Grain oriented electrical steel sheet and manufacturing method of the same
The method addresses magnetic inconsistencies and yield reduction in grain-oriented electrical steel sheets by using multiple cold rolling and decarburization annealing processes, achieving improved magnetic properties and productivity.
Patent Information
- Application Number
- KR1020210184604
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-12-22
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2041-12-22
AI Technical Summary
Existing grain-oriented electrical steel sheets face challenges such as temperature differences leading to magnetic inconsistencies, surface defects, and reduced yield due to multi-stage production processes, and previous methods fail to form sufficient Goss orientation grains effectively.
A manufacturing method involving multiple cold rolling and decarburization annealing processes, including specific temperature and dew point conditions, to achieve uniform magnetic properties and improve Goss orientation grain formation.
The method results in a grain-oriented electrical steel sheet with enhanced magnetic properties, particularly reduced high-frequency iron loss, and improved productivity by avoiding high-temperature treatments and surface defects.
Smart Images

Figure 112021148465218-PAT00001_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a grain-oriented electrical steel sheet and a method for manufacturing the same. Specifically, the invention relates to a grain-oriented electrical steel sheet with improved magnetism by including a plurality of cold rolling and decarburization annealing processes, and a method for manufacturing the same. Background Technology
[0002] Grain-oriented electrical steel sheets have a crystal orientation of {110} <001> It is a soft magnetic material with excellent magnetic properties in the rolling direction, composed of crystal grains having the so-called Goss orientation.
[0003] These oriented electrical steel sheets are manufactured by heating the slab, then rolling it to a final thickness through hot rolling, hot-rolled sheet annealing, and cold rolling, followed by primary recrystallization annealing and high-temperature annealing for secondary recrystallization formation.
[0004] Typically, the secondary recrystallization annealing process for oriented electrical steel sheets is a highly energy-consuming process because it requires a low heating rate and long-term circulating annealing at high temperatures. Since oriented electrical steel sheets with excellent magnetic properties are manufactured by forming secondary recrystallization through such extreme processes, the following difficulties arise in the process.
[0005] First, due to heat treatment in the coil state, a temperature difference occurs between the outer and inner parts of the coil, making it impossible to apply the same heat treatment pattern to each part, resulting in a magnetic difference between the outer and inner parts. Second, various surface defects occur during the process of coating the surface with MgO after decarburization annealing and forming a base coating during high-temperature annealing, which reduces the yield. Third, since the decarburized plate is wound into a coil shape after decarburization annealing, followed by high-temperature annealing and then flattening annealing to apply an insulating coating, the production process is divided into three stages, leading to a problem of reduced yield.
[0006] To overcome these process limitations, a technique has been proposed that utilizes normal crystal growth without using secondary recrystallization by controlling decarburization annealing and cold rolling rates. However, through continuous annealing, the crystal orientation is {110} due to the short heat treatment time. <001> A large number of exact Goss defense particles that exactly matched were not formed, and there were limitations in iron loss improvement. The problem to be solved
[0007] The present invention provides a grain-oriented electrical steel sheet and a method for manufacturing the same. Specifically, the invention provides a grain-oriented electrical steel sheet with improved magnetism and a method for manufacturing the same by including a plurality of cold rolling and decarburization annealing processes. means of solving the problem
[0008] A method for manufacturing a oriented electrical steel sheet according to one embodiment of the present invention comprises the steps of: hot rolling a slab to produce a hot-rolled steel sheet; annealing the hot-rolled steel sheet; first cold rolling the hot-rolled steel sheet that has been annealed; first decarburizing annealing the steel sheet that has been cold rolled; second cold rolling the steel sheet that has been decarburized; second decarburizing annealing the steel sheet that has been cold rolled; a first non-oxidizing annealing step in which the steel sheet that has been decarburized the second time is annealed at a temperature of 1000℃ to 1200℃ and a dew point temperature of -20℃ or lower; a third cold rolling step in which the steel sheet that has been cold rolled the first time is cold rolled the third time; and a second non-oxidizing annealing step in which the steel sheet that has been cold rolled the third time is annealed at a cracking temperature of 750 to 1050℃ for 30 seconds to 5 minutes.
[0009] The slab may contain, in weight percent, Si: 1.0% to 4.0%, C: 0.1% to 0.4%, and the remainder being Fe and unavoidable impurities.
[0010] The slab may further contain Mn: 0.1 wt% or less and S: 0.005 wt% or less.
[0011] The annealing step of the hot-rolled plate may include a decarburization process.
[0012] The step of annealing the hot-rolled plate can be performed at a temperature of 850°C to 1000°C and a dew point temperature of 70°C or lower.
[0013] The first decarburization annealing step can be performed at a temperature of 850°C to 1000°C and a dew point temperature of 50°C to 70°C.
