Clay and method for producing same
The clay composition, featuring a modified polyvinyl alcohol polymer and specific additives, addresses the limitations of traditional clays by enhancing elongation, formability, and smoothness, offering superior performance for craft applications.
Patent Information
- Application Number
- PCT/JP2024/007428
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-02-28
- Publication Date
- 2024-10-03
AI Technical Summary
Existing clay products with added polyvinyl alcohol lack sufficient performance in elongation, formability, and smoothness for craft applications, despite improvements in finish and prevention of shrinkage and cracking.
A clay composition containing a modified polyvinyl alcohol polymer with an alkyl vinyl ether unit, specific viscosity average degree of polymerization, saponification degree, and particle size distribution, combined with fibrous or inorganic powders and water, to enhance extensibility, formability, and smoothness.
The clay exhibits excellent stretchability, formability, and smoothness, surpassing the performance of traditional PVA-based clays, with optimal properties achieved through a synergistic effect of the polymer structure and composition.
Smart Images

Figure JP2024007428_03102024_PF_FP_ABST
Abstract
Description
Clay and its manufacturing method
[0001] The present invention relates to clay and a method for producing the same.
[0002] Clay products (hereinafter simply referred to as "clay") have long been used in a variety of applications, and various compositions have been proposed to improve their physical properties. It is also known to add polyvinyl alcohol as an adhesive component to clay, as described in Patent Document 1, for example.
[0003] Furthermore, Patent Document 2 discloses a clay characterized by comprising (A) a polyvinyl alcohol-α-olefin copolymer with a degree of saponification of 60 mol% or more, obtained by saponifying a copolymer of 90 to 99.99 mol% of vinyl acetate and 0.01 to 10 mol% of an α-olefin having 8 to 30 carbon atoms, (B) cellulose powder and / or mineral components, and (C) water, and claims that the clay improves workability, such as ductility, softness, and shape retention, and improves the finish by preventing shrinkage, cracking, unevenness, etc. due to drying.
[0004] Japanese Patent Publication No. 60-27033 Publication No. 63-289581
[0005] However, the clay to which polyvinyl alcohol has been added in the prior art has the problem that it still does not provide sufficient performance for craft applications, particularly in terms of extensibility, shaping ability, and smoothness.
[0006] The present invention has been made to solve the above-mentioned problems by using clay containing polyvinyl alcohol having a novel structure. That is, the present invention can provide the following aspects.
[0007] Aspect 1. A polymer having alkyl vinyl ether units represented by the following formula (wherein X represents an integer of 1 or more and 20 or less) in an amount of 0.1% by mass or more and 10.0% by mass or less, a modified polyvinyl alcohol-based polymer (A) having a viscosity average degree of polymerization of 500 to 5000, a degree of saponification of 65 to 99 mol%, and an undissolved matter content of 1 to 500 ppm, as measured by the method described in JIS K 6726:1994; a content of particles of 1000 μm or larger of 10.0 mass% or less, and a content of particles of 50 μm or smaller of 30.0 mass% or less; 5 to 50 mass% of one or more powders (B) selected from the group consisting of fibrous materials, inorganic materials, and synthetic resins; and 40 to 90 mass% of water (C).
[0008] Aspect 2. The clay according to Aspect 1, wherein the content of particles of 1000 μm or larger in size of component (A) is 2.0% by mass or less, or the content of particles of 50 μm or smaller in size is 10.0% by mass or less, or both of these conditions are satisfied.
[0009] Aspect 3. The clay of Aspect 1 or 2, wherein the content of component (A) is 2% by weight or more and 15% by weight or less, the content of component (B) is 5% by weight or more and 35% by weight or less, and the content of component (C) is 50% by weight or more and 80% by weight or less.
[0010] The clay according to the present invention exhibits excellent performance in craft applications, particularly excellent extensibility, shaping ability, and smoothness.
