Electrode, battery, and battery pack

The electrode with a titanium-containing oxide coated in aluminum oxide, featuring specific particle and aggregate structures, addresses the challenges of resistance and temperature limitations in lithium-ion batteries, achieving enhanced performance and energy density.

WO2024201552A1PCT designated stage expired Publication Date: 2024-10-03KK TOSHIBA
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/011713
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Lithium-ion batteries face challenges in maintaining high current performance and low-temperature functionality due to increased electrical resistance and surface side reactions, particularly when using spinel-type lithium titanate as the negative electrode material.

Method used

The electrode is designed with a titanium-containing oxide coated with an aluminum oxide compound, featuring primary particles and aggregates, which suppresses resistance increase and enhances energy density by controlling the radial distribution function and aggregate size, thereby improving lithium ion acceptance and reducing side reactions.

Benefits of technology

The solution effectively reduces electrical resistance, enhances low-temperature performance, and maintains high current capability, resulting in improved energy density and prolonged battery life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023011713_03102024_PF_FP_ABST
    Figure JP2023011713_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided, according to an embodiment of the present invention, is an electrode having an active material-containing layer including: an active material comprising a titanium-containing oxide; and an aluminum oxide compound present on the surface of the active material. Forms of the titanium-containing oxide include primary particles and aggregates containing a plurality of primary particles. According to a radial distribution function obtained by Fourier transform of an extended X-ray absorption fine structure spectrum of the K-edge of aluminum of the active material-containing layer, the value of the peak intensity ratio IA / IB, where peak A appears between 1.1 Å and 1.5 Å and peak B appears between 2.8 Å and 3.2 Å, is 3.5 to 9. The smallest square circle diameter Dg of the aggregate is at least 1 / 20 but less than 1 / 2 with respect to the thickness Te of the active material-containing layer.
Need to check novelty before this filing date? Find Prior Art

Description

Electrodes, batteries, and battery packs

[0001] FIELD OF THE INVENTION Embodiments of the present invention relate to electrodes, batteries, and battery packs.

[0002] Lithium-ion secondary batteries, which are charged and discharged by the movement of lithium ions between the positive and negative electrodes, are being widely used in a wide range of applications, from small-scale applications such as portable electronic devices to large-scale applications such as electric vehicles and power supply and demand adjustment, taking advantage of their high energy density and high output.

[0003] Instead of a carbon material, a negative electrode active material having a lithium absorption / desorption potential of about 1.55 V (vs. Li / Li) based on a lithium electrode was used. + Non-aqueous electrolyte batteries using spinel-type lithium titanate with high conductivity (e.g., 1000kJ / s) have also been put to practical use. Spinel-type lithium titanate exhibits excellent cycle performance due to minimal volume change during charging and discharging. Furthermore, negative electrodes containing spinel-type lithium titanate do not precipitate lithium metal during lithium absorption and desorption, enabling secondary batteries equipped with such negative electrodes to be charged at high currents and low temperatures. To further improve high-current and low-temperature performance, attempts have been made to coat spinel-type lithium titanate particles with aluminum oxide compounds.

[0004] Japanese Patent Application Publication No. 2019-169276

[0005] B. Ravel and M. Newville, ATHENA, ARTHEMIS, HEPHAESTUS: data analysis for X-ray absorption spectroscopy using IFEFFIT, Journal of Synchrotron Radiation 12, 537-541 (2005)

[0006] The object is to provide an electrode that can realize a battery with suppressed electrical resistance and resistance increase, and excellent energy density and low-temperature performance, a battery including this electrode, and a battery pack including this battery.

[0007] According to an embodiment, an electrode is provided having an active material-containing layer including an active material containing a titanium-containing oxide and an aluminum oxide compound present on the surface of the titanium-containing oxide. The titanium-containing oxide has a morphology including primary particles and aggregates containing a plurality of primary particles. The active material-containing layer includes a peak A appearing in the range of 1.1 Å to 1.5 Å and a peak B appearing in the range of 2.8 Å to 3.2 Å in the radial distribution function obtained by Fourier transform of a broadened X-ray absorption fine structure spectrum at the Al K absorption edge. The peak intensity I of peak B is B The peak intensity I of peak A A Ratio I A / I B The value of the least squares circle diameter D of the aggregate is 3.5 or more and 9 or less. g is the thickness T of the active material-containing layer e It is 1 / 20 or more and less than 1 / 2 of the above.

[0008] According to another embodiment, there is provided a battery comprising a positive electrode, a negative electrode, and an electrolyte. The negative electrode comprises the electrode described above.

[0009] According to yet another embodiment, there is provided a battery pack, the battery pack including the battery described above.

[0010] FIG. 1 is a plan view schematically illustrating an example of an electrode according to an embodiment. FIG. 2 is a schematic cross-sectional view of the electrode shown in FIG. 1 taken along line II-II. FIG. 3 is a conceptual diagram illustrating an example of a portion of a binarized cross-sectional image of the electrode according to an embodiment, obtained by a scanning electron microscope. FIG. 4 is a conceptual diagram illustrating another example of a portion of a binarized cross-sectional image of the electrode according to an embodiment, obtained by a scanning electron microscope. FIG. 5 is a conceptual diagram illustrating another example of a portion of a binarized cross-sectional image of the electrode according to an embodiment, obtained by a scanning electron microscope. FIG. 6 is a graph showing a radial distribution function obtained by Fourier transform of an extended X-ray absorption fine structure spectrum at the Al K-edge for the surface of an example of an electrode according to an embodiment. FIG. 7 is a cross-section of an example of a battery according to an embodiment, cut in the thickness direction. FIG. 8 is an enlarged cross-sectional view of portion E in FIG. 7. FIG. 9 is a partially cutaway perspective view of another example of a battery according to an embodiment. FIG. 10 is an exploded perspective view of an example of a battery pack according to an embodiment. FIG. 11 is a block diagram showing an electrical circuit of the battery pack shown in FIG. 10. Embodiment

[0011] It has been reported that coating active material particles with an aluminum oxide compound can improve resistance. However, because aluminum oxide compounds are insulating, the inclusion of an aluminum oxide compound increases the initial resistance. Therefore, coating with an aluminum oxide compound has the drawback of reducing charge / discharge rate performance.

[0012] Hereinafter, embodiments will be described with reference to the drawings. Note that common components throughout the embodiments will be denoted by the same reference numerals, and duplicated descriptions will be omitted.

[0013] Furthermore, each figure is a schematic diagram intended to facilitate explanation and understanding of the embodiment, and the shape, dimensions, ratios, etc. may differ from those of the actual device, but these can be appropriately modified in design by taking into consideration the following explanation and known technology.

[0014] (First Embodiment) According to the first embodiment, an electrode is provided. The electrode comprises an active material-containing layer containing an active material and an aluminum oxide compound. The active material includes a titanium-containing oxide. The aluminum oxide compound is present on the surface of the titanium-containing oxide. The titanium-containing oxide may be in the form of primary particles or aggregates containing a plurality of these primary particles. The radial distribution function obtained by Fourier transform of the broadened X-ray absorption fine structure spectrum at the Al K absorption edge for the active material-containing layer includes peak A appearing in the range of 1.1 Å to 1.5 Å and peak B appearing in the range of 2.8 Å to 3.2 Å. The peak intensity I of peak B is B The peak intensity I of peak A A Ratio I A / I B The value of the least squares circle diameter D of the aggregate is 3.5 or more and 9 or less. g is the thickness T of the active material-containing layer e It is 1 / 20 or more and less than 1 / 2 of the above.

[0015] The electrode according to the embodiment may be a battery electrode. Examples of batteries that may include the electrode according to the embodiment include secondary batteries such as lithium ion secondary batteries. Secondary batteries include non-aqueous electrolyte secondary batteries that include a non-aqueous electrolyte. The electrode may be, for example, a negative electrode for the battery.

[0016] Secondary batteries with anodes containing titanium-containing oxides have excellent cycle life and storage performance, and are capable of high-current charging and discharging and charging under low-temperature conditions. To further improve these high-current and low-temperature performance, attempts have been made to reduce the size of the active material particles. While reducing the size of the active material particles improves input / output performance, it also increases resistance due to surface side reactions.

[0017] The present inventors have conducted extensive research to solve this problem in nonaqueous electrolyte batteries equipped with a negative electrode containing a titanium-containing oxide, and as a result have discovered the electrode according to the first embodiment. Specifically, they have found that the presence of a specific aluminum oxide compound on the surface of the titanium-containing oxide can suppress an increase in resistance due to a surface side reaction, and that agglomeration of some particles can suppress the increase in resistance while improving rate performance and energy density.

[0018] The electrode according to the first embodiment is an electrode containing a titanium-containing oxide as an electrode active material, and has an aluminum oxide compound on the surface of titanium-containing oxide particles. In the active material-containing layer of the electrode, the titanium-containing oxide coated with the aluminum oxide compound exists in two states: primary particles and aggregates formed by aggregation of the primary particles. The radial distribution function obtained by Fourier transform of the extended X-ray absorption fine structure (EXAFS) spectrum at the Al K absorption edge for the electrode surface includes Peak A appearing in the range of 1.1 Å to 1.5 Å and Peak B appearing in the range of 2.8 Å to 3.2 Å. The peak intensity I of Peak B is B The peak intensity I of peak A A Ratio I A / I B The value of the least squares circle diameter D g is the thickness T of the active material-containing layer e The electrode has a size that is 1 / 20 or more and less than 1 / 2 of the electrode. By having such a configuration, it is possible to provide a battery that has good rate performance, suppresses an increase in resistance during storage, and is excellent in low-temperature output performance.

[0019] The mechanism by which such an electrode improves storage performance is not fully understood, but it is thought to be, for example, as follows.

[0020] When the primary particle size of the active material particles is reduced, for example, to 1 μm or less, the specific surface area increases, improving the lithium ion acceptance of the active material itself. However, as the primary particle size decreases, the proportion of active sites on the active material surface increases. This increases side reactions between the active material and the electrolyte, etc., and increases the electrical resistance during storage.

[0021] The presence of aluminum oxide compounds in a specific state on the surface of the active material can suppress side reactions with the electrolyte, etc. Specifically, the radial distribution function of the EXAFS spectrum of Al obtained by Fourier transform (FT-EXAFS) includes peak A in the range of 1.1 Å to 1.5 Å and peak B in the range of 2.8 Å to 3.2 Å, and the peak intensity ratio I A / I B In an electrode in which the value of is 3.5 or more and 9 or less, it is determined that the aluminum oxide compound is present on the active material surface in a state that is effective in suppressing the above-mentioned side reactions. It is believed that at least a part of the aluminum oxide compound condenses with functional groups that can become active sites present on the active material surface, thereby suppressing the side reactions.

