Electrochemical cell
The electrochemical cell addresses heat-induced deterioration in the central portion by varying nickel content in the electrode layer and using a metal support with communicating holes, enhancing durability and performance through effective heat management.
Patent Information
- Application Number
- PCT/JP2023/012123
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-03
AI Technical Summary
In electrochemical cells, heat accumulation in the central portion leads to a temperature difference with the outer circumferential portion, causing current concentration and increased susceptibility to deterioration of the central electrode layer.
The electrochemical cell design includes a first electrode layer with a lower nickel content in the central portion compared to the outer peripheral portion, and a metal support with communicating holes, where the nickel content is further varied across different regions to manage heat distribution and reduce expansion/contraction, thereby suppressing deterioration.
This design effectively reduces current concentration and heat-related deterioration in the central portion, improving the cell's durability and maintaining electrode performance by managing temperature differences and expansion/contraction.
Smart Images

Figure JP2023012123_03102024_PF_FP_ABST
Abstract
Description
electrochemical cell
[0001] The present invention relates to electrochemical cells.
[0002] BACKGROUND ART Conventionally, electrochemical cells (electrolysis cells, fuel cells, etc.) that include a cell body having an electrolyte layer disposed between a first electrode layer and a second electrode layer are known (see, for example, Patent Document 1).
[0003] Also known is an electrochemical cell in which the cell body is disposed on a metal support (see, for example, Patent Document 2).
[0004] JP 2014-049322 A JP 2020-155337 A
[0005] In the electrochemical cell described above, heat tends to accumulate in the center of the first electrode layer when viewed from above. This creates a temperature difference between the center and the peripheral portion surrounding the center, causing current to concentrate in the center. As a result, the center is more susceptible to deterioration than the peripheral portion.
[0006] An object of the present invention is to provide an electrochemical cell capable of suppressing deterioration of the central portion of the first electrode layer.
[0007] An electrochemical cell according to a first aspect of the present invention includes a cell body. The cell body has a first electrode layer, a second electrode layer, and an electrolyte layer disposed between the first and second electrode layers. The first electrode layer includes a central portion and an outer peripheral portion surrounding the central portion. The central portion and the outer peripheral portion each contain nickel and an ion-conductive material. The nickel content in the central portion is lower than the nickel content in the outer peripheral portion.
[0008] The electrochemical cell according to a second aspect of the present invention is the electrochemical cell according to the first aspect, and includes a metal support for supporting a cell body, the metal support having a main surface on which the first electrode layer is formed and a plurality of communication holes formed in the main surface.
[0009] According to a third aspect of the present invention, there is provided an electrochemical cell according to the first or second aspect, further comprising a metal support supporting the cell body and having a plurality of through holes formed in a main surface thereof. The central portion has a first region within 5 μm of a first surface in contact with the metal support, a second region within 5 μm of a second surface in contact with the electrolyte layer, and a third region between the first and second regions. The nickel content in the first region is lower than the nickel content in the third region.
[0010] An electrochemical cell according to a fourth aspect of the present invention is the electrochemical cell according to the third aspect, wherein the content of nickel in the second region is lower than the content of nickel in the third region.
[0011] An electrochemical cell according to a fifth aspect of the present invention is related to the third or fourth aspect, wherein the central portion has a fourth region disposed inside at least one of the plurality of communicating holes, and the nickel content in the fourth region is lower than the nickel content in the third region.
[0012] According to the present invention, it is possible to provide an electrochemical cell capable of suppressing deterioration of the central portion of the first electrode layer.
[0013] Fig. 1 is a plan view of an electrolysis cell according to an embodiment. Fig. 2 is a cross-sectional view taken along line AA in Fig. 1. Fig. 3 is a partially enlarged view of Fig. 2. Fig. 4 is a cross-sectional view of an electrolysis cell 100 according to a first modification.
[0014] (Electrolytic cell 1) Fig. 1 is a plan view of an electrolytic cell 1 according to an embodiment. Fig. 2 is a cross-sectional view taken along line AA in Fig. 1. Fig. 2 shows a cross section passing through the geometric center CP of a hydrogen electrode layer 6, which will be described later.
[0015] The electrolytic cell 1 is an example of an "electrochemical cell" according to the present invention. The electrolytic cell 1 is a so-called metal-supported electrolytic cell.
[0016] The electrolytic cell 1 is formed in a plate shape extending in the X-axis and Y-axis directions. In the present embodiment, the electrolytic cell 1 is formed in a rectangular shape extending in the Y-axis direction when viewed in a plan view from the Z-axis direction perpendicular to the X-axis and Y-axis directions. However, the planar shape of the electrolytic cell 1 is not particularly limited, and may be a polygon other than a rectangle, an ellipse, a circle, or the like.
[0017] The X-axis direction and the Y-axis direction are the surface directions of the electrolytic cell 1, and the Z-axis direction is the thickness direction of the electrolytic cell 1.
[0018] As shown in FIG. 2 , the electrolysis cell 1 includes a metal support 10 , a cell main body 20 , and a flow path member 30 .
[0019] [Metal Support 10] The metal support 10 supports the cell main body 20. The metal support 10 is formed in a plate shape. The metal support 10 may be in the shape of a flat plate or a curved plate.
[0020] The metal support 10 may have any thickness as long as it can support the electrolysis cell 1, and may have a thickness of, for example, 0.1 mm or more and 2.0 mm or less. The thermal expansion coefficient of the metal support 10 is not particularly limited, but may be, for example, 10×10 ―6 / ℃ or more 18 x 10 ―6 / °C or less.
