Ceramic scintillator, ceramic scintillator production method, radiation detector, and radiological examination device

The ceramic scintillator with gadolinium oxysulfide phosphor and controlled heat treatment conditions addresses the challenge of maintaining high light output and short afterglow time, enhancing radiation detection sensitivity and resolution in X-ray CT devices.

WO2024203234A1PCT designated stage expired Publication Date: 2024-10-03KK TOSHIBA +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/009361
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-11
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional ceramic scintillator manufacturing processes face challenges in achieving high light output while minimizing afterglow time, as high heat treatment temperatures can lead to surface oxidation and decreased optical output, and low temperatures are insufficient for complete removal of internal coloring.

Method used

A ceramic scintillator with a sintered body of gadolinium oxysulfide phosphor containing praseodymium as a main activator, with specific chromaticity coordinates and heat treatment conditions, including a temperature range of 900°C to 1600°C and a double-structured container setup, to control body color and prevent surface oxidation.

Benefits of technology

The solution effectively suppresses afterglow time while maintaining high light output, ensuring improved radiation detection sensitivity and resolution in X-ray CT devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024009361_03102024_PF_FP_ABST
    Figure JP2024009361_03102024_PF_FP_ABST
Patent Text Reader

Abstract

A ceramic scintillator according to an embodiment comprises a sintered body of a gadolinium oxysulfide phosphor containing praseodymium as a main activator. Where the color of the sintered body is expressed using chromaticity coordinates (x, y) based on CIE 1931 chromaticity values, the sintered body is a color satisfying (1) 0.4≤x≤0.505... and (2) 0.83x+0.075≤y≤0.83x+0.095... The ceramic scintillator according to the embodiment is obtained using a ceramic scintillator production method comprising a heat treatment step for reacting a reactive gas containing oxygen and sulfur with the sintered body. The duration of the heat treatment in the heat treatment step is 1-50 hours, inclusive.
Need to check novelty before this filing date? Find Prior Art

Description

Ceramic scintillator, ceramic scintillator manufacturing method, radiation detector, and radiation inspection device

[0001] SUMMARY OF THE INVENTION Embodiments according to the present invention relate to a ceramic scintillator, a method for manufacturing a ceramic scintillator, a radiation detector, and a radiation inspection device.

[0002] In the fields of medical diagnosis and industrial nondestructive testing, inspections are performed using radiological inspection devices such as X-ray tomography devices (hereinafter referred to as "X-ray CT devices"). X-ray CT devices include an X-ray tube (X-ray source) that irradiates a fan-shaped beam of X-rays and an X-ray detector with multiple X-ray detection elements arranged in parallel. The X-ray tube and X-ray detector are arranged opposite each other so that the tomographic plane of the object to be inspected is at the center. In X-ray CT devices, the X-ray tube and X-ray detector are rotated while irradiating the object with the fan-beam X-rays, and the intensity of the X-rays that pass through the object is measured with the X-ray detector to collect X-ray absorption data. The obtained X-ray absorption data is then analyzed by a computer to reconstruct a tomographic image of the object to be inspected.

[0003] The X-ray detectors of X-ray CT systems often use solid scintillators as detector elements, which emit visible light when stimulated by X-rays. X-ray detectors using solid scintillators can easily reduce the size of the X-ray detector elements and increase the number of channels, which can further improve the resolution of X-ray CT systems. Various materials are known as solid scintillators, but Gd 2 O 2 A ceramic scintillator made of a sintered body of a rare earth oxysulfide such as S:Pr (see, for example, Patent Document 1) has a large X-ray absorption coefficient, excellent luminous efficiency, and a short afterglow, and is therefore suitable as a scintillator material for X-ray detectors.

[0004] For example, scintillator pieces obtained by sintering rare earth oxysulfide phosphor powder using a hot pressing method or HIP (hot isostatic pressing) method, etc., and then cutting the resulting high-density sintered body into the desired shape and dimensions using a blade saw or wire saw, etc., are used as this type of ceramic scintillator.

[0005] JP-A-58-204088 JP-A-6-201834 JP-A 2000-171563

[0006] Ceramic scintillators are required to be transparent to achieve high detection sensitivity. However, simply sintering rare earth oxysulfide phosphor powder often results in internal distortion due to the pressure applied during sintering, and the composition of the sintered body is often slightly deviated from the stoichiometric ratio, resulting in a dark coloration. Furthermore, when cutting scintillator pieces from the sintered body, crystals may be crushed at the cut surface, resulting in a fractured layer approximately 3 μm to 5 μm from the surface, or a colored layer may be formed due to the pressure applied during cutting. Internal distortion of the sintered body, internal coloration due to compositional variations, or fractured or colored layers formed during cutting may reduce the light output and stability of the ceramic scintillator and may also increase its afterglow time. Therefore, in conventional ceramic scintillator manufacturing processes, heat treatments are performed in various atmospheres after scintillator pieces are cut from the rare earth oxysulfide sintered body (see, for example, Patent Documents 2 and 3). Among these, Patent Document 3 discloses a method for storing a rare earth oxysulfide sintered body and oxysulfide powder in a substantially sealed container, placing the container in a normal atmospheric firing furnace, and heat-treating the container at a temperature of 900°C to 1200°C, and absorbing sulfur and oxygen (e.g., SO ) generated by decomposition of the oxysulfide powder during the heat treatment. 2 or SO 3 (2003) describes a technique for removing coloration and internal strain of a sintered body by reacting a rare earth oxysulfide phosphor powder with a rare earth oxysulfide sintered body. The heat treatment method for a ceramic scintillator described in Patent Document 3 has been shown to be effective in removing internal coloration of a sintered body or colored layers that occur during cutting. However, if the particle size of the starting rare earth oxysulfide phosphor powder is large, it may be impossible to completely remove coloration (especially internal coloration) at temperatures between 900°C and 1200°C, and the afterglow may not be sufficiently shortened. As a result, pseudo images (artifacts) may appear in images obtained by X-ray CT scanners, leaving room for improvement.

