Method for producing substrate stacks for further processing into composite sheets for optical light guide elements

The method of precisely connecting disk-shaped substrates with a controlled adhesive layer addresses the challenge of achieving excellent geometry and optical quality in substrate stacks for augmented reality applications, resulting in improved imaging performance.

WO2024200671A1PCT designated stage expired Publication Date: 2024-10-03SCHOTT AG
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2024/058514
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-28
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing methods for producing substrate stacks for optical light guide elements in augmented reality applications face challenges in achieving excellent geometry and optical quality due to geometric deviations and inadequate adhesive layer control, leading to insufficient imaging quality.

Method used

A method involving the precise connection of disk-shaped substrates with an adhesive layer, where substrates are pretreated, and the adhesive is applied and distributed using spin coating to achieve a thin, uniform layer with controlled viscosity, ensuring high parallelism and quality standards, and subsequent curing to form a stack with improved optical properties.

Benefits of technology

The method produces substrate stacks with enhanced geometric and optical quality, minimizing deviations and improving imaging performance in optical light guide elements for augmented reality applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure EP2024058514_03102024_PF_FP_ABST
    Figure EP2024058514_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a method for producing a stack for further processing into composite sheets, said method comprising bonding two or more sheet-like substrates with an adhesive layer; also to a method for producing a composite sheet and to a composite sheet, preferably for use as an optical light guide element or in an optical light guide element, in particular for use in the field of augmented reality.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Process for producing substrate stacks for further processing into composite discs for optical light guide elements

[0002] Description

[0003] The present invention relates to a method for producing a stack for further processing into composite panes, comprising bonding two or more disc-shaped substrates with an adhesive layer, as well as to a composite pane and a method for producing a composite pane, preferably for use as or in an optical light guide element, in particular for use in the field of augmented reality.

[0004] Fiber optic elements fulfill a central function in imaging optical systems for augmented reality applications. Such imaging optical systems in the field of augmented reality can, for example, be wearable head-mounted systems that present a user with an additional image in their field of vision. The additional image can be used to display additional information to the user in a variety of ways, for example, to show a surgeon invisible elements that were previously recorded using tomography. Other applications relate to navigation, for example in aircraft or vehicles. Diffractive or reflective optical elements can be used here.

[0005] Such imaging optical systems can comprise an eyepiece to visualize images projected onto them for the user. The eyepieces can comprise very thin, preferably highly refractive optical glasses or composites with corresponding very thin optical materials, for example glasses. Light guide elements, particularly when using a composite of several thin optical materials or substrates, must meet high requirements, particularly with regard to the internal quality of the substrates or wafers incorporated therein, as well as a precisely adjusted geometry of the individual substrates and the light guide elements produced from them. Such light guide elements typically comprise a plurality of coated and / or uncoated substrates which are bonded together with an adhesive. Light guide elements are then obtained from the resulting stack by means of singulation steps.Particularly for the use of substrates for such composite components, comprising a large number of such substrates, it is of great importance that the individual substrates meet strict requirements with regard to the aforementioned quality factors. Otherwise, there is a risk that geometric deviations in the individual substrates will accumulate in the resulting light guide elements and lead to inadequate imaging quality. Furthermore, the contributions of the numerous adhesive layers in such a composite must also be taken into account when controlling the geometry and optical properties of the composite.

[0006] It was therefore an object of the present invention to provide a method for producing a stack for further processing into an optical light guide element, which has excellent properties of the stack and the light guide element with regard to geometry and internal and surface quality. It was also an object of the invention to provide an optical light guide element with excellent optical properties.

[0007] The problem was solved by the subject matter of the patent claims.

[0008] This object was achieved in particular by a method for producing a stack for further processing into composite panes, comprising bonding two or more disc-shaped substrates with an adhesive layer, wherein the disc-shaped substrates each have a first and a second surface which are parallel to one another, comprising the steps: a) providing a first disc-shaped substrate, wherein optionally at least the first surface of the first disc-shaped substrate is pretreated by means of cleaning, plasma treatment and / or application of an adhesion promoter, b) applying an adhesive with a first viscosity to the first surface of the first substrate and rotating the first substrate, wherein the adhesive is distributed on the first surface of the first substrate, and wherein the resulting adhesive layer has a layer thickness of 0.2 μm to 5.0 μm,c) optionally varying the viscosity of the adhesive by heating or cooling, d) joining the first disc-shaped substrate to a second disc-shaped substrate to form a first stack, comprising bringing the first surface of the first substrate into contact with the second surface of the second substrate and curing the adhesive layer.

[0009] "Parallel" in the context of the present invention means that two surfaces have a parallelism of no more than 280 arcsec, preferably no more than 250 arcsec, preferably no more than 200 arcsec, or no more than 180 arcsec, preferably no more than 150 arcsec, preferably no more than 120 arcsec in both spatial directions, independently of each other. The parallelism is preferably determined as follows:

[0010] 1. A surface is approximated by regression of a mathematically perfect two-dimensional plane such that the deviations of the real topography of the surface from the regression plane are minimized in both spatial directions. 2. Another surface is approximated by regression of a mathematically perfect two-dimensional plane such that the deviations of the real topography of the other surface from the regression plane are minimized in both spatial directions.

[0011] 3. The angle between the two mathematically perfect planes is then determined for both spatial directions.

[0012] Preferably, the first and second surfaces of the disc-shaped substrates have a parallelism of no more than 90 arcsec, preferably no more than 60 arcsec or no more than 50 arcsec, further preferably no more than 40 arcsec or no more than 30 arcsec, particularly preferably no more than 20 arcsec for both spatial directions independently of one another. This applies regardless of whether the first and / or second surface is provided with an inorganic coating.

[0013] Preferably, the first and the first surfaces of the stack according to the invention have a parallelism of no more than 120 arcsec, preferably no more than 110 arcsec or no more than 100 arcsec, further preferably no more than 90 arcsec or no more than 80 arcsec, particularly preferably no more than 60 arcsec or no more than 50 arcsec, likewise preferably no more than 40 arcsec or no more than 30 arcsec for both spatial directions independently of one another. This applies regardless of whether the first and / or the second surface is provided with an inorganic coating.

[0014] The parallelism of the surfaces of the disc-shaped substrates or the stack can be determined, for example, within the volume of the stack using an autocollimator. Preferably, the parallelism at the edges of the stack is determined using a videometric or optical measurement, for example, using a coordinate measuring machine, such as a Zeiss O-Inspect multisensor measuring machine from Carl Zeiss AG. In the method according to the invention, two or more disc-shaped substrates, hereinafter also referred to as "substrates," are bonded together, resulting in a stack comprising at least two disc-shaped substrates.

