Laminate

The laminate configuration with a protective layer, light absorption anisotropic layer, and pressure-sensitive adhesive layer addresses the flexibility issue in bending applications, enhancing the performance of image display devices by maintaining optical properties and privacy.

WO2024203224A1PCT designated stage expired Publication Date: 2024-10-03FUJIFILM CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/009324
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-03-11
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing laminates with light absorption anisotropic layers used in image display devices lack sufficient flexibility when applied to bending applications, such as foldable and curved displays.

Method used

A laminate configuration featuring a protective layer, a light absorption anisotropic layer with a dichroic substance, a liquid crystal compound, and a vertical alignment agent, along with a pressure-sensitive adhesive layer, arranged in a specific order to enhance flexibility.

Benefits of technology

The laminate achieves good flexibility even when applied to bending applications, improving the performance of image display devices by maintaining optical properties and preventing display content from being viewed from unwanted angles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024009324_03102024_PF_FP_ABST
    Figure JP2024009324_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention addresses the problem of providing a laminate having a light-absorbing anisotropic layer, the laminate exhibiting satisfactory flexibility even when used in bending applications. The laminate of the present invention comprises a protective layer, a light-absorbing anisotropic layer, an alignment film, and a bonding layer which are successively adjacently arranged in this order, wherein the light-absorbing anisotropic layer contains a dichroic substance, a liquid-crystalline compound and a vertical alignment agent, the angle θ formed by a transmittance center axis of the light-absorbing anisotropic layer and a normal direction of the surface of the light-absorbing anisotropic layer is 0° to 45° inclusive, and the bonding layer is a pressure-sensitive adhesive agent layer or an adhesive agent layer.
Need to check novelty before this filing date? Find Prior Art

Description

Laminate

[0001] The present invention relates to a laminate.

[0002] Image display devices such as liquid crystal display devices and organic electroluminescence (hereinafter abbreviated as "EL") display devices are widely used as displays for smartphones, laptop computers, and the like. In recent years, these devices have become thinner and lighter, making them easier to carry, and as a result, they are increasingly being used in transportation such as trains and airplanes, as well as in public places such as libraries and restaurants. Therefore, due to the need to protect personal information, confidential information, and the like, there is a demand for technology that prevents others from peeking at the content displayed on the image display device.

[0003] As a technology for controlling the viewing angle, for example, Patent Document 1 describes "an optical film having an optically absorptive anisotropic layer containing a liquid crystal compound and a dichroic substance, wherein the angle θ between the transmittance central axis of the optically absorptive anisotropic layer and the normal to the surface of the optically absorptive anisotropic layer is from 0° to 45°, and the haze value of the optical film is from 1% to 20%" ([Claim 1]). Furthermore, Patent Document 2 describes "an optically absorptive anisotropic layer formed from a liquid crystal composition containing a liquid crystal compound, a dichroic substance, and an alignment agent, wherein the liquid crystal compound exhibits a smectic liquid crystal state, the content of the dichroic substance is 5.0% by mass or more with respect to the total solid mass of the liquid crystal composition, and the angle θ between the transmittance central axis of the optically absorptive anisotropic layer and the normal to the surface of the optically absorptive anisotropic layer is from 0° to 45°" ([Claim 1]).

[0004] International Publication No. WO 2022 / 270466 International Publication No. WO 2023 / 276679

[0005] The present inventors have studied the laminates having the optically absorbing anisotropic layers described in Patent Documents 1 and 2, and have found that there is room for improvement in flexibility when the laminates are used in applications where bending occurs in components such as foldable displays and curved displays (hereinafter abbreviated as "bending applications").

[0006] Therefore, an object of the present invention is to provide a laminate having an optically absorptive anisotropic layer that exhibits good flexibility even when applied to bending applications.

[0007] As a result of intensive research to achieve the above object, the present inventors have found that by using a laminate having a protective layer, a light absorption anisotropic layer, an alignment film, and an attachment layer adjacent to each other in this order, flexibility is improved even when the laminate is used for bending applications, and have completed the present invention. That is, the present inventors have found that the above object can be achieved by the following configuration.

[0008] [1] A laminate comprising a protective layer, an optically absorbing anisotropic layer, an alignment film, and an attachment layer, arranged adjacently in this order, wherein the optically absorbing anisotropic layer contains a dichroic substance, a liquid crystal compound, and a vertical alignment agent, the angle θ between the transmittance central axis of the optically absorbing anisotropic layer and the normal direction to the surface of the optically absorbing anisotropic layer being 0° or more and 45° or less, and the attachment layer being a pressure-sensitive adhesive layer or an adhesive layer. [2] The laminate according to [1], wherein the optically absorbing anisotropic layer is a layer formed by fixing the alignment state of a liquid crystal composition containing a dichroic substance, a liquid crystal compound, a vertical alignment agent, and an additive having a crosslinkable group. [3] The laminate according to [2], wherein the crosslinkable group is an active hydrogen-reactive group, and the vertical alignment agent is an ionic vertical alignment agent. [4] The laminate according to any one of [1] to [3], wherein the vertical alignment agent comprises an ionic vertical alignment agent and a vertical alignment agent having a boronic acid group. [5] The laminate according to any one of [1] to [4], wherein at least one of the protective layer and the alignment film contains an additive having an active hydrogen reactive group. [6] The content of the dichroic material contained in the light absorption anisotropic layer is 20 to 650 mg / cm 3[7] The laminate according to any one of [1] to [6], wherein the degree of orientation of the optically absorptive anisotropic layer at a wavelength of 550 nm is 0.90 or more. [8] The laminate according to any one of [1] to [7], wherein the difference in the degree of orientation of the optically absorptive anisotropic layer at wavelengths of 450 nm, 550 nm, and 650 nm is 0.025 or less. [9] The laminate according to any one of [1] to [8], wherein the haze value of the optically absorptive anisotropic layer is 0.3% or less.

[10] The laminate according to any one of [1] to [9], wherein the thickness of the optically absorptive anisotropic layer is 1.5 μm or more.

[11] The laminate according to [2] or [3], wherein the dichroic substance contained in the liquid crystal composition is a compound having a polymerizable group.

[12] The laminate according to any one of [1] to

[11] , wherein at least one of the protective layer and the alignment film is either a polyvinyl alcohol-based resin or an acrylate-based resin.

[13] The laminate according to any one of [1] to

[12] , wherein the alignment film contains any one of a polyvinyl alcohol resin, a cinnamoyl group-containing resin, and an epoxy resin.

[14] The laminate according to any one of [1] to

[13] , wherein the protective layer is an acrylic resin film made of a polymer of a polyfunctional (meth)acrylate.

[15] The laminate according to any one of [1] to

[14] , further comprising at least one layer of a polarizer layer, an antireflection layer, and a retardation layer.

[16] The laminate according to

[15] , wherein the polarizer layer is a coating-type polarizer layer.

[0009] According to the present invention, it is possible to provide a laminate having an optically absorptive anisotropic layer that exhibits good flexibility even when applied to bending applications.

[0010] FIG. 1 is a schematic diagram showing an example of a head-mounted display having a laminate of the present invention (hereinafter also abbreviated as "head-mounted display of the present invention"); FIG. 2 is a schematic diagram showing an example of the configuration of a light guide plate for AR (Augmented Reality) glasses; FIG. 3 is a schematic diagram showing a plan view of an evaluation system for the head-mounted display of the present invention; and FIG. 4 is a schematic diagram showing an elevation view of an evaluation system for the head-mounted display of the present invention.

[0011] The present invention will be described in detail below. The following description of the constituent elements may be based on a representative embodiment of the present invention, but the present invention is not limited to such an embodiment. In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the upper and lower limits. In this specification, the upper or lower limit of a numerical range described in stages may be replaced with the upper or lower limit of another numerical range described in stages. In addition, the upper or lower limit of a numerical range described in this specification may be replaced with a value shown in an example.

[0012] In this specification, parallel and perpendicular do not mean parallel and perpendicular in the strict sense, but rather mean a range of parallel ±5° and a range of perpendicular ±5°, respectively.

[0013] In addition, in this specification, for each component, a substance corresponding to the component may be used alone or in combination of two or more. Here, when two or more substances for each component are used in combination, the content of the component refers to the total content of the substances used in combination, unless otherwise specified.

[0014] In addition, in this specification, "(meth)acrylate" is a notation representing "acrylate" or "methacrylate", "(meth)acrylic" is a notation representing "acrylic" or "methacrylic", and "(meth)acryloyl" is a notation representing "acryloyl" or "methacryloyl".

[0015] In this specification, Re(λ) and Rth(λ) represent the in-plane retardation and the thickness direction retardation, respectively, at a wavelength λ. Unless otherwise specified, the wavelength λ is 550 nm. In the present invention, Re(λ) and Rth(λ) are values ​​measured at a wavelength λ using an AxoScan (manufactured by Axometrics). By inputting the average refractive index ((nx + ny + nz) / 3) and the film thickness (d (μm)) into AxoScan, the following slow axis direction (°) is calculated: Re(λ) = R0(λ) Rth(λ) = ((nx + ny) / 2 - nz) × d. Note that R0(λ) is displayed as a numerical value calculated by AxoScan, but it means Re(λ).

[0016] In this specification, the refractive indices nx, ny, and nz are measured using an Abbe refractometer (NAR-4T, manufactured by Atago Co., Ltd.) with a sodium lamp (λ = 589 nm) as a light source. Wavelength dependency can be measured using a multi-wavelength Abbe refractometer DR-M2 (manufactured by Atago Co., Ltd.) in combination with an interference filter. Values ​​from the Polymer Handbook (John Wiley & Sons, Inc.) and catalogs of various optical films can also be used. Examples of average refractive index values ​​for major optical films are listed below: cellulose acylate (1.48), cycloolefin polymer (1.52), polycarbonate (1.59), polymethyl methacrylate (1.49), and polystyrene (1.59).

[0017] [Laminate] The laminate of the present invention has a protective layer, a light-absorbing anisotropic layer, an alignment film, and an attachment layer, arranged adjacently in this order. The light-absorbing anisotropic layer of the laminate of the present invention contains a dichroic substance, a liquid crystal compound, and a vertical alignment agent, and the angle θ between the transmittance central axis of the light-absorbing anisotropic layer and the normal direction to the surface of the light-absorbing anisotropic layer is 0° or more and 45° or less. The attachment layer of the laminate of the present invention is a pressure-sensitive adhesive layer or an adhesive layer.

[0018] Here, the term "central axis of transmittance of the optically absorbing anisotropic layer" refers to the direction exhibiting the highest transmittance when the transmittance is measured while varying the tilt angle (polar angle) and tilt direction (azimuth angle) relative to the normal direction of the optically absorbing anisotropic layer surface. Specifically, the Mueller matrix at a wavelength of 550 nm is measured using an AxoScan (OPMF-2, manufactured by Axometrics). More specifically, during measurement, the azimuth angle at which the central axis of transmittance is tilted is first determined. Next, within a plane containing the normal direction of the optically absorbing anisotropic layer along that azimuth angle (a plane containing the central axis of transmittance and perpendicular to the layer surface), the polar angle, which is the angle relative to the normal direction of the optically absorbing anisotropic layer surface, is changed in 1° increments from -70 to 70°, and the Mueller matrix at a wavelength of 550 nm is measured, thereby deriving the transmittance of the optically absorbing anisotropic layer. The resulting direction with the highest transmittance is designated the central axis of transmittance. The central axis of transmittance means the direction of the absorption axis (the direction of the long axis of the molecule) of the dichroic material contained in each light absorption anisotropic layer.

[0019] In the present invention, as described above, by using a laminate having a protective layer, a light absorption anisotropic layer, an alignment film, and an attachment layer adjacent to each other in this order, flexibility is improved even when applied to bending applications. The reason for this effect is not clear in detail, but the inventors speculate as follows. That is, the laminate of the present invention differs from a conventionally known laminate such as that shown in Comparative Example 1, i.e., a laminate having a support between the alignment film and the attachment layer, in the presence or absence of a support. Therefore, it is believed that the flexibility is improved in the present invention due to the absence of a support between the alignment film and the attachment layer. Below, the layer structure of each of the laminates of the present invention will be described in detail.

[0020] [Protective Layer] The protective layer of the laminate of the present invention is a layer provided adjacent to the optically absorptive anisotropic layer from the viewpoint of suppressing mutual diffusion of components such as dichroic substances contained in the optically absorptive anisotropic layer. A resin film is preferably used as the protective layer. Examples of the resin film include a PVA-based resin film made of polyvinyl alcohol (PVA) or its derivatives, an acrylic-based resin film made of a polymer of a polyfunctional (meth)acrylate, an epoxy-based resin film, a cellulose ester-based resin film, a polyethylene terephthalate resin film, and a polycarbonate resin film.

[0021] In the present invention, among the above-mentioned examples of resin films, PVA-based resin films and acrylic-based resin films made of a polymer of polyfunctional (meth)acrylate are more preferred because they provide better flexibility.

[0022] The thickness of the protective layer is not particularly limited, but is preferably 0.01 to 10 μm, more preferably 0.05 to 5 μm, and even more preferably 0.1 to 2 μm.

[0023] [Light-Absorption Anisotropic Layer] The light-absorption anisotropic layer of the laminate of the present invention is a layer containing a dichroic substance, a liquid crystal compound, and a vertical alignment agent. The angle θ between the central transmittance axis of the light-absorption anisotropic layer and the normal direction to the surface of the light-absorption anisotropic layer (hereinafter also referred to as "transmittance central axis angle θ") is 0° or more and 45° or less, preferably 0° or more and less than 45°, more preferably 0° or more and 35° or less, and even more preferably 0° or more and less than 35°.

[0024] <Dichroic Material> The light absorption anisotropic layer contains a dichroic material. Here, the dichroic material refers to a dye whose absorbance varies depending on the direction. The dichroic material may or may not exhibit liquid crystallinity.

