Aluminum powder product

Aluminum powder products with enhanced surface treatment and phosphorus concentration improve fluidity and corrosion resistance, addressing clogging and shape maintenance issues, enabling effective sintering and additive manufacturing.

WO2024203930A1PCT designated stage expired Publication Date: 2024-10-03MITSUBISHI MATERIALS CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011444
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Aluminum powder products face challenges in achieving high fluidity while maintaining particle shape and size, particularly in powder sintering processes, due to low fluidity and clogging issues in feeders, which affects sintering density and precision in complex shape control.

Method used

The development of aluminum powder products with a specific BET surface area, high phosphorus concentration, and uneven phosphoric acid compound distribution near the surface, enhancing fluidity and corrosion resistance, and maintaining particle size and shape through surface treatment with phosphoric acid-based molecules.

Benefits of technology

The treated aluminum powder products exhibit improved fluidity, preventing clogging, maintaining desired particle size and packing density, and offering excellent corrosion resistance, suitable for additive manufacturing and sintering processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011444_03102024_PF_FP_ABST
    Figure JP2024011444_03102024_PF_FP_ABST
Patent Text Reader

Abstract

This aluminum powder product (1) has a BET specific surface area of 0.16 m2 / g or more and a phosphorus concentration of the powder product (1) of 1×10-3 mass % or more as measured by the molybdenum blue method, and in the photoelectron spectrum of the powder product (1) as measured by X-ray photoelectron spectroscopy (XPS method), the ratio IP2s / ICl2p of the P2s peak intensity IP2s at 191.5 eV to the Cl2p peak intensity ICl2p at 199.0 eV is 1.00 or more.
Need to check novelty before this filing date? Find Prior Art

Description

Aluminum powder products

[0001] The present invention relates to an aluminum powder product. This application claims priority to Japanese Patent Application No. 2023-055049, filed on March 30, 2023, the contents of which are incorporated herein by reference.

[0002] Aluminum is used for heat sinks in equipment due to its light weight and excellent electrical and thermal conductivity. However, it is a typical difficult-to-sinter metal, and achieving high densification of the structure has been a challenge in powder sintering. In particular, when complex and precise shape control is required, such as for heat exchanger fin materials, powder sintering methods such as metal injection molding and additive manufacturing are commonly used. In powder sintering, silos and hoppers are commonly used as powder feeders, but powders with low fluidity can form bridges or ratholes within the feeder, blocking the flow path. This results in impeded powder flow, causing some powder particles to solidify or change composition due to pressure from other powders, resulting in poor sintering. Generally, powder fluidity is believed to increase with particle shape, but controlling particle shape during the manufacturing process is often difficult.

[0003] Conventionally, when desired physical properties cannot be obtained during the manufacturing process, surface treatment of powders has been performed. For example, a technique for coating the surfaces of particles such as titanium alloys and nickel alloys by adding nanoparticles of silica or alumina surface-modified with an organic substance to the surfaces of these particles is known. Another technique is known for improving fluidity by precipitating nanostructures on the surfaces of particles through thermal plasma treatment, thereby reducing the contact area between particles (see Patent Document 1).

[0004] In addition, a technique is known in which powder whose shear adhesion force has increased due to deagglomeration and whose fluidity has decreased is subjected to heat treatment to form an oxide film on the particle surface, thereby reducing the shear adhesion force and restoring fluidity (see Patent Document 2).

[0005] JP 2019-112699 A JP 2019-183199 A

[0006] However, heat treatment and thermal plasma treatment of powders require specialized equipment and are not easily performed. Furthermore, because aluminum has a low melting point, thermal plasma treatment cannot be limited to treating the particle surface alone, and the particle shape changes, significantly affecting powder properties such as packing density, making it difficult to apply. Therefore, there is a need for a surface treatment technology that can give aluminum powder particles high fluidity while maintaining their outer diameter and shape.

[0007] The present invention has been made in view of the above problems, and its object is to provide an aluminum powder product that has high fluidity while retaining the outer diameter and shape of the particles.

[0008] As a result of various investigations, the present invention provides the following aluminum powder product.

[0009] (1) The aluminum powder product according to aspect (1) of the present invention has a BET specific surface area of ​​0.16 m 2 / g or more, and the phosphorus concentration of the whole powder product measured by the molybdenum blue method is 1 x 10 -3 % by mass or more, and in the photoelectron spectrum of the powder product measured by X-ray photoelectron spectroscopy (XPS method), a P2s peak intensity I of 191.5 eV P2s and the Cl2p peak intensity at 199.0 eV I Cl2p Relative to I P2s / I Cl2p is 1.00 or more.

[0010] The aluminum powder product has a predetermined BET specific surface area and a predetermined total phosphorus concentration, and in the photoelectron spectrum of the powder product particles, the P2s peak intensity at 191.5 eV is equal to or greater than the Cl2p peak intensity at 199.0 eV. That is, the phosphoric acid compound is present in an amount equal to or greater than the inevitable impurities of the chlorine-containing compound. This improves the fluidity of the aluminum powder product. This prevents clogging of the aluminum powder product in the flow passages of silos and hoppers that contain the aluminum powder product. The particle structure of the aluminum powder product can be easily achieved without affecting the particle size, making it easier to obtain an aluminum powder product with a desired particle size and whose packing density, etc., are controlled to desired values. Furthermore, the aluminum powder product can suppress hydrogen generation in hot water, thereby exhibiting excellent corrosion resistance.

[0011] (2) Aspect (2) of the present invention relates to the aluminum powder product of aspect (1), wherein the particles constituting the powder product have a high phosphorus concentration region in a region 30 nm or less deep from the outermost surface, the phosphorus concentration in the high phosphorus concentration region being 3.5 times higher than the phosphorus concentration in a region more than 30 nm deep from the outermost surface of the particle, and a phosphate compound is unevenly distributed in the high phosphorus concentration region. Specifically, the region more than 30 nm deep from the outermost surface of the particle is a region more than 30 nm deep but not more than 60 nm deep from the outermost surface. Analysis by XPS suggests that the phosphate compound is a phosphorus oxoacid.

[0012] If a high phosphorus concentration region exists in a region from the outermost surface to a depth of 30 nm and the phosphate compound is unevenly distributed in this region, an aluminum powder product having the above-mentioned excellent effects can be obtained.

