Secondary battery and electronic device

By using optimized silicon-oxygen composite materials in the negative electrode sheets of lithium-ion batteries, the problem of electrolyte consumption caused by silicon materials during charge and discharge cycles is solved, the cycle performance and rate performance of the battery are improved, and the service life of the battery is extended. .

WO2024198631A1PCT designated stage expired Publication Date: 2024-10-03NINGDE AMPEREX TECHNOLOGY LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/071599
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-01-10
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

During the charge and discharge cycle of lithium-ion batteries, due to the volume expansion and contraction of the silicon material, the electrolyte consumption increases, affecting the cycle performance.

Method used

A secondary battery was designed, and its negative electrode plate includes a silicon-oxygen composite material. By regulating the peak ratio of thermogravimetric analysis and Raman spectrum, the structure and composition of the silicon-oxygen composite material were optimized to reduce the contact between silicon and electrolyte. Reduce side reactions and electrolyte consumption.

Benefits of technology

The first Coulomb efficiency, rate performance, cycle performance and expansion performance of the secondary battery are improved, and the service life of the battery is extended.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024071599_03102024_PF_FP_ABST
    Figure CN2024071599_03102024_PF_FP_ABST
Patent Text Reader

Abstract

A secondary battery and an electronic device. The secondary battery comprises a negative electrode plate. The negative electrode plate comprises a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector. The negative electrode active material layer comprises a negative electrode active material. The negative electrode active material comprises a silicon-oxygen composite material. The negative electrode plate has a thermal weight primary differential curve having a peak-to-peak intensity of Y1 at 500℃ to 700℃. The negative electrode plate has a thermal weight primary differential curve having a peak-to-peak intensity of Y2 at 350℃ to 450℃, where 0.1≤Y1 / Y2≤4. The negative electrode plate of the secondary battery comprises a silicon-oxygen composite material, and Y1 / Y2 is adjusted and controlled to satisfy the relation above, such that side reaction and electrolyte consumption in a first lithium intercalation process of the secondary battery can be reduced, the first coulombic efficiency of the secondary battery is increased, and the rate capability, cycle performance and expansion performance of the secondary battery are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Secondary battery and electronic device

[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on March 31, 2023, with application number 202310341446.X and invention name “A Secondary Battery and Electronic Device”, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The present application relates to the field of electrochemical technology, and in particular to a secondary battery and an electronic device. Background Art

[0003] Secondary batteries, such as lithium-ion batteries, have the characteristics of high operating voltage, high energy density, long cycle life, and wide operating temperature range. These excellent characteristics have enabled lithium-ion batteries to be widely used in three major fields: consumer electronics, power batteries, and energy storage.

[0004] Silicon materials have a high theoretical specific capacity and hold broad application prospects in lithium-ion batteries. However, during the charge-discharge cycle, as lithium ions are inserted and removed, the silicon material expands and contracts in volume, leading to increased electrolyte consumption and affecting the cycle performance of lithium-ion batteries.

[0005] Summary of the Invention

[0006] The purpose of this application is to provide a secondary battery and an electronic device to improve the cycle performance of the secondary battery. The specific technical solution is as follows:

[0007] The first aspect of the present application provides a secondary battery comprising a negative electrode plate, the negative electrode plate comprising a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector, the negative electrode active material layer comprising a negative electrode active material, and the negative electrode active material comprising a silicon-oxygen composite material; the peak-to-peak intensity of the first differential curve of the thermogravimetric analysis of the negative electrode plate at 500°C to 700°C is Y1, the peak-to-peak intensity of the first differential curve of the thermogravimetric analysis of the negative electrode plate at 350°C to 450°C is Y2, and Y1 / Y2 satisfies 0.1≤Y1 / Y2≤4. The secondary battery provided by the present application comprises a silicon-oxygen composite material and regulates Y1 / Y2 to satisfy the above relationship, which can reduce side reactions and electrolyte consumption during the initial lithium insertion process of the secondary battery, increase the initial coulombic efficiency of the secondary battery, and improve the rate performance, cycle performance, and expansion performance of the secondary battery.

[0008] In some embodiments of the present application, 0.5≤Y1 / Y2≤2.5. By regulating the value of Y1 / Y2 within the above range, it is beneficial to further reduce side reactions and electrolyte consumption during the initial lithium insertion process of the secondary battery, increase the initial coulombic efficiency of the secondary battery, and improve the rate performance, cycle performance, and expansion performance of the secondary battery.

[0009] In some embodiments of the present application, the Raman spectrum of the negative electrode sheet is at 1200 cm -1 Up to 1500cm -1 The peak intensity is I1, and the Raman spectrum of the negative electrode is at 300cm -1 Up to 600cm -1 The peak-to-peak intensity is I2, and I1 / I2 satisfies 2≤I1 / I2≤15. By regulating the value of I1 / I2 within the above range, it is beneficial to further improve the rate performance, cycle performance and expansion performance of the secondary battery.

[0010] In some embodiments of the present application, the Dv50 of the silicon-oxygen composite material is 3 μm to 15 μm; the specific surface area of ​​the silicon-oxygen composite material is 0.2 m 2 / g to 8m 2 By regulating the Dv50 and specific surface area of ​​the silicon-oxygen composite material within the above range, it is beneficial to improve the cycle performance, expansion performance and fast charge and discharge performance of the secondary battery.

[0011] In some embodiments of the present application, the silicon-oxygen composite material has a core-shell structure, comprising a core and a first shell and a second shell disposed on at least a portion of the core's surface; the core comprises silicon grains and lithium silicate, the first shell comprises amorphous carbon, and the second shell comprises a metal oxide and a lithiated metal oxide; the metal oxide comprises at least one of aluminum oxide, titanium dioxide, or niobium pentoxide. A negative electrode comprising the silicon-oxygen composite material with these characteristics can reduce the likelihood of silicon contacting the electrolyte, reduce side reactions and electrolyte consumption during the initial lithium insertion process of a secondary battery, increase the initial coulombic efficiency of the secondary battery, and improve the rate capability, cycling performance, and expansion performance of the secondary battery.

[0012] In some embodiments of the present application, based on the mass of the silicon-oxygen composite material, the mass percentage of amorphous carbon is 1% to 5%, the sum of the mass percentages of the metal oxide and the lithiated metal oxide is 1% to 5%, and the sum of the mass percentages of the silicon grains and the lithium silicate is 92% to 98%. By adjusting the mass percentages of amorphous carbon, the sum of the mass percentages of the metal oxide and the lithiated metal oxide, and the sum of the mass percentages of the silicon grains and the lithium silicate within the above ranges, the initial coulombic efficiency of the secondary battery is further improved, as well as the rate capability, cycle performance, and expansion performance of the secondary battery.

[0013] In some embodiments of the present application, the size of the silicon grains is 0.5 nm to 10 nm. By adjusting the size of the silicon grains within the above range, the secondary battery can have a high energy density while improving the rate performance, cycle performance, and expansion performance of the secondary battery.

[0014] In some embodiments of the present application, the second shell of the silicon-oxygen composite material includes a metal element, wherein the metal element includes at least one of aluminum, titanium, or niobium, and the weight percentage of the metal element is 0.1% to 1% based on the weight of the second shell. A negative electrode plate including a silicon-oxygen composite material having the above characteristics can reduce the possibility of contact between silicon and electrolyte, reduce side reactions and electrolyte consumption during the initial lithium insertion process of the secondary battery, increase the initial coulombic efficiency of the secondary battery, and improve the rate performance, cycle performance, and expansion performance of the secondary battery.

[0015] In some embodiments of the present application, the negative electrode active material further includes graphite, and the mass percentage of the silicon-oxygen composite material is 1% to 15% based on the sum of the mass of the silicon-oxygen composite material and the graphite. By including graphite in the negative electrode active material and adjusting the mass percentage of the silicon-oxygen composite material to be within the above range, the secondary battery can have high energy density while also having good cycle performance and expansion performance.

[0016] In some embodiments of the present application, in a charge-discharge cycle test of the secondary battery at 25±1°C using 3C step charge and 0.5C discharge, when the secondary battery is cycled 800 times or more, the ratio of the expansion rate of the negative electrode plate to the expansion rate of the secondary battery is 0.5 to 4. This indicates that the expansion of the negative electrode plate accounts for a small proportion of the secondary battery during the cycle, and the expansion of the negative electrode active material is improved, that is, the secondary battery has good expansion performance.

