Flame-retardant thin film, current collector, electrode, and battery

Through the design of multi-layer film structure and current collector, combined with the copper metal layer, the contradiction between flame retardancy and energy density of traditional batteries is solved, efficient flame retardant effect and mechanical performance improvement are achieved, and the flame retardant problem in traditional batteries is solved. Agent affects lithium ion conduction.

WO2024198560A1PCT designated stage expired Publication Date: 2024-10-03JIANGYIN NANOPORE INNOVATIVE MATERIALS TECH LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/141123
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2023-12-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

There is a contradiction between improving flame retardancy and energy density in traditional batteries. Adding flame retardants will affect lithium ion conduction and reduce battery performance, and it is difficult to densely add flame retardant substances to pure metal films.

Method used

It adopts a multi-layer flame-retardant film structure, including inner layer, middle layer and outer film, which is blended with polytetrafluoroethylene, potassium perfluorobutane sulfonate, polybutylene terephthalate and triphenyl phosphate. Preparation, combining the copper metal layer and the current collector to form a sandwich-type multi-layer structure, which synergistically exerts the effects of gas-phase flame retardancy and solid-phase isolation.

Benefits of technology

The flame retardant effect and mechanical properties are significantly improved. Through the formation of fluorine radicals and carbon film, the flame propagation and heat release are effectively suppressed, and the safety and performance of the battery are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2023141123-FTAPPB-I100001
    Figure PCTCN2023141123-FTAPPB-I100001
Patent Text Reader

Abstract

A flame-retardant thin film, a current collector, an electrode, and a battery, relating to the technical field of flame-retardant batteries. An inner-layer thin film is prepared by blending polytetrafluoroethylene and potassium perfluorobutanesulfonate, a middle-layer thin film is prepared by blending polybutylene terephthalate and ytterbium trifluoromethanesulfonate, an outer-layer thin film is prepared by blending polystyrene and triphenyl phosphate, and a flame-retardant thin film is prepared by hot-pressing the three layers of thin films. Compared with a conventional single-layer flame-retardant thin film, the prepared sandwich-type multi-layer flame-retardant thin film has a synergistic effect and has more excellent flame retardance and mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Flame retardant film, current collector, electrode and battery Technical Field

[0001] The present application relates to the technical field of flame-retardant batteries, and in particular to a flame-retardant film, a current collector, an electrode and a battery. Background Art

[0002] There has always been a conflict between high safety and high energy density. Whether adding flame retardants to the electrolyte, separator, or positive and negative electrode materials, they introduce new substances into the lithium ion transmission path, thereby affecting ion conduction, which in turn affects battery performance and ultimately reduces energy density.

[0003] From a battery's internal structure, during the charging and discharging process, lithium ions flow from one electrode material to the other, through the electrolyte, and across the separator. Therefore, any new substance added during this process will affect battery performance. For example, adding a flame retardant to the electrolyte will reduce its conductivity. Therefore, the current collector, which is not involved in the lithium ion transport process, is an ideal location for storing flame retardants.

[0004] At present, traditional pure metal films use high-purity metals as raw materials, and it is difficult to add flame retardants into the dense metal layer. Therefore, it is of great significance to propose a flame retardant battery.

[0005] Summary of the Invention

[0006] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.

[0007] The purpose of this application is to provide a flame-retardant film, a current collector, an electrode and a battery to solve the problems raised in the above background technology.

[0008] In order to solve the above technical problems, this application provides the following technical solutions:

[0009] A flame retardant film comprises the following raw materials in percentage by weight: 85.0% to 99.0% of polymer and 1.0% to 15.0% of flame retardant.

[0010] Optionally, the flame retardant film is prepared as follows: a polymer and a flame retardant are mixed and then subjected to a melt-biaxial stretching method to obtain the flame retardant film.

[0011] Optionally, the polymer is one or more of polypropylene, polyethylene, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyimide, polypropylene, polyvinyl chloride, polyvinylidene fluoride, polytetrafluoroethylene, polyphenylene sulfide, polyphenylene oxide, polystyrene and polyamide.