[0022] Furthermore, a portion of the titanium-containing oxide contained in the electrode exists as aggregates formed by the aggregation of primary particles. For example, titanium-containing oxide aggregates can be formed by a reaction between an alcohol contained in a solution of an aluminum alkoxide compound that can function as an aluminum oxide compound source and a binder that the electrode may contain together with the active material. Titanium-containing oxide exhibits conductivity when lithium ions are inserted, for example, when an electrode containing titanium-containing oxide as a negative electrode active material is in a charged state. Therefore, in an electrode with the above configuration, current flows concentrated in the aggregates with small gaps between grain boundaries during short-term high current application. This reduces electrical resistance (IR drop) during short-term use. Furthermore, as described above, the aluminum oxide compound coating suppresses side reactions on the active material surface, which is thought to suppress uneven deterioration during high-current use. Furthermore, a battery with excellent low-temperature performance can be provided.

[0023] The mixture of primary particles and aggregates of the titanium-containing oxide in the active material-containing layer allows for close packing of the active material, resulting in an electrode with excellent energy density.

[0024] Least square circular diameter D of the aggregate g is the thickness T of the active material-containing layer e is 1 / 20 or more and less than 1 / 2 (1 / 20≦D g / T e < 1 / 2). The least squares circular diameter of the aggregate D g may be, for example, in the range of 4 μm to 20 μm.

[0025] Next, the electrode according to the first embodiment will be described in more detail.

[0026] The electrode includes an active material-containing layer (electrode mixture layer) and may further include a current collector. The active material-containing layer may be formed, for example, on one side or both sides of a strip-shaped current collector. The active material-containing layer may include an active material, an aluminum oxide compound, and optionally a conductive agent and a binder.

[0027] The active material contains, for example, a titanium-containing oxide having an average primary particle size of 600 nm or more and 1 μm or less. The titanium-containing oxide preferably contains a lithium-titanium composite oxide. An electrode containing a titanium-containing oxide such as a lithium-titanium composite oxide has a potential of 0.4 V (vs. Li / Li) relative to the oxidation-reduction potential of lithium. + ) or more, it is possible to prevent the deposition of metallic lithium on the electrode surface when a large current is repeatedly input and output. It is particularly preferable that the titanium-containing oxide contains a lithium-titanium composite oxide having a spinel-type crystal structure. Specific examples of such spinel-type lithium-titanium composite oxides include Li 4+a Ti 5 O 12 The value of the subscript a varies within the range of 0≦a≦3 upon charge and discharge.

[0028] The titanium-containing oxide is coated with an aluminum oxide compound. The titanium-containing oxide coated with the aluminum oxide compound exists in two states in the active material-containing layer: primary particles and aggregates formed by aggregation of the primary particles. The term "aggregate" here refers to a collection of active material that, when a binarization process is performed on the active material (titanium-containing oxide) and voids in an image obtained by observing a cross section of the active material-containing layer with a scanning electron microscope (SEM), does not contain any "0"s within the active material (titanium-containing oxide) and voids, and in an image obtained by observation with a transmission electron microscope (TEM), aluminum elements are confirmed within the active material by energy dispersive X-ray spectroscopy (EDX). For example, the "aggregate" in each embodiment is distinguished from secondary particles having internal voids. Furthermore, the "aggregate" in each embodiment is also distinguished from secondary particles that were formed as secondary particles before being coated with the aluminum oxide compound. While the active material particles at the center of the aggregate are coated with the aluminum oxide compound, the active material particles at the center of the secondary particles, as exemplified here, are not coated with the aluminum oxide compound. The presence of the aluminum oxide compound not only on the periphery of the aggregates but also on the surfaces of the primary particles located inside the aggregates can suppress side reactions between the electrolyte solution that gradually penetrates over time and the active material. It is desirable that the secondary particles of the titanium-containing oxide contained in the active material-containing layer of such an electrode are all aggregates as described above. SEM observation will be described in detail later. The aggregates may further contain an aluminum oxide compound and a binder in addition to the titanium-containing oxide.

[0029] The active material may contain an active material other than the titanium-containing oxide. Here, for convenience, the active material containing the titanium-containing oxide is sometimes referred to as the "first active material," and the other active material is sometimes referred to as the "second active material." When the second active material is further contained in addition to the first active material, the second active material is used as the active material having a potential of 0.4 V (vs. Li / Li + When the second active material is contained, the mass ratio of the second active material to the first active material is preferably 5% by mass or more and 40% by mass or less, and more preferably 10% by mass or more and 30% by mass or less.

[0030] The aluminum oxide compound can have the effect of coating the surface of the active material containing at least a titanium-containing oxide and suppressing an increase in resistance. The aluminum oxide compound is, for example, derived from an aluminum oxide compound.

[0031] The conductive agent can improve current collection performance and reduce contact resistance between the active material and the current collector. Examples of the conductive agent include carbonaceous materials such as acetylene black, carbon black, graphite, carbon nanofibers, and carbon nanotubes. These carbonaceous materials may be used alone or in combination.

[0032] The binder can bind the active material, conductive agent, and current collector together. Examples of the binder include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine-containing rubber, styrene-butadiene rubber, acrylic resin and its copolymer, polyacrylic acid, and polyacrylonitrile.

[0033] The compounding ratios of the active material, conductive agent, and binder are preferably in the ranges of 70% by mass or more and 97.5% by mass or less for the active material, 2% by mass or more and 20% by mass or less for the conductive agent, and 0.5% by mass or more and 10% by mass or less for the binder. By setting the amount of conductive agent to 2% by mass or more, the current collection performance of the active material-containing layer can be improved, and excellent high-current performance and low-temperature performance can be expected. Furthermore, by setting the amount of binder to 0.5% by mass or more, sufficient binding between the active material-containing layer and the current collector can be expected, and excellent life performance can be expected.

[0034] On the other hand, from the viewpoint of increasing capacity, the conductive agent and binder are each preferably contained in an amount of 20% by mass or less, and more preferably contained in an amount of 10% by mass or less.

[0035] Area S of the cross section of the active material-containing layer E Whereas, the cross-sectional area S of the aggregate occupying the cross section G The ratio S G / S EWhen the proportion of aggregates in the active material is such that 1 / 200 to 1 / 4 of the total cross-sectional area of ​​the cross section of the active material-containing layer is 1 / 200 to 1 / 4, the primary particles of the active material can enter the gaps between the aggregates. Therefore, the electrode described above has excellent energy density.

[0036] The current collector is preferably formed from an aluminum foil or an aluminum alloy foil containing elements such as Mg, Ti, Zn, Mn, Fe, Cu, and Si. The thickness of the current collector is preferably 20 μm or less, and more preferably 15 μm or less.

[0037] Next, specific examples of the electrodes according to the first embodiment will be described with reference to the drawings.

[0038] Fig. 1 is a partially cutaway plan view schematically showing an example of such an electrode, and Fig. 2 is a cross-sectional view taken along line II-II in Fig. 1. Here, an example of a negative electrode is shown as an example of the electrode.

[0039] The negative electrode 4 shown in Figures 1 and 2 includes a negative electrode current collector 4a and a negative electrode active material-containing layer 4b provided on the surface of the negative electrode current collector 4a. The negative electrode active material-containing layer 4b is supported on a main surface of the negative electrode current collector 4a. The negative electrode active material-containing layer 4b may be provided on both the front and back main surfaces of the negative electrode current collector 4a, as shown in Figure 2. Alternatively, the negative electrode active material-containing layer 4b may be provided on only one main surface of the negative electrode current collector 4a.

[0040] The negative electrode current collector 4a also includes a portion on its surface where the negative electrode active material-containing layer 4b is not provided. This portion functions, for example, as a negative electrode current collector tab 4c. In the illustrated example, the negative electrode current collector tab 4c is a narrow portion that is narrower than the negative electrode active material-containing layer 4b. The width of the negative electrode current collector tab 4c may be narrower than the width of the negative electrode active material-containing layer 4b, or may be the same as the width of the negative electrode active material-containing layer 4b. Instead of the negative electrode current collector tab 4c that is part of the negative electrode current collector 4a, a separate conductive member may be electrically connected to the negative electrode 4 and used as an electrode current collector tab (negative electrode current collector tab).

[0041] The negative electrode active material-containing layer 4b contains a negative electrode active material containing a titanium-containing oxide. The negative electrode active material is contained in the negative electrode active material-containing layer 4b in the form of primary particles and in the form of aggregates 4d formed by aggregation of the primary particles. In FIG. 2, the primary particles forming the aggregates 4d are not depicted. The negative electrode active material-containing layer 4b may further contain a conductive agent and a binder in addition to the negative electrode active material. In FIG. 2, each component other than the aggregates 4d contained in the negative electrode active material-containing layer 4b (other active materials such as titanium-containing oxide in the form of primary particles, the conductive agent, and the binder) is omitted, and the portion of the negative electrode active material-containing layer 4b other than the aggregates 4d is schematically depicted.

[0042] Thickness T of the negative electrode active material-containing layer 4b e On the other hand, the average least squares circle diameter D of the aggregates 4d contained in the negative electrode active material containing layer 4b is g (not shown) is 1 / 20 or more and less than 1 / 2.

[0043] In the aggregates 4d, the active material particles constituting the aggregates 4d are close to each other, and the grain boundaries between the particles are not separated. Therefore, the current 10 flows more easily through the aggregates 4d than through the remaining portions of the negative electrode active material-containing layer 4b. Therefore, when a large current is passed through the aggregates 4d for a short period of time, the current 10 flows concentratedly through the aggregates 4d.

[0044] <<Manufacturing of Electrode>> The electrode can be manufactured as follows.

[0045] First, an active material containing a titanium-containing oxide is prepared. The titanium-containing oxide can be synthesized by, for example, a solid-phase method. Alternatively, the titanium-containing oxide can be synthesized by a wet synthesis method such as a sol-gel method or a hydrothermal method.

[0046] First, a Ti source and a Li source are prepared according to the target composition. These raw materials may be compounds such as oxides or salts. Examples of the Li source that can be used include lithium hydroxide, lithium oxide, and lithium carbonate.

[0047] Next, the prepared raw materials are mixed in an appropriate stoichiometric ratio to obtain a mixture. For example, a mixture having the composition formula Li 4 Ti 5 O 12When synthesizing a spinel-type lithium-titanium composite oxide represented by the formula (I), titanium oxide TiO 2 and lithium carbonate Li 2 CO 3 and Ti may be mixed such that the molar ratio of Li:Ti in the mixture is 4:5.

[0048] When mixing the raw materials, Li may be mixed in an amount greater than the predetermined amount. In particular, Li may be added in an amount greater than the predetermined amount because there is a concern that Li may be lost during heat treatment.

[0049] In the wet method, the raw materials are dissolved in pure water, and the resulting solution is dried while being stirred to obtain a calcined precursor. The drying method can be spray drying, granulation drying, freeze drying, or a combination of these.

