Solid oxide electrochemical cell

The application of a barrier layer on the metal substrate of solid oxide electrochemical cells addresses corrosion and degradation issues, enhancing durability and structural integrity by preventing nitridation and hydrogen embrittlement, thus improving the cells' reliability and longevity.

WO2024201006A1PCT designated stage expired Publication Date: 2024-10-03CERES INTELLECTUAL PROPERTY COMPANY LIMITED
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
PCT/GB2024/050785
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2024-03-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Solid oxide electrochemical cells face corrosion and degradation issues due to high operating temperatures and exposure to reactive fluids, leading to nitridation and hydrogen embrittlement, which compromise their structural integrity and durability.

Method used

A solid oxide electrochemical cell design featuring a metal substrate with a porous region and a barrier layer applied to the second surface, which mitigates corrosion and degradation by preventing nitrogen diffusion and hydrogen embrittlement, using materials like aluminium oxide, titanium carbide, and titanium nitride that provide effective corrosion resistance and structural support.

Benefits of technology

The barrier layer significantly extends the lifespan of the cell by preventing nitridation and hydrogen embrittlement, maintaining the structural integrity and performance of the cell under harsh operating conditions, making it a more reliable alternative to fossil fuel combustion systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GB2024050785_03102024_PF_FP_ABST
    Figure GB2024050785_03102024_PF_FP_ABST
Patent Text Reader

Abstract

A solid oxide electrochemical cell, the cell comprising: a metal substrate comprising a porous region and a nonporous region bounding the porous region, wherein the porous region comprises multiple through apertures fluidly interconnecting a first surface of the metal substrate and a second surface of the metal substrate; an electrochemically active layer located on the first surface of the metal substrate wherein the electrochemically active layer is located over at least the porous region of the metal substrate; and a barrier layer applied to the second surface of the metal substrate, wherein the barrier layer is applied to at least the porous region of the metal substrate. Solid oxide cell stacks and systems comprising these cells, methods of their manufacture, operation, and use.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Solid Oxide Electrochemical Cell

[0002] The invention relates to a solid oxide electrochemical cell, and to solid oxide stacks and systems comprising the cell. In particular, the invention relates to metal supported solid oxide electrochemical cells. Methods of manufacturing the cell, methods of operation, and the use of the cell in the generation of electricity also form part of the invention.

[0003] Over the years there has been an increased drive towards "green energy" due to not only the detrimental impact fossil fuels have on the environment, but the finite resources available. There has been a growing interest in solid oxide electrochemical systems, such as solid oxide fuel cells (SOFC) and solid oxide electrolysis cells (SOEC), as they offer clean and efficient alternatives to the generation of energy or fuel. However, solid oxide electrochemical systems generally operate at high temperatures (typically above 450°C) over long periods of time in the presence of reactive fluids / fuel sources (such as hydrocarbon fuel sources and ammonia containing fuel sources). This results in a highly corrosive environment for the components of these systems.

[0004] One way that the mechanical strength of a solid oxide electrochemical cell can be improved is through the use of a metal substrate, which provides support to the electrochemically active layers of the cell. The use of such a support provides the cell with good thermal, mechanical, and stable chemical properties. For example, stainless-steel or nickel-based substrates have been incorporated into such cells. However, even "corrosion resistant" materials, such as stainless-steel, can degrade under the intense operating conditions.

[0005] For example, where the fuel source of a solid oxide electrochemical cell comprises ammonia, the elevated temperatures of the cell may result in nitridation. As used herein, the term "nitridation" is where nitrogen diffuses into the surface of a metal and leads to the formation of metal nitrides at the surface, this is the common meaning of this term in the art. In a solid oxide electrochemical cell, nitridation would be problematic as the formation of metal nitrides on metal components within the cell would have a detrimental impact on their structural integrity, making them more brittle and more prone to degradation. Moreover, nitridation can impact the compatibility of the metal components with the other parts of the cell. For example, in the case of the metal support, nitridation could result in poor adhesion of the support with the electrochemically active layers. In addition, nitrogen generated may also diffuse into the bulk of the metal components within the cell (such as the bulk of the metal substrate) which can bring about microstructural changes, such as for example the disruption of current metal precipitates in the metal components, as well as the formation of new metallic precipitates or new metallic phases. Microstructural changes can increase the fragility of these components, making them more prone to degradation.

[0006] In instances where the fuel comprises hydrogen (e.g., hydrogen per se, or a hydrocarbon, such as natural gas), hydrogen atoms or molecules can be absorbed by the metal components of the cell, which could lead to hydrogen embrittlement (also referred to as hydrogen induced cracking), causing said components to fail. Hydrocarbon fuels include, for instance, natural gas, methane, propane, butane, methanol, or renewable based feeds.

[0007] The durability of solid oxide electrochemical cells is crucial in them becoming a reliable and efficient alternative to fossil fuel combustion, particularly given the high costs often needed in their production. As such, there is a need for a solid oxide electrochemical cell that is better able to withstand corrosion when in operation. Moreover, given the variety of different fuel sources that can be used, there also remains a need for a solid oxide electrochemical cell that can better withstand said corrosion regardless of the fuel source / reactive fluid present when in operation.

[0008] The invention is intended to overcome or ameliorate at least some aspects of the problem of corrosion and degradation of solid oxide electrochemical cell components in operation.

[0009] Accordingly, in a first aspect of the invention there is provided a solid oxide electrochemical cell, the cell comprising: a metal substrate comprising a porous region and a nonporous region bounding the porous region, wherein the porous region comprises multiple through apertures fluidly interconnecting a first surface of the metal substrate and a second surface of the metal substrate; an electrochemically active layer located on the first surface of the metal substrate, wherein the electrochemically active layer is located over at least the porous region of the metal substrate; and a barrier layer applied to the second surface of the metal substrate, wherein the barrier layer is applied to at least the porous region of the metal substrate.

[0010] Solid oxide electrochemical cells operate at high temperatures (typically above 450°C). Accordingly, in order for a solid oxide electrochemical cell to withstand such conditions for the lifetime of product, which may be in the many thousands of hours of operation (including cycling on and off and up and down in power output), the solid oxide electrochemical cell must have a robust construction. This requires the electrochemically active layers of the cell to have a supporting substrate with good thermal, mechanical, and chemical properties, so that the cell resists degradation and maintains its performance for the lifetime of the product. The second surface of the substrate comes into direct contact with reactive fluids / fuel sources when the cell is in operation, and the inventors have discovered that the application of a barrier layer to this second surface of the metal substrate greatly mitigates corrosion of the metal substrate when the cell is in operation, regardless of the nature of the reactive fluid / fuel source.

[0011] As used herein, the term "electrochemically active layer" refers to the portion of the solid oxide electrochemical cell coated with electrochemically active materials, which include the electrolyte, anode, and cathode.

[0012] As used herein, the term "located on / over" is not intended to be limited to directly located on / over. Accordingly, additional layers may be incorporated between the electrochemically active layer and the substrate. However, the term "located on / over" may mean directly located on, although it is typically the case that the electrochemically active layer is not located directly on the metal substrate. The presence of additional layers between the metal substrate and the electrochemically active layers provides for the option of including further barrier layers on the first surface of the substrate, to further reduce corrosion and / or other degradation mechanisms that could impact the metal substrate.

[0013] As used herein, the term "applied to" means directly applied to or coated onto. The terms "coated on" and "applied to" can therefore be used interchangeably. Therefore, the barrier layer is generally coated directly onto the second surface of the metal substrate.

