Lithium replenishing material and preparation method therefor, positive electrode sheet and secondary battery
By using a core-shell structure of a lithium-rich core, a fluorine-containing organic coating layer, and a lithium fluoride transition layer in the lithium-supplementing material, combined with a functional encapsulation layer of oxygen-containing carbon materials, the problem of surface alkaline impurities and environmental reactions is solved. Improved electrochemical performance and stability, enabling more efficient lithium-ion battery performance.
Patent Information
- Application Number
- PCT/CN2024/081422
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-13
- Publication Date
- 2024-10-03
AI Technical Summary
Alkaline impurities remain on the surface of existing lithium-supplementing materials during the preparation process, resulting in a decrease in electrochemical performance, and they easily react with environmental moisture and CO2 to cause gelation, affecting the stability and performance of secondary batteries.
It adopts a core-shell structure with a lithium-rich core, a fluorine-containing organic coating layer, and a lithium fluoride transition layer. The transition layer is formed through chemical reactions to reduce the surface residual alkali content, and the functional encapsulation layer of oxygen-containing carbon materials improves isolation capabilities and conductivity. performance.
It effectively reduces the capacity loss of secondary batteries, avoids the gel state phenomenon, improves the electrochemical performance and processing performance of lithium supplement materials, and enhances the structure and electrochemical stability.
Smart Images

Figure CN2024081422_03102024_PF_FP_ABST
Abstract
Description
Lithium supplement material and preparation method thereof, positive electrode sheet and secondary battery
[0001] This disclosure claims priority to the Chinese patent application filed with the China Patent Office on March 29, 2023, with application number 202310373436.4, the entire contents of which are incorporated by reference into this disclosure. Technical Field
[0002] The present disclosure relates to the technical field of secondary batteries, and in particular to a lithium supplement material and a preparation method thereof, a positive electrode sheet, and a secondary battery. Background Art
[0003] During the first charge of lithium-ion batteries, the negative electrode surface is usually accompanied by the formation of a solid electrolyte membrane SEI film, which consumes a large amount of Li + , which means that Li released from the positive electrode material + Part of it is irreversibly consumed, and the reversible specific capacity of the corresponding battery cell is reduced. The negative electrode material, especially the silicon-based negative electrode material, will further consume Li + , resulting in lithium loss in the positive electrode material, reducing the battery's initial coulombic efficiency and battery capacity. For example, in a lithium-ion battery system using a graphite negative electrode, the first charge will consume about 10% of the lithium source. When using high-capacity negative electrode materials such as alloys (silicon, tin, etc.), oxides (silicon oxide, tin oxide) and amorphous carbon negative electrodes, the consumption of positive electrode lithium sources will be further exacerbated.
[0004] In recent years, lithium-supplementing materials have attracted much attention because they can compensate for the irreversible capacity loss caused by the formation of SEI film during the first week of charging of lithium-ion batteries. They are one of the key technologies to further improve the performance of lithium-ion batteries and have broad market applications and development prospects.
[0005] However, during the preparation process of lithium-supplementing materials, alkaline impurities will inevitably remain on the surface of the material. When the residual alkali content on the surface of the lithium-supplementing material is too high, it will have many negative effects on the electrochemical performance of the assembled secondary battery. The impact of surface alkaline compounds on electrochemical performance is mainly reflected in the increase of irreversible capacity loss and the deterioration of cycle performance. In addition, after the lithium-supplementing material is synthesized in an airless atmosphere and transferred to the next process, it is very easy to react with moisture and CO2 in the environment, resulting in deterioration and gelation, which has a great impact on the coating process. Therefore, it also leads to the instability of the interface of the lithium-supplementing material and low electronic conductivity, making the storage stability and processing stability of the existing lithium-supplementing material less than ideal, resulting in unsatisfactory lithium-supplementing effect.
[0006] Summary of the Invention
[0007] The purpose of the present disclosure is to provide a lithium supplement material and a preparation method thereof, a positive electrode plate and a secondary battery.
[0008] To achieve the purpose of this disclosure, the present disclosure provides the following technical solutions:
[0009] In a first aspect, the present disclosure provides a lithium-supplementing material, comprising a lithium-rich core, a coating layer and a transition layer, wherein the coating layer is coated on the outer surface of the lithium-rich core and contains fluorine-containing organic matter; the transition layer is located between the surface of the lithium-rich core and the coating layer and contains lithium fluoride. The present disclosure coats the surface of the lithium-rich core with a fluorine-containing organic compound. On the one hand, the fluorine-containing organic compound can react with the residual alkali on the surface of the lithium-rich core to convert the surface residual alkali into lithium fluoride to form a transition layer, thereby effectively reducing the surface residual alkali content, thereby avoiding the loss of secondary battery capacity caused by the residual alkali. It can also avoid the gel state phenomenon caused by the lithium-supplementing material mixing into the positive electrode material due to water absorption, thereby improving the electrochemical properties and processing performance of the lithium-supplementing material. On the other hand, the transition layer formed by lithium fluoride and the coating formed by the fluorine-containing organic compound can have a denser coating structure, and combined with the strong hydrophobicity of the fluorine atom itself, the combination of the coating layer and the transition layer provided by the present disclosure can have a stronger ability to isolate the entry of external water vapor than other coating methods, thereby avoiding the influence of the external environment on the lithium-rich core, and ensuring the structure and electrochemical stability of the lithium-supplementing material.
[0010] In one possible embodiment, the lithium-rich core and the coating are both chemically connected to the transition layer, and lithium fluoride is in situ bonded to the outer surface of the lithium-rich core. Specifically, since the transition layer is a secondary layer structure formed by chemical reaction between the lithium-rich core and the coating, a chemical bond can exist between the lithium-rich core and the transition layer, and a chemical bond can also exist between the coating and the transition layer, so that the connection between the three layer structures can be tightened. Moreover, lithium fluoride is in situ bonded to the outer surface of the lithium-rich core, that is, lithium fluoride is generated by the in situ reaction of the residual alkali and fluorine-containing organic matter on the surface of the lithium-rich core, and the position of lithium fluoride does not change compared to the original residual alkali. Therefore, compared to the method of physical coating, the present disclosure produces an in situ binding site through chemical reaction, thereby enhancing the connection strength between the lithium-rich core, the transition layer and the coating, and can avoid the phenomenon of the coating layer falling off under pressure.
[0011] In one possible embodiment, in the lithium supplement material, the relative mass ratio of the lithium fluoride to the fluorine-containing organic matter satisfies the relationship: 0.1≤G1 / G2≤10, wherein G1 is the mass of the lithium fluoride in the lithium supplement material, and G2 is the mass of the fluorine-containing organic matter in the lithium supplement material. By controlling the relative mass ratio of lithium fluoride to the fluorine-containing organic matter within the above range, the remaining amount of the fluorine-containing organic matter can be effectively controlled to avoid excessive content of the fluorine-containing organic matter, which leads to excessive weight of the lithium supplement material, thereby affecting the conductivity. When it is lower than the above range, it means that the content of the fluorine-containing organic matter is too little, which may cause the formed coating layer to be too thin, or the coating to be incomplete; when it is higher than the above range, it means that the content of the fluorine-containing organic matter is too much, resulting in the gram weight of the lithium supplement material being too high, and because the fluorine-containing organic matter does not contribute lithium ions and has no conductivity, it is easy to cause the overall conductivity of the lithium supplement material to be poor.
