Magnetic recording tape

The magnetic recording tape's innovative structure, featuring a boundary portion with high oxygen content in the underlayer and a central portion with lower oxygen content, addresses underlayer orientation and magnetic property issues, enhancing recording characteristics and durability.

WO2024203139A1PCT designated stage expired Publication Date: 2024-10-03NITTO DENKO CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/008895
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-07
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional magnetic recording tapes with perpendicular magnetic recording layers face issues with underlayer orientation and magnetic property deterioration due to specific alloy limitations, particularly with metals like Ti and Cr being prone to denaturation by oxygen or moisture.

Method used

A magnetic recording tape structure with a base material, underlayer, and perpendicular magnetic recording layer, where the underlayer has a boundary portion with a high oxygen content ratio and a central portion with lower oxygen content, enhancing orientation and adhesion without relying on specific alloys, and optionally including an oxide layer for improved durability.

Benefits of technology

This configuration improves underlayer orientation and magnetic recording characteristics, maintaining desired magnetic properties while increasing the productivity and durability of the tape.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024008895_03102024_PF_FP_ABST
    Figure JP2024008895_03102024_PF_FP_ABST
Patent Text Reader

Abstract

A magnetic recording tape 1a comprises a base material 10, a foundation layer 20, and a perpendicular magnetic recording layer 30. The base material 10, the foundation layer 20, and the perpendicular magnetic recording layer 30 are disposed in this order in the thickness direction of the foundation layer 20. The foundation layer 20 contains metal M. The foundation layer 20 has a boundary part 21 including a boundary surface closest to the base material 10 in the thickness direction of the foundation layer 20. The percentage of content of elements other than the metal M and oxygen in the boundary part 21 is less than 8% based on the number of atoms. The ratio of the content of oxygen in the boundary part 21 to the total amount of constituent elements and oxygen in a central part 22 is 5% or more based on the number of atoms.
Need to check novelty before this filing date? Find Prior Art

Description

magnetic recording tape

[0001] The present invention relates to magnetic recording tape.

[0002] Conventionally, magnetic recording tapes with perpendicular magnetic recording layers have been proposed.

[0003] For example, Patent Document 1 describes a magnetic recording medium including a substrate, a seed layer, an underlayer, and a magnetic recording layer. This magnetic recording medium is a single-layer perpendicular magnetic recording medium. The substrate is, for example, a long film. The seed layer is provided on the surface of the substrate. The underlayer is provided on the surface of the seed layer. The magnetic recording layer is provided on the surface of the underlayer. The seed layer is in an amorphous state and contains an alloy containing Ti, Cr, and O. The ratio of Ti to the total amount of Ti and Cr contained in the seed layer is 30 atomic % or more and 100 atomic % or less. The ratio of O to the total amount of Ti, Cr, and O contained in the seed layer is 15 atomic % or less.

[0004] JP 2014-241182 A

[0005] As the IoT society and digital transformation (DX) progress, the amount of data being processed is increasing, and it is expected to continue to grow in the future. In this context, magnetic recording tape is attracting attention as a data storage medium. Magnetic recording tape is a recording medium that can store a very large amount of data per volume and has few malfunctions or errors when writing. Another advantage is that, because data is stored offline, there is almost no risk of unauthorized access, such as hacking or ransomware. Furthermore, compared to hard disks, it generates less CO2 per data volume, which is why it is attracting attention from the perspective of the SDGs and the environment.

[0006] For example, a magnetic recording tape having a perpendicular magnetic recording layer formed by sputtering a material with high magnetic anisotropy can more easily increase the areal recording density than a coated magnetic recording tape. According to the technology described in Patent Document 1, it is understood that by adjusting the proportions of Ti and O contained in an amorphous seed layer containing Ti, Cr, and O within predetermined ranges, it is possible to suppress a decrease in the orientation of the underlayer and improve the magnetic properties.

[0007] In the magnetic recording medium described in Patent Document 1, the material for the seed layer is limited to a specific alloy, and problems caused by such alloys are expected to occur. For example, because Ti and Cr have a relatively high ionization tendency, it is expected that these metals will be denatured by oxygen or moisture, and that these metals will diffuse into the underlayer, resulting in a decrease in the performance of the magnetic recording medium. For this reason, the technology described in Patent Document 1 has room for reexamination from the perspective of improving the orientation of the underlayer without relying on a specific alloy.