[0012] Optionally, the flame retardant is one or more of ytterbium trifluoromethanesulfonate, potassium perfluorobutanesulfonate and triphenyl phosphate.

[0013] Optionally, the flame retardant film has a thickness of 1 μm-5 μm.

[0014] Optionally, the flame-retardant film is a polytetrafluoroethylene layer, and a polybutylene terephthalate layer and a polystyrene layer are symmetrically arranged on both sides of the polytetrafluoroethylene layer, and the polybutylene terephthalate layer is arranged between the polytetrafluoroethylene layer and the polystyrene layer;

[0015] Optionally, the polytetrafluoroethylene layer comprises the following raw materials in percentage by weight: 85.0% to 99.0% polytetrafluoroethylene and 1.0% to 15.0% potassium perfluorobutanesulfonate; the polybutylene terephthalate layer comprises the following raw materials in percentage by weight: 85.0% to 99.0% polybutylene terephthalate and 1.0% to 15.0% ytterbium trifluoromethanesulfonate; the polystyrene layer comprises the following raw materials in percentage by weight: 85.0% to 99.0% polystyrene and 1.0% to 15.0% triphenyl phosphate;

[0016] Optionally, on one side of the flame retardant film, the mass ratio of polytetrafluoroethylene in the polytetrafluoroethylene layer, polybutylene terephthalate in the polybutylene terephthalate layer, and polystyrene in the polystyrene layer is 3:(2-3):4, and the other side of the flame retardant film is the same.

[0017] Optionally, the polytetrafluoroethylene layer includes the following raw materials in percentage by mass: 85.0% to 99.0% polytetrafluoroethylene and 1.0% to 15.0% potassium perfluorobutanesulfonate; the polybutylene terephthalate layer includes the following raw materials in percentage by mass: 85.0% to 99.0% polybutylene terephthalate and 1.0% to 15.0% ytterbium trifluoromethanesulfonate; the polystyrene layer includes the following raw materials in percentage by mass: 85.0% to 99.0% polystyrene and 1.0% to 15.0% triphenyl phosphate.

[0018] A flame-retardant current collector is prepared according to the following method: conductive carbon black is added to water and stirred for 100 minutes to obtain a uniform conductive carbon black slurry; after stirring evenly, aluminum oxide and silicon carbide are added to a solvent and stirred evenly to obtain a first slurry; a binder is then added and stirred evenly to obtain a second slurry; the second slurry is applied to the surface of a metal layer through a coating system and then dried; the thickness of the final protective layer is controlled by controlling the coating amount, and finally a flame-retardant current collector is obtained.

[0019] Optionally, the metal layer is prepared as follows: the prepared flame-retardant film is placed in a vacuum evaporation chamber, and the high-purity copper wire (purity greater than 99.99%) in the metal evaporation chamber is melted and evaporated at a high temperature of 1500°C. The evaporated metal atoms pass through the cooling system in the vacuum coating chamber and are deposited on the two opposite surfaces of the flame-retardant film to form a copper metal conductive layer with a thickness of 1 μm to obtain a metal layer.

[0020] Optionally, the thickness of the metal layer is 500 nm to 2000 nm.

[0021] Optionally, the material of the metal layer includes one or more of titanium, silver, aluminum alloy, aluminum, nickel alloy, nickel, copper alloy and copper.

[0022] Optionally, a protective layer is provided on the surface of the metal layer.

[0023] Optionally, a protective layer is provided on the surface of the metal layer, and the thickness of the protective layer is 10 nm to 200 nm.

[0024] Optionally, a protective layer is provided on the surface of the metal layer, and a material of the protective layer includes one or both of aluminum oxide and silicon carbide.

[0025] A positive electrode sheet is prepared by the following method: adding a positive electrode active material, a conductive agent and a binder to N-methylpyrrolidone (NMP), mixing them evenly to prepare a positive electrode slurry, and evenly coating the positive electrode slurry on the surface of a flame-retardant current collector, and drying to obtain a positive electrode sheet.