[0014] The first decarburization annealing step can be performed in an austenite single-phase region or in a region where a complex phase of ferrite and austenite exists.
[0015] After the first decarburization annealing step, the average diameter of the crystal grains may be 150 to 250 μm.
[0016] The first decarburization annealing step and the second cold rolling step may be repeated two or more times.
[0017] The second decarburization annealing step can be performed at a temperature of 850°C to 1000°C and a dew point temperature of 50°C to 70°C.
[0018] The second decarburization annealing step can be performed for 30 seconds to 5 minutes.
[0019] The first non-oxidizing annealing step can be performed for 30 seconds to 5 minutes.
[0020] The first non-oxidizing annealing step may further include a subsequent pickling step.
[0021] The second non-oxidizing annealing step can be performed in an atmosphere with a dew point temperature of -20℃ or lower.
[0022] A oriented electrical steel sheet according to one embodiment of the present invention has grains in which the {111} planes form an angle of 15˚ or less with the rolled surface of the steel sheet, arranged continuously in a strip shape, wherein the aspect ratio of the strip shape is 10 or greater and the density of the strip shape is 100 mm 2 There can be 5 to 1,000 per unit.
[0023] A oriented electrical steel sheet according to one embodiment of the present invention has a grain density of 100 mm² in which the {111} plane forms an angle of 15˚ or less with the rolled plane of the steel sheet. 2 There are 500 to 100,000 pieces per unit.
[0024] The fraction of crystal grains with a grain diameter of 10㎛ to 100㎛ among the total crystal grains may be 20% to 99%.
[0025] A oriented electrical steel sheet according to one embodiment of the present invention is in the Gos direction ({110} <001> The fraction of crystal grains forming an angle of 15˚ or less with ) may be 10 to 95%.
[0026] A oriented electrical steel sheet according to one embodiment of the present invention may contain, in weight percent, Si: 1.0% to 4.0%, C: 0.005% or less (excluding 0%), and the remainder being Fe and unavoidable impurities.
[0027] A oriented electrical steel sheet according to one embodiment of the present invention may further include Mn: 0.1 wt% or less and S: 0.005 wt% or less. Effects of the invention
[0028] A oriented electrical steel sheet according to one embodiment of the present invention utilizes normal crystal growth and has excellent magnetic properties, and in particular, excellent high-frequency iron loss.
[0029] In addition, since AlN and MnS are not used as grain growth inhibitors, there is no need to heat the slab to a high temperature of 1300°C or higher.
[0030] In addition, since it is not necessary to remove precipitates N and S, the purification annealing time can be relatively shortened, and productivity can be improved.
[0031] In addition, it is possible to provide a oriented electrical steel sheet having uniform magnetic properties in the width direction. Brief explanation of the drawing
[0032] Figure 1 is a photograph showing the surface of a grain-oriented electrical steel sheet manufactured in the invention material 5 analyzed by an electron microscope, with {111} / / ND grains indicated in blue. FIG. 2 is a photograph showing the surface of a grain-oriented electrical steel sheet manufactured in invention material 5 analyzed by an electron microscope, and Goss ({110} <001> This is a photo showing the crystal grains in green. Specific details for implementing the invention
[0033] Terms such as first, second, and third are used to describe various parts, components, regions, layers, and / or sections, but are not limited thereto. These terms are used solely to distinguish one part, component, region, layer, or section from another part, component, region, layer, or section. Accordingly, the first part, component, region, layer, or section described below may be referred to as the second part, component, region, layer, or section without departing from the scope of the present invention.
[0034] The technical terms used herein are for the reference of specific embodiments only and are not intended to limit the invention. The singular forms used herein include plural forms unless phrases clearly indicate otherwise. As used in the specification, the meaning of “comprising” specifies certain characteristics, areas, integers, steps, actions, elements, and / or components, and does not exclude the presence or addition of other characteristics, areas, integers, steps, actions, elements, and / or components.
[0035] When it is stated that one part is "above" or "on" another part, it may be directly above or on the other part, or other parts may be involved in between. In contrast, when it is stated that one part is "directly above" another part, no other parts are interposed in between.
[0036] Unless otherwise defined, all terms used herein, including technical and scientific terms, have the same meaning as generally understood by those skilled in the art to which this invention pertains. Terms defined in commonly used dictionaries are further interpreted to have meanings consistent with relevant technical literature and the present disclosure, and are not interpreted in an ideal or highly formal sense unless otherwise defined.
[0037] Also, unless otherwise specified, % means weight %, and 1 ppm is 0.0001 weight %.
[0038] In one embodiment of the present invention, the meaning of including additional elements is that the remainder of iron (Fe) is replaced by an amount of the additional element.
[0039] Hereinafter, embodiments of the present invention are described in detail so that those skilled in the art can easily implement the invention. However, the present invention may be embodied in various different forms and is not limited to the embodiments described herein.