[0021] As shown in FIG. 2 , the metal support 10 has a plurality of through holes 11 , a first main surface 12 and a second main surface 13 .
[0022] Each communication hole 11 penetrates the metal support 10 from the first main surface 12 to the second main surface 13. Each communication hole 11 opens to both the first main surface 12 and the second main surface 13. The opening of each communication hole 11 on the first main surface 12 side is covered by the hydrogen electrode layer 6. The opening of each communication hole 11 on the second main surface 13 side is connected to a flow path 30a, which will be described later.
[0023] Each of the communication holes 11 can be formed by mechanical processing (for example, punching), laser processing, or chemical processing (for example, etching).
[0024] In this embodiment, each communication hole 11 is formed linearly along the Z-axis direction. However, each communication hole 11 may be inclined with respect to the Z-axis direction, or may not be linear. Furthermore, the communication holes 11 may be connected to each other.
[0025] The first main surface 12 is provided on the opposite side to the second main surface 13. The cell main body 20 is disposed on the first main surface 12. The flow path member 30 is bonded to the second main surface 13.
[0026] The metal support 10 is made of a metal material. For example, the metal support 10 is made of an alloy material containing Cr (chromium). Examples of such metal materials include Fe—Cr alloy steel (stainless steel, etc.) and Ni—Cr alloy steel. The Cr content in the metal support 10 is not particularly limited, but can be set to 4% by mass or more and 30% by mass or less.
[0027] The metal support 10 may contain Ti (titanium) or Zr (zirconium). The Ti content in the metal support 10 is not particularly limited, but may be 0.01 mol % or more and 1.0 mol % or less. The Al content in the metal support 10 is not particularly limited, but may be 0.01 mol % or more and 0.4 mol % or less. The metal support 10 may contain Ti in the form of TiO 2 (titania), or Zr may be contained as ZrO 2 It may be contained as (zirconia).
[0028] The metal support 10 may have an oxide film on its surface, which is formed by oxidation of the constituent elements of the metal support 10. A typical example of the oxide film is a chromium oxide film. The chromium oxide film covers at least a portion of the surface of the metal support 10. The chromium oxide film may also cover at least a portion of the inner wall surface of each communicating hole 11.
[0029] [Cell Body 20] The cell body 20 is disposed on the metal support 10. The cell body 20 is supported by the metal support 10. The cell body 20 has a hydrogen electrode layer 6 (cathode), an electrolyte layer 7, a reaction prevention layer 8, and an oxygen electrode layer 9 (anode).
[0030] The hydrogen electrode layer 6, electrolyte layer 7, reaction prevention layer 8, and oxygen electrode layer 9 are stacked in this order in the Z-axis direction from the metal support 10 side. The hydrogen electrode layer 6, electrolyte layer 7, and oxygen electrode layer 9 are essential components, while the reaction prevention layer 8 is optional.
[0031] [Hydrogen Electrode Layer 6] The hydrogen electrode layer 6 is an example of a "first electrode layer" according to the present invention. The hydrogen electrode layer 6 is disposed between the metal support 10 and the electrolyte layer 7. The hydrogen electrode layer 6 is formed on the first main surface 12 of the metal support 10. In this embodiment, a portion of the hydrogen electrode layer 6 is disposed inside each of the communication holes 11 of the metal support 10. The detailed configuration of the hydrogen electrode layer 6 will be described later.
[0032] A source gas is supplied to the hydrogen electrode layer 6 through each of the communication holes 11. The source gas contains at least H 2 Contains O.
[0033] The raw material gas is H 2 When only O is contained, the hydrogen electrode layer 6 converts H from the raw material gas according to the electrochemical reaction of water electrolysis shown in the following formula (1): 2 Hydrogen electrode layer 6: H 2 O + 2e - →H 2 +O 2- ...(1)
[0034] The raw material gas is H 2 O plus CO 2 In this case, the hydrogen electrode layer 6 converts the source gas into H according to the electrochemical reactions of co-electrolysis shown in the following formulas (2), (3), and (4). 2 , CO and O 2- Hydrogen electrode layer 6: CO 2 +H 2 O+4e - →CO+H 2 +20 2- ... (2) H 2 Electrochemical reaction of O: H 2 O + 2e - →H 2 +O 2- ... (3) CO 2 Electrochemical reaction of: CO 2 +2e - →CO+O2- ...(4)
[0035] The hydrogen electrode layer 6 is an electron-conductive porous body containing nickel (Ni) and an oxide ion conductive material.
[0036] Ni acts as an electron conductor. In the case of co-electrolysis, Ni acts as an electron conductor. 2 and CO contained in the raw material gas 2 It also functions as a thermal catalyst, promoting the thermal reaction with HCl to maintain an appropriate gas composition for methanation and reverse water-gas shift reactions.
[0037] Ni exists in the form of nickel oxide (NiO) in an oxidizing atmosphere and in the form of metallic Ni in a reducing atmosphere. The hydrogen electrode layer 6 is exposed to an oxidizing atmosphere when the electrolytic cell 1 is not in operation, and is exposed to a reducing atmosphere when the electrolytic cell 1 is in operation and during a reduction treatment performed before the operation of the electrolytic cell 1. The hydrogen electrode layer 6 expands and contracts as Ni is oxidized and reduced.
[0038] The oxide ion conductive material is an example of the "ion conductive material" according to the present invention. Examples of the oxide ion conductive material include YSZ, CSZ, ScSZ, GDC, SDC, and (La,Sr)(Cr,Mn)O. 3 , (La,Sr)TiO 3 , Sr 2 (Fe, Mo) 2 O 6 , (La, Sr)VO 3 , (La,Sr)FeO 3 , LDC (lanthanum doped ceria), LSGM (lanthanum gallate), and a mixed material of two or more of these can be used.