[0017] The second aspect of the present application provides an electronic device comprising the secondary battery provided in the first aspect of the present application. The secondary battery provided in the first aspect of the present application has good rate performance, cycle performance, and expansion performance, so that the electronic device of the present application has a long service life.

[0018] Beneficial effects of this application:

[0019] The present application provides a secondary battery and an electronic device. The secondary battery includes a negative electrode plate, the negative electrode plate includes a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector, the negative electrode active material layer includes a negative electrode active material, and the negative electrode active material includes a silicon-oxygen composite material. The peak-to-peak intensity of the first differential curve of the thermogravimetric analysis of the negative electrode plate at 500°C to 700°C is Y1, and the peak-to-peak intensity of the first differential curve of the thermogravimetric analysis of the negative electrode plate at 350°C to 450°C is Y2, and Y1 / Y2 satisfies 0.1≤Y1 / Y2≤4. The secondary battery provided in the present application includes a silicon-oxygen composite material and regulates Y1 / Y2 to satisfy the above relationship, which can reduce side reactions and electrolyte consumption during the initial lithium insertion process of the secondary battery, improve the initial coulombic efficiency of the secondary battery, and improve the rate performance, cycle performance, and expansion performance of the secondary battery.

[0020] Of course, it is not necessary to achieve all the advantages described above at the same time when implementing any product or method of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other embodiments can also be obtained based on these drawings.

[0022] FIG1 is a thermogravimetric (TG) curve and a thermogravimetric first differential (DTG) curve of the negative electrode sheet of Examples 1-8;

[0023] FIG2 is a TG curve and a DTG curve of the negative electrode sheet of Comparative Example 1;

[0024] FIG3 is a TG curve and a DTG curve of the negative electrode sheet of Example 2-5;

[0025] FIG4 is a Raman spectrum of the negative electrode sheet of Example 1-8;

[0026] FIG5 is a Raman spectrum of the negative electrode sheet of Example 2-5. DETAILED DESCRIPTION

[0027] The following will be combined with the drawings in the embodiments of this application to clearly and completely describe the technical solutions in the embodiments of this application. Obviously, the embodiments described are only part of the embodiments of this application, not all of the embodiments. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field based on this application are within the scope of protection of this application.

[0028] It should be noted that, in the specific embodiments of the present application, lithium-ion batteries are used as an example of secondary batteries to explain the present application, but the secondary batteries of the present application are not limited to lithium-ion batteries.

[0029] A first aspect of the present application provides a secondary battery, which includes a negative electrode plate, the negative electrode plate includes a negative electrode current collector and a negative electrode active material layer arranged on at least one surface of the negative electrode current collector, the negative electrode active material layer includes a negative electrode active material, and the negative electrode active material includes a silicon-oxygen composite material; the peak-to-peak intensity of the thermogravimetric first differential curve of the negative electrode plate at 500°C to 700°C is Y1, the peak-to-peak intensity of the thermogravimetric first differential curve of the negative electrode plate at 350°C to 450°C is Y2, and Y1 / Y2 satisfies 0.1≤Y1 / Y2≤4, for example, the value of Y1 / Y2 can be 0.1, 0.3, 0.5, 0.7, 0.9, 1.0, 1.2, 1.9, 2.5, 3, 3.5, 4 or a range consisting of any two of these values.

[0030] The peak of the thermogravimetric first differential curve of the above-mentioned negative electrode sheet between 500℃ and 700℃ corresponds to the decomposition of silicon-containing organic lithium salts (such as LixSiOy / ROCO2Li composite lithium salts, etc., where 0<x≤2, 0<y≤3, R is methyl, ethyl, etc.), and the peak between 350℃ and 450℃ corresponds to the decomposition of silicon-free lithium salts (such as LiF, Li2O, etc.). The value of Y1 / Y2 reflects the content ratio of silicon-containing organic lithium salts to silicon-free lithium salts. The higher the peak intensity, the higher the content of lithium salt corresponding to the peak. When the value of Y1 / Y2 is too small, it is not conducive to improving the energy density of the secondary battery; when the value of Y1 / Y2 is too large, it will affect the kinetic performance, cycle performance and expansion performance of the secondary battery. The secondary battery provided in the present application includes a silicon-oxygen composite material and regulates the value of Y1 / Y2 within the scope of the present application, which can reduce the side reactions and electrolyte consumption in the first lithium insertion process of the secondary battery, improve the first coulomb efficiency and energy density of the secondary battery, and improve the rate performance, cycle performance and expansion performance of the secondary battery.

[0031] In some embodiments of the present application, 0.5≤Y1 / Y2≤2.5. For example, the value of Y1 / Y2 can be 0.5, 0.7, 0.9, 1.0, 1.2, 1.5, 1.9, 2.2, 2.5, or a range consisting of any two of these values. By regulating the value of Y1 / Y2 within the above range, it is beneficial to reduce side reactions and electrolyte consumption during the initial lithium insertion process of the secondary battery, improve the initial coulombic efficiency and energy density of the secondary battery, and improve the rate performance, cycle performance, and expansion performance of the secondary battery.

[0032] In some embodiments of the present application, the Raman spectrum of the negative electrode sheet is at 1200 cm -1 Up to 1500cm -1 The peak intensity is I1, and the Raman spectrum of the negative electrode is at 300cm -1 Up to 600cm -1 The peak intensity is I2, and I1 / I2 satisfies 2≤I1 / I2≤15. For example, the value of I1 / I2 can be 2, 3, 5, 7, 9, 10, 12, 14, 15 or a range consisting of any two of these values. The Raman spectrum of the above negative electrode is at 1200 cm -1 Up to 1500cm -1 The peak corresponds to the characteristic D peak of graphite at 300 cm -1 Up to 600cm -1 The peak corresponds to the characteristic peak of amorphous silicon. The I1 / I2 value reflects the ratio of graphite to silicon in the negative electrode. The higher the peak intensity, the higher the content of the substance corresponding to the peak. By adjusting the I1 / I2 value within the above range, it is beneficial to further improve the rate performance, cycle performance, and expansion performance of the secondary battery.

[0033] In some embodiments of the present application, the Dv50 of the silicon-oxygen composite material is 3 μm to 15 μm, preferably 5 μm to 11 μm; the specific surface area of ​​the silicon-oxygen composite material is 0.2 m 2 / g to 8m 2 / g, preferably 0.5m 2 / g to 3m 2 For example, the Dv50 of the silicon-oxygen composite material can be 3 μm, 5 μm, 6 μm, 6.5 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 14 μm, 15 μm, or a range consisting of any two of these values. The specific surface area of ​​the silicon-oxygen composite material can be 0.2 m 2 / g, 0.5m 2 / g、1m 2 / g, 1.1m 2 / g, 1.2m 2 / g, 1.3m 2 / g, 1.5m 2 / g, 1.6m 2 / g, 1.7m 2 / g, 1.8m 2 / g, 2m 2 / g、3m 2 / g、5m 2 / g、7m 2 / g、8m 2 / g or a range consisting of any two of these values. During the cycle of the secondary battery, HF in the byproduct of the electrolyte reaction will etch the silicon-oxygen composite material, which will cause the solid electrolyte interface film (SEI film) to grow and erode into the interior of the particles. By regulating the Dv50 of the silicon-oxygen composite material within the above range, the proportion of silicon-oxygen particles eroded by the SEI film is reduced, which is beneficial to improving the cycle performance and expansion performance of the secondary battery; by regulating the specific surface area of ​​the silicon-oxygen composite material within the above range, the silicon-oxygen composite material has a larger specific surface area and a larger contact area with the electrolyte, which is beneficial to the active ions (such as Li + ) transmission, thereby improving the dynamic performance and fast charging and discharging performance of the secondary battery.

