Electrolytic cell

The electrolytic cell's innovative design with varying porosity regions in the oxygen electrode addresses the issue of oxide film growth, enhancing performance by directing oxygen flow and reducing exposure to a strongly oxidizing atmosphere, thus maintaining efficiency.

WO2024201667A1PCT designated stage expired Publication Date: 2024-10-03NGK INSULATORS LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/012264
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional electrolytic cells with metal members experience performance deterioration due to significant oxide film growth on the metal surfaces, especially at the oxygen electrode, caused by concentrated oxygen generation and heat accumulation, leading to a strongly oxidizing atmosphere that hampers efficient operation.

Method used

The electrolytic cell design includes a metal member electrically connected to the oxygen electrode, with a first region near the metal surface having lower porosity and a second region farther away having higher porosity, allowing oxygen generated in the central portion to flow towards the outer peripheral portion, reducing exposure to a strongly oxidizing atmosphere and minimizing oxide film growth.

Benefits of technology

This design effectively suppresses performance deterioration by ensuring oxygen generated in the central portion flows to the outer peripheral portion, reducing oxide film growth on the metal member and maintaining the electrolytic cell's efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023012264_03102024_PF_FP_ABST
    Figure JP2023012264_03102024_PF_FP_ABST
Patent Text Reader

Abstract

An electrolytic cell (1) comprises a cell body (20) and a metal member (25). An oxygen electrode (9) of the cell body (20) has a first region (91) within 5 μm from a metal member-side surface (93). The first region (91) includes a central part (91a) and an outer peripheral part (91b). The porosity of the central part (91a) is smaller than the porosity of the outer peripheral part (91b).
Need to check novelty before this filing date? Find Prior Art

Description

Electrolysis Cell

[0001] The present invention relates to an electrolysis cell.

[0002] Conventionally, there has been known an electrolytic cell having a cell body with an electrolyte disposed between a hydrogen electrode and an oxygen electrode (see, for example, Patent Document 1). A raw material gas is supplied to the hydrogen electrode, and oxygen (O 2 ) is generated.

[0003] Also known is an electrolysis cell in which the cell body is disposed on a metal support (see, for example, Patent Document 2).

[0004] JP 2023-004399 A JP 2020-155337 A

[0005] Here, the electrolytic cell may include a metal member that is in contact with or faces the oxygen electrode. Examples of the metal member include a separator used to stack the electrolytic cells and a current collecting member used for current collection.

[0006] When the electrolytic cell includes a metal member, oxygen generated at the oxygen electrode may cause a significant oxide film to grow on the surface of the metal member.

[0007] Specifically, in the center of the cathode when viewed from above, the amount of oxygen generated tends to increase due to current concentration caused by a temperature rise due to heat buildup. In addition, since the oxygen generated in the center is difficult to discharge to the outside of the stack, the portion of the metal member that contacts or faces the center of the cathode is exposed to a strongly oxidizing atmosphere. As a result, the performance of the electrolysis cell deteriorates due to the significant growth of an oxide film on the portion of the metal member that contacts or faces the center of the cathode.

[0008] An object of the present invention is to provide an electrolysis cell capable of suppressing performance degradation.

[0009] An electrolysis cell according to a first aspect of the present invention comprises a cell main body and a metal member. The cell main body has a hydrogen electrode, an oxygen electrode, and an electrolyte disposed between the hydrogen electrode and the oxygen electrode. The metal member is electrically connected to the oxygen electrode. The oxygen electrode has a first region within 5 μm from the surface of the metal member and a second region more than 5 μm from the surface of the metal member. The first region includes a central portion and an outer peripheral portion surrounding the central portion. The porosity of the central portion is smaller than the porosity of the outer peripheral portion.

[0010] An electrolysis cell according to a second aspect of the present invention is the electrolysis cell according to the first aspect, wherein the porosity of the second region is greater than the porosity of the central portion.

[0011] According to the present invention, it is possible to provide an electrolysis cell that can suppress performance degradation.

[0012] Fig. 1 is a plan view of an electrolysis cell according to an embodiment, and Fig. 2 is a cross-sectional view taken along line AA in Fig. 1.

