Polythiophene conductive polymer derivatives containing alkylene sulfonic acid side chain, manufacturing method thereof, and organic electronic devices, and infrared shielding composition containing the same

A polythiophene-based conductive polymer derivative with an alkylene sulfonic acid side chain addresses the challenges of deep blue light emission, high power conversion efficiency, and infrared shielding in organic electronic devices and solar cells, enhancing performance and stealth capabilities.

KR103046476B1Active Publication Date: 2026-11-11주식회사 케이알첨단전자재료
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
KR1020260067892
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2026-04-15
Publication Date
2026-11-11
Estimated Expiration
2046-04-15

AI Technical Summary

Technical Problem

Existing organic electronic devices and solar cells face challenges in achieving deep blue light emission, high power conversion efficiency, and infrared shielding or stealth capabilities, particularly in flexible and lightweight applications.

Method used

A polythiophene-based conductive polymer derivative with an alkylene sulfonic acid side chain is used in the hole injection layer of phosphorescent-sensitive superfluorescent organic electroluminescent devices and organic solar cells, along with an infrared shielding composition containing a conductive polymer derivative and a polyurethane-based binder.

Benefits of technology

The conductive polymer derivative enhances brightness, external quantum efficiency, current efficiency, and power efficiency in electroluminescent devices, improves power conversion efficiency in solar cells, and provides effective infrared shielding and stealth performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112026045870343-PAT00015_ABST
    Figure 112026045870343-PAT00015_ABST
Patent Text Reader

Abstract

The present invention relates to a polythiophene-based conductive polymer derivative having an alkylene sulfonic acid side chain substituent, a method for manufacturing the same, and an organic electronic device and an infrared shielding composition containing the same. The organic electronic device according to the present invention emits a super-fluorescent deep blue light and exhibits excellent brightness, external quantum efficiency, and color purity. Additionally, the organic solar cell according to the present invention exhibits excellent power conversion efficiency. Furthermore, the infrared shielding composition according to the present invention has a transmittance of less than 10% in the infrared region of 2,500 nm to 25,000 nm, which is an excellent effect of avoiding heat detection, i.e., infrared shielding and stealth performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a polythiophene-based conductive polymer derivative having an alkylene sulfonic acid side chain substituent, a method for manufacturing the same, and an organic electronic device and an infrared shielding composition containing the same. More specifically, the invention relates to a polythiophene-based conductive polymer derivative having an alkylene sulfonic acid side chain substituent that emits a deep blue color in a phosphorescent-sensitive superfluorescent organic electroluminescent device, can be applied as a hole injection layer in an organic solar cell, and can achieve heat detection avoidance, infrared shielding, and stealth performance based on low transmittance in the infrared region, a method for manufacturing the same, and an organic electronic device and an infrared shielding composition containing the same. Background Technology

[0003] Organic electronic devices are electronic devices based on organic compounds. Unlike conventional inorganic electronic devices that have stiffness, organic electronic devices are based on carbon and combined with various elements such as oxygen, nitrogen, and hydrogen. They exhibit excellent flexibility and display various electrochemical properties depending on the type of polymer compound applied to the device. Therefore, unlike conventional inorganic semiconductor devices, organic electronic devices are widely applied across industries depending on their applications, such as the development of wearable electronic devices like smartphones, smartwatches, and biosensors, as well as various flexible electronic products and organic solar cells. Various research and development efforts are underway to improve electrochemical properties, and as an example, a developed technology has been patented as described in Patent Document 1.

[0004] Meanwhile, organic solar cells, which possess flexible characteristics, are gaining attention as a future eco-friendly energy source, replacing conventional inorganic semiconductor devices whose application range is limited due to their planar structure caused by stiffness characteristics. By applying conductive polymers to achieve the characteristics described above, organic solar cells enable low-cost solution-based processes along with lightweight, flexible, and low-weight properties, and also allow for the manufacturing of large-area solar cells; however, there is also the issue of needing to improve power conversion efficiency (PCE) as an important characteristic. The two factors determining the PCE of an organic solar cell (OSC) are the materials forming the hole transport layer and the active layer, and significant research is being conducted on materials for a more efficient hole transport layer. As an example, a developed technology has been patented as described in Patent Document 2.

[0005] In addition, infrared shielding or stealth capabilities are key technologies that determine the survivability of weapon systems in modern battlefields. They serve to protect soldiers and weapon systems from heat-seeking missiles or drone surveillance equipment by concealing heat signals generated from them. Therefore, there is an urgent need to develop windows equipped with infrared shielding films for the defense of critical national infrastructure against drone attacks.

[0006] As such, there is a need to develop phosphorescent-sensitive superfluorescent organic light-emitting diodes with superior luminescence characteristics, such as deep blue light emission, brightness, and external quantum efficiency compared to conventional blue organic light-emitting diodes, hole transport layers of organic solar cells capable of realizing high power conversion efficiency, and compositions capable of realizing heat detection avoidance, infrared shielding, or stealth functions. Prior art literature

[0008] Korean Registered Patent Publication No. 10-0936140 (Registered Jan. 04, 2010) Korean Published Patent Publication No. 10-2024-0083404 (Published June 12, 2024) The problem to be solved

[0009] The present invention aims to solve the above-mentioned problems by providing a polythiophene-based conductive polymer derivative having an alkylene sulfonic acid side chain, a method for manufacturing the same, an organic electronic device containing the same, and a composition for infrared shielding.

[0010] The above conductive polymer derivative can be applied to phosphorescent-sensitive superfluorescent organic electroluminescent devices and organic solar cells, and can also be included in compositions that exhibit heat detection avoidance, infrared shielding, or stealth performance. means of solving the problem

[0012] A preferred embodiment of the present invention for achieving the above objectives is , A first electrode; a second electrode formed opposite to the first electrode; and one or more organic layers disposed between the first electrode and the second electrode, wherein one or more of the organic layers are as follows An electronic device characterized by comprising a conductive polymer derivative having an alkylene sulfonic acid side chain represented by Chemical Formula 1 is used as a means to solve the problem.

[0013] [Chemical Formula 1]

[0014]

[0015] (However, in the above Chemical Formula 1, R1 and R2 are each independently a straight-chain or branched-chain alkylene group having 1 to 10 carbon atoms, and n is 10 to 3,000.)

[0017] According to a preferred embodiment of the present invention, the organic layer may include one or more selected from a hole injection layer, a hole transport layer, a light-emitting layer, an electron transport layer, an electron injection layer, or a mixed layer thereof, or an infrared shielding or stealth solution or film.

[0018] The hole injection layer according to a preferred embodiment of the present invention is as follows It may include a conductive polymer derivative having an alkylene sulfonic acid side chain represented by chemical formula 1a.

[0019] [Chemical Formula 1a]

[0020]

[0021] (However, in the above chemical formula 1a, n is 10 to 3,000.)

[0022] According to a preferred embodiment of the present invention, the light-emitting layer is characterized in that the host and the dopant are deposited by a co-deposition method.

[0023] According to a preferred embodiment of the present invention, the host comprises 9-(3-(triphenylsilyl)phenyl)-9H-3,9'-bicarbazole (SiCzCz) and 9,9'-(6-(3-(Triphenylsilyl)phenyl)-1,3,5-triazine-2,4-diyl)bis(9H-carbazole) (SiTrzCz2); 4,4',4"-tris(N-carbazolyl)-triphenylamine (TCTA) and 1,3,5-tris(N-phenylbenzimidazole-2-yl)benzene (TPBi); 4,4',4"-tris(N-carbazolyl)-triphenylamine (TCTA) and tris(2,4,6-trimethyl-3-(pyridin-3-yl)phenyl)borane (3TPYMB); It may comprise an exciplex selected from the group consisting of 4,4',4"-tris(N-carbazolyl)-triphenylamine (TCTA) and 1,3-bis(3,5-dipyridin-3-ylphenyl)benzene (BmPyPB); or 4,4',4"-tris(N-carbazolyl)-triphenylamine (TCTA) and 9,9-bis(4-(9H-carbazol-9-yl)phenyl)-9H-fluorene (BSFM).

