Cathode active material coated with lithium carbonate doped with lithium borate and sulfide all-solid-state battery including the same
The use of lithium carbonate doped with lithium borate as a coating for cathode active materials in all-solid-state batteries addresses interfacial resistance and reaction issues, enhancing discharge capacity and cycle life stability.
Patent Information
- Application Number
- KR1020257018073
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2023-12-05
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2043-12-05
AI Technical Summary
Conventional high-capacity cathode active materials (CAMs) for all-solid-state batteries (ASSBs) face interfacial resistance issues due to surface impurities, severe reactions with sulfide solid electrolytes, and low ionic conductivity, leading to deteriorated electrochemical performance.
A cathode active material (CAM) coated with lithium carbonate doped with lithium borate (LCBO) is used, forming a coating layer that enhances ion conductivity and reduces interfacial resistance by minimizing surface impurities and reactions with sulfide solid electrolytes.
The LCBO-coated CAM improves discharge capacity and cycle life stability by maintaining high ion conductivity and reducing degradation, achieving initial discharge capacities up to 219.8 mAh/g and cycle life retention rates of 99.04% after 20 cycles at 0.5C.
Smart Images

Figure 112025061047133-PCT00003_ABST
Abstract
Description
Technology Field
[0001] Cross-reference
[0002] This application claims priority to U.S. Patent Application No. 18 / 194,145 filed on March 31, 2023, and the benefit of U.S. Patent Application No. 63 / 386,183 filed on December 6, 2022, the entire contents of which are incorporated herein by reference in their entirety.
[0003] field
[0004] The present disclosure relates to a cathode active material coated with lithium borate carbonate and a sulfide-based all-solid-state battery (ASSB) comprising the same. Background Technology
[0005] All-solid-state batteries (ASSBs) are considered promising candidates for future energy storage devices because they can use lithium metal as an anode material and can deliver higher specific energy compared to conventional lithium-ion batteries based on organic liquid electrolytes. Sulfide solid electrolyte (SE) materials are in the -2 oxidation state (S -2 It contains sulfur elements and has a narrow intrinsic electrochemical window. Thiophosphate-based solid electrolytes (SEs) contain phosphorus (P) and sulfur (S) elements and are particularly promising due to their high ionic conductivity, excellent mechanical compatibility, and relatively low cost. Passivation of SEs is essential for the reversible operation of all-solid-state batteries. In particular, lithium metal oxide CAMs (e.g., LiNi 0.88 Co 0.09 Al 0.03Interfacial resistance occurs when conventional high-capacity cathode active materials (CAMs), such as O2--NCA88, are applied to ASSBs. Interfacial resistance is attributed to various factors, including surface impurities on the CAM surface, severe reactions between lithium metal oxides and sulfide SEs, space charge layer effects, lattice mismatch, and poor wetting of the SEs. It is known that the electrochemical performance of conventional LIBs deteriorates when surface impurities, such as LiOH and Li2CO3, form on the CAM surface under ambient atmospheric conditions. In the case of ASSBs, S / O exchange at the CAM / SE interface and the low ionic conductivity of surface impurities are major issues. Zhang et al. 1 According to computational modeling, Li in crystalline Li2CO3 + The conductivity is about 10 at room temperature. -10 S cm -1 It has been reported that this can lead to high interfacial resistance.
[0006] Various protective coatings have been developed to lower interfacial resistance. LiNbO3 is approximately 10 -6 S cm -1 high Li + It has conductivity and is one of the most studied coating materials for sulfide ASSBs. US20110045348A1 discloses that coating a LiNbO3 layer on CAM can reduce interfacial resistance.
[0007] However, these coating materials may not completely solve these problems. Zhang et al. 2It has been reported that transition metals can diffuse from CAM into thin film coatings. According to first-principles calculations, the high binding energy of PO₄ groups generates a driving force that induces S / O substitution between oxygen atoms in lithium transition metal oxide coating layers, such as LiNbO₃ and LiTaO₃, and sulfur atoms in sulfide solid electrolytes (SE). Furthermore, the relatively low oxidation limit of these ternary metal oxide coatings raises concerns regarding stability at high voltages. Therefore, there remains a need for additional coating materials and all solid-state batteries containing them.
[0008] In this specification, Li 2+x C 1-x B x A cathode active material (CAM) at least partially coated with lithium carbonate doped with lithium borate having the chemical formula O3 and a method for manufacturing the same are disclosed, wherein 0 <x<0.5이다. 또한, 코팅된 CAM을 포함하는 캐소드 층과 캐소드 층을 포함하는 전고체 배터리가 개시된다. 본 명세서에 개시된 CAM은 붕산 리튬으로 도핑된 탄산 리튬을 포함하며, 이를 전고체 배터리에 통합하면 방전 비용량 및 / 또는 사이클 수명 안정성이 향상된다. 또 다른 측면에서, 본 명세서에서는 표면이 붕산 리튬으로 도핑된 CAM도 개시된다. Brief explanation of the drawing
[0009] FIG. 1 shows CAM particles (1), thin (1-10 nm) LCBO (Li 2+x C 1-x B x It shows a representative structure of a cathode layer comprising a coating layer (2) around a CAM particle composed of O3; 0.00 < x < 0.5), an electronically conductive carbon fiber (3), and a sulfide SE (4). FIG. 2 shows a typical structure of an all-solid-state battery (ASSB) comprising a cathode layer (5), a solid electrolyte (6), an anode layer (7), a first current collector (8-1) in contact with the anode layer, and a second current collector (8-2) in contact with the cathode layer. Figure 3 shows the Li metal anode, LPSCl (Li6PS5Cl) SE, and NCA88 (LiNi) as the CAM. 0.88 Co 0.09 Al 0.03 This shows a plot of specific capacity versus cycles for a half-cell containing a cathode layer with O2 particles and vapor-grown carbon fiber (VGCF). Cycles 1 and 2 are cycled with 0.1C charge / discharge, cycles 3 and 4 are cycled with 0.33C charge / discharge, cycle 5 is cycled with 1.0C charge / discharge, and cycles 6 through 25 are cycled with 0.5C charge / discharge. The cycle plots show Li of approximately 5 nm at x = 0, 0.05, 0.1, 0.15, 0.25, 0.3, 0.5, and 1. 