Silicon-carbon composite material and preparation method therefor, secondary battery, and electric device

The silicon-carbon composite material addresses the expansion and conductivity challenges of silicon-based batteries by using a carbon matrix with a porous structure and controlled V_A/V_B ratio, enhancing performance and efficiency.

KR1020260161665APending Publication Date: 2026-11-09CONTEMPORARY AMPEREX RUNZHI SOFTWARE TECH LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
KR1020267036013
Authority / Receiving Office
KR · KR
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-10-20
Filing Date
2024-04-23
Publication Date
2026-11-09

AI Technical Summary

Technical Problem

Silicon-based materials in secondary batteries exhibit high expansion characteristics and poor conductivity, leading to reduced recyclability and limited energy density advancements.

Method used

A silicon-carbon composite material is developed, featuring a carbon matrix with a porous structure and silicon-based material distributed within the pores, which acts as a buffer for volume expansion and improves conductivity, with a specific V_A/V_B ratio ≥1.40 to enhance cycling performance and initial charge/discharge efficiency.

Benefits of technology

The silicon-carbon composite material effectively mitigates volume expansion issues, improving cycling performance and initial charge/discharge efficiency by leveraging the carbon matrix's conductivity and buffering properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PAT00005_ABST
    Figure PAT00005_ABST
Patent Text Reader

Abstract

The present invention provides a silicon carbon composite material, a method for manufacturing the same, a secondary battery, and an electrical device; the silicon carbon composite material comprises a carbon matrix having a porous structure and a silicon-based material distributed in the porous structure; by charging and discharging the silicon carbon composite material with a button cell, and drawing a relationship curve between the differential value (dQ / dV) obtained by differentiating the charge / discharge capacity (Q) with respect to the voltage (V) of the button cell charge / discharge curve and the voltage (V), recording the maximum differential value (dQ / dV) between 0.26V and 0.35V as VA and the maximum differential value (dQ / dV) between 0.42V and 0.52V as VB, the silicon carbon composite material satisfies VA / VB≥1.40; and the cyclic performance and initial charge / discharge efficiency of the silicon carbon composite material can be significantly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] This application claims priority to the Chinese patent application filed on October 20, 2023, application number 202311360972.7, titled "Silicon carbon composite material and method of manufacturing the same, secondary battery and electrical device," the full text of which is incorporated herein by reference.

[0002] This application belongs to the field of secondary battery technology, and in particular relates to silicon-carbon composite materials and methods for manufacturing the same, secondary batteries, and electrical devices. Background Technology

[0003] Rechargeable batteries are widely applied in fields such as portable electronic devices and electric vehicles. With the continuous development of the new energy industry, users are presenting higher usage requirements for rechargeable batteries, such as high energy density. The problem to be solved

[0004] Silicon-based materials are widely applied in secondary batteries due to their high capacity. However, silicon exhibits high expansion characteristics and poor conductivity; consequently, while silicon-based materials increase the energy density of secondary batteries, they also affect the recyclability of the batteries, thereby limiting further advancements in battery technology. means of solving the problem

[0005] Based on this, it is necessary to provide a silicon-carbon composite material and a method for manufacturing the same, as well as a secondary battery and an electrical device, to mitigate the expansion of a secondary battery and improve the circulation performance of a secondary battery.

[0006] To achieve the above objective, a first aspect of the present application provides a silicon carbon composite material:

[0007] A carbon matrix having a porous structure; and

[0008] It includes a silicon-based material distributed in the pore structure of the carbon matrix;

[0009] The above silicon-carbon composite material is charged and discharged using a button cell, and a relationship curve is plotted between the voltage (V) and the derivative value (dQ / dV) obtained by differentiating the charge / discharge capacity (Q) with respect to the voltage (V) of the button cell's charge / discharge curve, and the maximum value of the derivative value (dQ / dV) between 0.26V and 0.35V is V A Record as, and the maximum value of the derivative (dQ / dV) between 0.42V and 0.52V is V B If recorded as such, the above silicon-carbon composite material is V A / V B Satisfies ≥1.40.

[0010] In the silicon-carbon composite material of the present application, at least a portion of the silicon-based material is distributed within the pore structure of the carbon matrix, and the carbon matrix can improve the conductivity of the silicon-based material while simultaneously acting as a buffer medium for the volume expansion of the silicon-based material during the charging and discharging process, thereby effectively mitigating the problem of increased secondary battery volume caused by the expansion of the silicon-based material. Furthermore, through the control of the manufacturing process, the silicon-carbon composite material V A / V B By satisfying ≥1.40, the cycling performance and initial charge / discharge efficiency of the silicon carbon composite material can be effectively improved.

[0011] In some embodiments, 1.42≤V A / V B ≤1.90.

[0012] In some embodiments, 1.50≤V A / V B ≤1.70.

[0013] In some embodiments, the grain size of the silicon-based material is ≤6 nm.

[0014] In some embodiments, the diameter of the pore structure is 0.5 nm to 8 nm.

[0015] In some embodiments, the pore structure includes micropores with a diameter of 0.5 nm or more and less than 2 nm, and mesopores with a diameter of 2 nm to 8 nm.

[0016] In some embodiments, the micropores account for 60%-90% of the quantity ratio in the pore structure.

[0017] In some embodiments, the specific surface area of ​​the silicon-carbon composite material is 2 m² 2 / g-10m 2 / g is.

[0018] In some embodiments, the silicon carbon composite material has at least one of the following features:

[0019] (1) The above silicon-based material comprises a silicon monomer;

[0020] (2) The shape of the silicon-based material includes one or more of spherical, pseudo-spherical, plate-like, and linear shapes;

[0021] (3) The specific surface area of ​​the carbon matrix is ​​1000 m² 2 / g-2000m 2 / g and;

[0022] (4) The mass ratio of the silicon-based material in the silicon-carbon composite material is 35%-60%;

[0023] (5) The volume distribution particle size (Dv50) of the silicon carbon composite material is 3μm-15μm;

[0024] (6) The volume distribution particle size (Dv90) of the silicon carbon composite material is less than or equal to 50 μm;

[0025] (7) The silicon carbon composite material satisfies 1 ≤ (Dv90 - Dv10) / Dv50 ≤ 3;

[0026] (8) The tap density of the silicon-carbon composite material is 0.8 g / cm³ 3 -1.2g / cm 3 And;

[0027] (9) The above silicon carbon composite material has a powder resistivity of less than or equal to 5 Ω·m at 16 MPa.

[0028] In some embodiments, a carbon coating layer is further included on at least a portion of the outer surface of the silicon-carbon composite material.

[0029] In some embodiments, the carbon coating layer has at least one of the following features:

[0030] (1) The material of the carbon coating layer above includes amorphous carbon;

[0031] (2) The thickness of the carbon coating layer is 50 nm to 200 nm.

[0032] A second aspect of the present application provides a method for manufacturing a silicon-carbon composite material:

[0033] Step of manufacturing a carbon substrate;

[0034] A step of obtaining a carbon matrix (A) having a pore structure by performing a pore-forming treatment on the carbon substrate;

[0035] A step of obtaining a carbon matrix (B) having a pore structure by performing a diameter control treatment on the carbon matrix (A) having a pore structure;

[0036] The method includes the step of manufacturing the silicon-carbon composite material by depositing a silicon-based material within the pore structure of a carbon matrix (B) having a pore structure; wherein the silicon-carbon composite material is charged and discharged using a button cell, and a relationship curve is drawn between the voltage (V) and the differential value (dQ / dV) obtained by differentiating the charge / discharge capacity (Q) with respect to the charge / discharge curve of the button cell, and the maximum value of the differential value (dQ / dV) between 0.26V and 0.35V is V A Record as, and the maximum value of the derivative (dQ / dV) between 0.42V and 0.52V is V B If recorded as such, the above silicon-carbon composite material is V A / V B Satisfies ≥1.40.

[0037] In some embodiments, the step of manufacturing the carbon substrate includes the step of manufacturing the carbon substrate by first sintering a carbon material precursor.

[0038] In some embodiments, the manufacture of the carbon substrate satisfies at least one of the following conditions:

[0039] (1) The temperature of the first sintering treatment above is 400℃-800℃;

[0040] (2) The time for the first sintering treatment above is 1h-12h;

[0041] (3) The atmosphere of the above first sintering treatment includes an inert gas;

[0042] (4) The inert gas comprises one or more of nitrogen and argon;

[0043] (5) The above carbon material precursor includes one or more of resinous carbon materials and biomass carbon materials.

[0044] In some embodiments, the pore-forming treatment step includes the step of alkaline etching of the carbon substrate with an alkaline substance.

[0045] In some embodiments, the pore-forming treatment satisfies at least one of the following conditions:

[0046] (1) The above alkaline substance comprises one or more of potassium hydroxide and sodium hydroxide;

[0047] (2) The mass ratio of the alkaline substance to the carbon substrate is (2-6):1.

[0048] In some embodiments, the aperture control processing step includes placing the carbon matrix (A) having the pore structure in a mixed gas containing a first carbon source and an inert gas, and performing a first vapor deposition.

[0049] In some embodiments, the temperature of the primary vapor deposition is 800℃-1000℃.

[0050] In some embodiments, the temperature of the first vapor deposition is 850℃-950℃.

[0051] In some embodiments, the time of the first vapor deposition is 1h-4h.

[0052] In some embodiments, the volume ratio of the first carbon source to the inert gas is (2-5):10.

[0053] In some embodiments, the primary vapor deposition further comprises at least one of the following conditions:

[0054] (1) The first carbon source comprises one or more of methane, ethylene and acetylene;

[0055] (2) The inert gas above includes one or more of nitrogen and argon.

[0056] In some embodiments, the carbon matrix (B) having the above-mentioned porous structure is placed in a mixed gas containing a silicon source and an inert gas, and a secondary vapor deposition is performed.

[0057] In some embodiments, the temperature of the secondary vapor deposition is 450℃-650℃.

[0058] In some embodiments, the temperature of the secondary vapor deposition is 500℃-600℃.

[0059] In some embodiments, the time of the secondary vapor deposition is 4h-8h.

[0060] In some embodiments, the secondary vapor deposition comprises at least one of the following conditions:

[0061] (1) The volume ratio of the silicon source in the mixed gas is 10%-40%;

[0062] (2) The volume ratio of the inert gas in the mixture is 60%-90%.

[0063] In some embodiments, the secondary vapor deposition further comprises at least one of the following conditions:

[0064] (1) The difference between the pressure of the second vapor deposition and the atmospheric pressure is 0.2KPa-0.6KPa;

[0065] (2) The silicon source comprises one or more of monosilane, disilane and trisilane;

[0066] (3) The inert gas above includes one or more of nitrogen and argon.

