Secondary battery and electronic apparatus

By using a laminated adhesive member in a lithium-ion battery, the friction coefficient of the adhesive member is increased by using a styrene-isoprene-styrene block copolymer and acrylonitrile-butadiene-styrene copolymer resin in a lithium-ion battery. and peel strength solve the problem that adhesive paper is prone to damage during the drop, significantly improving the safety performance and service life of the battery.

WO2024197940A9PCT designated stage expired Publication Date: 2024-11-28NINGDE AMPEREX TECHNOLOGY LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/085782
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

The adhesive paper in existing lithium-ion batteries is easily damaged during the drop, resulting in damage to the bonding interface between the electrode assembly and the housing, affecting the safety performance of the battery.

Method used

The adhesive member adopting the first glue layer and the second glue layer of a laminated structure, wherein the first glue layer includes a styrene-isoprene-styrene block copolymer and acrylonitrile-butadiene-styrene copolymer The resin is regulated to increase the friction coefficient and peel strength of the adhesive member, reducing the risk of relative movement and bonding interface damage between the electrode assembly and the housing.

Benefits of technology

It effectively improves the safety performance of lithium-ion batteries, reduces the risk of top seal flushing and liquid leakage, and extends the battery's service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023085782_28112024_PF_FP_ABST
    Figure CN2023085782_28112024_PF_FP_ABST
Patent Text Reader

Abstract

Provided in the present application are a secondary battery and an electronic apparatus. The secondary battery comprises an electrode assembly, an electrolyte, a casing and a bonding member, the bonding member being arranged between the electrode assembly and the casing. The bonding member comprises a first adhesive layer and a second adhesive layer which are stacked, the first adhesive layer bonding with the inner surface of the casing, and the second adhesive layer bonding with the outer surface of the electrode assembly. The first adhesive layer comprises a styrene-isoprene-styrene block copolymer and a first resin, the first resin comprising at least one of an acrylonitrile-butadiene-styrene copolymer, polyurethane or polystyrene. The secondary battery provided by the present application comprises the bonding member, thus helping to reduce the possibility of tearing the outer surface of the electrode assembly and the risk of breaking through a top seal of the secondary battery and leaking the electrolyte, and improving the safety performance of the secondary battery.
Need to check novelty before this filing date? Find Prior Art

Description

Secondary battery and electronic device Technical Field

[0001] The present application relates to the field of electrochemistry, and in particular to a secondary battery and an electronic device. Background Art

[0002] In secondary batteries, such as lithium-ion batteries, there is a certain gap between the electrode assembly and the packaging shell, and the electrode assembly will move relative to the shell. Therefore, an adhesive (such as adhesive tape) is required to insulate and fix the lithium-ion battery.

[0003] Commonly used adhesive tapes, such as styrene-isoprene-styrene block copolymer (SIS) tapes, have the problem of poor restraint effect on electrode assemblies. When a lithium-ion battery falls, such as when it falls head-on, tail-off, or sideways, the edge of the adhesive tape is subjected to great stress, and the bonding interface between the SIS tape and the electrode assembly is easily damaged, resulting in lithium-ion battery voltage failure, short circuit, etc., affecting the safety performance of the lithium-ion battery.

[0004] Summary of the Invention

[0005] The purpose of this application is to provide a secondary battery and an electronic device to improve the safety performance of the secondary battery. The specific technical solution is as follows:

[0006] The first aspect of the present application provides a secondary battery, comprising an electrode assembly, an electrolyte, a shell, and an adhesive, wherein the adhesive is disposed between the electrode assembly and the shell, and comprises a first adhesive layer and a second adhesive layer stacked together, wherein the first adhesive layer is bonded to the inner surface of the shell, and the second adhesive layer is bonded to the outer surface of the electrode assembly; the first adhesive layer comprises a styrene-isoprene-styrene block copolymer and a first resin, wherein the first resin comprises at least one of acrylonitrile-butadiene-styrene copolymer, polyurethane, or polystyrene. In the secondary battery provided by the present application, the first adhesive layer comprises the above-mentioned substance, which can increase the friction coefficient between the first adhesive layer and the inner surface of the shell. On the one hand, this is beneficial to reducing the stress at the edge of the adhesive, reducing the possibility of damage to the bonding interface between the adhesive and the electrode assembly, thereby reducing the possibility of tearing of the outer surface of the electrode assembly; on the other hand, it is also beneficial to delay the relative movement between the electrode assembly and the shell, thereby reducing the risk of the secondary battery top seal being broken and leaking, thereby improving the safety performance of the secondary battery.

[0007] In some embodiments of the present application, based on the mass of the first adhesive layer, the mass percentage of the styrene-isoprene-styrene block copolymer is 32.5% to 75%, and the mass percentage of the first resin is 15% to 45%. By regulating the contents of the styrene-isoprene-styrene block copolymer and the first resin within the scope of the present application, the friction coefficient between the first adhesive layer and the inner surface of the housing can be increased. This, on the one hand, helps reduce stress at the edge of the adhesive and reduces the possibility of damage to the bonding interface between the adhesive and the electrode assembly, thereby reducing the possibility of tearing of the outer surface of the electrode assembly; on the other hand, it helps slow the relative movement between the electrode assembly and the housing, thereby reducing the risk of the secondary battery top seal being broken and leaking, thereby improving the safety performance of the secondary battery.

[0008] In some embodiments of the present application, based on the mass of the first adhesive layer, the mass percentage of the first resin is 20% to 40%. By adjusting the mass percentage of the first resin within the above range, the safety performance of the secondary battery can be further improved.

[0009] In some embodiments of the present application, based on the mass of the first adhesive layer, the mass percentage of the first resin is 25% to 35%. By adjusting the mass percentage of the first resin within the above range, the safety performance of the secondary battery can be further improved.

[0010] In some embodiments of the present application, the first adhesive layer further comprises a functional resin, with the weight percentage of the functional resin being 5% to 25% based on the weight of the first adhesive layer; the functional resin comprises at least one of ethylene-vinyl acetate copolymer, polyurethane elastomer, polyurethane acrylate, polyisobutylene, or polybutadiene. Controlling the weight percentage of the functional resin within the aforementioned range and selecting the aforementioned materials can improve the bonding stability of the first adhesive layer during long-term high-temperature immersion in electrolyte, thereby enhancing the safety performance of the secondary battery.

[0011] In some embodiments of the present application, the first adhesive layer further includes an additive and an antioxidant; based on the mass of the first adhesive layer, the weight percentage of the additive is 1% to 5%, and the weight percentage of the antioxidant is 1% to 5%. The inclusion of additives and antioxidants in the first adhesive layer, with their contents regulated within the aforementioned ranges, can enhance the heat resistance of the first adhesive layer and its antioxidant capacity in the electrolyte, thereby improving the bonding properties of the first adhesive layer and enhancing the safety of the secondary battery. In some embodiments of the present application, the adhesive further includes a substrate layer positioned between the first and second adhesive layers; the substrate layer comprises at least one of polyethylene terephthalate, polyimide, or polypropylene. The inclusion of a substrate layer in the adhesive and the selection of the aforementioned materials can increase the friction between the adhesive and the housing, thereby enhancing the safety of the secondary battery.