[0041] A method for manufacturing a oriented electrical steel sheet according to one embodiment of the present invention comprises the steps of: hot rolling a slab to produce a hot-rolled steel sheet; annealing the hot-rolled steel sheet; first cold rolling the hot-rolled steel sheet that has been annealed; first decarburizing annealing the steel sheet that has been cold rolled; second cold rolling the steel sheet that has been decarburized; second decarburizing annealing the steel sheet that has been cold rolled; a first non-oxidizing annealing step in which the steel sheet that has been decarburized the second time is annealed at a temperature of 1000℃ to 1200℃ and a dew point temperature of -20℃ or lower; a third cold rolling step in which the steel sheet that has been cold rolled the first time is cold rolled the third time; and a second non-oxidizing annealing step in which the steel sheet that has been cold rolled the third time is annealed at a cracking temperature of 750 to 1050℃ for 30 seconds to 5 minutes.
[0042] Below, each step is explained in detail.
[0043] First, the slab is hot-rolled.
[0044] The slab may contain, in weight percent, Si: 1.0% to 4.0%, C: 0.1% to 0.4%, and the remainder being Fe and unavoidable impurities.
[0045] The reason for limiting the composition is as follows.
[0046] Silicon (Si) improves iron loss by lowering the magnetic anisotropy of electrical steel sheets and increasing their resistivity. When the Si content is less than 1.0 wt%, the iron loss becomes inferior, and when it exceeds 4.0 wt%, the brittleness increases. Therefore, the Si content in the oriented electrical steel sheet after the slab and final annealing steps may be 1.0 to 4.0 wt%. More specifically, the Si content may be 1.5 to 3.5 wt%.
[0047] Since a process is required for carbon (C) to escape from the center to the surface layer so that Goss grains in the surface layer diffuse to the center during intermediate decarburization and final decarburization, the carbon content in the slab may be 0.1 to 0.4 weight%. More specifically, the carbon content in the slab may be 0.15 to 0.3 weight%. In addition, the carbon content in the final oriented electrical steel sheet manufactured after the continuous annealing step in which decarburization is completed may be 0.0050 weight% or less. More specifically, it may be 0.002 weight% or less.
[0048] The slab may further contain Mn: 0.1 wt% or less and S: 0.005 wt% or less.
[0049] Mn and S form MnS precipitates, which hinder the growth of Goss grains that diffuse into the center during the decarburization process. Therefore, it is desirable not to add Mn and S. However, considering the amount inevitably incorporated during the steelmaking process, Mn and S in the oriented electrical steel sheet after the slab and final annealing stage can be controlled to Mn: 0.1 wt% or less and S: 0.005 wt% or less, respectively.
[0050] The remainder comprises Fe and unavoidable impurities. Unavoidable impurities are those introduced during the steelmaking stage and the manufacturing process of oriented electrical steel sheets; as this is widely known in the field, a detailed explanation is omitted. Specifically, since components such as Al, N, Ti, Mg, and Ca react with oxygen in the steel to form oxides, it is necessary to strongly suppress them; therefore, each component can be managed to a level of 0.005 weight% or less. In one embodiment of the present invention, the addition of elements other than the aforementioned alloy components is not excluded, and various elements may be included within a scope that does not impair the technical spirit of the present invention. If additional elements are included, they replace the remainder, Fe.
[0051] More specifically, the slab may consist of, in weight percent, Si: 1.0% to 4.0%, C: 0.1% to 0.4%, and the remainder being Fe and unavoidable impurities.
[0052] The slab may be heated before hot rolling. The slab heating temperature may be 1100°C to 1350°C, which is higher than the usual heating temperature. When the temperature is high during slab heating, there is a problem in that the hot-rolled structure becomes coarse, which has an adverse effect on magnetism. However, the method for manufacturing a oriented electrical steel sheet according to one embodiment of the present invention has a relatively high carbon content in the slab, so the hot-rolled structure does not become coarse even if the slab reheating temperature is high, and by reheating at a higher temperature than in the usual case, it is more advantageous during hot rolling.
[0053] Hot rolling can be used to produce hot-rolled plates with a thickness of 1.5 to 4.0 mm by applying an appropriate rolling reduction rate at the final cold rolling stage so that the final product thickness can be produced.
[0054] The hot rolling temperature or cooling temperature is not specifically limited, but as an example of excellent magnetic properties, the hot rolling end temperature can be set to 950°C or lower, and the cooling can be rapid with water and coiled at 600°C or lower.
[0055] Next, the hot-rolled steel sheet is annealed. At this time, the annealing of the hot-rolled sheet may include a decarburization process. Specifically, the annealing of the hot-rolled sheet may be performed at a temperature of 850°C to 1000°C and a dew point temperature of 70°C or lower. After the aforementioned annealing, additional annealing may be performed at a temperature of 1000°C to 1200°C and a dew point temperature of 0°C or lower. After performing the annealing of the hot-rolled sheet, pickling may be performed.