[0050] Next, the mixture or calcined precursor obtained by the previous mixing is heat-treated at a temperature of 750°C or higher and 1000°C or lower for a time of 30 minutes to 24 hours. At temperatures below 750°C, sufficient crystallization is difficult to obtain. On the other hand, at temperatures above 1000°C, excessive grain growth occurs, resulting in coarse particles, which is undesirable. Similarly, if the heat treatment time is less than 30 minutes, sufficient crystallization is difficult to obtain. Furthermore, if the heat treatment time is longer than 24 hours, excessive grain growth occurs, resulting in coarse particles, which is undesirable. Calcination may be carried out in the air. Calcination may also be carried out in an oxygen atmosphere, a nitrogen atmosphere, or an argon atmosphere.

[0051] The mixture is preferably heat-treated at a temperature of 800°C to 950°C for 1 hour to 5 hours. A titanium-containing oxide can be obtained by such heat treatment. Pre-calcination may also be performed before the main calcination. The pre-calcination is performed at a temperature of 450°C to 700°C for 5 hours to 24 hours.

[0052] When using a method that uses water, such as a wet method, attention must be paid to the amount of moisture remaining after firing. The remaining moisture can react with the aluminum alkoxide compound added later to form a resistive component. Therefore, adjusting the firing temperature and firing time also leads to control of the radial distribution function of Al measured by FT-EXAFS.

[0053] The sample obtained by the calcination can be subjected to a pulverization process to break down agglomerates (secondary particles) into primary particles. Examples of pulverization methods that can be used include a mortar, ball mill, sand mill, vibration ball mill, planetary ball mill, bead mill, jet mill, counter jet mill, and swirling air jet mill. Wet pulverization in the presence of a liquid pulverization aid, such as water, ethanol, ethylene glycol, benzene, or hexane, can also be used. The pulverization aid is effective in improving pulverization efficiency and increasing the amount of fine powder produced. A more preferred method is a ball mill using zirconia balls as media, and wet pulverization with the addition of a liquid pulverization aid is preferred. Furthermore, organic substances such as polyols may be added as pulverization aids to improve pulverization efficiency. The type of polyol is not particularly limited, but pentaerythritol, triethylolethane, trimethylolpropane, and the like can be used alone or in combination.

[0054] Furthermore, re-firing may be performed after the pulverization treatment. The average crystallite size of the titanium-containing oxide particles can be controlled by adjusting the firing conditions. Re-firing may be performed in the air or in an inert atmosphere using oxygen, nitrogen, argon, or the like. Re-firing may be performed at a temperature of 250°C to 900°C for approximately 1 minute to 10 hours. At 900°C or less, sintering between powder particles can be avoided. At 250°C or higher, impurities (organic substances) adhering during wet pulverization can be removed. Preferably, re-firing is performed at a temperature of 400°C to 700°C for 10 minutes to 3 hours. Furthermore, it is preferable to wash the powder with an aqueous solvent before re-firing.

[0055] Furthermore, in order to obtain primary particles having a specific particle size, classification can be carried out as necessary.

[0056] Next, an electrode slurry is prepared using the active material containing the titanium-containing oxide prepared as described above. When a second active material other than a titanium-containing oxide is further used, the electrode slurry is prepared using the second active material together with the active material containing the titanium-containing oxide (first active material). Specifically, the active material and the conductive agent are mixed to obtain a mixture, and then a binder, an aluminum alkoxide compound, and a solvent are added, followed by kneading and dispersion treatment to prepare a slurry. As the solvent (dispersion medium), for example, N-methylpyrrolidone (NMP) can be used.

[0057] Aluminum alkoxide is a type of metal alkoxide. Metal alkoxide has a structure in which an alkoxy group is coordinated around a metal element (M: Ti, Zr, Al, Si, etc.), and is represented by M(OR). n This material is expressed as follows. It reacts with a Lewis base to synthesize a material with a MOM bond as the main chain. The aluminum alkoxide compound added to the electrode slurry preferably has at least two alkoxy groups coordinated with each other, and the other substituents have a chain or cyclic structure consisting of C, O, N, or other functional groups. A chelate structure is even more preferable. It is also preferable to use an alkoxide compound with a substituent containing three or more carbon atoms. Examples of usable compounds include di-2-butoxyaluminum ethyl acetoacetate (Al(C4H9O)2(C6H9O3)), aluminum tri-2-butoxide (Al(OC4H9)3), di-2-butoxyaluminum acetylacetate (Al(C4H9O)2(C5H7O2)), and aluminum tri-sec-butoxide (Al(O-sec-C4H9)3). In electrodes to which the above aluminum alkoxide compounds have been added, the peak intensity ratio I of the radial distribution function of Al measured by FT-EXAFS is A / I BThe above-mentioned state, in which the value of is 3.5 or more and 9 or less, is easily achieved. In other words, the addition of these aluminum alkoxide compounds is effective in suppressing side reactions on the electrode. Other aluminum alkoxide compounds having a substituent with less than 4 carbon atoms include, for example, aluminum isopropoxide (Al(Oi-Pr)3). The aluminum alkoxide compound to be added may be one type, or two or more types.

[0058] Solvents are used in aluminum alkoxide compounds to maintain their structure during storage. Examples of solvents include alcohols such as ethanol, propanol, and butanol. Furthermore, alcohol is released from aluminum alkoxides through hydrolysis. Therefore, even when an aluminum alkoxide reagent is used with an alcohol-free solvent, alcohol is introduced into the system. As described above, the reaction between the alcohol and the binder forms aggregates containing the active material. In addition to the active material (titanium-containing oxide), the aggregates may contain the binder and, for example, an aluminum oxide compound formed by the release of organic components from the aluminum alkoxide.

[0059] The amount and size of the aggregates formed can be controlled by adjusting the content ratio of each component (active material, conductive agent, binder) contained in the electrode and the type and amount of aluminum alkoxide compound added. In addition, the size of the aggregates can be controlled by adjusting the timing of adding the aluminum alkoxide compound.

[0060] For example, when the amount of aluminum alkoxide compound added is reduced, the number of aggregates in the active material-containing layer decreases, and the ratio S G / S E Conversely, when the amount of aluminum alkoxide compound added is increased, the number of aggregates in the active material-containing layer increases, and the specific S G / S E tends to increase.

[0061] The aluminum alkoxide compound may be added before kneading, or may be added after kneading and dispersion.

[0062] The slurry prepared as described above is applied to one or both sides of a current collector, and the coating is then dried. Thus, an electrode mixture layer (active material-containing layer) can be formed. Thereafter, the electrode mixture layer is pressed. Thus, the electrode according to the first embodiment can be obtained.

[0063] <Measurement of Electrodes> Various measurement methods for electrodes will be described. Specifically, a method for confirming that the electrode contains a titanium-containing oxide, a method for observing the cross section of the electrode using a scanning electron microscope, and a method for measuring extended X-ray absorption fine structure (EXAFS) at the Al K absorption edge and then Fourier transforming the obtained EXAFS spectrum to obtain a radial distribution function will be described.

[0064] If the electrode to be measured is incorporated into a battery, the electrode to be used as the measurement sample is removed from the battery as follows: The battery is discharged, disassembled in a glove box with an inert atmosphere such as argon, and the electrode is removed. The electrode is washed with diethyl carbonate and then vacuum dried. This is how the measurement sample is obtained.

[0065] <Confirmation of Titanium-Containing Oxide> The active material contained in the electrode can be identified as follows to confirm whether or not the electrode contains a titanium-containing oxide.

[0066] After washing and drying the electrodes removed from the battery as described above, attach the resulting electrodes to a glass sample plate. At this time, care should be taken to prevent the electrodes from peeling or floating, using double-sided tape or similar. If necessary, the electrodes can be cut to a size appropriate for attaching to the glass sample plate. In addition, a Si standard sample can be added to the electrodes to correct the peak position.

[0067] The glass plate with the electrodes attached is then placed in a powder X-ray diffraction (XRD) device, and a diffraction pattern is obtained using Cu-Kα radiation. Measurements are performed using Cu-Kα radiation as the radiation source, with 2θ varied within the measurement range of 5° to 90°, to obtain an X-ray diffraction pattern.

[0068] The powder X-ray diffraction measurement device used is, for example, a SmartLab manufactured by Rigaku Co., Ltd. The measurement conditions are as follows: X-ray source: Cu target, Output: 45 kV, 200 mA, Soller slit: 5° for both incident and receiving, Step width: 0.02°, Scan rate: 20° / min, Semiconductor detector: D / teX Ultra 250, Sample plate holder: Flat glass sample plate holder (thickness: 0.5 mm), Measurement range: 5°≦2θ≦90°.

[0069] When using other equipment, measurements are carried out using standard Si powder for powder X-ray diffraction to obtain measurement results equivalent to those obtained by the above equipment, and conditions are found under which the peak intensities and peak top positions are equivalent to those obtained by the above equipment, and the sample is measured under those conditions.

[0070] When the active material to be measured contains a spinel-type lithium-titanium composite oxide, it can be confirmed by X-ray diffraction measurement that an X-ray diffraction pattern belonging to the space group Fd-3m is obtained.

[0071] Next, the sample containing the active material is observed using a scanning electron microscope (SEM). It is desirable to prevent the sample from coming into contact with the air during SEM observation as well, and to perform the observation in an inert atmosphere such as argon or nitrogen.

[0072] In a 3000x SEM observation image, several particles having the form of primary particles or secondary particles that can be confirmed within the field of view are selected. The selected particles are selected so that the particle size distribution is as wide as possible. The observed active material particles are then subjected to energy dispersive X-ray spectroscopy (EDX) to identify the type and composition of the constituent elements of the active material. This allows the type and amount of elements other than Li contained in each selected particle to be identified. The same procedure is performed on each of the multiple active material particles to determine the mixed state of the active material particles.

[0073] Next, the active material-containing layer is separated from the current collector using, for example, a spatula, to obtain a powdered electrode mixture sample containing the active material. The collected powdered sample is washed with acetone and dried. The obtained powder is dissolved in hydrochloric acid, the conductive agent is removed by filtration, and then the solution is diluted with ion-exchanged water to prepare a measurement sample. The metal content ratio in the measurement sample is calculated using inductively coupled plasma atomic emission spectroscopy (ICP-AES).

[0074] When multiple active materials are used, the mass ratio is estimated from the content ratio of elements specific to each active material. The mass ratio of the specific elements to the active material is determined from the composition of the constituent elements determined by energy dispersive X-ray spectroscopy.

[0075] Thus, the active material contained in the electrode can be identified.

[0076] <<Cross-Section Observation Using an Electron Microscope>> After the electrode removed from the battery is washed and dried as described above, the electrode is subjected to cross-section milling using, for example, an ion milling device. The resulting cross-section is observed using a scanning electron microscope (SEM-EDX) equipped with an energy dispersive X-ray analyzer. The magnification for SEM observation is 1500x. This observation allows the active material containing a titanium-containing oxide in the active material-containing layer to be identified.