[0015] Disc-shaped substrates according to the present invention each have a first and a second surface which are parallel to one another. The first and second surfaces of a substrate are the so-called "main surfaces". It is clear to those skilled in the art that the disc-shaped substrates also comprise at least one lateral surface. The distance from the first to the second surface of the substrate is also referred to below as the thickness of the substrate. The disc-shaped substrates preferably have a thickness of 0.2 mm to 2.0 mm, preferably of 0.3 mm to 1.8 mm, more preferably of 0.4 to 1.7 mm and particularly preferably of 0.5 to 1.5 mm.

[0016] The disc-shaped substrates are preferably round or square, preferably angular, particularly preferably rectangular or square.

[0017] If the disc-shaped substrates are square substrates, they have a length and / or width of 10 mm to 300 mm, preferably of 20 mm to 150 mm, further preferably of 30 mm to 100 mm, for example of 50 mm to 80 mm.

[0018] Round disc-shaped substrates preferably have a diameter of 10 mm to 300 mm, preferably 15 mm to 200 mm, preferably 20 mm to 150 mm, further preferably 30 mm to 100 mm, for example 50 mm to 80 mm. The thicknesses of the disc-shaped substrates in a stack can be different or the same.

[0019] The disc-shaped substrates preferably comprise or consist of a glass, a glass-ceramic, an optoceramic, or a plastic, preferably a glass and / or a plastic, particularly preferably a glass. The disc-shaped substrates preferably consist of a glass or a plastic, particularly preferably a glass. Preferably, it is a glass with a refractive index nd in the range from 1.45 to 2.30, preferably from 1.47 to 2.10, more preferably from 1.50 to 2.00, likewise preferably from 1.47 to 1.8.

[0020] Preferably, the disc-shaped substrates comprise a material which is transparent at least for one wavelength in the range from 450 nm to 650 nm, preferably transparent for all wavelengths in the range from 450 nm to 650 nm.

[0021] In some embodiments, the stack produced according to the invention comprises disc-shaped substrates made of different materials, but preferably all disc-shaped substrates in a stack produced according to the invention comprise the same material, preferably all disc-shaped substrates in a stack produced according to the invention consist of the same material.

[0022] In embodiments in which at least one disc-shaped substrate comprises or consists of a glass, the glass is preferably a silicate glass, e.g., a barium-containing silicate glass. For example, the substrate may comprise or consist of a flint glass or crown glass. Optionally, the glass is selected from an alkaline earth-containing flint glass, a barium flint glass, a barium crown glass, a boron-containing crown glass, a lanthanum flint glass, a lanthanum crown glass, and combinations thereof. Preferably, the disc-shaped substrates satisfy at least one of the following conditions: i) a total thickness variation of less than 10 pm; ii) Bow < 100 pm; iii) Warp < 100 pm; iv) Roughness Rq < 5 nm.

[0023] The disc-shaped substrates can be uncoated or have an inorganic coating on one or two surfaces.

[0024] Preferably, at least 50%, preferably at least 60% or at least 70%, preferably at least 80%, particularly preferably at least 90% or 100% of the disc-shaped substrates in the stack produced according to the invention satisfy at least one of the conditions i) to iv), preferably at least two of the conditions i) to iv), preferably at least three of the conditions i) to iv) and particularly preferably all conditions i) to iv).

[0025] The disk-shaped substrates preferably have a total thickness variation, hereinafter also referred to as “Total Thickness Variation” or “TTV,” of less than 10 pm, preferably less than 8 pm, preferably less than 5 pm, more preferably less than 4 pm, furthermore preferably less than 3 pm, particularly preferably less than 2 pm or less than 1 pm, furthermore particularly preferably less than 0.75 pm, likewise particularly preferably less than 0.5 pm. The total thickness variation can be determined, for example, according to SEMI MF 1530GBIR. The total thickness variation can also be determined by means of interferometric measurements of the thickness profile of the disk-shaped substrates, for example using an interferometer, in particular an interferometer from Zygo Corporation. In some embodiments, the disk-shaped substrates have a TTV of at least 0.1 pm or at least 0.2 pm.Disc-shaped substrates with a low TTV are particularly advantageous for the use of the manufactured stacks or the optical fiber elements manufactured from them in augmented reality applications. Disc-shaped substrates with a low TTV can be produced, for example, using suitable abrasive processes such as grinding, lapping, and / or polishing and / or using ion beam processing as described in German patent application DE 10 2021 125 476.

[0026] Preferably, the first and / or the second surfaces, preferably the first and the second surfaces of the disc-shaped substrates for producing the stack according to the invention have a roughness Rq of 0.1 nm to 5 nm, preferably not more than 5 nm, preferably less than 5 nm, preferably less than 4 nm or less than 3 nm, further preferably less than 2 nm or less than 1.5 nm or particularly preferably less than 1 nm or less than 0.5 nm.

[0027] In this context, the roughness Rq means the quadratic roughness, also called RMS (root mean squared) and can be measured, for example, using a white light interferometer or AFM technology, preferably according to DIN EN ISO 4287.

[0028] The disc-shaped substrates for producing a stack according to the invention preferably have a warp of more than 1 pm, more than 5 pm or more than 10 pm, and / or less than 100 pm, preferably less than 50 pm, furthermore preferably less than 20 pm and / or a bow of more than 1 pm, more than 5 pm or more than 10 pm, and / or less than 100 pm, preferably less than 50 pm, furthermore preferably less than 20 pm. The disc-shaped substrates preferably have a bow and / or a warp of less than 0.1%, preferably less than 0.075%, preferably less than 0.05%, preferably less than 0.01% of the substrate diameter. Warp and bow are preferably determined according to SEMI3D1203152015. Warp and bow are parameters used to express the shape of a disc-shaped substrate that is resting on something and is therefore not held by, for example, a chuck.The substrate is therefore held force-free or rests on a flat surface. The center surface in the thickness direction of the substrate acts as the measuring plane, with the plane that best fits the measuring plane being assumed to be a reference plane. The bending represents the maximum value of the offset from the reference plane to the measuring plane. The warping represents the difference between the reference plane and the measuring plane at the center of the substrate. If the substrate is held by a locally limited support, such as a 3-point mount or fork mount in the edge area, additional bending occurs under the influence of gravitational forces, which is referred to as sagging. The extent of this bending depends essentially on the geometric arrangement of the support. The mechanical properties of the material and the geometric shape of the substrate are also parameters that determine sagging.

[0029] In a first step a) of the method according to the invention, a first disc-shaped substrate, hereinafter also referred to as “first substrate”, is provided, comprising a first and a second surface, wherein the first and the second surface are parallel to each other.

[0030] In some embodiments, at least the first surface of the first disc-shaped substrate is pretreated by cleaning, plasma treatment, and / or the application of an adhesion promoter. The person skilled in the art selects the type of pretreatment depending on the material from which the first disc-shaped substrate is formed. In advantageous embodiments of the method according to the invention, at least the first surface of the first substrate and / or the second surface of the first substrate is cleaned, in particular by wet-chemical cleaning, for example with distilled or deionized water, with an aqueous solution of an acid, with an aqueous solution of a base, or with an organic solvent, preferably with distilled or deionized water.