2+x C 1-x B x Compare NCA88 CAM coated with O3. Figure 4 shows a plot of the initial 0.1C discharge specific capacity of a 5 nm LCBO-coated CAM, where x = 0, 0.05, 0.1, 0.15, 0.25, 0.3, 0.5, and 1 (values in Table 1). Figure 5 shows a plot of the cycle life capacity retention rate of a 5 nm LCBO-coated CAM, where x = 0, 0.05, 0.1, 0.15, 0.25, 0.3, 0.5, and 1 (values from Table 1). Figure 6 shows the Li metal anode, LPSCl (Li6PS5Cl) SE, and NCA88 (LiNi) as the CAM. 0.88 Co 0.09 Al 0.03This shows a plot of specific capacity versus cycles at 45°C for a cathode layer containing O2 particles and a half cell containing VGCF. Cycles 1 and 2 are cycled with 0.1C charge / discharge, cycles 3 and 4 are cycled with 0.33C charge / discharge, cycle 5 is cycled with 1.0C charge / discharge, and cycles 6 through 100 are cycled with 0.5C charge / discharge. The cycle plots show Li of approximately 5 nm at x = 0, 0.05, 0.15, and 0.25. 2+x C 1-x B x Compare NCA88 CAM coated with O3. Figure 7 shows a plot of specific capacity versus cycles at 75°C for a half cell containing a Li metal anode, LPSCl (Li6PS5Cl) SE, a cathode layer containing NCA88 particles as CAM, and VGCF. Cycles 1 and 2 were cycled with 0.1C charge / discharge, cycles 3 and 4 were cycled with 0.33C charge / discharge, cycles 5 and 6 were cycled with 0.5C charge / discharge, cycles 7 and 8 were cycled with 1C charge / discharge, cycles 9 and 10 were cycled with 2C charge / discharge, cycles 11 and 12 were cycled with 5C charge / discharge, and cycles 13-40 were cycled with 0.5C charge / discharge. The cycle plots show Li approximately 5 nm thick when coated using the sol-gel method at x = 0 and x = 0.15, and when coated using the spray coating method at x = 0.15, 0.20, and 0.25. 2+x C 1-x B x Compare NCA88 CAM with O3. Specific details for implementing the invention
[0010] In some embodiments, the cathode active material (CAM) is Li 2+x C 1-x B xIt is coated with LCBO having the chemical formula O3, where 0 < x < 0.5. Lithium carbonate borate (LCBO) is also referred to as lithium carbonate doped with lithium borate. In some embodiments, the coated CAM is incorporated into a cathode layer, for example, as shown in FIG. 1. The cathode layer may have a cathode active material (CAM) (1) particle coated with LCBO as a CAM coating layer (2), an electrically conductive material such as carbon fiber (3), and a solid electrolyte such as a sulfur-containing inorganic electrolyte or a sulfide-based solid electrolyte (4).
[0011] In some embodiments, CAM is Li x MO2, Li x Ni 1-y-z Co y M1 z O2 and Li x Ni 1-y-z Mn y M2 z At least one selected from the group consisting of O2, where M is at least one selected from the group consisting of Ni, Co, Mn, Al, B, Fe, Mg, Ca, Sr, Sc, Y, Ti, Zr, V, Nb, Ta, Cr, Mo, W, Rh, Pd, Cu, Zn, Cd, Ga, In, Sn, and rare earth elements, where M1 is at least one selected from the group consisting of Mn, Al, B, Fe, Mg, Ca, Sr, Sc, Y, Ti, Zr, V, Nb, Ta, Cr, Mo, W, Rh, Pd, Cu, Zn, Cd, Ga, In, Sn, and rare earth elements, where M2 is at least one selected from the group consisting of Co, Al, B, Fe, Mg, Ca, Sr, Sc, Y, Ti, Zr, V, Nb, Ta, Cr, Mo, W, Rh, Pd, Cu, Zn, Cd, Ga, In, Sn, and rare earth elements, where 0.95 ≤ x ≤ 1.1, 1-yz>0, 0< y ≤ 0.5, 0 ≤ z ≤ 0.5.
[0012] In some embodiments, CAM is Li x MO2, Li x Ni 1-y-z Co y M1 z O2 and Li x Ni 1-y-z Mn y M2 z At least one selected from the group consisting of O2, where M is at least one selected from the group consisting of Al, B, Fe, Mg, Ca, Sr, Sc, Y, Ti, Zr, V, Nb, Ta, Cr, Mo, W, Rh, Pd, Cu, Zn, Cd, Ga, In, Sn, and rare earth elements, where M1 is at least one selected from the group consisting of Mn, Al, B, Fe, Mg, Ca, Sr, Sc, Y, Ti, Zr, V, Nb, Ta, Cr, Mo, W, Rh, Pd, Cu, Zn, Cd, Ga, In, Sn, and rare earth elements, where M2 is at least one selected from the group consisting of Co, Al, B, Fe, Mg, Ca, Sr, Sc, Y, Ti, Zr, V, Nb, Ta, Cr, Mo, W, Rh, Pd, Cu, Zn, Cd, Ga, In, Sn, and rare earth elements, where 0.95 ≤ x ≤ 1.1, 1-yz>0, 0< y ≤ 0.5, 0 ≤ z ≤ 0.5.
[0013] In some embodiments, the CAM is surface-doped with at least one doping element selected from the group consisting of Ni, Co, Mn, Al, B, Fe, Mg, Ca, Sr, Sc, Y, Ti, Zr, V, Nb, Ta, Cr, Mo, W, Rh, Pd, Cu, Zn, Cd, Ga, In, Sn, Si, Ge, S, P, and rare earth elements.
[0014] In some embodiments, CAM includes, without limitation: Li x Mn 1-y M y A2(Chemical Formula 1), Lix Mn 1-y M y O 2-z X z (Chemical Formula 2), Li x Mn2O 4-z X z (Chemical Formula 3), Li x Mn 2-y M y A4 (Chemical Formula 4), Li x Co 1-y M y A2(Chemical Formula 5), Li x Co 1-y M y O 2-z X z (Chemical Formula 6), Li x Ni 1-y M y A2(Chemical Formula 7), Li x Ni 1-y M y O 2-z X z (Chemical Formula 8), Li x Ni 1-y Co y O 2-z X z (Chemical Formula 9), Li x Ni 1-y-z Co y M z A a (Chemical Formula 10), Li x Ni 1-y-z Co y M z O 2-a X a (Chemical Formula 11), Li x Ni 1-y-z Mn y M z A a (Chemical Formula 12), Li x Ni 1-y-z Mn y M z O 2-a X a (Chemical Formula 13), Li x Ni 1-y-z Mn y M zO2 (Chemical Formula 14) and combinations thereof, where 0.95 ≤ x ≤ 1.1, 0 ≤ y ≤ 0.5, 0 ≤ z ≤ 0.5, 0 ≤ a ≤ 2; M is selected from the group consisting of Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V and rare earth elements; A is selected from the group consisting of O, F, S and P; and X is selected from the group consisting of F, S and P. In some embodiments, the CAM is in the form of particles having an average diameter in the range of about 1 μm to about 15 μm, about 1 μm to about 12 μm, about 1 μm to about 10 μm, about 1 μm to about 7 μm, about 1 μm to about 6 μm, about 3 μm to about 15 μm, about 3 μm to about 12 μm, about 3 μm to about 10 μm, about 3 μm to about 7 μm, about 3 μm to about 6 μm, about 5 μm to about 15 μm, about 5 μm to about 12 μm, about 5 μm to about 10 μm, and any range in between and sub-ranges.In some embodiments, the coated CAM in the cathode layer is about 50 wt% to about 99 wt%, about 50 wt% to about 95 wt%, about 50 wt% to about 90 wt%, about 50 wt% to about 85 wt%, about 50 wt% to about 80 wt%, about 55 wt% to about 99 wt%, about 55 wt% to about 95 wt%, about 55 wt% to about 90 wt%, about 55 wt% to about 85 wt%, about 55 wt% to about 80 wt%, about 60 wt% to about 99 wt%, about 60 wt% to about 95 wt%, about 60 wt% to about 90 wt%, about 60 wt% to about 85 wt%, about 60 wt% to about 85 wt%, about 60 wt% to about 80 wt%, about 65 wt% to about 99 wt%, about 65 wt% to It may have a concentration of about 95 wt%, about 65 wt% to about 90 wt%, about 65 wt% to about 85 wt%, about 65 wt% to about 80 wt%, about 70 wt% to about 99 wt%, about 70 wt% to about 95 wt%, about 70 wt% to about 90 wt%, about 70 wt% to about 85 wt%, about 70 wt% to about 80 wt%, and any range and sub-range therebetween. In some embodiments, the CAM particles may be polycrystalline or single-crystal. In some embodiments, the CAM particles may have a single particle size distribution or a multiple particle size distribution.
