Electrochemical cell
The integration of a conductive gas diffusion layer with increased porosity and smaller pores addresses the inefficiencies in gas supply to the first electrode layer, improving gas distribution and cell performance in electrochemical cells.
Patent Information
- Application Number
- PCT/JP2023/013527
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional electrochemical cells face limitations in efficiently supplying gas to the first electrode layer due to inadequate gas diffusivity within the bonding layer, resulting in localized gas supply.
Incorporating a conductive gas diffusion layer with a higher porosity and smaller pore diameters than the first electrode layer, along with a greater number of pores per unit area, to enhance gas diffusion and distribution to the first electrode layer.
This configuration allows for efficient gas supply and diffusion to the first electrode layer, improving overall gas distribution and utilization, thereby enhancing the performance of the electrochemical cell.
Smart Images

Figure JP2023013527_03102024_PF_FP_ABST
Abstract
Description
electrochemical cell
[0001] The present invention relates to electrochemical cells.
[0002] Conventionally, electrochemical cells (electrolysis cells, fuel cells, etc.) have been known that include a cell body disposed on a metal support. The metal support has a plurality of through-holes formed in a main surface. The cell body is formed on the main surface of the metal support and includes a first electrode layer covering the through-holes, a second electrode layer, and an electrolyte layer disposed between the first and second electrode layers.
[0003] Patent Document 1 discloses a fuel cell having a bonding layer interposed between a metal support and a first electrode layer, and describes that forming through holes in the bonding layer that communicate with the communicating holes in the metal support makes it easier to supply gas from the communicating holes to the first electrode layer.
[0004] Japanese Patent Application Laid-Open No. 2020-079189
[0005] However, in Patent Document 1, gas diffusibility within the bonding layer is not considered, and therefore there is a limit to how easily gas can be supplied to the first electrode layer from the communicating holes.
[0006] That is, simply supplying gas to the first electrode layer from the communication holes via the through holes formed in the bonding layer only allows the gas to be supplied locally to the first electrode layer.
[0007] In order to efficiently supply gas to the first electrode layer, it is important that the gas supplied from the communication holes is diffused within the bonding layer.
[0008] An object of the present invention is to provide an electrochemical cell that can efficiently supply gas to a first electrode layer.
[0009] An electrochemical cell according to a first aspect of the present invention includes a metal support having a plurality of communicating holes formed in a main surface thereof, and a cell body portion disposed on the main surface. The cell body portion includes a conductive gas diffusion layer disposed on the main surface, a first electrode layer and a second electrode layer disposed on the gas diffusion layer, and an electrolyte layer disposed between the first and second electrode layers. The gas diffusion layer includes a plurality of first pores, and the first electrode layer includes a plurality of second pores. The average equivalent circular diameter of the first pores is smaller than the average equivalent circular diameter of the second pores. The porosity of the gas diffusion layer is larger than the porosity of the first electrode layer.
[0010] An electrochemical cell according to a second aspect of the present invention is the electrochemical cell according to the first aspect, wherein the number of first pores per unit area is greater than the number of second pores per unit area.
[0011] According to a third aspect of the present invention, there is provided an electrochemical cell according to the first or second aspect, wherein the gas diffusion layer includes a plurality of first conductive particles, the first electrode layer includes a plurality of second conductive particles, and the average neck diameter between the first conductive particles is smaller than the average neck diameter between the second conductive particles.
[0012] According to the present invention, it is possible to provide an electrochemical cell that can efficiently supply gas to the first electrode layer.
[0013] Fig. 1 is a plan view of an electrolysis cell according to an embodiment, Fig. 2 is a cross-sectional view taken along line AA in Fig. 1, and Fig. 2 is a partially enlarged view of Fig. 2.
[0014] (Electrolytic cell 1) Fig. 1 is a plan view of an electrolytic cell 1 according to an embodiment. Fig. 2 is a cross-sectional view taken along line AA in Fig. 1.