[0056] Next, a cold-rolled steel sheet is manufactured by performing a first cold rolling.
[0057] In the manufacturing process of conventional oriented electrical steel sheets, it is known that cold rolling is effective when performed once with a high reduction rate of nearly 90%. This is because it creates an environment favorable for grain growth for only the Goss grains among the primary recrystallized grains. However, since the method for manufacturing an oriented electrical steel sheet according to one embodiment of the present invention does not utilize abnormal grain growth of Goss orientation grains and instead diffuses the Goss grains in the surface layer generated by decarburization annealing and cold rolling inward, it is advantageous to form a large number of Goss orientation grains distributed in the surface layer.
[0058] Therefore, when cold rolling is performed at a reduction rate of 50% to 70%, a large number of Goss textures may be formed in the surface layer. More specifically, it may be 55% to 65%.
[0059] Next, the steel sheet that has been cold-rolled for the first time is subjected to a first decarburization annealing. At this time, the decarburization annealing step may be performed in an austenite single-phase region or in a region where a complex phase of ferrite and austenite exists. Specifically, annealing may be performed at a temperature of 850°C to 1000°C and a dew point temperature of 50°C to 70°C. In addition, the atmosphere may be a mixed gas atmosphere of hydrogen and nitrogen. Furthermore, the amount of decarburization during decarburization annealing may be 0.0300 wt% to 0.0600 wt%. After the aforementioned annealing, additional annealing may be performed at a temperature of 1000°C to 1200°C and a dew point temperature of 0°C or lower.
[0060] During this first decarburization annealing process, the grain size on the surface of the electrical steel sheet grows coarsely, while the grains inside the electrical steel sheet remain as a fine structure. After this first decarburization annealing, the average grain diameter can be 150㎛ to 250㎛. At this time, the grains are surface ferrite grains. Furthermore, the grain diameter refers to the diameter of a hypothetical circle having the same area as the grain. The reference plane is a plane parallel to the rolling plane (ND plane).
[0061] Next, the steel sheet that has completed the first decarburization annealing is subjected to a second cold rolling. Since the second cold rolling is identical to the first cold rolling, a detailed explanation is omitted.
[0062] The aforementioned first decarburization annealing step and second cold rolling step may be repeated two or more times. By repeating the process two or more times, a large number of Goss textures can be formed in the surface layer. In one embodiment of the present invention, a Goss texture refers to a texture that forms an angle of 15˚ or less with the Goss direction. That is, the rolling direction (RD direction) of the rolling surface (ND surface) of the steel sheet is {110} of the crystal grains <001> It refers to crystal grains that form an angle of 15˚ or less with the direction.
[0063] Next, the steel sheet that has completed secondary cold rolling is subjected to secondary decarburization annealing.
[0064] The second decarburization annealing step is performed at a temperature of 850°C to 1000°C and a dew point temperature of 50°C to 70°C. Prior to the second annealing, the cold-rolled sheet undergoes decarburization annealing, leaving a carbon content of 40% to 60% relative to the carbon weight of the slab. Therefore, during the second decarburization annealing step, as carbon is removed, the crystal grains formed on the surface layer diffuse inward. During the second decarburization annealing step, decarburization can be performed so that the carbon content in the steel sheet becomes 0.005 weight% or less. The atmosphere may be a mixed atmosphere of hydrogen and nitrogen.
[0065] The second decarburization annealing step can be performed for 30 seconds to 5 minutes. Decarburization can be sufficiently achieved within the aforementioned time range.
[0066] Next, the steel sheet subjected to secondary decarburization annealing is subjected to primary non-oxidizing annealing at a temperature of 1000°C to 1200°C and a dew point temperature of -20°C or lower. If the steel sheet subjected to secondary decarburization annealing is further subjected to tertiary cold rolling without non-oxidizing annealing, insufficient grain growth does not occur, which may result in a low Goss fraction. Furthermore, problems may arise in that not only does rolling roll wear occur due to the surface oxide layer, but productivity during rolling is also reduced. In one embodiment of the present invention, by improving the Goss fraction through the step of primary non-oxidizing annealing, the magnetic properties can be further improved through tertiary cold rolling and heat treatment. More specifically, annealing can be performed in an atmosphere of 99 volume% or more hydrogen at a dew point temperature of -50 to -30°C.
[0067] The first non-oxidizing annealing step can be performed for 30 seconds to 5 minutes. Within the aforementioned time range, sufficient growth of grains ({111} / / ND) can be achieved in which the {111} plane forms an angle of 15˚ or less with the rolled plane of the steel sheet.
