Battery module, manufacturing method of battery module, and inspection method of laser welding

The battery module's laser etching marks enable easy inspection of welding quality, addressing the challenge of detecting defects and maintaining consistent welding conditions, thus enhancing the reliability and efficiency of the laser welding process.

WO2024202308A1PCT designated stage expired Publication Date: 2024-10-03AESC JAPAN LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/045059
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2023-12-15
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Laser welding defects in battery modules are difficult to detect and diagnose due to random occurrences and the need for destructive inspections, making it challenging to identify factors affecting quality and respond to changes in welding conditions over time.

Method used

A battery module with laser etching marks on both sides of the welding area, allowing for inspection of differences between actual and designed marks, enabling easy detection of abnormalities and quality assessment.

Benefits of technology

Facilitates real-time monitoring and easy inspection of factors affecting laser welding quality, allowing for immediate identification of defects and maintenance needs, reducing production downtime and improving productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023045059_03102024_PF_FP_ABST
    Figure JP2023045059_03102024_PF_FP_ABST
Patent Text Reader

Abstract

A battery module (10) is provided with: a laser-welded part (200) formed in a positive electrode tab (120); and a left-side laser etching mark (210) and a right-side laser etching mark (220) formed on both sides of the laser-welded part (200) in the positive electrode tab (120).
Need to check novelty before this filing date? Find Prior Art

Description

Battery module, battery module manufacturing method, and laser welding inspection method

[0001] The present invention relates to a battery module, a manufacturing method for a battery module, and a method for inspecting laser welding.

[0002] In recent years, various battery modules including a plurality of battery cells have been developed. For example, as described in Patent Documents 1 and 2, the battery modules may be provided with an identifier formed by a laser.

[0003] International Publication No. 2019 / 193869 Japanese Patent Application Laid-Open No. 2006-40875

[0004] In battery modules, laser welding is sometimes used to join various workpieces, such as joining battery cell tabs, joining tabs and bus bars, and assembling housings. Laser welding requires various qualities, such as impact resistance, vibration resistance, and environmental resistance testing. However, laser welding equipment used for laser welding can develop abnormalities due to aging, and various abnormalities can occur in the workpieces, such as tab deformation and housing assembly accuracy issues. When such abnormalities occur, it can be difficult to prevent laser welding defects, such as poor laser welding joints and abnormal resistance values ​​in laser welds. However, such laser welding defects can be detected using methods such as laser welding monitoring (LWM) and resistance measurement. However, even with these methods, it can be relatively difficult to immediately identify the cause of the laser welding defects or respond to changes in the laser welding defects over time. Furthermore, the frequency of such laser welding defects can be random, making it relatively difficult to predict the occurrence of laser welding defects. Therefore, when a laser welding defect occurs, it may be necessary to stop the laser welding line and inspect the laser welds before and after the laser welding defect, for example, using destructive testing. Therefore, it can be relatively difficult to easily inspect factors that affect the quality of laser welding.

[0005] One object of the present invention is to easily inspect factors that affect the quality of laser welding. Other objects of the present invention will become apparent from the description of this specification.

[0006] An aspect of the present invention is as follows. [1] A battery module comprising: a laser weld formed on an object to be processed; and a laser etching mark formed on at least one of both sides of the laser weld on the object to be processed. [2] The battery module according to [1], wherein the laser etching mark has a corner. [3] The battery module according to [1] or [2], wherein the laser etching mark has a plurality of patterns that at least partially overlap each other. [4] The battery module according to any one of [1] to [3], wherein the laser etching mark has a plurality of patterns whose centers overlap each other. [5] The battery module according to any one of [1] to [4], wherein the laser etching mark and a pre-designed laser etching mark are inspected for similarity or difference. [6] A method for manufacturing a battery module, comprising: forming a laser weld on an object to be processed; and forming a laser etching mark on at least one of both sides of the laser weld on the object to be processed. [7] A method for inspecting laser welding, comprising: inspecting the laser etching mark formed on the object to be processed on which a laser weld is to be formed, for similarity or difference between a pre-designed laser etching mark.

[0007] According to the above-described aspects of the present invention, factors that affect the quality of laser welding can be easily inspected.

[0008] 1 is a perspective view of a portion of a battery module according to an embodiment; FIG. 2 is a view showing a cross section of a laser weld according to an embodiment; FIG. 3 is a view showing an example of a laser welding apparatus for laser welding a workpiece; FIG. 4 is a view showing a first example of a method for forming a laser weld; FIG. 5 is a view showing a second example of a method for forming a laser weld; FIG. 6 is a view showing a method for forming a left-side first laser etching pattern, a laser weld, and a right-side first laser etching pattern according to an embodiment; FIG. 7 is a view showing a method for forming a left-side laser etching mark and a right-side laser etching mark according to an embodiment; FIG. 8 is a view showing a method for forming a first laser etching pattern according to an embodiment; FIG. 9 is a graph showing an example of the relationship between laser output and laser spot size in a first laser etching pattern; FIG. 10 is a view showing a method for measuring a laser spot size in a first laser etching pattern; FIG. 11 is a cross-sectional view of a workpiece in an etching mode; FIG. 12 is a cross-sectional view of a workpiece in a melting mode; FIG. 13 is a view showing a first example of an abnormality in the shape of a first laser etching pattern; FIG. 14 is a view showing a second example of an abnormality in the shape of a first laser etching pattern; FIG. 15 is a view showing a third example of an abnormality in the shape of a first laser etching pattern; FIG. 16 is a view showing a fourth example of an abnormality in the shape of a first laser etching pattern; FIG. 17 is a view showing a fifth example of an abnormality in the shape of a first laser etching pattern; 1 is a diagram showing a second example of an abnormality in the shape of a laser-etched mark; FIG. 2 is a diagram showing a laser-etched mark according to a modified example; FIG. 3 is a diagram for explaining another example of a method for inspecting laser welding according to an embodiment; FIG. 4 is a diagram for explaining another example of a method for inspecting laser welding according to an embodiment;

[0009] Hereinafter, embodiments and modifications of the present invention will be described with reference to the drawings. In all the drawings, like components are designated by like reference numerals, and descriptions thereof will be omitted as appropriate.