[0007] Generally, increasing the heat treatment temperature is effective for removing internal coloration of a ceramic scintillator. However, in the heat treatment method described in Patent Document 3, if heat treatment is performed at a temperature exceeding 1200°C, the reaction between the sintered body and the oxygen contained in a considerable amount in the atmospheric air in the furnace becomes rapidly active, causing the surface of the sintered body to turn white due to oxidation, which may result in a decrease in the light output of the ceramic scintillator.

[0008] As described above, in ceramic scintillators, there is a trade-off between suppressing internal coloration and suppressing surface whitening, and it has been difficult to simultaneously suppress an increase in the afterglow time and a decrease in light output.

[0009] Embodiments according to the present invention provide a ceramic scintillator that suppresses the decrease in light output while suppressing the increase in afterglow time.

[0010] The above-described problems are solved by the following embodiments. <1> A ceramic scintillator comprising a sintered body of a gadolinium oxysulfide phosphor containing praseodymium as a main activator, wherein, when the body color of the sintered body is expressed in chromaticity coordinates (x, y) based on CIE 1931 chromaticity values, the sintered body has a body color that satisfies 0.4≦x≦0.505 ... (1) and 0.83x + 0.075≦y≦0.83x + 0.095 ... (2). <2> The ceramic scintillator according to <1>, wherein, when the body color of the sintered body is expressed in chromaticity coordinates (x, y) based on CIE 1931 chromaticity values, the sintered body has a body color that further satisfies 0.4≦x≦0.42 ... (1a) and 0.83x + 0.075≦y≦0.83x + 0.095 ... (2). <3> The ceramic scintillator according to <1> or <2>, wherein the gadolinium oxysulfide phosphor is a compound represented by the general formula: (Gd 1-a-b Pr a Ce b ) 2 O 2S (A) (wherein a is a number satisfying 0.0001≦a≦0.01, and b is a number satisfying 0≦b≦0.005). <4> A method for manufacturing a ceramic scintillator according to any one of <1> to <3>, comprising a heat treatment step of reacting the sintered body with a reactive gas containing oxygen and sulfur inside a heating furnace in an air atmosphere, wherein the heat treatment time in the heat treatment step is 1 hour or more and 50 hours or less. <5> A method for manufacturing a ceramic scintillator according to <4>, wherein the heat treatment step is carried out at a temperature in the range of 900°C or more and 1600°C or less. <6> A method for manufacturing a ceramic scintillator according to <4> or <5>, wherein the heat treatment step is carried out at a temperature in the range of more than 1100°C and less than 1300°C. <7> The method for manufacturing a ceramic scintillator according to any one of <4> to <6>, wherein the sintered body and oxysulfide powder are placed inside a container, and the heat treatment step is performed. <8> The method for manufacturing a ceramic scintillator according to <7>, wherein the container has a double or multiple layer structure including a first container and a second container inside the first container, and the sintered body is placed inside the second container, and the oxysulfide powder is placed outside the second container and inside the first container, and the heat treatment step is performed. <9> The method for manufacturing a ceramic scintillator according to <7> or <8>, wherein the oxysulfide powder is gadolinium oxysulfide powder. <10> A radiation detector comprising the ceramic scintillator according to any one of <1> to <3>. <11> A radiation inspection device comprising the radiation detector according to <10>.

[0011] Fig. 1 is a graph plotting the body colors of sintered bodies constituting ceramic scintillators of Examples and Comparative Examples on xy chromaticity coordinates. Fig. 2 is a schematic diagram showing a state when a heat treatment step is performed using a double-structured container in a manufacturing method of an embodiment. Fig. 3 is a schematic diagram showing an X-ray detector as an example of a radiation detector of an embodiment. Fig. 4 is a schematic diagram showing an X-ray CT device as an example of a radiation inspection device of an embodiment.

[0012] Various embodiments will be described below with reference to the drawings. Each figure is a schematic diagram for facilitating understanding of the embodiment, and the shapes, dimensions, ratios, etc. may differ from the actual ones in some places. However, these can be appropriately modified in design by taking into consideration the following explanation and known technologies.

[0013] <Ceramic scintillator> The ceramic scintillator of the embodiment comprises a sintered body of a gadolinium oxysulfide phosphor containing praseodymium (Pr) as a main activator. In the gadolinium oxysulfide phosphor, in addition to Pr as a main activator, a small amount of cerium (Ce), which is effective in suppressing afterglow, may be contained as a co-activator. Such gadolinium oxysulfide phosphors include those represented by the general formula: (Gd 1-a-b Pr a Ce b ) 2 O 2 Examples of suitable phosphors include phosphors having a composition represented by the formula: S ... (A) (wherein a is a number satisfying 0.0001≦a≦0.01, and b is a number satisfying 0≦b≦0.005). Note that a portion of Gd may be substituted with another rare earth element (such as at least one element selected from Y, La, and Lu), and in this case, the amount of substitution is preferably 30 mol % or less.