[0011] In this specification, polymers having a polyvinyl alcohol (PVA) backbone are collectively referred to as "polyvinyl alcohol-based polymers," "vinyl alcohol-based polymers," or simply "PVA." Numerical ranges in this specification include the lower and upper limits unless otherwise specified. The term "polymer" in this specification follows the definition of polymer by the International Union of Pure and Applied Chemistry (IUPAC) Commission on Macromolecular Nomenclature, namely, "a polymer molecule is a molecule having a large relative molecular mass and having a structure composed of multiple repetitions of units derived, substantially or conceptually, from molecules having a small relative molecular mass."
[0012] The clay according to the present invention is characterized by containing at least a modified polyvinyl alcohol polymer having a predetermined structure and physical properties as component (A), a predetermined powder as component (B), and water as component (C).
[0013] Component (A) may be a saponified polymer of a vinyl ester monomer or a copolymer of a vinyl ester monomer and another monomer, and is characterized by containing 0.1% by mass or more and 10.0% by mass or less of alkyl vinyl ether units having the following structure in its molecule: The content of these alkyl vinyl ether units is based on the total mass of component (A). In the above formula, X may be an integer of 1 or more and 20 or less, more preferably an integer of 5 or more and 18 or less, and even more preferably an integer of 7 or more and 17 or less.
[0014] By containing a certain amount of alkyl vinyl ether units, component (A) can provide clay with superior performance compared to existing PVA. Although this is only a hypothesis, it is thought that by having an appropriate amount of aliphatic side chains of an appropriate length in component (A), component (A) can be sufficiently dispersed in the clay, and by becoming entangled with the clay, it can impart excellent physical properties to the clay.
[0015] If the content of the alkyl vinyl ether unit is less than 0.1% by mass, the extensibility of the clay will be deteriorated. If the content of the alkyl vinyl ether unit is more than 10% by mass, the solubility in water will be reduced, the clay will become rough, and the smoothness will be deteriorated. Furthermore, from the viewpoint of improving the extensibility, shapeability, and smoothness of the clay, the content of the alkyl vinyl ether unit is preferably in the range of 0.5% by mass to 7.5% by mass, more preferably in the range of 0.5% by mass to 5.0% by mass, and even more preferably in the range of 0.5% by mass to 3.0% by mass.
[0016] The content of the alkyl vinyl ether unit is determined by the following procedure: 1 H-NMR and 13This can be calculated using C-NMR. For example, specifically, component (A) is saponified to a saponification degree of 99.95 mol % or more, and then thoroughly washed with methanol. The resulting polymer is dissolved in heavy water, and several drops of a heavy water solution of NaOH are added to adjust the pH to 14, and then 1 Measured at 80°C using H-NMR.
[0017] The viscosity average degree of polymerization of component (A), measured by the method described in JIS K 6726:1994, is in the range of 500 to 5000. If the viscosity average degree of polymerization is less than 500, the problem of deterioration in the extensibility of the clay occurs. If the viscosity average degree of polymerization is more than 5000, the solubility in water decreases, and the smoothness deteriorates. Furthermore, from the viewpoint of improving the extensibility, shaping ability, and smoothness of the clay, the viscosity average degree of polymerization is preferably in the range of 800 to 3000, more preferably in the range of 1200 to 3000, and even more preferably in the range of 1200 to 2500.
[0018] The saponification degree of component (A) is in the range of 65 mol% to 99 mol%. If the saponification degree is less than 65 mol%, the clay will be excessively hydrophobic, its solubility in water will decrease, and its extensibility will deteriorate. If the saponification degree is more than 99 mol%, the clay will be excessively crystalline, requiring high temperatures for dissolution in water, which will reduce workability during clay production and make the clay's performance more susceptible to deterioration. Furthermore, from the viewpoint of improving the extensibility, moldability, and smoothness of the clay, the saponification degree is preferably in the range of 75 mol% to 97 mol%, more preferably in the range of 75 mol% to 95 mol%. The saponification degree in this specification can be measured by the method described in Japanese Industrial Standard JIS K6726:1994, "3.5 Saponification Degree." After the saponification reaction of component (A), a washing process and a drying process may be performed, if necessary, to remove impurities such as sodium acetate.
