Composite positive electrode active material, battery cell, battery and electric device
By using composite cathode active materials in the battery cells, combined with nanosheet and spherical lithium iron manganese phosphate materials, the problem of voltage drop of the battery cell cathode active materials is solved, and the battery energy density and performance are improved.
Patent Information
- Application Number
- PCT/CN2024/073989
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2024-01-25
- Publication Date
- 2024-10-03
AI Technical Summary
The voltage drop of the cathode active material of existing battery cells is large during use, making it difficult to increase the energy density of the battery.
Composite cathode active materials are used, including the first lithium manganese iron phosphate material and the second lithium manganese iron phosphate material. By blending nanosheet and spherical lithium iron manganese phosphate materials, the lithium ion diffusion distance and voltage platform are improved. Form a conductive network structure to increase the energy density of the battery.
The energy density and average discharge voltage of the battery cells are significantly increased, and the rate performance and low-temperature performance are improved.
Smart Images

Figure CN2024073989_03102024_PF_FP_ABST
Abstract
Description
Composite positive electrode active material, battery cell, battery and electrical device
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to Chinese patent application No. 202310300449.9, filed on March 24, 2023, entitled “Composite positive electrode active material, battery cell, battery and electrical device,” the entire contents of which are incorporated herein by reference. Technical Field
[0003] The present application relates to the field of batteries, and in particular to a composite positive electrode active material, a battery cell, a battery, and an electrical device. Background Art
[0004] Battery cells have the characteristics of high capacity and long life, and are therefore widely used in electronic devices such as mobile phones, laptops, electric vehicles, electric airplanes, electric boats, electric toy cars, electric toy boats, electric toy airplanes and power tools, etc.
[0005] As battery applications become increasingly widespread, the requirements for battery performance are becoming increasingly stringent. However, in related technologies, the voltage drop of the positive electrode active material in battery cells during use is too large, which is not conducive to improving the energy density of the battery cells.
[0006] Summary of the Invention
[0007] The present application is made in view of the above-mentioned problems, and its purpose is to provide a composite positive electrode active material, a battery cell, a battery and an electrical device.
[0008] A first aspect of the present application provides a composite positive electrode active material, which includes a first lithium iron manganese phosphate material and a second lithium iron manganese phosphate material, wherein the first lithium iron manganese phosphate material has a nanosheet structure, and the (010) crystal plane area of the first lithium iron manganese phosphate material accounts for A1% of the total crystal plane area of the first lithium iron manganese phosphate material; the second lithium iron manganese phosphate material has a spherical and / or quasi-spherical structure, and the (010) crystal plane area of the second lithium iron manganese phosphate material accounts for A2% of the total crystal plane area of the second lithium iron manganese phosphate material; the composite positive electrode active material satisfies: A1>A2.
[0009] Therefore, the nanosheet structure of the first lithium iron manganese phosphate material in the embodiment of the present application makes the area of the (010) crystal plane of the first lithium iron manganese phosphate material larger, and its capacity is close to the theoretical capacity; after the first lithium iron manganese phosphate material and the second lithium iron manganese phosphate material are mixed to form a composite positive electrode active material, the overall capacity of the composite positive electrode active material is improved, and the average discharge voltage is improved, thereby making it possible for the composite positive electrode active material to be used in a battery cell. The energy density of the battery cell is significantly improved.
[0010] In some embodiments, the unit cell parameter b-axis length of the first manganese iron phosphate lithium material is b1, and its unit is nm; the unit cell parameter b-axis length of the second manganese iron phosphate lithium material is b2, and its unit is nm, wherein b1<b2.
[0011] Therefore, the unit cell parameter b-axis of the first lithium iron manganese phosphate material in the embodiment of the present application is relatively short, which can further shorten the lithium ion diffusion distance, facilitate the rapid transmission of lithium ions, and improve the rate performance of the battery cell.
[0012] In some embodiments, b1<100; further optionally, 10≤b1≤80.
[0013] In some embodiments, b2>100; further optionally, 200≤b2≤800.
[0014] In some embodiments, the average voltage of the composite cathode active material is 3.55V to 3.81V.
[0015] In some embodiments, the composite positive electrode active material has a first discharge voltage platform U1 and a second discharge voltage platform U2, 4.0V≤U1<4.1V; and / or 3.4V≤U2≤3.6V.
[0016] Therefore, the second lithium iron manganese phosphate material of the embodiment of the present application has two voltage platforms, a manganese platform of 4.1V and an iron platform of 3.5V, due to the addition of manganese elements, and has a relatively high voltage platform compared to materials such as lithium iron phosphate; due to the mixed use of the first lithium iron manganese phosphate material and the second lithium iron manganese phosphate material, the composite positive electrode active material has a significant voltage increase, which can significantly improve the energy density of the composite positive electrode active material.
[0017] In some embodiments, the powder resistivity of the composite cathode active material is 1 Ω·cm to 500 Ω·cm.
[0018] In some embodiments, the powder compaction density of the composite cathode active material is 2.19 g / ml to 2.40 g / ml.
[0019] In some embodiments, the first lithium manganese iron phosphate material has an X-ray diffraction pattern having a characteristic peak I(020) and a characteristic peak I(200), and I(020) / I(200)>2.1.
[0020] In some embodiments, the X-ray diffraction (XRD) pattern of the second lithium manganese iron phosphate material has a characteristic peak I(020) and a characteristic peak I(200), and I(020) / I(200)≤2.1.
[0021] In some embodiments, the thickness of the first lithium iron manganese phosphate material is H, measured in nm, with 10 ≤ H ≤ 80. When the thickness of the first lithium iron manganese phosphate material is within the above range, the first lithium iron manganese phosphate material is distributed between particles of the second lithium iron manganese phosphate material, forming a conductive network structure, thereby improving the intrinsic resistance of the composite positive electrode active material and enhancing the powder conductivity.
[0022] In some embodiments, based on the total mass of the composite positive electrode active material, the mass percentage of the first lithium iron manganese phosphate material is B1%, the mass percentage of the second lithium iron manganese phosphate material is B2%, and 1≤B2 / B1≤19. When the mass percentages of the first lithium iron manganese phosphate material and the second lithium iron manganese phosphate material meet the above ranges, the discharge voltage platform of the composite positive electrode active material can be significantly increased, thereby increasing the energy density of the battery cell.