[0034] In some embodiments of the present application, the silicon-oxygen composite material has a core-shell structure, comprising a core and a first shell and a second shell disposed on at least a portion of the surface of the core; the core comprises silicon grains and lithium silicate, the first shell comprises amorphous carbon, and the second shell comprises a metal oxide and a lithiated metal oxide; the metal oxide comprises at least one of aluminum oxide, titanium dioxide, or niobium pentoxide. In the silicon-oxygen composite material having the above characteristics, the silicon grains in the core are dispersed in the lithium silicate, which can improve silicon expansion; the first shell comprises amorphous carbon, which can reduce the likelihood of silicon contacting the electrolyte; and the second shell comprises a metal oxide and a lithiated metal oxide. The metal oxide or lithiated metal oxide can reduce electrolyte corrosion of silicon, reducing side reactions during the initial lithium insertion process and reducing electrolyte consumption. The first and second shells protect silicon, thereby reducing the content of silicon-containing organic lithium salts in the solid electrolyte interface film, which is beneficial for improving the energy density of the secondary battery and improving the kinetic and cycling performance of the secondary battery. The negative electrode plate includes a silicon-oxygen composite material with the above characteristics, which can reduce side reactions and electrolyte consumption during the initial lithium insertion process of the secondary battery, improve the initial coulombic efficiency of the secondary battery, and improve the rate performance, cycle performance and expansion performance of the secondary battery.

[0035] In some embodiments of the present application, the silicon-oxygen composite material includes an inner core and a first shell and a second shell sequentially disposed on at least a portion of the surface of the inner core. In other embodiments, the silicon-oxygen composite material includes an inner core and a second shell and a first shell sequentially disposed on at least a portion of the surface of the inner core. This application does not impose any particular limitation on this, as long as the objectives of this application can be achieved.

[0036] In some embodiments of the present application, based on the mass of the silicon-oxygen composite material, the mass percentage of amorphous carbon is 1% to 5%, the sum of the mass percentages of the metal oxide and the lithiated metal oxide is 1% to 5%, and the sum of the mass percentages of the silicon grains and the lithium silicate is 92% to 98%. For example, the mass percentage of amorphous carbon can be 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, or a range consisting of any two values ​​therein, the sum of the mass percentages of the metal oxide and the lithiated metal oxide can be 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, or a range consisting of any two values ​​therein, and the sum of the mass percentages of the silicon grains and the lithium silicate can be 92%, 92.5%, 93%, 94%, 95%, 96%, 97%, 98%, or a range consisting of any two values ​​therein. By adjusting the mass percentage of amorphous carbon, the sum of the mass percentages of metal oxide and lithiated metal oxide, and the sum of the mass percentages of silicon grains and lithium silicate within the above ranges, it is beneficial to better exert the protective effect of the first shell and the second shell, thereby further improving the initial coulombic efficiency and energy density of the secondary battery, and improving the rate performance, cycle performance and expansion performance of the secondary battery.

[0037] The present application does not particularly limit the mass ratio of the metal oxide to the lithiated metal oxide, as long as the purpose of the present application can be achieved. For example, the mass ratio of the metal oxide to the lithiated metal oxide can be 1:5 to 5:1. The present application does not particularly limit the mass ratio of the silicon grains to the lithium silicate, as long as the purpose of the present application can be achieved. For example, the mass ratio of the silicon grains to the lithium silicate can be 2:3 to 3.5:1. In the present application, the particle size of the core is 3 μm to 15 μm, preferably 4.5 μm to 8 μm.

[0038] In some embodiments of the present application, the size of the silicon grains is 0.5 nm to 10 nm. For example, the size of the silicon grains can be 0.5 nm, 1 nm, 2.5 nm, 5 nm, 5.5 nm, 6 nm, 6.5 nm, 7 nm, 7.5 nm, 8 nm, 9 nm, 10 nm, or a range consisting of any two of these values. By adjusting the size of the silicon grains within the above range, the secondary battery can have a high energy density while improving the rate performance, cycle performance, and expansion performance of the secondary battery.

[0039] In some embodiments of the present application, the second shell of the silicon-oxygen composite material includes a metal element, and the metal element includes at least one of aluminum, titanium, or niobium. Based on the mass of the second shell, the mass percentage of the metal element is 0.1% to 1%. For example, the mass percentage of the metal element can be 0.1%, 0.3%, 0.4%, 0.5%, 0.7%, 0.8%, 0.9%, 1%, or a range consisting of any two of these values. The negative electrode plate includes a silicon-oxygen composite material with the above characteristics, which can reduce the possibility of silicon contacting the electrolyte, reduce side reactions and electrolyte consumption during the initial lithium insertion process of the secondary battery, improve the initial coulombic efficiency of the secondary battery, and improve the cycle performance and expansion performance of the secondary battery.

[0040] The present application does not impose any particular restrictions on the preparation method of the silicon-oxygen composite material, as long as the purpose of the present application can be achieved. For example, it can be prepared by the following method: After uniformly mixing elemental silicon and silicon dioxide, the mixture is placed in an evaporation chamber of a deposition furnace, heated to 1100°C to 1300°C for the first deposition, and then the deposited SiO blocks are collected in the deposition chamber, and the silicon-oxygen material is obtained after crushing, grading, and other treatments. The silicon-oxygen material is deposited for a second time in an acetylene gas atmosphere, and amorphous carbon is deposited on the surface of the silicon-oxygen material to obtain a silicon-oxygen material with a first shell of amorphous carbon on the surface, which is recorded as C@SiO material. The C@SiO material is placed in an ethanol solution and a salt containing a metal element (such as aluminum isopropoxide) and polyvinyl pyrrolidone (PVP) are added. After stirring evenly, the mixture is spray-dried and then calcined for the first time under the protection of an inert atmosphere to obtain a C@SiO material silicon-oxygen material with Al2O3 on the surface, which is recorded as Al2O3@C@SiO material. The Al2O3@C@SiO material is uniformly mixed with lithium nitride (Li3N), and then calcined a second time under an inert atmosphere. During the calcination process, the Li3N decomposes into lithium and nitrogen. The lithium is molten at the calcination temperature and can react with the Al2O3 on the surface of the Al2O3@C@SiO material to form lithiated Al2O3. It can also react with the silicon oxide material within the Al2O3@C@SiO material, ultimately producing a silicon oxide composite material comprising a first shell and a second shell. The core is the product of the reaction between the molten lithium and the silicon oxide material, comprising lithium silicate and silicon grains dispersed within the lithium silicate. The first shell comprises amorphous carbon, and the second shell comprises Al2O3 and lithiated Al2O3. In the above preparation method, the molar ratio of elemental silicon to silicon dioxide is 1:(0.5 to 2), the molar ratio of aluminum isopropoxide to polyvinylpyrrolidone (PVP) is 1:(0.5 to 2), and the total mass ratio of aluminum isopropoxide and PVP to the mass of the C@SiO material is 2% to 8%. The mass ratio of Al2O3@C@SiO material to lithium nitride (Li3N) is (85:15) to (95:5). The second deposition temperature is 500°C to 700°C for 2 to 4 hours. The first calcination temperature is 500°C to 700°C for 4 to 6 hours. The second calcination temperature is 600°C to 800°C for 4 to 6 hours.

[0041] The present application does not particularly limit the above-mentioned classification method, as long as the objectives of the present application can be achieved. For example, the crushed silicon-oxygen material can be classified by screening, airflow classification, etc. The present application does not particularly limit the flow rate of the acetylene gas, and it can be selected according to conventional operations in the field, as long as the objectives of the present application can be achieved. For example, the flow rate of the acetylene gas can be 2L / min to 10L / min. The present application does not particularly limit the gas of the inert atmosphere, as long as the objectives of the present application can be achieved. For example, it can include but is not limited to at least one of helium or argon.

[0042] Generally, the mass ratio of aluminum isopropoxide and PVP to the silicon-oxygen material, the mass ratio of Al2O3@C@SiO to Li3N, the temperature and time of the second deposition, and the temperature and time of the second calcination can be adjusted to control the mass percentage of amorphous carbon, the mass percentage of metal oxides and lithiated metal oxides, and the mass percentage of silicon grains and lithium silicate in the silicon-oxygen composite. For example, increasing the mass ratio of aluminum isopropoxide and PVP to the silicon-oxygen material increases the mass percentage of metal oxides and lithiated metal oxides; decreasing the mass ratio of aluminum isopropoxide and PVP to the silicon-oxygen material decreases the mass percentage of metal oxides and lithiated metal oxides. Increasing the mass ratio of Al2O3@C@SiO to Li3N increases the mass percentage of silicon grains and lithium silicate; decreasing the mass ratio of Al2O3@C@SiO to Li3N decreases the mass percentage of silicon grains and lithium silicate. Increasing the temperature of the second deposition increases the mass percentage of amorphous carbon; decreasing the temperature of the second deposition decreases the mass percentage of amorphous carbon. Prolonging the second deposition time increases the mass percentage of amorphous carbon; shortening the second deposition time decreases the mass percentage of amorphous carbon. Increasing the second calcination temperature decreases the mass percentage of metal oxides and lithiated metal oxides, while increasing the mass percentage of silicon grains and lithium silicate. Lowering the second calcination temperature increases the mass percentage of metal oxides and lithiated metal oxides, while decreasing the mass percentage of silicon grains and lithium silicate. Prolonging the second calcination time decreases the mass percentage of metal oxides and lithiated metal oxides, while increasing the mass percentage of silicon grains and lithium silicate. Shortening the second deposition time increases the mass percentage of metal oxides and lithiated metal oxides, while decreasing the mass percentage of silicon grains and lithium silicate.