[0019] The amount of undissolved matter contained in component (A) is in the range of 1 ppm to 500 ppm. If the amount of undissolved matter exceeds 500 ppm, the smoothness of the clay deteriorates. This is thought to be because an excessive amount of undissolved matter increases the insoluble content of component (A) in the clay, causing adverse effects. Furthermore, if the amount of undissolved matter in component (A) is less than 1 ppm, the extensibility of the clay deteriorates. This undissolved matter content ratio is relative to the total mass of component (A). Furthermore, from the viewpoint of improving the extensibility, moldability, and smoothness of the clay, the content of undissolved matter is preferably in the range of 10 ppm to 500 ppm, more preferably in the range of 50 ppm to 500 ppm, and even more preferably in the range of 50 ppm to 450 ppm.
[0020] The particle size distribution of component (A) is determined by the method described in JIS Z8815:1994, and is sieved using sieves with 1000 μm and 50 μm openings.
[0021] From the viewpoint of dissolution resistance, it is necessary that component (A) does not contain too many particles of too small size. Specifically, the particle ratio (particle content) of particles of 50 μm or less (50 μm sieve size) must be 30.0 mass% or less, preferably 20.0 mass% or less, and more preferably 10.0 mass% or less. If the content of particles of 50 μm or less exceeds 30.0 mass%, lumps tend to form when dissolved in water, which deteriorates workability during clay production.
[0022] In addition, it is necessary that component (A) does not contain a large number of particles of excessive size in order to avoid impairing the physical properties of the clay. Specifically, the particle content of particles of 1000 μm or more (1000 μm sieve) must be 10.0 mass% or less, preferably 8.5 mass% or less, and more preferably 2.0 mass% or less. If the content of particles of 1000 μm or more exceeds 10.0 mass%, the water solubility decreases and the extensibility of the clay deteriorates.
[0023] In a preferred embodiment, the particle size distribution of component (A) may be such that the content of particles of 1000 μm or more is 8.5% by mass or less and the content of particles of 50 μm or less is 20.0% by mass or less, and more preferably the content of particles of 1000 μm or more is 2.0% by mass or less and the content of particles of 50 μm or less is 10.0% by mass or less.
[0024] The inventors have newly discovered that the physical properties of component (A) described above, i.e., the content of alkyl vinyl ether units having a predetermined structure, the viscosity-average degree of polymerization, the degree of saponification, the content of undissolved matter, and the particle size distribution, when combined, produce a synergistic effect in the clay. In other words, simply satisfying these parameters individually does not necessarily improve the extensibility, moldability, and smoothness of the clay.
[0025] The clay in the present invention may be of any type, and may be paper clay, oil clay, wheat clay, rice clay, resin clay, etc. The preferred clay is paper clay.
[0026] Examples of vinyl ester monomers that serve as raw materials for component (A) include vinyl acetate, vinyl propionate, vinyl butyrate, vinyl valerate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl benzoate, and vinyl pivalate, and mixtures of these may also be used. From the viewpoint of ease of polymerization, vinyl acetate is preferred.
[0027] Examples of monomers other than vinyl ester monomers that can be used as raw materials for component (A) include the following compounds: α-olefin monomers such as ethylene and propylene; (meth)acrylic acid alkyl ester monomers such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate; unsaturated amide monomers such as (meth)acrylamide and N-methylolacrylamide; unsaturated carboxylic acid monomers such as (meth)acrylic acid, crotonic acid, maleic acid, itaconic acid, and fumaric acid; alkyl (methyl, ethyl, propyl, etc.) ester monomers of unsaturated carboxylic acids; unsaturated carboxylic acid anhydrides such as maleic anhydride; sodium, potassium, ammonium, etc. salts of unsaturated carboxylic acids; sulfonic acid group-containing monomers or salts thereof such as 2-acrylamido-2-methylpropanesulfonic acid; and alkyl vinyl ether monomers. Triallyl ether compounds such as glycerin triallyl ether, trimethylolpropane triallyl ether, and pentaerythritol triallyl ether. Compounds containing three allylamino groups such as triallylamine. Compounds containing three allyl groups such as triallyl isocyanurate and triallyl phosphate. Compounds having three (meth)acrylic acids such as glycerin tri(meth)acrylate, pentaerythritol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, and isocyanuric acid tri(meth)acrylate. Trifunctional aromatic monomers such as trivinylbenzene.