[0012] In some embodiments of the present application, the area of ​​the first adhesive layer is S1, the orthographic projection area of ​​the electrode assembly along the stacking direction of the electrode assembly, the adhesive and the shell is S2, and S1 / S2 satisfies 10%≤S1 / S2≤95%. By regulating the value of S1 / S2 within the above range, it is beneficial to improve the safety performance of the secondary battery.

[0013] In some embodiments of the present application, the shell is a packaging bag. When the adhesive of the present application is applied to a secondary battery whose shell is a packaging bag, the secondary battery has high energy density and good safety performance.

[0014] In some embodiments of the present application, the thickness of the first adhesive layer is 2 μm to 20 μm. By adjusting the thickness of the first adhesive layer within the above range, the loss of energy density of the secondary battery can be reduced while improving the safety performance of the secondary battery.

[0015] In some embodiments of the present application, the peel strength between the adhesive and the housing is between 10 N / m and 500 N / m. By regulating the peel strength between the adhesive and the housing within this range, the likelihood of damage to the bonding interface between the adhesive and the electrode assembly can be reduced, thereby improving the safety performance of the secondary battery.

[0016] In some embodiments of the present application, the secondary battery has a liquid retention coefficient of 1 g / Ah to 2.5 g / Ah. A liquid retention coefficient within this range facilitates swelling of the first resin in the first adhesive layer in the electrolyte, further increasing the friction coefficient between the first adhesive layer and the inner surface of the housing, and improving issues such as bumps and swelling in the secondary battery, thereby enhancing the safety performance of the secondary battery.

[0017] The second aspect of the present application provides an electronic device, which includes the secondary battery provided by the first aspect of the present application. The secondary battery of the present application has good safety performance, so that the electronic device provided by the second aspect of the present application has a long service life.

[0018] The present application provides a secondary battery and an electronic device, wherein the secondary battery includes an electrode assembly, an electrolyte, a housing, and an adhesive. The adhesive is disposed between the electrode assembly and the housing and includes a first adhesive layer and a second adhesive layer laminated together. The first adhesive layer adheres to the inner surface of the housing, and the second adhesive layer adheres to the outer surface of the electrode assembly. The first adhesive layer includes a styrene-isoprene-styrene block copolymer and a first resin. The first resin includes at least one of an acrylonitrile-butadiene-styrene copolymer, polyurethane, or polystyrene. The first resin in the first adhesive layer has a highly flexible molecular chain and low cohesive force, enabling the first adhesive layer to quickly exert adhesive properties at low temperatures and exhibit good flexibility and stable bonding properties at high temperatures. In the secondary battery provided in the present application, the first resin in the first adhesive layer swells in the electrolyte, which can increase the friction coefficient between the first adhesive layer and the inner surface of the shell. On the one hand, it is beneficial to reduce the stress at the edge of the adhesive and reduce the possibility of damage to the bonding interface between the adhesive and the electrode assembly, thereby reducing the possibility of tearing the outer surface of the electrode assembly; on the other hand, it is also beneficial to delay the relative movement between the electrode assembly and the shell, thereby reducing the risk of the secondary battery top seal being broken and leaking, thereby improving the safety performance of the secondary battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The drawings described herein are used to provide further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute improper limitations on the present application.

[0020] FIG1 is a schematic diagram of a stacked structure of an adhesive member in one embodiment of the present application;

[0021] FIG2 is a schematic diagram showing the positions of the molecules of the first resin before and after swelling in the electrolyte;

[0022] FIG3 is a schematic diagram of a stacked structure of an adhesive member in another embodiment of the present application;

[0023] FIG4 is a schematic diagram of an adhesive member bonded to the outer surface of an electrode assembly in one embodiment of the present application.

[0024] Reference numerals: adhesive member 10 , first adhesive layer 11 , second adhesive layer 12 , substrate layer 13 , electrode assembly 20 , first resin 30 before swelling, first resin 31 after swelling. DETAILED DESCRIPTION

[0025] To make the objectives, technical solutions, and advantages of this application more clearly understood, the present application is further described below with reference to the accompanying drawings and examples. It is apparent that the described examples are only a portion of the embodiments of this application, and not all of them. All other embodiments derived by persons of ordinary skill in the art based on the examples in this application are intended to fall within the scope of protection of this application.

[0026] It should be noted that, in the specific embodiments of the present application, lithium-ion batteries are used as an example of secondary batteries to explain the present application, but the secondary batteries of the present application are not limited to lithium-ion batteries.

[0027] In a first aspect, the present application provides a secondary battery comprising an electrode assembly, an electrolyte, a housing, and an adhesive. The adhesive is disposed between the electrode assembly and the housing. As shown in FIG1 , the adhesive 10 comprises a first adhesive layer 11 and a second adhesive layer 12 stacked together. The first adhesive layer 11 is bonded to the inner surface of the housing, and the second adhesive layer 12 is bonded to the outer surface of the electrode assembly. The first adhesive layer 11 comprises a styrene-isoprene-styrene block copolymer and a first resin. The first resin comprises at least one of an acrylonitrile-butadiene-styrene copolymer, a polyurethane, or a polystyrene. The first adhesive layer comprises the first resin, and the molecular chain of the first resin has good flexibility and low cohesion, so that the first adhesive layer quickly exerts viscosity at low temperatures, has good flexibility at high temperatures, and has stable bonding properties. In the secondary battery provided by the present application, the first adhesive layer includes the above-mentioned substances and its content is regulated within the scope of the present application. The first resin in the first adhesive layer swells in the electrolyte. As shown in FIG2 , the positions between the molecules of the first resin 30 before swelling are relatively fixed. After swelling in the electrolyte, the relatively fixed positions between the molecules of the first resin 31 after swelling are amplified by the small molecules of the electrolyte. The swelling of the first resin can increase the friction force, thereby increasing the friction coefficient between the first adhesive layer and the inner surface of the shell. In the secondary battery provided by the present application, the first adhesive layer includes the first resin, which can take into account the friction coefficient between the first adhesive layer and the inner surface of the shell and the peel strength between the adhesive and the shell. On the one hand, it is beneficial to reduce the stress on the edge of the adhesive, reduce the possibility of damage to the bonding interface between the adhesive and the electrode assembly, and reduce the possibility of tearing the outer surface of the electrode assembly; on the other hand, it is also beneficial to delay the relative movement between the electrode assembly and the shell, reduce the risk of the secondary battery top seal being broken and leaking, and thus improve the safety performance of the secondary battery.