[0008] In view of the above circumstances, the present invention provides a novel magnetic recording tape that has a perpendicular magnetic recording layer and is advantageous from the viewpoint of enhancing the orientation of the underlayer.

[0009] The present invention provides a magnetic recording tape comprising: a substrate; an underlayer containing a metal; and a perpendicular magnetic recording layer, wherein the substrate, underlayer, and perpendicular magnetic recording layer are arranged in this order in the thickness direction of the underlayer, the underlayer having a boundary portion including a boundary surface closest to the substrate in the thickness direction of the underlayer, and a central portion located between the boundary portion and the perpendicular magnetic recording layer in the thickness direction of the underlayer, the content of elements other than the metal and oxygen in the boundary portion being less than 8% on an atomic number basis, and the ratio of the oxygen content in the boundary portion to the total amount of constituent elements and oxygen in the central portion being 5% or more on an atomic number basis.

[0010] The above magnetic recording tape is advantageous from the viewpoint of having a perpendicular magnetic recording layer and enhancing the orientation of the underlayer.

[0011] FIG. 1 is a cross-sectional view showing an example of an embodiment of a magnetic recording tape.

[0012] Hereinafter, embodiments of the present invention will be described with reference to the drawings. Note that the following description is for illustrative purposes only and is not intended to limit the scope of the present invention.

[0013] As shown in FIG. 1 , the magnetic recording tape 1a includes a substrate 10, an underlayer 20, and a perpendicular magnetic recording layer 30. In the thickness direction of the underlayer 20, the substrate 10, the underlayer 20, and the perpendicular magnetic recording layer 30 are arranged in this order. The underlayer 20 contains a metal M. The underlayer 20 has a boundary portion 21 and a central portion 22. The central portion 22 is located between the boundary portion 21 and the perpendicular magnetic recording layer 30 in the thickness direction of the underlayer 20. The boundary portion 21 includes the boundary surface closest to the substrate 10 in the thickness direction of the underlayer 20. The content of elements other than the metal M and oxygen in the boundary portion 21 is less than 8% on an atomic number basis. The constituent element C of the central portion 22 in the boundary portion 21 22 The ratio of the oxygen content to the total amount of oxygen is 5% or more based on the number of atoms. 22 contains at least metal M. By having such a boundary portion 21 in the underlayer 20, the orientation of the underlayer 20 is likely to be high in the portion of the underlayer 20 between the boundary portion 21 and the perpendicular magnetic recording layer 30 in the thickness direction of the underlayer 20. This makes it easier for the perpendicular magnetic recording layer 30 to have large perpendicular magnetic anisotropy, and for the magnetic recording tape 1a to have desired magnetic recording characteristics. Moreover, the orientation of the underlayer 20 can be improved without relying on the specific alloy used in the seed layer described in Patent Document 1. This ratio may be 5% or more, 10% or more, 12% or more, or 15% or more, from the viewpoint of improving the orientation of the underlayer 20 in the above-mentioned portion.

[0014] Constituent element C in the boundary portion 21 22 The upper limit of the ratio of the oxygen content to the total amount of oxygen is not limited to a specific value. This ratio is, for example, 50% or less on an atomic number basis. In this case, adhesion between the boundary portion 21 and the central portion 22 is likely to be high. From the viewpoint of adhesion between the boundary portion 21 and the central portion 22, this ratio may be 45% or less, 40% or less, 35% or less, or 30% or less. This ratio may be included in any of the ranges determined by all combinations of a lower limit of any one of 5%, 10%, 12%, and 15% and an upper limit of any one of 50%, 45%, 40%, 35%, and 30%.

[0015] The oxygen content in the boundary portion 21 is higher than the oxygen content in the central portion 22, for example. With this configuration, the underlayer 20 is more likely to have a high degree of orientation, and the magnetic recording tape 1a is more likely to have the desired magnetic recording characteristics.