[0012] In one possible embodiment, the lithium supplement material further includes a functional encapsulation layer, which is coated on the outer surface of the coating layer. The functional encapsulation layer may include an oxygen-containing carbon material containing hydroxyl groups, and the structural formula of the oxygen-containing carbon material is C d H e (OH) f , wherein 0<d<6, 0<e<3, 0<f<4. By coating the lithium-rich compound with a fluorine-containing organic compound, at least a portion of the fluorine-containing organic compound can react with the residual alkali to form lithium fluoride, thereby reducing the residual alkali content on the outer surface of the lithium-rich core and isolating the lithium-rich core from water vapor and carbon dioxide in the outside world, thereby ensuring the stability of the core body; then, by using a hydroxyl-containing oxygen-containing carbon material to perform a secondary coating on the lithium-rich core to form a functional encapsulation layer, not only can the isolation effect be further improved in conjunction with the coating layer, but the functional encapsulation layer can also improve the extraction efficiency of lithium ions in the lithium-rich core and improve the electrochemical performance.
[0013] In a possible implementation manner, the functional encapsulation layer contains a conductive agent and a fluorine-containing organic compound. In the functional encapsulation layer, the relative mass ratio of the conductive agent to the fluorine-containing organic compound is 0.5-20.
[0014] In one possible embodiment, the particle size D50 of the lithium supplement material is 0.2 μm to 15 μm.
[0015] In one possible implementation, the coating layer has a thickness ranging from 0.5 nm to 10 nm.
[0016] In one possible implementation, the transition layer has a thickness ranging from 0.5 nm to 10 nm.
[0017] In one possible implementation, the thickness of the functional encapsulation layer ranges from 1 to 100 nm.
[0018] In one possible implementation manner, the residual alkali accounts for 0.01% to 1% by mass.
[0019] In one possible implementation, the resistivity of the lithium-supplementing material is 0.3 Ω / cm to 500 Ω / cm.
[0020] In a second aspect, the present disclosure also provides a method for preparing a lithium-supplementing material, comprising: mixing a lithium-rich compound with a fluorine-containing organic substance to obtain a precursor mixture; heat-treating the precursor mixture to obtain a lithium-supplementing material, wherein the lithium-rich compound forms a lithium-rich core, the fluorine-containing organic substance forms a coating layer, and a transition layer is provided between the surface of the lithium-rich core and the coating layer, and the transition layer contains lithium fluoride.
[0021] In a third aspect, the present disclosure further provides a positive electrode plate, which includes a current collector and an active material layer arranged on the current collector, wherein the active material layer includes a positive electrode material and the lithium-supplementing material described in any one of the embodiments of the first aspect, or the active material layer includes a positive electrode material and a lithium-supplementing material obtained by the preparation method of the lithium-supplementing material described in any one of the embodiments of the second aspect.
[0022] In a fourth aspect, the present disclosure further provides a secondary battery comprising the positive electrode sheet described in the third aspect, or the battery comprises the lithium-supplementing material described in any one of the embodiments of the first aspect, or the battery comprises the lithium-supplementing material obtained by the preparation method of the lithium-supplementing material described in any one of the embodiments of the second aspect. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the embodiments of the present disclosure or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.
[0024] FIG1 is a schematic cross-sectional view of a lithium supplement material according to an embodiment;
[0025] FIG2 is a schematic cross-sectional view of a lithium supplement material according to another embodiment;
[0026] FIG3 is a schematic cross-sectional view of a lithium supplement material according to another embodiment;
[0027] FIG4 is a schematic cross-sectional view of a lithium-supplementing material having a functional encapsulation layer according to an embodiment;
[0028] FIG5 is a flow chart of a method for preparing a lithium supplementing material according to an embodiment. DETAILED DESCRIPTION
[0029] The following will be combined with the accompanying drawings in the embodiments of the present disclosure to clearly and completely describe the technical solutions in the embodiments of the present disclosure. Obviously, the embodiments described are only part of the embodiments of the present disclosure, not all of the embodiments. Based on the embodiments of the present disclosure, all other embodiments obtained by ordinary technicians in this field without making any creative efforts are within the scope of protection of the present disclosure.
[0030] It should be noted that when a component is referred to as being "fixed to" another component, it may be directly on the other component or there may be an intermediate component. When a component is referred to as being "connected to" another component, it may be directly connected to the other component or there may be an intermediate component.
[0031] Unless otherwise defined, all technical and scientific terms used in this disclosure have the same meanings as commonly understood by those skilled in the art to which this disclosure belongs. The terms used in this disclosure and in the specification are for the purpose of describing specific embodiments only and are not intended to limit this disclosure. The term "and / or" as used in this disclosure includes any and all combinations of one or more of the relevant listed items.
[0032] The following describes some embodiments of the present disclosure in detail with reference to the accompanying drawings. In the absence of conflict, the following embodiments and features therein may be combined with each other.
[0033] In the first aspect, the present disclosure provides a lithium-supplementing material, please refer to Figure 1, which includes a lithium-rich core 10, a coating layer 30 and a transition layer 20. The coating layer 30 is coated on the outer layer of the lithium-rich core 10, and the coating layer 30 contains fluorine-containing organic matter; the transition layer 20 is located between the surface of the lithium-rich core 10 and the coating layer 30, and the transition layer 20 contains lithium fluoride.
[0034] Specifically, the lithium-replenishing material has a core-shell structure, with the lithium-rich core comprising a lithium-rich compound. The lithium-rich compound can be lithium-replenishing material particles, acting as a "sacrificial agent" to replenish the lithium source and thus ensure initial charge efficiency. It can also be used as positive electrode material particles, used in conjunction with negative electrode materials to assemble a lithium battery.
[0035] The coating layer may be a fluorine-containing organic compound, such as polytetrafluoroethylene, etc. The lithium fluoride in the transition layer may be a product generated by the reaction of the fluorine-containing organic compound in the coating layer with the residual alkali on the surface of the lithium-rich core.
[0036] In one possible embodiment, the coating layer 30 may be coated on a portion of the surface of the lithium-rich core 10, or may be coated on the entire surface of the lithium-rich core 10. Please refer to Figures 1 to 3. It can be understood that after the lithium-rich core 10 is coated with the precursor of the coating layer 30, the fluorine-containing organic matter will react with the residual alkali, so that the coating layer 30 is converted into the transition layer 20, so there are many positional relationships that can be formed between the transition layer 20 and the coating layer 30. For example, as shown in Figure 1, the outer surface of the lithium-rich core 10 is completely coated by the transition layer 20, and then the coating layer 30 is provided outside the transition layer 20. It can also be shown in Figures 2 and 3, where part of the outer surface of the lithium-rich core 10 is covered by the transition layer 20, and the remaining part is coated by the coating layer 30, and there is also a coating layer 30 outside the position with the transition layer 20.
[0037] In a possible embodiment, the material of the coating layer includes but is not limited to polytetrafluoroethylene and / or fluorine-containing paraffin.