[0028] In some embodiments of the present application, based on the mass of the first adhesive layer, the mass percentage of the styrene-isoprene-styrene block copolymer is 32.5% to 75%, and the mass percentage of the first resin is 15% to 45%. Preferably, the mass percentage of the first resin is 20% to 40%, and further preferably, the mass percentage of the first resin is 25% to 35%. For example, the mass percentage of the styrene-isoprene-styrene block copolymer can be 32.5%, 35%, 45%, 50%, 55%, 65%, 75% or a range consisting of any two of these values, and the mass percentage of the first resin can be 15%, 20%, 25%, 27%, 30%, 33%, 35%, 40%, 45% or a range consisting of any two of these values. By regulating the content of the styrene-isoprene-styrene block copolymer and the first resin within the scope of this application, the friction coefficient between the first adhesive layer and the inner surface of the shell can be increased, which is beneficial to reducing the stress at the edge of the adhesive and the possibility of damage to the bonding interface between the adhesive and the electrode assembly, thereby reducing the possibility of tearing the outer surface of the electrode assembly; on the other hand, it is also beneficial to delay the relative movement between the electrode assembly and the shell, thereby reducing the risk of the secondary battery top seal being broken and leaking, thereby improving the safety performance of the secondary battery. When the first resin includes two or more of acrylonitrile-butadiene-styrene copolymer, polyurethane or polystyrene, there is no particular limitation on the content of each substance as long as the purpose of the present application can be achieved.

[0029] In the present application, the monomers of the acrylonitrile-butadiene-styrene copolymer include acrylonitrile, butadiene, and styrene. Based on the mass of the acrylonitrile-butadiene-styrene copolymer, the mass percentage of acrylonitrile is 5% to 35%, the mass percentage of butadiene is 20% to 55%, and the mass percentage of styrene is 10% to 45%. By regulating the mass percentages of the monomers acrylonitrile, butadiene, and styrene of the acrylonitrile-butadiene-styrene copolymer within the above ranges, it is beneficial to improve the comprehensive properties of the first resin, for example, the first resin has good chemical resistance and thermal stability, high elasticity and good toughness, high hardness, and good processability, wherein acrylonitrile provides chemical resistance and thermal stability, butadiene provides high elasticity and toughness, and styrene provides hardness and processability, thereby improving the bonding performance of the first adhesive layer, improving the problem of swelling of the electrode assembly surface and its four corners, increasing the friction coefficient between the first adhesive layer and the inner surface of the shell, reducing the possibility of tearing of the outer surface of the electrode assembly and the risk of the secondary battery top seal being broken and leaking, and improving the safety of the secondary battery.

[0030] In this application, the coefficient of friction between the first adhesive layer and the inner surface of the housing is 0.3 to 0.9. This indicates that the high coefficient of friction between the first adhesive layer and the inner surface of the housing helps reduce stress at the edge of the adhesive, reducing the likelihood of damage to the bonding interface between the adhesive and the electrode assembly, thereby reducing the likelihood of tearing on the outer surface of the electrode assembly. Furthermore, it helps slow the relative movement between the electrode assembly and the housing, thereby reducing the risk of the secondary battery top seal breaking and leaking, thereby improving the safety performance of the secondary battery.

[0031] In some embodiments of the present application, the first adhesive layer further comprises a functional resin. Based on the mass of the first adhesive layer, the weight percentage of the functional resin is between 5% and 25%. For example, the weight percentage of the functional resin can be 5%, 10%, 12%, 15%, 18%, 20%, 25%, or a range consisting of any two of these values. The functional resin comprises at least one of ethylene-vinyl acetate copolymer, polyurethane elastomer, polyurethane acrylate, polyisobutylene, or polybutadiene. Regulating the weight percentage of the functional resin within the above range and selecting the above materials can improve the morphological stability of the first adhesive layer during long-term high-temperature immersion in electrolyte, improve the bonding properties of the first adhesive layer, and thereby improve the safety performance of the secondary battery. In the present application, the above-mentioned high temperature refers to 80°C to 90°C.

[0032] In some embodiments of the present application, the first subbing layer further includes additives and antioxidants. Based on the mass of the first subbing layer, the additives may comprise 1% to 5% by weight, and the antioxidants may comprise 1% to 5% by weight. The additives may comprise 1%, 2%, 3%, 4%, 5%, or a range consisting of any two of these values. The antioxidants may comprise 1%, 2%, 3%, 4%, 5%, or a range consisting of any two of these values. The present application does not specifically limit the types of additives and oxidants, as long as they achieve the objectives of the present application. The additives may include, but are not limited to, at least one of titanium dioxide, talc, white carbon black, or calcium carbonate; the antioxidants may include, but are not limited to, at least one of diphenylamine, triester phosphite, or distearyl thiodipropionate. Including additives and antioxidants in the first subbing layer and regulating their contents within the aforementioned ranges can improve the heat resistance of the first subbing layer and its antioxidant capacity in the electrolyte, thereby improving the bonding properties of the first subbing layer, enhancing the stability of the first subbing layer, and enhancing the safety of the secondary battery.

[0033] In some embodiments of the present application, as shown in Figure 3, the adhesive member 10 further includes a substrate layer 13 positioned between the first adhesive layer 11 and the second adhesive layer 12. The substrate layer comprises at least one of polyethylene terephthalate, polyimide, or polypropylene. The present application does not specifically limit the content of the aforementioned substances in the substrate layer; those skilled in the art may adjust the content based on practical needs, as long as the objectives of the present application are achieved. The present application does not specifically limit the weight-average molecular weight of the aforementioned substances in the substrate layer; those skilled in the art may select the content based on practical needs, as long as the objectives of the present application are achieved. For example, the weight-average molecular weight may be between 10,000 and 500,000. When the substrate layer contains multiple substances, the content of each substance is not specifically limited, as long as the objectives of the present application are achieved. The adhesive member includes a substrate layer and is selected from the aforementioned materials to impart a certain degree of hardness to the adhesive member, thereby reducing wrinkling and air bubble issues during bonding and broadening the adhesive member's processing window, allowing for both surface pressing and roller pressing. This effectively prevents foreign matter such as burrs and debris, protects the electrode assembly, and thus improves the safety performance of the secondary battery.

[0034] The substrate layer of the present application may also include colorants such as cobalt green, cobalt blue, Prussian blue, indigo, and phthalocyanine blue to impart color to the substrate for easy identification by an inductively coupled device (CCD) or an active pixel sensor (CMOS) during the production process, for purposes such as adhesive positioning, adhesive application, and missed detection. The present application does not particularly limit the content of the colorant in the substrate layer, and those skilled in the art may adjust the content according to actual needs, as long as the objectives of the present application are achieved.

[0035] In some embodiments of the present application, as shown in FIG4 , the adhesive 10 is bonded to the outer surface of the electrode assembly 20, the area of ​​the first adhesive layer 11 is S1, the orthographic projection area of ​​the electrode assembly 20 along the stacking direction of the electrode assembly 20, the adhesive 10, and the shell is S2, and S1 / S2 satisfies 10%≤S1 / S2≤95%. For example, the value of S1 / S2 can be 10%, 15%, 25%, 35%, 40%, 45%, 55%, 65%, 75%, 85%, 95%, or a range consisting of any two of these values. By regulating the value of S1 / S2 within the above range, a higher peel strength can be achieved between the adhesive and the shell, and the packaging will not be affected by the adhesive being too large, which is beneficial to improving the safety performance and processing performance of the secondary battery.

[0036] In some embodiments of the present application, the housing is a packaging bag, for example, an aluminum-plastic film packaging bag. When the adhesive member of the present application is applied to a secondary battery whose housing is a packaging bag, the secondary battery has high energy density and good safety performance.