[0031] In advantageous embodiments of the method according to the invention, a plasma treatment of at least the first surface of the substrate is carried out, preferably after cleaning the first and optionally the second surface of the first substrate. This allows the first and optionally the second surface of the first substrate—optionally after wet-chemical cleaning—to be cleaned and / or modified and thereby activated, preferably increasing the wettability of the first surface.

[0032] In advantageous embodiments of the method according to the invention, an adhesion promoter is applied to the first surface of the first substrate, preferably after cleaning the first and optionally the second surface of the first substrate and / or after plasma treatment of the first surface and optionally the second surface of the first substrate.

[0033] Such adhesion promoters, also referred to as “primers” in the following, serve to act as an adhesive bridge between the first substrate and the adhesive and thereby improve adhesion.

[0034] The adhesion promoter is preferably a silane adhesion promoter, preferably of the general formula R-SiXs, where R is preferably an organically functionalized radical and X is preferably a hydrolyzable group, for example an alkoxy group. The person skilled in the art selects suitable adhesion promoters depending on the adhesive used. The adhesion promoter is preferably applied to the first surface of the first disc-shaped substrate as a monolayer and / or preferably with a layer thickness of less than 20 nm, preferably less than 15 nm, more preferably less than 10 nm, more preferably less than 5 nm, less than 3 nm, and likewise preferably less than 1 nm.

[0035] In step b) of the method according to the invention, an adhesive is applied to the - optionally pretreated - first surface of the first disc-shaped substrate and distributed on the first surface of the substrate by rotating the first substrate.

[0036] This process is also referred to as “rotational coating” or “spin coating”.

[0037] For this purpose, the first substrate is preferably placed on a rotatable substrate carrier (also called a “spin chuck”). The adhesive is applied to the first surface of the first substrate near the center, i.e. the axis of rotation. By so-called “spinning off” the excess adhesive, a thin film, i.e. an adhesive layer, is created on the first surface of the first substrate. The layer thickness of the adhesive film created is determined by the viscosity of the adhesive and the number of revolutions during spin coating. Typically, spin coating is carried out at a speed of up to 9000 rpm (“rounds per minute”). In an advantageous embodiment, spin coating is carried out at room temperature.In some embodiments, spin coating is performed at a temperature higher than room temperature, preferably at a temperature of at least 30°C, at least 40°C, at least 50°C, at least 60°C, at least 70°C, at least 80°C, at least 90°C, or at least 100°C. This can be particularly advantageous if the adhesive does not have a sufficiently low viscosity at room temperature. Spin coating is preferably performed at room temperature and / or under clean room conditions.

[0038] Preferably, an adhesive layer is formed on at least part of the first surface, preferably on the entire first surface of the first substrate. The adhesive layer has a thickness of 0.2 μm to 5.0 μm, preferably 0.5 μm to 4.5 μm, more preferably 1.0 μm to 4.0 μm, more preferably 1.5 μm to 3.5 μm, particularly preferably 2.0 μm to 3.0 μm. The adhesive layer has a homogeneous thickness over the entire area of ​​the first surface of the first substrate covered thereby.

[0039] Preferably, the adhesive layer satisfies at least one of the following conditions: i) a total thickness variation (TTV) of less than 20 pm; ii) no inclusions with a particle size which is higher than the thickness of the adhesive layer; iii) a refractive index nd which deviates from the refractive index nd of the disc-shaped substrates by no more than 0.005, preferably no more than 0.004, preferably no more than 0.003, or no more than 0.002, particularly preferably no more than 0.001.

[0040] According to the invention, the adhesive layer has a total thickness variation, hereinafter also referred to as “Total Thickness Variation” or “TTV”, of less than 20 pm, preferably less than 15 pm, furthermore preferably less than 12 pm, furthermore preferably less than 10 pm, likewise preferably less than 7 pm, preferably less than 5 pm, preferably less than 4 pm or less than 3 pm, preferably less than 2.5 pm or less than 2 pm, preferably less than 1.5 pm or less than 1 pm, particularly preferably less than 0.75 pm, furthermore preferably less than 0.5 pm, furthermore particularly preferably less than 0.3 pm or 0.2 pm. The above explanations regarding the significance of determining the TTV apply analogously here.

[0041] Preferably, the adhesive does not contain any inclusions with a particle size larger than the thickness of the adhesive layer. Inclusions within the meaning of the present invention include, for example, impurities and bubbles, such as air bubbles.

[0042] The term "adhesive" in the sense of the present invention encompasses both solvent-free adhesives and adhesive solutions. Reference to "adhesive" below encompasses both solvent-free adhesives and adhesive solutions. Suitable adhesives include acrylate adhesives, epoxy adhesives, silicone adhesives, polyurethane adhesives, nanoparticle-filled acrylate adhesives, nanoparticle-filled epoxy adhesives, nanoparticle-filled silicone adhesives, nanoparticle-filled polyurethane adhesives, and sol-gel adhesive systems. The adhesive is preferably an acrylate adhesive, an epoxy adhesive, a silicone adhesive, or a polyurethane adhesive, or solutions thereof, particularly preferably an acrylate adhesive or solutions thereof.

[0043] The adhesive can be a light-curing adhesive, a heat-curing adhesive, or an anaerobic-curing adhesive. It is preferably a light-curing adhesive, preferably a UV-curing adhesive. The adhesive is preferably a light-curing, preferably UV-curing, acrylate adhesive.

[0044] The adhesive preferably has a refractive index nd that deviates from the refractive index nd of the disc-shaped substrates by no more than 0.005, preferably no more than 0.004, preferably no more than 0.003, or no more than 0.002, particularly preferably no more than 0.001. Light-curing adhesives cure by irradiation with light of a suitable wavelength. It is preferably a UV-curing adhesive. Such UV-curing adhesives cure by irradiation with UV light. UV-curing adhesives suitable for the process according to the invention preferably cure at room temperature. Preferably, the UV-curing adhesive is an optically clearer adhesive, which preferably has a refractive index nd that essentially corresponds to the refractive index nd of the disc-shaped substrates, and which preferably has low shrinkage upon curing.In this way, stresses in the stack produced according to the invention can be avoided or at least minimized.

[0045] According to the invention, an adhesive having a first viscosity is applied to the first surface of the first substrate. The skilled person selects an adhesive having a viscosity sufficiently low to ensure a homogeneous distribution of the adhesive on the first surface of the first substrate during the spin-coating process.

[0046] The adhesive preferably has a first viscosity of not more than 1500 mPas, preferably not more than 1000 mPas or not more than 900 mPas, preferably not more than 800 mPas or not more than 700 mPas, further preferably not more than 600 mPas or 500 mPas, particularly preferably not more than 400 mPas and / or at least 20 mPas, preferably at least 25 mPas, preferably at least 50 mPas, further preferably at least 100 mPas. If the adhesive has an excessively high viscosity, it can preferably be used as an adhesive solution with a first viscosity in the stated ranges. Solvents for preparing adhesive solutions are, in particular, organic solvents, in particular ethers or alcohols, e.g., isobutyl alcohol or tetrahydrofurfuryl.