[0014] The term "barrier layer" refers to the layer of material directly applied to the second surface of the metal substrate, which enables mitigation of corrosion and / or other degradation mechanisms that could impact the metal substrate. For example, in instances where the fuel source or reactive fluid comprises ammonia, the barrier layer may mitigate nitridation or diffusion of nitrogen into the bulk of the metal substrate. As discussed above, nitridation leads to the formation of metal nitrides at the surface. In addition, diffusion of nitrogen into the bulk of the metal substrate can bring about microstructural changes to the substrate (such as the disruption of current metal precipitates in the metal substrate, as well as the formation of new metallic precipitates or new metallic phases). In instances where the barrier layer is in contact with a reactant gas comprising hydrogen atoms or molecules (such as natural gas), the barrier layer may mitigate hydrogen embrittlement. It is often the case that the barrier layer is substantially non-porous to fluids, in particular the barrier layer is often substantially non-porous to gases such as ammonia, nitrogen, dihydrogen or dioxygen. As used herein, the terms "fuel source" and "reactive fluid" are intended to refer to the gaseous component introduced into a solid oxide electrochemical cell when in operation. If the cell is being used as a solid oxide fuel cell, then the gaseous component would typically be referred to as a fuel source, and if the cell is being used as an electrolysis cell, then the gaseous component would typically be referred to as a reactive fluid.

[0015] The barrier layer may be any suitable thickness. Often, the barrier layer has a thickness in the range 100 nm to 2000 nm, optionally in the range 500 nm to 1750 nm, optionally in the range 1000 nm to 1500 nm. It may be the case that the barrier layer has a thickness in the range 1500 nm to 2000 nm. As the permeability of the barrier layer is partially dependent upon the thickness of the layer, the thickness will vary depending on the chemical nature of the barrier layer; however, in general terms, the thickness range allows for optimum mitigation of corrosion of the second surface of the metal substrate while not detrimentally impacting the efficiency of the cell. A barrier layer of a thickness lower than 100 nm may not be of a sufficient thickness to mitigate corrosion and / or other degradation mechanisms that could impact the second surface of the metal substrate, and the bulk of the metal substrate. For example, in instances where the fuel source comprises ammonia, the barrier layer is able to mitigate nitridation and diffusion of nitrogen into the bulk of the metal substrate.

[0016] There is no particular restriction on the type of materials from which the barrier layer can be made. However, it is typically the case that the material has a melting point of greater than or equal to 450°C, more typically greater than 600°C and more typically still greater than or equal to 650°C. These are the temperatures at which SOFCs are conventionally operated, and in instances where the cell is being used as a solid oxide fuel cell, the barrier layer would need to remain substantially solid (either in pure form or in an oxidised form) in order to prevent contact between the reactive fluids and the substrate, and to prevent migration of the metal substrate material.

[0017] The barrier layer may comprise a metal, a metallic compound, a ceramic compound, or a combination thereof. As used herein, the term "metallic compound" takes its usual meaning in the art and relates to a compound that contains one or more metal elements bonded to another element. As used herein, the term "ceramic compound" takes its usual meaning in the art and relates to inorganic non-metallic solids comprising either metal or non-metal compounds that have been shaped and then hardened by heating to high temperatures. The barrier layer may comprise a metal, a nitride, a carbide, a metal oxide, a metalloid oxide, or a combination thereof. These materials are not only physically stable at the operation temperatures found in fuel cells, but have high strength and thermal resistance, and their permeability properties together with their corrosion resistance to high temperatures enables mitigation of corrosion and / or other degradation mechanisms that could impact the metal substrate. Moreover, these materials have been found to provide effective corrosion barriers for a wide range of reactive fluids and fuel sources.

[0018] The metal may be selected from aluminium (Al), gallium (Ga), indium (In), thallium (Tl), or combinations thereof.

[0019] The nitride may comprise aluminium nitride, gallium nitride, indium nitride, thallium (I) nitride, titanium nitride, vanadium nitride, chromium nitride, zirconium nitride, boron nitride, silicon nitride, or combinations thereof. The nitride may comprise boron nitride, silicon nitride, zirconium nitride, titanium nitride, or combinations thereof. The nitride may comprise one or more of titanium nitride, zirconium nitride and chromium nitride. The nitride may comprise titanium nitride.

[0020] The carbide may comprise aluminium carbide, titanium carbide, zirconium carbide, hafnium carbide, vanadium carbide, niobium carbide, tantalum carbide, chromium carbide, molybdenum carbide, tungsten carbide, silicon carbide, or combinations thereof. The carbide may comprise titanium carbide, silicon carbide, or a combination thereof. The carbide may comprise titanium carbide.

[0021] The metal oxide may comprise aluminium oxide, chromium oxide, gallium oxide, indium oxide, thallium oxide, zirconium oxide, zinc oxide, erbium oxide, yttrium oxide, or a combination thereof. The metal oxide may comprise aluminium oxide. The metalloid oxide may comprise silicon dioxide.

[0022] The barrier layer may comprise aluminium, aluminium oxide, erbium oxide, boron nitride, silicon nitride, zirconium nitride, titanium nitride, titanium carbide, chromium nitride, or a combination thereof. The barrier layer may comprise one or more of aluminium oxide, titanium carbide, titanium nitride, zirconium nitride or chromium nitride. The barrier layer may comprise one or more of aluminium oxide and titanium carbide.

[0023] The barrier layer may comprise a metal and / or a metal oxide. Optionally, the barrier layer comprises aluminium and / or aluminium oxide. As with the other barrier layer materials, the presence of aluminium and / or aluminium oxide provides the second surface of the substrate with an effective corrosion barrier for a wide range of reactive fluids and fuel sources. In addition, it has been found that, a barrier layer comprising aluminium and / or aluminium oxide is particularly effective at preventing nitridation, diffusion of nitrogen into the bulk of the metal substrate, and / or hydrogen embrittlement.

[0024] It is typically the case that the metal substrate is an iron containing substrate (i.e., the substrate comprises the element iron). This may be an alloy which includes iron (i.e., wherein the main component of the alloy is iron), a material which includes iron as a dopant or additive, or even pure iron. Typical examples of iron containing substrates are steels. There is no particular limitation on the choice of steel which is used; however, it is typically the case that the steel is stainless-steel, and more typically ferritic stainless- steel, as this demonstrates excellent mechanical and thermal stability for these applications and has a very close thermal expansion coefficient match to the electrochemically active layers.

[0025] The metal substrate may have a thickness in the range of about 50 to 400 pm, often about 100 to 350 pm, in some cases about 300 pm. The thickness of the substrate is determined by the need to provide a stable substrate, which does not significantly change shape or warp during cell processing, assembly, or in use, but which is as thin as possible to allow efficient contact between the reactive fluid / fuel source and the electrochemically active layer. The metal substrate comprises a porous region and a nonporous region bounding the porous region. Provision of a porous region bounded by a non-porous region of the substrate provides superior contact.

[0026] The metal substrate may be planar or tubular. Often, the metal substrate is planar. Cells based on planar substrates are simpler to prepare, and easier to form into stacks than tubular systems, thereby reducing the overall manufacturing and implementation costs.

[0027] The porous region comprises multiple through apertures fluidly interconnecting a first surface of the metal substrate and a second surface of the metal substrate. The diameter of the aperture may not be the same on each side of the substrate, and the smaller diameter aperture may typically 5-100 pm diameter, more typically 10-50 pm diameter. These features contribute to an efficient transfer of the reactive fluid / fuel source (for instance one or more of ammonia, steam reformate, hydrogen, CO or unreformed gas, or a combination thereof) through the substrate to the electrochemically active layer, whilst allowing the metal substrate to support the solid oxide electrochemical cell. This facilitates the use of electrochemically active layers with dramatically reduced thicknesses within the cell. Optionally, the substrate may be a thin metal sheet or foil. Although a sintered substrate could also be used, creation of uniform through apertures is more challenging with sintered substrates. As such, metal sheets or foils may be used. Foils allow for better control of the structure of the porous region and facilitate handling during manufacture of the solid oxide electrochemical cell.

[0028] The barrier layer may additionally be applied to at least part of the walls that will be present within the apertures, as each aperture extends between the first and the second surface (forming said aperture walls). It may be the case that the barrier layer extends into some or all of the apertures and is applied to substantially all of any given aperture wall (i.e., a substantially full coating of the wall of the aperture), or the barrier layer may provide partial coverage of the wall of an aperture. The barrier layer may be applied (fully or partially) to some of the aperture walls, but not all of the aperture walls. As such, different apertures may exhibit a different level of extension of the barrier layer and application onto their walls. For instance, it may be the case that all aperture walls exhibit at least partial coverage, but with different degrees of coverage (for example, some may exhibit full coverage). When the barrier layer is additionally applied to at least part of the aperture walls, it is believed that the overall impact of corrosion and / or other degradation mechanisms that could impact the metal substrate is reduced.

