Anchor coating materials and laminates

The anchor coating material with a polyurethane dispersion improves the flexibility and gas barrier properties of paper laminates by using a specific composition of isocyanate-terminated prepolymer and macropolyols, ensuring high adhesion and gas barrier performance after folding.

KR1020260161625APending Publication Date: 2026-11-09MITSUI CHEMICALS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
KR1020267033762
Authority / Receiving Office
KR · KR
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-05-01
Filing Date
2025-04-23
Publication Date
2026-11-09

AI Technical Summary

Technical Problem

Existing paper laminates using a resin film substrate with a polyurethan-based resin undercoat layer suffer from reduced flexibility and gas barrier properties after folding.

Method used

An anchor coating material comprising a polyurethane dispersion with specific compositions of isocyanate-terminated prepolymer, chain extender, and active hydrogen group-containing components, including xylylene diisocyanate and macropolyols, to form a flexible anchor coat layer that enhances adhesion with an inorganic deposition layer.

Benefits of technology

The laminate achieves excellent gas barrier properties after folding, maintaining high flexibility and adhesion, suitable for paper substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCT00005_ABST
    Figure PCT00005_ABST
Patent Text Reader

Abstract

The anchor coating material comprises a polyurethan dispersion. The polyurethan dispersion comprises a polyurethan resin. The polyurethan resin is a reaction product of an isocyanate-terminated prepolymer and a chain extender. The isocyanate-terminated prepolymer comprises a reaction product of an isocyanate component and an active hydrogen group-containing component. The active hydrogen group-containing component comprises a short-chain diol having 2 to 6 carbon atoms, a macropolyol with a number average molecular weight of 300 to 3000, and an active hydrogen compound containing a hydrophilic group. The total concentration of urethan groups and urea groups in the polyurethan resin is 26 mass% to 37 mass%.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to an anchor coating material and a laminate. Background Technology

[0002] Conventionally, the deposition of metal on paper and anchor coating materials for the same are known. In addition, a paper laminate is proposed in which an inorganic material (including metal) is deposited on paper, and in order to increase recyclability and gas barrier properties, a clay coat layer, an undercoat layer, and a deposition layer are laminated on at least one side of a paper substrate, wherein the deposition layer comprises at least one material selected from the group consisting of metals and ceramics (e.g., Patent Document 1, etc.). Prior art literature

[0003] Japanese Patent Publication No. 2022-169426 The problem to be solved

[0004] However, the paper laminate described in Patent Document 1 uses paper rather than a resin film as a substrate in order to increase recyclability, and uses a polyurethan-based resin with high gas barrier properties as the resin forming the undercoat layer in order to increase gas barrier properties, so there is a problem that the flexibility of the resin is reduced and the gas barrier properties after folding are reduced.

[0005] The present invention provides a laminate with excellent gas barrier properties after folding and an anchor coating material applicable to the manufacture of the laminate. means of solving the problem

[0006] The present invention [1] is an anchor coating material comprising a polyuretane dispersion, wherein the polyuretane dispersion contains a polyuretane resin, wherein the polyuretane resin is a reaction product of an isocyanate group-terminated prepolymer and a chain extender, wherein the isocyanate group-terminated prepolymer comprises a reaction product of an isocyanate component and an active hydrogen group-containing component, wherein the active hydrogen group-containing component comprises a short-chain diol having 2 to 6 carbon atoms, a macropolyol having a number average molecular weight of 300 to 3000, and a hydrophilic group-containing active hydrogen compound, and wherein the total concentration of uretane groups and urea groups in the polyuretane resin is 26 mass% or more and 37 mass% or less.

[0007] The present invention [2] is an anchor coating material described in [1], wherein the chain extension agent comprises 50 mol% or more of a polyamine compound that does not contain hydroxyl groups.

[0008] The present invention [3] is an anchor coating material described in [1] or [2], wherein the isocyanate component contains 50 mol% or more of xylylene diisocyanate.

[0009] The present invention [4] is an anchor coating material described in any one of [1] to [3], wherein the concentration of the polyol with three or more functions among the active hydrogen group-containing components is 0.04 mol% or less.

[0010] The present invention [5] is an anchor coating material described in any one of [1] to [4], wherein the mass ratio of the macropolyol to the short-chain diol is 1.0 or more and 3.0 or less.

[0011] The present invention [6] comprises paper, a snow filling layer, an anchor coat layer, and an inorganic deposition layer in the thickness direction, wherein the anchor coat layer comprises a dried anchor coating material described in any one of [1] to [5].

[0012] The present invention [7] is a laminate described in [6], wherein the eye-filling layer does not contain an inorganic filler. Effects of the invention

[0013] According to the present invention, a laminate with excellent gas barrier properties after folding and an anchor coating material applicable to the manufacture of the laminate can be provided. Brief explanation of the drawing

[0014] FIG. 1 is a schematic cross-sectional view showing one embodiment of the laminate of the present invention. Specific details for implementing the invention

[0015] Anchor Coating Material

[0016] An anchor coating material is a coating material applied to a substrate before the formation of an inorganic deposition layer to enhance adhesion between the substrate and the inorganic deposition layer when manufacturing a laminate in which an inorganic deposition layer is formed on a substrate. The anchor coating material of the present invention comprises a polyuretain dispersion. Therefore, when the anchor coating material of the present invention is applied to a substrate and dried, a highly flexible anchor coating layer is formed, and an inorganic deposition layer with high gas barrier properties can be formed in close contact thereon. The anchor coating material of the present invention has high flexibility, allowing for the formation of an anchor coating layer with high adhesion and followability with respect to the substrate and the inorganic deposition layer. Therefore, it can be applied to the manufacture of a laminate with excellent gas barrier properties after folding.

[0017] The anchor coating material of the present invention is preferably an anchor coating material for paper, wherein the substrate is paper. Because the anchor coating material of the present invention has high flexibility, even when used on paper as a substrate, the adhesion and following properties between the paper and the inorganic deposition layer are high.

[0018] Here, paper is formed into a sheet by interlacing fibrous chemical substances (e.g., organic fibers, inorganic fibers). Specifically, paper is obtained, for example, by forming pulp. Examples of pulp include natural pulp and synthetic pulp. More specifically, examples include glassine paper, coated paper, single-sided glossy (bleached) kraft paper, roll paper, and cup paper. Paper may be single-layer paper or multi-layer paper. Paper is appropriately selected according to the application of the laminate.

[0019] [Polyuretain Dispersion]

[0020] Polyurethan dispersion is a water dispersion of polyurethan resin.

[0021] [Polyuretaine]

[0022] Polyuretane resin comprises a reaction product of an isocyanate-terminated prepolymer and a chain extender. Preferably, polyuretane resin consists of a reaction product of an isocyanate-terminated prepolymer and a chain extender. More specifically, polyuretane resin is obtained by the reaction of an isocyanate-terminated prepolymer and a chain extender.

[0023] (Isocyanate-terminated prepolymer)

[0024] The isocyanate-terminated prepolymer comprises a reaction product of an isocyanate component and an active hydrogen group-containing component. The isocyanate-terminated prepolymer is preferably composed of a reaction product of an isocyanate component and an active hydrogen group-containing component. More specifically, the isocyanate-terminated prepolymer is obtained by the reaction of an isocyanate component and an active hydrogen group-containing component.

[0025] That is, the isocyanate-terminated prepolymer is a primary reaction product of the isocyanate component and the active hydrogen group-containing component. In addition, the polyuretaine resin is a secondary reaction product of the isocyanate-terminated prepolymer and the chain extender.

[0026] (Isocyanate component)

[0027] The isocyanate component is not particularly limited, but in order to maintain high gas barrier properties after folding of the laminate, preferably comprises xylylene diisocyanate (XDI) (alias: bis(isocyanatomethyl)benzene), more preferably comprises at least 50 mol% of xylylene diisocyanate, even more preferably comprises at least 85 mol% of xylylene diisocyanate, and most preferably comprises 100 mol% of xylylene diisocyanate.

[0028] Examples of xylylene diisocyanates include xylylene diisocyanate monomers (XDI monomers) and xylylene diisocyanate derivatives (XDI derivatives).

[0029] Examples of xylylene diisocyanate monomers include 1,2-xylylene diisocyanate (alias: 1,2-bis(isocyanatomethyl)benzene), 1,3-xylylene diisocyanate (alias: 1,3-bis(isocyanatomethyl)benzene), and 1,4-xylylene diisocyanate (alias: 1,4-bis(isocyanatomethyl)benzene). These xylylene diisocyanate monomers may be used alone or in combination of two or more types. Examples of xylylene diisocyanate monomers include, preferably, 1,3-xylylene diisocyanate and 1,4-xylylene diisocyanate, and more preferably, 1,3-xylylene diisocyanate.

