Separator for power storage devices, and power storage device
The development of a multilayer microporous membrane separator for lithium-ion batteries addresses the need for high transparency, strength, and safety by optimizing molecular weight distribution and porosity, achieving effective battery performance and safety.
Patent Information
- Application Number
- PCT/JP2024/011678
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-08-09
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-03
AI Technical Summary
There is a demand for lithium-ion battery separators that offer high transparency, high puncture strength, and high withstand voltage to ensure safety and performance, particularly in applications requiring high energy capacity and energy density.
A separator for power storage devices is developed using a microporous membrane with a multilayer structure, primarily composed of polypropylene, where one layer has a higher melt tension and smaller pore diameter, and the other layer has a lower melt tension and larger pore diameter, with specific molecular weight distribution and porosity to achieve both strength and permeability.
The separator achieves high safety and performance by simultaneously providing high puncture strength, withstand voltage, and permeability, maintaining battery performance even at high temperatures, and preventing dendrite growth.
Smart Images

Figure JPOXMLDOC01-APPB-M000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Separator for power storage device and power storage device
[0001] The present disclosure relates to a separator for an electricity storage device.
[0002] Microporous membranes, particularly polyolefin-based microporous membranes, are used in many technical fields, such as microfiltration membranes, battery separators, capacitor separators, and fuel cell materials, and are particularly used as separators for power storage devices, such as lithium secondary batteries and lithium ion secondary batteries. Lithium ion batteries are used in a variety of applications, including small electronic devices such as mobile phones and notebook personal computers, as well as electric vehicles, including hybrid vehicles and plug-in hybrid vehicles.
[0003] In recent years, there has been a demand for lithium-ion batteries with high energy capacity, high energy density, and high output characteristics, and this has led to an increasing demand for thin-film separators that offer excellent battery performance, reliability, and safety.
[0004] For example, US Patent No. 6,299,999 describes a multilayer microporous thin film or membrane that can improve properties including dielectric breakdown and strength. A preferred multilayer microporous membrane comprises a microlayer and one or more stacked barriers.
[0005] Cited Document 2 describes a separator for an electricity storage device having a microporous membrane that is mainly composed of polyolefin and has a melt tension of 30 mN or less when measured at 230° C. from the viewpoint of membrane strength and thinning, and a melt flow rate (MFR) of 0.9 g / 10 min or less when measured under a load of 2.16 kg at 230° C. In addition, Patent Document 3 describes providing a peritoneal membrane film with few impurities from a cellulose raw material, and using the film as a separator to reduce the size and increase the capacity of an electrolytic capacitor.
[0006] International Publication No. WO 2018 / 089748 International Publication No. WO 2020 / 196120 International Publication No. WO 2013 / 069146
[0007] In view of the above background art, the present disclosure aims to provide a separator for an electricity storage device that can simultaneously achieve high permeability required for use in an electricity storage device, as well as high puncture strength and high withstand voltage to achieve high safety.
[0008] Examples of embodiments of the present disclosure are listed in the following items [1] to
[14] . [1] An electricity storage device separator comprising a microporous layer (A) containing polypropylene as a main component and a microporous layer (B) containing polypropylene as a main component laminated together, or a microporous membrane comprising at least one of the microporous layer (A) and the microporous layer (B), wherein the microporous membrane has a stem height of 500 nm or more and 1,000 nm or less, calculated by analyzing an SEM image of an MD-ND cross section. [2] The electricity storage device separator according to item 1, wherein the microporous layer (A) has an area-average long pore diameter of 100 nm or more and 280 nm or less, calculated by analyzing an SEM image of an MD-ND cross section of the microporous membrane. [3] The separator for an electric storage device according to item 1 or 2, wherein the area average pore diameter of the microporous layer (A) is smaller than the area average pore diameter of the microporous layer (B). [4] The melt tension Mt of the microporous layer (A) at 240°C A
[0014] The separator for an electricity storage device according to any one of items 1 to 3, wherein the microporous membrane has a thickness of 8 μm or more and 20 μm or less.
[0015] The separator for an electricity storage device according to any one of items 1 to 3, wherein the microporous layer (A) has a thickness of 5 μm or less.
[0016] The separator for an electricity storage device according to any one of items 1 to 5, wherein the microporous layer (A) has a molecular weight distribution (Mw / Mn) obtained by dividing the weight average molecular weight (Mw) by the number average molecular weight (Mn) of the polypropylene in the microporous layer (A) is 6.0 or more and 14 or less.
[0017] The separator for an electricity storage device according to any one of items 1 to 6, wherein the microporous layer (A) has a molecular weight distribution (Mw / Mn) obtained by dividing the weight average molecular weight (Mw) by the number average molecular weight (Mn) of the polypropylene in the microporous layer (A). [8] The separator for an electricity storage device according to any one of items 1 to 7, wherein the proportion of components having a molecular weight of 80,000 or less in the polypropylene of the microporous layer (A) is 10% or more and 20% or less, and the proportion of components having a molecular weight of 1,500,000 or more is 10% or more and 20% or less. [9] The separator for an electricity storage device according to any one of items 1 to 8, wherein the microporous layer (B) has a mean flow pore diameter of 20 nm or more and 25 nm or less.
[10] The separator for an electricity storage device according to any one of items 1 to 9, wherein the surface of the microporous layer (B) has an area average pore diameter of 140 nm or more and 300 nm or less.
[11] The separator for an electricity storage device according to any one of items 1 to 10, wherein the microporous membrane has a TD heat shrinkage of 5% or less at 105°C for 1 hour.
[12] The separator for an electric storage device according to any one of items 1 to 11, wherein the microporous membrane has a porosity of 40% or more and 54% or less.
[13] In the microporous membrane, the melt tension Mt A and the melt tension Mt of the microporous layer (B). B
[14] The separator for an electricity storage device according to any one of items 1 to 12, wherein the microporous membrane has an MD tensile strength of 1500 kgf / cm 2 14. The separator for an electricity storage device according to any one of items 1 to 13.
[0009] According to the present disclosure, a separator for an electricity storage device is provided that simultaneously achieves high permeability, high puncture strength for realizing high safety, and high withstand voltage.
[0010] <<Separator for Electricity Storage Device>> The separator for an electricity storage device of the present disclosure has, as a separator substrate, a microporous membrane having a microporous layer (A) primarily composed of a polyolefin and, optionally, a microporous layer (B) primarily composed of a polyolefin. The separator substrate may further have a coating layer (also called a "surface layer," "coating layer," etc.; hereinafter simply referred to as a "coating layer") on the microporous layer (A) and / or the microporous layer (B). In this specification, the term "microporous layer" refers to each microporous layer constituting the separator substrate, the term "separator substrate" refers to the separator substrate excluding any coating layers, and the term "separator" refers to the entire separator including any coating layers.
[0011] The separator for an electric storage device of the present disclosure can have a microporous membrane formed by laminating a microporous layer (A) containing polypropylene as a main component and a microporous layer (B) containing polypropylene as a main component. The separator for an electric storage device of the present disclosure can also have a microporous membrane including at least one of the microporous layer (A) and the microporous layer (B). A single-layer microporous membrane may include the microporous layer (A) or (B), and preferably consists of the microporous layer (A) or (B). In a multilayer microporous membrane, the microporous layers (A) and (B) are laminated, and preferably the microporous layers (A) and (B) are in contact with each other, the microporous layers (A) and (B) are adjacent to each other, or the interface between the microporous layers (A) and (B) can be observed.
[0012] The weight average molecular weight, number average molecular weight, and Mw / Mn of the polyolefin of the present disclosure are molecular weights calculated in terms of polystyrene obtained by GPC (gel permeation chromatography) measurement.