[0010] Fig. 1 is a perspective view of a portion of a battery module 10 according to an embodiment. Fig. 2 is a diagram showing a cross section of a laser welded portion 200 according to an embodiment.

[0011] For the sake of explanation, each figure illustrates an X-axis, a Y-axis, and a Z-axis that are orthogonal to one another. Hereinafter, as needed, the directions parallel to the X-axis, Y-axis, and Z-axis will be referred to as the X-direction, the Y-direction, and the Z-direction, respectively. Hereinafter, as needed, the side indicated by the arrow indicating the X-axis will be referred to as the +X-side, and the side opposite the side indicated by the arrow indicating the X-axis will be referred to as the -X-side. Hereinafter, as needed, the side indicated by the arrow indicating the Y-axis will be referred to as the +Y-side, and the side opposite the side indicated by the arrow indicating the Y-axis will be referred to as the -Y-side. Hereinafter, as needed, the side indicated by the arrow indicating the Z-axis will be referred to as the +Z-side, and the side opposite the side indicated by the arrow indicating the Z-axis will be referred to as the -Z-side. Hereinafter, as needed, the direction perpendicular to the Z-axis will be referred to as the XY-plane direction, the direction perpendicular to the Y-axis will be referred to as the ZX-plane direction, and the direction perpendicular to the X-axis will be referred to as the YZ-plane direction. Hereinafter, as needed, the direction of rotation around a direction parallel to the Z-direction will be referred to as the θ-direction.

[0012] In some of the drawings, a white circle with an X indicating the X-axis, Y-axis, or Z-axis indicates that the arrow of the axis indicated by the white circle is pointing from the front to the back of the page. A white circle with a black dot indicating the X-axis, Y-axis, or Z-axis indicates that the arrow of the axis indicated by the white circle is pointing from the back to the front of the page.

[0013] The battery module 10 according to the embodiment includes a plurality of battery cells 100. Each battery cell 100 extends substantially parallel to the XY plane. Each battery cell 100 has a thickness substantially parallel to the Z direction. The plurality of battery cells 100 are stacked substantially parallel to the Z direction. Each battery cell 100 includes a battery element (not shown), an exterior material 110, a positive electrode tab 120, and a negative electrode tab 130. In one example, the battery element includes a plurality of positive electrodes and a plurality of negative electrodes stacked alternately in the Z direction. Adjacent positive electrodes and negative electrodes in the Z direction are separated from each other by a separator (not shown). However, the structure of the battery element is not limited to this example.

[0014] The exterior material 110 contains a battery element (not shown) and an electrolyte (not shown) and is made of, for example, an aluminum laminate.

[0015] The positive electrode tab 120 is electrically connected to the positive electrode of the battery element. The positive electrode tab 120 is made of, for example, at least one of aluminum and an aluminum alloy. The surface of the positive electrode tab 120 may be subjected to secondary processing such as a corrosion-resistant protective coating or a plating film. However, the material constituting the positive electrode tab 120 is not limited to this example, as long as it is a material with relatively high electrical conductivity, i.e., a material with relatively low electrical resistivity.

[0016] The negative electrode tab 130 is electrically connected to the negative electrode of the battery element. The negative electrode tab 130 is made of, for example, at least one of copper and a copper alloy. The surface of the negative electrode tab 130 may be subjected to secondary processing such as a corrosion-resistant protective coating or a plating film. However, the material constituting the negative electrode tab 130 is not limited to this example, as long as it is a material with relatively high electrical conductivity, i.e., a relatively low electrical resistivity. The material constituting the positive electrode tab 120 and the material constituting the negative electrode tab 130 may be the same or different.

[0017] In each battery cell 100, the positive electrode tab 120 and the negative electrode tab 130 are pulled out on opposite sides of the exterior material 110 in the Y direction. However, the method for pulling out the positive electrode tab 120 and the negative electrode tab 130 is not limited to this example. For example, the positive electrode tab 120 and the negative electrode tab 130 may be pulled out from the same side on the +Y side or the −Y side of the exterior material 110. In this example, the positive electrode tab 120 and the negative electrode tab 130 are aligned approximately parallel to the X direction.

[0018] In the embodiment, a plurality of cell groups, each including a plurality of battery cells 100 electrically connected in parallel, are electrically connected in series. In the example shown in FIG. 1 , eight cell groups, each including two battery cells 100, are schematically illustrated. However, the number of cell groups included in an actual battery module 10 is not limited to the example shown in FIG. 1 . In the example shown in FIG. 1 , two positive electrode tabs 120 extend from two battery cells 100 included in the third cell group from the +Z side toward the −Y side, and two negative electrode tabs 130 extend from two battery cells 100 included in the fourth cell group from the +Z side toward the −Y side. As shown in FIG. 2 , these positive electrode tabs 120 and negative electrode tabs 130 are joined to each other by laser welds 200. Therefore, in the example shown in FIG. 1 , the two battery cells 100 included in the third cell group from the +Z side and the two battery cells 100 included in the fourth cell group from the +Z side are electrically connected in series. Such joints between the positive electrode tabs 120 and the negative electrode tabs 130 are provided alternately on the +Y side and the −Y side of the battery module 10. Therefore, in the example shown in FIG. 1 , eight cell groups are electrically connected in series.

[0019] The manner of electrical connection of the plurality of battery cells 100 is not limited to the above-described example. For example, a plurality of cell groups each including three or more battery cells 100 electrically connected in parallel may be electrically connected in series. Alternatively, a plurality of single battery cells 100 may simply be connected in series.