[0013] (Electrolytic cell 1) Fig. 1 is a plan view of an electrolytic cell 1 according to an embodiment. Fig. 2 is a cross-sectional view taken along line A-A in Fig. 1. Fig. 2 shows a cross section passing through the geometric center CP of the oxygen electrode 9, which will be described later. However, the metal member 25 is omitted from Fig. 1.

[0014] The electrolytic cell 1 is a so-called metal-supported electrolytic cell.

[0015] The electrolytic cell 1 is formed in a plate shape extending in the X-axis and Y-axis directions. In the present embodiment, the electrolytic cell 1 is formed in a rectangular shape extending in the Y-axis direction when viewed in a plan view from the Z-axis direction perpendicular to the X-axis and Y-axis directions. However, the planar shape of the electrolytic cell 1 is not particularly limited, and may be a polygon other than a rectangle, an ellipse, a circle, or the like.

[0016] The X-axis direction and the Y-axis direction are the surface directions of the electrolytic cell 1, and the Z-axis direction is the thickness direction of the electrolytic cell 1.

[0017] As shown in FIG. 2 , the electrolysis cell 1 includes a metal support 10 , a cell main body 20 , a metal member 25 , and a flow path member 30 .

[0018] [Metal Support 10] The metal support 10 supports the cell main body 20. The metal support 10 is formed in a plate shape. The metal support 10 may be in the shape of a flat plate or a curved plate.

[0019] The metal support 10 may have any thickness as long as it can support the cell body 20. The thickness is not particularly limited, but may be, for example, 0.1 mm or more and 2.0 mm or less. The thermal expansion coefficient of the metal support 10 is not particularly limited, but may be, for example, 10×10 ―6 / ℃ or more 18 x 10 ―6 / °C or less.

[0020] As shown in FIG. 2 , the metal support 10 has a plurality of through holes 11 , a first main surface 12 and a second main surface 13 .

[0021] Each communication hole 11 penetrates the metal support 10 from the first main surface 12 to the second main surface 13. Each communication hole 11 opens to the first main surface 12 and the second main surface 13. The opening of each communication hole 11 on the first main surface 12 side is covered by the hydrogen electrode 6. The opening of each communication hole 11 on the second main surface 13 side is connected to a flow path 30a, which will be described later.

[0022] Each of the communication holes 11 can be formed by mechanical processing (for example, punching), laser processing, or chemical processing (for example, etching).

[0023] In this embodiment, each communication hole 11 is formed linearly along the Z-axis direction. However, each communication hole 11 may be inclined with respect to the Z-axis direction, or may not be linear. Furthermore, the communication holes 11 may be connected to each other.

[0024] The first main surface 12 is provided on the opposite side to the second main surface 13. The cell main body 20 is disposed on the first main surface 12. The flow path member 30 is bonded to the second main surface 13.

[0025] The metal support 10 is made of a metal material. For example, the metal support 10 is made of an alloy material containing Cr (chromium). Examples of such metal materials include Fe—Cr alloy steel (stainless steel, etc.) and Ni—Cr alloy steel. The Cr content in the metal support 10 is not particularly limited, but can be set to 4% by mass or more and 30% by mass or less.

[0026] The metal support 10 may contain Ti (titanium) or Zr (zirconium). The Ti content in the metal support 10 is not particularly limited, but may be 0.01 mol % or more and 1.0 mol % or less. The Al content in the metal support 10 is not particularly limited, but may be 0.01 mol % or more and 0.4 mol % or less. The metal support 10 may contain Ti in the form of TiO 2 (titania), or Zr may be contained as ZrO 2 It may be contained as (zirconia).

[0027] The metal support 10 may have an oxide film on its surface, which is formed by oxidation of the constituent elements of the metal support 10. A typical example of the oxide film is a chromium oxide film. The chromium oxide film covers at least a portion of the surface of the metal support 10. The chromium oxide film may also cover at least a portion of the inner wall surface of each communicating hole 11.

