Positive electrode material, positive electrode sheet, secondary battery, and electric device
By controlling the Co content and proportion in the lithium-ion battery cathode material, the performance of the battery in low-temperature environments is improved, the problem of insufficient low-temperature power and capacity retention is solved, and the cost is reduced.
Patent Information
- Application Number
- PCT/CN2023/084068
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-03
AI Technical Summary
Existing lithium-ion batteries exhibit insufficient low-temperature power and low-temperature capacity retention in low-temperature environments. In particular, phosphate cathode materials have poor performance below -30°C, and the cost and controllability of ternary cathode materials are insufficient.
By controlling the Co content in the cathode material to satisfy the relationship of 0.032
The low-temperature power and low-temperature capacity retention rate of the battery are improved, while the cost of raw materials is reduced, and the problems of poor conductivity and rate performance caused by too low Co content are avoided.
Smart Images

Figure CN2023084068_03102024_PF_FP_ABST
Abstract
Description
Positive electrode material, positive electrode sheet, secondary battery and electrical device Technical Field
[0001] The present application relates to the field of battery technology, and in particular to a positive electrode material, a positive electrode sheet, a secondary battery, and an electrical device. Background Art
[0002] Since the commercialization of lithium-ion batteries, they have quickly become energy storage devices used in various fields of life due to their advantages such as high energy density, high battery voltage, long cycle life and no memory effect, and have also attracted widespread interest from expert researchers.
[0003] The NCM system, a ternary cathode material, offers high energy density, low cost, and long lifespan, but its safety and production process controllability are insufficient. Compared to ternary cathode materials, phosphate cathode materials offer advantages such as low cost, long cycle life, and stable charge and discharge cycles under high-temperature conditions, making them ideal cathode materials for lithium-ion batteries suitable for large-scale applications. However, lithium iron phosphate materials have low conductivity, poor rate performance, and unsatisfactory low-temperature performance (especially below -30°C).
[0004] Summary of the Invention
[0005] The present application provides a positive electrode material, a positive electrode plate, a secondary battery and an electrical device to improve the low-temperature power and low-temperature capacity retention rate of the battery.
[0006] In a first aspect of the present application, a positive electrode material is provided, including a phosphate positive electrode material and a ternary positive electrode material, and the positive electrode material satisfies the following equation 1:
[0007] Relationship 1: 0.032 <w(Co) / (w(Ni)+w(Mn)+w(A))≤0.075
[0008] Wherein, A is the doping element in the phosphate positive electrode material, w(Co) is the mass percentage of Co in the positive electrode material, w(Ni) is the mass percentage of Ni in the positive electrode material, w(Mn) is the mass percentage of Mn in the positive electrode material, and w(A) is the mass percentage of A in the positive electrode material.
[0009] The positive electrode material of the present application satisfies the above-mentioned equation 1 by controlling the Co content in the positive electrode material, thereby reducing the electron conductivity, increasing the impedance, and increasing the battery cycle temperature rise, thereby achieving improvements in the low-temperature power and low-temperature capacity retention rate of the battery; in addition, the reduction in the Co content is also beneficial to the raw material cost benefits.
[0010] In any embodiment of the first aspect, 1.55 < w(Co) < 3.25, optionally 1.8 < w(Co) < 2.9, further optionally 1.85 < w(Co) < 2.85; and / or 17.55 < w(Ni) < 29.55, optionally 19.2 < w(Ni) < 29.2, further optionally 19.9 < w(Ni) < 26.5; and / or 16.55 < w(Mn) < 21.55, optionally 18.2 < w(Mn) < 21.1, further optionally 18.4 < w(Mn) < 20.85; and / or 1.05 < w(A) < 6.55, optionally 2.2 < w(A) < 6.5, further optionally 2.35 < w(A) < 5.85. The control of the content of each of the above elements, especially the control of the Co content, can simultaneously ensure the low-temperature performance, energy density, cycle performance, and cost benefit of the battery.
[0011] In any embodiment of the first aspect, w(Co) / (w(Ni)+w(Mn)+w(A)) is 0.035 to 0.065, optionally 0.045 to 0.060. This further improves the low-temperature performance of the battery.
[0012] In any embodiment of the first aspect, the mass percentage of Ni element in the ternary cathode material is 20% < w’(Ni) ≤ 55%, optionally 25% ≤ w’(Ni) ≤ 50%, or 30% ≤ w’(Ni) ≤ 45%, or 30% ≤ w’(Ni) ≤ 40%. When the Ni element in the ternary cathode material is within the above range, the ternary cathode material can have good energy density and rate cycling performance.
[0013] In any embodiment of the first aspect, 0.062 < w'(Co) / w'(Ni) ≤ 0.410, optionally, w'(Co) / w'(Ni) is 0.062 to 0.158, further optionally w'(Co) / w'(Ni) is 0.083 to 0.136. The performance differences of different generations of ternary cathode materials with different Ni contents are large. Under the same generation of ternary cathode materials with the same Ni content, restricting the Co content within the above range can more prominently reduce costs and improve low-temperature performance, while also avoiding the problems of deterioration of the material's conductivity and poor rate performance caused by too low Co content.
[0014] In any embodiment of the first aspect, 0.08 < w(A) / w(Ni) ≤ 0.41, optionally w(A) / w(Ni) is 0.10 to 0.30, further optionally 0.12 to 0.28. Using the above relationship to further limit the ratio of the phosphate cathode material and the ternary cathode material can better exert the advantageous performance of both.
[0015] In any embodiment of the first aspect, the phosphate-based cathode material has a chemical formula of Li 1+x Mn 1-y A y P 1-z E z O4, wherein x is any value in the range of -0.100-0.100, y is any value in the range of 0.001-0.500, and z is any value in the range of 0.001-0.100. A includes one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ga, Sn, Sb, Nb, and Ge, and may optionally be one or more elements selected from the group consisting of Fe, Ti, V, and Mg. E includes one or more elements selected from the group consisting of B, Si, N, S, F, Cl, and Br, and may optionally be an element selected from the group consisting of B, Si, N, and S. Doping phosphates with elements A and E helps improve the structural stability of phosphate-based positive electrode materials and the rate performance of secondary batteries containing the same.
