrylonitrile, methacrylonitrile, α-chloroacrylonitrile, α-ethoxyacrylonitrile, fumaronitrile, and mixtures thereof. Among these, acrylonitrile and methacrylonitrile are particularly preferred. These may be used alone or in combination of two or more.
[0024] Examples of the polyfunctional monomer include monomers having two or more radically polymerizable double bonds, and specific examples include divinylbenzene, di(meth)acrylate, and tri- or higher functional (meth)acrylates. Examples of the di(meth)acrylate include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, and 1,4-butanediol di(meth)acrylate. Other examples include 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, glycerin di(meth)acrylate, trimethylolpropane di(meth)acrylate, and dimethylol-tricyclodecane di(meth)acrylate. Furthermore, di(meth)acrylate of polyethylene glycol having a weight average molecular weight of 200 to 600 may also be used. Examples of the trifunctional (meth)acrylates include trimethylolpropane tri(meth)acrylate, ethylene oxide-modified trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, triallyl formal tri(meth)acrylate, etc. Examples of the tetrafunctional or higher (meth)acrylates include pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, etc. Among these, trifunctional (meth)acrylates such as trimethylolpropane tri(meth)acrylate and bifunctional (meth)acrylates such as polyethylene glycol provide relatively uniform crosslinking to the acrylonitrile-based shell. By including the polyfunctional monomer, the strength of the shell can be enhanced.
[0025] Examples of the conjugated diene monomer include butadiene, isoprene, and chloroprene. Examples of the vinyl monomer include vinyl chloride, vinylidene chloride, vinyl acetate, and styrene. These may be used alone or in combination of two or more.
[0026] The resin may contain a thermosetting resin. Examples of the thermosetting resin include epoxy resin, phenol resin, melamine resin, urea resin, polyimide resin, and bismaleimide resin. Among these, epoxy resin and phenol resin are preferred.
[0027] The epoxy resin is not particularly limited, and examples thereof include bisphenol A epoxy resins, bisphenol F epoxy resins, phenol novolac epoxy resins, cresol novolac epoxy resins, dicyclopentadiene epoxy resins, and glycidylamine epoxy resins. Examples of the phenol resins include novolac phenol resins, resol phenol resins, and benzylic ether phenol resins. Of these, novolac phenol resins are preferred.
[0028] The thermosetting resin preferably has two or more functional groups reactive with carboxyl groups per molecule. Having two or more functional groups reactive with carboxyl groups can further strengthen the curing properties of the thermosetting resin. In particular, when the monomer composition contains a monomer having a carboxyl group, the heat generated during heating and foaming causes the carboxyl group and the thermosetting resin to bond more strongly, significantly improving heat resistance and durability. The thermosetting resin preferably does not have a radically polymerizable double bond.
[0029] Examples of the functional group reactive with the carboxyl group include a glycidyl group, a phenol group, a methylol group, and an amino group. Of these, a glycidyl group is preferred. The functional groups reactive with the carboxyl group may be the same or two or more different groups.
[0030] A polymerization initiator is added to the monomer composition to polymerize the monomers. Suitable examples of the polymerization initiator include dialkyl peroxides, diacyl peroxides, peroxyesters, peroxydicarbonates, and azo compounds. Specific examples include dialkyl peroxides such as methyl ethyl peroxide, di-t-butyl peroxide, and dicumyl peroxide; and diacyl peroxides such as isobutyl peroxide, benzoyl peroxide, 2,4-dichlorobenzoyl peroxide, and 3,5,5-trimethylhexanoyl peroxide. Other examples include t-butyl peroxypivalate, t-hexyl peroxypivalate, t-butyl peroxyneodecanoate, t-hexyl peroxyneodecanoate, 1-cyclohexyl-1-methylethyl peroxyneodecanoate, and 1,1,3,3-tetramethylbutyl peroxyneodecanoate. Other examples include peroxyesters such as cumyl peroxy neodecanoate and (α,α-bis-neodecanoylperoxy)diisopropylbenzene; bis(4-t-butylcyclohexyl)peroxydicarbonate, di-n-propyl-oxydicarbonate, and diisopropyl peroxydicarbonate. Further examples include peroxydicarbonates such as di(2-ethylethylperoxy)dicarbonate, dimethoxybutyl peroxydicarbonate, and di(3-methyl-3-methoxybutylperoxy)dicarbonate. Additionally, other examples include azo compounds such as 2,2'-azobisisobutyronitrile, 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), and 1,1'-azobis(1-cyclohexanecarbonitrile).
