Glass

The glass composition with specific oxide ratios addresses the deterioration issues of conventional glass by enhancing electron beam resistance and mechanical strength, improving solar cell performance and durability in space applications.

WO2024203958A1PCT designated stage expired Publication Date: 2024-10-03AGC INC

Patent Information

Application Number
PCT/JP2024/011493
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-09-06
Filing Date
2024-03-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional glass used in solar cell cover glasses deteriorates when exposed to ultraviolet rays, electron beams, and cosmic rays, leading to decreased transmission properties and reduced strength, making it difficult to enhance power generation efficiency while maintaining resistance and mechanical integrity.

Method used

A glass composition with specific ranges of CeO2, SiO2, Al2O3, and Fe2O3 is developed, optimizing electron beam resistance, ultraviolet shielding, and mechanical strength, allowing for larger glass sizes suitable for solar cell applications.

Benefits of technology

The glass exhibits superior electron beam resistance, enhanced ultraviolet shielding, and improved strength, enabling increased solar cell power generation efficiency and durability in space applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-M000001
    Figure JPOXMLDOC01-APPB-M000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

The purpose of the present invention is to provide glass which is superior in electron beam resistance and ultraviolet-shielding effect to conventional ones and has excellent strength. The present invention relates to glass comprising, in terms of oxide amount in percent by mass, 0.4-10% CeO2, 45-85% SiO2, and 0-25% Al2O3, and more specifically relates to cover glass for solar cells, ultraviolet cut glass, electron-beam cut glass, an optical lens for cosmic space or other optical members for cosmic space, and so on.
Need to check novelty before this filing date? Find Prior Art

Description

Glass

[0001] The present invention relates to glass, and more particularly to glass suitable for use as cover glass for solar cells, ultraviolet-blocking glass, electron-beam-blocking glass, optical lenses for space use, and other optical components for space use.

[0002] Glass tends to deteriorate and its transmission characteristics deteriorate with respect to ultraviolet rays, electron beams, proton beams, and cosmic rays (γ-rays, α-rays). Therefore, for example, glass used as a cover glass for solar cells in space applications is required to transmit the spectral sensitivity wavelength range of the solar cell, block ultraviolet rays, electron beams, proton beams, and cosmic rays, and not have its transmission characteristics deteriorated by these rays. For example, Patent Document 1 discloses CeO as a component that absorbs ultraviolet rays. 2 A glass comprising:

[0003] Japanese Patent Application Publication No. 2006-264994

[0004] In solar cell cover glass, it is desirable to improve the transmittance in the wavelength range of 300 to 1100 nm in order to increase the power generation efficiency of the solar cell. On the other hand, since ultraviolet rays lead to deterioration of the resin and the solar cell, it is necessary to design the glass in terms of electron beam resistance, ultraviolet resistance, and light transmission to obtain a sufficient ultraviolet blocking effect. However, as in the glass described in Patent Document 1, 2 When glass contains this compound, it can block UV light with a wavelength up to 340 nm, but there is a problem in that it is difficult to block light with a longer wavelength.

[0005] Furthermore, a new characteristic required of solar cell cover glass is the ability to increase the size of solar cells, but increasing the size of the glass brings with it the problem of reduced strength.

[0006] Therefore, an object of the present invention is to provide glass that is superior to conventional glass in electron beam resistance and ultraviolet ray shielding effect, and also has excellent strength.

[0007] The present inventors have found that the above problems can be solved by setting the composition of glass within a specific range, and have completed the present invention. That is, the present invention is as follows.

[0008] 1. Mass percentage based on oxide: CeO 2 0.3 to 10% of SiO 2 45 to 85% Al 2 O 3 2. Glass containing 0 to 25% of CeO, expressed as a mass percentage based on oxides. 2 2.0 to 10% of SiO 2 45 to 85% Al 2 O 3 3. The glass according to 1 above, containing 0 to 7% of Al, expressed as a mass percentage based on oxides. 2 O 3 4. The glass according to 1 above, containing 7.0 to 25% of Fe, expressed as a mass percentage based on oxides. 2 O 3 5. The glass according to any one of 1 to 3 above, containing 0.3 to 3.0% of CeO, expressed as a mass percentage based on oxides. 2 6. The glass according to any one of 1 to 3 above, wherein the content of B is 6.0% or more, expressed as a mass percentage based on oxides. 2 O 3 6. The glass according to any one of 1 to 3 above, containing 10% or less of Na. 2 O.K. 2 O and Li 2 Contains at least one of Na and O, expressed as a mass percentage based on oxides. 2 O.K. 2 O and Li 2 Total O content R 2 7. The glass according to any one of 1 to 3 above, wherein O is 7 to 25%. 8. The glass according to any one of 1 to 3 above, wherein BaO is substantially not contained. 9. The glass according to any one of 1 to 3 above, wherein the content of NiO is 0.08% or less, expressed as a mass percentage based on oxides. 10. The glass according to any one of 1 to 3 above, wherein the content of TiO is 0.08% or less, expressed as a mass percentage based on oxides. 2 11. The glass according to any one of 1 to 3 above, containing 0 to 0.8% of TiO, expressed as a mass percentage based on oxides. 212. The glass according to any one of 1 to 3 above, which has a thickness of 0.2 mm or less. 13. The glass according to any one of 1 to 3 above, which has a principal surface in the shape of a rectangle with one side of 50 cm or more and 300 cm or less. 14. The glass according to any one of 1 to 3 above, which has an energy of 1 MeV and a viscosity of 1×10 15 pieces / cm 2 15. The glass according to any one of 1 to 3 above, having an average visible light transmittance of 80% or more after irradiation with an electron beam of 150 to 350°C. -7 ~100 x 10 -7 / °C. 16. The glass according to any one of 1 to 3 above, which is chemically strengthenable. 17. The glass according to any one of 1 to 3 above, which is a cover glass for a solar cell. 18. The glass according to any one of 1 to 3 above, which is glass for blocking electron beams. 19. The glass according to any one of 1 to 3 above, which is glass for blocking ultraviolet rays.

[0009] The glass of the present invention has a specific composition, which makes it superior to conventional glasses in terms of electron beam resistance and ultraviolet light shielding effect, and also has excellent strength and can be made large. These properties make the glass of the present invention suitable as a cover glass for solar cells.

[0010] The present invention will be described in detail below, but the present invention is not limited to the following embodiments and can be practiced with any modifications within the scope of the present invention. In this specification, the term "to" indicating a numerical range is used to mean that the numerical values ​​before and after it are included as the lower limit and upper limit, and unless otherwise specified, "to" is used in the following description with the same meaning.

[0011] In this specification, "substantially free" means that the glass is not contained except as unavoidable impurities mixed in from raw materials, etc. In other words, it means that the glass is not intentionally contained. Specifically, it means that the content in the glass composition is less than 0.1 mass%.

[0012] <Glass> <<Composition>> The glass of the present embodiment contains, in terms of mass percentage based on oxides, CeO 20.3 to 10%, SiO 2 45 to 85%, Al 2 O 3 The composition of the glass of the present invention will be described below using the contents expressed as mass percentages unless otherwise specified.

[0013] As one embodiment of the present invention, CeO 2 2.0 to 10% of SiO 2 45 to 85%, Al 2 O 3 (hereinafter, such an embodiment will be referred to as "glass X"). a ").