[0077] Among active materials containing titanium-containing oxides, those in the form of primary particles and those in the form of aggregates are distinguished as follows. This also makes it possible to distinguish between secondary particles with internal voids and aggregates. A binarization process is performed on the active material and voids in a cross-sectional SEM image of the electrode. When binarized, a cluster of active material that does not have a "0" inside is considered to be an aggregate. A cluster of active material that has zeros on the periphery is also considered to be an aggregate as long as there are no zeros inside. An example will be explained with reference to the drawings. Figures 3 to 5 show conceptual diagrams illustrating clusters of binarized active material.

[0078] In the example shown in Figure 3, there are zeros inside that are isolated from the surroundings, so they are not considered to be aggregates. Such aggregates may be, for example, aggregates of electrode members that do not form aggregates, or secondary particles with internal voids. In the examples shown in Figures 4 and 5, there are no zeros inside, so they are considered to be aggregates.

[0079] Among active materials containing titanium-containing oxides, secondary particles that do not have aluminum oxide compounds on the surfaces of primary particles inside the secondary particles and aggregates are distinguished as follows. The cross section of the electrode obtained as described above is observed with a transmission electron microscope (TEM-EDX) equipped with an energy dispersive X-ray analyzer. The magnification of the TEM observation is 3,000,000 times. Among the active material aggregates in the cross-sectional TEM image of the electrode that are confirmed to have no "0" inside in the binarized SEM image as described above, those that have Al present inside confirmed by EDX are considered to be aggregates. Aggregates that are confirmed to have no "0" inside but also no Al inside can be determined to be secondary particles without voids, for example, secondary particles formed from primary particles that were not coated with aluminum oxide before being formed into secondary particles.

[0080] Based on the aggregate portion and the other portion in the active material-containing layer as determined in the cross-sectional SEM image of the electrode, the cross-sectional area S of the active material-containing layer was calculated. E (including the cross-sectional area of ​​the aggregate), the total cross-sectional area S of the aggregate G , the least squares circular diameter D of each aggregate g , and the thickness T of the active material-containing layer e Using the results obtained, the ratio S G / S E and D g / T e When active material-containing layers are provided on both the front and back surfaces of the current collector, these ratios are calculated separately for the active material-containing layers on each surface.

[0081] <<Extended X-ray Absorption Fine Structure Measurement and Fourier Transform>> Extended X-ray absorption fine structure measurement and Fourier transform can be performed as follows.

[0082] After removing the electrodes from the battery and drying them in an inert atmosphere, the sample is introduced into the vacuum chamber of the measuring instrument. X-ray absorption fine structure (XAFS) spectra are measured by irradiating the sample with X-rays and measuring the amount of absorption (electron yield method). In the XAFS spectrum, the structure near the absorption edge is called XANES (X-ray Absorption Near Edge Structure), and the extended X-ray absorption fine structure that appears approximately 100 eV higher in energy than the absorption edge is called EXAFS (Extended X-ray Absorption Fine Structure). Information about the valence and structure of the target atom is obtained from XANES. EXAFS analysis provides information about the sample's local structure (atomic species, valence, and distance around the target atom) through Fourier transformation of the actual spectrum (FT-EXAFS; equivalent to the radial distribution function). The obtained spectral data is normalized around the absorption edge to derive the XANES spectrum.

[0083] The EXAFS oscillation (χ(k)) obtained by EXAFS analysis is expressed by the following equation according to the plane wave single scattering theory:

[0084]

[0085] Here, the subscript i is the number of the coordination sphere, S 0 2 is the attenuation factor, N i is the number of atoms in the i-th coordination sphere, F i (k i ) is the backscattering intensity, k i is the wave number, r i is the bond distance, σ i is the Debye-Waller (DW) factor, φi(k i ) is the phase shift.

[0086] Generally, the number of atoms in each coordination sphere (N i ) decreases, the amplitude of the EXAFS vibration (χ(k)) decreases. i The shorter the atomic length, the greater the information reflected in the EXAFS oscillation (χ(k)).

[0087] k for EXAFS oscillation (χ(k)) 3 The EXAFS function (k 3 χ(k)). The EXAFS function (k 3 By comparing the amplitude of χ(k) the number of coordinated atoms of the measured atom can be estimated.

[0088] In this embodiment, the EXAFS function (k 3 The radial distribution function is obtained by Fourier transforming the EXAFS spectrum in the region of χ(k) where 2.5≦k≦7 (corresponding to the EXAFS region). Athena (Non-Patent Document 1) can be used as the analysis software.

[0089] An example of the radial distribution function obtained by FT-EXAFS for such an electrode is shown in the graph of FIG.

[0090] The spectrum obtained for the electrode is shown by the solid line 49, and the spectrum obtained for the aluminum alkoxide additive alone used in preparing the electrode is shown by the dashed line 90. As shown in Figure 6, the shapes of the two spectra are similar. This indicates that the added aluminum alkoxide is present on the active material at the electrode surface while maintaining the Al-O structure or Al-O-C structure, and has not been converted into other components such as alumina.

[0091] Peak A in the range of 1.1 Å to 1.5 Å can be attributed to Al—O bonds. Peak B in the range of 2.8 Å to 3.2 Å can be attributed to Al—O—C bonds. In an electrode in which the Al—O—C bonds of a simple aluminum alkoxide are intact on the active material surface, side reactions on the active material surface are suppressed.

[0092] The electrode according to the first embodiment includes an active material and an aluminum oxide compound in an active material-containing layer. The active material includes a titanium-containing oxide in the form of primary particles and aggregates thereof. The aluminum oxide compound coats the titanium-containing oxide. In the radial distribution function obtained by FT-EXAFS at the Al K absorption edge of the active material-containing layer, peak A appearing in the range of 1.1 Å to 1.5 Å and peak B appearing in the range of 2.8 Å to 3.2 Å each have a peak intensity I A and I B is 3.5≦I A / I B The relationship of the least squares circular diameter D of the aggregate is satisfied. g is the thickness T of the active material-containing layer e The electrode can realize a battery having excellent low-temperature performance with suppressed electrical resistance and resistance increase.

[0093] Second Embodiment According to a second embodiment, a battery is provided. The battery includes a positive electrode, a negative electrode, and an electrolyte. At least one of the positive electrode and the negative electrode includes the electrode according to the first embodiment. In a preferred embodiment of the battery, the negative electrode includes the electrode according to the first embodiment.

[0094] The battery may further include a separator disposed between the positive electrode and the negative electrode. The positive electrode, the negative electrode, and the separator may constitute an electrode assembly. The electrolyte may be held in the electrode assembly.

[0095] Moreover, such a battery may further include an exterior member that houses the electrode group and the electrolyte.

[0096] Furthermore, the battery may further include a positive electrode terminal electrically connected to the positive electrode and a negative electrode terminal electrically connected to the negative electrode, and at least a portion of the positive electrode terminal and at least a portion of the negative electrode terminal may extend outside the exterior member.

[0097] Such a battery may be, for example, a lithium ion secondary battery. The battery also includes, for example, a non-aqueous electrolyte battery that contains a non-aqueous electrolyte as the electrolyte.

[0098] The negative electrode, positive electrode, electrolyte, separator, exterior member, positive electrode terminal, and negative electrode terminal will be described in detail below.

[0099] (1) Negative Electrode The negative electrode includes a negative electrode current collector and a negative electrode active material-containing layer (negative electrode mixture layer) supported on one surface or both surfaces of the negative electrode current collector and containing a negative electrode active material, a conductive agent, and a binder.

[0100] The negative electrode may be the electrode according to the first embodiment. In the negative electrode mode, the negative electrode current collector, negative electrode active material, and negative electrode active material-containing layer of the negative electrode correspond to the current collector, active material, and active material-containing layer of the electrode according to the first embodiment, respectively. The electrode according to the first embodiment has been described in detail above, so a description of the negative electrode here will be omitted.

[0101] (2) Positive Electrode The positive electrode includes a positive electrode current collector and a positive electrode active material-containing layer (positive electrode mixture layer) supported on one surface or both surfaces of the positive electrode current collector and containing a positive electrode active material, a conductive agent, and a binder.

[0102] The battery according to the second embodiment may include the electrode according to the first embodiment as a positive electrode. Alternatively, the battery may include a positive electrode having a different configuration from the electrode according to the first embodiment. Hereinafter, a positive electrode having a different configuration from the electrode according to the first embodiment will be described.

[0103] The positive electrode active material is a lithium-containing nickel cobalt manganese oxide (e.g., Li w Ni x Co y Mn z O 2 wherein 0<w≦1 and x+y+z=1; or Li 1-w Ni 1-x-y-z Co x Mn y M1 z O 2 In the formula, M1 is at least one selected from the group consisting of Mg, Al, Si, Ti, Zn, Zr, Ca, and Sn, and -0.2<w<0.5, 0<x<0.5, 0<y<0.5, 0≦z<0.1, x+y+z<1). In addition, various oxides, for example, lithium-containing cobalt oxides (e.g., LiCoO 2), manganese dioxide, lithium manganese composite oxide (e.g., LiMn 2 O 4 , LiMnO 2 ), lithium-containing nickel oxide (e.g., LiNiO 2 ), lithium-containing nickel cobalt oxide (e.g., LiNi 0.8 Co 0.2 O 2 The positive electrode active material may contain one or more types of materials, such as lithium-containing iron oxide, lithium-containing vanadium oxide, or chalcogen compounds such as titanium disulfide and molybdenum disulfide.

[0104] Examples of the binder include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine-based rubber, styrene-butadiene rubber (SBR), carboxymethyl cellulose (CMC), polyimide, polyamide, etc. One or more types of binder may be used.

[0105] Examples of the conductive agent include carbon black such as acetylene black and ketjen black, graphite, carbon fiber, carbon nanotube, fullerene, etc. The type of conductive agent may be one or more types.

[0106] The blending ratios of the positive electrode active material, conductive agent, and binder in the positive electrode active material-containing layer are preferably 80% by mass or more and 95% by mass or less of the positive electrode active material, 3% by mass or more and 18% by mass or less of the conductive agent, and 2% by mass or more and 17% by mass or less of the binder.

[0107] The current collector is preferably an aluminum foil or an aluminum alloy foil, and its average crystal grain size is preferably 50 μm or less, more preferably 30 μm or less, and even more preferably 5 μm or less. A current collector made of an aluminum foil or an aluminum alloy foil having such an average crystal grain size can dramatically increase the strength, making it possible to densify the positive electrode with a high pressing pressure, and thereby increasing the battery capacity.

[0108] Aluminum foil or aluminum alloy foil having an average crystal grain size of 50 μm or less is affected in a complex manner by many factors such as material composition, impurities, processing conditions, heat treatment history, and annealing heating conditions, and the above (diameter) is adjusted by combining the above factors during the manufacturing process.

[0109] The thickness of the current collector is preferably 20 μm or less, more preferably 15 μm or less. The purity of the aluminum foil is preferably 99% or more. The aluminum alloy is preferably an alloy containing elements such as magnesium, zinc, and silicon. On the other hand, the content of transition metals such as iron, copper, nickel, and chromium is preferably 1% or less.