[0031] The weight-average molecular weight of the resin constituting the shell preferably has a lower limit of 50,000 and an upper limit of 2,000,000. That is, the weight-average molecular weight of the resin constituting the shell is preferably 50,000 to 2,000,000. A weight-average molecular weight of 50,000 or more can improve the strength of the shell, and a weight-average molecular weight of 2,000,000 or less can ensure that the strength of the shell is appropriate. The weight-average molecular weight is a value determined by measuring by gel permeation chromatography (GPC) using DMF as a solvent and calculated in terms of polymethyl methacrylate. Examples of columns used when measuring the weight-average molecular weight calculated in terms of polymethyl methacrylate by GPC include HSPgel RT MB-H (manufactured by Waters), and examples of molecular weight standards include M-75 (manufactured by Shodex).
[0032] The shell may contain a metal cation. When the copolymer constituting the shell contains a carboxyl group, the metal cation reacts with the carboxyl group to ionically crosslink the copolymer, improving heat resistance and enabling hollow particles to be produced that do not burst or shrink for long periods of time at high temperatures. Furthermore, since the elastic modulus of the shell is unlikely to decrease even at high temperatures, the hollow particles do not burst or shrink even when subjected to molding processes that apply strong shear forces, such as kneading, calendaring, extrusion, and injection molding. The ionic crosslinking described above means that crosslinks are formed between free carboxyl groups present as side chains of the copolymer. The number of carboxyl groups arranged per monovalent metal cation varies depending on the metal type.
[0033] The metal cation is not particularly limited as long as it reacts with the carboxyl groups of the copolymer to ionically crosslink the copolymer, and examples thereof include ions of Li, Na, K, Zn, Mg, Ca, Ba, Sr, Mn, Al, Ti, Ru, Fe, Ni, Cu, Cs, Sn, Cr, and Pb. These may be used alone or in combination of two or more. Among these, Ca, Zn, and Al ions are preferred, with Zn ions being particularly preferred. When two or more of the metal cations are used, the combination is not particularly limited, but it is preferable to use an alkali metal ion in combination with a metal cation other than the alkali metal. The presence of the alkali metal ion activates functional groups such as carboxyl groups, thereby promoting the reaction between the metal cations other than the alkali metal and the carboxyl groups of the copolymer. Examples of the alkali metal include Na, K, and Li.
[0034] The shell may further contain, as necessary, a stabilizer, an ultraviolet absorber, an antioxidant, an antistatic agent, a flame retardant, a silane coupling agent, a coloring agent, and the like.
[0035] The lower limit of the average particle diameter of the hollow particles is 3 μm, and the upper limit is 200 μm. By setting the average particle diameter to 3 μm or more, the porosity of the molded body can be increased, and by setting the average particle diameter to 200 μm or less, the appearance of the molded body can be improved. The lower limit of the average particle diameter is preferably 5 μm, more preferably 15 μm, and the upper limit is preferably 150 μm, more preferably 100 μm, even more preferably 80 μm, particularly preferably 60 μm, and especially more preferably 50 μm. That is, the average particle diameter of the hollow particles is 3 to 200 μm, preferably 5 to 150 μm, more preferably 15 to 100 μm, even more preferably 15 to 80 μm, particularly preferably 15 to 60 μm, and especially more preferably 15 to 50 μm. The CV value (coefficient of variation) of the average particle diameter of the hollow particles is preferably 40% or less, more preferably 30% or less, and even more preferably 20% or less. By setting the content to 40% or less, the cells in the resulting molded body will be uniform, allowing for a uniform thickness. Furthermore, the cells present on the surface of the molded body will also be uniform, resulting in an excellent appearance. While there are no particular restrictions on the preferred lower limit, 0% is preferred. The average particle diameter of the hollow particles refers to the number-average particle diameter, and can be measured by measuring the particle diameters of at least 50 hollow particles in a cross section obtained by cutting the molded body using a SEM or the like and calculating the average value. The CV value can also be calculated during the measurement. When the cross section of the hollow particles is not a perfect circle, the particle diameter is defined as the average value of (maximum diameter + minimum diameter) / 2.
[0036] The hollow particles preferably have a ratio (A / B) of the average particle diameter (A) of the black material to the shell thickness (B) of 0.01 to 20. By setting the ratio within this range, both shell strength and appearance can be achieved. A more preferred lower limit is 0.2, and a more preferred upper limit is 5. The shell thickness is preferably 0.01 μm or more and 1 μm or less. Furthermore, the hollow particles preferably have a ratio (B / C) of the shell thickness (B) to the average particle diameter (C) of the hollow particles of 0.001 to 0.01. The shell thickness can be measured by measuring the shell thickness of 10 hollow particles in a cross section obtained by cutting the molded body using a SEM or the like at any five locations per particle and calculating the average value.
[0037] The hollow particles preferably have an optical density (OD value) of 0.5 or more. By making the OD value 0.5 or more, it is possible to obtain a black coating film or black matrix that combines high light-blocking properties with jet blackness. A more preferred lower limit is 0.8, and a more preferred upper limit is 1.6. That is, the OD value of the hollow particles is preferably 0.5 to 1.6, and more preferably 0.8 to 1.6. The optical density (OD value) can be measured using a Macbeth densitometer or the like.
