Sintering method of gadolinium oxysulfide scintillation ceramic, gadolinium oxysulfide scintillation ceramic and application
By using a mixed gas of dry pressure and reducing gas mixture in the sintering process of sulphur oxide, the problems of high cost of equipment and complex sintering process in the prior art are solved, and gadolinium sulfur with fine grains and high density are achieved The preparation of ceramics is suitable for the sintering of large samples and special materials.
Patent Information
- Application Number
- CN202411032851.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-01
AI Technical Summary
The existing sulfur gadolinium oxide sintering equipment has high technical requirements and high cost, the sintering process is complicated, and it is prone to uneven stress leading to internal defects, and there are limitations on the sintering of large samples and special materials.
The sulfur gadolinium oxide raw material cake obtained by dry pressure was sintered under positive pressure conditions, and the mixed gas of reducing gas and inert gas was sintered. The sintering temperature was 800℃-1500℃, and the relative pressure was 1kpa-500kpa. The mixed gas was passed The pressure is applied to gadolinium sulfur oxide from all directions, reducing the sintering temperature and time, inhibiting grain growth, and improving density.
It realizes sulphur gadolinium oxide ceramic products with fine grains and high density, reduces sintering temperature and time, improves the mechanical properties of ceramic materials, simplifies equipment costs, and is suitable for sintering of large samples and special materials.
Smart Images

Figure BDA0004970351750000081 
Figure BDA0004970351750000091
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of scintillation ceramics, and in particular to a sintering method of gadolinium oxysulfide scintillation ceramics, gadolinium oxysulfide scintillation ceramics and applications thereof. Background Art
[0002] The current sintering methods of gadolinium oxysulfide are mainly hot pressing, hot sintering and spark plasma sintering, as well as hot pressing followed by hot sintering or hot pressing followed by spark plasma sintering. The purpose of these sintering methods is to obtain ultra-high purity ceramic products with fine grains and high density, but they have high requirements for equipment technology, complex sintering process and equipment, strict production control requirements, and high requirements for mold materials, resulting in large equipment investment and high operating costs. In addition, uneven stress may occur during the sintering process, which may lead to internal defects of the product. At the same time, there are certain limitations for the sintering of large samples or special materials.
[0003] In view of this, the present invention is proposed. Summary of the invention
[0004] The purpose of the present invention is to provide a sintering method of gadolinium oxysulfide scintillation ceramics, gadolinium oxysulfide scintillation ceramics and applications.
[0005] The present invention is achieved in that:
[0006] In a first aspect, the present invention provides a sintering method for gadolinium oxysulfide scintillating ceramics, comprising: sintering a gadolinium oxysulfide raw material cake obtained by dry pressing, the sintering temperature being 800°C-1500°C, the sintering atmosphere being a mixed gas of a reducing gas and an inert gas, and the relative pressure of the sintering step being 1 kPa-500 kPa.
[0007] In an optional embodiment, the relative pressure of the sintering step is 10-50 kPa;
[0008] And / or, the sintering temperature is 1000°C-1500°C.
[0009] In an optional embodiment, the volume ratio of reducing gas to inert gas in the sintering atmosphere is 1-1.5:1.
[0010] In an optional embodiment, the inert gas is selected from at least one of helium, neon and argon; and / or the reducing gas is selected from at least one of hydrogen, carbon monoxide and methane.
[0011] In an optional embodiment, the sintering time is 0.5-5h.
[0012] In an optional embodiment, the sintering is carried out in a sintering furnace:
[0013] Before the sintering step, the sintering furnace is heated to the sintering temperature at a temperature of 10-30°C / min;
[0014] And / or, after the sintering step, the sintering furnace is cooled to 15-50°C at a rate of 10-30°C / min.
[0015] In an optional embodiment, before the sintering furnace is heated, the vacuum is first evacuated to a vacuum degree of less than 10 -3 Pa, and then the mixed gas is introduced into the sintering furnace.
[0016] In an optional embodiment, the flow rate of the mixed gas is 10 ml / min-1500 ml / min, preferably 10 ml / min-100 ml / min.
[0017] In a second aspect, the present invention provides a gadolinium oxysulfide scintillating ceramic, which is prepared by the sintering method of the gadolinium oxysulfide scintillating ceramic described in any one of the aforementioned embodiments;
[0018] Preferably, the average grain size of the gadolinium oxysulfide scintillating ceramic is 5-20 μm and the density is 7.2-7.4 g / cm 3 .