[0020] The method for joining the positive electrode tab 120 and the negative electrode tab 130 to each other may be laser welding alone, or may be a combination of laser welding and another joining method. For example, joining methods such as caulking, FSW (friction stir welding), ultrasonic welding, TIG (Tungsten Inert Gas) welding, and MIG (Metal Inert Gas) welding may be combined.

[0021] The laser weld 200 is formed by irradiating the joint between the positive electrode tab 120 and the negative electrode tab 130 with a laser from the side where the positive electrode tab 120 is located. In the example shown in Fig. 2, the laser weld 200 is formed by irradiating the joint between the positive electrode tab 120 and the negative electrode tab 130 with a laser from the +Z side. As shown in Fig. 2, the laser weld 200 at least partially reaches the negative electrode tab 130. Therefore, the positive electrode tab 120 and the negative electrode tab 130 are joined to each other.

[0022] Fig. 3 is a diagram showing an example of a laser welding apparatus 50 for laser welding a workpiece W. In the example shown in Fig. 3, the workpiece W is mounted on a stage 550 that is approximately perpendicular to the Z direction. The workpiece W is laser welded by the laser welding apparatus 50 in the following manner. However, the structure of the laser welding apparatus for laser welding the workpiece W is not limited to the structure of the laser welding apparatus 50 shown in Fig. 3.

[0023] 3, a laser beam B is emitted from a laser oscillator 502 via an optical fiber 504. The laser beam B passes through a beam expander 506 and a focus lens 508 in this order, and is incident on a galvanometer mirror optical system 510. The beam diameter of the laser beam B is expanded by the beam expander 506. The position of the focus of the laser beam B on the workpiece W in the Z direction can be adjusted by moving the focus lens 508 in a direction approximately parallel to the optical axis of the laser beam B.

[0024] The laser beam B enters the galvanometer mirror optical system 510, passes through a condenser lens 512, and is then incident on a movable mirror 514. The laser beam B is reflected by the movable mirror 514, passes through a cover glass 516, and is irradiated onto the workpiece W. The movable mirror 514 makes it possible to adjust the irradiation position of the laser beam B on the workpiece W in the X and Y directions.

[0025] The tip of the optical fiber 504, the beam expander 506, the focus lens 508, and the galvanometer mirror optical system 510 can be moved in the XY plane by a moving unit 520. The moving unit 520 makes it possible to adjust the irradiation position of the laser beam B on the workpiece W in the X, Y, and Z directions.

[0026] The stage 550 is movable in the X, Y, Z, and θ directions, and the irradiation position of the laser beam B on the workpiece W can be adjusted in the X, Y, Z, and θ directions by the stage 550.

[0027] In the example shown in Fig. 2, two positive electrode tabs 120 and two negative electrode tabs 130 to be joined together correspond to the workpiece W shown in Fig. 3. In this example, a laser beam B is irradiated onto the joint between the positive electrode tabs 120 and the negative electrode tabs 130 from the +Z side.

[0028] The welding conditions for the workpiece W may vary depending on whether the materials being welded are homogeneous or heterogeneous. For example, when dissimilar materials are welded, if the welding conditions deviate from the optimal conditions at the weld of dissimilar materials such as aluminum-copper, an intermetallic compound film (IMC) may form at a high melting point. If an IMC is formed, defects such as high IMC hardness or IMC brittleness may occur. Alternatively, if the welding conditions deviate from the optimal conditions at the weld of homogeneous materials such as aluminum-aluminum, defects such as fusion cracking at the welded portion may occur. Therefore, to avoid these defects, the welding conditions for the workpiece W must be set to the optimal conditions. The welding conditions for the workpiece W may deviate from the optimal conditions due to various abnormalities, such as an abnormality in the laser oscillator 502 of the laser welding apparatus 50 or an abnormality in various optical systems such as the galvanometer mirror optical system 510. Therefore, these various abnormalities in the laser welding apparatus 50 may affect the joint strength of the laser weld 200. In other words, this embodiment can be used to determine whether the joining strength of the laser welded portion 200 is good or bad in the inspection described below.

[0029] FIG. 4 is a diagram for explaining a first example of a method for forming the laser welded portion 200. In FIG.

[0030] In FIG. 4 , the circles on the laser weld 200 indicate spots generated by a laser irradiated from the +Z side. In the example shown in FIG. 4 , multiple spots are continuously generated substantially parallel to the X direction from the left side to the right side of the positive electrode tab 120 to form the laser weld 200. The laser oscillator 502 can be either a continuous wave (CW) type or a pulsed type depending on predetermined conditions such as the welding purpose and the characteristics of the workpiece W. In the example shown in FIG. 4 , the laser oscillator 502 is a continuous wave (CW) type.

[0031] Fig. 5 is a diagram for explaining a second example of a method for forming the laser welded portion 200. The second example shown in Fig. 5 is similar to the first example shown in Fig. 4 except for the following points.

[0032] In the example shown in Fig. 5, wobbling welding is performed, as indicated by the imaginary dashed arrow on the right side of the laser weld 200. In the example shown in Fig. 5, multiple spots are generated continuously in a clockwise direction from the left side to the right side of the positive electrode tab 120, thereby forming the laser weld 200.

[0033] In the laser welding illustrated in FIGS. 4 and 5 , prolonged operation of the laser welding apparatus 50 can cause wear of the movable elements of the laser welding apparatus 50 and thermal lens effects of various optical lenses. For example, abnormal operation of the movable mirror 514 can cause the movable mirror 514 to burn or displace. Various optical lenses, such as the beam expander 506, the focus lens 508, the condenser lens 512, and the cover glass 516, can block the laser beam B, and the transmittance of the various optical lenses can decrease. It can be relatively difficult to detect such phenomena through routine pre-maintenance. It can also be relatively difficult to predict the occurrence of the aforementioned phenomena. Furthermore, simply shutting down production equipment and increasing the frequency of maintenance can result in reduced productivity.

