Amorphous composite metal oxide powder containing La and Zr, and a method for manufacturing the powder, a garnet-type lithium composite metal oxide, and an all-solid-state battery.
The amorphous composite metal oxide powder, manufactured through controlled heat treatment and specific composition, addresses the issue of low ionic conductivity in existing garnet-type lithium composite metal oxides, enabling high-performance all-solid-state batteries.
Patent Information
- Application Number
- KR1020267033556
- Authority / Receiving Office
- KR · KR
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-03-11
- Filing Date
- 2024-09-19
- Publication Date
- 2026-11-09
AI Technical Summary
Existing methods for manufacturing garnet-type lithium composite metal oxides result in low ionic conductivity due to impurities like carbon and require high temperatures, leading to potential short circuits and reduced conductivity.
An amorphous composite metal oxide powder with specific compositions and manufacturing processes, including controlled heat treatment below 700°C, to produce a garnet-type lithium composite metal oxide with high ionic conductivity.
The method produces a garnet-type lithium composite metal oxide with high ionic conductivity and a single-phase crystal structure, suitable for all-solid-state batteries, even at low calcination temperatures.
Smart Images

Figure PCT00005_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to an amorphous composite metal oxide powder comprising La (lanthanum) and Zr (zirconium) and a method for manufacturing the same. Furthermore, the invention relates to a method for manufacturing a garnet-type lithium composite metal oxide. Additionally, the invention relates to a method for manufacturing an all-solid-state battery using the garnet-type lithium composite metal oxide. Background Technology
[0002] Compared to conventional rechargeable batteries, lithium-ion rechargeable batteries are lightweight, high-capacity, and high-power, so they are widely used in electronic devices such as PCs and mobile phones, as well as in automotive batteries. In particular, the development of all-solid-state lithium-ion rechargeable batteries, which offer superior safety, has recently been underway.
[0003] Many lithium-ion conductors are used as solid electrolytes for all-solid-state batteries. Among them, complex metal oxides with a garnet-type crystal structure containing lithium are known. An example of such a garnet-type lithium complex metal oxide is Li7La3Zr2O containing Li, La, and Zr. 12 It is known that various metal elements have been added to (hereinafter also referred to as “LLZ”) or LLZ.
[0004] For example, Patent Document 1 describes a volume-based average particle diameter D in which Al, Ga, Y, Ce, Ca, Ba, Sr, Nb, and Ta are added to a garnet-type lithium composite metal oxide containing Li, La, and Zr in order to increase ionic conductivity. 50 A garnet-type lithium complex metal oxide containing Li with a thickness of 0.5 μm or more and 50 μm or less is disclosed. The complex metal oxide is said to be obtained by using a precipitate obtained by reacting a precipitate precipitated from an aqueous solution containing carbonate ions and La ions with a zirconium carbonate complex as a precursor, and by calcining a mixture of said precursor and a lithium compound.
[0005] Patent Document 2 describes a manufacturing method for obtaining a garnet-type lithium composite metal oxide that can be sintered at a low temperature and has a high ion conductivity upon sintering, wherein an amorphous composite metal oxide comprising La, Zr and Nb, Ta, V, and Bi is prepared as a raw material for the garnet-type lithium composite metal oxide, and a mixture of the amorphous composite metal oxide and a lithium salt is sintered.
[0006] Patent document 3 discloses a method for manufacturing an amorphous composite oxide containing La and Zr and not Li, to be used as a precursor for synthesizing a composite oxide containing a garnet-type composite oxide. Prior art literature
[0007] Japanese Patent Publication No. 6916406, Japanese Published Patent Application No. 2021-138554, Japanese Published Patent Application No. 2017-214247 The problem to be solved
[0008] In the industrial manufacturing process of all-solid-state batteries, it is generally assumed that an electrode active material and a solid electrolyte are mixed, and a sintering process is performed to form a good bond between the electrode active material and the solid electrolyte. In the above sintering process, the heating temperature is limited due to the need to prevent adverse effects such as the electrode active material and the solid electrolyte reacting, and it is desired to perform firing and sintering in a temperature range of, for example, 700°C or lower.
[0009] However, the garnet-type lithium composite metal oxide disclosed in Patent Document 1 is thought to have low ionic conductivity because it does not form a single-phase garnet structure when sintered at a low temperature of 700°C or lower.
[0010] The amorphous composite metal oxide powder, which serves as a raw material (precursor) for a garnet-type lithium composite metal oxide disclosed in Patent Document 2, is synthesized by a process including a reaction that esterifies a metal chelate compound and a chelate polymer; therefore, the resulting precursor contains hydrocarbons as impurities and has low ionic conductivity. Furthermore, Patent Document 2 states, for example, "Next, the gel obtained by the esterification reaction is calcined. By calcining the gel, the carbon-carbon bonds and carbon-hydrogen bonds contained in the gel are broken and carbonized, and a precursor consisting of an oxide in an amorphous state is obtained (paragraph 0050)." or "In addition, in the heat treatment process for heat-treating the precursor, it is not necessary to remove some or all of the organic residues, such as soot, remaining in the precursor. The organic residues remaining in the precursor acquire electronic conductivity by carbonizing." Therefore, there is a description such as, "If the remaining organic residue is not removed, the precursor becomes electronically conductive due to the organic residue (paragraph 0055)," and it is believed that the amorphous composite metal oxide powder is allowed to contain carbon. If the amorphous composite metal oxide powder has electronic conductivity, it is not desirable as a solid electrolyte material in an all-solid-state battery because there is a possibility of causing a partial short circuit when the metal oxide powder is used as an electrolyte in an electrochemical device. Furthermore, it is believed that the garnet-type lithium composite oxide produced by the technology disclosed in Patent Document 2 is prone to containing anomalies due to carbon as an impurity, and thus its ionic conductivity is reduced.
[0011] In the case of the method for manufacturing an amorphous composite oxide containing La and Zr and not containing Li described in Patent Document 3, an acetate is used as a starting material. The acetate remains as a carbonate after thermal decomposition, and in order to completely remove the carbonate, it is necessary to perform heat treatment on the amorphous powder at 800°C or higher.
[0012] To solve the above problem, the present invention aims to provide an amorphous composite metal oxide powder that can obtain a lithium composite metal oxide having a garnet-type crystal structure and high ionic conductivity even when calcined at a low temperature of 700°C or lower, as a precursor for synthesizing a garnet-type lithium composite metal oxide. In addition, the invention aims to provide a garnet-type lithium composite metal oxide and an all-solid-state battery using the same. means of solving the problem
[0013] [1] To achieve the above objective, the present invention provides an amorphous composite metal oxide powder containing La and Zr, wherein La is 40 mass% or more and 62 mass% or less, Zr is 8 mass% or more and 26 mass% or less, and a metal element M, excluding La and Zr, is 1 mass% or more and 20 mass% or less, and has a carbon content of 1.5 mass% or less, and the remainder is oxygen and unavoidable impurities.
[0014] [2] The amorphous composite metal oxide powder containing La and Zr of [1] above preferably has a molar ratio of La, Zr, and metal element M in the amorphous composite metal oxide powder of La:Zr:M = 3:1.2~1.95:0.05~0.8.
[0015] [3] The amorphous composite metal oxide powder containing La and Zr of [1] above is preferably one in which the oxidation number of the metal element M can take is 5.
[0016] [4] The amorphous composite metal oxide powder containing La and Zr of [1] above preferably has one or more of the metal elements M among Ta, Nb, V and Sb.
[0017] [5] The amorphous composite metal oxide powder containing La and Zr of [1] to [4] above preferably has a nitrogen content of 3 mass% or less as an unavoidable impurity.
[0018] [6] The present invention also provides a method for manufacturing an amorphous composite metal oxide powder containing La and Zr according to [1], comprising the steps of: obtaining a slurry containing a co-precipitate containing La, Zr and a metal element M excluding La and Zr, which is a metal element capable of taking an oxidation state of any one of 3 to 6; recovering the co-precipitate containing La, Zr and the metal element M by solid-liquid separation from the slurry containing the co-precipitate containing La, Zr and the metal element M; and heat treating the recovered co-precipitate containing La, Zr and the metal element M at less than 800°C.
[0019] [7] In the method for producing an amorphous composite metal oxide powder containing La and Zr according to [6] above, the process of obtaining a slurry containing a co-precipitate containing La, Zr and metal element M may be to simultaneously dissolve an inorganic La compound, an inorganic Zr compound and an inorganic metal element M compound in water.
[0020] [8] In the method for manufacturing an amorphous composite metal oxide powder containing La and Zr according to [6] above, the process of obtaining a slurry containing a co-precipitate containing La, Zr and a metal element M may include the process of dissolving an inorganic La compound and an inorganic Zr compound in water to prepare an aqueous solution containing La-Zr, the process of dissolving an inorganic metal element M compound in water to prepare an aqueous solution containing a metal element M, and the process of mixing the aqueous solution containing La-Zr and the aqueous solution containing a metal element M.
[0021] [9] In the method for manufacturing an amorphous composite metal oxide powder containing La and Zr of [6] above, it is preferable that the heat treatment temperature in the heat treatment process is 700°C or lower.
[0022]
[10] In the method for manufacturing an amorphous composite metal oxide powder containing La and Zr of [6] above, it is preferable that the heat treatment temperature in the heat treatment process be 150°C or higher.
[0023]
[11] In the method for preparing an amorphous composite metal oxide powder containing La and Zr of [7] above, it is preferable that the inorganic La compound, the inorganic Zr compound, and the inorganic metal element M compound each do not contain carbon in their molecular structures.
[0024]
[12] The method for preparing an amorphous composite metal oxide powder containing La and Zr according to [8] above is preferably such that the inorganic La compound, the inorganic Zr compound, and the inorganic metal element M compound each do not contain carbon in their molecular structures.
[0025]
[13] The method for preparing an amorphous composite metal oxide powder containing La and Zr of [8] above is preferably such that the aqueous solution containing the metal element M comprises a compound of the inorganic metal element M, water of ammonia, and a peroxo complex of the metal element M produced by mixing hydrogen peroxide and water.
[0026]
[14] The method for manufacturing an amorphous composite metal oxide powder containing La and Zr according to [6] above is preferably such that the metal element M is one or more of Ta, Nb, V and Sb.
[0027]
[15] The method for producing an amorphous composite metal oxide powder containing La and Zr according to [6] above is preferably such that the molar ratio of La, Zr and metal element M in a slurry containing a co-precipitate containing La, Zr and metal element M is La:Zr:M=3:1.2~1.95:0.05~0.8.
[0028]
[16] In the method for manufacturing an amorphous composite metal oxide powder containing La and Zr according to [6] to
[15] above, when separating solids and liquids from a slurry containing a co-precipitate containing La, Zr and a metal element M, it is preferable to wash the co-precipitate containing La, Zr and a metal element M.
[0029]
[17] The present invention also provides a method for producing a garnet-type lithium composite metal oxide by calcining a mixture of an amorphous composite metal oxide powder containing La and Zr as described in [1] and a Li compound.