[0067] In some embodiments, prior to the aperture adjustment processing step,

[0068] The method further includes a step of removing the alkaline substance remaining on the carbon substrate with an acidic substance after the pore formation treatment.

[0069] In some embodiments, the manufacturing method is,

[0070] The method further includes the step of placing the silicon carbon composite material in a mixed gas containing a second carbon source and an inert gas, and performing a third vapor deposition to form a carbon coating layer on at least a portion of the outer surface of the silicon carbon composite material.

[0071] In some embodiments, the tertiary vapor deposition satisfies at least one of the following conditions:

[0072] (1) The second carbon source comprises one or more of methane, ethylene and acetylene;

[0073] (2) The inert gas comprises one or more of nitrogen and argon;

[0074] (3) The volume ratio of the second carbon source in the mixed gas is 5%-20%;

[0075] (4) The temperature of the above 3rd vapor deposition is 500℃-700℃;

[0076] (5) The time for the third vapor deposition above is 1h-6h.

[0077] A third aspect of the present application provides a secondary battery comprising a negative electrode plate, wherein the negative electrode plate comprises a silicon-carbon composite material of the first aspect of the present application or a silicon-carbon composite material manufactured by the method of the second aspect of the present application.

[0078] The fourth aspect of the present application provides an electric device comprising the secondary battery of the third aspect of the present application. Effects of the invention

[0079] In the silicon-carbon composite material of the present application, at least a portion of the silicon-based material is distributed within the pore structure of the carbon matrix, and the carbon matrix can improve the conductivity of the silicon-based material while simultaneously acting as a buffer medium for the volume expansion of the silicon-based material during the charging and discharging process, thereby effectively mitigating the problem of increased secondary battery volume caused by the expansion of the silicon-based material. Furthermore, through the control of the manufacturing process, the silicon-carbon composite material V A / V B By satisfying ≥1.40, the cycling performance and initial charge / discharge efficiency of the silicon carbon composite material can be effectively improved. Brief explanation of the drawing

[0080] To more clearly explain the technical solution of the present application, the drawings used in the present application are briefly introduced. It is obvious that the drawings described below are merely partial embodiments of the present application, and a person skilled in the art may derive other drawings from these drawings without striving to create an inventive step. FIG. 1 is a schematic diagram of a secondary battery of an embodiment of the present application. FIG. 2 is an exploded view of a secondary battery of an embodiment of the present application shown in FIG. 1. FIG. 3 is a schematic diagram of an electric device using a secondary battery as a power source according to the embodiment of the present application. Figure 4 is a cross-sectional SEM image of a cathode plate made of a silicon-carbon composite material according to the embodiment of the present application. Figure 5 is a curve showing the relationship between the differential value (dQ / dV) and the operating electrode potential (V) of a battery cell made of the silicon-carbon composite material of Example 3. Specific details for implementing the invention

[0081] To aid in understanding the present application, the application is described in more detail below with reference to the relevant drawings. The drawings present preferred embodiments of the present application. However, the present application may be embodied in various forms and is not limited to the embodiments described herein. Rather, the purpose of providing these embodiments is to enable a more thorough and comprehensive understanding of the disclosure of the present application.

[0082] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by a person skilled in the art to which this application pertains. The terms used in the specification of this application are for the purpose of describing specific embodiments only and are not intended to limit this application.

[0083] The technical features described as open in this application include not only closed technical solutions composed of the listed features, but also open technical solutions that include the listed features.

[0084] With respect to numerical ranges in this application, unless otherwise specified, said numerical ranges are considered continuous and include the minimum and maximum values ​​of the range and all values ​​between these minimum and maximum values. Furthermore, if a range implies integers, it includes all integers between the minimum and maximum values ​​of the range. Additionally, if multiple ranges are provided when describing a feature or characteristic, such ranges may be merged. In other words, unless otherwise specified, all ranges disclosed in the text should be understood to include any and all sub-ranges contained therein.

[0085] In relation to the units of the data range in this application, if a unit is indicated only at the right end point, it indicates that the units of the left end point and the right end point are the same. For example, 10-1000 nm means that the units of the left end point "10" and the right end point "1000" are both nm (nanometers).

[0086] In this application, when terms such as "multiple," "various," or "multiple times" are mentioned, unless specifically limited, they mean that they are quantitatively greater than or equal to 2. For example, "various" indicates two or more. Only certain numerical ranges have been specifically disclosed in the text. However, any lower limit may be combined with any upper limit to form an unspecified range; any lower limit may be combined with another lower limit to form an unspecified range, and likewise, any upper limit may be combined with another upper limit to form an unspecified range. Furthermore, each individually disclosed point or individual numerical value itself may serve as a lower limit or an upper limit and may be combined with any other point or individual numerical value, or combined with another lower limit or upper limit, to form an unspecified range.

[0087] The "range" disclosed in this application is defined in the form of a lower limit and an upper limit, and a given range is defined by selecting the lower limit and the upper limit, wherein the selected lower limit and the upper limit define the boundaries of a specific range. A range defined in this manner may or may not include a single value.

[0088] The temperature parameters of the present application allow for constant temperature processing as well as processing within a constant temperature range, without specific limitations. The constant temperature processing allows for temperature fluctuation within the accuracy range of the equipment control.

[0089] Unless otherwise specified, all embodiments and optional embodiments of this application may be combined with one another to form a new technical solution. Unless otherwise specified, all technical features and optional technical features of this application may be combined with one another to form a new technical solution.

[0090] Unless otherwise specified, all steps of the present application may proceed in order or randomly, but are preferably proceeded in order.

[0091] Silicon-containing materials are widely used in secondary batteries, but silicon has high expansion characteristics and poor conductivity; therefore, in related technologies, secondary batteries using silicon-containing materials face problems of reduced expansion and circulation performance while simultaneously increasing energy density.

[0092] Based on the above-mentioned problem, the present application provides a silicon-carbon composite material, wherein the silicon-carbon composite material comprises a carbon matrix having a porous structure and a silicon-based material distributed in the porous structure, and the porous structure provides an expansion space for the silicon-based material, thereby mitigating the problem of increased secondary battery volume due to the expansion of the silicon-based material; furthermore, to explore the circulation performance of the silicon-carbon composite material, V A / V B By selecting silicon carbon composite materials with a value ≥1.4, the recycling performance of silicon carbon composite materials can be significantly improved.

[0093] The first aspect of the present application provides a silicon-carbon composite material comprising a carbon matrix and a silicon-based material; the carbon matrix has a porous structure, and the silicon-based material is distributed within the porous structure of the carbon matrix; charging and discharging are performed using a button cell, and a relationship curve is plotted between the voltage (V) and the differential value (dQ / dV) obtained by differentiating the charge / discharge capacity (Q) with respect to the charge / discharge curve of the button cell, such that the maximum value of the differential value (dQ / dV) between 0.26 volts (V) and 0.35 volts is V A Record as, and the maximum value of the derivative (dQ / dV) between 0.42 volts and 0.52 volts is V B If recorded as such, the above silicon-carbon composite material is V A / V B Satisfies ≥1.40.

[0094] The carbon matrix of the present application refers to a carbon-based material having a porous structure on its outer surface and / or inside, and the number of porous structures contained in the carbon matrix may be one or multiple. The silicon-carbon composite material comprises a silicon-based material distributed in the porous structure of the carbon matrix and may further comprise a silicon-based material distributed on the surface of a support of the carbon matrix.

[0095] For reference, when drawing a relationship curve between the differential value (dQ / dV) obtained by differentiating the charge / discharge capacity (Q) with respect to the operating electrode potential (V) and the operating electrode potential (V), a curve of voltage (V) and charge / discharge capacity (Q) can be obtained according to the button cell manufacturing method and test method, and then the curve can be differentially integrated. Here, the button cell is composed of an operating electrode having the silicon carbon composite material of the present application as an active material, a counter electrode composed of metallic lithium, and a lithium ion electrolyte, and the voltage is 0.005V-2.0V and the current is 0.1C.

[0096] As can be understood, the silicon-carbon composite material of the present application comprises a carbon matrix having a porous structure and a silicon-based material distributed within the porous structure, wherein the carbon matrix improves the conductivity of the silicon-based material while acting as a buffer medium for the volume expansion of the silicon-based material during the charging and discharging process, thereby effectively mitigating the problem of increased secondary battery volume due to the expansion of the silicon-based material, and furthermore, through the control of the manufacturing process, the silicon-carbon composite material V A / V B By satisfying ≥1.40, the cycling performance and initial charge / discharge efficiency of the silicon carbon composite material can be effectively improved.

[0097] In some embodiments, 1.40≤V A / V B ≤1.90 and; for example, V A / V B is 1.40, 1.41, 1.42, 1.43, 1.44, 1.45, 1.46, 1.47, 1.48, 1.49, 1.5, 1.51, 1.52, 1.53, 1.54, 1.55, 1.56, 1.57, 1.58, 1.59, 1.6, 1.61, 1.62, 1.63, 1.64, 1.65, 1.66, 1.67, 1.68, 1.69, 1.7, 1.71, 1.72, 1.73, 1.74, 1.75, 1.76, 1.77, 1.78, 1.79, 1.8, It may be one of 1.81, 1.82, 1.83, 1.84, 1.85, 1.86, 1.87, 1.88, 1.89, or 1.9, or a range between any two of the above values, but is not limited thereto.

[0098] For example, V A / V BRain is 1.40-1.88, 1.40-1.85, 1.40-1.73, 1.40-1.68, 1.40-1.60, 1.42-1.90, 1.45-1.90, 1.45-1.85, 1.45-1.8, 1.45-1.75, 1.45-1.7, 1.45-1.65, 1.65-1.9, 1.65-1.85, 1.65-1.8, 1.5-1.7, 1.51-1.69, 1.52-1.68, 1.53-1.67, 1.54-1.66, 1.55-1.65, 1.56-1.64, It may be 1.57-1.63, 1.58-1.62, or 1.59-1.61, etc., but is not specifically limited.

[0099] In some optional embodiments, 1.50≤V A / V B ≤1.70.

[0100] In some embodiments, the grain size of the silicon-based material is ≤6 nm; if the grain size of the silicon-based material exceeds the above range, the grain size of the silicon-based material may become too large during the cycle, which may cause the collapse of the silicon-carbon composite material structure. For example, the grain size of the silicon-based material may be one of 0.01 nm, 0.05 nm, 0.1 nm, 0.5 nm, 1 nm, 1.5 nm, 2 nm, 2.5 nm, 3 nm, 3.5 nm, 4 nm, 4.5 nm, 5 nm, 5.5 nm, or 6 nm, or may be a range between any two of the above values, but is not limited thereto. Optionally, the grain size of the silicon-based material is 1 nm to 4 nm.