[0039] The thickness of the hydrogen electrode layer 6 is not particularly limited, but may be, for example, 1 μm or more and 100 μm or less. The thermal expansion coefficient of the hydrogen electrode layer 6 is not particularly limited, but may be, for example, 10×10 ―6 / ℃ or more 13 x 10 -6 / °C or less.
[0040] The method for forming the hydrogen electrode layer 6 is not particularly limited, and may be a firing method, a spray coating method (such as a thermal spraying method, an aerosol deposition method, an aerosol gas deposition method, a powder jet deposition method, a particle jet deposition method, or a cold spray method), a PVD method (such as a sputtering method or a pulsed laser deposition method), or a CVD method.
[0041] [Electrolyte Layer 7] The electrolyte layer 7 is disposed between the hydrogen electrode layer 6 and the oxygen electrode layer 9. In this embodiment, the reaction prevention layer 8 is disposed between the electrolyte layer 7 and the oxygen electrode layer 9, and therefore the electrolyte layer 7 is sandwiched between the hydrogen electrode layer 6 and the reaction prevention layer 8.
[0042] The electrolyte layer 7 covers the hydrogen electrode layer 6 and also covers the region of the first main surface 12 of the metal support 10 that is exposed from the hydrogen electrode layer 6 .
[0043] The electrolyte layer 7 absorbs the O generated in the hydrogen electrode layer 6. 2- The electrolyte layer 7 is made of a dense material having oxide ion conductivity. The electrolyte layer 7 can be made of, for example, YSZ (yttria-stabilized zirconia, e.g., 8YSZ), GDC (gadolinium-doped ceria), ScSZ (scandia-stabilized zirconia), SDC (samarium-doped ceria), or LSGM (lanthanum gallate).
[0044] The porosity of the electrolyte layer 7 is not particularly limited, but may be, for example, 0.1% to 7%. The thickness of the electrolyte layer 7 is not particularly limited, but may be, for example, 1 μm to 100 μm. The thermal expansion coefficient of the electrolyte layer 7 is not particularly limited, but may be, for example, 9×10 ―6 / ℃ or more 12 x 10 ―6 / °C or less.
[0045] The method for forming the electrolyte layer 7 is not particularly limited, and may be a baking method, a spray coating method, a PVD method, a CVD method, or the like.
[0046] [Reaction prevention layer 8] The reaction prevention layer 8 is disposed between the electrolyte layer 7 and the oxygen electrode layer 9. The reaction prevention layer 8 is disposed on the opposite side of the electrolyte layer 7 from the hydrogen electrode layer 6. The reaction prevention layer 8 prevents the constituent elements of the electrolyte layer 7 from reacting with the constituent elements of the oxygen electrode layer 9 to form a layer with high electrical resistance.
[0047] The reaction prevention layer 8 is made of an oxide ion conductive material, such as GDC or SDC.
[0048] The porosity of the reaction prevention layer 8 is not particularly limited, but may be, for example, 0.1% to 50%. The thickness of the reaction prevention layer 8 is not particularly limited, but may be, for example, 1 μm to 50 μm.
[0049] The method for forming the reaction prevention layer 8 is not particularly limited, and may be a baking method, a spray coating method, a PVD method, a CVD method, or the like.
[0050] [Oxygen Electrode Layer 9] The oxygen electrode layer 9 is an example of a "second electrode layer" according to the present invention. The oxygen electrode layer 9 is disposed on the opposite side of the electrolyte layer 7 from the hydrogen electrode layer 6. In this embodiment, the reaction prevention layer 8 is disposed between the electrolyte layer 7 and the oxygen electrode layer 9, and therefore the oxygen electrode layer 9 is connected to the reaction prevention layer 8. If the reaction prevention layer 8 is not disposed between the electrolyte layer 7 and the oxygen electrode layer 9, the oxygen electrode layer 9 is connected to the electrolyte layer 7.
[0051] The oxygen electrode layer 9 reacts with O transferred from the hydrogen electrode layer 6 through the electrolyte layer 7 in accordance with the chemical reaction of the following formula (5): 2- From O 2 Oxygen electrode layer 9: 2O 2- →O 2 +4e - ...(5)
[0052] The oxygen electrode layer 9 is made of a porous material having oxide ion conductivity and electron conductivity, such as (La, Sr)(Co, Fe)O. 3 , (La,Sr)FeO 3 , La(Ni,Fe)O 3 , (La,Sr)CoO 3 , and (Sm,Sr)CoO3 and an oxide ion conductive material (such as GDC).
[0053] The porosity of the oxygen electrode layer 9 is not particularly limited, but may be, for example, 20% to 60%. The thickness of the oxygen electrode layer 9 is not particularly limited, but may be, for example, 1 μm to 100 μm.
[0054] The method for forming the oxygen electrode layer 9 is not particularly limited, and may be a firing method, a spray coating method, a PVD method, a CVD method, or the like.
[0055] [Flow Channel Member 30] The flow channel member 30 is bonded to the second main surface 13 of the metal support 10. A flow channel 30a is formed between the flow channel member 30 and the metal support 10. A source gas is supplied to the flow channel 30a. The source gas supplied to the flow channel 30a is supplied to the hydrogen electrode layer 6 of the cell main body 20 via each communication hole 11 of the metal support 10.