[0026] Optionally, the positive electrode active material is NMC811, the conductive agent is conductive carbon black, and the binder is polyvinylidene fluoride (PVDF).

[0027] A negative electrode sheet is prepared by the following method: adding a negative electrode active material, a conductive agent, a thickener and a binder to deionized water, mixing them evenly to obtain a negative electrode slurry, and evenly coating the negative electrode slurry on the surface of a flame retardant current collector, and drying to obtain a negative electrode sheet.

[0028] Optionally, the negative electrode active material is graphite powder, the conductive agent is conductive carbon black, the thickener is sodium carboxymethyl cellulose (CMC), and the binder is styrene-butadiene rubber (SBR).

[0029] A flame retardant battery is prepared as follows:

[0030] The positive electrode sheets, negative electrode sheets and separators are stacked to obtain a laminated battery cell, and then the tabs of all the positive electrode sheets of the laminated battery cell are ultrasonically welded, and the tabs of all the negative electrode sheets are ultrasonically welded. Then, the battery cell is placed in a shell, the electrolyte is injected, and the shell is sealed to obtain a flame retardant battery.

[0031] Optionally, the electrolyte is any one of dimethyl carbonate (DMC), ethylene carbonate (EC), ethyl methyl carbonate (EMC) and lithium hexafluorophosphate (LiPF6) with a concentration of 1M.

[0032] Compared with the prior art, the beneficial effects achieved by the present application are as follows: the present application prepares an inner layer film by blending polytetrafluoroethylene and potassium perfluorobutanesulfonate, prepares an intermediate layer film by blending polybutylene terephthalate and ytterbium trifluoromethanesulfonate, and prepares an outer layer film by blending polystyrene and triphenyl phosphate, and the three layers of film are prepared by hot pressing to obtain a flame-retardant film.

[0033] Compared with traditional single-layer flame-retardant films, the "sandwich" multi-layer flame-retardant film prepared in this application has a synergistic effect, synergistically exerting gas-phase flame retardancy and solid-phase isolation, effectively improving the flame retardant effect. In addition, the addition of flame retardants to the film also effectively improves the mechanical properties of the film.

[0034] The carbon-fluorine bonds in the structure of potassium perfluorobutanesulfonate in the inner layer can be broken when heated, releasing fluorine free radicals and effectively capturing free active free radicals generated by thermal degradation of polymer materials, which can effectively reduce the concentration of free radicals, thereby alleviating or terminating the free radical chain reaction of combustion and inhibiting flame propagation. Polytetrafluoroethylene, as a carrier of potassium perfluorobutanesulfonate, can help it release fluorine free radicals during the heating process.

[0035] The ytterbium trifluoromethanesulfonate in the intermediate layer has high thermodynamic stability and a high residual carbon content below 600°C. After combustion, it forms a carbonized layer on the surface of the current collector, providing a thermal insulation effect, thereby gradually reducing the heat release rate. The free radicals generated during thermal degradation by this substance have a stronger capture ability, which is the result of the combined action of anions and cations in the rare earth compound. Due to the strong electron-withdrawing ability of the fluorine atom, the trifluoromethanesulfonate (anion) is highly likely to generate free radicals under high temperature conditions, thereby capturing the free radicals generated by the base film. At the same time, the Yb (cation), due to its variable valence, captures free radicals through reversible valence transformation under high temperature conditions.

[0036] The triphenyl phosphate in the outer layer promotes the dehydration and carbonization of the base material, thereby preventing the polymer material from producing flammable gases. In addition, since the non-volatile phosphorus compound acts as a coagulant, the carbonized material forms a protective carbon film to isolate the external air and heat. Polystyrene, as a carrier of triphenyl phosphate, helps to disperse it and provides sufficient support for the carbon film formed after the triphenyl phosphate is heated and carbonized, making it less likely to collapse and greatly enhancing the stability of the carbon layer.