[0015] The electrolytic cell 1 is an example of an "electrochemical cell" according to the present invention. The electrolytic cell 1 is a so-called metal-supported electrolytic cell.
[0016] The electrolytic cell 1 is formed in a plate shape extending in the X-axis and Y-axis directions. In the present embodiment, the electrolytic cell 1 is formed in a rectangular shape extending in the Y-axis direction when viewed in a plan view from the Z-axis direction perpendicular to the X-axis and Y-axis directions. However, the planar shape of the electrolytic cell 1 is not particularly limited, and may be a polygon other than a rectangle, an ellipse, a circle, or the like.
[0017] As shown in FIG. 2 , the electrolysis cell 1 includes a metal support 10 , a cell main body 20 , and a flow path member 30 .
[0018] [Metal Support 10] The metal support 10 supports the cell main body 20. The metal support 10 is formed in a plate shape. The metal support 10 may be in the shape of a flat plate or a curved plate.
[0019] The metal support 10 is only required to be able to support the electrolysis cell 1, and its thickness is not particularly limited, but can be, for example, 0.1 mm or more and 2.0 mm or less.
[0020] As shown in FIG. 2 , the metal support 10 has a plurality of through holes 11 , a first main surface 12 and a second main surface 13 .
[0021] Each communication hole 11 penetrates the metal support 10 from the first main surface 12 to the second main surface 13. Each communication hole 11 opens to the first main surface 12 and the second main surface 13. In this embodiment, the opening of each communication hole 11 on the first main surface 12 side is covered by a gas diffusion layer 5 described later. The opening of each communication hole 11 on the second main surface 13 side is connected to a flow path 30a described later.
[0022] Each of the communication holes 11 can be formed by mechanical processing (for example, punching), laser processing, or chemical processing (for example, etching).
[0023] In this embodiment, each communication hole 11 is formed linearly along the Z-axis direction. However, each communication hole 11 may be inclined with respect to the Z-axis direction, or may not be linear. Furthermore, the communication holes 11 may be connected to each other.
[0024] The first main surface 12 is provided on the opposite side to the second main surface 13. The cell main body 20 is disposed on the first main surface 12. The flow path member 30 is bonded to the second main surface 13.
[0025] The metal support 10 is made of a metal material. For example, the metal support 10 is made of an alloy material containing Cr (chromium). Examples of such metal materials include Fe—Cr alloy steel (stainless steel, etc.) and Ni—Cr alloy steel. The Cr content in the metal support 10 is not particularly limited, but can be set to 4% by mass or more and 30% by mass or less.
[0026] The metal support 10 may contain Ti (titanium) or Zr (zirconium). The Ti content in the metal support 10 is not particularly limited, but may be 0.01 mol % or more and 1.0 mol % or less. The Al content in the metal support 10 is not particularly limited, but may be 0.01 mol % or more and 0.4 mol % or less. The metal support 10 may contain Ti in the form of TiO 2 (titania), or Zr may be contained as ZrO 2 It may be contained as (zirconia).
[0027] The metal support 10 may have an oxide film on its surface, which is formed by oxidation of the constituent elements of the metal support 10. A typical example of the oxide film is a chromium oxide film. The chromium oxide film covers at least a portion of the surface of the metal support 10. The chromium oxide film may also cover at least a portion of the inner wall surface of each communicating hole 11.
[0028] [Cell Body 20] The cell body 20 is disposed on the metal support 10. The cell body 20 is supported by the metal support 10. The cell body 20 has a gas diffusion layer 5, a hydrogen electrode layer 6 (cathode), an electrolyte layer 7, a reaction prevention layer 8, and an oxygen electrode layer 9 (anode).
[0029] The gas diffusion layer 5, hydrogen electrode layer 6, electrolyte layer 7, reaction prevention layer 8, and oxygen electrode layer 9 are stacked in this order in the Z-axis direction from the metal support 10 side. The gas diffusion layer 5, hydrogen electrode layer 6, electrolyte layer 7, and oxygen electrode layer 9 are essential components, while the reaction prevention layer 8 is optional.