[0038] The method for producing the hollow particles is not particularly limited. For example, the hollow particles can be produced by carrying out the steps of preparing an aqueous dispersion medium containing a dispersant, adding a monomer composition, a black material, and a hollowing agent, and polymerizing the monomer.
[0039] When producing the hollow particles, a step of preparing an aqueous dispersion medium is first carried out. Specifically, for example, water, a dispersant, and optionally a co-stabilizer are added to a polymerization reaction vessel to prepare an aqueous dispersion medium containing the dispersant.
[0040] As the dispersant, it is preferable to use an emulsifier such as polyvinyl alcohol and at least one inorganic compound selected from the group consisting of Si-based compounds and Mg-based compounds. By containing the inorganic compound, it is possible to suppress fusion between hollow particles during molding. Note that the inorganic compound is different from the black material.
[0041] The Si-based compound and Mg-based compound preferably contain an oxide, hydroxide, carbonate, or hydrogencarbonate of silicon or magnesium. These Si-based compounds and Mg-based compounds may be used alone or in combination of two or more.
[0042] Examples of the Si-based compounds include colloidal silica, silicate sol, No. 3 water glass, sodium orthosilicate, sodium metasilicate, etc. Among these, colloidal silica is preferred. Examples of the Mg-based compounds include magnesium oxide, magnesium hydroxide, magnesium oxide hydroxide, hydrotalcite, dihydrotalcite, magnesium carbonate, basic magnesium carbonate, magnesium calcium carbonate, magnesium phosphate, magnesium hydrogen phosphate, magnesium pyrophosphate, magnesium borate, etc. Among these, magnesium hydroxide is preferred.
[0043] Other examples of the inorganic compounds that may be added include calcium phosphate, aluminum hydroxide, ferric hydroxide, barium sulfate, calcium sulfate, sodium sulfate, calcium oxalate, calcium carbonate, barium carbonate, etc. Furthermore, inorganic salts such as sodium chloride and sodium sulfate, alkali metal nitrite, stannous chloride, stannic chloride, potassium dichromate, etc. may also be added as needed.
[0044] The inorganic compound is preferably in the form of fine particles. When the inorganic compound is in the form of fine particles, the primary particle diameter is preferably 0.5 μm or less, more preferably 5 to 100 nm (0.1 μm). By keeping the diameter within this range, fusion between hollow particles in the resin during molding can be suppressed. The primary particle diameter can be measured by observation using a scanning electron microscope (Regulus 8220, manufactured by Hitachi High-Technologies Corporation).
[0045] The preferred lower limit of the amount of the dispersant added relative to the total monomer composition is 0.5% by weight, and the preferred upper limit is 30% by weight. By setting the amount to 0.5% by weight or more, aggregation during hollow particle production can be suppressed. By setting the amount to 30% by weight or less, dispersibility can be further improved. A more preferred lower limit is 1% by weight, and a more preferred upper limit is 25% by weight. That is, the amount of the dispersant added is preferably 0.5 to 30% by weight, and more preferably 1 to 25% by weight.
[0046] Examples of the auxiliary stabilizer include a condensation product of diethanolamine and an aliphatic dicarboxylic acid, a condensation product of urea and formaldehyde, etc. Further examples include polyvinylpyrrolidone, polyethylene oxide, polyethyleneimine, tetramethylammonium hydroxide, gelatin, methylcellulose, dioctyl sulfosuccinate, sorbitan ester, various emulsifiers, etc.
[0047] In addition to the co-stabilizer, a condensation product or a water-soluble nitrogen compound may be added. As the condensation product, a condensation product of diethanolamine and an aliphatic dicarboxylic acid is preferred, and a condensation product of diethanolamine and adipic acid or a condensation product of diethanolamine and itaconic acid is particularly preferred.
[0048] Examples of the water-soluble nitrogen compounds include polyvinylpyrrolidone, polyethyleneimine, polyoxyethylene alkylamine, polydialkylaminoalkyl(meth)acrylates such as polydimethylaminoethyl methacrylate and polydimethylaminoethyl acrylate, polydialkylaminoalkyl(meth)acrylamides such as polydimethylaminopropyl acrylamide and polydimethylaminopropyl methacrylamide, polyacrylamide, polycationic acrylamide, polyamine sulfone, and polyallylamine. Among these, polyvinylpyrrolidone is preferably used.
[0049] An aqueous dispersion medium containing the dispersant and, if necessary, a co-stabilizer is prepared by blending it with deionized water, and the pH of the aqueous phase is determined appropriately depending on the types of dispersant and co-stabilizer used. For example, when a Si-based compound such as colloidal silica is used as the dispersant, polymerization is carried out using an acidic aqueous dispersion medium, and to make the aqueous dispersion medium acidic, an acid such as hydrochloric acid is added as necessary to adjust the pH of the system to 3 to 4. On the other hand, when a Mg-based compound such as magnesium hydroxide or calcium phosphate is used as the inorganic compound, polymerization is carried out using an alkaline aqueous dispersion medium adjusted to a pH of 8 to 11.