[0016] In any embodiment of the first aspect, the chemical formula of the phosphate positive electrode material is Li a A1 x Mn 1-y A2 y P 1- z D z O 4-n G n , wherein the A1 includes one or more elements from the group consisting of Zn, Al, Na, K, Mg, Nb, Mo and W, the A2 includes one or more elements from the group consisting of Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge, the D includes one or more elements from the group consisting of B (boron), S, Si and N, the G includes one or more elements from the group consisting of S, F, Cl and Br, the a is selected from the range of 0.9 to 1.1, the x is selected from the range of 0.001 to 0.1, the y is selected from the range of 0.001 to 0.5, the z is selected from the range of 0.001 to 0.1, the n is selected from the range of 0.001 to 0.1, and the phosphate-based positive electrode material is electrically neutral. By doping the above-mentioned specific elements at the above-mentioned four positions at the same time in specific amounts, the rate performance, cycle performance and / or high-temperature stability of the phosphate-based positive electrode material can be significantly improved.
[0017] In any embodiment of the first aspect, the phosphate cathode material further optionally has a core-shell structure, and the shell layer of the core-shell structure is a functional coating layer, and the functional coating layer is optionally one or more layers of pyrophosphate, phosphate, and carbon. The above-mentioned functional coating layer can effectively inhibit the dissolution of transition metals and reduce the side reactions on the surface of the phosphate cathode material.
[0018] In any embodiment of the first aspect, the ternary cathode material conforms to the chemical formula Li a Ni b Co c M1 d M2 e O f R g or Li with a coating layer on the surface a Ni b Co c M1 d M2 e O f R g , where 0.75 ≤ a ≤ 1.2, 0.38 < b < 0.85, 0.03 < c < 0.15, 0 < d < 1, 0 ≤ e ≤ 0.2, 1 ≤ f ≤ 2.5, 0 ≤ g ≤ 1, f + g ≤ 3, M1 includes one or both of Mn or Al, and optionally the molar ratio of Al to Mn is 0 to 1:4, M2 includes one or more of the group consisting of Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, Sr, Sb, Y, W, and Nb, and R includes one or more of the group consisting of N, F, S, and Cl.
[0019] The second aspect of the present application provides a positive electrode sheet, including a current collector and a positive electrode film layer, wherein the positive electrode film layer includes the positive electrode material of any one of the embodiments of the first aspect. The positive electrode sheet with the above positive electrode material of the present application can improve the low-temperature power and low-temperature capacity retention rate of the battery and reduce the raw material cost.
[0020] In any embodiment of the second aspect, the coating surface density of the above positive electrode film layer is 15.50 - 20.78 mg / cm 2 , and / or the tap density of the positive electrode active material is 2.4 - 3.40 g / cm 3 . The positive electrode sheet with the above coating surface density or tap density has a high capacity value, is also beneficial to the manufacturing process, and also has an improvement effect on the power performance of the battery cell.
[0021] The third aspect of the present application provides a secondary battery, which includes a positive electrode sheet, a separator, an electrolyte, and a negative electrode sheet, and the positive electrode sheet is any one of the above positive electrode sheets. The low-temperature power and low-temperature capacity retention rate of the secondary battery are effectively improved.
[0022] A fourth aspect of the present application provides an electrical device comprising a secondary battery, wherein the secondary battery comprises any one of the secondary batteries of the third aspect, and improves the power performance and charging capacity of the electrical device at low temperatures. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following is a brief introduction to the drawings required for use in the embodiments of the present application. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the drawings without creative work.
[0024] FIG1 is a schematic diagram of a secondary battery according to an embodiment of the present application.
[0025] FIG. 2 is an exploded view of the secondary battery according to the embodiment of the present application shown in FIG. 1 .
[0026] FIG3 is a schematic diagram of a battery module according to an embodiment of the present application.
[0027] FIG4 is a schematic diagram of a battery pack according to an embodiment of the present application.
[0028] FIG. 5 is an exploded view of the battery pack shown in FIG. 4 according to an embodiment of the present application.
[0029] FIG6 is a schematic diagram of an electric device using a secondary battery as a power source according to an embodiment of the present application.
[0030] In the drawings, the drawings are not drawn to scale.
[0031] Description of reference numerals:
[0032] 1 battery pack; 2 upper case; 3 lower case; 4 battery module; 5 secondary battery; 51 housing; 52 electrode assembly; 53 top cover assembly. DETAILED DESCRIPTION
[0033] The following detailed description of the embodiments of the present application is provided in conjunction with the accompanying drawings and examples. The following detailed description of the embodiments and the accompanying drawings are used to illustrate the principles of the present application, but are not intended to limit the scope of the present application, that is, the present application is not limited to the described embodiments.
[0034] Below, the embodiments of the positive electrode material, positive electrode sheet, negative electrode sheet, secondary battery and electric device of the present application are described in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0035] The "ranges" disclosed herein are defined in terms of lower and upper limits, where a given range is defined by selecting a lower limit and an upper limit, and the selected lower and upper limits define the boundaries of the particular range. Ranges defined in this manner can be inclusive or exclusive of the end values and can be combined arbitrarily, i.e., any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60 to 120 and 80 to 110 are listed for a particular parameter, it is understood that ranges of 60 to 110 and 80 to 120 are also contemplated. Furthermore, if minimum range values of 1 and 2 are listed, and if maximum range values of 3, 4, and 5 are listed, the following ranges are all contemplated: 1 to 3, 1 to 4, 1 to 5, 2 to 3, 2 to 4, and 2 to 5. In this application, unless otherwise indicated, the numerical range "a to b" is a shorthand representation of any combination of real numbers between a and b, where a and b are both real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0036] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0037] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0038] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0039] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.