[0029] Alternatively, it may be the case that the barrier layer is present on the second surface of the metal substrate, with minimal or no application to the aperture walls. The inventors have found that having the barrier layer substantially exclusively on the second surface of the substrate provides for rapid and simple deposition of the barrier layer.

[0030] The barrier layer may be a nitrogen diffusion barrier layer and / or a hydrogen diffusion barrier layer. Hydrogen diffusion barrier layers may also function to prevent the diffusion of larger molecules, such as nitrogen. As such, where the material selected for the barrier layer functions as a hydrogen barrier layer, it may also often function as a nitrogen barrier layer.

[0031] Where, when the cell is in operation, the second surface of the metal substrate comes into contact with ammonia, the elevated temperatures of the cell may result in nitridation. Nitridation can be problematic, as it leads to the formation of metal nitrides on the second surface of the substrate. Nitride formation at the surface of the substrate often has a detrimental impact on the structural integrity of the substrate, making it more brittle and prone to degradation. Moreover, nitridation can impact the compatibility of the metal substrate with the other parts of the cell, such as poor adhesion of the substrate with the electrochemically active layer. It may also be the case that, when the cell is in operation and the second surface of the metal substrate comes into contact with ammonia, the elevated temperatures of the cell may result in nitrogen diffusion into the bulk of the metal substrate. Nitrogen diffusion within the bulk of the metal substrate can bring about microstructural changes, such as increase in volume of the substrate, which could result in a more brittle and fragile substrate.

[0032] In instances where the fuel source comprises ammonia, the barrier layer of the invention will be a nitrogen diffusion barrier layer intended to prevent nitridation of the second surface of the metal substrate and diffusion of nitrogen into the bulk of the metal substrate. The inhibition of nitridation and diffusion of nitrogen into the bulk of the metal substrate would reduce the structural damage to the substrate material that would otherwise occur, ensuring that the structural integrity of the substrate is maintained. As a result, the life of the cell would be extended.

[0033] Where, when the cell is in operation, the second surface of the metal substrate comes into contact with a fuel source comprising hydrogen (e.g., hydrogen itself or a hydrocarbon, such as natural gas), hydrogen atoms or molecules can be absorbed by the metal substrate at the second surface, which could lead to hydrogen embrittlement. Hydrogen embrittlement can result in degradation of the substrate, impacting the overall efficiency of the cell. Such degradation can be prevented or minimised by the presence of a hydrogen barrier layer, which can help reduce embrittlement and prolong both the structural integrity of the metal substrate and the life of the cell.

[0034] Optionally, the electrochemical cell is a solid oxide fuel cell (SOFC), and it will often be the case that the cell is a SOFC. However, solid oxide electrolysis cells (SOEC) are also envisaged.

[0035] SOFCs typically operate as electrochemical devices with an oxidant environment on one side of the SOFC - traditionally called the cathode side of the fuel cell, and a reducing environment on the other side of the SOFC - traditionally called the anode side of the fuel cell. The oxidant environment is provided by way of a fluid stream (also referred to as a cathode fluid stream) and the reducing environment is provided by way of a fluid stream (also referred to as an anode fluid stream). When the electrochemical cell is a SOFC, the second surface of the metal substrate comes into contact with a fuel source present in (or consisting of) the anode fluid stream. As noted above, a wide range of fuel sources may be used. Examples of fuel sources include, but are not limited to, ammonia, steam reformate, hydrogen, CO or unreformed gas, or combinations of these.

[0036] The electrochemical cell comprises an electrochemically active layer, which itself comprises at least an anode layer, electrolyte layer, and cathode layer. A passivation layer may also be present. The anode layer is usually positioned between the substrate and the electrolyte layer, and the electrolyte layer is usually positioned between the anode layer and the cathode layer. Where present, the passivation layer will generally be between the substrate and the anode layer, such that the electrochemically active layer is formed on the passivation layer. Where absent, the electrochemically active layer will generally be formed on the first surface of the substrate. Examples of typical anode and cathode materials, as well as SOFC architectures comprising anode and cathodes of the invention, are described in GB 2 368 450, GB 2 524 638, GB 2 524 640, GB 2 400 486, GB 2 386 126, GB 2 517 927, GB 2 517 928, GB 2 522 522, and GB 2 440 038, the contents of which are incorporated herein in their entirety by reference.

[0037] The anode layer may be a composite cermet, which may be formed from a mixture of the electrolyte material and a metal (usually a metal oxide). The anode layer may be fabricated as a film with a thickness between 5 and 30 pm. The anode layer may be deposited by screen-printing an ink containing a metal oxide and powders of the electrolyte material, which may then be subsequently thermally processed into a porous cermet layer bonded to the metal substrate. The metal oxide may be nickel oxide.

[0038] There is no particular limitation on the choice of electrolyte material used to form the electrolyte layer. The electrolyte is generally a solid electrolyte, and typically has a melting point greater than 450°C, and more typically greater than 600°C. The electrolyte may be a ceramic material having oxygen-ion conducting properties, which may be an oxide such as a rare earth oxide. Examples of rare earth oxides include, but are not limited to, oxides of zirconium, yttrium, scandium, cerium, or combinations thereof. The electrolyte may be a cerium oxide which may be doped with one or more dopants. The electrolyte may be a cerium gadolinium oxide, which may have the formula Ceo.9Gdo.1O1.95. Typical dopants which can be used with the electrolyte include cobalt, samarium, or combinations thereof. It may be the case that the cerium gadolinium oxide further comprises cobalt. The amount of cobalt present in the cerium gadolinium oxide may be in the range 2% to 20%, and more typically in the range 5 to 15%, and most typically about 10%.

[0039] The cathode layer may comprise a sintered powdered mixture of a perovskite oxide mixed conductor and ceramic material, typically a rare earth-doped ceria, such as gadolinium doped ceria . The perovskite may comprise Lai-xSrxCoyFei-yO3-d, where 0.5 > x > 0.2 and 1 > y > 0.2. In particular, the perovskite oxide mixed conductor may comprise one or more of Lao.eSro^Coo.zFeo.aOa-a, Lao.sSro.sCoOs-a, Gdo.sCoOa-a, and Smo.sSro sCoOs-d. Other cathode materials include LCN60 / CGO, for example Lao.ggCoo^Nio.eOa-a and Ceo.9Gdo.1O1.95 or 60 / 40% PSC552 / CGO. It can be useful to use these compounds as they have a higher ionic conductivity than most perovskites, and similar thermal expansion co-efficients to rare earth-doped ceria, reducing the stress between cathode and electrolyte in use. In some cases, the mixture may comprise in the range 20 to 50 wt% rare earth-doped ceria, in some cases in the range 30 to 45 wt%, in some cases in the range 35 to 45 wt%, or around 40 wt% rare earth-doped ceria as defined above. This helps to enhance the compatibility between the cathode layer and electrolyte layer, both chemically, and in terms of the thermal expansion described above. In addition, as these ceria have high charge transfer rates, their inclusion ensures a good rate of charge transfer between the electrolyte and the cathode.

[0040] It is often the case that, where the substrate is iron-containing (for instance stainless- steel), the air side of the substrate will oxidise, forming a porous and non-passivating oxide layer (also referred to as the "passivation layer"). This may be, for instance, a chromium oxide passivation layer. This passivation layer protects the bulk metal of the substrate and provides a diffusion barrier between the anode and the bulk metal of the substrate.

[0041] In a second aspect of the invention there is provided a solid oxide cell stack comprising two or more cells according to the first aspect of the invention. Typically, when the solid oxide electrochemical cells are assembled into a stack, the individual solid oxide electrochemical cells are arranged to sealingly connect adjacent solid oxide electrochemical cells together, such that when a cathode fluid stream and an anode fluid stream are delivered to the solid oxide electrochemical cells in the solid oxide electrochemical cell stack, these streams are kept separate from one another and passed over the appropriate surfaces of the solid oxide electrochemical cell in order for the electrochemical reactions to occur.