[0034] 6 is a diagram illustrating a method for forming a left-side first laser-etched pattern 212 (hereinafter simply referred to as the left-side first pattern 212), a laser weld 200, and a right-side first laser-etched pattern 222 (hereinafter simply referred to as the right-side first pattern 222) according to an embodiment. FIG. 7 is a diagram illustrating a method for forming a left-side laser-etched mark 210 (hereinafter simply referred to as the left mark 210) and a right-side laser-etched mark 220 (hereinafter simply referred to as the right mark 220) according to an embodiment. Hereinafter, for the sake of explanation, the −X side will be referred to as the left side, and the +X side will be referred to as the right side, as necessary. However, the left side and the right side do not necessarily refer to the directions when the battery module 10 is in use.

[0035] 6, a laser beam is irradiated from the +Z side to form the first left pattern 212 on the left side of the positive electrode tab 120. The first left pattern 212 has a substantially infinity shape.

[0036] 6 , a laser weld 200 is formed from the left side to the right side of the positive electrode tab 120 by laser irradiation from the +Z side. The laser weld 200 extends substantially parallel to the X direction. The left-side first pattern 212 is located to the left of the left end of the laser weld 200.

[0037] Next, as shown in Fig. 6, a laser is irradiated from the +Z side to form a right-side first pattern 222 on the right portion of the positive electrode tab 120. The shapes of the left-side first pattern 212 and the right-side first pattern 222 are substantially identical. The right-side first pattern 222 is located on the right side of the right end of the laser welded portion 200. The left-side first pattern 212 and the right-side first pattern 222 are located on both the left and right sides of the laser welded portion 200 in the X direction.

[0038] Next, as shown in FIG. 7 , a left-side second laser etching pattern 214 (hereinafter simply referred to as the left-side second pattern 214) is formed on the left portion of the positive electrode tab 120 by laser irradiation from the +Z side. The left-side first pattern 212 and the left-side second pattern 214 are substantially symmetrical patterns. The left-side first pattern 212 and the left-side second pattern 214 at least partially overlap each other. Thus, a left-side mark 210 having the left-side first pattern 212 and the left-side second pattern 214 is formed. The left-side mark 210 is substantially in the shape of a + surrounded by a substantially square.

[0039] Next, as shown in FIG. 7 , a second right laser etching pattern 224 (hereinafter simply referred to as the second right pattern 224) is formed on the right portion of the positive electrode tab 120 by laser irradiation from the +Z side. The first right pattern 222 and the second right pattern 224 are substantially symmetrical patterns. The first right pattern 222 and the second right pattern 224 at least partially overlap each other. Thus, a right mark 220 having the first right pattern 222 and the second right pattern 224 is formed. The right mark 220 is substantially in the shape of a + surrounded by a substantially square. The left mark 210 and the right mark 220 are located on both the left and right sides of the laser welded portion 200 in the X direction.

[0040] The optimal conditions for laser irradiation to form the laser welded portion 200 are generally determined in advance depending on the type of workpiece W. For example, when the workpiece W is an aluminum alloy and a copper alloy and the aluminum alloy and the copper alloy are to be laser welded to each other, the optimal conditions for laser irradiation are, for example, a laser wavelength of 1064 nm, a focused laser spot diameter of 72 μm, and a laser output of 1000 W. These optimal conditions remain constant as long as the ambient environment of the workpiece W, the external environment of the workpiece W, such as the gas atmosphere, remains constant.

[0041] The laser output for forming the left mark 210 and the right mark 220 is lower than the laser output under the optimal conditions for laser irradiation for forming the laser weld 200. The left mark 210 and the right mark 220 are formed in an etching mode, which will be described later with reference to Figures 9 to 12. For example, if the optimal conditions for laser irradiation for forming the laser weld 200 are the example described above, the laser output for forming the left mark 210 and the right mark 220 is about one-third of the laser output under the optimal conditions, i.e., about 200 W to 400 W. In this example, a recess having a depth of about 10 μm to 30 μm is formed in the surface of the workpiece by laser etching.

[0042] 6 and 7 , a left mark 210 and a right mark 220 are formed on both sides in the X direction of the laser welded portion 200 in the positive electrode tab 120. However, one of the left mark 210 and the right mark 220 does not have to be formed.

[0043] Hereinafter, when there is no need to particularly distinguish between the left mark 210 and the right mark 220 in the description, the left mark 210 and the right mark 220 may be simply referred to as marks 210. Hereinafter, when there is no need to particularly distinguish between the left first pattern 212 and the right first pattern 222 in the description, the left first pattern 212 and the right first pattern 222 may be simply referred to as first patterns 212. Hereinafter, when there is no need to particularly distinguish between the left second pattern 214 and the right second pattern 224 in the description, the left second pattern 214 and the right second pattern 224 may be simply referred to as second patterns 214.

[0044] 8 is a diagram illustrating a method for forming a first pattern 212 according to an embodiment. For the purpose of explanation, six imaginary arrows, a first arrow A1 to a sixth arrow A6, are illustrated in FIG. 8. Circles shown along the first pattern 212 in FIG. 8 indicate laser spots generated by laser irradiation.

[0045] The first pattern 212 is formed as follows: The second pattern 214 is formed symmetrically with respect to the Y axis with respect to the method for forming the first pattern 212, which will be described below.

[0046] First, as indicated by the first arrow A1, a plurality of laser spots are sequentially generated substantially parallel to the X direction from the −X side toward the +X side. Thus, a first line pattern L1 substantially parallel to the X direction is generated. The first line pattern L1 includes a plurality of laser spots aligned substantially parallel to the X direction.

[0047] Next, as indicated by the second arrow A2, multiple laser spots are generated sequentially from the -Y side toward the +Y side, substantially parallel to the Y direction. Thus, a second line pattern L2 substantially parallel to the Y direction is generated. The second line pattern L2 includes multiple laser spots aligned substantially parallel to the Y direction. The +X side end of the first line pattern L1 and the -Y side end of the second line pattern L2 are substantially perpendicular to each other. Thus, the first pattern 212 has a substantially right-angled corner formed by the intersection of the +X side end of the first line pattern L1 and the -Y side end of the second line pattern L2.