[0025] The dichroic substance is not particularly limited, and examples thereof include visible light absorbing substances (dichroic dyes), luminescent substances (fluorescent substances, phosphorescent substances), ultraviolet absorbing substances, infrared absorbing substances, nonlinear optical substances, carbon nanotubes, and inorganic substances (e.g., quantum rods), and any conventionally known dichroic substance (dichroic dye) can be used. Specifically, for example, paragraphs

[0067] to

[0071] of JP 2013-228706 A, paragraphs

[0008] to

[0026] of JP 2013-227532 A, paragraphs

[0008] to

[0015] of JP 2013-209367 A, paragraphs

[0045] to

[0058] of JP 2013-14883 A, paragraphs

[0012] to

[0029] of JP 2013-109090 A, paragraphs

[0009] to

[0017] of JP 2013-101328 A, Paragraphs

[0051] to

[0065] of JP 2013-37353 A, paragraphs

[0049] to

[0073] of JP 2012-63387 A, paragraphs

[0016] to

[0018] of JP 11-305036 A, paragraphs

[0009] to

[0011] of JP 2001-133630 A, paragraphs

[0030] to

[0169] of JP 2011-215337 A, paragraphs

[0021] to

[0075] of JP 2010-106242 A, paragraphs

[0016] to

[0018] of JP 2010-215846 A

[0011] to

[0025] paragraphs,

[0017] to

[0069] paragraphs of JP 2011-048311 A,

[0013] to

[0133] paragraphs of JP 2011-213610 A,

[0074] to

[0246] paragraphs of JP 2011-237513 A,

[0005] to

[0051] paragraphs of JP 2016-006502 A,

[0014] to

[0032] paragraphs of JP 2018-053167 A, and

[0014] to

[0033] paragraphs of JP 2020-11716 A paragraphs

[0005] to

[0041] of International Publication No. 2016 / 060173, paragraphs

[0008] to

[0062] of International Publication No. 2016 / 136561, paragraphs

[0014] to

[0033] of International Publication No. 2017 / 154835, paragraphs

[0014] to

[0033] of International Publication No. 2017 / 154695, paragraphs

[0013] to

[0037] of International Publication No. 2017 / 195833, paragraphs

[0014] to

[0034] of International Publication No. 2018 / 164252,Examples include those described in paragraphs

[0021] to

[0030] of International Publication No. 2018 / 186503, paragraphs

[0043] to

[0063] of International Publication No. 2019 / 189345, paragraphs

[0043] to

[0085] of International Publication No. 2019 / 225468, paragraphs

[0050] to

[0074] of International Publication No. 2020 / 004106, and paragraphs

[0015] to

[0038] of International Publication No. 2021 / 044843.

[0026] As the dichroic substance, a dichroic azo dye compound is preferred. A dichroic azo dye compound refers to an azo dye compound whose absorbance varies depending on the direction. A dichroic azo dye compound may or may not exhibit liquid crystallinity. When a dichroic azo dye compound exhibits liquid crystallinity, it may exhibit either nematic or smectic properties. The temperature range in which the liquid crystal phase is exhibited is preferably room temperature (approximately 20 to 28°C) to 300°C, and more preferably 50 to 200°C from the viewpoints of handleability and manufacturing suitability.

[0027] In the present invention, from the viewpoint of adjusting color hue, it is preferable to use at least one dye compound (first dichroic azo dye compound) having a maximum absorption wavelength in the wavelength range of 560 to 700 nm, and at least one dye compound (second dichroic azo dye compound) having a maximum absorption wavelength in the wavelength range of 455 nm or more and less than 560 nm.

[0028] In the present invention, three or more kinds of dichroic azo dye compounds may be used in combination. For example, in order to make the light absorption anisotropic layer closer to black, it is preferable to use a first dichroic azo dye compound, a second dichroic azo dye compound, and at least one dye compound (third dichroic azo dye compound) having a maximum absorption wavelength in the wavelength range of 380 nm or more and less than 455 nm in combination.

[0029] In the present invention, the dichroic azo dye compound preferably has a crosslinkable group, such as a cationically polymerizable group such as an epoxy group, an epoxycyclohexyl group, or an oxetanyl group; or a radically polymerizable group such as an acryloyl group, a methacryloyl group, a vinyl group, a styryl group, or an allyl group.

[0030] The content of the dichroic material contained in the optically absorptive anisotropic layer is not particularly limited, but is preferably 3% by mass or more, more preferably 8% by mass or more, even more preferably 10% by mass or more, and particularly preferably 10 to 30% by mass, relative to the total mass of the optically absorptive anisotropic layer, because this increases the degree of orientation of the optically absorptive anisotropic layer that is formed. When multiple dichroic materials are used in combination, the total amount of the multiple dichroic materials is preferably within the above-mentioned range. Furthermore, the content of the dichroic material contained in the optically absorptive anisotropic layer is preferably 20 to 650 mg / cm, because this increases the degree of orientation of the optically absorptive anisotropic layer that is formed. 3 is preferably 25 to 500 mg / cm 3 is preferably 30 to 200 mg / cm 3 More preferably, it is 40 to 150 mg / cm 3 When a plurality of dichroic substances are used in combination, the total amount of the dichroic substances is preferably in the above-mentioned range. 3 The dichroic substance content can be obtained by measuring a solution in which a laminate having an optically absorptive anisotropic layer is dissolved or an extract obtained by immersing the laminate in a solvent using high-performance liquid chromatography (HPLC), but is not limited to the above method. Quantification can be performed using the dichroic substance contained in the optically absorptive anisotropic layer as a standard sample. One example of a method for calculating the content of the dichroic substance is to calculate the volume by multiplying the thickness of the optically absorptive anisotropic layer obtained from a microscopic image of the cross section of the laminate by the area of ​​the optical laminate used to measure the dye amount, and then dividing the volume by the amount of dye measured by HPLC to calculate the dye content.

[0031] <Liquid Crystal Compound> The light absorption anisotropic layer contains a liquid crystal compound. This allows the dichroic material to be aligned with a higher degree of orientation while suppressing precipitation of the dichroic material. As the liquid crystal compound, either a polymer liquid crystal compound or a low molecular weight liquid crystal compound can be used, with a polymer liquid crystal compound being preferred because it allows for a higher degree of orientation. Furthermore, as the liquid crystal compound, a polymer liquid crystal compound and a low molecular weight liquid crystal compound may be used in combination. Here, "polymer liquid crystal compound" refers to a liquid crystal compound having a repeating unit in its chemical structure. Furthermore, "low molecular weight liquid crystal compound" refers to a liquid crystal compound having no repeating unit in its chemical structure. Examples of polymer liquid crystal compounds include the thermotropic liquid crystal polymers described in JP 2011-237513 A and the polymer liquid crystal compounds described in paragraphs

[0012] to

[0042] of WO 2018 / 199096 A. Examples of low molecular weight liquid crystal compounds include those described in paragraphs

[0072] to

[0088] of JP 2013-228706 A, and among them, liquid crystal compounds exhibiting smectic properties are preferred. Examples of such liquid crystal compounds include those described in paragraphs

[0019] to

[0140] of WO 2022 / 014340 A, the disclosures of which are incorporated herein by reference.

[0032] The content of the liquid crystal compound in the light absorption anisotropic layer is preferably 25 to 2,000 parts by mass, more preferably 100 to 1,300 parts by mass, and even more preferably 200 to 900 parts by mass, relative to 100 parts by mass of the dichroic substance. When the content of the liquid crystal compound is within the above range, the degree of orientation of the dichroic substance is further improved. The liquid crystal compound may be contained alone, or two or more types may be contained. When two or more types of liquid crystal compounds are contained, the content of the liquid crystal compounds refers to the total content of the liquid crystal compounds.

[0033] <Vertical Alignment Agent> The optically absorptive anisotropic layer contains a vertical alignment agent. Here, the vertical alignment agent refers to an additive that has the function of aligning the liquid crystal compound in a direction perpendicular to the main plane of the optically absorptive anisotropic layer. Note that "vertical alignment" does not require alignment at a strict 90° angle, but means alignment at an angle of 70 to 110°.

[0034] Examples of vertical alignment agents include ionic vertical alignment agents and vertical alignment agents having a boronic acid group. It is preferable to use an ionic vertical alignment agent and a vertical alignment agent having a boronic acid group in combination, because this improves the transfer quality (the property of not causing stretching, tearing, wrinkles, creases, etc.) of the light absorption anisotropic layer when the laminate of the present invention is attached (transferred) to another member via the attachment layer of the laminate of the present invention.

[0035] Suitable examples of the ionic vertical alignment agent include onium compounds represented by the following formula (B1).

[0036] In the formula (B1), ring A represents a quaternary ammonium ion consisting of a nitrogen-containing heterocycle, and X represents an anion. 1 represents a divalent linking group. 2 represents a single bond or a divalent linking group. 1 represents a divalent linking group having a 5-membered or 6-membered ring as a partial structure. Z represents a divalent linking group having an alkylene group having 2 to 20 carbon atoms as a partial structure. P 1 and P 2 each independently represents a monovalent substituent having a polymerizable ethylenically unsaturated bond.

[0037] Ring A represents a quaternary ammonium ion consisting of a nitrogen-containing heterocycle. Examples of ring A include a pyridine ring, a picoline ring, a 2,2'-bipyridyl ring, a 4,4'-bipyridyl ring, a 1,10-phenanthroline ring, a quinoline ring, an oxazole ring, a thiazole ring, an imidazole ring, a pyrazine ring, a triazole ring, and a tetrazole ring, and are preferably a quaternary imidazolium ion or a quaternary pyridinium ion.

[0038] X represents an anion. Examples of X include halogen anions (e.g., fluorine ion, chloride ion, bromide ion, iodide ion, etc.), sulfonate ions (e.g., methanesulfonate ion, trifluoromethanesulfonate ion, methyl sulfate ion, vinyl sulfonate ion, allyl sulfonate ion, p-toluenesulfonate ion, p-chlorobenzenesulfonate ion, p-vinylbenzenesulfonate ion, 1,3-benzenedisulfonate ion, 1,5-naphthalenedisulfonate ion, 2,6-naphthalenedisulfonate ion, etc.), sulfate ion, carbonate ion, nitrate ion, thiocyanate ion, perchlorate ion, tetrafluoroborate ion, picrate ion, acetate ion, benzoate ion, p-vinylbenzoate ion, formate ion, trifluoroacetate ion, phosphate ion (e.g., hexafluorophosphate ion), hydroxide ion, etc. Preferred are halogen anions, sulfonate ions, and hydroxide ions. Particularly preferred are chloride ions, bromide ions, iodide ions, methanesulfonate ions, vinylsulfonate ions, p-toluenesulfonate ions, and p-vinylbenzenesulfonate ions.

[0039] L 1 represents a divalent linking group. 1 Examples of the group include an alkylene group, —O—, —S—, —CO—, and —SO 2 -, -NRa- (wherein Ra is an alkyl group having 1 to 5 carbon atoms or a hydrogen atom), an alkenylene group, an alkynylene group, or a divalent linking group having 1 to 20 carbon atoms formed in combination with an arylene group. 1 is preferably -AL-, -O-AL-, -CO-O-AL-, or -O-CO-AL- having 1 to 10 carbon atoms, more preferably -AL- or -O-AL- having 1 to 10 carbon atoms, and most preferably -AL- or -O-AL- having 1 to 5 carbon atoms. AL represents an alkylene group.

[0040] L2 represents a single bond or a divalent linking group. 2 Examples of the group include an alkylene group, —O—, —S—, —CO—, and —SO 2-, -NRa- (wherein Ra is an alkyl group having 1 to 5 carbon atoms or a hydrogen atom), an alkenylene group, a divalent linking group having 1 to 10 carbon atoms formed in combination with an alkynylene group or an arylene group, a single bond, -O-, -O-CO-, -CO-O-, -O-AL-O-, -O-AL-O-CO-, -O-AL-CO-O-, -CO-O-AL-O-, -CO-O-AL-O-CO-, -CO-O-AL-CO-O-, -O-CO-AL-O-, -O-CO-AL-O-CO-, -O-CO-AL-CO-O-, and the like. AL represents an alkylene group. L2 is preferably a single bond, -AL-, -O-AL-, or -NRa-AL-O- having 1 to 10 carbon atoms, more preferably a single bond, -AL-, -O-AL-, or -NRa-AL-O- having 1 to 5 carbon atoms, and most preferably a single bond, or -O-AL- or -NRa-AL-O- having 1 to 5 carbon atoms.

[0041] Y 1 represents a divalent linking group having a 5- or 6-membered ring as a partial structure. 1 Examples of the aromatic ring include a cyclohexyl ring, an aromatic ring, a heterocyclic ring, etc. Examples of the aromatic ring include a benzene ring, an indene ring, a naphthalene ring, a fluorene ring, a phenanthrene ring, an anthracene ring, a biphenyl ring, and a pyrene ring, with a benzene ring, a biphenyl ring, and a naphthalene ring being particularly preferred. The heteroatom constituting the heterocycle is preferably a nitrogen atom, an oxygen atom, or a sulfur atom, and examples thereof include a furan ring, a thiophene ring, a pyrrole ring, a pyrroline ring, a pyrrolidine ring, an oxazole ring, an isoxazole ring, a thiazole ring, an isothiazole ring, an imidazole ring, an imidazoline ring, an imidazolidine ring, a pyrazole ring, a pyrazoline ring, a pyrazolidine ring, a triazole ring, a furazan ring, a tetrazole ring, a pyran ring, a dioxane ring, a dithiane ring, a thiine ring, a pyridine ring, a piperidine ring, an oxazine ring, a morpholine ring, a thiazine ring, a pyridazine ring, a pyrimidine ring, a pyrazine ring, a piperazine ring, and a triazine ring. The heterocycle is preferably a 6-membered ring. Y 1 The divalent linking group having a 5- or 6-membered ring as a partial structure, represented by the following formula (I), may further have a substituent (for example, the above-mentioned substituent W).

[0042] Y 1 is preferably a divalent linking group having two or more 5- or 6-membered rings, and more preferably has a structure in which two or more rings are linked by a linking group. Examples of the linking group include the examples of the linking groups represented by L1 and L2, -C≡C-, -CH═CH-, -CH═N-, -N═CH-, and -N═N-.

[0043] Z represents a divalent linking group having an alkylene group having 2 to 20 carbon atoms as a partial structure and formed by combining -O-, -S-, -CO-, or -SO2-, and the alkylene group may have a substituent. Examples of the divalent linking group include an alkyleneoxy group and a polyalkyleneoxy group. The alkylene group represented by Z preferably has 2 to 16 carbon atoms, more preferably 2 to 12 carbon atoms, and particularly preferably 2 to 8 carbon atoms.