[0028] [Cell Body 20] The cell body 20 is disposed on the metal support 10. The cell body 20 is supported by the metal support 10. The cell body 20 has a hydrogen electrode 6 (cathode), an electrolyte 7, a reaction prevention layer 8, and an oxygen electrode 9 (anode).

[0029] The hydrogen electrode 6, electrolyte 7, reaction prevention layer 8, and oxygen electrode 9 are stacked in this order in the Z-axis direction from the metal support 10 side. The hydrogen electrode 6, electrolyte 7, and oxygen electrode 9 are essential components, while the reaction prevention layer 8 is optional.

[0030] [Hydrogen Electrode 6] The hydrogen electrode 6 is disposed between the metal support 10 and the electrolyte 7. The hydrogen electrode 6 is formed on the first main surface 12 of the metal support 10. In this embodiment, a portion of the hydrogen electrode 6 is disposed inside each of the communicating holes 11 of the metal support 10, but the hydrogen electrode 6 does not have to extend into each of the communicating holes 11 of the metal support 10.

[0031] A source gas is supplied to the hydrogen electrode 6 through each of the communication holes 11. The source gas contains at least H 2 Contains O.

[0032] The raw material gas is H 2 When the raw material gas contains only O, the hydrogen electrode 6 converts H 2 Generate.

[0033] Hydrogen electrode 6: H 2 O + 2e - →H 2 +O 2- ...(1)

[0034] The raw material gas is H 2 O plus CO 2 In this case, the hydrogen electrode 6 converts the raw material gas into H according to the electrochemical reactions of co-electrolysis shown in the following formulas (2), (3), and (4). 2 , CO and O 2- Generate.

[0035] Hydrogen electrode 6: CO 2 +H 2 O+4e - →CO+H 2 +20 2- ... (2) H 2 Electrochemical reaction of O: H 2 O + 2e - →H 2 +O 2- ... (3) CO 2 Electrochemical reaction of: CO 2 +2e - →CO+O 2- ...(4)

[0036] The hydrogen electrode 6 is an electron-conductive porous body containing nickel (Ni) and an oxide ion conductive material.

[0037] Ni acts as an electron conductor. In the case of co-electrolysis, Ni acts as an electron conductor. 2 and CO contained in the raw material gas 2 It also functions as a thermal catalyst that promotes the thermal reaction with Ni and maintains an appropriate gas composition for methanation, reverse water gas shift reaction, etc. Ni exists in the form of nickel oxide (NiO) in an oxidizing atmosphere and in the form of metallic Ni in a reducing atmosphere.

[0038] Examples of oxide ion conductive materials include YSZ, CSZ, ScSZ, GDC, SDC, and (La, Sr)(Cr, Mn)O. 3 , (La,Sr)TiO 3 , Sr 2 (Fe, Mo) 2 O 6 , (La, Sr)VO 3 , (La,Sr)FeO 3 and mixed materials of two or more of these.

[0039] The thickness of the hydrogen electrode 6 is not particularly limited, but can be, for example, 1 μm or more and 100 μm or less.

[0040] The method for forming the hydrogen electrode 6 is not particularly limited, and may be a firing method, a spray coating method (such as a thermal spraying method, an aerosol deposition method, an aerosol gas deposition method, a powder jet deposition method, a particle jet deposition method, or a cold spray method), a PVD method (such as a sputtering method or a pulsed laser deposition method), or a CVD method.

[0041] [Electrolyte 7] The electrolyte 7 is disposed between the hydrogen electrode 6 and the oxygen electrode 9. In this embodiment, the reaction prevention layer 8 is disposed between the electrolyte 7 and the oxygen electrode 9, and therefore the electrolyte 7 is sandwiched between the hydrogen electrode 6 and the reaction prevention layer 8.

[0042] The electrolyte 7 covers the hydrogen electrode 6 and also covers the region of the first main surface 12 of the metal support 10 that is exposed from the hydrogen electrode 6 .

[0043] The electrolyte 7 contains the O produced at the hydrogen electrode 6. 2-The electrolyte 7 is configured from a dense material having oxide ion conductivity. The electrolyte 7 can be configured from, for example, YSZ (yttria-stabilized zirconia, e.g., 8YSZ), GDC (gadolinium-doped ceria), ScSZ (scandia-stabilized zirconia), SDC (samarium-doped ceria), LSGM (lanthanum gallate), or the like.