[0110] The positive electrode is produced, for example, by suspending a positive electrode active material, a conductive agent, and a binder in an appropriate solvent, applying the resulting slurry to a current collector, drying the slurry, and then pressing the resulting slurry. Alternatively, the positive electrode active material, the conductive agent, and the binder may be formed into pellets and used as the positive electrode active material-containing layer.

[0111] The positive electrode active material-containing layer preferably has a porosity of 20% or more and 50% or less. A positive electrode having a positive electrode active material-containing layer with such a porosity has high density and excellent affinity with the electrolyte. A more preferred porosity is 25% or more and 40% or less.

[0112] The density of the positive electrode active material-containing layer is 2.5 g / cm 3 It is preferable to set it to more than this.

[0113] (3) Electrolyte Examples of the electrolyte include a liquid non-aqueous electrolyte prepared by dissolving an electrolyte salt (solute) in a non-aqueous solvent, and a gel non-aqueous electrolyte obtained by combining a liquid non-aqueous electrolyte with a polymer material.

[0114] The electrolyte salt is, for example, lithium perchlorate (LiClO 4 ), lithium hexafluorophosphate (LiPF 6 ), lithium tetrafluoroborate (LiBF 4 ), lithium arsenic hexafluoride (LiAsF 6 ), lithium difluorophosphate (LiPO 2 F 2 ), lithium trifluoromethanesulfonate (LiCF 3 SO 3 ), lithium bistrifluoromethylsulfonylimide [LiN(CF 3 SO 2 ) 2 These electrolyte salts may be used alone or in combination of two or more.

[0115] The electrolyte salt is preferably dissolved in the non-aqueous solvent in a range of 0.5 mol / L to 2.5 mol / L.

[0116] Examples of non-aqueous solvents include organic solvents such as cyclic carbonates such as ethylene carbonate (EC), propylene carbonate (PC), and vinylene carbonate (VC); chain carbonates such as dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC); cyclic ethers such as tetrahydrofuran (THF) and 2-methyl tetrahydrofuran (2MeTHF); chain ethers such as dimethoxyethane (DME); cyclic esters such as γ-butyrolactone (BL); chain esters such as methyl acetate, ethyl acetate, methyl propionate, and ethyl propionate; acetonitrile (AN); and sulfolane (SL). These organic solvents can be used alone or in the form of a mixture of two or more kinds.

[0117] Examples of polymer materials used for the gel-like non-aqueous electrolyte include polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), and polyethylene oxide (PEO).

[0118] (4) Separator The separator is not particularly limited as long as it has insulating properties, but porous films or nonwoven fabrics made of polymers such as polyolefin, cellulose, polyethylene terephthalate, polyimide, polyamideimide, polyvinylidene fluoride, and vinylon can be used. Inorganic oxides such as alumina, titania, and zirconia can also be used. The separator may be made of one material or a combination of two or more materials. The separator may also be integrated with the electrodes.

[0119] (5) Exterior Component The exterior component may be formed from a laminate film or may be a metal container. When a metal container is used, the lid may be integral with the container or may be a separate component. The thickness of the metal container is preferably 0.5 mm or less, more preferably 0.2 mm or less. Examples of the shape of the exterior component include flat, rectangular, cylindrical, coin, button, sheet, and laminated types. The exterior component may be for small batteries mounted in portable electronic devices, etc., as well as for large batteries mounted in two- or four-wheeled automobiles.

[0120] The thickness of the laminate film exterior component is preferably 0.2 mm or less. Examples of laminate films include multilayer films containing a resin film and a metal layer disposed between the resin films. The metal layer is preferably aluminum foil or aluminum alloy foil for weight reduction. Polymer materials such as polypropylene (PP), polyethylene (PE), nylon, and polyethylene terephthalate (PET) can be used for the resin film. The laminate film can be sealed by heat fusion to form it into the shape of the exterior component.

[0121] The metal container is made of aluminum or an aluminum alloy. The aluminum alloy is preferably an alloy containing elements such as magnesium, zinc, and silicon. In aluminum or an aluminum alloy, the content of transition metals such as iron, copper, nickel, and chromium is preferably 100 ppm or less, in order to significantly improve long-term reliability and heat dissipation in a high-temperature environment.

[0122] The metal container made of aluminum or an aluminum alloy desirably has an average crystal grain size of 50 μm or less, more preferably 30 μm or less, and even more preferably 5 μm or less. By setting the average crystal grain size to 50 μm or less, the strength of the metal container made of aluminum or an aluminum alloy can be dramatically increased, allowing the container to be made even thinner. As a result, a lightweight, high-power, and highly reliable battery suitable for use in vehicles can be realized.

[0123] An example of such a battery will be described with reference to Figures 7 and 8. The flat-type battery shown in Figure 7 includes a flat wound electrode group 1, a packaging member 2, a positive electrode terminal 7, a negative electrode terminal 6, and an electrolyte (not shown). The packaging member 2 is a bag-shaped packaging member made of a laminate film. The wound electrode group 1 is housed in the packaging member 2. As shown in Figure 8, the wound electrode group 1 includes a positive electrode 3, a negative electrode 4, and a separator 5, and is formed by spirally winding a laminate obtained by stacking the negative electrode 4, separator 5, positive electrode 3, and separator 5 in this order from the outside in, and then press-molding the laminate.

[0124] The positive electrode 3 includes a positive electrode current collector 3a and a positive electrode active material-containing layer 3b. The positive electrode active material-containing layer 3b contains a positive electrode active material. The positive electrode active material-containing layer 3b is formed on both sides of the positive electrode current collector 3a. The negative electrode 4 includes a negative electrode current collector 4a and a negative electrode active material-containing layer 4b. The negative electrode active material-containing layer 4b contains a negative electrode active material. The negative electrode active material-containing layer 4b is formed on both sides of the negative electrode current collector 4a.

[0125] 7 , a positive electrode terminal 7 is connected to the positive electrode 3 near the outer peripheral end of the wound electrode pack 1. A negative electrode terminal 6 is connected to the negative electrode 4 in the outermost layer portion. The positive electrode terminal 7 and the negative electrode terminal 6 extend to the outside through openings in the exterior member 2.

[0126] Such a battery is not limited to the configuration shown in FIGS. 7 and 8, but may have a configuration shown in FIG. 9, for example.

[0127] In the prismatic battery shown in Fig. 9, a wound electrode group 11 is housed in a metal rectangular cylindrical container 12 with a bottom, which serves as an exterior member. A rectangular lid 13 is welded to the opening of the container 12. The flat wound electrode group 11 may have a configuration similar to that of the wound electrode group 1 described with reference to Figs. 7 and 8, for example.

[0128] One end of the negative electrode tab 14 is electrically connected to the negative electrode current collector, and the other end is electrically connected to a negative electrode terminal 15. The negative electrode terminal 15 is fixed to the rectangular lid 13 by a hermetic seal with a glass material 16 interposed therebetween. One end of the positive electrode tab 17 is electrically connected to the positive electrode current collector, and the other end is electrically connected to a positive electrode terminal 18 fixed to the rectangular lid 13.

[0129] The negative electrode tab 14 is made of a material such as aluminum or an aluminum alloy containing elements such as Mg, Ti, Zn, Mn, Fe, Cu, Si, etc. The negative electrode tab 14 is preferably made of the same material as the negative electrode current collector in order to reduce contact resistance with the negative electrode current collector.

[0130] The positive electrode tab 17 is made of a material such as aluminum or an aluminum alloy containing elements such as Mg, Ti, Zn, Mn, Fe, Cu, Si, etc. The positive electrode tab 17 is preferably made of the same material as the positive electrode current collector in order to reduce contact resistance with the positive electrode current collector.

[0131] The battery shown in the figure uses a wound electrode group in which the separator is wound together with the positive and negative electrodes, but a stacked electrode group in which the separator is folded zigzag and the positive and negative electrodes are alternately arranged at the folded points may also be used.

[0132] The battery according to the second embodiment includes the electrode according to the first embodiment, and therefore the battery has reduced electrical resistance and resistance increase, and is excellent in low-temperature performance.

[0133] Third Embodiment According to a third embodiment, a battery pack is provided, which includes the battery according to the second embodiment.

[0134] The battery pack according to the third embodiment may include one or more batteries (single cells) according to the second embodiment described above. The batteries included in the battery pack may be electrically connected in series or parallel to each other to form a battery assembly. The battery pack may include a plurality of battery assemblies.

[0135] Next, an example of a battery pack according to a third embodiment will be described with reference to the drawings.

[0136] Fig. 10 is an exploded perspective view of an example battery pack according to the second embodiment, and Fig. 11 is a block diagram showing an electrical circuit of the battery pack of Fig. 10.

[0137] 10 and 11 includes a plurality of unit cells 21. The unit cells 21 may be the flat battery of the example according to the second embodiment described with reference to FIG.

[0138] The plurality of cells 21 are stacked so that the negative electrode terminals 51 and positive electrode terminals 61 extending outward are aligned in the same direction, and are fastened together with adhesive tape 22 to form a battery pack 23. These cells 21 are electrically connected in series with each other as shown in FIG.

[0139] The printed wiring board 24 is disposed opposite the side surface from which the negative electrode terminal 51 and the positive electrode terminal 61 of the cell 21 extend. As shown in Fig. 11 , the printed wiring board 24 is mounted with a thermistor 25, a protection circuit 26, and a terminal 27 for supplying current to an external device. An insulating plate (not shown) is attached to the surface of the printed wiring board 24 facing the assembled battery 23 to prevent unnecessary connection with the wiring of the assembled battery 23.

[0140] The positive electrode lead 28 is connected to a positive electrode terminal 61 located on the bottom layer of the battery pack 23, and its tip is inserted into and electrically connected to a positive electrode connector 29 on the printed wiring board 24. The negative electrode lead 30 is connected to a negative electrode terminal 51 located on the top layer of the battery pack 23, and its tip is inserted into and electrically connected to a negative electrode connector 31 on the printed wiring board 24. These connectors 29 and 31 are connected to the protection circuit 26 via wires 32 and 33 formed on the printed wiring board 24.

[0141] The thermistor 25 detects the temperature of the cell 21 and transmits the detection signal to the protection circuit 26. The protection circuit 26 can interrupt the positive wiring 34a and the negative wiring 34b between the protection circuit 26 and the power terminal 27 for connecting to the external device under predetermined conditions. An example of the predetermined condition is when the temperature detected by the thermistor 25 exceeds a predetermined temperature. Another example of the predetermined condition is when overcharge, overdischarge, overcurrent, or the like of a cell 21 is detected. This overcharge detection is performed for each cell 21 or the entire battery pack 23. When detecting an individual cell 21, the battery voltage may be detected, or the positive electrode potential or negative electrode potential may be detected. In the latter case, a lithium electrode used as a reference electrode is inserted into each cell 21. In the battery pack 20 shown in FIGS. 10 and 11 , wiring 35 for voltage detection is connected to each cell 21. A detection signal is transmitted to the protection circuit 26 via these wiring 35.