[0030]
[18] In the method for manufacturing the garnet-type lithium composite metal oxide of
[17] above, it is preferable that the temperature at which the mixture of amorphous composite metal oxide powder containing La and Zr and a Li compound is calcined is 300°C or higher and less than 700°C.
[0031]
[19] In the method for manufacturing the garnet-type lithium composite metal oxide of
[17] above, when mixing the amorphous composite metal oxide powder containing La and Zr with the Li compound, it is preferable to have the molar ratio of Li, La, Zr and metal element M as Li:La:Zr:M = 6.5~7.5:3:1.2~1.95:0.05~0.8.
[0032]
[20] In addition to the present invention, when manufacturing an all-solid-state battery having a battery unit having a structure in which a solid electrolyte layer is disposed between a positive electrode layer containing a positive electrode active material and a negative electrode layer containing a negative electrode active material,
[0033] A method for manufacturing an all-solid-state battery is provided, wherein at least one of the anode layer, the cathode layer, and the solid electrolyte layer comprises a garnet-type lithium composite metal oxide manufactured by a manufacturing method described in any one of
[17] to
[19] . Effects of the invention
[0034] According to the present invention, it is possible to provide an amorphous composite metal oxide powder containing La, Zr, and a metal element M capable of taking an oxidation state of 3 to 6, which becomes a raw material for a garnet-type lithium composite metal oxide that has a garnet-type crystal structure even when calcined at a low temperature of 700°C or lower and also exhibits high ionic conductivity. In addition, a method for manufacturing the amorphous composite metal oxide powder and a suitable method for manufacturing a garnet-type lithium composite metal oxide using the amorphous composite metal oxide powder as a raw material are also possible. Brief explanation of the drawing
[0035] [Fig. 1] FT-IR spectra of aqueous solutions of metal element M obtained in Example 1 and Example 11. [Fig. 2] XRD spectra of the amorphous composite metal oxide powders of Examples 1, 7, 9, and 10 and the composite metal oxide powder according to Comparative Example 2. [Fig. 3] This figure shows the charge / discharge characteristics of a battery composed of a mixture of the composite metal oxide powder obtained by Example 4-2 and a composite oxide (NCM powder) containing Li, Ni, Co, and Mn as the powder for the positive electrode composite electrode, and a mixture of the composite metal oxide powder obtained by Example 4-2 and a composite oxide powder of Li and Ti (LTO powder) as the powder for the negative electrode composite electrode. [Fig. 4] A cross-sectional view schematically illustrating one embodiment of an all-solid-state battery configuration. Specific details for implementing the invention
[0036] [Amorphous composite metal oxide powder]
[0037] In the present invention, an amorphous composite metal oxide powder containing La and Zr is used as a starting material (precursor) for synthesizing a garnet-type lithium composite metal oxide in which a portion of the metal elements of LLZ, a composite metal oxide with a garnet-type crystal structure containing lithium, is substituted with other metal elements. In order to synthesize a composite metal oxide with a garnet-type crystal structure in which a portion of the metal elements of LLZ is substituted with other metal elements, the amorphous composite metal oxide powder contains a metal element M excluding La and Zr, which ultimately become the substituent elements. At this time, the metal element M is a metal element capable of taking an oxidation state of any one of 3 to 6.
[0038] The amorphous composite metal oxide powder containing La and Zr according to the present invention is characterized by being amorphous. Since the amorphous composite metal oxide powder has high reactivity, a garnet-type lithium composite metal oxide having high ionic conductivity can be obtained even when a mixture obtained by mixing with a Li salt is calcined at a low temperature of 700° or lower. Here, "amorphous" refers to a case where, in powder X-ray diffraction (XRD) measurements using CuKα rays, no clear diffraction peak is observed in the region of 2θ: 10° to 60°, and a so-called halo pattern appears. Furthermore, "halo" refers to a gentle fluctuation in X-ray intensity that is observed as a broad ridge in the XRD spectrum, and the full width at half maximum of the halo is 2° or more with respect to 2θ.
[0039] The amorphous composite metal oxide powder containing La and Zr according to the present invention contains La in an amount of 40 mass% or more and 62 mass% or less. By setting the La content to 40 mass% or more and 62 mass% or less, when a mixture of the amorphous composite metal oxide powder and a lithium salt is calcined and crystallized, a garnet-type lithium composite metal oxide having a single-phase garnet-type crystal structure is obtained. From the perspective of making it easier to obtain a single-phase garnet-type crystal structure, the La content is preferably 45 mass% or more, more preferably 48 mass% or more, and preferably 60 mass% or less.
[0040] The amorphous composite metal oxide powder containing La and Zr according to the present invention contains Zr in an amount of 8 mass% or more and 26 mass% or less. By setting the Zr content to 8 mass% or more and 26 mass% or less, when a mixture of the amorphous composite metal oxide powder and a lithium salt is calcined and crystallized, a garnet-type lithium composite metal oxide having a single-phase garnet-type crystal structure is obtained. From the perspective of making it easier to obtain a single-phase garnet-type crystal structure, the Zr content is preferably 10 mass% or more, more preferably 14 mass% or more, and preferably 25 mass% or less.
[0041] The amorphous composite metal oxide powder containing La and Zr according to the present invention contains 1 mass% or more and 20 mass% or less of a metal element M, excluding La and Zr, which is a metal element capable of taking an oxidation state of 3 to 6. In a lithium composite metal oxide having a garnet-type crystal structure, there exist tetracoordinate lithium ions forming a tetrahedron with four oxygen ions as vertices and hexacoordinate lithium ions forming an octahedron with six oxygen ions as vertices. Here, if Zr sites are substituted with a metal element M capable of taking an oxidation state of 3 to 6, the atomic coordinates of the oxygen ions around the lithium ions change. At this time, it is presumed that ion conductivity is improved because the distance between the oxygen ions around the lithium ions widens and the movement of the lithium ions becomes easier when the amount of substitution is controlled. Therefore, the amorphous composite metal oxide powder needs to contain 1 mass% or more of the metal element M. In addition, since it is thought that ionic conductivity decreases when a large amount of metal element M capable of taking an oxidation state of 3 to 6 is contained, the metal element M in the amorphous composite metal oxide powder is kept at 20 mass% or less. From the perspective of ionic conductivity, the content of metal element M capable of taking an oxidation state of 3 to 6 is preferably 13 mass% or less, more preferably 10 mass% or less, and even more preferably 8 mass% or less.
[0042] The amorphous composite metal oxide powder containing La and Zr is preferably such that, in terms of ionic conductivity, the ratio of La, Zr, and metal element M is La:Zr:M = 3:1.2 to 1.95:0.05 to 0.8 in molar ratio.
[0043] The amorphous composite metal oxide powder containing La and Zr is preferably such that the total molar ratio of La, Zr, and M is 4.5 to 5.5, and more preferably 4.75 to 5.25.
[0044] In the amorphous composite metal oxide powder containing La and Zr according to the present invention, the metal element M comprises a metalloid element. As the metal element M capable of taking an oxidation state of 3 to 6, it is preferable that it be one or more of Ta (tantal), Nb (niobium), V (vanadium), Sb (antimony), Sc (scandium), Ti (titanium), Y (yttrium), Hf (hafnium), Mo (molybdenum), W (tungsten), Al (aluminum), Si (silicon), Ga (gallium), Ge (germanium), Bi (bismuth), and Sn (tin). From the perspective of increasing ionic conductivity, it is preferable that the metal element M be a metal element capable of taking an oxidation state of 5. Since the lattice volume of the garnet-type lithium composite oxide can be optimized, one or more of the elements among the pentavalent elements, such as Ta (0.64), Nb (0.64), Sb (0.60), and V (0.54), have ionic radii close to that of Zr (0.72), are preferred, and one or two of Ta and Nb are more preferred.
[0045] [Carbon content]
[0046] As described above, the amorphous composite metal oxide powder containing La and Zr according to the present invention is composed of La, Zr, the metal element M, and O (oxygen), but also contains C (carbon) which is inevitably incorporated during the manufacturing process. It is preferable that the carbon content of the amorphous composite metal oxide powder be 1.5 mass% or less. By controlling the carbon content to 1.5 mass% or less, the ionic conductivity of the garnet-type lithium composite metal oxide having a garnet-type crystal structure obtained can be increased. It is presumed that by lowering the carbon content of the amorphous composite metal oxide powder, the inhibition of Li ion movement by carbon in the garnet-type lithium composite metal oxide finally obtained through low-temperature calcination at 700°C or lower can be suppressed, thereby improving ionic conductivity. It is more preferable that the carbon content of the amorphous composite metal oxide powder be 1.4 mass% or less. However, since carbon is incorporated into the amorphous composite metal oxide powder due to carbon dioxide in the air, etc., it is practically difficult to keep the carbon content less than 0.01 mass%, and the lower limit of the carbon content of the amorphous powder is usually 0.01 mass% or more.
[0047] [Nitrogen content]
[0048] The amorphous composite metal oxide powder containing La and Zr according to the present invention is permitted to contain unavoidable impurities other than La, Zr, the metal element M, carbon, and O (oxygen) described below, to the extent that it does not impair the effects of the present invention. Among the unavoidable impurities contained in the amorphous composite metal oxide powder, N (nitrogen) may be considered as potentially lowering the ionic conductivity of the finally obtained garnet-type lithium composite metal oxide. In the present invention, the nitrogen content of the amorphous powder is preferably 3 mass% or less, more preferably 2 mass% or less, and even more preferably 1.5 mass% or less. The lower limit of the nitrogen content is not particularly limited, but, for example, it may be 0.1 mass% or more.
[0049] Furthermore, by using the manufacturing method of the present invention described below, the amount of unavoidable impurities contained in the amorphous composite metal oxide powder containing La and Zr of the present invention, other than the oxygen and nitrogen, becomes negligible.
[0050] [Oxygen Content]
[0051] The amorphous composite metal oxide powder containing La and Zr of the present invention, obtained by using the manufacturing method of the present invention described below, contains La, Zr, metal element M, carbon, and nitrogen as described above. Accordingly, the oxygen content (mass%) contained in the amorphous powder can be calculated by the following formula (1).
[0052] Oxygen content (mass%) = 100 - (La content + Zr content + metallic element M content + carbon content + nitrogen content)(mass%) … (1)
[0053] The oxygen content included in the amorphous composite metal oxide powder containing La and Zr of the present invention is preferably 5 mass% or more and 35 mass% or less.
[0054] [BET Specific Surface Area]
[0055] The amorphous composite metal oxide powder containing La and Zr according to the present invention preferably has a BET specific surface area of 10 m² / g or more and 150 m² / g or less in terms of low-temperature sinterability. If the BET specific surface area is 10 m² / g or more and 150 m² / g or less, it is presumed that when a mixture obtained by mixing the amorphous powder and a Li salt is sintered at a low temperature of 700°C or lower, heat is transferred uniformly to the mixture and crystallization proceeds uniformly throughout the particles, thereby improving the ion conductivity of the finally obtained garnet-type lithium composite metal oxide. The BET specific surface area of the amorphous powder is preferably 140 m² / g or less, more preferably 130 m² / g or less, even more preferably 100 m² / g or less, and even more preferably 90 m² / g or less in terms of improving ion conductivity.