[0101] For example, the grain size of the aforementioned silicon-based material can be calculated using an X-ray diffraction pattern or by performing a characterization analysis through a transmission electron microscope, or the size of the silicon-based material can be obtained.

[0102] In some embodiments, the silicon-based material includes a silicon monomer.

[0103] In some embodiments, the shape of the silicon-based material includes one or more of spherical, quasi-spherical, plate-like, and linear.

[0104] In some embodiments, the diameter of the pore structure of the carbon matrix is ​​0.5 nm to 8 nm; when the diameter of the pore structure of the carbon matrix is ​​within the above range, the silicon-based material deposited within the pore structure may have a relatively uniform size and the probability of depositing a large silicon-based material may be reduced. For example, the diameter of the pore structure of the carbon matrix may be one of 0.5 nm, 1 nm, 2 nm, 2.5 nm, 3 nm, 3.5 nm, 4 nm, 4.5 nm, 5 nm, 5.5 nm, 6 nm, 6.5 nm, 7 nm, 7.5 nm, or 8 nm, or may be a range between any two of the above values, but is not limited thereto. Optionally, the diameter of the pore structure of the carbon matrix is ​​0.5 nm to 6 nm.

[0105] For reference, if the carbon matrix has only a single pore structure, the pore diameter is the diameter of that single pore structure; if the carbon matrix has multiple pore structures, the pore diameter refers to the average diameter of the pore structures.

[0106] In some embodiments, the pore structure of the carbon matrix comprises micropores with a diameter of 0.5 nm or more and less than 2 nm and mesopores with a diameter of 2 nm to 8 nm; optionally, the pore structure of the carbon matrix comprises micropores with a diameter of 0.5 nm or more and less than 2 nm and mesopores with a diameter of 2 nm to 6 nm.

[0107] In some embodiments, the quantity ratio of micropores in the pore structure is 60%-90%; for example, it may be one of 60%, 63%, 65%, 68%, 70%, 72%, 75%, 78%, 80%, 83%, 85%, 88%, or 90%, or a range between any two of the above values, but is not limited thereto. When the quantity ratio of micropores in the pore structure is within the above range, the probability of large silicon-based material being deposited can be further reduced, V A / V B It is more advantageous for controlling the size. Optionally, the quantity ratio of micropores in the pore structure is 70%-80%.

[0108] As a possible embodiment, the specific surface area of ​​the carbon matrix is ​​1000 m² 2 / g-2000m 2 / g; if the specific surface area of ​​the carbon matrix is ​​below the above range, silicon can be easily deposited on the surface of the carbon matrix; and if the specific surface area of ​​the carbon matrix exceeds the above range, the amount of silicon deposited becomes too large, causing the silicon volume to expand excessively during the cycle, which may lead to the collapse of the carbon matrix. For example, the specific surface area of ​​the carbon matrix is ​​1000m² 2 / g, 1100m 2 / g, 1200m 2 / g, 1300m 2 / g, 1400m 2 / g, 1500m 2 / g, 1600m 2 / g, 1700m 2 / g, 1800m 2 / g, 1900m 2 / g, 2000m 2 It may be one of / g or a range between any two of the above values, but is not limited thereto. Optionally, the specific surface area of ​​the carbon matrix is ​​1300 m² 2 / g-2000m 2 / g. In some embodiments, the mass ratio of silicon-based material in the silicon-carbon composite material is 35%-60%; if the mass ratio of silicon-based material in the silicon-carbon composite material is less than the above range, the capacity and initial charge / discharge efficiency of the silicon-carbon composite material may be too low; and if the mass ratio of silicon-based material in the silicon-carbon composite material exceeds the above range, the cycling performance of the silicon-carbon composite material may be poor. For example, the mass proportion of silicon-based material in the silicon-carbon composite material may be one of 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, or 60%, or a range between any two of the above values, but is not limited thereto. Optionally, the mass proportion of silicon-based material in the silicon-carbon composite material is 40%-55%.

[0109] For example, the mass ratio of silicon-based materials in a silicon-carbon composite material can be measured using inductively coupled plasma (ICP) emission spectroscopy.

[0110] In some embodiments, the volume distribution particle size (Dv50) of the silicon carbon composite material is 3μm to 15μm; if the volume distribution particle size (Dv50) of the silicon carbon composite material exceeds the above range, the kinetic characteristics of the secondary battery are prone to deterioration; and if the volume distribution particle size (Dv50) of the silicon carbon composite material is less than the above range, a problem of non-uniform deposition of silicon-based material in the carbon matrix may occur. For example, the volume distribution particle size (Dv50) of the silicon carbon composite material may be one of 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, 16μm, 17μm, 18μm, 19μm, 20μm, or a range between any two of the above values, but is not limited thereto. Optionally, the volumetric distribution particle size (Dv50) of the silicon carbon composite material is 5 μm–13 μm.

[0111] In some embodiments, the volume distribution particle size (Dv90) of the silicon carbon composite material is less than or equal to 50 μm; if the volume distribution particle size (Dv90) of the silicon carbon composite material exceeds the above range, the cathode reagent bottle may penetrate the separator. For example, the volume distribution particle size (Dv90) of the silicon carbon composite material may be one of 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, or 50 μm, or a range between any two of the above values, but is not limited thereto. Optionally, the volume distribution particle size (Dv90) of the silicon carbon composite material is 20 μm-40 μm.

[0112] In some embodiments, the silicon-carbon composite material satisfies 1 ≤ (Dv90 - Dv10) / Dv50 ≤ 3; when the silicon-carbon composite material satisfies the above condition, it helps improve the compaction density of the cathode plate. For example, (Dv90 - Dv10) / Dv50 may be one of 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3, or a range between any two of the above values, but is not limited thereto. Optionally, 1 ≤ (Dv90 - Dv10) / Dv50 ≤ 2.

[0113] The Dv10, Dv50, and Dv90 of the material have meanings known in the art and can be measured by methods known in the art. For example, they can be measured using a laser particle size analyzer (e.g., Malvern Master Size 3000) by referring to the standard GB / T 19077-2016.

[0114] Here, the physical definitions of Dv10, Dv50, and Dv90 are as follows:

[0115] Dv10: The particle size corresponding when the cumulative volume distribution percentage of the material reaches 10%;

[0116] Dv50: The particle size corresponding when the cumulative volume distribution percentage of the material reaches 50%;

[0117] Dv90: The particle size corresponding when the cumulative volume distribution percentage of the material reaches 90%.

[0118] As a possible embodiment, the specific surface area of ​​the silicon-carbon composite material is 2 m² 2 / g- 20m 2 / g; if the specific surface area of ​​the silicon-carbon composite material exceeds the above range, it may lead to a decrease in the initial charge-discharge efficiency of the secondary battery. For example, the specific surface area of ​​the silicon-carbon composite material is 2m² 2 / g, 3m 2 / g, 4m2 / g, 5m 2 / g, 6m 2 / g, 7m 2 / g, 8m 2 / g, 9m 2 / g, 10m 2 / g, 11m 2 / g, 12m 2 / g, 13m 2 / g, 14m 2 / g, 15m 2 / g, 16m 2 / g, 17m 2 / g, 18m 2 / g, 19m 2 / g, 20m 2 It may be one of / g or a range between any two of the above values, but is not limited thereto. Optionally, the specific surface area of ​​the silicon-carbon composite material is 2m² 2 / g- 6m 2 / g is.

[0119] For example, the diameter of the pore structure of the carbon matrix mentioned above and the specific surface area of ​​the silicon-carbon composite material both have meanings known in the art and can be measured by methods known in the art. For example, by referring to GB / T 19587-2017, the nitrogen adsorption specific surface area analysis test method can be used to measure and the BET (Brunauer Emmett Teller) method can be used to calculate the specific surface area. The nitrogen adsorption specific surface area analysis test can be performed using the Tri-Star 3020 specific surface area diameter analysis tester from Micromeritics, USA.

[0120] In some possible embodiments, the tap density of the silicon-carbon composite material is 0.8 g / cm³ 3 -1.2g / cm 3 And; for example, the tap density of the silicon-carbon composite material is 0.8 g / cm³ 3 , 0.83g / cm 3 , 0.85g / cm 3 , 0.87g / cm 3 , 0.9g / cm3 , 0.92g / cm 3 , 0.95g / cm 3 , 0.98g / cm 3 , 1g / cm 3 , 1.02g / cm 3 , 1.05g / cm 3 , 1.08g / cm 3 , 1.1g / cm 3 , 1.12g / cm 3 , 1.15g / cm 3 , 1.18g / cm 3 , 1.2g / cm 3 It may be one of the above, or a range between any two values, but is not limited thereto. Optionally, the tap density of the silicon-carbon composite material is 0.85 g / cm³ 3 -1g / cm 3 am.

[0121] For reference, the tap density of the aforementioned silicon-carbon composite material refers to the mass per unit volume measured after the silicon-carbon composite material powder inside the container is tapped under specified conditions.

[0122] The tap density of the cathode active material has a meaning known in the art and can be measured by methods known in the art. For example, it can be measured using a powder tap density tester by referring to the standard GB / T 5162-2006. When using the FZS4-4B type tap densimeter of the Beijing Institute of Steel Research, the test parameters are as follows: vibration frequency: 250±15 times / min, amplitude: 3±0.2mm, number of vibrations: 5000 times, measuring cylinder: 25 mL.

[0123] In some embodiments, the silicon-carbon composite material has a powder resistivity of 5 Ω·m or less at 16 MPa; since the silicon-carbon composite material has excellent conductivity, it helps to improve the kinetic performance of the battery. Optionally, the silicon-carbon composite material has a powder resistivity of less than or equal to 2 Ω·m at 16 MPa.

[0124] For example, the powder resistivity of the aforementioned silicon carbon composite material at 16 MPa can be measured by the following method: a suitable amount of the sample to be measured is placed into the sample input cup of a resistivity meter and pressure is applied, and data is collected manually to record the powder resistivity test results at different pressure points, wherein the test pressure is 16 MPa.

[0125] In some embodiments, the initial charge-discharge cycling efficiency of the silicon carbon composite material is ≥90%; optionally, the initial charge-discharge cycling efficiency of the silicon carbon composite material is 92%-95%.

[0126] For example, the initial charge-discharge cycling efficiency of the aforementioned silicon-carbon composite material can be measured by the following method:

[0127] A button cell is constructed using a negative plate manufactured as a sample to be measured as the working electrode, metallic lithium as the counter electrode, and an electrolyte containing a lithium ion conductive material, and the button cell is left for 60 minutes, then discharged to 5mV with a constant current of 0.05C, then discharged to 5mV with 50μA, then left for 10 minutes, and then charged to 2.0V with 0.1C to conduct the test, wherein the lithium detachment capacity at 2.0V represents the capacity size of the sample, and the corresponding initial charge / discharge efficiency = 2.0V lithium detachment capacity / lithium insertion capacity.