[0056] The flow path member 30 can be made of, for example, an alloy material. The flow path member 30 may be made of the same material as the metal support 10. In this case, the flow path member 30 may be substantially integrated with the metal support 10.
[0057] The flow path member 30 has a frame 31 and an interconnector 32. The frame 31 is an annular member that surrounds the side of the flow path 30a. The frame 31 is joined to the second main surface 13 of the metal support 10. The interconnector 32 is a plate-like member for electrically connecting an external power source or another electrolytic cell to the electrolytic cell 1 in series. The interconnector 32 is joined to the frame 31.
[0058] In this embodiment, the frame body 31 and the interconnector 32 are separate members, but the frame body 31 and the interconnector 32 may be an integrated member.
[0059] (Configuration of Hydrogen Electrode Layer 6) As shown in Figs. 1 and 2, the hydrogen electrode layer 6 has a central portion 6a and an outer peripheral portion 6b.
[0060] The central portion 6a is a portion including the geometric center CP of the hydrogen electrode layer 6 in a plan view. In this embodiment, as shown in FIG. 1 , the planar shape of the hydrogen electrode layer 6 is rectangular in a plan view, and the planar shape of the central portion 6a in a plan view is also rectangular. In a plan view, the central portion 6a is located inside the hydrogen electrode layer 6. The planar shape of the central portion 6a is similar to the planar shape of the hydrogen electrode layer 6. That is, when the outer edge of the central portion 6a is enlarged by a predetermined magnification, the outer edge of the central portion 6a and the outer edge of the hydrogen electrode layer 6 become congruent. The predetermined magnification is not particularly limited, but can be, for example, 1.2 times or more and 4 times or less. In this embodiment, the predetermined magnification is 2.0 times, and when the outer edge of the central portion 6a is enlarged by 2 times, it becomes congruent with the outer edge of the hydrogen electrode layer 6.
[0061] However, as long as the central portion 6a includes the geometric center CP, the planar shapes and sizes of the hydrogen electrode layer 6 and the central portion 6a can be changed as appropriate. Therefore, the planar shapes of the hydrogen electrode layer 6 and the central portion 6a may each be a shape other than a rectangle (e.g., a polygon other than a rectangle, an ellipse, a circle, etc.). The planar shape of the central portion 6a may also be different from the planar shape of the hydrogen electrode layer 6. The total area of the hydrogen electrode layer 6 in plan view can be 1.44 to 16 times the area of the central portion 6a in plan view.
[0062] The outer peripheral portion 6b is a portion that surrounds the central portion 6a in a plan view. The outer peripheral portion 6b is formed in an annular shape in a plan view. The planar shape of the outer peripheral portion 6b can be appropriately changed depending on the planar shapes of the hydrogen electrode layer 6 and the central portion 6a.
[0063] The central portion 6a and the outer peripheral portion 6b each contain Ni and an oxide ion conductive material.
[0064] The Ni content in the central portion 6 a is lower than the Ni content in the outer peripheral portion 6 b. This intentionally reduces the current flowing through the central portion 6 a, where heat tends to build up, thereby preventing a temperature difference from occurring between the central portion 6 a and the outer peripheral portion 6 b. This prevents current concentration due to a temperature rise in the central portion 6 a and the resulting further temperature rise, thereby preventing deterioration of the central portion 6 a.
[0065] Furthermore, by making the Ni content in the central portion 6 a lower than the Ni content in the peripheral portion 6 b, the expansion / contraction of the first region 61 caused by the oxidation-reduction cycle can be reduced, thereby preventing the central portion 6 a from peeling off from the metal support 10.
[0066] The Ni content in each of the central portion 6a and the outer peripheral portion 6b is calculated as described below.
[0067] The method for measuring the Ni content in the central portion 6a will be described. First, a cross section of the hydrogen electrode layer 6 passing through the geometric center CP and taken along the Z-axis direction is exposed. Next, the Ni content is measured at four locations on the geometric center CP that divide the central portion 6a into five equal parts along the Z-axis direction. Next, the Ni content in the central portion 6a is calculated by averaging the four measured values. The value of the Ni content in the central portion 6a is not particularly limited, but can be 20 mol% or more and 50 mol% or less.
[0068] A method for measuring the Ni content in the outer peripheral portion 6b will be described. First, in the cross section of the hydrogen electrode layer 6 used to measure the Ni content in the central portion 6a, the distance between one end of the hydrogen electrode layer 6 and the geometric center CP in the X-axis direction is set to "100", and the Ni content is measured at four locations that divide the outer peripheral portion 6b into five equal parts in the Z-axis direction, at positions "90" away from the geometric center CP in the X-axis direction. Next, the Ni content in the outer peripheral portion 6b is calculated by averaging the four measured values. The Ni content in the outer peripheral portion 6b is not particularly limited, but can be 25 mol% or more and 55 mol% or less.
[0069] The Ni content is calculated by the following method. First, a Ni composition mapping image on a cross section is obtained at 5,000 to 10,000 magnifications using an SEM device (FE-SEM JSM-7900F, manufactured by JEOL Ltd.) and an EDS device (JED-2300) attached to the SEM device. Next, Ni particle portions are identified in the Ni composition mapping image by performing binarization processing through image analysis using image analysis software Image-Pro manufactured by MEDIACYBERNETICS. The Ni content is then calculated by dividing the total area of the Ni particle portions by the total area of the backscattered electron image.
[0070] (Detailed Configuration of Central Portion 6a) FIG. 3 is an enlarged view of the central portion 6a shown in FIG.