[0024] According to a preferred embodiment of the present invention, the dopant may comprise Platinum(II) 9-(4-(tert-butyl)pyridin-2-yl)-2-(3-(3-(quinolin-2-ylmethyl)-2,3-dihydro-1H-benzo[d]imidazol-1-yl)phenoxy)-9H-carbazole (Q(Bn)_Pt) or N7,N7,N13,N13,5,15-hexaphenyl-9,11-bis(4-(tert-butyl)phenyl)-5,9,11,15-tetrahydro-5,9,11,15-tetraaza-19b,20b-diboradinaphtho [3,2,1-de:1',2',3'-jk]pentacene-7,13-diamine (t-Bu-v-DABNA).

[0025] According to a preferred embodiment of the present invention, the electronic device is a phosphorescence-sensitive superfluorescent organic electroluminescent device that emits a deep blue color and is characterized by improved brightness, external quantum efficiency, current efficiency, and power efficiency.

[0026] The light-emitting layer according to a preferred embodiment of the present invention is 1×10 -5 Torr to 1×10 -8 It may be deposited under vacuum conditions of Torr.

[0028] And another preferred embodiment of the present invention is characterized by comprising a conductive polymer derivative having a butyl sulfonate side chain introduced therein having an alkylene sulfonic acid side chain represented by the following chemical formula 1. Organic solar cells are used as another means of solving the problem.

[0029] [Chemical Formula 1]

[0030]

[0031] (However, in the above Chemical Formula 1, R1 and R2 are each independently a straight-chain or branched-chain alkylene group having 1 to 10 carbon atoms, and n is 10 to 3,000.)

[0032] The organic solar cell according to a preferred embodiment of the present invention is as follows: A conductive polymer derivative having an alkylene sulfonic acid side chain represented by chemical formula 1a may be included in the hole transport layer.

[0033] [Chemical Formula 1a]

[0034]

[0035] (However, in the above chemical formula 1a, n is 10 to 3,000.)

[0036] According to a preferred embodiment of the present invention, the organic solar cell may have a photoactive layer disposed on top of the hole transport layer that is formed as a bulk heterojunction (BHJ) in which a non-fullerene electron donor and a fulllerene electron acceptor are stacked in a mixed state.

[0037] In a preferred embodiment of the present invention, the organic solar cell may have an electron transport layer disposed on top of the photoactive layer composed of N,N'-Bis(N,N-dimethylpropan-1-amine oxide)perylene-3,4,9,10-tetracarboxylic diimide (PDINO).

[0039] And another preferred embodiment of the present invention is as follows Another means of solving the problem is an infrared shielding composition characterized by comprising: a conductive polymer derivative having an alkylene sulfonic acid side chain represented by chemical formula 1a; a polyurethane-based (PU) binder; and a solvent.

[0040] [Chemical Formula 1a]

[0041]

[0042] (However, in the above chemical formula 1a, n is 10 to 3,000.)

[0043] According to a preferred embodiment of the present invention, the polyurethane-based (PU) binder may be included in an amount of 100 to 300 parts by weight per 100 parts by weight of the conductive polymer derivative. Effects of the invention

[0045] When a conductive polymer derivative having an alkylene sulfonic acid side chain according to the present invention is applied to the hole injection layer of a phosphorescence-sensitive superfluorescent organic electronic device, excellent brightness, external quantum efficiency, current efficiency, and power efficiency can be achieved along with deep blue light emission.

[0046] In addition, when a conductive polymer derivative having an alkylene sulfonic acid side chain according to the present invention is applied to the hole injection layer of an organic solar cell, it has the effect of exhibiting excellent power conversion efficiency.

[0047] In addition, when a conductive polymer derivative having an alkylene sulfonic acid side chain according to the present invention is included in an infrared shielding or stealth solution or film layer, the infrared shielding effect and mechanical stability are improved.

[0048] The effects of the present invention are not limited to those mentioned above, and other unmentioned effects will be clearly understood by those skilled in the art from the description in the claims. Brief explanation of the drawing

[0050] FIG. 1 is a schematic cross-sectional view illustrating a multi-layer electronic device in which a conductive polymer material having an alkylene sulfonic acid side chain synthesized according to a preferred embodiment of the present invention can be applied as a hole injection layer. FIGS. 2a to 2d are graphs showing the voltage-current density-luminance, EL spectrum, luminance-external quantum efficiency, and luminance-current efficiency-power efficiency results of a deep blue phosphorescent-sensitive superfluorescent electronic device in which a conductive polymer material having an alkylene sulfonic acid side chain is applied as a hole injection layer according to an embodiment of the present invention. FIG. 3 is a cross-sectional view illustrating an organic solar cell device according to an embodiment of the present invention. Figure 4 shows the voltage-current density characteristics of an organic solar cell device according to an embodiment of the present invention. FIG. 5 shows the transmittance characteristics in the infrared wavelength (2,500-25,000 nm) region of a conductive polymer material having an alkylene sulfonic acid side chain synthesized according to a preferred embodiment of the present invention. FIG. 6 is a photograph illustrating the results of heat detection avoidance, i.e., infrared shielding or stealth, before and after coating a fiber with a conductive polymer material having an alkylene sulfonic acid side chain synthesized according to a preferred embodiment of the present invention. Specific details for implementing the invention

[0051] The present invention will be described in detail below according to preferred embodiments with reference to the attached drawings, but specific descriptions of configurations and operations that are readily known to those skilled in the art will be omitted. Furthermore, it should be noted that the present invention is not necessarily limited by the following embodiments and that various modifications can be made to the invention within the scope of the technical concept of the invention.

[0052] The terms used in this specification have been selected to be as widely used as possible, taking into account their functions in the present invention; however, in specific cases, terms have been arbitrarily selected by the applicant, and in such cases, their meanings will be described in detail in the description of the invention. Accordingly, the terms used in this invention should be defined not merely by their names, but based on their meanings and the overall content of the invention.

[0054] Hereinafter, an electronic device comprising a polythiophene-based conductive polymer derivative having an alkylene sulfonic acid side chain according to a preferred embodiment of the present invention will be described with reference to the attached drawings.

[0056] For reference, FIG. 1 illustrates an electronic device according to the following Manufacturing Example 1 of the present invention.

[0058] As illustrated in FIG. 1, the present invention comprises a first electrode (110); a second electrode (180) formed opposite to the first electrode (110); and one or more organic layers disposed between the first electrode (110) and the second electrode (180), wherein one or more of the organic layers are as follows An electronic device (100) comprising a conductive polymer derivative having an alkylene sulfonic acid side chain represented by Chemical Formula 1 is provided.

[0059] [Chemical Formula 1]

[0060]

[0061] (However, in the above Chemical Formula 1, R1 and R2 are each independently a straight-chain or branched-chain alkylene group having 1 to 10 carbon atoms, and n is 10 to 3,000.)

[0062] More preferably, one or more of the organic layers are as follows It may include a conductive polymer derivative having an alkylene sulfonic acid side chain represented by chemical formula 1a.

[0063] [Chemical Formula 1a]

[0064]

[0065] (However, in the above chemical formula 1a, n is 10 to 3,000.)

[0066] The conductive polymer derivative having an alkylene sulfonic acid side chain of the above chemical formula 1a can be abbreviated as PSBM-EDT as poly[4-[(2,3-dihydrothieno[3,4-b][1,4]dioxin-2-yl)methoxy]butane-1-sulfonic acid][Poly{4-[(2,3-dihydrothieno[3,4-b][1,4]dioxin-2-yl)methoxy]butane-1-sulfonic acid}.