[0013] (3) Aspect (3) of the present invention is directed to the aluminum powder product of aspect (1) or (2), wherein the volume-based 50% cumulative particle diameter (median diameter D 50 ) is 15 μm or more and 45 μm or less, and the Hausner ratio of the powder product is preferably 1.14 or less.

[0014] Median diameter D 50If the aluminum powder product has a median diameter D of 15 μm or more, the powder product is safe in terms of handling. 50 When the particle size is 15 μm or more and 45 μm or less, the aluminum powder product has excellent handleability for additive manufacturing applications, making it possible to provide an aluminum powder product suitable for additive manufacturing. When the powder product has a Hausner ratio of 1.14 or less, it has excellent fluidity. Furthermore, excellent fluidity contributes to ensuring the fluidity necessary for powder sintering, making it possible to provide an aluminum powder product suitable for powder sintering.

[0015] (4) In aspect (4) of the present invention, in the aluminum powder product according to any one of aspects (1) to (3), it is preferable that the sphericity measured by image analysis is 0.93 or more.

[0016] If the sphericity of the particles is 0.93 or more, the particles have a shape that is close to a sphere, which is preferable in terms of imparting good flowability.

[0017] (5) Aspect (5) of the present invention is the aluminum powder product according to any one of aspects (1) to (4), wherein the aluminum powder product is preferably used for additive manufacturing.

[0018] According to an aspect of the present invention, an aluminum powder product has a predetermined BET specific surface area, a predetermined total phosphorus concentration, and in the photoelectron spectrum of the powder product, the P2s peak intensity at 191.5 eV is equal to or greater than the Cl2p peak intensity at 199.0 eV. This improves the fluidity of the aluminum powder product. This prevents clogging of the aluminum powder product in the flow passages of silos and hoppers that store the aluminum powder product. Since the particle structure of the aluminum powder product can be achieved without affecting the particle size, it is easy to obtain an aluminum powder product with a desired particle size and with packing density and other properties controlled to desired values. Furthermore, the aluminum powder product has excellent corrosion resistance because it can suppress hydrogen generation in hot water.

[0019] FIG. 1 is a partial cross-sectional view of a particle body of an aluminum powder product according to the first embodiment. FIG. 2A is a depth direction concentration profile of each element in the aluminum powder product of Example 1. FIG. 2B is a depth direction concentration profile of each element in the aluminum powder product of Example 2. FIG. 2C is a depth direction concentration profile of each element in the aluminum powder product of Example 3. FIG. 2D is a depth direction concentration profile of each element in the aluminum powder product of Example 4. FIG. 2E is a depth direction concentration profile of each element in the aluminum powder product of Comparative Example 1. FIG. 2F is a depth direction concentration profile of each element in the aluminum powder product of Comparative Example 2. FIG. 2G is a depth direction concentration profile of each element in the aluminum powder product of Comparative Example 3. FIG. 2H is a depth direction concentration profile of each element in the aluminum powder product of Comparative Example 4. FIG. 3 is a surface secondary electron SEM image of the aluminum powder product of Comparative Example 1. FIG. 4 is a surface secondary electron SEM image of the aluminum powder product of Example 1. FIG. 5A shows photoelectron spectra of the aluminum powder products of Example 1 and Comparative Example 1, with binding energies ranging from 190 to 210 eV. FIG. 5B shows photoelectron spectra of the aluminum powder products of Example 1 and Comparative Example 1, with binding energies ranging from 123 to 143 eV. FIG. 6A shows photoelectron spectra of the aluminum powder products of Example 2 and Comparative Example 2, with binding energies ranging from 190 to 210 eV. FIG. 6B shows photoelectron spectra of the aluminum powder products of Example 2 and Comparative Example 2, with binding energies ranging from 123 to 143 eV. FIG. 7A shows photoelectron spectra of the aluminum powder products of Example 3 and Comparative Example 3, with binding energies ranging from 190 to 210 eV. FIG. 7B shows photoelectron spectra of the aluminum powder products of Example 3 and Comparative Example 3, with binding energies ranging from 123 to 143 eV. FIG. 8A shows photoelectron spectra of the aluminum powder products of Example 4 and Comparative Example 4, with binding energies ranging from 190 to 210 eV. FIG. 8B is a diagram showing photoelectron spectra of the aluminum powder products of Example 4 and Comparative Example 4, in the binding energy range of 123 to 143 eV.

[0020] The present invention will be described in detail below, but is not limited to the embodiments described below. In this embodiment, an aluminum powder product 1 comprises a plurality of spherical particle bodies (particles constituting the powder product) 2. FIG. 1 shows a partial cross-sectional view of the particle body 2. The particle body 2 has a high-concentration region 2a of phosphorus (P) in the outermost surface region. While the high-concentration region 2a is preferably formed over the entire surface (100 area%) of the particle body 2, the high-concentration region 2a may be formed over almost the entire surface (90 area% or more) of the particle body 2, or over most of the surface (60 area% or more) of the particle body 2. It is difficult to accurately measure the area ratio of the high-concentration region 2a to the surface area of ​​the particle body 2. While approximate area ratios are exemplified above, the present invention is not limited to these area ratios. Since the high-concentration region 2a is formed by immersing the raw material powder in a chemical solution as described below, there may be unreacted regions on the surface of the particle body 2 where the high-concentration region 2a is not formed.

[0021] The aluminum powder product 1 is aluminum or aluminum alloy and 1 × 10 -3The aluminum powder product 1 contains at least 100% by mass of phosphorus. The aluminum has a purity of at least 99% and consists only of Al and unavoidable impurities. In this embodiment, the aluminum is also referred to as pure aluminum. The composition of aluminum or an aluminum alloy, which is a component other than phosphorus, in the aluminum powder product 1 will be described below. The amount of each element will be described assuming that the total composition of the aluminum or aluminum alloy is 100% by mass. The amount of phosphorus in the aluminum powder product 1 is significantly smaller than the amounts of other elements whose contents are specified. Therefore, the amount of each element calculated assuming that the total composition of the aluminum powder product 1 is 100% by mass is approximately the same as the amount of each element calculated assuming that the total composition of the aluminum or aluminum alloy is 100% by mass. The elements contained in the aluminum alloy are not particularly limited, and the aluminum alloy may contain any of the elements commonly known in aluminum alloys. For example, the aluminum alloy contains 13.5% or less Si, 5.6% or less Mg, 0.2% or less Ti, 0.35% or less Cr, 1.5% or less Mn, 0.7% or less Fe, 6.0% or less Cu, and 6.1% or less Zn, with the balance being Al and unavoidable impurities. In this composition, the range of the amount of each element includes 0%, so the aluminum composition is also included. Therefore, the aluminum powder product 1 has 13.5% or less Si, 5.6% or less Mg, 0.2% or less Ti, 0.35% or less Cr, 1.5% or less Mn, 0.7% or less Fe, 6.0% or less Cu, 6.1% or less Zn, and 1×10 -3 % or more, with the balance being Al and inevitable impurities. As an example, general aluminum or aluminum alloys such as those of the A1000 series, A2000 series, A3000 series, A4000 series, A5000 series, A6000 series, and A7000 series specified by JIS may be used. Alternatively, other general aluminum alloys containing elements not contained in aluminum alloys of these series may be used.