[0030] Additionally, the polyisocyanate component may include other polyisocyanates. The other polyisocyanates are polyisocyanates excluding xylylene diisocyanate.

[0031] Other polyisocyanates include industrially used polyisocyanates. More specifically, examples include aromatic polyisocyanates, aromatic aliphatic polyisocyanates (excluding xylylene diisocyanates), aliphatic polyisocyanates, and alicyclic polyisocyanates. In addition, other polyisocyanates include derivatives of the same type as those mentioned above. Other polyisocyanates may be used alone or in combination of two or more types.

[0032] As other polyisocyanates, alicyclic polyisocyanates are preferably cited from the perspective of maintaining high gas barrier properties after folding of the laminate. Examples of alicyclic polyisocyanates include bis(isocyanatomethyl)cyclohexane (H6XDI) and methylenebis(cyclohexyl isocyanate) (H 12 Examples include MDI), and isophorone diisocyanate (IPDI). As for alicyclic polyisocyanates, preferably, methylenebis(cyclohexyl isocyanate) may be used. These alicyclic polyisocyanates may be used alone or in combination of two or more types.

[0033] For example, when xylylene diisocyanate and alicyclic polyisocyanate are used in combination, with respect to their total moles, xylylene diisocyanate is preferably 50 mole% or more, more preferably 85 mole% or more. Also, with respect to their total moles, the alicyclic polyisocyanate is preferably 50 mole% or less, more preferably 15 mole% or less.

[0034] (Ingredients containing active hydrogen)

[0035] The active hydrogen group-containing component is a component containing an active hydrogen group that reacts with the isocyanate group in the isocyanate component, and includes a short-chain diol having 2 or more carbon atoms and 6 or fewer carbon atoms, a macropolyol having a number average molecular weight of 300 or more and 3000 or fewer, and an active hydrogen compound containing a hydrophilic group.

[0036] (short-chain diol)

[0037] Short-chain diols are diols having 2 to 6 carbon atoms. Such short-chain diols increase the gas barrier properties of the polyurethan resin contained in the anchor coating material, thereby increasing the gas barrier properties of the anchor coating layer. Examples of short-chain diols include alkane diols having 2 to 6 carbon atoms, ether diols having 2 to 6 carbon atoms, and alkene diols having 2 to 6 carbon atoms.

[0038] Examples of alkanediols having 2 to 6 carbon atoms include ethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butylene glycol, 1,3-butylene glycol, 1,2-butylene glycol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, 1,3-cyclohexanediol, and 1,4-cyclohexanediol. Examples of etherdiols having 2 to 6 carbon atoms include diethylene glycol, triethylene glycol, and dipropylene glycol. Examples of alkenediols having 2 to 6 carbon atoms include 1,4-dihydroxy-2-butene. These short-chain diols can be used alone or in combination of two or more types. As for the short-chain diol, from the perspective of high gas barrier properties, preferably, an alkane diol having 2 to 6 carbon atoms can be cited, and more preferably, ethylene glycol can be cited.

[0039] (Macropolyol)

[0040] Macropolyols are high molecular weight polyols having two or more hydroxyl groups and a number average molecular weight of 300 or more and 3000 or less. Such macropolyols increase the flexibility of the polyuretane resin included in the anchor coating material, thereby increasing the flexibility of the anchor coat layer. The number average molecular weight of the macropolyol is 300 or more, preferably 400 or more, and more preferably 800 or more, from the perspective of increasing the flexibility of the polyuretane resin to maintain high gas barrier properties after folding of the laminate. In addition, from the perspective of maintaining high gas barrier properties after folding of the laminate without damaging the gas barrier properties of the polyuretane resin, the number average molecular weight of the macropolyol is 3000 or less, preferably 2000 or less, and more preferably 1200 or less. Meanwhile, the method for measuring the number average molecular weight of the macropolyol will be described later.

[0041] Examples of macropolyols include polyether polyols, polyester polyols, polycarbonate polyols, polyurethane polyols, epoxy polyols, vegetable oil polyols, polyolefin polyols, acrylic polyols, and vinyl monomer modified polyols.

[0042] As a macropolyol, polyether polyol, polyester polyol, and polycarbonate polyol are preferably used to increase the flexibility of the anchor coat layer, thereby increasing adhesion and followability with the paper and inorganic deposition layer, and maintaining high gas barrier properties after folding of the laminate.

[0043] Examples of polyether polyols include polyoxyalkylene (2-3 carbon atoms) polyols and polytetramethylene ether polyols (PTMG). Examples of polyoxyalkylene (2-3 carbon atoms) polyols include polypropylene glycol (PPG), polyethylene glycol (PEG), and propylene glycol-ethylene glycol copolymer (PO-EO copolymer), and preferably, polypropylene glycol.

[0044] As a polyester polyol, for example, a polycondensate obtained by reacting a low molecular weight polyol described later with a polybasic acid under known conditions may be cited. In addition, as a polyester polyol, polycaprolactone polyol and polyvalerolactone polyol obtained by ring-opening polymerization of lactones, such as ε-caprolactone and γ-valerolactone, respectively, using a low molecular weight polyol described later as an initiator may be cited.

[0045] (Number average molecular weight of macropolyols)

[0046] The macropolyol has the number average molecular weight described above. The number average molecular weight of the macropolyol is the polyethylene oxide equivalent molecular weight measured by gel permeation chromatography (GPC). The number average molecular weight of the macropolyol is measured, for example, using the following apparatus under the following conditions.

[0047] Device: HLC-8220 GPC (Glossary)

[0048] Column: TSKgelG1000HXL, TSKgelG2000HXL, and TSKgelG3000HXL (dosage) connected in series

[0049] Detector: Differential refractive index meter

[0050] Sample: Tetrahydrofuran (10 mL) solution of macropolyol (30 mg)

[0051] Injection volume: 100μL

[0052] Eluent: Tetrahydrofuran

[0053] Flow rate: 0.8 mL / min

[0054] Temperature: 40℃

[0055] Calibration curve: Standard polyethylene oxide in the range of 106–22450 (coating agent, trade name: TSK Standard Polyethylene Oxide)

[0056] (Mass ratio of macropolyol to short-chain diol)

[0057] The mass ratio of macropolyol (macropolyol / short-chain diol) to short-chain diol having 2 to 6 carbon atoms is, for example, 0.95 or higher, preferably 1.0 or higher, more preferably 1.3 or higher, in terms of increasing the flexibility of the anchor coat layer and maintaining high gas barrier properties after folding of the laminate. In addition, the mass ratio of macropolyol (macropolyol / short-chain diol) to short-chain diol having 2 to 6 carbon atoms is, for example, 75 or lower, preferably 50 or lower, more preferably 3.0 or lower, and even more preferably 2.7 or lower, in terms of increasing the gas barrier properties of the anchor coat layer and maintaining high gas barrier properties after folding of the laminate.

[0058] Examples of polycarbonate polyols include, for instance, a ring-opening polymer of ethylene carbonate (crystalline polycarbonate polyol) in which a low molecular weight polyol (preferably a dihydric alcohol) described later is used as an initiator, and, for instance, an amorphous polycarbonate polyol copolymerized with a dihydric alcohol such as 1,4-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, or 1,6-hexanediol.

[0059] Here, the aforementioned low molecular weight polyol is a polyol having two or more hydroxyl groups in its molecule and a molecular weight of 50 or more and less than 300. Examples of such low molecular weight polyols include divalent to octavalent alcohols. As dihydric alcohols, for example, ethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butylene glycol, 1,3-butylene glycol, 1,2-butylene glycol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, 2,2,2-trimethylpentanediol, 3,3-dimethylolheptane, alkane (7–20 C)diols, 1,3- or 1,4-cyclohexanedimethanol and mixtures thereof, 1,3- or 1,4-cyclohexanediol and mixtures thereof, hydrogenated bisphenol A, 1,4-dihydroxy-2-butene, Examples include 2,6-dimethyl-1-octene-3,8-diol, bisphenol A, diethylene glycol, triethylene glycol, and dipropylene glycol. Examples of trihydric alcohols include glycerin, trimethylolpropane, and triisopropanolamine. Examples of tetrahydric alcohols include tetramethylolmethane (pentaerythritol) and diglycerin. Examples of pentahydric alcohols include xylitol. Examples of hexahydric alcohols include sorbitol, mannitol, alitol, iditol, dulcitol, altritol, inositol, and dipentaerythritol. Examples of heptahydric alcohols include perceitol. Examples of octahydric alcohols include sucrose. These low molecular weight polyols may be used alone or in combination of two or more types.