[0019] In a third aspect, the present invention provides an application of the gadolinium oxysulfide scintillating ceramic described in the aforementioned embodiment, wherein the application includes use in X-ray detectors, security inspection machines, non-destructive testing, gadolinium oxysulfide fluorescent screens in DR detectors, and computed tomography imaging.
[0020] The present invention has the following beneficial effects:
[0021] In the present invention, the gadolinium oxysulfide raw material cake obtained by dry pressing is sintered under positive pressure to obtain gadolinium oxysulfide scintillating ceramics. During the sintering process, the gadolinium oxysulfide raw material cake is simultaneously subjected to positive pressure and high temperature, wherein the pressure comes from the mixed gas, and the gadolinium oxysulfide can be pressed from all directions. At the same time, the powder is in a thermoplastic state, which is conducive to the contact diffusion of particles, the flow mass transfer process and the gas discharge. Therefore, the sintering temperature can be reduced and the sintering time can be shortened, thereby helping to inhibit the growth of grains and the discharge of gas between grains or particles, thereby facilitating the acquisition of ceramic products with fine grains and high density, and at the same time improving the mechanical properties of the ceramic material. DETAILED DESCRIPTION
[0022] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0023] An embodiment of the present invention provides a sintering method for gadolinium oxysulfide scintillating ceramics, comprising: sintering a gadolinium oxysulfide raw material cake obtained by dry pressing, the sintering temperature being 800° C.-1500° C., the sintering atmosphere being a mixed gas of a reducing gas and an inert gas, and the relative pressure of the sintering step being 1 kPa-500 kPa.
[0024] Usually, a mold is used to apply pressure to gadolinium oxysulfide during the sintering of gadolinium oxysulfide scintillating ceramics, but the mold usually only applies force to gadolinium oxysulfide in one-dimensional direction. In the embodiment of the present invention, the gadolinium oxysulfide raw material cake obtained by dry pressing is sintered under positive pressure conditions. During the sintering process, the gadolinium oxysulfide raw material cake is simultaneously subjected to positive pressure and high temperature. The pressure comes from the mixed gas, which can apply pressure to gadolinium oxysulfide from all directions. At the same time, the powder is in a thermoplastic state, which is conducive to the contact diffusion of particles, the flow mass transfer process and gas discharge. Therefore, the gadolinium oxysulfide raw material cake can be formed under a relatively low pressure to meet the needs. Specifically, the pressure of preparing the gadolinium oxysulfide raw material cake by dry pressing is 200-260MPa, which can meet the needs. For the specific composition of the cake, it has little effect on the sintering step. Specifically, the composition of the cake can be Gd 2 O 3 and sulfur, and one or more rare earth elements such as Tb, Pr, and Eu are doped in trace amounts. At the same time, the sintering method in the embodiment of the present invention can reduce the sintering temperature and shorten the sintering time, thereby helping to inhibit grain growth and the discharge of gas between grains or particles, thereby facilitating the acquisition of ceramic products with fine grains and high density, while improving the mechanical properties of the ceramic material.
[0025] The sintering method of the present invention does not require the addition of sintering aids or molding aids, thus being beneficial to improving the purity of ceramic products.
[0026] The sintering method of the present invention can use equipment similar to an atmosphere sintering furnace, the equipment cost is relatively low, multiple ceramics can be sintered in the furnace at the same time, the production cost is low, and it is conducive to improving production efficiency.
[0027] In an optional embodiment, the relative pressure of the sintering step is 10-50 kPa. Within this range, the grains of the prepared gadolinium oxysulfide scintillating ceramics are finer and the density is higher.
[0028] And / or, the sintering temperature is 1000° C.-1500° C. Within this range, the grains of the prepared gadolinium oxysulfide scintillating ceramics are finer and the density is higher.
[0029] In an optional embodiment, the volume ratio of reducing gas to inert gas in the sintering atmosphere is 1-1.5:1, and the reducing gas is diluted with inert gas to ensure the quality of the prepared gadolinium oxysulfide scintillation ceramic while reducing the cost.
[0030] In an optional embodiment, the inert gas is selected from at least one of helium, neon and argon; and / or the reducing gas is selected from at least one of hydrogen, carbon monoxide and methane.
[0031] In an optional embodiment, the sintering time is 0.5-5 h. Shortening the sintering time is beneficial to inhibiting grain growth.
