Lithium ion secondary battery and method for using lithium ion secondary battery after deterioration

The lithium-ion secondary battery design with a nickel-rich positive electrode and optimized usage ratios addresses the limited lifespan issue, achieving extended battery life and capacity recovery, aligning with the economic and resource efficiency needs of the electric vehicle market and shared mobility trends.

WO2024203702A1PCT designated stage expired Publication Date: 2024-10-03KRI INC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010964
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-21
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Lithium-ion secondary batteries used in electric vehicles have a limited lifespan, requiring frequent replacements and leading to economic and resource inefficiencies, which is unsustainable for the growing demand in the electric vehicle market, especially with the shift towards shared mobility and renewable energy integration.

Method used

A lithium-ion secondary battery design featuring a specific positive electrode active material with a lithium-containing metal oxide containing 70-100 atom% nickel, where the positive electrode usage is set between 50-70% of the total capacity, and the negative electrode usage is 80-95% of the maximum charge amount, allowing for extended lifespan and capacity recovery through reserved lithium.

Benefits of technology

This design significantly extends the battery lifespan, enabling the battery to maintain capacity and reduce the need for frequent replacements, aligning with the economic and resource efficiency requirements of the evolving electric vehicle market and shared mobility trends.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010964_03102024_PF_FP_ABST
    Figure JP2024010964_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a lithium ion secondary battery which uses, as a positive electrode active material, a lithium-containing metal oxide which contains nickel in an amount of 70 atomic % to 100 atomic %, with the total amount of metals other than lithium at 100 atomic %, wherein if charging is performed so that the positive electrode usage, as the volume of lithium extracted from the positive electrode active material in an initial cycle, is 50% to 70%, with the total volume of lithium contained in the positive electrode at 100%, then the negative electrode usage as the capacity that is charged in the initial cycle is adjusted to be 80% to 95%, with the negative electrode capacity as the maximum charge amount that can be inserted into the negative electrode at 100%. Consequently, the lithium ion secondary battery has an extremely long service life in comparison to conventional lithium ion secondary batteries. In addition, even if the capacity of the battery has deteriorated, the battery capacity can be recovered.
Need to check novelty before this filing date? Find Prior Art

Description

Lithium-ion secondary battery and method for using a deteriorated lithium-ion secondary battery

[0001] The present invention relates to a lithium ion secondary battery and a method for using a lithium ion secondary battery after deterioration.

[0002] The lithium-ion secondary battery (LIB) business has achieved dramatic growth thanks to relentless technological development aimed at miniaturizing and lightening mobile devices and enhancing their functionality (pursuing convenience) by leveraging their high energy density, high voltage, and safety features. With global environmental and resource issues now in the spotlight, policies such as promoting eco-cars and shifting to renewable energy are expected to continue to drive the growth of the LIB market. If this trend continues, lithium-ion secondary batteries will be needed for personal electric vehicles (EVs) and stationary energy storage (e.g., for renewable energy leveling), and the number of batteries needed will be estimated to be approximately 10 times that of 2018 by 2030. This could lead to economically unfavorable conditions for users, such as a sharp rise in battery costs due to resource shortages. Therefore, research and development into reuse and recycling, both from the perspective of extending the life of a single battery, is gaining momentum. Furthermore, extending battery life is also effective from the perspective of life cycle assessment (LCA).

[0003] Furthermore, new proposals have been made regarding the future of mobility, such as EVs. CASE, MaaS, and other technologies aimed at improving user convenience are becoming a reality, and there are signs that mobility, such as EVs, will shift from individual ownership to sharing (management of batteries, vehicles, etc. by management companies, etc.). Amid this trend, AIEVs (Artificial Intelligence Electric Vehicles), which are expected to be deployed in the market in the future, are EVs equipped with AI, with automated driving and vehicle sharing (CASE). The vehicles are not privately owned but are managed by management companies, which provide transportation services and various services required by users within the vehicle (MaaS). Furthermore, since management companies will be able to manage vehicle operation and charge / discharge control, it will also be possible to consider battery life (from an economic and resource perspective) and safety, rather than driving distance per charge (emphasis on energy density), in operation. Furthermore, vehicle sharing is also economically advantageous, as it can reduce the user's burden to about one-fifth of that of personal ownership. In other words, in the future, replacing private cars, which are mainly gasoline-powered, with AIEVs (sharing cars) is expected to contribute to the global environment, reduce traffic accidents and congestion, provide a new means of transportation in aging and depopulated areas, reduce personal expenses, and make effective use of travel time. Furthermore, AIEVs can also function as huge energy storage systems, automatically charging electricity generated from highly fluctuating renewable energy sources through a management company's management system and discharging it as needed.

[0004] However, to achieve this, it will be necessary to reconsider the development direction of lithium-ion batteries, which are currently the mainstream (Figure 1).

[0005] In particular, dramatically extending the lifespan of batteries installed in electric vehicles is essential. Unlike privately owned vehicles, AIEVs require a total vehicle mileage of, for example, 500,000 km or more. If battery life remains at the current level, multiple battery replacements will be necessary, undermining the economic benefits that AIEVs would offer and preventing resource problems from being resolved. The required battery performance emphasizes battery life over the currently mainstream requirements of energy density (mileage) and rapid charging. Specifically, the energy density must be at least 400 Wh / L for a single cell, and the vehicle mileage is 200-300 km with a 20-30 kWh battery. However, the target practical operational lifespan must be at least five times longer than the current level (ultra-long battery life).

[0006] Various approaches to extending battery life have been explored to date, but if the goal is to extend the practical operating life by more than five times (ultra-long life), a new approach will be required. The current main development direction for lithium-ion secondary batteries is to use high-capacity active materials to obtain high energy density, and to set the battery voltage as high as possible while suppressing battery degradation due to oxidative decomposition of the electrolyte, etc., and lithium-ion secondary batteries with a rated voltage of, for example, approximately 4.2 V are being deployed on the market. However, new developments that place emphasis on the aforementioned lifespan (such as solving resource and environmental issues, and developing ultra-long-life batteries for AIEVs and sharing applications) will require a different approach to battery design.