[0022] A1050, an example of the A1000 series, refers to aluminum with a purity of 99.5% or more, and may contain Fe, Si, and other inevitable impurities. The A1100 series refers to aluminum with a purity of 99% or more. As an example, A1100 aluminum contains a total of 1.0% or less of Fe and Si, approximately 0.05 to 0.20% of Cu, 0.05% or less of Mn, and 0.1% or less of Zn, with the remainder being Al and inevitable impurities. Elements other than Al can also be considered inevitable impurities. Note that the percentage indicating the content of an element refers to mass % unless otherwise specified. The A2000 series refers to aluminum alloys with a large amount of Cu added, and an example of this is the A2024 aluminum alloy, which contains up to 0.5% Si, up to 0.5% Fe, 3.8 to 4.9% Cu, 0.3 to 0.9% Mn, 1.2 to 1.8% Mg, 0.1% or less Cr, and 0.25% or less Zn, with the balance being Al and unavoidable impurities. The A3000 series refers to Al-Mn aluminum alloys, and an example of this is the A3003 aluminum alloy, which contains up to 0.6% Si, up to 0.7% Fe, 0.05% Cu, 1.0 to 1.5% Mn, and 0.1% or less Zn, with the balance being Al and unavoidable impurities.

[0023] The A4000 series refers to aluminum alloys containing Si, such as A4032, which contains 11.0 to 13.5% Si, 1.0% or less Fe, 0.5 to 1.3% Cu, 0.8 to 1.3% Mg, 0.10% or less Cr, and 0.25% or less Zn, with the balance being Al and unavoidable impurities. The A5000 series refers to aluminum alloys containing Mg, such as A5052, which contains 0.25% or less Si, 0.4% or less Fe, 0.10% or less Cu, 0.1% or less Mn, 2.2 to 2.8% Mg, 0.15 to 0.35% Cr, and 0.1% or less Zn, with the balance being Al and unavoidable impurities. The A6000 series refers to aluminum alloys to which Mg and Si are added. As an example, the A6061 aluminum alloy contains Si: 0.4 to 0.8%, Fe: 0.7% or less, Cu: 0.15 to 0.4%, Mn: 0.15% or less, Mg: 0.8 to 1.2%, Cr: 0.15 to 0.35%, Zn: 0.25% or less, Ti: 0.15% or less, and the balance being Al and unavoidable impurities.

[0024] The A7000 series refers to aluminum alloys with Zn and Mg added as the main elements. As an example, the A7075 aluminum alloy contains Si: 0.4% or less, Fe: 0.5% or less, Cu: 1.2 to 2.0%, Mn: 0.3% or less, Mg: 2.1 to 2.9%, Cr: 0.18 to 0.35%, Zn: 5.1 to 6.1%, Ti: 0.2% or less, and the balance being Al and unavoidable impurities.

[0025] "Phosphorus (P) concentration contained in the whole aluminum powder product: 1 x 10 -3 mass% or more (10 mass ppm or more)" The phosphorus concentration contained in the entire aluminum powder product 1 is less than 10 mass ppm (1 × 10 -3% by mass), effective high-concentration regions 2a tend not to be formed. Since the total phosphorus concentration of the aluminum powder product 1 according to this embodiment is 10 ppm by mass or more, high-concentration regions 2a of phosphorus that can impart good corrosion resistance and fluidity to the aluminum powder product 1 are formed on the outermost surface of the particle bodies 2. The total phosphorus concentration of the aluminum powder product 1 is preferably 10 ppm by mass or more and 100 ppm by mass or less, and more preferably 20 ppm by mass or more and 80 ppm by mass or less.

[0026] "I P2s / I Cl2p : 1.00 or more" In the photoelectron spectrum of aluminum powder product 1 measured by X-ray photoelectron spectroscopy (XPS method), the P2s peak intensity I P2s is the Cl2p peak intensity I Cl2p If the P2s peak intensity I is smaller than the P2s peak intensity I, the amount of phosphoric acid compounds present is less than the amount of chlorine-containing compounds present, which are inevitable impurities, and the effective phosphorus-rich region 2a tends not to be formed. P2s is the Cl2p peak intensity I Cl2p As a result, a high-concentration region 2a of phosphorus is formed on the outermost surface of the particle body 2. The high-concentration region 2a of phosphorus reduces the conductivity, causing the particle body 2 to be charged, and the electrostatic repulsion reduces friction between the particle bodies 2, improving the fluidity. In order to obtain such an effect, the P2s peak intensity I P2s and Cl2p peak intensity I Cl2p Ratio I P2s / I Cl2p is preferably 1.00 or more and 100 or less, and more preferably 1.00 or more and 10.0 or less.

[0027] “BET specific surface area: 0.16m 2 / g or more" BET specific surface area of ​​0.16 m 2 By making the BET specific surface area 0.16 m / g or more, it is possible to improve the Hausner ratio, which is an index of fluidity. 2 / g or more 0.9m 2 / g or less, more preferably 0.16m 2 / g or more 0.4m 2 / g or less.