[0128] In some embodiments, a carbon coating layer is further included on at least a portion of the outer surface of the silicon-carbon composite material. By installing the carbon coating layer, contact between the silicon-based material and the electrolyte is reduced, and side reactions of the battery are lowered, thereby improving the circulation performance of the battery.

[0129] For reference, the carbon coating layer may be a continuous and complete coating layer or an incomplete coating layer; where "complete" means that the material located inside the carbon coating layer is completely coated by the carbon coating layer, so that the carbon coating layer completely isolates the internal material from the outside. "Incomplete" means that the material located inside the carbon coating layer is not completely coated by the carbon coating layer, so that at least a portion of the internal material may come into contact with the outside of the carbon coating layer. Preferably, the carbon coating layer is a continuous and complete coating layer.

[0130] For example, a cross-sectional SEM image of a cathode plate made of the silicon-carbon composite material of the present application is shown in FIG. 4, and a uniform carbon coating layer (412) is further coated on the outside of the carbon matrix (411) to prevent exposure of the carbon matrix and reduce the reaction between the silicon-based material and the electrolyte.

[0131] In some embodiments, the material of the carbon coating layer includes amorphous carbon; the amorphous carbon acts as a fast ion circulation ring to improve the kinetic performance of the silicon-carbon composite material and can reduce contact between the silicon-based material and the electrolyte.

[0132] In some embodiments, the thickness of the carbon coating layer is 50 nm to 200 nm; if the thickness of the carbon coating layer is less than the above range, the silicon-based material may be exposed and affect processing performance; and if the thickness of the carbon coating layer exceeds the above range, the capacity of the secondary battery may decrease. For example, the thickness of the carbon coating layer may be one of 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 110 nm, 120 nm, 130 nm, 140 nm, 150 nm, 160 nm, 170 nm, 180 nm, 190 nm, or 200 nm, or may be a range between any two of the above values, but is not limited thereto.

[0133] For example, the thickness of the carbon coating layer mentioned above can be measured using a transmission electron microscope.

[0134] A second aspect of the present application provides a method for manufacturing a silicon-carbon composite material comprising: a step of manufacturing a carbon substrate; a step of performing a pore-forming treatment on the carbon substrate to obtain a carbon matrix (A) having a pore structure; a step of performing a diameter-regulating treatment on the carbon matrix (A) having a pore structure to obtain a carbon matrix (B) having a pore structure; and a step of manufacturing a silicon-carbon composite material by depositing a silicon-based material within the pore structure of the carbon matrix (B) having a pore structure; wherein the silicon-carbon composite material is charged and discharged using a button cell, and a relationship curve is drawn between the voltage (V) and the differential value (dQ / dV) obtained by differentiating the charge / discharge capacity (Q) with respect to the charge / discharge curve of the button cell, and the maximum value of the differential value (dQ / dV) between 0.26V and 0.35V is V A Record as, and the maximum value of the derivative (dQ / dV) between 0.42V and 0.52V is V B If recorded as such, the above silicon-carbon composite material is V A / V B Satisfies ≥1.40.

[0135] In some embodiments, the step of manufacturing a carbon substrate includes the step of manufacturing a carbon substrate by performing a primary sintering treatment on a carbon material precursor.

[0136] As a possible embodiment, the temperature of the first sintering treatment is 400℃-800℃, and may be, for example, one of 400℃, 430℃, 450℃, 480℃, 500℃, 530℃, 550℃, 570℃, 600℃, 630℃, 650℃, 680℃, 700℃, 730℃, 750℃, 770℃, 800℃, or a range between any two of the above values, but is not limited thereto. The time of the first sintering treatment is 1h-12h; for example, one of 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, or a range between any two of the above values, but is not limited thereto. The atmosphere of the primary sintering treatment includes an inert gas; optionally, the inert gas includes one or more of nitrogen and argon.

[0137] As a possible embodiment, the carbon material precursor comprises one or more of resinous carbon materials and biomass carbon materials.

[0138] Optionally, the resinous carbon material comprises one or more of phenolic resin, epoxy resin, urea formaldehyde resin, and furan resin.

[0139] Optionally, the biomass carbon material includes one or more of coconut shells, lignin, bamboo powder, and starch.

[0140] For reference, bamboo powder refers to powder manufactured using bamboo as a raw material.

[0141] In some embodiments, the pore formation treatment step includes the step of alkaline etching of a carbon substrate with an alkaline substance.

[0142] In some optional embodiments, the alkaline substance comprises one or more of potassium hydroxide and sodium hydroxide.

[0143] In some optional embodiments, the mass ratio of the alkaline material to the carbon substrate is (2-6):1; exemplarily, the mass ratio of the alkaline material to the carbon substrate may be one of 2:1, 2.5:1, 3:1, 3.5:1, 4:1, 4.5:1, 5:1, 5.5:1, 6:1, or a range between any two of the above ratios, but is not limited thereto.

[0144] As a possible embodiment, the following step is further included prior to the diameter control treatment step: removing alkaline substances remaining on the carbon substrate after the pore formation treatment with an acidic substance. Optionally, the acidic substance comprises hydrochloric acid.

[0145] In some embodiments, the aperture control treatment step includes placing a carbon matrix (A) having a porous structure in a mixed gas containing a first carbon source and an inert gas, and performing a first vapor deposition.

[0146] The diameter of the carbon substrate is controlled by depositing a first carbon source using a vapor deposition method, and when the volume ratio of the first carbon source to the inert gas during vapor deposition is (2-5):10, the diameter of the carbon substrate can be reduced to prevent the deposition of large silicon-based materials.

[0147] In some optional embodiments, the temperature of the first vapor deposition is 800°C to 1000°C; for example, it may be one of 800°C, 810°C, 820°C, 830°C, 840°C, 850°C, 860°C, 870°C, 880°C, 890°C, 900°C, 910°C, 920°C, 930°C, 940°C, 950°C, 960°C, 970°C, 980°C, 990°C, 1000°C, or a range between any two of the above values, but is not limited thereto. When the temperature of the first vapor deposition is in the above range, the decomposition of the carbon source is easy, which is advantageous for aperture control. For example, the temperature of the first vapor deposition may be 810°C-990°C, 820°C-980°C, 830°C-970°C, 840°C-960°C, 850°C-950°C, 860°C-940°C, 870°C-930°C, or 880°C-920°C, but is not specifically limited. Optionally, the temperature of the first vapor deposition is 850°C-950°C.

[0148] In some optional embodiments, the time of the first vapor deposition is 1h-4h; for example, one of 1h, 1.2h, 1.5h, 1.8h, 2h, 2.3h, 2.5h, 2.8h, 3h, 3.3h, 3.5h, 3.7h, 4h, or a range between any two of the above values, but is not limited thereto. When the time of the first vapor deposition is within the above range, it is advantageous for adjusting the aperture to an appropriate size and controlling the ratio of micropores to mesopores within the pore structure. Optionally, the time of the first vapor deposition is 1.5h-3h.

[0149] In some optional embodiments, the volume ratio of the first carbon source to the inert gas is (2-5):10; when the volume ratio of the first carbon source to the inert gas is within the above range, it is advantageous for controlling the diameter of the carbon matrix pore structure more uniformly. For example, the volume ratio of the first carbon source to the inert gas may be one of 2:10, 2.3:10, 2.5:10, 2.8:10, 3:10, 3.2:10, 3.5:10, 3.8:10, 4:10, 4.3:10, 4.5:10, 4.8:10, 5:10, or a range between any two of the above ratios, but is not limited thereto. Optionally, the volume ratio of the first carbon source to the inert gas is (2.5-4):10.

[0150] For reference, the temperature, time, and volume ratio of the first carbon source and the inert gas of the first vapor deposition all affect the aperture size of the pore structure, and the aperture size of the pore structure is V A / V B Affecting the value, by controlling the temperature and time of the first vapor deposition and the volume ratio of the first carbon source to the inert gas, V A / V B It is advantageous for further adjusting the value to an appropriate range; specifically, if the temperature of the primary vapor deposition is low, V A / V B The value generally decreases; if the time of the first vapor deposition is short, V A / V B The value generally decreases; if the volume ratio of the first carbon source to the inert gas is small, V A / V B The value generally becomes smaller.

[0151] In some optional embodiments, the first carbon source comprises one or more of methane, ethylene, and acetylene.

[0152] In some optional embodiments, the inert gas comprises one or more of nitrogen and argon.

[0153] In some embodiments, a carbon matrix (B) having a porous structure is placed in a mixed gas containing a silicon source and an inert gas, and a secondary vapor deposition is performed to deposit a silicon-based material into the porous structure of the carbon matrix; by depositing the silicon-based material into the porous structure using a vapor deposition method, the ratio of silicon-based material inserted into the porous structure can be increased.

[0154] In some optional embodiments, the temperature of the secondary vapor deposition is 450°C–650°C; for example, it may be one of 450°C, 460°C, 470°C, 480°C, 490°C, 500°C, 510°C, 520°C, 530°C, 540°C, 550°C, 560°C, 570°C, 580°C, 590°C, 600°C, 610°C, 620°C, 630°C, 640°C, or a range between any two of the above values, but is not limited thereto. When the temperature of the secondary vapor deposition is in the above range, it is advantageous to control the mass ratio of the silicon-based material in the silicon-carbon composite material to within an appropriate range; if the temperature of the secondary vapor deposition is too high, the silicon-based material is prone to crystallization, which affects the cycling performance of the battery; If the temperature of the secondary vapor deposition is too low, the decomposition efficiency of the silicon source is reduced. For example, the temperature of the secondary vapor deposition may be 460°C-640°C, 470°C-630°C, 480°C-620°C, 490°C-610°C, 500°C-600°C, 510°C-590°C, 520°C-580°C, or 530°C-570°C, but is not specifically limited. Optionally, the temperature of the secondary vapor deposition is 500°C-600°C; more optionally, the temperature of the secondary vapor deposition is 520°C-580°C.

[0155] In some optional embodiments, the time of the secondary vapor deposition is 4h to 8h; for example, it may be one of 4h, 4.2h, 4.5h, 4.8h, 5h, 5.2h, 5.5h, 5.8h, 6h, 6.3h, 6.5h, 6.7h, 7h, 7.3h, 7.5h, 7.7h, 8h, or a range between any two of the above values, but is not limited thereto. When the time of the secondary vapor deposition is within the above range, it is advantageous for controlling the mass ratio of the silicon-based material in the silicon-carbon composite material; if the time of the secondary vapor deposition is too long, the silicon-based material may easily accumulate excessively on the surface of the carbon matrix; and if the time of the secondary vapor deposition is too short, the amount of silicon-based material deposited is insufficient and does not meet the capacity design value. For example, the second vapor deposition time may be 4.2h-7.8h, 4.5h-7.5h, 4.8h-7.3h, 5h-7h, 5.2h-6.8h, 5.5h-6.5h, 5.8h-6.3h, etc., but is not specifically limited. Optionally, the second vapor deposition time is 4.5h-7h, and more optionally 5h-6h.