[0056] [Method for manufacturing amorphous composite metal oxide powder]
[0057] [Starting material]
[0058] In the present invention, as a method for manufacturing amorphous composite metal oxide powder containing La and Zr, a wet method is adopted that has excellent mass production efficiency and low manufacturing cost.
[0059] The method for manufacturing an amorphous composite metal oxide powder containing La and Zr according to the present invention comprises: a process of obtaining a slurry containing a co-precipitate containing La, Zr and a metal element M; a process of recovering the co-precipitate containing La, Zr and a metal element M by solid-liquid separation from the slurry containing the co-precipitate containing La, Zr and a metal element M; and a process of heat-treating the recovered co-precipitate containing La, Zr and a metal element M at less than 800°C.
[0060] A known coprecipitation method may be used for the process of obtaining a slurry containing a coprecipitate containing La, Zr, and a metal element M. In the present invention, the process of obtaining a slurry containing a coprecipitate containing La, Zr, and a metal element M can take two aspects as two embodiments. The first embodiment is to obtain the slurry by simultaneously dissolving La, Zr, and the metal element M in water. At this time, in order to reduce the carbon content contained in the amorphous composite metal oxide powder, organometallic compounds containing hydrocarbon groups or carboxyl groups, etc., are not preferred as starting materials for La, Zr, and the metal element M, and inorganic metal compounds are used. As inorganic metal compounds, inorganic La compounds, inorganic Zr compounds, and inorganic metal element M compounds may be used.
[0061] In the second embodiment, an aqueous solution containing La-Zr is prepared by first dissolving La and Zr in water, and an aqueous solution containing metal element M is prepared by dissolving metal element M, excluding La and Zr, in water as a metal element capable of taking an oxidation state of 3 to 6, and these solutions are mixed. In the second embodiment as well, in order to reduce the carbon content contained in the amorphous composite metal oxide powder, the inorganic metal compounds, such as an inorganic La compound, an inorganic Zr compound, and an inorganic metal element M compound, may be used as starting materials for La, Zr, and metal element M. The aqueous solution containing La-Zr may be prepared by simultaneously dissolving the inorganic La compound and the inorganic Zr compound in water, or by mixing an aqueous solution in which the inorganic La compound is dissolved in water and an aqueous solution in which the inorganic Zr compound is dissolved in water.
[0062] As for inorganic metal compounds that are soluble in water, for example, oxides, hydroxides, nitrates, chlorides, sulfates, carbonates, etc. of La, Zr, or metal element M can be used. When carbonates are used as inorganic metal compounds, carbonate ions can be released as gas by heat treatment at less than 800°C for the co-precipitates containing La, Zr and metal element M described later, so it is possible to reduce the carbon content in the amorphous composite metal oxide powder, but from the perspective of lowering the temperature of the heat treatment, it is preferable to use metal compounds that do not contain carbon in their molecular structure.
[0063] The above metal element M is preferably one or more of Ta, Nb, V, and Sb capable of taking a pentavalent oxidation state, and more preferably one or two of Ta and Nb. If the metal element M is a metal that is sparingly soluble in water, such as pentavalent Ta, Nb, V, Sb, etc., it is preferable to use a complexing agent to form a water-soluble metal complex from the metal compound, or to dissolve it in water by forming it into a polyoxide ion. As for the water-soluble metal complex, it is preferable to form a peroxo complex having a peroxy group, given that it does not contain carbon in its molecular structure. Peroxo complexes such as Ta or Nb can be obtained by mixing a Ta compound or an Nb compound with an alkaline water such as ammonia water and hydrogen peroxide water.
[0064] When preparing an aqueous solution of a peroxo complex of Ta or Nb, it is preferable to add and mix the ammonium ions in the ammonia solution in excess such that the amount of ammonium ions is preferably 3 moles or more, more preferably 10 moles or more, and even more preferably 30 moles or more per 1 mole of Ta or Nb. In addition, to suppress an increase in the nitrogen content of the amorphous composite metal oxide powder, it is preferable to add and mix the ammonium ions in the ammonia solution such that the amount of ammonium ions is preferably 80 moles or less, more preferably 70 moles or less, and even more preferably 50 moles or less per 1 mole of Ta or Nb.
[0065] It is preferable to add and mix hydrogen peroxide in excess such that, preferably, at least 8 moles, more preferably at least 10 moles, and even more preferably at least 30 moles per 1 mole of Ta or Nb. In addition, to suppress an increase in the nitrogen content in the amorphous composite metal oxide powder, it is preferable to add and mix hydrogen peroxide such that, preferably, at least 80 moles, more preferably at least 70 moles, and even more preferably at least 50 moles per 1 mole of Ta or Nb.
[0066] Whether Ta or Nb, etc. contained in the aqueous solution is a peroxo complex can be confirmed by FT-IR measurement. If Ta or Nb, etc. in the aqueous solution takes the form of a peroxo complex, the wavenumber is 820 cm⁻¹ -1 ±10cm -1 An absorption peak attributed to the OO bond of the peroxo is observed in the vicinity.
[0067] Polyacids are anionic species formed by the condensation of oxoacids, and polyacids of metal element M can be regarded as molecular ionic species of metal oxides. Furthermore, if there is only one type of metal element M, it is called an isopolyacid, and if there are multiple metal elements, it is called a heteropolyacid. When preparing an aqueous solution containing Nb polyacid ions, proceed as follows.
[0068] Although a potential-pH diagram for niobium is not currently established, since niobium hydroxide precipitates in the neutral region, it is thought that solid phases such as Nb(OH)5 or HNbO3 are stable chemical species in the aforementioned pH range. If an alkali is added to an aqueous solution containing these solid phases to raise the pH of the system, the presence of excess OH- ions causes niobium to, for example, Nb(OH)6 - or NbO3 - It begins to dissolve in the form of etc. If the pH of the system is further increased, it is thought that soluble niobium oxide will assume various condensation states depending on the pH of the system; however, in this specification, it is assumed that niobium oxide solubilized on the alkali side collectively becomes niobium polysate ions. That niobium in the aqueous solution is a polysate ion can be confirmed by FT-IR measurement. When niobium in the aqueous solution takes the form of a polysate ion, the wavenumber is 850 cm⁻¹ -1 ±10cm -1 An absorption peak attributed to the Nb-O bond is in the vicinity, 680±20 cm⁻¹ -1 An absorption peak attributed to the Nb-O-Nb bond is observed in the vicinity.
[0069] [Formation and Recovery of Co-precipitates]
[0070] In the method for manufacturing an amorphous composite metal oxide powder containing La and Zr according to the present invention, an aqueous solution containing La-Zr prepared in the above process and an aqueous solution containing a metal element M are mixed under stirring conditions, and the pH of the mixed aqueous solution is preferably set to 10 or higher and 12 or lower to produce a co-precipitate in which a hydroxide of La, Zr, and a metal element M is mixed, thereby obtaining a slurry containing said co-precipitate. Even if the aqueous solution containing La-Zr described below is acidic and the aqueous solution containing the metal element M is alkaline, each component element can be uniformly co-precipitated by stirring and mixing while maintaining the pH of the mixed solution within the above range.
[0071] It is preferable to mix the molar ratio of La, Zr, and metal element M contained in the above slurry such that La:Zr:M = 3:1.2 to 1.95:0.05 to 0.8. It is preferable that the sum of the molar ratios of La, Zr, and metal element M contained in the above slurry is 4.5 to 5.5, and more preferably 4.75 to 5.25. If the pH of the mixed aqueous solution is less than 10, the component elements are not uniformly co-precipitated, and there is a possibility that a variation in the composition of the obtained amorphous composite metal oxide powder may occur. If the pH of the mixed aqueous solution exceeds 12, the amount of alkali added for pH adjustment increases, and manufacturing costs rise, which is undesirable.
[0072] It is preferable that the molar ratio of La, Zr, and metal element M contained in the resulting co-precipitate be La:Zr:M = 3:1.2 to 1.95:0.05 to 0.8. It is preferable that the sum of the molar ratios of La, Zr, and metal element M contained in the co-precipitate be 4.5 to 5.5, and more preferably 4.75 to 5.25.
[0073] By using the coprecipitation method, a supersaturated state can be realized in which the ion concentration product of the constituent elements in the mixed slurry is higher than the solubility product, which contributes to improving the uniformity of the constituent elements and allows for the obtaining of the amorphous composite metal oxide powder of the present invention. It is believed that the slurry contains constituent elements precipitated as hydroxides and constituent elements existing in an ionic state.
[0074] When an aqueous solution containing a peroxo complex of a pentavalent metal or an aqueous solution containing a polyoxide ion is used as an aqueous solution containing a metal element M, since the aqueous solution itself is alkaline, the pH of the aqueous solution mixed with the La-Zr aqueous solution and the aqueous solution containing the metal element M automatically becomes the preferred pH range mentioned above, and a hydroxide is co-precipitated to obtain a slurry.
[0075] If the pH of the above-mentioned mixed aqueous solution is less than 10, an alkaline aqueous solution with a pH greater than 10 is added to produce a co-precipitate with the pH of the above-mentioned mixed aqueous solution within the preferred range. In this case, the alkaline aqueous solution to be added may include hydroxides of alkali metals or alkaline earth metals, aqueous carbonate solutions, or ammonia water, but it is preferable to use ammonia water, which is less likely to leave impurities in the finally obtained garnet-type lithium complex metal oxide.
[0076] The La content in the mixed slurry is preferably 1 mass% or more and 5 mass% or less. The Zr content in the mixed slurry is preferably 0.2 mass% or more and 2.5 mass% or less. The metal element M content in the mixed slurry is preferably 0.01 mass% or more and 1 mass% or less.
[0077] From a slurry containing a co-precipitate containing La, Zr, and a metal element M obtained in the above process, said co-precipitate is recovered using a solid-liquid separation means. As the solid-liquid separation means, known solid-liquid separation means such as filter filtration, ultrafiltration, or centrifugation may be used. At this time, it is desirable to wash the recovered co-precipitate to reduce impurities such as ammonia remaining in the precipitate. In terms of reducing impurities such as ammonia remaining in the precipitate, it is desirable to wash until the pH of the washing water becomes 9 or lower. By washing until the pH of the washing water becomes 9 or lower, the amount of ammonia, etc. remaining in the precipitate can be reduced. Accordingly, the nitrogen content in the amorphous composite metal oxide powder containing La and Zr can be reduced.
[0078] [Heat Treatment]
[0079] In the method for manufacturing an amorphous composite metal oxide powder containing La and Zr according to the present invention, by heat-treating a co-precipitate containing La, Zr and a metal element M recovered in the above process under an atmosphere or an inert atmosphere (nitrogen, argon, etc.), an amorphous composite metal oxide powder containing La and Zr, which serves as a precursor for synthesizing a garnet-type lithium composite metal oxide, can be obtained.