[0050] Next, in the method for producing hollow particles, a step of adding a monomer composition, a black material, and a hollowing agent is carried out. In this step, the monomer composition, the black material, and the hollowing agent may be added separately to an aqueous dispersion medium to prepare an oily mixture in the aqueous dispersion medium. However, typically, the two may be mixed together to prepare an oily mixture beforehand, which is then added to the aqueous dispersion medium. In this case, the oily mixture and the aqueous dispersion medium may be prepared in separate containers, and the oily mixture may be dispersed in the aqueous dispersion medium by stirring and mixing in the separate containers, and then added to the polymerization reaction vessel. In this step, the dispersant can be present at the interface between the oil droplets of the oily mixture and the aqueous dispersion medium. A polymerization initiator is used to polymerize the monomer. The polymerization initiator may be added to the oily mixture in advance, or may be added after stirring and mixing the aqueous dispersion medium and the oily mixture in the polymerization reaction vessel. The black material and dispersant may be added to the aqueous dispersion medium or later. In particular, the average particle size of the resulting hollow particles can be controlled by adjusting the components of the hollow particles (especially the monomer and hollowing agent) and the amounts added, or by adjusting the reaction process during production of the thermally expandable microcapsules. Examples of adjustments to the reaction process include thoroughly pre-stirring the oily mixture before emulsifying and dispersing it in the aqueous dispersion medium, or emulsifying and dispersing the oily mixture in the aqueous dispersion medium to a predetermined particle size. In particular, the amount of hollowing agent added is preferably 50 to 2,800 parts by weight per 10 parts by weight of the monomer composition.
[0051] Examples of methods for emulsifying and dispersing the oily mixture in an aqueous dispersion medium to a predetermined particle size include stirring with a homomixer (e.g., manufactured by Tokushu Kika Kogyo Co., Ltd.), a homogenizer, or the like, or passing the mixture through a static dispersion device such as a line mixer or an element-type static disperser. The average particle size of the resulting hollow particles can also be controlled by adjusting the stirring force (rotation speed, etc.) during stirring. The aqueous dispersion medium and the monomer composition may be supplied separately to the static dispersion device, or a dispersion liquid that has been mixed and stirred in advance may be supplied.
[0052] The hollowing agent is a substance for forming a hollow portion that becomes the core. The hollowing agent is preferably an organic solvent with a boiling point of −50 to 100° C., as this is easy to handle when drying is performed in the hollowing step.
[0053] Examples of the hollowing agent include low molecular weight hydrocarbons such as n-butane, isobutane, butane, butene, isobutene, n-pentane, isopentane, neopentane, n-hexane, cyclohexane, heptane, petroleum ether, isooctane, octane, decane, isododecane, dodecane, and hexanedecane. Other examples include ethyl acetate, methyl ethyl ketone, acetone, methylene chloride, chloroform, and carbon tetrachloride. Of these, cyclohexane, isobutane, n-butane, n-pentane, isopentane, n-hexane, isooctane, isododecane, and mixtures thereof are preferred. These hollowing agents may be used alone or in combination. Furthermore, pyrolytic compounds that decompose into gaseous form upon heating may also be used as hollowing agents.
[0054] The hollow particles can be produced by subjecting the dispersion obtained through the above-described steps to a step of polymerizing the monomer by heating and pressurizing the dispersion, and a step of washing the dispersion. In particular, in the step of polymerizing the monomer, the average particle size of the obtained hollow particles can be controlled by setting the heating temperature to 40 to 100°C and the pressurizing pressure to 0.2 to 1.0 MPa.
[0055] A molded article according to one embodiment of the present invention contains a base resin in addition to the hollow particles. The base resin is preferably a thermoplastic resin. Specific examples of the thermoplastic resin include polyolefins such as low-density polyethylene (LDPE) and polypropylene (PP), ethylene-vinyl acetate copolymer (EVA), vinyl chloride, polystyrene, thermoplastic elastomers, olefin-based thermoplastic elastomers (TPV), and ethylene-methyl methacrylate copolymer (EMMA). Among these, LDPE, EVA, EMMA, and the like are preferred due to their low melting points and ease of processing. These may be used alone or in combination of two or more.
[0056] The content of the hollow particles in the molded article according to one embodiment of the present invention is not particularly limited, but the preferred lower limit is 1 part by weight and the preferred upper limit is 90 parts by weight per 100 parts by weight of the base resin.