[0047] The adhesive is preferably applied to the center of the first surface of the first substrate. Optionally, the method according to the invention comprises a step c), wherein the viscosity of the adhesive is varied by heating or cooling. In one embodiment of the method according to the invention, step c) takes place while the adhesive is distributed on the first surface of the first substrate by rotating the first substrate. Here, for example, the viscosity of the adhesive can be reduced in order to achieve optimal distribution on the first surface or to control the thickness of the resulting adhesive layer. Alternatively or additionally, the viscosity is varied after the rotation of the applied adhesive or the applied adhesive layer has ended, after the rotation of the first substrate has ended. Preferably, step c) of the method according to the invention comprises heating or cooling.If the spin-coating process is carried out at temperatures above room temperature, in one advantageous embodiment, the viscosity of the adhesive is varied, in particular increased, by cooling to, for example, room temperature. In another embodiment, the first surface of the first substrate provided with an adhesive layer is preferably heated. This heating step is also called "soft baking." The temperature is selected such that a sufficient increase in the viscosity of the adhesive layer is achieved. If the adhesive is an adhesive solution, soft baking takes place at a temperature sufficiently high to remove the solvent.Depending on the solvent in the adhesive solution applied to the first surface of the first substrate, the soft baking can be carried out at a temperature of more than 50°C and / or not more than 300°C, not more than 150°C, preferably not more than 120°C.

[0048] According to the invention, the method comprises step d), wherein the first disc-shaped substrate provided with an adhesive layer is joined to a second disc-shaped substrate to form a first stack, comprising bringing the first surface of the first substrate into contact with the second surface of the second substrate and curing the adhesive layer.

[0049] It is understood that the second surface of the second substrate is brought into contact with the adhesive layer on the first surface of the first substrate.

[0050] Preferably, the first and second substrates are bonded to each other over their entire surface with an adhesive layer.

[0051] Typically, the bonding of the first substrate to the second substrate takes place at room temperature and / or under application of pressure, preferably less than 5 Mpa, preferably less than 3 Mpa, further preferably less than 2 Mpa and particularly preferably less than 1 Mpa.

[0052] The curing of the adhesive layer depends on the adhesive used, for example by irradiation with light, in particular UV light, for example with a wavelength of 400 nm.

[0053] After the adhesive layer has cured, a first stack is obtained, comprising a first disc-shaped substrate and a second disc-shaped substrate, which are bonded together by means of an adhesive layer. A further step can then be performed in which the first stack is heated. This can serve, in particular, to increase the strength of the bond through the adhesive layer, for example, through stronger crosslinking in the adhesive layer. This step is also called "hardbaking."

[0054] The method according to the invention preferably comprises joining the first stack to a third disc-shaped substrate (hereinafter also referred to as “third substrate”), comprising the following steps: a1) providing a third disc-shaped substrate, wherein optionally at least the first surface of the third disc-shaped substrate is pretreated by cleaning, plasma treatment and / or applying an adhesion promoter, b1) applying an adhesive having a first viscosity to the first surface of the third substrate and rotating the third substrate, wherein the adhesive is distributed on the first surface of the third substrate, and wherein the resulting adhesive layer has a layer thickness of 0.2 μm to 5.0 μm, c1) optionally varying the viscosity of the adhesive by heating or cooling, d1) joining the third disc-shaped substrate to the first stack,comprising bringing the first surface of the third substrate into contact with a surface of the first stack and curing the adhesive layer, thereby obtaining a second stack.

[0055] After curing of the adhesive layer, a second stack is obtained which comprises a first, a second and a third disc-shaped substrate, wherein the first and the second substrate as well as the second and the third substrate are each connected with an adhesive layer.

[0056] The method according to the invention preferably comprises joining the second stack to a further disc-shaped substrate (hereinafter also referred to as “further substrate”), for which purpose the above-mentioned steps a1) to d1) are repeated, the second stack being used as the first stack and a further stack being obtained. This produces a further stack comprising four disc-shaped substrates which are joined by means of three adhesive layers. This can be repeated as often as desired until the desired stack comprising 2 to 50, preferably 4 to 45, further preferably 6 to 35 or 6 to 30, particularly preferably 8 to 25 or 8 to 20 disc-shaped substrates is obtained, wherein in each case a further substrate is subjected to steps a1), b1) and c1) and then in step d1) is joined to an existing further stack which is used as the first stack.

[0057] The preferred embodiments and explanations in connection with the production of the first stack apply accordingly to the production of the second and each subsequent stack.

[0058] Particularly in embodiments in which the stack produced according to the invention comprises a comparatively large number of disc-shaped substrates, it may be advantageous to first produce several further stacks by means of the method according to the invention and then to glue them together.

[0059] Preferably, the stack produced according to the invention comprises at least one disc-shaped substrate which has an inorganic coating on the first and / or the second surface.

[0060] The inorganic coating may comprise one or more layers; preferably, the coating comprises at least two layers. The inorganic coating preferably comprises 2 to 100 layers, preferably 4 to 50 layers, preferably 5 to 40 layers, and particularly preferably 7 to 35 layers.

[0061] Preferably, the inorganic coating comprises one or more components selected from one or more oxides, one or more fluorides, one or more nitrides, one or more sulfides, one or more selenides, one or more metals, and combinations of two or more thereof. For example, the inorganic coating comprises or consists of one or more components selected from one or more metal oxides, one or more metal fluorides, one or more metal nitrides, one or more metal sulfides, one or more metal selenides, and combinations of two or more thereof. Oxides according to the present invention are preferably selected from silicon oxide, aluminum oxide, hafnium oxide, tantalum oxide, niobium oxide, titanium oxide, zirconium oxide, yttrium oxide, praseodymium oxide, scandium oxide, tin oxide, chromium oxide, indium oxide, and combinations of two or more thereof.In some embodiments, combinations of two or more oxides comprise mixed oxides.

[0062] Fluorides according to the invention are preferably selected from aluminum fluoride, magnesium fluoride, neodymium fluoride, lanthanum fluoride, yttrium fluoride, gadolinium fluoride, ytterbium fluoride and combinations of two or more thereof.

[0063] Nitrides within the meaning of the present invention are preferably selected from aluminum nitride, silicon nitride, and combinations thereof. Sulfides within the meaning of the present invention are, for example, zinc sulfide. Selenides within the meaning of the present invention are, for example, zinc selenides. Metals within the meaning of the present invention are preferably selected from aluminum, silver, gold, chromium, nickel, and combinations thereof. Optionally, the combination of two or more metals is an alloy. The metallic layer preferably has a thickness of no more than 10 nm to ensure sufficient transparency.