[0068] After the first non-oxidizing annealing step, a step of pickling the steel sheet may be further included. By including the pickling step, the oxide layer formed on the surface of the steel sheet during the first and second decarburization annealing processes can be removed. Since this oxide layer remains on the surface even after rolling and hinders the movement of magnetic domains, thereby adversely affecting magnetism, it can be removed through pickling. The pickling method is not particularly limited, but it may be performed by immersing the steel sheet in a hydrochloric acid solution of 3.0 to 22.0 wt% for 15 to 200 seconds during the pickling step. At this time, the hydrochloric acid temperature may be 50 to 90°C. If the concentration of hydrochloric acid is too low or the immersion time is too short, the oxide layer present on the surface of the steel sheet may not be sufficiently removed; if the concentration is too high or the immersion time is too long, damage to the surface of the steel sheet may occur beyond the removal of the oxide layer. More specifically, it can be performed by immersing in a 10.0 to 18.0 weight% hydrochloric acid solution for 20 seconds to 100 seconds.
[0069] Next, the steel sheet that has been annealed without oxidation is cold-rolled a third time. By performing the third cold-rolling, a steel sheet with a final thickness of 20 to 150 μm can be manufactured. When the third cold-rolling is added, the {111} / / ND grain density increases, and as a result, magnetic properties, particularly high-frequency iron loss, can be improved.
[0070] Next, the steel sheet, after the third cold rolling is completed, can be subjected to a second non-oxidizing annealing at a cracking temperature of 750 to 1050°C for 30 seconds to 5 minutes. The purpose of the second non-oxidizing annealing step is to grow the crystal grains to a certain size or larger. Through this, the {111} / / ND crystal grain density increases, and as a result, magnetic properties, particularly high-frequency iron loss, can be improved. If the cracking temperature is too low or the time is too short, the Goss crystal grains may not develop properly. If the cracking temperature is too high or the time is too long, the Goss crystal grains do not remain at a fine size advantageous for high-frequency iron loss but grow, and a problem may occur in which the fraction of Goss crystal grains actually decreases during the growth process. More specifically, the cracking temperature of the second non-oxidizing annealing can be 800 to 1000°C. More specifically, it can be 900 to 970°C.
[0071] The second non-oxidizing annealing step can be performed at a dew point temperature of -20°C or lower. If the dew point temperature is too high, an oxide layer may form on the surface, which may adversely affect magnetism. More specifically, annealing can be performed in an atmosphere of 99% or more by volume of hydrogen at a dew point temperature of -50 to -30°C.
[0072] After the first cold rolling step, the process can be performed as a continuous process up to the second non-oxidizing annealing step. A continuous process means that there is no batch process, such as winding the steel sheet into a coil and annealing it. As previously mentioned, a continuous process is possible because the first decarburization annealing step and the second non-oxidizing annealing step are completed within a few minutes.
[0073] As such, by adding a third cold rolling step and adding first and second non-oxidizing annealing steps before and after the third cold rolling step, the density of {111} / / ND grains increases and the Goss fraction increases. This leads to an improvement in magnetism, and in particular, high-frequency iron loss is dramatically improved.
[0075] The final oriented electrical steel sheet manufactured after completing the second non-oxidizing annealing step has a grain density of 100 mm² where the {111} planes form an angle of 15˚ or less with the rolled plane of the steel sheet. 2 There are 500 to 100,000 grains per. In one embodiment of the present invention, the {111} grains, i.e., {111} / / ND grains, in which the {111} plane forms an angle of 15˚ or less with the rolled plane of the steel plate, serve to reduce high-frequency iron loss by reducing the size of the magnetic domains. If too few {111} / / ND grains exist, the size of the magnetic domains increases and the magnetic properties may be inferior. Conversely, if a large number of {111} / / ND grains are formed, it may become a problem because the number of grains with a Goss orientation favorable for magnetism decreases. More specifically, there may be 1,000 to 50,000 {111} / / ND grains. More specifically, there may be 2,000 to 20,000. The reference plane is not significantly limited and may be a plane parallel to the rolled plane (ND plane). The density of {111} / / ND grains can be formed in large numbers through the aforementioned secondary non-oxidation step. This has been specifically explained in relation to the manufacturing method of the aforementioned grain-oriented electrical steel sheet, so a redundant explanation is omitted. {111} / / ND The number of grains can be calculated starting from grains with a grain size of 5 μm or more.
[0076] Crystal grains in which the {111} plane forms an angle of 15˚ or less with the rolled surface of the steel sheet are continuously arranged in a strip shape. The density of the strip shape is 100 mm 2 There can be 5 to 1,000 per unit. If the number of band shapes is too small, it is difficult for the effect of reducing magnetic domain size due to the band shape to be fully manifested. If the number of band shapes is too large, the number of crystal grains with the Goss orientation, which is favorable for magnetism, may decrease. More specifically, the density of band shapes is 100 mm 2 There may be 20 to 500 pieces per unit. More specifically, the density of the strip shape is 100 mm 2 There can be 50 to 200 pieces per.