[0037] Still other aspects will become apparent upon reading and understanding the detailed description. DETAILED DESCRIPTION

[0038] The following is a clear and complete description of the technical solutions in the embodiments of this application. Obviously, the embodiments described are only part of the embodiments of this application, not all of them. Based on the embodiments of this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.

[0039] In the following examples, polytetrafluoroethylene has a CAS registration number of 9002-84-0, polybutylene terephthalate has a CAS registration number of 26062-94-2, polystyrene has a CAS registration number of 9003-53-6, and polyethylene terephthalate has a CAS registration number of 25038-59-9.

[0040] Example 1: Preparation of a flame retardant film, comprising the following steps:

[0041] S1: 95.0 g of polyethylene terephthalate and 5.0 g of ytterbium trifluoromethanesulfonate were mixed and then prepared into a film by a melt-biaxial stretching method, which includes the following steps: crystallization drying - melt extrusion - sheet casting - longitudinal stretching - transverse stretching - heat setting; a film with a thickness of 5 μm was prepared.

[0042] Example 2: Preparation of a flame-retardant film: basically the same as Example 1, the main difference is that the flame retardant is 7.0% ytterbium trifluoromethanesulfonate.

[0043] Example 3: Preparation of a flame-retardant film: basically the same as Example 1, the main difference is that the flame retardant is 10.0% ytterbium trifluoromethanesulfonate.

[0044] Example 4: Preparation of a flame-retardant film: basically the same as Example 1, the main difference is that the flame retardant is 15.0% ytterbium trifluoromethanesulfonate.

[0045] Example 5: Preparation of a flame-retardant film: basically the same as Example 1, the main difference is that the flame retardant is 3% ytterbium trifluoromethanesulfonate and 4% potassium perfluorobutanesulfonate.

[0046] Example 6: Preparation of a flame-retardant film: basically the same as Example 1, the main difference is that the flame retardant is 3% ytterbium trifluoromethanesulfonate and 4% triphenyl phosphate.

[0047] Example 7: Preparation of a flame-retardant film: basically the same as Example 1, the main difference is that the flame retardant is 7% triphenyl phosphate.

[0048] Example 8: Preparation of a flame-retardant film: basically the same as Example 1, the main difference is that the flame retardant is 7% potassium perfluorobutanesulfonate.

[0049] Example 9: Preparation of a flame-retardant battery: S1: 71.25g of polytetrafluoroethylene and 3.75g of potassium perfluorobutanesulfonate, 47.5g of polybutylene terephthalate and 2.5g of ytterbium trifluoromethanesulfonate, 95g of polystyrene and 5g of triphenyl phosphate are mixed respectively, and then a melt-biaxial stretching method is used to prepare a film, which includes the following steps: crystallization drying-melt extrusion-casting-longitudinal stretching-transverse stretching-heat setting, to obtain an inner layer, an intermediate layer and an outer layer of the film respectively, the intermediate layer is placed on both sides of the inner layer, the outer layer is placed on the two intermediate layers and the outer layers, and hot pressing is performed to prepare a flame-retardant film with a thickness of 5μm.

[0050] S2: The prepared flame-retardant film is placed in a vacuum evaporation chamber. A high-purity copper wire (purity greater than 99.99%) is melted and evaporated at a high temperature of 1500°C in the metal evaporation chamber. The evaporated metal atoms pass through the cooling system in the vacuum coating chamber and are deposited on the two opposite surfaces of the flame-retardant film, forming a copper metal layer with a thickness of 1 μm.