[0057] The molded article according to one embodiment of the present invention preferably further contains a colorant. While typical dyes, organic pigments, and inorganic pigments can be used as the colorant, organic pigments are preferred. Examples of the organic pigment include blue, red, yellow, green, purple, and orange pigments. Examples of the organic pigment include azo pigments such as phthalocyanine pigments, monoazo pigments, diazo pigments, and condensed diazo pigments, as well as polycyclic pigments such as diketopyrrolopyrrole pigments, isoindolinone pigments, isoindoline pigments, quinacridone pigments, indigo pigments, thioindigo pigments, quinophthalone pigments, dioxazine pigments, anthraquinone pigments, perylene pigments, and perinone pigments. The colorant may be the same as the black material.
[0058] Examples of the blue pigment include organic pigments whose main component is an organic compound, such as phthalocyanine pigments, anthraquinone pigments, and dioxazine pigments. Among these, phthalocyanine pigments are preferred, with metal phthalocyanine pigments and monohalogenated metal phthalocyanine pigments (halogenated metal phthalocyanine pigments having one halogen atom in the molecule) being more preferred. As the phthalocyanine pigment, copper phthalocyanine pigments and monohalogenated copper phthalocyanine pigments are preferred.
[0059] Specific examples of the blue pigments classified as pigments in the Color Index (C.I.) include C.I. Pigment Blue 1, 1:2, 9, 14, 15, 15:1, 15:2, 15:3, 15:4, 15:5, 15:6, 16, 17, 17:1, 19, 22, 25, 27, 28, 29, 33, 35, 36, 56, 56:1, 60, 61, 61:1, 62, 63, 66, 67, 68, 71, 72, 73, 74, 75, 76, 78, 79, and 80. Phthalocyanine pigments include C.I. C.I. Pigment Blue 15, 15:1, 15:2, 15:3, 15:4, 15:6, 16, 17, 17:1, 75 are preferred, and as copper phthalocyanine pigments and monohalogenated copper phthalocyanine pigments, C.I. Pigment Blue 15, 15:1, 15:2, 15:3, 15:4, 15:6, 16, 17, 17:1 are preferred. As an anthraquinone pigment, C.I. Pigment Blue 60 is preferred. As a dioxazine pigment, C.I. Pigment Blue 80 is preferred.
[0060] The red pigments include C.I. Pigment Red 1, 2, 3, 4, 5, 6, 7, 8, 9, 12, 14, 15, 16, 17, 21, 22, 23, 31, 32, 37, 38, 41, 47, 48:1, 48:2, 48:3, 48:4, 49, 49:1, 49:2, 50:1, 52:2, 53, 53:1, 53:2, 53:3, 57, 57:1, 57:2, 58:4, 60 , 63, 63:1, 63:2, 64, 64:1, 68, 69, 81, 81:1, 81:2, 81:3, 81:4, 83, 88, 90:1, 101, 101:1, 104, 108, 108:1, 109, 112, 113, 114, 122, 123, 144, 146, 147, 149, 151, 166, 168, 169, 170, 172, 173, 174, 175, 176, 177, 178, 179, 181, 184, 185, 187, 188, 190, 193, 194, 200, 202, 206, 207, 208, 209, 210, 214, 215, 216, 221, 224, 230, 231, 232, 233, 235, 236, 2 37, 238, 239, 242, 243, 245, 247, 249, 250, 251, 253, 254, 255, 256, 257, 258, 259, 260, 262, 263, 264, 265, 266, 267, 268, 269, 270, 271, 272, 273, 274, 275, 276, 291, etc.
[0061] Examples of the yellow pigment include C.I. Pigment Yellow 1, 1; 1, 2, 3, 4, 5, 6, 9, 10, 12, 13, 14, 16, 17, 24, 31, 32, 34, 35, 35:1, 36, 36:1, 37, 37:1, 40, 41, 42, 43, 48, 53, 55, 60, 61, 62, 62:1, 63, 65, 73, 74, 75, 77, 81, 83, 87, 93, 94, 95, 97, 98, 100, 101, 104, 105, 108, 109, 110, 111, 116, 117, 119, 120, 126, 127, 127:1, 128, 129, 133, 134, 1 36, 138, 139, 142, 147, 148, 150, 151, 153, 154, 155, 157, 158, 159, 160, 161, 162, 163, 164, 165, 166, 167, 168, 169, 170, 172, 180, 181, 182, 183, 184, 185, 188, 189, 190, 191, 191:1, 192, 193, 194, 195, 196, 197, 198, 199, 200, 202, 203, 204, 205, 206, 207, 208, 213, 215, etc.