[0040] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0041] [Secondary battery]
[0042] Secondary batteries, also known as rechargeable batteries or storage batteries, are batteries that can be recharged to activate the active materials after discharge and continue to be used.
[0043] Typically, a secondary battery includes a positive electrode sheet, a negative electrode sheet, a separator, and an electrolyte. During the battery's charge and discharge process, active ions (such as lithium ions) are embedded and released back and forth between the positive and negative electrode sheets. The separator is set between the positive and negative electrode sheets, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing active ions to pass through. The electrolyte between the positive and negative electrode sheets mainly plays the role of conducting active ions.
[0044] [Cathode material]
[0045] One embodiment of the present application provides a positive electrode material, which includes a phosphate positive electrode material and a ternary positive electrode material, and the positive electrode material satisfies the following relationship 1:
[0046] Relationship 1: 0.032 <w(Co) / (w(Ni)+w(Mn)+w(A))≤0.075
[0047] Wherein, A is the doping metal element in the phosphate positive electrode material, w(Co) is the mass percentage of Co in the positive electrode material, w(Ni) is the mass percentage of Ni in the positive electrode material, w(Mn) is the mass percentage of Mn in the positive electrode material, and w(A) is the mass percentage of A in the positive electrode material.
[0048] The content of each metal element in the positive electrode material can be tested by referring to the following method: using aqua regia in a 1+1 ratio, microwave digestion is used to digest the mixed positive electrode powder sample at a high temperature and high pressure of 200°C, and an inductively coupled plasma emission spectrometer (model: ICAP-7400) is used to perform ICP main element testing on the mixed positive electrode by inductively coupled plasma emission spectrometry.
[0049] The positive electrode material of the present application satisfies the above-mentioned relationship 1 by controlling the Co content in the positive electrode material, so that the Co content of the positive electrode material is relatively low, thereby reducing the electron conductivity, increasing the impedance, and increasing the battery cycle temperature rise, thereby achieving improvements in the low-temperature power and low-temperature capacity retention rate of the battery; in addition, the reduction in Co content is also beneficial to the cost benefits of raw materials.
[0050] In some embodiments, 1.55 <w(Co)<3.25,16.20<w(Ni)<29.55,16.55<w(Mn)<21.55,1.05<w(A)<6.55。
[0051] The above w(Co) can be selected within the above range, including but not limited to 1.55, 165, 1.75, 1.80, 1.85, 1.95, 2.0, 2.02, 2.05, 2.10, 2.15, 2.20, 2.25, 2.30, 2.35, 2.40, 2.45, 2.50, 2.55, 2.60, 2.65, 2.70, 2.75, 2.80, 2.85, 2.90, 2.95, 3.0, 3.05, 3.10, 3.15, 3.20 or 3.25.
[0052] The above w(Ni) can be selected within the above range, including but not limited to 16.20, 16.50, 17.00, 17.50, 18.00, 18.50, 18.70, 19.0, 19.50, 19.60, 18.80, 20.00, 22.30, 20.50, 21.00, 21.10, 21.20, 21.50, 21.60, 22.00, 22.50, 23.00, 23.50, 24.00, 24.50, 25.00, 25.20, 25.50, 26.00, 26.50, 27.00, 27.50, 28.00, 28.50, 29.00, and 29.50.
[0053] The above w(Mn) can be arbitrarily selected within the above range, including but not limited to 17.55, 18.00, 18.25, 18.40, 18.50, 19.00, 19.50, 20.00, 20.10, 20.15, 20.50, 21.00, 21.10, 21.20, 21.30, 21.40, 21.50, 21.55.
[0054] The above w(A) can be arbitrarily selected within the above range, including but not limited to 1.05, 1.10, 1.50, 2.00, 2.10, 2.30, 2.40, 2.70, 2.80, 2.90, 3.00, 3.20, 3.40, 3.50, 3.70, 3.80, 4.00, 4.10, 4.30, 4.50, 4.70, 4.90, 5.00, 5.20, 5.40, 5.60, 5.80, 6.00, 6.30, 6.50.
[0055] If the Co content is too low, the conductivity of the positive electrode sheet is poor, which is likely to cause deterioration of the battery rate performance and cycle performance. When the Co content is higher than a certain level, the relative content of Ni / Mn will decrease, resulting in losses in battery energy density and platform voltage, and an increase in raw material costs. In some embodiments, 1.8 < w(Co) < 2.9, optionally 1.85 < w(Co) < 2.85; and / or 19.2 < w(Ni) < 29.2, optionally 19.9 < w(Ni) < 26.5; and / or 18.2 < w(Mn) < 21.1, optionally 18.4 < w(Mn) < 20.85; and / or 2.2 < w(A) < 6.5, optionally 2.35 < w(A) < 5.85. The control of the content of each of the above elements, especially the control of the Co content, can simultaneously ensure the low-temperature performance, energy density, low-temperature cycle performance, and cost-benefit of the battery.
[0056] In some embodiments, the value of w(Co) / (w(Ni)+w(Mn)+w(A)) includes but not limited to 0.032, 0.033, 0.035, 0.036, 0.037, 0.038, 0.040, 0.042, 0.045, 0.048, 0.050, 0.054, 0.059, 0.60, 0.063, 0.065, 0.070, 0.075. In some embodiments, w(Co) / (w(Ni)+w(Mn)+w(A)) is 0.035 - 0.065, optionally 0.045 - 0.060, so as to further improve the low-temperature performance of the battery.
[0057] The performance differences of different generations of ternary cathode materials with different Ni contents are significant. In some embodiments, the mass percentage of Ni element in the ternary cathode material is 20% < w’(Ni) ≤ 55%, optionally 25% ≤ w’(Ni) ≤ 50%, or 30% ≤ w’(Ni) ≤ 45%, or 30% ≤ w’(Ni) ≤ 40%. The Ni element in the ternary cathode material within the above range can endow the ternary cathode material with better energy density and rate cycling performance. The ternary cathode material with the above w’(Ni) generally belongs to the ternary cathode material in which the proportion of Ni in the total amount of the three elements of Ni, Co, and Mn is 50-60% or the proportion of Ni in the total amount of the three elements of Ni, Co, and Mn is 60-70%.