[0007] It has been known for some time that lowering the charging voltage of a battery is an effective way to prevent battery degradation due to oxidative decomposition of the electrolyte on the positive electrode side and extend the battery's lifespan. In this case, the actual energy obtained is significantly lower than the battery's designed energy density. For example, to obtain the above-mentioned 400 Wh / L of energy by lowering the charging voltage, a battery with a higher energy density, such as 450 to 500 Wh / L, must be used. In this case, using a battery with an energy density higher than the required energy density raises issues in terms of safety, cost, and the like.

[0008] The present invention is intended to solve the above-mentioned problems, and aims to provide a lithium ion secondary battery that has an ultra-long life compared to conventional lithium ion secondary batteries, and to provide a lithium ion secondary battery that is capable of restoring its battery capacity even if the capacity of the battery deteriorates.

[0009] In view of the above-mentioned problems, the present inventors have conducted extensive research. As a result, they have found that by using a specific positive electrode active material and appropriately setting the amount of positive electrode utilization, it is possible to manufacture a lithium ion secondary battery with a significantly improved lifespan compared to conventional lithium ion secondary batteries. Furthermore, they have found that such lithium ion secondary batteries have usable lithium as a reserve, and that when the battery deteriorates, the battery capacity can be restored by using the reserved lithium in the positive electrode, thereby further extending the battery life.

[0010] That is, the present invention includes the following configurations.

[0011] Item 1. A lithium ion secondary battery comprising at least a positive electrode and a negative electrode, wherein the positive electrode contains a positive electrode active material, and the positive electrode active material contains a lithium-containing metal oxide containing nickel, and the lithium-containing metal oxide contains 70 to 100 atomic % of nickel, with a total amount of metals other than lithium being 100 atomic %, and when charging is performed such that the total capacity of lithium contained in the positive electrode is 100% and the capacity of lithium extracted from the positive electrode active material in an initial cycle is 50 to 70%, the negative electrode utilization amount is 100% and the negative electrode capacity as the maximum charge amount at which lithium can be inserted into the negative electrode is 80 to 95%.

[0012] Item 2. The lithium ion secondary battery according to Item 1, which is a reserve-type lithium ion secondary battery that holds available lithium as a reserve.

[0013] Item 3. The lithium ion secondary battery according to Item 1 or 2, which is used in an electric vehicle for car sharing.

[0014] Item 3-1. Use of the lithium ion secondary battery according to Item 1 or 2 in an electric vehicle for car sharing.

[0015] Item 4. A method for improving the life of a lithium ion secondary battery, comprising: a lithium ion secondary battery having at least a positive electrode and a negative electrode; wherein the positive electrode contains a positive electrode active material; and the positive electrode active material contains a lithium-containing metal oxide containing nickel; and the lithium-containing metal oxide contains 70 to 100 atomic % of nickel, assuming a total amount of metals other than lithium as 100 atomic %, and adjusting the positive electrode utilization amount so that, when the total capacity of lithium contained in the positive electrode is 100%, the capacity of lithium extracted from the positive electrode active material during charging is 50 to 70%, and the negative electrode utilization amount is, when the negative electrode capacity as the maximum charge amount at which lithium can be inserted into the negative electrode is 100%, the charged capacity during charging is 80 to 95%.

[0016] Item 5. The method according to Item 4, wherein the lithium ion secondary battery is a reserve-type lithium ion secondary battery that holds available lithium as a reserve.

[0017] Item 6. The method according to Item 4 or 5, wherein the lithium ion secondary battery is used in an electric vehicle for car sharing.

[0018] Item 7. A method for using the lithium ion secondary battery according to any one of Items 1 to 3 after the lithium ion secondary battery has deteriorated, comprising using available lithium reserved in the lithium ion secondary battery.

[0019] Item 8. The method according to Item 7, wherein the charging voltage is increased until available lithium reserved in the lithium ion secondary battery is supplied.

[0020] According to the present invention, by using a specific positive electrode active material and appropriately setting the positive electrode utilization amount and the negative electrode utilization amount, it is possible to significantly improve the lifespan of a conventional lithium ion secondary battery. Furthermore, according to the present invention, even when such a lithium ion secondary battery deteriorates, the lifespan of the lithium ion secondary battery can be extended by using the Li reserved in the positive electrode.

[0021] This is a schematic diagram showing the direction of lithium-ion battery development, taking into account a worldview in which the use and operation of automobiles will undergo major changes. This shows an outline of the analysis method used in measuring AC impedance. This shows the results of cycle tests using batteries 1 to 4 of Examples 1 and 2 and Comparative Examples 1 and 2. This shows the results of calculations using a power law to determine the relationship between the total charge and discharge capacity and the cycle for batteries 1 to 4 of Examples 1 and 2 and Comparative Examples 1 and 2.

[0022] In this specification, the term "containing" is a concept that encompasses all of "comprise," "consist essentially of," and "consist only of."

[0023] In addition, in this specification, the expression "A to B" means "A or more and B or less."

[0024] 1. Lithium-ion secondary battery and method for improving the life of a lithium-ion secondary battery The lithium-ion secondary battery of the present invention is a lithium-ion secondary battery comprising at least a positive electrode and a negative electrode, wherein the positive electrode contains a positive electrode active material, and the positive electrode active material contains a lithium-containing metal oxide containing nickel, and the lithium-containing metal oxide contains 70 to 100 atomic % of nickel, where the total amount of metals other than lithium is 100 atomic %, and the positive electrode utilization amount is 100% of the total capacity of lithium contained in the positive electrode, and when charging is performed such that the capacity of lithium extracted from the positive electrode active material in the first cycle is 50 to 70%, and the negative electrode utilization amount is 80 to 95% of the capacity charged in the first cycle, where the negative electrode capacity as the maximum charge amount at which lithium can be inserted into the negative electrode is 100%.