[0028] "Phosphorus-rich region containing phosphate-based compounds" From the analysis results (depth concentration profiles of each element) of the sample by EDS (energy dispersive spectroscopy) in the examples described below, it is estimated that the phosphorus-rich region 2a is present in a region 30 nm or less deep from the outermost surface of the particle body 2. The phosphorus concentration in the phosphorus-rich region 2a is 3.5 times higher than the phosphorus concentration in a region more than 30 nm deep from the outermost surface of the particle body 2. Furthermore, from the analysis results (photoelectron spectrum) of this sample by XPS (X-ray photoelectron spectroscopy) described below, the P2p spectrum (P2p peak) and P2s spectrum (P2s peak) obtained indicate that phosphorus is present in the form of a phosphate-based compound in the phosphorus-rich region 2a. From the analysis by XPS, it is estimated that the phosphate-based compound is a phosphorus oxoacid. Examples of phosphate compounds include phosphinic acid, phosphonic acid, phosphorous acid, phosphoric acid, diphosphate, triphosphate, and metatriphosphate, as well as phosphate derivatives such as etidronic acid. However, it is difficult to identify specific compounds using XPS analysis. Furthermore, when examining the elemental distribution of Al in the depth direction concentration profile of each element, the EDS spectrum intensity (detection signal intensity) of Al gradually increases from the outermost surface toward the depth direction, and the EDS spectrum intensity of Al becomes stable in the depth region beyond 30 nm from the outermost surface. From this, it can be inferred that some kind of coating is formed in the powder body 2 from the outermost surface to a depth of about 30 nm, and that a high-phosphorus concentration region 2a is formed within that coating.

[0029] "Volume-based 50% cumulative particle diameter (median diameter D 50 In the aluminum powder product 1, the 50% cumulative particle diameter on a volume basis is preferably 15 μm or more and 45 μm or less. The 50% cumulative particle diameter on a volume basis is more preferably 20 μm or more and 35 μm or less. Regarding the aluminum powder product 1, the median diameter D 50When the median diameter (D) is 15 μm or more and 45 μm or less, when the aluminum powder product 1 is used in powder metallurgy, it is possible to obtain good molding accuracy while ensuring suitable fluidity. Therefore, it is possible to obtain an aluminum powder product 1 having good fluidity and excellent sinterability. 50 If the median diameter (D) is less than 15 μm, the fluidity decreases and the risk of fire and scattering increases. 50 If the diameter exceeds 45 μm, the fluidity is improved, but it becomes difficult to obtain a high-density sintered body when using the aluminum powder product 1 in a powder metallurgy manufacturing device.

[0030] "Sphericity: 0.93 or more" The sphericity of the particle body 2 of the aluminum powder product 1 is measured by image analysis using an image analyzer such as the Morphologi4 dry image measuring instrument manufactured by Malvern. If the sphericity is less than 0.93, the particle shape deviates from a spherical shape, which is likely to cause a decrease in packing density and a decrease in fluidity when subjected to additive manufacturing. For this reason, the sphericity is preferably 0.93 or more. The sphericity is more preferably 0.93 or more and 1.00 or less, and even more preferably 0.97 or more and 1.00 or less.

[0031] "Hausner ratio: 1.14 or less" If the Hausner ratio exceeds 1.14, the fluidity decreases, and clogging of flow paths such as hoppers becomes more likely. The Hausner ratio is preferably 1.14 or less, and in this case, the fluidity required for powder sintering can be ensured. The Hausner ratio is more preferably 1.00 or more and 1.14 or less, and even more preferably 1.00 or more and 1.10 or less.

[0032] "Method for manufacturing an aluminum powder product" The method for manufacturing an aluminum powder product 1 includes the steps of preparing a raw material powder, removing an oxide film using a rust remover, and forming a film using a rust inhibitor. A rust remover containing a phosphoric acid-based inorganic or organic molecule and a rust inhibitor containing a phosphoric acid-based inorganic or organic molecule are used. This reduces the overall phosphorus concentration of the aluminum powder product 1 to 1×10 -3% by mass or more. A high phosphorus concentration region 2a is also formed. The phosphorus-based inorganic or organic molecule is one or more selected from phosphorus oxoacids, phosphorus oxoacid derivatives, phosphorus oxoacid salts, and salts of phosphorus oxoacid derivatives. Specific examples include phosphoric acid, etidronic acid, and sodium phosphate. To produce the aluminum powder product 1, a raw material powder is first prepared. To produce the raw material powder, a powder production method such as atomization can be used, for example. In the atomization method, a molten metal of a desired composition is prepared, and the molten metal is sprayed at high speed through a nozzle into an atmosphere such as air, nitrogen gas, or a vacuum atmosphere, and the molten metal droplets are quenched to produce the raw material powder. When producing an aluminum powder product 1 containing pure aluminum, pure aluminum molten metal is used. When producing an aluminum powder product 1 containing an aluminum alloy, an aluminum alloy molten metal of a desired composition is used.

[0033] Examples of methods for producing a molten aluminum alloy of a target composition include a method using an aluminum alloy of a target composition ratio as a base material, or a method of combining high-purity aluminum of 99.5% or more with a base material of multiple additive elements that will result in a molten alloy of a target composition ratio. When a molten metal is sprayed into an atmosphere to produce a raw material powder, the particles of the raw material powder usually have a spherical shape or a shape similar thereto. The volume-based 50% cumulative average particle diameter (D 50 : μm) is, for example, 15 μm or more and 45 μm or less.

[0034] When raw powder is produced, an aluminum oxide film is formed on the outer peripheral surfaces of the raw powder particles. When the raw powder is produced by atomization in a nitrogen gas atmosphere or a vacuum atmosphere, even if the particle surfaces are not oxidized immediately after production, when the raw powder is removed from the atomization apparatus or production atmosphere and subjected to the next process in air, an oxide film inevitably forms on the surface of the raw powder particles over time. Since the aluminum oxide film can hinder sintering during the sintering process described below, it is desirable to remove it as much as possible. For this reason, in this embodiment, a step of immersing the produced raw powder in a rust remover solution to remove the oxide film is carried out.

[0035] When immersing the raw material powder in a rust remover solution, the rust remover solution can be appropriately diluted with a solvent such as water. Furthermore, stirring may be performed during immersion in the rust remover solution to promote the rust removal effect. For stirring, an ultrasonic cleaner or a stirrer with a rotating blade may be used. The raw material powder may be immersed in the rust remover solution, and then the surface of the raw material powder may be washed with a cleaning solution such as pure water or tap water. If the possibility of re-oxidation is low after removing rust from the surface of the raw material powder particles with a rust remover, it is preferable to remove the rust remover by washing with pure water or tap water. If the rust remover is effective in removing the oxide film, it is believed that re-oxidation will not occur easily even if the particles are washed after rust removal. When removing the oxide film, it is desirable to remove it from the entire surface of the raw material powder particles. However, if the oxide film is sufficiently thin or the remaining area of ​​the oxide film is small, it is acceptable for the oxide film to remain on part of the surface.