[0015] In some embodiments, the CAM contains a Ni element in a mole fraction of 50% or more, 55% or more, 60% or more, 65% or more, 70% or more, 75% or more, 80% or more, or 85% or more among all metal elements excluding lithium.
[0016] In some embodiments, the cathode coating material is Li2CO3 (LCBO) doped with Li3BO3, where the ratio of Li2CO3 to Li3BO3 is Li 2+x C 1-x B xIt is expressed as O3. In some embodiments, 0 < x < 1, 0 < x ≤ 0.90, 0 < x ≤ 0.80, 0 < x ≤ 0.70, 0 < x ≤ 0.60, 0 < x ≤ 0.50, 0 < x ≤ 0.45, 0 < x ≤ 0.40, 0 < x ≤ 0.35, 0 < x ≤ 0.30, 0 < x ≤ 0.25, 0 < x ≤ 0.20, 0 < x ≤ 0.15, 0 < x ≤ 0.10, 0.10 ≤ x < 1, 0.10 ≤ x ≤ 0.90, 0.10 ≤ x ≤ 0.80, 0.10 ≤ x ≤ 0.70, 0.10 ≤ x ≤ 0.60, 0.10 ≤ x ≤ 0.50, 0.10 ≤ x ≤ 0.45, 0.10 ≤ x ≤ 0.40, 0.10 ≤ x ≤ 0.35, 0.10 ≤ x ≤ 0.30, 0.10 ≤ x ≤ 0.25, 0.10 ≤ x ≤ 0.20, 0.15 ≤ x < 1, 0.15 ≤ x ≤ 0.90, 0.15 ≤ x ≤ 0.80, 0.15 ≤ x ≤ 0.70, 0.15 ≤ x ≤ 0.60, 0.15 ≤ x ≤ 0.50, 0.15 ≤ x ≤ 0.45, 0.15 ≤ x ≤ 0.40, 0.15 ≤ x ≤ 0.35, 0.15 ≤ x ≤ 0.30, 0.15 ≤ x ≤ 0.25, 0.20 ≤ x < 1, 0.20 ≤ x ≤ 0.90, 0.20 ≤ x ≤ 0.80, 0.20 ≤ x ≤ 0.70, 0.20 ≤ x ≤ 0.60, 0.20 ≤ x ≤ 0.50, 0.20 ≤ x ≤ 0.45, 0.20 ≤ x ≤ 0.35, 0.20 ≤ x ≤ 0.35 0.30, 0.25 ≤ x < 1, 0.25 ≤ x ≤ 0.90, 0.25 ≤ x ≤ 0.80, 0.25 ≤ x ≤ 0.70, 0.25 ≤ x ≤ 0.60, 0.25 ≤ x ≤ 0.50, 0.25 ≤ x ≤ 0.45, 0.25 ≤ x ≤ 0.40, 0.25 ≤ x ≤ 0.35, 0.30 ≤ x < 1, 0.30 ≤ x ≤ 0.90, 0.30 ≤ x ≤ 0.80, 0.30 ≤ x ≤ 0.70, 0.30 ≤ x ≤ 0.60, 0.30 ≤ x ≤ 0.50, 0.30 ≤ x ≤ 0.45, 0.30 ≤ x ≤ 0.40, 0.35 ≤ x < 1, 0.35 < 0.60, 0.35 ≤ x ≤ 0.50, 0.35 ≤ x ≤ 0.45, 0.40 ≤ x < 1, 0.40 ≤ x ≤ 0.90, 0.40 ≤ x ≤ 0.80, 0.40 ≤ x ≤ 0.70, 0.40 ≤ x ≤ 0.60, 0.40 ≤ x ≤ 0.50, 0.45 ≤ x < 1, 0.45 ≤ x ≤ 0.90, 0.45 ≤ x ≤ 0.80, 0.45 ≤ x ≤ 0.70, 0.45 ≤ x ≤ 0.60, 0.50 ≤ x < 1, 0.50 ≤ x ≤ 0.90, 0.50 ≤ x ≤ 0.80, 0.50 ≤ x ≤ 0.70, 0.50 ≤ x ≤ 0.60, 0.70 ≤ x < 1, 0.70 ≤ x ≤ 0.90, 0.70 ≤ x ≤ 0.80, and any range and sub-range in between. The disclosed range of x improves ion conductivity by doping lithium carbonate with lithium borate, which in turn improves the discharge capacity of the all-solid-state battery. Doping lithium carbonate with lithium borate increases cycle life stability because the BO bonds are stronger than the CO bonds, which reduces OS exchange between the cathode active material and the sulfide solid electrolyte. It has been found that doping lithium carbonate with a large amount of lithium borate can reduce ion conductivity and cycle life stability, potentially leading to lower discharge capacity. While I do not wish to be bound by theory, the decrease in cycle life capacity of high-level lithium borate-doped compositions may be due to the higher hardness of lithium borate (4 on the Mohs hardness scale) compared to lithium carbonate (0.6 on the Mohs hardness scale). A harder lithium borate coating is prone to cracking due to the volume expansion and contraction of the cathode active material during cycling, which exposes the cathode active material surface to the solid electrolyte and lowers cycle life stability.
[0017] In some embodiments, the LCBO coating layer may have a thickness in the range of 0.5 to 20 nm, 0.8 to 20 nm, 1 to 20 nm, 2 to 20 nm, 4 to 20 nm, 10 to 20 nm, 0.5 to 10 nm, 1.0 to 10 nm, 2 to 10 nm, or 4 to 10 nm. In some embodiments, the thickness is measured by observing the cross-section of the dissected particle using a scanning electron microscope (SEM). In some embodiments, the thickness is measured by a transmission electron microscope (TEM). In some embodiments, the thickness is calculated using the weight content of lithium carbonate, the content of lithium carbonate borate after doping, and the surface area (e.g., BET specific surface area).