[0060] (Active hydrogen compound containing hydrophilic groups)

[0061] An active hydrogen compound containing a hydrophilic group is a compound containing one or more hydrophilic groups, preferably one, such as a nonionic group or an ionic group, and two or more active hydrogen groups, preferably two, such as an amino group or a hydroxyl group. Specifically, examples include an active hydrogen group containing a nonionic group and an active hydrogen group containing an ionic group.

[0062] A compound containing an active hydrogen group containing a nonionic group is a compound having one or more, preferably one, nonionic group and two or more, preferably two, active hydrogen groups. Examples of nonionic groups include polyoxyethylene groups. Examples of compounds containing active hydrogen groups containing a nonionic group include polyoxyethylene glycol and polyols containing polyoxyethylene side chains. These compounds containing active hydrogen groups containing a nonionic group may be used alone or in combination of two or more types.

[0063] A compound containing an active hydrogen group containing an ionic group is a compound having one or more, preferably one, ionic group and two or more, preferably two, active hydrogen groups. Examples of compounds containing an active hydrogen group containing an ionic group include compounds containing an active hydrogen group containing an anionic group and compounds containing an active hydrogen group containing a cationic group. Examples of anionic groups include a carboxyl group (carboxylic acid group) and a sulfo group (sulfonic acid group). Examples of cationic groups include a quaternary ammonium group.

[0064] As a compound containing an active hydrogen group containing an ionic group, preferably, a compound containing an active hydrogen group containing an anionic group may be cited, more preferably, an organic compound having one or more anionic groups and two or more active hydrogen groups together may be cited, and even more preferably, an organic compound having one carboxyl group and two active hydrogen groups together (a compound containing an active hydrogen group containing a carboxyl group). In the compound containing an active hydrogen group containing an ionic group, as the active hydrogen group, preferably, a hydroxyl group may be cited.

[0065] Examples of active hydrogen compounds containing a carboxyl group include dihydroxycarboxylic acids such as 2,2-dimethylolacetic acid, 2,2-dimethylolactic acid, 2,2-dimethylolpropionic acid (DMPA), 2,2-dimethylolbutyric acid (DMBA), 2,2-dimethylolbutyric acid, and 2,2-dimethylolvaleric acid; diaminocarboxylic acids such as lysine and arginine; or their metal salts or ammonium salts. Preferably, 2,2-dimethylolpropionic acid (DMPA) and 2,2-dimethylolbutyric acid (DMBA) may be used.

[0066] (Polyols with three or more functions)

[0067] The active hydrogen group-containing component may include a polyol with three or more functions, provided that it does not impair the properties of the anchor coating material of the present invention. Examples of polyols with three or more functions include trihydric alcohols such as glycerin, trimethylolpropane, and triisopropanolamine; tetrahydric alcohols such as tetramethylolmethane (pentaerythritol) and diglycerin; pentahydric alcohols such as xylitol; hexahydric alcohols such as sorbitol, mannitol, alitol, iditol, dulcitol, altritol, inositol, and dipentaerythritol; heptahydric alcohols such as perceitol; and octahydric alcohols such as sucrose.

[0068] The concentration of polyols with three or more functions among the active hydrogen-containing components is preferably 0.05 mol% or less, more preferably 0.04 mol% or less, and particularly preferably 0 mol% (i.e., not containing polyols with three or more functions) with respect to the total amount of active hydrogen-containing components, in order not to impair the flexibility of the anchor coat layer and not to impair the gas barrier properties after folding of the laminate.

[0069] [Preparation of Isocyanate-Terminated Prepolymers]

[0070] An isocyanate-terminated prepolymer is obtained by mixing an isocyanate component and an active hydrogen group-containing component in a ratio in which the equivalent ratio of the isocyanate group in the isocyanate component to the active hydrogen group (e.g., hydroxyl group and / or amino group) in the active hydrogen group-containing component exceeds 1, preferably in a ratio of 1.1 to 10, and reacting them by a known polymerization method. Examples of known polymerization methods include bulk polymerization or solution polymerization.

[0071] In bulk polymerization, for example, the above components are mixed and reacted under a nitrogen atmosphere. The reaction temperature is, for example, 20 to 80°C. The reaction time is, for example, 1 to 20 hours.

[0072] In solution polymerization, for example, the above components are mixed and reacted in an organic solvent as a solvent under a nitrogen atmosphere. The reaction temperature is, for example, 20 to 80°C. The reaction time is 1 to 20 hours. The organic solvent is a low-boiling viscosity solvent that is inert to isocyanate groups, highly hydrophilic, and easy to remove. Examples of organic solvents include ketones (acetone, methyl ethyl ketone, etc.), ethers (tetrahydrofuran, etc.), cellosolve acetates (methyl cellosolve acetate, ethyl cellosolve acetate, etc.), carbitol acetates (methyl carbitol acetate, ethyl carbitol acetate, etc.), nitriles (acetonitrile, etc.), and esters (ethyl acetate, butyl acetate, etc.).

[0073] In addition, a catalyst may be added to the above polymerization as needed. Examples of catalysts include amine-based catalysts and organometallic (organotin-based, organolead-based, organobismuth-based) catalysts. These catalysts may be used alone or in combination of two or more types.

[0074] The above polymerization is terminated when the concentration of isocyanate groups in the reaction solution containing the reaction product reaches a range of, for example, 3 mass% or more, preferably 4 mass% or more, more preferably 5 mass% or more, for example, 15 mass% or less, preferably 10 mass% or less, more preferably 8 mass% or less, with respect to the total amount of the reaction product. In the above polymerization, unreacted isocyanate components may be removed by known removal methods, for example, distillation or extraction. By this, an isocyanate group-terminated prepolymer is obtained.

[0075] In the obtained isocyanate-terminated prepolymer, if an anionic or cationic group is included as the hydrophilic group of the hydrophilic group-containing active hydrogen compound, a neutralizing agent is added to form a salt of the anionic or cationic group.

[0076] For example, in cases where anionic groups are included, common bases may be used as neutralizing agents, such as organic bases (e.g., tertiary amines (trialkylamines such as trimethylamine, triethylamine, etc.; alkanolamines such as dimethylethanolamine, methyldiethanolamine, triethanolamine, etc.; heterocyclic amines such as morpholin, etc.)), inorganic bases (ammonia, alkali metal hydroxides (sodium hydroxide, potassium hydroxide, etc.), alkaline earth metal hydroxides (magnesium hydroxide, calcium hydroxide, etc.), alkali metal carbonates (sodium carbonate, potassium carbonate, etc.)).

[0077] These neutralizing agents may be used alone or in combination of two or more types. As neutralizing agents, organic bases are preferably used, tertiary amines are more preferably used, trialkylamines are even more preferably used, and particularly preferably triethylamines are preferably used.

[0078] The amount of neutralizing agent added is, for example, 0.4 equivalents or more, preferably 0.6 equivalents or more, per 1 equivalent of the ionic group. In addition, the amount of neutralizing agent added is, for example, 1.2 equivalents or less, preferably 1.0 equivalent or less, per 1 equivalent of the ionic group.

[0079] [Preparation of Polyurethan Dispersion Containing Polyurethan Resin]

[0080] A polyuretane dispersion containing a polyuretane resin is obtained by reacting the isocyanate-terminated prepolymer and a chain extender in water (chain extension reaction).

[0081] (Crushing agent)

[0082] The chain extender comprises, for example, a polyamine compound in order to obtain an anchor coating material comprising a polyurethan dispersion capable of forming an anchor coat layer with high gas barrier properties and flexibility. In order to further enhance the gas barrier properties of the anchor coat layer, the chain extender preferably comprises a polyamine compound that does not contain hydroxyl groups, more preferably comprises 50 mol% or more of a polyamine compound that does not contain hydroxyl groups, and particularly preferably comprises 100 mol% of a polyamine compound that does not contain hydroxyl groups.

[0083] Here, examples of polyamine compounds include polyamines and polyamino alcohols. Examples of polyamines that are polyamine compounds not containing hydroxyl groups include aromatic aliphatic polyamines, alicyclic polyamines, aliphatic polyamines, and polyoxyethylene group-containing polyamines.

[0084] Examples of aromatic polyamines include 4,4'-diphenylmethanediamine and tolylenediamine.

[0085] Examples of aromatic aliphatic polyamines include 1,3-xylylenediamine and 1,4-xylylenediamine.