[0025] The lithium ion secondary battery of the present invention uses a specific positive electrode active material, and its characteristic is that the amount of positive electrode usage and the amount of negative electrode usage are appropriately set, thereby making it possible to extend the lifespan.

[0026] The positive electrode utilization amount in the lithium ion secondary battery of the present invention is, for example, 100% of the total capacity of lithium contained in the positive electrode (positive electrode theoretical capacity), and the battery is charged so that the capacity of Li extracted from the positive electrode active material in the first cycle (the first charge that can obtain the rated capacity) is 50% or more and 70% or less, preferably 60% or more and 70% or less, and more preferably 60% or more and 65% or less. As will be described later, the negative electrode utilization amount is 100% of the negative electrode capacity as the maximum charge amount at which lithium can be inserted into the negative electrode, and the capacity charged in the first cycle is 80 to 95%. Therefore, the lithium ion secondary battery of the present invention will satisfy the above-mentioned positive electrode utilization amount when charged to satisfy this negative electrode utilization amount. For example, LiNi, which is a Li-containing metal oxide, 0.8 Co 0.15 Al 0.05 O 2 is a specific positive electrode active material used in the present invention, in which Ni accounts for 80 atomic % of the total amount of metals other than Li contained in the Li-containing metal oxide, with 100 atomic % being the total amount of metals other than Li. When all of the Li in this active material is removed, the capacity is 279 mAh / g. When 70% of this is removed, the initial charge capacity can be determined as 195 mAh / g, for example. When using a Li-containing metal oxide in which Ni exceeds 80% of the metals other than Li in atomic ratio, conventional lithium-ion secondary batteries are usually designed with a positive electrode capacity of 75% or more, and in this case, sufficient cycle characteristics cannot be obtained. In other words, when the positive electrode capacity exceeds the above upper limit, sufficient cycle characteristics cannot be obtained, the lifespan is not improved, and the capacity cannot be restored after battery degradation. When the positive electrode capacity is less than the above lower limit, the lifespan is improved but sufficient cycle characteristics cannot be obtained.

[0027] The negative electrode utilization capacity of the lithium-ion secondary battery of the present invention is, for example, 80% to 95% of the negative electrode capacity, preferably 80% to 90%, as the capacity charged in the first cycle. As described above, the positive electrode utilization capacity is 50% to 70% as the capacity of lithium extracted from the positive electrode active material in the first cycle, assuming the total capacity of lithium contained in the positive electrode to be 100%. Therefore, the lithium-ion secondary battery of the present invention satisfies the negative electrode utilization capacity when charged to satisfy this positive electrode utilization capacity. Here, the negative electrode capacity refers to the maximum charge capacity at which Li can be inserted into the negative electrode. This is measured by creating a half-cell using lithium metal as the counter electrode and slowly inserting Li at 0.01 C. The charge capacity may also include Li consumption during SEI formation, etc. If the utilization capacity exceeds the upper limit, there is a risk of Li metal precipitation due to overvoltage factors such as battery degradation. If the utilization capacity is below the lower limit, the negative electrode cannot be fully utilized, resulting in a decrease in energy density. When using a Li-containing metal oxide in which Ni is more than 80% in atomic ratio among metals other than Li, the positive electrode utilization is usually designed to be 75% or more, and the negative electrode is often designed to be 80% or more but not more than 95% for the above-mentioned reasons. In this case, if the charging voltage is reduced, the negative electrode utilization will be less than 80%, and the energy density will decrease.

[0028] (1-1) Positive Electrode The positive electrode can generally include a positive electrode layer containing a positive electrode active material on a positive electrode current collector.

[0029] Positive Electrode Active Material The positive electrode active material is, in particular, a lithium (Li)-containing metal oxide containing nickel (Ni), and a compound containing Ni in an atomic ratio of 70% to 100%, preferably 75% to 95%, and more preferably 75% to 85%, where the total amount of metals other than Li contained in the Li-containing metal oxide is 100 atomic %. If the Ni content is below the lower limit, the energy density will be too low from a practical standpoint, and if it exceeds the upper limit, the stability of the material will be reduced, making it difficult to achieve effects such as good life and safety. Specifically, for example, α-NaFeO 2 As a lithium metal composite oxide having a crystalline structure, Li [Li x1 Ni γ1 Mnβ1 Co(1-x1-γ1-β1)]O 2 (0≦x1<0.5, 0.7≦γ1≦1, 0≦β1≦0.3, 0≦γ1+β1≦0.3), Li[Li x2 Ni γ2 Co β2 Al(1-x2-γ2-β2)]O 2 (0≦x2<0.5, 0.7≦γ2≦1, 0≦β2≦0.3, 0≦γ2+β2≦0.3), etc. Here, examples of metals other than Ni contained in the Li-containing metal oxide include Mn, Co, Al, etc., but other transition metals and alkaline earth metals such as Mg may also be contained. Furthermore, elements that can replace a portion of O, such as alkali metals other than Li, S, F, etc., may also be contained. It is also possible to appropriately adjust the amount of positive electrode utilization depending on the type of positive electrode active material, etc.

[0030] The particle form of the positive electrode active material is not particularly limited, and various forms such as secondary particles and single particles can be used. The shape is also not particularly limited, and various forms such as spherical, scale-like, block-like, fibrous, whisker-like, and crushed can be used. Positive electrode active materials of multiple shapes can also be used in combination. Note that the spherical form may be a perfect sphere or an elliptical form.

[0031] The particle size of the positive electrode active material is not particularly limited, but from the viewpoint of facilitating current collection between particles and further extending the life of the battery, the average particle size is preferably 0.1 to 25 μm, more preferably 1 to 20 μm, and even more preferably 5 to 15 μm. The average particle size of the electrode active material (positive electrode active material) is measured by a laser diffraction / scattering method.