[0077] The term "continuous" means that the boundaries between {111} / / ND grains are adjacent and adjacent to each other. A strip shape refers to an elongated arrangement with an aspect ratio of 10 or more. Specifically, it can be arranged with a width of 0.05 mm to 1.0 mm and a height of 0.5 mm to 10 mm. In this case, the horizontal direction can be the direction perpendicular to the rolling process. Each strip shape may contain 10 to 300 {111} / / ND grains. This strip shape serves to improve high-frequency iron loss by reducing the size of magnetic domains. The strip shape is formed through a secondary non-oxidizing heat treatment step at the location of the grain boundaries created by rolling. Since this has been specifically explained in relation to the aforementioned manufacturing method of oriented electrical steel sheets, redundant explanations are omitted.
[0078] In one embodiment of the present invention, the fraction of grains with a grain diameter of 10 μm to 100 μm among the total grains may be 20% to 99%. This is because in one embodiment of the present invention, first and second decarburization annealing and first and second non-oxidation annealing were performed for a short period of time. If annealing is performed for a long period of time, such as for one hour or more through batch annealing as in the prior art, the average grain diameter increases by 5 mm or more, which is completely different from the grain diameter distribution of the oriented electrical steel sheet according to one embodiment of the present invention. More specifically, the fraction of grains with a grain diameter of 10 μm to 100 μm among the total grains may be 50% or more. More specifically, the fraction of grains with a grain diameter of 10 μm to 100 μm among the total grains may be 90% to 99%. Such fine grains contribute to improving high-frequency iron loss. The grain fraction refers to the volume fraction, and the area of a grain having the corresponding grain size in any cross-section of the steel plate is calculated and considered as the volume fraction. In one embodiment of the present invention, the grain size may not vary in the thickness direction. The grain size is calculated by assuming a virtual circle having the same area as the grain and using the diameter of that circle.
[0079] A oriented electrical steel sheet according to one embodiment of the present invention is in the Gos direction ({110} <001> The fraction of grains forming an angle of 15° or less with ) may be 10 to 95%. The fraction of Goss grains also contributes to improving high-frequency iron loss. More specifically, the fraction of Goss grains may be 50 to 90%. In one embodiment of the present invention, the area of grains having the corresponding orientation is calculated at any cross-section of the steel plate and considered as a volume fraction. The fraction of Goss grains may not fluctuate. In one embodiment of the present invention, by forming an elongated {111} / / ND grain set around the grains of Goss orientation, the size of the magnetic domains formed by the Goss orientation grains can be finely divided using the band-shaped {111} / / ND grains, thereby improving high-frequency iron loss.
[0080] In one embodiment of the present invention, the effect may be manifested by the unique manufacturing process and the unique microstructure generated by the manufacturing process, rather than by the alloy composition of the grain-oriented electrical steel sheet. Additionally, regarding the alloy composition of the grain-oriented electrical steel sheet, the grain-oriented electrical steel sheet according to one embodiment of the present invention may contain, in weight percent, Si: 1.0% to 4.0%, C: 0.005% or less (excluding 0%), and the remainder being Fe and unavoidable impurities. Furthermore, the grain-oriented electrical steel sheet according to one embodiment of the present invention may further contain Mn: 0.1% by weight or less and S: 0.005% by weight or less. Since the description of the alloy composition of the grain-oriented electrical steel sheet is identical to the description of the alloy composition of the slab described above, a redundant description is omitted.
[0081] In one embodiment of the present invention, the oriented electrical steel sheet has excellent magnetic properties, particularly high-frequency iron loss. Specifically, W 10 / 400 This may be 10.00 W / kg or less. W 2 / 5000 It may be 11.00 W / kg or less. W 0.5 / 20000It may be 5.00 W / kg or less. More specifically, W 10 / 400 This can be 6.00 to 10.00 W / kg. W 2 / 5000 It can be 8.00 to 11.00 W / kg. W 0.5 / 20000 It can be 2.00 to 5.00 W / kg.
[0082] Iron Hand W 10 / 400 is the magnitude (W / kg) of the induced iron loss under conditions of 1.0 Tesla and 400 Hz. Iron loss W 2 / 5000 is the magnitude of the induced iron loss (W / kg) under conditions of 0.2 Tesla and 5000 Hz. Iron loss W 0.5 / 20000 is the magnitude of the iron loss induced under conditions of 0.05 Tesla and 20,000 Hz (W / kg).
[0084] Specific embodiments of the present invention are described below. However, the following embodiments are merely specific examples of the present invention, and the present invention is not limited to the following embodiments.
[0086] Examples
[0087] A slab containing 2.8% Si and 0.204% C by weight, with the remainder being Fe and unavoidable impurities, was heated at a temperature of 1150°C and then hot-rolled, followed by annealing of the hot-rolled sheet at an annealing temperature of 950°C and a dew point temperature of 60°C. Afterward, the steel sheet was cooled, pickled, and then cold-rolled once with a reduction rate of 65% to produce a cold-rolled sheet with a thickness of 0.8 mm.