[0044] The porosity of the electrolyte 7 is not particularly limited, but may be, for example, 0.1% to 7%. The thickness of the electrolyte 7 is not particularly limited, but may be, for example, 1 μm to 100 μm.

[0045] The method for forming the electrolyte 7 is not particularly limited, and may be a baking method, a spray coating method, a PVD method, a CVD method, or the like.

[0046] [Reaction prevention layer 8] The reaction prevention layer 8 is disposed between the electrolyte 7 and the oxygen electrode 9. The reaction prevention layer 8 is disposed on the opposite side of the electrolyte 7 from the hydrogen electrode 6. The reaction prevention layer 8 prevents the constituent elements of the electrolyte 7 from reacting with the constituent elements of the oxygen electrode 9 to form a layer with high electrical resistance.

[0047] The reaction prevention layer 8 is made of an oxide ion conductive material, such as GDC or SDC.

[0048] The porosity of the reaction prevention layer 8 is not particularly limited, but may be, for example, 0.1% to 50%. The thickness of the reaction prevention layer 8 is not particularly limited, but may be, for example, 1 μm to 50 μm.

[0049] The method for forming the reaction prevention layer 8 is not particularly limited, and may be a baking method, a spray coating method, a PVD method, a CVD method, or the like.

[0050] [Oxygen Electrode 9] The oxygen electrode 9 is disposed on the opposite side of the hydrogen electrode 6 with respect to the electrolyte 7. In this embodiment, the reaction prevention layer 8 is disposed between the electrolyte 7 and the oxygen electrode 9, and therefore the oxygen electrode 9 is connected to the reaction prevention layer 8. If the reaction prevention layer 8 is not disposed between the electrolyte 7 and the oxygen electrode 9, the oxygen electrode 9 is connected to the electrolyte 7.

[0051] The oxygen electrode 9 has a surface 93 on the metal member 25 side (hereinafter referred to as the "metal member side surface").

[0052] The oxygen electrode 9 converts O 2 transferred from the hydrogen electrode 6 through the electrolyte 7 according to the chemical reaction of the following formula (5): 2- to oxygen (O 2 ) to generate the

[0053] Oxygen electrode 9:2O 2- →O 2 +4e - ...(5)

[0054] The porosity of the oxygen electrode 9 is not particularly limited, but may be, for example, 20% to 60%. The thickness of the oxygen electrode 9 is not particularly limited, but may be, for example, 1 μm to 100 μm. The detailed configuration of the oxygen electrode 9 will be described later.

[0055] The method for forming the oxygen electrode 9 is not particularly limited, and may be a baking method, a spray coating method, a PVD method, a CVD method, or the like.

[0056] [Metal Member 25] The metal member 25 is electrically connected to the oxygen electrode 9. In this embodiment, the metal member 25 is electrically connected to the oxygen electrode 9 via a conductive bonding material 26. However, the metal member 25 may also be electrically connected to the oxygen electrode 9 by direct contact with the oxygen electrode 9. In this case, the metal member 25 does not need to be fixed to the oxygen electrode 9.

[0057] The metal member 25 according to this embodiment functions as a current collecting member and is electrically connected to an interconnector 32 (described later) provided in another electrolysis cell.

[0058] The metal member 25 may be made of, for example, ferritic stainless steel, but there is no particular limitation on the material of the metal member 25. The surface of the metal member 25 may be covered with a conductive coating.

[0059] At least a portion of the surface of the metal member 25 may be covered with an oxide film formed by oxidation of the constituent elements of the metal member 25. A typical example of the oxide film is a chromium oxide film. When an oxide film is present, the oxide film constitutes a part of the metal member 25.

[0060] Furthermore, at least a portion of the surface of the metal member 25, or at least a portion of the oxide film covering the surface of the metal member 25, may be covered with an oxidation-resistant coating film. A typical example of the oxidation-resistant coating film is a manganese-cobalt composite oxide film. In this embodiment, the oxide film constitutes a part of the metal member 25. When an oxidation-resistant coating film is present, the oxidation-resistant coating film constitutes a part of the metal member 25.