[0032] Other Constituent Materials and Composition The composition of the positive electrode of the lithium ion secondary battery of the present invention and the method for producing the same are not particularly limited, and the positive electrode is formed using the above-mentioned positive electrode active material as the main component, and optionally using a conductive material, a binder, etc., to form a positive electrode.

[0033] When a binder is used, the type of binder is not particularly limited, and examples include fluorine-based resins such as polyvinylidene fluoride and polyethylene tetrafluoride; fluorine rubber, SBR, acrylic resin, polyethylene, polypropylene, and other polyolefins. The amount of binder is not particularly limited and is determined appropriately depending on the average particle size, shape, and the like of the positive electrode active material; for example, it is preferable that the amount of binder be about 0.1 to 30 parts by mass per 100 parts by mass of the positive electrode active material.

[0034] Furthermore, when a conductive material is used, the type and amount of the conductive material are not particularly limited, but are appropriately determined depending on the average particle size, shape, electrical conductivity, etc. of the positive electrode active material, and examples of the material include carbon black, acetylene black, graphite, carbon fiber, carbon nanotubes, etc. The amount of the conductive material is not particularly limited, and is preferably, for example, about 0.01 to 20 parts by mass per 100 parts by mass of the positive electrode active material.

[0035] The positive electrode used in the lithium ion secondary battery of the present invention can be produced by using a positive electrode active material, and, if necessary, materials necessary for molding such as a conductive material and a binder, using a known general electrode molding method such as coating molding, press molding, or roll molding.

[0036] In the lithium-ion secondary battery of the present invention, when a very small amount of carbon nanotubes is contained in the positive electrode, current collection between positive electrode active material particles and maintenance of the shape of the positive electrode can be achieved. As a result, by not including any positive electrode constituent materials other than the conductive material, the amount of positive electrode constituent materials other than the positive electrode active material can also be reduced. As a result, the positive electrode is likely to have sufficient strength to maintain its shape and is less likely to inhibit the movement of lithium ions, which makes the reaction within the battery uniform and increases the battery life. Examples of conductive materials other than carbon nanotubes include one or more of carbon blacks such as acetylene black, furnace black, and ketjen black; flake graphite; graphene; and amorphous carbon obtained by heat-treating organic materials.

[0037] In this case, the total amount of the positive electrode active material, the carbon nanotubes, and the conductive material other than the carbon nanotubes (total amount of the composition) is taken as 100% by mass, and the content of the positive electrode active material can be 88.6 to 99.9% by mass, preferably 90.8 to 98.4% by mass, and more preferably 93.0 to 97.8% by mass; the content of the carbon nanotubes can be 0.01 to 1.4% by mass, preferably 0.1 to 1.2% by mass, and more preferably 0.2 to 1.0% by mass; and the content of the conductive material other than the carbon nanotubes can be 0 to 10.0% by mass, preferably 1.0 to 8.0% by mass, and more preferably 2.0 to 6.0% by mass. Also, for the same reason, the total amount of the positive electrode active material, the carbon nanotubes, and the conductive material other than the carbon nanotubes (total volume of the composition) is 100% by volume. The volume ratio of the positive electrode active material is 75.06 to 99.97% by volume, preferably 79.20 to 94.99% by volume, and more preferably 83.63 to 93.93% by volume. The volume ratio of the carbon nanotubes is 0.03 to 4.55% by volume, preferably 0.30 to 3.73% by volume, and more preferably 0.60 to 3.12% by volume. The volume ratio of the conductive material other than the carbon nanotubes is 0 to 21.56% by volume, preferably 2.41 to 17.52% by volume, and more preferably 4.82 to 13.49% by volume.

[0038] The positive electrode is usually formed by forming a positive electrode layer containing the positive electrode constituent material on a positive electrode current collector or by bonding (including crimping) the positive electrode layer onto the positive electrode current collector. Depending on the shape of the battery, such as a coin-type battery, the outer case may also function as a current collector. In such cases, the positive electrode layer is formed on the outer case or by bonding (including crimping) the outer case.

[0039] The positive electrode current collector is preferably made of a material that is electrochemically stable at the potential used and has high electronic conductivity, such as aluminum, stainless steel, or a carbon material. This positive electrode current collector can be, for example, a foil-shaped or mesh-shaped member.

[0040] The thickness of the positive electrode for a lithium ion secondary battery of the present invention is not particularly limited, but is preferably 1 to 300 μm, more preferably 10 to 150 μm, and even more preferably 50 to 100 μm. The porosity of the positive electrode for a lithium ion secondary battery of the present invention is preferably 20 to 50%, more preferably 25 to 40%, from the viewpoints of easily improving the ionic conductivity of the electrolyte that enters the voids, improving the lifespan, and also easily improving the energy density.

[0041] (1-2) Negative Electrode The negative electrode can usually include a negative electrode layer containing a negative electrode active material on a negative electrode current collector.