[0042] In a third aspect of the invention there is provided a method of manufacturing a solid oxide electrochemical cell, the method comprising the following steps:

[0043] (i) providing a coated metal substrate comprising a porous region and a nonporous region bounding the porous region, wherein the porous region comprises multiple through apertures fluidly interconnecting a first surface of the metal substrate and a second surface of the metal substrate, and wherein the coating is thermally decomposable;

[0044] (ii) applying a barrier layer material to at least the porous region of the second surface of the metal substrate; (Hi) heating the metal substrate to remove the coating and, optionally form the barrier layer by sintering the barrier layer material; and

[0045] (iv) forming an electrochemically active layer on the first surface of the metal substrate, and sintering.

[0046] It will often be the case that the coating is a thermally decomposable material, often a resin. As used herein the term "thermally decomposable material" is intended to include any material (or any thermally decomposable resin) which will thermally degrade during step (iii). Often, the thermally decomposable resin comprises an organic resin. Examples of thermally decomposable resins include, but are not limited to, epoxy resin, polyester resin, vinyl ester resin, polyurethane resin, or combinations thereof.

[0047] As the metal substrate of step (i) is coated, it will generally be the case that the coating is applied to the metal substrate prior to step (i). This may be as part of a single manufacturing process / production line, or the metal substrate may be pre-coated by a third party or at another production site and purchased or shipped to the point of manufacture of the cell. Coating the metal substrate protects the coated areas from contact with the barrier layer, ensuring that the barrier layer is applied only to those regions of the substrate where it is required. The coating is located on the regions of the substrate where the barrier layer is not required. Typically, the coating is located on the surface of the substrate that will be in contact with the electrochemically active layer upon formation of the cell. Typically, the coating is located on at least part of the first surface of the metal substrate. The coating may be located on substantially all of the first surface of the metal substrate. Typically, the coating is located on at least the porous region of the first surface of the metal substrate. It may be the case that the coating substantially covers the porous region of the first surface of the metal substrate and the nonporous region of the first surface of the metal substrate, which bounds the porous region. As used herein, the term "located on" is not intended to be limited to directly located on. Accordingly, an additional layer (or layers) may be incorporated between the first surface of the substrate and the coating. However, it is often the case that the coating is located directly on the first surface of the metal substrate.

[0048] Optionally, the multiple through apertures are formed before applying the coating. In doing so, this provides for simplicity of manufacture and easy control of the aperture formation process, and ease of removal (for instance using solvent materials) or any particulates or fines produced during aperture formation. This particulate removal is slightly more complex where the coating is already present, as mechanical or chemical cleaning may damage the coating. Further, in some instances it can be advantageous for the coating to at least partly seal the through apertures on the first surface of the metal substrate. It may be the case that the coating fully seals the through apertures on the first surface of the substrate. At least partly sealing or fully sealing the through apertures is more easily achieved when the coating is applied after formation of the apertures and has the advantage of reducing transfer of the barrier layer through the apertures to the first surface of the metal substrate during barrier material application, ensuring that the barrier layer is applied, and remains, in those locations where it is required. Moreover, application of the coating after formation of the through apertures allows for precise control of at least partly or fully sealing said through apertures, as the through apertures are visible.

[0049] Alternatively, the multiple through apertures are formed after applying the coating. Formation of the through apertures after application of the coating provides for a more efficient manufacturing process, which, where sealing of the apertures from the first surface is not required, results in lower costs.

[0050] Optionally, the one or more through apertures are formed by laser drilling, erosion, etching, or a combination thereof. Often, the apertures are formed by laser drilling. Laser drilling is accurate and can also be readily automated, allowing for better precision in aperture formation. Laser drilling also allows for the formation of well-defined aperture patterns, ensuring the highest rates of reactive fluid / fuel source transfer to the electrochemically active layers.

[0051] As used herein, the term "barrier layer material" is intended to include materials that form a barrier layer on deposition with no further treatment required to perform the diffusion and corrosion prevention functions; and also materials that undergo a chemical or physical change when subjected to the conditions of step (iii). Materials that undergo a chemical or physical change when subjected to the conditions of step (iii) could also be considered to be "barrier layer precursors" as they are not, for instance, adequately dense to prevent diffusion until they are subjected to the optional sintering conditions of step (iii). With such "precursor" barrier layer materials, the barrier layer is not fully formed until after the application of heat and pressure, as seen in the optional sintering of said barrier precursor material in step (iii).

[0052] As noted above, the barrier layer material is applied to at least the porous region of the metal substrate on the second surface. Application may be carried out using standard techniques as would be known to the person skilled in the art. The barrier layer may be applied via chemical vapour deposition (CVD); metal organic chemical vapor deposition (MOCVD); physical vapor deposition (also commonly known as physical vapor transport); a sol-gel process; plasma spraying, pack cementation, a slurry (for instance, brushing or spraying a slurry on the surface of the substrate); printing (for instance, screen printing); tape casting; vacuum slip casting; electrophoretic deposition; and calendaring. The barrier layer may be applied via chemical vapour deposition (CVD), metal organic chemical vapor deposition (MOCVD), or physical vapor deposition. These techniques provide for effective and controlled application of the barrier layer, high deposition rates, and a high-quality resultant coating. In instances where chemical vapour deposition is used, it may involve low pressure chemical vapour deposition, for instance, where the thin film deposition is carried out at low or high substrate temperatures under reduced pressures in the range 0.13 to 13332 Pa. In instances where Physical vapour deposition is used, the vaporisation stage may involve cathodic arc deposition, electron beam PVD, evaporative deposition, pulsed laser deposition, sputter deposition, or sublimation. This application may be all that is needed to form the barrier layer. Alternatively, it may be that heating to provide for solvent removal or sintering to provide for densification of the barrier layer material, thereby forming the barrier layer, is also desirable to provide for an impermeable layer that prevents gas diffusion to the second surface of the metal substrate.

[0053] The barrier layer material may comprise a metal, a metallic compound, a ceramic compound, or a combination thereof. The barrier layer material may comprise a metal, a nitride, a carbide, a metal oxide, a metalloid oxide, or a combination thereof. These materials are not only physically stable at the operation temperatures found in fuel cells, but have high strength and thermal resistance, and their permeability properties together with their corrosion resistance to high temperatures enables mitigation of corrosion and / or other degradation mechanisms that could impact the metal substrate. Moreover, these materials have been found to provide effective corrosion barriers for a wide range of reactive fluids and fuel sources.

[0054] The metal may be selected from aluminium (Al), gallium (Ga), indium (In), thallium (Tl), or combinations thereof.

[0055] The nitride may comprise aluminium nitride, gallium nitride, indium nitride, thallium (I) nitride, titanium nitride, vanadium nitride, chromium nitride, zirconium nitride, boron nitride, silicon nitride, or combinations thereof. The nitride may comprise boron nitride, silicon nitride, zirconium nitride, titanium nitride, or combinations thereof. The nitride may comprise one or more of titanium nitride, zirconium nitride or chromium nitride. The nitride may comprise titanium nitride. The carbide may comprise aluminium carbide, titanium carbide, zirconium carbide, hafnium carbide, vanadium carbide, niobium carbide, tantalum carbide, chromium carbide, molybdenum carbide, tungsten carbide, silicon carbide, or combinations thereof. The carbide may comprise titanium carbide, silicon carbide, or a combination thereof. The carbide may comprise titanium carbide.

[0056] The metal oxide may comprise aluminium oxide, chromium oxide, gallium oxide, indium oxide, thallium oxide, zirconium oxide, zinc oxide, erbium oxide, yttrium oxide, or combinations thereof. The metal oxide may comprise aluminium oxide. The metalloid oxide may comprise silicon dioxide.

[0057] The barrier layer material may comprise aluminium, aluminium oxide, erbium oxide, boron nitride, silicon nitride, zirconium nitride, titanium nitride, titanium carbide, chromium nitride, or combinations thereof. The barrier layer material may comprise one or more of aluminium oxide, titanium carbide, titanium nitride, zirconium nitride or chromium nitride. The barrier layer may comprise one or more of aluminium oxide and titanium carbide.