[0058] In some embodiments, 0.062 < w'(Co) / w'(Ni) ≤ 0.410, and the w'(Co) / w'(Ni) includes but is not limited to 0.062, 0.065, 0.066, 0.070, 0.074, 0.078, 0.080, 0.082, 0.083, 0.085, 0.087, 0.090, 0.093, 0.095, 0.100, 0.110, 0.120, 0.125, 0.128, 0.130, 0.135, 0.140, 0.145, 0.155, 0.160, 0.167, 0.2, 0.3, 0.4. Optionally, w'(Co) / w'(Ni) is 0.062-0.158, and further optionally w'(Co) / w'(Ni) is 0.083-0.136. Under the same generation of ternary cathode materials with the same Ni content, restricting the Co content within the above range can more prominently reduce costs and improve low-temperature performance, while also avoiding the problems of deterioration of the material's conductivity and poor rate performance caused by too low Co content.
[0059] Since the ternary cathode material has a higher capacity energy density and voltage platform compared to the phosphate cathode material, and the phosphate cathode material has better cycle stability and cost advantages compared to the ternary cathode material. In some embodiments, 0.08 < w(A) / w(Ni) ≤ 0.41, and the w(A) / w(Ni) includes but is not limited to 0.080, 0.085, 0.09, 0.093, 0.095, 0.10, 0.11, 0.12, 0.13, 0.14, 0.15, 0.2, 0.22, 0.25, 0.26, 0.28, 0.3, 0.4. Optionally, w(A) / w(Ni) is 0.10-0.30, and further optionally 0.12-0.28. Using the above relationship to further limit the ratio of the phosphate cathode material and the ternary cathode material can better exert the advantageous properties of both.
[0060] The phosphate cathode material used in the present application can be a non-doped phosphate cathode material, a doped phosphate cathode material, or a coated phosphate cathode material commonly used as a cathode material. In some embodiments, the phosphate cathode material has a chemical formula of Li 1+x Mn 1-y A y P 1-z E z O4, wherein x is any value in the range of -0.100-0.100, y is any value in the range of 0.001-0.500, and z is any value in the range of 0.001-0.100. A includes one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ga, Sn, Sb, Nb, and Ge, and may optionally be one or more elements selected from the group consisting of Fe, Ti, V, and Mg. E includes one or more elements selected from the group consisting of B, Si, N, S, F, Cl, and Br, and may optionally be an element selected from the group consisting of B, Si, N, and S. Doping phosphates with elements A and E helps improve the structural stability of phosphate-based positive electrode materials and the rate performance of secondary batteries containing the same.
[0061] In some embodiments, the chemical formula of the phosphate cathode material is Li a A1 x Mn 1-y A2 y P 1-z D z O 4-n G n, wherein A1 comprises one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Nb, Mo and W, A2 comprises one or more elements selected from the group consisting of Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge, D comprises one or more elements selected from the group consisting of B (boron), S, Si and N, G comprises one or more elements selected from the group consisting of S, F, Cl and Br, a is selected from the range of 0.9 to 1.1, for example, 0.97, 0.977, 0.984, 0.988, 0.99, 0.991, 0.992, 0.993, 0.994, 0.995, 0.996, 0.997, 0.998, 1.01, and x is selected from the range of 0.001 to 0. 1, for example, 0.001, 0.005, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, y is selected from the range of 0.001 to 0.5, for example, 0.001, 0.005, 0.02, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.34, 0.345, 0.349, 0.35, 0.4, 0.5, z is selected from the range of 0.001 to 0.1, for example, 0.001, 0.005, 0.08, 0.1, n is selected from the range of 0.001 to 0.1, for example, 0.001, 0.005, 0.08, 0.1, and the phosphate positive electrode material is electrically neutral. A1, A2, D and G are elements doped at the Li, Mn, P and O positions of the compound LiMnPO4, respectively. Without wishing to be bound by theory, it is currently believed that the performance improvement of phosphate cathode materials is related to reducing the lattice change rate and surface activity of phosphate cathode materials during lithium insertion and extraction. Reducing the lattice change rate can reduce the lattice constant difference between the two phases at the grain boundary, reduce interfacial stress, and enhance Li +The transport capacity at the interface improves the rate performance of the positive electrode active material. However, high surface activity can easily lead to serious side reactions at the interface, exacerbating gas production, electrolyte consumption and interface damage, thereby affecting the cycle performance of the battery. The above-mentioned phosphate positive electrode materials reduce the lattice change rate by doping at Li and Mn sites. Mn site doping also effectively reduces surface activity, thereby inhibiting Mn dissolution and side reactions at the interface between the positive electrode active material and the electrolyte. P site doping makes the change rate of the Mn-O bond length faster, reduces the migration barrier of the small polaron of the material, and is beneficial to electronic conductivity. O site doping has a good effect on reducing side reactions at the interface. P and O site doping also affect the Mn dissolution and kinetic properties of antisite defects. Therefore, doping reduces the concentration of antisite defects in the material, improves the kinetic properties of the material, and can also change the morphology of the particles, thereby increasing the compaction density. The applicant has unexpectedly discovered that by simultaneously doping the Li, Mn, P, and O positions of the LiMnPO4 compound with specific elements in specific amounts, significantly improved rate performance can be achieved, while significantly reducing the dissolution of Mn and the Mn-doping element, resulting in significantly improved cycling performance and / or high-temperature stability, and increasing the material's compaction density. The combination of A1 and A2 is the metal doping element in the phosphate-based positive electrode material defined above.