[0071] As shown in FIG. 3, the central portion 6 a has a first region 61 , a second region 62 , a third region 63 , and a fourth region 64 .
[0072] The first region 61 is a region of the central portion 6a that is within 5 μm in the Z-axis direction from the first surface S1 that contacts the metal support 10. The second region 62 is a region of the central portion 6a that is within 5 μm in the Z-axis direction from the second surface S2 that contacts the electrolyte layer 7. The third region 63 is a region of the central portion 6a that is between the first region 61 and the second region 62. The fourth region 64 is a region of the central portion 6a that is located inside the communicating hole 11 formed in the metal support 10. The fourth region 64 exerts an anchor effect on the metal support 10 by being engaged with the communicating hole 11.
[0073] The first to third regions 61 to 63 are essential components, while the fourth region 64 is optional. The fourth region 64 only needs to be located inside at least one of the plurality of communicating holes 11 formed in the metal support 10. Therefore, the number of fourth regions 64 may be the same as or less than the number of communicating holes 11.
[0074] The first surface S1 of the central portion 6a is in contact with the first main surface 12 of the metal support 10. When identifying the first region 61, an approximation line of the first surface S1 obtained by the least squares method is used in a cross section along the Z axis direction. Specifically, the region of the surface of the hydrogen electrode layer 6 that is in contact with the first main surface 12 of the metal support 10 is approximated as a straight line by the least squares method, and the obtained approximation line is defined as the first surface S1 of the hydrogen electrode layer 6. Note that the region of the surface of the hydrogen electrode layer 6 that is in contact with the first main surface 12 of the metal support 10 does not include the inner circumferential surfaces of the through holes 11 of the metal support 10.
[0075] The second surface S2 of the central portion 6a is in contact with the hydrogen electrode layer-side surface S3 of the electrolyte layer 7. When identifying the second region 62, an approximation line of the second surface S2 obtained by the least squares method is used in a cross section along the Z axis direction. Specifically, the region of the surface of the hydrogen electrode layer 6 that is in contact with the hydrogen electrode layer-side surface S3 of the electrolyte layer 7 is approximated as a straight line by the least squares method, and the obtained approximation line is defined as the second surface S2 of the hydrogen electrode layer 6.
[0076] Each of the first to fourth regions 61 to 64 contains Ni and an oxide ion conductive material.
[0077] The Ni content in the first region 61 is preferably lower than the Ni content in the third region 63. This reduces the expansion / contraction of the first region 61 due to the oxidation-reduction cycle, thereby further preventing the central portion 6 a from peeling off from the metal support 10. Furthermore, the third region 63 can improve the electronic conductivity and catalytic performance. This makes it possible to both prevent peeling of the central portion 6 a and maintain electrode performance.
[0078] The Ni content in the second region 62 is preferably lower than the Ni content in the third region 63. This reduces expansion / contraction not only in the first region 61 but also in the second region 62, making it possible to suppress an increase in internal resistance due to deterioration in adhesion between the hydrogen electrode layer 6 and the electrolyte layer 7 when oxidation-reduction cycles are repeated, while maintaining electrode performance.
[0079] The Ni content in the fourth region 64 is preferably lower than the Ni content in the third region 63. This reduces the expansion / contraction of the fourth region 64 caused by the oxidation-reduction cycle, thereby suppressing changes in the shape of the fourth region 64. As a result, the anchoring effect of the fourth region 64 can be maintained.
[0080] The Ni contents in the first to fourth regions 61 to 64 are calculated by the same method, as will be described next.
[0081] The method for measuring the Ni content in the first region 61 will be described. First, in the cross section of the hydrogen electrode layer 6 used to measure the Ni content in the central portion 6 a, the Ni content is measured at three locations (randomly selected) spaced apart in the planar direction at the geometric center CP in the thickness direction central portion of the first region 61. Next, the Ni content in the first region 61 is calculated by averaging the three measured values. The value of the Ni content in the first region 61 is not particularly limited, but can be 20 mol% or more and 45 mol% or less.
[0082] The method for measuring the Ni content in the second region 62 will be described. First, in the cross section of the hydrogen electrode layer 6 used to measure the Ni content in the central portion 6 a, the Ni content is measured at three locations (randomly selected) spaced apart in the plane direction at the center of the thickness direction of the second region 62 on the geometric center CP. Next, the Ni content in the second region 62 is calculated by averaging the three measured values. The value of the Ni content in the second region 62 is not particularly limited, but can be 20 mol% or more and 45 mol% or less.
[0083] The method for measuring the Ni content in the third region 63 will be described. First, in the cross section of the hydrogen electrode layer 6 used to measure the Ni content in the central portion 6 a, the Ni content is measured at four locations that divide the third region 63 into five equal parts in the Z-axis direction at the geometric center CP. Next, the Ni content in the third region 63 is calculated by averaging the four measured values. The value of the Ni content in the third region 63 is not particularly limited, but can be 30 mol% or more and 50 mol% or less.
[0084] The method for measuring the Ni content in the fourth region 63 will be described. First, in the cross section of the hydrogen electrode layer 6 used to measure the Ni content in the central portion 6 a, the communicating hole 11 passing through the geometric center CP or the communicating hole 11 closest to the geometric center CP is identified. Next, the Ni content is measured at three locations (randomly selected) spaced apart in the planar direction in the thickness direction central portion of the fourth region 63 located inside the identified communicating hole 11. Next, the Ni content in the fourth region 64 is calculated by averaging the three measured values. The value of the Ni content in the fourth region 64 is not particularly limited, but can be 20 mol% or more and 45 mol% or less.