[0062] Examples of the green pigment include C.I. Pigment Green 1, 2, 4, 7, 8, 10, 13, 14, 15, 17, 18, 19, 26, 36, 45, 48, 50, 51, 54, 55, 58, 59, 62, and 63, aluminum phthalocyanine, polyhalogenated aluminum phthalocyanine, aluminum phthalocyanine hydroxide, diphenoxyphosphinyloxyaluminum phthalocyanine, diphenylphosphinyloxyaluminum phthalocyanine, polyhalogenated diphenoxyphosphinyloxyaluminum phthalocyanine, and polyhalogenated diphenylphosphinyloxyaluminum phthalocyanine.
[0063] Examples of the purple pigment include C.I. Pigment Violet 1, 1:1, 2, 2:2, 3, 3:1, 3:3, 5, 5:1, 14, 15, 16, 19, 23, 25, 27, 29, 31, 32, 37, 39, 42, 44, 47, 49, and 50.
[0064] Examples of the orange pigment include C.I. Pigment Orange 1, 2, 5, 13, 16, 17, 19, 20, 21, 22, 23, 24, 34, 36, 38, 39, 43, 46, 48, 49, 61, 62, 64, 65, 67, 68, 69, 70, 71, 72, 73, 74, 75, 78, and 79.
[0065] Examples of the inorganic pigment include barium sulfate, lead sulfate, titanium oxide (rutile type, anatase type, etc.), yellow lead, red iron oxide, and chromium oxide.
[0066] By using the hollow particles, a molded article having high appearance quality such as an uneven shape can be obtained, and the molded article can be suitably used for applications such as wallpaper for homes, interior materials for automobiles, etc. The molding method of the molded article according to one embodiment of the present invention is not particularly limited, and examples thereof include kneading molding, calendar molding, extrusion molding, injection molding, etc.
[0067] According to the present invention, a molded article having high strength and which is less likely to suffer from poor appearance due to surface irregularities or whitening can be obtained.
[0068] The following examples will further illustrate the present invention, but the present invention is not limited to these examples.
[0069] Example 1 (Preparation of Hollow Particles) 2.0 parts by weight of polyvinyl alcohol (PVA, manufactured by Mitsubishi Chemical Corporation, GH-20, viscosity 40-46 mPa·s, degree of saponification 86.5-89.0 mol%) as a dispersant was added to 250 parts by weight of ion-exchanged water and mixed to prepare an aqueous medium. Furthermore, 10 parts by weight of divinylbenzene as a monomer composition, 0.2 parts by weight of an amine salt of polyether ester acid (Disparlon-234, manufactured by Kusumoto Chemicals Co., Ltd.) as an additive, and 0.26 parts by weight of carbon black as a black material were added, and the mixture was dispersed by ultrasonic irradiation, followed by the addition of 200 parts by weight of cyclohexane to prepare a mixed solution. 0.8 parts by weight of a polymerization initiator (2,2′-azobisisobutyronitrile) was added to this mixed solution, and the mixture was then charged into an autoclave and mixed. The carbon black used was MA100 (manufactured by Mitsubishi Chemical Corporation, average primary particle size 24 nm, specific surface area 110 m). 2 / g, DBP oil absorption 100cm 3 / 100g) was used. The mixture was then added to an aqueous medium and suspended to prepare a dispersion. The resulting dispersion was stirred and mixed using a homogenizer, placed in a nitrogen-purged pressure polymerization vessel, and reacted at 60°C for 20 hours under pressure (0.5 MPa), yielding a reaction product. The resulting reaction product was repeatedly filtered and washed with water, and then dried to obtain hollow particles. The content of the black material was calculated from the amounts of the added black material and other components. The resulting hollow particles were added to an embedding resin (Technovit 4000, manufactured by Kulzer) and dispersed to prepare a hollow particle-embedded resin. A thin film was prepared using a microtome (EM UC7, manufactured by LEICA) so as to pass through the center of the hollow particles dispersed in the embedding resin. The location of the black material was confirmed using a transmission electron microscope (JEM-2100, manufactured by JEOL Ltd.). It was confirmed that some of the black material was exposed and some was present inside the shell of the particles (present on the surface and inside).
[0070] (Preparation of Molded Article) 5 g of the obtained hollow particles and 195 g of a TPV resin (Milastomer 7030BS, containing carbon black, manufactured by Mitsui Chemicals, Inc.) were weighed and mixed in a cup, and a molded article was prepared at 110°C using an 8-inch roll (191-TM, manufactured by Yasuda Seiki Seisakusho, Ltd.).
[0071] Example 2 Hollow particles and a molded body were produced in the same manner as in Example 1, except that the amount of cyclohexane added was changed from 200 parts by weight to 500 parts by weight.
[0072] Example 3 Hollow particles and a molded body were produced in the same manner as in Example 1, except that the amount of cyclohexane added was changed from 200 parts by weight to 800 parts by weight.
[0073] (Example 4) Carbon black #2350 (manufactured by Mitsubishi Chemical Corporation, primary average particle size 15 nm, specific surface area 320 m 2 / g, DBP oil absorption 65cm 3 Hollow particles and a molded article were produced in the same manner as in Example 2, except that the amount of the powder was changed to 100g / 100g.