[0086] Examples of cycloaliphatic polyamines include, for instance, 3-aminomethyl-3,5,5-trimethylcyclohexylamine (also known as isophoronediamine), 4,4'-dicyclohexylmethanediamine, 2,5-bis(aminomethyl)bicyclo[2.2.1]heptane, 2,6-bis(aminomethyl)bicyclo[2.2.1]heptane, 1,4-cyclohexanediamine, 1-amino-3-aminomethyl-3,5,5-trimethylcyclohexane, bis-(4-aminocyclohexyl)methane, diaminocyclohexane, 3,9-bis(3-aminopropyl)-2,4,8,10-tetraoxaspiro[5,5]undecaeine, 1,3-bis(aminomethyl)cyclohexane, and 1,4-bis(aminomethyl)cyclohexane.

[0087] Examples of aliphatic polyamines include ethylenediamine, propylenediamine, 1,3-propanediamine, 1,4-butanediamine, 1,5-pentanediamine, 1,6-hexamethylenediamine, hydrazine, hydrazine hydrate, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, 1,2-diaminoethane, 1,2-diaminopropane, and 1,3-diaminopentane.

[0088] These chain extenders may be used alone or in two or more types. The chain extender is preferably an aliphatic polyamine, and more preferably an ethylenediamine, in order to further enhance the gas barrier properties of the anchor coat layer.

[0089] In the chain extension reaction, for example, the isocyanate-terminated prepolymer and the chain extender are reacted in water. More specifically, for example, first, the isocyanate-terminated prepolymer is dispersed in water. Subsequently, a chain extender is added to the water dispersion of the isocyanate-terminated prepolymer to extend the chain of the isocyanate-terminated prepolymer by the chain extender. Here, the method of dispersing the isocyanate-terminated prepolymer in water is not particularly limited. For example, the isocyanate-terminated prepolymer is added to water while stirring. In this case, the amount of water is 100 to 1000 parts by mass for every 100 parts by mass of the isocyanate-terminated prepolymer.

[0090] Afterward, a chain extender is added dropwise to the water in which the isocyanate-terminated prepolymer is dispersed while stirring. In this case, the equivalent ratio of the active hydrogen group of the chain extender to the isocyanate group of the isocyanate-terminated prepolymer (active hydrogen group / isocyanate group) is, for example, 0.6 to 1.2. The chain extending reaction is completed, for example, at room temperature (e.g., 25°C). The time until the reaction is completed is, for example, 0.1 to 10 hours.

[0091] In addition, in this method, organic solvent and / or water may be removed after the reaction is complete in order to adjust the solid content concentration. In addition, in this method, water may be added after the reaction is complete in order to adjust the solid content concentration.

[0092] Additionally, in this method, a solvent may be added to adjust the solid content concentration. Examples of solvents include water, methanol, ethanol, propanol, isopropanol, acetone, methyl ethyl ketone, ethyl acetate, tetrahydrofuran, acetonitrile, etc. These solvents may be used alone or in combination of two or more types.

[0093] By this, a polyuretain dispersion (PUD) containing polyuretain resin is obtained.

[0094] Polyurethane dispersions may additionally contain additives in addition to polyurethane resin. Examples of additives include fillers, silane coupling agents, alkoxysilane compounds, thickeners, antioxidants, heat stabilizers, UV absorbers, plasticizers, antistatic agents, lubricants, anti-blocking agents, surfactants, dispersion stabilizers, colorants, pigments, dyes, colloidal silica, inorganic particles, inorganic oxide particles, layered inorganic compounds, leveling agents, crystallization nucleating agents, crosslinking agents, and curing agents. These additives may be used alone or in combination of two or more types. Meanwhile, the ratio of additives is not particularly limited and is appropriately adjusted according to the purpose and application.

[0095] The solid content concentration of the polyuretane dispersion is, for example, 10 mass% or more, preferably 15 mass% or more, more preferably 20 mass% or more. In addition, the solid content concentration of the polyuretane dispersion is, for example, 60 mass% or less, preferably 50 mass% or less, more preferably 40 mass% or less.

[0096] The pH of the polyuretaine dispersion is, for example, 5 or higher, preferably 6 or higher. In addition, the pH of the polyuretaine dispersion is, for example, 11 or lower, preferably 10 or lower.

[0097] The average particle size of the polyuretane dispersion is, for example, 10 nm or more, preferably 20 nm or more, more preferably 50 nm or more. In addition, the average particle size of the polyuretane dispersion is, for example, 500 nm or less, preferably 300 nm or less, more preferably 200 nm or less.

[0098] (Sanga)

[0099] The acid value of the polyuretaine resin in the polyuretaine dispersion is, for example, 20 mgKOH / g or higher, and preferably 25 mgKOH / g or higher, from the perspective of high storage stability. In addition, the acid value of the polyuretaine resin is, for example, 35 mgKOH / g or lower, and preferably 30 mgKOH / g or lower, from the perspective of high bending resistance.

[0100] (Total mass concentration of urea groups and urea groups)

[0101] In the polyuretane dispersion, the total mass concentration of uretane groups and urea groups in the polyuretane resin is, for example, 26 mass% or more, and preferably 30 mass% or more, with respect to the total amount of polyuretane resin, from the perspective of increasing the gas barrier properties of the anchor coat layer and maintaining high gas barrier properties after folding of the laminate. In addition, the total mass concentration of uretane groups and urea groups in the polyuretane resin is, for example, 37 mass% or less with respect to the total amount of polyuretane resin, from the perspective of increasing the flexibility of the anchor coat layer and maintaining high gas barrier properties after folding of the laminate. Meanwhile, the total mass concentration of uretane groups and urea groups in the polyuretane resin is calculated according to the following formula.

[0102] Total mass concentration (mass%) of urethan groups and urea groups in polyurethan resin

[0103] = 100 × [{(Amount of active hydrogen group-containing component (g) / Hydroxyl equivalent of active hydrogen group-containing component (g / eq)) × Molecular weight of urea group 59} + {(Amount of chain extender (g) / Amine equivalent of chain extender (g / eq)) × Molecular weight of urea group 58}] / Amount of polyurea resin (g)

[0104] Meanwhile, in the above formula, the active hydrogen group-containing component comprises the above short-chain diol, the above macropolyol, and the above hydrophilic group-containing active hydrogen compound.

[0105] (Mass concentration of short-chain diols)

[0106] In the polyuretane dispersion, the mass concentration of short-chain diols having 2 to 6 carbon atoms (constituent units derived from short-chain diols) in the polyuretane resin is, for example, 0.4 mass% or more, preferably 0.8 mass% or more, with respect to the total amount of polyuretane resin, in order to increase the gas barrier properties of the anchor coat layer and maintain high gas barrier properties after folding of the laminate. In addition, the mass concentration of short-chain diols having 2 to 6 carbon atoms (constituent units derived from short-chain diols) in the polyuretane resin is, for example, 9.5 mass% or less, preferably 9.2 mass% or less, with respect to the total amount of polyuretane resin, in order to increase the flexibility of the anchor coat layer and maintain high gas barrier properties after folding of the laminate.

[0107] (Mass concentration of macropolyols)

[0108] In the polyuretane dispersion, the mass concentration of a number average molecular weight of 300 or more and 3000 or less macropolyol (constituent unit derived from macropolyol) in the polyuretane resin is, for example, 11 mass% or more, preferably 12 mass% or more, with respect to the total mass of the polyuretane resin, in order to increase the flexibility of the anchor coat layer and maintain high gas barrier properties after folding of the laminate. In addition, the mass concentration of a number average molecular weight of 300 or more and 3000 or less macropolyol (constituent unit derived from macropolyol) in the polyuretane resin is, for example, 40.5 mass% or less, preferably 40 mass% or less, with respect to the total mass of the polyuretane resin, in order to increase the gas barrier properties of the anchor coat layer and maintain high gas barrier properties after folding of the laminate.

[0109] (Mass ratio of macropolyol to short-chain diol)

[0110] The mass ratio of macropolyol (constituent unit derived from macropolyol) to short-chain diol (constituent unit derived from short-chain diol) in the polyuretane dispersion (mass ratio of (macropolyol / short-chain diol)) is, for example, 0.95 or higher, preferably 1.0 or higher, more preferably 1.3 or higher, in order to increase the flexibility of the anchor coat layer and maintain high gas barrier properties after folding of the laminate. In addition, the mass ratio of macropolyol (constituent unit derived from macropolyol) to short-chain diol (constituent unit derived from short-chain diol) having 2 to 6 carbon atoms in the polyurethan resin (mass ratio of (macropolyol / short-chain diol)) is, for example, 75 or less, preferably 50 or less, more preferably 3.0 or less, and even more preferably 2.7 or less, in order to increase the gas barrier properties of the anchor coat layer and maintain high gas barrier properties after folding of the laminate.