[0030] [Gas Diffusion Layer 5] The gas diffusion layer 5 is formed on the first main surface 12 of the metal support 10. In this embodiment, the gas diffusion layer 5 covers each of the communicating holes 11 of the metal support 10. A portion of the gas diffusion layer 5 may extend inside each of the communicating holes 11 of the metal support 10.
[0031] The gas diffusion layer 5 is a porous body having electrical conductivity. The gas diffusion layer 5 has gas diffusibility. The gas diffusion layer 5 supplies the source gas supplied from each of the communication holes 11 to the hydrogen electrode layer 6, and discharges the product gas generated in the hydrogen electrode layer 6 to each of the communication holes 11.
[0032] The gas diffusion layer 5 includes a conductive material, such as a metal material such as Ni (nickel) or Fe (iron), or a conductive ceramic material.
[0033] The gas diffusion layer 5 may include a substrate that supports a conductive material. The substrate may be insulating. Examples of the substrate include YSZ, CSZ, ScSZ, GDC, SDC, and (La, Sr)(Cr, Mn)O. 3 , (La,Sr)TiO 3 , Sr 2 (Fe, Mo) 2 O 6 , (La, Sr)VO 3 , (La,Sr)FeO 3 , LDC (lanthanum doped ceria), LSGM (lanthanum gallate), and a mixed material of two or more of these can be used.
[0034] The gas diffusion layer 5 may contain the metal element contained in the metal support 10. This is preferable because it improves the adhesion between the gas diffusion layer 5 and the metal support 10. Note that the above-mentioned conductive material is different from the metal element contained in the metal support 10. Therefore, the conductive material contained in the gas diffusion layer 5 does not need to be contained in the metal support 10.
[0035] The thickness of the gas diffusion layer 5 is not particularly limited, but can be, for example, 1 μm or more and 50 μm or less. In this specification, the term "thickness" refers to the thickness in the thickness direction of the cell main body 20. The thickness direction is the direction perpendicular to the plane direction parallel to the first main surface 12 of the metal support 10. The plane direction is defined by an approximate straight line of the first main surface 12 obtained by the least squares method in a cross section of the metal support 10 along the Z-axis direction.
[0036] The method for forming the gas diffusion layer 5 is not particularly limited, and may be a firing method, a spray coating method (such as a thermal spraying method, an aerosol deposition method, an aerosol gas deposition method, a powder jet deposition method, a particle jet deposition method, or a cold spray method), a PVD method (such as a sputtering method or a pulsed laser deposition method), or a CVD method.
[0037] [Hydrogen Electrode Layer 6] The hydrogen electrode layer 6 is an example of the "first electrode layer" according to the present invention. The hydrogen electrode layer 6 is formed on the gas diffusion layer 5. The hydrogen electrode layer 6 is disposed between the gas diffusion layer 5 and the electrolyte layer 7.
[0038] The source gas is supplied to the hydrogen electrode layer 6 through the gas diffusion layer 5 and the communication holes 11. The source gas contains at least H 2 Contains O.
[0039] The raw material gas is H 2 When only O is contained, the hydrogen electrode layer 6 converts H from the raw material gas according to the electrochemical reaction of water electrolysis shown in the following formula (1): 2 Generate.
[0040] Hydrogen electrode layer 6: H 2 O + 2e - →H 2 +O 2- ...(1)
[0041] The raw material gas is H 2 O plus CO 2 In this case, the hydrogen electrode layer 6 converts H from the source gas according to the co-electrolytic electrochemical reactions shown in the following formulas (2), (3), and (4). 2 , CO and O 2- Generate.