[0038] The present disclosure coats the surface of the lithium-rich core with a fluorine-containing organic compound. On the one hand, the fluorine-containing organic compound can react with the residual alkali on the surface of the lithium-rich core to convert the residual alkali on the surface into lithium fluoride to form a transition layer, thereby effectively reducing the residual alkali content on the surface, thereby avoiding the loss of secondary battery capacity caused by the residual alkali. It can also avoid the gel state phenomenon caused by the lithium-supplementing material mixing into the positive electrode material due to water absorption, thereby improving the electrochemical properties and processing performance of the lithium-supplementing material. On the other hand, the transition layer formed by lithium fluoride and the coating formed by the fluorine-containing organic compound can have a denser coating structure, and combined with the strong hydrophobicity of the fluorine atom itself, the combination of the coating layer and the transition layer provided by the present disclosure can have a stronger ability to isolate the entry of external water vapor than other coating methods, thereby avoiding the influence of the external environment on the lithium-rich core and ensuring the structure and electrochemical stability of the lithium-supplementing material.
[0039] The lithium supplement material can be a ternary lithium supplement material or a binary lithium supplement material. For example, the lithium supplement material can include but is not limited to lithium-rich transition metal oxides, Li w A. Li 1+x+y Al x M y N z Ti 2-x-y-z (PO4)3; wherein, 0<w≤5, A is at least one element selected from C, N, O, P, S, F, B, Se, N is selected from at least one element selected from Si, Ge, Sn, M is selected from at least one element selected from Sc, Ga, Y, La, 0≤y≤0.5, 0≤z≤0.5, 0≤x+y≤0.5. In a specific embodiment, the lithium supplement material may include, but is not limited to, Li2MnO2, Li6MnO4, aLiFeO2·bLi2O·cM x Oy , Li6CoO4, Li2NiO2, Li4SiO4, Li2S, Li3N, Li8SnO6, Li 1.3 Al 0.3 Ti 1.7 (PO4)3. Among them, the chemical formula is aLiFeO2·bLi2O·cM x O y Where a+b≥0.98, c≤0.02, 1.8≤b / a≤2.1, 1≤y / x≤2.5, and M is at least one of Ni, Co, Mn, Ti, Al, Cu, V, and Zr.
[0040] In one possible embodiment, the lithium-rich core and the coating are both chemically connected to the transition layer, and lithium fluoride is in situ bonded to the outer surface of the lithium-rich core. Specifically, since the transition layer is a secondary layer structure formed by chemical reaction between the lithium-rich core and the coating, a chemical bond can exist between the lithium-rich core and the transition layer, and a chemical bond can also exist between the coating and the transition layer, so that the connection between the three layer structures can be tightened. Moreover, lithium fluoride is in situ bonded to the outer surface of the lithium-rich core, that is, lithium fluoride is generated by the in situ reaction of the residual alkali and fluorine-containing organic matter on the surface of the lithium-rich core, and the position of lithium fluoride does not change compared to the original residual alkali. Therefore, compared to the method of physical coating, the present disclosure produces an in situ binding site through chemical reaction, thereby enhancing the connection strength between the lithium-rich core, the transition layer and the coating, and can avoid the phenomenon of the coating layer falling off under pressure.
[0041] In one possible embodiment, in the lithium-replenishing material, the relative mass ratio of lithium fluoride to the fluorine-containing organic matter satisfies the relationship: 0.1≤G1 / G2≤10, wherein G1 is the mass of lithium fluoride in the lithium-replenishing material, and G2 is the mass of the fluorine-containing organic matter in the lithium-replenishing material. Specifically, the ratio of G1 / G2 can be 0.1, 0.2, 0.3, 0.5, 1, 2, 3, 5, 7, 10. By controlling the relative mass ratio of lithium fluoride to the fluorine-containing organic matter within the above range, the remaining amount of the fluorine-containing organic matter can be effectively controlled to avoid excessive content of the fluorine-containing organic matter, which leads to excessive weight of the lithium-replenishing material, thereby affecting the conductivity. When it is lower than the above range, it means that the content of the fluorine-containing organic matter is too little, which may cause the formed coating layer to be too thin, or the coating to be incomplete; when it is higher than the above range, it means that the content of the fluorine-containing organic matter is too much, resulting in the gram weight of the lithium-replenishing material being too high, and because the fluorine-containing organic matter does not contribute lithium ions and does not have conductivity, it is easy to cause the overall conductivity of the lithium-replenishing material to be poor.
[0042] In a possible embodiment, referring to FIG4 , the lithium supplement material further includes a functional encapsulation layer 40, which is coated on the outer surface of the coating layer. The functional encapsulation layer 40 further includes an oxygen-containing carbon material containing hydroxyl groups, and the structural formula of the oxygen-containing carbon material is C d H e (OH) f , where 0<d<6, 0<e<3, 0<f<4.
[0043] Specifically, after the coating layer is completed, the lithium-rich core can be secondary coated with an organic matter containing hydroxyl groups. And the organic matter containing hydroxyl groups is pre-carbonized by high-temperature heat treatment to obtain an oxygen-containing carbon material containing hydroxyl groups. It can be understood that the pre-carbonization temperature is lower than the carbonization temperature, the organic matter containing hydroxyl groups cannot be completely carbonized, and the oxygen atoms are not completely removed, so what is obtained is an oxygen-containing carbon material. Compared with the existing carbon source (completely carbonized carbon source), the oxygen-containing carbon material containing hydroxyl groups has a better effect on the extraction of lithium ions because it includes oxygen-containing functional groups. In addition, the heating temperature required to prepare the oxygen-containing carbon material containing hydroxyl groups is lower, which can greatly save energy consumption when preparing lithium-supplementing materials.
[0044] In one possible embodiment, the precursor of the oxygen-containing carbon material may be, but is not limited to, glucose, starch, polyethylene glycol, polyvinyl alcohol, and the like.
[0045] In one possible embodiment, at least part of the lithium fluoride is located in the functional encapsulation layer, and the lithium fluoride content in the functional encapsulation layer is less than the lithium fluoride content in the transition layer.
[0046] In one possible embodiment, at least part of the fluorinated organic matter is located in the functional encapsulation layer, and the content of the fluorinated organic matter in the functional encapsulation layer is less than the content of the fluorinated organic matter in the coating layer.
[0047] Specifically, after the lithium-rich compound is coated with a fluorinated organic compound, the fluorinated organic compound in contact with the lithium-rich compound will first react with the residual alkali to form lithium fluoride. The further away the fluorinated organic compound is from the lithium-rich core, the less likely it is to react with the residual alkali. Therefore, after the fluorinated organic compound reacts with the residual alkali, lithium fluoride will be pre-formed and coated on the outer surface of the lithium-rich core, while excess fluorinated organic compound will form on the outer surface of part of the lithium fluoride. The functional encapsulation layer is then coated on the outer surface of the fluorinated organic compound and / or lithium fluoride.