[0156] In some optional embodiments, the volume proportion of the silicon source in the mixed gas is 10% to 40%, and the volume proportion of the inert gas in the mixed gas is 60% to 90%. Controlling the volume proportion of the silicon source in the mixed gas within the above range is advantageous for depositing silicon-based materials of relatively uniform size. For example, the volume proportion of the silicon source in the mixed gas may be one of 10%, 15%, 20%, 25%, 30%, 35%, 40%, or a range between any two of the above values, but is not limited thereto; correspondingly, the volume proportion of the inert gas in the mixed gas may be one of 90%, 85%, 80%, 75%, 70%, 65%, 60%, or a range between any two of the above values, but is not limited thereto.

[0157] For reference, the temperature and time of the secondary vapor deposition, as well as the volume ratio of the silicon source to the inert gas, all affect the mass ratio of silicon-based materials in the silicon-carbon composite material, and the mass ratio of silicon-based materials in the silicon-carbon composite material is V A / V B By affecting the value and controlling the temperature and time of the secondary vapor deposition and the volume ratio of the silicon source to the inert gas, V A / V B It is advantageous for further adjusting the value to an appropriate range; specifically, the higher the temperature of the secondary vapor deposition, the more V A / V B The value generally decreases; as the secondary vapor deposition time increases, V A / V B The value generally decreases; as the volume ratio of the silicon source to the inert gas increases, V A / V B The value generally becomes smaller.

[0158] In some optional embodiments, the difference between the pressure of the secondary vapor deposition and the amount of atmospheric pressure is 0.2KPa-0.6KPa, and may be, for example, one of 0.2KPa, 0.25KPa, 0.3KPa, 0.35KPa, 0.4KPa, 0.45KPa, 0.5KPa, 0.55KPa, 0.6KPa, or a range between any two of the above values, but is not limited thereto.

[0159] In some optional embodiments, the silicon source comprises one or more of monosilane, disilane, and trisilane.

[0160] In some optional embodiments, the inert gas comprises one or more of nitrogen and argon.

[0161] In some embodiments, a method for manufacturing a silicon-carbon composite material further comprises the step of placing the silicon-carbon composite material in a mixed gas containing a second carbon source and an inert gas, and performing a third vapor deposition to form a carbon coating layer on at least a portion of the outer surface of the silicon-carbon composite material. By manufacturing the carbon coating layer by vapor deposition, the amount of coating can be easily controlled to improve the surface conductivity of the silicon-carbon composite material and help in the capacity development of the material, while simultaneously helping to maintain the stability and safety of the silicon-carbon composite material.

[0162] In some optional embodiments, the second carbon source comprises one or more of methane, ethylene, and acetylene.

[0163] In some optional embodiments, the inert gas comprises one or more of nitrogen and argon.

[0164] In some optional embodiments, the volume ratio of the second carbon source in the mixed gas is 5%-20%, and may be, for example, one of 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, or a range between any two of the above values, but is not limited thereto. Controlling the volume ratio of the second carbon source in the mixed gas to within the above range is advantageous for improving the uniformity of the carbon coating.

[0165] In some optional embodiments, the temperature of the tertiary vapor deposition is 500°C to 700°C, and may be, for example, one of 500°C, 510°C, 520°C, 530°C, 540°C, 550°C, 560°C, 570°C, 580°C, 590°C, 600°C, 610°C, 620°C, 630°C, 640°C, 650°C, 660°C, 670°C, 680°C, 690°C, 700°C, or a range between any two of the above values, but is not limited thereto. For example, the temperature of the tertiary vapor deposition may be 550°C to 650°C. The time for the third vapor deposition is 1h-6h, and may be one of, for example, 1h, 2h, 3h, 4h, 5h, or 6h, or may be a range between any two of the above values, but is not limited thereto.

[0166] For reference, the aforementioned "first carbon source," "second carbon source," "first vapor deposition," "second vapor deposition," "third vapor deposition," "first sintering treatment," and "second sintering treatment" are used for illustrative purposes only and should not be understood as indicating or implying relative importance or quantity, nor should they be understood as implying the importance or quantity of the indicated technical features.

[0167] In some embodiments, a method for manufacturing a silicon-carbon composite material comprises the following steps:

[0168] A step of manufacturing a carbon substrate by performing a primary sintering treatment on a carbon material precursor; wherein the temperature of the primary sintering treatment is 400℃-800℃, the sintering time is 1h-12h, and the sintering atmosphere includes an inert gas; the carbon material precursor includes one or more of a resinous carbon material and a biomass carbon material, the resinous carbon material includes one or more of a phenolic resin, an epoxy resin, a urea formaldehyde resin, and a furan resin, and the biomass carbon material includes one or more of a coconut shell, lignin, bamboo powder, and starch.

[0169] A step of preparing a carbon matrix (A) having a porous structure by alkaline etching a carbon substrate with an alkaline substance; wherein the alkaline substance comprises one or more of potassium hydroxide and sodium hydroxide; and the mass ratio of the alkaline substance to the carbon substrate is (2-6):1.

[0170] A step of removing residual alkaline substances on a carbon substrate having a porous structure using an acidic substance, followed by heating and drying; the acidic substance includes hydrochloric acid.

[0171] A carbon matrix (A) having a porous structure is placed in a mixed gas containing a first carbon source and an inert gas, and a first vapor deposition is performed to produce a carbon matrix (B) having a porous structure. Here, the first carbon source includes one or more of methane, ethylene, and acetylene. The inert gas includes one or more of nitrogen and argon. The volume ratio of the first carbon source to the inert gas is (2-5):10, and optionally (2.5-4):10. The temperature of the first vapor deposition is 800°C-1000°C, and optionally 850°C-950°C. The time of the first vapor deposition is 1h-4h, and optionally 1.5h-3h.

[0172] A carbon matrix (B) having a porous structure is placed in a mixed gas containing a silicon source and an inert gas, and a secondary vapor deposition is performed; wherein the temperature of the secondary vapor deposition is 450°C–650°C, optionally 500°C–600°C, and more optionally 520°C–580°C. The time of the secondary vapor deposition is 4h–8h; optionally 4.5h–7h, and more optionally 5h–6h. The difference between the pressure of the secondary vapor deposition and the amount of atmospheric pressure is 0.2kPa–0.6kPa. The silicon source comprises one or more of monosilane, disilane, and trisilane. The inert gas comprises one or more of nitrogen and argon. The volume ratio of the silicon source in the mixed gas is 10%–40%, and the volume ratio of the inert gas in the mixed gas is 60%–90%.

[0173] The method comprises the step of manufacturing a silicon-carbon composite material by placing a carbon matrix in a mixed gas containing a second carbon source and an inert gas, and performing a third vapor deposition to form a carbon coating layer on the outer surface of at least a portion of the carbon matrix. Here, the second carbon source comprises one or more of methane, ethylene, and acetylene. The inert gas comprises one or more of nitrogen and argon. The volume ratio of the second carbon source in the mixed gas is 5% to 20%. The temperature of the third vapor deposition is 500°C to 700°C, and optionally 550°C to 650°C. The time of the third vapor deposition is 1h to 6h.

[0174] A third aspect of the present application provides a secondary battery comprising a negative electrode plate, wherein the negative electrode plate comprises a silicon-carbon composite material of the first aspect of the present application or a silicon-carbon composite material manufactured by the method of the second aspect of the present application.

[0175] In the present application, the secondary battery using the silicon-carbon composite material has improved magnification performance and circulation performance.

[0176] Generally, a secondary battery includes a positive plate, a negative plate, an electrolyte, and a separator. During the charging and discharging process, active ions move back and forth between the positive and negative plates, undergoing insertion and extraction. The electrolyte serves to conduct ions between the positive and negative plates. The separator is installed between the positive and negative plates and primarily serves to prevent short circuits between them while allowing ions to pass through.

[0177] cathode plate

[0178] The cathode plate comprises a cathode current collector and a cathode film layer installed on at least one surface of the cathode current collector, and the cathode film layer comprises a silicon-carbon composite material of the first embodiment of the present application or a silicon-carbon composite material manufactured by the method of the second embodiment of the present application.

[0179] For example, the cathode current collector has two surfaces facing each other in the direction of its own thickness, and the cathode film layer is installed on either one or both of the two facing surfaces of the cathode current collector.

[0180] In some embodiments, the cathode current collector may use a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer material substrate and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material on a polymer material substrate. Here, the metal material includes, but is not limited to, copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, and the polymer material substrate includes, but is not limited to, polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.

[0181] In some embodiments, the negative electrode active material may simultaneously use a negative electrode active material for a battery known in the art. For example, the negative electrode active material may include at least one of materials such as synthetic graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate. The silicon-based material may be selected from at least one of monomeric silicon, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of monomeric tin, tin oxide, and tin alloys. The present application is not limited to these materials, and other traditional materials that can be used as battery negative electrode active materials may also be used. Such negative electrode active materials may be used as a single type or in combination of two or more types. The negative electrode active material accounts for 70-100 weight% of the negative electrode layer based on the total weight of the negative electrode layer.

[0182] In some embodiments, the cathode film layer may optionally include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS). The binder accounts for 0 to 30 weight percent of the cathode film layer based on the total weight of the cathode film layer.

[0183] In some embodiments, the cathode film layer may optionally include a conductive agent. The conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. The conductive agent accounts for 0-20 weight% of the cathode film layer based on the total weight of the cathode film layer.

[0184] In some embodiments, the cathode film layer may optionally further include other auxiliary agents, such as a thickener (e.g., sodium carboxymethylcellulose (CMC-Na)). The other auxiliary agents account for 0-15 weight percent of the cathode film layer based on the total weight of the cathode film layer.

[0185] In some embodiments, the cathode plate may be manufactured by the following method: components for manufacturing the cathode plate, e.g., a cathode active material, a conductive agent, a binder, and other optional components are dispersed in a solvent (e.g., deionized water) to form a cathode slurry, wherein the solid content of the cathode slurry is 30-70 wt% and the viscosity at room temperature is controlled to 2000-10000 mPa·s; the obtained cathode slurry is applied to both surfaces of a cathode current collector, and after a drying process, the cathode plate is obtained by cold pressing, for example, using a roll. The cross-sectional coverage unit areal density of the cathode powder is 75-220 mg / m² 2 and the compaction density of the cathode plate is 1.2-2.0 g / m² 3 am.