[0142] Protective sheets 36 made of rubber or resin are disposed on the three sides of the battery pack 23 excluding the sides from which the positive electrode terminal 61 and the negative electrode terminal 51 protrude.

[0143] The battery pack 23 is housed in a storage container 37 together with the protective sheets 36 and the printed wiring board 24. That is, the protective sheets 36 are disposed on both inner surfaces along the long sides and the inner surface along the short sides of the storage container 37, and the printed wiring board 24 is disposed on the inner surface on the opposite side along the short sides. The battery pack 23 is located in a space surrounded by the protective sheets 36 and the printed wiring board 24. A lid 38 is attached to the top surface of the storage container 37.

[0144] Heat-shrinkable tape may be used to secure the battery pack 23 instead of the adhesive tape 22. In this case, protective sheets are placed on both sides of the battery pack, and the heat-shrinkable tape is wrapped around the battery pack, and then the heat-shrinkable tape is thermally shrunk to bind the battery pack.

[0145] 10 and 11 show the cells 21 connected in series, they may be connected in parallel to increase the battery capacity. Furthermore, assembled battery packs may be connected in series and / or in parallel.

[0146] The configuration of the battery pack may be changed as appropriate depending on the application. The battery pack is preferably used in applications where good cycle performance is desired when a large current is drawn. Specific applications include power sources for digital cameras and in-vehicle applications such as two- to four-wheel hybrid electric vehicles, two- to four-wheel electric vehicles, and power-assisted bicycles. The battery pack is particularly suitable for in-vehicle applications.

[0147] The battery pack according to the third embodiment includes the battery according to the second embodiment, and therefore the battery pack has reduced electrical resistance and resistance increase, and is excellent in low-temperature performance.

[0148] Examples will be described below, but the present invention is not limited to the examples listed below as long as they do not depart from the gist of the present invention.

[0149] Example 1 In Example 1, a nonaqueous electrolyte battery of Example 1 was fabricated by the following procedure.

[0150] <<Preparation of negative electrode>> Li 4 Ti 5 O 12 A powder of lithium titanium composite oxide having the above composition and a spinel structure was prepared.

[0151] First, anatase-type titanium oxide was added to a solution of lithium hydroxide dissolved in pure water, and the mixture was stirred and dried. These raw materials were mixed so that the molar ratio of Li:Ti in the mixture was 4:5.

[0152] The mixed raw materials were fired in an air atmosphere at 900°C for 3 hours. The fired product was then pulverized in a ball mill using zirconia balls as media and washed with water. The product was then subjected to heat treatment in an air atmosphere at 600°C for 30 minutes and then classified. Thus, the product powder was obtained.

[0153] The average primary particle size of the obtained product powder was analyzed by SEM. As a result, it was found that the obtained product powder was a primary particle-like particle with an average primary particle size of 700 nm. In addition, the composition and crystalline structure of the obtained product were analyzed using ICP and X-ray diffraction measurements. As a result, it was found that the obtained product had a spinel-type crystalline structure and contained Li. 4 Ti 5 O 12 The powder of this product was used as the negative electrode active material.

[0154] Next, carbon was added as a conductive agent to a powder of spinel-type lithium-titanium composite oxide as the negative electrode active material, and the mixture was mixed in a Henschel mixer to obtain a mixture. To this mixture, polyvinylidene fluoride (PVdF) as a binder, aluminum alkoxide, and N-methylpyrrolidone (NMP) as a dispersion medium were added, and the mixture was kneaded in a planetary mixer. Di-2-butoxyaluminum ethyl acetoacetate was added as the aluminum alkoxide. The mixture was kneaded at a relatively high solids content (thick kneading), applying a relatively strong dispersing force. Next, NMP was further added to adjust the final solids content. Thus, a slurry (slurry for producing a negative electrode) was obtained.

[0155] In the above mixing, the amounts of carbon, PVdF, and aluminum alkoxide compound added were adjusted so that the ratio of negative electrode active material:carbon:PVdF:aluminum alkoxide compound in the resulting slurry was 90 parts by mass:5 parts by mass:4 parts by mass:1 part by mass.

[0156] After mixing with the planetary mixer, the mixture was dispersed with a bead mill.

[0157] This slurry was applied to both sides of a current collector made of aluminum foil with a thickness of 15 μm, and the coating film was dried at 125°C. Next, the dried coating film was subjected to a roll press treatment. Further, it was vacuum dried in an environment of 90°C for 12 hours. Thus, the current collector and the electrode formed on both sides of this current collector and having an electrode density (excluding the current collector) of 2.0 g / cm were obtained. 3 The thickness of the negative electrode active material-containing layer formed on each surface of the current collector was 40 μm.

[0158] <<Preparation of Positive Electrode>> First, a lithium nickel cobalt manganese composite oxide (LiNi) was used as a positive electrode active material. 0.5 Co 0.3 Mn 0.2 O 2 ) powder was prepared. 5 parts by mass of acetylene black as a conductive agent was added to 90 parts by mass of the positive electrode active material, and the mixture was mixed in a Henschel mixer to obtain a mixture. Next, 5 parts by mass of PVdF and N-methylpyrrolidone (NMP) were added to this mixture in a certain ratio, and the mixture was kneaded in a planetary mixer to obtain a slurry. This slurry was applied to both sides of a current collector made of aluminum foil with a thickness of 15 μm, and the coating film was dried. Furthermore, the dried coating film was subjected to a roll press treatment. Thus, a current collector and an electrode formed on both sides of this current collector and having an electrode density (excluding the current collector) of 3.0 g / cm were obtained. 3 A positive electrode having a positive electrode active material-containing layer was fabricated.

[0159] <<Preparation of Electrode Group>> Two separators each made of a 20 μm thick porous polyethylene film were prepared.

[0160] Next, the previously prepared positive electrode, one separator, the previously prepared negative electrode, and another separator were stacked in this order to obtain a laminate. This laminate was then spirally wound and hot-pressed at 90°C to produce a flat electrode group.

[0161] The obtained electrode group was housed in a pack made of a laminate film and vacuum dried for 12 hours at 95° C. The laminate film used was made by forming polypropylene layers on both sides of an aluminum foil.

[0162] <Preparation of Liquid Non-Aqueous Electrolyte> Propylene carbonate (PC) and methyl ethyl carbonate (MEC) were mixed in a volume ratio of 1:1 to prepare a mixed solvent. The electrolyte, LiPF 6, was added to this mixed solvent. 6 A liquid non-aqueous electrolyte was prepared by dissolving 1M of the above in water.

[0163] <<Manufacture of Non-Aqueous Electrolyte Secondary Battery>> A liquid non-aqueous electrolyte was poured into the laminate film pack containing the electrode group as described above. The pack was then completely sealed by heat sealing. In this way, a non-aqueous electrolyte secondary battery having the structure shown in FIGS. 7 and 8 was manufactured.

[0164] Next, the fabricated nonaqueous electrolyte secondary battery was charged at a charge rate of 1 A (1 C) in an environment of 25° C. to adjust the SOC (state of charge) to 40%, and subjected to heat treatment for 24 hours at 70° C. Next, the battery was allowed to cool to room temperature, discharged to 1.5 V at 1 A in an environment of 25° C., and then charged at 1 A to adjust the SOC to 50%.

[0165] (Example 2) In Example 2, D G / T e In order to control the above, a nonaqueous electrolyte battery was produced in the same manner as in Example 1, except that, in preparing the negative electrode slurry, aluminum alkoxide was not added during kneading with a planetary mixer, but was added after dispersion with a bead mill.

[0166] (Example 3) In Example 3, the amount of aluminum alkoxide added to the slurry for preparing the negative electrode was reduced to reduce the S G / S e A nonaqueous electrolyte battery was manufactured in the same manner as in Example 1, except that the value of was controlled to be small.

[0167] (Example 4) In Example 4, D G / T e and S G / S e A nonaqueous electrolyte battery was manufactured in the same manner as in Example 1, except that D G / T e The same means as in Example 2 was applied to control S. G / Se was controlled to be small by the same means as in Example 3.

[0168] Example 5 In Example 5, the amount of aluminum alkoxide added to the negative electrode slurry was increased to improve the S G / S e A nonaqueous electrolyte battery was manufactured in the same manner as in Example 1, except that the value of was controlled to be large.

[0169] (Example 6) In Example 6, D G / T e and S G / S e A nonaqueous electrolyte battery was manufactured in the same manner as in Example 1, except that D G / T e The same means as in Example 2 was applied to control S. G / S e was largely controlled by the same means as in Example 5.

[0170] Example 7 In Example 7, a nonaqueous electrolyte battery was produced in the same manner as in Example 1, except that the aluminum alkoxide added to the negative electrode slurry was changed from di-2-butoxyaluminum ethyl acetoacetate to aluminum trisec-butoxide.

[0171] Example 8 In Example 8, a nonaqueous electrolyte battery was produced in the same manner as in Example 1, except that the aluminum alkoxide added to the negative electrode-forming slurry was changed from di-2-butoxyaluminum ethyl acetoacetate to aluminum trisec-butoxide, and that the aluminum alkoxide was not added during kneading with a planetary mixer but was added after dispersion with a bead mill.

[0172] In Example 9, a nonaqueous electrolyte battery was produced in the same manner as in Example 1, except that the amount of residual moisture was adjusted by changing the heat treatment conditions after washing with water when preparing the negative electrode active material. Specifically, the heat treatment conditions were changed to lower the heat treatment temperature and shorten the heat treatment time.

[0173] Example 10 In Example 10, the amount of residual water in the negative electrode active material was adjusted as follows. G / Te A nonaqueous electrolyte battery was manufactured in the same manner as in Example 1, except that the amount of water remaining in the negative electrode active material was controlled in the same manner as in Example 9. G / T e The same means as in Example 2 was applied to the control.

[0174] Comparative Example 1 In Comparative Example 1, aluminum alkoxide was not added during kneading with a planetary mixer when preparing the negative electrode slurry, but aluminum alkoxide was added after kneading to dilute the slurry with a low solid content by further adding a dispersion medium. G / T e A nonaqueous electrolyte battery was manufactured in the same manner as in Example 1, except that the temperature was controlled.

[0175] (Comparative Examples 2 to 4) In Comparative Examples 2 to 4, nonaqueous electrolyte batteries were produced using the same procedure as in Example 1, except that the conditions for kneading in a planetary mixer during preparation of the negative electrode slurry were changed as follows. In all of Comparative Examples 2 to 4, the solid content during kneading was set relatively low so as to weaken the dispersing force during kneading in the planetary mixer. In Comparative Example 2, aluminum alkoxide was not added during kneading in the planetary mixer, and aluminum alkoxide was added in a low solid content state by further adding a dispersion medium after kneading to dilute the mixture. In Comparative Example 4, aluminum alkoxide was not added during kneading in the planetary mixer, and aluminum alkoxide was added after dispersion using a bead mill.