[0016] Constituent element C in the central portion 22 22 The ratio of the oxygen content to the total amount of oxygen is, for example, less than 5% on an atomic number basis, and may be 3% or less, or 1% or less, which makes it easier for the underlayer 20 to have high orientation and the magnetic recording tape 1a to have desired magnetic recording characteristics.

[0017] For example, in the underlayer 20, the oxygen content decreases from the boundary portion 21 toward the central portion 22 in the thickness direction of the underlayer 20. On the other hand, in the underlayer 20, the metal M content increases from the boundary portion 21 toward the central portion 22 in the thickness direction of the underlayer 20.

[0018] Thickness t of the underlayer 20 20 is not limited to a specific value. 20 is, for example, 2 nm or more, and may be 5 nm or more, 10 nm or more, or 15 nm or more. This makes it easier for the underlayer 20 to have high orientation, and the magnetic recording tape 1a to have the desired magnetic recording characteristics. 20 is, for example, 100 nm or less, and may be 90 nm or less, 80 nm or less, or 70 nm or less. This tends to increase the productivity of the magnetic recording tape 1a.

[0019] Thickness t of the underlayer 20 20 The thickness t of the boundary portion 21 21 The ratio t 21 / t 20 is not limited to a specific value. 21 / t 20 is, for example, 0.07 or more, and may be 0.10 or more, or 0.14 or more. This promotes crystal growth in the underlayer 20, making it easier to obtain high orientation. 21 / t 20 is, for example, 0.50 or less, and may be 0.35 or less, or 0.28 or less. This makes it easier for the adhesion of the underlayer 20 to be increased.

[0020] The metal M contained in the underlayer 20 is not limited to a specific metal as long as the perpendicular magnetic recording layer 30 can be formed. The metal M is, for example, Ru. The underlayer 20 may contain at least one selected from the group consisting of elemental Ru and alloys containing Ru. Examples of alloys containing Ru are RuTi, RuCr, RuCo, and RuPt. The alloys containing Ru preferably have a hexagonal close-packed crystal structure. With this configuration, the underlayer 20 is more likely to have high orientation, and the magnetic recording tape 1a is more likely to have desired magnetic recording characteristics.

[0021] 1, the magnetic recording tape 1a includes, for example, an oxide layer 40. As described above, the boundary portion 21 tends to increase the orientation of the underlayer 20, so, for example, it becomes possible to select a material for the oxide layer 40 without being bound by the orientation of the underlayer 20. For example, it is also possible to select a material for the oxide layer 40 that is considered advantageous from the standpoint of improving durability.

[0022] The material of the oxide layer 40 is not limited to a specific material. Examples of the material include SiO2, aluminum-doped ZnO (AZO), titanium oxide (TiO x ), aluminum oxide (AlO x ), zirconium oxide (ZrO x ), and cobalt oxide (CoO x ) In this case, the magnetic recording tape 1a is likely to have high durability. The oxygen content in the oxide layer 40 is, for example, higher than 30% on an atomic number basis. In this case, it is possible to prevent the performance of the magnetic recording tape 1a from being reduced due to components contained in the oxide layer 40.

[0023] 1 , the underlayer 20 is in contact with, for example, an oxide layer 40. The boundary portion 21 forms, for example, the interface between the underlayer 20 and the oxide layer 40. When forming a metal film on an oxide, the wettability of the metal to the oxide may be reduced, making it difficult to form the film so that the desired crystal plane faces in the film thickness direction. On the other hand, in the magnetic recording tape 1 a, because the boundary portion 21 forms the interface between the underlayer 20 and the oxide layer 40, the oxide layer 40 is less likely to affect the orientation of the underlayer 20 in, for example, the central portion 22, and the orientation of the underlayer 20 is likely to be high.

[0024] The thickness t of the oxide layer 40 40 is not limited to a specific value. 40 is, for example, 2 to 20 nm, and may be 4 to 15 nm or 6 to 10 nm.

[0025] The substrate 10 is not limited to a specific substrate. The substrate 10 includes a surface 11 having, for example, an arithmetic mean roughness Ra of 1.0 nm or less. For example, the oxide layer 40, the underlayer 20, and the perpendicular magnetic recording layer 30 are disposed on the surface 11. When the surface 11 has an arithmetic mean roughness Ra of 1.0 nm or less, the underlayer 20 is more likely to have high orientation, and the magnetic recording tape 1a is more likely to have desired magnetic recording characteristics. The arithmetic mean roughness Ra of the surface 11 can be determined, for example, in accordance with Japanese Industrial Standards (JIS) B0601 B:2013 from a roughness curve obtained by measuring the surface of the surface 11 using an atomic force microscope (AFM).