[0186] positive plate

[0187] The anode plate comprises an anode current collector and an anode film layer installed on at least one surface of the anode current collector, and the anode film layer comprises an anode active material.

[0188] For example, the positive current collector has two surfaces facing each other in the direction of its own thickness, and the positive film layer is installed on either one or both of the two facing surfaces of the positive current collector.

[0189] In some embodiments, the positive current collector may use a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material substrate and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material on a polymer material substrate. Here, the metal material includes, but is not limited to, aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. The polymer material substrate includes one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).

[0190] In some embodiments, the lithium-ion cathode active material may include a positive active material for a battery known in the art. For example, the positive active material may include at least one of a material which is a lithium-containing phosphate with an olivine structure, a lithium transition metal oxide, and a modified compound thereof. However, the present application is not limited to these materials, and other traditional materials that can be used as a positive active material for a battery may also be used. Such positive active materials may be used as a single type or in combination of two or more types. Here, examples of lithium transition metal oxides include lithium cobalt oxide (e.g., LiCoO2), lithium nickel oxide (e.g., LiNiO2), lithium manganese oxide (e.g., LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, and lithium nickel cobalt manganese oxide (e.g., LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (NCM 333 Abbreviated as ),LiNi 0.5 Co 0.2 Mn 0.3 O2 (NCM 523 Abbreviated as ), LiNi0.5 Co 0.25 Mn 0.25 O2 (NCM 211 Abbreviated as ), LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM 622 Abbreviated as ), LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM 811 Abbreviated as ), lithium nickel cobalt aluminum oxide (e.g., LiNi 0.80 Co 0.15 Al 0.05 It includes, but is not limited to, at least one of O2) and its modified compounds. Examples of lithium-containing phosphates of an olivine structure include, but are not limited to, at least one of lithium iron phosphate (e.g., LiFePO4 (abbreviated as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (e.g., LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium manganese iron phosphate, and a composite material of lithium manganese iron phosphate and carbon. The above-mentioned cathode active material accounts for 80-100% by weight of the cathode film layer based on the total weight of the cathode film layer.

[0191] In some embodiments, the anode film layer may optionally include a binder. For example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene ternary copolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene ternary copolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin. The binder accounts for 0 to 20 weight percent of the anode film layer based on the total weight of the anode film layer.

[0192] In some embodiments, the anode film layer may optionally further include a conductive agent. For example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. The conductive agent accounts for 0-20 weight% of the anode film layer based on the total weight of the anode film layer.

[0193] In some embodiments, the anode plate may be manufactured by the following method: components for manufacturing the anode plate, e.g., an anode active material, a conductive agent, a binder, and any other optional components, are dispersed in a solvent (e.g., N-methylpyrrolidone) to form an anode slurry, wherein the solid content of the anode slurry is 40-80 wt% and the viscosity at room temperature is controlled to 5000-25000 mPa·s; the anode slurry is applied to both surfaces of an anode current collector, and after drying, the anode plate is formed by cold pressing through a cold rolling mill; and the cross-sectional coating unit areal density of the anode powder is 15-35 mg / m² 2 and the compaction density of the anode plate is 3.0-3.6 g / cm³ 3 is, and optionally 3.3-3.5 g / cm³ 3 is. The calculation formula for the above compaction density is as follows:

[0194] Compaction density = Coating surface density / (Electrode plate thickness after compression - Current collector thickness).

[0195] electrolytes

[0196] The electrolyte serves to transfer ions between the positive and negative plates. This application does not impose any specific restrictions on the type of electrolyte and may be selected as necessary. For example, the electrolyte may be in a liquid state, a gel state, or a completely solid state.

[0197] In some embodiments, the electrolyte uses an electrolyte solution. The electrolyte solution comprises an electrolyte salt and a solvent.

[0198] In some embodiments, the electrolyte salt may be selected from one or more types of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethylsulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalate borate (LiDFOB), lithium dioxalate borate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorodioxalate phosphate (LiDFOP), and lithium tetrafluorooxalate phosphate (LiTFOP). The concentration of the electrolyte salt is typically 0.5-5 mol / L.

[0199] In some embodiments, the solvent may be selected from one or more types of fluorocarbonate ethylene (FEC), ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS), and diethyl sulfone (ESE).

[0200] In some embodiments, the electrolyte may optionally further include an auxiliary agent. For example, the auxiliary agent may include a negative electrode film-forming additive and a positive electrode film-forming additive, and may include an additive capable of improving specific performance of the battery, such as an additive that improves battery overcharge performance, an additive that improves battery high or low temperature performance, etc.

[0201] Separator

[0202] In some embodiments, the secondary battery further includes a separator. The present application does not impose any particular limitation on the type of separator, and any known porous structure separator having good chemical stability and mechanical stability may be selected and used.

[0203] In some embodiments, the material of the separator may be selected from at least one of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene difluoride. The separator may be a single-layer thin film or a multilayer composite thin film, and there are no particular limitations. If the separator is a multilayer composite thin film, the material of each layer may be the same or different, and there are no particular limitations.

[0204] In some embodiments, the thickness of the separator is 6-40 μm, and optionally 12-20 μm.

[0205] In some embodiments, the positive plate, the negative plate, and the separator may be manufactured into an electrode assembly through a winding process or a stacking process; and the electrode assembly and the electrolyte are packaged using the cell packaging material of the first aspect of the present application.

[0206] The present application does not impose any particular restrictions on the shape of the secondary battery, and it may be cylindrical, rectangular, or any other shape. For example, FIG. 1 is an exemplary secondary battery (1) with a rectangular structure.

[0207] In some embodiments, referring to FIG. 2, the exterior material may include a housing (11) and a cover plate (13). Here, the housing (11) may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate surround to form a receiving chamber. The housing (11) has an opening communicating with the receiving chamber, and the cover plate (13) may cover the opening to seal the receiving chamber.

[0208] The positive electrode plate, the negative electrode plate, and the separator can form an electrode assembly (12) through a winding process or a stacking process. The electrode assembly (12) is sealed in the receiving chamber. The electrolyte is infiltrated into the electrode assembly (12). The number of electrode assemblies (12) included in the lithium-ion battery (1) may be one or multiple, and can be adjusted as needed.

[0209] In some embodiments, the secondary battery may be assembled into a battery module, and the number of secondary batteries included in the battery module may be multiple, and the specific number may be adjusted according to the application and capacity of the battery module.

[0210] In the battery module, a plurality of secondary batteries can be arranged and installed in sequence along the length direction of the battery module. Of course, they may also be arranged in any other arbitrary manner. Furthermore, the plurality of lithium-ion batteries can be secured using fasteners.

[0211] Optionally, the battery module may further include a case having a receiving space, and a plurality of secondary batteries are accommodated in the receiving space.

[0212] In some embodiments, the battery module may also be assembled into a battery pack, and the number of battery modules included in the battery pack may be adjusted according to the application and capacity of the battery pack.

[0213] A battery pack may include a battery box and a plurality of battery modules installed in the battery box. The battery box includes an upper box and a lower box, and the upper box may cover the lower box to form a sealed space for accommodating the battery modules. The plurality of battery modules may be arranged in any manner within the battery box.

[0214] electrical devices

[0215] The fourth aspect of the present application provides an electric device, said electric device comprising at least one of the secondary battery, battery module, or battery pack of the third aspect of the present application. The secondary battery, battery module, or battery pack may be used as a power source for said device and may also be used as an energy storage unit of said device. The device includes, but is not limited to, mobile devices, electric vehicles, electric trains, ships and satellites, energy storage systems, etc., wherein the mobile device may include, but is not limited to, at least one of a mobile phone, a laptop, etc.; and the electric vehicle may include, but is not limited to, at least one of a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.

[0216] The above device can select a secondary battery, battery module, or battery pack depending on usage requirements.

[0217] FIG. 3 shows an exemplary electric device (2). This electric device (2) is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the secondary battery required by this device, a battery pack or battery module may be used.

[0218] Other examples of devices include mobile phones, tablet PCs, and laptops. These devices typically require a slim design, allowing them to use lithium-ion batteries as a power source.

[0219] The advantageous effects of the present application are further explained through the following examples.

[0220] To further clarify the technical problem, technical solution, and advantageous effects to be solved by this application, the following description combines the embodiments and drawings for a more detailed explanation. It is obvious that the described embodiments are only some of the embodiments of this application, not all. The description of at least one exemplary embodiment below is merely illustrative and should not be construed as any limitation on this application and its application. All other embodiments obtained by a person skilled in the art based on the embodiments of this application, without striving to create an inventive step, fall within the scope of protection of this application.

[0221] Where specific technical or conditional terms are not specified in the examples, they shall be in accordance with the technical or conditional terms or product specifications described in the literature of the art. Where the manufacturer of the reagent or instrument used is not specified, it shall be a general product available on the market. For example, phenolic resin may be purchased from China Jining Huakai Resin Co., Ltd.

[0222] A. Manufacturing of silicon-carbon composite materials

[0223] Example 1

[0224] Step 1: 1 kg of coconut shell (carbon material precursor) is placed in a box-type electric furnace and nitrogen is passed through it, then heated to 600°C at a heating rate of 5°C / min and maintained for 2 hours to perform the first sintering treatment, and after the electric furnace cools, the carbon substrate is removed;

[0225] Step 2: Potassium hydroxide (an alkaline substance) and a carbon substrate are mixed in a mass ratio of 4:1, placed in a box-type electric furnace, and nitrogen is passed through; the mixture is then heated to 800°C at a heating rate of 5°C / min and maintained for 4 hours to perform the pore formation treatment;

[0226] Step 3: The pore-forming treated carbon substrate is uniformly mixed with a 0.1 mol / L hydrochloric acid solution (acidic substance) to remove residual potassium hydroxide in the carbon matrix, and then heated and dried at 80°C for 12 hours;

[0227] Step 4: A pore-forming treated carbon substrate is placed in a vapor deposition rotary furnace, acetylene (first carbon source) and nitrogen are mixed in a volume ratio of 2:10, and then heated to 950°C at a heating rate of 5°C / min to perform a first vapor deposition for 2 hours to control the aperture and produce a carbon matrix having a pore structure;

[0228] Step 5: A carbon matrix is ​​placed in a vapor deposition furnace and heated to 500°C at a heating rate of 5°C / min, after which a mixed gas of monosilane (silicon source) and nitrogen is passed through, wherein the volume ratio of monosilane is 20% and the volume ratio of nitrogen is 80%, the total gas flow rate is 5L / min, and the internal pressure of the deposition furnace is controlled to be slightly higher than atmospheric pressure by 200Pa, and secondary vapor deposition is carried out for 6h;

[0229] Step 6: Stop the passage of monosilane and continue raising the temperature to 600°C, then pass a mixed gas of acetylene (second carbon source) and nitrogen, wherein the volume ratio of acetylene is 20% and the volume ratio of nitrogen is 80%, perform a third vapor deposition for 1 hour, and after cooling, filter through a sieve to obtain a silicon-carbon composite material.