[0080] The temperature of the above heat treatment is set to less than 800°C. If the temperature of the heat treatment is 800°C or higher, the complex metal oxide powder containing La and Zr may crystallize and take on a fluorite-type crystal structure, which is undesirable. More preferably, the temperature of the heat treatment is 700°C or lower, and even more preferably 600°C or lower. In the present invention, the time of the heat treatment is not specifically specified, but from a process perspective, it is preferable that the time of the heat treatment be 1 hour or more and 6 hours or less.
[0081] In terms of reducing the nitrogen content of the above-mentioned co-precipitate, it is preferable to set the temperature of the heat treatment to 150°C or higher. More preferably, it is 300°C or higher, and even more preferably 400°C or higher.
[0082] In the method for manufacturing an amorphous composite metal oxide powder containing La and Zr according to the present invention, a drying process for removing moisture from the co-precipitate may be provided before the heat treatment process. In this case, the drying temperature is preferably 80 to 110°C.
[0083] [Garnet-type lithium complex metal oxide]
[0084] When using the amorphous composite metal oxide powder containing La and Zr obtained in the above process, a single-phase garnet-type lithium composite metal oxide having high ionic conductivity can be obtained even when the mixture of the amorphous powder and the Li compound is calcined at a low temperature of 600°C or lower, which is 700°C or lower.
[0085] From the perspective of ionic conductivity, it is preferable that the garnet-type lithium composite metal oxide is single-phase. Whether the composite metal oxide is garnet-type can be confirmed by comparing the XRD spectrum measured using an X-ray diffraction (XRD) device with the diffraction pattern of a garnet-type oxide (garnet-type structure of space group Ia-3d) embedded in an electronic computer attached to the device. In addition, whether the garnet-type lithium composite metal oxide is single-phase can be confirmed in the same way.
[0086] The garnet-type lithium composite metal oxide of the present invention is of the general formula Li7La3Zr 2-y M y O 12 It is preferable that it be represented as follows. Here, M is a metal element capable of taking oxidation states from 3 to 6. y is 0 <y≤1.0을 만족하는 값이다. 또한, 가넷형 리튬 복합 산화물로 했을 때의 이온 전도도와 격자 체적의 관계로부터 0.05≤y≤0.8인 것이 바람직하다.
[0087] The metal element M capable of taking oxidation states of 3 to 6 includes metalloid elements such as Ge and Si. The metal element M is preferably one or more of Ta, Nb, V, Sb, Sc, Ti, Y, Hf, Mo, W, Al, Si, Ga, Ge, and Sn. To increase ionic conductivity, one or more of Ta, Nb, V, and Sb capable of taking oxidation states of 5 are more preferable, and even more preferably Ta and Nb. The garnet-type lithium composite metal oxide of the present invention, even if obtained at a calcination temperature of 600°C or lower, has a ion conductivity of 9.0 × 10⁻⁶ in the measurement of ionic conductivity described later. -6 It has an ionic conductivity of S / cm or higher.
[0088] [Method for manufacturing garnet-type lithium composite metal oxide]
[0089] In the method for manufacturing a garnet-type lithium composite metal oxide of the present invention, a mixture of an amorphous composite metal oxide powder obtained by the method for manufacturing an amorphous composite metal oxide powder containing La and Zr and a Li compound is calcined to obtain a garnet-type lithium composite metal oxide.
[0090] As the Li compound mixed with the above-mentioned amorphous composite metal oxide powder, inorganic lithium compounds such as Li2O, Li2O2, and Li(OH)2 can be used. It is preferable to mix the amorphous powder and the Li compound by adjusting the ratio so that the molar ratio of Li, La, Zr, and the metal element M is Li:La:Zr:M = 6.5 to 7.5:3:1.2 to 1.95:0.05 to 0.8. It is preferable that the sum of the molar ratios of Li, La, Zr, and the metal element M is 11 to 13, and more preferably 11.5 to 12.5.
[0091] The above mixing method is not particularly limited in the method for manufacturing the garnet-type lithium composite metal oxide of the present invention, but it is preferable to mix wetly or dryly using a known mixing device such as a mixer or a ball mill.
[0092] It is preferable to perform the calcination of the mixture under a decarbonized atmosphere or an inert atmosphere (nitrogen, argon, etc.). By making the calcination atmosphere a decarbonized atmosphere or an inert atmosphere (nitrogen, argon, etc.), moisture or carbon dioxide in the atmosphere can be adsorbed, thereby suppressing the formation of abnormalities such as lithium carbonate in the garnet-type lithium complex metal oxide.
[0093] The calcination temperature of the above mixture is preferably 300°C or higher and less than 700°C from the perspective of obtaining a garnet-type lithium composite metal oxide at low temperature, and more preferably 600°C or lower. From the perspective of obtaining a garnet-type lithium composite metal oxide with higher ion conductivity, it is preferable to calcin at a temperature of 400°C or higher.
[0094] [All-solid-state battery]
[0095] FIG. 4 schematically illustrates a cross-sectional structure for one embodiment of an all-solid-state battery configuration. An anode layer and a cathode layer face each other with a solid electrolyte layer in between. The embodiment of FIG. 4 is an example of an all-solid-state battery having a single battery unit composed of an anode layer, a solid electrolyte layer, and a cathode layer. The anode layer includes an anode active material and, if necessary, includes a solid electrolyte or a conductive agent that exhibits lithium ion conductivity. The cathode layer includes a cathode active material and, if necessary, includes a solid electrolyte or a conductive agent that exhibits lithium ion conductivity. The solid electrolyte layer is composed of one or more solid electrolytes that exhibit lithium ion conductivity. The exchange of electrons with the outside during the charging and discharging of the battery is typically carried out through a current collector arranged to contact the anode layer and the cathode layer, respectively. The garnet-type lithium composite metal oxide obtained according to the present invention is useful as a solid electrolyte included in the anode layer, a solid electrolyte included in the cathode layer, and a solid electrolyte included in the solid electrolyte layer.
[0096] An all-solid-state battery using the garnet-type lithium composite metal oxide obtained according to the present invention can be obtained by a method for manufacturing an all-solid-state battery having a structure in which a solid electrolyte layer is disposed between a positive electrode layer containing a positive electrode active material and a negative electrode layer containing a negative electrode active material, for example, wherein at least one of the positive electrode layer, the negative electrode layer, and the solid electrolyte layer comprises the garnet-type lithium composite metal oxide.
[0097] In addition, as a cathode active material, not only can known materials be applied, but if a new cathode active material is developed, it can also be applied. Representative known cathode active materials include LiCoO2 (LCO type), LiNiO2 (LNO type), LiMn2O4 (LMO type), LiNiCoAlO2 (NCA type), LiNiCoMnO2 (NCM type), Li2MnO3-LiNiCoMnO2 (solid solution type), LiNiMnO4 (spinel type), LiMnFePO4 (phosphate type), and Li2FeSiO4 (silicate type).
[0098] Furthermore, as the negative electrode active material, not only can known materials be applied, but if a new negative electrode active material is developed, it can also be applied. Representative known negative electrode active materials include carbonaceous materials such as natural graphite, artificial graphite, resin carbon, carbon fiber, activated carbon, hard carbon, and soft carbon; conductive polymers such as polyacene, polyacetylene, and polypyrrole; metallic materials such as lithium, tin, silicon, gallium, indium, and aluminum; alloy-based materials such as lithium alloys, tin alloys, silicon alloys, gallium alloys, indium alloys, and aluminum alloys; and inorganic compounds such as lithium compounds, tin compounds, silicon compounds, gallium compounds, indium compounds, aluminum compounds, and titanium niobium oxide. Additionally, lithium compounds include lithium-titanium composite oxides, such as Li4Ti5O. 12 It is desirable.
[0099] As for the solid electrolyte constituting the solid electrolyte layer, the garnet-type lithium composite metal oxide obtained according to the present invention may be applied to part or all thereof, or only other solid electrolytes may be applied. As for the applicable solid electrolytes, in addition to the garnet-type lithium composite metal oxide obtained according to the present invention, a garnet-type lithium composite metal oxide containing Li, La, and Zr, for example, Li7La3Zr2O 12NASICON-type lithium complex metal oxides containing ), Li, Al, Ge, and P, for example, Li 1.5 Al 0.5 Ge 1.5 NASICON-type lithium complex metal oxides containing (PO4)3), Li, Al, Ti, and P, e.g., Li 1.5 Al 0.5 Ti 1.5 Perovskite-type lithium complex metal oxides containing (PO4)3), La, Li, and Ti, e.g., La 0.55 Li 0.35 Known materials include γII-Li3VO4 type lithium composite metal oxides containing TiO3), Li, and V.
[0100] Examples
[0101] [Elemental Analysis]
[0102] 0.05 g of a powder sample was taken from an amorphous composite metal oxide powder containing La and Zr or a garnet-type lithium composite metal oxide powder obtained in the examples and comparative examples, and 2 ml of 35 mass% hydrochloric acid, 2 ml of 60 mass% nitric acid, and 2 ml of 47.5 mass% sulfuric acid were added to dissolve it, and the obtained solution was appropriately diluted and volumetric as needed, and then elemental analysis was performed using an inductively coupled plasma emission spectrometer (ICP-AES, CP-720 manufactured by Agilent Technologies Co., Ltd.) to calculate the content of constituent elements in the powder sample.
[0103] [Carbon Content Measurement]
[0104] The carbon content in the powder obtained in the examples and comparative examples was analyzed using a trace carbon analyzer (EMIA-U510 manufactured by Horiba, Inc.).
[0105] [Nitrogen Content Measurement]
[0106] The nitrogen content in the powder obtained in the examples and comparative examples was analyzed using a nitrogen analyzer (EMGA-920 manufactured by Horiba, Inc.).
[0107] [BET Specific Surface Area Measurement]
[0108] The BET specific surface area of the amorphous composite metal oxide powder containing La and Zr obtained in the examples and comparative examples was measured using the BET single-point method with a BET specific surface area measuring instrument (Macsorb manufactured by Mountec Co., Ltd.). The measurement was performed by degassing by flowing nitrogen gas through the measuring instrument at 105°C for 20 minutes, and then flowing a mixed gas of nitrogen and helium (nitrogen: 30 vol%, helium: 70 vol%).
[0109] [XRD Measurement Conditions]
[0110] XRD measurements were performed on the amorphous composite metal oxide powder or garnet-type lithium composite metal oxide powder containing La and Zr obtained in the examples and comparative examples under the following measurement conditions.
[0111] Measuring device: XRD-6100 (Manufactured by Shimadzu Corporation)
[0112] Tube: Cu
[0113] Tube voltage: 40kV
[0114] Tube current: 30mA
[0115] Diverging slit: 1.0°
[0116] Scattering slit: 1.0°
[0117] Light receiving slit: 0.3mm
[0118] Step width: 0.02° / step
[0119] Measurement time: 0.25 sec
[0120] For peak search, the XRD-6100 software manufactured by Shimadzu Corporation was used.