[0026] The arithmetic mean roughness Ra of the surface 11 may be 0.7 nm or less, or 0.5 nm or less. The arithmetic mean roughness Ra of the surface 11 is, for example, 0.01 nm or more.

[0027] The material of the substrate 10 is not limited to a specific material. The substrate 10 is, for example, a long film. Materials known as substrates for magnetic recording tapes can be used as the material of the substrate 10. Examples of materials for the substrate 10 include polyesters such as polyethylene terephthalate (PET), polyolefins, cellulose derivatives, vinyl resins, polyimides, polyamides, and polycarbonates.

[0028] Thickness t of the substrate 10 10 is not limited to a specific value. 10 is, for example, 2 to 75 μm.

[0029] The perpendicular magnetic recording layer 30 is not limited to a specific layer as long as it is compatible with perpendicular magnetic recording. The perpendicular magnetic recording layer 30 includes, for example, a Co-containing alloy. In this case, the magnetic recording tape 1a is likely to have a high areal recording density.

[0030] The perpendicular magnetic recording layer 30 is preferably a granular magnetic layer containing a Co-containing alloy. The granular magnetic layer includes, for example, ferromagnetic crystal grains containing a Co-containing alloy and nonmagnetic grain boundaries (nonmagnetic materials) surrounding the ferromagnetic crystal grains. For example, the granular magnetic layer includes columns (columnar crystals) containing a Co-containing alloy and nonmagnetic grain boundaries surrounding the columns and magnetically separating each column. This configuration allows the formation of a perpendicular magnetic recording layer 30 having a structure in which each column is magnetically separated.

[0031] The Co-containing alloy has, for example, a hexagonal close-packed (hcp) structure, and its c-axis is oriented in a direction perpendicular to the film surface of the perpendicular magnetic recording layer 30 (thickness direction). An example of the Co-containing alloy is a CoCrPt-based alloy containing Co, Cr, and Pt. The CoCrPt-based alloy may contain elements other than Co, Cr, and Pt. Examples of elements that can be added to the CoCrPt alloy are Ni and Ta. The CoCrPt-based alloy may contain only Co, Cr, and Pt.

[0032] The nonmagnetic grain boundaries in the granular magnetic layer contain, for example, a nonmagnetic metal material. Here, the metal may include a semimetal. The nonmagnetic grain boundaries contain, for example, at least one material selected from the group consisting of metal oxides and metal nitrides. An example of a metal oxide is a metal oxide containing at least one element selected from the group consisting of Si, Cr, Co, Al, Ti, Ta, Zr, Ce, Y, and Hf. The metal oxide preferably contains SiO. Other examples of metal oxides are CrO, CoO, AlO, TiO, TaO, ZrO, and HfO. An example of a metal nitride is a metal nitride containing at least one element selected from the group consisting of Si, Cr, Co, Al, Ti, Ta, Zr, Ce, Y, and Hf. Specific examples of metal nitrides are SiN, TiN, and AlN.

[0033] The magnetic recording tape 1a can be provided, for example, in a state where it is wound around the side surface of a cylindrical core material.

[0034] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0035] Example 1: A 50 μm-thick long PET film was transported at a predetermined speed, and a SiO layer approximately 10 nm thick was formed on the PET film by RF magnetron sputtering. In this RF magnetron sputtering, a Si target was used as the target, and a mixed gas of argon gas and oxygen gas was supplied as the process gas. The volume ratio of oxygen gas in the mixed gas was 20% based on standard cc / min (sccm). Next, while the PET film was transported at a predetermined speed, a base layer was formed on the SiO layer by DC magnetron sputtering. In this DC magnetron sputtering, a Ru target was used as the target. In the initial stage of this DC magnetron sputtering, a mixed gas of argon gas and oxygen gas was supplied as the process gas to form a boundary portion of the base layer. The thickness of the boundary portion was approximately 7 nm. The volume ratio of oxygen gas in the mixed gas was 16% based on sccm. In the steps following this initial step of DC magnetron sputtering, only argon gas was supplied as the process gas, resulting in the formation of a Ru-containing portion of approximately 40 nm on the boundary.