[0013] <Microporous Layer (A)> The separator for an electricity storage device of the present disclosure has a microporous layer (A). The separator for an electricity storage device may have only one microporous layer (A), or two or more microporous layers (A). The microporous layer (A) is primarily composed of polyolefin, more preferably polypropylene and / or polyethylene. This allows for good pore openability and good battery performance. The microporous layer (A) is even more preferably composed of polypropylene. This allows for good battery performance to be maintained even after storage at high temperatures (e.g., 130°C). In this specification, "primarily composed of polypropylene" means that the microporous layer (A) contains 50% by mass or more of polypropylene, based on the total mass of the microporous layer (A). The lower limit of the polypropylene content in the microporous layer (A) is 50% by mass or more, and preferably 55% by mass or more, 60% by mass or more, 70% by mass or more, 80% by mass or more, 90% by mass or more, or 95% by mass or more, from the viewpoints of the wettability, thinning, and shutdown characteristics of the separator, etc. The upper limit of the polypropylene content in the microporous layer (A) is not limited, and may be, for example, 60% by mass or less, 70% by mass or less, 80% by mass or less, 90% by mass or less, 95% by mass or less, 98% by mass or less, or 99% by mass or less, or may be 100% by mass.
[0014] <Material of Microporous Layer (A)> The microporous layer (A) is primarily composed of polyolefin, more preferably polypropylene and / or polyethylene. This allows for good pore opening and good battery performance. The microporous layer (A) is more preferably composed of polypropylene. This allows for good battery performance to be maintained even after storage at high temperatures (e.g., 130°C). The polypropylene of the microporous layer (A) may be the same material as the polypropylene of the microporous layer (B) described below, or may be a polypropylene with a different chemical structure, more specifically, a polypropylene differing in at least one of monomer composition, stereoregularity, molecular weight, and crystalline structure. The stereoregularity of the polypropylene is not limited, and examples include atactic, isotactic, or syndiotactic homopolymers. The polypropylene according to the present disclosure is preferably a highly crystalline isotactic or syndiotactic homopolymer.
[0015] The polypropylene of the microporous layer (A) is preferably a homopolymer, but may also be a copolymer, such as a block polymer, in which a small amount of a comonomer other than propylene, such as an α-olefin comonomer, is copolymerized. The amount of propylene structures contained as repeating units in the polypropylene is not limited, but may be, for example, 70 mol% or more, 80 mol% or more, 90 mol% or more, 95 mol% or more, or 99 mol% or more. The amount of repeating units derived from comonomers other than the propylene structure contained in the polypropylene is not limited, but may be, for example, 30 mol% or less, 20 mol% or less, 10 mol% or less, 5 mol% or less, or 1 mol% or less. The polypropylene can be used alone or in combination of two or more types.
[0016] The weight-average molecular weight (Mw) of the polypropylene of the microporous layer (A) is preferably 300,000 or more from the viewpoints of the strength of the microporous layer and voltage resistance, and is preferably 1,300,000 or less from the viewpoints of ensuring good film-forming properties and productivity and good air permeability. The Mw of the polypropylene is more preferably 500,000 or more and 1,200,000 or less, even more preferably 650,000 or more and 1,100,000 or less, still more preferably 750,000 or more and 1,000,000 or less, and particularly preferably 800,000 or more and 1,000,000 or less.
[0017] The upper limit of the molecular weight distribution (Mw / Mn), which is the weight-average molecular weight (Mw) of the polypropylene of the microporous layer (A) divided by the number-average molecular weight (Mn), is preferably 14 or less, more preferably 12 or less, 10 or less, or 8 or less. Setting Mw / Mn to 14 or less tends to ensure good film-forming properties and productivity. The lower limit of Mw / Mn is preferably 6.0 or more, more preferably 6.5 or more, and even more preferably 7.0 or more. The larger the Mw / Mn value of the polypropylene, the higher the melt tension of the resulting microporous layer tends to be. Therefore, from the viewpoints of good dendrite suppression and voltage resistance, it is preferable to increase the melt tension of the microporous layer (A). Therefore, a polypropylene Mw / Mn value of 6.0 or more is preferable for controlling the melt tension of the microporous layer (A) to a high level.
[0018] Conventional polypropylenes with a narrow molecular weight distribution (Mw / Mn<6.0) obtained by single-stage polymerization have a sufficient distribution of high molecular weight components but a low distribution of low molecular weight components, making it difficult to achieve good dendrite suppression performance, voltage resistance, and permeability. However, the polypropylene for the microporous layer (A) used in embodiments of the present disclosure is characterized by a wide molecular weight distribution, for example, by multi-stage polymerization. For example, a high molecular weight component and a low molecular weight component can be produced by two-stage polymerization to ultimately produce polypropylene with an Mw / Mn value in the range of 6.0 to 14. The polypropylene for the microporous layer (A) used in embodiments of the present disclosure also has a wide distribution of both high and low molecular weight components, with the low molecular weight component improving pore opening and permeability, and the high molecular weight component controlling the melt tension to a high level to achieve a sufficiently fine pore structure and / or small pore size. Therefore, according to the present invention, good dendrite suppression performance, voltage resistance, and permeability can be achieved simultaneously.
[0019] The upper limit of the proportion of components having a molecular weight of 80,000 or less contained in the polypropylene of the microporous layer (A) is preferably 20% or less, more preferably 18% or less, 16% or less, or 14% or less. Setting the proportion of components having a molecular weight of 80,000 or less to 20% or less is preferred from the viewpoint of strength. Furthermore, the proportion of components having a molecular weight of 80,000 or less contained in the polypropylene of the microporous layer (A) is preferably 10% or more, more preferably 11% or more, and even more preferably 12% or more. The greater the proportion of components having a molecular weight of 80,000 or less contained in the polypropylene, the better the pore opening of the resulting microporous layer, and the more excellent permeability it can exhibit.
[0020] The upper limit of the proportion of components having a molecular weight of 1,500,000 or more contained in the polypropylene of the microporous layer (A) is preferably 20% or less, more preferably 19% or less, 18% or less, or 17% or less. By setting the proportion of components having a molecular weight of 1,500,000 or more to 20% or less, good film-forming properties or productivity tend to be ensured. Furthermore, the proportion of components having a molecular weight of 1,500,000 or more contained in the polypropylene of the microporous layer (A) is preferably 10% or more, more preferably 11% or more, and even more preferably 12% or more. The greater the proportion of components having a molecular weight of 1,500,000 or more contained in the polypropylene, the greater the melt tension of the resulting microporous layer tends to be. Therefore, it is preferable to increase the melt tension of the microporous layer (A) in terms of dendrite suppression and voltage resistance characteristics. Therefore, it is preferable that the proportion of components having a molecular weight of 1,500,000 or more contained in the polypropylene be 10% or more in order to control the melt tension of the microporous layer (A) to a high level.
[0021] The density of the polypropylene of the microporous layer (A) is preferably 0.85 g / cm 3 or more, for example, 0.88 g / cm 3 Above, 0.89g / cm 3 or more, or 0.90 g / cm 3 The density of polypropylene is preferably 1.1 g / cm or more. 3 Below, for example, 1.0 g / cm 3 Below, 0.98g / cm 3 Below, 0.97g / cm 3 Below, 0.96g / cm 3 Below, 0.95g / cm 3 Below, 0.94g / cm 3 Below, 0.93g / cm 3 or less, or 0.92 g / cm 3 The density of polyolefins is related to the crystallinity of polypropylene, and the density of polypropylene can be 0.85 g / cm or less. 3 By setting the above, the productivity of the microporous layer is improved, which is particularly advantageous in the dry method.