[0048] Next, as indicated by the third arrow A3, multiple laser spots are sequentially generated substantially parallel to the X direction from the +X side toward the -X side. Thus, a third line pattern L3 is generated that is substantially parallel to the X direction. The third line pattern L3 includes multiple laser spots aligned substantially parallel to the X direction. The +Y side end of the second line pattern L2 and the +X side end of the third line pattern L3 are substantially perpendicular to each other. Thus, the first pattern 212 has a substantially right-angled corner formed by the intersection of the +Y side end of the second line pattern L2 and the +X side end of the third line pattern L3.

[0049] Next, as indicated by the fourth arrow A4, multiple laser spots are generated sequentially from the +Y side toward the -Y side, substantially parallel to the Y direction. Thus, a fourth line pattern L4 is generated that is substantially parallel to the Y direction. The fourth line pattern L4 includes multiple laser spots that are aligned substantially parallel to the Y direction. The -X side end of the third line pattern L3 and the +Y side end of the fourth line pattern L4 are substantially perpendicular to each other. Thus, the first pattern 212 has a substantially right-angled corner formed by the intersection of the -X side end of the third line pattern L3 and the +Y side end of the fourth line pattern L4.

[0050] Next, as indicated by the fifth arrow A5, multiple laser spots are sequentially generated substantially parallel to the X direction from the +X side toward the -X side. Thus, a fifth line pattern L5 is generated that is substantially parallel to the X direction. The fifth line pattern L5 includes multiple laser spots aligned substantially parallel to the X direction. The -Y side end of the fourth line pattern L4 and the +X side end of the fifth line pattern L5 are substantially perpendicular to each other. Thus, the first pattern 212 has a substantially right-angled corner formed by the intersection of the -Y side end of the fourth line pattern L4 and the +X side end of the fifth line pattern L5.

[0051] Next, as indicated by the sixth arrow A6, multiple laser spots are sequentially generated substantially parallel to the Y direction from the -Y side toward the +Y side. Thus, a sixth line pattern L6 is generated that is substantially parallel to the Y direction. The sixth line pattern L6 includes multiple laser spots that are aligned substantially parallel to the Y direction. The -X side end of the fifth line pattern L5 and the -Y side end of the sixth line pattern L6 are substantially perpendicular to each other. Thus, the first pattern 212 has a substantially right-angled corner formed by the intersection of the -X side end of the fifth line pattern L5 and the -Y side end of the sixth line pattern L6.

[0052] In the first pattern 212, the third line pattern L3 and the fifth line pattern L5 are positioned at approximately equal distances in the Y direction from the first line pattern L1. In the first pattern 212, the second line pattern L2 and the sixth line pattern L6 are positioned at approximately equal distances in the X direction from the fourth line pattern L4.

[0053] 8, the −X side end of the first line pattern L1 protrudes toward the −X side further than the +Y side end of the sixth line pattern L6. This makes it easier to identify the starting position for forming the first pattern 212. However, the −X side end of the first line pattern L1 does not have to protrude toward the −X side further than the +Y side end of the sixth line pattern L6.

[0054] Fig. 9 is a graph showing an example of the relationship between laser output and laser spot size in the first pattern 212. Fig. 10 is a diagram for explaining a method for measuring the laser spot size in the first pattern 212. Fig. 11 is a cross-sectional view of the workpiece W in the etching mode. Fig. 12 is a cross-sectional view of the workpiece W in the melting mode. In the examples shown in Figs. 9 to 12, the workpiece W is an aluminum alloy. However, the workpiece W is not limited to an aluminum alloy and may be, for example, copper.

[0055] 9 represents the laser output (unit: W) for forming the first pattern 212. The vertical axis of the graph shown in Fig. 9 represents the laser spot size (unit: μm) in the first pattern 212.

[0056] The plot of M(X) in the graph shown in Fig. 9 indicates M(X) = (X1 + X2 + X3 + X4) / 4. As shown in Fig. 10, X1 indicates the X-direction width of the second line pattern L2 at approximately the center in the Y direction. X2 indicates the X-direction width of the fourth line pattern L4 at a portion located approximately equidistant from the first line pattern L1 and the third line pattern L3. X3 indicates the X-direction width of the fourth line pattern L4 at a portion located approximately equidistant from the first line pattern L1 and the fifth line pattern L5. X4 indicates the X-direction width of the sixth line pattern L6 at approximately the center in the Y direction.

[0057] The plot of M(Y) in the graph shown in Fig. 9 indicates M(Y) = (Y1 + Y2 + Y3 + Y4) / 4. As shown in Fig. 10, Y1 indicates the Y-direction width of the first line pattern L1 at a portion located at approximately equal distances from the fourth line pattern L4 and the sixth line pattern L6. Y2 indicates the Y-direction width of the first line pattern L1 at a portion located at approximately equal distances from the fourth line pattern L4 and the second line pattern L2. Y3 indicates the Y-direction width of the third line pattern L3 at approximately the center in the X direction. Y4 indicates the Y-direction width of the fifth line pattern L5 at approximately the center in the X direction.

[0058] As shown in FIG. 9, M(X) and M(Y) are both approximately 100 μm when the laser output is around 240 W to 350 W. When the laser output is around 240 W to 350 W, the laser irradiation by the laser welding device 50 is in etching mode. In etching mode, as shown in FIG. 11, a recess W1 is formed on the +Z side surface of the workpiece W by laser etching. When M(X) and M(Y) in etching mode are equal to or close to the theoretical value of the laser spot diameter when focused, it can be said that the focus lens 508 is focused on the workpiece W. In other words, in this embodiment, the laser spot diameter can be measured from M(X) and M(Y) without using special equipment. Therefore, the laser spot diameter can be measured in a shorter time than when using special equipment. Even if the laser spot system is not theoretically accurate, similar geometries can be performed by always maintaining the above-mentioned approximately 100 μm as a constant default value.