[0062] In some embodiments, the phosphate-based positive electrode material may further optionally have a core-shell structure, wherein the shell layer of the core-shell structure is a functional coating layer, and the functional coating layer may optionally be one or more layers of pyrophosphate, phosphate, and carbon. Since the migration barrier of transition metals in pyrophosphate is relatively high (>1eV), the dissolution of transition metals can be effectively suppressed. Phosphate has excellent lithium ion conductivity and can reduce the surface impurity lithium content. The carbon layer can effectively improve the electrical conductivity and desolvation ability of LiMnPO4, and can also act as a "barrier" to further hinder the migration of manganese ions into the electrolyte and reduce the corrosion of the electrolyte on the active material; at the same time, the above-mentioned carbon layer can also optimize the conductive network around the ternary positive electrode material in the mixture, thereby improving the mixing uniformity of the phosphate-based positive electrode material and the ternary positive electrode material.
[0063] The ternary cathode material used in this application can be a ternary cathode material commonly used in cathode materials. In some embodiments, the ternary cathode material conforms to the chemical formula Li a Ni b Co c M1 d M2 e O f R g or Li with a coating layer on the surface a Ni b Co c M1 d M2e O f R g , where 0.75 ≤ a ≤ 1.2, 0.38 < b < 0.85, 0.03 < c < 0.15, 0 < d < 1, 0 ≤ e ≤ 0.2, 1 ≤ f ≤ 2.5, 0 ≤ g ≤ 1, f + g ≤ 3, M1 includes one or both of Mn or Al, and optionally the molar ratio of Al to Mn is 0 to 1:4, M2 includes one or more of the group consisting of Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, Sr, Sb, Y, W, and Nb, and R includes one or more of the group consisting of N, F, S, and Cl.
[0064] The phosphate cathode material and the ternary cathode material used in this application can both be made of existing materials in the prior art or prepared by known methods. For example, a series of lithium iron manganese phosphate cathode materials produced by Shenzhen Defang Nano Technology Co., Ltd. (abbreviated as Defang Nano in the examples); a series of ternary cathode materials produced by Ningbo Ronbay New Energy Technology Co., Ltd. (abbreviated as Ronbay in the examples).
[0065] [Positive electrode sheet]
[0066] The positive electrode sheet generally includes a positive electrode current collector and a positive electrode film layer provided on at least one side of the positive electrode current collector. The positive electrode film layer includes the positive electrode material of any of the above embodiments of this application. The positive electrode sheet with the above positive electrode material of this application can improve the low-temperature power and low-temperature capacity retention rate of the battery and reduce the raw material cost.
[0067] As an example, the positive electrode current collector has two surfaces opposite to each other in its own thickness direction, and the positive electrode film layer is provided on either or both of the two opposite surfaces of the positive electrode current collector. In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0070] In some embodiments, the positive electrode film layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), a vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, a vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, and a fluorine-containing acrylate resin.
[0071] In some embodiments, the positive electrode film layer may further include a conductive agent. For example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0072] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.
[0073] [Negative electrode]
[0074] The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer arranged on at least one side of the negative electrode current collector, wherein the negative electrode film layer includes a negative electrode active material.
[0075] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.
[0076] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base material. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer base material (such as a base material of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0077] In some embodiments, the negative electrode active material may be a negative electrode active material for a battery that is well known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate. The silicon-based material may be selected from at least one of elemental silicon, silicon oxides, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxides, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0078] In some embodiments, the negative electrode film layer may further include a binder. For example, the binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0079] In some embodiments, the negative electrode film layer may further include a conductive agent. For example, the conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0080] In some embodiments, the negative electrode film layer may optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).
[0081] In some embodiments, the negative electrode sheet can be prepared by the following method: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.
[0082] [Electrolytes]
[0083] The electrolyte conducts ions between the positive and negative electrodes. This application does not specify the type of electrolyte, and the electrolyte can be selected based on the needs. For example, the electrolyte can be liquid, gel, or solid.
[0084] In some embodiments, the electrolyte is liquid and includes an electrolyte salt and a solvent.
[0085] In some embodiments, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.
[0086] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.
[0087] In some embodiments, the electrolyte may optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, and additives that improve battery high or low temperature performance.
[0088] [Isolation film]
[0089] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.
[0090] In some embodiments, the material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0091] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator can be formed into an electrode assembly through a winding process or a lamination process.
[0092] In some embodiments, the secondary battery may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.
[0093] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. Alternatively, the outer packaging of the secondary battery can be a soft shell, such as a pouch-type soft shell. The soft shell can be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0094] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square, or any other shape. For example, FIG1 shows a secondary battery 5 with a square structure as an example.
[0095] In some embodiments, referring to Figure 2, the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can be formed into an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.
[0096] In some embodiments, secondary batteries can be assembled into a battery module. The number of secondary batteries contained in the battery module can be one or more. The specific number can be selected by those skilled in the art according to the application and capacity of the battery module.
[0097] Figure 3 shows an example battery module 4. Referring to Figure 3 , within the battery module 4, multiple secondary batteries 5 may be arranged sequentially along the length of the battery module 4. Of course, any other arrangement is also possible. Furthermore, the multiple secondary batteries 5 may be secured together using fasteners.
[0098] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.
[0099] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art based on the application and capacity of the battery pack.
[0100] Figures 4 and 5 illustrate an example battery pack 1. Referring to Figures 4 and 5 , the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 can be placed over the lower case 3 to form an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.
[0101] In addition, the present application also provides an electric device, which includes at least one of the secondary battery, battery module, or battery pack provided in the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electric device, and can also be used as an energy storage unit for the electric device. The electric device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but is not limited thereto.
[0102] As the electrical device, a secondary battery, a battery module or a battery pack can be selected according to its usage requirements.
[0103] Figure 6 shows an example of an electric device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the secondary battery, a battery pack or battery module can be used.
[0104] [Example]
[0105] The following examples are provided. The examples described below are illustrative and are intended only to explain the present invention and are not to be construed as limiting the present invention. Where specific techniques or conditions are not specified in the examples, the methods described in the literature in this area or the product specifications are used. Where the manufacturer of the reagents or instruments is not specified, they are all commercially available conventional products.