[0058] The barrier layer material may comprise a metal, wherein the metal may be oxidised during step (Hi) to form the barrier layer. Formation of a metal oxide through oxidation of a barrier layer precursor material provides a structurally robust and dense barrier layer that exhibits superior corrosion resistance against a reactive fluid / fuel source.

[0059] Optionally, the barrier layer material comprises a metal oxide. When a metal oxide is deposited directly onto the second surface of the metal substrate, step (iii) may serve only to remove the thermally decomposable resin, as the barrier layer is formed in step (ii). Application of a metal oxide allows for lower temperature heating conditions, providing the coating is thermally decomposable at such temperatures, which provides a more cost- effective manufacturing process.

[0060] Optionally, the barrier layer material comprises a metal oxide, wherein the metal oxide is sintered in step (iii). Sintering the metal oxide allows for formation of a denser and more structurally robust barrier layer, which results in improved corrosion resistance.

[0061] Examples of techniques used to manufacture SOFCs of the present invention, in particular methods of forming cermet electrodes and electrolyte layers on metal substrates such as ferritic stainless-steel, are disclosed in GB 2 368 450, GB 2 386 126 and GB 2 400 486, the contents of which are incorporated herein in their entirety by reference. In a fourth aspect of the invention there is provided a method of operation of a solid oxide electrochemical cell, wherein the method comprises the following steps:

[0062] (i) provision of a cell, wherein the cell comprises a metal substrate comprising a porous region and a nonporous region bounding the porous region, wherein the porous region comprises multiple through apertures fluidly interconnecting a first surface of the metal substrate and a second surface of the metal substrate; an electrochemically active layer located on the first surface of the metal substrate, wherein the electrochemically active layer is located over at least the porous region of the metal substrate; and a barrier layer applied to the second surface of the metal substrate, wherein the barrier layer is applied to at least the porous region of the metal substrate; and

[0063] (ii) introduction of a gas source into the cell, wherein the gas source is in fluid communication with the barrier layer.

[0064] As used herein, the term "gas source" is intended to refer to the gaseous component introduced into a solid oxide electrochemical cell when in operation. The gas source comes into contact with the electrochemically active area via the second surface of the metal substrate, as the gas source is in fluid communication with the barrier layer applied to the second surface of the metal substrate. The term "gas source" is intended to include a fuel source or a reactive fluid as defined above. If the cell is being used as a solid oxide fuel cell, then the gas source would typically comprise a fuel source, and if the cell is being used as an electrolysis cell (otherwise known as a solid oxide electrolyser cell (SOEC)), then the gas source would typically comprise a reactive fluid.

[0065] It may be the case that the solid oxide electrochemical cell is being operated as a solid oxide electrolyser cell, and the gas source may comprise a reactive fluid.

[0066] It may be the case that the solid oxide electrochemical cell is being operated as a solid oxide fuel cell, and the gas source may comprise a fuel source. Additionally, the method may further comprise the additional step of introduction of an air source, wherein the air source is in fluid communication with the electrochemically active layer. The fuel source may comprise ammonia.

[0067] In a fifth aspect of the invention there is provided a system comprising: a solid oxide electrochemical cell comprising a metal substrate comprising a porous region and a nonporous region bounding the porous region, wherein the porous region comprises multiple through apertures fluidly interconnecting a first surface of the metal substrate and a second surface of the metal substrate; an electrochemically active layer located on the first surface of the metal substrate, wherein the electrochemically active layer is located over at least the porous region of the metal substrate; and a barrier layer applied to the second surface of the metal substrate, wherein the barrier layer is applied to at least the porous region of the metal substrate; a gas source; and a fluid flow path from the gas source to the solid oxide electrochemical cell, wherein the gas source is in fluid communication with the barrier layer of the solid oxide electrochemical cell.

[0068] It may be the case that the solid oxide electrochemical cell is being operated as a solid oxide electrolyser cell, and the system is a SOEC system. Where the system is a SOEC system, the gas source may comprise a reactive fluid.

[0069] It may be the case that the solid oxide electrochemical cell is being operated as a solid oxide fuel cell, and the system is a SOFC system. Where the system is a SOFC system, the gas source may comprise a fuel source. The fuel source may comprise ammonia, or a hydrogen-containing source (e.g., hydrogen or a hydrocarbon); and the system may further comprise an air source, and a fluid flow path from the air source to the solid oxide electrochemical cell, wherein the air source is in fluid communication with the electrochemically active layer of the solid oxide electrochemical cell.

[0070] It may be the case that the fuel source comprises ammonia.

[0071] When the fuel source comprises ammonia, the barrier layer is believed to act as a nitrogen diffusion barrier layer and thereby able to reduce the extent of nitridation of the second surface of the metal substrate and the level of diffusion of nitrogen within the bulk of the metal substrate. As discussed above, nitridation leads to the formation of metal nitrides at the surface. In addition, diffusion of nitrogen into the bulk of the metal substrate can bring about microstructural changes to the substrate (such as the disruption of current metal precipitates in the metal substrate, as well as the formation of new metallic precipitates or new metallic phases). Optionally, the fuel source comprises hydrogen or a hydrocarbon.

[0072] When the fuel source comprises hydrogen or a hydrocarbon, the barrier layer acts as a hydrogen diffusion barrier layer and thereby reduces the extent of hydrogen embrittlement of the second surface of the metal substrate.

[0073] In a sixth aspect of the invention there is provided use of a solid oxide electrochemical cell according to a first aspect of the invention or a solid oxide cell stack according to the second aspect of the invention in the generation of electricity, and optionally heat.

[0074] Unless otherwise stated, each of the integers described may be used in combination with any other integer as would be understood by the person skilled in the art. Further, although all aspects of the invention preferably "comprise" the features described in relation to that aspect, it is specifically envisaged that they may "consist" or "consist essentially" of those features outlined in the claims. In addition, all terms, unless specifically defined herein, are intended to be given their commonly understood meaning in the art.

[0075] Further, in the discussion of the invention, unless stated to the contrary, the disclosure of alternative values for the upper or lower limit of the permitted range of a parameter, is to be construed as an implied statement that each intermediate value of said parameter, lying between the smaller and greater of the alternatives, is itself also disclosed as a possible value for the parameter.

[0076] In addition, unless otherwise stated, all numerical values appearing in this application are to be understood as being modified by the term "about".

[0077] In order that the invention may be more readily understood, it will be described further with reference to the figures and to the specific examples hereinafter.

[0078] Figure 1 is a schematic diagram of a cross section of a solid oxide electrochemical cell of the invention wherein the barrier layer is applied to the second surface of the metal substrate;

[0079] Figure 2 is an enlarged view of a schematic diagram of a cross section of a solid oxide electrochemical cell of the invention, wherein the barrier layer extends into all of the apertures and is applied to substantially all of the aperture walls;

[0080] Figure 3 is an enlarged view of a schematic diagram of a cross section of a solid oxide electrochemical cell of the invention, wherein the barrier layer is present on the second surface of the metal substrate, but not present on the aperture walls; Figure 4 is a flow chart illustrating a method of applying a barrier layer to a metal substrate;

[0081] Figure 5 is a flow chart illustrating an alternative method of applying a barrier layer to a metal substrate;

[0082] Figure 6 is a SEIM cross section image of two separate metal components of a solid oxide electrochemical cell following exposure to ammonia under solid oxide cell operating conditions. The field of view (FOV) is 2.00 mm, the working distance (WD) (i.e. the distance between the bottom of the SEIM column and the top of the sample) is 14.04 mm, the beam current is 1 nA, and the energy is 10keV;