[0111] (Oxygen permeability of the dried product of the anchor coating material)

[0112] The oxygen permeability of the dried anchor coating material is preferably 60cc / (m²) in terms of forming a laminate with high gas barrier properties after folding. 2 (·day·atm) or more, more preferably 70cc / (m 2 ☐ day· atm) or more, preferably 95cc / (m 2 ·day·atm) or less, more preferably 90cc / (m 2 It is less than 80cc / (m² / day·atm), and more preferably 80cc / (m² / day·atm²). 2 It is less than ·day·atm)

[0113] (Break elongation of a structure of anchor coating material)

[0114] The elongation at break of the anchor coating material is preferably 2.5 or higher, more preferably 3.0 or higher, and preferably 200 or lower, more preferably 80 or lower, in terms of forming a laminate with high gas barrier properties after bending the laminate.

[0115] (Young's modulus of the dried anchor coating material)

[0116] The Young's modulus of the dried anchor coating material is preferably 750 MPa or more, more preferably 1000 MPa or more, and preferably 2500 MPa or less, more preferably 2200 MPa or less, in terms of forming a laminate with high gas barrier properties after folding of the laminate.

[0117] Laminated structure

[0118] Referring to FIG. 1, a laminate (1) of one embodiment of the present invention comprises a paper (10), a snow-filling layer (12), an anchor coat layer (14), and an inorganic deposition layer (16) in the thickness direction. The anchor coat layer (14) includes a dried product of the anchor coating material. Since the anchor coat layer (10) of the laminate (1) of this embodiment includes a dried product of the anchor coating material, the gas barrier properties after folding are excellent.

[0119] [paper]

[0120] Paper (10) is formed by interlacing fibrous chemical substances (e.g., organic fibers, inorganic fibers) into a sheet. Specifically, paper (10) is obtained, for example, by forming pulp. Examples of pulp include natural pulp and synthetic pulp. More specifically, examples include glassine paper, coated paper, single-sided glossy (bleached) kraft paper, roll paper, and cup paper. Paper (10) may be single-layer paper or multi-layer paper. Paper (10) is appropriately selected according to the use of the laminate (1).

[0121] The weight of the paper (10) is not particularly limited, but is preferably 30 g / m² in order to maintain high gas barrier properties after folding of the laminate. 2 The above is the standard, and more preferably, 40 g / m² 2 That concludes the explanation. Furthermore, from the perspective of controlling paper costs, preferably 140 g / m² 2 It is as follows.

[0122] [Snow filling layer]

[0123] A snow-filling layer (12) is laminated onto the paper (10) to suppress the impregnation of the anchor coating material into the paper (10). Additionally, the snow-filling layer (12) is laminated onto the paper (10) to absorb irregularities on the surface of the paper (10) and to smooth the surface. More specifically, it is disposed on at least one side of the surface of the paper (10).

[0124] The snow-filling layer (12) contains, for example, a snow-filling resin. Specifically, the snow-filling layer (12) is formed by applying and drying a snow-filling coating material containing a snow-filling resin on the surface of the paper (10).

[0125] The opacity-filling resin is a resin that inhibits the impregnation of the anchor coating material into the paper (10). Examples of opacity-filling resins include polyolefin resin, polyester resin, polyamide resin, polyvinyl resin, (meth)acrylic resin, polycarbonate resin, polyuretaine resin, and cellulose resin. These may be used alone or in combination of two or more types. For the above purpose, polyolefin resin and (meth)acrylic resin may be used as opacity-filling resins.

[0126] The eye-filling layer (12) preferably does not contain an inorganic filler in order to maintain high gas barrier properties after folding of the laminate. The inorganic filler is a filler made of an inorganic chemical substance. There are no particular limitations on the inorganic filler, and examples include kaolin, clay, and talc.

[0127] The weight of the eye-filling layer (12) is not particularly limited, but in terms of suppressing the impregnation of the anchor coating material into the paper (10) and maintaining high gas barrier properties after folding of the laminate, it is preferably 4 g / m² 2 The above is the case, and more preferably, 5 g / m² 2 That is all. In addition, from the perspective of suppressing the cost of forming the snowfill layer, preferably 20g / m² 2 It is as follows.

[0128] [Anchor Court Floor]

[0129] An anchor coat layer (14) is placed on the surface of the snow-filling layer (12) to increase the adhesion between the paper (10), the snow-filling layer (12), and the inorganic deposition layer (16). The anchor coat layer (14) comprises a dried product of the above anchor coating material. Specifically, the anchor coat layer (14) is formed by applying and drying an anchor coating material comprising a polyuretain dispersion containing the above polyuretain resin on the surface of the snow-filling layer (12). Because of this, the laminate (1) having such an anchor coat layer (14) maintains high gas barrier properties after folding.

[0130] The weight of the anchor coat layer (14) is not particularly limited, but is preferably 0.05 g / m² in order to maintain high gas barrier properties after folding of the laminate. 2 That is the ideal, and more preferably, 0.1 g / m² 2 That is all. In addition, from the perspective of suppressing the cost of forming the anchor coat layer, preferably 5.0 g / m² 2 It is as follows.

[0131] [Inorganic deposition layer]

[0132] An inorganic deposition layer (16) is placed on the surface of the anchor coat layer (14) to increase the gas barrier properties of the laminate. Specifically, the inorganic deposition layer (16) is formed on the surface of the anchor coat layer (14) by, for example, vacuum deposition, sputtering, ion plating, or chemical vapor deposition (CVD).

[0133] Examples of inorganic materials (including metals) used in the inorganic deposition layer (16) include magnesium, calcium, and barium from Group 2 of the periodic table; titanium and zirconium from Group 4; aluminum and indium from Group 13; and silicon, germanium, and tin from Group 14. Additionally, specifically, examples of such inorganic materials include aluminum (Al), aluminum oxide (AlxOy), magnesium oxide (MgOx), titanium oxide (TiOx), indium oxide (InxOy), silicon oxide (SiOx), silicon nitride oxide (SiOxNy), cerium oxide (CeOx), calcium oxide (CaOx), tin oxide (SnOx), diamond-like carbon films, or mixtures thereof. Among these, aluminum, silicon, and their oxides are preferred from the viewpoint of excellent gas barrier properties, and aluminum and its oxides are more preferred. Furthermore, the inorganic deposition layer may be formed in a multilayer structure by combining multiple layers.

[0134] The thickness of the inorganic deposition layer (16) is not particularly limited, but is preferably 5 nm or more, more preferably 20 nm or more, and even more preferably 50 nm or more in terms of maintaining high gas barrier properties after folding of the laminate. In addition, it is preferably 250 nm or less in terms of suppressing the cost of forming the inorganic deposition layer.

[0135] (Overcoat layer)

[0136] In order to protect the inorganic deposition layer (16) and maintain high gas barrier properties after folding of the laminate (1), an overcoat layer (17) may be disposed on the surface of the inorganic deposition layer (16). The overcoat layer (17) contains, for example, an overcoat resin. Specifically, the overcoat layer (17) is formed by applying and drying an overcoating material containing an overcoat resin on the surface of the inorganic deposition layer (16).

[0137] The overcoat resin is a resin that protects the inorganic deposition layer (16). Examples of overcoat resins include polyolefin resin, polyester resin, polyamide resin, polyvinyl resin, (meth)acrylic resin, polycarbonate resin, polyuretaine resin, and cellulose resin. These may be used alone or in combination of two or more types. For the above purpose, polyvinyl resin or polyuretaine resin may be preferably used as the overcoat resin.

[0138] (Heat sealing layer)

[0139] In the laminate (1), a heat sealing layer (18) may be disposed on the surface of an inorganic deposition layer (16) or an overcoat layer (17) in order to enable heat sealing. The heat sealing layer (18) contains, for example, a heat sealing resin. Specifically, the heat sealing layer (18) is formed by applying and drying a heat sealing coating material containing a heat sealing resin on the surface of the inorganic deposition layer (16) or the overcoat layer (17).

[0140] The heat sealing resin is a resin that enables heat sealing (thermal fusion) of the laminate (1) and thus enables heat sealing of the laminate. The heat sealing resin is not particularly limited, and any known heat sealing resin is used. More specifically, examples of heat sealing resins include polyolefin resin, (meth)acrylic resin, and polyuretaine resin. These can be used individually or in combination of two or more types.