[0048] Understandably, there's no clear interface between the coating layer and the functional encapsulation layer. When the amount of fluorinated organic matter is low, the coating layer should be thinner, and the fluorinated organic matter is more likely to have partial defects, allowing at least a portion of the coating layer to embed into the aforementioned defects. When the amount of precursor is high, the coating layer should be thicker and denser, resulting in a clearer boundary between the coating layer and the functional encapsulation layer.
[0049] By coating the lithium-rich compound with a fluorine-containing organic compound, at least part of the fluorine-containing organic compound can react with the residual alkali to form lithium fluoride, thereby reducing the residual alkali content on the outer surface of the lithium-rich core, and at the same time isolating the lithium-rich core from water vapor and carbon dioxide in the outside world, thereby ensuring the stability of the core body; and then by using an oxygen-containing carbon material containing hydroxyl groups to perform a secondary coating on the lithium-rich core to form a functional encapsulation layer, not only can the isolation effect be further improved by cooperating with the coating layer, but the functional encapsulation layer can also improve the extraction efficiency of lithium ions in the lithium-rich core and improve the electrochemical performance.
[0050] In one possible embodiment, the functional encapsulation layer comprises a conductive agent and a fluorine-containing organic compound, wherein the relative mass ratio of the conductive agent to the fluorine-containing organic compound in the functional encapsulation layer is 0.5 to 20. The conductive agent may be the oxygen-containing carbon material mentioned above.
[0051] In one possible embodiment, the thickness of the coating layer is 0.5 mm to 10 nm. Specifically, the thickness of the coating layer can be, but is not limited to, 0.5 nm, 0.7 nm, 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 7 nm, and 10 nm. Controlling the thickness of the coating layer within the above range is beneficial for adjusting the particle size of the lithium-supplementing material, while also ensuring the specific capacity and electronic conductive environment of the lithium-supplementing material. When the thickness of the coating layer is less than the above range, the coating layer will not completely cover the lithium-rich core, which is not only not conducive to building a good water vapor barrier environment, but also very likely to cause incomplete reaction of residual alkali; when the thickness of the coating layer is greater than the above range, the particle size of the lithium-supplementing material will be too large, and since the fluorine-containing organic matter in the coating layer does not contribute lithium ions, the overall gram capacity of the lithium-supplementing material will be reduced.
[0052] In one possible embodiment, the thickness of the transition layer is 0.5 mm to 10 nm. Specifically, the thickness of the transition layer can be, but is not limited to, 0.5 nm, 0.7 nm, 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 7 nm, and 10 nm. Controlling the thickness of the transition layer within the above range is beneficial for adjusting the particle size of the lithium-supplementing material, while also ensuring the specific capacity and electronic conductive environment of the lithium-supplementing material. When the thickness of the transition layer is less than the above range, the transition layer will not completely cover the lithium-rich core, which is not only not conducive to building a good water vapor barrier environment, but also very likely to cause incomplete reaction of residual alkali; when the thickness of the transition layer is greater than the above range, the particle size of the lithium-supplementing material will be too large, and since the fluorine-containing organic matter in the transition layer does not contribute lithium ions, the overall gram capacity of the lithium-supplementing material will be reduced.
[0053] In one possible embodiment, the thickness of the functional encapsulation layer is 1 mm to 100 nm. Specifically, the thickness of the functional encapsulation layer can be, but is not limited to, 1 nm, 2 nm, 3 nm, 5 nm, 10 nm, 20 nm, 30 nm, 50 nm, 70 nm, and 100 nm. Controlling the thickness of the functional encapsulation layer within the above range is conducive to adjusting the particle size of the lithium-supplementing material, while also ensuring the specific capacity and electronic conductive environment of the lithium-supplementing material. When the thickness of the functional encapsulation layer is less than the above range, the functional encapsulation layer does not completely cover the coating layer, which is not conducive to building a good electronic conductive environment; when the thickness of the functional encapsulation layer is greater than the above range, the particle size of the lithium-supplementing material will be too large, and since the functional encapsulation layer does not contribute lithium ions, the overall gram capacity of the lithium-supplementing material will be reduced.
[0054] In one possible embodiment, the particle size D50 of the lithium supplementing material is 0.2 μm to 15 μm; specifically, the particle size D50 of the lithium supplementing material can be, but is not limited to, 0.2 μm, 0.5 μm, 1 μm, 2 μm, 5 μm, 10 μm, or 15 μm.
[0055] In one possible embodiment, the particle size of the lithium-supplementing material satisfies the relationship: D10 / D50 ≥ 0.3. D10 is the particle size distribution curve corresponding to a particle size that is less than 10% of the total volume. By controlling the particle size range and ratio within the lithium-supplementing material, the particles of the lithium-supplementing material can be effectively controlled to be more uniform.
[0056] In one possible embodiment, the particle size of the lithium-supplementing material satisfies the relationship: D90 / D50 ≤ 2. The particle size distribution curve indicates a particle size smaller than the particle size corresponding to 90% of the total volume. By controlling the particle size range within the lithium-supplementing material, the particles of the lithium-supplementing material can be effectively controlled to be more uniform.
[0057] In one possible embodiment, the residual alkali content in the lithium-supplementing material is 0.01% to 1% by weight. It is understood that this residual alkali content represents the amount of residual alkali remaining in the positive electrode material after removal by the fluorinated organic compound. Residual alkali within this range has minimal impact on the performance of the positive electrode material and also demonstrates that the residual alkali content in the positive electrode material is significantly reduced after coating with the fluorinated organic compound.
[0058] In one possible embodiment, the specific surface area of the lithium supplement material is 0.3 m 2 / g~20m 2 / g.
[0059] In one possible implementation, the resistivity of the lithium-supplementing material is 0.3 Ω / cm to 500 Ω / cm.
[0060] In a second aspect, the present disclosure further provides a method for preparing a lithium-supplementing material, as shown in FIG5 , which is specifically used for preparing the lithium-supplementing material in the first aspect. The preparation method comprises the following steps:
[0061] Step S10: mixing the lithium-rich compound with the fluorine-containing organic compound to obtain a precursor mixture.
[0062] In step S20, the precursor mixture is heat-treated to obtain a lithium-supplementing material. The lithium-rich compound forms a lithium-rich core, the fluorine-containing organic compound forms a coating layer, and a transition layer is provided between the surface of the lithium-rich core and the coating layer. The transition layer contains lithium fluoride.
[0063] Specifically, the lithium-rich compound may be one or more of the various lithium-rich compounds provided in the first aspect. The fluorine-containing organic compound may be one or more of the various fluorine-containing organic compounds provided in the first aspect.
[0064] In one possible embodiment, the present disclosure does not specifically limit the method for preparing the lithium-rich core in the above step S10, as long as a lithium-rich compound can be prepared. For example, the method for preparing the lithium-rich compound can adopt solid phase sintering. In one possible embodiment, the steps of preparing the lithium-rich compound include:
[0065] Step S001, adding the first metal compound and the second metal compound into a solvent according to a molar ratio, and crushing them after drying and spraying to obtain a mixture; Step S002, sintering the above mixture under an inert atmosphere, and crushing them after cooling to obtain a lithium-rich compound.
[0066] The first metal compound in step S001 may be a lithium salt, the second metal compound may be one or more non-lithium metal salts, and the solvent may be a mixture of one or more of deionized water, ethanol, and methanol.