[0022] The microporous layer (A) may contain other resins as long as it is primarily composed of polyolefin. Examples of other resins include polyolefins other than polypropylene (also referred to as "other polyolefins") and copolymers of polystyrene and polyolefin. Polyolefins are polymers containing a monomer having a carbon-carbon double bond as a repeating unit. Monomers constituting polyolefins other than polypropylene include, but are not limited to, monomers having 2 or 4 to 10 carbon atoms and a carbon-carbon double bond, such as ethylene, 1-butene, 4-methyl-1-pentene, 1-hexene, and 1-octene. Polyolefins are, for example, homopolymers, copolymers, or multistage polymers, and polyethylene may also be contained. Preferred examples of copolymers of polystyrene and polyolefin include styrene-(ethylene-propylene)-styrene copolymer (SEPS), styrene-(ethylene-butene)-styrene copolymer, and styrene-ethylene-styrene copolymer, with styrene-(ethylene-propylene)-styrene copolymer (SEPS) being particularly preferred.
[0023] <Melt flow rate (MFR) of microporous layer (A)> The upper limit of the melt flow rate (MFR) of the microporous layer (A) (MFR of a single layer) is preferably 4.0 g / 10 min or less, and may be, for example, 3.0 g / 10 min or less, 2.0 g / 10 min or less, 1.5 g / 10 min or less, 1.1 g / 10 min or less, or 0.5 g / 10 min or less, from the viewpoint of obtaining a microporous layer (A) with a higher strength and a small pore size exhibiting good withstand voltage. The lower limit of the MFR of the microporous layer (A) (MFR of a single layer) is not limited from the viewpoint of the formability of the microporous layer (A), and may be, for example, 0.2 g / 10 min or more, 0.25 g / 10 min or more, 0.3 g / 10 min or more, or 0.35 g / 10 min or more. The MFR of the microporous layer (A) is measured under conditions of a load of 2.16 kg and a temperature of 230°C for polypropylene, and under conditions of a load of 2.16 kg and a temperature of 190°C for polyethylene. An MFR of the microporous layer (A) of 4.0 g / 10 min or less means that the molecular weight of the polyolefin contained in the microporous layer (A) is relatively high. A high molecular weight polyolefin tends to increase the number of tie molecules that bond crystalline substances together, which tends to result in a microporous layer (A) with high strength and also makes it possible to impart a sufficiently high melt tension, which tends to facilitate the achievement of a pore structure with small pore diameters that achieves good voltage resistance. An MFR of the microporous layer (A) of 0.2 g / 10 min or more prevents the melt tension of the microporous layer (A) from becoming too high, making it possible to ensure good film-forming properties and productivity. From the viewpoint of obtaining a microporous layer (A) with high strength and high melt tension, the MFR of the polypropylene of the microporous layer (A) is preferably 0.2 to 4.0 g / 10 min when measured under conditions of a load of 2.16 kg and a temperature of 230°C. From the viewpoint of obtaining a microporous layer with even higher strength, the upper limit of the MFR of the polypropylene may be, for example, 4.0 g / 10 min or less, 3.0 g / 10 min or less, 2.0 g / 10 min or less, 1.5 g / 10 min or less, 1.1 g / 10 min or less, or 0.5 g / 10 min or less. The lower limit of the MFR of the polypropylene is not limited, but from the viewpoint of the moldability of the microporous layer (A), it may be, for example, 0.2 g / 10 min or more, 0.25 g / 10 min or more, 0.3 g / 10 min or more, or 0.35 g / 10 min or more.
[0024] <Pentad fraction of microporous layer (A)> From the viewpoint of obtaining a microporous layer with low air permeability, the lower limit of the pentad fraction of the polypropylene of the microporous layer (A) is preferably 94.0% or more, for example, 95.0% or more, 96.0% or more, 96.5% or more, 97.0% or more, 97.5% or more, 98.0% or more, 98.5% or more, or 99.0% or more. The upper limit of the pentad fraction of the polypropylene is not limited, but may be 99.9% or less, 99.8% or less, or 99.5% or less. The pentad fraction of the polypropylene is 13 Measured by C-NMR (nuclear magnetic resonance).
[0025] A pentad fraction of 94.0% or more of polypropylene indicates high crystallinity of the polypropylene. In separators obtained by the stretching method, particularly the dry method, pores are formed by stretching the amorphous portions between crystalline portions. Therefore, if the polypropylene has high crystallinity, the pores become good and the air permeability can be kept low, which enables the battery to have high output.
[0026] <Melt tension of microporous layer (A)> Melt tension Mt of microporous layer (A) at 240°C A The melt tension Mt is preferably 10 mN or more and 35 mN or less. A The lower limit of the melt tension Mt is preferably 10 mN or more, more preferably 13 mN or more, even more preferably 16 mN or more, particularly preferably 20 mN or more, and most preferably 23 mN or more, from the viewpoint of achieving a sufficiently fine pore structure or a small pore diameter and exhibiting good withstand voltage. A The upper limit of the elastic modulus is preferably 35 mN or less, more preferably 32 mN or less, from the viewpoint of good film-forming properties and productivity, and from the viewpoint of obtaining good air permeability.
[0027] <Area-average pore diameter of microporous layer (A)> The area-average pore diameter of the microporous layer (A) in the MD-ND cross section (hereinafter also simply referred to as "area-average pore diameter") is preferably 100 nm or more and 280 nm or less. In this specification, "ND" refers to the thickness direction of the microporous layer, and "MD" refers to the film-forming direction of the microporous layer. For example, the MD of a separator having a microporous layer is the longitudinal direction of a roll. "Long pore diameter" means the pore diameter in the MD. When a microporous membrane or separator has microporous layers with different melt tensions, the microporous layer with the smaller area-average pore diameter is used as the microporous layer (A). By using a microporous layer with a smaller area-average pore diameter as the microporous layer (A), a stronger correlation with voltage resistance can be obtained. When two or more microporous layers (A) and / or two or more microporous layers (B) are present, the area-average pore diameters of the microporous layer (A) and the microporous layer (B) are compared based on the average area-average pore diameter of each layer. From the viewpoint of ensuring good output in the power storage device and obtaining good air permeability, the lower limit of the area-average pore diameter of the microporous layer (A) is preferably 100 nm or more, more preferably 120 nm or more, even more preferably 130 nm or more, and particularly preferably 140 nm or more. From the viewpoint of obtaining good withstand voltage, the upper limit of the area-average pore diameter of the microporous layer (A) is preferably 280 nm or less, more preferably 260 nm or less, even more preferably 240 nm or less, particularly preferably 210 nm or less, and most preferably 190 nm or less.
[0028] The area-average pore diameter can be measured by performing cross-sectional SEM observation of the MD-ND cross section of the separator and analyzing the obtained image. Detailed conditions are shown in the Examples. When measuring the average pore diameter from a cross-sectional SEM image, the number-average pore diameter and the area-average pore diameter can be calculated, but in this specification, the area-average pore diameter is used as the average pore diameter to better correlate with the physical properties of the separator.
[0029] <Porosity of Microporous Layer (A)> The porosity of the microporous layer (A) is preferably 20% or more from the viewpoint of avoiding clogging in the electricity storage device and obtaining good separator air permeability, and is preferably 70% or less from the viewpoint of maintaining separator strength. The porosity of the microporous layer (A) is more preferably 25% or more and 65% or less, even more preferably 30% or more and 60% or less, and particularly preferably 35% or more and 60% or less.