[0068] The first electrode (110) is a part coated on bare glass (G) and functions as an anode, and any material having transparency and conductivity with a larger work function than the second electrode (180) described later can be used. Examples include indium tin oxide (ITO), fluorine-doped tin oxide (FTO), aluminum-doped zinc oxide (AZO), and indium zinc oxide (IZO), and preferably, ITO can be used.

[0070] The second electrode (180) is a portion formed on the second electron injection layer (170) that functions as a cathode, and can be formed opposite to the first electrode (110) and can be selected from metals. Specifically, for example, it may include one or more alloys selected from Al, Ca, Mg, and Ag, and preferably, an alloy containing Al or Al that is sequentially coated may be used.

[0071] The above It is preferable to deposit aluminum in a chamber separated from the organic chamber to prevent contamination by organic matter.

[0073] The above organic layer may include one or more selected from a hole injection layer (HIL) (120), a hole transport layer (HTL) (130), an emission layer (EML) (140), a first electron transport layer (ETL) (150), a second electron transport layer (ETL) (160), an electron injection layer (EIL) (170), or a mixture thereof.

[0075] The hole injection layer (120) may include PSBM-EDT, a conductive polymer having an alkylene sulfonic acid side chain represented by the chemical formula 1.

[0077] The above hole injection layer (120) is preferably formed by UV-ozone treatment for 20 minutes on a bare glass (G) on which ITO, the first electrode (110), is deposited, to remove organic matter from the surface and make it hydrophilic, then sufficiently mixing PSBM-EDT, and then spin-coating at 1800~2200 rpm on the UV-ozone-treated first electrode (110) to form a film, and then heating on a hot plate at 140~160℃ for 15~25 minutes.

[0079] The hole transport layer (130) is a layer capable of stably supplying holes that have entered through the hole injection layer to the light-emitting layer, and can be placed on the hole injection layer (120). In order to smoothly transport and deliver holes, a material can be selected in which the highest occupied molecular orbital (HOMO) level of the hole transport layer (130) is deeper than the HOMO level of the light-emitting layer (140).

[0081] The hole transport layer (130) may include Poly(9-vinylcarbazole) (PVK), and a thin film may be formed by spin-coating the PVK at 1000 to 4000 rpm.

[0083] The light-emitting layer (140) may be a super-fluorescent light-emitting layer disposed on the hole injection layer (120) or hole transport layer (130) and may consist of a host and a dopant for charge transfer.

[0084] The above-mentioned light-emitting layer (140) may be formed by the host and dopant being deposited by a co-deposition method.

[0085] The light-emitting layer (140) is 1×10 -5 Torr to 1×10 -8It may be deposited under vacuum conditions of Torr.

[0086] The host is, for example, 9-(3-(triphenylsilyl)phenyl)-9H-3,9'-bicarbazole (SiCzCz), 9,9'-(6-(3-(Triphenylsilyl)phenyl)-1,3,5-triazine-2,4-diyl)bis(9H-carbazole) (SiTrzCz2), 4,4',4"-tris(N-carbazolyl)-triphenylamine (TCTA), 1,3,5-tris(N phenylbenzimidazole-2-yl)benzene (TPBi), tris(2,4,6-trimethyl-3-(pyridin-3-yl)phenyl)borane (3TPYMB), 1,3-bis(3,5-dipyridin-3-ylphenyl)benzene (BmPyPB), It may be selected from 9,9-bis(4-(9H-carbazol-9-yl)phenyl)-9H-fluorene (BSFM), 1,3-bis(9-carbazolyl)benzene (mCP), 4,4'-Bis(N-carbazolyl)-1,1'-biphenyl (CBP), 3,3-bis(carbazol-9-yl)biphenyl (mCBP), or mixtures thereof, but is not limited thereto, and specifically, SiCzCz and SiTrzCz2 are more preferable.

[0088] The above host may consist of a pair of hole-transporting hosts and electron-transporting hosts forming an exciplex, for example, 9-(3-(triphenylsilyl)phenyl)-9H-3,9'-bicarbazole (SiCzCz) and 9,9'-(6-(3-(Triphenylsilyl)phenyl)-1,3,5-triazine-2,4-diyl)bis(9H-carbazole) (SiTrzCz2); 4,4',4"-tris(N-carbazolyl)-triphenylamine (TCTA) and 1,3,5-tris(N-phenylbenzimidazole-2-yl)benzene (TPBi); 4,4',4"-tris(N-carbazolyl)-triphenylamine (TCTA) and tris(2,4,6-trimethyl-3-(pyridin-3-yl)phenyl)borane (3TPYMB); An exciplex can be formed by selecting from the group consisting of 4,4',4"-tris(N-carbazolyl)-triphenylamine (TCTA) and 1,3-bis(3,5-dipyridin-3-ylphenyl)benzene (BmPyPB); or 4,4',4"-tris(N-carbazolyl)-triphenylamine (TCTA) and 9,9-bis(4-(9H-carbazol-9-yl)phenyl)-9H-fluorene (BSFM).

[0090] The above dopant may be selected from Platinum(II) 9-(4-(tert-butyl)pyridin-2-yl)-2-(3-(3-(quinolin-2-ylmethyl)-2,3-dihydro-1H-benzo[d]imidazol-1-yl)phenoxy)-9H-carbazole (Q(Bn)_Pt), N7,N7,N13,N13,5,15-hexaphenyl-9,11-bis(4-(tert-butyl)phenyl)-5,9,11,15-tetrahydro-5,9,11,15-tetraaza-19b,20b-diboradinaphtho [3,2,1-de:1',2',3'-jk]pentacene-7,13-diamine (t-Bu-v-DABNA) or a mixture thereof.

[0092] The first electron transport layer (150) may be disposed on the light-emitting layer (140) and may be composed of a material containing a chemical component that primarily attracts electrons. For this purpose, high electron mobility is required, and electrons can be stably supplied to the light-emitting layer (140) through smooth electron transport.

[0093] The first electron transport layer (150) and the second electron transport layer (160) may be selected from 2-Phenyl-4,6-bis(3-(triphenylsilyl)phenyl)-1,3,5-triazine (mSiTrz), 9,9'-(6-(3-(Triphenylsilyl)phenyl)-1,3,5-triazine-2,4-diyl)bis(9H-carbazole) (SiTrzCz2), 1,3,5-tris(N-phenylbenzimidazole-2-yl)benzene (TPBi), 1,3,5-tri(m-pyridin-3-ylphenyl)benzene (TmPyPB), 2-(4-(9,10-di(naphthalen-2-yl)anthracen-2-yl)phenyl)-1-phenyl-1H-benzo[d]imidazole (LG201) or a mixture thereof. However, it is not limited to this, and specifically, it is more preferable that it be mSiTrz and TPBi.

[0095] The electron injection layer (170) may be disposed on the second electron transport layer (160) and may be formed as a single layer in which electron injection and electron transport occur simultaneously, and may use the same material as the example of the electron transport layer (150, 160), or may be selected from lithium fluoride (LiF), (8-quinolinolato)lithium (Liq), 2,6-bis(1,3,4,6,7,8-tetrahydro-2H-pyrimido[1,2-a]pyrimidin-1-yl) pyridine (Py-hpp2), or a mixture thereof, but is not limited thereto.

[0097] The above electronic device may be a phosphorescent-sensitive superfluorescent organic electroluminescent device that emits a deep blue color.

[0098] The bare glass (G) of the above electronic device (100) is a substrate for coating the first electrode (110), and other usable materials may be selected from flexible and transparent materials such as quartz plates, PET (polyethyleneterephthalate), PEN (polyethylene naphthelate), PP (polyperopylene), PI (polyimide), PC (polycarbonate), PS (polystyrene), POM (polyoxyethylene), AS resin (acrylonitrile styrene copolymer), ABS resin (acrylonitrile butadienestyrene copolymer), and TAC (triacetyl cellulose), but are not limited thereto.