[0042] Hydrogen electrode layer 6: CO2 +H 2 O+4e - →CO+H 2 +20 2- ... (2) H 2 Electrochemical reaction of O: H 2 O + 2e - →H 2 +O 2- ... (3) CO 2 Electrochemical reaction of: CO 2 +2e - →CO+O 2- ...(4)
[0043] The hydrogen electrode layer 6 is a porous body having electrical conductivity. The hydrogen electrode layer 6 has gas diffusibility. A source gas is supplied to the hydrogen electrode layer 6 from the gas diffusion layer 5. The hydrogen electrode layer 6 discharges the product gas generated inside to the gas diffusion layer 5 side.
[0044] The hydrogen electrode layer 6 contains a conductive material. As the conductive material, a metal material such as Ni (nickel) or Fe (iron), or a conductive ceramic material can be used. In the case of co-electrolysis, Ni is used as the catalyst for the generated H 2 and CO contained in the raw material gas 2 It also functions as a thermal catalyst, promoting the thermal reaction with HCl to maintain an appropriate gas composition for methanation and reverse water-gas shift reactions.
[0045] When the conductive material is a metal material, the conductive material exists in an oxide state (e.g., NiO) in an oxidizing atmosphere and in a metal state (e.g., Ni) in a reducing atmosphere. In this embodiment, it is assumed that the electrolysis cell 1 is exposed to a reducing atmosphere.
[0046] The hydrogen electrode layer 6 contains an oxide ion conductive material. The oxide ion conductive material is an example of the "ion conductive material" according to the present invention. Examples of the oxide ion conductive material include YSZ, CSZ, ScSZ, GDC, SDC, and (La, Sr)(Cr, Mn)O. 3 , (La,Sr)TiO 3 , Sr 2 (Fe, Mo) 2 O 6 , (La, Sr)VO 3, (La,Sr)FeO 3 , LDC, LSGM, and a mixed material of two or more of these can be used.
[0047] In this embodiment, the hydrogen electrode layer 6 has a single-layer structure made of a single composition, but may have a multi-layer structure made of different compositions.
[0048] The thickness of the hydrogen electrode layer 6 is not particularly limited, but can be, for example, 1 μm or more and 500 μm or less.
[0049] The method for forming the hydrogen electrode layer 6 is not particularly limited, and may be a firing method, a spray coating method, a PVD method, a CVD method, or the like.
[0050] [Electrolyte Layer 7] The electrolyte layer 7 is disposed between the hydrogen electrode layer 6 and the oxygen electrode layer 9. In this embodiment, the reaction prevention layer 8 is disposed between the electrolyte layer 7 and the oxygen electrode layer 9, and therefore the electrolyte layer 7 is sandwiched between the hydrogen electrode layer 6 and the reaction prevention layer 8.
[0051] The electrolyte layer 7 covers the hydrogen electrode layer 6 and also covers the region of the first main surface 12 of the metal support 10 that is exposed from the gas diffusion layer 5 .
[0052] The electrolyte layer 7 absorbs the O generated in the hydrogen electrode layer 6. 2- The electrolyte layer 7 is made of a dense material having oxide ion conductivity. The electrolyte layer 7 can be made of, for example, YSZ (yttria-stabilized zirconia, e.g., 8YSZ), GDC (gadolinium-doped ceria), ScSZ (scandia-stabilized zirconia), SDC (samarium-doped ceria), or LSGM (lanthanum gallate).
[0053] The porosity of the electrolyte layer 7 is not particularly limited, but may be, for example, 0.1% to 7%. The thickness of the electrolyte layer 7 is not particularly limited, but may be, for example, 1 μm to 100 μm.
[0054] The method for forming the electrolyte layer 7 is not particularly limited, and may be a baking method, a spray coating method, a PVD method, a CVD method, or the like.
[0055] [Reaction prevention layer 8] The reaction prevention layer 8 is disposed between the electrolyte layer 7 and the oxygen electrode layer 9. The reaction prevention layer 8 is disposed on the opposite side of the electrolyte layer 7 from the hydrogen electrode layer 6. The reaction prevention layer 8 prevents the constituent elements of the electrolyte layer 7 from reacting with the constituent elements of the oxygen electrode layer 9 to form a layer with high electrical resistance.