[0037] In some embodiments of the present application, the thickness of the first adhesive layer is 2 μm to 20 μm. For example, the thickness of the first adhesive layer can be 2 μm, 4 μm, 7 μm, 10 μm, 14 μm, 18 μm, 20 μm, or a range consisting of any two of these values. By regulating the thickness of the first adhesive layer within the above range, the loss of energy density of the secondary battery can be reduced while improving the safety performance of the secondary battery.

[0038] The present application has no particular limitation on the thickness of the second adhesive layer and the thickness of the substrate layer, as long as the purpose of the present application can be achieved. For example, the thickness of the second adhesive layer is 2 μm to 10 μm, and the thickness of the substrate layer is 4 μm to 30 μm.

[0039] In some embodiments of the present application, the peel strength between the adhesive and the shell is 10 N / m to 500 N / m. For example, the peel strength between the adhesive and the shell can be 10 N / m, 30 N / m, 50 N / m, 70 N / m, 100 N / m, 150 N / m, 200 N / m, 250 N / m, 300 N / m, 400 N / m, 500 N / m, or a range consisting of any two of these values. By regulating the peel strength between the adhesive and the shell to be within the above range, the problem of tearing of the electrode surface at the edge of the adhesive can be improved, thereby improving the safety performance of the secondary battery.

[0040] In some embodiments of the present application, the secondary battery has a liquid retention coefficient of 1 g / Ah to 2.5 g / Ah. For example, the liquid retention coefficient of the secondary battery can be 1 g / Ah, 1.2 g / Ah, 1.5 g / Ah, 1.7 g / Ah, 2 g / Ah, 2.3 g / Ah, 2.5 g / Ah, or a range consisting of any two of these values. A liquid retention coefficient of the secondary battery within the above range is conducive to the first resin in the first adhesive layer swelling in the electrolyte, which helps to further increase the friction coefficient between the first adhesive layer and the inner surface of the housing, improve the problems of bulges and liquid swelling in the secondary battery, and thus improve the safety performance of the secondary battery.

[0041] The present application does not particularly limit the method for preparing the adhesive component, as long as the purpose of the present application can be achieved. For example, the present application can be prepared using the following method: styrene-isoprene-styrene block copolymer, a first resin, a functional resin, additives, and an antioxidant are uniformly mixed, heat-melted at 100°C to 150°C, and then coated on one surface of a substrate layer, and dried to form a first adhesive layer; the material for a second adhesive layer is coated on the other surface of the substrate layer, and dried to form a second adhesive layer, thereby obtaining the adhesive component.

[0042] The weight average molecular weight of the styrene-isoprene-styrene block copolymer, the first resin, and the functional resin is not particularly limited in this application, and those skilled in the art can make selections according to actual needs, as long as the purpose of this application can be achieved. For example, the weight average molecular weight of the styrene-isoprene-styrene block copolymer can be 50,000 to 150,000, the weight average molecular weight of the first resin can be 10,000 to 500,000, and the weight average molecular weight of the functional resin can be 100,000 to 300,000. The material of the second adhesive layer is not particularly limited in this application, as long as the purpose of this application can be achieved. For example, the material of the second adhesive layer can include at least one of polymethyl methacrylate (PMMA, commonly known as acrylic), polypropylene (PP), polyethylene (PE), or polyamide.

[0043] The secondary battery of the present application includes an electrode assembly, an electrolyte, a shell and an adhesive, and the electrode assembly and the electrolyte are contained in the shell. The present application has no particular restrictions on the structure of the electrode assembly, as long as the purpose of the present application can be achieved. For example, the structure of the electrode assembly is a laminated structure or a wound structure. The electrode assembly includes a positive electrode sheet, a negative electrode sheet and a diaphragm, and the diaphragm is arranged between the positive electrode sheet and the negative electrode sheet. The diaphragm is used to separate the positive electrode sheet and the negative electrode sheet to prevent internal short circuits in the secondary battery. It allows electrolyte ions to pass freely without affecting the electrochemical charge and discharge process.

[0044] The present application has no particular restrictions on the positive electrode sheet, as long as the purpose of the present application can be achieved. For example, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer provided on at least one surface of the positive electrode current collector. The present application has no particular restrictions on the positive electrode current collector, as long as the purpose of the present application can be achieved. For example, the positive electrode current collector may include aluminum foil or aluminum alloy foil, etc. The positive electrode active material layer of the present application includes positive electrode active material. The present application has no particular restrictions on the type of positive electrode active material, as long as the purpose of the present application can be achieved. For example, the positive electrode active material may include lithium nickel cobalt manganese oxide (NCM811, NCM622, NCM523, NCM111), lithium nickel cobalt aluminum oxide, lithium iron phosphate, lithium-rich manganese-based material, lithium cobalt oxide (LiCoO2), lithium manganese oxide, lithium iron manganese phosphate or lithium titanate, etc. In the present application, there is no particular restriction on the thickness of the positive electrode current collector and the positive electrode active material layer, as long as the purpose of the present application can be achieved. For example, the thickness of the positive electrode current collector is 4μm to 20μm, preferably 4μm to 18μm. The thickness of the single-sided positive electrode active material layer is 30μm to 120μm. In the present application, the positive electrode active material layer can be arranged on one surface in the thickness direction of the positive electrode current collector, or on two surfaces in the thickness direction of the positive electrode current collector. It should be noted that the "surface" here can be the entire area of ​​the positive electrode current collector or a partial area of ​​the positive electrode current collector. This application is not particularly limited as long as the purpose of this application can be achieved. The positive electrode active material layer of the present application may also include a conductive agent and a binder. The above-mentioned conductive agent and binder are not particularly limited as long as the purpose of this application can be achieved. For example, the conductive agent may include at least one of conductive carbon black (Super P), carbon nanotubes (CNTs), carbon nanofibers, flake graphite, carbon dots or graphene. The binder may include at least one of polypropylene alcohol, sodium polyacrylate, potassium polyacrylate, lithium polyacrylate, polyimide, polyamide-imide, styrene-butadiene rubber (SBR), polyvinyl alcohol (PVA), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl butyral (PVB), water-based acrylic resin, lithium carboxymethyl cellulose (CMC-Li) or sodium carboxymethyl cellulose (CMC-Na), etc.