[0018] In some embodiments, the electrically conductive material may be a carbon fiber and includes, but is not limited to, vapor-grown carbon fiber (VGCF), carbon nanotubes (CNT), multi-walled carbon nanotubes (MWCNT), carbon nanofibers, and graphite fibers. In some embodiments, the electrically conductive material may have a BET-measured specific surface area in the range of 1 to 600 m² / g and / or an electrical resistance of 0.5 Ω·cm or less. In some embodiments, the electrically conductive material may be coated with an oxide material. In some embodiments, the oxide material may be, without limitation, lithium borate, alumina, lithium zirconate (Li2ZrO3), LiNbO3, Li4SiO4, Li3PO4, Li2SiO3, LiPO3, Li2SO4, Li2WO4, Li2MoO4, LiAlO2, Li2TiO3, Li4Ti5O 12 ..., or includes a complex oxide thereof. In some embodiments, lithium borate for electrically conductive material coating is Li3B 11 O 18, Li3BO3, Li4B2O5, Li6B4O9, LiBO2, Li2B4O7, Li3B7O 12 ...and LiB3O5, but are not limited thereto. In some embodiments, the electrically conductive material (coated or uncoated) has a concentration in the cathode layer of 0.01 wt% to 5 wt%, 0.01 wt% to 4 wt%, 0.01 wt% to 3 wt%, 0.01 wt% to 2 wt%, 0.5 wt% to 5 wt%, 0.5 wt% to 4 wt%, 0.5 wt% to 3 wt%, 0.5 wt% to 2 wt%, 1 wt% to 5 wt%, 1 wt% to 4 wt%, 1 wt% to 3 wt%, 2 wt% to 5 wt%, 2 wt% to 4 wt%, and any or all ranges and sub-ranges in between.
[0019] In some embodiments, the method for preparing a coated cathode active material disclosed herein may include the step of determining the weight percentage of lithium carbonate in an uncoated cathode active material using, for example, thermal gravimetric analysis (TGA) or titration. A coating solution comprising a solvent, a lithium precursor, and a borate precursor may be prepared, wherein the amounts of the lithium precursor and the borate precursor are given by the formula Li 2+x C 1-x B x It is calculated based on the weight percentage of lithium carbonate previously determined to be present in O3 and the uncoated cathode active material. In some embodiments, the solvent for preparing the coating solution is non-aqueous and methanol, ethanol, isopropanol, n -Propanol, t- Selected from the group consisting of butanol and mixtures thereof. The coating solution may be applied to an uncoated cathode active material, and the coating solution may then be annealed, wherein the lithium precursor and borate precursor are converted into lithium carbonate ions doped with lithium borate to form a coating layer on the cathode active material. In some embodiments, annealing is performed in an oxygen atmosphere for 0.5 to 3 hours at a temperature in the range of 150 to 600°C. In some embodiments, the coating solution may be applied by spray coating the coating solution onto the uncoated cathode active material, which is referred to herein as the spray coating method. In other embodiments, the coating solution may be applied by mixing the uncoated cathode active material with the coating solution to form a mixture, and then removing the solvent under vacuum to form a gel, which is referred to herein as the sol-gel method.
[0020] In some embodiments, the solid electrolyte used may be any sulfide solid electrolyte as long as it contains Li and S and has the desired lithium ion conductivity. The sulfide solid electrolyte may be any crystalline material, glass ceramic, and glass. In some embodiments, the solid electrolyte is a lithium-phosphate-sulfur (LPS) electrolyte. Examples of sulfide solid electrolytes include Li2S-P2S5, Li2S-P2S5-LiHa ("Ha" is one or more halogen elements), Li2S-P2S5-P2O5, Li2S-Li3PO4-P2S5, Li3PS4, Li4P2S6, Li 10 GeP2S 12 , Li 3.25 Ge 0.25 P 0.75 S4, Li7P3S 11 , Li 3.25 P 0.95 S4, and Li 7-x PS 6-x Ha x(contains an argyrodite-type solid electrolyte, where "Ha" is one or more halogen elements, where 0.2 < x < 1.8). In some embodiments, the sulfide solid electrolyte may have a concentration in the cathode layer of 1 wt% to 35 wt%, 1 wt% to 30 wt%, 1 wt% to 25 wt%, 1 wt% to 20 wt%, 1 wt% to 15 wt%, 1 wt% to 10 wt%, 5 wt% to 35 wt%, 5 wt% to 30 wt%, 5 wt% to 25 wt%, 5 wt% to 20 wt%, 5 wt% to 15 wt%, 10 wt% to 35 wt%, 10 wt% to 30 wt%, 10 wt% to 25 wt%, 10 wt% to 20 wt%, 15 wt% to 35 wt%, 15 wt% to 30 wt%, 15 wt% to 25 wt%, 20 wt% to 30 wt%, and any and all ranges and sub-ranges in between. there is.
[0021] In some embodiments, the cathode layer is sandwiched between the cathode current collector and the solid electrolyte layer. In some embodiments, the cathode layer is sandwiched between the solid electrolyte layer and the current collector, respectively, and lithium ions (Li + It includes a cathode active material (CAM) that requires both ) and electron (e-) connectivity. Li + Connectivity is primarily provided by small particles of the sulfide-based solid electrolyte within the cathode layer, while electronic connectivity is primarily provided by the electrically conductive material. Sulfide-based solid electrolytes (such as the exemplary sulfide solid electrolyte presented above) possess high Li+ conductivity. However, generally, Li / Li at the CAM / SE, CF / SE, and current collector / SE interfaces +It decomposes at a potential of less than 1.7 V or greater than 2.1 V. The decomposed byproduct generally has lower Li+ conductivity, and in return, a higher proportion of SE is required in the cathode composite layer, resulting in a lower proportion of CAM. Without being bound by theory, the LCBO coating layer disclosed herein extends the decomposition time, maintains relatively high Li+ conductivity, and thus improves cycle performance.
[0022] The cathode layer disclosed above can be incorporated into an all-solid-state battery. For example, as shown in FIG. 2, the cathode layer (5) can serve as the positive electrode in an all-solid-state battery (ASSB), and the all-solid-state battery may also include a negative electrode (or anode layer) (7) and a solid electrolyte layer (6) between the cathode layer (5) and the negative electrode (7). In some embodiments, the solid electrolyte of the solid electrolyte layer may be the same as or different from the solid electrolyte of the cathode layer. In some embodiments, the solid electrolyte layer is an inorganic solid electrolyte layer, for example, Li2S-P2S5, Li2S-P2S5-LiHa ("Ha" is one or more halogen elements), Li2S-P2S5-P2O5, Li2S-Li3PO4-P2S5, Li3PS4, Li4P2S6, Li 10 GeP2S 12 , Li 3.25 Ge 0.25 P 0.75 S4, Li7P3S 11 , Li 3.25 P 0.95 S4, and Li 7-x PS 6-x Ha x It is a sulfur-containing inorganic electrolyte that includes, but is not limited to, (an azyrodite-type solid electrolyte, where "Ha" is one or more halogen elements, where 0.2 < x < 1.8).