[0043] In some embodiments of the present application, the negative electrode active material further includes graphite, and the mass percentage of the silicon-oxygen composite material is 1% to 15% based on the sum of the mass of the silicon-oxygen composite material and the graphite. For example, the mass percentage of the silicon-oxygen composite material can be 1%, 3%, 4%, 5%, 7%, 8%, 9%, 10%, 12%, 15%, or a range consisting of any two of these values. By including graphite in the negative electrode active material and adjusting the mass percentage of the silicon-oxygen composite material to be within the above range, the secondary battery can have high energy density while having good cycling performance and expansion performance.

[0044] In the present application, the mass percentage of silicon is 0.1% to 10% based on the mass of the negative electrode active material layer. When the mass percentage of silicon is within the above range, the secondary battery can have high energy density and good expansion performance.

[0045] Typically, the Y1 / Y2 ratio can be controlled by varying the silicon-oxygen composite material content, the mass percentage of silicon crystals, and the lithium silicate content in the negative electrode active material layer. For example, increasing the silicon-oxygen composite material content in the negative electrode active material layer increases the Y1 / Y2 ratio; decreasing the silicon-oxygen composite material content decreases the Y1 / Y2 ratio. Increasing the mass percentage of silicon crystals and lithium silicate increases the Y1 / Y2 ratio; decreasing the mass percentage of silicon crystals and lithium silicate decreases the Y1 / Y2 ratio.

[0046] In some embodiments of the present application, in a charge-discharge cycle test of a secondary battery at 25±1°C using 3C step charge and 0.5C discharge, when the secondary battery is cycled 800 times or more, the ratio of the expansion rate of the negative electrode plate to the expansion rate of the secondary battery is 0.5 to 4. For example, the ratio of the expansion rate of the negative electrode plate to the expansion rate of the secondary battery can be 0.5, 0.8, 1, 1.5, 2, 2.5, 3, 3.5, 4, or a range consisting of any two of these values. This indicates that the expansion of the negative electrode plate accounts for a small proportion of the secondary battery during the cycle, and the expansion of the negative electrode active material is improved, that is, the secondary battery has good expansion performance. In this application, the above-mentioned 3C step charge and 0.5C discharge charge and discharge cycle test process is: the secondary battery is left to stand in a 45°C environment for 5 minutes, then charged to 4.25V at a 3C constant current, then charged to 4.4V at a 2C constant current, then charged to 4.4V at a 1C constant current, and then charged to 0.05C at a 4.45V constant voltage, left to stand for 5 minutes, and then discharged to 3.0V at a 0.5C constant current, and left to stand for 5 minutes.

[0047] The present application has no special restrictions on the negative electrode current collector, as long as the purpose of the present application can be achieved. For example, the negative electrode current collector may include copper foil, copper alloy foil, nickel foil, titanium foil, nickel foam or copper foam, etc. In the present application, there is no special restriction on the thickness of the negative electrode current collector and the negative electrode active material layer, as long as the purpose of the present application can be achieved. For example, the thickness of the negative electrode current collector is 4μm to 12μm, and the thickness of the single-sided negative electrode active material layer is 30μm to 130μm. In the present application, the negative electrode active material layer can be arranged on one surface in the thickness direction of the negative electrode current collector, or on two surfaces in the thickness direction of the negative electrode current collector. It should be noted that the "surface" here can be the entire area of ​​the negative electrode current collector or a partial area of ​​the negative electrode current collector. The present application has no special restrictions, as long as the purpose of the present application can be achieved. The negative electrode active material layer of the present application may also include a conductive agent and a binder.

[0048] The secondary battery of the present application also includes a positive electrode sheet. The present application has no special restrictions on the positive electrode sheet, as long as the purpose of the present application can be achieved. For example, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer provided on at least one surface of the positive electrode current collector. The present application has no special restrictions on the positive electrode current collector, as long as the purpose of the present application can be achieved. For example, the positive electrode current collector may include aluminum foil or aluminum alloy foil, etc. The positive electrode active material layer of the present application includes a positive electrode active material. The present application has no special restrictions on the type of positive electrode active material, as long as the purpose of the present application can be achieved. For example, the positive electrode active material may include at least one of lithium nickel cobalt manganese oxide (NCM811, NCM622, NCM523, NCM111), lithium nickel cobalt aluminum oxide, lithium iron phosphate, lithium-rich manganese-based material, lithium cobalt oxide (LiCoO2), lithium manganese oxide, lithium iron manganese phosphate or lithium titanate, etc. In the present application, the positive electrode active material may further contain non-metallic elements, for example, non-metallic elements include at least one of fluorine, phosphorus, boron, chlorine, silicon, sulfur, etc. These elements can further improve the stability of the positive electrode active material. In the present application, there is no particular restriction on the thickness of the positive electrode current collector and the positive electrode active material layer, as long as the purpose of the present application can be achieved. For example, the thickness of the positive electrode current collector is 5μm to 20μm, preferably 6μm to 18μm. The thickness of the single-sided positive electrode active material layer is 30μm to 120μm. In the present application, the positive electrode active material layer can be arranged on one surface in the thickness direction of the positive electrode current collector, or on two surfaces in the thickness direction of the positive electrode current collector. It should be noted that the "surface" here can be the entire area of ​​the positive electrode current collector or a partial area of ​​the positive electrode current collector. This application has no particular restrictions, as long as the purpose of the present application can be achieved. The positive electrode active material layer of the present application may also contain a conductive agent and a binder.

[0049] The above-mentioned conductive agent and binder are not particularly limited, as long as the purpose of the present application can be achieved. For example, the conductive agent may include at least one of conductive carbon black (Super P), carbon nanotubes (CNTs), carbon nanofibers, flake graphite, carbon dots or graphene, etc. The binder may include at least one of polypropylene alcohol, sodium polyacrylate, potassium polyacrylate, lithium polyacrylate, polyimide, polyamide-imide, styrene-butadiene rubber (SBR), polyvinyl alcohol (PVA), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl butyral (PVB), water-based acrylic resin, carboxymethyl cellulose (CMC) or sodium carboxymethyl cellulose (CMC-Na), etc.

[0050] In the present application, the secondary battery also includes an electrolyte, and the electrolyte includes a lithium salt and a non-aqueous solvent. The lithium salt may include at least one of LiPF6, LiBF4, LiAsF6, LiClO4, LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiN(SO2CF3)2, LiC(SO2CF3)3, Li2SiF6, lithium bis(oxalatoborate) (LiBOB) or lithium difluoroborate. The present application has no particular restrictions on the concentration of the lithium salt in the electrolyte, as long as the purpose of the present application can be achieved. For example, the concentration of the lithium salt in the electrolyte is 0.9 mol / L to 1.5 mol / L. The present application has no particular restrictions on the non-aqueous solvent, as long as the purpose of the present application can be achieved, for example, it may include but is not limited to at least one of a carbonate compound, a carboxylate compound, an ether compound or other organic solvents. The above-mentioned carbonate compound may include but is not limited to at least one of a chain carbonate compound, a cyclic carbonate compound or a fluorinated carbonate compound. The above-mentioned linear carbonate compound may include but is not limited to at least one of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methylpropyl carbonate (MPC), ethylpropyl carbonate (EPC) or methyl ethyl carbonate (MEC). The above-mentioned cyclic carbonate may include but is not limited to at least one of ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC) or vinyl ethylene carbonate (VEC). The fluorinated carbonate compound may include but is not limited to at least one of fluoroethylene carbonate (FEC), 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate or trifluoromethylethylene carbonate. The carboxylate compound may include but is not limited to at least one of methyl formate, methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decanoic acid, valerolactone or caprolactone. The ether compound may include but is not limited to at least one of dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, 1-ethoxy-1-methoxyethane, 2-methyltetrahydrofuran or tetrahydrofuran. The other organic solvents may include but are not limited to at least one of dimethyl sulfoxide, 1,2-dioxolane, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate or trioctyl phosphate.