[0042] Negative electrode active material The negative electrode active material is not particularly limited, and any material that can be used as a negative electrode active material in a lithium ion secondary battery, that is, a material that can absorb and release lithium ions, can be used. Examples of the negative electrode active material include carbon materials such as natural graphite, artificial graphite, amorphous carbon, and amorphous carbon materials, or composite carbon-based materials in which a different type of carbon-based material is composited on the surface of these carbon-based materials; metal materials that can be alloyed with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Si alloys, Sn alloys, and Al alloys; and SiO. x (0<x<2), SnO x (0<x<2), titanium oxide (TiO 2 etc.), lithium-containing titanium oxide (Li 2 TiO 3 etc.), hydrogen-containing titanium oxide (H 2 TiO 3Examples of such negative electrode active materials include metal oxides capable of absorbing and releasing lithium ions, such as vanadium oxide, and composite materials containing a metal material and a carbon material, such as Si-C composites and Sn-C composites. These negative electrode active materials can be used alone or in combination of two or more. From the perspective of particularly suppressing the volume change of the electrode active material (negative electrode active material) during charge and discharge and particularly improving the charge and discharge cycle characteristics, metal oxides capable of absorbing and releasing lithium ions, such as carbon materials, titanium oxides, lithium-containing titanium oxides, and hydrogen-containing titanium oxides, can also be used. Preferred negative electrode active materials include carbon materials such as natural graphite, artificial graphite, amorphous carbon, and amorphous carbon materials, as well as composite carbon-based materials in which a different carbon-based material is composited on the surface of such carbon-based materials, titanium oxides, lithium-containing titanium oxides, and hydrogen-containing titanium oxides. The volume change of the negative electrode active material during charge and discharge is preferably 50% or less, and preferably 20% or less. The smaller the volume change, the better. While there is no set lower limit, if a lower limit were to be set, it would be 0%. The volume change value indicates the degree to which the negative electrode active material at the time of full charge has expanded compared to the negative electrode active material at the time of full discharge, with the case where there is no volume change being taken as 0%. The volume change value is calculated using the following formula: ((volume at the time of full charge) - (volume at the time of full discharge)) / (volume at the time of full discharge) x 100.

[0043] The shape of the negative electrode active material is not particularly limited, and various shapes such as spheres, scales, chunks, fibers, whiskers, and crushed shapes can be used. A combination of negative electrode active materials of different shapes can also be used. The spherical shape may be a perfect sphere or an elliptical shape.

[0044] The particle size of the negative electrode active material is not particularly limited, but from the viewpoint of easily extending the life of the battery, the average particle size is preferably 0.1 to 25 μm, more preferably 1 to 20 μm. Furthermore, in consideration of uniformity of the reaction at low temperatures, the average particle size of the negative electrode active material can be set to 0.1 to 13.0 μm, preferably 0.5 to 10.0 μm, more preferably 1.0 to 8.0 μm. The average particle size of the negative electrode active material is measured by a laser diffraction / scattering method.

[0045] Other Constituent Materials and Composition The composition of the negative electrode of the lithium ion secondary battery of the present invention and the method for producing the same are not particularly limited, and the negative electrode is formed using the above-mentioned negative electrode active material as the main component, and optionally using a conductive material, a binder, etc., to form the negative electrode.

[0046] When a binder is used, the type of binder is not particularly limited, and examples include fluorine-based resins such as polyvinylidene fluoride and polyethylene tetrafluoride; fluorine rubber, SBR, acrylic resin, polyethylene, polypropylene, and other polyolefins. The amount of binder is not particularly limited and is determined appropriately depending on the average particle size, shape, and the like of the negative electrode active material; for example, it is preferable that the amount of binder be about 0.1 to 30 parts by mass per 100 parts by mass of the negative electrode active material.

[0047] Furthermore, when a conductive material is used, the type and amount of the conductive material are not particularly limited, but are appropriately determined depending on the average particle size, shape, electrical conductivity, etc. of the negative electrode active material, and examples of the material include carbon black, acetylene black, graphite, carbon fiber, carbon nanotubes, etc. The amount of the conductive material is not particularly limited, and is preferably, for example, about 0.01 to 20 parts by mass per 100 parts by mass of the negative electrode active material.

[0048] The negative electrode used in the lithium ion secondary battery of the present invention can be produced by using a negative electrode active material and, as necessary, materials required for molding, such as a conductive material and a binder, using a known general electrode molding method such as coating molding, press molding, or roll molding.

[0049] In the lithium ion secondary battery of the present invention, when a very small amount of carbon nanotubes is included in the negative electrode, current collection between negative electrode active material particles and maintenance of the shape of the negative electrode can be achieved, and as a result, the amount of negative electrode constituent materials other than the negative electrode active material can also be reduced.As a result, the negative electrode is likely to have enough strength to maintain its shape and is less likely to inhibit the movement of lithium ions, which makes the reaction within the battery uniform and increases the battery's lifespan.

[0050] Examples of negative electrode constituent materials other than the negative electrode active material and carbon nanotubes include conductive materials such as acetylene black, ketjen black, carbon black, graphene, and amorphous carbon obtained by heat-treating organic materials. Examples of binders, thickeners, or dispersants include fluorine-based polymers (polyvinylidene fluoride resin, polytetrafluoroethylene resin, vinylidene fluoride-hexafluoropropylene copolymer, etc.), polyolefin resins (styrene butadiene copolymer resin, ethylene vinyl alcohol copolymer resin, etc.), synthetic rubbers (styrene butadiene rubber, acrylonitrile butadiene rubber, ethylene propylene diene rubber, etc.), polyacrylonitrile, polyamide, polyimide, polyacrylic acid, polyacrylic acid esters, polyvinyl ethers, carboxymethyl cellulose, carboxymethyl cellulose sodium salt, carboxymethyl cellulose ammonium, polyurethane, hydroxypropyl cellulose, hydroxyethyl cellulose, methyl cellulose, etc. In addition, amorphous carbon materials can also be used as amorphous carbon. These negative electrode active materials and electrode constituent materials (negative electrode constituent materials) other than carbon nanotubes can be used alone or in combination of two or more.

[0051] In this case, the total amount of the negative electrode active material, the carbon nanotubes, and the negative electrode constituent materials other than the negative electrode active material and the carbon nanotubes is 100% by mass. The content of the negative electrode active material can be 97.4 to 99.9% by mass, preferably 97.7 to 99.7% by mass, and more preferably 98.0 to 99.5% by mass. The content of the carbon nanotubes can be 0.01 to 1.4% by mass, preferably 0.1 to 1.2% by mass, and more preferably 0.2 to 1.0% by mass. The content of the negative electrode constituent materials other than the negative electrode active material and the carbon nanotubes can be 0 to 1.2% by mass, preferably 0.2 to 1.1% by mass, and more preferably 0.4 to 1.0% by mass. Also, for the same reason, the total amount of the negative electrode active material, the carbon nanotubes, and the negative electrode constituent materials other than the negative electrode active material and the carbon nanotubes is 100% by volume. The volume ratio of the negative electrode active material is 96.19 to 99.98% by volume, preferably 97.00 to 99.70% by volume, more preferably 97.50 to 99.50% by volume. The volume ratio of the carbon nanotubes is 0.02 to 2.18% by volume, preferably 0.20 to 2.00% by volume, more preferably 0.40 to 1.75% by volume. The volume ratio of the negative electrode constituent materials other than the negative electrode active material and the carbon nanotubes is 0 to 1.63% by volume, preferably 0.20 to 1.50% by volume, more preferably 0.40 to 1.40% by volume.