[0014] In another embodiment of the present invention, CeO 2 0.4 to 10%, SiO 2 45 to 85%, Al 2 O 3 is 7 to 25% (hereinafter, such an embodiment is referred to as "glass X"). b ").

[0015] In another embodiment of the present invention, CeO 2 0.3 to 10%, SiO 2 45 to 85%, Al 2 O 3 is 2.0 to 10% (hereinafter, such an embodiment will be referred to as "glass X"). c ").

[0016] CeO 2 is an essential component that improves the ultraviolet ray shielding effect and suppresses coloration due to electron beams. 2 The content of CeO is 0.3% or more, preferably 0.4% or more, more preferably 0.6% or more, further preferably 0.8% or more, and particularly preferably 1.0% or more, 1.2% or more, 1.5% or more, 2.0% or more, 3.0% or more, 4.0% or more, 5.0% or more, 6.0% or more, and 7.0% or more, in the following order. 2 The content of CeO is 10.0% or less, preferably 9.5% or less, more preferably 9.0% or less, even more preferably 8.5% or less, still more preferably 8.0% or less, and particularly preferably 7.5% or less.2 By making the content of CeO 0.4% or more, the coloring of the glass by electron beams and the ultraviolet ray shielding effect can be sufficiently ensured. 2 When the content of CeO is 6.0% or more, the ultraviolet ray blocking effect for wavelengths having a transmittance of 2% can be further improved. 2 By setting the content of to 10.0% or less, devitrification can be suppressed. b In the 2 The content is preferably 9.0% or less, more preferably 8.0% or less, even more preferably 7.0% or less, particularly preferably 5.0% or less, and most preferably 3.0% or less.

[0017] SiO 2 is an essential component that forms the glass skeleton. 2 The content of SiO is 45% or more, preferably 48% or more, more preferably 50% or more, even more preferably 55% or more, and particularly preferably 60% or more. 2 The content of SiO is 85% or less, preferably 80% or less, more preferably 75% or less, even more preferably 73% or less, and particularly preferably 70% or less. 2 By making the content of SiO 45% or more, chemical durability can be improved. 2 By making the content of T 85% or less, 2 or T 4 This can suppress an increase in the melting point of the glass and improve the melting property or formability of the glass.

[0018] Al 2 O 3 is a component that improves the mechanical properties of the glass, such as Young's modulus and fracture toughness, and improves the ion exchange performance and weather resistance. 2 O 3 When Al is contained, it is preferably 1.0% or more, more preferably 2.0% or more, further preferably 4.0% or more, and particularly preferably 5.0% or more, 5.5% or more, 6.0% or more, 6.5% or more, 7.0% or more, 7.5% or more, 8.0% or more, 9.0% or more in the following order. 2 O 3The content of Al is 25% or less, more preferably 24% or less, even more preferably 23% or less, and particularly preferably 22% or less, 20% or less, 18% or less, 17% or less, 15% or less, 13% or less, 11% or less, and 10% or less, in that order. 2 O 3 By setting the value to 25% or less, T 2 or T 4 This can suppress an increase in the meltability or formability of the glass. 2 When added together with Glass X, it is also a component that worsens devitrification. a In the above, Al 2 O 3 By keeping the content of SiO2 in the range of 0 to 7%, the strength required for larger glass sizes can be further improved. a In the above, Al 2 O 3 When glass X is contained, its content is preferably 7% or less, more preferably 5% or less, further preferably 4% or less, and particularly preferably 3% or less and 2% or less, in that order. a In the above, Al 2 O 3 When glass X contains glass X, its content is preferably 0.5% or more, more preferably 1.0% or more, and even more preferably 1.5% or more. b In the above, Al 2 O 3 By setting the content of Glass X to 7.0 to 25%, the chemical strengthening properties can be further improved. C In the above, Al 2 O 3 By setting the content to 2.0 to 10%, the chemical strengthening properties can be further improved.

[0019] SiO 2 and Al 2 O 3 The total content of (SiO 2 +Al 2 O 3 ) is preferably 65% ​​or more, more preferably 67% or more, even more preferably 70% or more, and particularly preferably 72% or more. 2 +Al 2 O3 When the (SiO ) is 65% or more, the strength can be further improved. 2 +Al 2 O 3 ) is preferably 85% or less, more preferably 80% or less, and even more preferably 75% or less. a In (SiO 2 +Al 2 O 3 ) is preferably 68% or more and 75% or less, more preferably 70% or more and 74% or less, and even more preferably 71% or more and 73% or less. b In (SiO 2 +Al 2 O 3 ) is preferably 65% ​​or more and 80% or less, more preferably 70% or more and 78% or less, and even more preferably 72% or more and 77% or less. C In (SiO 2 +Al 2 O 3 ) is preferably 68% or more and 75% or less, more preferably 70% or more and 74% or less, and even more preferably 71% or more and 73% or less.

[0020] CeO 2、 SiO 2 and Al 2 O 3 The total content of (CeO 2 +SiO 2 +Al 2 O 3 ) is preferably 71% or more, more preferably 72% or more, even more preferably 73% or more, and particularly preferably 74% or more, from the viewpoint of increasing the devitrification viscosity while maintaining the ultraviolet ray shielding property. 2 +SiO 2 +Al 2 O 3 ) is preferably 87% or less, more preferably 82% or less, even more preferably 80% or less, and particularly preferably 77% or less, from the viewpoint of improving the melting characteristics from the glass batch to vitrification.

[0021] Fe2 O 3 is an optional component, but is preferably contained from the viewpoint of enhancing the ultraviolet ray shielding effect and suppressing coloration due to electron beams. 2 O 3 When Fe is contained, its content is preferably 0.01% or more, more preferably 0.05% or more, 0.1% or more, 0.2% or more, 0.3% or more, further preferably 0.5% or more, further more preferably 0.7% or more, and particularly preferably 0.8% or more. 2 O 3 The content of Fe is preferably 3.0% or less, more preferably 2.0% or less, even more preferably 1.5% or less, particularly preferably 1.0% or less, and most preferably 0.85% or less. 2 O 3 By setting the content of Fe to 0.3% or more, it is possible to sufficiently ensure the ultraviolet ray blocking effect and further suppress coloring due to electron beams. 2 O 3 By making the content 3.0% or less, the visible light transmittance can be made to exceed 87%.

[0022] In one embodiment of the present invention, CeO 2 2.0 to 10% of SiO 2 45 to 85%, Al 2 O 3 When glass contains 0 to 7% of a ), from the viewpoint of achieving both ultraviolet shielding properties and mechanical properties, CeO 2 , Al 2 O 3 , Fe 2 O 3 The total content of (CeO 2 +Al 2 O 3 +Fe 2 O 3 ) is preferably 3.0% or more, more preferably 3.5% or more, even more preferably 4.0% or more, and particularly preferably 4.5% or more. a ) in order to lower the devitrification temperature, (CeO 2 +Al 2 O 3 +Fe2 O 3 ) is preferably 10% or less, more preferably 9% or less, even more preferably 8% or less, and particularly preferably 7% or less.

[0023] In another embodiment of the present invention, CeO 2 0.4 to 10%, SiO 2 45 to 85%, Al 2 O 3 When glass contains 7 to 25% of b ), from the viewpoint of achieving both ultraviolet shielding properties and mechanical properties, CeO 2 , Al 2 O 3 , Fe 2 O 3 The total content of (CeO 2 +Al 2 O 3 +Fe 2 O 3 ) is preferably 10% or more, more preferably 12% or more, even more preferably 13% or more, particularly preferably 14% or more, and most preferably 15% or more. b ) in order to lower the devitrification temperature, (CeO 2 +Al 2 O 3 +Fe 2 O 3 ) is preferably 22% or less, more preferably 20% or less, even more preferably 18% or less, and particularly preferably 16% or less.