[0051] S3: Add 2 kg of conductive carbon black to 20 kg of water and stir for 100 minutes to obtain a uniform conductive carbon black slurry; after stirring evenly, add 1 g of aluminum oxide and 1 g of silicon carbide to the solvent and stir evenly to obtain a first slurry, then add a binder and stir evenly to obtain a second slurry. The obtained second slurry is applied to the surface of the metal layer through a coating system and then dried. The final protective layer thickness is controlled by controlling the coating amount, and finally a current collector with a protective layer thickness of 100 nm is obtained;

[0052] S4: The method for preparing the positive electrode sheet includes the following steps: adding 96 g of positive electrode active material NMC811, 2 g of conductive agent carbon black, and 2 g of binder PVDF to 80 g of NMP, mixing them evenly to prepare a ternary positive electrode slurry, and evenly coating the ternary positive electrode slurry on the surface of the composite aluminum foil current collector obtained above, and drying to obtain a positive electrode sheet;

[0053] S5: The negative electrode sheet preparation method includes the following steps: adding 95.4 g of negative electrode active material graphite powder, 2.6 g of conductive agent carbon black, 1 g of thickener CMC and 1 g of binder SBR to 90 g of deionized water, mixing them evenly to obtain a negative electrode slurry, and evenly coating the negative electrode slurry on the surface of a negative electrode sheet current collector copper foil with a thickness of 10 μm, and drying to obtain a negative electrode sheet;

[0054] S6: After stacking the positive electrode sheets, negative electrode sheets and separators, a laminated battery cell is obtained. Then, the tabs of all the positive electrode sheets of the laminated battery cell are ultrasonically welded, and the tabs of all the negative electrode sheets are ultrasonically welded. Then, the laminated battery cell is placed in a shell, dimethyl carbonate is injected, and the shell is sealed to obtain a battery.

[0055] Comparative Example 1: Preparation of a flame-retardant film: basically the same as Example 1, with the main difference being that the flame retardant is 20% ytterbium trifluoromethanesulfonate.

[0056] Comparative Example 2: Preparation of a flame-retardant film: basically the same as Example 1, the main difference is that no flame retardant is added.

[0057] Comparative Example 3: Preparation of a flame-retardant battery: basically the same as Example 9, with the main difference being: S1: 71.25g of polytetrafluoroethylene and 3.75g of potassium perfluorobutanesulfonate, 47.5g of polybutylene terephthalate and 2.5g of ytterbium trifluoromethanesulfonate, 125g of polystyrene and 15g of triphenyl phosphate were mixed respectively, and then a melt-biaxial stretching method was used to prepare a film, comprising the following steps: crystallization drying-melt extrusion-casting-longitudinal stretching-transverse stretching-heat setting, to obtain an inner layer, an intermediate layer and an outer layer of the film respectively, the intermediate layer was placed on both sides of the inner layer, the outer layer was placed between the two intermediate layers and the outer layer, and hot pressed to prepare a film with a thickness of 5μm.

[0058] Comparative Example 4: Preparation of a flame-retardant battery: basically the same as Example 9, the main difference is that the inner layer raw material and the outer layer raw material are exchanged.

[0059] test:

[0060] The films with metal layers prepared in Examples 1-9 and Comparative Examples 1-4 were tested for tensile strength and elongation at break according to the national standard GB / T 1040.3-2006, wherein all the data were in the longitudinal direction.

[0061] Acupuncture test:

[0062] Batteries prepared from the films of Examples 1-8 and Comparative Examples 1-2, as well as the batteries described in Example 9 and Comparative Examples 3-4, were tested. Ten samples of each battery were fully charged at 0.7C at room temperature, allowed to stand for 3 hours, and then subjected to a needle penetration test according to GB / T 31485-2015. Passing was determined if no smoke or fire occurred. The needle penetration test pass rate = number of lithium-ion batteries passing the test / 10. The test results are shown in Table 1.

[0063] Surface temperature rise:

[0064] The batteries prepared from the films of Examples 1-8 and Comparative Examples 1-2, as well as the batteries described in Example 9 and Comparative Examples 3-4, were tested for surface temperature rise. The test was performed using a real-time temperature tester. The thermocouple sensing probe of the temperature tester was placed on the surface of the batteries prepared from the examples and comparative examples, and temperature detection was performed to calculate the maximum surface temperature rise.