[0023] In some embodiments, the volume average particle size of the first lithium manganese iron phosphate material is D v50-1 , whose unit is nm; the volume average particle size of the second manganese iron phosphate lithium material is D v50-2 , whose unit is nm, where 1≤D v50-2 / D v50-1 ≤16; optionally, 2≤D v50-2 / D v50-1 ≤16;
[0024] Therefore, the embodiment of the present application prepares a composite material by mixing two lithium manganese iron phosphate particles with different particle sizes. The packing density between particles is improved through the gradation relationship between the particles, thereby enabling the composite material to have a relatively high compaction density and to improve the energy density of the battery cell.
[0025] In some embodiments, 50≤D v50-1 ≤300; and / or 200≤D v50-2 ≤800.
[0026] In some embodiments, the specific surface area of the first lithium manganese iron phosphate material is S1, and its unit is m 2 / g; the specific surface area of the second manganese iron phosphate lithium material is S2, and its unit is m 2 / g; wherein, 0.4≤S2 / S1<1.0.
[0027] Therefore, when the specific surface area of the first lithium iron manganese phosphate material and the specific surface area of the second lithium iron manganese phosphate material in the embodiment of the present application are within the above range, it is more conducive to the first lithium iron manganese phosphate material to form a connected conductive network structure, thereby improving the electronic powder conductivity and electronic powder conductivity of the composite positive electrode active material.
[0028] In some embodiments, 20≤S1≤50; and / or 8≤S2≤20.
[0029] In some embodiments, the first lithium iron manganese phosphate material and the second lithium iron manganese phosphate material each independently include a molecular formula of LiFe (1-x) Mn x PO4 compounds and modified compounds thereof, wherein 0.5≤x<1.
[0030] The second aspect of the present application further provides a battery cell, comprising a positive electrode plate, wherein the positive electrode plate comprises a composite positive electrode active material according to any embodiment of the first aspect of the present application.
[0031] The third aspect of the present application further provides a battery, comprising a battery cell according to any embodiment of the second aspect of the present application.
[0032] The fourth aspect of the present application further provides an electrical device comprising a battery according to any embodiment of the third aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the embodiments of the present application. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the drawings without creative work.
[0034] FIG1 is a schematic diagram of a battery cell according to an embodiment of the present application.
[0035] FIG. 2 is an exploded schematic diagram of an embodiment of the battery cell of FIG. 1 .
[0036] FIG3 is a schematic diagram of an embodiment of a battery module of the present application.
[0037] FIG4 is a schematic diagram of an embodiment of a battery pack of the present application.
[0038] FIG. 5 is an exploded schematic diagram of the embodiment of the battery pack shown in FIG. 4 .
[0039] FIG6 is a schematic diagram of an embodiment of an electric device including the battery cell of the present application as a power source.
[0040] FIG. 7 a is a scanning electron microscope (SEM) image of the first lithium manganese iron phosphate composite positive electrode active material in Example 1. FIG.
[0041] FIG7 b is a scanning electron microscope (SEM) image of the second lithium manganese iron phosphate composite positive electrode active material in Example 1. FIG.
[0042] FIG. 8 is a transmission electron microscope (TEM) image of the composite positive electrode active material of Example 1.
[0043] FIG. 9 is a scanning electron microscope (SEM) image of the composite positive electrode active material of Example 1.
[0044] FIG10 is a charge and discharge curve diagram of the composite positive electrode active material of Example 1 and Comparative Example 1.
[0045] The drawings are not necessarily drawn to scale.
[0046] The following are the descriptions of the reference numerals:
[0047] 1. Battery pack; 2. Upper box; 3. Lower box; 4. Battery module;
[0048] 5. Battery cell; 51. Housing; 52. Electrode assembly;
[0049] 53. Cover plate;
[0050] 6. Electrical equipment. DETAILED DESCRIPTION
[0051] The following detailed description specifically discloses the embodiments of the composite positive electrode active material, battery cell, battery and electrical device of the present application. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there may be cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0052] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0053] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution. Unless otherwise specified, all technical features and optional technical features of the present application can be combined with each other to form a new technical solution.
[0054] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, a method includes steps (a) and (b), which indicates that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, a method may further include step (c), which indicates that step (c) may be added to the method in any order, for example, the method may include steps (a), (b), and (c), or may include steps (a), (c), and (b), or may include steps (c), (a), and (b), etc.
[0055] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may indicate that other components not listed may also be included or that only the listed components are included.
[0056] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0057] In this application, the terms "plurality" and "multiple" refer to two or more.
[0058] Polyanionic compounds are a series of compounds containing tetrahedral or octahedral anion structural units. The crystal framework structure of this type of compound is stable and can maintain a stable structure even if a large number of lithium ions are intercalated or deintercalated. For example, when lithium ions are intercalated or deintercalated in the positive electrode material, the structural rearrangement of the material is very small. In addition, the discharge potential platform of the material can be adjusted by configuring different chemical elements.
[0059] Polyanionic compounds include lithium iron phosphate, lithium manganese phosphate, lithium manganese iron phosphate, etc. Among them, lithium manganese iron phosphate combines the excellent properties of lithium iron phosphate and lithium manganese phosphate, with stable chemical properties and high safety performance; its crystal structure is an orthorhombic olivine crystal structure, the material has good thermal stability and low oxidizability. In order to improve the performance of the material, in related technologies, by compounding materials of different particle sizes, or even compounding polyanionic compounds and ternary materials, etc., although the above methods can complement each other and improve the physical parameters of the materials, they have little effect on the electrochemical and intrinsic properties of the materials, and the voltage drop of lithium manganese iron phosphate is still too large, resulting in a low energy density of the battery cell when it is used in the battery cell.
[0060] In view of the above problems, an embodiment of the present application proposes a composite positive electrode active material, which includes two types of mixed lithium manganese iron phosphate materials, especially one of the lithium manganese iron phosphate materials is a material with an exposed (010) crystal plane. The capacity of this type of material is close to the theoretical capacity, and can significantly improve the average discharge voltage of lithium manganese iron phosphate, thereby improving the energy density of the battery cell.