[0051] The secondary battery of the present application also includes a diaphragm. The present application does not particularly limit the diaphragm, as long as the purpose of the present application can be achieved. For example, the material of the diaphragm may include but is not limited to polyethylene (PE), polypropylene (PP), polytetrafluoroethylene-based polyolefin (PO) diaphragms, polyester films (such as polyethylene terephthalate (PET) films), cellulose films, polyimide films (PI), polyamide films (PA), spandex or aramid films, etc. At least one of the types of diaphragms may include but is not limited to woven films, non-woven films (non-woven fabrics), microporous films, composite films, rolled films or spun films, etc. The diaphragm of the present application may have a porous structure, and the size of the pore size is not particularly limited, as long as the purpose of the present application can be achieved. For example, the size of the pore size can be 0.01 μm to 1 μm. In the present application, the thickness of the diaphragm is not particularly limited, as long as the purpose of the present application can be achieved. For example, the thickness can be 5 μm to 500 μm.

[0052] The secondary battery of this application also includes a packaging bag for containing the positive electrode sheet, separator, negative electrode sheet, and electrolyte, as well as other components of the secondary battery known in the art. This application does not limit these other components. This application does not specifically limit the packaging bag and can be any packaging bag known in the art, as long as it can achieve the purpose of this application. For example, an aluminum-plastic film packaging bag can be used.

[0053] The secondary battery of the present application is not particularly limited, and it may include any device in which an electrochemical reaction occurs. In one embodiment of the present application, the secondary battery may include but is not limited to: a lithium-ion secondary battery (lithium-ion battery), a sodium-ion secondary battery (sodium-ion battery), a lithium polymer secondary battery or a lithium-ion polymer secondary battery, etc. The lithium-ion battery structure of the present application includes a winding structure or a laminated structure, etc. The present application has no particular restrictions on the shape of the secondary battery, as long as the purpose of the present application can be achieved. For example, it may include but is not limited to cylindrical batteries, square batteries, special-shaped batteries or button batteries, etc.

[0054] The preparation process of the secondary battery of the present application is well known to those skilled in the art and is not particularly limited in the present application. For example, it may include but is not limited to the following steps: stacking the positive electrode sheet, the separator and the negative electrode sheet in order, and winding, folding and other operations as needed to obtain an electrode assembly with a wound structure, placing the electrode assembly in a packaging bag, injecting the electrolyte into the packaging bag and sealing it to obtain a secondary battery; or stacking the positive electrode sheet, the separator and the negative electrode sheet in order, and then fixing the four corners of the entire stacked structure with tape to obtain an electrode assembly with a stacked structure, placing the electrode assembly in a packaging bag, injecting the electrolyte into the packaging bag and sealing it to obtain a secondary battery. In addition, as needed, overcurrent protection elements, guide plates, etc. may be placed in the packaging bag to prevent pressure rise and overcharge and discharge inside the secondary battery.

[0055] The second aspect of the present application provides an electronic device comprising the secondary battery provided in the first aspect of the present application. The secondary battery provided in the first aspect of the present application has good rate performance, cycle performance, and expansion performance, so that the electronic device of the present application has a long service life.

[0056] The electronic device of the present application is not particularly limited and can be any electronic device known in the art. In some embodiments, the electronic device can include, but is not limited to, a laptop computer, a pen-type computer, a mobile computer, an e-book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a headset, a video recorder, an LCD television, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, an automobile, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, a power tool, a flashlight, a camera, a large household battery or a lithium-ion capacitor, etc.

[0057] Example

[0058] The following examples and comparative examples are provided to more specifically illustrate the embodiments of the present invention. Various tests and evaluations were performed according to the following methods. In addition, unless otherwise specified, "parts" and "%" are based on mass.

[0059] Test methods and equipment

[0060] Thermogravimetric (TG) curve test:

[0061] A fully discharged lithium-ion battery was disassembled, the negative electrode was removed, and the electrolyte was removed by soaking it in dimethyl carbonate (DMC) for 20 minutes. The negative electrode was then placed in an oven and baked at 80°C for 12 hours to obtain the treated negative electrode. Using N2 as the purge gas, the temperature was increased at a rate of 10°C / min from 35°C to 800°C. Thermogravimetric analysis (TG) of the TG test sample prepared from the treated negative electrode was performed to obtain the TG curve and thermogravimetric first differential (DTG) curve of the negative electrode.

[0062] Raman spectroscopy test:

[0063] A fully discharged lithium-ion battery was disassembled, the negative electrode was removed, and the electrolyte was removed by soaking it in dimethyl carbonate (DMC) for 20 minutes. The negative electrode was then placed in an oven and baked at 80°C for 12 hours to obtain the treated negative electrode. Raman spectroscopy was performed on the Raman test sample prepared from the treated negative electrode using a Raman spectrometer (Jobin Yvon LabRAM HR) with a light source of 532nm and a test range of 0cm. -1 Up to 4000cm-1 , the test sample area is 100μm×100μm.

[0064] Test of the content of each component in silicon-oxygen composite materials:

[0065] The mass percentage of amorphous carbon in silicon-oxygen composites is measured using a high-frequency infrared carbon-sulfur analyzer (Shanghai Dekai HCS-140). The silicon-oxygen composite sample is heated in a high-frequency furnace under oxygen-rich conditions, causing the amorphous carbon to oxidize into carbon dioxide. This treated gas then enters a corresponding absorption cell, where it absorbs the corresponding infrared radiation and is converted into a corresponding signal by a detector. This signal is sampled and analyzed by a computer to output the mass percentage of amorphous carbon in the silicon-oxygen composite.

[0066] The silica composite material is immersed in a 0.5 mol / L acetic acid solution for 30 minutes. The lithiated metal oxide (such as LiAlO2) coated on the surface of the silica composite material can be dissolved without dissolving Al2O3. The content of metal elements (non-lithium elements) in the solution is then tested using an inductively coupled plasma spectrometer (ICP-OES (PE Avio 200)) to obtain the lithiated metal oxide content.

[0067] Soak the silicon-oxygen composite material in a 1 mol / L nitric acid solution for 30 minutes to dissolve the metal oxide and the lithiated metal oxide coated on the surface of the silicon-oxygen composite material simultaneously. The same method is then used to measure the metal element (non-lithium element) content in the solution (when the metal is aluminum, the mass percentage of the aluminum element can be obtained). The sum of the mass percentages of the metal oxide and the lithiated metal oxide can be obtained. The mass percentage of the metal oxide can be calculated by subtracting the measured lithiated metal oxide content from the sum of the mass percentages of the metal oxide and the lithiated metal oxide. The mass percentage of the metal oxide divided by the mass percentage of the lithiated metal oxide can be obtained to obtain the mass ratio of the two.

[0068] After measuring the silicon and lithium contents in the silicon-oxygen composite using an ICP-OES (PE Avio 200) device, the lithium content in the lithium silicate is subtracted from the lithium content in the lithiated metal oxide. This yields the lithium content in the lithium silicate, which can then be used to calculate the mass percentage of the lithium silicate. The mass percentage of the silicon grains can be calculated by dividing the silicon content in the lithium silicate by the silicon content. The sum of the mass percentages of the silicon grains and the lithium silicate can then be calculated. The mass percentage of the silicon grains divided by the mass percentage of the lithium silicate yields the mass ratio of the two.

[0069] Particle size test:

[0070] The particle size distribution of the silicon-oxygen composite material was measured by a laser particle size analyzer (MasterSizer 2000). In the volume-based particle size distribution of the material, the particle size at which the volume accumulation reaches 50% is Dv50, measured from the smallest particle size.

[0071] Specific surface area test:

[0072] The nitrogen adsorption-desorption curve of the silicon-oxygen composite material was tested by a specific surface area tester (TriStar 3020), and the specific surface area of ​​the silicon-oxygen composite material was calculated according to the BET calculation method.