[0100] The thickness of each layer constituting the electronic device according to the present invention is preferably a first electrode (ITO) / hole injection layer (PSBM-EDT, 45-50 nm) / hole transport layer (PVK, 15 nm) / emissive layer (EML, 60 nm) / first electron transport layer (mSiTrz, 5 nm) / second electron transport layer (TPBi, 10 nm) / electron injection layer (LiF, 1 nm) / second electrode (Al, 100 nm), but is not limited thereto.

[0102] An organic solar cell comprising a polythiophene-based conductive polymer derivative having an alkylene sulfonic acid side chain according to another preferred embodiment of the present invention will be described with reference to the attached drawings.

[0103] For reference, FIG. 3 illustrates an organic solar cell device according to Manufacturing Example 2 of the present invention.

[0105] As illustrated in FIG. 3, the present invention provides an organic solar cell (200) comprising: a first electrode (210); a hole transport layer (220) disposed on the first electrode (210); a photoactive layer (230) disposed on the hole transport layer (220); an electron transport layer (240) disposed on the photoactive layer (230); and a second electrode (250) disposed on the electron transport layer (240).

[0107] The first electrode (210) above is bare glass (G ) It is deposited on the surface and treated with UV-ozone for 20 minutes to remove organic matter from the surface and make it hydrophilic.

[0108] The first electrode (210) above is a material that has a large work function and can accept holes well, and it is preferable to use ITO (indium tin oxide), but other materials such as those described in the description of the organic electronic device may also be used.

[0110] It is preferable to form a film with a thickness of 10 nm on an ITO, which is a first electrode (210) that has been sufficiently mixed with PSBM-EDT and then heated at 150°C for 20 minutes on a hot plate.

[0112] The photoactive layer (230) may include one or more types selected from the group consisting of photoactive molecules such as non-fullerene electron donors and fullerene electron acceptors, and may include a bulk heterojunction (BHJ) structure in which electron donors and electron acceptors are stacked in a mixed state.

[0114] 상기 비풀러렌계 전자주개는 PBDB-T-2F (PM6, poly[(2,6-(4,8-bis(5-(2-ethylhexyl-3-fluoro)thiophen-2-yl)-benzo[1,2-b:4,5-b']dithiophene))-alt-(5,5-(1',3'-di-2-thienyl-5',7'-bis(2-ethylhexyl)benzo[1',2'-c:4',5'-c']dithiophene-4,8-dione)]), PBDB-T-2Cl (PM7, Poly[(2,6-(4,8-bis(5-(2-ethylhexyl-3-chloro)thiophen-2-yl)-benzo[1,2-b:4,5-b']dithiophene))-alt-(5,5-(1',3'-di-2-thienyl-5',7'-bis(2-ethylhexyl)benzo[1',2'-c:4',5'-c']dithiophene-4,8-dione)]), PTB7 (poly[[4,8-bis[(2-ethylhexyl)oxy]benzo[1,2-b:4,5-b']dithiophene-2,6-diyl][3-fluoro-2-[(2-ethylhexyl)carbonyl]thieno[3,4-b]thiophenediyl]]), PCPDTBT (poly[2,6-(4,4-bis-(2-ethylhexyl)-4H-cyclopenta[2,1-b;3,4-b']dithiophene)-alt-4,7-(2,1,3-benzothiadiazole)]), PDPP2T-TT (poly[3,6-bis(5-thiophen-2-yl)-2,5-bis(2-octyldodecyl)pyrrolo[3,4-c]pyrrole-1,4(2H,5H)-dione-2,2'-diyl-alt-thieno[3,2-b]thiophen-2,5-diyl]), PPV (poly(p-phenylene vinylene)), MDMO-PPV (poly(2-methoxy-5-(3',7'-dimethyloctyloxy)-1,4-phenylenevinylene)), MEH-PPV (poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenylenevinylene]), P3HT (poly(3-hexylthiophene)), and It may be one or more selected from the group consisting of PBDTTT-CF (poly[1-(6-{4,8-bis[(2-ethylhexyl)oxy]-6-methylbenzo[1,2-b:4,5-b]dithiophen-2-yl}-3-fluoro-4-methylthieno[3,4-b]thiophen-2-yl)-1-octanone]), preferably PBDB-T-2F (PM6), but is not limited thereto.;

[0115] 상기 비풀러렌계 전자받개는 L8-BO (2,2'-((2Z,2'Z)-((12,13-bis(2-ethylhexyl)-3,9-(2-butyloctyl)-12,13-dihydro -[1,2,5]thiadiazole[3,4-e]thieno[2'',3'':4',5']thieno[2',3':4,5]pyrrolo[3, 2-g]thieno[2',3':4,5]thieno[3,2-b]indole-2,10-diyl)bis(methanylylidene))bis(5,6-difluoro-3-oxo-2,3-dihydro-1H-indene-2,1-diylidene))dimalononitrile), Y6 (BTP-4F, 2,2'-((2Z,2'Z)-((12,13-bis(2-ethylhexyl)-3,9-diundecyl-12,13-dihydro-[1,2,5]thiadiazolo[3,4-e]thieno[2'',3'':4',5']thieno[2'',3',3'':4',5']thieno[2',3',3',3'[ ]thieno[2',3':4,5]thieno[3,2-b]indole-2,10-diyl)bis(methanylylidene))bis(5,6-difluoro-3-oxo-2,3-dihydro-1H-indene-2,1-diylidene))dimalononitrile), Y7 (BTP-4Cl, 2,2'-((2Z,2'Z)-((12,13-bis(2-ethylhexyl)-3,9-diundecyl-12,13-dihydro-[1,2,5]thiadiazolo[3,4-e]thieno[2'',3'':4',5']thieno[2'',3',3'':4',5']thieno[2',3',3',3'[ ]thieno[2',3':4,5]thieno[3,2-b]indole-2,10-diyl)bis(methanylylidene))bis(5,6-dichloro-3-oxo-2,3-dihydro-1H-indene-2,1-diylidene))dimalononitrile), Y6-BO (BTP-4F-12, Y12, 2,2'-((2Z,2'Z)-((12,13-bis(2-butyloctyl)-3,9-diundecyl-12,13-dihydro-[1,2,5]thiadiazolo[3,4-e]thieno[2'',3'':4',5']thieno[2',3':4,5]pyrrolo[3,2-g]thieno[2',3':4,5]thie no[3,2-b]indole-2,10-diyl)bis(methanylylidene))bis(5,6-difluoro-3-oxo-2,3-dihydro-1H-indene-2,1-diylidene))dimalononitrile), and Y7-BO (BTP-4Cl-12, It may be one or more selected from the group consisting of 2,2'-((2Z,2'Z)-((12,13-bis(2-butyloctyl)-3,9-diundecyl-12,13-dihydro-[1,2,5]thiadiazolo[3,4-e]thieno[2'',3'':4',5']thieno[2',3':4,5]pyrrolo[3,2-g]thieno[2',3':4,5]thieno[3,2-b]indole-2,10-diyl)bis(methanylylidene))bis(5,6-dichloro-3-oxo-2,3-dihydro-1H-indene-2,1-diylidene))dimalononitrile), preferably selected from L8-BO, but is not limited thereto.

[0117] The above photoactive layer (230) is formed by dissolving an electron donor PM6 and an electron acceptor L8-BO in chlorobenzene, blending with 0.3 wt.% of 1-chloronaphthalene (1-CN) as an additive, and then spin-coating at 3800–4200 rpm. It is desirable to form a thin film of 120 nm.

[0119] The electron transport layer (240) functions to transport electrons generated in the photoactive layer (230) to the second electrode (250) and can be formed of PDINO (N,N'-Bis(N,N-dimethylpropan-1-amine oxide)perylene-3,4,9,10-tetracarboxylic diimide) or a metal oxide, such as a nanoparticle oxide of zinc oxide (ZnO), titanium dioxide (TiO2), tin dioxide (SnO2), etc., and preferably can be selected from PDINO, but is not limited thereto.