[0061] Composite positive electrode active materials
[0062] In the first aspect, the present application proposes a composite positive electrode active material, which includes a first lithium iron manganese phosphate material and a second lithium iron manganese phosphate material; the first lithium iron manganese phosphate material has a nanosheet structure, and the (010) crystal plane area of the first lithium iron manganese phosphate material accounts for A1% of the total crystal plane area of the first lithium iron manganese phosphate material; the second lithium iron manganese phosphate material has a spherical and / or quasi-spherical structure, and the (010) crystal plane area of the second lithium iron manganese phosphate material accounts for A2% of the total crystal plane area of the second lithium iron manganese phosphate material; the composite positive electrode active material satisfies: A1>A2.
[0063] The second lithium manganese iron phosphate material is a spherical and / or quasi-spherical material. This type of material can be secondary particles composed of agglomerates of primary particles, or primary particles, or a mixture of primary particles and secondary particles.
[0064] The first lithium iron manganese phosphate material has a nanosheet structure, which can be understood as a material with a thickness much smaller than its length or width. It can be in the form of one or more triangular flakes, square flakes, or hexagonal flakes. Due to the nanosheet structure of the first lithium iron manganese phosphate material, the (010) crystal plane of the first lithium iron manganese phosphate material is relatively large, and its capacity approaches the theoretical capacity. After the first lithium iron manganese phosphate material and the second lithium iron manganese phosphate material are blended to form a composite positive electrode active material, the overall capacity of the composite positive electrode active material is increased, and the average discharge voltage is also increased. As a result, when the composite positive electrode active material is used in a battery cell, the energy density of the battery cell is significantly improved.
[0065] In some embodiments, 40≤A1≤80. Alternatively, 40≤A1≤74. For example, the ratio of the (010) crystal plane area of the first manganese iron phosphate lithium-based material to the total crystal plane area of the first manganese iron phosphate lithium-based material may be 40%, 42%, 45%, 48%, 50%, 52%, 55%, 58%, 60%, 65%, 70%, 74%, 75%, 80%, or a range consisting of any two of the above values.
[0066] In some embodiments, 20≤A2≤40. Alternatively, 31≤A2≤38. The (010) crystal plane area of the second manganese iron phosphate lithium-based material relative to the total crystal plane area of the second manganese iron phosphate lithium-based material may be 20%, 22%, 25%, 28%, 30%, 31%, 32%, 35%, 38%, 40%, or a range consisting of any two of the foregoing values.
[0067] During the spontaneous growth process, a crystal can develop a polyhedral shape composed of planes of different orientations. The planes in the polyhedral shape are called crystal faces. Crystal faces refer to planes formed by any three lattice points in the crystal structure that are not on the same straight line, representing the direction of the atomic planes in the crystal. A coordinate system (crystal axis system) is determined in the crystal. The crystal axis system has three crystal axes that intersect at the center of the crystal, namely the a-axis, the b-axis and the c-axis. The exposed crystal face refers to the crystal face composed of atoms on the surface of the material, and can also be considered as the crystal face in contact with the external environment. In this application, the largest surface of the particle is used as the observation point, and the lattice spacing is measured by high-resolution transmission electron microscopy (TEM). The (200) and (002) crystal faces can be determined based on the lattice spacing. After the two crystal faces are confirmed, the one perpendicular to these two crystal faces is the (010) crystal face.
[0068] Of course, the embodiment of the present application can also use an X-ray powder diffractometer to determine the crystal structure of the composite positive electrode active material, for example, using a Brucker D8A_A25 X-ray diffractometer from BruckerAxS of Germany, with CuKα rays as the radiation source, the ray wavelength scanning 2θ angle range of 10° to 90°, and the scanning rate of 4° / min.
[0069] During the charge and discharge process of the battery cell, lithium ions are transmitted one-dimensionally along the (010) crystal plane, that is, the b-axis direction, and charge transfer mainly occurs on the (010) crystal plane. The main exposed crystal plane of the first lithium iron manganese phosphate material of the present application is the (010) crystal plane. The first lithium iron manganese phosphate material is used in combination with the second lithium iron manganese phosphate material to reduce the internal resistance of the composite positive electrode active material, improve the ion powder conductivity and electronic powder conductivity of the composite positive electrode active material, reduce the intrinsic resistance, and improve the low temperature performance and rate performance of the battery cell.
[0070] In some embodiments, the first lithium iron manganese phosphate-based material has a unit cell parameter b-axis length of b1, measured in nm; the second lithium iron manganese phosphate-based material has a unit cell parameter b-axis length of b2, measured in nm, where b1 < b2. The first lithium iron manganese phosphate-based material has a relatively short unit cell parameter b-axis, which can further shorten the lithium ion diffusion distance, facilitate rapid lithium ion transport, and improve the rate performance of the battery cell.
[0071] In some embodiments, b1<100. Optionally, 10≤b1≤80. For example, the unit cell parameter b-axis length of the first lithium manganese iron phosphate material can be 5 nm, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 85 nm, or a range consisting of any two of the above values.
[0072] In some embodiments, b2>100. Optionally, 200≤b2≤800. For example, the unit cell parameter b-axis length of the second lithium manganese iron phosphate material can be 110nm, 120nm, 150nm, 180nm, 200nm, 250nm, 300nm, 400nm, 450nm, 500nm, 600nm, 700nm, 800nm, 850nm, or a range consisting of any two of the above values.
[0073] In some embodiments, the average voltage of the composite positive electrode active material is 3.55 V to 3.81 V, and the average voltage of the composite positive electrode active material is significantly improved. For example, the average voltage of the composite positive electrode active material can be 3.55 V, 3.60 V, 3.65 V, 3.70 V, 3.75 V, 3.80 V, 3.81 V, or a range consisting of any two of the foregoing values.
[0074] In the embodiment of the present application, the average voltage of the composite positive electrode active material is the ratio of the discharge energy density to the specific capacity of the battery cell using the composite positive electrode active material, for example, the above value is obtained by a charge and discharge test at a 0.1C rate.
[0075] In some embodiments, the composite positive electrode active material has a first discharge voltage platform U1 and a second discharge voltage platform U2, 4.0V≤U1<4.1V; and / or 3.4V≤U2≤3.6V. For example, U1 can be 4.0V, 4.02V, 4.05V, 4.08V, 4.09V, 4.091V, 4.095V, 4.099V, or a range consisting of any two of the above values. U2 can be 3.40V, 3.42V, 3.45V, 3.48V, 3.49V, 3.50V, 3.51V, 3.52V, 3.53V, 3.55V, 3.58V, 3.60V, or a range consisting of any two of the above values.