[0023] In some embodiments, the ASSB has an initial discharge capacity of at least 180 mAh / g, at least 185 mAh / g, or at least 190 mAh / g at a discharge rate of 0.5C at 45℃.
[0024] In some embodiments, the ASSB has an initial discharge capacity of at least 190 mAh / g, at least 195 mAh / g, at least 200 mAh / g, or at least 205 mAh / g at a discharge rate of 0.1C at 45°C.
[0025] In some embodiments, when the ASSB is charged and discharged for 20 cycles at 45°C, each cycle is charged to 4.25V and discharged to 2.8V at 0.1C for cycles 1 and 2, 0.33C for cycles 3 and 4, 1.0C for cycle 5, and 0.5C for cycles 6 through 20, and the ASSB has a 20-cycle discharge of at least 180 mAh / g, at least 185 mAh / g, or at least 190 mAh / g and / or a 20th-cycle life retention rate of at least 95%, at least 96%, at least 97%, or at least 98%. The 20th-cycle life retention rate is the ratio of the discharge specific capacity in the 20th cycle to the initial discharge specific capacity at 0.5C at 45°C.
[0026] In one embodiment, the present disclosure provides a cathode layer for an all-solid-state battery, wherein the layer comprises a cathode active material (CAM) coated with LCBO. In one embodiment, the LCBO is formed between lithium carbonate on the surface of the CAM particles and lithium borate or a precursor thereof. In some embodiments, the lithium borate for doping the lithium carbonate on the surface of the CAM is Li3B 11 O 18 , Li3BO3, Li4B2O5, Li6B4O9, LiBO2, Li2B4O7, Li3B7O 12LiB3O5 is included but not limited to. In some embodiments, lithium borate for doping lithium carbonate onto the CAM surface is doped with a doping element. In some embodiments, the doping element is fluorine (F), sulfur (S), silicon (Si), germanium (Ge), or a mixture thereof. In some embodiments, the lithium borate comprises one or more undoped or doped lithium borates as described above. In some embodiments, the lithium borate is structurally similar to lithium carbonate so that lithium carbonate doped with lithium borate can be formed on the CAM surface.
[0027] In some embodiments, the LCBO formed on the CAM surface appears less uniform in terms of the concentrations of lithium carbonate and lithium borate. In some embodiments, lithium carbonate exhibits a concentration gradient in the LCBO coating layer on the CAM particle surface. In some embodiments, the concentration of lithium carbonate is relatively higher near or close to the CAM particle surface, or the concentration of lithium carbonate decreases from the CAM particle surface toward the outer surface of the LCBO coating layer. In some embodiments, lithium borate exhibits a concentration gradient in the LCBO coating layer on the CAM particle surface. In some embodiments, the concentration of lithium borate is relatively higher on or near the outer surface of the LCBO coating layer, or the concentration of lithium borate decreases from the outer surface of the LCBO coating layer toward the CAM particle surface. In some embodiments, the exposure of lithium carbonate is minimized to reduce or prevent side reactions between the cathode active material and the sulfide electrolyte. In some embodiments, LCBO is formed based on lithium carbonate on the surface of CAM particles without an external lithium carbonate source. The gradient can be determined using elemental mapping such as high-resolution TEM and energy dispersive spectroscopy (EDS) line scans across the coating layer thickness.
[0028] In some embodiments, CAM particles coated with an LCBO coating exhibit a core-shell structure, where the core is a CAM particle and the shell is an LCBO coating layer.
[0029] In one embodiment, the present disclosure provides an all-solid-state battery (ASSB) comprising the cathode layer described above.
[0030] In some embodiments, the present disclosure provides a cathode active material whose surface is doped with lithium borate.
[0031] In some embodiments, the solid electrolyte layer of the ASSB is an inorganic solid electrolyte layer, e.g., Li2S-P2S5, Li2S-P2S5-LiHa ("Ha" is one or more halogen elements), Li2S-P2S5-P2O5, Li2S-Li3PO4-P2S5, Li3PS4, Li4P2S6, Li 10 GeP2S 12 , Li 3.25 Ge 0.25 P 0.75 S4, Li7P3S 11 , Li 3.25 P 0.95 S4, and Li 7-x PS 6-x Ha x It is a sulfur-containing inorganic electrolyte that includes, but is not limited to, (an azyrodite-type solid electrolyte, where "Ha" is one or more halogen elements, where 0.2 < x < 1.8).
[0032] The present disclosure will be better understood by referring to the experimental details that follow; however, those skilled in the art will readily understand that the specific experiments described in detail are merely illustrative and are not intended to limit the content of the disclosure set forth herein as defined by the claims that follow.
[0033] It should be noted that the transitional term "comprising," which is synonymous with "including," "containing," or "characterized by," is inclusive or open and does not exclude unmentioned additional elements or method steps.
[0034] Example 1:
[0035] Since Li2CO3 is inherently present on the CAM surface in standard manufacturing processes, the weight percentage of Li2CO3 relative to the CAM can be determined, for example, using thermogravimetric analysis (TGA). The stoichiometric amount of Li3BO3 required to produce the LCBO coating layer is further calculated. For the LCBO coating layer, x = 0.15, stoichiometric amounts of a Li precursor (e.g., lithium acetate or lithium metal) and a B precursor (e.g., triisopropyl borate) were dissolved in a dry solvent (e.g., ethanol) to form a coating solution containing the lithium precursor and the borate precursor. The coating solution was added to a predetermined amount of CAM to calculate the desired Li3BO3 doping ratio from the TGA data. After stirring the mixture for 30 minutes, the solvent was removed via vacuum while sonicating to obtain a CAM gel coated with the Li precursor and the B precursor. The gel was then annealed at 300°C for 1 hour under an oxygen flow to form the LCBO coating layer.
[0036] Specific discharge capacity and cycle life retention rates for various LCBO coating layer compositions for x = 0 to 1.00 are summarized in Table 1. For LCBO x = 1.00 (no lithium carbonate in the coating layer), the CAM is first annealed in air at 600°C for 16 hours to remove surface-embedded Li2CO3, and then coated with a stoichiometric amount of Li3BO3 sol-gel reagent. The cathode layer comprises 65 wt% CAM (NCA88), 5 wt% carbon fiber, and 30 wt% lithium phosphate sulfur chloride (LPSCl) (Li6PS5Cl). The cathode layer in a torque cell was electrochemically evaluated using Li metal over copper as the anode and LPSCl (Li6PS5Cl) as the SE. The cell is cycled from 2.8V to 4.25V with 0.1C charge / discharge for 1 and 2 cycles, 0.33C charge / discharge for 3 and 4 cycles, 1.0C charge / discharge for 5 cycles, and 0.5C charge / discharge for 6 to 25 cycles.