[0024] In another embodiment of the present invention, CeO 2 0.3 to 10%, SiO 2 45 to 85%, Al 2 O 3 When glass contains 2.0 to 10% of c ), from the viewpoint of achieving both ultraviolet shielding properties and mechanical properties, CeO 2 , Al 2 O 3 , Fe 2 O 3 The total content of (CeO 2 +Al 2 O 3 +Fe2 O 3 ) is preferably 5.0% or more, more preferably 5.5% or more, even more preferably 6.0% or more, particularly preferably 6.5% or more, and most preferably 7.0% or more. c ) in order to lower the devitrification temperature, (CeO 2 +Al 2 O 3 +Fe 2 O 3 ) is preferably 11.0% or less, more preferably 10.0% or less, even more preferably 9.0% or less, and particularly preferably 8.0% or less.

[0025] In one embodiment of the present invention, CeO 2 2.0 to 10% of SiO 2 45 to 85%, Al 2 O 3 When glass contains 0 to 7% of a From the viewpoint of achieving both ultraviolet shielding properties and mechanical properties, the value of X represented by the following formula 1 is preferably 2 or more, more preferably 3 or more, even more preferably 4 or more, and particularly preferably 6 or more. a In order to lower the devitrification temperature, the value of X represented by the following formula 1 is preferably 10 or less, more preferably 9 or less, even more preferably 8 or less, and particularly preferably 7 or less. (Formula 1) X=[CeO 2 ]+1 / 2×[Al 2 O 3 ]+[Fe 2 O 3 In the formula 1, the brackets [ ] indicate the content expressed as a mass percentage based on the oxide.

[0026] In another embodiment of the present invention, CeO 2 0.4 to 10%, SiO 2 45 to 85%, Al 2 O 3 When glass contains 7 to 25% of bFrom the viewpoint of achieving both ultraviolet shielding properties and mechanical properties, the value of X represented by the formula 1 is preferably 5 or more, more preferably 6 or more, even more preferably 7 or more, particularly preferably 8 or more, and most preferably 9 or more. b In the above, from the viewpoint of lowering the devitrification temperature, the value of X represented by the following formula 1 is preferably 13 or less, more preferably 12 or less, even more preferably 11 or less, and particularly preferably 10 or less.

[0027] In another embodiment of the present invention, CeO 2 0.3 to 10%, SiO 2 45 to 85%, Al 2 O 3 When glass contains 2.0 to 10% of c From the viewpoint of achieving both ultraviolet shielding properties and mechanical properties, the value of X represented by the formula 1 is preferably 3.0 or more, more preferably 3.5 or more, even more preferably 4.0 or more, and particularly preferably 4.5 or more. c In the above, from the viewpoint of lowering the devitrification temperature, the value of X represented by the following formula 1 is preferably 8.0 or less, more preferably 7.0 or less, even more preferably 6.0 or less, and particularly preferably 5.0 or less.

[0028] B 2 O 3 may be contained in order to improve the melting property at high temperatures or the strength of the glass. 2 O 3 If the content of B is large, the Young's modulus decreases, the fracture toughness decreases, and the strength tends to decrease. In addition, the acid resistance of the glass may deteriorate, the glass may be prone to phase separation, the transparency may be lost, and it may become difficult to obtain a homogeneous glass, which may decrease the formability of the glass. 2 O 3 Even when it contains, the content is preferably 10% or less, more preferably 8% or less, even more preferably 6% or less, particularly preferably 5% or less, 4% or less, 3% or less, 2% or less, 1% or less, 0.5%, in the following order, and most preferably 0%.

[0029] Na 2 O is an optional component that forms a surface compressive stress layer by ion exchange or improves the meltability of the glass, and may be contained. 2 When O is contained, the content thereof is preferably 5.0% or more, more preferably 7.0% or more, further preferably 8.0% or more, and particularly preferably 9.0% or more, 9.5% or more, 10.0% or more, 10.5% or more, 11.0% or more, and 11.5% or more, in the following order. 2 The O content is preferably 20.0% or less, more preferably 19.0% or less, 18.0% or less, 17.0% or less, even more preferably 16.5% or less, still more preferably 16.0% or less, particularly preferably 15.8% or less, and most preferably 15.5% or less. 2 By making the O content 5.0% or more, it is easy to form a desired surface compressive stress layer by ion exchange. 2 By setting the O content to 20.0% or less, it is possible to suppress a decrease in weather resistance or a decrease in strength.

[0030] K 2 O is an optional component that is not essential but increases the ion exchange rate. 2 When O is contained, the content is preferably 0.1% or more, more preferably 1% or more, even more preferably 3% or more, and particularly preferably 5% or more. 2 The O content is preferably 8.0% or less, more preferably 7.0% or less, even more preferably 6.5% or less, still more preferably 6.0% or less, particularly preferably 5.0% or less, and most preferably 4.0% or more. 2 By setting the O content to 8.0% or less, it is possible to suppress a decrease in strength.

[0031] In the glass according to this embodiment, Na 2 O and K 2 The total content of O (Na 2 O+K 2O) is preferably 22% or less, more preferably 21% or less, even more preferably 20% or less, particularly preferably 19% or less, and most preferably 18% or less. 2 O+K 2 O) is preferably 13% or more, more preferably 14% or more, even more preferably 15% or more, particularly preferably 15.5% or more, and most preferably 16% or more. 2 O+K 2 By making the content of SiO2 22% or less, it is possible to suppress a decrease in weather resistance or a decrease in strength.

[0032] Li 2 O is an optional component that improves the Young's modulus and fracture toughness of the glass, improves the mechanical properties, and also forms surface compressive stress by ion exchange. 2 When O is contained, the content thereof is preferably 0.1% or more, more preferably 3% or more, further preferably 5% or more, and particularly preferably 7% or more. 2 By setting the O content to 20% or less, a decrease in the strain point is suppressed, and stress relaxation is suppressed, making it easier to obtain a stable surface compressive stress layer, and also making it possible to suppress a significant decrease in the acid resistance of the glass.

[0033] In the glass according to this embodiment, from the viewpoint of improving chemical strengthening properties, Na 2 O.K. 2 O and Li 2 It may contain at least one of Na and O. 2 O.K. 2 O and Li 2 When at least one of O is contained, the total content R 2 The O content is preferably 7% or more, more preferably 8% or more, even more preferably 9% or more, particularly preferably 10% or more, and most preferably 13% or more. 2 By making the O content 7% or more, it is possible to reduce the viscosity of the glass to a level that allows continuous production. 2O is preferably 25% or less, more preferably 22% or less, further preferably 20% or less, and particularly preferably 18% or less. 2 When the O content is 25% or less, sufficient weather resistance is obtained.

[0034] MgO is a component that may reduce the ion exchange rate, but is an optional component that suppresses a decrease in strength or improves melting property. When MgO is contained, its content is preferably 3.5% or more, more preferably 4.0% or more, even more preferably 5.0% or more, and particularly preferably 6.0% or more. The MgO content is preferably 13.0% or less, more preferably 12.5% ​​or less, even more preferably 12.0% or less, and particularly preferably 11.5% or less, 11.0% or less, 10.5% or less, 10.0% or less, 9.5% or less, 9.0% or less, 8.5% or less, 8.0% or less, 7.5% or less, and 7.0% or less, in that order.