[0076] The second lithium iron manganese phosphate material has two voltage platforms, the manganese platform and the iron platform, due to the addition of manganese elements. Compared with materials such as lithium iron phosphate, it has a relatively high voltage platform; due to the mixed use of the first lithium iron manganese phosphate material and the second lithium iron manganese phosphate material, the composite positive electrode active material has a significant voltage increase, and has an ideal voltage platform of 4.1V close to manganese, which can significantly improve the energy density of the composite positive electrode active material.
[0077] In the embodiment of the present application, the discharge voltage platform has a meaning well known in the art and can be detected using methods and equipment well known in the art. For example, a charge and discharge curve is obtained by a 0.1C rate charge and discharge test, and the discharge curve has a first discharge voltage platform and a second discharge voltage platform.
[0078] In some embodiments, the powder resistivity of the composite positive electrode active material is 1 Ω·cm to 500 Ω·cm. Alternatively, the powder resistivity is 5 Ω·cm to 480 Ω·cm. Illustratively, the powder resistivity of the composite positive electrode active material may be 1 Ω·cm, 5 Ω·cm, 10 Ω·cm, 15 Ω·cm, 16 Ω·cm, 20 Ω·cm, 28 Ω·cm, 30 Ω·cm, 40 Ω·cm, 43 Ω·cm, 50 Ω·cm, 60 Ω·cm, 68 Ω·cm, 80 Ω·cm, 100 Ω·cm, 102 Ω·cm, 120 Ω·cm, 150 Ω·cm, 160 Ω·cm, 180 Ω·cm, 200 Ω·cm, 250 Ω·cm, 280 Ω·cm, 300 Ω·cm, 313 Ω·cm, 320 Ω·cm, 350 Ω·cm, 400 Ω·cm, 450 Ω·cm, 500 Ω·cm, or a range consisting of any two of the above values.
[0079] In the embodiments of the present application, the powder resistivity of the composite positive electrode active material has a well-known meaning in the art and can be measured using instruments and methods well-known in the art, such as a four-probe instrument.
[0080] In some embodiments, the powder compaction density of the composite cathode active material is 2.19 g / ml to 2.40 g / ml. For example, the powder compaction density of the composite cathode active material can be 2.19 g / ml, 2.20 g / ml, 2.22 g / ml, 2.25 g / ml, 2.30 g / ml, 2.35 g / ml, 2.38 g / ml, 2.40 g / ml, or a range consisting of any two of the foregoing values. When the powder compaction density of the composite cathode active material is within the above range, it is beneficial to improve the energy density.
[0081] In some embodiments, the X-ray diffraction (XRD) pattern of the first lithium manganese iron phosphate material has a characteristic peak I(020) and a characteristic peak I(200), and I(020) / I(200)>2.1.
[0082] The X-ray diffraction (XRD) pattern of the second lithium manganese iron phosphate material has a characteristic peak I(020) and a characteristic peak I(200), and I(020) / I(200)≤2.1.
[0083] In some embodiments, the first lithium manganese iron phosphate-based material has a nanosheet structure, and the thickness of the first lithium manganese iron phosphate-based material is H, in nm, where 10≤H≤80. For example, the thickness of the first lithium manganese iron phosphate-based material can be 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, or a range consisting of any two of the foregoing values.
[0084] When the thickness of the first lithium manganese iron phosphate material is within the above range, it is beneficial for the first lithium manganese iron phosphate material to be distributed between the particles of the second lithium manganese iron phosphate material to form a conductive network structure, which can improve the intrinsic resistance of the composite positive electrode active material and improve the powder conductivity.
[0085] In the embodiment of the present application, the thickness of the material has a meaning well known in the art and can be tested using instruments and methods well known in the art; for example, a certain amount of the above-mentioned composite positive electrode active material is taken, and then the material is subjected to a transmission electron microscope TEM analysis test to obtain a TEM image, and then the thickness of multiple (for example, more than 30) particles is measured on the TEM image, and the average value is taken as the average thickness of the material.
[0086] In some embodiments, based on the total mass of the composite positive electrode active material, the mass percentage of the first lithium iron manganese phosphate material is B1%, the mass percentage of the second lithium iron manganese phosphate material is B2%, and 1≤B2 / B1≤19. When the mass percentages of the first lithium iron manganese phosphate material and the second lithium iron manganese phosphate material meet the above ranges, the discharge voltage platform of the composite positive electrode active material can be significantly improved, thereby increasing the energy density of the battery cell. For example, the mass percentage ratio B2 / B1 of the second lithium iron manganese phosphate material to the first lithium iron manganese phosphate material can be 1, 2, 5, 6, 7, 8, 10, 12, 14, 15, 16, 17, 18, 19, or a range consisting of any two of the above values.
[0087] In some embodiments, 5≤B1≤50; alternatively, 10≤B1≤30. For example, the mass percentage B1% of the first lithium manganese iron phosphate material may be 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, or a range consisting of any two of the above values.
[0088] In some embodiments, 50≤B2≤95; alternatively, 70≤B2≤90. For example, the mass percentage B2% of the second lithium manganese iron phosphate material may be 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, or a range consisting of any two of the foregoing values.
[0089] In some embodiments, the volume average particle size of the first lithium manganese iron phosphate material is D v50-1 , whose unit is nm; the volume average particle size of the second manganese iron phosphate lithium material is D v50-2 , its unit is nm; 1≤D v50-2 / D v50-1 ≤16; optionally, 2≤D v50-2 / D v50-1≤16. For example, D v50-2 / D v50-1 It can be 1, 1.2, 1.5, 2.0, 2.5, 3.0, 4.0, 5.0, 6.0, 8.0, 10.0, 11, 12, 15, 16, or a range consisting of any two of the above values.
[0090] In the embodiment of the present application, a composite material is prepared by mixing lithium manganese iron phosphate particles of two different particle sizes. The packing density between particles is improved by the gradation relationship between the particles, thereby enabling the composite material to have a relatively high compaction density and to improve the energy density of the battery cell.