[0067] In a possible implementation, in step S002 , the inert atmosphere may be an atmosphere formed by any protective gas selected from nitrogen, argon, and a nitrogen-argon mixture.
[0068] In a possible embodiment, in step S002 , the sintering temperature of the mixture may be 500° C. to 1000° C., the sintering time may be 0.5 h to 10 h, and the heating rate may be 100° C. / h to 500° C. / h.
[0069] In a possible implementation, in step S20, the temperature for heat treatment of the precursor mixture may be 250° C. to 400° C., and the heat treatment time may be 2 h to 10 h.
[0070] In one possible embodiment, the method for preparing the lithium supplement material further includes:
[0071] Step S30: preparing an oxygen-containing carbon material containing hydroxyl groups, and fully mixing the oxygen-containing carbon material and the lithium-rich core with a coating layer to obtain a lithium-supplementing material. The oxygen-containing carbon material is coated on the outer surface of the coating layer to form a functional encapsulation layer.
[0072] Specifically, the oxygen-containing carbon material containing hydroxyl groups may be one or more of the oxygen-containing carbon materials provided in the first aspect.
[0073] In one possible embodiment, the raw material of the oxygen-containing carbon material is placed in an inert atmosphere at a temperature of 250° C. to 400° C. and kept warm for 2 hours to 10 hours to obtain the oxygen-containing carbon material.
[0074] In one possible embodiment, in step S30, the oxygen-containing carbon material and the lithium-rich core with the coating layer are fused at a rotation speed of 1500 rpm to 5000 rpm for a processing time of 5 min to 60 min.
[0075] In a third aspect, the present disclosure further provides a positive electrode plate, comprising a current collector and an active material layer disposed on the current collector, wherein the active material layer comprises a positive electrode material and the lithium-supplementing material of the first aspect, or the active material layer comprises the positive electrode material and a lithium-supplementing material obtained by the preparation method of the lithium-supplementing material of the second aspect. The positive electrode plate provided by the present disclosure, because it contains the above-mentioned lithium-supplementing material, and the lithium-supplementing material can provide active lithium ions that compensate for the formation of the SEI film during the first charge of the battery, thereby effectively maintaining the gram capacity of the positive electrode plate and improving the capacity retention rate of the positive electrode plate; at the same time, the lithium-supplementing material can release lithium polysulfide to eliminate lithium plating, thereby not only maintaining the performance of the positive electrode plate, but also improving the service life of the positive electrode plate.
[0076] In one possible embodiment, the positive electrode sheet includes a positive electrode current collector, which has a positive electrode active layer on it. The positive electrode active layer includes components such as positive electrode material, conductive agent, binder, etc. The present disclosure does not specifically limit these materials, and suitable materials can be selected according to actual application requirements. The positive electrode current collector includes but is not limited to any one of copper foil and aluminum foil. The positive electrode active material can be a phosphate positive electrode active material and a ternary positive electrode active material. In a specific embodiment, it includes one or more of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, lithium manganese iron phosphate, lithium vanadium phosphate, lithium vanadium oxyphosphate, lithium fluorovanadium phosphate, lithium titanate, lithium nickel cobalt manganese oxide, and lithium nickel cobalt aluminum oxide. The conductive agent includes one or more of graphite, carbon black, acetylene black, graphene, carbon fiber, C60 and carbon nanotubes, and the content of the conductive agent in the positive electrode active layer is 3wt%-5wt%. The types of binders include one or more of polyvinylidene chloride, soluble polytetrafluoroethylene, styrene-butadiene rubber, hydroxypropyl methylcellulose, methylcellulose, carboxymethyl cellulose, polyvinyl alcohol, acrylonitrile copolymer, sodium alginate, chitosan and chitosan derivatives, and the content of the binder in the positive electrode active layer is 2wt% to 4wt%.
[0077] In one possible implementation, the content of the lithium-supplementing material in the positive electrode material can be controlled at 1% to 6% of the mass of the positive electrode active material. This ratio can just compensate for the loss of active lithium during the first charging process of the battery. If the amount of lithium-supplementing material added to the positive electrode sheet is too low, the active lithium lost in the positive electrode material cannot be fully replenished, which is not conducive to improving the energy density and capacity retention rate of the battery. If the amount of lithium-supplementing material added to the positive electrode material is too high, it may cause lithium plating at the negative electrode to become serious and increase costs. In some specific embodiments, the mass percentage of the lithium-supplementing material in the positive electrode material can be 1%, 2%, 4%, 6%, etc.
[0078] In a fourth aspect, the present disclosure further provides a secondary battery comprising the aforementioned positive electrode sheet. The aforementioned lithium-supplementing material is added to the positive electrode sheet, effectively compensating for the active lithium ions consumed by the formation of the SEI film during the initial charge of the battery, thereby effectively maintaining the gram capacity of the positive electrode sheet and improving the capacity retention rate of the positive electrode sheet. Furthermore, the shape of the secondary battery can be maintained, the service life of the secondary battery can be increased, and the charge capacity of the secondary battery can be increased due to the elimination of lithium plating, reducing the possibility of natural battery failure.
[0079] The technical solution of the present disclosure is described in detail below through specific embodiments.
[0080] Example 1
[0081] This embodiment provides a lithium-replenishing material and a preparation method thereof. The lithium-replenishing material comprises a lithium-rich core composed of LiFeO2·1.99Li2O, a transition layer comprising lithium fluoride, a coating layer comprising a fluorine-containing organic compound, and a functional encapsulation layer comprising an oxygen-containing carbon material containing hydroxyl groups.
[0082] The preparation method of the lithium supplement material comprises the following steps:
[0083] (1) Fe(NO3)3·9H2O and LiNO3 were added to deionized water at a molar ratio of 1:4.98, mixed thoroughly, spray-dried at 280°C, and crushed;
[0084] (2) In a nitrogen atmosphere, the temperature was raised to 850°C at a rate of 300°C / h and kept at that temperature for 15 h. After cooling, the product was mechanically crushed and classified to obtain LiFeO2·1.99Li2O powder;
[0085] (3) LiFeO2·1.99Li2O powder and polytetrafluoroethylene wax powder were placed in a rotary kiln; wherein the LiFeO2·1.99Li2O powder and polytetrafluoroethylene wax powder were mixed in a mass ratio of 9.5:0.5. Nitrogen was introduced into the rotary kiln, and the temperature was increased to 350°C at a heating rate of 200°C / h, maintained at that temperature for 1 hour, and then cooled to obtain LiFeO2·1.99Li2O powder coated with lithium fluoride and a fluorine-containing organic compound.
[0086] (4) Glucose was placed in a nitrogen atmosphere and heated to 320°C and kept warm for 2 hours to obtain an oxygen-containing carbon material.
[0087] (5) The coated LiFeO2·1.99Li2O powder obtained in step (3) and the oxygen-containing carbon material are uniformly mixed; wherein the coated LiFeO2·1.99Li2O powder and the oxygen-containing carbon material are mixed in a mass ratio of 5:1. The mixture is subjected to a fusion treatment under a nitrogen atmosphere at a fusion treatment speed of 2500 rpm for 40 minutes to obtain a lithium supplement material.