[0176] (Comparative Examples 5 to 7) In Comparative Examples 5 to 7, nonaqueous electrolyte batteries were produced using the same procedure as in Example 1, except that the conditions for kneading in a planetary mixer during preparation of the negative electrode slurry were changed as follows. In all of Comparative Examples 5 to 7, the solid content during kneading was increased to strengthen the dispersing force during kneading in the planetary mixer. In Comparative Example 5, aluminum alkoxide was not added during kneading in the planetary mixer, and aluminum alkoxide was added in a low solid content state by further diluting it with a dispersion medium after kneading. In Comparative Example 7, aluminum alkoxide was not added during kneading in the planetary mixer, and aluminum alkoxide was added after dispersion using a bead mill.

[0177] Comparative Example 8 In Comparative Example 8, the aluminum alkoxide added to the negative electrode slurry was converted from di-2-butoxyaluminum ethyl acetoacetate to methylaluminoxane (MAO) ((Al(CH3)O) n A nonaqueous electrolyte battery was manufactured in the same manner as in Example 1, except that the temperature was changed to 100°C.

[0178] In Comparative Examples 9 and 10, nonaqueous electrolyte batteries were manufactured in the same manner as in Example 1, except that the aluminum alkoxide added to the negative electrode slurry and the timing of its addition were changed as follows. In both Comparative Examples 9 and 10, methylaluminoxane (MAO) ((Al(CH3)O)) was used instead of di-2-butoxyaluminum ethylacetoacetate. n In Comparative Example 9, aluminum alkoxide was not added during kneading with the planetary mixer, but was added after kneading in a state of dilution with a low solid content by further adding a dispersion medium. In Comparative Example 10, aluminum alkoxide was not added during kneading with the planetary mixer, but was added after dispersion with a bead mill.

[0179] In Comparative Example 11, a nonaqueous electrolyte battery was produced in the same manner as in Example 1, except that the heat treatment conditions after washing with water in preparing the negative electrode active material were changed to adjust the amount of residual moisture. Specifically, the heat treatment conditions were changed to a lower temperature and a shorter time than in Example 9.

[0180] (Comparative Examples 12 and 13) In Comparative Examples 12 and 13, nonaqueous electrolyte batteries were produced using the same procedure as in Example 1, except that the residual moisture content of the negative electrode active material was adjusted as follows and the timing of adding aluminum alkoxide to the negative electrode preparation slurry was changed as follows. The residual moisture content of the negative electrode active material was controlled by the same means as in Comparative Example 11. In Comparative Example 12, aluminum alkoxide was not added during kneading with the planetary mixer, but was added after kneading in a state of low solids content by further diluting with a dispersion medium. In Comparative Example 13, aluminum alkoxide was not added during kneading with the planetary mixer, but was added after dispersion with a bead mill.

[0181] Comparative Example 14 In Comparative Example 14, the amount of aluminum alkoxide added to the negative electrode slurry was significantly reduced, resulting in a low S G / S e A nonaqueous electrolyte battery was manufactured in the same manner as in Example 1, except that the value of was controlled to be significantly small.

[0182] (Comparative Examples 15 and 16) In Comparative Examples 15 and 16, the amount of aluminum alkoxide added to the negative electrode slurry was significantly reduced, thereby reducing the S G / S e A nonaqueous electrolyte battery was manufactured in the same manner as in Example 1, except that the value of was controlled to be significantly small and the timing of adding the alkoxide was changed as follows: In Comparative Example 15, the aluminum alkoxide was not added during kneading with the planetary mixer, but was added after kneading in a state of dilution with a low solids content by further adding a dispersion medium; in Comparative Example 16, the aluminum alkoxide was not added during kneading with the planetary mixer, but was added after dispersion with a bead mill.

[0183] Comparative Example 17 In Comparative Example 17, the amount of aluminum alkoxide added to the negative electrode slurry was significantly increased, resulting in a high S G / S e A nonaqueous electrolyte battery was manufactured in the same manner as in Example 1, except that the value of was controlled to be significantly larger.

[0184] (Comparative Examples 18 and 19) In Comparative Examples 18 and 19, the amount of aluminum alkoxide added to the negative electrode slurry was significantly increased, resulting in a high S G / S e A nonaqueous electrolyte battery was manufactured in the same manner as in Example 1, except that the value of was controlled to be significantly larger and the timing of addition was changed as follows: In Comparative Example 18, aluminum alkoxide was not added during kneading with the planetary mixer, but was added after kneading in a state of dilution with a low solid content by further adding a dispersion medium; in Comparative Example 19, aluminum alkoxide was not added during kneading with the planetary mixer, but was added after dispersion with a bead mill.

[0185] Comparative Example 20 In Comparative Example 20, a nonaqueous electrolyte battery was produced in the same manner as in Example 1, except that the addition of aluminum alkoxide to the negative electrode-forming slurry was omitted and the solid content during kneading was relatively low so as to weaken the dispersing force during kneading with a planetary mixer.

[0186] Comparative Example 21 In Comparative Example 21, a nonaqueous electrolyte battery was produced in the same manner as in Example 1, except that the addition of aluminum alkoxide to the negative electrode-forming slurry was omitted.

[0187] Comparative Example 22 In Comparative Example 22, a nonaqueous electrolyte battery was produced in the same manner as in Example 1, except that the addition of aluminum alkoxide to the negative electrode-forming slurry was omitted and the solid content during kneading was increased so as to strengthen the dispersing force during kneading with a planetary mixer.

[0188] In Comparative Example 23, a nonaqueous electrolyte battery was produced in the same manner as in Example 1, except that the negative electrode active material was converted into secondary particles as follows before being used in a slurry for producing a negative electrode. Primary particle-like lithium-titanium composite oxide powder as the negative electrode active material was granulated using a spray dryer to form secondary particles.

[0189] In Comparative Examples 24 and 25, nonaqueous electrolyte batteries were produced in the same manner as in Example 1, except that the negative electrode active material was converted into secondary particles and then used in a slurry for producing a negative electrode, as in Comparative Example 23, and the timing of adding the aluminum alkoxide was changed as follows: In Comparative Example 24, the aluminum alkoxide was not added during kneading with the planetary mixer, but was added after kneading in a state of a low solids content by further adding a dispersion medium to dilute the mixture; in Comparative Example 25, the aluminum alkoxide was not added during kneading with the planetary mixer, but was added after dispersion with a bead mill.

[0190] The conditions for producing the negative electrode in the nonaqueous electrolyte battery production in Examples 1 to 10 and Comparative Examples 1 to 25 are summarized in Tables 1 and 2 below. Specifically, Table 1 shows the conditions for the heat treatment performed after water washing following ball mill pulverization when the titanium-containing oxide used as the negative electrode active material was synthesized, as well as the morphology (primary particles or secondary particles) of the titanium-containing oxide powder when mixed into the negative electrode production slurry. Table 2 shows the aluminum alkoxide added to the negative electrode production slurry, the amount of Al (in mg) relative to the amount of Ti (in mg) in the slurry depending on the amount of aluminum alkoxide added, the timing at which the aluminum alkoxide was added to the negative electrode production slurry, and the dispersion strength during kneading (kneading) using a planetary mixer.

[0191]

[0192]

[0193] <Measurement> For each of the nonaqueous electrolyte batteries manufactured as described above, the negative electrode components were analyzed by the FT-EXAFS described above. In the radial distribution function obtained, a peak A in the range of 1.1 Å to 1.5 Å and a peak B in the range of 2.8 Å to 3.2 Å were confirmed, and the intensity ratio I between these peaks was calculated. A / I B The results are shown in Table 3 below.

[0194] In addition, the cross section of the negative electrode was observed with an SEM by the method described above. In the obtained cross-sectional SEM image, the cross-sectional area S E , the total cross-sectional area of ​​the aggregate S G , the average least squares circular diameter D of each aggregate g , and the thickness T of the active material-containing layer e are measured, and the ratio S G / S E and D g / T e The calculated ratios are shown in Table 3 below.

[0195] <Evaluation> The performance of each of the nonaqueous electrolyte batteries produced in Examples 1 to 10 and Comparative Examples 1 to 25 was evaluated as follows. Specifically, the large current performance and life performance of each battery were evaluated.

[0196] (Large Current Performance) In order to confirm the initial resistance of the battery, the large current performance under low temperature conditions was evaluated by measuring the low temperature output resistance as described below.

[0197] First, the battery was charged at a constant current of 600 mA (1 C) in a thermostatic chamber at 25°C until the battery voltage reached 2.7 V. Subsequently, the battery was charged at a constant voltage of 30 mA, followed by a 10-minute rest period. Next, the battery was discharged at a constant current of 120 mA to 1.5 V. The discharge capacity obtained at this time was measured.

[0198] Next, the battery was charged at a constant current of 600 mA (1 C) until the battery voltage reached 2.7 V, and then charged at a constant voltage until the current value reached 30 mA, after which 50% of the discharge capacity was discharged.

[0199] The temperature of the thermostatic bath was then set to -20°C, and the battery was left to stand in the thermostatic bath for 3 hours. The battery was discharged for 10 seconds at a constant current of 6 A in the thermostatic bath at low temperature (-20°C), and the voltage change was measured. The value calculated by dividing the voltage change during 10 seconds of discharge under low temperature conditions by the current value was used as the low-temperature output resistance.

[0200] (Life Performance) The life performance of the battery was evaluated by measuring the increase in resistance in a calendar test under low temperature conditions as follows.

[0201] The battery was charged to a state of charge (SOC) of 50%, and then stored for 3 weeks in a thermostatic chamber set at 85° C. Thereafter, the resistance increase rate was measured by the following method.

[0202] The battery was removed from the 85°C thermostatic chamber and allowed to stand at room temperature until the battery temperature reached room temperature. The battery was then placed in a 25°C thermostatic chamber and discharged at 600 mA to 1.5 V, followed by a 10-minute rest period. The battery was then charged at 1 A to 2.7 V, and then subjected to constant voltage charging until the current reached 30 mA at 2.7 V. A 10-minute rest period was then allowed. The battery was then discharged at a constant current of 120 mA to 1.5 V. The resulting discharge capacity was measured and used as the recovery capacity. The battery was then charged at 600 mA to a capacity equivalent to 50% of the recovery capacity. The temperature of the thermostatic chamber was set to -20°C, and the battery was left in the thermostatic chamber for 3 hours, after which it was discharged at 6 A for 10 seconds. The discharge resistance of the 10-second 10C discharge was measured.

[0203] The ratio of the discharge resistance measured after storage to the discharge resistance measured before storage was calculated and used as the resistance increase rate.

[0204] (Volumetric Energy Density) The energy density per volume of the battery was evaluated as follows.

[0205] To confirm the volumetric energy density of the battery, the discharge capacity of the cell was measured.

[0206] First, the battery was charged at a constant current of 600 mA (1 C) in a thermostatic chamber at 25°C until the battery voltage reached 2.7 V. Subsequently, the battery was charged at a constant voltage of 30 mA, followed by a 10-minute rest period. Next, the battery was discharged at a constant current of 120 mA to 1.5 V. The discharge capacity obtained at this time was measured.