[0091] The second lithium iron manganese phosphate material is in the form of spherical and / or quasi-spherical particles with a relatively large particle size and interspheric spaces between the particles. The first lithium iron manganese phosphate material, which has a relatively small particle size, is filled within the pores of the second lithium iron manganese phosphate material. This can be understood as the first lithium iron manganese phosphate material being evenly distributed on the surface of the second lithium iron manganese phosphate material. The first lithium iron manganese phosphate materials are interconnected to form a three-dimensional conductive network structure, thereby reducing the intrinsic resistance of the composite positive electrode active material and increasing the overall ionic and electronic powder conductivity of the composite positive electrode active material, thereby improving the low-temperature performance and rate performance of the battery cell.
[0092] In some embodiments, 50≤D v50-1 ≤300. For example, the volume average particle size of the first lithium manganese iron phosphate material may be 50 nm, 80 nm, 100 nm, 150 nm, 180 nm, 200 nm, 250 nm, 300 nm, or a range consisting of any two of the above values.
[0093] In some embodiments, 200≤D v50-2 ≤800. For example, the volume average particle size of the second lithium manganese iron phosphate material can be 200 nm, 230 nm, 250 nm, 300 nm, 400 nm, 450 nm, 500 nm, 550 nm, 600 nm, 650 nm, 700 nm, 800 nm, or a range consisting of any two of the above values.
[0094] In this application, the volume average particle size Dv50 of a material is generally known in the art and represents the particle size corresponding to 50% of the cumulative volume distribution percentage of the material. This can be measured using instruments and methods known in the art. For example, it can be conveniently measured using a laser particle size analyzer, such as the Mastersizer 2000E laser particle size analyzer from Malvern Instruments Ltd. in the United Kingdom, in accordance with GB / T 19077-2016 Particle Size Distribution Laser Diffraction Method.
[0095] In some embodiments, the specific surface area of the first lithium manganese iron phosphate material is S1, and its unit is m 2 / g; the specific surface area of the second manganese iron phosphate lithium material is S2, and its unit is m 2 / g; 0.4≤S2 / S1<1.0. For example, S2 / S1 can be 0.4, 0.6, 0.7, 0.8, 0.9 or a range consisting of any two of the above values.
[0096] When the specific surface area of the first lithium manganese iron phosphate material and the specific surface area of the second lithium manganese iron phosphate material are within the above range, it is more conducive to the first lithium manganese iron phosphate material to form a connected conductive network structure, thereby improving the electronic powder conductivity and electronic powder conductivity of the composite positive electrode active material.
[0097] In some embodiments, 20≤S1≤50. Alternatively, 22≤S1≤35. For example, the specific surface area of the first lithium manganese iron phosphate material may be 20m 2 / g, 25m 2 / g、30m 2 / g, 40m 2 / g, 50m 2 / g or a range consisting of any two of the above values.
[0098] In some embodiments, 8≤S2≤20. For example, the specific surface area of the second lithium manganese iron phosphate material can be 8m 2 / g、10m 2 / g、15m 2 / g、18m 2 / g, 20m 2 / g or a range consisting of any two of the above values.
[0099] In this application, the specific surface area of a material has a meaning well known in the art and can be tested using instruments and methods well known in the art. For example, it can be tested using a nitrogen adsorption specific surface area analysis test method and calculated using the BET (Brunauer Emmett Teller) method, wherein the nitrogen adsorption specific surface area analysis test can be performed using a NOVA2000e specific surface area and pore size analyzer from Quantachrome Inc., USA.
[0100] In some embodiments, the first lithium iron manganese phosphate material and the second lithium iron manganese phosphate material each independently include a molecular formula of LiFe (1-x) Mn x PO4 compounds and modified compounds thereof, wherein 0.5≤x<1. In the present application, modification refers to doping modification or coating modification of the material.
[0101] For example, the first lithium manganese iron phosphate material includes LiFe 0.5 Mn 0.5 PO4、LiFe 0.4 Mn 0.6 PO4、LiFe 0.3 Mn 0.7 PO4 and LiFe 0.2 Mn 0.8 One or more of PO4.
[0102] For example, the second lithium manganese iron phosphate material includes LiFe 0.5 Mn 0.5 PO4、LiFe 0.4 Mn 0.6 PO4、LiFe 0.3 Mn 0.7 PO4 and LiFe 0.2 Mn 0.8 One or more of PO4.
[0103] battery cells
[0104] In a second aspect, an embodiment of the present application further provides a battery cell.
[0105] A battery cell, also known as a rechargeable battery or storage battery, is a battery that can be recharged after discharge to activate the active materials and continue to be used. Typically, a battery cell includes an electrode assembly and an electrolyte. The electrode assembly includes a positive electrode sheet, a negative electrode sheet, and a separator. The separator is placed between the positive and negative electrode sheets to prevent short circuits between the positive and negative electrodes while allowing active ions, such as lithium ions, to pass through.
[0106] The battery cell of the embodiment of the present application includes a positive electrode sheet, which includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, wherein the positive electrode film layer includes the composite positive electrode active material of the first aspect of the embodiment of the present application. As a result, the battery cell of the present application can improve energy density.
[0107] [Positive electrode]
[0108] In some embodiments, the positive electrode current collector has two opposite surfaces in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive electrode current collector.
[0109] In some embodiments, the positive electrode film layer may further optionally include a positive electrode conductive agent. The present application does not particularly limit the type of the positive electrode conductive agent. By way of example, the positive electrode conductive agent may include at least one of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. In some embodiments, the mass percentage of the positive electrode conductive agent is ≤5 wt % based on the total weight of the positive electrode film layer.
[0110] In some embodiments, the positive electrode film layer may further optionally include a positive electrode binder. The present application does not particularly limit the type of positive electrode binder. As an example, the positive electrode binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylic resin. In some embodiments, based on the total weight of the positive electrode film layer, the mass percentage of the positive electrode binder is ≤5wt%.
[0111] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, aluminum foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include at least one of aluminum, an aluminum alloy, nickel, a nickel alloy, titanium, a titanium alloy, silver, and a silver alloy. As an example, the polymer material base layer may include at least one of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).