[0036] Rust removers containing inorganic or organic phosphoric acid molecules can be solutions containing organic acids such as citric acid, acidic solvents such as phosphoric acid, or basic solvents such as sodium hydroxide. For example, rust removers containing inorganic or organic phosphoric acid molecules and amine-based carboxylates can be used. Alternatively, for example, a composition containing 2.5 to 10 mass% citric acid, 2.5 to 10 mass% propylene glycol monobutyl ether, and 2.5 to 10 mass% phosphoric acid as main components, and further containing 2.5 mass% or less of phosphonic acid and 2.5 mass% or less of mineral spirits (aliphatic hydrocarbons) can be used. A specific example of a rust remover containing inorganic or organic phosphoric acid molecules and amine-based carboxylates is the rust remover BF4-26 manufactured by Tanimura Corporation.

[0037] For example, 100 to 500 ml of the above-mentioned rust remover aqueous solution containing the inorganic or organic phosphoric acid molecule and the amine-based carboxylate salt and approximately 150 to 700 g of raw material powder are placed in a container, the solution is stirred for 1 to 60 minutes, and the supernatant is removed after the raw material powder has settled. The raw material powder that has settled in the rust remover aqueous solution can be rinsed with a sufficient amount of pure water or the like and sent to the next process. In the rinsing process, pure water is added to the container and the solution is stirred, and then the solution is allowed to stand and the supernatant is removed. Alternatively, as an alternative to rinsing, a weakly basic, water-soluble agent may be used to neutralize the remaining rust remover.

[0038] After removing the oxide film from the raw material powder, the raw material powder is then immersed in a solution of rust inhibitor to form a rust inhibitor coating on the surface of the raw material powder. In this case, the raw material powder can be stored in the container described above and rinsed with pure water as many times as necessary. The following rust inhibitor can then be added to the container and immersed in the rust inhibitor. When immersing the raw material powder in the rust inhibitor solution, the rust inhibitor solution can be diluted appropriately by adding a solvent such as water. Furthermore, when immersing in the aqueous solution of the rust inhibitor, stirring or the like can be performed to promote the formation of a coating. After immersion in the rust inhibitor solution, the surface of the raw material powder can be washed with a cleaning solution such as tap water. When removing rust from the raw material powder and then immersing it in the rust inhibitor solution, the following steps can be performed in the same container, or the rust removal and rust prevention can be performed in separate containers. (1) Immerse aluminum powder in a solution containing the rust remover and stir the solution. (2) The supernatant is then removed and pure water is added to the container to rinse and clean the raw material powder. (3) The supernatant is then removed and the rust inhibitor is added to the same container and the solution is stirred.

[0039] Examples of rust inhibitors containing phosphate-based inorganic or organic molecules include aqueous solutions of volatile rust inhibitors containing one or a mixture of amine-based nitrites, amine-based carboxylates, amine-based chromates, carboxylic acid esters, and heterocyclic compounds, and phosphate-based inorganic or organic molecules. Organic solvents containing these salts, esters, and compounds may also be used. An example of a rust inhibitor containing phosphate-based inorganic or organic molecules and amine-based carboxylates is an aqueous solution containing 2.5 to 10% by mass of potassium hydrogen phthalate as the main component, and further containing 2.5% by mass or less of cyclocarboxylic acid, 2.5% by mass or less of disodium metasilicate, and 2.5% by mass or less of trisodium phosphate. Other examples include solutions of surfactants containing phosphate-based inorganic or organic molecules and carboxylates. A specific example of a rust inhibitor containing phosphate-based inorganic or organic molecules and amine-based carboxylates is the rust inhibitor BF4-16 manufactured by Tanimura Corporation. Other examples of the rust inhibitor that can be used include Mechahibitor #325 manufactured by Nippon Mecha Chemical Co., Ltd., and inhibitors containing amine-based carboxylic acids as components for rust prevention, chelating agents, water-soluble rust inhibitors, and volatile rust inhibitors.

[0040] The aluminum powder product 1 shown in FIG. 1 can be obtained by immersing the raw material powder in a solution of rust inhibitor and then removing it from the solution. The raw material powder particles may be immersed in the solution of rust inhibitor and then washed with a cleaning solution such as pure water or tap water. If a coating is formed on the surface of the raw material powder particles by the rust inhibitor, the coating can be washed with pure water or tap water. If the coating formed by the rust inhibitor is sufficient, it is believed that the coating will not easily peel off even when washed after rust prevention treatment.

[0041] The aluminum powder product 1 with the coating is recovered from the solution and dried in an atmosphere such as the air. This drying process can be carried out in an atmosphere of room temperature to 70°C, for example, drying at 45°C in the air. By going through the above steps, the aluminum powder product 1 (aluminum powder product 1 with a coating) targeted in this embodiment can be obtained. That is, the produced aluminum powder product 1 has the following characteristics: (1) BET specific surface area of ​​0.16 m 2 (2) The phosphorus concentration of the entire aluminum powder product 1 is 1×10 -3 (3) In the photoelectron spectrum, the ratio I P2s / I Cl2p (4) Preferably, D 50 is 15 μm or more and 45 μm or less. (5) Preferably, the Hausner ratio is 1.14 or less. (6) Preferably, the sphericity is 0.93 or more. (7) Preferably, the particle body 2 has a high phosphorus concentration region 2a in a region 30 nm or less deep from the outermost surface. The phosphorus concentration in the high phosphorus concentration region 2a is 3.5 times or more higher than the phosphorus concentration in an internal region 30 nm or more and 60 nm or less deep from the outermost surface. Phosphate-based compounds are unevenly distributed in the high phosphorus concentration region 2a. Note that, while the high phosphorus concentration region 2a is preferably present over the entire surface of the particle body 2, it does not have to be completely formed over the entire surface, and may be formed over most of the surface.

[0042] The aluminum powder product 1 described above exhibits excellent corrosion resistance because it can suppress the generation of hydrogen in hot water. Because the aluminum powder product 1 has sufficient corrosion resistance to water, it can be suitably used in the binder jet metal additive manufacturing process described below, which uses a binder containing water. If the aluminum powder product 1 satisfies the particle size described above, when it is made into a laminate of the aluminum powder product 1, it has good fluidity and the bulk density of the aluminum powder product layer can be stably obtained at a high level. Therefore, when a sintered body is manufactured, a dense sintered body can be obtained.