[0207] The volumetric energy density was calculated by multiplying the discharge capacity by the average operating voltage and dividing the result by the cell volume.

[0208] Table 3 below summarizes the results of performance evaluation for each of the nonaqueous electrolyte batteries manufactured in Examples 1 to 10 and Comparative Examples 1 to 25. As the results of performance evaluation, the evaluation results of the above-mentioned low-temperature output resistance (large current performance), the rate of increase in resistance during high-temperature storage (lifetime performance), and the energy density per volume are shown as relative values ​​to the reference value of 100% which is the measured value for Comparative Example 21. Note that Table 3 also shows the ratio I obtained by the above measurements. A / I B , SG / S E , and D g / T e Also shown.

[0209]

[0210] In Examples 1 to 10, D is in the range of 1 / 20 or more and less than 1 / 2. g / T e It is presumed that in Examples 1 to 10, the agglomerations were not large and had an appropriate size, which is why good properties were obtained. Note that, for example, as in the difference in the manufacturing conditions between Example 1 and Example 2, the D g / T e However, as shown in the results in Table 3, no effect was observed when changing the timing of adding aluminum alkoxide between when the mixture was kneaded with a planetary mixer and when the mixture was dispersed in a bead mill.

[0211] In contrast, in Comparative Example 1, the aluminum alkoxide was added at a low solids content, diluted by further adding a dispersion medium after kneading, and the frequency of reaction between the aluminum alkoxide and the negative electrode active material decreased. The part of the aluminum alkoxide that did not react with the negative electrode active material reacted only with the binder contained in the negative electrode mixture. It is presumed that the reaction product with the binder became a resistor, resulting in poorer high-current performance than in Example 1.

[0212] In Comparative Examples 2, 3, and 4, the dispersion was weaker than in Example 1. Since the dispersion was insufficient, g / T e As shown by the fact that the amount of aluminum alkoxide was reduced to 1 / 2 or more, the aggregation became large. Because the dispersion was insufficient, the aluminum alkoxide was not uniformly dispersed on the surface of the negative electrode active material, resulting in uneven coating of the aluminum alkoxide. The aggregated negative electrode active material was coated, but the negative electrode active material remaining as primary particles was not coated. It is presumed that the presence of uncoated negative electrode active material was the reason why the resistance increase rate was inferior to that of Example 1.

[0213] In Comparative Examples 5, 6, and 7, the dispersion was stronger than in Example 1. It is presumed that the dispersion was too strong, resulting in smaller aggregates and making the large current performance inferior to that of Example 1.

[0214] In Comparative Examples 8, 9, and 10, the ratio I obtained by FT-EXAFS of Al for the negative electrode A / I B The values ​​of methylaluminoxane ((Al(CH3)O)) added to the negative electrodes of Comparative Examples 8, 9, and 10 were low. n ) is presumed to have failed to produce any effect because no Al—O—C bonds were formed on the surface of the active material, resulting in a resistor.

[0215] In Comparative Examples 11, 12, and 13, the ratio I obtained by FT-EXAFS of Al for the negative electrode A / I B The value of was high. It is presumed that the conditions for the heat treatment after water washing during the preparation of the negative electrode active material (spinel-structure lithium titanate) used in Comparative Examples 11, 12, and 13 were moderate, resulting in a large amount of residual moisture, which resulted in the excessive formation of aluminum alkoxide-derived components on the active material surface. The formed alkoxide-derived components contained a hydrolysis reaction product of aluminum alkoxide, and the hydrolysis reaction product acted as a resistor, which is presumed to be the reason for the inferior high-current performance compared to Example 1. It is also presumed that, although the negative electrode active material was coated, the residual moisture caused a side reaction, resulting in a worsened resistance increase.

[0216] In Comparative Examples 14, 15, and 16, the amount of aluminum alkoxide solution added was reduced. Since the amount of alcohol contained in the aluminum alkoxide solution was reduced, the amount of reactants generated by the reaction with the binder was also reduced. G / S E and D g / T e As shown by the small values ​​of σ and σ, the number of aggregates decreased, which is presumed to be the reason for the poor high-current performance. In addition, the surface of the negative electrode active material was insufficiently coated, which caused a side reaction with the electrolyte, which is presumed to be the reason for the poor life performance.

[0217] In Comparative Examples 17, 18, and 19, the amount of aluminum alkoxide solution added was increased. Since the amount of alcohol contained in the aluminum alkoxide solution also increased, the amount of reactants generated by the reaction with the binder also increased. G / S E and D g / T e As shown by the large size of both agglomerates, the amount of agglomerates increased. The large size of agglomerates made close packing impossible, resulting in a decrease in electrode density and a decrease in energy density.

[0218] In Comparative Examples 20, 21, and 22, no aluminum alkoxide solution was added, and therefore no aggregates resulting from the reaction between the alcohol component contained in the aluminum alkoxide solution and the binder were formed, which is presumably why the large current performance was inferior to that of Example 1. Furthermore, it is presumed that the life performance was also inferior because the surface of the negative electrode active material was not covered with aluminum alkoxide.

[0219] In Comparative Examples 23, 24, and 25, secondary particle powder was used instead of primary particle powder of lithium titanate. Because the interior of the secondary particles could not be coated with aluminum alkoxide, no reaction product with the binder was formed, and no resistor was present, improving output resistance. On the other hand, it is believed that the interior of the secondary particles could not be coated with aluminum alkoxide, resulting in poor life performance. Furthermore, because the secondary particles were already large in size before the addition of the alkoxide, agglomerates increased. The large number of large agglomerates produced made close packing impossible, resulting in reduced electrode density and reduced energy density.

[0220] According to one or more of the embodiments and examples described above, an electrode is provided that includes an active material containing a titanium-containing oxide and an active material-containing layer that includes an aluminum oxide compound present on the surface of the titanium-containing oxide. The titanium-containing oxide may be in the form of both primary particles and aggregates containing multiple primary particles. In addition, the radial distribution function of Al measured by FT-EXAFS for the active material-containing layer includes peak A in the range of 1.1 Å to 1.5 Å and peak B in the range of 2.8 Å to 3.2 Å, and the peak intensity of peak B is I BThe peak intensity I of peak A A Ratio I A / I B The value of the least squares circle diameter D of the aggregate is 3.5 or more and 9 or less. g is the thickness T of the active material-containing layer e The electrode has suppressed electrical resistance and resistance increase, and can realize a battery and a battery pack that are excellent in low-temperature performance.

[0221] Although several embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be embodied in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are intended to be included within the scope and spirit of the invention, as well as within the scope of the invention and its equivalents as defined in the claims.

[0222]

[0023] The following are some embodiments of the present invention. [1] An active material-containing layer is provided, which includes an active material containing a titanium-containing oxide and an aluminum oxide compound present on the surface of the titanium-containing oxide, the titanium-containing oxide having a form including primary particles and a form of aggregates including a plurality of the primary particles, and the radial distribution function obtained by Fourier transform of a broadened X-ray absorption fine structure spectrum at the Al K absorption edge of the active material-containing layer includes a peak A appearing in the range of 1.1 Å to 1.5 Å and a peak B appearing in the range of 2.8 Å to 3.2 Å, and the peak intensity I B The peak intensity I of the peak A relative to A Ratio I A / I B The value of the least squares circle diameter D of the aggregate is 3.5 or more and 9 or less. g is the thickness T of the active material-containing layer e [2] An electrode in which the cross-sectional area S of the active material-containing layer is 1 / 20 or more and less than 1 / 2. E the cross-sectional area S of the aggregate occupying the cross section G The ratio S G / S E[1] The electrode according to [1], wherein the ratio of the titanium-containing oxide to the total mass of the battery is 1 / 200 or more and 1 / 4 or less. [3] The electrode according to [1] or [2], wherein the titanium-containing oxide contains lithium titanate having a spinel structure. [4] A battery comprising a positive electrode, a negative electrode, and an electrolyte, wherein the negative electrode contains the electrode according to any one of [1] to [3]. [5] A battery pack comprising the battery according to [4].

[0223] DESCRIPTION OF SYMBOLS 1...electrode group, 2...exterior member, 3...positive electrode, 3a...positive electrode current collector, 3b...positive electrode active material-containing layer, 4...negative electrode, 4a...negative electrode current collector, 4b...negative electrode active material-containing layer, 4c...negative electrode current collector tab, 4d...aggregate, 5...separator, 6...negative electrode terminal, 7...positive electrode terminal, 11...electrode group, 12...container, 13...rectangular lid, 14...negative electrode tab, 16...glass material, 17...positive electrode tab, 18...positive electrode terminal, 20...battery pack, 21...single cell, 22...adhesive Adhesive tape, 23... battery pack, 24... printed wiring board, 25... thermistor, 26... protection circuit, 27... terminal for supplying power to external device, 28... positive electrode lead, 29... positive electrode connector, 30... negative electrode lead, 31... negative electrode connector, 32... wiring, 33... wiring, 34a... positive electrode wiring, 34b... negative electrode wiring, 35... wiring, 36... protective sheet, 37... storage container, 38... lid, 51... negative electrode terminal, 61... positive electrode terminal.

Claims

1. An active material-containing layer is provided which includes an active material containing a titanium-containing oxide and an aluminum oxide compound present on the surface of the titanium-containing oxide, the titanium-containing oxide having a form including a primary particle form and an aggregate form including a plurality of the primary particles, wherein the radial distribution function obtained by Fourier transform of a broadband X-ray absorption fine structure spectrum at the Al K absorption edge of the active material-containing layer includes a peak A appearing in the range of 1.1 Å to 1.5 Å and a peak B appearing in the range of 2.8 Å to 3.2 Å, and a peak intensity I B The peak intensity I of the peak A A Ratio I A / I B The value of the least square circle diameter D of the aggregate is 3.5 or more and 9 or less. g is the thickness T of the active material-containing layer e The electrode is 1 / 20 or more and less than 1 / 2.

2. Area S of the cross section of the active material-containing layer E The cross-sectional area S of the aggregate occupying the cross section G The ratio S G / S E The electrode according to claim 1 , wherein the ratio is 1 / 200 or more and 1 / 4 or less.

3. The electrode of claim 1, wherein the titanium-containing oxide comprises lithium titanate having a spinel structure.

4. A battery comprising a positive electrode, a negative electrode, and an electrolyte, the negative electrode including an electrode according to any one of claims 1 to 3.

5. A battery pack comprising the battery according to claim 4.

Citation Information

Patent Citations

  • Double-coated lithium titanate battery material and preparation method

    CN108281641A

  • Nonstoichiometric titanium compound, and metal oxide-coated composite material of nonstoichiometric titanium compound, manufacturing method thereof, and negative electrode active material for lithium ion secondary battery, and lithium ion secondary battery

    JP2012123952A

  • Active material for battery, nonaqueous electrolyte battery and battery pack

    JP2015099746A

  • Negative electrode active material with improved output characteristics and electrode for electrochemical device containing the same

    JP2018537833A