[0014] Gadolinium oxysulfide phosphors containing Pr as a main activator have a large X-ray absorption coefficient and excellent light output, making them particularly effective as fluorescence-generating materials for radiation detectors. The content of Pr as a main activator is preferably in the range of 0.0001 to 0.01 as the value of a in the above general formula (A). If the value of a, indicating the Pr content, is less than 0.0001, the effect as a main activator cannot be fully obtained, and the luminous efficiency tends to decrease. On the other hand, if the value of a exceeds 0.01, the luminous efficiency tends to decrease. The value of a, indicating the Pr content, is more preferably in the range of 0.0002 to 0.005. The content of Ce as a co-activator is preferably in the range of 0.005 to 0.005 as the value of b in the above general formula (A). Care must be taken when the value of b, indicating the Ce content, exceeds 0.005, as this may result in a decrease in light output.

[0015] In the ceramic scintillator of the embodiment, when the body color of the sintered body of the above-mentioned gadolinium oxysulfide phosphor (hereinafter simply referred to as "sintered body") is expressed in chromaticity coordinates (x, y) based on CIE 1931 chromaticity values, the sintered body has a body color that satisfies the following chromaticity coordinates: 0.4≦x≦0.505 ... (1) 0.83x+0.075≦y ... (2-1)

[0016] Figure 1 shows the xy chromaticity coordinates of the sintered bodies constituting the ceramic scintillators of Examples 1 to 7 and Comparative Examples 1 and 2, as described below, plotted after measuring the body color. The body color of the sintered bodies in the embodiment represents the xy chromaticity in a 10° field of view. This xy chromaticity measurement was performed using a spectrophotometer CM-3500d (trade name, manufactured by Minolta Co., Ltd.) with a D65 light source as the irradiating light, a specular reflection method, and an 8 mm measurement diameter. The surface of the measurement sample was polished with an abrasive of grit size 700 or higher to a thickness of 1.0 mm ± 0.1 mm. The measurement sample was placed in close contact with the window of the spectroscope, and a cylindrical box with a black interior, known as a zero calibration box, was placed on the opposite side of the measurement sample from the spectroscope window. The body color of the sintered bodies in the embodiment represents the xy chromaticity values ​​measured in this manner.

[0017] As described above, the fact that the sintered body has a body color (yellow or very pale orange and highly transparent color tone) that satisfies the chromaticity coordinates expressed by the above formulas (1) and (2-1) means that the internal coloring of the sintered body, which is a factor in increasing the afterglow time, has been sufficiently removed, and that whitening of the sintered body surface, which is a cause of a decrease in light output, has not occurred. Therefore, by using a sintered body having such a body color, it is possible to reproducibly provide a ceramic scintillator that is excellent in light output and has a short afterglow time.

[0018] When the x value in the xy chromaticity coordinate indicating the body color of the sintered body is less than 0.4, the opacity (degree of whiteness) increases. Ceramic scintillators using such opaque sintered bodies experience light scattering, resulting in reduced light output when irradiated with X-rays or the like. Various factors can be considered to cause the opacity of sintered bodies, but whitening due to oxidation of the sintered body surface is particularly cited. In an embodiment, highly transparent body colors can be obtained with good reproducibility by preventing oxidation of the sintered body surface, for example, based on the manufacturing method described below.

[0019] Furthermore, when the y value in the xy chromaticity coordinates indicating the body color of the sintered body is smaller than the value of the above formula (2-1) (0.83x + 0.075 > y: chromaticity below the line y = 0.83x + 0.075 in Figure 1), it means that the color tone of the sintered body as a whole is dark. This means that coloring (especially internal coloring) that occurred during sintering or processing of the sintered body has not been sufficiently removed. Ceramic scintillators using such sintered bodies will have an increased afterglow time. In other words, in sintered bodies whose y value satisfies the above formula (2-1) (sintered bodies having a chromaticity on or above the line y = 0.83x + 0.075 in Figure 1), internal coloring has been sufficiently removed, and the afterglow time of the ceramic scintillator can be sufficiently shortened. Note that even in sintered bodies of gadolinium oxysulfide phosphors activated with Ce in addition to Pr, ceramic scintillators with sufficiently short afterglow times can be obtained by satisfying the above formula (2-1) for the y value of the body color.

[0020] In the xy chromaticity coordinates, the sum of the x and y values ​​(x + y) is 1 or less. When the above formula (2-1) is satisfied and x + y ≦ 1 is satisfied, the maximum value of the x value is approximately 0.505. Therefore, the upper limit of the x value of the xy chromaticity coordinates in the embodiment is 0.505 as expressed by the above formula (1). Furthermore, the upper limit of the y value of the xy chromaticity coordinates is not necessarily limited. Within the range of the x value of the xy chromaticity coordinates defined by the above formula (1), an increase in the y value means that the green tone becomes stronger. A gadolinium oxysulfide phosphor activated with Pr has a green emission spectrum, and even if the body color of the sintered compact becomes more green, the light output of the ceramic scintillator does not decrease significantly.

[0021] The green hue of the body color of the sintered body is mainly determined by the Pr concentration. Therefore, taking into consideration a practical Pr concentration and in order to obtain a higher-output scintillator, it is preferable that the y value of the body color of the sintered body satisfies y≦0.83x+0.095 ... (2-2). That is, the sintered body in the embodiment satisfies the x value in the above formula (1) and has a body color that satisfies 0.83x+0.075≦y≦0.83x+0.095 ... (2).