[0028] Component (A) can be produced by polymerizing the above-mentioned raw materials in an organic solvent (such as an alcohol) using a catalyst as needed. Such production can be carried out, for example, by referring to the description in International Publication No. 2019 / 163490 by the present applicant.
[0029] The content of component (A) in the clay is 1% by mass or more and 20% by mass or less, when the total of components (A) to (C) is 100% by mass. In a preferred embodiment, the amount of component (A) may be 2% by mass or more and 15% by mass or less, and more preferably 2% by mass or more and 10% by mass or less. When the amount of component (A) is within the above range, the extensibility, moldability, and smoothness of the clay are improved.
[0030] The component (B) contained in the clay is one or more powders selected from the group consisting of fibrous materials, inorganic materials, and synthetic resins, and is a component that functions as a base material for the clay.
[0031] Examples of fibrous materials include pulp, sawdust, cellulose, kenaf, vinylon fiber, etc. Pulp is preferably used.
[0032] Examples of inorganic substances that can be used include talc, kaolin, bentonite, calcium carbonate, shirasu balloon, and silica, with talc being preferred.
[0033] Examples of synthetic resins that can be used include cellulose derivatives such as carboxymethyl cellulose, styrene resins, and olefin resins, with carboxymethyl cellulose being preferred.
[0034] In a preferred embodiment, component (B) may contain two or more types selected from the group consisting of fibrous materials, inorganic materials, and synthetic resins, and more preferably may contain all three types.
[0035] The content of component (B) in the clay is 5% to 50% by mass, where the total of components (A) to (C) is 100% by mass. In a preferred embodiment, the amount of component (B) may be 5% to 35% by mass, and more preferably 10% to 35% by mass. When the amount of component (B) is within the above range, the extensibility, moldability, and smoothness of the clay are improved.
[0036] The water (C) acts as a solvent, and preferably pure water or ion-exchanged water with few impurities can be used. The content of the (C) component in the clay is 40% to 90% by mass when the total of the (A) to (C) components is 100% by mass. In a preferred embodiment, the amount of the (C) component may be 50% to 80% by mass, and more preferably 55% to 80% by mass. When the amount of the (C) component is within the above range, the clay's extensibility, moldability, and smoothness are improved.
[0037] In a preferred embodiment, when the total of components (A) to (C) is 100% by mass, the content of component (A) may be 2% to 15% by mass, the content of component (B) may be 5% to 35% by mass, and the content of component (C) may be 50% to 80% by mass. By having the amount of each component satisfy this condition, the extensibility, moldability, and smoothness of the clay can be further improved.
[0038] The present invention will be described in more detail below with reference to examples. Note that the examples described below are representative examples of the present invention, and the present invention is not limited to the following examples.
[0039] [Examples 1 to 8] PVA was produced with the physical properties adjusted as shown in the table in reference to the description of WO 2019 / 163490. The PVA and powder were mixed with water according to the formulation shown in the table to obtain clay according to each example.
[0040] Comparative Example 1 A polymer was prepared in the same manner as in Example 1, except that the PVA did not contain alkyl vinyl ether units.
[0041] Comparative Example 2 A polymer was prepared in the same manner as in Example, except that the PVA contained an excess of alkyl vinyl ether units and the viscosity-average degree of polymerization was excessively high.
[0042] Comparative Example 3 Preparation was carried out in the same manner as in Example, except that the degree of saponification of PVA was made excessively high and the amount of undissolved matter was made excessive.
[0043] Comparative Example 4 The same preparation as in Example was carried out except that the degree of saponification of PVA was too low and the amount of undissolved matter was too high.
[0044] Comparative Example 5 A resin was prepared in the same manner as in Example 1, except that the viscosity average degree of polymerization of PVA was made too low.
[0045] Comparative Example 6 The same preparation as in Example was carried out except that the proportion of particles of 1000 μm or more in the particle size distribution of the PVA was made excessively large.
[0046] Comparative Example 7 The same preparation as in Example was carried out except that the proportion of particles of 50 μm or less in the particle size distribution of the PVA was made excessively large.
[0047] Comparative Example 8 The same preparation as in Example 1 was carried out except that the PVA content was excessively high and the amount of water was excessively low.