[0044] P1 and P2 each independently represent a monovalent substituent having a polymerizable ethylenically unsaturated group. Examples of the monovalent substituent having a polymerizable ethylenically unsaturated group include the following formulae (M-1) to (M-8). That is, the monovalent substituent having a polymerizable ethylenically unsaturated group may be a substituent consisting only of an ethenyl group, as in (M-8).

[0045]

[0046] In formulas (M-3) and (M-4), R represents a hydrogen atom or an alkyl group, preferably a hydrogen atom or a methyl group. Among the formulas (M-1) to (M-8), (M-1), (M-2), and (M-8) are preferred, with (M-1) or (M-8) being more preferred. In particular, (M-1) is preferred as P1. Furthermore, (M-1) or (M-8) is preferred as P2. In compounds in which ring A is a quaternary imidazolium ion, P2 is preferably (M-8) or (M-1), and in compounds in which ring A is a quaternary pyridinium ion, P2 is preferably (M-1).

[0047] Examples of the onium compound represented by formula (B1) include the onium salts described in paragraphs

[0052] to

[0058] of JP-A No. 2012-208397, the onium salts described in paragraphs

[0024] to

[0055] of JP-A No. 2008-026730, and the onium salts described in JP-A No. 2002-37777.

[0048] As the ionic vertical alignment agent, in addition to the onium compound represented by the above formula (B1), for example, those described in paragraphs

[0017] to

[0029] of JP-A-2020-181150 can be mentioned.

[0049] A preferred example of the vertical alignment agent having a boronic acid group is a boronic acid compound represented by the following formula (B2).

[0050] In (B2) above, R 1 and R 2 each independently represents a hydrogen atom, an aliphatic hydrocarbon group which may have a substituent, an aryl group which may have a substituent, or a heterocyclic group which may have a substituent. 3 represents a substituent.

[0051] R 1 and R 2 Examples of the aliphatic hydrocarbon group represented by one embodiment of the formula include substituted or unsubstituted linear or branched alkyl groups having 1 to 20 carbon atoms (e.g., methyl, ethyl, isopropyl, etc.), substituted or unsubstituted cyclic alkyl groups having 3 to 20 carbon atoms (e.g., cyclohexyl, etc.), and alkenyl groups having 2 to 20 carbon atoms (e.g., vinyl, etc.). 1 and R 2 Examples of the aryl group represented by one embodiment of R include a substituted or unsubstituted phenyl group having 6 to 20 carbon atoms (for example, a phenyl group, a tolyl group, etc.), and a substituted or unsubstituted naphthyl group having 10 to 20 carbon atoms. 1 and R 2Examples of the heterocyclic group represented by one embodiment of R include substituted or unsubstituted 5- or 6-membered ring groups containing at least one heteroatom (e.g., nitrogen atom, oxygen atom, sulfur atom, etc.), and specific examples include a pyridyl group, an imidazolyl group, a furyl group, a piperidyl group, and a morpholino group. 1 and R 2 may be linked together to form a ring, for example, R 1 and R 2 The isopropyl groups may be linked to form a 4,4,5,5-tetramethyl-1,3,2-dioxaborolane ring.

[0052] R 1 and R 2 is preferably a hydrogen atom, a linear or branched alkyl group having 1 to 3 carbon atoms, or a ring formed by linking these groups, and more preferably a hydrogen atom.

[0053] R 3 is preferably a substituent containing a functional group capable of bonding to a (meth)acrylic group. Here, examples of the functional group capable of bonding to a (meth)acrylic group include a vinyl group, an acrylate group, a methacrylate group, an acrylamide group, a styryl group, a vinyl ketone group, a butadiene group, a vinyl ether group, an oxiranyl group, an aziridinyl group, and an oxetane group. Among these, a vinyl group, an acrylate group, a methacrylate group, a styryl group, an oxiranyl group, or an oxetane group is preferred, and a vinyl group, an acrylate group, an acrylamide group, or a styryl group is more preferred.

[0054] R 3is preferably a substituted or unsubstituted aliphatic hydrocarbon group, an aryl group, or a heterocyclic group having a functional group capable of bonding to a (meth)acrylic group. Examples of the aliphatic hydrocarbon group include a substituted or unsubstituted linear or branched alkyl group having 1 to 30 carbon atoms (e.g., methyl group, ethyl group, isopropyl group, n-propyl group, butyl group, pentyl group, hexyl group, heptyl group, octyl group, nonyl group, decyl group, undecyl group, dodecyl group, tridecyl group, hexadecyl group, octadecyl group, eicosyl group, isopropyl group, isobutyl group, sec-butyl group, tert Examples of the aryl group include substituted or unsubstituted phenyl groups having 6 to 50 carbon atoms (e.g., phenyl, tolyl, styryl, 4-benzoyloxyphenyl, 4-phenoxycarbonylphenyl, 4-biphenyl, 4-(4-octyloxybenzoyloxy)phenoxycarbonylphenyl), and substituted or unsubstituted naphthyl groups having 10 to 50 carbon atoms (e.g., unsubstituted naphthyl).Examples of heterocyclic groups include substituted or unsubstituted 5- or 6-membered ring groups containing at least one heteroatom (e.g., nitrogen atom, oxygen atom, sulfur atom, etc.), and examples thereof include pyrrole, furan, thiophene, pyrazole, imidazole, triazole, oxazole, isoxazole, oxadiazole, thiazole, thiadiazole, indole, carbazole, benzofuran, dibenzofuran, thianaphthene, dibenzothiophene, indazole, benzimidazole, anthranil, benzisoxazole, benzoxazole, benzothiazole, purine, pyridine, pyridazine, pyrimidine, pyrazine, triazine, quinoline, acridine, isoquinoline, phthalazine, quinazoline, quinoxaline, naphthyridine, phenanthroline, pteridine, morpholine, and piperidine groups.

[0055] Examples of the boronic acid compound represented by formula (B2) include the boronic acid compounds represented by general formula (I) described in paragraphs 0023 to 0032 of JP-A No. 2008-225281. Preferred examples of the compound represented by formula (B2) include the compounds exemplified below.

[0056]

[0057] The content of the vertical alignment agent in the light absorption anisotropic layer is preferably 1.0 to 7.0 parts by mass, more preferably 1.5 to 8.0 parts by mass, and even more preferably 2.5 to 6.0 parts by mass, relative to 100 parts by mass of the liquid crystal compound. The vertical alignment agent may be contained alone or in combination of two or more types. When two or more types of liquid crystal compounds are contained, the content of the vertical alignment agent refers to the total content of the vertical alignment agents.

[0058] In the present invention, the optically absorptive anisotropic layer is preferably a layer obtained by fixing the alignment state of a liquid crystal composition containing the above-mentioned dichroic substance, liquid crystal compound, and vertical alignment agent, and more preferably a layer obtained by fixing the alignment state of a liquid crystal composition containing the above-mentioned dichroic substance, liquid crystal compound, and vertical alignment agent, as well as an additive having a crosslinkable group (hereinafter also referred to as a "crosslinkable group-containing additive") that does not fall under these components, because this improves the transfer quality of the optically absorptive anisotropic layer. Furthermore, the dichroic substance contained in the liquid crystal composition is preferably a dichroic substance having a polymerizable group among the above-mentioned dichroic substances, and more preferably a dichroic substance having a radically polymerizable group.

[0059] <Crosslinking Group-Containing Additive> Examples of the crosslinking group contained in the crosslinking group-containing additive include a radical polymerizable group and an active hydrogen reactive group. Among these, an active hydrogen reactive group is preferred. Here, the "active hydrogen reactive group" refers to a carboxyl group (-COOH), a hydroxyl group (-OH), an amino group (-NH 2 The term "active hydrogen reactive group" refers to a group reactive to a group having active hydrogen (active hydrogen group), such as an epoxy group, a glycidyl group, an isocyanate group, a thioisocyanate group, an alkoxysilyl group, an oxazoline group, a carbodiimide group, an aziridine group, an imide group, or a maleic anhydride group. Examples of such active hydrogen reactive groups include an epoxy group, a glycidyl group, an isocyanate group, a thioisocyanate group, an alkoxysilyl group, an oxazoline group, a carbodiimide group, an aziridine group, an imide group, and a maleic anhydride group. These active hydrogen reactive groups may be used alone or in combination of two or more. Of these, an epoxy group or a glycidyl group is preferred because it improves the flexibility of the laminate, improves the transfer quality of the light absorption anisotropic layer, and provides excellent safety.

[0060] Examples of compounds containing an epoxy group or a glycidyl group include bisphenol types such as bisphenol A type, bisphenol F type, bisphenol S type, and hydrogenated types thereof; novolac types such as phenol novolac type and cresol novolac type; nitrogen-containing ring types such as triglycidyl isocyanurate type and hydantoin type; alicyclic types and aliphatic types; aromatic types such as naphthalene type; glycidyl ether types; low water absorption types such as biphenyl type; dicyclo types; ester types; ether ester types; and modified types thereof.

[0061] In the present invention, it is preferable that the crosslinking group-containing additive is a compound having an active hydrogen reactive group and the vertical alignment agent is an ionic vertical alignment agent, because the transfer quality of the optically absorbing anisotropic layer is good. Here, the reason why the transfer quality of the optically absorbing anisotropic layer is good is not clear, but it is thought that the intermediate (especially, intermediate cation) generated when the crosslinking group-containing additive crosslinks is stabilized in the presence of the ionic vertical alignment agent, thereby increasing the crosslinking efficiency.

[0062] The content of the crosslinking group-containing additive in the light absorption anisotropic layer is preferably 3.0 to 20.0 parts by mass, more preferably 5.0 to 16.0 parts by mass, and even more preferably 8.0 to 12.0 parts by mass, relative to 100 parts by mass of the liquid crystal compound. The crosslinking group-containing additive may be contained alone or in combination with two or more types. When two or more types of liquid crystal compounds are contained, the content of the crosslinking group-containing additive refers to the total content of the crosslinking group-containing additives.

[0063] <Solvent> From the viewpoint of workability and the like, the liquid crystal composition preferably contains a solvent. Examples of the solvent include ketones (e.g., acetone, 2-butanone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, acetylacetone, etc.), ethers (e.g., dioxane, tetrahydrofuran, tetrahydropyran, dioxolane, tetrahydrofurfuryl alcohol, cyclopentyl methyl ether, dibutyl ether, etc.), aliphatic hydrocarbons (e.g., hexane, etc.), alicyclic hydrocarbons (e.g., cyclohexane, etc.), aromatic hydrocarbons (e.g., benzene, toluene, xylene, tetralin, trimethylbenzene, etc.), halogenated carbons (e.g., dichloromethane, trichloromethane (chloroform), dichloroethane, dichlorobenzene, 1,1,2,2-tetrachloroethane, chlorotoluene, etc.), esters (e.g., methyl acetate, ethyl acetate, butyl acetate, diethyl carbonate, ethyl acetoacetate, n-pentyl acetate, ethyl benzoate, benzyl benzoate, butyl carbitol acetate, diethylene glycol monoethyl ether acetate, Examples of suitable solvents include organic solvents such as ethanol, isopropanol, butanol, cyclohexanol, furfuryl alcohol, 2-ethylhexanol, octanol, benzyl alcohol, ethanolamine, ethylene glycol, propylene glycol, diethylene glycol, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, phenols (e.g., phenol, cresol, etc.), cellosolves (e.g., methyl cellosolve, ethyl cellosolve, 1,2-dimethoxyethane, etc.), cellosolve acetates, sulfoxides (e.g., dimethyl sulfoxide, etc.), amides (e.g., dimethylformamide, dimethylacetamide, N-methylpyrrolidone, N-ethylpyrrolidone, 1,3-dimethyl-2-imidazolidinone, etc.), and heterocyclic compounds (e.g., pyridine, 2,6-lutidine, etc.), as well as water. These solvents may be used alone or in combination of two or more.

[0064] When the liquid crystal composition contains a solvent, the content of the solvent is preferably 60 to 99.5% by mass, more preferably 70 to 99% by mass, and particularly preferably 75 to 98% by mass, relative to the total mass (100% by mass) of the liquid crystal composition.

[0065] <Polymerization initiator> The liquid crystal composition may contain a polymerization initiator. There are no particular restrictions on the polymerization initiator, but it is preferably a photosensitive compound, i.e., a photopolymerization initiator. As the photopolymerization initiator, various compounds can be used without particular restrictions. Examples of the photopolymerization initiator include α-carbonyl compounds (U.S. Pat. Nos. 2,367,661 and 2,367,670), acyloin ethers (U.S. Pat. No. 2,448,828), α-hydrocarbon-substituted aromatic acyloin compounds (U.S. Pat. No. 2,722,512), polynuclear quinone compounds (U.S. Pat. Nos. 3,046,127 and 2,951,758), and combinations of triarylimidazole dimers and p-aminophenyl ketones (U.S. Pat. No. 3,549,367). ), acridine and phenazine compounds (JP 60-105667 A and U.S. Pat. No. 4,239,850 A), oxadiazole compounds (U.S. Pat. No. 4,212,970 A), o-acyloxime compounds (JP 2016-27384 A

[0065] ), and acylphosphine oxide compounds (JP 63-40799 A, JP 5-29234 A, JP 10-95788 A, and JP 10-29997 A). Commercially available photopolymerization initiators can also be used, including Irgacure-184, Irgacure-907, Irgacure-369, Irgacure-651, Irgacure-819, Irgacure-OXE-01, and Irgacure-OXE-02 manufactured by BASF.

[0066] When the liquid crystal composition contains a polymerization initiator, the content of the polymerization initiator is preferably 0.01 to 30% by mass, more preferably 0.1 to 15% by mass, based on the total solid mass of the liquid crystal composition.

[0067] <Polymerizable Compound> The liquid crystal composition may contain a polymerizable compound. Examples of the polymerizable compound include compounds containing acrylate (for example, (meth)acrylate monomers).