[0112] The positive electrode film layer is usually formed by coating the positive electrode slurry on the positive electrode current collector, drying and cold pressing. The positive electrode slurry is usually formed by dispersing the composite positive electrode active material, optional conductive agent, optional binder and any other components in a solvent and stirring them evenly. The solvent can be N-methylpyrrolidone (NMP), but is not limited to this. In some embodiments, the first manganese iron phosphate lithium material and the second manganese iron phosphate lithium material can be mixed in proportion in advance, and then the optional conductive agent, optional binder and any other components are added and dispersed in the solvent and stirred evenly.
[0113] [Negative electrode]
[0114] The battery cell also includes a negative electrode plate.
[0115] In some embodiments, the negative electrode sheet includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector and comprising a negative electrode active material. For example, the negative electrode current collector has two opposing surfaces in the thickness direction of the negative electrode current collector, and the negative electrode film layer is disposed on either or both of the two opposing surfaces of the negative electrode current collector.
[0116] The negative electrode active material can be any negative electrode active material known in the art for use in battery cells. For example, the negative electrode active material may include, but is not limited to, at least one of natural graphite, artificial graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate. Silicon-based materials may include at least one of elemental silicon, silicon oxide, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. Tin-based materials may include at least one of elemental tin, tin oxide, and tin alloys.
[0117] In some embodiments, the negative electrode film layer may further optionally include a negative electrode conductive agent. The present application does not particularly limit the type of negative electrode conductive agent. For example, the negative electrode conductive agent may include at least one of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. In some embodiments, the mass percentage of the negative electrode conductive agent is ≤5 wt % based on the total weight of the negative electrode film layer.
[0118] In some embodiments, the negative electrode film layer may further optionally include a negative electrode binder. The present application does not particularly limit the type of negative electrode binder. For example, the negative electrode binder may include at least one of styrene-butadiene rubber (SBR), a water-soluble unsaturated resin SR-1B, a water-based acrylic resin (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), and carboxymethyl chitosan (CMCS). In some embodiments, the mass percentage of the negative electrode binder is ≤5 wt% based on the total weight of the negative electrode film layer.
[0119] In some embodiments, the negative electrode film layer may optionally include other additives. For example, the other additives may include a thickener, such as sodium carboxymethyl cellulose (CMC), a PTC thermistor material, or the like. In some embodiments, the weight percentage of the other additives is ≤ 2 wt % based on the total weight of the negative electrode film layer.
[0120] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, copper foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include at least one of copper, a copper alloy, nickel, a nickel alloy, titanium, a titanium alloy, silver, and a silver alloy. As an example, the polymer material base layer may include at least one of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).
[0121] The negative electrode film layer is typically formed by coating the negative electrode slurry onto the negative electrode current collector, drying it, and cold pressing it. The negative electrode slurry is typically formed by dispersing the negative electrode active material, an optional conductive agent, an optional binder, and other optional additives in a solvent and stirring them uniformly. The solvent can be, but is not limited to, N-methylpyrrolidone (NMP) or deionized water.
[0122] The negative electrode plate does not exclude other additional functional layers in addition to the negative electrode film layer. For example, in some embodiments, the negative electrode plate of the present application further includes a conductive primer layer (e.g., composed of a conductive agent and a binder) sandwiched between the negative electrode current collector and the negative electrode film layer and disposed on the surface of the negative electrode current collector. In other embodiments, the negative electrode plate of the present application further includes a protective layer covering the surface of the negative electrode film layer.
[0123] [Electrolyte]
[0124] The battery cells also include an electrolyte.
[0125] During the charge and discharge process of a battery cell, active ions are embedded and released back and forth between the positive and negative electrodes, and the electrolyte conducts the active ions between the positive and negative electrodes. This application does not specifically limit the type of electrolyte, and it can be selected according to actual needs.
[0126] The electrolyte solution includes an electrolyte salt and a solvent. The types of the electrolyte salt and the solvent are not particularly limited and can be selected according to actual needs.
[0127] As an example, the electrolyte salt may include, but is not limited to, at least one of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bisfluorosulfonyl imide (LiFSI), lithium bistrifluoromethanesulfonyl imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium bisoxalatoborate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobisoxalatophosphate (LiDFOP) and lithium tetrafluorooxalatophosphate (LiTFOP).
[0128] As an example, the solvent may include, but is not limited to, at least one of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS), and diethyl sulfone (ESE).
[0129] In some embodiments, the electrolyte may optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, or additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high-temperature performance, and additives that improve battery low-temperature power performance.
[0130] [Isolation film]
[0131] The battery cell also includes a separator.
[0132] In some embodiments, the battery cell further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.
[0133] In some embodiments, the material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0134] In some embodiments, the positive electrode sheet, the separator, and the negative electrode sheet may be formed into an electrode assembly through a winding process and / or a lamination process.
[0135] In some embodiments, the battery cell may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.
[0136] In some embodiments, the outer packaging of the battery cell can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the battery cell can also be a soft shell, such as a bag-type soft shell. The soft shell can be made of plastic, such as at least one of polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS).
[0137] The present application has no particular limitation on the shape of the battery cell, which can be cylindrical, square or any other shape. FIG1 shows a battery cell 5 of a square structure as an example.
[0138] In some embodiments, as shown in FIG2 , the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 is used to cover the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the separator may be formed into an electrode assembly 52 through a winding process and / or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is impregnated in the electrode assembly 52. The number of electrode assemblies 52 contained in the battery cell 5 may be one or more, which can be adjusted according to demand.
[0139] The preparation method of the battery cell of the present application is well known. In some embodiments, a positive electrode sheet, a separator, a negative electrode sheet, and an electrolyte can be assembled to form a battery cell. As an example, the positive electrode sheet, separator, and negative electrode sheet can be wound and / or laminated to form an electrode assembly. The electrode assembly is placed in an outer packaging, dried, and then injected with electrolyte. The battery cell is then vacuum packaged, allowed to stand, formed, and shaped.
[0140] In some embodiments of the present application, the battery cells according to the present application can be assembled into a battery module. The battery module can contain multiple battery cells, and the specific number can be adjusted according to the application and capacity of the battery module.
[0141] Figure 3 is a schematic diagram of an exemplary battery module 4. As shown in Figure 3 , within the battery module 4, multiple battery cells 5 may be arranged sequentially along the length of the battery module 4. Of course, any other arrangement is also possible. Furthermore, the multiple battery cells 5 may be secured together using fasteners.