[0043] From the analytical results of the examples described below, it can be inferred that the concentrated phosphorus is present on the surface side of the particle body 2 as a phosphate-based compound, and it has also been found that the particle size of the particle body 2 remains almost unchanged even after the above-mentioned rust removal and rust prevention treatments. Therefore, with the above-mentioned aluminum powder product 1, the fluidity of the powder can be ensured by a simple method. This allows a dense sintered body to be produced using the aluminum powder product 1. Because the aluminum powder product 1 has high fluidity, clogging of the flow passages in silos and hoppers is also unlikely to occur. Furthermore, with the above-mentioned aluminum powder product 1, hydrogen generation in hot water can be suppressed, thereby improving corrosion resistance. Furthermore, since the appropriate particle size can be maintained even after the above-mentioned rust removal and rust prevention treatments, a powder that is highly safe and easy to handle can be provided.

[0044] "Method for manufacturing an aluminum sintered body" To manufacture an aluminum sintered body (additive manufacturing product) using the aluminum powder product 1 described above, a green body is manufactured using the aluminum powder product 1 as a material powder (powder for metal additive manufacturing). The green body is manufactured by a mold forming method or an additive manufacturing method. In the mold forming method, a material powder is filled into a mold having a predetermined shape to manufacture the green body. In the additive manufacturing method, the material powder is spread on a powder bed. A binder containing a thermosetting resin, a thermoplastic resin, or a photocurable resin is selectively sprayed onto this material powder, and the material powder is solidified to manufacture a first shaped piece. Next, the material powder is supplied to the powder bed, and the material powder is placed on the first shaped piece. The binder is selectively sprayed, and the material powder is solidified to manufacture a second shaped piece on the first shaped piece. This process is repeated to stack multiple shaped pieces to manufacture a laminate.

[0045] In additive manufacturing, a binder is selectively sprayed onto raw material powder, which is then solidified to create a shaped piece. This process is repeated to stack multiple shaped pieces to form a laminate. By repeatedly stacking the shaped pieces, the raw material powder is solidified to form a shape that matches the desired three-dimensional shape. After the raw material powder has solidified, unnecessary raw material powder is removed and degreased as necessary to obtain a green body.

[0046] Once the green body is obtained, it is placed in a heating furnace and heated to a temperature of about 560 to 650°C for the required time in a vacuum atmosphere, a reducing atmosphere, an inert gas atmosphere, or a reduced pressure gas flow atmosphere using a reducing gas or an inert gas, without pressure, to be sintered.

[0047] The obtained sintered body can be finished as needed by heat treatment, processing with a cutting tool, surface polishing, etc. to obtain a sintered body (layer-additive manufactured object). As a result, for example, the aluminum powder product 1 can be used to further improve the performance of heat exchange members, conductive members, and strength members.

[0048] An aluminum base material (aluminum purity of 99.5% or more) or an A6061 aluminum alloy base material was charged into a melting furnace to produce molten aluminum or molten aluminum alloy, and aluminum powder products of Comparative Examples 1 to 4 in Table 1, which will be described later, were produced from the molten aluminum or aluminum alloy by an inert gas atomization method.

[0049] Each aluminum powder product of Comparative Examples 1 to 4 was used as a raw material powder, and the raw material powder was subjected to rust removal and rust prevention treatment according to the following procedure. 650 g of raw material powder and 300 mL of rust remover (2x diluted BF4-26: Tanimura Corporation product name) were placed in a container and stirred at room temperature and atmospheric pressure. A mechanical stirrer was used for stirring at 350 rpm. After stirring for 15 minutes, 500 mL of pure water was added and the mixture was allowed to stand. The supernatant was removed after the raw material powder had settled. This pure water was added to increase the total volume of the solution and facilitate separation of the raw material powder and the rust remover solution.

[0050] Next, 100 mL of rust inhibitor (3x diluted BF4-16: Tanimura Co., Ltd. product name) was added to the container to neutralize the remaining rust remover. Pure water was then added again, and the mixture was left to stand. The powder precipitated, and the supernatant was removed. The rust remover was an acidic agent, while the rust inhibitor was a basic agent. This process prevented the remaining rust remover from functioning as an acid. Next, 300 mL of rust inhibitor (3x diluted BF4-16: Tanimura Co., Ltd. product name) was added, and the mixture was stirred with a stirrer for approximately one minute to form a rust-preventing film on the surface of the raw powder particles. Pure water was then added, and the container was shaken to mix gently, allowed to stand, and then the supernatant was removed. This process was repeated three times, and the remaining raw powder in the container was collected and dried in a drying oven at 45°C. The dried raw powder was collected and stored in a container together with silica gel. The aluminum powder products of Comparative Examples 1 to 4 were subjected to rust removal treatment and rust prevention treatment to obtain the aluminum powder products of Examples 1 to 4. Specifically, the aluminum powder product of Comparative Example 1 was used as a raw material powder to produce the aluminum powder product of Example 1. The aluminum powder product of Comparative Example 2 was used as a raw material powder to produce the aluminum powder product of Example 2. The aluminum powder product of Comparative Example 3 was used as a raw material powder to produce the aluminum powder product of Example 3. The aluminum alloy powder product of Comparative Example 4 was used as a raw material powder to produce the aluminum alloy powder product of Example 4.

[0051] The volume-based 50% cumulative average particle diameter (D 50 : μm), BET specific surface area (m 2The measurement results of the sphericity (roundness) and Hausner ratio are shown in Table 1 below. The P2p spectrum, P2s spectrum, and Cl2p spectrum of the obtained aluminum powder product were measured using the XPS method. The cross section of the particle was observed using a TEM, and the concentration profile of each element in the depth direction was measured using the EDS method. The phosphorus concentration (mass%) in the entire powder was measured. ○ "Particle Size Distribution Measurement" Using a Microtrac MT3300EXII, particle size distribution was measured using a wet laser diffraction / scattering method. From the obtained results, the 50% cumulative particle size on a volume basis was calculated as the average particle size. ○ "BET Specific Surface Area Measurement" Using an AUTOSORB-iQ2 manufactured by QUANTACHROME, the aluminum powder product was degassed at 200°C for 60 minutes, and then the amount of krypton gas adsorption at 77.35K was measured. The BET specific surface area was calculated from the amount of krypton gas adsorption.