[0074] (Example 5) Carbon black was MA14 (manufactured by Mitsubishi Chemical Corporation, average primary particle size 40 nm, specific surface area 56 m 2 / g, DBP oil absorption 73cm 3 Hollow particles and a molded article were produced in the same manner as in Example 2, except that the amount of the powder was changed to 100g / 100g.
[0075] (Example 6) Carbon black was MA220 (manufactured by Mitsubishi Chemical Corporation, primary average particle size 55 nm, specific surface area 36 m 2 / g, DBP oil absorption 93cm 3 Hollow particles and a molded article were produced in the same manner as in Example 2, except that the amount of the powder was changed to 100g / 100g.
[0076] Example 7: 75 parts by weight of sodium chloride, 30 parts by weight of colloidal silica containing 20% by weight of active ingredient, 2.0 parts by weight of polyvinylpyrrolidone, and 0.6 parts by weight of ethylenediaminetetraacetic acid tetrasodium salt were added to 250 parts by weight of ion-exchanged water, and the pH of the resulting mixture was adjusted to 2.0 to 3.0 to prepare an aqueous dispersion medium. Separately, an oily mixture was prepared by mixing 500 parts by weight of cyclohexane and 1.6 parts by weight of a di-sec-butyl peroxydicarbonate-containing solution containing 50% by weight of active ingredient with a monomer composition of 0.2 parts by weight of acrylonitrile, 5.5 parts by weight of methacrylonitrile, 4 parts by weight of methacrylic acid, and 0.3 parts by weight of methyl acrylate. To this oily mixture, 0.2 parts by weight of an amine salt of polyether ester acid (Disparlon-234, manufactured by Kusumoto Chemicals Co., Ltd.) and carbon black (MA100, manufactured by Mitsubishi Chemical Corporation, primary average particle diameter 24 nm, specific surface area 110 m) were added as a black material. 2 0.39 parts by weight of hydroxybenzoates (1 / g) was added, and the mixture was dispersed by ultrasonic irradiation, followed by mixing in an autoclave. The mixture was then added to an aqueous medium and suspended to prepare a dispersion. The resulting dispersion was stirred and mixed using a homogenizer, and then placed in a nitrogen-substituted pressure polymerization vessel. The reaction was carried out at 60°C for 20 hours under pressure (0.5 MPa), yielding a reaction product. The resulting reaction product was repeatedly filtered and washed with water, and then dried to yield hollow particles. Furthermore, a molded body was produced using the resulting hollow particles in the same manner as in Example 1.
[0077] Example 8 Hollow particles and a molded body were produced in the same manner as in Example 8, except that 3.3 parts by weight of acrylonitrile, 2.5 parts by weight of methacrylonitrile, 3 parts by weight of methacrylic acid, and 1.2 parts by weight of methyl methacrylate were used as the monomer composition.
[0078] Example 9 30 parts by weight of colloidal silica (manufactured by Asahi Denka Corporation, primary average particle size: 20 nm) containing 20% by weight of the active ingredient as a dispersant, and 2.0 parts by weight of polyvinylpyrrolidone (manufactured by BASF) were added to 250 parts by weight of ion-exchanged water and mixed to prepare an aqueous dispersion medium. 2 parts by weight of acrylonitrile, 3 parts by weight of methacrylonitrile, 4 parts by weight of methacrylic acid, and 1 part by weight of methyl methacrylate were mixed to prepare a monomer composition in the form of a homogeneous solution. 0.2 parts by weight of an amine salt of polyether ester acid (Disparlon-234, manufactured by Kusumoto Chemicals Co., Ltd.) was added as an additive, and 0.2 parts by weight of carbon black (MA100, manufactured by Mitsubishi Chemical Corporation, primary average particle size: 24 nm, specific surface area: 110 m) was added as a black material. 2 0.39 parts by weight of 2,2'-azobisisobutyronitrile (2,2'-azobisisobutyronitrile), 0.6 parts by weight of 2,2'-azobis(2,4-dimethylvaleronitrile), and 500 parts by weight of cyclohexane were added and mixed in the autoclave. The mixture was then added to an aqueous medium and suspended to prepare a dispersion. The resulting dispersion was stirred and mixed using a homogenizer, charged into a nitrogen-substituted pressure polymerization vessel, and reacted at 60°C for 20 hours under pressure (0.5 MPa), to obtain a reaction product. The resulting reaction product was repeatedly filtered and washed with water, and then dried to obtain hollow particles.
[0079] Example 10 Hollow particles and a molded body were produced in the same manner as in Example 1, except that the amount of cyclohexane added was changed from 200 parts by weight to 100 parts by weight.