[0121] Peak search conditions were performed under the following conditions.
[0122] Smoothing: Automatic
[0123] Background processing: Automatic
[0124] Kα1-α2 ratio: 50
[0125] Peak Search: Automatic
[0126] [Measurement of Ion Conductivity]
[0127] A powder sample of 0.15 g was taken from the garnet-type lithium composite metal oxide powder obtained in the examples and comparative examples, placed into a cylindrical container with a diameter of 10 mm, and after reaching 340°C, hot pressing was performed using a press machine at a pressure of 360 MPa for 2 hours to produce a compact with a thickness of 0.5 to 1 mm. For the compact, AC impedance measurements were performed in the range of 100 Hz to 4 MHz using a potentiometer / galvanostat (Solartron 1470E) and a frequency response analyzer (Solartron 1255B) under atmospheric conditions and a temperature of 25°C. The obtained measurements were plotted on a Cole-Cole plot (complex impedance plane plot), and the resistance value of the compact of the garnet-type lithium composite metal oxide powder was obtained from the intercept, and the ionic conductivity was calculated from the obtained resistance value.
[0128] [FT-IR Measurement]
[0129] The FT-IR spectrum of an aqueous solution of the metal element M described below was measured using a JASCO FT-IR instrument (FT-IR 4X) with water as a reference sample. For the measurement, the single-reflection ATR method was used, and the FT-IR measurement was performed at an angle of incidence of 45° to the germanium prism.
[0130] [Example 1]
[0131] In this embodiment, Ta, having an oxidation number of 5, is used as the metal element M. 4.50 g of TaCl5 (manufactured by Fujifilm Wako Pure Chemical), an inorganic metal element M compound that does not contain hydrocarbon groups in its molecular structure, was mixed with 100 g of pure water and stirred to prepare a slurry containing a precipitate containing Ta. The Ta-containing precipitate slurry was filtered and washed using a 0.5 μm membrane filter to recover the Ta-containing precipitate. The recovered Ta-containing precipitate was transferred to a 1 L beaker, repulped with 400 g of pure water, and then heated to 40°C. After heating, 40.0 g of ammonia water (manufactured by Fujifilm Wako Pure Chemical) with a concentration of 28 mass% and 30 g of hydrogen peroxide water (manufactured by Fujifilm Wako Pure Chemical) with a concentration of 35 mass% were added to the solution, and the mixture was stirred until the Ta-containing precipitate dissolved to obtain an aqueous solution of the metal element M. As a result of performing FT-IR measurements on a small sample of the obtained aqueous solution of metal element M, at 820 cm⁻¹ -1 ±10cm -1 Since an absorption peak attributable to the OO bond of the peroxo was observed, it was confirmed that a peroxo complex of Ta was being formed in the aqueous solution of the metal element M.
[0132] Figure 1 shows the FT-IR spectrum of an aqueous solution containing Ta as the metal element M obtained in this embodiment.
[0133] Next, 32.7 g of lanthanum nitrate hexahydrate (manufactured by Fujifilm Wako Pure Chemical), an inorganic La compound, and 1.01 g of zirconium oxynitrate dihydrate (manufactured by Kishida Chemical), a Zr compound that does not contain hydrocarbon groups in its molecular structure, were added to 400 g of pure water and heated to 40°C while stirring to dissolve them, thereby obtaining an aqueous solution containing La-Zr.
[0134] Next, the La-Zr containing aqueous solution was added to the above-mentioned aqueous solution of metal element M to produce a co-precipitate containing La, Zr, and Ta, thereby obtaining a slurry containing the co-precipitate. At this time, the La-Zr containing aqueous solution was continuously added to the aqueous solution of metal element M at a rate of 10 g / min so that the molar ratio of La, Zr, and Ta in the slurry was La:Zr:Ta = 3:1.5:0.5. At this time, the pH of the slurry was 10.5. Next, the slurry was filtered and washed filtration was performed until the pH of the filtrate was 9 or less, thereby recovering the co-precipitate. The recovered co-precipitate was dried at 100°C for 8 hours to obtain a powder of the co-precipitate. By heating the dried powder of the co-precipitate at 500°C for 6 hours under an atmospheric environment, a composite metal oxide powder containing La and Zr according to Example 1 was obtained. As a result of measuring the above composite metal oxide powder by XRD, no clear diffraction peaks were observed in the XRD spectrum, and a halo was observed in the region of 2θ: 10° to 60°, so it was found that the above composite metal oxide powder is an amorphous powder.
[0135] The XRD spectrum of the composite metal oxide powder obtained in Example 1 is shown in Figure 2.
[0136] In addition, the carbon content of the above composite metal oxide powder was 0.7 mass%.
[0137] Table 1 shows the manufacturing conditions for obtaining the amorphous composite metal oxide powder containing La and Zr of the present example. In addition, Table 2 shows the results of performing elemental analysis, measurement of carbon content, measurement of nitrogen content, measurement of BET specific surface area, and XRD measurement on the amorphous composite metal oxide powder containing La and Zr.
[0138] 2.5 g of the amorphous composite metal oxide powder containing La and Zr obtained in Example 1 above and 0.393 g of lithium oxide (manufactured by High Purity Chemical Research Institute) were mixed with φ5 mm zirconia balls using a planetary ball mill (P-7 manufactured by Fritchu) at 350 rpm for 4 hours to obtain a mixture containing La, Zr, Ta, and Li. At this time, the molar ratio of Li, La, Zr, and Ta in the mixture was Li:La:Zr:Ta = 7:3:1.5:0.5. A portion of the obtained mixture was extracted and calcined at a temperature of 400°C for 12 hours in a nitrogen atmosphere to obtain the lithium-containing composite metal oxide powder according to Example 1-1. XRD measurements were performed on the composite metal oxide powder, and clear diffraction peaks were observed in the XRD spectrum. When compared with the database embedded in the electronic calculator attached to the XRD device, the diffraction peaks matched those of a garnet-type oxide (garnet-type structure of space group Ia-3d), and it was confirmed that the lithium-containing composite metal oxide powder according to Example 1-1 is a garnet-type lithium composite metal oxide. In addition, it was confirmed that the garnet-type lithium composite metal oxide is single-phase.
[0139] Next, a lithium-containing composite metal oxide powder according to Example 1-2 was obtained in the same order as Example 1-1, except that the calcination temperature was 600℃, but the composite metal oxide powder was also a single-phase garnet-type lithium composite metal oxide.
[0140] Elemental analysis, XRD measurement, and ionic conductivity measurement were performed on the garnet-type lithium composite metal oxide powders obtained in Examples 1-1 and 1-2. The measurement results are shown in Table 3. The ionic conductivity of the compacts of the garnet-type lithium composite metal oxide powder according to Examples 1-1 and 1-2 was 2.3 × 10⁻⁶, respectively. -5 S / cm and 3.4×10 -5 It was S / cm.
[0141] [Example 2]
[0142] A slurry containing a co-precipitate of La, Zr, and Ta according to Example 2 was obtained by following the same procedure as in Example 1, except that 2.25 g of TaCl5 (manufactured by Fujifilm Wako Pure Chemical) was mixed with 100 g of pure water and 11.8 g of zirconium oxynitrate dihydrate (manufactured by Kishida Chemical) was added. The molar ratio of La, Zr, and Ta content in the obtained mixed slurry was La:Zr:Ta = 3:1.75:0.25, and the pH of the slurry was 10.7. Additionally, a composite metal oxide powder containing La and Zr according to Example 2 was obtained by following the same procedure as in Example 1. As a result of XRD measurement, it was confirmed that the composite metal oxide powder was amorphous. Furthermore, the carbon content of the composite metal oxide powder was 0.8 mass%.
[0143] The manufacturing conditions of Example 2 are shown in Table 1, and the results of elemental analysis, measurement of carbon content, measurement of nitrogen content, measurement of BET specific surface area, and XRD measurement for the amorphous composite metal oxide powder containing La and Zr obtained by Example 2 are shown together in Table 2.
[0144] Lithium-containing composite metal oxide powders according to Examples 2-1 and 2-2 were obtained in the same order as Examples 1-1 and 1-2, except that the amorphous composite metal oxide powder containing La and Zr obtained in Example 2 was used; however, XRD measurements confirmed that they were all single-phase garnet-type lithium composite metal oxides. The results of elemental analysis, XRD measurements, and ionic conductivity measurements performed on the garnet-type lithium composite metal oxide powders obtained by Examples 2-1 and 2-2 are shown together in Table 3. The ionic conductivity of the compacts of the garnet-type lithium composite metal oxide powders according to Examples 2-1 and 2-2 was 1.7 × 10⁻⁶, respectively. -5 S / cm and 2.5×10 -5It was S / cm.
[0145] [Example 3]
[0146] A slurry containing a co-precipitate of La, Zr, and Ta according to Example 3 was obtained in the same order as in Example 1, except that 0.90 g of TaCl5 (manufactured by Fujifilm Wako Pure Chemical) was mixed with 100 g of pure water and 2.8 g of zirconium oxynitrate dihydrate (manufactured by Kishida Chemical) was added. The molar ratio of the content of La, Zr, and Ta in the obtained mixed slurry was La:Zr:Ta = 3:1.90:0.10, and the pH of the slurry was 10.7. Additionally, a composite metal oxide powder containing La and Zr according to Example 3 was obtained in the same order as in Example 1. As a result of XRD measurement, it was confirmed that the composite metal oxide powder was amorphous. Furthermore, the carbon content of the composite metal oxide powder was 0.7 mass%.
[0147] The manufacturing conditions of Example 3 are shown in Table 1, and the results of elemental analysis, measurement of carbon content, measurement of nitrogen content, measurement of BET specific surface area, and XRD measurement for the amorphous composite metal oxide powder containing La and Zr obtained in Example 3 are shown together in Table 2.
[0148] Lithium-containing composite metal oxide powders according to Examples 3-1 and 3-2 were obtained in the same order as Examples 1-1 and 1-2, except that the amorphous composite metal oxide powder containing La and Zr obtained in Example 3 was used; however, XRD measurements confirmed that they were all single-phase garnet-type lithium composite metal oxides. The results of elemental analysis, XRD measurements, and ionic conductivity measurements performed on the garnet-type lithium composite metal oxide powders obtained by Examples 3-1 and 3-2 are shown together in Table 3. The ionic conductivity of the garnet-type lithium composite metal oxide powders according to Examples 3-1 and 3-2 was 1.3 × 10⁻⁶, respectively. -5S / cm and 1.4×10 -5 It was S / cm.