[0064] In an advantageous embodiment, the inorganic coating comprises at least one dielectric layer; preferably, all layers of the inorganic coating are dielectric layers. In a further advantageous embodiment, the inorganic coating comprises at least one metallic layer consisting of or comprising at least one metal, for example, Ag, wherein the at least one metallic layer has a thickness of no more than 10 nm.

[0065] The inorganic coating preferably has a thickness of 200 nm to 2000 nm, preferably of 300 nm to 1900 nm, further preferably of 400 nm to 1800 nm or 500 to 1700 nm, particularly preferably of 600 nm to 1600 nm.

[0066] In preferred embodiments, the inorganic coating is a multilayer coating comprising two or more layers, wherein the respective layers have a thickness of 1 nm to 200 nm, from 4 to 100 nm, from 8 nm to 800 nm, from 10 nm to 700 nm, from 15 nm to 600 nm or from 15 nm to 500 nm.

[0067] Preferably, the inorganic coating has a refractive index of 1.45 to 3.00, of 1.47 to 2.50, of 1.50 to 2.00 or of 1.51 to 1.90 or of 1.60 to 1.90.

[0068] In advantageous embodiments, the inorganic coating has a refractive index that corresponds to the refractive index of the substrate. The ratio of the refractive index of the substrate to the refractive index of the inorganic coating is preferably between 0.9 and 1.1, preferably between 0.95 and 1.05, and further preferably between 0.98 and 1.03.

[0069] Preferably, the refractive index of the inorganic coating is the average refractive index of the coating. For example, the following formula can be used to determine the average refractive index n of the coating for a total thickness of the coating, where the local refractive index of the coating / its layers is n(x): n = J^nCx) dx / dx .

[0070] The stack produced according to the invention has a first and a second surface and at least one interface. Interface, within the meaning of the present invention, refers to the area between two disc-shaped substrates and, depending on the manufacturing process, can have an adhesive layer and preferably one or two inorganic coatings. Preferably, the interface between two disc-shaped substrates comprises an adhesive layer and an inorganic coating.

[0071] Preferably, the stack produced according to the invention comprises alternating disc-shaped substrates and inorganic coatings - without taking the adhesive layers into account.

[0072] Preferably, the stack according to the invention comprises, alternatingly—without taking the adhesive layers into account—a disc-shaped substrate (S) and an inorganic coating (B), wherein the combination (SB) is repeated x times. In other words, the stack (SB) comprises x . In this embodiment, the first or second surface of the stack is uncoated. In some embodiments, the stack comprises the sequence (SB)xS. In these embodiments, the first and second surfaces of the stack are uncoated. In some embodiments, the stack comprises the sequence B-(S-B) xIn these embodiments, the first and second surfaces of the stack are coated. The production of stacks according to the invention, comprising alternating layers of a disc-shaped substrate and an inorganic coating, is preferably carried out in one embodiment by bonding a plurality of disc-shaped substrates, each of which is coated on a first or second surface with an inorganic coating.

[0073] In another embodiment, the production of a stack according to the invention comprises the alternating bonding of disc-shaped substrates having an inorganic coating on the first and second surfaces with disc-shaped substrates having no coating on the first and second surfaces.

[0074] It is also possible to combine both methods, in particular to control whether the first and / or second surface of the stack is coated or uncoated.

[0075] In one embodiment of the method according to the invention, the first and second surfaces of the first substrate are uncoated, and the first and second surfaces of the second substrate are coated. In other words, the method in this embodiment comprises joining a disc-shaped substrate comprising two uncoated surfaces to a disc-shaped substrate coated on the first and second surfaces to form a first stack. In embodiments in which the stack comprises more than two disc-shaped substrates, the first stack is preferably joined to a third substrate, the first and second surfaces being coated, to form a second stack. Alternatively, the first and second surfaces of the first substrate are uncoated, and the first and second surfaces of the second substrate are coated.In other words, the method in this embodiment comprises bonding a disc-shaped substrate comprising two uncoated surfaces to a disc-shaped substrate coated on the first and second surfaces to form a first stack. In embodiments in which the stack comprises more than two disc-shaped substrates, the first stack is preferably bonded to a third substrate, wherein the first and second surfaces are coated, to form a second stack.

[0076] In one embodiment of the stack according to the invention, all coated surfaces comprise the same inorganic coating. In another embodiment, all coated surfaces have different inorganic coatings. In a further embodiment, some coated surfaces of the disc-shaped substrates have the same inorganic coatings, and other coated surfaces of the disc-shaped substrates have different inorganic coatings.

[0077] When we talk about the same coating here, we mean an inorganic coating which essentially has the same materials, the same layer sequence of materials in the same layer thickness and the same total layer thickness.

[0078] In a further aspect, the invention relates to a stack, preferably produced or producible by means of the method according to the invention.

[0079] The stack produced according to the invention has a first surface and a second surface, wherein the first and second surfaces are parallel to one another. Preferably, the first and second surfaces of the stack are parallel to the first and second surfaces of the respective disc-shaped substrates. The first and / or second surface of the stack can be coated or uncoated. In some embodiments, the first and second surfaces of the stack are coated, preferably with an inorganic coating. In other embodiments, the first and second surfaces of the stack are uncoated. In further embodiments, the first or second surface of the stack is coated, preferably with an inorganic coating.

[0080] The stack according to the invention preferably comprises 2 to 50, preferably 4 to 45, further preferably 6 to 35 or 6 to 30, particularly preferably 8 to 25 or 8 to 20 disc-shaped substrates.

[0081] In some embodiments, the thicknesses of the disc-shaped substrates in a stack may vary. Preferably, all disc-shaped substrates have the same thickness.

[0082] In one embodiment of the method according to the invention or of the stack according to the invention, the disc-shaped substrates are stacked with edge-to-edge precision, i.e., the disc-shaped substrates are connected to one another in such a way that the edges of all substrates are essentially flush with one another. The stack thus obtained is also referred to below as a "straight stack."

[0083] Alternatively, the disc-shaped substrates can be stacked offset from one another, resulting in what is referred to as a "slanted stack." Further explanations regarding straight stacks and slanted stacks can be found in the accompanying figures.

[0084] In a further aspect, the invention comprises a method for producing a composite pane, as well as a composite pane, preferably for use as or in an optical light guide element.

[0085] The composite pane according to the invention comprises a first surface and a second surface which are parallel to one another, as well as at least one side surface, and two or more disc-shaped substrates, each having a first and a second surface which are parallel to one another, wherein the at least two disc-shaped substrates are connected by at least one adhesive layer.

[0086] The first and second surfaces of the disc-shaped substrates are preferably parallel to the first and second surfaces of the composite disc. The above statements regarding parallelism apply analogously here.

[0087] The explanations and preferred embodiments mentioned in connection with the method according to the invention apply analogously in connection with the composite pane according to the invention and the subsequent manufacturing process of the composite pane according to the invention, as far as applicable.