[0052] "Measurement of sphericity (roundness)" Using a dry image measuring instrument Morphologi 4 manufactured by Malvern, 5 mm 3 A volume of aluminum powder product was sprayed onto a glass plate, and images of 20,000 particles were taken using a microscope. Circularity was calculated from the ratio of the circumference of a circle having the same area as the object projected from one particle to the perimeter of the object. The average circularity of the 20,000 particles was then calculated. "Hausner Ratio Measurement" Approximately 15 g of aluminum powder product was weighed and poured into a 20 mL glass graduated cylinder. The volume of the aluminum powder product at that time was measured, and the bulk density was calculated from the volume and the amount poured. In this state, the bottom of the graduated cylinder was tapped 150 times against a table, and the volume of the aluminum powder product at that time was measured. The tapped density was calculated from the volume and the amount poured. The tapped density was divided by the bulk density to obtain the Hausner ratio.

[0053] "Photoelectron Spectroscopy Measurement by XPS" Aluminum powder products were embedded in indium foil and sampled. Using an ULVAC-PHI PHI5000 VersaProbe II, AlKα radiation (50 W output) was used as the X-ray source to measure the P2p spectrum, P2s spectrum, and Cl2p spectrum. "TEM Observation of Particle Cross-Sections and Measurement of Depth Concentration Profiles of Each Element by EDS" Using a Hitachi High-Tech Science SMI3050, FIB processing was performed on the aluminum powder product particles at an accelerating voltage of 30 kV to prepare measurement samples with exposed particle cross-sections. The particle cross-sections were observed using a Thermo Fisher Scientific Titan G2 80-200 transmission electron microscope at an accelerating voltage of 200 kV. The depth concentration profiles of each element were measured using a Bruker Super-X EDS. "Measurement of phosphorus concentration in the entire powder product" The phosphorus concentration in the entire aluminum powder product was measured by the molybdenum blue method as follows. The aluminum powder product was dissolved in an acidic aqueous solution. An aqueous solution of ammonium molybdate was added to the acidic aqueous solution to form a phosphomolybdic acid complex. The phosphomolybdic acid complex was extracted with an organic solvent and reduced with a stannous chloride solution. The absorbance of the solution at a wavelength of 720 nm was then measured, and the phosphorus concentration was calculated from the absorbance.

[0054]

[0055] As shown in Table 1, the aluminum powder products of Examples 1 to 4 had a BET specific surface area of ​​0.16 m 2 / g or more, phosphorus concentration: 1 × 10 -3 Specifically, the BET specific surface area was 0.17 to 0.80 m 2 / g, phosphorus concentration: 3×10 -3 ~7 x 10 -3 The mass %, sphericity: 0.94 to 0.97, and Hausner ratio: 1.09 to 1.23. The BET specific surface area was larger in Example 1 than in Comparative Example 1, larger in Example 2 than in Comparative Example 2, larger in Example 3 than in Comparative Example 3, and larger in Example 4 than in Comparative Example 4. Median diameter D 50With regard to the particle size, Example 1 was slightly smaller than Comparative Example 1, Example 2 was slightly smaller than Comparative Example 2, Example 3 was slightly smaller than Comparative Example 3, and Example 4 was slightly larger than Comparative Example 4. This shows that raw material powder with a particle size suitable for additive manufacturing applications can be produced, and even when the raw material powder is subjected to rust removal and rust prevention treatments, the particle size suitable for additive manufacturing applications can be maintained. Therefore, the aluminum powder products of Examples 1 to 4 are suitable for additive manufacturing.

[0056] Figures 2A to 2H show the concentration profiles of each element in the depth direction measured by energy dispersive X-ray spectroscopy (EDS) in the particle cross-sections of the aluminum powder products of Examples 1 to 4 and Comparative Examples 1 to 4. The EDS spectral intensity of Al rapidly decreases near the particle surface. In Figures 2A to 2H, the minimum point of the EDS spectral intensity of Al is the position of the outermost surface of the particle, which is designated as the zero point on the horizontal axis. The range of the horizontal axis from -30 nm to less than 0 nm represents the outside of the particle. As shown in Figures 2A to 2H, the Al content (EDS spectral intensity of Al) gradually increases with increasing depth from the outermost surface. In Comparative Examples 1 to 4, the Al content was stable at depths greater than 20 nm. In Examples 1 to 4, the Al content was stable at depths greater than 30 nm. In Examples 1 to 4, the region up to a depth of 30 nm where the amount of Al gradually increased on the particle surface was thought to be the region where a coating (anti-rust film) was formed under the influence of the rust remover and rust inhibitor, and the region deeper than 30 nm was thought to be the internal region of the particle body.

[0057] 2A to 2D , it was found that in the aluminum powder products of Examples 1 to 4, a high-phosphorus concentration region was present in a region 30 nm deep from the outermost surface, and the phosphorus concentration in the high-phosphorus concentration region was 3.5 times or more higher than the average phosphorus concentration in the inner region from a depth of more than 30 nm to 60 nm. In contrast, in the aluminum powder products of Comparative Examples 1 to 4 shown in FIGS. 2E to 2H , the presence of a region with a phosphorus concentration 3.5 times or more higher than the phosphorus concentration in the inner region was not confirmed in the region from the outermost surface to a depth of 30 nm or less. For the surface region from the outermost surface to a depth of 30 nm or less and the inner region from a depth of more than 30 nm to 60 nm in Examples 1 to 4 and Comparative Examples 1 to 4, the EDS intensity ratio integral value shown by the following formula (1) was calculated, and the ratio of the EDS intensity ratio integral value of the surface region to the EDS intensity ratio integral value of the inner region (the ratio of the phosphorus concentration in the surface region to the phosphorus concentration in the inner region) was calculated. In the measurement of the concentration profile of each element in the depth direction (line analysis in the depth direction) using EDS, the step width between measurement points was approximately 0.769 nm. Therefore, there were 39 measurement points within a depth length of 30 nm (30 / 0.769=39). The integral value of the EDS intensity ratio in equation (1) is the sum of the phosphorus concentrations (P / (C+N+O+F+Al+Si+P)) at the 39 measurement points. The results are shown in Table 1. The ratio of the phosphorus concentration in the surface region to the phosphorus concentration in the internal region was larger in Examples 1 to 4 than in Comparative Examples 1 to 4, and it was found that in Examples 1 to 4, phosphorus was unevenly distributed in the surface region at a depth of 30 nm or less from the outermost surface. In Comparative Examples 1 to 4, the EDS spectrum intensity of Al rapidly decreased in the surface region at a depth of 30 nm or less from the outermost surface. Therefore, the value of the denominator of the phosphorus concentration (P / (C+N+O+F+Al+Si+P)) suddenly became small. As a result, in Comparative Examples 1 to 4 as well, the EDS intensity ratio integral value of the surface region became larger than the EDS intensity ratio integral value of the inner region.