[0083] Figures 7(a) - 7(c) are SEIM-EDX cross-sections of the second surface of a VDIM® Crofer 22 ferritic stainless-steel substrate absent a barrier layer according to the invention following exposure to ammonia. Figure 7(a) relates to site position 5 (referred to as "site 5" in Figure 7(a) and Figure 8) on the second surface of the substrate; Figure 7(b) relates to site position 7 (referred to as "site 7" in Figure 7(b) and Figure 8) on the second surface of the substrate; and Figure 7(c) relates to site position 12 (referred to as "site 12" in Figure 7(c) and Figure 8) on the second surface of the substrate. The numerical values "5", "7", and "12", are arbitrary numbers which are merely used to denote different sample positions on the second surface of the substrate;

[0084] Figure 8 is a graph illustrating the nitrogen penetration of the second surface of the substrate of Figures 7(a) to (c) by distance from the second surface in direct contact with the ammonia fuel source. The data points for 7(a) (i.e., site 5) are denoted by a circle; the data points for 7(b) (i.e., site 7) are denoted by a triangle; and the data points for 7(c) (i.e., site 12) are denoted by a square. The term "bottom surface" relates to the surface of the substrate in contact with the ammonia fuel source. The term "Distance from bottom" (i.e., the X-axis) relates to the distance from the surface of the substrate in contact with the ammonia fuel source (i.e., 0 pm = the surface in direct contact with the ammonia fuel source);

[0085] Figures 9(a) - 9(h) are images of variants of cells after exposure to ammonia conducted in a short stack. The cell of Figure 9(a) serves as a control and is absent a barrier layer. The cells of Figures 9(b) - 9(h) include a barrier layer according to the invention. The cell of Figure 9(b) includes a titanium carbide barrier layer having a thickness of 0.2 pm. The cell of Figure 9(c) includes a chromium nitride barrier layer having a thickness of 0.2 pm. The cell of Figure 9(d) includes an aluminium oxide barrier layer having a thickness of 0.5 pm. The cell of Figure 9(e) includes a zirconium nitride barrier layer having a thickness of 0.2 pm. The cell of Figure 9(f) includes a titanium nitride barrier layer having a thickness of 1 pm. The cell of Figure 9(g) includes a zirconium nitride barrier layer having a thickness of 1 m. The cell of Figure 9(h) includes a titanium carbide barrier layer having a thickness of 1 pm. The metal substrate used in the cells of 9(a) to 9(h) is stainless-steel and has a thickness of 300 pm;

[0086] Figures 10(a) and 10(b) show SEM cross section images of the cell of Figure 9(a). In Figure 10(a), the top layer represents the stainless-steel substrate, the central layer represents the spacer, and the bottom layer represents the interconnect. The field of view (FOV) is 2.15 mm, the working distance (WD) (i.e. the distance between the bottom of the SEM column and the top of the sample) is 10.00 mm, the beam current is 1 nA, and the energy is 20 keV. In Figure 10(b), the top layer represents the stainless-steel substrate, the central layer represents the spacer, and the bottom layer represents the interconnect. The field of view (FOV) is 2.15 mm, the working distance (WD) (i.e. the distance between the bottom of the SEM column and the top of the sample) is 10.03 mm, and the beam current is 998 pA;

[0087] Figures 11(a) and 11(b) show SEM cross section images of a cell of Figure 9(d). In Figure 11(a), the top layer represents the stainless-steel substrate, the central layer represents the spacer, and the bottom layer represents the interconnect. The substrate has an aluminium oxide barrier layer of thickness 0.5 pm, wherein the barrier layer is located on the surface of the substrate adjacent to the spacer. The field of view (FOV) is 1.11 mm, the working distance (WD) (i.e. the distance between the bottom of the SEM column and the top of the sample) is 9.95 mm, and the beam current is 997 pA. In Figure 11(b), the top layer represents the stainless-steel substrate, the central layer represents the spacer, and the bottom layer represents the interconnect. The field of view (FOV) is 1.50 mm, the working distance (WD) (i.e. the distance between the bottom of the SEM column and the top of the sample) is 9.97 mm, and the beam current is 996 pA; and

[0088] Figures 12(a) and 12(b) show SEM cross section images of a cell of Figure 9(h). In Figure 12(a), the top layer represents the stainless-steel substrate, the central layer represents the spacer, and the bottom layer represents the interconnect. The substrate has a titanium carbide barrier layer of thickness 1 pm, wherein the barrier layer is located on the surface of the substrate adjacent to the spacer. The field of view (FOV) is 1.83 mm, the working distance (WD) (i.e. the distance between the bottom of the SEM column and the top of the sample) is 10.02 mm, the beam current is 1 nA, and the energy is 20keV. In Figure 12(b), the top layer represents the stainless-steel substrate, the central layer represents the spacer, and the bottom layer represents the interconnect. The field of view (FOV) is 1.83 mm, the working distance (WD) (i.e. the distance between the bottom of the SEM column and the top of the sample) is 10.02 mm, the beam current is 1 nA, and the energy is 20keV.

[0089] Figure 1 shows a schematic diagram of a cross section of a solid oxide electrochemical cell according to the invention. The solid oxide electrochemical cell comprises a ferritic stainless-steel substrate 4, made from a nonporous metal foil, and consisting of a porous region 4a surrounded by a nonporous region 4b. The porous region 4a comprises through apertures fluidly interconnecting a first surface of the substrate and a second surface of the substrate. The through apertures are formed by laser-drilling. An electrochemically active layer 6 is located over the first surface of the substrate. The electrochemically active layer 6 includes a porous anode layer 6a comprising nickel oxide and cobalt doped cerium gadolinium oxide (similar to that described in GB 2 368 450, GB 2 517 927, GB 2 517 928) covering at least the porous region of the substrate. The electrochemically active layer 6 further comprises a cobalt doped cerium gadolinium oxide electrolyte layer 6b (similar to that described in GB 2 524 640) deposited over the anode layer 6a. The electrochemically active layer 6 further comprises a cathode layer 6c located on the electrolyte layer 6b. A barrier layer 2 comprising aluminium oxide is located on the second surface of the substrate 4.

[0090] Figure 2 shows an enlarged schematic diagram of a cross section of a solid oxide electrochemical cell according to the invention. The solid oxide electrochemical cell comprises a ferritic stainless-steel substrate 14, made from a nonporous metal foil and consisting of a porous region 14a surrounded by a nonporous region 14b. The porous region comprises through apertures 18 fluidly interconnecting a first surface of the substrate 14 and a second surface of the substrate 14. The through apertures 18 are formed by laser-drilling. An electrochemically active layer 16 is located on the first surface of the substrate 14. The electrochemically active layer 16 includes a porous anode layer 16a comprising nickel oxide and cobalt doped cerium gadolinium oxide (similar to that described in GB 2 368 450, GB 2 517 927, GB 2 517 928) covering at least the porous region of the substrate 14. The electrochemically active layer 16 further comprises a cobalt doped cerium gadolinium oxide electrolyte layer 16b (similar to that described in GB 2 524 640) deposited over the anode layer 16a. The electrochemically active layer 16 further comprises a cathode layer 16c located on the electrolyte layer 16b. A barrier layer 12 comprising aluminium oxide is located on the second surface of the substrate 14. The barrier layer 12 extends into all of the apertures 18 and is applied to substantially all of the walls of apertures 18.

[0091] Figure 3 shows an enlarged schematic diagram of a cross section of a solid oxide electrochemical cell according to the invention. The solid oxide electrochemical cell comprises a ferritic stainless-steel substrate 24, made from a nonporous metal foil and consisting of a porous region 24a surrounded by a nonporous region 24b. The porous region 24a comprises through apertures 28 fluidly interconnecting a first surface of the substrate 24 and a second surface of the substrate 24. The through apertures 28 are formed by laser-drilling. The electrochemically active layer 26 includes a porous anode layer 26a comprising nickel oxide and cobalt doped cerium gadolinium oxide (similar to that described in GB 2 368 450, GB 2 517 927, GB 2 517 928) covering at least the porous region of the substrate 24. The electrochemically active layer 26 further comprises a cobalt doped cerium gadolinium oxide electrolyte layer 26b (similar to that described in GB 2 524 640) deposited over the anode layer 26a. The electrochemically active layer 26 further comprises a cathode layer 26c located on the electrolyte layer 26b. A barrier layer 22 comprising aluminium oxide is located on the second surface of the substrate 24. The barrier layer 22 is present on the second surface of the metal substrate 24, with no application to the walls of apertures 28.