[0088] Preferably, the method for producing a composite pane comprises the following steps: a) providing a stack, preferably produced or producible according to the method described above, b) dividing the stack, preferably by cutting the stack, whereby at least one composite pane is obtained, c) optionally polishing the resulting composite pane.

[0089] In step a), a stack is provided, which is preferably produced using the manufacturing method described in detail above. If the stack comprises round, disc-shaped substrates, the round stack can optionally be cut in a first step to produce a square stack.

[0090] Step b) of the method comprises dividing the stack, preferably by cutting the stack, wherein the division can comprise several cutting steps, and wherein at least one composite disc is obtained. Depending on the cutting step, the composite disc can have one or more side surfaces. Preferably, the composite disc comprises one side surface or four side surfaces. The division takes place from the first to the second surface or from the second to the first surface of the stack. The discs obtained thereby naturally have the same number and layer sequence with regard to the disc-shaped substrates, adhesive layers and optionally inorganic coatings, as well as the same materials as the original stack. The disc has a first surface which was part of the first surface of the stack, and a second surface which was part of the second surface of the stack.If multiple cutting steps are performed, these always occur from one surface of the original stack to the other surface of the stack.

[0091] The division steps can be carried out in such a way that cuboid-shaped discs or cuboid composite discs are obtained. Preferably, a straight stack is divided, with the cut edge being orthogonal to the first and second surfaces of the stack. This results in a so-called "straight composite disc." In another embodiment, the division steps are carried out in such a way that the cut edge is not orthogonal to the first and second surfaces, resulting in a so-called "slanted composite disc." This is preferably done with slanted stacks and reduces waste by minimizing the unusable portions.

[0092] The cutting steps can be carried out in such a way that cylindrical composite discs are obtained.

[0093] The composite panes according to the invention are preferably used as an optical light guide element or in an optical light guide element. In some embodiments, the composite pane obtained in step b) is combined, preferably glued, with other optical components to form a block in a further step b1), and the resulting block is then subjected to one or more division steps, thereby obtaining a light guide element. Preferably, the main surfaces of the resulting light guide element comprise, at least in some regions, side surfaces of the composite pane.

[0094] Preferably, the composite discs obtained in step b) or the optical fiber elements obtained in step b1) are polished in step c).

[0095] Preferably, at least one, preferably at least two, side surfaces of the composite panes obtained in step b) are polished. Preferably, two opposite side surfaces of the composite pane are polished.

[0096] If the method comprises step b1), in step c), preferably at least the regions of the main surfaces that comprise side surfaces of the composite pane are polished. The following explanations in connection with the side surfaces of the composite panes apply analogously to the regions of the main surface of the light guide elements that comprise the side surfaces of the composite pane.

[0097] In a further aspect, the invention therefore encompasses a light guide element comprising the composite pane according to the invention. The light guide element preferably has a first and a second main surface, which are preferably parallel to one another, wherein the first and / or second main surface of the light guide element comprises side surfaces of the composite pane.

[0098] Polishing the side surfaces can result in the polished surface having depressions and elevations. This occurs when the stack comprises layers of different hardness. For example, many materials suitable for the disc-shaped substrates, and in particular typical inorganic coatings, have a significantly greater hardness than the adhesive layer. Accordingly, the polished surfaces typically have depressions, also referred to as "dig-ins" in the following, in the adhesive layer and / or elevations in the substrate layers and in particular in the coating layers. Such elevations and depressions can lead to disadvantageous properties of the optical light guide elements because they cause undesirable light scattering. Polishing is preferably carried out in step d), whereby controlled conditions must be maintained in order to minimize or avoid the formation of elevations and depressions.

[0099] The composite pane according to the invention preferably has depressions or elevations of no more than 1 pm, preferably no more than 300 nm, preferably no more than 150 nm, preferably no more than 120 nm, and further preferably no more than 100 nm. The measurement is carried out, for example, using an AFM or a white-light interferometer. If an elevation or depression is referred to, it is measured from the otherwise flat side surface of the substrates in the composite pane ("zero line").

[0100] The composite pane preferably meets at least one of the following conditions: i) the first and / or the second surface of the composite pane has a roughness Rq of < 5 nm; ii) the composite pane has a TTV of less than 10 pm based on the first and the second surface of the composite pane; iii) the composite has a warp of < 100 pm based on the first and the second surface of the composite pane; iv) the composite has a bow of < 100 pm based on the first and the second surface of the composite pane. According to the invention, the composite comprises at least 2 and preferably no more than 100 disc-shaped substrates. In advantageous embodiments, the composite comprises 2 to 50, preferably 4 to 45, further preferably 6 to 35 or 6 to 30, particularly preferably 8 to 25 or 8 to 20, further particularly preferably from 6 to 15 disc-shaped substrates.

[0101] The invention is described in more detail below using preferred embodiments and with reference to the accompanying drawings.

[0102] Fig. 1 shows schematically the manufacture of a stack according to the invention.

[0103] Fig. 2 shows a first embodiment of a stack which alternately contains substrate and coating.

[0104] Fig. 3 shows a second embodiment of a stack which alternately contains substrate and coating.

[0105] Fig. 4a and Fig. 4b show a stack in which the substrates are stacked offset from each other.

[0106] Fig. 5a and Fig. 5b show schematically the division of a straight and an inclined stack

[0107] In the following detailed description, identical reference numerals in the various embodiments designate identical or equivalent assemblies and components. Where significant functional differences exist, these will be explained in more detail with reference to the respective embodiment.

[0108] Fig. 1 schematically depicts the side view of an embodiment of the method according to the invention for producing a stack 1. The surfaces of the disc-shaped substrates can have an inorganic coating or be free of a coating. For reasons of clarity, however, optional inorganic coatings are not depicted in Fig. 1. In a first step, a first disc-shaped substrate 21, comprising a first surface 411 and a second surface 412, is provided with an adhesive layer 3 on the first surface 411. Preferred embodiments of the method steps required for this, such as cleaning, pretreatment and / or application of an adhesion promoter layer, as well as optionally varying the viscosity of the adhesive layer 3 by heating or cooling, have already been explained above and apply here accordingly.The first substrate 21, comprising an adhesive layer 3 on the first surface 411, is then brought into contact with the second surface 422 of a second substrate 22 and preferably bonded over their entire surface, thereby obtaining a first stack 11. If a stack comprising only two disc-shaped substrates is to be produced, the first stack 11 corresponds to stack 1. Stack 11, or stack 1, has a first surface 101, which corresponds to the second surface 412 of the first substrate 21, and a second surface 102, which corresponds to the first surface 421 of the second substrate 22.If the first stack 11 is not the final stack 1, a further step involves connecting the first stack 11 to a third disc-shaped substrate 23, comprising a first surface 431 and a second surface 432, to form a second stack 12, or - if the final stack is to comprise three disc-shaped substrates - to form a stack 1. Preferably, the second surface 432 of the third substrate 23 is provided with an adhesive layer 3 and connected to the first surface 101 (not shown) or the second surface 102 of stack 11, preferably over its entire surface. Alternatively, in an embodiment not shown, the second surface 102 of the first stack 11 can be provided with an adhesive layer 3. In order to avoid process-related difficulties during rotation orIn order to avoid spin coatings, the adhesive layer 3 is preferably always applied to the surface of a substrate that has not yet been connected to another disc-shaped substrate. In a further step, the second stack 12 can be connected to a further disc-shaped substrate 24, comprising a first surface 441 and a second surface 442, to form a further stack 13 or - if the final stack is to comprise four disc-shaped substrates - to form a stack 1. Preferably, the second surface 442 of the further substrate is first provided with an adhesive layer 3 and connected to the first surface 101 (not shown) or the second surface 102 of stack 12, preferably over its entire surface. The described steps are repeated until stack 1 comprises the desired number of disc-shaped substrates.