[0073] Silicon grain size test:

[0074] The material was subjected to XRD testing using an X-ray powder diffractometer (POWDIX 600 / 300), and the peak near 28.5° was calculated using the Scherrer formula to obtain the size of the silicon grains.

[0075] Gram capacity and first coulombic efficiency test:

[0076] The silicon-oxygen composite material, conductive carbon black, and styrene-butadiene rubber (SBR) binder from the example were mixed in a mass ratio of 8:1:1. Deionized water was then added as a solvent to prepare a negative electrode slurry with a solid content of 25 wt%, and the mixture was stirred evenly. The negative electrode slurry was evenly coated onto one surface of a 10 μm thick negative electrode current collector copper foil using a 50 μm scraper and dried at 70°C to produce a negative electrode sheet coated on one side with a 45 μm thick negative electrode active material layer. After drying and roller pressing, the sheet was punched into small discs with a diameter of 14 mm using a sheet puncher to serve as the working electrode. The mass of these small discs was weighed and recorded. A 15 mm diameter circular lithium sheet was used as the counter electrode. The separator and electrolyte were prepared according to the method described in Example 1-1. The separator was cut into 16 mm diameter discs and assembled into CR2032 button-type half-cells in a dry argon atmosphere glove box. The coin-shaped half-cell was left at a test temperature of 25°C for 5 minutes. The cell was then discharged at a constant current of 0.1C to 0.005V. The cell was then charged at a constant voltage of 0.005V to 0.005C, and the lithium insertion capacity (C0) was recorded. After 5 minutes of rest, the cell was then charged at a constant current of 0.1C to 0.8V, and the lithium removal capacity (C1) was recorded. The gram capacity of the silicon-oxygen composite material (mAh / g) was obtained by dividing C1 by the mass of the silicon-oxygen composite material. Here, the mass of the silicon-oxygen composite material = (mass of the small disc - mass of the copper foil) × 0.8. The initial coulombic efficiency = C1 / C0 × 100%.

[0077] The test methods for the gram capacity and first coulombic efficiency of the graphite / ordinary silicon oxide material / pre-lithiated silicon oxide material in the comparative example are the same as the test steps for the gram capacity and first coulombic efficiency of the above silicon oxide composite material, except that the above materials are used to replace the silicon oxide composite material.

[0078] AC impedance test:

[0079] A lithium-ion battery according to the embodiment / comparative example to be tested was prepared by inserting a copper wire into the lithium-ion battery as a reference electrode to obtain a three-electrode battery. The reference electrode copper wire was lithium-plated at a current of 20 μA for 6 h. After the lithium plating was completed, the electrochemical impedance spectroscopy (EIS) of the three-electrode battery was measured. The lithium-plated three-electrode battery was connected to an electrochemical workstation (Bio-Logic VMP3B, Bio-Roger, France) for EIS measurement. The test frequency range was 30 mHz to 50 kHz, and the amplitude was 5 mV. After data collection, the data was analyzed using an impedance complex plane plot to obtain the AC impedance Rct of the lithium-ion battery in mΩ.

[0080] Rate performance test:

[0081] Take the lithium-ion battery of the embodiment / comparative example to be tested and let it rest for 5 minutes at a test temperature of 25°C. Then, charge the lithium-ion battery with a constant current of 0.7C to 4.45V. Then, charge it with a constant voltage of 4.45V to 0.05C. After letting it rest for 5 minutes, discharge it with a constant current of 0.2C to 3.0V. Record the 0.2C discharge capacity. Then, let it rest for 5 minutes, repeat the above charging process, and then discharge it with a constant current of 2C. Record the 2C discharge capacity. Rate performance = 2C discharge capacity / 0.2C discharge capacity × 100%.

[0082] Cyclic performance and expansion performance test:

[0083] At a test temperature of 45°C, the lithium-ion battery to be tested was allowed to stand for 5 minutes, and the initial thickness MMC0 of the lithium-ion battery was recorded. The lithium-ion battery was constant-current charged to 4.25V at a current of 3C, then charged to 4.4V at 2C, then charged to 4.45V at 1C, and then charged to 0.05C at a constant voltage of 4.45V, and the discharge capacity C4 of the lithium-ion battery was recorded; it was allowed to stand for 5 minutes, and then discharged to 3.0V at a constant current of 0.5C, and allowed to stand for 5 minutes. After the above 3C step charge / 0.5C discharge charge and discharge cycle process was repeated 400 times, the thickness MMC1 and discharge capacity C5 of the lithium-ion battery were recorded. The capacity retention rate (%) after 400 cycles = C5 / C4×100%, and the expansion rate (%) after 400 cycles = (MMC1-MMC0) / MMC0×100%.

[0084] The expansion ratio test of the negative electrode and lithium-ion battery after 800 cycles:

[0085] The lithium-ion batteries to be tested were divided into two groups. One group was cycled 800 times according to the steps in the above-mentioned cycling performance and expansion performance testing process. The initial thickness of the lithium-ion batteries was MMC0, and the thickness of the lithium-ion batteries after 800 cycles was MMC2. The lithium-ion batteries, which had been fully discharged after 800 cycles, were then disassembled to measure the thickness of the negative electrode plate, H1. The other group was directly disassembled to measure the initial thickness of the negative electrode plate, H0. The expansion ratio of the negative electrode plate to the lithium-ion battery after 800 cycles was calculated as (MMC2 - MMC0) / (H1 - H0).

[0086] Energy density test:

[0087] In an environment of 25°C, the lithium ion battery of the embodiment is charged according to the following operating process and then discharged to obtain the discharge capacity of the lithium ion battery: the lithium ion battery is charged to 4.45V at a constant current of 0.7C, then charged to 0.05C at a constant voltage of 4.45V, left to stand for 5 minutes, discharged to 3.0V at a constant current of 0.2C, left to stand for 5 minutes, and the discharge capacity D is obtained. After the above lithium ion battery is charged to 3.85V at a constant current of 0.7C, then charged to 0.05C at a constant voltage of 3.85V, the length L, width W, and height H of the lithium ion battery are measured with a laser thickness gauge to obtain the volume V=L×W×H of the lithium ion battery. Its energy density (E D )=D / V, unit is Wh / L.

[0088] Example 1-1

[0089] <Preparation of Silicon-Oxygen Composite Material>

[0090] Step 1: Mix elemental silicon and silicon dioxide in a molar ratio of 1:1 and place them in the evaporation chamber of a deposition furnace. After heating to 1200°C for evaporation, collect the deposited SiO blocks (first deposition) in the deposition chamber. After crushing and grading, a silicon oxide material with a Dv50 of 7 μm is obtained.

[0091] Step 2: Place the material obtained in step 1 in a vapor deposition furnace, introduce acetylene gas at a flow rate of 3 L / min, and deposit at 600°C for 3 hours (second deposition). Deposit a first layer of amorphous carbon on the surface of the silicon-oxygen material to obtain a silicon-oxygen material with amorphous carbon on the surface, which is recorded as C@SiO material.

[0092] Step 3: The C@SiO material was placed in an ethanol solution and aluminum isopropoxide and polyvinylpyrrolidone (PVP) were added in a 1:1 molar ratio. The mixture was stirred evenly and spray-dried. The mixture was then calcined under an argon atmosphere to obtain a C@SiO material with Al2O3 on its surface, designated as Al2O3@C@SiO material. The first calcination temperature was 600°C for 5 hours. The mass ratio of the total mass of aluminum isopropoxide and PVP to the mass of the C@SiO material was A%, and A% was 2%.

[0093] Step 4: The Al2O3@C@SiO material and lithium nitride (Li3N) are mixed uniformly in a mass ratio of 95:5, and then calcined a second time under argon atmosphere to obtain a silicon-oxygen composite material with a first and second shells on the surface. The second calcination temperature is 700°C for 5 hours. The silicon-oxygen composite material has a core composed of silicon grains and lithium silicate, a first shell composed of amorphous carbon, and a second shell composed of Al2O3 and lithiated Al2O3.

[0094] <Preparation of negative electrode sheet>

[0095] The silicon-oxygen composite material and graphite prepared above were mixed evenly to obtain a negative electrode active material. The mass percentage of the silicon-oxygen composite material was 3% based on the sum of the mass of the silicon-oxygen composite material and the graphite. The graphite particle size Dv50 was 14.2 μm and the specific surface area was 1.02 m 2 / g.