[0141] From the perspective of manufacturability of a heat-sealing coating material, the heat-sealing resin preferably contains anionic groups. That is, as a heat-sealing resin, preferably, a heat-sealing resin containing anionic groups can be cited. If the heat-sealing resin contains anionic groups, the heat-sealing resin is easily dissolved and / or dispersed in water, so the heat-sealing coating material is obtained efficiently. Examples of anionic groups include carboxyl groups (carboxylic acid groups) and sulfo groups (sulfonic acid groups), and preferably, carboxyl groups. Examples of heat-sealing resins containing anionic groups include polyolefin resins containing anionic groups, (meth)acrylic resins containing anionic groups, and polyurethane resins containing anionic groups. In other words, the heat sealing resin containing anionic groups contains at least one type selected from the group consisting of, for example, anionic group-containing polyolefin resin, anionic group-containing (meth)acrylic resin, and anionic group-containing polyurethan resin.

[0142] (Variation Example)

[0143] In the above description, the laminate (1) comprises paper (10), a snow-filling layer (12), an anchor coat layer (14), and an inorganic deposition layer (16), but the composition of the laminate (1) is not limited to the above as long as it includes the anchor coat layer (14). For example, the laminate (1) may not have a snow-filling layer (12). Also, for example, the laminate (1) may not have an inorganic deposition layer (16).

[0144] Additionally, the laminate (1) may be provided with a substrate other than paper instead of paper (10). More specifically, the laminate (1) may be provided with a resin film instead of paper (10) as a substrate, for example. In the resin film, examples of resins include polyolefin resin, polyester resin, polyamide resin, vinyl resin, (meth)acrylic resin, and engineering plastic. Examples of polyolefin resins include polyethylene and polypropylene. Examples of polyester resins include polyethylene terephthalate and polybutylene terephthalate. Examples of polyamide resins include nylon 6 and nylon 66. Examples of vinyl resins include polystyrene, polyvinyl acetate, and ethylene-vinyl acetate copolymer. Examples of (meth)acrylic resins include homopolymers and copolymers of (meth)acrylic monomers, specifically polymethyl methacrylate and polyacrylonitrile. Examples of engineering plastics include polycarbonate and polyimide. Additionally, cellulose (cellophane) may be used as a resin. The resin may be used alone or in combination of two or more types. That is, the resin film may contain a single type of resin or may contain two or more types of resins. Furthermore, the resin film may be, for example, a single-layer film or a multi-layer film.

[0145] Furthermore, excellent gas barrier properties are obtained even when a substrate other than paper (e.g., the resin film mentioned above) is used as the substrate. That is, the anchor coat layer mentioned above possesses excellent flexibility, adhesion, and conformability. Therefore, if the laminate is equipped with the anchor coat layer mentioned above, a laminate with excellent gas barrier properties after folding is obtained even when a substrate other than paper (e.g., the resin film mentioned above) is used as the substrate.

[0146] Examples

[0147] Next, the present invention will be described based on examples and comparative examples, but the present invention is not limited to the following examples. Furthermore, specific numerical values ​​such as mixing ratios (content ratios), physical properties, and parameters used in the description below may be replaced with the upper limits (numerical values ​​defined as “less than” or “less than”) or lower limits (numerical values ​​defined as “greater than” or “greater than”) of the mixing ratios (content ratios), physical properties, parameters, etc. described in the “Specific Details for Implementing the Invention” above, which correspond thereto.

[0148] Production of Anchor Coating Material

[0149] (Example A1)

[0150] The following raw material components were reacted under a nitrogen atmosphere at 50–70°C until the isocyanate group concentration (NCO%) was 5.15 mass% or less. By doing so, a reaction solution containing an isocyanate group-terminated prepolymer was obtained.

[0151] Ingredients

[0152] 1,3-Xylylene diisocyanate

[0153] (Takenate 500, 1,3-XDI, manufactured by Mitsui Chemical Co.) 173.2 parts by mass

[0154] 4,4'-Methylenebis(cyclohexyl isocyanate)

[0155] (Vestanat H 12 MDI (manufactured by Evonik) 30.2 parts by mass

[0156] 23.8 parts by mass of ethylene glycol

[0157] 23.7 parts by mass of dimethylolpropionic acid

[0158] 71.6 parts by mass of polypropylene glycol (Actcol D-400, manufactured by Mitsui Chemical Co., Ltd.)

[0159] 160.0 parts by mass of methyl ethyl ketone (solvent)

[0160] Next, the obtained reaction solution was cooled to 40°C. Subsequently, 17.5 parts by mass of triethylamine were added to the reaction solution to neutralize the isocyanate-terminated prepolymer. Then, the neutralized reaction solution was dispersed in 1113.6 parts by mass of ion-exchanged water using a homodisperser. Subsequently, an aqueous amine solution was added to the obtained dispersion to perform a chain extension reaction, followed by aging for 1 hour. Meanwhile, the aqueous amine solution was a mixture of 50.0 parts by mass of ion-exchanged water and 16.7 parts by mass of ethylenediamine. Afterward, methyl ethyl ketone and ion-exchanged water were removed by distillation using an evaporator. By doing so, the solid content concentration was adjusted to 25% by mass. As a result, a polyuretain dispersion (PUD) containing polyuretain resin was obtained as an anchor coating material. The results are shown in Table 1.

[0161] (Examples A2~A19 and Comparative Examples AR1~AR3)

[0162] According to the formulations listed in Tables 1 to 4, a polyuretain dispersion (PUD) containing a polyuretain resin was obtained as an anchor coating material by the same method as in Example A1.

[0163] [Physical properties of anchor coating materials]

[0164] For the obtained anchor coating material, the molar concentration of xylylene diisocyanate (XDI) in the isocyanate component, the molar concentration of trimethylolpropane (TMP) in the active hydrogen group-containing component, the total mass concentration of uretain groups and urea groups in the polyuretain resin, the mass concentration of short-chain diols in the polyuretain resin, the mass concentration of macropolyols in the polyuretain resin, and the mass ratio of the macropolyols to the short-chain diols were calculated and summarized in Tables 1 to 4.

[0165] Here, in Example A4, the molar concentration of trimethylolpropane (TMP), a polyol with three or more functions in the active hydrogen group-containing component, was calculated by a known method based on the hydroxyl group equivalent (molecular weight / number of hydroxyl groups) and the amount of blending. More specifically, the molar concentration of TMP in the active hydrogen group-containing component was calculated by the following formula and was 0.035 mol%.

[0166] (2.5 parts by mass / 44.725) / [(31.1 parts by mass / 31.034) + (2.5 parts by mass / 44.725) + (23.8 parts by mass / 67.066) + (41.7 / 200)] × 100 = 0.035 (mol%)

[0167] Hydroxyl equivalent of ethylene glycol: 31.034

[0168] Hydroxyl equivalent of trimethylolpropane: 44.725

[0169] Hydroxyl equivalent of dimethylolpropanoic acid: 67.066

[0170] Hydroxyl equivalent of Actcol D-400: 200

[0171] In addition, in Example A5, the molar concentration of trimethylolpropane (TMP), a polyol with three or more functions in the active hydrogen group-containing component, was calculated in the same way as in Example A5 and was 0.044 mol%.

[0172] Additionally, in Example A18, the molar concentration of ethylenediamine for the chain extender was calculated by a known method based on the molecular weight and the amount of formulation. More specifically, the molar concentration of ethylenediamine for the chain extender was calculated by the following formula and was 40 mol%.

[0173] (6.4 parts by mass / 30.05) / [(16.6 parts by mass / 52.10) + (6.4 parts by mass / 30.05)] × 100 = 40 (mol%)

[0174] Molecular weight of ethylenediamine (EDA): 30.05

[0175] Hydroxyl equivalent of 2-(2-aminoethylamino)ethanol (AEA): 52.10

[0176] In addition, in Example A19, the molar concentration of ethylenediamine (EDA) for the chain extender was calculated in the same way as in Example A18 and was 50 mol%.

[0177] In addition, the total mass concentration of urea groups and urea groups in the polyurethane resin was calculated according to the following formula.

[0178] Total mass concentration (mass%) of urethan groups and urea groups in polyurethan resin

[0179] = 100 × [{(Amount of active hydrogen group-containing component (g) / Hydroxyl equivalent of active hydrogen group-containing component (g / eq)) × Molecular weight of urea group 59} + {(Amount of chain extender (g) / Amine equivalent of chain extender (g / eq)) × Molecular weight of urea group 58}] / Amount of polyurea resin (g)

[0180] Meanwhile, in the above formula, the active hydrogen group-containing component comprises the above short-chain diol, the above macropolyol, and the above hydrophilic group-containing active hydrogen compound.

[0181] Additionally, the fracture strength, Young's modulus, and oxygen permeability of the anchor coating material were measured and summarized in Tables 1 to 4.

[0182] (Measurement of fracture strength and Young's modulus)

[0183] First, a dried film of the anchor coating material was prepared as follows. Polyuretaine dispersion (PUD), which is the anchor coating material, was placed in a polypropylene container to a uniform thickness so that the thickness after drying was 200 μm. Subsequently, the PUD contained in the container was dried at room temperature (25°C) for 24 hours, and then further dried in a drying oven set to 110°C for 60 minutes.