[0120] The electron transport layer (240) can be formed by spin-coating PDINO at 3800 to 4200 rpm to form a thin film of 12 nm.

[0122] The second electrode (250) is a material that can effectively move electrons into an electric conductor, and while it is preferable to use silver (Ag), other materials such as those described above for organic electronic devices may also be used.

[0123] It is preferable to load the second electrode (250) into a vacuum chamber and deposit silver (Ag) to a thickness of 120 nm in a vacuum.

[0125] The thickness of each layer constituting the organic solar electronic device according to the present invention is preferably a first electrode (ITO) / hole transport layer (PSBM-EDT) (10 nm) / photoactive layer (PM6:L8-BO) (120 nm) / electron transport layer (PDINO) (12 nm) / second electrode (Ag) (120 nm), but is not limited thereto.

[0127] Infrared shielding compositions characterized by comprising a polythiophene-based conductive polymer derivative having an alkylene sulfonic acid side chain according to another preferred embodiment of the present invention; a polyurethane-based (PU) binder; and a solvent will be described with reference to the attached drawings.

[0128] The above polyurethane-based (PU) binder may be included in an amount of 100 to 300 parts by weight per 100 parts by weight of the conductive polymer derivative.

[0129] The above infrared shielding composition is characterized by the introduction of a polythiophene-based conductive polymer derivative with an alkylene sulfonic acid side chain into a solution or film, which improves heat detection avoidance, i.e., infrared shielding and stealth performance, with a transmittance of less than 10% in the infrared region from 2,500 nm to 25,000 nm.

[0130] For example, the above solution can be impregnated into a fiber to form an infrared shielding layer, wherein the fiber may be one or more selected from the group consisting of polyester fiber, polyamide fiber, acrylic fiber, polyolefin fiber, rayon fiber, and cotton fiber.

[0131] For example, the above film can form an infrared shielding layer by applying the infrared shielding composition to the surface of a polyethylene terephthalate film, a polyimide film, a polycarbonate film, a polypropylene film, or a polyethylene film, followed by solvent removal and thermal annealing.

[0133] Hereinafter, the present invention will be described in detail with reference to examples to aid in understanding. However, the following examples are merely illustrative of the content of the present invention and the scope of the present invention is not limited to the following examples.

[0135] 1. Synthesis of the conductive polymer poly[4-[(2,3-dihydrothieno[3,4-b][1,4]dioxin-2-yl)methoxy]butane-1-sulfonic acid] : PSBM-EDT}

[0136] <Example 1> Synthesis of Poly[4-[(2,3-dihydrothieno[3,4-b][1,4]dioxin-2-yl)methoxy]butane-1-sulfonate]{Poly[sodium 4-[(2,3-dihydrothieno[3,4-b][1,4]dioxin-2-yl)methoxy]butane-1-sulfonate] : PSBM-EDT-Na}

[0137] In Example 1, the compound PSBM-EDT was synthesized according to the procedure briefly illustrated in Reaction Scheme 1 below.

[0139] [Reaction Equation 1]

[0140]

[0142] <Example 1.1> Synthesis of 2-(Chloromethyl)-2,3-dihydrothieno[3,4-b]-1,4-dioxin {2-(Chloromethyl)-2,3-dihydrothieno[3,4-b]-1,4-dioxin: 3}

[0143] 3,4-dimethoxythiophene (compound 1,3,4-dimethoxythiophene, 22 g, 152.6 mmol), 3-chloro-1,2-propanediol (compound 2,3-chloro-1,2-propanediol, 50.6 g, 457.8 mmol), methanesulfonic acid (2 mL, 30 mmol), and 2,6-di-tert-butyl-4-methylphenol (0.03 g, 0.1 mmol) were dissolved in a 500 mL toluene solution under a nitrogen atmosphere at 110°C o Stir at C for 24 hours.

[0144] After the reaction is finished, the reaction mixture is cooled to room temperature, and the organic reactant is extracted three times with ethyl acetate, washed with brine, and then washed again with an aqueous solution of sodium carbonate (Na2CO3). After removing the organic solvent by vacuum distillation of the organic reactant using a rotary evaporator, the product is separated by column chromatography using hexane / ethyl acetate as the developing solvent in a ratio of 10:0.5 to 10:1 (v / v), yielding a colorless compound 3, (2-(chloromethyl)-2,3-dihydrothieno[3,4-b]-1,4-dioxine), (22 g, 115.4 mmol)) with a yield of 76%.

[0145] Compound 3: 1 H NMR (400 MHz, CDCl3, δ (ppm)): 6.38-6.40 (q, 2H), 4.37-4.42 (m, 1H), 4.29-4.32 (dd, 1H), 4.16-4.20 (q, 1H), 3.67-3.77 (m, 2H).

[0147] <Example 1.2> Synthesis of (2,3-Dihydrothieno[3,4-b]-1,4-dioxin-2-yl)methyl acetate {(2,3-Dihydrothieno[3,4-b]-1,4-dioxin-2-yl)methyl acetate: 4}

[0148] In a three-necked flask, compound 3 synthesized in Example 1.1 (2-(chloromethyl)-2,3-dihydrothieno[3,4-b][1,4]dioxine (2-(chloromethyl)-2,3-dihydrothieno[3,4-b][1,4]dioxine, 22 g, 115.4 mmol)) and potassium acetate (45.3 g, 461.6 mmol) were dissolved in dimethyl sulfoxide (DMSO, 500 mL), and then 110 o The reaction is carried out at C for 6 hours under a nitrogen atmosphere while stirring.

[0149] After cooling the reaction mixture to room temperature, washing it three times with iced water and removing moisture with anhydrous sodium sulfate, the organic reactant is subjected to vacuum distillation using a rotary evaporator to remove the organic solvent, and then the product is separated by column chromatography using hexane / ethyl acetate as the developing solvent in a ratio of 10:1 to 10:2 (v / v), resulting in a colorless compound 4, ((2,3-dihydrothieno[3,4-b][1,4]dioxin-2-yl)methyl acetate, 20g, 93.35 mmol) with a yield of 81%.

[0150] Compound 4: 1 H NMR (400 MHz, CDCl3, δ (ppm)):: 6.37-6.40 (q, 2H), 4.38-4.43 (m, 1H), 4.32-4.33 (dd, 2H), 4.23-4.27 (dd, 1H), 4.04-4.09 (m, 1H), 2.14 (s, 3H).

[0152] <Example 1.3> Synthesis of (2,3-Dihydrothieno[3,4-b][1,4]dioxin-2-yl)methanol {(2,3-Dihydrothieno[3,4-b][1,4]dioxin-2-yl)methanol: 5}

[0153] Dissolve sodium hydroxide (33 g, 825 mmol) in distilled water (450 mL) in a three-necked flask. Then, add compound 4 ((2,3-dihydrothieno[3,4-b][1,4]dioxin-2-yl)methyl acetate) (22 g, 102.7 mmol) and the reaction mixture 7 o Stirring at C for 3 hours. After cooling the reaction mixture to room temperature, the reaction product is extracted with ethyl acetate, water is removed with sodium sulfate, and the organic solvent is removed by vacuum distillation of the organic reactant using a rotary evaporator. Then, the product is separated by column chromatography using hexane / ethyl acetate as the developing solvent in a ratio of 10:2.5 (v / v), and a white solid compound 5, (2,3-dihydrothieno[3,4-b][1,4]dioxin-2-yl)methanol, (15 g, 87.41 mmol)) can be synthesized with a yield of 85%.

[0154] Compound 5: 1 H NMR (400 MHz, CDCl3, δ (ppm)):: 6.36-6.38 (q, 2H), 4.24-4.30 (m, 2H), 4.10-4.15 (dd, 1H), 3.84-3.94 (m, 2H).