[0088] After testing, the average particle size of the lithium supplement material is 2um and the specific surface area is 2.4m 2 / g, the measured resistivity is 260Ω / cm. The thickness of the transition layer is 8nm, the thickness of the coating layer is 6nm, and the thickness of the functional encapsulation layer is 82nm.
[0089] Example 2
[0090] This embodiment provides a lithium-replenishing material and a preparation method thereof. The lithium-replenishing material comprises a lithium-rich core composed of LiFeO2·1.99Li2O·0.005Al2O3, a transition layer comprising lithium fluoride, a coating layer comprising a fluorine-containing organic compound, and a functional encapsulation layer comprising an oxygen-containing carbon material containing hydroxyl groups.
[0091] The preparation method of the lithium supplement material comprises the following steps:
[0092] (1) Fe(NO3)3·9H2O, LiNO3, and Al(NO3)3 were added to deionized water at a molar ratio of 1:4.98:0.01, mixed thoroughly, spray-dried at 280°C, and crushed;
[0093] (2) In a nitrogen atmosphere, the temperature was raised to 800°C at a rate of 300°C / h and kept at that temperature for 10 h. After cooling, the product was mechanically crushed and classified to obtain LiFeO2·1.99Li2O·0.005Al2O3 powder;
[0094] (3) LiFeO2·1.99Li2O·0.005Al2O3 powder and polytetrafluoroethylene wax powder were placed in a rotary kiln; wherein the LiFeO2·1.99Li2O·0.005Al2O3 powder and polytetrafluoroethylene wax powder were mixed in a mass ratio of 9.5:0.5. Nitrogen was introduced into the rotary kiln, and the temperature was increased to 400°C at a heating rate of 200°C / h, maintained at that temperature for 2h, and then cooled to obtain LiFeO2·1.99Li2O·0.005Al2O3 powder coated with lithium fluoride and a fluorine-containing organic compound.
[0095] (4) Glucose was placed in a nitrogen atmosphere and heated to 350°C for 4 hours to obtain an oxygen-containing carbon material.
[0096] (5) The coated LiFeO2·1.99Li2O·0.005Al2O3 powder obtained in step (3) is uniformly mixed with an oxygen-containing carbon material; wherein the coated LiFeO2·1.99Li2O·0.005Al2O3 powder and the oxygen-containing carbon material are mixed in a mass ratio of 5:1. The mixture is fused under a nitrogen atmosphere at a fusion speed of 2500 rpm for 40 minutes to obtain a lithium supplement material.
[0097] After testing, the average particle size of the lithium supplement material is 5um and the specific surface area is 1.6m 2 / g, and the measured resistivity is 130Ω / cm. The thickness of the transition layer is 4nm, the thickness of the coating layer is 3nm, and the thickness of the functional encapsulation layer is 57nm.
[0098] Example 3
[0099] This embodiment provides a lithium-replenishing material and a preparation method thereof. The lithium-replenishing material comprises a lithium-rich core composed of LiFeO2·1.99Li2O·0.01CuO, a transition layer comprising lithium fluoride, a coating layer comprising a fluorine-containing organic compound, and a functional encapsulation layer comprising an oxygen-containing carbon material containing hydroxyl groups.
[0100] The preparation method of the lithium supplement material comprises the following steps:
[0101] (1) Fe2O3, LiOH, and CuO were added to deionized water at a molar ratio of 1:10.1:0.01, mixed thoroughly, spray-dried at 280°C, and crushed;
[0102] (2) In a nitrogen atmosphere, the temperature was raised to 900°C at a rate of 300°C / h and kept at this temperature for 10 h. After cooling, the product was mechanically crushed and classified to obtain LiFeO2·1.99Li2O·0.01CuO powder;
[0103] (3) LiFeO2·1.99Li2O·0.01CuO powder and polytetrafluoroethylene wax powder are placed in a rotary kiln; wherein the coated LiFeO2·1.99Li2O·0.01CuO powder and polytetrafluoroethylene wax powder are mixed in a mass ratio of 9:1. Nitrogen is introduced into the rotary kiln, and the temperature is increased to 400°C at a heating rate of 200°C / h, maintained at this temperature for 2h, and then cooled to obtain LiFeO2·1.99Li2O·0.01CuO powder coated with lithium fluoride and a fluorine-containing organic compound.
[0104] (4) Glucose was placed in a nitrogen atmosphere and heated to 400°C and kept warm for 4 hours to obtain an oxygen-containing carbon material.
[0105] (5) The coated LiFeO2·1.99Li2O·0.01CuO powder obtained in step (3) is uniformly mixed with an oxygen-containing carbon material; wherein the LiFeO2·1.99Li2O·0.01CuO powder and the oxygen-containing carbon material are mixed in a mass ratio of 5:1. The mixture is subjected to a fusion treatment under a nitrogen atmosphere at a fusion speed of 2500 rpm for 40 minutes to obtain a lithium supplement material.
[0106] After testing, the average particle size of the lithium supplement material is 10um and the specific surface area is 0.9m 2 / g, the measured resistivity is 180Ω / cm. The thickness of the transition layer is 3.5nm, the thickness of the coating layer is 2.7nm, and the thickness of the functional encapsulation layer is 32nm.
[0107] Example 4
[0108] This embodiment provides a lithium-replenishing material and a preparation method thereof. The lithium-replenishing material comprises a lithium-rich core composed of LiFeO2·2.025Li2O·0.01MnO, a transition layer comprising lithium fluoride, a coating layer comprising a fluorine-containing organic compound, and a functional encapsulation layer comprising an oxygen-containing carbon material containing hydroxyl groups.
[0109] The preparation method of the lithium supplement material comprises the following steps:
[0110] (1) Fe2O3, LiOH, and MnO2 were added to deionized water at a molar ratio of 1:10.1:0.01 and mixed thoroughly, spray-dried at 280°C, and crushed;
[0111] (2) In a nitrogen atmosphere, the temperature was raised to 700°C at a rate of 300°C / h and kept at this temperature for 10 h. After cooling, the product was mechanically crushed and classified to obtain LiFeO2·2.025Li2O·0.01MnO powder;
[0112] (3) LiFeO2·2.025Li2O·0.01MnO powder and polytetrafluoroethylene wax powder were placed in a rotary kiln; wherein the LiFeO2·2.025Li2O·0.01MnO powder and polytetrafluoroethylene wax powder were mixed in a mass ratio of 9:1. Nitrogen was introduced into the rotary kiln, and the temperature was increased to 400°C at a heating rate of 200°C / h, maintained at that temperature for 2h, and then cooled to obtain LiFeO2·2.025Li2O·0.01MnO powder coated with lithium fluoride and a fluorine-containing organic compound.
[0113] (4) Glucose is placed in a nitrogen atmosphere and heated to 440°C and kept warm for 1 hour to obtain an oxygen-containing carbon material.
[0114] (5) The coated LiFeO2·2.025Li2O·0.01MnO powder obtained in step (3) is uniformly mixed with an oxygen-containing carbon material; wherein the coated LiFeO2·2.025Li2O·0.01MnO powder and the oxygen-containing carbon material are mixed in a mass ratio of 5:1. The mixture is subjected to a fusion treatment under a nitrogen atmosphere at a fusion speed of 2500 rpm for 40 minutes to obtain a lithium supplement material.