[0096] The negative electrode active material, conductive carbon black, binder styrene-butadiene rubber, and thickener sodium carboxymethyl cellulose were mixed in a mass ratio of 97:0.5:0.4:2.1. Deionized water was then added as a solvent to prepare a negative electrode slurry with a solid content of 46 wt%, which was then stirred evenly. The negative electrode slurry was evenly coated on one surface of a 12 μm thick copper foil for the negative electrode current collector. The foil was then dried at 85°C for 4 hours to obtain a negative electrode sheet coated on one side with a negative electrode active material layer and a thickness of 60 μm. The above steps were repeated on the other surface of the aluminum foil to obtain a negative electrode sheet coated on both sides with a negative electrode active material layer. After drying at 85°C under vacuum for 4 hours, the sheet was cold pressed, cut, and slit to obtain a negative electrode sheet with a size of 76.6 mm x 875 mm.

[0097] <Preparation of positive electrode sheet>

[0098] The positive electrode active material, lithium cobalt oxide, the conductive agent, conductive carbon black, and the binder, PVDF, were mixed in a mass ratio of 96:2:2. NMP was added as a solvent and stirred thoroughly to prepare a positive electrode slurry with a solid content of 75 wt%. The positive electrode slurry was evenly coated on one surface of a 13 μm thick positive electrode current collector aluminum foil and dried at 90°C to obtain a single-sided positive electrode active material-coated positive electrode sheet with a thickness of 50 μm. The above steps were repeated on the other surface of the aluminum foil to obtain a double-sided positive electrode active material-coated positive electrode sheet. After drying under vacuum at 90°C for 4 hours, the sheet was cold pressed, cut, and slit to obtain a 74 mm x 867 mm positive electrode sheet.

[0099] <Preparation of Electrolyte>

[0100] In a dry argon atmosphere glove box, lithium salt LiPF6 was added to a mixed solvent of basic organic solvent DMC:DEC:EC=1:1:1, dissolved and mixed evenly to obtain an electrolyte, and vinylene carbonate was added thereto as an additive. Based on the mass of the electrolyte, the mass percentage of the lithium salt was 12.5%, the mass percentage of the vinylene carbonate was 2%, and the balance was the basic organic solvent.

[0101] <Preparation of Separator>

[0102] PVDF and alumina were mixed in a mass ratio of 9:1, NMP was added as a solvent, and a slurry with a solid content of 12 wt% was prepared. The mixture was stirred evenly and the slurry was evenly coated on one surface of a substrate PP film with a thickness of 7 μm. After drying, a diaphragm with a single-side coating of 2 μm was obtained.

[0103] <Preparation of lithium-ion batteries>

[0104] The prepared positive electrode sheet, separator, and negative electrode sheet are stacked in order, with the separator positioned between the positive and negative electrodes to provide insulation. The electrodes are then wound to form an electrode assembly. After welding the tabs, the electrode assembly is packaged in an aluminum-plastic film bag and dried in an 85°C vacuum oven for 12 hours to remove moisture. The prepared electrolyte is then injected, and the lithium-ion battery is produced through vacuum packaging, resting, formation, and shaping.

[0105] Example 1-2 to Example 1-10

[0106] Except for adjusting the preparation parameters in <Preparation of Silicon Oxygen Composite Material> according to Table 1, the rest is the same as Example 1-1

[0107] Examples 1-11

[0108] Except that the silicon-oxygen composite material was prepared using the following <Preparation of Silicon-Oxygen Composite Material> process, the rest was the same as Example 1-1.

[0109] <Preparation of Silicon-Oxygen Composite Material>

[0110] Step 1: Mix elemental silicon and silicon dioxide in a molar ratio of 1:1 and place them in the evaporation chamber of a deposition furnace. After heating to 1200°C for evaporation, collect the deposited SiO blocks (first deposition) in the deposition chamber. After crushing and grading, a silicon oxide material with a Dv50 of 7 μm is obtained.

[0111] Step 2: The silica material is placed in an ethanol solution and aluminum isopropoxide and polyvinylpyrrolidone (PVP) are added in a 1:1 molar ratio. The mixture is stirred thoroughly and spray-dried. The mixture is then calcined under an argon atmosphere to obtain a silica material with Al2O3 on its surface, designated as Al2O3@SiO. The calcination temperature is 600°C for 5 hours. The mass ratio of the combined aluminum isopropoxide and PVP to the silica material is A%, where A% is 4%.

[0112] Step 3: The Al2O3@SiO material obtained in step 2 is placed in a vapor deposition furnace, acetylene gas is introduced, and the acetylene gas flow rate is 3 L / min. Deposition is carried out at 600°C for 5 hours (second deposition). The first layer of amorphous carbon is deposited on the surface of the Al2O3@SiO material to obtain an Al2O3@SiO material with amorphous carbon on the surface, which is recorded as C@Al2O3@SiO material.

[0113] Step 4: Mix the C@Al2O3@SiO material and Li3N in a mass ratio of 90:10, then calcine the mixture a second time under argon to obtain a silicon-oxygen composite material with a first and second shells on the surface. The second calcination temperature is 600°C for 5 hours. The silicon-oxygen composite material has a core composed of silicon grains and lithium silicate, a first shell composed of amorphous carbon, and a second shell composed of Al2O3 and lithiated Al2O3.

[0114] Example 2-1

[0115] Except for adjusting the mass percentage of the silicon-oxygen composite material according to Table 3, the rest is the same as that of Examples 1-8.

[0116] Example 2-2 to Example 2-6

[0117] Except for adjusting the mass percentage of the silicon-oxygen composite material according to Table 3, the rest is the same as Example 2-1.

[0118] Comparative Example 1

[0119] Except that the purchased artificial graphite material (Aladdin, G434784) was used to replace the silicon-oxygen composite material, the rest was the same as Example 1-1.

[0120] Comparative Example 2

[0121] Except that the purchased common silicon-oxygen material (Aladdin, S431223) was used to replace the silicon-oxygen composite material, the rest was the same as Example 1-1.

[0122] Comparative Example 3

[0123] Except that the silicon-oxygen composite material is replaced by the pre-lithiated silicon-oxygen material prepared by the following <Preparation of Pre-lithiated Silicon-oxygen Material> process, the rest is the same as Example 1-1.

[0124] <Preparation of pre-lithiated silicon oxide material> Step 1: Mix elemental silicon and silicon dioxide in a molar ratio of 1:1 and place in the evaporation chamber of a deposition furnace. After heating to 1200°C for evaporation, the deposited SiO blocks (first deposition) are collected in the deposition chamber. After crushing and grading, a silicon oxide material with a Dv50 of 7μm is obtained.

[0125] Step 2: Place the material obtained in step 1 in a vapor deposition furnace, introduce acetylene gas at a flow rate of 3 L / min, and deposit at 600°C for 3 hours (second deposition) to deposit amorphous carbon on the surface of the silicon-oxygen material to obtain a silicon-oxygen material with a first shell of amorphous carbon on the surface, which is recorded as C@SiO material.

[0126] Step 3: Mix the C@SiO material and lithium nitride (Li3N) in a 95:5 mass ratio, then calcine the mixture a second time under argon to obtain a pre-lithiated silicon-oxygen material with a first shell on the surface. The second calcination temperature is 700°C for 5 hours; the first shell consists of amorphous carbon.

[0127] The preparation parameters and performance parameters of each embodiment and comparative example are shown in Tables 1 to 3.

[0128] Table 1

[0129] From Examples 1-1 to 1-11 and Comparative Examples 1 to 3, it can be seen that when the value of Y1 / Y2 is too small, the gram capacity of the corresponding negative electrode active material is low, which is not conducive to improving the capacity of the lithium-ion battery. For example, compared with Comparative Example 1, the gram capacity of the negative electrode active material in the embodiment of the present application is more than 3 times the gram capacity of the artificial graphite material in Comparative Example 1, that is, the lithium-ion battery in the embodiment of the present application has a higher capacity. Although the lithium-ion battery in Comparative Example 1 has good rate performance, cycle performance, and expansion performance, it cannot achieve high capacity at the same time. When the value of Y1 / Y2 is too large, the AC impedance of the lithium-ion battery is large, the rate performance and cycle capacity retention rate are low, and the expansion rate ratio of the negative electrode plate to the battery is high after 800 cycles. For example, compared with Comparative Examples 2 and 3, the lithium-ion battery in the embodiment of the present application has lower AC impedance, higher rate performance and cycle capacity retention rate, and its expansion rate ratio of the negative electrode plate to the battery is lower after 800 cycles. The negative electrode plate of the lithium-ion battery in the embodiment of the present application includes a silicon-oxygen composite material, and when Y1 / Y2 satisfies 0.1≤Y1 / Y2≤4, the lithium-ion battery has lower AC impedance, higher capacity, rate performance and cycle capacity retention rate, and the expansion rate ratio of the negative electrode plate to the battery after 800 cycles is lower, indicating that the lithium-ion battery provided by the present application can simultaneously have better rate performance, cycle performance and expansion performance.