[0061] Although the oxidation-resistant coating film can suppress oxidation of the metal member 25, it is generally difficult for the oxidation-resistant coating film to completely prevent oxidation of the metal member 25. In particular, when the metal member 25 is exposed to a strongly oxidizing atmosphere, the oxidation of the metal member 25 cannot be completely prevented even if an oxidation-resistant coating film is formed, and an oxide film grows on the surface of the metal member 25.

[0062] [Flow Channel Member 30] The flow channel member 30 is joined to the second main surface 13 of the metal support 10. The flow channel member 30 forms a flow channel 30a between itself and the metal support 10. A source gas is supplied to the flow channel 30a. The source gas supplied to the flow channel 30a is supplied to the hydrogen electrode 6 of the cell main body 20 via each communication hole 11 of the metal support 10.

[0063] The flow path member 30 can be made of, for example, an alloy material. The flow path member 30 may be made of the same material as the metal support 10. In this case, the flow path member 30 may be substantially integrated with the metal support 10.

[0064] The flow path member 30 has a frame 31 and an interconnector 32. The frame 31 is an annular member that surrounds the side of the flow path 30a. The frame 31 is joined to the second main surface 13 of the metal support 10. The interconnector 32 is a plate-like member for electrically connecting an external power source or another electrolytic cell to the electrolytic cell 1 in series. The interconnector 32 is joined to the frame 31.

[0065] In this embodiment, the frame body 31 and the interconnector 32 are separate members, but the frame body 31 and the interconnector 32 may be an integrated member.

[0066] 2 , the oxygen electrode 9 has a first region 91 and a second region 92. The first region 91 is a region of the oxygen electrode 9 that is within 5 μm from the surface 93 of the oxygen electrode 9 that faces the metal member. The second region 92 is a region of the oxygen electrode 9 that is more than 5 μm from the surface 93 of the oxygen electrode 9 that faces the metal member. In other words, the second region 92 is a region of the oxygen electrode 9 excluding the first region 91.

[0067] The first region 91 is made of a porous material having electron conductivity, such as (La, Sr)(Co, Fe)O. 3 , (La,Sr)FeO 3 , La(Ni,Fe)O 3 , (La,Sr)CoO 3 , (Sm,Sr)CoO 3 , La(Ni,Fe,Cu)O 3 , (La,Sr)MnO 3 The first region 91 may further include an oxide ion conductive material (such as GDC).

[0068] The second region 92 is made of a porous material having electron conductivity. The first region 91 is made of, for example, (La, Sr)(Co, Fe)O 3 , (La,Sr)FeO 3 , La(Ni,Fe)O 3 , (La,Sr)CoO 3 , (Sm,Sr)CoO 3 , La(Ni,Fe,Cu)O 3 , (La,Sr)MnO 3The second region 92 may further include an oxide ion conductive material (such as GDC).

[0069] The composition of the first region 91 may be the same as or different from the composition of the second region 92 .

[0070] As shown in FIG. 2, the first region 91 has a central portion 91a and an outer peripheral portion 91b.

[0071] The central portion 91a is a portion including the geometric center CP of the oxygen electrode 9 in a planar view. In this embodiment, as shown in FIG. 1 , the planar shape of the oxygen electrode 9 in a planar view is rectangular, and the planar shape of the central portion 91a in a planar view is also rectangular. In a planar view, the central portion 91a is located inside the oxygen electrode 9. The planar shape of the central portion 91a is similar to the planar shape of the oxygen electrode 9. That is, when the outer edge of the central portion 91a is enlarged by a predetermined magnification, the outer edge of the central portion 91a and the outer edge of the oxygen electrode 9 become congruent. The predetermined magnification is not particularly limited, but can be, for example, 1.2 times or more and 4 times or less. In this embodiment, the predetermined magnification is 2.0 times, and when the outer edge of the central portion 91a is enlarged by 2 times, it becomes congruent with the outer edge of the oxygen electrode 9.