[0030] <Thickness of Microporous Layer (A)> The thickness of the microporous layer (A) is preferably 5 μm or less, more preferably 4.5 μm or less, from the viewpoint of increasing the energy density of the electricity storage device, etc. The lower limit of the thickness of the microporous layer (A) may be preferably 1 μm or more, for example, 2 μm or more, 3 μm or more, or 3.5 μm or more, from the viewpoint of strength, etc.
[0031] <Additives for Microporous Layer (A)> The microporous layer (A) containing polypropylene as a main component may further contain, in addition to polypropylene, additives such as elastomers, crystal nucleating agents, antioxidants, fillers, etc. The amount of the additives is not particularly limited, and may be, for example, 0.01% by mass or more, 0.1% by mass or more, or 1% by mass or more, and 20% by mass or less, 10% by mass or less, or 7% by mass or less, based on the total mass of the microporous layer (A).
[0032] <Microporous Layer (B)> The separator for an electricity storage device of the present disclosure optionally has a microporous layer (B). The separator for an electricity storage device may have only one microporous layer (B), or two or more microporous layers (B). The microporous layer (B) is also primarily composed of polyolefin, more preferably polypropylene and / or polyethylene. This allows for good pore openability and good battery performance. The microporous layer (B) is more preferably primarily composed of polypropylene, which allows for good battery performance to be maintained even after storage at high temperatures (e.g., 130°C). In this specification, the term "primarily composed of" polypropylene means that the microporous layer (B) contains 50% by mass or more of polypropylene, based on the total mass of the microporous layer (B). The lower limit of the polypropylene content in the microporous layer (B) may be preferably 55% by mass or more, 60% by mass or more, 70% by mass or more, 80% by mass or more, 90% by mass or more, or 95% by mass or more from the viewpoint of the wettability of the separator, thinning of the film, etc. The upper limit of the polypropylene content in the microporous layer (B) is not limited, and may be, for example, 60% by mass or less, 70% by mass or less, 80% by mass or less, 90% by mass or less, 95% by mass or less, 98% by mass or less, or 99% by mass or less, or may be 100% by mass.
[0033] <Material of Microporous Layer (B)> The microporous layer (B) is primarily composed of polyolefin, more preferably polypropylene and / or polyethylene. This allows for good pore opening and good battery performance. The microporous layer (B) is more preferably composed of polypropylene. This allows for good battery performance to be maintained even after storage at high temperatures (e.g., 130°C). The polypropylene of the microporous layer (B) may be the same material as the polypropylene of the microporous layer (A), or may be a polypropylene with a different chemical structure, more specifically, a polypropylene differing in at least one of monomer composition, stereoregularity, molecular weight, and crystalline structure. The stereoregularity of the polypropylene of the microporous layer (B) is not limited, and examples include atactic, isotactic, or syndiotactic homopolymers. The polypropylene according to the present disclosure is preferably a highly crystalline isotactic or syndiotactic homopolymer.
[0034] The polypropylene of the microporous layer (B) is preferably a homopolymer, but may also be a copolymer, such as a block polymer, in which a small amount of a comonomer other than propylene, such as an α-olefin comonomer, is copolymerized. The amount of propylene structures contained as repeating units in the polypropylene is not limited, but may be, for example, 70 mol% or more, 80 mol% or more, 90 mol% or more, 95 mol% or more, or 99 mol% or more. The amount of repeating units derived from comonomers other than the propylene structure contained in the polypropylene is not limited, but may be, for example, 30 mol% or less, 20 mol% or less, 10 mol% or less, 5 mol% or less, or 1 mol% or less. The polypropylene may be used alone or in combination of two or more types.
[0035] The weight-average molecular weight (Mw) of the polypropylene of the microporous layer (B) is preferably 250,000 or more from the viewpoints of the strength of the microporous layer and voltage resistance, and is preferably 1,000,000 or less from the viewpoints of increasing the pore size of the microporous layer and achieving good air permeability. The Mw of the polypropylene is more preferably 400,000 or more and 950,000 or less, even more preferably 550,000 or more and 900,000 or less, still more preferably 600,000 or more and 900,000 or less, and particularly preferably 700,000 or more and 900,000 or less.
[0036] The upper limit of the molecular weight distribution (Mw / Mn), which is the weight average molecular weight (Mw) of the polypropylene of the microporous layer (B) divided by the number average molecular weight (Mn), is preferably 7 or less, more preferably 6.5 or less, 6 or less, 5.5 or less, or 5 or less. The smaller the Mw / Mn value of the polypropylene, the lower the melt tension of the resulting microporous layer tends to be. Therefore, it is preferable that the Mw / Mn value of the polypropylene is 7 or less in order to control the melt tension of the microporous layer (B) to a low level. Furthermore, Mw / Mn may be preferably 1 or more, for example, 1.3 or more, 1.5 or more, 2.0 or more, or 2.5 or more. When Mw / Mn is 1 or more, appropriate molecular entanglement is maintained, which may improve stability during film formation.
[0037] The density of the polypropylene of the microporous layer (B) is preferably 0.85 g / cm 3 or more, for example, 0.88 g / cm 3 Above, 0.89g / cm 3 or more, or 0.90 g / cm 3 The density of polypropylene is preferably 1.1 g / cm or more. 3 Below, for example, 1.0 g / cm 3 Below, 0.98g / cm 3 Below, 0.97g / cm 3 Below, 0.96g / cm 3 Below, 0.95g / cm 3 Below, 0.94g / cm 3 Below, 0.93g / cm 3 or less, or 0.92 g / cm 3The density of polyolefins is related to the crystallinity of polypropylene, and the density of polypropylene can be 0.85 g / cm or less. 3 By setting the above, the productivity of the microporous layer is improved, which is particularly advantageous in the dry method.
[0038] The microporous layer (B) may contain other resins as long as it is primarily composed of polyolefin. Examples of other resins include polyolefins other than polypropylene (also referred to as "other polyolefins"). Polyolefins are polymers containing a monomer having a carbon-carbon double bond as a repeating unit. Monomers constituting polyolefins other than polypropylene include, but are not limited to, monomers having 2 or 4 to 10 carbon atoms and a carbon-carbon double bond, such as ethylene, 1-butene, 4-methyl-1-pentene, 1-hexene, and 1-octene.
[0039] The microporous layer (B) may contain a thermoplastic elastomer other than polypropylene. Examples of thermoplastic elastomers include, but are not limited to, polypropylene, polyolefins other than polypropylene (also referred to as "other polyolefins"), and copolymers of polystyrene and polyolefin. Examples of polypropylene include low-crystalline polypropylenes having low stereoregularity regions. Polyolefins are polymers containing a monomer having a carbon-carbon double bond as a repeating unit. Examples of monomers constituting polyolefins other than polypropylene include, but are not limited to, monomers having 2 or 4 to 10 carbon atoms and a carbon-carbon double bond, such as ethylene, 1-butene, 4-methyl-1-pentene, 1-hexene, and 1-octene. Examples of polyolefins include homopolymers, copolymers, and multi-stage polymers. For example, polyethylene may be contained. Preferred examples of copolymers of polystyrene and polyolefin include styrene-(ethylene-propylene)-styrene copolymer (SEPS), styrene-(ethylene-butene)-styrene copolymer (SEBS), hydrogenated styrene-(ethylene-butene)-styrene copolymer (hydrogenated SEBS), styrene-ethylene-styrene copolymer, olefin crystalline-(ethylene-butene)-olefin crystalline copolymer (CEBC), hydrogenated olefin crystalline-(ethylene-butene)-olefin crystalline copolymer (hydrogenated CEBC), styrene-(ethylene-butene)-olefin crystalline copolymer (SEBC), hydrogenated styrene-(ethylene-butene)-olefin crystalline copolymer (hydrogenated SEBC), etc. Particularly preferred are hydrogenated styrene-(ethylene-butene)-styrene copolymer (hydrogenated SEBS), hydrogenated styrene-(ethylene-butene)-olefin crystalline copolymer (hydrogenated SEBC), and styrene-(ethylene-propylene)-styrene copolymer (SEPS).