[0230] The manufacturing methods of Examples 2-5 and Example 1 are similar, and the differences can be seen in detail in Table 1.

[0231] Comparative Example 1

[0232] The manufacturing methods of Comparative Example 1 and Example 1 are similar, but the difference is that a primary vapor deposition step is not used when manufacturing the silicon carbon composite material.

[0233] Comparative Example 2-4

[0234] The manufacturing methods of Comparative Examples 2-4 and Example 1 are similar, and the differences can be seen in detail in Table 1.

[0235] By group Primary sintering treatment Pore ​​formation treatment Primary vapor deposition Secondary vapor deposition 3rd vapor deposition carbon material precursor T1(℃) t1(h) alkaline substances n1 T2(℃) t2(h) First carbon source n2 T3(℃) t3(h) Silicon source n3 T4(℃) t4(h) Second carbon source n4 T5(℃) t5(h) Example 1 coconut shell 600 4 KOH 4:1 800 4 acetylene 2:10 950 2 monosilan 20% 500 6 acetylene 20% 600 1 Example 2 bamboo powder 800 3 KOH 2:1 800 4 acetylene 2:10 850 3 monosilan 20% 520 6 acetylene 20% 600 1 Example 3 bamboo powder 800 2 KOH 3:1 800 4 acetylene 2:10 850 1.5 monosilan 20% 500 6 acetylene 20% 600 1 Example 4 coconut shell 700 3 KOH 4:1 800 4 acetylene 2:10 850 2 monosilan 20% 540 6 acetylene 20% 600 1 Example 5 phenolic resin 700 3 KOH 3:1 800 4 acetylene 2:10 850 2 monosilan 20% 500 6 acetylene 20% 600 1 Comparative Example 1 coconut shell 600 4 KOH 4:1 800 4 / / / / monosilan 20% 500 6 acetylene 20% 600 1 Comparative Example 2 coconut shell 600 4 KOH 4:1 800 4 acetylene 2:10 700 2 monosilan 20% 500 6 acetylene 20% 600 1 Comparative Example 3 coconut shell 600 4 KOH 4:1 800 4 acetylene 2:10 700 2 monosilan 20% 500 6 acetylene 20% 800 1 Comparative Example 4 coconut shell 600 4 KOH 4:1 800 4 acetylene 2:10 700 2 monosilan 20% 750 6 acetylene 20% 800 1

[0236] Here, n1 represents the mass ratio of the alkaline substance to the carbon substrate, n2 represents the volume ratio of the first carbon source to the inert gas, n3 represents the volume ratio of the silicon source in the mixed gas during the second vapor deposition, n4 represents the volume ratio of the second carbon source in the mixed gas during the third vapor deposition, T1 represents the temperature of the first sintering treatment, t1 represents the time of the first sintering treatment, T2 represents the sintering temperature during the pore formation treatment, t2 represents the sintering time during the pore formation treatment, T3 represents the temperature of the first vapor deposition, t3 represents the time of the first vapor deposition, T4 represents the temperature of the second vapor deposition, t4 represents the time of the second vapor deposition, T5 represents the temperature of the third vapor deposition, t5 represents the time of the third vapor deposition, and the pressure difference represents the difference between the pressure of the second vapor deposition and atmospheric pressure.

[0237] B. Manufacturing of button cells

[0238] 1. Cathode plate

[0239] The above-mentioned silicon carbon composite material, conductive carbon black, and polyacrylic acid as a binder are mixed in a mass ratio of 8:1:1, and deionized water is added and mixed while stirring sufficiently to form a cathode slurry; the cathode slurry is uniformly coated on one surface of a copper foil serving as a cathode current collector, and a cathode plate is obtained through drying and cold rolling.

[0240] 2. Electrolyte

[0241] Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) are mixed in a volume ratio of 20:20:60, LiPF6 is uniformly dissolved in the solution, and fluorocarbonate ethylene (FEC), an additive, is added to obtain an electrolyte. In this electrolyte, the concentration of LiPF6 is 1 mol / L, and FEC accounts for 5% of the total mass of the electrolyte.

[0242] 3. Separator

[0243] Polyethylene film is used as a separator.

[0244] 4. Manufacture of button cells

[0245] The above-mentioned negative plate is used as the working electrode and metallic lithium as the counter electrode; the negative plate, separator, and metallic lithium are stacked in order so that the separator is positioned between the working electrode and the counter electrode, and the above-mentioned electrolyte is injected to assemble a button cell.

[0246] C. Manufacturing of secondary batteries (full batteries)

[0247] 1. Cathode plate

[0248] A cathode slurry is formed by mixing the above-mentioned silicon-carbon composite material, a mixture of carbon nanotubes and SP as a conductive agent, styrene-butadiene rubber as a binder, and sodium carboxymethylcellulose as a thickener in an appropriate amount of deionized water as a solvent while stirring sufficiently, according to a weight ratio of 95.5:1:2:1. The cathode slurry is applied to both surfaces of a copper foil serving as a cathode current collector, and a cathode plate is obtained through drying and cold rolling.

[0249] 2. Anode plate

[0250] LiNi, a positive active material 0.8 Co 0.1 Mn 0.1O2 (NCM811), conductive carbon black, and polyvinylidene fluoride are mixed in a weight ratio of 97.5:1.2:1.3, and an appropriate amount of solvent NMP is added and uniformly stirred to obtain an anode slurry. The anode slurry is applied to both surfaces of an aluminum foil serving as an anode current collector, and an anode plate is obtained through drying and cold rolling.

[0251] 3. Electrolyte

[0252] A mixture of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) is used as an organic solvent, wherein the volume ratio of EC, EMC, and DEC is 20%:20%:60%. A lithium salt (LiPF6) that has been sufficiently dried in an argon atmosphere glove box with a moisture content <10 ppm is dissolved in the above organic solvent, and an electrolyte is obtained by adding fluorocarbonate ethylene (FEC) as an additive. In this electrolyte, the concentration of LiPF6 is 1 mol / L, and FEC accounts for 5% of the total mass of the electrolyte.

[0253] 4. Separator

[0254] Polyethylene film is used as a separator.

[0255] 5. Manufacturing of secondary batteries

[0256] A separator and the above-manufactured positive and negative plates are sequentially positioned, with the separator placed between the positive and negative plates to act as an isolator, and then wound to obtain an electrode assembly; the electrode assembly is placed on an outer casing, dried, and then the above-manufactured electrolyte is injected, and a pouch-type secondary battery is obtained through processes such as vacuum sealing, standing, formation, and capacity testing. The dimensions of the secondary battery are 135mm × 72mm × 60mm, and the capacity is 4.65Ah.

[0257] D. Battery performance test

[0258] 1. Initial charge / discharge efficiency

[0259] After leaving the above-manufactured button cell for 60 minutes, it is discharged to 5mV with a constant current of 0.05C, discharged to 5mV with 50μA and left for 10 minutes, and charged to 1.5V with 0.1C; where the lithium detachment capacity of 1.5V represents the capacity size of the sample to be measured, the initial charge / discharge efficiency = lithium detachment capacity of 1.5V / lithium insertion capacity × 100%, and the results are as shown in Table 2.

[0260] 2. V A / V B

[0261] After leaving the above-manufactured button cell for 60 minutes, discharge it to 5mV with a constant current of 0.05C, discharge it to 5mV with 50μA and leave it for 10 minutes, and charge it to 1.5V with 0.1C; plot a relationship curve between the differential value (dQ / dV) obtained by differentiating the charge / discharge capacity (Q) with respect to the operating electrode potential (V) and the operating electrode potential (V), and when current is applied to the negative electrode material in the lithium desorption direction, the maximum value of the differential value (dQ / dV) between 0.26V and 0.33V is V A Record as, and the maximum value of the derivative (dQ / dV) between 0.42V and 0.52V is V B By recording as, V A / V B Calculate the values, and the results are as shown in Table 2.

[0262] Figure 5 shows a relationship curve between the differential value (dQ / dV) and the operating electrode potential (V) of a battery cell manufactured with the silicon-carbon composite material of Example 3. In Figure 5, V of this battery cell A / V B It can be seen that it is 1.62.

[0263] 3. Cyclic Performance Test

[0264] The secondary battery (full battery) manufactured above is charged to 4.25V at 0.5C at 25℃, and then discharged to 2.5V at 1C. This constitutes one charge-discharge cycle, and the discharge capacity at this time is recorded as the initial discharge capacity. The secondary battery is continuously subjected to a cycle charge-discharge test using the above method, and the discharge capacity after each cycle is recorded. The test is continued until the discharge capacity of the secondary battery decreases to 80% of the initial discharge capacity, and the number of cycles at this time is recorded.

[0265] By group V A / V B Initial charge / discharge efficiency Cycle Performance / Cycle Example 1 1.55 82.3% 943 Example 2 1.59 81.9% 1023 Example 3 1.62 82.1% 1107 Example 4 1.71 82.9% 1265 Example 5 1.99 82.7% 1147 Comparative Example 1 1.32 81.0% 557 Comparative Example 2 1.38 81.4% 589 Comparative Example 3 1.34 81.2% 572 Comparative Example 4 1.25 81.7% 335

[0266] Comparing the results of the examples and comparative examples in Table 2, the silicon-carbon composite material of the present application comprises a carbon matrix having a porous structure and a silicon-based material distributed in the pore structure of the carbon matrix, and furthermore, the V of the material A / V B It can be seen that controlling ≥1.4 significantly improves the initial charge / discharge efficiency and cycling performance of silicon carbon composite materials.

[0267] In Comparative Example 1, when manufacturing the silicon-carbon composite material, a primary vapor deposition treatment was not performed and the diameter of the pore structure was not controlled; as a result, the diameter of the pore structure was large, causing the silicon-based material to be deposited on the surface of the carbon matrix, and the grain size of the silicon-based material increased, and the V of the manufactured silicon-carbon composite material A / V B Since <1.4, the initial charge / discharge efficiency and cycling performance of silicon carbon composite materials cannot be significantly improved.

[0268] In Comparative Example 2, when manufacturing the silicon-carbon composite material, the primary vapor deposition temperature is low, resulting in insufficient pore structure pretreatment and a low micropore ratio, causing some silicon-based material to be deposited on the carbon matrix surface, and the large grain size of the silicon-based material results in V of the silicon-carbon composite material A / V B It becomes <1.4.