[0068] When the liquid crystal composition contains a polymerizable compound, the content of the polymerizable compound is preferably 0.5 to 50% by mass, more preferably 1.0 to 40% by mass, based on the total solid mass of the liquid crystal composition.

[0069] <Interfacial improver> The liquid crystal composition may contain an interfacial improver. There are no particular limitations on the interfacial improver, and polymer-based interfacial improvers and low-molecular-weight interfacial improvers can be used, including the compounds described in paragraphs

[0253] to

[0293] of JP-A No. 2011-237513. Furthermore, fluorine (meth)acrylate polymers described in paragraphs

[0018] to

[0043] of JP-A No. 2007-272185 can also be used as interfacial improvers. Examples of the interface improver include compounds described in paragraphs

[0079] to

[0102] of JP-A-2007-069471, polymerizable liquid crystal compounds represented by formula (4) described in JP-A-2013-047204 (particularly compounds described in paragraphs

[0020] to

[0032] ), polymerizable liquid crystal compounds represented by formula (4) described in JP-A-2012-211306 (particularly compounds described in paragraphs

[0022] to

[0029] ), and liquid crystal alignment promoters represented by formula (4) described in JP-A-2002-129162 (particularly compounds described in paragraphs

[0032] to

[0032] ). The compounds described in paragraphs

[0076] to

[0078] and

[0082] to

[0084] of JP-A-2005-099248 (particularly the compounds described in paragraphs

[0092] to

[0096] ) are represented by formulas (4), (II), and (III), the compounds described in paragraphs

[0013] to

[0059] of Japanese Patent No. 4,385,997, the compounds described in paragraphs

[0018] to

[0044] of Japanese Patent No. 5,034,200, and the compounds described in paragraphs

[0019] to

[0038] of Japanese Patent No. 4,895,088 can also be used. Furthermore, silicon-based polymers can also be used as interfacial modifiers. The interfacial modifiers may be used alone or in combination of two or more.

[0070] When the liquid crystal composition contains an interfacial modifier, the content of the interfacial modifier is preferably 0.005 to 15% by mass, more preferably 0.01 to 5% by mass, and even more preferably 0.015 to 3% by mass, based on the total mass of the solid content of the liquid crystal composition. When multiple interfacial modifiers are used in combination, the total amount of the multiple interfacial modifiers is preferably in the above-mentioned range.

[0071] <Method for forming optically absorptive anisotropic layer> The method for forming the optically absorptive anisotropic layer is not particularly limited, and examples thereof include a method comprising, in this order: a step of applying the above-described liquid crystal composition (hereinafter also referred to as "optically absorptive anisotropic layer-forming composition") to form a coating film (hereinafter also referred to as "coating film formation step"); and a step of orienting the liquid crystalline component and dichroic substance contained in the coating film (hereinafter also referred to as "orientation step"). Note that the liquid crystalline component is a component that includes not only the above-described liquid crystal compound, but also the dichroic substance having liquid crystallinity, if the above-described dichroic substance has liquid crystallinity.

[0072] (Coating film forming process) The coating film forming process is a process of forming a coating film by applying a composition for forming an optically absorbing anisotropic layer. By using a composition for forming an optically absorbing anisotropic layer containing the above-mentioned solvent, or by using a composition for forming an optically absorbing anisotropic layer that has been converted into a liquid such as a molten liquid by heating, etc., it becomes easier to apply the composition for forming an optically absorbing anisotropic layer. Specific examples of methods for applying the composition for forming an optically absorbing anisotropic layer include known methods such as roll coating, gravure printing, spin coating, wire bar coating, extrusion coating, direct gravure coating, reverse gravure coating, die coating, spraying, and inkjet printing.

[0073] In the present invention, the coating amount of the dichroic material in the coating film forming step is set to 15 mg / m because the optical effect (for example, viewing angle control) is enhanced. 2 It is preferable that the concentration is 50 to 1000 mg / m or more. 2 More preferably, it is 200 to 800 mg / m 2 It is more preferable that:

[0074] (Orientation Step) The orientation step is a step of orienting the liquid crystalline component contained in the coating film. This results in an optically absorptive anisotropic layer. The orientation step may include a drying treatment. Components such as the solvent can be removed from the coating film by the drying treatment. The drying treatment may be performed by leaving the coating film at room temperature for a predetermined time (e.g., natural drying), or by heating and / or blowing air. Here, the liquid crystalline component contained in the composition for forming an optically absorptive anisotropic layer may be aligned by the above-described coating film formation step or drying treatment. For example, in an embodiment in which the composition for forming an optically absorptive anisotropic layer is prepared as a coating liquid containing a solvent, the coating film is dried to remove the solvent from the coating film, thereby obtaining a coating film with optical absorptive anisotropy (i.e., an optically absorptive anisotropic layer). When the drying treatment is performed at a temperature equal to or higher than the transition temperature of the liquid crystalline component contained in the coating film to a liquid crystal phase, the heat treatment described below may not be performed.

[0075] The transition temperature of the liquid crystalline component contained in the coating film to the liquid crystal phase is preferably 10 to 250°C, more preferably 25 to 190°C, from the viewpoint of manufacturability and the like. When the transition temperature is 10°C or higher, no cooling treatment or the like is required to lower the temperature to the temperature range in which the liquid crystal phase is exhibited, and this is preferable. Furthermore, when the transition temperature is 250°C or lower, high temperatures are not required even when the film is once converted to an isotropic liquid state at a temperature higher than the temperature range in which the liquid crystal phase is exhibited, and this is preferable because waste of thermal energy and deformation and deterioration of the substrate can be reduced.

[0076] The orientation step preferably includes a heat treatment. This allows the liquid crystalline component contained in the coating film to be oriented, and the heat-treated coating film can be suitably used as a light absorption anisotropic layer. From the viewpoint of manufacturability, the heat treatment is preferably performed at a temperature of 10 to 250°C, more preferably 25 to 190°C. The heating time is preferably 1 to 300 seconds, more preferably 1 to 60 seconds.

[0077] The alignment step may include a cooling treatment carried out after the heating treatment. The cooling treatment is a treatment in which the coated film after heating is cooled to about room temperature (20 to 25°C). This allows the alignment of the liquid crystalline component contained in the coated film to be fixed. The cooling method is not particularly limited and can be carried out by a known method. A light absorption anisotropic layer can be obtained by the above steps. In this embodiment, drying treatment and heating treatment are mentioned as methods for aligning the liquid crystalline component contained in the coated film, but the method is not limited thereto and can be carried out by a known alignment treatment.

[0078] <Other Steps> The method for forming the optically absorbing anisotropic layer may include a step of curing the optically absorbing anisotropic layer (hereinafter also referred to as a "curing step") after the alignment step. For example, when the optically absorbing anisotropic layer has a crosslinkable group (polymerizable group), the curing step is performed by heating and / or light irradiation (exposure). Among these, the curing step is preferably performed by light irradiation. Various light sources, such as infrared, visible light, or ultraviolet light, can be used as the light source for curing, but ultraviolet light is preferred. Furthermore, ultraviolet light may be irradiated while heating during curing, or ultraviolet light may be irradiated through a filter that transmits only specific wavelengths. When exposure is performed while heating, the heating temperature during exposure is preferably 25 to 140°C, although this depends on the transition temperature of the liquid crystal component contained in the liquid crystal film to the liquid crystal phase. Furthermore, exposure may be performed under a nitrogen atmosphere. When curing of the liquid crystal film proceeds by radical polymerization, exposure under a nitrogen atmosphere is preferred because inhibition of polymerization by oxygen is reduced.

[0079] In the present invention, the thickness of the optically absorptive anisotropic layer is not particularly limited, but is preferably 1.5 μm or more, more preferably 2 to 10 μm, and even more preferably 2 to 8 μm, because this improves the light-shielding properties in oblique directions and increases the degree of orientation of the optically absorptive anisotropic layer. Here, the thickness of the optically absorptive anisotropic layer is measured by cutting the layer with a microtome to prepare a cross-section of the layer, and then observing the cross-section with a scanning electron microscope from the normal direction to the cross-section.

[0080] In the present invention, because the difference in the degree of orientation of the optically absorptive anisotropic layer at wavelengths of 450 nm, 550 nm, and 650 nm can be suppressed when the layer is applied to an image display device, it is preferable that the difference be 0.025 or less, more preferably 0.020 or less, and even more preferably 0.010 or less. Here, the degree of orientation of the optically absorptive anisotropic layer at wavelengths of 450 nm, 550 nm, and 650 nm is calculated by the following method. Specifically, using an AxoScan (manufactured by Axometrics), the Mueller matrix is ​​measured in the in-plane slow axis direction at polar angles ranging from -70 to 70° at 5° intervals, and kx(λ), ky(λ), and kz(λ) are determined by fitting. Next, the absorption anisotropies Ao(λ) and Ae(λ) are calculated according to the following formulas (A) to (D), and the degree of orientation S is calculated according to the following formula (E). To(λ) = EXP{-4 x π x (kx(λ) + ky(λ)) / 2 x d / λ} (A) Te(λ) = EXP{-4 x π x kz(λ) x d / λ} (B) Ao(λ) = -log(To(λ)) (C) Ae(λ) = -log(Te(λ)) (D) Degree of orientation S(λ) = [Ao(λ) / Ae(λ) - 1] / [Ao(λ) / Ae(λ) + 2] (E) Here, d represents the film thickness (nm) of the optically absorptive anisotropic layer, To(λ) and Te(λ) represent the transmittance, and Ao(λ) and Ae(λ) represent the absorbance. The difference in the degree of orientation (0.025 or less) specified in the above-mentioned requirement 3 refers to the maximum difference among the difference in the degree of orientation at wavelengths of 450 nm and 550 nm, the difference in the degree of orientation at wavelengths of 450 nm and 650 nm, and the difference in the degree of orientation at wavelengths of 550 nm and 650 nm.

[0081] In the present invention, the optically absorptive anisotropic layer preferably has a degree of orientation of 0.90 or more, more preferably 0.93 to 1.00, and even more preferably 0.96 to 1.00 at a wavelength of 550 nm, for the reason that the optically absorptive anisotropic layer absorbs a larger amount of polarized light incident on the layer from a specific direction and thus obtains favorable optical performance. Here, the degree of orientation of the optically absorptive anisotropic layer at a wavelength of 550 nm can be calculated by the method described above.

[0082] In addition, it is preferable to perform the heat treatment in the above-mentioned orientation step multiple times (particularly twice) because this makes it easier to make the difference in the degree of orientation of the optically absorptive anisotropic layer at wavelengths of 450 nm, 550 nm, and 650 nm 0.025 or less. Furthermore, the cooling treatment performed between two heat treatments is preferably a treatment in which the coating film after the first heat treatment is cooled to about 30 to 45°C.

[0083] In the present invention, the haze value of the optically absorptive anisotropic layer is preferably 0.3% or less, more preferably 0.2% or less, and even more preferably 0.1% or less, because this maintains a high degree of polarization of light passing through the optically absorptive anisotropic layer and results in more favorable optical performance. Here, the haze value refers to the haze measured in accordance with JIS K7136:2000 "Method of determining haze for plastic transparent materials," and refers to the value measured using a haze meter (e.g., NDH2000 (manufactured by Nippon Denshoku Industries Co., Ltd.)) in an environment of 25°C and a relative humidity of 55%.

[0084] Furthermore, it is preferable to perform the heat treatment in the above-mentioned orientation step multiple times (particularly twice) because this makes it easier to set the haze ratio of the optically absorptive anisotropic layer to 0.3% or less. In particular, it is preferable to lower the temperature in the two heat treatments, more preferably to set it to 65 to 80°C.

[0085] [Alignment Film] The alignment film of the laminate of the present invention may be any film capable of vertically aligning the liquid crystal compound contained in the light-absorbing anisotropic layer. Methods for forming the alignment film include, for example, rubbing an organic compound (preferably a polymer) onto the film surface, oblique vapor deposition of an inorganic compound, formation of a layer with microgrooves, and accumulation of an organic compound (e.g., ω-tricosanoic acid, dioctadecylmethylammonium chloride, methyl stearate, etc.) by the Langmuir-Blodgett method (LB film). Furthermore, alignment films that exhibit alignment function upon application of an electric field, a magnetic field, or light irradiation are also known. Among these, in the present invention, alignment films formed by rubbing are preferred in terms of ease of control of the pretilt angle of the alignment film, and photo-alignment films formed by light irradiation are also preferred in terms of uniformity of alignment.

[0086] <Rubbing Treatment Alignment Film> Polymer materials used for the alignment film formed by rubbing treatment are described in numerous literatures, and many commercially available products are available. In the present invention, polyvinyl alcohol or polyimide, and derivatives thereof are preferably used. For details of the alignment film, see WO 2001 / 88574 A1, page 43, line 24 to page 49, line 8. The thickness of the alignment film is preferably 0.01 to 10 μm, and more preferably 0.01 to 2 μm.

[0087] <Photo-alignment film> Photo-alignment compounds used in alignment films formed by light irradiation are described in many documents, etc. In the present invention, for example, azo compounds described in JP-A Nos. 2006-285197, 2007-76839, 2007-138138, 2007-94071, 2007-121721, 2007-140465, 2007-156439, 2007-133184, 2009-109831, Japanese Patent Nos. 3883848 and 4151746, and compounds described in JP-A No. 2002-229039 are used. Preferred examples include aromatic ester compounds of the above, maleimide and / or alkenyl-substituted nadimide compounds having a photo-alignable unit described in JP-A Nos. 2002-265541 and 2002-317013, photo-crosslinkable silane derivatives described in Japanese Patent Nos. 4205195 and 4205198, and photo-crosslinkable polyimides, polyamides, or esters described in Japanese Patent Publication Nos. 2003-520878, 2004-529220, or Japanese Patent No. 4162850. Azo compounds, photo-crosslinkable polyimides, polyamides, or esters are more preferred.

[0088] Among these, it is preferable to use a photosensitive compound having a photo-alignment group that undergoes at least one of dimerization and isomerization under the action of light as the photo-alignment compound.In addition, as the photo-alignment group, for example, a group having a cinnamic acid (cinnamoyl) structure (skeleton), a group having a coumarin structure (skeleton), a group having a chalcone structure (skeleton), a group having a benzophenone structure (skeleton), and a group having an anthracene structure (skeleton) can be mentioned.Among these groups, a group having a cinnamoyl structure and a group having a coumarin structure are preferred, and a group having a cinnamoyl structure is more preferred.