[0040] The thermoplastic elastomer contained in the microporous layer (B) is preferably an elastomer incompatible with polypropylene from the viewpoints of pore opening and increasing the pore size. The elastomer incompatible with polypropylene is not particularly limited, but preferred examples include copolymers of polyethylene and other polyolefins and copolymers of polystyrene and polyolefins. Preferred examples of the copolymer of polystyrene and polyolefin include styrene-(ethylene-propylene)-styrene copolymer (SEPS), styrene-(ethylene-butene)-styrene copolymer (SEBS), hydrogenated styrene-(ethylene-butene)-styrene copolymer (hydrogenated SEBS), styrene-ethylene-styrene copolymer, olefin crystalline-(ethylene-butene)-olefin crystalline copolymer (CEBC), hydrogenated olefin crystalline-(ethylene-butene)-olefin crystalline copolymer (hydrogenated CEBC), styrene-(ethylene-butene)-olefin crystalline copolymer (SEBC), and hydrogenated styrene-(ethylene-butene)-olefin crystalline copolymer (hydrogenated SEBC). Particularly preferred are hydrogenated styrene-(ethylene-butene)-styrene copolymer (hydrogenated SEBS), hydrogenated styrene-(ethylene-butene)-olefin crystalline copolymer (hydrogenated SEBC), and styrene-(ethylene-propylene)-styrene copolymer (SEPS).
[0041] <Melt flow rate (MFR) of microporous layer (B)> From the viewpoint of obtaining a microporous layer (B) with higher strength, the upper limit of the melt flow rate (MFR) of the microporous layer (B) (MFR of a single layer) is preferably 8.0 g / 10 min or less, and may be, for example, 6.0 g / 10 min or less, 4.0 g / 10 min or less, 3.0 g / 10 min or less, 2.0 g / 10 min or less, or 1.1 g / 10 min or less. From the viewpoint of exhibiting good air permeability, the lower limit of the MFR of the microporous layer (B) (MFR of a single layer) is not limited, and may be, for example, 0.3 g / 10 min or more, 0.35 g / 10 min or more, 0.4 g / 10 min or more, 0.45 g / 10 min or more, or 0.5 g / 10 min or more. The MFR of the microporous layer (B) is measured under conditions of a load of 2.16 kg and a temperature of 230°C in the case of polypropylene, and under conditions of a load of 2.16 kg and a temperature of 190°C in the case of polyethylene.
[0042] An MFR of the microporous layer (B) of 8.0 g / 10 min or less means that the molecular weight of the polyolefin contained in the microporous layer (B) is relatively high. A high molecular weight polyolefin increases the number of tie molecules that bond crystalline substances together, tending to result in a microporous layer (B) with high strength. An MFR of the microporous layer (B) of 0.3 g / 10 min or more prevents the melt tension of the microporous layer (B) from becoming too high, making it easier to obtain a separator that exhibits good air permeability.
[0043] The MFR of the polypropylene of the microporous layer (B) is preferably 8.0 g / 10 min or less, and may be, for example, 6.0 g / 10 min or less, 4.0 g / 10 min or less, 3.0 g / 10 min or less, 2.0 g / 10 min or less, or 1.1 g / 10 min or less, from the viewpoint of obtaining a microporous layer (B) with higher strength. The lower limit of the MFR of the microporous layer (B) (single-layer MFR) is not limited, from the viewpoint of exhibiting good air permeability, and may be, for example, 0.3 g / 10 min or more, 0.35 g / 10 min or more, 0.4 g / 10 min or more, 0.45 g / 10 min or more, or 0.5 g / 10 min or more.
[0044] When the main components of the microporous layer (A) and the microporous layer (B) are both polypropylene, or when the main components of the microporous layer (A) and the microporous layer (B) are both polyethylene, the MFR of the microporous layer (B) is preferably higher than the MFR of the microporous layer (A). By making the MFR of the microporous layer (B) higher than the MFR of the microporous layer (A), the pore size of the microporous layer (B) in the obtained separator can be controlled to be larger than the pore size of the microporous layer (A).
[0045] <Pentad fraction of microporous layer (B)> From the viewpoint of obtaining a microporous layer with low air permeability, the lower limit of the pentad fraction of the polypropylene of the microporous layer (B) is preferably 94.0% or more, for example, 95.0% or more, 96.0% or more, 96.5% or more, 97.0% or more, 97.5% or more, 98.0% or more, 98.5% or more, or 99.0% or more. The upper limit of the pentad fraction of the polypropylene is not limited, but may be 99.9% or less, 99.8% or less, or 99.5% or less. The pentad fraction of the polypropylene is 13Measured by C-NMR (nuclear magnetic resonance).
[0046] A pentad fraction of 94.0% or more of polypropylene indicates high crystallinity of the polypropylene. In separators obtained by the stretching method, particularly the dry method, pores are formed by stretching the amorphous portions between crystalline portions. Therefore, if the polypropylene has high crystallinity, the pores become good and the air permeability can be kept low, which enables the battery to have high output.
[0047] <Melt tension of microporous layer (B)> Melt tension Mt of microporous layer (B) at 240°C B The melt tension Mt is preferably 4 mN or more and 30 mN or less. B From the viewpoint of good film-forming properties and productivity of the separator substrate having the microporous layer (A) and the microporous layer (B), the lower limit of the melt tension Mt is preferably 4 mN or more, more preferably 7 mN or more, even more preferably 10 mN or more, particularly preferably 13 mN or more, and most preferably 16 mN or more. B The upper limit of the melt tension Mt of the microporous layers (A) and (B) at a temperature of 240°C is preferably 30 mN or less, more preferably 28 mN or less, even more preferably 26 mN or less, and most preferably 24 mN or less, from the viewpoint of achieving a large pore diameter and exhibiting good air permeability. A and Mt. B may be different from each other in terms of the area average long pore diameter of the microporous membrane.
[0048] <Area-average pore diameter of microporous layer (B)> The area-average pore diameter (hereinafter also simply referred to as "area-average pore diameter") in the MD-ND cross section of the microporous layer (B) is larger than the area-average pore diameter of the microporous layer (A). For details about the relationship with the area-average pore diameter of the microporous layer (A), see the section <Area-average pore diameter of microporous layer (A)>.
[0049] The area average pore diameter of the microporous layer (B) in the MD-ND cross section is preferably 100 nm to 600 nm, more preferably 120 nm to 500 nm, even more preferably 140 nm to 400 nm, and still more preferably 160 nm to 350 nm. When the area average pore diameter of the microporous layer (B) is within this range, better withstand voltage can be obtained.
[0050] <Porosity of Microporous Layer (B)> The porosity of the microporous layer (B) is preferably 20% or more from the viewpoint of avoiding clogging in the electricity storage device and obtaining good separator air permeability, and is preferably 70% or less from the viewpoint of maintaining separator strength. The porosity of the microporous layer (B) is more preferably 25% or more and 65% or less, even more preferably 30% or more and 60% or less, and particularly preferably 35% or more and 60% or less.
[0051] <Thickness of Microporous Layer (B)> The thickness of the microporous layer (B) according to the present disclosure may be preferably 10 μm or less, for example, 8 μm or less, 7 μm or less, 6 μm or less, 5 μm or less, 4.5 μm or less, or 4 μm or less, from the viewpoint of increasing the energy density of the power storage device, etc. The lower limit of the thickness of the microporous layer (B) may be preferably 1 μm or more, for example, 2 μm or more, 3 μm or more, or 3.5 μm or more, from the viewpoint of strength, etc.