[0130] It can be seen from Examples 1-1 to 1-11 that the lithium-ion battery with the mass percentage of amorphous carbon, the mass percentage of metal oxide and lithiated metal oxide, the mass percentage of silicon grains and lithium silicate, the size of silicon grains, and the mass percentage of metal elements within the scope of the present application has low AC impedance, high rate performance and cycle capacity retention rate, and the expansion rate ratio of the negative electrode plate to the battery after 800 cycles is low, indicating that the lithium-ion battery provided in the present application has low AC impedance, good rate performance, cycle performance and expansion performance.

[0131] Table 3

[0132] The I1 / I2 value and the mass percentage of the silicon-oxygen composite material generally affect the performance of lithium-ion batteries, such as energy density, rate performance, cycle performance, and expansion performance. As can be seen from Examples 1-8 and Examples 2-1 to 2-6, lithium-ion batteries with I1 / I2 values ​​and the mass percentage of the silicon-oxygen composite material within the scope of this application have high energy density, rate performance, and cycle capacity retention, and low cycle expansion rate, indicating that the lithium-ion batteries provided by this application have high energy density while also having good rate performance, cycle performance, and expansion performance.

[0133] Figures 1 and 2 show the thermogravimetric (TG) curves and thermogravimetric first differential (DTG) curves of the negative electrode sheets of Examples 1-8 and Comparative Example 1, respectively. As can be seen from Figure 1, the DTG curves of the negative electrode sheets of Examples 1-8 of the present application have a peak intensity Y1 of -0.13% min at 587.9°C and a peak intensity Y2 of -0.15% min at 427.3°C. The calculated value of Y1 / Y2 is 0.87. In Figure 1, the peaks between 500°C and 700°C correspond to the decomposition of silicon-containing organic lithium salts, and the peaks between 350°C and 450°C correspond to the decomposition of silicon-free lithium salts. The value of Y1 / Y2 reflects the content ratio of silicon-containing organic lithium salts to silicon-free lithium salts. The higher the peak intensity, the higher the content of lithium salt corresponding to the peak. As can be seen from Figure 2, the DTG curve of the negative electrode sheet of Comparative Example 1 does not show an endothermic peak at 500°C to 700°C, indicating that the negative electrode sheet of Comparative Example 1 does not contain silicon-containing organic lithium salt, that is, Y1 is 0%min, and the peak intensity Y2 at 391.8°C between 350°C and 450°C is -0.24%min, corresponding to the decomposition of silicon-free lithium salt, and the calculated value of Y1 / Y2 is 0.

[0134] Figure 3 shows the TG curve and DTG curve of the negative electrode sheet of Example 2-5. As can be seen from Figure 3, the peak-to-peak intensity Y1 of the DTG curve of the negative electrode sheet of Example 2-5 at 594.8°C is -0.36%min, and the peak-to-peak intensity Y2 at 401.8°C is -0.10%min, so the value of Y1 / Y2 is 3.6.

[0135] Figure 4 shows the Raman spectra of the negative electrode sheets of Examples 1-8. The Raman spectra of the negative electrode sheets of Examples 1-8 are at 1342.1 cm -1 The peak intensity I1 at 421.9cm is 632.9. -1 The peak intensity I2 at is 111.2, and the calculated value of I1 / I2 is 5.69.

[0136] Figure 5 shows the Raman spectrum of the negative electrode sheet of Example 2-5. The Raman spectrum of the negative electrode sheet of Example 2-5 is at 1345.4 cm -1 The peak intensity I1 is 459.3 at 429.2cm -1 The peak-to-peak intensity I2 is 116.3, and the calculated I1 / I2 value is 3.95.

[0137] It should be noted that, in this document, relational terms such as first and second, etc., are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship or order between these entities or operations. Moreover, the terms "comprises," "comprising," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that includes a list of elements includes not only those elements but also other elements not explicitly listed, or elements inherent to such process, method, article, or apparatus.

[0138] Each embodiment in this specification is described in a related manner. The same or similar parts between the embodiments can be referred to each other. Each embodiment focuses on the differences from other embodiments.

[0139] The above description is only a preferred embodiment of the present application and is not intended to limit the scope of protection of the present application. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principles of the present application are included in the scope of protection of the present application.

Claims

1. A secondary battery, comprising a negative electrode plate, the negative electrode plate comprising a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector, the negative electrode active material layer comprising a negative electrode active material, and the negative electrode active material comprising a silicon-oxygen composite material; The peak intensity of the first differential curve of the thermogravimetric curve of the negative electrode sheet at 500°C to 700°C is Y 1 The peak intensity of the first differential curve of the thermogravimetric curve of the negative electrode sheet at 350°C to 450°C is Y 2 , 0.1≤Y 1 / Y 2 ≤4.

2. The secondary battery according to claim 1, in, 0.5≤Y 1 / AND 2 ≤2.5。 3. The secondary battery according to claim 1 or 2, in, The Raman spectrum of the negative electrode sheet is at 1200 cm -1 Up to 1500cm -1 The peak intensity is I 1 The Raman spectrum of the negative electrode is at 300 cm -1 Up to 600cm -1 The peak intensity is I 2 , 2≤I 1 / I 2 ≤15.

4. The secondary battery according to any one of claims 1 to 3, in, The Dv50 of the silicon-oxygen composite material is 3 μm to 15 μm; the specific surface area of ​​the silicon-oxygen composite material is 0.2 m 2 / g to 8m 2 / g.

5. The secondary battery according to any one of claims 1 to 4, in, The silicon-oxygen composite material is a core-shell structure, comprising a core and a first shell and a second shell disposed on at least a portion of the surface of the core; the core comprises silicon grains and lithium silicate, the first shell comprises amorphous carbon, and the second shell comprises metal oxide and lithiated metal oxide; The metal oxide includes at least one of aluminum oxide, titanium oxide or niobium pentoxide.

6. The secondary battery according to claim 5, in, Based on the mass of the silicon-oxygen composite material, the mass percentage of the amorphous carbon is 1% to 5%, the mass percentage of the metal oxide and the lithiated metal oxide is 1% to 5%, and the sum of the mass percentages of the silicon grains and the lithium silicate is 92% to 98%.

7. The secondary battery according to claim 5 or 6, in, The size of the silicon grains is 0.5 nm to 10 nm.

8. The secondary battery according to any one of claims 5 to 7, in, The second shell layer includes a metal element, and the metal element includes at least one of aluminum, titanium or niobium. Based on the mass of the second shell layer, the mass percentage of the metal element is 0.1% to 1%.

9. The secondary battery according to any one of claims 1 to 8, in, The negative electrode active material further comprises graphite. Based on the sum of the mass of the silicon-oxygen composite material and the graphite, the mass percentage of the silicon-oxygen composite material is 1% to 15%.

10. The secondary battery according to any one of claims 1 to 9, in, In a charge-discharge cycle test of the secondary battery at 25±1°C with 3C stage charge and 0.5C discharge, when the number of cycles of the secondary battery is greater than or equal to 800, the ratio of the expansion rate of the negative electrode plate to the expansion rate of the secondary battery is 0.5 to 4. 11 . An electronic device comprising the secondary battery according to claim 1 .

Citation Information

Patent Citations

  • Secondary battery and electronic device

    CN116344766A

  • Negative pole piece, electrochemical device comprising negative pole piece and electronic device comprising negative pole piece

    CN115148960A

  • Secondary battery and electric device

    CN115172705A

  • Secondary battery, and battery module, battery pack, and device including same

    CN115295791A

  • Negative pole piece, electrochemical device comprising negative pole piece and electronic device

    CN115332483A