[0088] The steel sheet that was cold-rolled once was subjected to first decarburization annealing for 80 seconds in a humid mixed gas atmosphere of hydrogen and nitrogen (dew point temperature 60°C) at a temperature of 950°C, and then cold-rolled again with a reduction rate of 65% to produce a second cold-rolled sheet with a thickness of 0.28 mm.
[0089] Subsequently, a second decarburization annealing was performed for 2 minutes in a humid mixed gas atmosphere of hydrogen and nitrogen (dew point temperature 60°C) at a temperature of 950°C, followed by a first non-oxidizing annealing for 3 minutes in a hydrogen atmosphere at 1100°C (dew point temperature -40°C). Afterward, the oxide layer on the surface was removed by pickling for 30 seconds in an 18.5 mass% HCl solution at 80°C.
[0090] The pickled electrical steel sheets were cold-rolled three times to a thickness of 50 µm and subjected to secondary non-oxidizing annealing for 150 seconds in a hydrogen atmosphere (dew point temperature -40°C) at the temperatures listed in Table 1 below. The Goss fraction of the grains and the number of bands composed of {111} / / ND grains were determined through EBSD analysis. The iron loss distribution was calculated while varying the applied frequency from 50 to 20,000 Hz and summarized in Table 1.
[0091] Comparative material 4 is an example in which the first non-oxidizing annealing was omitted and the third cold rolling was performed, and Comparative material 5 is an example in which the third cold rolling and the second non-oxidizing annealing were omitted and the process was terminated at the first non-oxidizing annealing.
[0092] note Heat treatment temperature (°C) Goss share (%) Band density ( / 100mm 2 ) Iron loss (W / Kg) W15 / 50 W10 / 400 W2 / 5000 W0.5 / 20000 Comparative Material 1 600 2 0 5.20 27.50 17.20 11.40 Comparative Material 2 700 5 0 2.40 12.40 11.40 7.91 Invention Material 1 800 67 72 1.06 6.34 10.50 3.52 Invention Material 2 850 76 86 0.99 7.15 10.10 3.14 Invention Material 3 880 66 165 0.98 7.15 10.20 2.94 Invention Material 4 900 76 111 0.95 7.55 9.45 2.75 Invention Material 5 930 55 177 0.95 7.85 9.67 2.45 Invention Material 6 950 78 133 0.87 7.34 10.11 2.86 Invention Material 7 970 69 188 0.99 8.01 9.87 2.33 Invention Material 8 980 80 115 1.00 7.45 9.99 2.87 Invention Material 9 1000 48 29 0.99 7.36 9.54 3.19 Comparative Material 3 1100 11 2 1.12 11.50 12.50 8.52 Comparative material 4 900 8 70 1.88 12.44 12.34 8.44 Comparative material 5 omission 75 0 1.14 8.99 19.22 16.72
[0093] As shown in Table 1, during the second non-oxidizing annealing process, depending on the temperature, a band shape of {111} / / ND grains and a number of Goss grains are formed, and it can be confirmed that high-frequency iron loss is improved through this.
[0094] It can be confirmed that Comparative Material 1 and Comparative Material 2, for which the temperature of the second non-oxidizing annealing is too low, do not undergo recrystallization, and that a band shape of {111} / / ND grains and a large number of Goss grains are not formed.
[0095] It can be confirmed that Comparative Material 3, which has a very high temperature for secondary non-oxidizing annealing, fails to form a band shape of {111} / / ND grains and a large number of Goss grains during the recrystallization growth process.
[0096] It can be confirmed that Comparative Material 4 had a large number of band shapes of {111} / / ND grains but failed to form a large number of Goss grains, resulting in inferior high-frequency iron loss, and Comparative Material 5 had a large number of Goss grains but failed to form a large number of {111} / / ND grains, resulting in relatively inferior high-frequency iron loss.
[0097] Figure 1 is an electron microscope image of the surface of a grain-oriented electrical steel sheet manufactured in Invention Material 5, where {111} / / ND grains are indicated in blue. It can be seen that grains with {111} / / ND orientations are arranged continuously in a band-like pattern. Figure 2 is a Goss ({110} <001> This is a photograph showing the grains in green. It can be seen that most of the Goss grains are distributed between the band-shaped arrangement of {111} / / ND grains in Fig. 2.
[0099] The present invention is not limited to the above embodiments and / or examples but can be manufactured in various different forms, and those skilled in the art will understand that the invention can be implemented in other specific forms without changing the technical concept or essential features of the invention. Therefore, the embodiments and / or examples described above should be understood as illustrative in all respects and not restrictive.