[0156] <Example 1.4> Synthesis of 4-[(2,3-dihydrothieno[3,4-b][1,4]dioxin-2-yl)methoxy]butane-1-sulfonate {Sodium 4-[(2,3-dihydrothieno[3,4-b][1,4]dioxin-2-yl)methoxy]butane-1-sulfonate : SBM-EDT-Na, 6}

[0157] 0 in a three-necked flask under a nitrogen atmosphere oSodium hydride (1.7 g, 70.8 mmol) is added to tetrahydrofuran (THF, 100 mL) at C and stirred. Compound 5 (2,3-dihydrothieno[3,4-b][1,4]dioxin-2-yl)methanol (10 g, 58.1 mmol) is dissolved in tetrahydrofuran (THF, 100 mL) and slowly added dropwise to a three-necked flask, then stirred at 60 °C for 1 hour. After cooling the reaction mixture to -20 °C, 2,4-butanesultone (9.5 g, 69.8 mmol) dissolved in tetrahydrofuran (THF, 100 mL) is slowly added to the flask. The reaction mixture is stirred at 60 °C for 6 hours, then methanol is added to terminate the reaction. After removing the organic solvent by vacuum distillation of the organic reactants, the product can be separated by column chromatography using methylene chloride / methanol as the developing solvent in a ratio of 10:0.5-10:1 (v / v), thereby synthesizing the white solid compound 6, (4-[(2,3-dihydrothieno[3,4-b][1,4]dioxin-2-yl)methoxy]butane-1-sulfonate {Sodium 4-[(2,3-dihydrothieno[3,4-b][1,4]dioxin-2-yl)methoxy]butane-1-sulfonate : SBM-EDT-Na, (11.6 g, 35.1 mmol)) with a yield of 60%.

[0158] SBM-EDT-Na : 1 HNMR (400MHz, CDCl3, δ): 6.57-6.60 (q, 2H), 4.23-4.32 (m, 2H), 3.94-3.99(dd, 1H), 3.55-3.62 (m, 2H), 3.41-3.44 (t, 2H), 2.39-2.43 (t, 2H), 1.54-.62 (m, 4H).

[0160] <Example 2> Polymerization method of multifunctional conductive polymer derivative

[0161] PSBM-EDOT, a multifunctional conductive polymer, was synthesized by polymerizing compound 6 into monomers according to the procedure briefly illustrated in reaction scheme 2.

[0162] [Reaction Equation 2]

[0163]

[0165] <Example 2.1> Synthesis of Poly[4-[(2,3-dihydrothieno[3,4-b][1,4]dioxin-2-yl)methoxy]butane-1-sulfonate]{Poly[sodium 4-[(2,3-dihydrothieno[3,4-b][1,4]dioxin-2-yl)methoxy]butane-1-sulfonate] : PSBM-EDT-Na, 7}

[0166] Sodium (4-[(2,3-dihydrothieno[3,4-b][1,4]dioxin-2-yl)methoxy]butane-1-sulfonate) (3 g, 151 mmol) and FeSO4·7H2O (1.54 g, 5.54 mmol) were added to a 1 M aqueous sulfuric acid solution. (NH4)2S2O8 (4.2 g, 18.18 mmol) was dissolved in ultrapure purified water under a nitrogen atmosphere and added to the reaction mixture. The mixture was then stirred at 20 °C for 3 hours to perform oxidative polymerization. The polymerization reaction product was added dropwise to an excess amount of acetone to precipitate as a solid. The precipitated solid was filtered under nitrogen pressure, washed with acetone, and vacuum dried at 60 °C for 8 hours to obtain a multifunctional conductive polymer precursor (7, yield 60%, 1.8 g).

[0168] <Example 2.2> Synthesis of Poly[4-[(2,3-dihydrothieno[3,4-b][1,4]dioxin-2-yl)methoxy]butane-1-sulfonic acid] : PSBM-EDT [Ion exchange, dialysis and coagulation]

[0169] A 1.9 wt.% solution was prepared by dissolving 7 (1.8 g) of a multifunctional conductive polymer precursor in water (105 g), and 22.2 g of H-Type cation exchange resin (Lewatit Monoplus S108H) was added and stirred at room temperature for 3 hours. Once ion exchange (Na→H) was completed, the ion exchange resin was filtered and washed with water (100 mL) to obtain a PSBM-EDOT aqueous solution. Inorganic salts were removed by dialysis using a Spectra / Por 3 RC dialysis membrane (MWCO 3.5 kD) until the yellow color of the dialyzed aqueous solution disappeared.

[0170] After completing the dialyzation of the PSBM-EDOT aqueous solution, the water was distilled using a rotary evaporator to concentrate the PSBM-EDOT solution, and then the PSBM-EDOT was precipitated by adding it dropwise to acetone (500 mL). The precipitated PSBM-EDOT was filtered using nitrogen pressure, washed with acetone, and vacuum dried at 60°C for 8 hours to obtain PSBM-EDOT (yield 70%, 1.26 g).

[0172] 2. Fabrication of deep blue phosphorescence-sensitive superfluorescent organic electroluminescent devices and organic solar cells

[0173] <Preparation Example 1> Preparation of a deep blue phosphorescence-sensitive superfluorescent organic electroluminescent device using PSBM-EDT as a hole injection layer

[0174] The ITO-deposited glass was treated with UV-ozone for 20 minutes to remove surface organic matter and make it hydrophilic. PSBM-EDT, serving as the hole injection layer (HIL), was thoroughly mixed, and a 45–50 nm layer was applied to the UV-ozone-treated ITO using the spin-coating method. After forming the film, it was heated on a hot plate at 150°C for 20 minutes. A hole transport layer (HTL) PVK (0.5 wt.%, cyclohexanone) was spin-coated at 2000 rpm to form a 15 nm thin film.

[0175] Afterwards, load into a vacuum chamber and 1×10 -7 To deposit an emission layer (EML) under a Torr vacuum, SiCzCz and SiTrzCz2 were applied as hosts, and Q(Bn)_Pt and t-Bu-v-DABNA were deposited at 60 nm using a co-deposition method with various compositions. After forming the thin film, electron transport layers (ETL) of mSiTrz (5 nm) and TPBi (10 nm) were deposited in sequence. 1 nm of LiF and 100 nm of aluminum were deposited in a chamber separated from the organic chamber to prevent contamination by the organic material.

[0177] The abbreviations of the compounds used in the manufacture of the above phosphorescent-sensitive superfluorescent organic electroluminescent device are summarized as shown in [Table 1] below.

[0178] abbreviation Full name (Korean / English) PVK Poly(9-vinylcarbazole) mSiTrz 2-Phenyl-4,6-bis(3-(triphenylsilyl)phenyl)-1,3,5-triazine TPBi 2,2,2"-(1,3,5-benzinetriyl)-tris(1-phenyl-1-H-benzimidazole) SiCzCz 9-(3-(triphenylsilyl)phenyl)-9H-3,9'-bicarbazole SiTrzCz2 9,9'-(6-(3-(triphenylsilyl)phenyl)-1,3,5-triazine-2,4-diyl)bis(9H-carbazole) t-Bu-ν-DABNA N7,N7,N13,N13,5,15-hexaphenyl-9,11-bis(4-(tert-butyl)phenyl)-5,9,11,15-tetrahydro-5,9,11,15-tetraaza-19b,20b-diboradinaphtho[3,2,1-de:1',2',3'-jk]pentacene-7,13-diamine Q(Bn)_Pt Platinum(II) 9-(4-(tert-butyl)pyridin-2-yl)-2-(3-(3-(quinolin-2-ylmethyl)-2,3-dihydro-1H-benzo[d]imidazol-1-yl)phenoxy)-9H-carbazole

[0180] <Preparation Example 2> Preparation of an organic solar cell device using PSBM-EDT as a hole transport layer

[0181] UV-ozone treatment was applied to the glass coated with ITO for 20 minutes to remove organic matter from the surface and make it hydrophilic. PSBM-EDT, a hole transport layer (HTL), was thoroughly mixed, and a film with a thickness of 10 nm was formed on the UV-ozone-treated ITO using a spin coating method, after which it was heated at 150 ℃ for 20 minutes on a hot plate.