[0058]

[0059] Figure 3 shows an SEM image of the particle surface of Comparative Example 1, and Figure 4 shows an SEM image of the particle surface of Example 1. Comparing Figure 3 with Figure 4, it can be seen that many fine irregularities were formed on the surface of the powder of Example 1. The presence of these fine surface irregularities is thought to be the cause of the increase in the BET specific surface area of ​​Examples 1 to 4 shown in Table 1.

[0060] Figures 5A to 8B show photoelectron spectra of aluminum powder products measured by X-ray photoelectron spectroscopy (XPS). Figures 5A and 5B show the P2p, P2s, and Cl2p spectra of Example 1 and Comparative Example 1. Figures 6A and 6B show the P2p, P2s, and Cl2p spectra of Example 2 and Comparative Example 2. Figures 7A and 7B show the P2p, P2s, and Cl2p spectra of Example 3 and Comparative Example 3. Figures 8A and 8B show the P2p, P2s, and Cl2p spectra of Example 4 and Comparative Example 4. In the photoelectron spectrum of Comparative Example 1 shown in Figures 5A and 5B, a broad peak is observed in the energy range of the P2p spectrum, but no clear peak is observed in the energy range of the P2s spectrum. From this, it is believed that the peak of Comparative Example 1 shown in Figure 5B is not derived from phosphorus species but is a satellite peak of Al.

[0061] In the photoelectron spectrum of Example 1 shown in Figures 5A and 5B, a clear peak (191.5 eV) is present in the energy range of the P2s spectrum, and therefore the peak observed in the energy range of the P2p spectrum is also likely to be contributed by phosphorus species. From the positions of the P2s and P2p peaks shown in Figures 5A and 5B, it can be inferred that phosphorus is present in the near-surface region not as an elemental or alloy species but as a phosphate-based compound (phosphorus oxoacid). A similar trend was observed for the P2s and P2p peaks in the photoelectron spectra of Examples 2 to 4 shown in Figures 6A to 8B. In the photoelectron spectra shown in Figures 5A to 8B, the detected intensity (counts) of the baseline (background) was approximately 1,000 to 3,000. The detected intensity (counts) of the peak tops of the P2s and P2p peaks was approximately +400 from the baseline. Therefore, the detected intensities (counts) of the P2s, P2p, and Cl2p peaks were not significantly different from the detected intensity (counts) of the baseline. Therefore, the P2s peak intensity I P2s and Cl2p peak intensity I Cl2p Relative to I P2s / I Cl2p As shown in Table 1, the value was around 1.

[0062] Analysis of the results of Figures 2A to 2H and Figures 5A to 8B revealed the following: (1) The aluminum powder products of Examples 1 to 4 had a high phosphorus concentration region in a region 30 nm or less deep from the outermost surface. (2) The phosphorus concentration in the high phosphorus concentration region was 3.5 times or more higher than the phosphorus concentration in the internal region 30 nm to 60 nm deep from the outermost surface. (3) Phosphate-based compounds were unevenly distributed in the high phosphorus concentration region. For example, the measurement result of Figure 2A revealed that in Example 1, the high phosphorus concentration region was present in a region 30 nm or less deep from the outermost surface of the particle. Furthermore, in Examples 1 to 4, the P2s peak intensity I of 191.5 eV P2s and the Cl2p peak intensity at 199.0 eV I Cl2p Relative to I P2s / I Cl2p In contrast, the ratio I of Comparative Examples 1 to 4 P2s / ICl2p was less than 1.00. In detail, the I values ​​of Examples 1 to 4 in Table 1 P2s / I Cl2p In contrast, the I of Comparative Examples 1 to 4 P2s / I Cl2p was 0.943 to 0.976.

[0063] The aluminum powder product of this embodiment is suitably used as a material powder for metal additive manufacturing.

[0064] 1...aluminum powder product, 2...particle body, 2a...high concentration region

Claims

1. The BET specific surface area of ​​the powder product is 0.16 m 2 / g or more, and the phosphorus concentration of the whole powder product measured by the molybdenum blue method is 1×10 -3 % by mass or more, and in the photoelectron spectrum of the powder product measured by X-ray photoelectron spectroscopy (XPS method), the P2s peak intensity I at 191.5 eV P2s and Cl2p peak intensity at 199.0 eV I Cl2p Comparison with I P2s / I Cl2p An aluminum powder product, characterized in that 2. The aluminum powder product according to claim 1, wherein the powder product has a high phosphorus concentration region in a region 30 nm or less deep from the outermost surface of the particles, the phosphorus concentration in the high phosphorus concentration region is 3.5 times or more higher than the phosphorus concentration in a region more than 30 nm deep from the outermost surface of the particles, and phosphate compounds are unevenly distributed in the high phosphorus concentration region.

3. The volume-based 50% cumulative particle diameter (median diameter D 50 3. The aluminum powder product according to claim 1, wherein the diameter of the powder product is 15 μm or more and 45 μm or less, and the powder product has a Hausner ratio of 1.14 or less.

4. An aluminum powder product according to claim 1 or 2, characterized in that the sphericity measured by image analysis is 0.93 or more.

5. The aluminum powder product according to claim 3, characterized in that the sphericity measured by image analysis is 0.93 or more.

6. An aluminum powder product according to claim 1 or 2, characterized in that it is used for additive manufacturing.

7. The aluminum powder product according to claim 3, characterized in that it is used for additive manufacturing.

8. The aluminum powder product according to claim 4, characterized in that it is used for additive manufacturing.

9. The aluminum powder product according to claim 5, characterized in that it is used for additive manufacturing.

Citation Information

Patent Citations

  • Metal powder material

    JP2019112699A

  • Metal powder material, and production method of metal powder material

    JP2019183199A

  • Measuring device

    JP2023055049A

  • Conductive aluminum filler, conductive paste composition including the same, and conductive film formed using the conductive paste composition

    JP2012072441A

  • Powder material, method for producing three-dimensional molded article, and three-dimensional molding device

    WO2016185966A1