[0052] The negative electrode is usually formed by forming or adhering (including crimping) a negative electrode layer containing the negative electrode constituent material on a negative electrode current collector. Depending on the shape of the battery, such as a coin-type battery, the outer case may also have a current collecting function, and in such cases, the negative electrode layer is formed or adhering (including crimping) to the outer case.

[0053] The negative electrode current collector is preferably made of a material that is electrochemically stable at the potential used and has high electronic conductivity, such as copper, stainless steel, nickel, or a carbon material. This negative electrode current collector can be, for example, a foil-shaped or mesh-shaped member.

[0054] The thickness of the negative electrode for a lithium ion secondary battery of the present invention is not particularly limited, but is preferably 1 to 300 μm, more preferably 10 to 150 μm, and even more preferably 50 to 100 μm. The amount of positive electrode used can be appropriately adjusted by adjusting the thickness of the negative electrode for a lithium ion secondary battery of the present invention. The porosity of the negative electrode for a lithium ion secondary battery of the present invention is preferably 20 to 50%, more preferably 25 to 40%, from the viewpoints of easily improving the ionic conductivity of the electrolyte solution that enters the voids, improving the lifespan, and also improving the energy density.

[0055] (1-3) Electrolyte The positive electrode, negative electrode, and optionally the voids in the separator of the lithium ion secondary battery of the present invention may be filled with, impregnated with, or the like.

[0056] The electrolyte solution is not particularly limited, and known electrolytes can be used. Examples of suitable electrolytes include those prepared by dissolving a Li salt in an aprotic organic solvent and adding additives having predetermined functions. Examples of suitable aprotic organic solvents include esters such as ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, γ-butyrolactone, methyl formate, and methyl acetate; furans such as tetrahydrofuran and 2-methyltetrahydrofuran; ethers such as dioxolane, diethyl ether, dimethoxyethane, diethoxyethane, and methoxyethoxyethane; dimethyl sulfoxide; sulfolanes such as sulfolane and methylsulfolane; and acetonitrile. These aprotic organic solvents may be used alone or in combination of two or more.

[0057] On the other hand, examples of salts that can be dissolved in such aprotic organic solvents include lithium salts such as lithium perchlorate, lithium fluoroborate, lithium hexafluorophosphate, lithium hexafluoroarsenate, lithium trifluoromethanesulfonate, lithium halides, lithium chloroaluminate, and lithium bis(fluorosulfonyl)imide. These salts may be used alone or in combination of two or more.

[0058] (1-4) Lithium-ion secondary battery The lithium-ion secondary battery of the present invention uses a specific positive electrode active material, and the positive electrode utilization amount and negative electrode utilization amount are appropriately set. The positive electrode and negative electrode are manufactured to satisfy this utilization amount setting. However, the shape, structure, etc. of the battery are not particularly limited, and the battery can usually have a structure in which the above-mentioned positive electrode and negative electrode face each other with a separator interposed therebetween. The shape of the lithium-ion secondary battery of the present invention is not particularly limited, and can be appropriately determined depending on the purpose, such as a coin type, a cylindrical type, a square type, a film type, etc.

[0059] Furthermore, in the present invention, the positive electrode active material is limited and its design utilization amount is restricted, which makes it possible to reduce the amount of additives added to suppress degradation in a highly oxidized state of the positive electrode compared to conventional lithium-ion secondary batteries. This allows for an improvement in battery life if an additive necessary for suppressing degradation in a highly oxidized state of the positive electrode, but which would otherwise cause reactions on the negative electrode, affecting battery life. Furthermore, if an additive necessary for suppressing degradation in a reduced state of the negative electrode, but which would otherwise cause reactions on the positive electrode exceeding the upper limit of the design utilization amount in the present invention (as in conventional designs), would result in an improvement in battery life if the additive is kept within the design utilization amount in the present invention.

[0060] 2. Method of Using a Degraded Lithium-Ion Secondary Battery In the lithium-ion secondary battery of the present invention, the positive electrode utilization is designed during battery manufacture such that, for example, the total capacity of lithium contained in the positive electrode (positive electrode theoretical capacity) is 100%, and the capacity of Li extracted from the positive electrode active material is 50% or more and 70% or less, thereby maintaining usable Li as a reserve. Furthermore, in the present invention, during battery manufacture and initial charge / discharge, for example, the total capacity of lithium contained in the positive electrode (positive electrode theoretical capacity) is 100%, and the amount of Li extracted from the positive electrode active material is 70% or less, preferably 65% ​​or less. This results in very little gas generation during cycling and aging, and the electrode reaction proceeds uniformly. Therefore, in many cases, deterioration occurs under ideal conditions. Supplying Li to restore capacity can extend the battery's life. Furthermore, by extracting more Li from the positive electrode active material after a protective coating, such as an active material field, has fully grown due to cycling and aging, deterioration during cycling can be minimized. For example, if the end of life is defined as the time when the battery has deteriorated to 80% of its rated capacity, the capacity of the battery that has reached the end of its life can be restored by using available reserved Li after the end of life, thereby extending the cycle life. To restore capacity, the amount of Li shared from the positive electrode reserve must be limited to an amount that the negative electrode can accept (an amount that does not cause unexpected reactions such as Li metal precipitation). It is desirable to share an amount of Li that does not exceed the deteriorated capacity from the initial capacity. Sharing Li from the positive electrode reserve can be easily implemented and controlled by increasing the battery charging voltage until the desired amount of Li is supplied.