[0149] [Example 4]
[0150] 2.26 g of Nb(OH)5 (manufactured by Taniobis), a metal compound of metal element M with an oxidation state of pentavalent and not containing hydrocarbon groups in its molecular structure, was mixed with 400 g of pure water and heated to 40°C to obtain a slurry containing a precipitate of Nb hydroxide. After heating, 40.0 g of ammonia solution with a concentration of 28 mass% and 30 g of hydrogen peroxide solution with a concentration of 35 mass% (manufactured by Fujifilm Wako Pure Chemical) were added to the solution and stirred until the precipitate dissolved to obtain an aqueous solution of metal element M according to Example 4. As a result of performing FT-IR measurements on the aqueous solution of metal element M, 820 cm⁻¹ -1 ±10cm -1 From the observation of an absorption peak attributed to the OO bond of the peroxo, it was confirmed that a peroxo complex of Nb was formed in the aqueous solution.
[0151] Next, a slurry containing a co-precipitate of La, Zr, and Nb according to Example 4 was obtained in the same order as in Example 1, except that the molar ratio of the content of La, Zr, and Nb in the slurry was set to La:Zr:Nb = 3:1.50:0.50. In this case, the pH of the slurry was 10.5. Additionally, a composite metal oxide powder containing La and Zr according to Example 4 was obtained in the same order as in Example 1. As a result of XRD measurement, it was confirmed that the composite metal oxide powder was amorphous. Furthermore, the carbon content of the composite metal oxide powder was 0.6 mass%.
[0152] The manufacturing conditions of Example 4 are shown in Table 1, and the results of elemental analysis, measurement of carbon content, measurement of nitrogen content, measurement of BET specific surface area, and XRD measurement for the amorphous composite metal oxide powder containing La and Zr obtained by Example 4 are shown together in Table 2.
[0153] Lithium-containing composite metal oxide powders according to Examples 4-1 and 4-2 were obtained in the same order as Examples 1-1 and 1-2, except that the amorphous composite metal oxide powder containing La and Zr obtained in Example 4 was used; however, XRD measurements confirmed that they were all single-phase garnet-type lithium composite metal oxides. The results of elemental analysis, XRD measurements, and ionic conductivity measurements performed on the garnet-type lithium composite metal oxide powders obtained by Examples 4-1 and 4-2 are shown together in Table 3. The compact ionic conductivity of the garnet-type lithium composite metal oxide powders according to Examples 4-1 and 4-2 was 2.2 × 10⁻⁶, respectively. -5 S / cm and 3.1×10 -5 It was S / cm.
[0154] In addition, the ion conductivity of the prepared compacts was measured in the same manner as the ion conductivity measurement above, except that the garnet-type lithium composite metal oxide powder according to Example 4-2 was hot-pressed after reaching 400°C (Example 4-2a), 500°C (Example 4-2b), and 600°C (Example 4-2c) to produce compacts. As a result, the ion conductivity of Example 4-2a was 4.0 × 10⁻⁶. -5 S / cm, Example 4-2b is 6.5×10 -5 S / cm, Example 4-2c is 1.8×10 -4 It was S / cm.
[0155] [Measurement of Charge / Discharge Characteristics of All-Solid State Batteries]
[0156] Li1Ni as a positive electrode active material 1 / 3 Co 1 / 3 Mn1 / 3 O2 (NCM manufactured by Toda Industrial Co., Ltd.) powder, Li4Ti5O as the cathode active material 12 (LTO manufactured by Ishihara Sangyo Co., Ltd.) powder and the garnet-type lithium composite metal oxide powder obtained by Example 4-2 were prepared, and each powder was dried in a vacuum at 200°C for 12 hours to remove moisture.
[0157] Next, a powder sample for a positive electrode composite electrode was prepared by mixing the positive active material powder dried at 200°C and the garnet-type lithium composite metal oxide powder of Example 4-2 in a mass ratio of 50:50 under a dry environment using an agate mortar. In addition, a powder sample for a negative electrode composite electrode was prepared by mixing the negative active material powder dried at 200°C and the garnet-type lithium composite metal oxide powder in a mass ratio of 50:50 under a dry environment using an agate mortar.
[0158] Next, a plate made of platinum and gold (Pt+Au) as a current collector, 18 mg of powder of the anode material obtained in the above sequence, 100 mg of powder of the garnet-type lithium composite metal oxide obtained in Example 4-2, 14 mg of powder of the cathode material obtained in the above sequence, and a plate of gold (Au) as a current collector were stacked in a φ10 mm container in the order described above, and sintered by applying pressure of 375 MPa under an atmospheric atmosphere and firing at 300°C for 2 hours to form a battery cell (all-solid-state battery) with the configuration shown in Fig. 4. The above battery cell has a structure in which a sintered pellet of three layers, comprising a positive composite electrode, a garnet-type lithium composite metal oxide, and a negative composite electrode, is fitted with a current collector (the positive side is a plate made of platinum and gold, and the negative side is a gold plate), and the portion of the positive composite electrode, the portion of the garnet-type lithium composite metal oxide, and the portion of the negative composite electrode constituting the three layers of the sintered pellet correspond to the positive layer, the solid electrolyte layer, and the negative layer of FIG. 4, respectively.
[0159] Using a charge / discharge measuring device (HOKUTO DENKO HJ1020mSD8), the charge / discharge characteristics of the battery cell fabricated in the above sequence were evaluated by repeating the charge / discharge 10 times at 60°C with a voltage range of 1.0 to 3.0 V and a constant current density of 0.021 mA / ㎠ (3 mA / g per unit mass of LTO).
[0160] From the fabricated battery cell, a flat charge / discharge region around 2V was observed, a good charge / discharge curve was obtained, and it was confirmed that charging and discharging are possible at 60℃.
[0161] Figure 3 shows an example of measuring charge / discharge characteristics.
[0162] [Example 5]
[0163] A slurry containing a co-precipitate of La, Zr, and Nb according to Example 5 was obtained in the same order as in Example 4, except that 1.13 g of Nb(OH)5 (manufactured by Taniobis) was mixed with 400 g of pure water and 11.8 g of zirconium oxynitrate dihydrate (manufactured by Kishida Chemical) was added. The molar ratio of La, Zr, and Nb in the obtained mixed slurry was La:Zr:Ta = 3:1.75:0.25, and the pH of the slurry was 10.8. Additionally, a composite metal oxide powder containing La and Zr according to Example 5 was obtained in the same order as in Example 1. As a result of XRD measurement, it was confirmed that the composite metal oxide powder was amorphous. Furthermore, the carbon content of the composite metal oxide powder was 0.7 mass%.
[0164] The manufacturing conditions of Example 5 are shown in Table 1, and the results of elemental analysis, measurement of carbon content, measurement of nitrogen content, measurement of BET specific surface area, and XRD measurement for the amorphous composite metal oxide powder containing La and Zr obtained by Example 5 are shown together in Table 2.
[0165] Lithium-containing composite metal oxide powders according to Examples 5-1 and 5-2 were obtained in the same order as Examples 1-1 and 1-2, except that the amorphous composite metal oxide powder containing La and Zr obtained in Example 5 was used; however, XRD measurements confirmed that they were all single-phase garnet-type lithium composite metal oxides. The results of elemental analysis, XRD measurements, and ionic conductivity measurements performed on the garnet-type lithium composite metal oxide powders obtained by Examples 5-1 and 5-2 are shown together in Table 3. The ionic conductivity of the compacts of the garnet-type lithium composite metal oxide powders according to Examples 5-1 and 5-2 was 1.7 × 10⁻⁶, respectively. -5 S / cm and 2.2×10 -5 It was S / cm.
[0166] [Example 6]
[0167] A slurry containing a co-precipitate of La, Zr, and Nb according to Example 6 was obtained in the same order as in Example 4, except that 0.45 g of Nb(OH)5 (manufactured by Taniobis) was mixed with 400 g of pure water and 12.8 g of zirconium oxynitrate dihydrate (manufactured by Kishida Chemical) was added. The molar ratio of La, Zr, and Nb in the obtained mixed slurry was La:Zr:Ta = 3:1.90:0.10, and the pH of the slurry was 10.8. Additionally, a composite metal oxide powder containing La and Zr according to Example 6 was obtained in the same order as in Example 1. As a result of XRD measurement, it was confirmed that the composite metal oxide powder was amorphous. Furthermore, the carbon content of the composite metal oxide powder was 0.6 mass%.
[0168] The manufacturing conditions of Example 6 are shown in Table 1, and the results of elemental analysis, measurement of carbon content, measurement of nitrogen content, measurement of BET specific surface area, and XRD measurement for the amorphous composite metal oxide powder containing La and Zr obtained by Example 6 are shown together in Table 2.
[0169] Lithium-containing composite metal oxide powders according to Examples 6-1 and 6-2 were obtained in the same order as Examples 1-1 and 1-2, except that the amorphous composite metal oxide powder containing La and Zr obtained in Example 6 was used; however, XRD measurements confirmed that they were all single-phase garnet-type lithium composite metal oxides. The results of elemental analysis, XRD measurements, and ionic conductivity measurements performed on the garnet-type lithium composite metal oxide powders obtained by Examples 5-1 and 5-2 are shown together in Table 3. The ionic conductivity of the compacts of the garnet-type lithium composite metal oxide powders according to Examples 6-1 and 6-2 was 1.1 × 10⁻⁶, respectively. -5 S / cm and 1.9×10 -5 It was S / cm.
[0170] [Example 7]
[0171] A composite metal oxide powder containing La and Zr according to Example 7 was obtained by following the same procedure as in Example 1, except that the dry co-precipitate containing La, Zr, and Nb obtained in Example 4 was not heated at 500°C for 6 hours under an atmospheric environment. As a result of XRD measurements, it was confirmed that the composite metal oxide powder was amorphous, even though it had not undergone heat treatment. The XRD spectrum of the composite metal oxide powder obtained in Example 7 is shown together in Figure 2. In addition, the carbon content of the composite metal oxide powder was 1.1 mass%.
[0172] The manufacturing conditions of Example 7 are shown in Table 1, and the results of elemental analysis, measurement of carbon content, measurement of nitrogen content, measurement of BET specific surface area, and XRD measurement for the amorphous composite metal oxide powder containing La and Zr obtained by Example 7 are shown together in Table 2.
[0173] A lithium-containing composite metal oxide powder according to Example 7-1 was obtained in the same procedure as in Example 1-1, except that the amorphous composite metal oxide powder containing La and Zr obtained in Example 7 was used; however, as a result of XRD measurement, it was confirmed that the lithium-containing composite metal oxide powder was a single-phase garnet-type lithium composite metal oxide. The results of elemental analysis, XRD measurement, and ionic conductivity measurement performed on the garnet-type lithium composite metal oxide powder obtained by Example 7-1 are shown together in Table 3. The ionic conductivity of the compact of the garnet-type lithium composite metal oxide powder according to Example 7-1 is 1.0 × 10⁻⁶. -5 It was S / cm.
[0174] [Example 8]
[0175] A composite metal oxide powder containing La and Zr according to Example 8 was obtained in the same order as in Example 4, except that the dry co-precipitate containing La, Zr, and Nb obtained in Example 4 was heated at 400°C for 6 hours under an atmospheric environment. As a result of XRD measurement, it was confirmed that the composite metal oxide powder was amorphous. In addition, the carbon content of the composite metal oxide powder was 1.1 mass%.