[0052] <Additives for Microporous Layer (B)> The microporous layer (B) containing polypropylene as a main component may further contain, in addition to polypropylene, additives such as elastomers, crystal nucleating agents, antioxidants, fillers, etc. The amount of the additives is not particularly limited, and may be, for example, 0.01% by mass or more, 0.1% by mass or more, or 1% by mass or more, and 10% by mass or less, 7% by mass or less, or 5% by mass or less, based on the total mass of the microporous layer (B).
[0053] <Relationship between microporous layer (A) and microporous layer (B)> Melt tension Mt of microporous layer (A) at 240°C A and the melt tension Mt of the microporous layer (B) at 240°C. B Relative to Mt A / Mt B is preferably 1.05 or more and 4.0 or less. A / Mt B By making Mt 1.05 or more, the pore size of the microporous layer (A) of the obtained separator can be controlled to be sufficiently small and the pore size of the microporous layer (B) can be controlled to be sufficiently large, thereby achieving both good voltage resistance and air permeability. A / Mt B By making Mt 4.0 or less, it is possible to obtain a separator having good pore opening and air permeability. A / Mt B is more preferably 1.1 or more and 3.5 or less, even more preferably 1.15 or more and 3.3 or less, particularly preferably 1.2 or more and 3.0 or less, and most preferably 1.25 or more and 2.5 or less.
[0054] When the main components of the microporous layer (A) and the microporous layer (B) are both polypropylene, or when the main components of the microporous layer (A) and the microporous layer (B) are both polyethylene, the MFR (MFR B ) and the MFR of the microporous layer (A) (MFR A ) ratio, MFR B / MFR A is preferably 1.02 or more and 10.0 or less. B / MFR A By making the MFR equal to or greater than 1.02, the pore size of the microporous layer (A) of the obtained separator can be controlled to be sufficiently small, and the pore size of the microporous layer (B) can be controlled to be sufficiently large, thereby achieving both good voltage resistance and air permeability. B / MFR A By making the MFR equal to or less than 10.0, it is possible to obtain a separator having stable film-forming properties, productivity, and good pore opening and air permeability. B / MFR A is more preferably 1.05 or more and 6.0 or less, even more preferably 1.1 or more and 5.0 or less, particularly preferably 1.1 or more and 4.0 or less, and most preferably 1.1 or more and 3.0 or less.
[0055] Weight average molecular weight Mw of polypropylene of microporous layer (A) A and the weight average molecular weight Mw of the polypropylene of the microporous layer (B). B The ratio of Mw A / MwB is preferably 1.02 or more and 2.0 or less. A / Mw B By making the melt tension ratio Mt of the microporous layer (A) to the microporous layer (B) 1.02 or more, A / Mt B It is possible to control the value to a high value, and as a result, it is possible to achieve both good voltage resistance and air permeability. A / Mt B By making the Mw 2.0 or less, it is possible to obtain a separator having stable film-forming properties, productivity, and good pore opening properties and air permeability. A / Mw B is preferably 1.02 or more and 1.8 or less, more preferably 1.03 or more and 1.6 or less, and most preferably 1.05 or more and 1.4 or less.
[0056] <Layer Structure of Separator Substrate> The substrate of the separator for an electricity storage device (also simply referred to as "separator substrate" in this specification) has at least one microporous layer (A) and one microporous layer (B), or has at least one microporous layer (A). The separator substrate may have a multilayer structure of three or more layers, including two or more microporous layers (A) and / or two or more microporous layers (B). Examples of such a multilayer structure include a two-layer structure of microporous layer (A) / microporous layer (B) and a three-layer structure of microporous layer (A) / microporous layer (B) / microporous layer (A). The separator substrate may also have layers other than the microporous layer (A) and the microporous layer (B). For example, layers other than the microporous layer (A) and the microporous layer (B) may include, for example, a microporous layer primarily composed of a polyolefin other than (A) and (B), a layer containing an inorganic substance, and a layer containing a heat-resistant resin. For example, the separator substrate may have a multilayer structure of four or more layers, such as microporous layer (A) / microporous layer (B) / microporous layer (C) / microporous layer (A). From the viewpoints of ease of production and suppression of separator curling, a symmetrical laminate structure is preferred. The microporous membrane used as the separator substrate of the present disclosure may have any of the layer structures described above. From the viewpoint of the mechanism of action of the microporous layers (A) and (B) primarily composed of polypropylene, it is preferred that the layer structure be such that the microporous layers (A) and (B) are laminated, the microporous layers (A) and (B) are in contact, the microporous layers (A) and (B) are adjacent, or the interface between the microporous layers (A) and (B) is observable.
[0057] <Trunk Height of Separator Substrate> The trunk height in the MD-ND cross section of the separator substrate is preferably 1000 nm or less. The separator substrate used for trunk height measurement may be the microporous membrane described above. The trunk height correlates with the pore tortuosity and is a numerical value indicating the pore structure different from the pore diameter. As the trunk height increases, the pore tortuosity decreases, and as the trunk height decreases, the pore tortuosity increases, resulting in good voltage resistance. From the viewpoint of voltage resistance, the upper limit of the trunk height is preferably 1000 nm or less, more preferably 950 nm or less, even more preferably 920 nm or less, particularly preferably 900 nm or less, and most preferably 850 nm or less. From the viewpoint of good air permeability, the lower limit of the trunk height is preferably 500 nm or more, more preferably 520 nm or more, even more preferably 550 nm or more, particularly preferably 580 nm or more, and most preferably 600 nm or more.
[0058] The trunk height can be calculated by performing cross-sectional SEM observation of the MD-ND cross section of a separator substrate or the MD-ND cross section of a microporous membrane that can be used as a separator substrate, removing fibrils by image analysis, and measuring the ND length of the remaining lamellae by image analysis. Detailed conditions are shown in the Examples. When measuring the trunk height from a cross-sectional SEM image, the number average trunk height and the length average trunk height can be calculated, but in this specification, the length average trunk height is used as the trunk height to better correlate with the physical properties of the separator.
[0059] <Thickness of Separator Substrate> The upper limit of the thickness of the separator substrate, or the upper limit of the thickness of the microporous membrane usable as the separator substrate, is preferably 20 μm or less, more preferably 18 μm or less, even more preferably 16 μm or less, particularly preferably 14 μm or less, and most preferably 13 μm or less, from the viewpoint of increasing the energy density of the power storage device, etc. The lower limit of the thickness of the separator substrate, or the lower limit of the thickness of the microporous membrane usable as the separator substrate, is preferably 8 μm or more, more preferably 9 μm or more, and even more preferably 10 μm or more, from the viewpoint of strength, etc.
[0060] <Air Permeability (Air Permeability Resistance) of Separator Substrate> The upper limit of the air permeability of the separator substrate is preferably 400 sec / 100 cm from the viewpoint of ensuring good output in the electricity storage device. 3 Less than 350 seconds / 100 cm, more preferably 3 More preferably, 300 seconds / 100 cm or less 3 Particularly preferably 250 seconds / 100 cm or less 3 Below 200 seconds / 100 cm, most preferably 3 The lower limit of the air permeability of the separator substrate is not limited, but is, for example, 10 seconds / 100 cm 3 Above, 20 seconds / 100cm 3 or more, or 30 seconds / 100 cm 3 The separator substrate used for measuring the air permeability may be the microporous membrane described above.