[0080] Example 11 Hollow particles and a molded body were produced in the same manner as in Example 1, except that the amount of cyclohexane added was changed from 200 parts by weight to 2,700 parts by weight.
[0081] Example 12 Hollow particles and a molded body were produced in the same manner as in Example 2, except that the amount of cyclohexane added was changed from 200 parts by weight to 3,500 parts by weight.
[0082] Example 13 Hollow particles and a molded body were produced in the same manner as in Example 2, except that the amount of carbon black added was changed from 0.26 parts by weight to 0.52 parts by weight.
[0083] Example 14 Hollow particles and a molded body were produced in the same manner as in Example 2, except that the amount of carbon black added was changed from 0.26 parts by weight to 1.12 parts by weight.
[0084] Example 15 Hollow particles and a molded body were produced in the same manner as in Example 2, except that 0.26 parts by weight of Solvent Black 3 (black dye, OIL BLACK 860, manufactured by Orient Chemical Co., Ltd.) was added instead of 0.26 parts by weight of carbon black.
[0085] Example 16 Hollow particles and a molded body were produced in the same manner as in Example 1, except that the amount of cyclohexane added was changed from 200 parts by weight to 250 parts by weight.
[0086] Example 17 Hollow particles and a molded body were produced in the same manner as in Example 1, except that the amount of cyclohexane added was changed from 200 parts by weight to 90 parts by weight.
[0087] Comparative Example 1 Hollow particles and a molded body were produced in the same manner as in Example 1, except that no black material was added.
[0088] Comparative Example 2 Hollow particles and a molded body were produced in the same manner as in Example 1, except that the amount of cyclohexane added was changed from 200 parts by weight to 40 parts by weight.
[0089] Comparative Example 3 Hollow particles and a molded body were produced in the same manner as in Example 1, except that the amount of cyclohexane added was changed from 200 parts by weight to 4,500 parts by weight.
[0090] (Evaluation Method) The performance of the obtained hollow particles and molded bodies was evaluated by the following methods. The results are shown in Table 1.
[0091] (1) Evaluation of hollow particles (1-1) Measurement of number average particle diameter The particle diameters of at least 50 hollow particles in a cross section obtained by cutting the molded body were measured using a SEM or the like, and the average value was taken as the number average particle diameter.
[0092] (1-2) Shell Thickness The shell thickness of 10 hollow particles in a cross section obtained by cutting the molded body was measured at any five points per particle using an SEM or the like, and the average value was calculated.
[0093] (2) Evaluation of Molded Articles (2-1) Evaluation of Appearance (White Spots) The number of white spots on the surface (1 mm square) of the obtained molded article was counted using an optical microscope and evaluated according to the following criteria.
[0094] Less than 10: ○○○ 10 or more but less than 20: ○○ 20 or more but less than 50: ○ 50 or more but less than 70: △ 70 or more: ×
[0095] (2-2) Appearance (Color Difference) Evaluation The obtained molded body samples were evaluated using a color difference meter (CM-26dG, manufactured by Konica Minolta Inc.) * , a * , b * The color difference ΔE from the base resin without particles was measured at five random points. * ab = √((ΔL * )^2+(Δa * )^2(Δb * )^2) were calculated and evaluated according to the following criteria.
[0096] Less than 0.5: ○○○ 0.5 or more and less than 1.0: ○○ 1.0 or more and less than 2.0: ○ 2.0 or more and less than 3.0: △ 3.0 or more: ×
[0097] (2-3) Surface Roughness The surface roughness (Rz value) of the molded body surface was measured using a 3D shape measuring instrument (manufactured by Keyence Corporation). The measured Rz value was evaluated according to the following criteria.
[0098] Less than 50 μm: ○○ 50 μm or more and 80 μm or less: ○ More than 80 μm and 100 μm or less: △ More than 100 μm: ×
[0099] (2-4) Strength The 25% compressive strength of the molded product was measured at 23°C by a method in accordance with JIS K 6767. The obtained 25% compressive strength was evaluated according to the following criteria: Less than 30 kPa: ◯ 30 kPa or more but less than 40 kPa: O 40 kPa or more but less than 50 kPa: Δ 50 kPa or more: ×
[0100]
[0101] According to the present invention, it is possible to provide a molded article that is less likely to suffer from poor appearance due to surface irregularities or whitening and that has high strength.
Claims
1. A molded article comprising hollow particles containing a resin and a black material in a shell, the hollow particles having an average particle size of 3 to 200 μm.
2. The molded article according to claim 1 , wherein the black material is a black pigment or a black dye.
3. The molded article according to claim 2 , wherein the black pigment is at least one selected from the group consisting of carbon-based black pigments and oxide-based black pigments.
4. The molded article according to claim 2 , wherein the black dye is an organic black dye.
5. The molded article according to any one of claims 1 to 4, wherein the content of the black material is 0.01 to 30% by weight based on the total weight of the hollow particles.