[0045] This application places no particular restrictions on the negative electrode sheet, as long as the objectives of this application can be achieved. For example, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer provided on at least one surface of the negative electrode current collector. This application places no particular restrictions on the negative electrode current collector, as long as the objectives of this application can be achieved. For example, the negative electrode current collector can include copper foil, copper alloy foil, nickel foil, stainless steel foil, titanium foil, nickel foam or copper foam, etc. The negative electrode active material layer of this application contains a negative electrode active material. This application places no particular restrictions on the type of the negative electrode active material, as long as the objectives of this application can be achieved. For example, the negative electrode active material can include natural graphite, artificial graphite, mesocarbon microbeads (MCMB), hard carbon, soft carbon, silicon, silicon-carbon composite, SiO x (0 < x ≤ 2), Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO2, lithium titanate Li4Ti5O with a spinel structure 12 , Li-Al alloy or at least one of metallic lithium. In this application, there are no particular restrictions on the thickness of the negative electrode current collector and the negative electrode active material layer, as long as the objectives of this application can be achieved. For example, the thickness of the negative electrode current collector is 4 μm to 10 μm, and the thickness of the negative electrode active material layer is 30 μm to 130 μm. In this application, the negative electrode active material layer can be provided on one surface in the thickness direction of the negative electrode current collector, or can be provided on both surfaces in the thickness direction of the negative electrode current collector. It should be noted that the "surface" here can be the entire area of the negative electrode current collector or a partial area of the negative electrode current collector. This application places no particular restrictions, as long as the objectives of this application can be achieved. Optionally, the negative electrode active material layer can further include a conductive agent and a binder. This application places no particular restrictions on the types of the conductive agent and the binder in the negative electrode active material layer, as long as the objectives of this application can be achieved. For example, the negative electrode active material layer of this application can include the above-mentioned conductive agent and binder. This application places no particular restrictions on the mass ratio of the negative electrode active material, the conductive agent and the binder in the negative electrode active material layer, as long as the objectives of this application can be achieved.

[0046] The present application has no particular restrictions on the diaphragm, as long as the purpose of the present application can be achieved. For example, the material of the diaphragm may include but is not limited to polyethylene (PE), polypropylene (PP), polytetrafluoroethylene-based polyolefin (PO) diaphragms, polyester films (such as polyethylene terephthalate (PET) films), cellulose films, polyimide films (PI), polyamide films (PA), spandex or aramid films, etc. The type of diaphragm may include but is not limited to at least one of woven membranes, non-woven membranes (non-woven fabrics), microporous membranes, composite membranes, rolled membranes or spun membranes, etc. The diaphragm of the present application may have a porous structure, and the porous layer is provided on at least one surface of the diaphragm, and the porous layer includes inorganic particles and a binder. The inorganic particles may include at least one of aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide or barium sulfate. The binder may include at least one of polyvinylidene fluoride, a copolymer of vinylidene fluoride and hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylate, sodium carboxymethyl cellulose, polyvinyl pyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene or polyhexafluoropropylene. The present application does not particularly limit the size of the pore size of the porous structure, as long as the purpose of the present application can be achieved. For example, the pore size can be 0.01 μm to 1 μm. In the present application, the thickness of the diaphragm is not particularly limited, as long as the purpose of the present application can be achieved. For example, the thickness can be 5 μm to 500 μm.

[0047] In the present application, the electrolyte includes a lithium salt and a non-aqueous solvent. The lithium salt may include at least one of LiPF6, LiBF4, LiClO4, LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiN(SO2CF3)2, LiC(SO2CF3)3, Li2SiF6, lithium bis(oxalatoborate) (LiBOB) or lithium difluoroborate. The present application has no particular restrictions on the concentration of the lithium salt in the electrolyte, as long as the purpose of the present application can be achieved. The present application has no particular restrictions on the non-aqueous solvent, as long as the purpose of the present application can be achieved, for example, it may include but is not limited to at least one of a carbonate compound, a carboxylate compound, an ether compound or other organic solvents. The above-mentioned carbonate compound may include but is not limited to at least one of a chain carbonate compound, a cyclic carbonate compound or a fluorinated carbonate compound. The above-mentioned linear carbonate compound may include but is not limited to at least one of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methylpropyl carbonate (MPC), ethylpropyl carbonate (EPC) or methyl ethyl carbonate (MEC). The above-mentioned cyclic carbonate may include but is not limited to at least one of ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC) or vinyl ethylene carbonate (VEC). The fluorinated carbonate compound may include but is not limited to at least one of fluoroethylene carbonate (FEC), 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate or trifluoromethylethylene carbonate. The carboxylate compound may include but is not limited to at least one of methyl formate, methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decanoic acid, valerolactone or caprolactone. The ether compound may include but is not limited to at least one of dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, 1-ethoxy-1-methoxyethane, 2-methyltetrahydrofuran or tetrahydrofuran. The other organic solvents may include but are not limited to at least one of dimethyl sulfoxide, 1,2-dioxolane, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate or trioctyl phosphate.

[0048] This application does not specifically limit the type of secondary battery; it may include any device that undergoes an electrochemical reaction. For example, secondary batteries may include, but are not limited to, lithium metal secondary batteries, lithium ion batteries, sodium ion batteries, lithium polymer secondary batteries, and lithium ion polymer secondary batteries. This application does not specifically limit the shape of the secondary battery, as long as it can achieve the purpose of this application.

[0049] The preparation process of a secondary battery is well known to those skilled in the art and is not particularly limited in this application. For example, it may include but is not limited to the following steps: stacking the positive electrode sheet, the separator, and the negative electrode sheet in order, and performing operations such as winding and folding as needed to obtain an electrode assembly with a wound structure, placing the electrode assembly in a packaging bag, injecting an electrolyte into the packaging bag and sealing it to obtain a secondary battery; or stacking the positive electrode sheet, the separator, and the negative electrode sheet in order, and then fixing the four corners of the entire stacked structure with tape to obtain an electrode assembly with a stacked structure, placing the electrode assembly in a packaging bag, injecting an electrolyte into the packaging bag and sealing it to obtain a secondary battery. In addition, as needed, overcurrent protection elements, guide plates, etc. may be placed in the packaging bag to prevent pressure rise and overcharge and discharge inside the secondary battery.

[0050] The second aspect of the present application provides an electronic device, which includes the secondary battery provided by the first aspect of the present application. The secondary battery of the present application has good safety performance, so that the electronic device provided by the second aspect of the present application has a long service life.

[0051] The electronic device of the present application is not particularly limited and can be any electronic device known in the art. For example, the electronic device can include, but is not limited to, a laptop computer, a pen-type computer, a mobile computer, an electronic book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a headset, a video recorder, an LCD television, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, an automobile, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, a power tool, a flashlight, a camera, a large household battery, and a lithium-ion capacitor.

[0052] Example

[0053] The following examples and comparative examples are provided to more specifically illustrate the embodiments of the present invention. Various tests and evaluations were performed according to the following methods. In addition, unless otherwise specified, "parts" and "%" are based on mass.

[0054] Test methods and equipment:

[0055] First adhesive layer composition test:

[0056] The lithium-ion battery was disassembled, the first glue layer was removed, and then the components and proportions of the components in the first glue layer were tested by Fourier transform infrared spectroscopy (FTIR) and pyrolysis-gas chromatography-mass spectrometry (PY-GCMS) mass spectrometry (GCMS).