[0085] (Modifications of the Embodiment) Although the embodiment of the present invention has been described above, the present invention is not limited to these, and various modifications are possible without departing from the spirit of the present invention.
[0086] [Variation 1] In the above embodiment, when the first main surface 12 of the metal support 10 is planar (i.e., linear in a cross section along the Z-axis direction as shown in FIG. 3 ), the first surface S1 of the hydrogen electrode layer 6 is defined by the first main surface 12 of the metal support 10.
[0087] However, if the first main surface 12 of the metal support 10 is not planar (for example, if the metal support 10 is made of porous metal), it is difficult to identify the first surface S1 of the hydrogen electrode layer 6 using the first main surface 12 of the metal support 10.
[0088] A method for identifying the first surface S1 of the hydrogen electrode layer 6 when the first main surface 12 of the metal support 10 is not planar will now be described with reference to Fig. 4. Fig. 4 is a cross section of the electrolysis cell 100 taken along the Z-axis direction (thickness direction).
[0089] The electrolysis cell 100 has the same configuration as the electrolysis cell 1 according to the above embodiment, except that the metal support 110 is made of porous metal. The metal support 110 has metal particles 111 connected in a three-dimensional network and a plurality of interconnected communication holes 112. The first main surface 113 of the metal support 10 has projections and recesses formed along the outer edges of the metal particles 111.
[0090] In the electrolysis cell 100, first, the second surface S2 of the hydrogen electrode layer 6 is identified by the hydrogen electrode layer-side surface S3 of the electrolyte layer 7. Next, when the second surface S2 of the hydrogen electrode layer 6 is moved horizontally in the Z-axis direction toward the metal support 110, the intersection points P where the second surface S2 intersects with the metal particles 111 are identified. At this time, the intersection points P are identified for each cluster of metal particles 111 that are separated on the cross section. In the example shown in FIG. 4, the metal particles 111 are divided into three clusters, and therefore intersection points P1 to P3 are identified in FIG. 4. Finally, the lines sequentially connecting the intersection points P1 to P3 are defined as the first surface S1 of the hydrogen electrode layer 6.
[0091] As described above, when the first main surface 113 of the metal support 110 is not flat, the first surface S1 of the hydrogen electrode layer 6 can be identified based on the hydrogen electrode layer-side surface S3 of the electrolyte layer 7.
[0092] [Modification 2] In the above embodiment, the hydrogen electrode layer 6 has the fourth region 64 , but it does not have to have the fourth region 64 .
[0093] [Variation 3] In the above embodiment, the metal-supported electrolytic cell 1 has been described as an example of an electrolytic cell. However, the electrolytic cell according to the present invention may be a flat-plate type that does not include a metal support 10.
[0094] [Variation 4] In the above embodiment, the electrolysis cell 1 has been described as an example of an electrochemical cell, but the electrochemical cell is not limited to an electrolysis cell. An electrochemical cell is a general term for an element in which a pair of electrodes are arranged so that an electromotive force is generated from an overall oxidation-reduction reaction in order to convert electrical energy into chemical energy, and an element for converting chemical energy into electrical energy. Therefore, electrochemical cells include, for example, fuel cells that use oxide ions or protons as carriers. The electrochemical cell may be a metal-supported type or a flat-plate type.
[0095] Examples of the electrochemical cell according to the present invention will be described below, but the present invention is not limited to the examples described below.
[0096] Comparative Examples 1 and 2 Electrolytic cells according to Comparative Examples 1 and 2 were prepared as follows.
[0097] First, a metal support made of Fe-Cr-Mn alloy steel and having a plurality of communicating holes formed therein was prepared.
[0098] Next, a slurry for the hydrogen electrode layer was prepared by mixing GDC powder, NiO powder, butyral resin, polymethyl methacrylate beads as a pore-forming material, a plasticizer, a dispersant, and a solvent, and the slurry for the hydrogen electrode layer was then printed onto the first main surface of the metal support by a doctor blade method to form a green body for the hydrogen electrode layer.
[0099] Next, a slurry for the electrolyte layer was prepared by mixing YSZ powder, butyral resin, a plasticizer, a dispersant, and a solvent, and then the slurry for the electrolyte was printed by a doctor blade method so as to cover the green body for the hydrogen electrode layer, thereby forming a green body for the electrolyte layer.
[0100] Next, a slurry for the reaction prevention layer was prepared by mixing GDC powder, polyvinyl alcohol, and a solvent, and the slurry for the reaction prevention layer was then printed on the green body of the electrolyte layer by a doctor blade method to form a green body of the reaction prevention layer.
[0101] Next, the molded bodies of the hydrogen electrode layer, electrolyte layer, and reaction prevention layer arranged in this order on the metal support were fired in air (1050°C, 1 hour) to form the hydrogen electrode layer, electrolyte layer, and reaction prevention layer.
[0102] Next, (La,Sr)(Co,Fe)O 3 The powder, polyvinyl alcohol, and a solvent were mixed to prepare a slurry for the oxygen electrode layer, which was then printed onto the reaction prevention layer by a doctor blade method to form a green body for the oxygen electrode layer.
[0103] Next, the compact for the oxygen electrode layer was fired in air (1000° C., 1 hour) to form an oxygen electrode.
[0104] Finally, a flow path member made of Fe-Cr-Mn alloy steel was connected to the second main surface of the metal support using crystallized glass. In this way, the electrolytic cells according to Examples 1 to 9 were completed.
[0105] Examples 1 to 5 Electrolytic cells according to Examples 1 to 5 were fabricated using the same steps as those of Comparative Examples 1 and 2, except that the hydrogen electrode layer had a double structure.