[0106] Sources of positive electrode materials, including phosphate positive electrode materials LiMn 0.6 Fe 0.4 PO4 was purchased from Defang Nano DY-3 type phosphate, ternary cathode materials were purchased from Rongbai Technology S760 series ternary materials, and the remaining cathode materials were prepared using the following methods.
[0107] Preparation Example 1
[0108] 1) Preparation of positive electrode active materials
[0109] Preparation of doped manganese oxalate: 1.3 mol of MnSO4﹒H2O and 0.7 mol of FeSO4﹒H2O were thoroughly mixed in a mixer for 6 hours. The mixture was transferred to a reactor and 10 L of deionized water and 2 mol of oxalic acid dihydrate (calculated as oxalic acid) were added. The reactor was heated to 80°C and stirred at 600 rpm for 6 hours. The reaction was terminated (no bubbles were generated) to obtain an Fe-doped manganese oxalate suspension. The suspension was then filtered and the filter cake was dried at 120°C and then ground to obtain a median particle size Dv50 Fe-doped manganese oxalate particles with a size of about 100 nm.
[0110] Preparation of doped lithium manganese phosphate: Take 1 mol of the above-mentioned manganese oxalate particles, 0.4985 mol of lithium carbonate, 0.0005 mol of Al2(SO4)3, an 85% phosphoric acid aqueous solution containing 0.999 mol of phosphoric acid, 0.001 mol of H4SiO4, 0.0005 mol of NH4HCl2 and 0.005 mol of sucrose and add them to 20L of deionized water. Transfer the mixture to a sand mill and grind and stir it for 10 hours to obtain a slurry. Transfer the slurry to a spray drying equipment for spray drying and granulation, set the drying temperature to 250°C, dry it for 4 hours, and obtain particles. In a protective atmosphere of nitrogen (90 volume %) + hydrogen (10 volume %), sinter the above powder at 700°C for 10 hours to obtain carbon-coated Li 0.997 Al 0.001 Mn 0.65 Fe 0.35 P 0.999 Si 0.001 O 3.999 Cl 0.001 .
[0111] Preparation Example 2
[0112] (1) Preparation of co-doped lithium manganese phosphate core
[0113] Preparation of Fe co-doped manganese oxalate: 689.5g of manganese carbonate (in terms of MnCO3, the same below) and 463.4g of ferrous carbonate (in terms of FeCO3, the same below) were thoroughly mixed in a blender for 6 hours. The mixture was transferred to a reactor, and 5 liters of deionized water and 1260.6g of oxalic acid dihydrate (in terms of C2H2O4.2H2O, the same below) were added. The reactor was heated to 80°C and stirred at 600rpm for 6 hours until the reaction terminated (no bubbles were generated) to obtain an Fe co-doped manganese oxalate suspension. The suspension was then filtered, and the filter cake was dried at 120°C and then ground to obtain Fe and S co-doped manganese oxalate dihydrate particles with a median particle size Dv50 of 100nm.
[0114] Preparation of Fe and S co-doped lithium manganese phosphate: Add 1793.4 g of manganese oxalate dihydrate particles obtained in the previous step, 369.0 g of lithium carbonate (calculated as Li2CO3, the same below), 1.6 g of 60% dilute sulfuric acid (calculated as 60% H2SO4, the same below) and 1148.9 g of ammonium dihydrogen phosphate (calculated as NH4H2PO4, the same below) to 20 liters of deionized water, and stir the mixture for 10 hours to mix it evenly to obtain a slurry. The slurry is transferred to a spray drying equipment for spray drying and granulation, and the drying temperature is set to 250°C and dried for 4 hours to obtain a powder. In a nitrogen (90 volume %) + hydrogen (10 volume %) protective atmosphere, the above powder is sintered at 700°C for 4 hours to obtain 1572.1 g of Fe and S co-doped lithium manganese phosphate Li 0.999 Mn 0.60 Fe 0.40 P 0.999 S 0.001 O4.
[0115] The method for determining the content of each element in the material is as follows:
[0116] Take about 0.4g of dry positive electrode sheet / powder or about 1g of wet positive electrode sheet / powder (both accurate to 0.0001g) in a 25ml beaker, add 2ml~5ml nitric acid, leave overnight, then place on a hot plate, heat at about 100℃ (use a voltage-regulating transformer to adjust the input voltage and temperature) until the positive electrode sheet / powder is digested, add 0.5ml of perchloric acid, and heat to digest at about 140℃ until the white smoke is gone. The residue should be white, otherwise nitric acid and perchloric acid should be added to repeat the digestion. Finally, use 7% (volume % of acid, the same below) hydrochloric acid to dissolve and extract. Depending on the content of the element to be measured, the volume is adjusted to an appropriate volume and then the test is started on the ICP-OES test instrument.
[0117] The test and corresponding calculation results are recorded in Table 1.
[0118] The ternary mass content in Table 1 represents the mass content of the ternary positive electrode material in the total of the ternary positive electrode material and the phosphate-based positive electrode material.
[0119] 1. Square aluminum shell battery:
[0120] The positive electrode materials in Table 1 were used as the positive electrode active materials of the positive electrode sheets to prepare square aluminum shell batteries, and the preparation method was as follows.
[0121] ① Preparation of positive electrode sheet:
[0122] The positive electrode active material, polyvinylidene fluoride (PVDF), and conductive carbon were added to a certain amount of N-methylpyrrolidone (NMP) with a mass ratio of active material: binder: conductive agent of 98:1:1. The mixture was stirred in a drying room to form a uniform slurry with a viscosity controlled at 3000-10000 mPa·s. The slurry was then coated on aluminum foil with a coating surface density of 18.77 mg / cm 2 , after drying and cold pressing, the final positive electrode sheet is made.
[0123] ② Preparation of negative electrode sheet:
[0124] Graphite, sodium carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR), and conductive carbon were added to a certain amount of deionized water. The mass ratio of graphite: sodium carboxymethyl cellulose: styrene-butadiene rubber: conductive agent was 90:2:3:5. The mixture was stirred to form a uniform slurry with a viscosity controlled at 3000-10000 mPa·s. The slurry was then coated on copper foil and dried and cold-pressed to form a negative electrode sheet.