[0022] Examples of sintered bodies that do not have a body color that satisfies the y value in the above formula (2) include sintered bodies in which impurities are partially segregated, etc. In particular, if elements that cause coloring or the like are segregated in the sintered body, there is a risk that the performance as a scintillator will vary.

[0023] In the ceramic scintillator of the embodiment, as described above, Ce may or may not be added to the gadolinium oxysulfide phosphor. When Ce is not added, the internal coloring of the sintered body can be sufficiently removed, thereby sufficiently shortening the afterglow time. By not adding Ce to the gadolinium oxysulfide phosphor, homogeneous material properties can be easily obtained and light output can be improved. Therefore, when a gadolinium oxysulfide phosphor without Ce addition is used in the radiological inspection device described below, high-resolution images can be easily obtained even with a low X-ray dose. Since a ceramic scintillator without Ce addition can reduce the exposure dose of the subject, it is suitable for use in X-ray inspection devices for medical diagnosis. On the other hand, adding Ce to the gadolinium oxysulfide phosphor can further shorten the afterglow time. Therefore, when a gadolinium oxysulfide phosphor with Ce addition is used in the radiological inspection device described below, high-resolution images can be easily obtained even with continuous irradiation of a large X-ray dose. A ceramic scintillator with Ce addition can be suitable for use in industrial X-ray nondestructive inspection devices.

[0024] The body color of a sintered body without Ce addition exhibits a lower x value in the xy chromaticity coordinates than when Ce is added. Therefore, in embodiments, it is preferable that the x value satisfy the following relationship: 0.4≦x≦0.42 (1a). When the x value in the xy chromaticity coordinates, which indicates the body color of the sintered body, satisfies the above formula (1a), a particularly large light output can be obtained with good reproducibility. That is, in the ceramic scintillator of the embodiment, it is preferable that the sintered body has a body color that satisfies the above formulas (1a) and (2). Furthermore, if the heat treatment time in the heat treatment step described below is short, the x value tends to be small, reaching 0.42 or less. It is also preferable that the x value satisfy the above formula (1a) from the viewpoint of increasing the rotation rate of the heating furnace by shortening the heat treatment time and preventing an increase in manufacturing costs.

[0025] The x value of the xy chromaticity coordinates that indicate the body color of the sintered body is preferably 0.407 or more, from the viewpoint of obtaining a larger light output.

[0026] The color difference of the sintered body is preferably small. For example, the difference between the x value at any point on the measurement surface of the x-y chromaticity coordinates and the x value at any point 5 mm or more away from that point is preferably 0.01 or less. Furthermore, the difference between the y value at any point on the measurement surface of the x-y chromaticity coordinates and the y value at any point 5 mm or more away from that point is also preferably 0.01 or less. For example, the difference between the x value at any point on the measurement surface of the x-y chromaticity coordinates and the x value at any point on the surface opposite to the measurement surface is preferably 0.01 or less. Furthermore, the difference between the y value at any point on the measurement surface of the x-y chromaticity coordinates and the y value at any point on the surface opposite to the measurement surface is also preferably 0.01 or less. By controlling the color difference to be small at all measurement points, partial performance variation of the scintillator can be suppressed.

[0027] In the sintered body constituting the ceramic scintillator of the embodiment, it is preferable that other properties other than the body color are equal to or better than those of conventional ceramic scintillators. For example, with regard to the sintered body density, which affects the light transmittance, it is preferable that the relative density (density ratio to true density) is 99.5% or more. If the relative density of the Pr-activated gadolinium oxysulfide sintered body is less than 99.5%, light scattering is likely to occur, and care should be taken as this may result in a decrease in the light transmittance or light output of the ceramic scintillator.

[0028] <Method for manufacturing ceramic scintillator> Next, details of the method for manufacturing the ceramic scintillator of the embodiment will be described. The manufacturing method of the embodiment is suitable for manufacturing the ceramic scintillator described above, but is not necessarily limited thereto, and can be applied to manufacturing ceramic scintillators made of sintered bodies of various rare earth oxysulfide phosphors.

[0029] In the manufacturing method of the embodiment, first, a gadolinium oxysulfide phosphor powder, which is the raw material for the sintered body, is prepared. Specifically, predetermined amounts of rare earth elements such as Gd, Pr, and Ce are weighed and thoroughly mixed. In this process, oxides such as gadolinium oxide or praseodymium oxide are used as the starting materials. It is preferable to use a homogeneous mixed oxide obtained by firing an oxalic acid coprecipitate or the like as the mixture of these starting materials.

[0030] The resulting mixture is then mixed with a sulfurizing agent such as sulfur (S) powder and a 3 P.O. 4 or A 2 CO 3 (A is at least one element selected from Li, Na, K, Rb, and Cs) and a flux such as ZnO. The mixed powder is fired at a temperature of 1100°C to 1300°C for 5 to 10 hours, and then washed with acid and water to obtain a gadolinium oxysulfide phosphor powder.

[0031] The gadolinium oxysulfide phosphor powder thus obtained is used as a raw material for a sintered body that will be a constituent material of a ceramic scintillator. In the embodiment, the average particle size of the gadolinium oxysulfide phosphor powder is not particularly limited, but if the average particle size is too small, it becomes difficult to produce a large sintered body, and if the average particle size is too large, a higher temperature will be required during sintering. From this perspective, the average particle size of the gadolinium oxysulfide phosphor powder is preferably, for example, 1 μm or more and 50 μm or less, and more preferably 5 μm or more and 20 μm or less.