[0056] The reaction prevention layer 8 is made of an oxide ion conductive material, such as GDC or SDC.
[0057] The porosity of the reaction prevention layer 8 is not particularly limited, but may be, for example, 0.1% to 50%. The thickness of the reaction prevention layer 8 is not particularly limited, but may be, for example, 1 μm to 50 μm.
[0058] The method for forming the reaction prevention layer 8 is not particularly limited, and may be a baking method, a spray coating method, a PVD method, a CVD method, or the like.
[0059] [Oxygen Electrode Layer 9] The oxygen electrode layer 9 is an example of a "second electrode layer" according to the present invention. The oxygen electrode layer 9 is disposed on the opposite side of the electrolyte layer 7 from the hydrogen electrode layer 6. In this embodiment, the reaction prevention layer 8 is disposed between the electrolyte layer 7 and the oxygen electrode layer 9, and therefore the oxygen electrode layer 9 is connected to the reaction prevention layer 8. If the reaction prevention layer 8 is not disposed between the electrolyte layer 7 and the oxygen electrode layer 9, the oxygen electrode layer 9 is connected to the electrolyte layer 7.
[0060] The oxygen electrode layer 9 reacts with O 2 transferred from the hydrogen electrode layer 6 through the electrolyte layer 7 in accordance with the chemical reaction of the following formula (5): 2- From O 2 Generate.
[0061] Oxygen electrode layer 9: 2O 2- →O 2 +4e - ...(5)
[0062] The oxygen electrode layer 9 is a porous body having oxide ion conductivity and electrical conductivity. The oxygen electrode layer 9 is made of, for example, (La, Sr)(Co, Fe)O 3 , (La,Sr)FeO 3 , La(Ni,Fe)O 3 , (La,Sr)CoO 3, and (Sm,Sr)CoO 3 and an oxide ion conductive material (such as GDC).
[0063] The porosity of the oxygen electrode layer 9 is not particularly limited, but may be, for example, 20% to 60%. The thickness of the oxygen electrode layer 9 is not particularly limited, but may be, for example, 1 μm to 100 μm.
[0064] The method for forming the oxygen electrode layer 9 is not particularly limited, and may be a firing method, a spray coating method, a PVD method, a CVD method, or the like.
[0065] [Flow Channel Member 30] The flow channel member 30 is bonded to the second main surface 13 of the metal support 10. A flow channel 30a is formed between the flow channel member 30 and the metal support 10. A source gas is supplied to the flow channel 30a. The source gas supplied to the flow channel 30a is supplied to the hydrogen electrode layer 6 of the cell main body 20 via each communication hole 11 of the metal support 10.
[0066] The flow path member 30 can be made of, for example, an alloy material. The flow path member 30 may be made of the same material as the metal support 10. In this case, the flow path member 30 may be substantially integrated with the metal support 10.
[0067] The flow path member 30 has a frame 31 and an interconnector 32. The frame 31 is an annular member that surrounds the side of the flow path 30a. The frame 31 is joined to the second main surface 13 of the metal support 10. The interconnector 32 is a plate-like member for electrically connecting an external power source or another electrolytic cell to the electrolytic cell 1 in series. The interconnector 32 is joined to the frame 31.
[0068] In this embodiment, the frame body 31 and the interconnector 32 are separate members, but the frame body 31 and the interconnector 32 may be an integrated member.
[0069] (Detailed Structure of Gas Diffusion Layer 5 and Hydrogen Electrode Layer 6) FIG. 3 is a partially enlarged view of FIG.
[0070] The gas diffusion layer 5 has a plurality of first conductive particles 5 a, a plurality of base particles 5 b, and a plurality of first pores 5 c. The plurality of first conductive particles 5 a and the plurality of first pores 5 c are essential components, while the plurality of base particles 5 b is optional.