[0035] Na 2 The total content of O and MgO (Na 2 O+MgO) is preferably 15.0% or more, more preferably 16.0% or more, even more preferably 17.0% or more, particularly preferably 17.5% or more, and most preferably 18.0% or more. 2 O+MgO) is preferably 25% or less, more preferably 24% or less, even more preferably 22% or less, and particularly preferably 21% or less. 2 O + MgO) is 15.0% or more, 2 or T 4 The increase in the amount of Na is suppressed, and the meltability or formability of the glass is improved. 2 By making the content of MgO (O+MgO) 25% or less, it is possible to suppress a decrease in strength.

[0036] BaO may be contained to improve melting property at high temperatures or to make devitrification less likely to occur, but it is preferable that BaO is not substantially contained because it may decrease the ion exchange rate. When BaO is contained, its content is preferably 1.0% or less, more preferably 0.5% or less, and even more preferably 0.1% or less.

[0037] CaO and SrO may be contained to improve melting property at high temperatures or to make devitrification less likely to occur, but it is preferable that they are not substantially contained because there is a risk of a decrease in the ion exchange rate. When CaO is contained, its content is preferably 8% or less, more preferably 6% or less, even more preferably 4% or less, and particularly preferably 2% or less.

[0038] SrO may be contained to improve melting property at high temperatures or to make devitrification less likely to occur, but it is preferable that it is not substantially contained because there is a risk of a decrease in the ion exchange rate. When SrO is contained, its content is preferably 1.0% or less, more preferably 0.5% or less, and even more preferably 0.1% or less.

[0039] When one or more of BaO, CaO and SrO are contained, the total content of these three components is preferably 1.0% or less, and more preferably 0.5% or less.

[0040] From the viewpoint of increasing the transmittance in the wavelength range of 300 to 1100 nm and improving the power generation efficiency of the solar cell, it is preferable that NiO is substantially not contained. If NiO is contained, the content is preferably 1.0% or less, more preferably 0.5% or less, even more preferably 0.1% or less, and particularly preferably 0.08% or less.

[0041] TiO 2 may be contained because it has an excellent effect of suppressing solarization caused by UVC. From the viewpoint of suppressing solarization caused by UVC and preventing coloring of glass, TiO 2 When TiO is contained, its content is preferably 1.5% or less, more preferably 1.0% or less, 0.9% or less, 0.8% or less, 0.75% or less, 0.7% or less, 0.6% or less, 0.5% or less, 0.1% or less, still more preferably 0.05% or less, and still more preferably 0.01% or less. 2 is preferably 0.001% or more.

[0042] ZrO 2is not an essential component, but may be contained in an amount of 5.0% or less in order to reduce viscosity at high temperatures or increase surface compressive stress. 2 By making the content of 5.0% or less, it is possible to suppress a decrease in strength. It is preferably 5.0% or less, more preferably 4.0% or less, 3.0% or less, 2.0% or less, 1.5% or less, 1.4% or less, further preferably 1.3% or less, and particularly preferably 1.1% or less.

[0043] ZnO may be contained to improve the meltability of the glass at high temperatures, but in that case, the content is preferably 1.0% or less, more preferably 0.5% or less, and even more preferably 0.25% or less. When produced by the float process, the ZnO content is preferably 0.5% or less, more preferably 0.25% or less, and even more preferably substantially no ZnO is contained, and most preferably 0%. By keeping the ZnO content at 0.5% or less, reduction during float forming can be suppressed, and the occurrence of product defects can be prevented.

[0044] V 2 O 5 may be contained in order to improve the ultraviolet ray shielding effect. 2 O 5 When V is contained, its content is preferably 0.01% or more, more preferably 0.05% or more, even more preferably 0.1% or more, and particularly preferably 0.2% or more. 2 O 5 When it is contained, the content is preferably 1.0% or less, more preferably 0.8% or less, further preferably 0.6% or less, and particularly preferably 0.4% or less.

[0045] SO 4 is used as a fining agent when melting glass. 3 However, in order to improve the power generation efficiency of solar cells when used as a cover glass for solar cells, Cr, which has absorption in the wavelength range of 300 to 1100 nm, may be contained. 2 O 3It is preferable to reduce the amount of such components that are mixed in as impurities in the raw materials as much as possible, and if they are contained, it is preferable that the amount is 0.15% or less, more preferably 0.1% or less, and particularly preferably 0.05% or less.

[0046] Specific examples of the composition of the glass according to this embodiment include the following: (1) CeO, expressed as a mass percentage based on oxides 2 0.4 to 10.0%, SiO 2 45 to 85%, Al 2 O 3 7.0 to 25%, Fe 2 O 3 The content of 0.1 to 2%, MgO 0 to 10.0%, Na 2 O is 0 to 20.0%, K is 2 O is 0 to 8.0%, B 2 O 3 When it contains ZrO, its content is 10% or less. 2 When TiO is contained, its content is 5.0% or less. 2 (2) Glass containing CeO, expressed as a mass percentage based on oxides, in which the content is 1.5% or less, and in which CaO is contained, the content is 3% or less. 2 2.0 to 10.0%, SiO 2 45 to 85%, Al 2 O 3 0 to 7%, Fe 2 O 3 The content of 0 to 1.0%, MgO 0 to 10.0%, Na 2 O is 0 to 20.0%, K is 2 O is 0 to 4.0%, B 2 O 3 When it contains ZrO, its content is 10% or less. 2 When TiO is contained, its content is 2% or less. 2 (3) Glass containing CeO, if present, in a mass percentage based on oxides, in which the content is 0.1% or less, and in which CaO, if present, in a mass percentage based on oxides, in which the content is 10.0% or less. 2 0.4 to 2.0%, SiO 2 45 to 85%, Al 2 O 3 0 to 7%, Fe2 O 3 The content of 0.5 to 2.0%, MgO 0 to 10.0%, Na 2 O is 0 to 20.0%, K is 2 O is 0 to 4.0%, B 2 O 3 When it contains ZrO, its content is 10% or less. 2 When TiO is contained, its content is 2.0% or less. 2 (4) Glass containing CeO, if present, in a mass percentage based on oxides, in which the content is 0.1% or less, and in which CaO, if present, in a mass percentage based on oxides, in which the content is 10% or less. 2 2.0 to 10.0%, SiO 2 45 to 85%, Al 2 O 3 6.0 to 15%, Fe 2 O 3 The content of 0.1 to 1.8%, MgO 0 to 10.0%, Na 2 O is 0 to 20.0%, K is 2 O is 0 to 5.0%, B 2 O 3 When it contains ZrO, its content is 10% or less. 2 When TiO is contained, its content is 3.0% or less. 2 If it contains CaO, the content thereof is 1.0% or less, and if it contains CaO, the content thereof is 6% or less.

[0047] <<Other Properties>> The glass of this embodiment preferably has a thickness of 0.2 mm or less, more preferably 0.15 mm or less, and particularly preferably 0.1 mm or less. In particular, for space applications, the thickness is preferably 0.2 mm or less from the viewpoint of weight reduction. There is no particular lower limit on the thickness, but from the viewpoint of ensuring strength and sufficient shielding against electron beams and proton beams, it is preferably 0.03 mm or more, more preferably 0.05 mm or more, or 0.07 mm or more.