[0106] Specifically, a slurry for the central portion was prepared by mixing GDC powder, NiO powder, butyral resin, polymethyl methacrylate beads as a pore-forming material, a plasticizer, a dispersant, and a solvent. The amount of NiO powder added was adjusted to change the Ni content in the central portion as shown in Table 1. The slurry for the central portion was then printed on the first main surface of the metal support by a doctor blade method to form a compact for the central portion of the hydrogen electrode layer.
[0107] Next, a slurry for the outer periphery was prepared by mixing GDC powder, NiO powder, butyral resin, polymethyl methacrylate beads as a pore-forming material, a plasticizer, a dispersant, and a solvent. The amount of NiO powder added was adjusted to change the Ni content in the outer periphery as shown in Table 1. The slurry for the outer periphery was then printed on the first main surface by a doctor blade method so as to surround the central compact, thereby forming a compact for the outer periphery of the hydrogen electrode layer.
[0108] (Steady-state durability evaluation) First, the electrolytic cells of Examples 1 to 5 and Comparative Examples 1 and 2 were heated to 750°C, and hydrogen was supplied to the hydrogen electrode layer from the flow path in the flow path member, thereby reducing NiO contained in the hydrogen electrode layer to Ni.
[0109] Next, a mixed gas of water vapor and hydrogen (mixing ratio 90:10) was supplied to the hydrogen electrode layer, and the current density per hydrogen electrode layer area was adjusted to 0.5 A / cm 2 The cell voltage when electrolysis was performed by passing a current so as to be constant at 1000 kJ / min (hereinafter referred to as "initial cell voltage") was measured.
[0110] Subsequently, the current density was increased to 0.5 A / cm while supplying the mixed gas. 2 The cell voltage after being held in a fixed state for 1000 hours (hereinafter referred to as "cell voltage after steady-state durability") was measured.
[0111] Then, the steady-state deterioration rate was calculated using the following formula (6): Steady-state deterioration rate (%)=100×(cell voltage after steady-state durability test−initial cell voltage) / initial cell voltage (6).
[0112] In Table 1, a steady-state deterioration rate of less than 7% was evaluated as "good", and a steady-state deterioration rate of 7% or more was evaluated as "poor".
[0113] (Observation of Delamination) After the steady-state durability evaluation, the cross section of the hydrogen electrode layer and the metal support along the thickness direction was observed using an SEM (magnification 1000x) in 10 fields at 200 μm intervals in the surface direction from each end of the interface between the center of the hydrogen electrode layer and the metal support to check for the presence or absence of interfacial delamination (a portion where the non-bonded region at the interface continues for 50 μm or more in the surface direction).
[0114] In Table 1, the case where peeling was observed in one or more visual fields was judged as "x", and the case where no peeling was observed was judged as "good".
[0115]
[0116] As shown in Table 1, in Examples 1 to 5, in which the Ni content in the central portion of the hydrogen electrode layer was lower than the Ni content in the peripheral portion of the hydrogen electrode layer, the deterioration rate after the steady-state durability evaluation was lower than in Comparative Examples 1 and 2. Such results were obtained because the current flowing through the central portion, where heat tends to accumulate, was intentionally reduced, thereby suppressing the temperature difference between the central portion and the peripheral portion.
[0117] Furthermore, in Examples 1 to 5, peeling after the steady-state durability evaluation could be suppressed compared to Comparative Example 1. Such results were obtained because the expansion / contraction of the first region caused by reduction could be reduced.
[0118] Examples 6 to 11 Electrolytic cells according to Examples 6 to 11 were fabricated using the same process as in Examples 1 to 5, except that the central portion of the hydrogen electrode layer had a multilayer structure.
[0119] Specifically, a slurry for the first region was prepared by mixing GDC powder, NiO powder, butyral resin, polymethyl methacrylate beads as a pore-forming material, a plasticizer, a dispersant, and a solvent. The amount of NiO powder added was adjusted to change the Ni content in the first region as shown in Table 2. The slurry for the first region was then printed on the first main surface of the metal support by a doctor blade method to form a compact for the first region in the central portion of the hydrogen electrode layer.
[0120] Next, a slurry for the third region was prepared by mixing GDC powder, NiO powder, butyral resin, polymethyl methacrylate beads as a pore-forming material, a plasticizer, a dispersant, and a solvent. The amount of NiO powder added was adjusted to change the Ni content in the third region as shown in Table 2. The slurry for the third region was then printed onto the compact for the first region by a doctor blade method to form a compact for the third region in the central portion of the hydrogen electrode layer.
[0121] Next, a slurry for the second region was prepared by mixing GDC powder, NiO powder, butyral resin, polymethyl methacrylate beads as a pore-forming material, a plasticizer, a dispersant, and a solvent. The amount of NiO powder added was adjusted to change the Ni content in the second region as shown in Table 2. The slurry for the second region was then printed on the compact for the third region by a doctor blade method to form a compact for the second region in the center of the hydrogen electrode layer.
[0122] (Initial Evaluation of Electrolytic Cell Performance) First, the electrolytic cells of Examples 2 and 4 and Examples 6 to 11 described above were heated to 750°C, and hydrogen was supplied to the hydrogen electrode layer from the flow path in the flow path member, thereby reducing the NiO contained in the hydrogen electrode layer to Ni.