[0071] The first conductive particles 5 a are connected to each other, thereby forming a conductive path that extends in the thickness direction within the gas diffusion layer 5. The first conductive particles 5 a are connected to each other at neck portions L1. The neck portions L1 are formed by mass transfer between the first conductive particles 5 a that occurs during heating when the gas diffusion layer 5 is formed.
[0072] The base particles 5b are connected to each other. This forms a skeleton that maintains the conductive paths. The base particles 5b are connected to each other at neck portions L2. The neck portions L2 are formed by mass transfer between the base particles 5b that occurs during heating when the gas diffusion layer 5 is formed.
[0073] The first pores 5c are connected to each other, thereby forming gas flow paths that extend three-dimensionally within the gas diffusion layer 5. The first pores 5c are voids between the first conductive particles 5a and the base particles 5b.
[0074] The hydrogen electrode layer 6 has a plurality of second conductive particles 6a, a plurality of ion conductive particles 6b, and a plurality of second pores 6c.
[0075] The second conductive particles 6 a are connected to one another, thereby forming a conductive path that extends in the thickness direction within the hydrogen electrode layer 6. The second conductive particles 6 a are connected to one another at neck portions M1. The neck portions M1 are formed by mass transfer between the second conductive particles 6 a that occurs during heating when the hydrogen electrode layer 6 is formed.
[0076] The ion conductive particles 6 b are connected to one another, thereby forming an ion conduction path that extends three-dimensionally within the hydrogen electrode layer 6. The ion conductive particles 6 b are connected to one another at neck portions M2, which are formed by mass transfer between the ion conductive particles 6 b that occurs during heating when the hydrogen electrode layer 6 is formed.
[0077] The second pores 6c are connected to each other, thereby forming gas flow paths that extend three-dimensionally within the hydrogen electrode layer 6. The second pores 6c are voids between the second conductive particles 6a and the ion conductive particles 6b.
[0078] The average circular equivalent diameter of the first pores 5c in the gas diffusion layer 5 is smaller than the average circular equivalent diameter of the second pores 6c in the hydrogen electrode layer 6. That is, the gas diffusion layer 5 contains more small-diameter pores than the hydrogen electrode layer 6. The porosity of the gas diffusion layer 5 is also greater than that of the hydrogen electrode layer 6. That is, the volume ratio of the gas flow paths per unit volume of the gas diffusion layer 5 is greater than the volume ratio of the gas flow paths per unit volume of the hydrogen electrode layer 6. This improves the gas diffusibility of the gas diffusion layer 5, allowing gas to diffuse not only in the thickness direction but also in the planar direction of the gas diffusion layer 5. Therefore, the gas diffusion layer 5 can efficiently supply the source gas supplied from each of the communicating holes 11 in the metal support 10 to the entire hydrogen electrode layer 6, and can efficiently discharge the product gas generated in the hydrogen electrode layer 6 from the entire hydrogen electrode layer 6 to each of the communicating holes 11.
[0079] The average equivalent circle diameter of pores is the arithmetic mean value of the equivalent circle diameters of a plurality of pores. The equivalent circle diameter of a pore is the diameter of a circle having the same area as the area of the pores appearing in a cross section along the thickness direction.
[0080] The porosity of the gas diffusion layer 5 and the hydrogen electrode layer 6 can be obtained as follows. Since the porosity measurement method is common to each layer, the following description will be given taking the case of obtaining the porosity of the gas diffusion layer 5 as an example.
[0081] First, the electrolytic cell 1 is heated to 750° C., and hydrogen is supplied to the gas diffusion layer 5 and the hydrogen electrode layer 6 to reduce the conductive material contained in the gas diffusion layer 5 and the hydrogen electrode layer 6 .
[0082] Next, the temperature of the electrolytic cell 1 is lowered while the reducing atmosphere is maintained, and the electrolytic cell 1 is cut along the thickness direction (Z-axis direction) to expose cross sections of the gas diffusion layer 5 and the hydrogen electrode layer 6 .