[0061] <Porosity of Separator Substrate> The lower limit of the porosity of the separator substrate is preferably 40% or more, more preferably 41% or more, even more preferably 42% or more, and particularly preferably 43% or more, from the viewpoint of avoiding clogging in the power storage device and obtaining good separator air permeability. The upper limit of the porosity of the separator substrate is preferably 54% or less, more preferably 53% or less, and even more preferably 52% or less, from the viewpoint of maintaining the separator strength and obtaining good withstand voltage. The separator substrate used for porosity measurement may be the microporous membrane described above.
[0062] <Withstand voltage of separator substrate> From the viewpoint of suppressing short circuits in an electricity storage device, the withstand voltage of the separator substrate, calculated as a thickness of 10 μm, is preferably 0.80 kV or more, more preferably 0.90 kV or more, even more preferably 0.95 kV or more, particularly preferably 1.00 kV or more, and most preferably 1.05 kV or more. The separator substrate used for measuring the withstand voltage may be the microporous membrane described above.
[0063] <Puncture Strength of Separator Substrate> The lower limit of the puncture strength of the separator substrate, calculated as a 10 μm thickness of the separator substrate, is preferably 150 gf or more (approximately 1.47 N or more), more preferably 180 gf or more, 200 gf or more, 220 gf or more, or 250 gf or more, and particularly preferably 270 gf or more. The upper limit of the puncture strength of the separator substrate is not limited, but may be preferably 400 gf or less, for example 380 gf or less, or 350 gf or less, calculated as a 10 μm thickness of the separator substrate. The separator substrate used for measuring the puncture strength may be the microporous membrane described above.
[0064] <Thermal Shrinkage of Separator Substrate> The separator substrate preferably has a thermal shrinkage in the width direction (TD) of 5% or less after heat treatment at 105°C for 1 hour, and more preferably a thermal shrinkage of -1.0% to 3.0%. That is, a separator substrate with a TD thermal shrinkage of 5% or less at 105°C exhibits very little thermal shrinkage in the TD even at high temperatures. Furthermore, a thermal shrinkage of 5% or less or 3.0% or less can effectively suppress short circuits at high temperatures. The reason for the thermal shrinkage of -1.0% or more is that, during thermal shrinkage measurement, the substrate may expand in the TD, resulting in a negative value below 0%. The thermal shrinkage may be 0% or more, or greater than 0%. Examples of methods for producing a separator substrate with a thermal shrinkage of 5% or less or -1.0% to 3.0% include, for example, a separator production method using uniaxial stretching in the MD, preferably a dry uniaxial stretching method. In separator manufacturing methods using biaxial stretching in MD and TD, as typified by wet separators, the thermal shrinkage in TD is generally very large, whereas uniaxial stretching of dry separators makes it easier to obtain separator substrates with a thermal shrinkage rate of 5% or less, or -1.0% to 3.0%. The separator substrate used for measuring the thermal shrinkage rate may be the microporous membrane described above.
[0065] <Tensile Strength of Separator Substrate> The tensile strength of the separator substrate in the MD is preferably 1500 kgf / cm from the viewpoint of ease of handling when winding the battery. 2 or more (approximately 14.7 kN / cm2 or more), more preferably 1600 kgf / cm 2 More preferably, 1700 kgf / cm 2 More preferably, 1800 kgf / cm 2 More than 1900 kgf / cm, most preferably 2 The upper limit of the tensile strength in the MD of the separator substrate is not limited, but is preferably 4000 kgf / cm 2 For example, 3800 kgf / cm 2 or less, or 3500 kgf / cm 2 The separator substrate subjected to the tensile strength measurement may be the microporous membrane described above.
[0066] <Mean flow pore diameter of separator substrate> <Mean flow pore diameter> The mean flow pore diameter of the microporous layer is within the range of 15 nm to 30 nm. The microporous layer having a mean flow pore diameter within the above range preferably contains polypropylene as a main component, and may be, for example, the above-described microporous layer (A) or (B), more preferably microporous layer (B). The lower limit of the mean flow pore diameter is preferably 15 nm or more, for example 20 nm or more. The upper limit of the mean flow pore diameter, which can be arbitrarily combined with these lower limits, is preferably 30 nm or less, for example 25 nm or less. The mean flow pore diameter is one of the characteristics related to the pore structure within the microporous layer. A mean flow pore diameter within the range of 15 nm to 30 nm indicates that the microporous layer has a pore structure within which current does not progress linearly (a structure with high tortuosity), and it is believed that having such a pore structure improves the withstand voltage. Furthermore, a mean flow pore diameter of 15 nm or more indicates that the microporous layer has a pore structure in which dense pores are connected, and such a pore structure allows for the production of a separator with high ion permeability. Therefore, a mean flow pore diameter of 15 nm or more allows for the production of a separator that maintains low resistance and is well-balanced with high withstand voltage. On the other hand, a mean flow pore diameter of 30 nm or less indicates that the pores in the microporous layer are less straight, which allows for the maintenance of high withstand voltage and improves the safety and yield of the energy storage device. Furthermore, a mean flow pore diameter of 30 nm or less makes it difficult for the pore structure to become a starting point for stress concentration, making it easier to maintain the strength of the separator.
[0067] The mean flow pore size is measured using a perm porometer. The mean flow pore size can be controlled mainly by the MFR of the microporous layer. A low MFR can impart strong orientation to the microporous layer, which can generate many pore initiation points during cold stretching, resulting in a small mean flow pore size during hot stretching. Details of how the mean flow pore size can be controlled by the stretching ratio will be described later, but when the cold stretching ratio is small and the hot stretching ratio is large, the pores become larger, resulting in a larger mean flow pore size. This is because a small cold stretching ratio reduces the number of pore initiation points, and the initiation points are enlarged by hot stretching, making it easier to obtain a large mean flow pore size.
[0068] <Area-average pore diameter> The area-average pore diameter of the surface of the microporous layer is 140 nm or more and 300 nm or less. The microporous layer having a surface area-average pore diameter within the above numerical range preferably contains polypropylene as a main component, and may be, for example, the above-described microporous layer (A) or (B), more preferably microporous layer (B). The lower limit of the area-average pore diameter is preferably 140 nm or more, for example, 150 nm or more, 160 nm or more, or 170 nm or more. The upper limit of the area-average pore diameter, which can be arbitrarily combined with these lower limits, is preferably 300 nm or less, for example, 290 nm or less, 280 nm or less, 270 nm or less, 260 nm or less, 250 nm or less, 240 nm or less, 230 nm or less, 220 nm or less, 210 nm or less, 200 nm or less, 190 nm or less, or 180 nm or less. When the area average pore diameter of the surface of the microporous layer is 140 nm or more, high permeability can be maintained, clogging can be reduced, and high output can be easily maintained.When the area average pore diameter is 300 nm or less, the pore diameter (porosity) is not increased more than necessary, and a separator having sufficient strength and an excellent balance with high voltage resistance can be obtained.
[0069] The area-average pore diameter of the surface is measured by SEM. The area-average pore diameter of the surface of the microporous layer can be controlled mainly by the MFR of the resin constituting the surface of the microporous layer. When the resin constituting the surface of the microporous layer has a high MFR, the orientation of the microporous layer is weakened, so that the number of origins of pores during cold stretching decreases, and a large area-average pore diameter of the surface can be obtained during hot stretching. This is because a small cold stretch ratio reduces the number of origins, and the origins are enlarged by hot stretching, making it easy to obtain large pores on the surface. The influence of the hot stretch ratio is particularly large.
[0070] When the polypropylene-based microporous layer satisfies the above-mentioned pore mean flow pore diameter and surface area average long pore diameter, it can exhibit the effects of high withstand voltage and high strength. Optionally, the microporous layer can exhibit more significant effects by further satisfying the following requirements, such as MFR, porosity, thickness, and TD heat shrinkage.