[0057] Peel strength test:

[0058] The peel strength between the adhesive and the housing (packaging bag) was tested using a high-speed rail tensile testing machine according to GB / T 2792-2014, "Test Method for Peel Strength of Adhesive Tapes." The test procedure is as follows: The lithium-ion battery is discharged to 0V, then disassembled. The adhesive, along with the electrode assembly and packaging bag attached to it, is removed as a whole. The electrolyte on the surface is wiped clean with dust-free paper. The specimen is then cut into 20mm x 60mm strips. Along the length of the specimen, the electrode assembly side of the specimen is adhered to a steel plate using double-sided tape (Nitto 5000NS), with the adhesion length being at least 40mm. Fix the steel plate at the corresponding position of the high-speed rail tensile testing machine, pull up the other end of the packaging bag that is not adhered to the adhesive, and place the sample in the chuck and clamp it. The angle between the pulled-up sample part and the steel plate in space is 180°. The chuck pulls the sample at a speed of 5±0.2mm / s. The average tensile force in the stable area is finally measured and recorded as the peel strength between the adhesive and the shell, recorded as F, in units of N / m.

[0059] Peel strength-temperature change test:

[0060] Lithium-ion batteries were prepared according to the method of Example 1-1, and the formation temperatures of the lithium-ion batteries were set to 65°C, 75°C, 80°C, 85°C, and 90°C, respectively, which were recorded as five samples. Samples were then prepared according to the above-mentioned peel strength test method, and the peel strength between the adhesive and the shell of the above-mentioned five samples was measured according to the above-mentioned peel strength test method, and the unit is N / m.

[0061] Static friction coefficient test:

[0062] According to GB / T 10006-2021 "Plastic Film and Sheeting - Determination of the Coefficient of Friction", the friction coefficient of the first adhesive layer and the inner surface of the shell was tested using an MXD-02 friction coefficient tester. The test process is as follows: Place the test plate on a horizontal operating table, adhere the adhesive to the aluminum foil through the second adhesive layer, cut into 50mm×50mm specimens, and soak the above specimens in an electrolyte at 85°C for 4 hours. After soaking, wipe the electrolyte on the surface with dust-free paper. At room temperature, use double-sided tape (Nitto 5000NS) to fix the above specimen to the test plate and record it as the first specimen. Cut the packaging bag into 100mm×100mm as the second specimen and fix it on a slider with a weight of 65g. Place the two specimen test surfaces horizontally relative to each other, apply uniform contact pressure, and move the surfaces of the two specimens relative to each other. Record the force required for initial sliding (static friction). The static friction force divided by the weight of the slider is the static friction coefficient, which is also the friction coefficient x between the first adhesive layer and the inner surface of the shell. The preparation method of the above electrolyte is the same as that of the electrolyte in Example 1-1.

[0063] Roller test:

[0064] The lithium-ion battery is allowed to rest at room temperature for 60 minutes before the voltage test. The voltage of the lithium-ion battery is measured before the roller test. The lithium-ion battery is placed in a fixture and tested using a roller device in a test environment of 20±5°C. The lithium-ion battery is placed 1m above the ground and is allowed to freely drop 250 times at a speed of 12 cycles / min (two drops constitute one cycle). At the end of the test, the voltage of the lithium-ion battery is measured and recorded. The lithium-ion battery is inspected and photographed before and after the test. The roller test passing criteria include no smoke, no leakage, and a voltage drop of <50mV.

[0065] Drop test:

[0066] The lithium-ion battery was preconditioned at 25°C and allowed to stand at room temperature for 60 minutes. The voltage of the lithium-ion battery was then measured before the drop test. The lithium-ion battery was then placed in a fixture and dropped from 1.5m above the ground in the following sequence: head-to-tail-head right corner-tail right corner-head left corner-tail left corner (angle: 45±15°), repeated six times. After the drop, the lithium-ion battery voltage was measured and recorded. The appearance of the lithium-ion battery was inspected and photographed before and after the test. Drop test passing criteria: no smoke, no leakage, and a voltage drop of <30mV.

[0067] Liquid retention coefficient test:

[0068] At 25°C, charge the lithium-ion battery to 4.5V at 0.5C, then charge it to 0.05C at a constant voltage, let it stand for 5 minutes, and then discharge it to 3V at 0.1C. Record the discharge capacity C. pDisassemble the lithium-ion battery and centrifuge it in a high-speed centrifuge to obtain the free electrolyte. Weigh it and record the mass of the electrolyte m. The electrolyte retention coefficient of the lithium-ion battery is y = m / C. p , unit is g / Ah.

[0069] Swelling performance test:

[0070] The adhesives used in the examples and comparative examples were cut into 50 mm x 50 mm sections, with a test mass of ag. After immersion in an 85°C electrolyte for 7 days, the adhesives were observed for morphology and tested for mass bg. The swelling ratio = (ba) / b x 100%. The swelling ratio was used to determine the adhesive's performance. An adhesive with a swelling ratio between 5% and 30% was considered to have good swelling performance.

[0071] The preparation method of the above electrolyte is the same as that of the electrolyte in Example 1-1.

[0072] Example 1-1

[0073] <Preparation of positive electrode sheet>

[0074] The positive electrode active material LiCoO2, the conductive agent conductive carbon black, and the binder polyvinylidene fluoride (PVDF) are mixed in a weight ratio of 97.5:1:1.5, and N-methylpyrrolidone (NMP) is added as a solvent to prepare a slurry with a solid content of 75wt%, and stirred evenly. The slurry is evenly coated on one surface of a positive electrode current collector aluminum foil with a thickness of 9μm and dried at 90°C to obtain a positive electrode sheet with a coating thickness of 110μm. After completing the above steps, the single-sided coating of the positive electrode sheet is completed. Thereafter, the above steps are repeated on the other surface of the positive electrode sheet to obtain a positive electrode sheet coated with the positive electrode active material on both sides. After coating, after cold pressing, cutting, slitting, and drying under vacuum conditions at 85°C for 4h, a positive electrode sheet with a specification of 35mm×867mm is obtained.

[0075] <Preparation of negative electrode sheet>

[0076] Graphite powder (negative electrode active material), conductive carbon black (Super P), and styrene-butadiene rubber (SBR) (binder) were mixed in a weight ratio of 96:1.5:2.5. Deionized water was then added as a solvent to form a slurry with a solids content of 70 wt%, which was then stirred evenly. The slurry was evenly coated on one surface of a 5 μm thick copper foil for the negative electrode current collector and dried at 110°C to produce a negative electrode sheet with a single-sided coating of negative electrode active material and a coating thickness of 130 μm. After completing these steps, the negative electrode sheet was coated on one side. The above steps were then repeated on the other side of the negative electrode sheet to produce a negative electrode sheet coated on both sides with negative electrode active material. After coating, the sheet was cold pressed, cut, and slit, and then dried under vacuum at 120°C for 12 hours to produce a negative electrode sheet measuring 37.5 mm x 875 mm.

[0077] <Preparation of Separator>

[0078] PVDF and alumina ceramics were mixed in a mass ratio of 9:1, deionized water was added as a solvent, and a slurry with a solid content of 25 wt% was prepared. The mixture was stirred evenly and the slurry was evenly coated on one surface of a 5 μm thick polyethylene porous polymer film (provided by Celgard). After drying, the slurry was evenly coated on the other surface of the polyethylene porous polymer film to obtain a diaphragm coated with a 2 μm alumina ceramic layer on both sides.