[0032] Furthermore, in the embodiment, even when a gadolinium oxysulfide phosphor powder having an average particle size of 20 μm or more is used, the internal coloring of the sintered body can be effectively removed by the heat treatment described below. In other words, even when a gadolinium oxysulfide phosphor powder having a relatively large average particle size is used to improve light output, the afterglow time caused by internal coloring can be sufficiently shortened.

[0033] Next, the gadolinium oxysulfide phosphor powder is sintered to produce a sintered body that will be a constituent material of the ceramic scintillator. When sintering the gadolinium oxysulfide phosphor powder, known sintering methods such as hot pressing or HIP can be applied. Among these, it is preferable to carry out sintering by applying the HIP method, particularly from the viewpoint of easily obtaining a sintered body with high density.

[0034] Sintering using the HIP method is performed, for example, by first molding gadolinium oxysulfide phosphor powder into an appropriate shape using a rubber press, then filling and sealing it in a metal container or the like and subjecting it to HIP treatment. The HIP conditions here are preferably a HIP temperature of 1300°C to 1600°C, a HIP pressure of 98 MPa or more, and a HIP time of 1 hour to 10 hours. The HIP temperature is more preferably 1350°C to 1600°C. By performing HIP treatment under these conditions, a sintered body with a relative density of, for example, 99.5% or more can be reproducibly obtained. If the relative density of the sintered body is less than 99.5%, the properties required for a ceramic scintillator, such as light transmittance or light output, cannot be satisfied.

[0035] Next, the resulting sintered body is cut into the desired shape and dimensions using a blade saw or wire saw to produce scintillator pieces, etc. Sintered bodies can suffer from internal distortion due to the pressure during sintering, or slight deviations in the sintered body's composition from the stoichiometric ratio, resulting in internal coloration. Furthermore, when cutting scintillator pieces, etc. from the sintered body, a colored layer can form on the surface due to the pressure during cutting. These coloration phenomena reduce the light output or stability of the ceramic scintillator and increase its afterglow time. Therefore, after cutting the sintered body into the desired shape, it is subjected to heat treatment to restore the light output and remove the coloration. This heat treatment process involves reacting the cut sintered body with a reactive gas containing oxygen and sulfur in, for example, a heating furnace in an atmospheric atmosphere. Specifically, a sealable container is placed in the furnace in an atmospheric atmosphere, and the cut sintered body is reacted with the reactive gas containing oxygen and sulfur in this container.

[0036] In the manufacturing method of the embodiment, the inside of the heating furnace may be filled with an inert gas atmosphere such as nitrogen gas or argon gas instead of the air atmosphere. However, from the viewpoint of eliminating the need to replace the inside of the heating furnace with an inert gas flow and preventing an increase in manufacturing costs, it is preferable to fill the inside of the heating furnace with the air atmosphere.

[0037] The heat treatment is preferably carried out at a temperature in the range of 900°C to 1600°C. This relieves the internal strain of the sintered body generated during sintering and fills oxygen and sulfur vacancies, thereby removing the internal coloring of the sintered body. Furthermore, colored layers generated during cutting can also be removed at the same time. If the heat treatment temperature is less than 900°C, oxygen and sulfur may not be sufficiently diffused into the sintered body, and the internal coloring may not be sufficiently removed. On the other hand, if the heat treatment temperature exceeds 1600°C, the crystal grains of the sintered body may become coarse, and the processed shape may not be maintained.

[0038] In the manufacturing method of the embodiment, even when the heat treatment temperature is set to a high temperature exceeding 1100°C, for example, the surface of the sintered body is not oxidized, and whitening of the surface of the sintered body, which causes a decrease in light output, can be prevented. Therefore, it is possible to reproducibly provide a ceramic scintillator that is excellent in light output and stability and has a short afterglow time. In particular, in the manufacturing method of the embodiment, it is preferable to perform the heat treatment at a temperature exceeding 1100°C and less than 1300°C.

[0039] The heat treatment time is set appropriately depending on the heat treatment temperature, the state of the sintered body to be treated, the concentration of the reactive gas, the type of reactive gas, etc., but in practice it is preferably in the range of 1 hour to 50 hours. If the heat treatment time is less than 1 hour, there is a risk that internal coloring may not be sufficiently removed in some cases. On the other hand, even if the heat treatment time is set to more than 50 hours, no further effect will be obtained and production costs will increase. In particular, in the production method of the embodiment, the heat treatment time is preferably 3 hours to 14 hours, and more preferably 5 hours to 7 hours.

[0040] That is, in the manufacturing method of the embodiment, the problems of the prior art associated with high-temperature heat treatment (oxidation of the sintered body surface and the resulting whitening) are prevented by adjusting the heat treatment time. Therefore, the heat treatment can be performed in a high temperature range of over 1100°C, which is effective for removing internal coloring. In other words, according to the manufacturing method of the embodiment, by setting the heat treatment time within a certain range, it is possible to prevent whitening of the sintered body surface and remove internal coloring, thereby further shortening the afterglow time of the ceramic scintillator and maintaining good light output.

[0041] In the heat treatment step in the embodiment, a reaction gas containing oxygen and sulfur is used. Although the method for generating the reaction gas is not particularly limited, it is preferable to use an oxysulfide powder as a reaction gas source from the viewpoint of obtaining a reaction gas with an appropriate concentration of oxygen and sulfur. For example, the sintered body and the oxysulfide powder are housed in a sealable container, and the container is placed in a heating furnace in an airtight atmosphere for heat treatment. As a result, the oxysulfide powder decomposes near the heat treatment temperature to produce SO x Gas (e.g., SO 2 or SO 3 In the embodiment, it is preferable to react the reaction gas thus obtained with the sintered body.