[0089] The photosensitive compound having the photoalignable group may further have a crosslinkable group. The crosslinkable group is preferably a thermally crosslinkable group that undergoes a curing reaction under the action of heat, or a photocrosslinkable group that undergoes a curing reaction under the action of light, and may be a crosslinkable group having both a thermally crosslinkable group and a photocrosslinkable group. Examples of the crosslinkable group include an epoxy group, an oxetanyl group, -NH-CH 2 Examples of the group include at least one selected from the group consisting of a group represented by -O-R (R represents a hydrogen atom or an alkyl group having 1 to 20 carbon atoms), a group having an ethylenically unsaturated double bond, and a blocked isocyanate group. Among these, an epoxy group, an oxetanyl group, and a group having an ethylenically unsaturated double bond are preferred. A three-membered cyclic ether group is also called an epoxy group, and a four-membered cyclic ether group is also called an oxetanyl group. Specific examples of the group having an ethylenically unsaturated double bond include a vinyl group, an allyl group, a styryl group, an acryloyl group, and a methacryloyl group, with an acryloyl group or a methacryloyl group being preferred.

[0090] A photo-alignment film formed from the above materials is irradiated with linearly polarized or non-polarized light to produce a photo-alignment film. In this specification, "linearly polarized light irradiation" and "non-polarized light irradiation" refer to operations for causing a photoreaction in the photo-alignment material. The wavelength of the light used varies depending on the photo-alignment material used, and is not particularly limited as long as it is the wavelength necessary for the photoreaction. The peak wavelength of the light used for photoirradiation is preferably 200 nm to 700 nm, and ultraviolet light with a peak wavelength of 400 nm or less is more preferred.

[0091] Examples of light sources used for light irradiation include commonly used light sources, such as lamps such as tungsten lamps, halogen lamps, xenon lamps, xenon flash lamps, mercury lamps, mercury xenon lamps, and carbon arc lamps, various lasers [e.g., semiconductor lasers, helium-neon lasers, argon ion lasers, helium-cadmium lasers, and YAG (yttrium aluminum garnet) lasers], light-emitting diodes, and cathode ray tubes.

[0092] As a means for obtaining linearly polarized light, a method using a polarizing plate (e.g., an iodine polarizing plate, a dichroic dye polarizing plate, and a wire grid polarizing plate), a method using a prism element (e.g., a Glan-Thompson prism) or a reflective polarizer utilizing the Brewster angle, or a method using light emitted from a polarized laser light source can be employed. Alternatively, a filter or a wavelength conversion element may be used to selectively irradiate only light of a required wavelength.

[0093] When the light to be irradiated is linearly polarized light, a method is adopted in which the light is irradiated from the top or back surface of the alignment film, perpendicular or oblique to the surface of the alignment film. The incident angle of the light varies depending on the photo-alignment material, but is preferably 0 to 90° (perpendicular), and more preferably 40 to 90°. When the light is non-polarized light, the alignment film is irradiated with non-polarized light obliquely. The incident angle is preferably 10 to 80°, more preferably 20 to 60°, and even more preferably 30 to 50°. The irradiation time is preferably 1 to 60 minutes, and more preferably 1 to 10 minutes.

[0094] When patterning is required, a method of irradiating light using a photomask the number of times required to form a pattern, or a method of writing a pattern by laser light scanning can be used.

[0095] In the present invention, the alignment film preferably contains any one of a polyvinyl alcohol resin, a cinnamoyl group-containing resin, and an epoxy resin, and more preferably contains a cinnamoyl group-containing resin, because this can increase the degree of alignment of the optical absorption anisotropy.

[0096] In addition, in the present invention, in order to improve the transfer quality of the light absorption anisotropic layer, it is preferable that at least one of the above-mentioned protective layer and alignment film contains an additive having an active hydrogen reactive group. Examples of the additive having an active hydrogen reactive group include the above-mentioned crosslinking group-containing additives, whose crosslinkable group is an active hydrogen reactive group. For the same reason, it is preferable that at least one of the above-mentioned protective layer and alignment film is either a polyvinyl alcohol-based resin or an acrylate-based resin.

[0097] [Attachment Layer] The attachment layer of the laminate of the present invention is a pressure-sensitive adhesive layer or an adhesive layer.

[0098] <Adhesive Layer> Examples of adhesives contained in the adhesive layer include rubber-based adhesives, acrylic-based adhesives, silicone-based adhesives, urethane-based adhesives, vinyl alkyl ether-based adhesives, polyvinyl alcohol-based adhesives, polyvinylpyrrolidone-based adhesives, polyacrylamide-based adhesives, cellulose-based adhesives, etc. Among these, acrylic-based adhesives (pressure-sensitive adhesives) are preferred from the viewpoints of transparency, weather resistance, heat resistance, etc.

[0099] The pressure-sensitive adhesive layer can be formed, for example, by a method in which a solution of the pressure-sensitive adhesive is applied to a release sheet, dried, and then transferred to the surface of the transparent resin layer; or a method in which the solution of the pressure-sensitive adhesive is applied directly to the surface of the transparent resin layer and dried. The pressure-sensitive adhesive solution is prepared, for example, as a solution of about 10 to 40% by mass in which the pressure-sensitive adhesive is dissolved or dispersed in a solvent such as toluene or ethyl acetate. The application method can be a roll coating method such as reverse coating or gravure coating, a spin coating method, a screen coating method, a fountain coating method, a dipping method, a spray method, or the like.

[0100] Examples of materials constituting the release sheet include appropriate thin sheets such as synthetic resin films such as polyethylene, polypropylene, and polyethylene terephthalate; rubber sheets; paper; cloth; nonwoven fabrics; nets; foam sheets; and metal foils.

[0101] <Adhesive Layer> The adhesive layer is a layer that develops adhesiveness upon drying or reaction after lamination. Polyvinyl alcohol-based adhesives (PVA-based adhesives) develop adhesiveness upon drying, making it possible to bond materials together. Specific examples of curable adhesives that develop adhesiveness through a reaction include active energy ray-curable adhesives such as (meth)acrylate-based adhesives and cationic polymerization-curable adhesives. Note that (meth)acrylate refers to acrylate and / or methacrylate. Examples of curable components in (meth)acrylate-based adhesives include compounds having a (meth)acryloyl group and compounds having a vinyl group. Furthermore, compounds having an epoxy group or an oxetanyl group can also be used as cationic polymerization-curable adhesives. The epoxy group-containing compound is not particularly limited as long as it has at least two epoxy groups in the molecule, and various commonly known curable epoxy compounds can be used. Examples of preferred epoxy compounds include compounds having at least two epoxy groups and at least one aromatic ring in the molecule (aromatic epoxy compounds), and compounds having at least two epoxy groups in the molecule, at least one of which is formed between two adjacent carbon atoms constituting an alicyclic ring (alicyclic epoxy compounds).

[0102] The thickness of the laminating layer is not particularly limited, but is preferably 3 μm to 50 μm, more preferably 4 μm to 40 μm, and even more preferably 5 μm to 30 μm.

[0103] [Other Layer Structure] The laminate of the present invention preferably further comprises at least one layer selected from the group consisting of a polarizer layer, an antireflection layer, and a retardation layer.

[0104] <Polarizer Layer> The polarizer layer is not particularly limited as long as it is a member capable of converting light into specific linearly polarized light, and conventionally known absorptive polarizers and reflective polarizers can be used. Examples of absorptive polarizers include iodine-based polarizers, dye-based polarizers using dichroic dyes, and polyene-based polarizers. Iodine-based polarizers and dye-based polarizers include coated polarizers and stretched polarizers, both of which can be used. However, coated polarizers are preferred. Furthermore, methods for obtaining a polarizer by stretching and dyeing a laminated film having a polyvinyl alcohol layer formed on a substrate are described in Japanese Patent Nos. 5048120, 5143918, 4691205, 4751481, and 4751486. ​​These known techniques related to polarizers can also be preferably used. Examples of coated polarizers include those disclosed in WO2018 / 124198, WO2018 / 186503, WO2019 / 132020, WO2019 / 132018, WO2019 / 189345, JP2019-197168A, JP2019-194685A, and JP2019-139222A, and known techniques relating to these polarizers can also be preferably utilized. Examples of reflective polarizers that can be used include polarizers in which thin films with different birefringences are laminated, wire grid polarizers, and polarizers in which a cholesteric liquid crystal having a selective reflection region is combined with a quarter-wave plate. Among these, polyvinyl alcohol-based resins (-CH 2A polymer containing -CHOH- as a repeating unit. In particular, a polarizer containing at least one selected from the group consisting of polyvinyl alcohol and an ethylene-vinyl alcohol copolymer is preferred. Furthermore, from the viewpoint of imparting crack resistance, the polarizer may have depolarizing portions formed along opposing edges. Examples of depolarizing portions include those described in JP 2014-240970 A. The polarizer may also have non-polarizing portions arranged at predetermined intervals in the longitudinal direction and / or width direction. The non-polarizing portions are partially bleached portions. The arrangement pattern of the non-polarizing portions can be appropriately set depending on the purpose. For example, when the polarizer is cut (cut, punched, etc.) to a predetermined size for installation in an image display device of a predetermined size, the non-polarizing portions are arranged in positions corresponding to the camera portion of the image display device. Examples of arrangement patterns of non-polarizing portions include those described in JP 2016-27392 A.

[0105] <Antireflection Layer> The antireflection layer is not particularly limited, and a known antireflection layer can be used. Examples of the antireflection layer include the antireflection layers described in paragraphs 0108 to 0121 of WO 2016 / 047648, the contents of which are incorporated herein by reference.

[0106] <Retardation layer> The retardation layer is not particularly limited, and can use a known retardation layer.For example, the retardation layer can be a stretched polycarbonate film, a stretched norbornene polymer film, a transparent film containing and oriented inorganic particles having birefringence such as strontium carbonate, a thin film obtained by obliquely depositing an inorganic dielectric on a support, or a film in which a liquid crystal compound is uniaxially oriented and fixed in orientation.In addition, the retardation layer is preferably a film in which the above-mentioned liquid crystal compound is uniaxially oriented and fixed in orientation.

[0107] [Image Display Device] The image display device is an image display device having the laminate of the present invention. The display element used in the image display device of the present invention is not particularly limited, and examples thereof include a liquid crystal cell, an organic EL display panel, an inorganic EL display panel, and a plasma display panel.

[0108] [Liquid Crystal Display Device] A preferred example of a liquid crystal display device, which is an example of an image display device of the present invention, is an embodiment having the above-described laminate of the present invention and a liquid crystal cell. A specific configuration is one in which the laminate of the present invention is disposed on a front-side polarizing plate or a rear-side polarizing plate. In these configurations, viewing angle control is possible, with light shielding in the vertical or horizontal directions. The laminate of the present invention may also be disposed on both the front-side polarizing plate and the rear-side polarizing plate. This configuration enables viewing angle control, with light shielding in all directions and light transmitting only in the front direction. Furthermore, multiple laminates of the present invention may be laminated via a retardation layer. Controlling the retardation value and optical axis direction can control the transmission performance and light-blocking performance. For example, by arranging a polarizer, the laminate of the present invention, a λ / 2 wavelength plate (the axis angle is shifted 45° from the orientation direction of the polarizer), and the laminate of the present invention, viewing angle control is possible, with light shielding in all directions and light transmitting only in the front direction. A positive A plate, a negative A plate, a positive C plate, a negative C plate, a B plate, an O plate, or the like can be used as the retardation layer. From the viewpoint of reducing the thickness of the viewing angle control system, the thickness of the retardation layer is preferably as thin as possible as long as the optical properties, mechanical properties, and manufacturability are not impaired, and specifically, the thickness is preferably 1 to 150 μm, more preferably 1 to 70 μm, and even more preferably 1 to 30 μm. The liquid crystal cell constituting the liquid crystal display device will be described in detail below.

[0109] <Liquid Crystal Cell> The liquid crystal cell used in the liquid crystal display device is preferably, but not limited to, a VA (Vertical Alignment) mode, an OCB (Opticaly Compensated Bend) mode, an IPS (In-Plane-Switching) mode, or a TN (Twisted Nematic) mode. In a TN mode liquid crystal cell, when no voltage is applied, rod-shaped liquid crystal molecules are aligned substantially horizontally and further twisted at an angle of 60 to 120 degrees. TN mode liquid crystal cells are most commonly used in color TFT liquid crystal display devices and are described in many literatures. In a VA mode liquid crystal cell, rod-shaped liquid crystal molecules are aligned substantially vertically when no voltage is applied. VA mode liquid crystal cells include (1) narrowly defined VA mode liquid crystal cells in which rod-shaped liquid crystal molecules are aligned substantially vertically when no voltage is applied and substantially horizontally when a voltage is applied (described in JP-A-2-176625), (2) multi-domain VA mode liquid crystal cells (described in SID97, Digest of Tech. Papers (Proceedings) 28 (1997) 845) in order to widen the viewing angle (MVA mode liquid crystal cells), (3) n-ASM mode liquid crystal cells in which rod-shaped liquid crystal molecules are aligned substantially vertically when no voltage is applied and substantially horizontally when a voltage is applied (described in Proceedings of the Japan Liquid Crystal Symposium 58-59 (1998)), and (4) SURVIVAL mode liquid crystal cells (announced at LCD International 98). The liquid crystal display may be of any of a PVA (Patterned Vertical Alignment) type, an optical alignment type, and a PSA (Polymer-Sustained Alignment) type. Details of these modes are described in detail in Japanese Patent Laid-Open No. 2006-215326 and Japanese Patent Laid-Open No. 2008-538819.

[0110] In an IPS mode liquid crystal cell, the liquid crystal compound is oriented substantially parallel to the substrate, and when an electric field parallel to the substrate surface is applied, the liquid crystal molecules respond in a planar manner. That is, when no electric field is applied, the liquid crystal compound is oriented in-plane. In an IPS mode, when no electric field is applied, a black display is achieved, and the absorption axes of a pair of upper and lower polarizing plates are perpendicular to each other. Methods of using an optical compensation sheet to reduce light leakage during black display in an oblique direction and improve the viewing angle are disclosed in, for example, JP-A Nos. 10-54982, 11-202323, 9-292522, 11-133408, 11-305217, and 10-307291.