[0092] Figure 4 shows a flow chart illustrating a method of applying a barrier layer to a metal substrate. In step (i), a metal substrate is provided. In step (ii), the metal substrate is coated with a coating as described herein, such as a thermally decomposable resin. The coating is deposited on the surface of the substrate that will be in contact with the electrochemically active layer upon formation of the cell. In step (iii), one or more through apertures are formed by laser drilling, erosion, etching, or a combination thereof. In step (iv), a barrier layer material, such as alumina, is applied to at least the porous region of the substrate and is applied to the surface of the substrate opposing the coated surface. In step (v), the metal substrate is then heated to remove the coating. Following removal of the coating, the electrochemically active layer (not shown) may be formed on the surface of the substrate opposite the barrier layer.

[0093] Figure 5 shows a flow chart illustrating a method of applying a barrier layer to a metal substrate. In step (i), a metal substrate is provided. In step (ii), one or more through apertures are formed by laser drilling, erosion, etching, or a combination thereof. In step (iii), the metal substrate is then coated with a coating as described herein, such as a thermally decomposable resin. The coating is deposited on the surface of the substrate that will be in contact with the electrochemically active layer upon formation of the cell. In step (iv), a barrier layer material, such as alumina, is applied to at least the porous region of the substrate and is applied to the surface of the substrate opposing the coated surface. In step (v), the metal substrate is then heated to remove the coating. Following removal of the coating, the electrochemically active layer (not shown) may be formed on the surface of the substrate opposite the barrier layer. Examples

[0094] Figure 6 shows a SEM cross section image of two separate metal components of a solid oxide electrochemical cell following exposure to ammonia under solid oxide fuel cell operating conditions. The field of view (FOV) is 2.00 mm, the working distance (WD) (i.e. the distance between the bottom of the SEM column and the top of the sample) is 14.04 mm, the beam current is 1 nA, and the energy is lOkeV. The top part of the image shows the cross section of a ferritic stainless-steel metal substrate without a barrier layer applied to either surface. The bottom part of the image shows a ferritic stainless-steel interconnect, wherein a 500 nm barrier layer comprising alumina according to the invention has been applied to the underside. As can be seen from Figure 6, surface damage can be seen on the second surface (underside) of the substrate (top left in particular), whereas there is no surface damage to the interconnect comprising a barrier layer applied to the underside. This illustrates that when applied to metal substrates, the barrier layer can function to prevent corrosion of the substrate.

[0095] Figures 7(a) to 7(c) shows SEM-EDX images of cross-sections of the second surface (surface opposite the electrochemically active layers) of a ferritic stainless-steel substrate absent a barrier layer according to the invention following exposure to ammonia. As noted above, Figure 7(a) relates to site position 5 (referred to as "site 5" in Figure 7(a) and Figure 8) on the second surface of the substrate; Figure 7(b) relates to site position 7 (referred to as "site 7" in Figure 7(b) and Figure 8) on the second surface of the substrate; and Figure 7(c) relates to site position 12 (referred to as "site 12" in Figure 7(c) and Figure 8) on the second surface of the substrate. As noted above, the numerical values "5", "7", and "12", are arbitrary numbers which are merely used to denote different sample positions on the second surface of the substrate. The SEM-EDX images demonstrate that there is a greater proportion of damage to the surface of the substrate as opposed to the bulk of the substrate. Therefore, Figures 7(a) to (c) serve as visual evidence that exposure of a ferritic stainless-steel substrate (absent a barrier layer) to ammonia will result in structural damage, primarily to the surface, of said substrate. Moreover, structural damage can be observed along the length of the second surface of the substrate.

[0096] Figure 8 is a graph illustrating the nitrogen penetration by depth from the second surface for the cross-sections shown in Figures 7(a) to 7(c). As noted above, the term "bottom surface" relates to the surface of the substrate in contact with the ammonia fuel source. The term "Distance from bottom" (i.e., the X-axis) relates to the distance of the site position from the surface of the substrate in contact with the ammonia fuel source. As can be seen from Figure 8, the amount of nitrogen absorbed is greatest at the surface or proximal to the surface and decreases through the bulk of the substrate. As nitrogen absorption is linked to nitriding and microstructural changes to the bulk of the substrate, this provides additional evidence that in the absence of some form of protection, damage to the metal substrate is likely.

[0097] Figures 9(a) - 9(h) are images of variants of cells after exposure to ammonia conducted in a short stack. The cell of Figure 9(a) serves as a control and is absent a barrier layer. The cells of Figures 9(b) - 9(h) include a barrier layer according to the invention. The cell of Figure 9(b) includes a titanium carbide barrier layer having a thickness of 0.2 pm. The cell of Figure 9(c) includes a chromium nitride barrier layer having a thickness of 0.2 pm. The cell of Figure 9(d) includes an aluminium oxide barrier layer having a thickness of 0.5 pm. The cell of Figure 9(e) includes a zirconium nitride barrier layer having a thickness of 0.2 pm. The cell of Figure 9(f) includes a titanium nitride barrier layer having a thickness of 1 pm. The cell of Figure 9(g) includes a zirconium nitride barrier layer having a thickness of 1 pm. The cell of Figure 9(h) includes a titanium carbide barrier layer having a thickness of 1 pm. The metal substrate used in the cells of 9(a) to 9(h) is stainless-steel and has a thickness of 300 pm. The tests were conducted in a short stack to evaluate various barrier layer coatings of the invention. The exposure test was conducted at 610 °C for 500 hours with a concentration of 10 mol% of ammonia on the fuel side (concentration and duration based on the lack of tolerance to ammonia observed for stacks over 8 % after 120 hours). It is evident that when no barrier layer is present (Figure 9(a)) the cell has a high level of ammonia damage. There is considerably less ammonia damage when the cells include a barrier layer according to the invention. In particular, as evident from Figure 9(d), an aluminium oxide barrier layer provides a considerably high degree of protection.

[0098] Figures 10(a) and 10(b) show SEM cross section images of the cell of Figure 9(a). In Figure 10(a), the top layer represents the stainless-steel substrate, the central layer represents the spacer, and the bottom layer represents the interconnect. The field of view (FOV) is 2.15 mm, the working distance (WD) (i.e. the distance between the bottom of the SEM column and the top of the sample) is 10.00 mm, the beam current is 1 nA, and the energy is 20 keV. In Figure 10(b), the top layer represents the stainless-steel substrate, the central layer represents the spacer, and the bottom layer represents the interconnect. The field of view (FOV) is 2.15 mm, the working distance (WD) (i.e. the distance between the bottom of the SEM column and the top of the sample) is 10.03 mm, and the beam current is 998 pA. As is evident from figures 10(a) and 10(b), the substrate was heavily affected as well as the spacer. Neither the substrate nor spacer were coated and were only protected from the nitrogen ingress by the oxide scale formed during the heat treatment of the parts. Figures 11(a) and 11(b) show SEN cross section images of a cell of Figure 9(d). In Figure 11(a), the top layer represents the stainless-steel substrate, the central layer represents the spacer, and the bottom layer represents the interconnect. The substrate has an aluminium oxide barrier layer of thickness 0.5 pm, wherein the barrier layer is located on the surface of the substrate adjacent to the spacer. The field of view (FOV) is 1.11 mm, the working distance (WD) (i.e. the distance between the bottom of the SEM column and the top of the sample) is 9.95 mm, and the beam current is 997 pA. In Figure 11(b), the top layer represents the stainless-steel substrate, the central layer represents the spacer, and the bottom layer represents the interconnect. The field of view (FOV) is 1.50 mm, the working distance (WD) (i.e. the distance between the bottom of the SEM column and the top of the sample) is 9.97 mm, and the beam current is 996 pA. As is evident from both Figures 11(a) and l l(b, the presence of the aluminium oxide coating on the substrate decreases the ingress of atomic nitrogen, thereby limiting the damage that the ammonia fuel source can cause.