[0125] ③Preparation of square aluminum shell battery:
[0126] The prepared and cut positive electrode sheet, negative electrode sheet and diaphragm (polyethylene (PE) porous polymer film) are wound, and then the positive and negative electrode tabs are ultrasonically welded. The positive electrode uses an aluminum tab and the negative electrode uses a copper tab. The positive and negative electrode tabs are located on the same side of the battery cell. The battery cell after the tab welding is placed in an aluminum shell of a suitable size for soft connection and top cover welding. The battery cell is vacuum dried at 175°C for 24 hours, and then injected with liquid (the electrolyte is 1mol / L LiPF6 / (ethylene carbonate (EC) + diethyl carbonate (DEC) + dimethyl carbonate (DMC)) (volume ratio 1:1:1) + 5wt.% fluoroethylene carbonate (FEC)), allowed to stand, formed, aged, exhausted, sealed, and capacity tested to obtain the prepared square aluminum shell battery.
[0127] 2. Low temperature performance test: -20℃ test current and power / -7℃ working condition test
[0128] -7℃ working condition test: The square aluminum shell battery prepared above was subjected to CLTC national standard working condition test at -7℃ (in the range of 2.1V-4.4V) and 25℃ (in the range of 2.5V-4.4V), and the discharge capacity C0 and C1 at room temperature of 25℃ and -7℃ were recorded respectively. The calculated C1 / C0 is the low-temperature capacity retention rate.
[0129] -20℃ test current power test: At -20℃, within the range of 2.1V-4.4V, first charge the battery cell at a constant current of 0.33C, then fully charge it to 4.4V at a constant voltage of 0.05C, and then discharge it to 10% SOC at 0.33C. Apply any current to discharge for 10s, and record the voltage value after 10s of discharge. When the current is maximum and the voltage is still >2.1V after 10s, record the corresponding discharge current I0 and U0 at this moment respectively. The test current power shown is I0*U0.
[0130] 3. 25℃ cycle performance test:
[0131] The prepared battery was charged to 4.4 V at 0.5C0 at 2.5-4.4 V in a constant temperature environment of 25°C, then charged at a constant voltage at 4.4 V to a current ≤ 0.05C0, allowed to stand for 5 minutes, and then discharged to 2.5 V at 1C0. The capacity was recorded as Cn (n = 1, 2, 3...). The above operation was repeated. After 500 charge and discharge cycles, the capacity retention rate was calculated according to the ratio of C500 / C3, and the corresponding capacity retention rate was used as the examination indicator of the cycle capacity.
[0132] 4. 25℃ rate performance test:
[0133] At 25°C, the above-mentioned battery cell is charged to 4.4V at a constant current of 0.33C, charged to 0.05C at a constant voltage, and then discharged to 2.5V at a constant current of 0.33C. The charge and discharge cycle is repeated three times, and the third discharge capacity is taken as C1. At 25°C, the above-mentioned battery cell is charged to 4.4V at a constant current of 0.33C, charged to 0.05C at a constant voltage, and then discharged to 2.5V at a constant current of 2C. The charge and discharge cycle is repeated three times, and the third discharge capacity is taken as C2. C2 / C1 can characterize the discharge rate capability of the battery cell at 2C.
[0134] The results are recorded in Table 2.
[0135] Table 2
[0136] According to the test results, it can be seen that the Co content in the ternary material NCM and the content ratio of NCM in the mixed positive electrode will affect the low-temperature power and low-temperature capacity retention rate of the battery. Examples 1-6 adjust the mass percentage of Co in the limiting electrode compared to Ni+Mn+A, and Examples 7-10 adjust the mass percentage range of Co in the electrode. After comparing the data of Examples 1 to 10, it is found that by controlling the Co content in the positive electrode material at a relatively low level, reducing the electron conductivity, increasing the impedance, and increasing the battery cycle temperature rise, the battery low-temperature power and low-temperature capacity retention rate can be improved. However, the Co content of Examples 1 and 2 is low, and the conductivity of the positive electrode is poor, which can easily cause the battery rate performance and cycle performance to deteriorate. When the Co content in Example 6 is high, it will cause a decrease in the relative content of Ni / Mn, the battery energy density and platform voltage will be lost, and the raw material cost will increase.
[0137] Examples 11-15 adjust the mass percentage range of Ni in the electrode, Examples 16-19 adjust the mass percentage range of Mn, Examples 20-26 adjust the mass percentage range of A, and Examples 41-46 adjust the A / Ni ratio range in the electrode. The adjustment of the content of the above elements, especially the Co content in Examples 8 and 9, can simultaneously ensure the low temperature performance, energy density, cycle performance and cost-effectiveness of the battery.
[0138] The performance of ternary positive electrode material generations with different Ni contents varies greatly. Examples 27-35 adjust the mass percentage of Ni in the ternary material NCM. Among them, the Ni element in the ternary positive electrode material in Example 31 enables the positive electrode material to have better low-temperature performance while also having higher energy density and rate cycling performance.
[0139] Examples 36-38 adjust the relative levels of Co / Ni in NCM. Under the generation system of ternary positive electrode materials with the same Ni content, limiting the Co content within the above range can more significantly reduce costs and improve low-temperature performance. At the same time, it also avoids the problem that too low Co content will cause the material's conductivity to deteriorate and the rate performance to deteriorate.
[0140] Comparative Examples 1 and 2 show that when the LMAP content in the electrode is too large, the battery energy density gain will deteriorate; Comparative Examples 3 and 4 show that when the Co content in the electrode NCM is too large, the battery cycle rate performance is improved and the internal resistance is reduced, but the advantages of the battery's low-temperature power and low-temperature capacity retention rate will be deteriorated, and the cost will also increase.
[0141] Although the present application has been described with reference to preferred embodiments, various modifications may be made thereto and components may be substituted with equivalents without departing from the scope of the present application. In particular, the various technical features described in the various embodiments may be combined in any manner as long as there are no structural conflicts. The present application is not limited to the specific embodiments disclosed herein, but encompasses all technical solutions within the scope of the claims.