[0111] [Organic EL Display Device] An organic EL display device, which is an example of the image display device of the present invention, preferably has, from the viewing side, the above-described laminate of the present invention, a λ / 4 plate, and an organic EL display panel, in this order. Furthermore, similar to the above-described liquid crystal display device, multiple laminates of the present invention may be stacked with a retardation layer interposed therebetween and placed on the organic EL display panel. By controlling the retardation value and the optical axis direction, it is possible to control the transmission performance and light-blocking performance. Furthermore, the organic EL display panel is a display panel constructed using organic EL elements in which an organic light-emitting layer (organic electroluminescence layer) is sandwiched between electrodes (cathode and anode). The configuration of the organic EL display panel is not particularly limited, and a known configuration may be adopted.

[0112] [Viewing Angle Switching Device] The image display device of the present invention may be an image display device having the laminate of the present invention and an electronically controlled viewing angle switching cell, i.e., a viewing angle switching device. Here, the electronically controlled viewing angle switching cell includes a first substrate, a second substrate, a first electrode, a second electrode, and a liquid crystal layer. The first electrode and the second electrode, which are arranged opposite to each other, are disposed on the first substrate and the second substrate, respectively. The first electrode and the second electrode are, for example, planar electrodes, but are not limited thereto. The liquid crystal layer is disposed between the first electrode and the second electrode and includes a plurality of liquid crystal molecules. The first substrate and the second substrate may be made of glass, quartz, an organic polymer, or other suitable transparent material. Meanwhile, the first electrode and the second electrode may be, for example, light-transmitting electrodes. The light-transmitting electrodes may be made of indium tin oxide, indium zinc oxide, aluminum tin oxide, aluminum zinc oxide, or other suitable oxides, ultrathin metals, hollow metal layers (metal mesh or wire grid), carbon nanotubes, silver nanowires, or graphene. For example, when a voltage is applied between the first electrode and the second electrode, this voltage can create an electric field between the two electrodes, causing the liquid crystal molecules in the liquid crystal layer to rotate. In other words, different electric field magnitudes and distributions can change the orientation axes (or long axes) of multiple liquid crystal molecules, thereby adjusting the polarization state of light and switching the display device between anti-peeping mode and shared mode. To align the optical axes of multiple liquid crystal molecules in the liquid crystal layer in a specific direction when no electric field is applied, the electronically controlled viewing angle switching cell further includes an alignment film 1 and an alignment film 2. The alignment film 1 is disposed between the first electrode and the liquid crystal layer, the alignment film 2 is disposed between the second electrode and the liquid crystal layer, and the liquid crystal layer LCL is disposed between the alignment film 1 and the alignment film 2. Specific examples include optical devices / viewing angle switching devices, such as those described in US 2021 / 0349335. The laminate of the present application can also be used in these devices.

[0113] In the present invention, when the electronically controlled viewing angle switching cell is used in the privacy mode, the viewing angle control performance, i.e., the difference in screen contrast between when the screen is observed from the front and when it is observed from an oblique angle, is likely to be highest, and therefore it is preferable that the maximum phase difference of the electronically controlled viewing angle switching cell is ¼ wavelength or ½ wavelength.

[0114] [Optical Device / Head-Mounted Display] The optical device is an optical device having an optical filter including the laminate of the present invention described above and a light guide plate having a diffraction element disposed on the surface thereof. Also, the head-mounted display of the present invention is a head-mounted display having the optical device described above and an image display element.

[0115] Fig. 1 is a schematic diagram of an example of a head-mounted display of the present invention. The head-mounted display 80 shown in Fig. 1 is, as an example, an AR glass, and includes a light guide plate 82, an incident diffraction element 90 and an exit diffraction element 92 arranged on one surface of the light guide plate 82, an optical filter 10, and an image display element 86. The light guide plate 82, the incident diffraction element 90 and the exit diffraction element 92, and the optical filter 10 constitute the optical device of the present invention.

[0116] 1, an incident diffraction element 90 is disposed on the surface (principal surface) on one end side of the light guide plate 82. An output diffraction element 92 is disposed on the surface on the other end side of the light guide plate 82. The position of the incident diffraction element 90 is determined by the angle at which the image light I from the image display element 86 to the light guide plate 82 is incident. 1 On the other hand, the position of the output diffraction element 92 corresponds to the incident position of the image light I from the light guide plate 82. 1 The exit position of the image light I 11 corresponds to the observation position of the light guide plate 82. The incident diffraction element 90 and the exit diffraction element 92 are disposed on the same surface of the light guide plate 82. The optical filter 10 is disposed on the surface of the light guide plate 82 opposite to the surface on which the exit diffraction element 92 is disposed, facing the exit diffraction element 92. As shown in FIG. 1, the optical filter 10 has the same planar shape as the exit diffraction element 92. An intermediate diffraction element 94 may be provided on the light guide plate 82 (see FIG. 2). The positions of the diffraction elements are not limited to the ends of the light guide plate, and various positions can be used depending on the shape of the light guide plate, etc.

[0117] In the head-mounted display 80 (AR glasses) configured as described above, the image light I displayed by the image display element 86 is 1 As shown by the arrow, the image light I is diffracted by the incident diffraction element 90 and enters the light guide plate 82 at an angle at which it is totally reflected at the interface between the light guide plate 82 and the air. 1 is totally reflected by both surfaces of the light guide plate 82, is guided through the light guide plate 82, and is incident on the output diffraction element 92. 1 is diffracted by the output diffraction element 92 in a direction perpendicular to the surface of the output diffraction element 92. 1 The light is emitted to a viewing position outside the light guide plate 82 for the user to view, and is viewed by the user.

[0118] As shown in FIG. 1, external light I entering the head-mounted display 80 from the front direction 0 That is, the background light passes through the optical filter 10, enters the light guide plate 82, passes through the output diffraction element 92, and reaches the observation position of the user. In the following description, external light that enters the head-mounted display 80 from the front direction is referred to as front external light I. 0 As a result, the head mounted display 80 causes the image displayed by the image display element 86 to enter one end of the light guide plate 82, propagate therethrough, and exit from the other end, thereby superimposing a virtual image on the view that the user is actually seeing.

[0119] The planar shape of the optical filter 10 is not limited to be the same as the planar shape of the diffraction element, and may be different in shape and size. s and the background, i.e., the front external light I 0 In order to prevent unnecessary light blocking, it is preferable that the diffraction element and the optical filter have the same planar shape, including the same size.

[0120] There are no particular limitations on the light guide plate 82, and any conventional light guide plate used in image display devices, etc., such as light guide plates used in various types of AR glasses and light guide plates used in backlight units of liquid crystal display devices, can be used.

[0121] There are no limitations on the image display element 86, and various known image display elements (displays) used in various image display devices such as AR glasses can be used. Examples of the image display element 86 include a liquid crystal display (including LCOS (Liquid Crystal On Silicon)), an organic electroluminescence display, an inorganic electroluminescence display, a DLP (Digital Light Processing), a MEMS (Micro-Electro-Mechanical Systems) display, and a micro LED (Light-Emitting Diode) display. Note that the image display element 86 may be one that displays monochrome images, two-color images, or color images.

[0122] The optical device of the present invention has an optical filter including the laminate of the present invention covering the diffraction element, preferably an optical filter including the laminate 14 and a polarizer 12 as in the illustrated example. By having such an optical filter 10 (10m), the optical device of the present invention can reduce the amount of light emitted from the front direction (front external light I) when used in a head-mounted display such as AR glasses. 0 ) has a high light transmittance, i.e., the visibility of the background is excellent, and external light (oblique external light I) incident from above the observer's head (diagonally above and in front of the observer's head) is also excellent. sFurthermore, the optical device of the present invention can preferably suppress rainbow unevenness caused by external light incident not only from above and in front of the viewer's head, but also from diagonally ahead of the viewer's head (above and in a diagonal direction from above).

[0123] In the optical device of the present invention, the angle between the absorption axis (the alignment direction of the liquid crystal compound) of the laminate 14 constituting the optical filter 10 and the normal direction of the laminate 14 is 0 to 45°. That is, the laminate 14 has an absorption axis extending in the normal direction to the principal surface of the laminate 14 and the principal surface of the light guide plate 82. On the other hand, the polarizer 12 constituting the optical filter 10 is a polarizer having an absorption axis in the principal surface. That is, the polarizer has an absorption axis parallel to the principal surface of the laminate 14 and the principal surface of the light guide plate 82. Note that in the present invention, when the optical filter includes the laminate 14 and the polarizer 12, it is preferable to place the laminate 14 on the light guide plate 82 side from the viewpoint of improving light resistance.

[0124] The present invention will be described in more detail below with reference to examples. The materials, amounts used, ratios, treatment details, and treatment procedures shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be construed as being limited by the examples shown below.

[0125] Example 1 (1) Support A cellulose acylate film 1 (TG40, a TAC substrate having a thickness of 40 μm, manufactured by Fujifilm Corporation) was used as a support after its surface was saponified with an alkaline solution.

[0126] (2) Preparation of Alignment Film The following composition 1 for forming an alignment film was applied onto a cellulose acylate film 1. The support on which the coating film was formed was dried with hot air at 145°C for 120 seconds to form an alignment film 1. The thickness of the alignment film 1 was 0.25 µm.

[0127] ------------------------------------------------------------------ Composition 1 for forming alignment film -------------------------------------------------- Polymer PA-1 (described below) 10.0 parts by mass Acid generator PAG-1 (described below) 0.83 parts by mass Stabilizer DIPEA (described below) 0.06 parts by mass Butyl acetate 100 parts by mass Methyl ethyl ketone 25 parts by mass ------------------------------------------------------------------

[0128] Polymer PA-1

[0129] Acid generator PAG-1

[0130] Stabilizer DIPEA

[0131] (3) Preparation of Optically Absorbent Anisotropic Layer A composition 1 for forming an optically absorbent anisotropic layer having the following composition was applied to the obtained TAC film with an alignment layer using a wire bar, heated at 120°C for 60 seconds, and then cooled to 35°C. The layer was then heated at 75°C for 60 seconds and cooled again to room temperature. Thereafter, under nitrogen purging conditions (oxygen concentration 100 ppm or less), an LED lamp (center wavelength 365 nm) was used to illuminate the layer from the direction normal to the film at an illuminance of 200 mW / cm. 2 The alignment film was irradiated for 2 seconds under the irradiation conditions of 1.0 to 1.5, thereby forming an optically absorptive anisotropic layer 1 on the alignment film. The thickness of the optically absorptive anisotropic layer 1 was 4.5 μm.

[0132] 0.17 parts by mass of dichroic substance D-2 below; 1.13 parts by mass of dichroic substance D-3 below; 8.67 parts by mass of polymer liquid crystal compound P-1 below; 1.97 parts by mass of liquid crystal compound L-1 below; 0.20 parts by mass of IRGACUE OXE-2 (manufactured by BASF); 0.16 parts by mass of vertical alignment agent E-2 below; 0.007 parts by mass of surfactant F-1 below; 78.17 parts by mass of cyclopentanone; 8.69 parts by mass of benzyl alcohol

[0133] Dichroic substance D-1

[0134] Dichroic substance D-2

[0135] Dichroic substance D-3

[0136] Polymer liquid crystal compound P-1 (weight average molecular weight: 15000)

[0137] Liquid crystal compound L-1 (a mixture of the following liquid crystal compounds (RA), (RB), and (RC) in a mass ratio of 84:14:2)

[0138] Orientation agent E-2

[0139] Surfactant F-1 (weight average molecular weight: 9000)

[0140] (4) Preparation of Protective Layer The surface of the obtained optically absorptive anisotropic layer 1 was subjected to a corona treatment under conditions of 4.0 m / min, 440 W, and a clearance of 2.0 mm. Next, a protective layer-forming coating solution 1 having the following composition was applied to the corona-treated optically absorptive anisotropic layer 1 using a wire bar to form a coating film. Next, the support on which the coating film had been formed was dried with hot air at 60°C for 60 seconds and then with hot air at 100°C for 120 seconds to form protective layer 1. Thereafter, under nitrogen purging conditions (oxygen concentration 100 ppm or less), an LED lamp (center wavelength 365 nm) was used to illuminate the film normal direction at an illuminance of 200 mW / cm. 2 The protective layer 1 was formed on the optically absorptive anisotropic layer 1 by irradiating the light for 2 seconds under the irradiation conditions of [Irradiation Condition], thereby producing a laminate precursor 1 (layer structure: support 1 / alignment film 1 / optically absorptive anisotropic layer 1 / protective layer 1). The thickness of the protective layer was 0.5 μm.

[0141] -------------------------------------------------- Coating liquid 1 for forming protective layer -------------------------------------------------- 3.80 parts by mass of modified polyvinyl alcohol PVA-1 shown below 0.20 parts by mass IRGACURE 2959 (manufactured by BASF) 0.08 parts by mass of dye compound G-1 shown below Water 70 parts by mass Methanol 30 parts by mass --------------------------------------------------

[0142] Modified polyvinyl alcohol PVA-1

[0143] Dye compound G-1

[0144] (5) Preparation of Pressure-Sensitive Adhesive Sheet An acrylate polymer was prepared according to the following procedure. First, 95 parts by mass of butyl acrylate and 5 parts by mass of acrylic acid were polymerized by solution polymerization in a reaction vessel equipped with a cooling tube, a nitrogen inlet tube, a thermometer, and a stirrer to obtain an acrylate polymer A1 having an average molecular weight of 2,000,000 and a molecular weight distribution (Mw / Mn) of 3.0. Next, the obtained acrylate polymer A1 (100 parts by mass) was mixed with Coronate L (a 75% by mass ethyl acetate solution of a trimethylolpropane adduct of tolylene diisocyanate, number of isocyanate groups per molecule: 3, manufactured by Nippon Polyurethane Industry Co., Ltd.) (1.0 part by mass), and a silane coupling agent KBM-403 (manufactured by Shin-Etsu Chemical Co., Ltd.) (0.2 parts by mass), and finally, ethyl acetate was added so that the total solids concentration was 10% by mass to prepare a pressure-sensitive adhesive-forming composition. This composition was applied to a release PET film (Film Vina, light release type, manufactured by Fujimori Kogyo Co., Ltd.) using a die coater and dried for 1 minute in an environment of 90°C to obtain an acrylate-based pressure-sensitive adhesive sheet consisting of a pressure-sensitive adhesive layer and a release PET film. The film thickness was 25 μm and the storage modulus was 0.1 MPa.