[0115] After testing, the average particle size of the lithium supplement material is 4.2um and the specific surface area is 2.6m 2 / g, the measured resistivity is 35Ω / cm. The thickness of the transition layer is 5.5nm, the thickness of the coating layer is 5nm, and the thickness of the functional encapsulation layer is 61nm.
[0116] Example 5
[0117] This embodiment provides a lithium-replenishing material and a preparation method thereof. The lithium-replenishing material comprises a lithium-rich core composed of LiFeO2·2.025Li2O·0.01MnO, a transition layer comprising lithium fluoride, a coating layer comprising a fluorine-containing organic compound, and a functional encapsulation layer comprising an oxygen-containing carbon material containing hydroxyl groups.
[0118] The preparation method of the lithium supplement material comprises the following steps:
[0119] (1) Fe2O3, LiOH, and MnO2 were added to deionized water at a molar ratio of 1:10.1:0.01 and mixed thoroughly, spray-dried at 280°C, and crushed;
[0120] (2) In a nitrogen atmosphere, the temperature was raised to 700°C at a rate of 300°C / h and kept at this temperature for 10 h. After cooling, the product was mechanically crushed and classified to obtain LiFeO2·2.025Li2O·0.01MnO powder;
[0121] (3) LiFeO2·2.025Li2O·0.01MnO powder and polytetrafluoroethylene wax powder were placed in a rotary kiln; wherein the LiFeO2·2.025Li2O·0.01MnO powder and polytetrafluoroethylene wax powder were mixed in a mass ratio of 9:1. Nitrogen was introduced into the rotary kiln, and the temperature was increased to 400°C at a heating rate of 200°C / h, maintained at that temperature for 2h, and then cooled to obtain LiFeO2·2.025Li2O·0.01MnO powder coated with lithium fluoride and a fluorine-containing organic compound.
[0122] (4) Glucose is placed in a nitrogen atmosphere and heated to 440°C and kept warm for 1 hour to obtain an oxygen-containing carbon material.
[0123] (5) The coated LiFeO2·2.025Li2O·0.01MnO powder obtained in step (3) is uniformly mixed with an oxygen-containing carbon material; wherein the coated LiFeO2·2.025Li2O·0.01MnO powder and the oxygen-containing carbon material are mixed in a mass ratio of 5:1. The mixture is subjected to a fusion treatment under a nitrogen atmosphere at a fusion speed of 2500 rpm for 40 minutes to obtain a lithium supplement material.
[0124] After testing, the average particle size of the lithium supplement material is 5.7um and the specific surface area is 3.1m 2 / g, the measured resistivity is 31Ω / cm. The thickness of the transition layer is 7.3nm, the thickness of the coating layer is 7nm, and the thickness of the functional encapsulation layer is 95nm.
[0125] Comparative Example 1
[0126] This embodiment provides a lithium-supplementing material and a preparation method thereof. The lithium-supplementing material comprises a lithium-rich core composed of LiFeO2·1.99Li2O and a functional encapsulation layer composed of an oxygen-containing carbon material containing hydroxyl groups.
[0127] Comparative Example 1 provides a preparation method thereof, which does not include step (3) compared with Example 1.
[0128] Comparative Example 2
[0129] This comparative example provides a lithium supplement material and a preparation method thereof. The lithium supplement material is LiFeO2·1.99Li2O and does not have a transition layer, a coating layer, or a functional encapsulation layer.
[0130] Comparative Example 1 provides a preparation method which, compared with Example 1, only includes steps (1) and (2).
[0131] The lithium supplement materials provided in Examples 1-5 and the lithium supplement materials provided in Comparative Examples 1-2 were assembled into positive electrodes and lithium-ion batteries respectively according to the following methods:
[0132] Positive electrode: A lithium supplement additive and lithium cobalt oxide were mixed in a mass ratio of 5:95 to obtain a mixture. The mixture was mixed with polyvinylidene fluoride and SP-Li in a mass ratio of 93:3:4 and stirred by ball milling to obtain a positive electrode slurry. The positive electrode slurry was coated on the surface of aluminum foil, roll-pressed, and vacuum-dried at 110°C overnight to obtain a positive electrode sheet.
[0133] Negative electrode: lithium metal sheet;
[0134] Electrolyte: Ethylene carbonate and ethyl methyl carbonate were mixed in a volume ratio of 3:7, and LiPF6 was added to form an electrolyte. The concentration of LiPF6 was 1 mol / L.
[0135] Diaphragm: Polypropylene microporous separator;
[0136] Lithium-ion battery assembly: Lithium-ion batteries are assembled in an inert atmosphere glove box in the order of lithium metal sheet-diaphragm-electrolyte-positive electrode sheet.
[0137] The electrochemical performance of each lithium-ion battery assembled in the above lithium-ion battery examples was tested. The test conditions were: the assembled batteries were placed at room temperature for 24 hours and then charged and discharged. The charge and discharge voltage was 2.7V-4.3V. The electrochemical performance of the secondary batteries of Examples 1-5 and Comparative Examples 1-2 is shown in Table 1.
[0138] Table 1
[0139] As can be seen from Table 1, the positive electrode slurries prepared from the lithium-supplementing materials of Examples 1-5 of the present disclosure after being coated with a coating layer and a transition layer do not exhibit a gel state. This is because the lithium-supplementing materials coated with the coating layer, transition layer, and functional encapsulation layer can effectively isolate external moisture, preventing the residual alkali in the lithium-supplementing materials from reacting with external moisture, thereby preventing the positive electrode slurry from exhibiting a gel state and making the positive electrode slurry easier to coat. Furthermore, when added to a secondary battery, the positive electrode can achieve a higher initial gram capacity and lower initial efficiency, thereby compensating for the reduced energy density caused by irreversible lithium loss in the initial negative electrode.
[0140] As can be seen from Example 1 and Comparative Example 1, coating the lithium-rich core with a single oxygen-containing carbon material can prevent the gel state for a short period of time, but it cannot achieve the same effect over a sustained period of time. This is because the oxygen-containing carbon material is not fully carbonized, and the oxygen-containing functional groups attract water vapor in the external environment. Although this improves the electrochemical performance of the secondary battery compared to Comparative Example 2, it still cannot be stored for a long time.
[0141] It can be seen from Example 1 and Comparative Example 2 that the lithium supplement material that has not been coated easily absorbs water during the preparation of the positive electrode slurry, resulting in the formation of a gel state, which is not conducive to the coating of the positive electrode slurry.