[0032] In an optional embodiment, the sintering is carried out in a sintering furnace:
[0033] Before the sintering step, the sintering furnace is heated to the sintering temperature at a temperature of 10-30°C / min;
[0034] And / or, after the sintering step, the sintering furnace is cooled to 15-50°C at a rate of 10-30°C / min.
[0035] In the implementation manner of the present invention, sintering can be performed in a sintering furnace, and the cake material can be directly placed in a crucible, wherein the crucible can be made of materials such as corundum, high-purity alumina, high-purity zirconia, etc., which can resist high temperatures while reducing the introduction of impurities.
[0036] In the scope of the present invention, increasing the heating rate before sintering or the cooling rate after sintering is beneficial to shortening the sintering time, thereby facilitating obtaining gadolinium oxysulfide scintillating ceramics with fine grains.
[0037] In an optional embodiment, before the sintering furnace is heated, the vacuum is first evacuated to a vacuum degree of less than 10 -3 Pa, and then the mixed gas is introduced into the sintering furnace to prevent the residual air in the sintering furnace from reacting with the reducing agent and even affecting the sintering of gadolinium oxysulfide.
[0038] In an optional embodiment, the flow rate of the mixed gas is 10ml / min-1500ml / min, preferably 10ml / min-100ml / min. The mixed gas is continuously passed into the sintering furnace, which is more conducive to obtaining ceramic products with fine grains and high density, while improving the mechanical properties of ceramic materials.
[0039] An embodiment of the present invention further provides a gadolinium oxysulfide scintillating ceramic, which is prepared by the sintering method of the gadolinium oxysulfide scintillating ceramic described in any one of the above embodiments;
[0040] Preferably, the average grain size of the gadolinium oxysulfide scintillating ceramic is 5-20 μm and the density is 7.2-7.4 g / cm3 .
[0041] An embodiment of the present invention also provides an application of the gadolinium oxysulfide scintillating ceramic described in the aforementioned embodiment, wherein the application includes use in X-ray detectors, security inspection machines, non-destructive testing, gadolinium oxysulfide fluorescent screens in DR detectors, and computed tomography imaging fields.
[0042] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0043] Embodiment 1:
[0044] This embodiment provides a sintering method for gadolinium oxysulfide scintillating ceramic, comprising:
[0045] The gadolinium oxysulfide raw material cake obtained after dry pressing is placed in a sintering furnace, wherein the composition of the cake is Gd 2 O 3 and sulfur, doped with trace amounts of Pr, with a dry pressing pressure of 240 MPa. After vacuuming, a mixed gas of hydrogen and argon is introduced into the sintering furnace, the flow rate of the mixed gas is 50 ml / min, the volume ratio of hydrogen and argon in the mixed gas is 1.25:1, the relative pressure in the sintering furnace is 30 kpa, the sintering temperature is 1100 ° C, and the temperature is kept constant for 2 hours. The heating and cooling rates before sintering are 20 ° C / min, and the heating and cooling rates after sintering are 20 ° C / min. After cooling, the gadolinium oxysulfide scintillating ceramics are taken out of the furnace.
[0046] Embodiment 2:
[0047] This embodiment provides a sintering method for gadolinium oxysulfide scintillating ceramic, comprising:
[0048] The gadolinium oxysulfide raw material cake obtained after dry pressing (the same as in Example 1) was placed in a sintering furnace, and a mixed gas of hydrogen and argon was introduced into the sintering furnace after vacuuming. The flow rate of the mixed gas was 10 ml / min, and the volume ratio of hydrogen and argon in the mixed gas was 1.5:1. The relative pressure in the sintering furnace was 1 kPa, the sintering temperature was 1500° C., the temperature was kept constant for 0.5 h, the heating and cooling rate before sintering was 30° C. / min, and the heating and cooling rate after sintering was 30° C. / min. After cooling, the gadolinium oxysulfide scintillation ceramic was taken out of the furnace to obtain.
[0049] Embodiment 3:
[0050] This embodiment provides a sintering method for gadolinium oxysulfide scintillating ceramic, comprising:
[0051] The gadolinium oxysulfide raw material cake obtained after dry pressing (same as in Example 1) was placed in a sintering furnace, and after evacuation, a mixed gas of hydrogen and argon was introduced into the sintering furnace, the flow rate of the mixed gas was 1500 ml / min, the volume ratio of hydrogen and argon in the mixed gas was 1:1, the relative pressure in the sintering furnace was 500 kPa, the sintering temperature was 800° C., the temperature was kept constant for 5 h, the heating and cooling rate before sintering was 10° C. / min, the heating and cooling rate after sintering was 10° C. / min, and the gadolinium oxysulfide scintillation ceramic was taken out of the furnace after cooling.