[0072] However, as long as the central portion 91a includes the geometric center CP, the planar shape and size of each of the oxygen electrode 9 and the central portion 91a can be changed as appropriate. Therefore, the planar shapes of the oxygen electrode 9 and the central portion 91a may each be a shape other than a rectangle (for example, a polygon other than a rectangle, an ellipse, a circle, etc.). Furthermore, the planar shape of the central portion 91a may be different from the planar shape of the oxygen electrode 9. The total area of ​​the oxygen electrode 9 in a planar view can be 1.44 to 16 times the area of ​​the central portion 91a in a planar view.

[0073] The outer peripheral portion 91b is a portion that surrounds the central portion 91a in a plan view. The outer peripheral portion 91b is formed in an annular shape in a plan view. The planar shape of the outer peripheral portion 91b can be appropriately changed depending on the planar shapes of the oxygen electrode 9 and the central portion 91a.

[0074] Here, the porosity of the central portion 91a is smaller than the porosity of the outer peripheral portion 91b. This prevents the significant growth of an oxide film on the metal member 25. Specifically, this is as follows. In the oxygen electrode 9, heat tends to accumulate in the central portion 92a (see FIG. 2 ) of the second region 92, which contacts the central portion 91a of the first region 91. Therefore, a large amount of oxygen is generated in the central portion 92a due to current concentration caused by a temperature increase. However, because the porosity of the central portion 91a is smaller than the porosity of the outer peripheral portion 91b, the oxygen generated in the central portion 92a tends to flow toward the outer peripheral portion 91b rather than the central portion 91a. This prevents the large amount of oxygen generated in the central portion 92a from being released from the central portion 91a, thereby preventing the portion of the metal member 25 in contact with the central portion 91a from being exposed to a strongly oxidizing atmosphere. As a result, it is possible to suppress a decrease in performance of the electrolysis cell 1 due to a significant growth of an oxide film on the portion of the metal member 25 that contacts the central portion 91a.

[0075] The porosity of the second region 92 is preferably greater than the porosity of the central portion 91 a. This allows oxygen generated in the central portion 92 a of the second region 92 to more easily flow toward the outer circumferential portion 91 b. Therefore, the growth of an oxide film on the portion of the metal member 25 that contacts the central portion 91 a can be further suppressed.

[0076] The porosity of the central portion 91a is not particularly limited, but may be, for example, 20% to 40%. The porosity of the outer peripheral portion 91b is not particularly limited, but may be, for example, 25% to 45%.

[0077] The porosity of the second region 92 is not particularly limited, but can be, for example, 20% or more and 45% or less.

[0078] The porosity of the central portion 91a of the first region 91 is calculated by the following method. First, a cross section of the central portion 91a along the Z-axis direction is exposed. Next, a backscattered electron image of the cross section of the central portion 91a is acquired at 10,000x magnification using an SEM device (FE-SEM JSM-7900F, manufactured by JEOL Ltd.). Next, using image analysis software Image-Pro manufactured by MEDIACYBERNETICS, the areas displayed in black in the backscattered electron image (corresponding to pores) are identified. The porosity of the central portion 91a is then calculated by dividing the total area of ​​the pores by the total area of ​​the backscattered electron image of the central portion 91a.

[0079] The porosity of the outer peripheral portion 91b of the first region 91 is calculated by dividing the total area of ​​the pores by the total area of ​​the backscattered electron image of the outer peripheral portion 91b, similar to the porosity of the central portion 91a.

[0080] The porosity of the second region 92 is calculated by dividing the total area of ​​the pores by the total area of ​​the backscattered electron image of the second region 92, similar to the porosity of the central portion 91a.

[0081] The oxygen electrode 9 is fabricated by forming a second region 92 on the reaction prevention layer 8 using a constituent material for the second region, then forming a central portion 91a on the second region 92 using a constituent material for the central portion of the first region 91, and further forming a peripheral portion 91b surrounding the central portion 91a using a constituent material for the peripheral portion of the first region 91.

[0082] The porosity of each of the central portion 91a of the first region 91, the peripheral portion 91b of the first region 91, and the second region 92 can be adjusted by the amount of pore-forming material added, the particle size of the raw material powder, the material composition, and the type of material, but adjustment by the amount of pore-forming material added is preferred because it has little impact on electrode performance.