[0048] [Saponification degree] Measured and calculated in accordance with the method described in Japanese Industrial Standard JIS K6726:1994 "3.5 Saponification degree".
[0049] [Viscosity Average Degree of Polymerization] Measured and calculated in accordance with Japanese Industrial Standard JIS K6726:1994 "3.7 Average Degree of Polymerization."
[0050] [Alkyl vinyl ether unit content] After saponifying the component (A) to a saponification degree of 99.95 mol % or more, the saponification degree is sufficiently washed with methanol, the resulting polymer is dissolved in heavy water, and then several drops of a heavy water solution of NaOH are added to adjust the pH to 14. 1 The content of alkyl vinyl ether units in component (A) was determined by H-NMR at 80°C.
[0051] [Amount of undissolved matter] 500 g of purified water and 10 g of component (A) were placed in a 1 L flask equipped with a stirrer, stirred at 90°C for 1 hour, and then cooled to 30°C. The resulting aqueous solution of component (A) was filtered using a nylon screen with 150 μm openings, and the amount of undissolved matter was calculated from the weight after drying at 150°C for 1 hour. The concentration of undissolved matter is relative to the total mass of component (A).
[0052]
[0053]
[0054] [Evaluation of stretchability] Each clay was molded into a sample measuring 100 mm x 100 mm x 50 mm in length x width x height. The clay sample was held at both ends with both hands and slowly pulled for at least one minute until it broke, and the stretched length was measured and evaluated according to the following criteria: ◎ (Excellent): Over 500 mm ○ (Good): Over 300 mm and up to 500 mm △ (Fair): Over 100 mm and up to 300 mm × (Fail): 100 mm or less
[0055] [Evaluation of shaping properties] Each clay was molded into a size of 100 mm length x width x height x 100 mm x 50 mm to create a sample. The clay sample was kneaded by hand, and the time it took to form a string with a diameter of 10 mm or less was measured and evaluated according to the following criteria: ◎ (Excellent): Can be formed into a string within 1 minute ○ (Good): Can be formed into a string within 1 to 2 minutes △ (Fair): Can be formed into a string within 2 to 3 minutes × (Fail): Cannot be formed into a string even after kneading for more than 3 minutes
[0056] [Evaluation of smoothness] Each clay was molded into a sample measuring 100 mm length x width x height x 100 mm x 5 mm. The clay sample was evaluated based on the number of bumps (lumps of components not sufficiently dispersed in the clay) that appeared on the surface, using the following criteria: ◎ (Excellent): 1 or less ○ (Good): 2 to 10 △ (Fair): 11 to 30 × (Poor): 31 or more
Claims
1. The alkyl vinyl ether unit represented by the following formula (wherein X is an integer of 1 or more and 20 or less) is contained in an amount of 0.1% by mass to 10.0% by mass.
1. A clay comprising: 1% by mass or more and 20% by mass or less of a modified polyvinyl alcohol-based polymer (A) having a viscosity average degree of polymerization of 500 to 5000, a degree of saponification of 65 to 99 mol%, and a content of undissolved matter in the range of 1 ppm to 500 ppm, as measured by the method described in JIS K 6726:1994; a content of particles of 1000 μm or more of 10.0 mass% or less, and a content of particles of 50 μm or less of 30.0 mass% or less; 5% by mass or more and 50% by mass or less of one or more powders (B) selected from the group consisting of fibrous substances, inorganic substances, and synthetic resins; and 40% by mass or more and 90% by mass or less of water (C).
2. A clay as described in claim 1, in which the content of particles of 1000 μm or larger in component (A) is 2.0 mass% or less, or the content of particles of 50 μm or smaller is 10.0 mass% or less, or both of these conditions are satisfied.
3. A clay according to claim 1 or 2, having a content of component (A) of 2% by mass or more and 15% by mass or less, a content of component (B) of 5% by mass or more and 35% by mass or less, and a content of component (C) of 50% by mass or more and 80% by mass or less.
Citation Information
Patent Citations
clay
JP1988289581A
Clay with excellent water resistance
JP2006243303A
Clay having water resistance and adhesiveness
JP2007331971A