[0109] Fig. 2 shows a schematic side view of an embodiment of the layer sequence in stack 1. The resulting stack 1 alternately comprises a disk-shaped substrate 2, 21, 22, 23, 24 and an inorganic coating 5. In the embodiment shown, a first substrate 21, comprising an inorganic coating 5 on the first surface 411, is successively connected to further disk-shaped substrates 22, 23, 24, each having an inorganic coating 5 on the first surfaces 421, 431, 441, via the method steps described in connection with Fig. 1. In an alternative embodiment not shown, the stack alternately comprises an inorganic coating 5 and a disk-shaped substrate 2, 21, 22, 23, 24.For this purpose, a first substrate 21 comprising an inorganic coating 5 on the second surface 412 is successively connected via the method steps described above to further disc-shaped substrates 22, 23, 24, which each have an inorganic coating 5 on the second surfaces 422, 432, 442.

[0110] Fig. 3 shows a schematic side view of an embodiment of the layer sequence in stack 1. The resulting stack 1 alternately comprises a disk-shaped substrate 2, 21, 22, 23, 24 and an inorganic coating 5. In the embodiment shown, for this purpose, an uncoated first substrate 21 is first connected to a second substrate 22, comprising an inorganic coating 5 on the first surface 421 and the second surface 422, by means of an adhesive layer 3. The resulting first stack is connected to an uncoated third substrate by means of an adhesive layer 3 to form a second stack, which in turn is connected to a further substrate 24 comprising an inorganic coating 5 on the first surface 441 and the second surface 442 by means of an adhesive layer 3.In an alternative embodiment not shown, it is of course possible to connect the stack 1 comprising a first substrate 21 comprising an inorganic coating 5 on the first surface 411 and the second surface 412 with an uncoated second substrate 22, a third substrate 23 comprising an inorganic coating 5 on the first surface 431 and second surface 432, and an uncoated fourth substrate 24.

[0111] Fig. 4a and Fig. 4b show an embodiment of the stack 1 produced according to the invention, in which the disc-shaped substrates 2 are connected to one another in an offset manner such that the individual substrates 2 are not connected to one another over their entire surface, resulting in a stack 1 which is also referred to below as an “oblique stack”. The substrates 2 in such a stack are preferably rectangular disc-shaped substrates 2. It is possible to stack the individual disc-shaped substrates 2 in an offset manner such that no edge of one substrate 2 is flush with the edge of another substrate 2. Preferably, however, the stacking is carried out such that two opposite edges of one substrate are flush with the two opposite edges of another substrate. For reasons of clarity, Fig. 4a and Fig.4b shows a stack 1 with only a first substrate 21 and a second substrate 22, which are connected to one another by means of an adhesive layer 3. It goes without saying that the inclined stack can comprise more than two disc-shaped substrates 2, for example 4 to 50 disc-shaped substrates 2. Fig. 4a shows the side view, Fig. 4b the top view of a stack 1 comprising a first substrate 21 and a second substrate 22. The first substrate 21 comprises two opposite edges 611a, 611b, and two opposite edges 612a, 612b. The second substrate 22 comprises two opposite edges 621a, 621b and two opposite edges 622a, 622b. Preferably, the first substrate 21 and the second substrate 22 are connected by means of an adhesive layer 3 such that the edges 611a and 611b of the first substrate do not end with the edges 621a and 621b of the second substrate, but are offset from each other by a distance 7 (in Fig.4a (not shown). Furthermore, the opposite edges 612a, 612b of the first substrate 21 preferably terminate with the opposite edges 622a, 622b of the second substrate. In some embodiments, stack 1 comprises more than two disc-shaped substrates, wherein the distance 7 is preferably always the same for two substrates stacked offset from one another.

[0112] Fig. 5a shows a side view of a straight stack 1, Fig. 5b the side view of an inclined stack 1, each comprising four disc-shaped substrates 2, 21, 22, 23, 24, which are connected to one another by means of adhesive layers 3. The number of disc-shaped substrates 2 is merely an example; it goes without saying that stack 1 can also have more disc-shaped substrates 2, for example up to 50 disc-shaped substrates 2 or up to 30 disc-shaped substrates or up to 20 substrates 2. The stack 1 according to the invention is preferably further processed into discs or optical light guide elements, wherein the stack 1 is subjected to one of the several division steps.For this purpose, a first dicing step is carried out from the first surface of the stack 101 to the second surface 102 of the stack, or alternatively from the second surface 102 of the stack to the first surface 101 of the stack, along the dashed lines 8a and 8b, and preferably a third and fourth dicing step is carried out along the lines 8c and 8d (not shown), whereby a disk or optical light guide element is obtained. The dicing is preferably carried out such that the lines 8a and 8b, as well as the lines 8c and 8d, are parallel to one another. If the stack 1 is straight, as shown in Fig. 5a, the dicing steps are preferably carried out such that the lines 8a and 8b are orthogonal to the first surface 101 and the second surface 102 of the stack 1.In embodiments in which stack 1 is an inclined stack, the dicing steps can also be carried out such that lines 8a and 8b are orthogonal to the first surface 101 and the second surface 102 of stack 1. However, in order to minimize rejects and offcuts during the dicing process and thus increase the yield of wafers or optical light guide elements from a stack 1, the dicing of inclined stacks is preferably carried out such that lines 8a and 8b are not orthogonal to the first surface 101 and the second surface 102 of stack 1.