[0052] Embodiment 4:
[0053] This embodiment provides a sintering method for gadolinium oxysulfide scintillating ceramics, which is different from Embodiment 1 mainly in that the relative pressure of the sintering step is 10 kPa.
[0054] Embodiment 5:
[0055] This embodiment provides a sintering method for gadolinium oxysulfide scintillating ceramics, which is different from Embodiment 1 mainly in that the relative pressure of the sintering step is 50 kPa.
[0056] Embodiment 6:
[0057] This embodiment provides a sintering method for gadolinium oxysulfide scintillating ceramics, which is different from Embodiment 1 mainly in that the flow rate of the mixed gas is 100 ml / min.
[0058] Embodiment 7:
[0059] This embodiment provides a sintering method for gadolinium oxysulfide scintillating ceramics, which is different from Embodiment 1 mainly in that the flow rate of the mixed gas is 10 ml / min.
[0060] Embodiment 8:
[0061] This embodiment provides a sintering method for gadolinium oxysulfide scintillating ceramic, comprising:
[0062] The gadolinium oxysulfide raw material cake obtained after dry pressing (the same as in Example 1) was placed in a sintering furnace, and a mixed gas of hydrogen and argon was introduced into the sintering furnace after vacuuming. The flow rate of the mixed gas was 10 ml / min, and the volume ratio of hydrogen and argon in the mixed gas was 1:1. The relative pressure in the sintering furnace was 10 kPa, the sintering temperature was 1100° C., the temperature was kept constant for 0.5 h, the heating and cooling rate before sintering was 10° C. / min, and the heating and cooling rate after sintering was 10° C. / min. After cooling, the gadolinium oxysulfide scintillation ceramic was taken out of the furnace to obtain.
[0063] Embodiment 9:
[0064] This embodiment provides a sintering method for gadolinium oxysulfide scintillating ceramic, comprising:
[0065] The gadolinium oxysulfide raw material cake obtained after dry pressing (the same as in Example 1) was placed in a sintering furnace, and after evacuation, a mixed gas of carbon monoxide and argon was introduced into the sintering furnace, the flow rate of the mixed gas was 50 ml / min, the volume ratio of hydrogen and argon in the mixed gas was 1.5:1, the relative pressure in the sintering furnace was 20 kPa, the sintering temperature was 1000° C., the temperature was kept constant for 2 h, the heating and cooling rate before sintering was 30° C. / min, the heating and cooling rate after sintering was 30° C. / min, and the gadolinium oxysulfide scintillation ceramic was taken out of the furnace after cooling.
[0066] Embodiment 10:
[0067] This embodiment provides a sintering method for gadolinium oxysulfide scintillating ceramic, comprising:
[0068] The gadolinium oxysulfide raw material cake obtained after dry pressing (the same as in Example 1) was placed in a sintering furnace, and a mixed gas of carbon monoxide and argon was introduced into the sintering furnace after vacuuming. The flow rate of the mixed gas was 100 ml / min, and the volume ratio of hydrogen and argon in the mixed gas was 1.2:1. The relative pressure in the sintering furnace was 50 kPa, the sintering temperature was 1100° C., and the temperature was kept constant for 5 hours. The heating and cooling rate before sintering was 20° C. / min, and the heating and cooling rate after sintering was 20° C. / min. After cooling, the gadolinium oxysulfide scintillation ceramic was taken out of the furnace to obtain.
[0069] Embodiment 11:
[0070] This embodiment provides a sintering method for gadolinium oxysulfide scintillating ceramic, comprising:
[0071] The gadolinium oxysulfide raw material cake obtained after dry pressing (the same as in Example 1) was placed in a sintering furnace, and after evacuation, a mixed gas of carbon monoxide and argon was introduced into the sintering furnace, the flow rate of the mixed gas was 80 ml / min, the volume ratio of hydrogen and argon in the mixed gas was 1.2:1, the relative pressure in the sintering furnace was 30 kPa, the sintering temperature was 900° C., the constant temperature was maintained for 1 h, the heating and cooling rate before sintering was 15° C. / min, the heating and cooling rate after sintering was 15° C. / min, and the gadolinium oxysulfide scintillation ceramic was obtained after cooling.