[0048] The shape of the glass of the present embodiment is not particularly limited, but is typically preferably a rectangular plate or sheet. The size of satellite (space) cover glasses used to date has generally been about 10 cm per side. From the perspective of increasing size, the length of one side of the rectangular main surface is preferably 20 cm or more, 30 cm or more, 40 cm or more, and 50 cm or more, in the following order: more preferably 70 cm or more, 80 cm or more, and 90 cm or more, even more preferably 100 cm or more, 120 cm or more, and particularly preferably 150 cm or more. By having the specific composition range described above, the glass of the present embodiment can ensure strength even when increased in size. Furthermore, from the perspective of handling thin glass without breaking, the length of one side of the rectangular main surface is typically preferably 400 cm or less, 350 cm or less, more preferably 300 cm or less, even more preferably 250 cm or less, and particularly preferably 200 cm or less.

[0049] The glass of this embodiment preferably has an average transmittance of 89% or more in the wavelength range of 380 to 780 nm, more preferably 90% or more, even more preferably 90.5% or more, and particularly preferably 91% or more. By having an average transmittance of 89% or more in the wavelength range of 380 to 780 nm, when used as a cover glass for a solar cell, the power generation characteristics of the solar cell can be further improved.

[0050] In the glass of this embodiment, the wavelength at which the transmittance becomes 2% is preferably 270 nm or more, more preferably 270 nm or more, 290 nm or more, 310 nm or more, 330 nm or more, and 350 nm or more, in the following order. The wavelength at which the transmittance becomes 2% is preferably 400 nm or less, more preferably 390 nm or less, even more preferably 380 nm or less, and particularly preferably 370 nm or less. By having the wavelength at which the transmittance becomes 2% be 270 nm or more, the ultraviolet blocking effect can be further enhanced. Furthermore, by having the wavelength at which the transmittance becomes 2% be 400 nm or less, when used as a cover glass for a solar cell, the spectral sensitivity of the solar cell can be improved, and power generation efficiency can be increased.

[0051] The glass of this embodiment has an energy dose of 1 MeV of 1×10 for a glass having a thickness of 0.1 mm. 15 pieces / cm 2 The average visible light transmittance after irradiation with an electron beam is preferably 70% or more, more preferably 80% or more, more preferably 83% or more, even more preferably 85% or more, and particularly preferably 88% or more. When the average visible light transmittance is particularly 80% or more, degradation of solar cell characteristics due to electron beams can be effectively suppressed, for example, in space applications. There is no particular upper limit for the average visible light transmittance, but considering that there is essentially glass for shielding electron beams, it is usually preferably 93% or less.

[0052] The glass of this embodiment absorbs ultraviolet light with a wavelength of 254 nm at a rate of 22,500 mJ / cm 2 The average visible light transmittance after irradiation is preferably 80% or more, more preferably 83% or more, even more preferably 85% or more, and particularly preferably 88% or more. 2 By ensuring that the average visible light transmittance after irradiation is 80% or more, deterioration of the resin fixing the solar cell due to UV can be effectively suppressed, particularly when the glass is used as a cover glass for a solar cell. There is no particular upper limit to the average visible light transmittance after UV irradiation, but considering that the glass is substantially used for shielding electron beams, it is usually preferably 93% or less.

[0053] The glass of this embodiment has an average thermal expansion coefficient of 10×10 at 50 to 350° C. from the viewpoint of improving adhesion to resin and thermal shock resistance. -7 / °C or more, and more preferably, in the following order: 20 × 10 -7 / ℃ or more, 30 x 10 -7 / ℃ or more, 40 x 10 -7 / ℃ or more, 50 × 10 -7 / ℃ or more, 60 x 10 -7 / °C or more, more preferably 65 x 10 -7 / °C or more, particularly preferably 70 x 10 -7 / °C or more. The average thermal expansion coefficient at 50 to 350°C is 100 x 10 -7 / °C or less, and more preferably 90 × 10 -7 / °C or less, more preferably 80 x 10 -7 / °C or less, particularly preferably 75 x 10 -7 / °C or less.

[0054] The glass of this embodiment has an average thermal expansion coefficient of 20×10 at 50 to 350° C., particularly from the viewpoint of improving adhesion to resin. -7 / °C or more, and more preferably 30 × 10 -7 / °C or more, more preferably 40 x 10 -7 / °C or more, particularly preferably 50 x 10 -7 / °C or more. In particular, from the viewpoint of improving the adhesiveness to resin, the average thermal expansion coefficient at 50 to 350°C is 100 x 10 -7 / °C or less, and more preferably 80 × 10 -7 / °C or less, more preferably 70 x 10 -7 / °C or less, particularly preferably 60 x 10 -7 / °C or less.

[0055] Average thermal expansion coefficient between 50 and 350°C is 20 x 10 -7 / °C or more, the thermal shock resistance can be improved. -7 / °C or more, the average thermal expansion coefficient can be adapted to the thermal expansion properties of the resin used in the solar cell, and the solar cell characteristics can be improved. -7 / °C or less, it is possible to match the thermal expansion property of the resin used in the solar cell, and improve the solar cell characteristics.

[0056] In particular, from the viewpoint of improving thermal shock resistance, the glass of this embodiment has an average thermal expansion coefficient of 10×10 at 50 to 350° C. -7 / ℃ or more 40 x 10 -7 / °C or less, and more preferably 15 × 10 -7 / ℃ or more 35 x 10 -7 / °C or less, more preferably 20 x 10 -7 / ℃ or more 30 x 10 -7 / °C or less. The average thermal expansion coefficient at 50 to 350°C is 10 x 10-7 By keeping the temperature in this range at or above 100°C, it is possible to improve the thermal shock resistance in particular, suppress the deterioration of the glass in space applications, and improve the power generation characteristics of solar cells.

[0057] The glass of the present embodiment is preferably chemically strengthenable. In this specification, "chemically strengthenable" means that a surface compressive stress layer is formed by chemical strengthening treatment.

[0058] The surface compressive stress and compressive stress layer depth obtained by chemical strengthening depend on the thickness of the glass, but here we will discuss the surface compressive stress and compressive stress layer depth obtained when a glass with a thickness of 0.5 mm is chemically strengthened. 3 The surface compressive stress obtained when chemically strengthened using salt at 425 ° C for 6 hours is preferably 500 MPa or more, more preferably 600 MPa or more, 700 MPa or more, 800 MPa or more, 900 MPa or more, and even more preferably 1000 MPa or more, in the following order. Furthermore, the depth of the compressive stress layer obtained when chemically strengthened under these conditions is preferably 5 μm or more, more preferably 10 μm or more, and even more preferably 20 μm or more, 30 μm or more, and particularly preferably 40 μm or more, in the following order. By having a surface compressive stress of 600 MPa or more when chemically strengthened under these conditions, strength can be sufficiently ensured even when the glass is made large (specifically, for example, when the length of one side is 50 cm or more).

[0059] From the viewpoint of improving productivity, when float molding is adopted as the molding method, the glass of this embodiment preferably has a devitrification viscosity η of log η = 3 [dPa s] or more, more preferably log η = 3.5 [dPa s] or more, even more preferably log η = 4 [dPa s] or more, and particularly preferably log η = 5 [dPa s] or more. The devitrification viscosity η is the viscosity value at the devitrification temperature. There is no particular upper limit to the devitrification viscosity, but it is usually preferably log η = 2 [dPa s] or less.