[0059] As shown in Fig. 9, at a laser output of 400 W or more, both M(X) and M(Y) are approximately 200 µm or more. At a laser output of 400 W or more, the laser irradiation by the laser welding device 50 is in melting mode. In the melting mode, as shown in Fig. 12, an expanded portion W2 is formed on the +Z side surface of the workpiece W by laser melting. The expanded portion W2 is formed by a volume expansion of the molten workpiece W.

[0060] The relationship between the pattern width and laser power illustrated in Fig. 9 varies depending on the type of workpiece. This is because the threshold laser power for laser etching the workpiece may vary depending on the material properties of the workpiece (e.g., laser absorptivity, thermal conductivity, expansion coefficient, etc.). Therefore, multiple relationships between laser power and laser spot size illustrated in Fig. 9 may be prepared in advance depending on the type of workpiece.

[0061] Next, a first example of a method for inspecting laser welding using the laser welding apparatus 50 will be described with reference to FIGS. 13 to 17. In FIGS. 13 to 17, the laser welding is inspected by inspecting whether the shape of the actual first pattern 212 is the same as the shape of a pre-designed first pattern. In other words, the presence or absence of various abnormalities, such as equipment abnormalities, and signs of various abnormalities can be determined in real time each time welding is performed, and the stability of the quality of the laser welding can be monitored. Note that even when the left-side second pattern 214, the right-side first pattern 222, and the right-side second pattern 224 are used, the laser welding can be inspected in the same way as when the first pattern 212 is used.

[0062] FIG. 13 is a diagram showing a first example of an abnormality in the shape of the first pattern 212. In FIG.

[0063] 13, the width of the first line pattern L1 in the Y direction between the end of the first line pattern L1 on the −X side and the intersection of the first line pattern L1 and the fourth line pattern L4 is narrower than the pre-designed width. From this abnormality in the shape of the first pattern 212, it can be inferred that there is an abnormality in the laser welding device 50, such as a decrease in the matching and tracking function of the laser oscillator 502 and the galvanometer mirror optical system 510, a decrease in the initial output of the laser oscillator 502, or an abnormality in the focus lens 508, or an abnormality on the side of the workpiece W, such as a misalignment of the workpiece W due to a setting error or a jig abnormality, or a deviation in the assembly accuracy of the workpiece W.

[0064] FIG. 14 is a diagram showing a second example of an abnormal shape of the first pattern 212. In FIG.

[0065] 14, the widths of all the line patterns in the first pattern 212 are narrower than the pre-designed width. From this shape abnormality in the first pattern 212, it can be inferred that there is an abnormality in the laser welding device 50, such as an abnormality in the focus lens 508, a decrease in the output of the laser oscillator 502, or an abnormality in the galvanometer mirror optical system 510, or an abnormality on the side of the workpiece W, such as a misalignment of the workpiece W due to a setting error or a jig abnormality, or a deviation in the assembly precision of the workpiece W.

[0066] FIG. 15 is a diagram showing a third example of an abnormal shape of the first pattern 212. In FIG.

[0067] 15 , the widths of all the line patterns of the first pattern 212 are wider than the pre-designed width. This abnormality in the shape of the first pattern 212 suggests an abnormality in the laser welding device 50, such as a decrease in the tracking function of the galvanometer mirror optical system 510, a malfunction of the galvanometer mirror optical system 510, a synchronization problem between the laser oscillator 502 and the galvanometer mirror optical system 510, or an excessive or reduced output of the laser oscillator 502, particularly an abnormality in the laser focus due to an abnormal operation of the focus lens 508.

[0068] FIG. 16 is a diagram showing a fourth example of an abnormal shape of the first pattern 212. In FIG.

[0069] In the example shown in Figure 16, the shape from the +X side end of the first line pattern L1, via the second line pattern L2 and the third line pattern L3, to the +Y side end of the fourth line pattern L4 is deformed from the pre-designed shape. Specifically, the shape from the +X side end of the first line pattern L1, via the second line pattern L2 and the third line pattern L3, to the +Y side end of the fourth line pattern L4 is a substantially circular pattern. Furthermore, the shape from the -Y side end of the fourth line pattern L4, via the fifth line pattern L5, to the sixth line pattern L6 is deformed from the pre-designed shape. Specifically, the shape from the -Y side end of the fourth line pattern L4, via the fifth line pattern L5, to the sixth line pattern L6 is a substantially elliptical pattern. This abnormality in the shape of the first pattern 212 suggests an abnormality in the laser welding device 50, such as a decrease in the tracking function of the galvanometer mirror optical system 510, a malfunction of the galvanometer mirror optical system 510, a poor synchronization between the laser oscillator 502 and the galvanometer mirror optical system 510, a decrease in the output of the laser oscillator 502, or an abnormality in the stage 550.

[0070] FIG. 17 is a diagram showing a fifth example of an abnormal shape of the first pattern 212. In FIG.

[0071] In the example shown in Figure 17, the shape from the +X side end of the first line pattern L1, via the second line pattern L2 and the third line pattern L3, to the +Y side end of the fourth line pattern L4 is deformed from the pre-designed shape. Specifically, the shape from the +X side end of the first line pattern L1, via the second line pattern L2 and the third line pattern L3, to the +Y side end of the fourth line pattern L4 is a substantially elliptical pattern. Furthermore, the corner between the -Y side end of the fourth line pattern L4 and the +X side end of the fifth line pattern L5, and the corner between the -X side end of the fifth line pattern L5 and the -Y side end of the sixth line pattern L6 are deformed from the pre-designed shape. Specifically, these corners are rounded. This abnormality in the shape of the first left pattern 212 suggests an abnormality in the laser welding device 50, such as an abnormality in the reduction ratio of the galvanometer mirror optical system 510, a decrease in the tracking function of the galvanometer mirror optical system 510, poor synchronization between the laser oscillator 502 and the galvanometer mirror optical system 510, or an abnormality in various optical systems.