[0065] Finally, it should be noted that the above description is merely a preferred embodiment of the present application and is not intended to limit the present application. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art may still modify the technical solutions described in the aforementioned embodiments or substitute equivalents for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included within the scope of protection of the present application.

Claims

1. A flame retardant film comprising the following raw materials in percentage by weight: 85.0% to 99.0% polymer and 1.0% to 15.0% flame retardant.

2. The flame retardant film according to claim 1, wherein: The polymer is one or more of polypropylene, polyethylene, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyimide, polypropylene, polyvinyl chloride, polyvinylidene fluoride, polytetrafluoroethylene, polyphenylene sulfide, polyphenylene oxide, polystyrene and polyamide.

3. The flame retardant film according to claim 1 or 2, wherein: The flame retardant is one or more of ytterbium trifluoromethanesulfonate, potassium perfluorobutanesulfonate and triphenyl phosphate.

4. The flame retardant film according to any one of claims 1 to 3, wherein: The thickness of the flame retardant film is 1 μm-5 μm.

5. The flame retardant film according to any one of claims 1 to 4, wherein: The flame retardant film is a polytetrafluoroethylene layer, on both sides of which a polybutylene terephthalate layer and a polystyrene layer are symmetrically arranged in sequence, and the polybutylene terephthalate layer is arranged between the polytetrafluoroethylene layer and the polystyrene layer; the polytetrafluoroethylene layer comprises the following raw materials in percentage by weight: 85.0% to 99.0% polytetrafluoroethylene and 1.0% to 15.0% potassium perfluorobutyl sulfonate; the polybutylene terephthalate layer comprises the following raw materials in percentage by weight: 85.0% to 99.0% polytetrafluoroethylene and 1.0% to 15.0% potassium perfluorobutyl sulfonate; Butylene terephthalate, 1.0% to 15.0% ytterbium trifluoromethanesulfonate; the polystyrene layer comprises the following raw materials in percentage by mass: 85.0% to 99.0% polystyrene, 1.0% to 15.0% triphenyl phosphate; in one side of the flame retardant film, the mass ratio of polytetrafluoroethylene in the polytetrafluoroethylene layer, polybutylene terephthalate in the polybutylene terephthalate layer, and polystyrene in the polystyrene layer is 3: (2 to 3): 4, and the other side of the flame retardant film is the same.

6. A flame-retardant current collector, comprising a flame-retardant film and a metal layer located on at least one side of the flame-retardant film, wherein the flame-retardant film is the flame-retardant film according to any one of claims 1 to 5.

7. The flame-retardant current collector according to claim 6, wherein: The invention comprises at least one of the following features (1) to (5): (1) The thickness of the metal layer is 500nm to 2000nm; (2) The material of the metal layer includes one or more of titanium, silver, aluminum alloy, aluminum, nickel alloy, nickel, copper alloy and copper; (3) A protective layer is provided on the surface of the metal layer; (4) A protective layer is provided on the surface of the metal layer, and the thickness of the protective layer is 10 nm to 200 nm; (5) A protective layer is provided on the surface of the metal layer, and the material of the protective layer includes one or both of aluminum oxide and silicon carbide.

8. A flame-retardant electrode, comprising the flame-retardant current collector according to claim 6 or 7, and an active material layer attached to at least one side of the flame-retardant current collector; The active material layer is positive electrode slurry or negative electrode slurry.

9. A flame-retardant battery, comprising the flame-retardant electrode according to claim 8.

10. A flame retardant electrical device comprising the flame retardant battery according to claim 9.

Citation Information

Patent Citations

  • Negative current collector, negative pole piece and electrochemical device

    CN110943228A

  • Current collector and preparation method and application thereof

    CN111048788A

  • Lithium ion battery, novel current collector and preparation method of novel current collector

    CN112786895A

  • Lightweight flame-retardant current collector, preparation method thereof, electrode and battery

    CN114156486A

  • Composite current collector and preparation method and application thereof

    CN114597338A