[0060] The glass of this embodiment has an acid resistance of 0.3 mg / cm calculated by the following method.2 It is preferably 0.2 mg / cm or less, and more preferably 0.2 mg / cm 2 or less, and more preferably 0.1 mg / cm 2 and even more preferably 0.05 mg / cm or less. 2 or less, and particularly preferably 0.04 mg / cm 2 or less, most preferably 0.01 mg / cm 2 Evaluation method for acid resistance: A glass sample was prepared as a rectangular glass plate with sides of 40±0.5 mm and a thickness of 0.4 to 1.0 mm, and immersed in an acid aqueous solution (aqueous solution containing 0.1 mol / L HCl at 90°C) for 20 hours, and the amount of eluted glass components per unit surface area (mg / cm 2 ) is calculated as acid resistance.

[0061] The glass of the present embodiment has a temperature (T 2 ) is preferably 1650°C or less, more preferably 1600°C or less, and even more preferably 1550°C or less. 2 is usually 1400°C or higher.

[0062] The glass of the present embodiment has a temperature (T 4 ) is preferably 1300°C or less, more preferably 1250°C or less, further preferably 1200°C or less, 1150°C or less, 1100°C or less, and most preferably 1050°C or less. 4 is usually 800°C or higher.

[0063] In the glass of this embodiment, five 50 mm x 50 mm pieces of glass are cut from a piece of glass measuring 50 cm or more, starting from the center and five pieces near each of the four corners. The average flatness (Ra) of each 1 μm x 1 μm measured with an AFM is preferably 2.0 nm or less, more preferably 1.5 nm or less, even more preferably 1.0 nm or less, and even more preferably 0.8 nm or less. Having a flatness of 2.0 nm or less provides strength that makes the glass less likely to break during handling. A certain degree of roughness in the flatness can reduce static electricity between the glass and the interleaf paper sandwiched between the glass pieces during handling, so the lower limit of the average value is preferably 0.2 nm or more, more preferably 0.3 nm or more, even more preferably 0.4 nm or more, and even more preferably 0.5 nm or more.

[0064] From the viewpoint of increasing fracture toughness and improving strength, the glass of this embodiment preferably has a Young's modulus of 60 GPa or more, more preferably 70 GPa or more, even more preferably 75 GPa or more, and particularly preferably 80 GPa or more. On the other hand, from the viewpoint of suppressing a decrease in ion diffusion during chemical strengthening, the Young's modulus is preferably 105 GPa or less, more preferably 100 GPa or less, even more preferably 95 GPa or less, and particularly preferably 90 GPa or less. The Young's modulus can be measured, for example, by an ultrasonic pulse method.

[0065] The glass of this embodiment preferably has a specific gravity of 2.3 or more, more preferably 2.4 or more, and even more preferably 2.5 or more. A specific gravity of 2.3 or more effectively shields electron beams and proton beams, and can suppress deterioration of solar cells, particularly when used as a cover glass for solar cells. Furthermore, from the viewpoint of weight reduction, the specific gravity is preferably 3 or less, more preferably 2.8 or less, and even more preferably 2.6 or less. The specific gravity is measured by the Archimedes method.

[0066] <Production Method> The glass of this embodiment can be produced by a conventional method. For example, the raw materials for the glass components are blended and heated and melted in a glass melting furnace. The glass is then homogenized by a known method, formed into a desired shape such as a glass plate, and slowly cooled.

[0067] Examples of glass sheet forming methods include the float method, press method, fusion method, and down-draw method. In particular, the float method, which is suitable for mass production, is preferred. Continuous forming methods other than the float method, i.e., the fusion method and down-draw method, are also preferred.

[0068] The molded glass is then subjected to grinding, polishing, and etching to form a glass substrate. The thickness of the glass substrate can be adjusted to a desired thickness by adjusting the conditions of the treatments. Specific examples of etching include a method in which the glass substrate is immersed in a solution containing hydrofluoric acid or the like to etch the glass surface, thereby polishing the glass surface.

[0069] The glass substrate may be subjected to a chemical strengthening treatment described later. When the glass substrate is cut to a predetermined shape and size or chamfered, it is preferable to perform the cutting or chamfering of the glass substrate before performing the chemical strengthening treatment described later, because a compressive stress layer is also formed on the end surface by the subsequent chemical strengthening treatment.

[0070] Chemical strengthening is a process in which glass is brought into contact with a metal salt (e.g., potassium nitrate) by immersion in a melt of a metal salt containing metal ions with a large ionic radius (typically Na ions or K ions), thereby replacing metal ions with a small ionic radius (typically Na ions or Li ions) in the glass with metal ions with a large ionic radius (typically Na ions or K ions for Li ions, and K ions for Na ions).

[0071] To increase the speed of chemical strengthening, it is preferable to use "Li-Na exchange," in which Li ions in the glass are exchanged with Na ions. Also, to create a large compressive stress by ion exchange, it is preferable to use "Na-K exchange," in which Na ions in the glass are exchanged with K ions.

[0072] Examples of molten salts used in chemical strengthening include nitrates, sulfates, carbonates, and chlorides. Nitrates include lithium nitrate, sodium nitrate, potassium nitrate, cesium nitrate, and silver nitrate. Sulfates include lithium sulfate, sodium sulfate, potassium sulfate, cesium sulfate, and silver sulfate. Carbonates include lithium carbonate, sodium carbonate, and potassium carbonate. Chlorides include lithium chloride, sodium chloride, potassium chloride, cesium chloride, and silver chloride. These molten salts may be used alone or in combination.

[0073] The conditions for the chemical strengthening treatment can be selected, such as time and temperature, taking into account the glass composition and the type of molten salt. For example, a chemical strengthening treatment is preferably performed at 450°C or less for 1 hour or less. Specifically, for example, a treatment is performed in which the glass is immersed in a molten salt (e.g., a mixed salt of lithium nitrate and sodium nitrate) containing 0.3% by mass of Li and 99.7% by mass of Na at 450°C for about 0.5 hours.

[0074] The chemical strengthening treatment may involve two or more stages of ion exchange. Specifically, the two-stage ion exchange is carried out, for example, as follows: First, the glass for chemical strengthening is immersed in a metal salt (e.g., sodium nitrate) containing Na ions at a temperature of preferably about 350 to 500°C for preferably about 0.1 to 10 hours. This causes ion exchange between the Li ions in the glass for chemical strengthening and the Na ions in the metal salt, forming a relatively deep compressive stress layer.

[0075] <Uses> The glass of this embodiment is suitable for use as cover glass for solar cells, glass for blocking electron beams, glass for blocking ultraviolet rays, optical lenses for space use, and other optical components for space use. The glass of this embodiment is superior to conventional glasses in terms of electron beam resistance and ultraviolet ray shielding effect, and also has excellent strength and can be made large, making it particularly suitable for use as cover glass for solar cells, optical lenses for space use, and other optical components for space use, which require these properties.