[0079] <Preparation of Electrolyte>

[0080] In a dry argon atmosphere, organic solvents ethylene carbonate, ethyl methyl carbonate and diethyl carbonate were mixed in a mass ratio of 30:50:20 to obtain an organic solution, and then lithium salt LiPF6 was added to the organic solvent, dissolved and mixed evenly to obtain an electrolyte with a lithium salt concentration of 1.15 mol / L.

[0081] <Preparation of Adhesive>

[0082] Styrene-isoprene-styrene block copolymer (SIS, weight-average molecular weight 100,000), first resin acrylonitrile-butadiene-styrene copolymer (ABS, weight-average molecular weight 300,000), functional resin ethylene-vinyl acetate copolymer (EVA, weight-average molecular weight 120,000), additive titanium dioxide, and antioxidant diphenylamine are mixed evenly, heated to 150°C for hot melting, and then coated on one surface of a substrate layer polyethylene terephthalate film (PET) with a thickness of 8 μm, and then dried at 120°C to form a first adhesive layer with a thickness of 8 μm. Polyacrylic acid (PAA) is coated on the other surface of the substrate layer and dried at 80°C to form a second adhesive layer with a thickness of 4 μm, thereby obtaining an adhesive component comprising a first adhesive layer, a substrate layer, and a second adhesive layer stacked in sequence. Based on the mass of the first adhesive layer, the weight percentage of SIS is 45%, the weight percentage of the first resin ABS is 30%, the weight percentage of the functional resin EVA is 15%, the weight percentage of the additive titanium dioxide is 5%, and the weight percentage of the antioxidant diphenylamine is 5%. The weight ratio of the three monomers forming ABS is 20:35:45 for acrylonitrile:butadiene:styrene.

[0083] <Preparation of lithium-ion batteries>

[0084] The positive electrode sheet, separator and negative electrode sheet prepared above are stacked in order, the separator is placed between the positive electrode sheet and the negative electrode sheet to play a role of isolation, and then wound to obtain an electrode assembly with a wound structure. The adhesive prepared above is adhered to the outer surface of the electrode assembly through the second adhesive layer, and then the electrode assembly is placed in an aluminum-plastic film packaging bag, and then through the top and side sealing, vacuum drying, liquid injection, formation (temperature 85°C, pressure 1.05MPa, 3.5V), capacity, and exhaust processes to obtain a lithium-ion battery. Among them, the liquid retention coefficient of the lithium-ion battery is 1.75g / Ah. The size of the first adhesive layer is 20mm×30mm, and the orthographic projection size of the electrode assembly along the stacking direction of the electrode assembly, adhesive and shell is 30mm×40mm, that is, S1=600mm 2 , S2=1200mm 2 .

[0085] Example 1-2 to Example 1-18

[0086] Except for adjusting the preparation parameters according to Table 1, the rest is the same as Example 1-1.

[0087] Example 2-1 to Example 2-3

[0088] Except for adjusting the thickness of the first adhesive layer according to Table 2, the rest is the same as Example 1-1.

[0089] Example 2-4 to Example 2-7

[0090] The same as Example 1-1 except that the area S1 of the first adhesive layer is adjusted according to Table 2 and the area S2 of the electrode assembly remains unchanged. As the area S1 of the first adhesive layer changes, the length and width of the first adhesive layer are scaled proportionally.

[0091] Example 2-8 to Example 2-9

[0092] Except for adjusting the liquid retention coefficient y according to Table 2, the rest is the same as Example 1-1.

[0093] Comparative Example 1

[0094] Except that the first adhesive layer does not contain the first resin and the preparation parameters are adjusted according to Table 1, the rest are the same as Example 1-1.

[0095] The relevant preparation parameters and performance tests of each embodiment and comparative example are shown in Table 1 and Table 2.

[0096] Table 1

[0097] Note: “ / ” in Table 1 indicates no relevant parameters, x is the friction coefficient between the first adhesive layer and the inner surface of the shell, F is the peel strength between the adhesive and the shell; the weight average molecular weight of the above-mentioned polyurethane is 800,000, and the weight average molecular weight of the above-mentioned polystyrene is 200,000.

[0098] As can be seen from Examples 1-1 to 1-10, Examples 1-17 to 1-18, and Comparative Example 1, when the first adhesive layer does not include the first resin, as in Comparative Example 1, while the peel strength between the adhesive and the housing is high, the coefficient of friction between the first adhesive layer and the inner surface of the housing is low. In other words, when the first adhesive layer does not include the first resin, both the coefficient of friction between the first adhesive layer and the inner surface of the housing and the peel strength between the adhesive and the housing cannot be achieved. When the first adhesive layer includes SIS and the first resin, both the coefficient of friction between the first adhesive layer and the inner surface of the housing and the peel strength between the adhesive and the housing can be achieved. The values ​​of x and F are both larger, and the ratio of the number of failures to the total number of failures in the roller test and drop test of the lithium-ion battery is smaller, indicating that the lithium-ion battery has better safety performance.

[0099] The weight percentages of SIS and the first resin affect the safety performance of lithium-ion batteries. As can be seen from Examples 1-1 to 1-10, and 1-17 to 1-18, by adjusting the weight percentages of SIS and the first resin within the range of this application, both the coefficient of friction between the first adhesive layer and the inner surface of the housing and the peel strength between the adhesive and the housing can be balanced. The values ​​of x and F are both large, and the ratio of the number of failures to the total number of lithium-ion batteries in the roller test and drop test is smaller, indicating that the lithium-ion batteries have better safety performance.

[0100] The type of first resin can affect the safety performance of lithium-ion batteries. Examples 1-1, 1-11, and 1-16 show that the type of first resin, within the scope of this application, balances the coefficient of friction between the first adhesive layer and the inner surface of the housing, as well as the peel strength between the adhesive and the housing. The values ​​of x and F are both large, and the ratio of the number of failures to the total number of failures in the roller test and drop test of the lithium-ion battery is small, indicating that the lithium-ion battery has good safety performance.

[0101] When the first resin is an acrylonitrile-butadiene-styrene copolymer, the mass percentage of the monomers that form the acrylonitrile-butadiene-styrene copolymer can affect the safety performance of the lithium-ion battery. As can be seen from Examples 1-1, 1-11, and 1-14, the mass percentage of the monomers of the acrylonitrile-butadiene-styrene copolymer within the range of this application can balance the coefficient of friction between the first adhesive layer and the inner surface of the housing, as well as the peel strength between the adhesive member and the housing. Both x and F have large values, which can improve the bonding performance of the first adhesive layer and alleviate the problem of swelling on the surface and corners of the electrode assembly. The ratio of the number of failures to the total number of failures in the roller test and drop test of the lithium-ion battery is small, indicating that the lithium-ion battery has good safety performance.

[0102] The change in the mass percentage of the functional resin will affect the friction coefficient x between the first adhesive layer and the inner surface of the shell, the peel strength F between the adhesive and the shell, and thus affect the safety performance of the lithium-ion battery.

[0103] As can be seen from Examples 1-10, the mass percentage of the functional resin is within the range of the present application, which can take into account both the friction coefficient between the first adhesive layer and the inner surface of the shell and the peel strength between the adhesive and the shell. The values ​​of x and F are both large, and the ratio of the number of failures to the total number in the roller test and drop test of the lithium-ion battery is small, indicating that the lithium-ion battery has good safety performance.