[0176] The manufacturing conditions of Example 8 are shown in Table 1, and the results of elemental analysis, measurement of carbon content, measurement of nitrogen content, measurement of BET specific surface area, and XRD measurement for the amorphous composite metal oxide powder containing La and Zr obtained by Example 7 are shown together in Table 2.
[0177] A lithium-containing composite metal oxide powder according to Example 8-1 was obtained in the same procedure as in Example 1-1, except that the amorphous composite metal oxide powder containing La and Zr obtained in Example 8 was used; however, as a result of XRD measurement, it was confirmed that the lithium-containing composite metal oxide powder was a single-phase garnet-type lithium composite metal oxide. The results of elemental analysis, XRD measurement, and ionic conductivity measurement performed on the garnet-type lithium composite metal oxide powder obtained by Example 8-1 are shown together in Table 3. The ionic conductivity of the compact of the garnet-type lithium composite metal oxide powder according to Example 8-1 is 2.5 × 10⁻⁶. -5 It was S / cm.
[0178] [Example 9]
[0179] A composite metal oxide powder containing La and Zr according to Example 9 was obtained in the same order as in Example 4, except that the dry co-precipitate containing La, Zr, and Nb obtained in Example 4 was heated at 300°C for 6 hours under an atmospheric environment. As a result of XRD measurements, it was confirmed that the composite metal oxide powder was amorphous. The XRD spectrum of the composite metal oxide powder obtained in Example 9 is shown together in Figure 2. In addition, the carbon content of the composite metal oxide powder was 1.1 mass%.
[0180] The manufacturing conditions of Example 9 are shown in Table 1, and the results of elemental analysis, measurement of carbon content, measurement of nitrogen content, measurement of BET specific surface area, and XRD measurement for the amorphous composite metal oxide powder containing La and Zr obtained by Example 9 are shown together in Table 2.
[0181] A lithium-containing composite metal oxide powder according to Example 9-1 was obtained in the same procedure as in Example 1-1, except that the amorphous composite metal oxide powder containing La and Zr obtained in Example 9 was used; however, as a result of XRD measurement, it was confirmed that the lithium-containing composite metal oxide powder was a single-phase garnet-type lithium composite metal oxide. The results of elemental analysis, XRD measurement, and ionic conductivity measurement performed on the garnet-type lithium composite metal oxide powder obtained by Example 9-1 are shown together in Table 3. The ionic conductivity of the compact of the garnet-type lithium composite metal oxide powder according to Example 9-1 is 2.1 × 10⁻⁶. -5 It was S / cm.
[0182] [Example 10]
[0183] A composite metal oxide powder containing La and Zr according to Example 10 was obtained in the same order as in Example 4, except that the dry co-precipitate containing La, Zr, and Nb obtained in Example 4 was heated at 200°C for 6 hours under an atmospheric environment. As a result of XRD measurements, it was confirmed that the composite metal oxide powder was amorphous. The XRD spectrum of the composite metal oxide powder obtained in Example 10 is shown together in Figure 2. In addition, the carbon content of the composite metal oxide powder was 1.3 mass%.
[0184] The manufacturing conditions of Example 10 are shown in Table 1, and the results of elemental analysis, carbon content measurement, nitrogen content measurement, BET specific surface area measurement, and XRD measurement performed on the amorphous composite metal oxide powder containing La and Zr obtained in Example 10 are shown together in Table 2.
[0185] A lithium-containing composite metal oxide powder according to Example 10-1 was obtained in the same procedure as in Example 1-1, except that the amorphous composite metal oxide powder containing La and Zr obtained in Example 10 was used; however, as a result of XRD measurement, it was confirmed that the lithium-containing composite metal oxide powder was a single-phase garnet-type lithium composite metal oxide. The results of elemental analysis, XRD measurement, and ionic conductivity measurement performed on the garnet-type lithium composite metal oxide powder obtained by Example 10-1 are shown together in Table 3. The ionic conductivity of the compact of the garnet-type lithium composite metal oxide powder according to Example 10-1 is 1.3 × 10⁻⁶. -5 It was S / cm.
[0186] [Example 11]
[0187] 780 g of pure water, 169.6 g of hydrated niobium oxide (Nb2O5·nH2O, Nb concentration: 76.4 mass%), and 87.76 g of 48 mass% NaOH aqueous solution were mechanically stirred at 70°C for 7 hours to solubilize the hydrated niobium oxide and obtain a clear aqueous solution. 31.8 g of 35 mass% hydrogen peroxide aqueous solution was added to this solution, and the solution was washed with water by ultrafiltration to remove impurities such as Na ions, thereby obtaining an aqueous solution of metal element M. A small sample of the obtained aqueous solution of metal element M was taken, and FT-IR measurements were performed in the same manner as in Example 1, with a wavenumber of 850 cm⁻¹. -1 ±10cm -1 An absorption peak attributed to the Nb-O bond is observed in the vicinity at 680 cm⁻¹. -1 ±20cm -1 From the observation of an absorption peak attributable to an Nb-O-Nb bond in the vicinity, it was confirmed that polyacid ions of Nb were generated in the aqueous solution of the metal element M. Figure 1 shows the FT-IR spectrum of an aqueous solution containing Nb as the metal element M obtained in this example.
[0188] Next, a slurry containing a co-precipitate of La, Zr, and Nb according to Example 7 was obtained in the same order as in Example 1, except that the molar ratio of the content of La, Zr, and Nb in the slurry was set to La:Zr:Nb = 3:1.50:0.50. In this case, the pH of the slurry was 10.5. Additionally, a composite metal oxide powder containing La and Zr according to Example 11 was obtained in the same order as in Example 1. As a result of XRD measurement, it was confirmed that the composite metal oxide powder was amorphous. Furthermore, the carbon content of the composite metal oxide powder was 1.3 mass%.
[0189] The manufacturing conditions of Example 11 are shown in Table 1, and the results of elemental analysis, measurement of carbon content, measurement of nitrogen content, measurement of BET specific surface area, and XRD measurement for the amorphous composite metal oxide powder containing La and Zr obtained by Example 11 are shown together in Table 2.
[0190] A lithium-containing composite metal oxide powder according to Example 11-1 was obtained in the same procedure as in Example 1-1, except that the amorphous composite metal oxide powder containing La and Zr obtained in Example 11 was used; however, as a result of XRD measurement, it was confirmed that the lithium-containing composite metal oxide powder was a single-phase garnet-type lithium composite metal oxide. The results of elemental analysis, XRD measurement, and ionic conductivity measurement performed on the garnet-type lithium composite metal oxide powder obtained by Example 11-1 are shown together in Table 3. The ionic conductivity of the compact of the garnet-type lithium composite metal oxide powder according to Example 11-1 is 2.0 × 10⁻⁶. -5 It was S / cm.
[0191] [Comparative Example 1]
[0192] 50.0 g of ammonium bicarbonate was dissolved in 200 g of water, and 50.32 g of an aqueous solution of niobium ammonium oxalate was added to the aqueous solution (Nb concentration 5 mass%). Then, while maintaining the temperature of the aqueous solution at 40°C, 84.19 g of an aqueous solution of lanthanum nitrate (La concentration 16 mass%) was added dropwise at a rate of 8.5 g / min to obtain a co-precipitate A of Nb and La. Then, while maintaining the temperature at 40°C, 44.69 g of an aqueous solution of ammonium zirconium carbonate (Zr concentration 10 mass%) was added dropwise to the obtained co-precipitate A at a rate of 0.5 g / min to obtain a slurry containing co-precipitate B.
[0193] In addition, the molar ratio of the content of La, Zr, and Nb in the obtained slurry is La:Zr:Nb = 3:1.50:0.50.
[0194] Next, the pH was adjusted using ammonia water to be within the range of 9 to 11, and then heated at 90°C for 180 minutes. The slurry containing the obtained co-precipitate B was subjected to suction filtration, the filtrate was washed with pure water, and moisture was removed to separate the co-precipitate B from the slurry. The obtained co-precipitate B was calcined at 750°C for 5 hours to obtain a composite metal oxide powder containing La and Zr according to Comparative Example 1. XRD measurements were performed on the composite metal oxide powder, and it was a crystalline powder without a halo pattern in which a ZrO2 peak and a peak of unknown attribution were observed in the 2θ: 10° to 60° region. In addition, the carbon content of the composite metal oxide powder was 2.5 mass%.
[0195] The manufacturing conditions of Comparative Example 1 are shown in Table 1, and the results of elemental analysis, measurement of carbon content, measurement of nitrogen content, measurement of BET specific surface area, and XRD measurement for the crystalline composite metal oxide powder obtained in Comparative Example 1 are shown together in Table 2.
[0196] Next, lithium-containing composite metal oxide powders of Comparative Examples 1-1 and 1-2 were obtained in the same order as in Examples 1-1 and 1-2, except that the crystalline composite metal oxide powder obtained in Comparative Example 1 was used. XRD measurements were performed on the lithium-containing composite metal oxide powders obtained in Comparative Examples 1-1 and 1-2, and it was found that all of the lithium-containing composite metal oxide powders were compound garnet-type lithium composite metal oxides in which a ZrO2 peak was observed in addition to a garnet-type crystal structure. The results of elemental analysis, XRD measurements, and ionic conductivity measurements performed on the garnet-type lithium composite metal oxide powders obtained by Comparative Examples 1-1 and 1-2 are shown together in Table 3. The ionic conductivity of the compacts of the garnet-type lithium composite metal oxide powders according to Comparative Examples 1-1 and 1-2 was 4.4 × 10⁻⁶, respectively. -8 S / cm and 4.4×10 -8 It was S / cm.
[0197] From the results of the comparative example, it can be seen that a single-phase garnet-type lithium composite metal oxide cannot be obtained when a crystalline composite metal oxide powder containing La and Zr is used as a precursor. Furthermore, it can be seen that if the carbon content of the composite metal oxide powder containing La and Zr is high, the ionic conductivity of the compact of the finally obtained garnet-type lithium composite metal oxide powder decreases.
[0198] [Comparative Example 2]
[0199] A composite metal oxide powder containing La and Zr according to Comparative Example 2 was obtained in the same order as in Example 1, except that the dried co-precipitate containing La, Zr, and Ta obtained in Example 1 was heated at 800°C for 6 hours under an atmospheric environment. XRD measurements were performed on the composite metal oxide powder obtained in Comparative Example 2, and the composite metal oxide powder was a crystalline powder in which a peak of a fluorite-type crystal structure was observed in the region of 2θ: 10° to 60°. In addition, the carbon content of the composite metal oxide powder was 0.3 mass%.
[0200] The XRD spectrum of the composite metal oxide powder obtained in Comparative Example 2 is shown together in Figure 2. The manufacturing conditions of Comparative Example 2 are shown in Table 1, and the results of elemental analysis, measurement of carbon content, measurement of nitrogen content, measurement of BET specific surface area, and XRD measurement performed on the crystalline composite metal oxide powder obtained in Comparative Example 2 are shown together in Table 2.