[0123] Next, a mixed gas of water vapor and hydrogen (mixing ratio 90:10) was supplied to the hydrogen electrode layer, and the current density per hydrogen electrode layer area was adjusted to 0.5 A / cm 2The initial cell voltage was measured when electrolysis was performed by passing a current so that the current was constant at 1.300 [V]. In Table 2, a cell voltage of less than 1.300 [V] was evaluated as "Good", and a cell voltage of 1.300 [V] or more was evaluated as "Poor".
[0124] (Evaluation of Redox Cycle Durability of Electrolytic Cell Performance) Following measurement of the initial cell voltage, the electrolytic cells of Examples 2 and 4 and Examples 6 to 11 were evaluated for redox cycle durability.
[0125] Specifically, 100 oxidation-reduction cycles were performed in which the following steps were performed in sequence: supplying a mixed gas of water vapor and hydrogen (mixing ratio 90:10) to the hydrogen electrode layer for 10 hours, supplying a mixed gas of water vapor and hydrogen (mixing ratio 98:2) to the hydrogen electrode layer for 10 hours, and supplying a mixed gas of water vapor and hydrogen (mixing ratio 90:10) to the hydrogen electrode layer for 10 hours.
[0126] Next, a mixed gas of water vapor and hydrogen (mixing ratio 90:10) was supplied to the hydrogen electrode layer, and the current density per hydrogen electrode layer area was adjusted to 0.5 A / cm 2 The cell voltage when electrolysis was performed by passing a current so that the current was constant (hereinafter referred to as "cell voltage after oxidation-reduction cycle durability") was measured.
[0127] Then, the oxidation-reduction cycle deterioration rate was calculated using the following formula (7): Oxidation-reduction cycle deterioration rate (%)=100×(cell voltage after oxidation-reduction cycle durability−initial cell voltage) / initial cell voltage (7).
[0128] In Table 2, the oxidation-reduction cycle deterioration rate of less than 5% was evaluated as "good", and the rate of 5% or more was evaluated as "poor".
[0129] After the oxidation-reduction cycle, the cross section of the hydrogen electrode layer and the metal support along the thickness direction was observed using an SEM (magnification: 1000x) at 10 fields of view at 200 μm intervals in the planar direction from each end of the interface between the center of the hydrogen electrode layer and the metal support to check for the presence or absence of interfacial delamination (a portion where the non-bonded region at the interface continued for 50 μm or more in the planar direction).
[0130] In Table 2, the case where peeling was observed in one or more visual fields was judged as "x", and the case where no peeling was observed was judged as "good".
[0131]
[0132] As shown in Table 2, in Examples 6 to 11, in which the Ni content in the first region was lower than the Ni content in the third region in the center of the hydrogen electrode layer, interfacial peeling was suppressed compared to Example 4 after the oxidation-reduction cycle durability evaluation. This result was obtained because the expansion / contraction of the first region due to oxidation-reduction cycles was reduced. Furthermore, in Examples 6 to 11, the electrolytic cell performance in the initial evaluation was improved compared to Example 2. This result was obtained because the electronic conductivity and catalytic performance in the third region were improved. Thus, in Examples 6 to 11, it was possible to achieve both suppression of peeling and maintenance of electrode performance.
[0133] Furthermore, in Examples 9 to 11, in which the Ni content in the second region was lower than the Ni content in the third region in the center of the hydrogen electrode layer, the deterioration rate after the oxidation-reduction cycle durability evaluation was able to be suppressed compared to Examples 1, 4, and 6 to 8. Such results were obtained because the expansion / contraction caused by the oxidation-reduction cycle could be reduced not only in the first region but also in the second region.
[0134] REFERENCE SIGNS LIST 1 electrolysis cell 10 metal support 11 communicating hole 12 first main surface 13 second main surface 20 cell main body 6 hydrogen electrode layer 6a central portion 6b outer peripheral portion 61 first region 62 second region 63 third region 64 fourth region 7 electrolyte layer 8 reaction prevention layer 9 oxygen electrode layer 30 flow path member 30a flow path
Claims
1. An electrochemical cell comprising: a cell body having a first electrode layer, a second electrode layer, and an electrolyte layer disposed between the first electrode layer and the second electrode layer, the first electrode layer including a central portion and an outer peripheral portion surrounding the central portion, the central portion and the outer peripheral portion each containing nickel and an ionically conductive material, and the nickel content in the central portion is lower than the nickel content in the outer peripheral portion.
2. The electrochemical cell according to claim 1, further comprising a metal support for supporting the cell body, the metal support having a main surface on which the first electrode layer is formed and a plurality of communicating holes formed in the main surface.
3. An electrochemical cell as described in claim 1 or 2, further comprising a metal support supporting the cell main body and having a plurality of communicating holes formed in a main surface, wherein the central portion has: a first region within 5 μm of a first surface in contact with the metal support; a second region within 5 μm of a second surface in contact with the electrolyte layer; and a third region between the first region and the second region, wherein the nickel content in the first region is lower than the nickel content in the third region.
4. The electrochemical cell of claim 3, wherein the nickel content in said second region is lower than the nickel content in said third region.
5. The electrochemical cell according to claim 3, wherein the central portion has a fourth region disposed inside at least one of the plurality of communicating holes, and the nickel content in the fourth region is lower than the nickel content in the third region.
Citation Information
Patent Citations
Solid oxide fuel cell
JP2005085524A
Horizontally inclined structure for electrochemical and electronic device
JP2009059699A
Electrochemical device, solid oxide fuel battery cell, and their manufacturing methods
JP2016066616A
Solid oxide fuel cell
WO2011036729A1
Electrolyte layer-anode composite member for fuel cell and method for manufacturing said member
WO2017014069A1