Claims
1. A cathode material, comprising a phosphate cathode material and a ternary cathode material, and the cathode material satisfies the following relational expression 1: Relational expression 1: 0.032 < w(Co) / (w(Ni) + w(Mn) + w(A)) ≤ 0.075 in, A is a metal doping element in the phosphate cathode material, w(Co) is the mass percentage of Co in the cathode material, w(Ni) is the mass percentage of Ni in the cathode material, w(Mn) is the mass percentage of Mn in the cathode material, and w(A) is the mass percentage of A in the cathode material.
2. The positive electrode material according to claim 1, wherein 1.55 < w(Co) < 3.25, optionally 1.8 < w(Co) < 2.9, further optionally 1.85 < w(Co) < 2.85; and / or 17.55 < w(Ni) < 29.55, optionally 19.2 < w(Ni) < 29.2, further optionally 19.9 < w(Ni) < 26.5; and / or 16.55 < w(Mn) < 21.55, optionally 18.2 < w(Mn) < 21.1, further optionally 18.4 < w(Mn) < 20.85; and / or 1.05 < w(A) < 6.55, optionally 2.2 < w(A) < 6.5, further optionally 2.50 < w(A) < 5.
0.
3. The positive electrode material according to claim 1 or 2, wherein w(Co) / (w(Ni) + w(Mn) + w(A)) is 0.035 to 0.065, optionally 0.045 to 0.
060.
4. The positive electrode material according to any one of claims 1 to 3, wherein The mass percentage content of Ni element in the ternary cathode material is 20% < w’(Ni) ≤ 55%, optionally 25% ≤ w’(Ni) ≤ 50%, or 30% ≤ w’(Ni) ≤ 45%, or 30% ≤ w’(Ni) ≤ 40%.
5. The positive electrode material according to any one of claims 1 to 4, wherein 0.062 < w'(Co) / w'(Ni) ≤ 0.410, optionally, w'(Co) / w'(Ni) is 0.062 to 0.158, further optionally w'(Co) / w'(Ni) is 0.083 to 0.
136.
6. The positive electrode material according to any one of claims 1 to 5, wherein 0.08 < w(A) / w(Ni) ≤ 0.41, optionally w(A) / w(Ni) is 0.10 to 0.30, further optionally 0.12 to 0.
28.
7. The positive electrode material according to any one of claims 1 to 6, wherein The phosphate-based cathode material has a chemical formula of Li 1+x Mn 1-y A y P 1-z E z O4, wherein x is any value in the range of -0.100-0.100, y is any value in the range of 0.001-0.500, z is any value in the range of 0.001-0.100, A includes one or more elements in the group consisting of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ga, Sn, Sb, Nb and Ge, and can be one or more elements in the group consisting of Fe, Ti, V and Mg, and E includes one or more elements in the group consisting of B, Si, N, S, F, Cl and Br, and optionally, E is an element selected from the group consisting of B, Si, N and S; 8. The positive electrode material according to any one of claims 1 to 6, wherein The chemical formula of the phosphate positive electrode material is Li a A1 x Mn 1-y A2 y P 1-z D z O 4-n G n , wherein the A1 includes one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Nb, Mo and W, the A2 includes one or more elements selected from the group consisting of Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge, the D includes one or more elements selected from the group consisting of B (boron), S, Si and N, the G includes one or more elements selected from the group consisting of S, F, Cl and Br, the a is selected from the range of 0.9 to 1.1, the x is selected from the range of 0.001 to 0.1, the y is selected from the range of 0.001 to 0.5, the z is selected from the range of 0.001 to 0.1, the n is selected from the range of 0.001 to 0.1, and the phosphate-based positive electrode material is electrically neutral.
9. The positive electrode material according to claim 7 or 8, wherein The phosphate cathode material further optionally has a core-shell structure, and the shell layer of the core-shell structure is a functional coating layer, and the functional coating layer is optionally one or more layers of pyrophosphate, phosphate, and carbon.
10. The positive electrode material according to any one of claims 1 to 9, wherein The ternary cathode material conforms to the chemical formula Li a Ni b Co c M1 d M2 e O f R g or Li with a coating layer on the surface a Ni b Co c M1 d M2 e O f A g , where 0.75 ≤ a ≤ 1.2, 0.38 < b < 0.85, 0.03 < c < 0.15, 0 < d < 1, 0 ≤ e ≤ 0.2, 1 ≤ f ≤ 2.5, 0 ≤ g ≤ 1, f + g ≤ 3, M1 includes one or both of Mn or Al, and optionally the molar ratio of Al to Mn is 0 to 1:4; M2 includes one or more of the group consisting of Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, Sr, Sb, Y, W, and Nb, and R includes one or more of the group consisting of N, F, S, and Cl.
11. A positive electrode sheet, comprising a current collector and a positive electrode film layer, wherein: The positive electrode film layer comprises the cathode material according to any one of claims 1 to 10.
12. A secondary battery, comprising a positive electrode sheet, a separator, an electrolyte and a negative electrode sheet, wherein: The positive electrode tab is the positive electrode tab according to claim 10 or 11.
13. An electrical device, comprising a secondary battery, wherein: The secondary battery comprises the secondary battery according to claim 12.
Citation Information
Patent Citations
Thermochemical blocking type composite positive electrode material, positive electrode plate and preparation method therefor, and lithium ion battery
CN107146875A
Lithium ion battery positive active substance, anode material, anode material sizing agent, anode piece, preparation method and lithium ion battery
CN107528050A
Lithium manganese ferric phosphate-ternary material composite positive electrode material and preparation method therefor
CN107546379A
Lithium ion battery positive electrode material, lithium ion battery positive pole plate and lithium ion battery
CN107565094A
Lithium ion battery positive electrode material, positive plate and lithium ion battery
CN111883771A
Cited By
Positive electrode sheet, battery comprising same, and electric device
WO2026143988A1