[0113] List of reference symbols

[0114] 1 stack

[0115] 101 first surface of the stack

[0116] 102 second surface of the stack

[0117] 11 first stack

[0118] 12 second stack

[0119] 13 more stacks

[0120] 2 disc-shaped substrate

[0121] 21 first disc-shaped substrate

[0122] 22 second disc-shaped substrate

[0123] 23 third disc-shaped substrate

[0124] 24 further disc-shaped substrate

[0125] 3 adhesive layer

[0126] 41 first surface of the disc-shaped substrates

[0127] 42 second surface of the disc-shaped substrates

[0128] 411 first surface of the first substrate

[0129] 412 second surface of the first substrate

[0130] 421 first surface of the second substrate

[0131] 422 second surface of the second substrate

[0132] 431 first surface of the third substrate

[0133] 432 second surface of the third substrate

[0134] 441 first surface of the further substrate

[0135] 442 second surface of the further substrate

[0136] 5 Coating

[0137] 611a, 611b opposite edges of the first substrate

[0138] 612a, 612b opposite edges of the first substrate

[0139] 621a, 621b opposite edges of the second substrate

[0140] 622a, 622b opposite edges of the second substrate

[0141] 7 Distance

[0142] 8a, b division lines

Claims

Patent claims 1. A method for producing a stack (1) for further processing into composite panes, comprising bonding two or more disk-shaped substrates (2) with an adhesive layer (3), wherein the disk-shaped substrates (2) each have a first (41) and a second surface (42) that are parallel to one another, comprising the steps: a) providing a first disk-shaped substrate (21), wherein optionally at least the first surface (411) of the first disk-shaped substrate is pretreated by cleaning, plasma treatment, and / or applying an adhesion promoter, b) applying an adhesive with a first viscosity to the first surface of the first substrate and rotating the first substrate, wherein the adhesive is distributed over the first surface of the first substrate, and wherein the resulting adhesive layer (3) has a layer thickness of 0.2 μm to 5.0 μm,c) optionally varying the viscosity of the adhesive by heating or cooling, d) bonding the first disc-shaped substrate (21) to a second disc-shaped substrate (22) to form a first stack (1, 11), comprising bringing the first surface (411) of the first substrate into contact with the second surface (422) of the second substrate (22) and curing the adhesive layer (3)., 2. Method according to claim 1, comprising connecting the first stack (1, 11) to a third disc-shaped substrate (23), comprising the following steps: a1) providing a third disc-shaped substrate (23), wherein optionally at least the first surface (431) of the third disc-shaped substrate (23) is pretreated by means of cleaning, plasma treatment and / or application of an adhesion promoter, b1) applying an adhesive having a first viscosity to the first surface of the third substrate (23) and rotating the third substrate (23), wherein the adhesive is distributed on the first surface (431) of the third substrate (23), and wherein the resulting adhesive layer (3) has a layer thickness of 0.2 pm to 5.0 pm, c1) optionally varying the viscosity of the adhesive by heating or cooling, d1) connecting the third disc-shaped substrate (23) to the first stack (11), comprising bringing the first surface of the third substrate (431) into contact with a surface of the first stack (411, 412) and curing the adhesive layer (3), whereby a second stack (1, 12) is obtained.

3. Method according to claim 2, wherein the second stack (1, 12) is connected to a further disc-shaped substrate (24), for which purpose steps a1) to d1) are repeated, the second stack (12) being used as the first stack (1) and a further stack (13) being obtained.

4. Method according to at least one of claims 1 to 3, wherein the stack (1) comprises at least one disc-shaped substrate (2) which has an inorganic coating (5) on the first surface (41) and / or on the second surface (42).

5. The method according to at least one of claims 1 to 4, wherein the stack (1) comprises alternating disc-shaped substrates (2) and inorganic coatings (5).

6. The method according to at least one of claims 1 to 5, wherein the stack (1) has a first surface (101) and a second surface (102) which are parallel to each other.

7. Method according to at least one of claims 1 to 6, wherein the disc-shaped substrates (2) are round or square, preferably square.

8. Method according to at least one of claims 1 to 7, wherein the disc-shaped substrates (2) are stacked with edge precision.

9. Method according to at least one of claims 1 to 7, wherein the disc-shaped substrates (2) are stacked offset from one another.

10. The method according to at least one of claims 1 to 9, wherein the stack (1) comprises 4 to 50 disc-shaped substrates (2).

11. Method according to at least one of claims 1 to 10, wherein the disc-shaped substrates (2) comprise or consist of a glass, a glass ceramic, an optoceramic or a plastic.

12. The method according to at least one of claims 1 to 11, wherein the disc-shaped substrates (2) satisfy at least one of the following conditions: i) TTV of less than 10 pm; ii) Bow < 100 pm; iii) Warp < 100 pm; iv) Roughness Rq < 5 nm.

13. The method according to at least one of claims 1 to 12, wherein the adhesive layers (3) satisfy at least one of the following conditions i) thickness variation (TTV) of less than 20 pm; ii) no inclusions with a particle size which is greater than the thickness of the adhesive layer (3); iii) a refractive index which deviates from the refractive index of the disc-shaped substrates (2) by no more than 0.005, preferably no more than 0.004, preferably no more than 0.003, or no more than 0.002, particularly preferably no more than 0.

001.

14. The method according to at least one of claims 1 to 13, wherein the adhesive has a refractive index which corresponds to the refractive index of the disc-shaped substrates (2).

15. The method according to at least one of claims 1 to 14, wherein the adhesive is a light-curing adhesive, preferably a UV-curing adhesive.

16. A method for producing a composite pane, comprising the following steps: a) providing a stack, preferably produced or producible by means of the method according to at least one of claims 1 to 15, b) dividing the stack, preferably by cutting the stack, whereby at least one composite disc is obtained, c) optionally polishing the resulting composite disc.

17. A composite pane, preferably produced or producible by means of the method according to at least one of claims 1 to 15 and / or according to claim 16, comprising a first surface and a second surface which are parallel to one another, as well as at least one side surface, and two or more disc-shaped substrates, each having a first and a second surface which are parallel to one another, wherein the at least two disc-shaped substrates are connected by at least one adhesive layer, wherein the composite pane preferably fulfills at least one of the following conditions: i) the first and / or the second surface of the composite pane has a roughness Rq of < 5 nm; ii) the composite pane has, based on the first and the second surface of the composite pane, a TTV of less than 10 pm; iii) the composite has, based on the first and the second surface of the composite pane, a warp of < 100 pm;iv) the composite has a bow of < 100 pm relative to the first and second surfaces of the composite disc; 18. Composite pane according to claim 17, wherein the adhesive layers satisfy at least one of the following conditions: i) thickness variation (TTV) of less than 20 pm; ii) no inclusions with a particle size which is greater than the thickness of the adhesive layer (3); iii) a refractive index which deviates from the refractive index of the disc-shaped substrates (2) by no more than 0.005, preferably no more than 0.004, preferably no more than 0.003, or no more than 0.002, particularly preferably no more than 0.001.

Citation Information

Patent Citations

  • Method for modifying at least one area of ​​a surface or a section of a substrate and substrate

    DE102021125476A1

  • Bonding of glass substrate

    JP1986251543A

  • Laminate, method for cutting laminate, method for processing laminate, and device and method for cutting brittle plate-like object

    US20150110991A1

  • Glass product

    WO2007057459A1