[0083] (Modifications of the Embodiment) Although the embodiment of the present invention has been described above, the present invention is not limited to these, and various modifications are possible without departing from the spirit of the present invention.

[0084] [Variation 1] In the above embodiment, the metal member 25 functions as a current collecting member, but this is not limiting. The metal member 25 may be electrically connected to the air electrode 9. For example, the metal member 25 may be an interconnector 32 provided in another electrolysis cell.

[0085] [Modification 2] In the above embodiment, the metal-supported electrolytic cell 1 has been described as an example of an electrolytic cell. However, the electrolytic cell according to the present invention may be a flat-plate type that does not include a metal support 10.

[0086] Examples of the electrochemical cell according to the present invention will be described below, but the present invention is not limited to the examples described below.

[0087] Comparative Examples 1 and 2 Electrolytic cells according to Comparative Examples 1 and 2 were prepared as follows.

[0088] First, a metal support made of Fe-Cr-Mn alloy steel and having a plurality of communicating holes formed therein was prepared.

[0089] Next, a slurry for the hydrogen electrode layer was prepared by mixing GDC powder, NiO powder, butyral resin, polymethyl methacrylate beads as a pore-forming material, a plasticizer, a dispersant, and a solvent, and the slurry for the hydrogen electrode layer was then printed onto the first main surface of the metal support by a doctor blade method to form a green body for the hydrogen electrode layer.

[0090] Next, a slurry for the electrolyte layer was prepared by mixing YSZ powder, butyral resin, a plasticizer, a dispersant, and a solvent, and then the slurry for the electrolyte was printed by a doctor blade method so as to cover the green body for the hydrogen electrode layer, thereby forming a green body for the electrolyte layer.

[0091] Next, a slurry for the reaction prevention layer was prepared by mixing GDC powder, polyvinyl alcohol, and a solvent, and the slurry for the reaction prevention layer was then printed on the green body of the electrolyte layer by a doctor blade method to form a green body of the reaction prevention layer.

[0092] Next, the molded bodies of the hydrogen electrode layer, electrolyte layer, and reaction prevention layer arranged in this order on the metal support were fired in air (1050°C, 1 hour) to form the hydrogen electrode layer, electrolyte layer, and reaction prevention layer.

[0093] Next, (La,Sr)(Co,Fe)O 3 The powder, polyvinyl alcohol, solvent, and pore-forming material were mixed to prepare a slurry for the oxygen electrode layer. The amount of pore-forming material added was adjusted to change the porosity of the entire oxygen electrode for each comparative example, as shown in Table 1. The slurry for the oxygen electrode layer was then printed on the reaction prevention layer by a doctor blade method to form a green body for the oxygen electrode layer.

[0094] Next, the compact for the oxygen electrode layer was fired in air (1000° C., 1 hour) to form an oxygen electrode.

[0095] Finally, a metal member and a current plate were attached in this order on the oxygen electrode layer, and a current wire was attached to the metal support.

[0096] Examples 1 to 7 Electrolytic cells according to Examples 1 to 7 were fabricated using the same steps as those of Comparative Examples 1 and 2, except that the oxygen electrode layer had a two-layer structure.

[0097] Specifically, (La,Sr)(Co,Fe)O 3 A slurry for the second region was prepared by mixing the powder, polyvinyl alcohol, a solvent, and a pore-forming material. The amount of pore-forming material added was adjusted to change the porosity of the second region of the oxygen electrode for each example, as shown in Table 1. The slurry for the second region was then printed on the reaction prevention layer by a doctor blade method to form a compact for the second region of the oxygen electrode.

[0098] Next, (La,Sr)(Co,Fe)O 3A slurry for the central portion of the first region was prepared by mixing the powder, polyvinyl alcohol, a solvent, and a pore-forming material. The amount of pore-forming material added was adjusted to change the porosity of the central portion of the first region of the oxygen electrode for each example, as shown in Table 1. The slurry for the central portion of the first region was then printed on the central portion of the green body for the second region by a doctor blade method, thereby forming a green body for the central portion of the first region of the oxygen electrode.