[0076] As described above, the present specification discloses the following: 1. In terms of mass percentage based on oxides, CeO 2 0.3 to 10% of SiO 2 45 to 85% Al 2 O 3 2. Glass containing 0 to 25% of CeO, expressed as a mass percentage based on oxides. 2 2.0 to 10% of SiO 2 45 to 85% Al 2 O 3 3. The glass according to 1 above, containing 0 to 7% of Al, expressed as a mass percentage based on oxides. 2 O 3 4. The glass according to 1 above, containing 7.0 to 25% of Fe, expressed as a mass percentage based on oxides. 2 O 3 5. The glass according to any one of 1 to 3 above, containing 0.3 to 3.0% of CeO, expressed as a mass percentage based on oxides. 2 5. The glass according to any one of 1 to 4 above, wherein the content of B is 6.0% or more, expressed as a mass percentage based on oxides. 2 O 3 6. The glass according to any one of 1 to 5 above, containing 10% or less of Na. 2 O.K. 2 O and Li 2 Contains at least one of Na and O, expressed as a mass percentage based on oxides. 2 O.K. 2 O and Li 2 Total O content R 2 7. The glass according to any one of 1 to 6 above, containing 7 to 25% O. 8. The glass according to any one of 1 to 7 above, which is substantially free of BaO. 9. The glass according to any one of 1 to 8 above, which has a NiO content of 0.08% or less, expressed as a mass percentage based on oxides. 10. The glass according to any one of 1 to 8 above, which has a TiO content of 0.08% or less, expressed as a mass percentage based on oxides. 2 11. The glass according to any one of 1 to 9 above, containing 0 to 0.8% of TiO, expressed as a mass percentage based on oxides. 211. The glass according to any one of 1 to 10 above, containing 0 to 0.1% of. 12. The glass according to any one of 1 to 11 above, having a thickness of 0.2 mm or less. 13. The glass according to any one of 1 to 12 above, having a principal surface in the shape of a rectangle with one side of 50 cm or more and 300 cm or less. 14. The glass according to any one of 1 to 12 above, containing 0 to 0.1% of 15 pieces / cm 2 14. The glass according to any one of 1 to 13 above, having an average visible light transmittance of 80% or more after irradiation with an electron beam of 1000 kJ / cm2 or less. -7 ~100 x 10 -7 / °C. 16. The glass according to any one of 1 to 15 above, which is chemically strengthenable. 17. The glass according to any one of 1 to 16 above, which is a cover glass for solar cells. 18. The glass according to any one of 1 to 17 above, which is glass for blocking electron beams. 19. The glass according to any one of 1 to 18 above, which is glass for blocking ultraviolet rays.

[0077] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples.

[0078] (Glass Production) Commonly used glass raw materials such as oxides, hydroxides, carbonates, or nitrates were appropriately selected to obtain the glass compositions shown in Tables 1 to 17, expressed in mass percentage or mole percentage based on oxides, placed in a platinum crucible, and melted by heating to a high temperature of 1550 to 1650°C or higher in an electric furnace. The molten glass was then poured onto a carbon mold and held at Tg + 50°C for 30 minutes, after which it was cooled at a rate of 1.0°C / min to obtain glass blocks. The obtained glass blocks were cut, ground, and polished to obtain glass substrates measuring 50 mm long x 50 mm wide x 0.1 mm thick and 50 mm long x 50 mm wide x 0.5 mm thick.

[0079] (Preparation of chemically strengthened glass) Subsequently, the obtained glass substrate having a thickness of 0.5 mm was subjected to a chemical strengthening treatment using 100% by mass of potassium nitrate at 425 ° C. for 6 hours to obtain a chemically strengthened glass substrate. The glass substrate was subjected to evaluation of chemical strengthening characteristics, and the surface compressive stress (CS) and the depth of the compressive stress layer (DOL) were measured.

[0080] (Evaluation of Properties) The properties of the obtained glass substrates and chemically strengthened glass substrates were evaluated by the following procedures.

[0081] [Transmittance] The transmittance was measured using a spectrophotometer (product name U-4100) manufactured by Hitachi High-Tech Corporation. (Transmittance after UV irradiation) UVA irradiation was performed by placing the glass substrate to be irradiated horizontally on a table and irradiating it with light from a high-pressure mercury lamp (manufactured by Oak Manufacturing Co., Ltd., model number: QRU-2161-DYB) from a position 15 cm above the glass substrate for 10 minutes. The cumulative light dose was 24.6 J / cm. 2 After irradiation, the transmittance of each glass substrate was measured. The average illuminance at the location where the glass substrate was placed was 41 mW / cm at a wavelength of 365 nm. 2 The UVC irradiation was performed by placing the glass substrate to be irradiated horizontally on a table and irradiating it with light from a low-pressure mercury lamp (a tabletop surface treatment device manufactured by Sen Special Light Sources Co., Ltd. (Model: SSP16-110, dominant wavelengths: 185 nm and 254 nm) from a position 50 cm above the glass substrate for 15 minutes. The cumulative light intensity was 27.9 J / cm. 2 After irradiation, the transmittance of each glass substrate was measured. The average illuminance at the location where the glass substrate was placed was 31 mW / cm at a wavelength of 254 nm. 2 (measured using an illuminance meter UV-M08-25 manufactured by Oak Manufacturing Co., Ltd.).

[0082] (Transmittance after electron beam irradiation) For electron beam irradiation, a glass substrate to be irradiated was placed horizontally on a table, and an electron beam was irradiated onto the glass substrate at an energy dose of 1 MeV at a rate of 1×10 using an electron beam irradiation device (manufactured by NHV Corporation, model number: EPS-3000 kV). 15 pieces / cm 2The transmittance of each glass substrate after electron beam irradiation was measured. The measurement was carried out within one week.

[0083] [Average thermal expansion coefficient] Measured using a differential thermal dilatometer in accordance with the method specified in JIS R3102 (1995). The measurement temperature range was 50 to 350°C, and the unit was ×10 -7 The temperature was expressed as / °C.

[0084] [Stress Profile (CS, DOL)] The stress value of the chemically strengthened glass substrate obtained above was measured using an optical waveguide surface stress meter FSM-6000 manufactured by Orihara Manufacturing Co., Ltd.

[0085] [T 2 (Temperature at which the logarithm of viscosity η (dPa s) becomes 2) T 2 The viscosity was measured using a rotational high-temperature viscometer according to the method specified in ASTM C 965-96 (2017), and 2 The viscosity was determined as the temperature at which the viscosity reached dPa·s. NBS710 and NIST717a were used as reference samples for calibrating the device.

[0086] [Devitrification Temperature] The devitrification temperature was measured by placing a glass on a platinum dish, putting it into an electric furnace, and holding it at 1300°C for 1 hour, then holding it at a predetermined temperature for 17 hours. The sample was then removed from the electric furnace and cooled. After the temperature had dropped to room temperature, the occurrence of devitrification was confirmed using a microscope. The test was repeated at 10°C intervals for each temperature held for 17 hours, and the highest temperature at which devitrification was confirmed was determined as the devitrification temperature of the glass.

[0087] [Devitrification viscosity] The devitrification viscosity is [T 2 Using the rotary high-temperature viscometer described above in the section above, viscosity was measured while decreasing the temperature from 1700°C to 1000°C (or until the viscosity began to increase rapidly due to devitrification) at a rate of 10°C / min, and the viscosity value at the devitrification temperature was taken as the devitrification viscosity log η.

[0088] [Chemical durability] (Acid resistance) A glass plate having a square shape with sides of 40±0.5 mm and a thickness of 0.4 to 1.0 mm was prepared. The glass sample was immersed in an acid aqueous solution (aqueous solution containing 0.1 mol / L HCl at 90°C) for 20 hours, and the amount of eluted glass components per unit surface area (mg / cm 2 The weight before immersion was measured. Before , the weight after immersion After When the length and width of the glass sample are represented as length, width, and thickness, respectively, the amount of eluted glass components per unit surface area was calculated by the following formula.