[0201] Next, lithium-containing composite metal oxide powders of Comparative Examples 2-1 and 2-2 were obtained in the same order as in Examples 1-1 and 1-2, except that the crystalline composite metal oxide powder obtained in Comparative Example 2 was used. XRD measurements were performed on the lithium-containing composite metal oxide powders obtained in Comparative Examples 2-1 and 2-2, and it was found that all of the lithium-containing composite metal oxide powders were compound garnet-type lithium composite metal oxides in which a La2Zr2O7 peak was observed in addition to a garnet-type crystal structure. The results of elemental analysis, XRD measurements, and ionic conductivity measurements performed on the garnet-type lithium composite metal oxide powders obtained in Comparative Examples 2-1 and 2-2 are shown together in Table 3. The ionic conductivity of the compacts of the garnet-type lithium composite metal oxide powders according to Comparative Examples 2-1 and 2-2 was 4.4 × 10⁻⁶, respectively. -8 S / cm and 4.4×10 -8It was S / cm.
[0202] From the results of the present comparative example, it can be seen that a single-phase garnet-type lithium composite metal oxide cannot be obtained when a composite metal oxide powder containing crystalline La and Zr is used as a precursor. Furthermore, in the case of the present comparative example, it was found that the ionic conductivity of the compact of the finally obtained garnet-type lithium composite metal oxide powder is low, even though the carbon content of the composite metal oxide powder containing La and Zr is low.
[0203] [Comparative Example 3]
[0204] La(NO3)3·6H2O (manufactured by Fujifilm Wako Pure Chemical), ZrOCl2·8H2O (manufactured by Fujifilm Wako Pure Chemical), and TaCl5 (manufactured by Fujifilm Wako Pure Chemical) were weighed so that the molar ratio of the content of La, Zr, and Ta was La:Zr:Ta = 3:1.5:0.5, and dissolved in ethanol, which is a solvent.
[0205] Citric acid (manufactured by Fujifilm Wako Pure Chemicals) as a chelating agent and ethylene glycol (manufactured by Fujifilm Wako Pure Chemicals) as a chelating polymerizing agent were added to the solvent in which La, Zr, and Ta were dissolved, and a gel was obtained by heating at 140°C for 5 hours using a hot plate and esterifying the chelating compound with ethylene glycol. The obtained gel was calcined at 350°C using a mantle heater to obtain a composite metal oxide powder containing La and Zr according to Comparative Example 3. In addition, the manufacturing conditions of this Comparative Example are based on the manufacturing method of the Example described in Patent Document 2.
[0206] XRD measurements were performed on the powder obtained in Comparative Example 3. Since no clear diffraction peaks were observed in the XRD spectrum and a halo was observed in the region of 2θ: 10° to 60°, it was determined that the composite metal oxide powder was an amorphous powder. In addition, the carbon content of the composite metal oxide powder was 2.8 mass%.
[0207] The manufacturing conditions of Comparative Example 3 are shown in Table 1, and the results of elemental analysis, measurement of carbon content, measurement of nitrogen content, measurement of BET specific surface area, and XRD measurement for the crystalline composite metal oxide powder obtained in Comparative Example 3 are shown together in Table 2.
[0208] Next, lithium-containing composite metal oxide powders of Comparative Examples 3-1 and 3-2 were obtained in the same order as in Examples 1-1 and 1-2, except that the crystalline composite metal oxide powder obtained in Comparative Example 3 was used. XRD measurements were performed on the lithium-containing composite metal oxide powders obtained in Comparative Examples 3-1 and 3-2, and it was confirmed that all of the lithium-containing composite metal oxide powders were single-phase garnet-type lithium composite metal oxides. The results of elemental analysis, XRD measurements, and ionic conductivity measurements performed on the garnet-type lithium composite metal oxide powders obtained in Comparative Examples 3-1 and 3-2 are shown together in Table 3. The ionic conductivity of the compacts of the garnet-type lithium composite metal oxide powders according to Comparative Examples 3-1 and 3-2 was 5.0 × 10⁻⁶, respectively. -6 S / cm and 1.8×10 -6 It was S / cm.
[0209] From the results of this comparative example, it can be seen that when the manufacturing method described in Patent Document 2 is used, the La and Zr-containing composite metal oxide powder obtained is amorphous but has a high carbon content. Furthermore, it can be seen that when the amorphous composite metal oxide powder containing La and Zr with high carbon content is used as a precursor, a single-phase garnet-type lithium composite metal oxide can be obtained, but the ionic conductivity of the compact of the finally obtained garnet-type lithium composite metal oxide powder is reduced.
[0210] From the above results, it was found that a single-phase garnet-type lithium composite metal oxide with high ion conductivity can be obtained by using an amorphous composite metal oxide powder as a precursor, which contains La in an amount of 40 mass% or more and 62 mass% or less, Zr in an amount of 8 mass% or more and 26 mass% or less, a metal element M capable of taking an oxidation state of 3 to 6, in an amount of 1 mass% or more and 20 mass% or less, a carbon content of 1.5 mass% or less, and the remainder being oxygen and unavoidable impurities such as La and Zr, and mixing and calcining it with a Li compound.
[0211] If a crystalline complex metal oxide powder containing La and Zr is used as a precursor, the final garnet-type lithium complex metal oxide powder becomes polymorphic, resulting in a decrease in ionic conductivity. Furthermore, even if an amorphous complex metal oxide powder containing La and Zr is used as a precursor, if one with a high carbon content is used, the carbon content of the final garnet-type lithium complex metal oxide powder increases, leading to a decrease in ionic conductivity.
[0212]
[0213]
[0214]
Claims
Claim 1 An amorphous composite metal oxide powder containing La and Zr, wherein La is 40 mass% or more and 62 mass% or less, Zr is 8 mass% or more and 26 mass% or less, and a metal element M excluding La and Zr is 1 mass% or more and 20 mass% or less, the carbon content is 1.5 mass% or less, and the remainder is oxygen and unavoidable impurities. Claim 2 An amorphous composite metal oxide powder containing La and Zr, wherein the molar ratio of the content ratio of La, Zr, and metal element M in the amorphous composite metal oxide powder is La:Zr:M = 3:1.2 to 1.95:0.05 to 0.
8. Claim 3 In claim 1, an amorphous composite metal oxide powder comprising La and Zr, wherein the oxidation number that the metal element M can take is 5. Claim 4 The amorphous composite metal oxide powder comprising La and Zr, wherein the metal element M is one or more of Ta, Nb, V, and Sb in claim 1. Claim 5 An amorphous composite metal oxide powder comprising La and Zr, wherein, in any one of claims 1 to 4, the nitrogen content as an unavoidable impurity is 3 mass% or less. Claim 6 A method for manufacturing an amorphous composite metal oxide powder containing La and Zr as described in claim 1, comprising: a process of obtaining a slurry containing a co-precipitate containing La, Zr, and a metal element M excluding La and Zr, wherein M is a metal element capable of taking an oxidation state of any one of 3 to 6; a process of recovering the co-precipitate containing La, Zr and the metal element M by solid-liquid separation from the slurry containing the co-precipitate containing La, Zr and the metal element M; and a process of heat-treating the recovered co-precipitate containing La, Zr and the metal element M at a temperature below 800°C. Claim 7 A method for producing an amorphous composite metal oxide powder containing La and Zr, wherein, in claim 6, the process of obtaining a slurry containing a co-precipitate containing La, Zr and a metal element M involves simultaneously dissolving an inorganic La compound, an inorganic Zr compound, and an inorganic metal element M compound in water. Claim 8 A method for manufacturing an amorphous composite metal oxide powder containing La and Zr, wherein, in claim 6, the process of obtaining a slurry containing a co-precipitate containing La, Zr and a metal element M comprises: a process of preparing an aqueous solution containing La-Zr by dissolving an inorganic La compound and an inorganic Zr compound in water; a process of preparing an aqueous solution containing a metal element M by dissolving an inorganic metal element M compound in water; and a process of mixing the aqueous solution containing La-Zr and the aqueous solution containing the metal element M. Claim 9 A method for manufacturing an amorphous composite metal oxide powder containing La and Zr, wherein, in claim 6, the heat treatment temperature in the heat treatment process is 700℃ or lower. Claim 10 A method for manufacturing an amorphous composite metal oxide powder containing La and Zr, wherein, in claim 6, the heat treatment temperature in the heat treatment process is 150°C or higher. Claim 11 A method for preparing an amorphous composite metal oxide powder containing La and Zr, wherein, in claim 7, the inorganic La compound, the inorganic Zr compound, and the inorganic metal element M compound each do not contain carbon in their molecular structures. Claim 12 A method for preparing an amorphous composite metal oxide powder containing La and Zr, wherein, in claim 8, the inorganic La compound, the inorganic Zr compound, and the inorganic metal element M compound each do not contain carbon in their molecular structures. Claim 13 A method for preparing an amorphous composite metal oxide powder containing La and Zr according to claim 8, wherein the aqueous solution containing the metal element M comprises a compound of the inorganic metal element M, water of ammonia, and a peroxo complex of the metal element M produced by mixing hydrogen peroxide and water. Claim 14 A method for manufacturing an amorphous composite metal oxide powder comprising La and Zr, wherein the metal element M is one or more of Ta, Nb, V, and Sb, in accordance with claim 6. Claim 15 A method for producing an amorphous composite metal oxide powder containing La and Zr according to claim 6, wherein the molar ratio of the content of La, Zr, and metal element M in a slurry containing a co-precipitate containing La, Zr, and metal element M is La:Zr:M = 3:1.2 to 1.95:0.05 to 0.
8. Claim 16 A method for producing an amorphous composite metal oxide powder containing La and Zr, wherein, in any one of claims 6 to 15, the co-precipitate containing La, Zr and metal element M is washed when separating the solid and liquid of a slurry containing the co-precipitate containing La, Zr and metal element M. Claim 17 A method for manufacturing a garnet-type lithium composite metal oxide by calcining a mixture of an amorphous composite metal oxide powder containing La and Zr as described in claim 1 and a Li compound. Claim 18 A method for manufacturing a garnet-type lithium composite metal oxide according to claim 17, wherein the temperature at which a mixture of the amorphous composite metal oxide powder containing La and Zr and a Li compound is calcined is 300°C or higher and less than 700°C. Claim 19 A method for manufacturing a garnet-type lithium composite metal oxide according to claim 17, wherein when mixing the amorphous composite metal oxide powder containing La and Zr with a Li compound, the molar ratio of Li, La, Zr and metal element M is Li:La:Zr:M = 6.5 to 7.5:3:1.2 to 1.95:0.05 to 0.
8. Claim 20 A method for manufacturing an all-solid-state battery having a battery unit having a structure in which a solid electrolyte layer is disposed between a positive electrode layer containing a positive electrode active material and a negative electrode layer containing a negative electrode active material, wherein at least one of the positive electrode layer, the negative electrode layer, and the solid electrolyte layer comprises a garnet-type lithium composite metal oxide manufactured by a manufacturing method described in any one of claims 17 to 19.