[0184] The elongation at break and Young's modulus of the obtained dried film of the anchor coating material were measured using a tensile testing machine (INTESCO, Model Measurements were taken using 205N. The results are summarized in Tables 1 to 4. The measurement conditions are shown below.

[0185] Sample size: Width 5mm

[0186] Film thickness: 200μm

[0187] Interval: 5cm

[0188] Tensile speed: 10mm / min

[0189] Young's modulus was calculated using the following formula.

[0190] Young's modulus = Stress at yield point (MPa) / Elongation at yield point

[0191] (Measurement of Oxygen Permeability (OTR))

[0192] First, a dried film of the anchor coating material was prepared as follows. On a polyethylene terephthalate film (biaxially stretched polyester film, product name: Toyobo Ester Film E5102, manufactured by Toyobo, thickness 12 μm) used as a substrate, a film having a dry mass of 3 g / m² 2 Polyuretaine dispersion (PUD), an anchor coating material, was applied using a bar coater. Subsequently, the applied PUD was placed in a drying oven set to 110°C for 1 minute to dry, thereby obtaining a laminate.

[0193] Using an oxygen permeability measuring device (OX-TRAN2 / 20, manufactured by MOCON), JIS Based on K7126-2 (2006), 1m of a laminate at 20°C and 80% relative humidity (80%RH). 2 Oxygen permeability (cc) per day and per atmosphere was measured. The results are summarized in Tables 1–4.

[0194]

[0195]

[0196]

[0197]

[0198] Meanwhile, the meanings of the English abbreviations listed in Tables 1 to 4 are as follows.

[0199] 1,3-XDI: 1,3-Xylylene diisocyanate (Alias: 1,3-Bis(isocyanatomethyl)benzene)

[0200] 1,3-H6XDI: 1,3-bis(isocyanatemethyl)cyclohexane

[0201] 4,4'-H 12 MDI: 4,4'-Dicyclohexylmethane diisocyanate

[0202] EG: Ethylene glycol

[0203] DMPA: Dimethylolpropionic acid

[0204] TMP: Trimethylolpropane

[0205] D-400: Trade Name: Actcol (Registered Trademark) D-400, Polypropylene Glycol, Number Average Molecular Weight 400, Average Number of Functional Groups 2

[0206] D-1000: Trade Name: Actcol (Registered Trademark) D-1000, Polypropylene Glycol, Number Average Molecular Weight 1000, Average Number of Functional Groups 2

[0207] D-2000: Trade Name: Actcol (Registered Trademark) D-2000, Polypropylene Glycol, Number Average Molecular Weight 2000, Average Number of Functional Groups 2

[0208] D-3000: Trade Name: Actcol (Registered Trademark) D-3000, Polypropylene Glycol, Number Average Molecular Weight 3000, Average Number of Functional Groups 2

[0209] PTMG-1000: Polytetramethylene ether glycol, number average molecular weight 1,000

[0210] UH-50: Trade Name: ETERNACOLL (Registered Trademark) DH-50, Polycarbonate Diol, Number Average Molecular Weight 500

[0211] UH-100: Trade Name: ETERNACOLL (Registered Trademark) DH-100, Polycarbonate Diol, Number Average Molecular Weight 1000

[0212] U-5610W: (Takelac (Trademark) U-5610W) Polyester Glycol (Composition: Adipic Acid / 1,6-Hexanediol / Neopentyl Glycol), Number Average Molecular Weight 1000

[0213] Fluxel 210W: Polycaprolactone diol, number average molecular weight 1000

[0214] TEA: Triethylamine

[0215] EDA: Ethylenediamine

[0216] AEA: 2-(2-aminoethylamino)ethanol

[0217] MEK: Methyl ethyl ketone

[0218] OTR: Oxygen permeability (Unit: cc / (m²) 2 ·day·atm))

[0219] A1: Example A1

[0220] PVA: Polyvinyl alcohol

[0221] Fabrication of Laminated Structures

[0222] [Preparation of each ingredient]

[0223] 1. Paper

[0224] As paper, single-sided glossy (bleached) kraft paper (Product name: Silver, manufactured by Nippon Paper, basis weight 65 g / m²) 2 Prepared ).

[0225] 2. Glow-filling coating material

[0226] The following two types of eye-filling coating materials were prepared.

[0227] (1) No weapon filler

[0228] 2193 parts by mass of ion-exchanged water (solvent) and 2.5 parts by mass of sodium dodecyl sulfate (surfactant) were added to a reaction vessel equipped with a stirrer, a reflux condenser, a dropping device, and a thermometer. The contents of the reaction vessel were heated until the temperature reached 75°C while stirring and nitrogen purging.

[0229] While maintaining the internal temperature of the reaction vessel at 75°C, 7.5 parts by mass of potassium persulfate (polymerization initiator) were added to the reaction vessel and dissolved in the contents of the reaction vessel. Then, a pre-prepared monomer emulsion was continuously added dropwise to the reaction vessel over a period of 5 hours.

[0230] Meanwhile, the monomer emulsion is a raw material composition containing the following components.

[0231] 900 parts by mass of ion-exchanged water (solvent)

[0232] 5 parts by mass of sodium dodecyl sulfate (surfactant)

[0233] 25 parts by mass of acrylamide (raw material monomer)

[0234] 175 parts by mass of methyl methacrylate (raw material monomer)

[0235] 1088 parts by mass of 2-ethylhexyl acrylate (raw material monomer)

[0236] 80 parts by mass of methacrylic acid (raw material monomer)

[0237] 1133 parts by mass of styrene (raw material monomer)

[0238] After the dropwise loading of the monomer emulsion was completed, the contents of the reaction vessel were aged for 3 hours. By doing so, the raw monomer was polymerized to obtain a (meth)acrylic resin. In addition, an acrylic emulsion in which the (meth)acrylic resin was water-dispersed was obtained.

[0239] The acrylic emulsion was cooled to room temperature. Then, ion-exchanged water and ammonia water (neutralizing agent) were added to the acrylic emulsion to adjust the solid content concentration to 41 mass% and the pH to 8.0. By doing so, an acrylic emulsion formed by the water dispersion of (meth)acrylic resin was obtained.

[0240] The average particle size of the acrylic emulsion was 140 nm. The average particle size was measured by dynamic light scattering (measuring device FPAR-1000, manufactured by Otsuka Electronics Co., Ltd.) (the same applies hereinafter).

[0241] After that, water was added to the above acrylic emulsion (solid content 41 mass%) and mixed with a mixer for 5 minutes. By doing so, an inorganic filler-free anti-glare coating material (solid content 40 mass%) was prepared.

[0242] (2) Weapon filler (kaolin) present

[0243] Kaolin (Imeris Barisurf HX) was added to the inorganic filler-free eye-filling coating material obtained in (1) above so that the solid content ratio (mass ratio) of the eye-filling coating material:kaolin = 20:80, thereby preparing an eye-filling coating material containing inorganic filler (kaolin).

[0244] 3. Anchor coating material

[0245] Anchor coating materials described in Examples A1 to A18 and Comparative Examples AR1 to AR3 above were prepared.

[0246] 4. Overcoating material

[0247] As overcoating materials, an overcoating material prepared according to the same formula as the anchor coating material described in Example A1 (Example B29) and polyvinyl alcohol (trademark: Guraray Poval (registered trademark) PVA-110) (Example B30) were prepared.

[0248] 5. Heat-sealing coating material

[0249] The following heat sealing coating materials were prepared.

[0250] 50 parts by mass of an ethylene-acrylic acid copolymer and 50 parts by mass of an ethylene-acrylic acid isobutyl-methacrylic acid copolymer were melt-kneaded. By doing so, an anionic group-containing polyolefin resin composition was obtained as a resin composition.

[0251] Meanwhile, regarding the total amount of the ethylene-acrylic acid copolymer, the content ratio of constituent units derived from ethylene was 79.5 mass%, and the content ratio of constituent units derived from acrylic acid was 20.5 mass%.

[0252] In addition, regarding the total amount of the ethylene-isobutyl acrylate-methacrylic acid copolymer, the content ratio of constituent units derived from ethylene was 80.0 mass%, the content ratio of constituent units derived from isobutyl acrylate was 10.0 mass%, and the content ratio of constituent units derived from methacrylic acid was 10.0 mass%.