[0142] In summary, the present disclosure coats the surface of the lithium-rich core with fluorine-containing organic matter. On the one hand, the fluorine-containing organic matter can react with the residual alkali on the surface of the lithium-rich material to convert the surface residual alkali into lithium fluoride, thereby effectively reducing the surface residual alkali content, thereby avoiding the loss of secondary battery capacity caused by residual alkali, and can also avoid the gel state phenomenon caused by water absorption when the lithium-supplementing material is mixed into the positive electrode material, thereby improving the electrochemical properties and processing performance of the lithium-supplementing material; on the other hand, the present disclosure also coats the oxygen-containing carbon material outside the coating layer to form a functional encapsulation layer, so that the coating layer and the functional encapsulation layer can be closely matched to form a denser coating structure. On the basis of utilizing the strong hydrophobicity of the fluorine atom itself, the conductive properties of the lithium-supplementing material are improved by the oxygen-containing carbon material, further enhancing the water-isolating ability of the lithium-supplementing material, and ensuring the structure and electrochemical stability of the lithium-supplementing material.
[0143] In the description of the embodiments of the present disclosure, it should be noted that the orientation or positional relationship of terms such as "center", "up", "down", "left", "right", "vertical", "horizontal", "inside", and "outside" are based on the orientation or positional relationship described in the accompanying drawings, and are only for the convenience of describing the present disclosure and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present disclosure.
[0144] The above disclosure is only a preferred embodiment of the present disclosure, and it is certainly not intended to limit the scope of the rights of the present disclosure. A person skilled in the art can understand that all or part of the processes of the above embodiment and equivalent changes made in accordance with the claims of the present disclosure are still within the scope of the present disclosure.
Claims
1. A lithium supplement material, characterized in that: include: Lithium-rich core; A coating layer, covering the outer surface of the lithium-rich core, wherein the coating layer contains fluorine-containing organic matter; A transition layer is located between the surface of the lithium-rich core and the coating layer, and the transition layer contains lithium fluoride.
2. The lithium supplement material according to claim 1, characterized in that: The lithium-rich core and the coating layer are both chemically connected to the transition layer, and the lithium fluoride is in-situ bonded to the outer surface of the lithium-rich core.
3. The lithium supplement material according to claim 1, characterized in that: In the lithium supplement material, the relative mass ratio of the lithium fluoride to the fluorine-containing organic matter satisfies the relationship 0.1≤G1 / G2≤10, wherein G1 is the mass of the lithium fluoride in the lithium supplement material, and G2 is the mass of the fluorine-containing organic matter in the lithium supplement material.
4. The lithium supplement material according to claim 1, characterized in that: The transition layer is coated on the outer surface of the lithium-rich core, and the coating layer is coated on the outer surface of the transition layer; or, Part of the outer surface of the lithium-rich core is covered by the transition layer, and the coating layer coats the remaining outer surface of the lithium-rich core and the outer surface of the transition layer.
5. The lithium supplement material according to claim 1, characterized in that: The lithium supplement material further includes a functional encapsulation layer, and the functional encapsulation layer is coated on the outer surface of the coating layer.
6. The lithium supplement material according to claim 5, characterized in that: The functional encapsulation layer contains a conductive agent and a fluorine-containing organic substance. In the functional encapsulation layer, the relative mass ratio of the conductive agent to the fluorine-containing organic substance is 0.5-20.
7. The lithium supplement material according to claim 5, characterized in that: The functional encapsulation layer comprises an oxygen-containing carbon material, the structural formula of which is C d H e (OH) f , where 0<d<6, 0<e<3, 0<f<4.
8. The lithium supplement material according to claim 5, characterized in that: The functional encapsulation layer contains lithium fluoride, and the content of lithium fluoride in the functional encapsulation layer is less than the content of lithium fluoride in the transition layer.
9. The lithium supplement material according to claim 1, characterized in that: The particle size D50 of the lithium supplement material is 0.2 μm to 15 μm; And / or, the coating layer has a thickness ranging from 0.5 nm to 10 nm; And / or, the thickness of the transition layer is in the range of 0.5 nm to 10 nm; And / or, the thickness of the functional encapsulation layer is in the range of 1 to 100 nm.
10. The lithium supplement material according to claim 1, characterized in that: The particle size of the lithium supplement material satisfies the relationship: D10 / D50≥0.3; and / or The particle size of the lithium supplement material satisfies the relationship: D90 / D50≤2.
11. The lithium supplement material according to claim 1, characterized in that: The specific surface area of the lithium supplement material is 0.3 m 2 / g~20m 2 / g.
12. The lithium supplement material according to claim 1, characterized in that: In the lithium supplement material, the mass proportion of the residual alkali is 0.01% to 1%; And / or, the resistivity of the lithium supplement material is 0.3Ω / cm to 500Ω / cm.
13. The lithium supplement material according to claim 1, characterized in that: The fluorine-containing organic compound includes one or both of polytetrafluoroethylene and fluorine-containing paraffin.
14. A method for preparing a lithium supplement material, characterized in that: include: mixing a lithium-rich compound with a fluorine-containing organic compound to obtain a precursor mixture; The precursor mixture is heat treated to obtain a lithium-supplementing material, wherein the lithium-rich compound forms a lithium-rich core, and the The fluorine-containing organic matter forms a coating layer, and a transition layer is provided between the surface of the lithium-rich core and the coating layer, wherein the transition layer contains lithium fluoride.
15. The preparation method according to claim 14, characterized in that: The temperature for heat treating the precursor mixture is 250° C. to 400° C., and the heat treatment time is 2 h to 10 h.
16. The preparation method according to claim 14, characterized in that: The preparation of the lithium-rich compound comprises: The first metal compound and the second metal compound are mixed in proportion, and then dried, sprayed and crushed to obtain a mixture; sintering the mixture under an inert atmosphere, and crushing it after cooling to obtain a lithium-rich compound; The first metal compound is a lithium salt, and the second metal compound is one or more non-lithium metal salts.
17. The preparation method according to claim 16, characterized in that: The sintering temperature of the mixture is 500° C. to 1000° C., the sintering time is 0.5 h to 10 h, and the heating rate is 100° C. / h to 500° C. / h.
18. The preparation method according to claim 14, characterized in that: After the precursor mixture is heat treated, the method comprises: An oxygen-containing carbon material containing hydroxyl groups is prepared, and the oxygen-containing carbon material and the lithium-rich core having the coating layer are fully mixed to obtain the lithium supplement material, and the oxygen-containing carbon material is coated on the outer surface of the coating layer to form a functional encapsulation layer.
19. A positive electrode plate, characterized in that: The positive electrode plate includes a current collector and an active material layer disposed on the current collector, wherein the active material layer includes the lithium supplement material according to any one of claims 1 to 13; or, the active material layer includes the lithium supplement material obtained by the preparation method of the lithium supplement material according to any one of claims 14 to 18.
20. A secondary battery, characterized in that: The method comprises the positive electrode sheet as claimed in claim 19; or the secondary battery comprises the lithium supplement material as claimed in any one of claims 1 to 13; or the secondary battery comprises the lithium supplement material obtained by the preparation method of the lithium supplement material as claimed in any one of claims 14 to 18.
Citation Information
Patent Citations
Positive electrode lithium supplement additive and preparation method and application thereof
CN115215376A
Lithium supplement additive and preparation method and application thereof
CN115312770A
Positive electrode lithium supplement additive and preparation method and application thereof
CN115312885A
Lithium-rich composite material, preparation method thereof and secondary battery
CN115347153A
Lithium supplement material and preparation method thereof, positive pole piece and secondary battery
CN116314713A