[0061] The present invention will be specifically explained below with reference to examples, but the present invention is not limited to these examples.

[0062] Examples 1 and 2 and Comparative Examples 1 and 2 (Positive Electrode: Examples 1 and 2 and Comparative Example 1) The positive electrode active material was a Li transition metal oxide, LiNi 0.8 Co 0.15 Al 0.05 O 2A cathode composite slurry was obtained by mixing 92 parts by mass of Li transition metal oxide, 4 parts by mass of acetylene black as a conductive material, 4 parts by mass of PVdF (polyvinylidene fluoride) as a binder with 70 parts by mass of NMP (N-methyl-2-pyrrolidone). This slurry was applied to one side of a 15 μm thick aluminum foil, dried, and then pressed to form a cathode layer (excluding the current collector) with a thickness of 76 μm and a density of 2.8 g / cm. 3 This positive electrode 1 was used in Examples 1 and 2 and Comparative Example 1.

[0063] (Positive electrode: Comparative Example 2) The positive electrode active material was a Li transition metal oxide, LiNi 1/3 Co 1/3 Mn 1/3 O 2 A cathode composite slurry was prepared by mixing 92 parts by mass of Li transition metal oxide, 4 parts by mass of acetylene black as a conductive material, 4 parts by mass of PVdF (polyvinylidene fluoride) as a binder with 70 parts by mass of NMP (N-methyl-2-pyrrolidone). This slurry was applied to one side of a 15 μm thick aluminum foil, dried, and then pressed to form an electrode layer (excluding the current collector) with a thickness of 76 μm and a density of 2.8 g / cm. 3 In Comparative Example 2, this positive electrode 2 was used.

[0064] (Negative electrode) Graphite particles (graphitized MCMB; average particle diameter 25 μm) were used as the negative electrode active material. 93 parts by mass of graphite particles, 2 parts by mass of acetylene black as a conductive material, 5 parts by mass of PVdF (polyvinylidene fluoride) as a binder, and 95 parts by mass of NMP (N-methyl-2-pyrrolidone) were mixed to obtain a negative electrode composite slurry. This slurry was applied to one side of a 10 μm thick copper foil, dried, and then pressed to obtain four types of negative electrodes 1 to 4 having the thickness and density of the negative electrode layer (excluding the negative electrode current collector) shown in Table 1. The obtained negative electrode was used as the working electrode, and lithium metal was used as the counter electrode and reference electrode. LiPF at a concentration of 1 mol / L was used as the electrolyte in a solvent mixture of ethylene carbonate and methyl ethyl carbonate in a 3:7 (volume ratio) ratio. 6A triode cell (half cell) for evaluating the negative electrode was prepared in a dry room using a solution of the graphite particles. Using this triode cell, lithium was inserted at a current of 3 mA / g per weight of graphite until the potential reached 10 mV relative to lithium. The negative electrode capacity of each graphite particle was measured, and was found to be 371 mAh / g based on the weight of the graphite particles.

[0065]

[0066] (Lithium-ion secondary battery) Positive electrodes 1 and 2 were combined with negative electrodes 1 to 4 to prepare four types of lithium-ion secondary batteries (single-layer laminate cells) shown in Table 2 (Batteries 1 to 4). The opposing areas of the positive and negative electrodes were 5 × 3 cm. 2 The separator was a polyethylene porous membrane separator (thickness 20 μm, porosity 40%), and the electrolyte was a 1 mol / l concentration of LiPF in a solvent made by mixing ethylene carbonate and methyl ethyl carbonate in a volume ratio of 3:7. 6 The battery was fabricated in a dry room with a dew point of -50°C, and the electrodes used in the battery were dried at 170°C and the other components at 60°C under vacuum for 10 hours.

[0067] The fabricated lithium-ion secondary batteries were charged at 8 mA to a predetermined voltage (4.0-4.2 V) at varying charging voltages to vary the amount of Li extracted from the positive electrode active material. After charging, the batteries were subjected to constant-current constant-voltage charging at the predetermined voltage (4.0-4.2 V) until the current decayed to 0.8 mA. Subsequently, the batteries were discharged at a constant current of 8 mA to 2.75 V. This charge-discharge cycle was repeated three times. Table 2 shows the positive electrode utilization (the ratio of the amount of Li extracted from the positive electrode active material during battery charge to the amount of Li contained in the positive electrode at the time of battery manufacture) and the resulting discharge capacity. The energy density (assuming an actual battery) calculated using the resulting discharge capacity is also listed. The energy density was calculated assuming an actual battery filled to 70% with electrodes, including a separator, based on the opposing area of ​​a single-layer laminate cell. Although Battery 1 of Example 1 has a low positive electrode utilization amount, it has an energy density equivalent to Battery 4 of Comparative Example 2 (a general-purpose positive electrode with a low Ni ratio). When a battery having the configuration of Battery 3 of Comparative Example 1 was charged and discharged under the same conditions as Battery 1 of Example 1, the energy density was 370 Wh / L, and a sufficient energy density was not obtained. When a battery having the configuration of Battery 1 of Example 1 was charged under the same conditions as Battery 3 of Comparative Example 1 and the negative electrode utilization amount was changed, Li metal deposition was observed on the negative electrode.

[0068]

[0069] AC impedance measurements were performed on each battery. The smallest intercept on the Z' axis in the Nyquist plot was taken as the bulk resistance, and the value obtained by subtracting the bulk resistance from the arc termination resistance was analyzed as the reaction resistance. Measurement conditions were 25°C, SOC (State of Charge) was 100% based on the cell voltage, an amplitude of 10 mV, and frequencies ranging from 500 kHz to 0.1 Hz. An outline of the analysis method for AC impedance measurements is shown in Figure 2.