[0253] The above anionic group-containing polyolefin resin composition, 4.0 parts by mass of potassium hydroxide (neutralizing agent), and 140 parts by mass of deionized water were placed in a reaction vessel and stirred. The contents of the reaction vessel were heated to 150°C and held for 4 hours. In this way, the anionic group-containing polyolefin resin composition was neutralized by potassium hydroxide (neutralizing agent). Afterward, the contents of the reaction vessel were cooled to room temperature (e.g., 25°C).

[0254] As a result, a water dispersion of a neutralized anionic group-containing polyolefin resin composition was obtained. This water dispersion was a polyolefin dispersion. The solid content of this water dispersion was 42 mass%. In addition, the average particle size of this water dispersion was 0.5 μm.

[0255] [Formation of Laminated Structures]

[0256] (Examples B1–B31 and Comparative Examples BR1–BR3)

[0257] 1. Formation of the filling layer

[0258] On the glossy surface of each prepared single-sided glossy kraft paper, a prepared anti-glare coating material without inorganic fillers (Examples B1–B30 and Comparative Examples BR1–BR3) or a prepared anti-glare coating material containing inorganic fillers (kaolin) (Example B31) was applied using a bar coater. The application amount was 10 g / m² with a dry mass (weighed weight of the anti-glare layer). 2 (Examples B1–B22 and B26–B31 and Comparative Examples BR1–BR3), 20g / m² 2 (Example B23), 5g / m² 2 (Example B24), or 4 g / m 2 (Example B25) was adjusted. Subsequently, each film of the glare-filling coating material was dried at 120°C for 1 minute to form each glare-filling layer.

[0259] 2. Formation of the anchor coat layer

[0260] Each anchor coating material prepared in Examples A1 to A18 and Comparative Examples AR1 to AR3 was applied to the surface of each formed gap-filling layer using a bar coater. The application amount was 2.5 g / m² with a dry mass (weighed weight of the anchor coat layer). 2 (Examples B1–B25, B29, B30, and B31 and Comparative Examples BR1–BR3), 5.0 g / m² 2 (Example B26), 0.1 g / m² 2 (Example B27), or 0.05 g / m² 2 (Example B28) was adjusted. Subsequently, each anchor coating film was dried at 80°C for 1 minute to form each anchor coat layer.

[0261] 3. Formation of the inorganic deposition layer

[0262] Each sample with an anchor coat layer formed is set in a vacuum deposition apparatus (Alvacz resistance heating method), and 1×10 -4 Under vacuum conditions of Pa, aluminum was deposited on the surface of each anchor coat layer to form an inorganic deposition layer. The thickness of each inorganic deposition layer was 65 nm.

[0263] In this way, in Examples B1 to B31 and Comparative Examples BR1 to BR3, each 4-layer laminate was obtained in which 4 layers of paper, a gypsum layer, an anchor coat layer, and an inorganic deposition layer were laminated in this order in the thickness direction.

[0264] 4. Formation of the overcoat layer

[0265] On the surface of the inorganic deposition layer of the 4-layer laminate of Example B29, an overcoating material (A1) prepared according to the same formula as the anchor coating material described in Example A1 was applied with a bar coater.

[0266] In addition, polyvinyl alcohol (trade name: Kuraray Poval (registered trademark) PVA-110) (PVA) was applied to the surface of the inorganic deposition layer of the 4-layer B30 laminate using a bar coater. The application amount was 0.5 g / m² with a dry mass (weighing of the overcoating material). 2 It was adjusted to be such. Subsequently, the film of the overcoating material was dried at 120°C for 1 minute to form an overcoat layer. In this way, in Example B29, a 5-layer laminate was obtained in which the 5 layers of paper, a gypsum layer, an anchor coat layer, an inorganic deposition layer, and an overcoat layer were laminated in this order in the thickness direction.

[0267] 5. Formation of the heat sealing layer

[0268] The prepared heat-sealable coating material was applied using a bar coater to the surface of the inorganic deposition layer of each 4-layer laminate of Examples B1–B28 and B31 and Comparative Examples BR1–BR3, or to the surface of the overcoat layer of the 5-layer laminate of Examples B29 and B30. The application amount was 6 g / m² with a dry mass (weighed weight of the heat-sealable coating material). 2 It was adjusted to be so. Subsequently, the film of the heat sealing coating material was dried at 120°C for 1 minute to form each sealing layer.

[0269] In this way, in Examples B1 to B28 and B31 and Comparative Examples BR1 to BR3, a laminate (without overcoat layer) was obtained in which five layers, including paper, a glazing layer, an anchor coat layer, an inorganic deposition layer, and a heat sealing layer, were laminated in this order in the thickness direction. Additionally, in Example B29, a laminate (with overcoat layer) was obtained in which six layers, including paper, a glazing layer, an anchor coat layer, an inorganic deposition layer, an overcoat layer, and a heat sealing layer, were laminated in this order in the thickness direction.

[0270] [Material Properties of Laminated Materials]

[0271] The oxygen permeability (OTR) before and after the bending (valley bending or mountain bending) described below is measured by an oxygen permeability measuring device (MOCON, OX-TRAN Measurements were taken using 2 / 22H. The measured temperature was 20℃. In addition, the relative humidity was 80%RH. The results are summarized in Tables 1 to 4.

[0272] In Examples B1 to B31 and Comparative Examples BR1 to BR3, the following fracture bending test was performed. Fracture bending was performed twice according to the following procedure. In the first attempt, the laminate was subjected to a fracture bending of 2 kg / cm² so that the deposition surface (gloss filling layer, anchor coat layer, inorganic deposition layer (, overcoat layer), heat sealing layer) side was fractured. 2 The laminate was bent for 10 seconds under pressure. For the second bend, the bending direction was changed 90° from the first bend to create a cross-shaped fold mark, and the laminate was bent again at 2 kg / cm² so that the deposition surface (gloss filler layer, anchor coat layer, inorganic deposition layer (, overcoat layer), heat sealing layer) side formed a ridge fold. 2 It was bent for 10 seconds under pressure.

[0273] In addition, for Examples B8, B29, and B30, the following crest bending test was also performed. The crest bending was performed twice according to the following procedure. For the first time, the laminate was subjected to 2 kg / cm² so that the deposition surface (eye-filling layer, anchor coat layer, inorganic deposition layer (, overcoat layer), heat sealing layer) side was crest-folded. 2The laminate was bent for 10 seconds under a pressure of []. For the second bend, the bending direction was changed 90° from the first bend to create a cross-shaped fold mark, and the laminate was bent again at 2 kg / cm² so that the deposition surface (eye-filling layer, anchor coat layer, inorganic deposition layer (, overcoat layer), heat sealing layer) side formed a mountain fold. 2 It was bent for 10 seconds under pressure.

[0274] Meanwhile, although the above invention has been provided as an exemplary embodiment of the present invention, it is merely an example and should not be interpreted restrictively. Variations of the present invention that are obvious to those skilled in the art are included in the scope of the subsequent claims. Industrial applicability

[0275] The anchor coating material and laminate of the present invention are suitably used, particularly in the field of packaging materials. Explanation of the symbols

[0276] 1 laminate 10 papers 12 Eye filling layer 14 Undercoat layer 16 Inorganic deposition layer 17 Overcoat layer 18 Heat sealing layer

Claims

Claim 1 An anchor coating material comprising a polyurethan dispersion, wherein the polyurethan dispersion contains a polyurethan resin, wherein the polyurethan resin is a reaction product of an isocyanate group-terminated prepolymer and a chain extender, wherein the isocyanate group-terminated prepolymer comprises a reaction product of an isocyanate component and an active hydrogen group-containing component, wherein the active hydrogen group-containing component comprises a short-chain diol having 2 to 6 carbon atoms, a macropolyol having a number average molecular weight of 300 to 3000, and a hydrophilic group-containing active hydrogen compound, and wherein the total concentration of urethan groups and urea groups in the polyurethan resin is 26 mass% or more and 37 mass% or less. Claim 2 In claim 1, the chain elongator is an anchor coating material comprising 50 mol% or more of a polyamine compound that does not contain hydroxyl groups. Claim 3 In claim 1, the isocyanate component is an anchor coating material containing 50 mol% or more of xylylene diisocyanate. Claim 4 An anchor coating material according to claim 1, wherein the concentration of a polyol with three or more functions among the active hydrogen group-containing components is 0.04 mol% or less. Claim 5 An anchor coating material according to claim 1, wherein the mass ratio of the macropolyol to the short-chain diol is 1.0 or more and 3.0 or less. Claim 6 A laminate comprising paper, a snow-filling layer, an anchor coat layer, and an inorganic deposition layer in the thickness direction, wherein the anchor coat layer comprises a dried product of an anchor coating material described in any one of claims 1 to 5. Claim 7 In paragraph 6, the above-mentioned eye-filling layer is a laminate that does not contain an inorganic filler.