[0072] Comparative Example 1
[0073] This comparative example provides a sintering method for gadolinium oxysulfide scintillating ceramics, which is different from Example 1 mainly in that the absolute pressure of the sintering step is 500 kPa.
[0074] Comparative Example 2
[0075] The present comparative example provides a sintering method for gadolinium oxysulfide scintillating ceramics, which is different from Example 1 mainly in that a mixed gas of hydrogen and argon is introduced into the sintering furnace after vacuuming, and the flow rate of the mixed gas is 1000 ml / min. After the residual gas in the sintering furnace is squeezed out, the air inlet and outlet of the sintering furnace are closed, and the volume ratio of hydrogen and argon in the mixed gas is 1.25:1.
[0076] Comparative Example 3
[0077] This comparative example provides a sintering method for gadolinium oxysulfide scintillating ceramic, which specifically includes:
[0078] The raw material powder of gadolinium oxysulfide to be sintered (with the same composition as the cake material in Example 1) is placed in a mold for molding, the molding pressure is 160 MPa, and the mold loaded with the powder is placed in a vacuum sintering furnace for sintering. The sintering temperature is 1100° C., the absolute sintering pressure is 30 kPa, the sintering time is 2 h, the heating and cooling rate before sintering is 20° C. / min, and the heating and cooling rate after sintering is 20° C. / min. After cooling, the gadolinium oxysulfide scintillation ceramic is taken out of the furnace to obtain.
[0079] The gadolinium oxysulfide scintillating ceramics obtained in the above examples and comparative examples were tested, and the results are shown in the following table.
[0080]
[0081]
[0082] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A sintering method for gadolinium oxysulfide scintillating ceramics, characterized in that: include: The gadolinium oxysulfide raw material cake obtained by dry pressing is sintered at a sintering temperature of 800° C.-1500° C., a sintering atmosphere of a mixed gas of a reducing gas and an inert gas, and a relative pressure of the sintering step of 1 kpa-500 kpa.
2. The sintering method of gadolinium oxysulfide scintillating ceramic according to claim 1, characterized in that: The relative pressure of the sintering step is 10-50 kPa; And / or, the sintering temperature is 1000°C-1500°C.
3. The sintering method of gadolinium oxysulfide scintillating ceramic according to claim 1, characterized in that: The volume ratio of reducing gas to inert gas in the sintering atmosphere is 1-1.5:
1.
4. The sintering method of gadolinium oxysulfide scintillating ceramic according to claim 1, characterized in that: The inert gas is selected from at least one of helium, neon and argon; and / or the reducing gas is selected from at least one of hydrogen, carbon monoxide and methane.
5. The sintering method of gadolinium oxysulfide scintillating ceramic according to claim 1, characterized in that: The sintering time is 0.5-5h.
6. The sintering method of gadolinium oxysulfide scintillating ceramic according to claim 1, characterized in that: The sintering is carried out in a sintering furnace: Before the sintering step, the sintering furnace is heated to the sintering temperature at a temperature of 10-30°C / min; And / or, after the sintering step, the sintering furnace is cooled to 15-50°C at a rate of 10-30°C / min.
7. The sintering method of gadolinium oxysulfide scintillating ceramic according to claim 6, characterized in that: Before the sintering furnace is heated up, the vacuum is first evacuated to a vacuum degree of less than 10 -3 Pa, and then the mixed gas is introduced into the sintering furnace.
8. The sintering method of gadolinium oxysulfide scintillating ceramic according to claim 7, characterized in that: The flow rate of the mixed gas is 10ml / min-1500ml / min, preferably 10ml / min-100ml / min.
9. A gadolinium oxysulfide scintillating ceramic, characterized in that: Prepared by the sintering method of the gadolinium oxysulfide scintillating ceramic according to any one of claims 1 to 7; Preferably, the average grain size of the gadolinium oxysulfide scintillating ceramic is 5-20 μm and the density is 7.2-7.4 g / cm 3 .
10. An application of the gadolinium oxysulfide scintillating ceramic according to claim 9, characterized in that: The applications include use in X-ray detectors, security inspection machines, non-destructive testing, gadolinium oxysulfide fluorescent screens in DR detectors, and computed tomography imaging.
Citation Information
Patent Citations
Method for preparing sulfuric oxide ceramic scintillating medium
CN107686349A