[0070] The internal resistance of each battery was measured using the current-rest method. Specifically, at 25°C, the battery was subjected to constant-current, low-voltage charging (CCCV charging) at a charge rate of 0.5C and a cut current of 0.05C up to an upper voltage of 4.2V, corresponding to an SOC of 100%. Next, after a 10-minute rest, the battery was discharged to an SOC of 90% (12 minutes) at a discharge rate of 0.5C, followed by a 1-minute rest. The resistance obtained by dividing the voltage change 1 second after the rest by the discharge current was defined as the rest method resistance (1-second rate), the resistance obtained by dividing the voltage change 60 seconds after the rest by the discharge current was defined as the rest method resistance (60-second rate), and the resistance calculated by subtracting the rest method resistance (1-second rate) from the rest method resistance (equilibrium component) was defined as the rest method resistance.

[0071] After completing the above initial measurements, each battery was charged at 50°C to a predetermined voltage (Table 2) at a current equivalent to 0.5 C based on the discharge capacity at the third cycle, and then constant-current constant-voltage charging was performed at the predetermined voltage until the current decayed to a current equivalent to 0.05 C. A cycle test was then performed by repeatedly discharging at a constant current equivalent to 0.5 C to 2.75 V. The results are shown in Figure 3. The batteries of the present invention, batteries 1 and 2 of Examples 1 and 2, have superior cycle characteristics compared to battery 3 of Comparative Example 1 (high positive electrode utilization rate) and battery 4 of Comparative Example 2 (high positive electrode utilization rate, low positive electrode Ni ratio).

[0072] From this discharge data, a power law (Δ [change in capacity] = α × [number of cycles]) β The relationship between the total charge / discharge capacity and the number of cycles was calculated using the above formula (2), and the results are shown in Figure 4. The total charge / discharge capacity up to 5,000 cycles was 146,660 mAh for Battery 1 of Example 1 and 148,553 mAh for Battery 2 of Example 2, which allows for the storage of approximately 1.3 times the amount of electricity as Battery 3 of Comparative Example 1 (114,306 mAh). It can also be seen that Battery 4 of Comparative Example 2 cannot be charged / discharged up to 5,000 cycles.

[0073] After the cycle test, the resistance (AC, rest resistance) of each battery was measured in the same manner as in the initial state. The initial and post-cycle values ​​are shown in Table 3. Battery 1 of Example 1 showed little change in resistance and almost no increase in the equilibrium component indicating gas generation, and it is believed that the cycle was carried out under near-ideal conditions (no excessive side reactions, gas generation, etc.), making this battery suitable for reuse after degradation.

[0074]

[0075] The cycle-degraded Batteries 1-3 of Examples 1-2 and Comparative Example 1 were charged at 25°C to 4.2 V at a current equivalent to 0.5 C, and then subjected to constant-current constant-voltage charging at a predetermined voltage until the current decayed to a current equivalent to 0.05 C. Subsequently, constant-current discharge was performed to 2.75 V at a current equivalent to 0.5 C. Because Batteries 1-2 of Examples 1-2 had reserve Li, their capacity was restored. The results are shown in Table 4. After 300 cycles, a cycle test was conducted. The results are also shown in Table 4. For Batteries 1-2 of Examples 1-2, the capacity was restored to more than 80% of the initial capacity. Subsequent cycling under the same conditions did not result in significant degradation.

[0076]

Claims

1. A lithium ion secondary battery comprising at least a positive electrode and a negative electrode, wherein the positive electrode contains a positive electrode active material, and the positive electrode active material contains a lithium-containing metal oxide containing nickel, and the lithium-containing metal oxide contains 70 to 100 atomic % of nickel, with a total amount of metals other than lithium being 100 atomic %, and wherein, when the positive electrode utilization amount is 100% as the total capacity of lithium contained in the positive electrode and charging is performed to a capacity of 50 to 70% as the capacity of lithium extracted from the positive electrode active material in a first cycle, the negative electrode utilization amount is 80 to 95% of the capacity charged in the first cycle, with a negative electrode capacity as the maximum charge amount at which lithium can be inserted into the negative electrode being 100%.

2. The lithium ion secondary battery according to claim 1, which is a reserve type lithium ion secondary battery that holds available lithium as a reserve.

3. The lithium-ion secondary battery according to claim 1 or 2, which is used in an electric vehicle for car sharing.

4. A method for improving the life of a lithium ion secondary battery, comprising: at least a positive electrode and a negative electrode; the positive electrode contains a positive electrode active material; the positive electrode active material contains a lithium-containing metal oxide containing nickel; and the lithium-containing metal oxide contains 70 to 100 atomic % of nickel, with a total amount of metals other than lithium being 100 atomic %, the method comprising adjusting a positive electrode utilization amount to be 50 to 70% as the capacity of lithium extracted from the positive electrode active material during charging, assuming that the total capacity of lithium contained in the positive electrode is 100%, and adjusting a negative electrode utilization amount to be 80 to 95% as the capacity charged during charging, assuming that the negative electrode capacity as the maximum charge amount at which lithium can be inserted into the negative electrode is 100%.

5. The method of claim 4, wherein the lithium ion secondary battery is a reserve type lithium ion secondary battery that holds available lithium in reserve.

6. The method according to claim 4 or 5, wherein the lithium ion secondary battery is used in an electric vehicle for car sharing.

7. A method for using a lithium ion secondary battery according to any one of claims 1 to 3 after the lithium ion secondary battery has deteriorated, comprising using available lithium reserved within the lithium ion secondary battery.

8. The method of claim 7, further comprising increasing the charging voltage until the available lithium reserve within the lithium ion secondary battery is supplied.

Citation Information

Patent Citations

  • Lithium secondary battery and manufacturing method thereof

    JP2012221681A

  • Lithium-ion cells with improved aging behavior

    JP2013543243A

  • Lithium ion secondary battery and method for manufacturing same

    WO2017082083A1