[0104] Variations in the mass percentage of additives and antioxidants affect the friction coefficient x between the first adhesive layer and the inner surface of the housing, as well as the peel strength F between the adhesive and the housing, and thus the safety performance of the lithium-ion battery. As can be seen from Examples 1-1, 1-7, and 1-9, the mass percentages of additives and antioxidants within the ranges of this application balance the friction coefficient between the first adhesive layer and the inner surface of the housing, as well as the peel strength between the adhesive and the housing. The values ​​of x and F are both relatively high, and the ratio of the number of failures to the total number of lithium-ion batteries in the roller test and drop test is relatively low, indicating that the lithium-ion batteries have good safety performance.

[0105] The peel strength between the adhesive and the packaging bag of Examples 1-7 changes over temperature as follows: At the lithium-ion battery formation temperatures of 65°C, 75°C, 80°C, 85°C, and 90°C, the peel strengths between the adhesive and the packaging bag of Examples 1-7 of the present application were 376 N / m, 379 N / m, 383 N / m, 384 N / m, and 387 N / m, respectively. It can be seen that the peel strength between the adhesive and the packaging bag of Examples 1-7 remains at the same level from 65°C to 90°C, broadening the process window (65°C to 90°C) for the lithium-ion battery formation process. This is because the molecular chains of the first resin in the first adhesive layer are more flexible, the cohesive force of the first adhesive layer is relatively low, and it can quickly exert its adhesiveness at a lower temperature (65°C). The peel strength-temperature variation between the adhesive and the packaging bag of Comparative Example 1 is as follows: when the formation temperatures of the lithium-ion battery are 65°C, 75°C, 80°C, 85°C, and 90°C, respectively, the peel strengths between the adhesive and the packaging bag of Comparative Example 1 are 37 N / m, 142 N / m, 417 N / m, 423 N / m, and 434 N / m, respectively. It can be seen that the peel strength gradually increases and then remains constant, resulting in a narrow process window (80°C to 90°C) for the lithium-ion battery formation process.

[0106] The adhesives in Example 1-1 and Comparative Example 1 were cut into 5g rectangular blocks and immersed in an 85°C electrolyte for 24 hours. The adhesive in Example 1-1 swelled to 5.720g, with a swelling ratio of 14.4%. In contrast, the adhesive in Comparative Example 1 swelled to 6.805g, with a swelling ratio of 36.1%, and remained shapeless. This demonstrates that the adhesives in this application can swell in the electrolyte and maintain a stable shape.

[0107] Table 2

[0108] Note: In Table 2, y is the liquid retention coefficient, x is the friction coefficient between the first adhesive layer and the inner surface of the shell, and F is the peel strength between the adhesive and the shell.

[0109] The thickness of the first adhesive layer affects the safety performance of lithium-ion batteries. As can be seen from Examples 1-1, 2-1, and 2-3, the thickness of the first adhesive layer is within the range of this application, ensuring both the coefficient of friction between the first adhesive layer and the inner surface of the housing and the peel strength between the adhesive and the housing. The values ​​of x and F are both large, and the ratio of the number of failures to the total number of failures in the roller test and drop test of the lithium-ion battery is small, indicating that the lithium-ion battery has good safety performance.

[0110] The S1 / S2 ratio affects the safety performance of lithium-ion batteries. As can be seen from Examples 1-1, 2-4, and 2-7, the S1 / S2 ratio is within the range of this application, ensuring a balanced balance between the coefficient of friction between the first adhesive layer and the inner surface of the housing and the peel strength between the adhesive and the housing. Furthermore, the values ​​of x and F are both large, and the ratio of the number of failures to the total number of failures in the roller test and drop test of the lithium-ion battery is small, indicating that the lithium-ion battery has good safety performance.

[0111] The liquid retention coefficient of a secondary battery can affect the safety performance of a lithium-ion battery. As can be seen from Examples 1-1, 2-8, and 2-9, the liquid retention coefficient of the secondary battery is within the range of this application, taking into account both the friction coefficient between the first adhesive layer and the inner surface of the housing and the peel strength between the adhesive and the housing. The values ​​of x and F are both large, and the ratio of the number of failures to the total number of lithium-ion batteries in the roller test and drop test is small, indicating that the lithium-ion battery has good safety performance.

[0112] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.

Claims

1. A secondary battery, comprising an electrode assembly, an electrolyte, a shell and an adhesive, wherein the adhesive is arranged between the electrode assembly and the shell, The adhesive member includes a stacked first adhesive layer and a second adhesive layer, the first adhesive layer is bonded to the inner surface of the shell, and the second adhesive layer is bonded to the outer surface of the electrode assembly; the first adhesive layer includes styrene-isoprene-styrene block copolymer and a first resin, and the first resin includes at least one of acrylonitrile-butadiene-styrene copolymer, polyurethane or polystyrene.

2. The secondary battery according to claim 1, It is characterized in that Based on the mass of the first adhesive layer, the mass percentage of the styrene-isoprene-styrene block copolymer is 32.5% to 75%, and the mass percentage of the first resin is 15% to 45%.

3. The secondary battery according to claim 1, It is characterized in that Based on the mass of the first adhesive layer, the mass percentage of the first resin is 20% to 40%.

4. The secondary battery according to claim 1, It is characterized in that Based on the mass of the first adhesive layer, the mass percentage of the first resin is 25% to 35%.

5. The secondary battery according to claim 1, It is characterized in that The first adhesive layer also includes a functional resin, and based on the mass of the first adhesive layer, the mass percentage of the functional resin is 5% to 25%; the functional resin includes at least one of ethylene-vinyl acetate copolymer, polyurethane elastomer, polyurethane acrylate, polyisobutylene or polybutadiene.

6. The secondary battery according to claim 1, It is characterized in that The first adhesive layer further includes an additive and an antioxidant; based on the mass of the first adhesive layer, the mass percentage of the additive is 1% to 5%, and the mass percentage of the antioxidant is 1% to 5%.

7. The secondary battery according to claim 1, It is characterized in that The adhesive component further includes a substrate layer, and the substrate layer is located between the first adhesive layer and the second adhesive layer; the substrate layer includes at least one of polyethylene terephthalate, polyimide or polypropylene.

8. The secondary battery according to claim 1, It is characterized in that The area of ​​the first adhesive layer is S 1 The orthographic projection area of ​​the electrode assembly along the stacking direction of the electrode assembly, the adhesive and the shell is S 2 , S 1 / S 2 Satisfy 10%≤S 1 / S 2 ≤95%.

9. The secondary battery according to claim 1, It is characterized in that The shell is a packaging bag.

10. The secondary battery according to claim 1, It is characterized in that The thickness of the first adhesive layer is 2 μm to 20 μm.

11. The secondary battery according to claim 1, It is characterized in that The peel strength between the adhesive and the shell is 10N / m to 500N / m.

12. The secondary battery according to claim 9, It is characterized in that The secondary battery has a liquid retention coefficient of 1 g / Ah to 2.5 g / Ah. 13 . An electronic device comprising the secondary battery according to claim 1 .