[0145] (6) Preparation of Pressure-Sensitive Adhesive Layer The pressure-sensitive adhesive layer surface of the acrylate-based pressure-sensitive adhesive sheet obtained above was attached to the protective layer of the laminate precursor 1, and then the release PET on the pressure-sensitive adhesive sheet side was peeled off to form a pressure-sensitive adhesive layer 1 on the protective layer 1, resulting in the following layer structure: Support 1 / Alignment film 1 / Light absorption anisotropic layer 1 / Protective layer 1 / Pressure-Sensitive Adhesive Layer 1

[0146] (7) Peeling of Support The pressure-sensitive adhesive layer 1 exposed by peeling off the release PET was bonded to another release PET film (Film Vina, medium release type, manufactured by Fujimori Kogyo Co., Ltd.), and then the support 1 adjacent to the alignment film 1 was peeled off to obtain the following layer structure: alignment film 1 / light absorption anisotropic layer 1 / protective layer 1 / pressure-sensitive adhesive layer 1 / release PET (medium release type).

[0147] (8) Preparation of Laminating Layer The adhesive layer surface of the adhesive sheet prepared in (5) above was laminated to the surface of the alignment film 1 exposed by peeling off the support 1, and then the release PET (light release type) on the adhesive sheet side was peeled off to prepare a laminate having the following layer structure. The adhesive layer thus exposed corresponds to the laminating layer. Layer structure: adhesive layer (laminating layer) / alignment film 1 / light absorption anisotropic layer 1 / protective layer 1 / adhesive layer 1 / release PET (medium release type).

[0148] Example 2 A laminate of Example 2 was produced in the same manner as in Example 1, except that the composition 1 for forming an optically absorptive anisotropic layer was changed to the composition 2 for forming an optically absorptive anisotropic layer described below. ------------------------------------------------ Optically absorptive anisotropic layer forming composition 2---------------------------------------------------------------- 0.69 parts by mass of the dichroic material D-1 0.17 parts by mass of the dichroic material D-2 1.13 parts by mass of the dichroic material D-3 8.67 parts by mass of the polymer liquid crystal compound P-1 1.97 parts by mass of the liquid crystal compound L-1 1.00 parts by mass of crosslinking group-containing additive 1 (1,10-decanediol diacrylate, A-600 manufactured by Shin-Nakamura Chemical Co., Ltd.) 0.20 parts by mass of IRGACUE OXE-2 (manufactured by BASF) 0.16 parts by mass of the vertical alignment agent E-2 0.007 parts by mass of the surfactant F-1 78.17 parts by mass of cyclopentanone Benzyl alcohol 8.69 parts by mass ----------------------------------------------------------------

[0149] Example 3 A laminate of Example 3 was produced in the same manner as in Example 1, except that the composition 1 for forming an optically absorptive anisotropic layer was changed to the composition 3 for forming an optically absorptive anisotropic layer described below. ------------------------------------------------ Composition 3 for forming optically absorptive anisotropic layer------------------------------------------------ 0.69 parts by mass of the above-mentioned dichroic material D-1 0.17 parts by mass of the above-mentioned dichroic material D-2 1.13 parts by mass of the above-mentioned dichroic material D-3 8.67 parts by mass of the above-mentioned polymer liquid crystal compound P-1 1.97 parts by mass of the above-mentioned liquid crystal compound L-1 1.00 parts by mass of crosslinking group-containing additive 2 (bisphenol A type bifunctional epoxy resin, jER828US manufactured by Mitsubishi Chemical Corporation) 0.10 parts by mass of photoacid generator (CPI-100P, San-Apro Ltd.) 0.20 parts by mass of IRGACUE OXE-2 (manufactured by BASF) 0.16 parts by mass of the following vertical alignment agent E-1 Surfactant F-1 0.007 parts by mass Cyclopentanone 78.17 parts by mass Benzyl alcohol 8.69 parts by mass

[0150] Vertical alignment agent E-1

[0151] Example 4 A laminate of Example 4 was produced in the same manner as in Example 1, except that the composition 1 for forming an optically absorptive anisotropic layer was changed to the composition 4 for forming an optically absorptive anisotropic layer described below. ------------------------------------------------ Optically absorptive anisotropic layer forming composition 4---------------------------------------------------------------- 0.69 parts by mass of the dichroic material D-1 0.17 parts by mass of the dichroic material D-2 1.13 parts by mass of the dichroic material D-3 8.67 parts by mass of the polymer liquid crystal compound P-1 1.97 parts by mass of the liquid crystal compound L-1 1.00 parts by mass of crosslinking group-containing additive 2 (bisphenol A type bifunctional epoxy resin, jER828US manufactured by Mitsubishi Chemical Corporation) 0.10 parts by mass of photoacid generator (CPI-100P, San-Apro Ltd.) 0.20 parts by mass of IRGACUE OXE-2 (manufactured by BASF) 0.16 parts by mass of the alignment agent E-1 (ionic) Alignment agent E-2 (boronic acid) 0.16 parts by mass Surfactant F-1 0.007 parts by mass Cyclopentanone 78.17 parts by mass Benzyl alcohol 8.69 parts by mass

[0152] Example 5 A laminate of Example 5 was produced in the same manner as in Example 4, except that the alignment film-forming composition 1 was changed to the alignment film-forming composition 2 below. ------------------------------------------------ Alignment film-forming composition 2 ------------------------------------------------ Polymer PA-1 10.0 parts by mass Crosslinking group-containing additive 2 (bisphenol A-type bifunctional epoxy resin, jER828US manufactured by Mitsubishi Chemical Corporation) 3.00 parts by mass Acid generator PAG-1 0.83 parts by mass Stabilizer DIPEA 0.06 parts by mass Butyl acetate 100 parts by mass Methyl ethyl ketone 25 parts by mass

[0153] Example 6 A laminate of Example 6 was prepared in the same manner as in Example 3, except that the coating amount of the composition for forming an optically absorptive anisotropic layer was adjusted to a thickness of 1.0 μm.

[0154] Example 7 A laminate of Example 7 was produced in the same manner as in Example 3, except that the alignment film-forming composition 1 was changed to the alignment film-forming composition 3 below. ------------------------------------------------ Alignment film-forming composition 3 ------------------------------------------------ Polymer PA-1 10.0 parts by mass Acid generator PAG-1 0.83 parts by mass Stabilizer DIPEA 0.06 parts by mass Butyl acetate 60 parts by mass Methyl ethyl ketone 60 parts by mass

[0155] Example 8 A laminate of Example 8 was produced in the same manner as in Example 3, except that the alignment film-forming composition 1 was changed to the alignment film-forming composition 4 below. ------------------------------------------------ Alignment film-forming composition 4 ------------------------------------------------ Polymer PA-1 10.0 parts by mass Acid generator PAG-1 0.83 parts by mass Stabilizer DIPEA 0.06 parts by mass Butyl acetate 125 parts by mass

[0156] Example 9 A laminate of Example 9 was produced in the same manner as in Example 1, except that the composition 1 for forming an optically absorptive anisotropic layer was changed to the composition 5 for forming an optically absorptive anisotropic layer described below. ------------------------------------------------ Optically absorptive anisotropic layer forming composition 5------------------------------------------------ 0.69 parts by mass of the dichroic material D-1 0.17 parts by mass of the dichroic material D-2 1.13 parts by mass of the dichroic material D-3 8.67 parts by mass of the polymer liquid crystal compound P-1 1.97 parts by mass of the liquid crystal compound L-1 1.00 parts by mass of crosslinking group-containing additive 2 (bisphenol A type bifunctional epoxy resin, jER828US manufactured by Mitsubishi Chemical Corporation) 0.10 parts by mass of photoacid generator (CPI-100P, San-Apro Ltd.) 0.20 parts by mass of IRGACUE OXE-2 (manufactured by BASF) 0.16 parts by mass of the alignment agent E-2 (boronic acid) Surfactant F-1 0.007 parts by mass Cyclopentanone 78.17 parts by mass Benzyl alcohol 8.69 parts by mass

[0157] Example 10 A laminate of Example 10 was produced in the same manner as in Example 3, except that the composition 3 for forming an optically absorptive anisotropic layer was changed to the composition 6 for forming an optically absorptive anisotropic layer described below. ------------------------------------------------ Composition 6 for forming optically absorptive anisotropic layer ------------------------------------------------ 1.82 parts by mass of dichroic material D-4 below 0.49 parts by mass of dichroic material D-5 below 3.25 parts by mass of dichroic material D-6 below 18.21 parts by mass of the above polymer liquid crystal compound P-1 4.13 parts by mass of the above liquid crystal compound L-1 2.10 parts by mass of crosslinking group-containing additive 2 (bisphenol A type bifunctional epoxy resin, jER828US manufactured by Mitsubishi Chemical Corporation) 0.21 parts by mass of photoacid generator (CPI-100P, San-Apro Ltd.) 1.67 parts by mass of IRGACUE 369 (manufactured by BASF) 0.37 parts by mass of the above alignment agent E-1 Alignment agent E-2 0.37 parts by mass BYK-361N (BYK-Chemie) 0.084 parts by mass o-xylene 69.60 parts by mass

[0158] Dichroic substance D-4

[0159] Dichroic substance D-5

[0160] Dichroic substance D-6

[0161] Example 11 A laminate of Example 11 was produced in the same manner as in Example 3, except that the composition 3 for forming an optically absorptive anisotropic layer was changed to the composition 7 for forming an optically absorptive anisotropic layer described below. ---------------------------------------------------------------- Composition 7 for forming optically absorptive anisotropic layer ---------------------------------------------------------------- 0.79 parts by mass of the above-mentioned dichroic material D-1 0.21 parts by mass of the above-mentioned dichroic material D-2 1.41 parts by mass of the above-mentioned dichroic material D-3 7.52 parts by mass of the following liquid crystal compound L-2 2.51 parts by mass of the following liquid crystal compound L-3 0.94 parts by mass of crosslinking group-containing additive 2 (bisphenol A type bifunctional epoxy resin, jER828US manufactured by Mitsubishi Chemical Corporation) 0.094 parts by mass of photoacid generator (CPI-100P, San-Apro Ltd.) 0.73 parts by mass of IRGACUE 369 (manufactured by BASF) BYK-361N (BYK-Chemie) 0.036 parts by mass Cyclopentanone 78.13 parts by mass Benzyl alcohol 8.67 parts by mass

[0162] Liquid crystal compound L-2

[0163] Liquid crystal compound L-3

[0164] Example 12 A laminate of Example 12 was produced in the same manner as in Example 3, except that the composition 3 for forming an optically absorptive anisotropic layer was changed to the composition 8 for forming an optically absorptive anisotropic layer described below. ---------------------------------------------------------------- Composition 8 for forming optically absorptive anisotropic layer ---------------------------------------------------------------- 0.78 parts by mass of the dichroic material D-4 0.21 parts by mass of the dichroic material D-5 1.39 parts by mass of the dichroic material D-6 7.39 parts by mass of the liquid crystal compound L-2 2.46 parts by mass of the liquid crystal compound L-3 0.99 parts by mass of crosslinking group-containing additive 2 (bisphenol A type bifunctional epoxy resin, jER828US manufactured by Mitsubishi Chemical Corporation) 0.099 parts by mass of photoacid generator (CPI-100P, San-Apro Ltd.) 0.71 parts by mass of IRGACUE 369 (manufactured by BASF) BYK-361N (BYK-Chemie) 0.036 parts by mass o-xylene 87.02 parts by mass

[0165] Example 13 A laminate of Example 15 was produced in the same manner as in Example 5, except that the protective layer-forming coating liquid 1 was changed to the protective layer-forming coating liquid 2 described below.

[0166] ------------------------------------------------------------------ Coating liquid 2 for forming protective layer ------------------------------------------------------------------ Polyfunctional acrylate (dipentaerythritol hexaacrylate) 9.71 parts by mass IRGACUE OXE-2 (manufactured by BASF) 0.28 parts by mass Surfactant F-1 above 0.01 parts by mass Methyl ethyl ketone 90.00 parts by mass ------------------------------------------------------------------

[0167] [Comparative Example 1] A laminate of Comparative Example 1 was produced in the same manner as in Example 3, except that the support adjacent to the alignment film 1 was not peeled off. The layer structure of Comparative Example 1 is shown below. Layer structure: pressure-sensitive adhesive layer (affixing layer) / support 1 / alignment film 1 / light absorption anisotropic layer 1 / protective layer 1 / pressure-sensitive adhesive layer 1 / release PET (medium release type)

[0168] [Evaluation] (1) Transmittance central axis angle θ The transmittance central axis angle θ was measured by the method described above for the laminates produced in Examples 1 to 13 and Comparative Example 1. The results are shown in Table 1 below.

[0169] (2) Transfer Quality of Optically Absorbent Anisotropic Layer The laminates produced in Examples 1 to 13 and Comparative Example 1 were placed on a polarizer with the surface of the adhesive layer of the laminate facing downwards, and visually observed from a polar angle of 45° to the transmission axis direction of the polarizer. The transfer quality of the optically absorptive anisotropic layer was evaluated according to the following criteria. The results are shown in Table 1 below. <Evaluation Criteria> A: No stretching, tears, wrinkles, folds, etc. were observed even when viewed with a magnifying glass. B: No stretching, tears, wrinkles, folds, etc. that were immediately apparent to the naked eye, but very slight stretching was apparent when viewed with a magnifying glass. C: No stretching, tears, wrinkles, folds, etc. that were immediately apparent to the naked eye, but some slight stretching was apparent when viewed with a magnifying glass. D: No stretching, tears, wrinkles, folds, etc. that were immediately apparent to the naked eye, but relatively significant stretching, tears, wrinkles, folds, etc. that were apparent when viewed with a magnifying glass. E: Very slight stretching, tears, wrinkles, folds, etc. that were immediately apparent to the naked eye. F: There is some stretching, tearing, wrinkles, creases, etc. that can be seen at a glance.