[0036] Next, while the PET film was being transported at a predetermined speed, a perpendicular magnetic recording layer having a thickness of about 25 nm was formed on the underlayer by DC magnetron sputtering. 74 Pt 16 Cr 10 ) 92 A target having a composition of -(SiO2)8 was used. Argon gas was supplied as the process gas. A granular magnetic layer was formed in the perpendicular magnetic recording layer, and columns (columnar crystals) containing a CoPtCr alloy and non-magnetic grain boundaries made of SiO2 that surrounded the columns and magnetically separated each column were present. In this way, the magnetic recording tape of Example 1 was produced.

[0037] Example 2 A magnetic recording tape according to Example 2 was produced in the same manner as Example 1, except for the following points: The volume ratio of oxygen gas in the process gas supplied in the initial stage of DC magnetron sputtering for forming the underlayer was adjusted to 10% on a sccm basis.

[0038] Example 3 A magnetic recording tape according to Example 3 was produced in the same manner as Example 1, except for the following points: The volume ratio of oxygen gas in the process gas supplied in the initial stage of DC magnetron sputtering for forming the underlayer was adjusted to 6% on a sccm basis.

[0039] Comparative Example 1 A magnetic recording tape according to Comparative Example 1 was produced in the same manner as in Example 1, except for the following points: Only argon gas was supplied as the process gas throughout the DC magnetron sputtering for forming the underlayer.

[0040] [Composition Analysis by XPS] Using a Quantera SXM X-ray photoelectron spectroscopy (XPS) system manufactured by ULVAC-PHI, Inc., XPS depth profile analysis was performed on the magnetic recording tapes according to each Example and Comparative Example 1. In this analysis, sputter etching using Ar ions was performed from the underlayer toward the substrate, and the composition of elements contained in the sample was identified at 1 nm intervals. The depth at which the content of Si, an element other than Ru and O, was less than 8% on an atomic basis was identified as the depth corresponding to the underlayer, and the boundary between the underlayer and the SiO2 layer was defined. Table 1 shows the ratio of the O content to the total amount of Ru and O on an atomic basis at the maximum depth at which the Si content was less than 8% on an atomic basis in the portions corresponding to the underlayer and SiO2 layer. Table 1 also shows the O content in the Ru-containing portion forming the center of the underlayer.

[0041] [Evaluation of Underlayer Orientation] Samples were prepared from the magnetic recording tapes of each Example and Comparative Example 1, with the underlayer forming the principal surface. Using a Smart Lab X-ray diffractometer manufactured by Rigaku Corporation, rocking curve measurements were performed on the principal surfaces of these samples for the Ru (0002) plane. From the measurement results, the full width at half maximum (FWHM) of the rocking curve (RC) for the Ru (0002) plane was calculated. The results are shown in Table 1.

[0042] [Evaluation of Magnetic Properties] Using a vibrating sample magnetometer option of the Versalab compact cryogen-free physical property evaluation system manufactured by Japan Quantum Design, the magnetic properties of samples prepared from the magnetic recording tapes according to each Example and Comparative Example 1 were evaluated, and M-H curves of the granular magnetic layers of the magnetic recording tapes according to each Example and Comparative Example 1 were obtained. The coercive force [kOe] and squareness ratio were determined from the obtained M-H curves. The squareness ratio is calculated by multiplying the saturation magnetization M s Remanent magnetization M r The results are shown in Table 1.

[0043] [Evaluation of Surface Roughness of Substrate] Using a Bruker Multimode 8 atomic force microscope, the surface condition of the PET film used in the examples and comparative examples on which the SiO layer and the like were formed was measured, and a roughness curve of the surface was obtained. From the obtained roughness curve, the arithmetic mean roughness Ra of the PET film surface was calculated according to JIS B0601 B:2013. As a result, the arithmetic mean roughness Ra of this surface was 0.27 nm.