Claims
Claim 1 A method for manufacturing a oriented electrical steel sheet, comprising the steps of: hot rolling a slab to produce a hot-rolled steel sheet; annealing the hot-rolled steel sheet; first cold rolling the hot-rolled steel sheet annealed thereto; first decarburization annealing the steel sheet cold-rolled thereto; second cold rolling the steel sheet after the first decarburization annealing is completed; second decarburization annealing the steel sheet after the second cold rolling is completed; first non-oxidizing annealing step of annealing the steel sheet after the second decarburization annealing is completed at a temperature of 1000℃ to 1200℃ and a dew point temperature of -20℃ or lower; third cold rolling the steel sheet after the first non-oxidizing annealing is completed; and second non-oxidizing annealing step of annealing the steel sheet after the third cold rolling is completed at a cracking temperature of 750 to 1050℃ for 30 seconds to 5 minutes. Claim 2 A method for manufacturing a oriented electrical steel sheet according to claim 1, wherein the slab comprises, in weight percent, Si: 1.0% to 4.0%, C: 0.1% to 0.4%, and the remainder being Fe and unavoidable impurities. Claim 3 A method for manufacturing a oriented electrical steel sheet according to claim 2, wherein the slab further comprises Mn: 0.1 wt% or less and S: 0.005 wt% or less. Claim 4 A method for manufacturing a oriented electrical steel sheet according to claim 1, comprising a decarburization process in the step of annealing the hot-rolled sheet. Claim 5 In claim 1, the step of annealing the hot-rolled sheet is a method for manufacturing a oriented electrical steel sheet, wherein the annealing is performed at a temperature of 850°C to 1000°C and a dew point temperature of 70°C or lower. Claim 6 A method for manufacturing a oriented electrical steel sheet according to claim 1, wherein the first decarburization annealing step is annealed at a temperature of 850°C to 1000°C and a dew point temperature of 50°C to 70°C. Claim 7 A method for manufacturing a oriented electrical steel sheet according to claim 1, wherein the first decarburization annealing step is annealed in an austenite single-phase region or in a region where a complex phase of ferrite and austenite exists. Claim 8 A method for manufacturing a oriented electrical steel sheet having an average grain diameter of 150 to 250 μm after the first decarburization annealing step according to claim 1. Claim 9 A method for manufacturing a oriented electrical steel sheet according to claim 1, wherein the first decarburization annealing step and the second cold rolling step are repeated two or more times. Claim 10 A method for manufacturing a oriented electrical steel sheet according to claim 1, wherein the second decarburization annealing step is annealed at a temperature of 850°C to 1000°C and a dew point temperature of 50°C to 70°C. Claim 11 In claim 1, the second decarburization annealing step is a method for manufacturing a oriented electrical steel sheet, annealing for 30 seconds to 5 minutes. Claim 12 A method for manufacturing a oriented electrical steel sheet according to claim 1, wherein the first non-oxidizing annealing step is annealed for 30 seconds to 5 minutes. Claim 13 A method for manufacturing a oriented electrical steel sheet according to claim 1, wherein the first non-oxidizing annealing step further comprises a subsequent pickling step. Claim 14 A method for manufacturing a oriented electrical steel sheet according to claim 1, wherein the second non-oxidizing annealing step is performed in an atmosphere with a dew point temperature of -20℃ or lower. Claim 15 Crystal grains in which the {111} planes form an angle of 15˚ or less with the rolled plane of the steel sheet are continuously arranged in a strip shape, the aspect ratio of the strip shape is 10 or greater, and the density of the strip shape is 100 mm 2 Grain-oriented electrical steel sheets with 5 to 1,000 pieces per sheet. Claim 16 In paragraph 15, the density of grains in which the {111} plane forms an angle of 15˚ or less with the rolled plane of the steel sheet is 100 mm 2 Grain-oriented electrical steel sheets with 500 to 100,000 individual units. Claim 17 In item 15, a grain-oriented electrical steel sheet having a fraction of grains with a grain diameter of 10㎛ to 100㎛ among the total grains of 20% to 99%. Claim 18 In item 15, an oriented electrical steel sheet having a fraction of grains forming an angle of 15˚ or less with the Gos direction of 10 to 95%. Claim 19 In item 15, the electrical steel sheet is a grain-oriented electrical steel sheet comprising, in weight percent, Si: 1.0% to 4.0%, C: 0.005% or less (excluding 0%), and the remainder being Fe and unavoidable impurities. Claim 20 In claim 19, the electrical steel sheet is a grain-oriented electrical steel sheet further comprising Mn: 0.1 wt% or less and S: 0.005 wt% or less.
Citation Information
Patent Citations
Ferritic stainless steel sheet and manufacturing method therefor
JP2019123892A
Oriented electrical steel sheet and method for manufacturing the same
KR1020160074350A
Grain oriented electrical steel sheet and manufacturing method of the same
KR1020210079753A