[0089]

[0090] [Specific Gravity] The specific gravity was measured by the Archimedes method.

[0091] [Young's Modulus] Young's modulus was measured by the ultrasonic pulse method (JIS R1602, 1995).

[0092] Tables 1 to 10 show the glass compositions and evaluation results of their properties expressed in mass percentages based on oxides. Tables 11 to 17 show the glass compositions shown in Tables 1 to 10 in mole percentages based on oxides.

[0093] In Tables 1 to 17, Examples A-1 to A-20, B-1 to B-8, B-11 to B-14, C-1 to C-7, C-12 to C-23, and D-1 to D-5 are working examples, and A-21, A-22, B-9, B-10, B-15 to B-20, and C-8 to C-11 are comparative examples. In Tables 1 to 10, "-" indicates that the results were not evaluated.

[0094] When considering the transmittance at 0.1 mm from the transmittance at 0.5 mm, the amount of light-absorbing elements can be considered to be 1 / 5 according to the Beer-Lambert law.

[0095]

[0096]

[0097]

[0098]

[0099]

[0100]

[0101]

[0102]

[0103]

[0104]

[0105]

[0106]

[0107]

[0108]

[0109]

[0110]

[0111]

[0112] As shown in Tables 1 to 3, Examples A-1 to A-20, which are working examples, have a larger wavelength (@0.1 mm) at which a transmittance of 2% is exhibited than Example A-22, which is a comparative example, and CeO 2 It was found that an excellent ultraviolet shielding effect can be obtained by including the compound in the range of 0.4 to 10%.

[0113] Comparative Example A-21 is CeO 2 By not containing CeO, the wavelength (@0.1 mm) showing a transmittance of 2% was low, at less than 210 nm, and the average visible light transmittance (@0.1 mm and @0.5 mm) after electron beam irradiation was lower than that before irradiation. 2 It was found that the inclusion of the compound effectively blocks ultraviolet rays and also suppresses coloration caused by electron beam irradiation.

[0114] Furthermore, in Examples A-19 and A-20, the wavelength at which the transmittance was 2% was higher, at 310 nm or more, compared to Example A-10. 2 In addition to Fe 2 O3 It has been found that the ultraviolet ray shielding effect can be further improved by including

[0115] As shown in Tables 4 to 6, Examples B-1, B-2, and B-14, which are working examples, have wavelengths (@0.1 mm and @0.5 mm) at which a transmittance of 2% is exhibited that are larger than Examples B-16 to B-20, which are comparative examples, and CeO 2 It was found that an excellent ultraviolet shielding effect can be obtained by including CeO in the range of 0.4 to 10%. 2 In addition to Fe 2 O 3 It has been found that the ultraviolet ray blocking effect can be enhanced by including

[0116] As shown in Tables 7 to 10, Examples C-1 to C-7 and C-12 to C-23, which are working examples, have a larger wavelength (@0.1 mm) at which a transmittance of 2% is exhibited than Examples C-10 to C-11, which are comparative examples, and CeO 2 It was found that by containing the above, an excellent ultraviolet shielding effect can be obtained.

[0117] Furthermore, Examples C-6 and C-7, which are working examples, showed comparable average visible light transmittance (@0.5 mm) after electron beam irradiation, without any decrease, compared to Comparative Examples C-10 and C-11. Furthermore, Comparative Examples C-10 and C-11 showed a significant decrease in average visible light transmittance (@0.5 mm) after electron beam irradiation, compared to Examples C-6 and C-7. From these results, it can be seen that CeO 2 It was found that the inclusion of the compound effectively blocks ultraviolet rays and suppresses coloration caused by electron beam irradiation.

[0118] As shown in Table 9, Examples D-1 to D-3 are examples containing 100% by mass of KNO 3 The surface compressive stress was 600 MPa or more when chemically strengthened using salt at 425°C for 6 hours. This result shows that the glass of the present embodiment can be chemically strengthened and can sufficiently ensure strength even when enlarged.

[0119] Although various embodiments have been described above, it goes without saying that the present invention is not limited to such examples. It is clear that a person skilled in the art can conceive of various modifications or alterations within the scope of the claims, and it is understood that these also naturally fall within the technical scope of the present invention. Furthermore, the components of the above embodiments may be combined in any manner as long as they do not deviate from the spirit of the invention.

[0120] This application is based on a Japanese patent application filed on March 29, 2023 (Patent Application No. 2023-054194) and a Japanese patent application filed on September 6, 2023 (Patent Application No. 2023-144621), the contents of which are incorporated by reference into this application.

Claims

1. Mass percentage based on oxide: CeO 2 0.3 to 10% SiO 2 45 to 85% Al 2 O 3 Glass containing 0 to 25%.

2. Mass percentage based on oxide: CeO 2 2.0 to 10% SiO 2 45 to 85% Al 2 O 3 The glass according to claim 1, containing 0 to 7%.

3. Mass percentage based on oxide: Al 2 O 3 The glass according to claim 1, containing 7.0 to 25%.

4. Mass percentage based on oxide: Fe 2 O 3 The glass according to any one of claims 1 to 3, containing 0.3 to 3.0% of 5. Mass percentage based on oxide: CeO 2 The glass according to any one of claims 1 to 3, wherein the content of is 6.0% or more.

6. Mass percentage based on oxides: B 2 O 3 The glass according to any one of claims 1 to 3, containing 10% or less of 7. Na 2 O.K. 2 O and Li 2 Contains at least one of Na and O, expressed as a mass percentage based on the oxide. 2 O.K. 2 O and Li 2 Total O content R 2 The glass according to any one of claims 1 to 3, wherein O is 7 to 25%.

8. The glass according to any one of claims 1 to 3, which is substantially free of BaO.

9. The glass according to any one of claims 1 to 3, wherein the content of NiO is 0.08% or less, expressed as a mass percentage based on oxides.

10. In terms of mass percentage based on oxide, TiO 2The glass according to any one of claims 1 to 3, containing 0 to 0.8%.

11. In terms of mass percentage based on oxide, TiO 2 The glass according to any one of claims 1 to 3, containing 0 to 0.1%.

12. The glass according to any one of claims 1 to 3, having a thickness of 0.2 mm or less.

13. The glass according to any one of claims 1 to 3, wherein one side of the main surface is a rectangle having a length of 50 cm or more and 300 cm or less.

14. 1 x 10 at 1 MeV of energy 15 pieces / cm 2 4. The glass according to claim 1, wherein the average visible light transmittance after irradiation with an electron beam is 80% or more.

15. The average thermal expansion coefficient at 50 to 350°C is 20 x 10 -7 ~100 x 10 -7 The glass according to any one of claims 1 to 3, wherein the temperature is 0.15°C.

16. The glass according to any one of claims 1 to 3, which is chemically strengthenable.

17. The glass according to any one of claims 1 to 3, which is a cover glass for a solar cell.

18. The glass according to any one of claims 1 to 3, which is an electron beam blocking glass.

19. The glass according to any one of claims 1 to 3, which is an ultraviolet ray blocking glass.

Citation Information

Patent Citations

  • Infrared light absorbing green glass composition

    JP2006264994A

  • Bofutsushosan extract

    JP2023054194A

  • Illuminating device

    JP2023144621A

  • Components of flexible base glass for spaceflight

    CN103833223A

  • Borosilicate glass composition and same for solar battery protection cover

    JP1988095138A

Cited By

  • Glass sheet

    WO2026216324A1

  • Glass plate

    WO2026216325A1