[0170] (3) Flexibility of Laminates For the laminates produced in Examples 1 to 13 and Comparative Example 1, the surface of the adhesive layer of the laminate was attached to a 40 μm-thick TAC film, and then the release PET (medium release type) was peeled off to obtain laminates with the following layer structure: TAC / adhesive layer (adhesive layer) / alignment film / light absorption anisotropic layer / protective layer. The laminates were then placed in a mandrel tester, placed on a polarizer, and visually observed from a polar angle of 45° to the transmission axis direction of the polarizer. The flexibility of the laminates was evaluated according to the following criteria. The results are shown in Table 1 below. <Evaluation Criteria> A: No visible stretching, tears, wrinkles, folds, etc. B: Significant visible stretching, tears, wrinkles, folds, etc.

[0171]

[0172] The results shown in Table 1 indicate that a laminate having a support between the alignment film and the lamination layer exhibits poor flexibility when used in bending applications (Comparative Example 1). In contrast, laminates having a protective layer, an optically absorbing anisotropic layer, an alignment film, and an lamination layer adjacent to each other in this order exhibited good flexibility (Examples 1 to 13). In particular, a comparison between Example 1 and Example 2 indicated that the transfer quality of the optically absorbing anisotropic layer was improved when a crosslinking group-containing additive was incorporated into the composition forming the optically absorbing anisotropic layer. Furthermore, a comparison between Example 3 and Example 9 indicated that the transfer quality of the optically absorbing anisotropic layer was further improved when a composition forming the optically absorbing anisotropic layer contained an additive having an active hydrogen-reactive group as a crosslinking agent and an ionic vertical alignment agent. Furthermore, a comparison between Example 3 and Example 4 indicated that the transfer quality of the optically absorbing anisotropic layer was further improved when an ionic vertical alignment agent and a vertical alignment agent having a boronic acid group were used in combination as the vertical alignment agent. Furthermore, a comparison between Example 4 and Example 5 revealed that the transfer quality of the optically absorptive anisotropic layer was particularly good when the alignment film contained an additive having an active hydrogen reactive group. Although not shown in Table 1, a comparison between Example 5 and Example 13 revealed that, after the pressure-sensitive adhesive layer was attached to the protective layer, samples were placed in an environment of 80°C and 85% relative humidity for 500 hours before the release PET on the pressure-sensitive adhesive sheet side was peeled off. The results showed that Example 13 was better able to suppress changes in transmittance.

[0173] Example 14 (1) Preparation of Laminate X A laminate precursor 1 (layer structure: support 1 / alignment film 1 / light absorption anisotropic layer 1 / protective layer 1) was prepared in the same manner as in Example 1. Next, a pressure-sensitive adhesive sheet was attached to the protective layer of the laminate precursor 1, and then the support of the pressure-sensitive adhesive sheet was peeled off. Cosmoshine double-sided easy-adhesion type A4360 (thickness 75 μm, manufactured by Toyobo Co., Ltd.) was attached to the exposed pressure-sensitive adhesive layer, thereby preparing a laminate X having the following layer structure: Layer structure: alignment film 1 / light absorption anisotropic layer 1 / protective layer 1 / pressure-sensitive adhesive layer / support (Cosmoshine double-sided easy-adhesion type A4360).

[0174] (2) Preparation of PVA Polarizing Plate A 30 μm-thick PVA film with an average degree of polymerization of 2400 and a degree of saponification of 99.9 mol% was immersed in warm water at 25°C for 120 seconds to swell. The PVA film was then immersed in a 0.6 wt% aqueous solution of iodine / potassium iodide (weight ratio = 2 / 3) and dyed while being stretched 2.1 times. The film was then stretched in a boric acid ester aqueous solution at 55°C to a total stretch ratio of 5.5 times, washed with water, and dried to prepare a PVA polarizer. The PVA polarizer had a thickness of 8 μm. Saponified cellulose acylate films (40 μm-thick TAC substrate, TG40UL, manufactured by FUJIFILM Corporation) were laminated on both sides of the PVA polarizer using a 5% aqueous solution of fully saponified polyvinyl alcohol as an adhesive. Next, the polarizing element on which the TAC film was laminated was passed through a nip roll machine and then dried at 60° C. for 10 minutes to obtain a PVA polarizing plate.

[0175] (3) Preparation of Optical Filter X The TAC surface of the PVA polarizing plate and the surface of the alignment film 1 of the laminate X were bonded together with a photocurable adhesive (Aronix LCR, manufactured by Toa Gosei Co., Ltd.), and the pressure-sensitive adhesive layer and the support on the laminate X side were peeled off to prepare an optical filter X having the following layer structure: Layer structure: PVA polarizing plate / photocurable adhesive / alignment film 1 / light absorption anisotropic layer 1 / protective layer 1.

[0176] (4) Fabrication of Head-Mounted Display X The light-shielding lens on the right side opposite the observation side of the AR glasses (BLADE manufactured by Vuzix) was removed, and an optical filter was prepared so that it could be superimposed on the light guide plate with the protective layer side facing the light guide plate. The optical filter X was superimposed on the opposite side of the light guide plate to cover the entire light guide plate, and a cover glass was attached to the opposite side of the optical filter X from the light guide plate side via an adhesive, thereby fabricating the head-mounted display X. This AR glass has an incident diffraction element, an exit diffraction element, and an intermediate diffraction element similar to those shown in FIG. 1 on the surface of the light guide plate. As mentioned above, the observation side refers to the side facing the user who uses the AR glasses, and the opposite side refers to the side opposite the user who uses the AR glasses, i.e., the side on which external light is incident.

[0177] Example 15 (1) Preparation of Laminate X Two laminates X having the following layer structure were prepared in the same manner as in Example 14. Layer structure: alignment film 1 / light absorption anisotropic layer 1 / protective layer 1 / adhesive layer / support

[0178] (2) Preparation of retardation film laminate X having a twist structure <Preparation of photo-alignment film> Coating liquid 1 for photo-alignment film was prepared with reference to the description in Example 3 of JP 2012-155308 A. The previously prepared coating liquid 1 for photo-alignment film was applied to one side of a cellulose acetate film "Z-TAC" (film thickness 40 μm) manufactured by Fujifilm Corporation using a bar coater. After application, the coating was dried on a hot plate at 120° C. for 2 minutes to remove the solvent, thereby forming a coating film. The obtained coating film was irradiated with polarized ultraviolet light (10 mJ / cm 2 , using an ultra-high pressure mercury lamp) to prepare a TAC film 4 on which a photo-alignment film AL4 was formed.

[0179] <Formation of retardation layer having a twisted structure containing a rod-like liquid crystal compound> A liquid crystal layer-forming composition 1 having the following composition was prepared. The liquid crystal layer-forming composition 1 was applied to a photo-alignment film AL4 using a bar coater to form a composition layer. The formed composition layer was heated to 110°C on a hot plate and then cooled to 60°C to stabilize the alignment. Thereafter, the layer was kept at 60°C and irradiated with ultraviolet light (500 mJ / cm) in a nitrogen atmosphere (oxygen concentration 100 ppm). 2 The alignment was fixed by a photo-alignment lamp (using an ultra-high pressure mercury lamp), and a retardation layer having a thickness of 3.5 μm and a 90° twist structure was formed by adjusting the amount of chiral agent, thereby producing a twist layer type retardation film laminate X having the following layer structure. The resulting retardation layer having a twist structure had a Δnd of 450 nm (wavelength 550 nm). Layer structure: Z-TAC / photo-alignment film / retardation layer having twist structure

[0180] ------------------------------------------------ Liquid crystal layer forming composition 1 -------------------------------------------------- 84.00 parts by mass of liquid crystal compound R1 described below 16.00 parts by mass of polymerizable compound B2 described below 0.50 parts by mass of polymerization initiator P3 described below 0.15 parts by mass of surfactant S3 described below Chiral agent 0.1 parts by mass HYSOLV MTEM (manufactured by Toho Chemical Industry Co., Ltd.) 2.00 parts by mass NK Ester A-200 (manufactured by Shin-Nakamura Chemical Co., Ltd.) 1.00 part by mass Methyl ethyl ketone 424.8 parts by mass ------------------------------------------------

[0181] Liquid crystal compound R1

[0182] Polymerizable compound B2

[0183] Polymerization initiator P3

[0184] Surfactant S3 (a = 67.5, b = 32.5, c = 0, weight average molecular weight: 20,000)

[0185] Chiral Agents

[0186] (3) Lamination of Laminate X and Twist Layer Type Retardation Film Laminate X The Z-TAC surface of the twist layer type retardation film laminate X and the surface of the alignment film 1 of the laminate X were bonded together using a photo-curable adhesive (Aronix LCR, Toa Gosei), and then the support and the adhesive layer on the laminate X side were peeled off and removed to obtain an optical filter Y. Layer structure: retardation layer having a twist structure / photo-alignment film / Z-TAC / photo-curable adhesive / alignment film 1 / light absorption anisotropic layer 1 / protective layer 1 Next, the retardation layer having a twist structure and the surface of the alignment film 1 of the second laminate X were bonded together using a photo-curable adhesive (Aronix LCR, Toa Gosei), and then the support and the adhesive layer on the laminate X side were peeled off and removed to obtain an optical filter Z. Layer structure: protective layer 1 / light-absorption anisotropic layer 1 / alignment film 1 / photo-curable adhesive / twisted retardation layer / photo-alignment film / Z-TAC / light-curable adhesive / alignment film 1 / light-absorption anisotropic layer 1 / protective layer 1

[0187] (4) Fabrication of Head Mounted Display Y A head mounted display Y was fabricated in the same manner as in Example 14, except that optical filter Z was used instead of optical filter X.

[0188] [Evaluation] An observer with a height of 180 cm wore the manufactured head-mounted display and evaluated rainbow unevenness caused by external light from fluorescent lamps placed in three locations above the head. The positions of the fluorescent lamps in the evaluation system for the head-mounted display of the present invention are shown in Figures 3 and 4, and the results are shown in Table 2. Table 2 below also lists the visibility through the AR glasses, i.e., the visibility of the background. 0: Rainbow unevenness is clearly visible 1: Rainbow unevenness is visible 2: Rainbow unevenness is weakly visible 3: Rainbow unevenness is slightly visible 4: Rainbow unevenness is very slightly visible 5: Rainbow unevenness is not visible at all

[0189]

[0190] From the results shown in Table 2, it was found that the head-mounted displays produced in Examples 14 and 15 had sufficient visibility of the background and effectively suppressed rainbow unevenness caused by external light entering from above and in front of the head.

[0191] REFERENCE SIGNS LIST 10 Optical filter 12 Polarizer 14 Laminate 80 Head-mounted display 82 Light guide plate 90 Incident diffraction element 92 Outgoing diffraction element 94 Intermediate diffraction element I 0 Front external light I 1 Video Light I s Oblique external light

Claims

1. A laminate having a protective layer, an optically absorptive anisotropic layer, an alignment film and an attachment layer adjacent to each other in this order, the optically absorptive anisotropic layer containing a dichroic material, a liquid crystal compound and a vertical alignment agent, the angle θ between the central axis of transmittance of the optically absorptive anisotropic layer and the normal direction to the surface of the optically absorptive anisotropic layer being 0° or more and 45° or less, and the attachment layer being a pressure-sensitive adhesive layer or an adhesive layer.

2. The laminate according to claim 1, wherein the light absorption anisotropic layer is a layer formed by fixing the alignment state of a liquid crystal composition containing the dichroic substance, the liquid crystal compound, the vertical alignment agent, and an additive having a crosslinkable group.

3. The laminate according to claim 2, wherein the crosslinkable group is an active hydrogen reactive group, and the vertical alignment agent is an ionic vertical alignment agent.

4. The laminate according to any one of claims 1 to 3, wherein the vertical alignment agent comprises an ionic vertical alignment agent and a vertical alignment agent having a boronic acid group.

5. The laminate according to any one of claims 1 to 3, wherein at least one of the protective layer and the alignment film contains an additive having an active hydrogen reactive group.

6. The content of the dichroic material contained in the light absorption anisotropic layer is 20 to 650 mg / cm 3 The laminate according to any one of claims 1 to 3, 7. The laminate according to any one of claims 1 to 3, wherein the degree of orientation of the optically absorptive anisotropic layer at a wavelength of 550 nm is 0.90 or more.

8. The laminate according to any one of claims 1 to 3, wherein the difference in the degree of orientation of the optically absorptive anisotropic layer at wavelengths of 450 nm, 550 nm and 650 nm is 0.025 or less.

9. The laminate according to any one of claims 1 to 3, wherein the light absorption anisotropic layer has a haze value of 0.3% or less.

10. The laminate according to any one of claims 1 to 3, wherein the optically absorptive anisotropic layer has a thickness of 1.5 µm or more.

11. The laminate according to claim 2 or 3, wherein the dichroic substance contained in the liquid crystal composition is a compound having a polymerizable group.

12. The laminate according to any one of claims 1 to 3, wherein at least one of the protective layer and the alignment film is made of either a polyvinyl alcohol-based resin or an acrylate-based resin.

13. The laminate according to any one of claims 1 to 3, wherein the alignment film contains any one of a polyvinyl alcohol resin, a cinnamoyl group-containing resin, and an epoxy resin.

14. The laminate according to any one of claims 1 to 3, wherein the protective layer is an acrylic resin film made of a polymer of a polyfunctional (meth)acrylate.

15. The laminate according to any one of claims 1 to 3, further comprising at least one layer selected from the group consisting of a polarizer layer, an antireflection layer, and a retardation layer.

16. The laminate of claim 15, wherein the polarizer layer is a coated polarizer layer.

Citation Information

Patent Citations

  • Film, process for producing film, and use thereof

    JP2007298967A

  • Transfer film and optical film

    WO2014178395A1

  • Production method for polarizing plate

    WO2015016296A1

  • Composition, polarizer layer, layered product, and image display device

    WO2021045192A1

  • Light-absorbing anisotropic film, laminate, and image display device