[0182] PM6 and L8-BO, which are photoactive layers, were dissolved in chlorobenzene, blended with 0.3 wt.% of 1-chloronaphthalene (1-CN) as an additive, and spin-coated at 4000 rpm to form a 120 nm thin film. PDINO was spin-coated at 4000 rpm as an electron transport layer (ETL) to form a 12 nm thin film.

[0183] Afterwards, load into a vacuum chamber and 1×10 -7 Silver (Ag) in a vacuum of Torr It was deposited to a thickness of 120 nm.

[0184] The above organic solar cell device structure is ITO / PSBM-EDT (10 nm) / PM6:L8-BO (120 nm) / PDINO (12 nm) / Ag (120 nm).

[0186] The abbreviations of the compounds used in the manufacture of the above organic solar cell device are summarized as shown in [Table 2] below.

[0187] abbreviation Full name (Korean / English) PDINO N,N'-Bis(N,N-dimethylpropan-1-amine oxide)perylene-3,4,9,10-tetracarboxylic diimide PM6 Poly[(2,6-(4,8-bis(5-(2-ethylhexyl-3-fluoro)thiophene-2-yl)-benzo[1,2-b:4,5-b']dithiophene))-alt-(5,5-(1',3'-di-2-thienyl-5',7'-bis(2-ethylhexyl)benzo[1',2'-c:4',5'-c']dithiophene-4,8-dione)) / Poly[(2,6-(4,8-bis(5-(2-ethylhexyl-3-fluoro)thiophen-2-yl)-benzo[1,2-b:4,5-b']dithiophene))-al t-(5,5-(1',3'-di-2-thienyl-5',7'-bis(2-ethylhexyl)benzo[1',2'-c:4',5'-c']dithiophene-4,8-dione)] L8-BO 2,2'-((2Z,2'Z)-((12,13-bis(2-ethylhexyl)-3,9-(2-butyloctyl)-12,13-dihydro-[1,2,5]thiadiazole[3,4-e]thieno[2'',3'':4',5']thieno[2',3':4,5]pyrrolo[3,2-g]thieno[2',3':4,5]thieno[3,2-b]indole-2,10-diyl)bis(methanylylidene))bis(5,6-difluoro-3-oxo-2,3-dihydro-1H-indene-2,1-diylidene))dimalononitrile / 2,2'-((2Z,2'Z)-((12,13-bis(2-ethylhexyl)-3,9-(2-butyloctyl)-12,13-dihydro-[1,2,5]thiadiazolo[3,4-e]thieno[2'',3'':4',5']thieno[2',3':4,5]pyrrolo[3, 2-g]thieno[2',3':4,5]thieno[3,2-b]indole-2,10-diyl)bis(methanylylidene))bis(5,6-difluoro-3-oxo-2,3-dihydro-1H-indene-2,1-diylidene))dimalononitrile

[0189] 3. Characterization of conductive polymer derivatives, phosphorescence-sensitive superfluorescent organic electroluminescent devices, and organic solar cells

[0190] 3-1. Experimental Method

[0191] 11H NMR spectra were recorded on a Bruker 400 MHz spectrometer in CDCl3 and DMSO-d6 using tetramethylsilane as an internal reference. Chemical shifts were for CDCl3 and DMSO-d6, respectively. 1 It was reported as a singlet at 7.26 and 2.54 ppm in 1H NMR.

[0192] UV-Vis and emission spectra were reported at room temperature using JASCO V-570 and Hitachi F-4500 fluorescence spectrophotometers. Photoluminescence (PL) measurements were performed at room temperature using a compact fluorescence lifetime spectrometer C11367. Thermal analysis was performed using a Mettler Toledo TGA / SDTA 851e analyzer at a heating rate of 10°C / min under a nitrogen atmosphere.

[0193] Cyclic voltammetry (CV) analysis was performed using a CHI 600C potentiostat (CH Instruments) at a scan rate of 100 mV / s in anhydrous DCM solvent using 0.1 M TBAClO4 (Tetrabutylammonium Perchlorate) as the supporting electrolyte. A platinum wire was used as the counter electrode, and an Ag / AgCl electrode was used as the reference electrode. The potential was determined by the ferrocene / ferrocenium redox couple (Fc / Fc + It was based on ).

[0194] Layer thickness was measured using an Alpha-step IQ surface profiler (KLA Tencor, San Jose, CA). Current density, voltage, and luminance characteristics were measured, and electroluminescence (EL) spectrum analysis was performed using a Keithley 2635A source meter and a CS2000 spectroradiometer (Konica Minolta).

[0195] External quantum efficiency (EQE), current efficiency (CE), and power efficiency (PE) values ​​were determined using the M6100 electrical analysis system (McScience).

[0197] 3-2. Experimental Results

[0198] <Experimental Example 1> 4-Point Probe Conductivity Measurement and Characteristics

[0199] A PSBM-EDT / IPA aqueous solution was prepared by dissolving the synthesized PSBM-EDT in a 50% isopropyl alcohol (IPA) aqueous solution at a concentration of 1 wt.% using an ultrasonic disperser (Ultrasonic Homogenizer STH-750S, Sonictopia).

[0200] A film was prepared by spin-coating an aqueous PSBM-EDT / IPA solution onto a bare glass substrate (25 mm length, 25 mm width, 0.7 mm thickness) using a spin-coating machine (Spin-1200T, MIDAS) at a speed of 2000 rpm / 20 sec to 4000 rpm / 10 sec, and then annealing was performed at 160 ℃ for 20 minutes under atmospheric pressure conditions using a hot plate to prepare a solid thin film.

[0201] The thickness of the solid thin film was measured to be 57 nm using an Alpha-step instrument (Alpha-step IQ, KLA-Tencor), and the conductivity was measured after measuring the surface resistance using a 4-Point Probe surface resistance meter (Keithley 2400 source meter, JANDEL 4-Point Probe Head), resulting in a conductivity of 120 S / cm.

[0203] <Experimental Example 2> Luminescence Characteristics of Deep Blue Phosphorescence-Sensitive Superfluorescent Organic Electroluminescent Device

[0204] FIGS. 2a, 2b, 2c, and 2d respectively show the current density-voltage-luminance, EL spectrum, luminance-external quantum efficiency, and luminance-current efficiency-power efficiency of a deep blue phosphorescent-sensitive superfluorescent electronic device according to an embodiment of the present invention.

[0206] Referring to FIGS. 2a to 2d, the turn-on voltage is 5.5 V, the maximum emission peak is 468 nm, the color coordinates are (0.132, 0.122), indicating a deep blue color, and the maximum luminance is 11406 cd / m². 2 It can be seen that the maximum external quantum efficiency, current efficiency, and power efficiency are 6.9%, 6.8 cd / A, and 2.7 lm / W, respectively.

[0208] The results of the characteristic evaluation of the above electronic device are shown in [Table 3] and [Table 4] below.

[0209] (Driving voltage, luminance, EL spectrum, and CIE color coordinates) division Voltage(V) Luminance(cd / m 2 ) ELmax(nm) CIE(x,y) Turn-on At 1000 cd / m 2 Max. At 10 mA / m 2 At 10 mA / m 2 PSBM-EDT 5.5 8.4 11406 468 (0.132, 0122)

[0210] (External quantum efficiency, current efficiency, and power efficiency) division EQE(%) Current efficiency(cd / A) Power efficiency (Im / W) Max. At 1000 cd / m 2 Max. At 1000 cd / m 2 Max. At 1000 cd / m 2 PSBM-EDT 6.9 6.8 6.8 6.7 2.7 2.5

[0212] <Experimental Example 3> Luminescence Characteristics of Organic Solar Cell Devices

[0213] Figure 4 shows the voltage-current density characteristics of an organic solar cell device according to an embodiment of the present invention.