[0269] In Comparative Example 3, when manufacturing the silicon-carbon composite material, the primary vapor deposition temperature is low, resulting in insufficient pore structure pretreatment and a low micropore ratio, causing some silicon-based material to be deposited on the carbon matrix surface and the grain size of the silicon-based material to increase; furthermore, the tertiary vapor deposition temperature is high, causing the silicon grains to grow further, and V of the finally manufactured silicon-carbon composite material A / V B It becomes <1.4.

[0270] In Comparative Example 4, when manufacturing the silicon-carbon composite material, the primary vapor deposition temperature was low, resulting in insufficient pore structure pretreatment and a low micropore ratio; furthermore, the secondary vapor deposition temperature was too high, leading to a rapid decomposition rate of the silicon-based material, with most of it deposited on the surface of the carbon matrix, and the silicon grains aggregated and grew rapidly, causing the V of the silicon-carbon composite material A / V B <1.4. Each technical feature of the embodiments mentioned above may be combined arbitrarily, and for the sake of brevity, not all possible combinations of each technical feature of the embodiments are described, but as long as such combinations of technical features are not contradictory, they should be deemed to be included within the scope described in this specification.

[0271] The embodiments described above represent only a few modes of implementation of this application. Although the description is relatively specific and detailed, it should not be understood as a limitation on the claims. A person skilled in the art may make minor modifications and improvements without departing from the spirit of this application, and all such modifications fall within the scope of protection of this application. Accordingly, the scope of protection of this patent application is defined by the appended claims. Explanation of the symbols

[0272] 1-Secondary battery; 11-Housing; 12-Electrode assembly; 13-Cover plate; 2-Electric device; 411-Carbon matrix; 412-Carbon coating layer.

Claims

Claim 1 In a secondary battery, a negative electrode plate is included, wherein the negative electrode plate comprises a silicon-carbon composite material, and the silicon-carbon composite material comprises: a carbon matrix having a porous structure; and a silicon-based material distributed in the porous structure of the carbon matrix; and the silicon-carbon composite material is charged and discharged using a button cell, and a relationship curve is plotted between the voltage (V) and the derivative value (dQ / dV) obtained by differentiating the charge / discharge capacity (Q) with respect to the charge / discharge curve of the button cell, such that the maximum value of the derivative value (dQ / dV) between 0.26V and 0.35V is V A Record as, and the maximum value of the derivative (dQ / dV) between 0.42V and 0.52V is V B If recorded as such, the above silicon-carbon composite material is V A / V B A secondary battery characterized by satisfying ≥1.40; and having a pore diameter of 0.5nm-8nm. Claim 2 In paragraph 1, 1.42≤V A / V B A secondary battery characterized by ≤1.

90. Claim 3 In paragraph 1, 1.50≤V A / V B A secondary battery characterized by ≤1.

70. Claim 4 A secondary battery according to claim 1, characterized in that the crystal grain size of the silicon-based material is ≤6 nm. Claim 5 A secondary battery according to claim 1, characterized in that the pore structure comprises micropores with a diameter of 0.5 nm or more and less than 2 nm, and mesopores with a diameter of 2 nm to 8 nm. Claim 6 A secondary battery according to claim 5, characterized in that the quantity ratio of the micropores in the pore structure is 60%-90%. Claim 7 In claim 1, the specific surface area of ​​the silicon-carbon composite material is 2m 2 / g-10m 2 A secondary battery characterized by having / g. Claim 8 In claim 1, the silicon-carbon composite material has at least one of the following features: (1) the silicon-based material comprises a silicon monomer; (2) the shape of the silicon-based material comprises one or more of spherical, pseudo-spherical, plate-like, and linear; and (3) the specific surface area of ​​the carbon matrix is ​​1000 m² 2 / g-2000m 2 / g; (4) the mass ratio of the silicon-based material in the silicon-carbon composite material is 35%-60%; (5) the volumetric distribution particle size (Dv50) of the silicon-carbon composite material is 3μm-15μm; (6) the volumetric distribution particle size (Dv90) of the silicon-carbon composite material is less than or equal to 50μm; (7) the silicon-carbon composite material satisfies 1 ≤ (Dv90 - Dv10) / Dv50 ≤ 3; (8) the tap density of the silicon-carbon composite material is 0.8g / cm³ 3 -1.2g / cm 3 (9) A secondary battery characterized by the powder resistivity of the silicon carbon composite material at 16 MPa being less than or equal to 5 Ω·m. Claim 9 A secondary battery according to claim 1, characterized in that a carbon coating layer is further included on at least a portion of the outer surface of the silicon-carbon composite material. Claim 10 A secondary battery according to claim 9, wherein the carbon coating layer has at least one of the following features: (1) the material of the carbon coating layer comprises amorphous carbon; and (2) the thickness of the carbon coating layer is 30 nm to 200 nm. Claim 11 In a method for manufacturing a secondary battery according to claim 1, the step of manufacturing a negative electrode plate of the secondary battery comprises: a step of manufacturing a carbon substrate; a step of performing a pore-forming treatment on the carbon substrate to obtain a carbon matrix (A) having a pore structure; a step of performing a diameter-regulating treatment on the carbon matrix (A) having a pore structure to obtain a carbon matrix (B) having a pore structure; and a step of manufacturing a silicon-carbon composite material by depositing a silicon-based material within the pore structure of the carbon matrix (B) having a pore structure; and a step of charging and discharging the silicon-carbon composite material with a button cell, drawing a relationship curve between the voltage (V) and the differential value (dQ / dV) obtained by differentiating the charge / discharge capacity (Q) with respect to the charge / discharge curve of the button cell, and the maximum value of the differential value (dQ / dV) between 0.26V and 0.35V V A Record as, and the maximum value of the derivative (dQ / dV) between 0.42V and 0.52V is V B If recorded as such, the above silicon-carbon composite material is V A / V B A method for manufacturing a secondary battery characterized by satisfying ≥1.40; having a diameter of the pore structure of 0.5 nm to 8 nm; and manufacturing the negative electrode plate using the silicon carbon composite material to obtain the secondary battery. Claim 12 A method for manufacturing a secondary battery according to claim 11, wherein the step of manufacturing the carbon substrate comprises the step of manufacturing the carbon substrate by first sintering a carbon material precursor. Claim 13 A method for manufacturing a secondary battery according to claim 12, wherein the method for manufacturing the carbon substrate satisfies at least one of the following conditions: (1) the temperature of the first sintering treatment is 400℃-800℃; (2) the time of the first sintering treatment is 1h-12h; (3) the atmosphere of the first sintering treatment includes an inert gas; (4) the inert gas includes one or more of nitrogen and argon; and (5) the carbon material precursor includes one or more of a resin carbon material and a biomass carbon material. Claim 14 A method for manufacturing a secondary battery according to claim 11, wherein the pore-forming treatment step comprises the step of alkaline etching of the carbon substrate with an alkaline substance. Claim 15 A method for manufacturing a secondary battery according to claim 14, wherein the pore-forming treatment satisfies at least one of the following conditions: (1) the alkaline substance comprises one or more of potassium hydroxide and sodium hydroxide; and (2) the mass ratio of the alkaline substance to the carbon substrate is (2-6):

1. Claim 16 A method for manufacturing a secondary battery according to any one of claims 11 to 15, wherein the aperture control treatment step comprises the step of placing a carbon matrix (A) having the pore structure in a mixed gas containing a first carbon source and an inert gas, and performing a first vapor deposition. Claim 17 A method for manufacturing a secondary battery according to claim 16, characterized in that the temperature of the first vapor deposition is 800℃-1000℃. Claim 18 A method for manufacturing a secondary battery according to claim 16, characterized in that the temperature of the first vapor deposition is 850℃-950℃. Claim 19 A method for manufacturing a secondary battery according to claim 16, characterized in that the time of the first vapor deposition is 1h-4h. Claim 20 A method for manufacturing a secondary battery according to claim 16, characterized in that the volume ratio of the first carbon source and the inert gas is (2-5):

10. Claim 21 A method for manufacturing a secondary battery according to claim 16, wherein the first vapor deposition further comprises at least one of the following conditions: (1) the first carbon source comprises one or more of methane, ethylene, and acetylene; and (2) the inert gas comprises one or more of nitrogen and argon. Claim 22 A method for manufacturing a secondary battery according to any one of claims 11 to 15, characterized in that the carbon matrix (B) having the porous structure is placed in a mixed gas comprising a silicon source and an inert gas, and a secondary vapor deposition is performed. Claim 23 A method for manufacturing a secondary battery according to claim 22, characterized in that the temperature of the secondary vapor deposition is 450℃-650℃. Claim 24 A method for manufacturing a secondary battery according to claim 22, characterized in that the temperature of the secondary vapor deposition is 500℃-600℃. Claim 25 A method for manufacturing a secondary battery according to claim 22, characterized in that the time of the secondary vapor deposition is 4h-8h. Claim 26 A method for manufacturing a secondary battery according to claim 22, wherein the secondary vapor deposition comprises at least one of the following conditions: (1) the volume ratio of the silicon source in the mixed gas is 10%-40%; and (2) the volume ratio of the inert gas in the mixed gas is 60%-90%. Claim 27 A method for manufacturing a secondary battery according to claim 22, wherein the secondary vapor deposition further comprises at least one of the following conditions: (1) the difference between the pressure of the secondary vapor deposition and the amount of atmospheric pressure is 0.2 kPa to 0.6 kPa; (2) the silicon source comprises one or more of monosilane, disilane, and trisilane; and (3) the inert gas comprises one or more of nitrogen and argon. Claim 28 A method for manufacturing a secondary battery, characterized in that, in any one of claims 11 to 15, prior to the diameter control treatment step, the method further comprises a step of removing the alkaline substance remaining on the carbon substrate after the pore formation treatment with an acidic substance. Claim 29 A method for manufacturing a secondary battery according to any one of claims 11 to 15, wherein the manufacturing method further comprises the step of placing the silicon carbon composite material in a mixed gas containing a second carbon source and an inert gas, and performing a third vapor deposition to form a carbon coating layer on at least a portion of the outer surface of the silicon carbon composite material. Claim 30 A method for manufacturing a secondary battery according to claim 29, wherein the third vapor deposition satisfies at least one of the following conditions: (1) the second carbon source comprises one or more of methane, ethylene, and acetylene; (2) the inert gas comprises one or more of nitrogen and argon; (3) the volume ratio of the second carbon source in the mixed gas is 5%-20%; (4) the temperature of the third vapor deposition is 500℃-700℃; and (5) the time of the third vapor deposition is 1h-6h. Claim 31 An electrical device characterized by comprising a secondary battery according to claim 1 or a secondary battery obtained by employing the manufacturing method of claim 11.