[0044] As shown in Table 1, the half-width of the RC of the Ru (0002) plane of the underlayer according to each example was smaller than the half-width of the RC of the Ru (0002) plane of the underlayer according to Comparative Example 1. In addition, the magnetic properties of the perpendicular magnetic recording layer of the magnetic recording tape according to each example were better than the magnetic properties of the perpendicular magnetic recording layer of the magnetic recording tape according to Comparative Example 1. A comparison between the examples and the comparative examples suggests that when the ratio of the O content to the total amount of Ru and O at the boundary portion of the underlayer that forms the boundary with the SiO layer is 5% or more, the orientation of the underlayer is likely to be high, and the magnetic recording tape is likely to have the desired magnetic properties.

[0045]

[0046] A first aspect of the present disclosure provides a magnetic recording tape comprising: a substrate; an underlayer containing a metal; and a perpendicular magnetic recording layer, wherein the substrate, underlayer, and perpendicular magnetic recording layer are arranged in this order in the thickness direction of the underlayer, the underlayer having a boundary portion including a boundary surface closest to the substrate in the thickness direction of the underlayer, and a central portion located between the boundary portion and the perpendicular magnetic recording layer in the thickness direction of the underlayer, the content of elements other than the metal and oxygen in the boundary portion being less than 8% on an atomic number basis, and the ratio of the oxygen content in the boundary portion to the total amount of constituent elements and oxygen in the central portion being 5% or more on an atomic number basis.

[0047] A second aspect of the present disclosure provides the magnetic recording tape according to the first aspect, wherein the oxygen content in the boundary portion is higher than the oxygen content in the central portion.

[0048] A third aspect of the present disclosure provides a magnetic recording tape according to the first or second aspect, further comprising an oxide layer disposed between the substrate and the underlayer in a thickness direction of the underlayer.

[0049] A fourth aspect of the present disclosure provides the magnetic recording tape according to the third aspect, wherein the underlayer is in contact with the oxide layer.

[0050] A fifth aspect of the present disclosure provides a magnetic recording tape according to any one of the first to fourth aspects, wherein the substrate includes a surface having an arithmetic mean roughness Ra of 1.0 nm or less.

[0051] A sixth aspect of the present disclosure provides a magnetic recording tape according to any one of the first to fifth aspects, wherein the underlayer includes at least one selected from the group consisting of elemental Ru and alloys containing Ru.

[0052] A seventh aspect of the present disclosure provides the magnetic recording tape according to any one of the first to sixth aspects, wherein the perpendicular magnetic recording layer includes a Co-containing alloy.

Claims

1. A magnetic recording tape comprising: a substrate; an underlayer containing a metal; and a perpendicular magnetic recording layer, wherein the substrate, underlayer, and perpendicular magnetic recording layer are arranged in this order in the thickness direction of the underlayer, the underlayer having a boundary portion including a boundary surface closest to the substrate in the thickness direction of the underlayer, and a central portion located between the boundary portion and the perpendicular magnetic recording layer in the thickness direction of the underlayer, the content of elements other than the metal and oxygen in the boundary portion being less than 8% on an atomic number basis, and the ratio of the oxygen content in the boundary portion to the total amount of constituent elements and oxygen in the central portion being 5% or more on an atomic number basis.

2. The magnetic recording tape according to claim 1, wherein the oxygen content in the boundary portion is higher than the oxygen content in the central portion.

3. The magnetic recording tape of claim 1, further comprising an oxide layer disposed between said substrate and said underlayer in the thickness direction of said underlayer.

4. The magnetic recording tape of claim 3, wherein the underlayer is in contact with the oxide layer.

5. The magnetic recording tape of claim 1, wherein the substrate includes a surface having an arithmetic mean roughness Ra of 1.0 nm or less.

6. The magnetic recording tape of claim 1, wherein the underlayer comprises at least one selected from the group consisting of elemental Ru and alloys containing Ru.

7. The magnetic recording tape of claim 1 , wherein the perpendicular magnetic recording layer comprises a Co-containing alloy.

Citation Information

Patent Citations

  • Perpendicular magnetic recording medium and method of manufacturing the same

    JP2009070540A

  • Perpendicular magnetic recording medium

    JP2011141940A