[0214] Referring to Fig. 4, Voc (Open-circuit voltage) is 0.84 V and Jsc (Short-circuit current density) is 16.2 mA / cm 2 It can be seen that the fill factor is 60.7% and the power conversion efficiency is 8.3%.

[0215] The results of the characteristic evaluation of the above organic solar cell device are shown in [Table 5] below.

[0216] Photoactive layer (Active layer) Voc(V) Jsc(mA / cm 2 ) FF(%) PCE(%) PM6;L8-BO containing PSBM-EDT 1 wt.% 0.84 16.2 60.7 8.3

[0218] 4. Preparation of infrared shielding coating composition and fiber

[0219] <Preparation Example 3> Preparation of a coating liquid composition for heat detection evasion, infrared shielding, or stealth containing PSBM-EDT

[0220] A solution was prepared by dissolving and dispersing poly[4-[(2,3-dihydrothieno[3,4-b][1,4]dioxin-2-yl)methoxy]butane-1-sulfonic acid][Poly{4-[(2,3-dihydrothieno[3,4-b][1,4]dioxin-2-yl)methoxy]butane-1-sulfonic acid (hereinafter referred to as 'PSBM-EDT')) at a concentration of 1 wt.% in a solvent composed of 30% water and 70% isopropyl alcohol, and then filtering the solution through a 0.45 micrometer sealing paper filter. A polyurethane dispersion solution was added to the above solution, in an amount of approximately twice the weight of the solid content (PSBM-EDT) in the above solution. Subsequently, the solution was stirred sufficiently to prepare an impregnation solution. After impregnating the fiber with the above impregnation solution, the fiber was heat-treated for 45 minutes at 120 degrees Celsius using a hot air circulating dryer for solvent removal and thermal annealing to produce an infrared-shielding fiber.

[0222] <Experimental Example 4> Evaluation of a heat detection evasion, infrared shielding, or stealth coating liquid composition containing PSBM-EDT

[0223] Figure 5 shows the transmittance characteristics of PSBM-EDT synthesized according to a preferred embodiment of the present invention in the infrared wavelength (2,500-25,000 nm) region.

[0224] Figure 6 is a photograph showing the results of heat detection avoidance, i.e., infrared shielding or stealth, before and after PSBM-EDT synthesized according to a preferred embodiment of the present invention is coated on a fiber.

[0226] Although the polythiophene-based conductive polymer derivative having a preferred alkylene sulfonic acid side chain substituent, the method for manufacturing the same, and the organic electronic device and infrared shielding composition containing the same have been described as described above, those skilled in the art will understand that this is merely an example and that various changes and modifications are possible within the scope of the technical spirit of the present invention. Explanation of the symbols

[0229] 100 : Organic electronic devices 110: First electrode 120: Hole injection layer 130: Hole transport layer 140: Emitting layer 150: 1st electron transport layer 160: 2nd electron transport layer 170: Electron injection layer 180: Second electrode 200 : Organic solar cell device 210: First electrode 220: Hole transport layer 230: Photoactive layer 240: Electron transport layer 250: Second electrode G: Bare glass

Claims

Claim 1 A first electrode; a second electrode formed opposite to the first electrode; and one or more organic layers disposed between the first electrode and the second electrode, comprising The above organic layer is, It includes a hole injection layer, a hole transport layer, an emission layer, an electron transport layer, and an electron injection layer, The hole injection layer comprises a conductive polymer derivative having an alkylene sulfonic acid side chain represented by the following chemical formula 1a, and The above light-emitting layer is, As a host forming an exciplex 9-(3-(triphenylsilyl)phenyl)-9H-3,9'-bicarbazole (SiCzCz) and 9,9'-(6-(3-(Triphenylsilyl)phenyl)-1,3,5-triazine-2,4-diyl)bis(9H-carbazole) (SiTrzCz2); and Platinum(II)9-(4-(tert-butyl)pyridin-2-yl)-2-(3-(3-(quinolin-2-ylmethyl)-2,3-dihydro-1H-benzo[d]imidazol-1-yl)phenoxy)-9H-carbazole (Q(Bn)_Pt) as a dopant and N7,N7,N13,N13,5,15-hexaphenyl-9,11-bis(4-(tert-butyl)phenyl)-5,9,11,15-tetrahydro-5, 9,11,15-tetraaza-19b,20b-diboradinaphtho[3,2,1-de:1',2',3'-jk]pentacene-7,13-diamine (t-Bu-v-DABNA); The electronic device is characterized by emitting a deep blue color as a phosphorescence-sensitive superfluorescent organic electroluminescent device, electronic devices [Chemical Formula 1a] (However, in the above chemical formula 1a, n is 10 to 3,000.) Claim 2 delete Claim 3 delete Claim 4 my 1 In the clause, the light-emitting layer is, The above Host and The above An electronic device characterized by a dopant being deposited by a co-deposition method Claim 5 delete Claim 6 delete Claim 7 delete Claim 8 my 1 In the clause, the light-emitting layer is 1×10 -5 Torr to 1×10 -8 An electronic device characterized by being deposited under vacuum conditions of Torr Claim 9 First electrode; A hole transport layer disposed on the first electrode; A photoactive layer disposed on the above-mentioned hole transport layer; An electron transport layer disposed on the above photoactive layer; and It includes a second electrode disposed on the electron transport layer, and The above hole transport layer is do Chemical formula 1a It comprises a conductive polymer derivative having an alkylene sulfonic acid side chain represented by, The above photoactive layer is, Electronic host PBDB-T-2F (PM6, poly[(2,6-(4,8-bis(5-(2-ethylhexyl-3-fluoro)thiophen-2-yl)-benzo[1,2-b:4,5-b']dithiophene))-alt- (5,5-(1',3'-di-2-thienyl-5',7'-bis(2-ethylhexyl)benzo[1',2'-c:4',5'-c']dithiophene-4,8-dione)]); and electronic recipient L8-BO(2,2'-((2Z,2'Z)-((12,13-bis(2-ethylhexyl)-3,9-(2-butyloctyl)-12,13-dihydro-[1,2,5]thiadiazolo[3,4-e]thieno[2'',3'':4',5']thieno[2',3 ':4,5]pyrrolo[3,2-g]thieno[2',3':4,5]thieno[3,2-b]indole-2,10-diyl)bis(methanylylidene))bis(5,6-difluoro-3-oxo-2,3-dihydro-1H-indene-2,1- Contains diylidene))dimalononitrile), The above electron transport layer is, Characterized by including N,N'-bis(N,N-dimethylpropan-1-amineoxide)perylene-3,4,9,10-tetracarboxylic diimide (PDINO), Organic solar cells [Chemical Formula 1a] (However, in the above chemical formula 1a, n is 10 to 3,000.) Claim 10 delete Claim 11 my 9 In the clause, the above photoactive layer is, The above PBDB-T-2F(PM6) and the above L8-BO An organic solar cell characterized by being composed of a bulkhetero junction (BHJ) stacked in a mixed phase Claim 12 delete Claim 13 do A conductive polymer derivative having an alkylene sulfonic acid side chain represented by chemical formula 1a; a polyurethane-based (PU) binder; and a solvent, comprising The above polyurethane-based (PU) binder is included in an amount of 100 to 300 parts by weight per 100 parts by weight of the conductive polymer derivative. Infrared shielding composition [Chemical Formula 1a] characterized by (However, in the above chemical formula 1a, n is 10 to 3,000.) Claim 14 delete

Citation Information

Patent Citations

  • Light emitting device and display apparatus

    JP2026031490A

  • A quinone-based ionic compound, a method for producing the same, transparent near infrared ray shielding film containing the quinone-based ionic compound and a method for producing the same

    KR1020200071039A

  • Intrinsically stretchable organic solar cell, manufacturing method thereof and electronic device using the same

    KR1020210128905A

  • Highly flexible transparent electrode with infrared blocking function and mehtod of manufacturing the same

    KR1020220160334A