[0099] Next, (La,Sr)(Co,Fe)O 3 A slurry for the outer periphery of the first region was prepared by mixing the powder, polyvinyl alcohol, a solvent, and a pore-forming material. The amount of pore-forming material added was adjusted to change the porosity of the outer periphery of the first region of the oxygen electrode for each example, as shown in Table 1. The slurry for the outer periphery of the first region was then printed by a doctor blade method so as to surround the compact for the first region, thereby forming a compact for the outer periphery of the first region of the oxygen electrode.

[0100] Next, the compacts of the first and second regions were fired in air (1000° C., 1 hour) to form an oxygen electrode.

[0101] (Durability Evaluation) First, the electrolytic cells of Examples 1 to 7 and Comparative Examples 1 and 2 were heated to 700°C, and hydrogen was supplied to the hydrogen electrode layer while air was supplied to the oxygen electrode layer, thereby reducing NiO contained in the hydrogen electrode layer to Ni.

[0102] Next, a mixed gas of water vapor and hydrogen (mixing ratio 90:10) was supplied to the hydrogen electrode layer, while a mixed gas of oxygen and nitrogen (mixing ratio 21:79) was supplied to the oxygen electrode layer, and the current density per hydrogen electrode layer area was 0.5 A / cm 2 The cell voltage when electrolysis was performed by passing a current so as to be constant at 1000 kJ / min (hereinafter referred to as "initial cell voltage") was measured.

[0103] Subsequently, the current density was increased to 0.5 A / cm while supplying the mixed gas to each of the hydrogen electrode layer and the oxygen electrode layer. 2 The cell voltage after being held in a fixed state for 1000 hours (hereinafter referred to as "cell voltage after durability") was measured.

[0104] Then, the performance degradation rate was calculated using the following formula (6).

[0105] Performance degradation rate (%) = 100 × (cell voltage after endurance test - initial cell voltage) / initial cell voltage (6) In Table 1, a performance degradation rate of less than 4% was evaluated as "◎", a rate of 4% or more but less than 7% was evaluated as "◯", and a rate of 7% or more was evaluated as "×".

[0106]

[0107] As shown in Table 1, in Examples 1 to 7, in which the porosity of the central part of the first region in the oxygen electrode layer was made smaller than the porosity of the peripheral part of the first region, the performance degradation rate was lower than in Comparative Examples 1 and 2. This result was obtained because the significant growth of an oxide film on the metal member was suppressed by flowing oxygen generated in the second region to the peripheral part of the first region.

[0108] Furthermore, in Examples 6 and 7, in which the porosity of the second region in the oxygen electrode layer was made larger than the porosity of the central part of the first region, the performance degradation rate was lower than in Examples 1 to 5. This result was obtained because oxygen generated in the second region was able to flow more easily to the outer periphery of the first region.

[0109] REFERENCE SIGNS LIST 1 electrolysis cell 10 metal support 11 communicating hole 12 first main surface 13 second main surface 20 cell main body 6 hydrogen electrode 7 electrolyte 8 reaction prevention layer 9 oxygen electrode 91 first region 91a central portion 91b outer peripheral portion 92 second region 92a central portion 30 flow path member 30a flow path

Claims

1. An electrolytic cell comprising: a cell body having a hydrogen electrode, an oxygen electrode, and an electrolyte disposed between the hydrogen electrode and the oxygen electrode; and a metal member electrically connected to the oxygen electrode, wherein the oxygen electrode has a first region within 5 μm from a surface of the metal member and a second region more than 5 μm from the surface of the metal member, the first region including a central portion and an outer peripheral portion surrounding the central portion, and the porosity of the central portion is smaller than the porosity of the outer peripheral portion.

2. An electrolytic cell, wherein the porosity of the second region is greater than the porosity of the central portion.

Citation Information

Patent Citations

  • Flame splaying electrode material of solid electrolyte type electrolytic cell

    JP1995057737A

  • Solid oxide electrochemical cell and production method therefor

    WO2018198352A1

  • Cell, cell stack device, module, and module accommodating device

    WO2022045141A1