[0099] Figures 12(a) and 12(b) show SEM cross section images of a cell of Figure 9(h). In Figure 12(a), the top layer represents the stainless-steel substrate, the central layer represents the spacer, and the bottom layer represents the interconnect. The substrate has a titanium carbide barrier layer of thickness 1 pm, wherein the barrier layer is located on the surface of the substrate adjacent to the spacer. The field of view (FOV) is 1.83 mm, the working distance (WD) (i.e. the distance between the bottom of the SEM column and the top of the sample) is 10.02 mm, the beam current is 1 nA, and the energy is 20keV. In Figure 12(b), the top layer represents the stainless-steel substrate, the central layer represents the spacer, and the bottom layer represents the interconnect. The field of view (FOV) is 1.83 mm, the working distance (WD) (i.e. the distance between the bottom of the SEM column and the top of the sample) is 10.02 mm, the beam current is 1 nA, and the energy is 20keV.As is evident from both Figures 12(a) and 12(b), the presence of the titanium carbide coating on the substrate decreases the ingress of atomic nitrogen, thereby limiting the damage that the ammonia fuel source can cause.

[0100] It would be appreciated that the process and apparatus of the invention are capable of being implemented in a variety of ways, only a few of which have been illustrated and described above.

Claims

Claims1. A solid oxide electrochemical cell, the cell comprising : a metal substrate comprising a porous region and a nonporous region bounding the porous region, wherein the porous region comprises multiple through apertures fluidly interconnecting a first surface of the metal substrate and a second surface of the metal substrate; an electrochemically active layer located on the first surface of the metal substrate wherein the electrochemically active layer is located over at least the porous region of the metal substrate; and a barrier layer applied to the second surface of the metal substrate, wherein the barrier layer is applied to at least the porous region of the metal substrate.

2. A cell according to claim 1, wherein the barrier layer has a thickness in the range 100 nm to 2000 nm.

3. A cell according to claim 1 or claim 2, wherein the barrier layer comprises a metal, a metallic compound, a ceramic compound, or a combination thereof.

4. A cell according to any preceding claim, wherein the barrier layer comprises a metal, a nitride, a carbide, a metal oxide, a metalloid oxide, or a combination thereof.

5. A cell according to any preceding claim, wherein the barrier layer comprises a metal and / or metal oxide.

6. A cell according to any preceding claim, wherein the barrier layer comprises aluminium, aluminium oxide, erbium oxide, boron nitride, silicon nitride, zirconium nitride, titanium nitride, titanium carbide, chromium nitride, or combinations thereof.

7. A cell according to any preceding claim, wherein the barrier layer comprises aluminium oxide, titanium carbide, titanium nitride, zirconium nitride, chromium nitride, or a combination thereof.

8. A cell according to any preceding claim, wherein the barrier layer comprises aluminium and / or aluminium oxide.

9. A cell according to any preceding claim, wherein the through apertures include aperture walls, and wherein the barrier layer is additionally applied to at least part of the aperture walls.

10. A cell according to any preceding claim, wherein the barrier layer is only present on the second surface of the metal substrate, or wherein the barrier layer is present on the aperture walls and on the second surface of the substrate.

11. A cell according to any preceding claim, wherein the barrier layer is a nitrogen diffusion barrier layer and / or a hydrogen diffusion barrier layer.

12. A cell according to any preceding claim, wherein the metal substrate comprises a metal foil.

13. A cell according to any preceding claim, wherein the electrochemical cell is a solid oxide fuel cell (SOFC).

14. A solid oxide cell stack comprising two or more cells according to any one of claims 1 to 13.

15. A method of manufacturing a solid oxide electrochemical cell, the method comprising the following steps:(i) providing a coated metal substrate comprising a porous region and a nonporous region bounding the porous region, wherein the porous region comprises multiple through apertures fluidly interconnecting a first surface of the metal substrate and a second surface of the metal substrate, and wherein the coating is thermally decomposable;(ii) applying a barrier layer material to at least the porous region of the second surface of the metal substrate;(iii) heating the metal substrate to remove the coating and optionally form the barrier layer by sintering the barrier layer material; and(iv) forming an electrochemically active layer on the first surface of the metal substrate and sintering.

16. A method according to claim 15, wherein the barrier layer material is applied via chemical vapour deposition (CVD), metal organic chemical vapor deposition (MOCVD), or physical vapor deposition.

17. A method according to claim 15 or claim 16, wherein the coating is applied to the metal substrate prior to step (i).

18. A method according to any of claims 15 to 17, wherein the multiple through apertures are formed before applying the coating.

19. A method according to claim 18, wherein the coating at least partly seals the multiple through apertures on the first surface of the metal substrate.

20. A method according to any of claims 15 to 19, wherein the barrier layer material comprises a metal, a metallic compound, a ceramic compound, or a combination thereof.

21. A method according to any of claims 15 to 20, wherein the barrier layer material comprises a metal, a nitride, a carbide, a metal oxide, a metalloid oxide, or a combination thereof.

22. A method according to any of claims 15 to 21, wherein the barrier layer material comprises aluminium, aluminium oxide, erbium oxide, boron nitride, silicon nitride, zirconium nitride, titanium nitride, titanium carbide, chromium nitride, or a combination thereof.

23. A method according to any of claims 15 to 22, wherein the barrier layer material comprises aluminium oxide, titanium carbide, titanium nitride, zirconium nitride, chromium nitride, or a combination thereof.

24. A method according to any one of claims 15 to 23, wherein the barrier layer material comprises a metal, and wherein the metal is oxidised during step (iii) to form the barrier layer.

25. A method according to any one of claims 15 to 24, wherein the barrier layer comprises a metal oxide.

26. A method of operation of a solid oxide electrochemical cell, wherein the method comprises the following steps:(i) provision of a cell, wherein the cell comprises a metal substrate comprising a porous region and a nonporous region bounding the porous region, wherein the porous region comprises multiple through apertures fluidly interconnecting a first surface of the metal substrate and a second surface of the metal substrate; an electrochemically active layer located on the first surface of the metal substrate, wherein the electrochemically active layer islocated over at least the porous region of the metal substrate; and a barrier layer located on the second surface of the metal substrate, wherein the barrier layer is applied to at least the porous region of the metal substrate; and(ii) introduction of a gas source into the cell, wherein the gas source is in fluid communication with the barrier layer.

27. A system comprising : a solid oxide electrochemical cell according to any one of claims 1 to 13 comprising a metal substrate comprising a porous region and a nonporous region bounding the porous region, wherein the porous region comprises multiple through apertures fluidly interconnecting a first surface of the metal substrate and a second surface of the metal substrate; an electrochemically active layer located on the first surface of the metal substrate, wherein the electrochemically active layer is located over at least the porous region of the metal substrate; and a barrier layer applied to the second surface of the metal substrate, wherein the barrier layer is applied to at least the porous region of the metal substrate; a gas source; and a fluid flow path from the gas source to the solid oxide electrochemical cell, wherein the gas source is in fluid communication with the barrier layer of the solid oxide electrochemical cell.

28. A method according to claim 26, wherein the gas source comprises a fuel source, and wherein the method further comprises introduction of an air source, wherein the air source is in fluid communication with the electrochemically active layer.

29. A system according to claim 27, wherein the gas source comprises a fuel source; and wherein the system further comprises an air source, and a fluid flow path from the air source to the solid oxide electrochemical cell, wherein the air source is in fluid communication with the electrochemically active layer of the solid oxide electrochemical cell.

30. A method according to claim 28 or a system according to claim 29, wherein the fuel source comprises ammonia.

31. A method according to claim 26 or a system according to claim 27, wherein the gas source comprises a reactive fluid.

32. Use of a solid oxide electrochemical cell according to any of claims 1 to 13 or a solid oxide cell stack according to claim 14 in the generation of electricity.

Citation Information

Patent Citations

  • Fuel cells

    GB2368450A

  • Impermeable sintered ceramic electrolyte layer for a solid oxide fuel cell

    GB2386126A

  • Densification of ceria based electrolytes

    GB2400486A

  • Metal substrate for fuel cells

    GB2440038A

  • Process for forming a metal supported solid oxide fuel cell

    GB2517927A