[0037] The LCBO coating layer with x=0.15 maintained a high level of initial battery performance while simultaneously reducing the fading of the discharge capacity. For example, as shown in Table 1 and Figure 4, for a half battery containing undoped CAM (x=0.00), the initial discharge capacity is 205.95 mAh / g at a discharge rate of 0.1C. When Li3BO3 is doped into Li2CO3 (x = 0.05, 0.10, and 0.15), the initial discharge capacities are 211.00 mAh / g, 208.03 mAh / g, and 204.46 mAh / g, respectively. At x=1.00 (100% Li3BO3), the initial discharge capacity decreases to 186.39 mAh / g. LCBO-coated CAM effectively reduces cell degradation, which is clearly evident in the cycle life capacity retention rate after 20 cycles at 0.5C in Table 1 and Figure 4, and the initial discharge capacity increases at a rate of 0.1C, thereby increasing the theoretical capacity of the CAM (NCA88 - LiNi 0.88 Co0.09 Al 0.03 As it approaches 219.8 mAh / g in the case of O2, it may be important for realizing a high-capacity SSB.
[0038] [Table 1]
[0039] Initial discharge (dChg.) specific capacity (mAh / g) of a half-battery using an LCBO-coated CAM at 45°C and various C-rates for x=0 to 1.
[0040]
[0041] a: The cycle life 0.5C discharge capacity retention rate is calculated by dividing the 20th cycle 0.5C discharge capacity by the initial 0.5C discharge capacity and multiplying by 100%.
[0042] In addition, as shown in Table 1 and Figure 5, the cycle life capacity retention rate increases from 95.87% for x=0 to 99.22%, 98.21%, 99.63%, 98.83%, and 99.04% for x=0.05, 0.10, 0.15, 0.25, and 0.3, respectively. When x is 0.5 or 1.0, the cycle life capacity retention rate drops to a level equal to or lower than that of the uncoated CAM (x=0). In some situations, when x is higher than 0.5, it can bring benefits such as short- to medium-term cycle life capacity retention rates.
[0043] Figure 6 is a plot of the specific capacity from cycle 1 to cycle 100. This shows that the cycle performance of x=0.05 and 0.15 improved compared to the uncoated (x=0). Although the specific capacity was higher in the initial cycles, the cycle performance of x=0.25 gradually dropped to a level lower than that of the uncoated case.
[0044] Example 2:
[0045] The LCBO coating layer was applied to the CAM surface via a spray coating method using the same method as that used to prepare the coating solution described in detail in Example 1. The coating solution was applied to the CAM powder using a Powrex rolling fluid bed granulator and coater model FD-MP-01D. The coated CAM was then annealed at 300°C for 1 hour under an oxygen flow to form the LCBO coating layer.
[0046] The specific capacity and cycle life retention rates of the LCBO coating compositions for x = 0.00, x = 0.15, x = 0.15, 0.20, and 0.25 at 0.1C to 5C charge / discharge rates are shown in Fig. 7 and summarized in Table 2. When comparing the sol-gel and spray-coated x = 0.15 material, the spray-coated material exhibited similar rate and discharge performance but higher stability; this is likely due to the more uniform and complete coating application, which is an inherent advantage of using the spray coating method over the sol-gel method. When comparing the x = 0.15 and 0.25 LCBO spray-coated materials, the x = 0.15 material showed a higher rate capacity of over 200 mAh / g at 5C charge / discharge. The x = 0.25 material showed lower discharge capacity and rate performance but exhibited a slight improvement in cycle life capacity retention rate. All coated materials showed improved performance compared to x = 0.00 CAM.
[0047] [Table 2]
[0048] Li approximately 5 nm thick coated using the sol-gel method at x = 0 and x = 0.15, and using the spray coating method at x = 0.15, 0.20, and 0.25 2+x C 1-x B xInitial discharge (dChg.) specific capacity (mAh / g) at 75°C and other C-rates for a half battery using NCA88 CAM with O3. The 0.5C cycle life capacity retention rate is calculated by dividing the 20th cycle 0.5C discharge capacity by the initial 0.5C cycle discharge capacity and multiplying by 100%.
[0049]
[0050] SG : Material coated using the sol-gel method.
[0051] SC : A material coated using a spray coating method.
[0052] In a first aspect of the present disclosure, a coated cathode active material comprises a cathode active material (CAM) and a coating layer in contact with the cathode active material, wherein the coating layer is Li 2+x C 1-x B x It comprises lithium carbonate doped with lithium borate (LCBO) having the chemical formula O3, wherein 0 <x<0.5이다.
[0053] In the second aspect according to the first aspect, the coating layer has a thickness in the range of 0.5 to 20 nm.
[0054] In the third aspect according to all preceding aspects, 0.00 < x ≤ 0.30.
[0055] In the fourth aspect according to all preceding aspects, the cathode active material is in the form of particles and has an average diameter of 1 to 15 μm.
[0056] In the fifth aspect according to all preceding aspects, CAM is Li x MO2, Li x Ni 1-y-z Co y M1 z O2 and Li x Ni 1-y-z Mn y M2z At least one selected from the group consisting of O2, where M is at least one selected from the group consisting of Ni, Co, Mn, Al, B, Fe, Mg, Ca, Sr, Sc, Y, Ti, Zr, V, Nb, Ta, Cr, Mo, W, Rh, Pd, Cu, Zn, Cd, Ga, In, Sn, and rare earth elements, where M1 is at least one selected from the group consisting of Mn, Al, B, Fe, Mg, Ca, Sr, Sc, Y, Ti, Zr, V, Nb, Ta, Cr, Mo, W, Rh, Pd, Cu, Zn, Cd, Ga, In, Sn, and rare earth elements, where M2 is at least one selected from the group consisting of Co, Al, B, Fe, Mg, Ca, Sr, Sc, Y, Ti, Zr, V, Nb, Ta, Cr, Mo, W, Rh, Pd, Cu, Zn, Cd, Ga, In, Sn, and rare earth elements, where 0.95 ≤ x ≤ 1.1, 1-yz>0, 0< y ≤ 0.5, 0 ≤ z ≤ 0.5.
[0057] In the sixth aspect, CAM is Li x MO2, Li x Ni 1-y-z Co y M1 z O2 and Li x Ni 1-y-z Mn y M2 zAt least one selected from the group consisting of O2, where M is at least one selected from the group consisting of Al, B, Fe, Mg, Ca, Sr, Sc, Y, Ti, Zr, V, Nb, Ta, Cr, Mo, W, Rh, Pd, Cu, Zn, Cd, Ga, In, Sn, and rare earth elements, where M1 is at least one selected from the group consisting of Mn, Al, B, Fe, Mg, Ca, Sr, Sc, Y, Ti, Zr, V, Nb, Ta, Cr, Mo, W, Rh, Pd, Cu, Zn, Cd, Ga, In, Sn, and rare earth elements, where M2 is at least one selected from the group consisting of Co, Al, B, Fe, Mg, Ca, Sr, Sc, Y, Ti, Zr, V, Nb, Ta, Cr, Mo, W, Rh, Pd, Cu, Zn, Cd, Ga, In, Sn, and rare earth elements, where 0.95 ≤ x ≤ 1.1, 1-yz>0, 0< y ≤ 0.5, 0 ≤ z ≤ 0.5.