[0142] Optionally, the battery module 4 may further include a housing having an accommodation space, and the plurality of battery cells 5 are accommodated in the accommodation space.
[0143] In some embodiments, the battery modules described above may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.
[0144] Figures 4 and 5 are schematic diagrams of an exemplary battery pack 1. As shown in Figures 4 and 5, the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 covers the lower case 3 and forms an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.
[0145] In the embodiment of the present application, the battery may include one or more battery cells. In the case where the battery includes a plurality of battery cells, the battery may include a battery module or a battery pack.
[0146] Electrical devices
[0147] The embodiments of the present application also provide an electric device, which includes at least one of the battery cells, battery modules, or battery packs of the present application. The battery cells, battery modules, or battery packs can be used as a power source for the electric device, and can also be used as an energy storage unit for the electric device. The electric device can be, but is not limited to, a mobile device (such as a mobile phone, a laptop computer, etc.), an electric vehicle (such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship, a satellite, an energy storage system, etc.
[0148] The electrical device may select a battery cell, a battery module or a battery pack according to its usage requirements.
[0149] Figure 6 is a schematic diagram of an exemplary electric device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of this device, a battery pack or battery module may be used.
[0150] As another example, an electric device may be a mobile phone, a tablet computer, a laptop computer, etc. Such an electric device is usually required to be lightweight and thin, and may use a battery cell as a power source.
[0151] Example
[0152] The following examples describe the present disclosure in more detail. These examples are intended to be illustrative only, as various modifications and variations within the scope of the present disclosure will be apparent to those skilled in the art. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are by mass, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing. The instruments used in the examples are commercially available.
[0153] Example 1
[0154] Preparation of lithium-ion batteries
[0155] 1. Preparation of positive electrode sheet
[0156] Aluminum foil with a thickness of 12 μm was used as the positive electrode current collector.
[0157] The positive electrode active material, the conductive agent carbon black, and the binder polyvinylidene fluoride (PVDF) are fully stirred and mixed in an appropriate amount of solvent NMP in a weight ratio of 97.5:1.4:1.1 to form a uniform positive electrode slurry; the positive electrode slurry is evenly coated on the surface of the positive electrode current collector aluminum foil, and after drying and cold pressing, a positive electrode sheet is obtained.
[0158] 2. Preparation of negative electrode sheet
[0159] A copper foil with a thickness of 8 μm was used as the negative electrode current collector.
[0160] The negative electrode active material graphite, binder styrene-butadiene rubber (SBR), thickener sodium carboxymethyl cellulose (CMC-Na), and conductive agent carbon black (Super P) are fully stirred and mixed in an appropriate amount of solvent deionized water in a weight ratio of 96.2:1.8:1.2:0.8 to form a uniform negative electrode slurry; the negative electrode slurry is evenly coated on the surface of the negative electrode current collector copper foil, and after drying and cold pressing, a negative electrode sheet is obtained.
[0161] 3. Isolation film
[0162] A porous polyethylene (PE) film is used as the separator.
[0163] 4. Preparation of electrolyte
[0164] In an environment with a water content of less than 10 ppm, non-aqueous organic solvents ethylene carbonate EC and diethyl carbonate DMC are mixed in a volume ratio of 1:1 to obtain an electrolyte solvent, and then lithium salt lithium hexafluorophosphate and the mixed solvent are mixed to prepare an electrolyte with a lithium salt concentration of 1 mol / L.
[0165] 5. Preparation of lithium-ion batteries
[0166] The positive electrode sheet, separator, and negative electrode sheet are stacked in order, with the separator placed between the positive electrode sheet and the negative electrode sheet to serve as an isolation, and then wound to obtain an electrode assembly; the electrode assembly is placed in an outer packaging shell, dried, and then injected with electrolyte, and after vacuum packaging, standing, forming, shaping and other processes, a lithium-ion battery is obtained.
[0167] Comparative Example 1
[0168] Comparative Example 1 was prepared by a method similar to that of Example 1. The difference from Example 1 was that the positive electrode active material of Comparative Example 1 was LiFe 0.4 Mn0.6 PO4, which is a spherical particle.
[0169] Comparative Example 2
[0170] Comparative Example 1 was prepared by a method similar to that of Example 1. The difference from Example 1 was that the positive electrode active material of Comparative Example 2 was LiFe 0.4 Mn 0.6 PO4 and spherical LiFe 0.4 Mn 0.6 PO4, and A1=A2, the volume average particle sizes of the two materials are different.
[0171] Example 2-1 to Example 2-4
[0172] Comparative Example 1 was prepared using a method similar to Example 1. Unlike Example 1, Examples 2-1 to 2-4 adjusted the mass percentage ratio of the first lithium iron manganese phosphate material and the second lithium iron manganese phosphate material.
[0173] Example 3-1 to Example 3-6
[0174] Comparative Example 1 was prepared by a method similar to Example 1. Unlike Example 1, the volume average particle size ratio of the first lithium manganese iron phosphate material and the second lithium manganese iron phosphate material was adjusted in Examples 3-1 to 3-6.
[0175] Example 4-1 and Example 4-2
[0176] Comparative Example 1 was prepared by a method similar to Example 1. Unlike Example 1, the molecular formulas of the first lithium iron manganese phosphate material and the second lithium iron manganese phosphate material were adjusted in Examples 4-1 and 4-2.
[0177] The data of the examples and comparative examples are shown in Table 1.
[0178] Test section
[0179] 1. Powder compaction density of composite positive electrode active material
[0180] Take a certain amount of the above composite positive electrode active material sample and add it to the bottom area of 1.327cm of UTM7305 electronic pressure testing machine. 2 In a mold, pressurize to 2000 kg (equivalent to 20,000 N), maintain pressure for 30 seconds, then release the pressure and maintain for 10 seconds. The powder compaction density of the composite positive electrode active material under a force of 20,000 N is recorded and calculated. The test standard is in accordance with GB / T24533-2009.
[0181] 2. Average voltage of battery cells
[0182] A button-type half-cell was formed by a positive electrode sheet per unit area and a lithium metal sheet per unit area, wherein the electrolyte composition adopted the electrolyte composition of the embodiment, and the battery was fully charged at a 0.1C rate. A 0.1C rate charge and discharge test was performed, and the discharge energy density / specific capacity was the average voltage.