[0072] 13 to 17, various abnormalities, such as abnormalities in the laser welding device 50, can be detected from abnormalities in the shape of the first pattern 212, and signs of these various abnormalities can be identified. Abnormalities in the shape of the first pattern 212 can be detected by relatively simple methods such as microscope observation or automatic image inspection. When observing abnormalities in the shape of the first pattern 212 using such methods, it is also possible to inspect the quality of the laser welding inline without stopping the production line. Therefore, factors that affect the quality of the laser welding can be inspected relatively easily.

[0073] 18 and 19, a second example of a method for inspecting laser welding using laser welding apparatus 50 will be described. In Fig. 18 and Fig. 19, laser welding is inspected by inspecting whether the shape of actual mark 210 is the same as or different from the shape of a pre-designed mark.

[0074] FIG. 18 is a diagram showing a first example of an abnormal shape of the mark 210. In FIG.

[0075] 18 , at least one of the first pattern 212 and the second pattern 214 is shifted in the Y direction from a pre-designed position. From this abnormality in the shape of the mark 210, it can be inferred that there is an abnormality in the laser welding device 50, such as an abnormality in the Y direction of the stage 550, an abnormality in the mechanical system of the galvanometer mirror optical system 510, or an abnormality in the irradiation position of the laser beam B, or an abnormality on the side of the workpiece W, such as an abnormality in the fixing jig for the workpiece W or an abnormality in the assembly of a structure including the workpiece W.

[0076] FIG. 19 is a diagram showing a second example of an abnormality in the mark 210. In FIG.

[0077] 19 , at least one of the first pattern 212 and the second pattern 214 is displaced in the X and Y directions from a pre-designed position. From this abnormality in the shape of the mark 210, it can be inferred that there is an abnormality in the laser welding device 50, such as an abnormality in the X and Y directions of the stage 550, an abnormality in the mechanical system of the galvanometer mirror optical system 510, or an abnormality in the irradiation position of the laser beam B, or an abnormality on the side of the workpiece W, such as an abnormality in the fixing jig for the workpiece W or an abnormality in the assembly of a structure including the workpiece W.

[0078] 18 to 19, similarly to the inspections described with reference to Figures 13 to 17, various abnormalities, such as abnormalities in the laser welding device 50, can be detected from abnormalities in the shape of the mark 210, and signs of the various abnormalities can be grasped. Therefore, factors that affect the quality of laser welding can be inspected relatively easily.

[0079] Next, a third example of the method for inspecting laser welding performed by the laser welding device 50 will be described with reference to FIG.

[0080] In this example, the laser welding is inspected by inspecting whether the actual positions of the left mark 210 and the right mark 220 are different from the predesigned positions of the left mark and the right mark. Specifically, heat generated during the formation of the laser weld 200 may cause deformation of the workpiece, such as elongation or displacement of the positive electrode tab 120. Deformation of the workpiece may cause fluctuations in at least one of the X-direction distance between the X-direction position of the left mark 210 and the X-direction position of the right mark 220, and the Y-direction distance between the Y-direction position of the left mark 210 and the Y-direction position of the right mark 220. For example, the deviation of the position of the right-side first pattern 222 relative to the left-side first pattern 212 from the design position can be used to determine deformation of the positive electrode tab 120 due to the influence of heat generated during the formation of the laser weld 200. Furthermore, after the influence of heat generated during the formation of the laser weld 200 has disappeared, the laser used to form the first right-side pattern 222 and the second left-side pattern 214 is irradiated. Even if the deformation of the positive electrode tab 120 returns to normal or the position of the first left-side pattern 212 shifts, various deformations of the positive electrode tab 120, such as the return of deformation of the positive electrode tab 120 and the shift in the position of the first left-side pattern 212, can be grasped. Therefore, the deformation of the workpiece due to laser welding can be estimated from the positions of the left-side mark 210 and the right-side mark 220. Therefore, factors that affect the quality of laser welding can be inspected relatively easily.

[0081] In addition, laser welding may be inspected by inspecting whether the shape of the actual mark 210 is the same as the shape of a pre-designed mark. For example, if an abnormality occurs in the laser output and the laser output becomes high, the mark 210 becomes distorted and cannot be read. Therefore, an abnormality in the laser output can be inferred from this abnormality in the mark 210. Therefore, factors that affect the quality of laser welding can be inspected relatively easily.

[0082] FIG. 20 is a diagram showing a laser-etched mark 210A according to a modified example.

[0083] The laser-etched mark 210A has an outer laser-etched pattern 212A (hereinafter simply referred to as the outer pattern 212A) and an inner laser-etched pattern 214A (hereinafter simply referred to as the inner pattern 214A). The outer pattern 212A is a substantially square frame pattern. The inner pattern 214A is a substantially square pattern. The inner pattern 214A is surrounded by the outer pattern 212A. In one example, the outer pattern 212A is formed, and then the inner pattern 214A is formed. In this example, the inner pattern 214A can be formed while there is an area surrounded by the outer pattern 212A. Therefore, compared to when the outer pattern 212A is formed after the inner pattern 214A is formed, visual inspection or inspection using a camera or the like to form the inner pattern 214A at the center of the outer pattern 212A in the XY plane can be simplified. However, the outer pattern 212A may be formed after the inner pattern 214A is formed. Alternatively, the inner pattern 214A and the outer pattern 212A may be formed simultaneously.

[0084] In the design of the laser etching mark 210A, the center of the outer pattern 212A in the XY plane and the center of the inner pattern 214A in the XY plane overlap each other in the Z direction. Therefore, if an abnormality occurs in the laser welding device 50, the center of the outer pattern 212A in the XY plane and the center of the inner pattern 214A in the XY plane may be misaligned. Therefore, from this abnormality in the laser etching mark 210A, it is possible to infer an abnormality in the laser welding device 50. Therefore, it is possible to relatively easily inspect factors that affect the quality of laser welding.