[0083] Next, the cross section is polished by precision machinery, and then subjected to ion milling processing using an IM4000 manufactured by Hitachi High-Technologies Corporation.
[0084] Next, an FE-SEM (Field Emission Scanning Electron Microscope) using an in-lens secondary electron detector is used to obtain an enlarged SEM image of the cross section of the gas diffusion layer 5 at a magnification (for example, 5,000 to 30,000 times) sufficient to confirm the first conductive particles 5 a, the base particles 5 b, and the first pores 5 c.
[0085] Next, the brightness of the SEM image is classified into 256 gradations, and the brightness differences of the first conductive particles 5 a, the base particles 5 b, and the first pores 5 c are ternarized. For example, the first conductive particles 5 a can be displayed in dark gray, the base particles 5 b in light gray, and the first pores 5 c in black.
[0086] Next, the SEM image is analyzed using image analysis software HALCON manufactured by MVTec (Germany) to obtain an analysis image in which the first pores 5c are highlighted.
[0087] Next, the total area of the first pores 5c (gas phase) is obtained from the analysis image, and the total area of the first pores 5c is divided by the area of the entire analysis image to calculate the porosity in one analysis image.
[0088] The above analysis is performed at five randomly selected locations on the same cross section of the gas diffusion layer 5, and the arithmetic mean value of the porosities calculated at the five locations is taken as the porosity of the gas diffusion layer 5.
[0089] 3, the number of first pores 5c per unit area of the gas diffusion layer 5 is preferably greater than the number of second pores 6c per unit area of the hydrogen electrode layer 6. This allows gas to diffuse to every corner of the gas diffusion layer 5, thereby further improving the gas diffusibility of the gas diffusion layer 5. The number of pores can be obtained from the analysis image used to obtain the porosity.
[0090] Furthermore, the average neck diameter between the first conductive particles 5 a contained in the gas diffusion layer 5 is preferably smaller than the average neck diameter between the second conductive particles 6 a contained in the hydrogen electrode layer 6. This makes it easier to form the gas diffusion layer 5 with a structure that includes many small-diameter pores and has a large volume ratio of gas flow paths.
[0091] The average neck diameter between the first conductive particles 5a is the arithmetic mean value of the neck diameters of the neck portions L1 between the first conductive particles 5a. The neck diameter of the neck portions L1 is the width of the narrowest part between two first conductive particles 5a. The average neck diameter between the first conductive particles 5a can be obtained by arithmetically averaging the neck diameters of the neck portions L1 at 10 locations randomly selected from the analysis image used to obtain the porosity. The average neck diameter between the first conductive particles 5a is not particularly limited, but can be, for example, 0.05 μm or more and 0.5 μm or less.
[0092] Similarly, the average neck diameter between the second conductive particles 6a is the arithmetic mean value of the neck diameters of the neck portions M1 between the second conductive particles 6a. The neck diameter of the neck portions M1 is the width of the narrowest part between two second conductive particles 6a. The average neck diameter between the second conductive particles 6a can be obtained by arithmetically averaging the neck diameters of the neck portions M1 at 10 locations randomly selected from the analysis image used to obtain the porosity. The average neck diameter between the second conductive particles 6a is not particularly limited, but can be, for example, 0.1 μm or more and 3 μm or less.
[0093] Furthermore, the average neck diameter between the base particles 5 b contained in the gas diffusion layer 5 is preferably smaller than the average neck diameter between the ion conductive particles 6 b contained in the hydrogen electrode layer 6. This makes it easier to form the gas diffusion layer 5 into a structure that contains many small-diameter pores and has a large volume ratio of gas flow paths.
[0094] The average neck diameter between base particles 5b is the arithmetic mean value of the neck diameters of the neck portions L2 between base particles 5b. The neck diameter of the neck portions L2 is the width of the narrowest part between two base particles 5b. The average neck diameter between base particles 5b can be obtained by arithmetically averaging the neck diameters of the neck portions L2 at 10 locations randomly selected from the analysis image used to obtain the porosity. The average neck diameter between base particles 5b is not particularly limited, but can be, for example, 0.1 μm or less.