[0058] In the seventh aspect, the CAM is surface-doped with at least one doping element selected from the group consisting of Ni, Co, Mn, Al, B, Fe, Mg, Ca, Sr, Sc, Y, Ti, Zr, V, Nb, Ta, Cr, Mo, W, Rh, Pd, Cu, Zn, Cd, Ga, In, Sn, Si, Ge, S, P, and rare earth elements.
[0059] In the eighth aspect according to all preceding aspects, CAM contains a Ni element in a mole fraction of at least 70% among all metal elements excluding lithium.
[0060] In the ninth aspect according to all preceding aspects, the cathode active material is a polycrystalline particle or a single-crystal particle.
[0061] In the tenth aspect according to all preceding aspects, the concentration of lithium carbonate in the coating layer decreases from the surface of the CAM to the outside of the coating layer, and the concentration of lithium borate decreases from the outer surface of the coating layer to the surface of the CAM.
[0062] In the eleventh aspect, a method for manufacturing a coated cathode active material of any one of the above aspects is,
[0063] a) A step of determining the weight percentage of lithium carbonate in an uncoated cathode active material,
[0064] b) a step of preparing a coating solution comprising a solvent, a lithium precursor, and a borate precursor, wherein the amounts of the lithium precursor and the borate precursor are calculated based on the chemical formula and the weight percentage of lithium carbonate in step a).
[0065] c) a step of applying a coating solution to an uncoated cathode active material, and
[0066] d) a step of annealing the coating solution, wherein the lithium precursor and the borate precursor are converted into lithium carbonate (LCBO) doped with lithium borate to obtain a coated cathode active material.
[0067] In the 12th aspect according to the 11th aspect, the solvent for preparing the coating solution is non-aqueous and is methanol, ethanol, isopropanol, n -Propanol, t - It is selected from the group consisting of butanol and mixtures thereof.
[0068] In the 13th aspect according to either of the 11th and 12th aspects, the coating solution is annealed in an oxygen atmosphere for 0.5 to 3 hours at a temperature in the range of 150 to 600°C.
[0069] In the 14th aspect according to any one of the 11th to 13th aspects, the step of applying the coating solution includes the step of spraying the coating solution onto the cathode active material.
[0070] In the 15th aspect according to any one of the 11th to 13th aspects, the step of applying the coating solution includes the step of mixing the cathode active material into the coating solution.
[0071] In the 16th aspect, the cathode layer comprises a coated cathode active material described in any one of the 1st to 15th aspects.
[0072] In the 17th aspect according to the 16th aspect, the coated cathode active material has at least 65% by weight of the cathode layer.
[0073] In the 18th aspect according to the 16th or 17th aspect, the cathode layer further comprises an electrically conductive material.
[0074] In the 19th aspect according to the 18th aspect, the electrically conductive material is selected from carbon fibers, vapor-grown carbon fibers, carbon nanotubes, graphite fibers, and mixtures thereof.
[0075] In the 20th aspect according to the 16th to 19th aspects, the cathode layer further comprises a sulfur-containing inorganic electrolyte.
[0076] In the 21st aspect according to the 20th aspect, the sulfur-containing inorganic electrolyte is Li2S-P2S5, Li2S-P2S5-LiHa, Li2S-P2S5-P2O5, Li2S-Li3PO4-P2S5, Li3PS4, Li4P2S6, Li 10 GeP2S 12 , Li 3.25 Ge 0.25 P 0.75 S4, Li7P3S 11 , Li 3.25 P 0.95 S4, Li 7-x PS 6-x Ha x It is selected from the group consisting of and mixtures thereof, where "Ha" is one or more halogen elements and 0.2 < x < 1.
[0077] In the 22nd aspect, the all-solid-state battery (ASSB) includes a cathode layer described in any one of the 16 to 21 aspects.
[0078] In the 23rd aspect according to the 22nd aspect, the ASSB further includes an inorganic solid electrolyte layer.
[0079] In the 24th aspect according to the 23rd aspect, the inorganic solid electrolyte layer comprises an inorganic electrolyte containing sulfur.
[0080] In the 25th aspect according to the 24th aspect, the sulfur-containing inorganic electrolyte is Li2S-P2S5, Li2S-P2S5-LiHa, Li2S-P2S5-P2O5, Li2S-Li3PO4-P2S5, Li3PS4, Li4P2S6, Li 10 GeP2S 12 , Li 3.25 Ge 0.25 P 0.75 S4, Li7P3S 11 , Li 3.25 P 0.95 S4, Li 7-x PS 6-x Ha x It is selected from the group consisting of and mixtures thereof, where "Ha" is one or more halogen elements and 0.2 < x < 1.
[0081] In the 26th aspect according to aspects 22 through 25, LCBO is Li 2.05 C 0.95 B 0.05 O3(x=0.05), Li 2.10 C 0.90 B 0.10 O3(x=0.10), Li 2.15 C 0.85 B 0.15 O3(x=0.15), Li 2.25 C 0.75 B 0.25 O3(x=0.25), and Li 2.30 C 0.70 B 0.30 It has a chemical formula selected from the group consisting of O3 (x=0.30).
[0082] In the 27th aspect according to any one of the 22nd to 26th aspects, when the ASSB is charged and discharged for 20 cycles from 2.8V to 4.25V at 45°C, the 1st and 2nd cycles are performed at 0.1C, the 3rd and 4th cycles at 0.33C, the 5th cycle at 1.0C, and the 6th to 20th cycles at 0.5C, the ASSB exhibits a 20th cycle life retention rate of at least 98%, each cycle is charged to 4.25V and discharged to 2.8V, and the 20th cycle life retention rate is the ratio of the discharge specific capacity in the 20th cycle to the initial discharge specific capacity at 45°C and 0.5C.
[0083] In the 28th aspect according to any one of the 22nd to 27th aspects, the ASSB has an initial discharge specific capacity of at least 190 mAh / g at 0.1C at 45℃.
[0084] References
[0085] 1. Zhang, et al. Achieving Both High Ionic Conductivity and High Interfacial Stability with the Li2+xC1-xBxO3 Solid-State Electrolyte: Design from Theoretical Calculations. ACS Appl. Mater. Interfaces 2020, 12, 5, 6007-6014. DOI: 10.1021 / acsami.9b22185.
[0086] 2. Zhang, et al. Direct Visualization of the Interfacial Degradation of Cathode Coatings in Solid State Batteries: A Combined Experimental and Computational Study. Adv. Energy Mater.2020, 10, 1903778. DOI: 10.1002 / aenm.201903778.