[0085] The shape of the laser-etched mark is not limited to the shapes described in the above-described embodiment and modified examples.

[0086] For example, the laser etching mark may have corners. In this example, an abnormality in the laser welding device 50 can be inferred from the roundness of the corners.

[0087] Alternatively, the laser etching mark may include a plurality of laser etching patterns that at least partially overlap each other. In this example, a malfunction of the laser welding apparatus 50 can be inferred from a misalignment of the plurality of laser etching patterns.

[0088] Alternatively, the laser etching mark may have a plurality of laser etching patterns whose centers overlap each other. In this example, an abnormality in the laser welding apparatus 50 can be inferred from the misalignment of the centers of the plurality of laser etching patterns.

[0089] FIG. 21 is a diagram for explaining another example of the laser welding inspection method according to the embodiment.

[0090] In the example shown in Fig. 21 , each of the positive electrode tab 120 and the negative electrode tab 130 and the bus bar 140 are joined to each other by a laser weld 200. In the example shown in Fig. 21 , the laser weld 200 that joins the positive electrode tab 120 and the bus bar 140 to each other is divided into two in the X direction. A left mark 210 and a right mark 220 are formed on both sides of the two divided laser welds 200 in the X direction. Similarly, the laser weld 200 that joins the negative electrode tab 130 and the bus bar 140 to each other is divided into two in the X direction. A left mark 210 and a right mark 220 are formed on both sides of the two divided laser welds 200 in the X direction.

[0091] 21 , as in the above-described example, factors that affect the quality of laser welding can be easily inspected using the left mark 210 and the right mark 220. Furthermore, from the inspection results of the left mark 210 and the right mark 220 provided on the positive electrode tab 120 or the negative electrode tab 130, the assembly position accuracy of various components during the manufacturing process of the battery module 10 or a product including the battery module 10 can be visualized, and can also be used for quality assurance of the battery module 10 or a product including the battery module 10.

[0092] FIG. 22 is a diagram for explaining another example of the laser welding inspection method according to the embodiment.

[0093] The housing 150 shown in Fig. 22 houses, for example, multiple battery cells 100 shown in Fig. 1 . The housing 150 has a top plate 151, a bottom plate 152, a front plate 153, a rear plate 154, a first side plate 155, and a second side plate 156. A portion of the top plate 151 that overlaps with the first side plate 155 and an upper end of the first side plate 155 are joined together by a laser weld 200. A first left pattern 212 and a first right pattern 222 are formed on both sides of the laser weld 200. A portion of the top plate 151 that overlaps with the second side plate 156 and an upper end of the second side plate 156 are joined together by the laser weld 200. A first left pattern 212 and a first right pattern 222 are formed on both sides of the laser weld 200.

[0094] In the example shown in Figure 22, as in the example described above, factors that affect the quality of laser welding can be easily inspected using the left-side first pattern 212 and the right-side first pattern 222.

[0095] Although the embodiments and modifications of the present invention have been described above with reference to the drawings, these are merely examples of the present invention, and various configurations other than those described above can also be adopted.

[0096] This application claims priority based on Japanese Patent Application No. 2023-056202, filed on March 30, 2023, the disclosure of which is incorporated herein in its entirety.

[0097] REFERENCE SIGNS LIST 10 battery module, 50 laser welding device, 100 battery cell, 110 exterior material, 120 positive electrode tab, 130 negative electrode tab, 140 bus bar, 150 housing, 151 top plate, 152 bottom plate, 153 front plate, 154 rear plate, 155 first side plate, 156 second side plate, 200 laser welded portion, 210 left side laser etching mark, left side mark, mark, 210A laser etching mark, 212 left side first laser etching pattern, left side first pattern, first pattern, 212A outer laser etching pattern, outer pattern, 214 left side second laser etching pattern, left side second pattern, second pattern, 214A inner laser etching pattern, inner pattern, 220 right side laser etching mark, right side mark, 222 right side first laser etching pattern, right side first pattern, 224 right side second laser etching pattern, right side second pattern, 502 Laser oscillator, 504 optical fiber, 506 beam expander, 508 focus lens, 510 galvanometer mirror optical system, 512 condenser lens, 514 movable mirror, 516 cover glass, 520 moving unit, 550 stage, A1 first arrow, A2 second arrow, A3 third arrow, A4 fourth arrow, A5 fifth arrow, A6 sixth arrow, B laser beam, L1 first line pattern, L2 second line pattern, L3 third line pattern, L4 fourth line pattern, L5 fifth line pattern, L6 sixth line pattern, W workpiece

Claims

1. A battery module comprising: a laser weld formed on an object to be processed; and a laser etching mark formed on at least one of both sides of the laser weld on the object to be processed.

2. The battery module according to claim 1, wherein the laser etched mark has a corner.

3. The battery module of claim 1, wherein the laser etched marks have a plurality of patterns that at least partially overlap one another.

4. The battery module of claim 1, wherein the laser etched marks have a plurality of patterns whose centers overlap each other.

5. The battery module according to any one of claims 1 to 4, wherein the laser-etched mark is inspected for similarity or difference from a predesigned laser-etched mark.

6. A method for manufacturing a battery module, comprising: a step of forming a laser weld in a workpiece; and a step of forming a laser etching mark on at least one of both sides of the laser weld in the workpiece.

7. A method for inspecting laser welding, comprising a step of inspecting whether a laser etching mark formed on a workpiece on which a laser weld is to be formed is different from a pre-designed laser etching mark.

Citation Information

Patent Citations

  • Electrode assembly and lithium secondary battery using it

    JP2006040875A

  • Surface-modified inorganic oxide, and toner composition containing surface-modified inorganic oxide

    JP2023056202A

  • Electrode plate, electrode body, and battery

    WO2019193869A1

  • Method and device for inspecting laser welding quality

    JP2005111538A

  • Laser weldment and laser welding quality determination method for battery