[0042] Here, the oxysulfide powder that is the source of the reaction gas may be a mixed powder obtained by mixing an oxide powder and a sulfide powder in a predetermined composition ratio. 2 O 2 S) powder or yttrium oxysulfide (Y 2 O 2 Alternatively, a rare earth oxysulfide powder such as a gadolinium oxysulfide (S) powder may be used. Among these, it is preferable to use a gadolinium oxysulfide powder as the oxysulfide powder, from the viewpoint of generating oxygen and sulfur in the composition ratio of the gadolinium oxysulfide phosphor. Furthermore, the rare earth oxysulfide powder may be composed of a pure compound, or may have a composition containing an activator, similar to the gadolinium oxysulfide phosphor.

[0043] The sintered body and the oxysulfide powder (particularly the rare earth oxysulfide powder) may be contained in a single-walled container so as not to be in direct contact with each other, but it is preferable to use a container with a double or more walled structure. For example, by using a double-walled container as shown in Figure 2, reaction control becomes easier and internal coloring of the sintered body can be removed with good reproducibility.

[0044] FIG. 2 is a schematic diagram illustrating a heat treatment process using a double-layered container in the manufacturing method according to the embodiment. A scintillator piece, e.g., a sintered body 2 after cutting, is placed inside a small crucible serving as the second container 1, and the opening of the second container 1 is covered with a small lid 3. Next, the second container 1 is placed inside a large crucible serving as the first container 4, and the outside (surrounding area) of the second container 1 is tightly filled with oxysulfide powder 5. In other words, the second container 1 containing the sintered body 2 is embedded in the oxysulfide powder 5. The opening of the first container 4 is then sealed with a large lid 6. Next, the double-layered containers containing the sintered body 2 in the second container 1 and the oxysulfide powder 5 in the first container 4 are placed inside a heating furnace 7, and the atmospheric gas 8 inside the heating furnace 7 is, for example, air, and heat treatment is performed at the above-mentioned temperature. This heat treatment allows the reaction gas (e.g., SO ) generated by the decomposition of the oxysulfide powder 5 to be released. x The reaction gas (reaction gas containing oxygen and sulfur as catalysts) reacts with the sintered body 2, removing any internal coloring of the sintered body 2 and providing a ceramic scintillator with a short afterglow time. In addition, the surface of the sintered body 2 can be prevented from whitening during heat treatment, allowing the ceramic scintillator to maintain its excellent light output.

[0045] According to the manufacturing method of the embodiment, the body color of the sintered body can be made to a predetermined color tone with good reproducibility, so that a ceramic scintillator with excellent light output and a short afterglow time can be obtained with good reproducibility.

[0046] The ceramic scintillators of the embodiments, or ceramic scintillators obtained by the manufacturing methods of the embodiments, have excellent light output and short afterglow times. Therefore, by using such ceramic scintillators as fluorescence-generating materials in radiation detectors, it is possible to improve radiation detection sensitivity and suppress false images. This greatly contributes to the miniaturization and high resolution of radiation detectors.

[0047] <Radiation Detector and Radiation Inspection Apparatus> Next, a radiation detector and a radiation inspection apparatus according to an embodiment will be described with reference to FIGS.

[0048] Fig. 3 is a schematic diagram showing the configuration of an X-ray detector, which is an example of a radiation detector according to an embodiment. The X-ray detector 11 shown in Fig. 3 has a ceramic scintillator 12 as a fluorescence generating material. The ceramic scintillator 12 is made of, for example, a scintillator piece cut into a desired shape from a sintered body, or a scintillator block formed by stacking a plurality of scintillator pieces vertically and horizontally.

[0049] The rectangular rod-shaped ceramic scintillator 12 is covered on all but one surface with a reflective film 13, and a photoelectric conversion element such as a silicon photodiode 15 is attached as a photoelectric conversion member via an adhesive layer 14 to the surface not covered with the reflective film 13. When a scintillator block in which multiple scintillator pieces are integrated is used as the ceramic scintillator 12, a silicon photodiode 15 is arranged corresponding to each scintillator piece.

[0050] In the above-described X-ray detector 11, X-rays are incident on the ceramic scintillator 12, which emits light in accordance with the amount of X-rays incident thereon. The light emitted from the ceramic scintillator 12 is detected by a silicon photodiode 15. The output of the light emitted in accordance with the amount of X-rays incident thereon is converted into an electrical output by the silicon photodiode 15 and then sent from an output terminal 16 to, for example, a computer in the X-ray CT device.

[0051] Fig. 4 is a schematic diagram showing the configuration of an X-ray CT device, which is an example of a radiological inspection device according to an embodiment. The X-ray CT device 20 shown in Fig. 4 has the above-mentioned X-ray detector 11. The X-ray detector 11 is attached to the inner wall of a cylinder on which an imaging region of an inspected object 21 is placed. An X-ray tube 22 that emits X-rays is disposed approximately at the center of the arc on which the X-ray detector 11 is attached.

[0052] A fixed object under inspection 21 is placed between the X-ray detector 11 and the X-ray tube 22. The X-ray detector 11 and the X-ray tube 22 are configured to rotate around the fixed object under inspection 21 while taking an image using X-rays. In this way, image information of the object under inspection 21 is collected three-dimensionally from different angles.