[0183] Test results
[0184] The test results are shown in Table 1.
[0185] Table 1
[0186] In Table 1, the molecular formula 64 represents LiFe 0.4 Mn 0.6 PO4; molecular formula 73 represents LiFe 0.3 Mn 0.7 PO4; molecular formula 55 represents LiFe 0.5 Mn 0.5 PO4.
[0187] As shown in Table 1, Comparative Example 1 uses spherical lithium manganese iron phosphate material as the positive electrode active material. Compared with Comparative Example 1, Comparative Example 2 additionally adds smaller particles of nano-spherical lithium manganese iron phosphate material, which can improve the average voltage to a certain extent, but the improvement effect is very small.
[0188] As can be seen from Figures 7a to 9, the first lithium iron manganese phosphate material in Example 1 has a flaky nanostructure, while the second lithium iron manganese phosphate material has a spherical structure. The composite positive electrode active material formed by mixing the two is a blend of the two. As can be seen from Figure 10, both discharge platform 1 (corresponding to the first discharge voltage platform) and discharge platform 2 (corresponding to the second discharge voltage platform) of Example 1 have been significantly improved.
[0189] It can be seen that the embodiment of the present application adds a lithium manganese iron phosphate material with a (010) crystal plane exposed. The capacity of this type of material is close to the theoretical capacity, which can significantly improve the average discharge voltage of the lithium manganese iron phosphate.
[0190] Although this application has been described with reference to preferred embodiments, various modifications may be made thereto and components may be substituted with equivalents without departing from the scope of this application. In particular, the various technical features described in the various embodiments may be combined in any manner, provided there are no structural conflicts. This application is not limited to the specific embodiments disclosed herein, but encompasses all technical solutions within the scope of the claims.
Claims
1. A composite positive electrode active material comprising: The first lithium manganese iron phosphate material has a nano-sheet structure, and the (010) crystal plane area of the first lithium manganese iron phosphate material accounts for A1% of the total crystal plane area of the first lithium manganese iron phosphate material; and The second lithium iron manganese phosphate material has a spherical and / or quasi-spherical structure, and the (010) crystal plane area of the second lithium iron manganese phosphate material accounts for A2% of the total crystal plane area of the second lithium iron manganese phosphate material; The composite positive electrode active material satisfies: A1>A2.
2. The composite positive electrode active material according to claim 1, wherein The unit cell parameter b axis length of the first manganese iron phosphate lithium material is b1, and its unit is nm; The unit cell parameter b axis length of the second manganese iron phosphate lithium material is b2, and its unit is nm. Among them, b1<b2; Optionally, b1<100; further optionally, 10≤b1≤80; and / or b2>100; further optionally, 200≤b2≤800.
3. The composite positive electrode active material according to claim 1 or 2, wherein: The average voltage of the composite positive electrode active material is 3.55V to 3.81V; and / or The composite positive electrode active material has a first discharge voltage platform U1 and a second discharge voltage platform U2, 4.0V≤U1<4.1V; and / or 3.4V≤U2≤3.6V.
4. The composite positive electrode active material according to any one of claims 1 to 3, wherein The powder resistivity of the composite positive electrode active material is 1 Ω·cm to 500 Ω·cm; and / or The powder compaction density of the composite positive electrode active material is 2.19 g / ml to 2.40 g / ml.
5. The composite positive electrode active material according to any one of claims 1 to 4, wherein The X-ray diffraction spectrum of the first lithium manganese iron phosphate material has a characteristic peak I(020) and a characteristic peak I(200), and I(020) / I(200)>2.1; and / or The X-ray diffraction (XRD) spectrum of the second lithium manganese iron phosphate material has a characteristic peak I(020) and a characteristic peak I(200), and I(020) / I(200)≤2.
1.
6. The composite positive electrode active material according to any one of claims 1 to 5, wherein The thickness of the first lithium manganese iron phosphate material is H, with the unit being nm, and 10≤H≤80.
7. The composite positive electrode active material according to any one of claims 1 to 6, wherein Based on the total mass of the composite positive electrode active material, the mass percentage of the first lithium iron manganese phosphate material is B1%, the mass percentage of the second lithium iron manganese phosphate material is B2%, and 1≤B2 / B1≤19.
8. The composite positive electrode active material according to any one of claims 1 to 7, wherein The volume average particle size of the first lithium manganese iron phosphate material is D v50-1 , its unit is nm; The volume average particle size of the second lithium manganese iron phosphate material is D v50-2 , its unit is nm, Where 1≤D v50-2 / D v50-1 ≤16; optionally, 2≤D v50-2 / D v50-1 ≤16; Further optionally, 50≤D v50-1 ≤300; and / or 200≤D v50-2 ≤800.
9. The composite positive electrode active material according to any one of claims 1 to 8, wherein The specific surface area of the first lithium manganese iron phosphate material is S1, and its unit is m 2 / g; The specific surface area of the second lithium manganese iron phosphate material is S2, and its unit is m 2 / g; Among them, 0.4≤S2 / S1<1.0; Optionally, 20≤S1≤50; and / or 8≤S2≤20.
10. The composite positive electrode active material according to any one of claims 1 to 9, wherein The first lithium iron manganese phosphate material and the second lithium iron manganese phosphate material each independently include a molecular formula of LiFe (1-x) Mn x PO4 compounds and modified compounds thereof, wherein 0.5≤x<1. 11 . A battery cell comprising a positive electrode sheet, wherein the positive electrode sheet comprises the composite positive electrode active material according to claim 1 .
12. A battery comprising the battery cell according to claim 11.
13. An electrical device comprising the battery according to claim 12.
Citation Information
Patent Citations
Lithium ion battery anode material manganese lithium phosphate and preparation method thereof
CN101320809A
Preparation method and application of b-axial LiFePO<4> / C nano flake material
CN105244500A
Lithium iron phosphate positive electrode material and preparation method thereof and battery
CN110048109A
Lithium iron manganese phosphate compound, preparing method thereof, and lithium ion battery positive electrode
CN112436120A
Preferentially oriented nano lithium manganese phosphate or composite material thereof, preparation method thereof, lithium ion battery positive electrode material and lithium ion battery
CN112635758A