[0095] Similarly, the average neck diameter between the ion-conductive particles 6b is the arithmetic mean value of the neck diameters of the neck portions M2 between the ion-conductive particles 6b. The neck diameter of the neck portion M2 is the width of the narrowest part between two ion-conductive particles 6b. The average neck diameter between the ion-conductive particles 6b can be obtained by arithmetically averaging the neck diameters of the neck portions M2 at 10 locations randomly selected from the analysis image used to obtain the porosity. The average neck diameter between the ion-conductive particles 6b is not particularly limited, but can be, for example, 1 μm or more and 3 μm or less.
[0096] (Modifications of the Embodiment) Although the embodiment of the present invention has been described above, the present invention is not limited to these, and various modifications are possible without departing from the spirit of the present invention.
[0097] [Variation 1] In the above embodiment, the openings of each communication hole 11 on the first main surface 12 side of the metal support 10 are covered by the gas diffusion layer 5, but this is not limited to this. The gas diffusion layer 5 does not have to cover the openings of each communication hole 11 on the first main surface 12 side. In this case, through holes communicating with each communication hole 11 are formed in the gas diffusion layer 5, allowing for more efficient supply and exhaust of gas via the through holes.
[0098] [Variation 2] In the above embodiment, the electrolysis cell 1 has been described as an example of an electrochemical cell, but the electrochemical cell is not limited to an electrolysis cell. An electrochemical cell is a general term for an element in which a pair of electrodes are arranged so that an electromotive force is generated from an overall oxidation-reduction reaction in order to convert electrical energy into chemical energy, and an element for converting chemical energy into electrical energy. Therefore, electrochemical cells include, for example, fuel cells that use oxide ions or protons as carriers.
[0099] REFERENCE SIGNS LIST 1 Electrolysis cell 10 Metal support 11 Through hole 12 First main surface 13 Second main surface 20 Cell body 5 Gas diffusion layer 5a First conductive particle 5b Base particle 5c First pore 5d Neck portion of first conductive particle 5e Neck portion of base particle 6 Hydrogen electrode layer 6a Second conductive particle 6b Ion conductive particle 6c Second pore 6d Neck portion of second conductive particle 6e Neck portion of ion conductive particle 7 Electrolyte layer 8 Reaction prevention layer 9 Oxygen electrode layer 30 Flow path member 30a Flow path
Claims
1. An electrochemical cell comprising: a metal support having a plurality of communicating holes formed in a principal surface; and a cell body portion disposed on the principal surface, wherein the cell body portion has: a conductive gas diffusion layer disposed on the principal surface; a first electrode layer disposed on the gas diffusion layer; a second electrode layer; and an electrolyte layer disposed between the first electrode layer and the second electrode layer, wherein the gas diffusion layer includes a plurality of first pores, and the first electrode layer includes a plurality of second pores, an average circular equivalent diameter of the plurality of first pores is smaller than an average circular equivalent diameter of the plurality of second pores, and the porosity of the gas diffusion layer is greater than the porosity of the first electrode layer.
2. The electrochemical cell of claim 1, wherein the number of said first pores per unit area is greater than the number of said second pores per unit area.
3. The electrochemical cell according to claim 1 or 2, wherein the gas diffusion layer contains a plurality of first conductive particles, the first electrode layer contains a plurality of second conductive particles, and an average neck diameter between the first conductive particles is smaller than an average neck diameter between the second conductive particles.
Citation Information
Patent Citations
Electrochemical element, electrochemical module, electrochemical device, energy system, solid oxide fuel cell, and solid oxide electrolytic cell
JP2021163764A
Electrochemical element, solid oxide type fuel battery cell, and method for manufacturing same
WO2016043328A1
Fuel cell
WO2017010435A1
Electrochemical cell
WO2023013205A1