Claims
Claim 1 A coated cathode active material comprising a cathode active material (CAM); and a coating layer in contact with the cathode active material, wherein the coating layer is Li 2+x C 1-x B x It comprises lithium carbonate doped with lithium borate (LCBO) having the chemical formula O3, wherein 0 <x≤0.3이고,상기 코팅층 내 탄산 리튬의 농도는 CAM의 표면으로부터 코팅층의 외부로 갈수록 감소하고, 붕산 리튬의 농도는 코팅층의 외부 표면으로부터 CAM의 표면으로 갈수록 감소하는 것인, 코팅된 캐소드 활물질. Claim 2 A coated cathode active material according to claim 1, wherein the coating layer has a thickness in the range of 0.5 to 20 nm. Claim 3 A coated cathode active material according to claim 1, wherein the cathode active material is in the form of particles and the particles have an average diameter of 1 to 15 μm. Claim 4 In claim 1, the CAM is Li x MO2, Li x Ni 1-y-z Co y M1 z O2 and Li x Ni 1-y-z Mn y M2 z Selected from the group consisting of O2, wherein M is at least one selected from the group consisting of Ni, Co, Mn, Al, B, Fe, Mg, Ca, Sr, Sc, Y, Ti, Zr, V, Nb, Ta, Cr, Mo, W, Rh, Pd, Cu, Zn, Cd, Ga, In, Sn, and rare earth elements, M1 is at least one selected from the group consisting of Mn, Al, B, Fe, Mg, Ca, Sr, Sc, Y, Ti, Zr, V, Nb, Ta, Cr, Mo, W, Rh, Pd, Cu, Zn, Cd, Ga, In, Sn, and rare earth elements, M2 is at least one selected from the group consisting of Co, Al, B, Fe, Mg, Ca, Sr, Sc, Y, Ti, Zr, V, Nb, Ta, Cr, Mo, W, Rh, Pd, Cu, Zn, Cd, Ga, In, Sn, and rare earth elements, and 0.95 ≤ A coated cathode active material having x ≤ 1.1, 1-yz>0, 0< y ≤ 0.5, and 0 ≤ z ≤ 0.
5. Claim 5 A coated cathode active material according to claim 1, wherein the CAM contains a Ni element having a mole fraction of at least 50% among all metal elements excluding lithium. Claim 6 In claim 1, the LCBO is Li 2.05 C 0.95 B 0.05 O3, Li 2.10 C 0.90 B 0.10 O3, Li 2.15 C 0.85 B 0.15 O3, Li 2.25 C 0.75 B 0.25 O3 and Li 2.30 C 0.70 B 0.30 A coated cathode active material having a chemical formula selected from the group consisting of O3. Claim 7 delete Claim 8 A method for manufacturing a coated cathode active material as described in claim 1, wherein the method comprises: a) determining a weight percentage of lithium carbonate in an uncoated cathode active material; b) preparing a coating solution comprising a solvent, a lithium precursor, and a borate precursor, wherein the amounts of the lithium precursor and the borate precursor are of the formula Li 2+x C 1-x B x O3 - here 0 <x≤0.3임 - 및 단계 a)의 탄산 리튬의 중량 백분율을 기반으로 계산되는 것인, 단계;c) 코팅되지 않은 캐소드 활물질에 상기 코팅 용액을 도포하는 단계; 및d) 상기 코팅 용액을 어닐링(annealing)하는 단계로서, 상기 리튬 전구체와 붕산염 전구체를 붕산 리튬으로 도핑된 탄산 리튬(LCBO)으로 전환하여 코팅된 캐소드 활물질을 얻는 것인, 단계를 포함하는, 방법. Claim 9 In claim 8, the solvent for preparing the coating solution is non-aqueous and includes methanol, ethanol, isopropanol, n -Propanol, t - A method selected from the group consisting of butanol and mixtures thereof, wherein the coating solution is annealed in an oxygen atmosphere at a temperature range of 150 to 600°C for 0.5 to 3 hours. Claim 10 A cathode layer comprising the coated cathode active material described in claim 1. Claim 11 In claim 10, the cathode layer further comprises an electrically conductive material, wherein the electrically conductive material is selected from carbon fibers, vapor growth carbon fibers, carbon nanotubes, graphite fibers, and mixtures thereof. Claim 12 In claim 10, the cathode layer further comprises a sulfur-containing inorganic electrolyte, and the sulfur-containing inorganic electrolyte is Li2S-P2S5, Li2S-P2S5-LiHa, Li2S-P2S5-P2O5, Li2S-Li3PO4-P2S5, Li3PS4, Li4P2S6, Li 10 GeP2S 12 , Li 3.25 Ge 0.25 P 0.75 S4, Li7P3S 11 , Li 3.25 P 0.95 S4, Li 7-x PS 6-x Ha x A cathode layer selected from the group consisting of and mixtures thereof, wherein "Ha" is one or more halogen elements and 0.2 < x < 1. Claim 13 An all-solid-state battery (ASSB) comprising a cathode layer and an inorganic solid electrolyte layer as described in claim 10, wherein the inorganic solid electrolyte layer comprises a sulfur-containing inorganic electrolyte, and the sulfur-containing inorganic electrolyte comprises Li2S-P2S5, Li2S-P2S5-LiHa, Li2S-P2S5-P2O5, Li2S-Li3PO4-P2S5, Li3PS4, Li4P2S6, Li 10 GeP2S 12 , Li 3.25 Ge 0.25 P 0.75 S4, Li7P3S 11 , Li 3.25 P 0.95 S4, Li 7-x PS 6-x Ha x Selected from the group consisting of and mixtures thereof, where "Ha" is one or more halogen elements and 0.2 < x < 1, ASSB. Claim 14 In claim 13, when the ASSB is charged and discharged for 20 cycles from 2.8V to 4.25V at 45℃, cycles 1 and 2 are performed at 0.1C, cycles 3 and 4 at 0.33C, cycle 5 at 1.0C, and cycles 6 through 20 at 0.5C, the ASSB exhibits a 20th-cycle life retention rate of at least 97%, each cycle is charged to 4.25V and discharged to 2.8V, and the 20th-cycle life retention rate is the ratio of the discharge specific capacity in the 20th cycle to the initial discharge specific capacity at 0.5C at 45℃. Claim 15 In paragraph 13, the ASSB is an ASSB having an initial discharge specific capacity of at least 180 mAh / g at 45℃ and 0.1C. Claim 16 delete Claim 17 delete Claim 18 delete Claim 19 delete Claim 20 delete Claim 21 delete Claim 22 delete Claim 23 delete Claim 24 delete Claim 25 delete Claim 26 delete Claim 27 delete Claim 28 delete
Citation Information
Patent Citations
Preparation method of multi-layer coated ternary positive electrode material
CN113363477A
Positive active material for all solid secondary battery and manufacturing method thereof
KR1020190067465A