[0053] The signal obtained by the X-ray imaging (electrical signal converted by the silicon photodiode 15) is processed by a computer 23 and displayed on a display 24 as an image 25 of the object to be inspected. The image 25 of the object to be inspected is, for example, a tomographic image of the object to be inspected 21. In this case, by using a scintillator block in which a plurality of scintillator pieces are integrated as the ceramic scintillator 12, a multi-tomographic image type X-ray CT device is constructed, which makes it possible to simultaneously capture a plurality of tomographic images of the object to be inspected 21. Such a multi-tomographic image type X-ray CT device can also depict the imaging results in three dimensions.

[0054] The X-ray CT scanner 20 described above uses ceramic scintillators with a short decay time, which effectively prevents the appearance of false images. Furthermore, the output from each ceramic scintillator is high, which improves resolution. These features significantly improve the medical diagnostic capabilities of the X-ray CT scanner 20.

[0055] The radiation inspection apparatus of the embodiment is not limited to an X-ray inspection apparatus for medical diagnosis, but can also be applied to an X-ray non-destructive inspection apparatus for industrial use, etc. The radiation inspection apparatus of the embodiment also contributes to improving the inspection accuracy of the X-ray non-destructive inspection apparatus.

[0056] Next, specific examples of the embodiment and their evaluation results will be described.

[0057] [Example 1] Average particle size is 10 μm, (Gd 0.999 , Pr 0.001 ) 2 O 2Gadolinium oxysulfide phosphor powder having a composition of S was molded using a rubber press. The molded body was sealed in a Ta capsule and then set in a HIP treatment device. Argon gas was sealed in the HIP treatment device as a pressure medium, and a sintered body was produced by processing for 3 hours under conditions of a pressure of 148 MPa and a temperature of 1500°C. After cooling, the sintered body was removed, and 1 × 2 × 30 mm rod-shaped samples were cut out of the sintered body using a blade saw to produce multiple scintillator pieces.

[0058] Next, as shown in Figure 2, the scintillator pieces were placed in a second container (small crucible: capacity 500 cc) made of high-purity alumina, and the opening of the second container was covered with a small lid. A first container (large crucible) made of high-purity alumina, which was slightly larger than the second container, was prepared, and the second container containing the scintillator pieces was placed inside the first container, and gadolinium oxysulfide (Gd oxysulfide powder) was placed around the second container. 2 O 2 S) The powder was filled in tightly, and the opening of the first container was then sealed with a large lid.

[0059] Next, the double-walled container, in which the second container was housed inside the first container, was placed inside heating furnace 7, and heat treatment was performed for 1 hour in an atmospheric environment. During this heat treatment process, the oxysulfide powder packed inside the first container so as to cover the periphery of the second container was decomposed, generating a reaction gas containing oxygen and sulfur. The ceramic scintillator of Example 1, consisting of a sintered body, was produced by reacting this reaction gas with the scintillator pieces.

[0060] Example 2 A ceramic scintillator of Example 2 was produced in the same manner as in Example 1, except that the heat treatment was carried out for 5 hours.

[0061] Example 3 A ceramic scintillator of Example 3 was produced in the same manner as in Example 1, except that the heat treatment was carried out for 7 hours.

[0062] Example 4 A ceramic scintillator of Example 4 was produced in the same manner as in Example 1, except that the heat treatment was carried out for 10 hours.

[0063] Example 5 A ceramic scintillator of Example 5 was produced in the same manner as in Example 1, except that the heat treatment was carried out for 12 hours.

[0064] Example 6 A ceramic scintillator of Example 6 was produced in the same manner as in Example 1, except that the heat treatment was carried out for 14 hours.

[0065] Comparative Example 1 A ceramic scintillator of Comparative Example 1 was produced in the same manner as in Example 1, except that the scintillator pieces were not subjected to heat treatment.

[0066] [Comparative Example 2] (Gd 0.999 , Pr 0.001 ) 2 O 2 Instead of the gadolinium oxysulfide phosphor powder having the composition of S (Gd 0.9989 , Pr 0.0009 , Ce 0.0002 ) 2 O 2 A ceramic scintillator of Comparative Example 2 was produced in the same manner as in Example 1, except that a gadolinium oxysulfide phosphor powder having a composition of S was used.

[0067] Example 7 A ceramic scintillator of Example 7 was produced in the same manner as in Comparative Example 2, except that the heat treatment was carried out for 5 hours.

[0068] [Body Color Measurement] The body colors of the ceramic scintillators (sintered bodies) of Examples 1 to 7 and Comparative Examples 1 and 2 were measured according to the method described above. The measurement results are shown in Table 1. FIG. 1 is a graph plotting the xy chromaticity coordinates showing the body colors of the ceramic scintillators of Examples 1 to 7 and Comparative Examples 1 and 2. In FIG. 1, ○ indicates the results of the Examples, and △ indicates the results of the Comparative Examples. Furthermore, for each of the ceramic scintillators of Examples 1 to 7 and Comparative Examples 1 and 2, body color was measured at four arbitrary locations in addition to the above measurement locations. That is, body color was measured at a total of five locations on one surface (front surface) of the ceramic scintillator. The five measurement locations were 5 mm or more apart from each other. Furthermore, body color was measured at five arbitrary locations 5 mm or more apart from each other on the surface opposite the front surface (rear surface). In all of the ceramic scintillators of Examples 1 to 7 and Comparative Examples 1 and 2, the difference between the maximum and minimum x values ​​at a total of 10 measurement locations (five locations on the front surface and five locations on the back surface) was 0.01 or less, and the difference between the maximum and minimum y values ​​at a total of 10 measurement locations was also 0.01 or less. In other words, the color difference of the sintered body was small.

[0069] [Measurement of Light Output and Afterglow] Next, an X-ray detector shown in FIG. 3 was constructed for each of the ceramic scintillators of Examples 1 to 7 and Comparative Examples 1 and 2. The current flowing through the silicon photodiode when the X-ray detector was irradiated with X-rays of 120 kVP and 200 mA was measured. Cadmium tungstate (CdWO 4 The light output of the ceramic scintillators of Examples 1 to 7 and Comparative Examples 1 and 2 was determined as a relative value when the current value when a scintillator made of a single crystal of the above compound was used in an X-ray detector was set to 100. The light emission intensity I 0 and the emission intensity I 10 ms after the X-ray irradiation was stopped. 10 and were measured. 0 I against 10 The ratio of the two was calculated and used as the afterglow intensity. The measurement results are shown in Table 1.

[0070]

[0071] As is clear from Table 1 and FIG. 1 , the ceramic scintillators of Examples 1 to 7 had body colors that satisfied the above formulas (1) and (2). The ceramic scintillators of Examples 1 to 6 had light outputs that were approximately 1.14 to 1.22 times greater and afterglow intensities after 10 ms were approximately 0.10 to 0.33 times smaller than the ceramic scintillator of Comparative Example 1. Furthermore, the ceramic scintillator of Example 7 had light outputs that were approximately 1.13 times greater and afterglow intensities after 10 ms were approximately 0.33 times smaller than the ceramic scintillator of Comparative Example 2. As described above, it can be seen that the ceramic scintillators of the embodiments suppress a decrease in light output while suppressing an increase in afterglow time. Furthermore, it was found that the ceramic scintillators of Examples 1 to 6, which did not contain a co-activator, had relatively greater light outputs and were more suitable for suppressing a decrease in light output than the ceramic scintillator of Example 7, which contained Ce as a co-activator.

[0072] Although several embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be embodied in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are included within the scope and spirit of the invention, and are also included in the scope of the invention and its equivalents as defined in the claims.

[0073] REFERENCE SIGNS LIST 1 Second container (small crucible) 2 Sintered body (scintillator piece) 3 Small lid 4 First container (large crucible) 5 Oxysulfide powder 6 Large lid 7 Heating furnace 8 Atmospheric gas 11 X-ray detector 12 Ceramic scintillator 13 Reflective film 14 Adhesive layer 15 Silicon photodiode 16 Output terminal 20 X-ray CT device 21 Inspected object 22 X-ray tube 23 Computer 24 Display 25 Inspected object image

Claims

1. A ceramic scintillator comprising a sintered body of a gadolinium oxysulfide phosphor containing praseodymium as a main activator, wherein, when the body color of the sintered body is expressed in chromaticity coordinates (x, y) based on the CIE 1931 chromaticity values, the body color satisfies 0.4≦x≦0.505 ... (1) and 0.83x + 0.075≦y≦0.83x + 0.095 ... (2).

2. A ceramic scintillator according to claim 1, wherein, when the body color of the sintered body is expressed in chromaticity coordinates (x, y) based on the CIE 1931 chromaticity values, the sintered body has a body color that further satisfies: 0.4≦x≦0.42 ... (1a) and 0.83x + 0.075≦y≦0.83x + 0.095 ... (2).

3. The ceramic scintillator according to claim 1 or 2, wherein the gadolinium oxysulfide phosphor is represented by the general formula: (Gd 1-a-b P a C.E. b ) 2 O 2 A ceramic scintillator having a composition represented by the formula: S(A) (wherein a is a number satisfying 0.0001≦a≦0.01, and b is a number satisfying 0≦b≦0.005).

4. A method for manufacturing a ceramic scintillator according to claim 1 or 2, comprising a heat treatment step of reacting the sintered body with a reactive gas containing oxygen and sulfur, the heat treatment time in the heat treatment step being 1 hour or more and 50 hours or less.

5. A method for producing a ceramic scintillator according to claim 4, wherein the heat treatment step is carried out at a temperature in the range of 900°C to 1600°C.

6. The method for producing a ceramic scintillator according to claim 4, wherein the heat treatment step is carried out at a temperature in the range of more than 1100°C and less than 1300°C.

7. A method for producing a ceramic scintillator according to claim 4, wherein the sintered body and oxysulfide powder are placed inside a container and the heat treatment step is carried out.

8. A method for manufacturing a ceramic scintillator as described in claim 7, wherein the container has a double or multiple structure including a first container and a second container inside the first container, the sintered body is contained inside the second container, the oxysulfide powder is contained outside the second container and inside the first container, and the heat treatment process is performed.

9. A method for producing a ceramic scintillator according to claim 7, wherein the oxysulfide powder is gadolinium oxysulfide powder.

10. A radiation detector comprising the ceramic scintillator according to claim 1 or 2.

11. A radiation inspection device comprising the radiation detector according to claim 10.

Citation Information

Patent Citations

  • Scintillation detector

    JP1983204088A

  • Ceramic scintillator

    JP1994201834A

  • Producing method for ceramic scintillator, ceramic scintillator, scintillator block, x-ray detector and x-ray ct imaging device

    JP2000171563A

  • Ceramic scintillator

    JP2000178547A

  • Ceramic scintillator and method for producing the same, and radioactive ray detector and radioactive ray- surveying instrument by using the same