[0071] <<Method for manufacturing separator for power storage device>> The method for manufacturing a separator for a power storage device includes a melt-extrusion step of melt-extruding a resin composition containing polypropylene as a main component (hereinafter also referred to as a "polypropylene-based resin composition") to obtain a resin sheet (precursor sheet), and a pore-forming step of opening holes in the obtained precursor sheet to make it porous. Methods for manufacturing a microporous layer are broadly divided into dry methods, in which no solvent is used in the pore-forming step, and wet methods, in which a solvent is used.
[0072] Examples of dry methods include a method in which a polypropylene-based resin composition is melt-kneaded and extruded, and then the polypropylene crystal interface is peeled off by heat treatment and stretching; and a method in which a polypropylene-based resin composition and an inorganic filler are melt-kneaded and formed into a film, and then the interface between the polypropylene and the inorganic filler is peeled off by stretching.
[0073] Examples of the wet method include a method in which a polypropylene resin composition and a pore-forming material are melt-kneaded to form a film, which is stretched as necessary, and then the pore-forming material is extracted; and a method in which a polypropylene resin composition is dissolved, and then the film is immersed in a poor solvent for polypropylene to solidify the polypropylene and simultaneously remove the solvent.
[0074] A single-screw extruder or a twin-screw extruder can be used for melt-kneading the polypropylene-based resin composition. In addition to these, for example, a kneader, a Laboplastomill, a kneading roll, a Banbury mixer, etc. can also be used.
[0075] The polypropylene resin composition may optionally contain resins other than polypropylene, additives, etc., depending on the method for producing the microporous layer or the desired physical properties of the microporous layer. Examples of additives include pore-forming materials, fluorine-based flow modifiers, waxes, crystal nucleating materials, antioxidants, metal soaps such as metal salts of aliphatic carboxylic acids, ultraviolet absorbers, light stabilizers, antistatic agents, antifogging agents, and coloring pigments. Examples of pore-forming materials include plasticizers, inorganic fillers, and combinations thereof.
[0076] Examples of the plasticizer include hydrocarbons such as liquid paraffin and paraffin wax; esters such as dioctyl phthalate and dibutyl phthalate; and higher alcohols such as oleyl alcohol and stearyl alcohol.
[0077] Examples of inorganic fillers include oxide ceramics such as alumina, silica (silicon oxide), titania, zirconia, magnesia, ceria, yttria, zinc oxide, and iron oxide; nitride ceramics such as silicon nitride, titanium nitride, and boron nitride; ceramics such as silicon carbide, calcium carbonate, aluminum sulfate, aluminum hydroxide, potassium titanate, talc, kaolin clay, kaolinite, halloysite, pyrophyllite, montmorillonite, sericite, mica, amesite, bentonite, asbestos, zeolite, calcium silicate, magnesium silicate, diatomaceous earth, and silica sand; and glass fiber.
[0078] A preferred method for producing a separator substrate is a dry lamellar crystal opening process in which the polypropylene crystal interface is peeled off by heat treatment and stretching. Here, a separator substrate having a microporous layer (A) and a microporous layer (B) is preferably produced by at least one of the following methods (i) and (ii): (i) a method for producing a separator substrate by coextrusion, in which the microporous layer (A) and the microporous layer (B) are coextruded to obtain a precursor sheet, which is then subjected to annealing, cold stretching, hot stretching, and heat relaxation; and (ii) a method for producing a separator substrate by lamination, in which the microporous layer (A) and the microporous layer (B) are separately extruded to obtain a precursor sheet, which is then subjected to annealing, cold stretching, hot stretching, and heat relaxation.
[0079] The specific mean flow pore size and / or area average long pore size of the microporous layer in the present disclosure can be controlled by the cold stretching and hot stretching conditions. It is more preferable to set the average MFR of the microporous layer to be 0.25 g / 10 min or more and 0.90 g / 10 min or less and then appropriately set the cold stretching and hot stretching conditions.
[0080] Of the co-extrusion process (i) and lamination process (ii), the co-extrusion process (i) is preferred from the viewpoint of production costs, etc. In the co-extrusion process (i), the extrusion film formation conditions for the microporous layers (A) and (B) are preferably such that the resin is discharged at as low a temperature as possible and effectively quenched by blowing low-temperature air. After film formation, it is preferable to quench with air, and the temperature of the blown air is preferably 20°C or less, more preferably 15°C or less. By blowing cold air controlled at such a low temperature, the resin after film formation is uniformly oriented in the MD.
[0081] In both the co-extrusion process (i) and the lamination process (ii), the separator substrate manufacturing method may include an annealing step after extrusion film formation. The annealing step tends to grow the crystalline structure of the microporous layers (A) and (B), improving pore openness. Annealing at a specific temperature for a predetermined time tends to enable a good area-average long pore diameter to be obtained in both the microporous layers (A) and (B). This is thought to be because the crystals grow without disrupting the crystalline structure, resulting in high pore openness. The temperature range for the annealing step is preferably 115°C or higher and 160°C or lower, more preferably 125°C or higher, even more preferably 135°C, particularly preferably 140°C or higher, and most preferably 150°C or higher. The annealing step is preferably performed for 20 minutes or longer, more preferably 60 minutes or longer. The annealing temperature range and / or annealing time mentioned above tends to facilitate high orientation, provide good pore opening, and provide good air permeability even when stretched at a high ratio as described below.
[0082] The manufacturing method of the separator substrate may include a stretching step after the annealing step. Either uniaxial stretching or biaxial stretching can be used as the stretching treatment. While not limited thereto, uniaxial stretching is preferred from the viewpoints of production costs when using a dry method and reducing thermal shrinkage in the TD. The MD stretch ratio in cold stretching ((dimension after stretching - dimension before stretching) / dimension before stretching x 100 (%)) is preferably 5% or more and 50% or less. The lower limit of the MD stretch ratio in cold stretching is more preferably 8% or more, or 10% or more, thereby forming a uniform pore structure and achieving good pore openability. The lower limit of the MD stretch ratio in cold stretching is even more preferably 20% or more, 25% or more, or 30% or more, which tends to enable the design of a small area-average long pore diameter and is preferred from the viewpoint of achieving good voltage resistance. The upper limit of the MD stretch ratio in cold stretching is more preferably 40% or less. When a high cold draw ratio is used, a good withstand voltage is obtained, but there is a concern that the area average pore diameter will be reduced, resulting in a deterioration in air permeability, and achieving both becomes a challenge. To overcome this challenge, it is effective to set or adjust a high cold draw ratio and / or a high annealing temperature. This tends to achieve good pore opening while designing a small area average pore diameter, and thus achieve both good withstand voltage and air permeability.
[0083] By performing cold stretching and hot stretching under the above-mentioned stretching conditions, it is easy to control the mean flow pore size and / or area average long pore size to a specific value. Furthermore, by using a polypropylene resin whose microporous layer has an MFR of 0.25 g / 10 min or more and 0.90 g / 10 min or less, it is easier to control the mean flow pore size and / or area average long pore size.
[0084] In order to suppress thermal shrinkage of the separator substrate, a heat treatment step may be performed for the purpose of heat setting after the stretching step or the hole-forming step. The heat treatment step may include a stretching operation performed at a predetermined temperature and a predetermined stretch ratio for the purpose of adjusting physical properties, and / or a relaxation operation performed at a predetermined temperature and a predetermined relaxation ratio for the purpose of reducing shrinkage stress imparted during film formation and stretching. The relaxation operation may be performed after the stretching operation. These heat treatment steps may be performed using a tenter or a roll stretching machine.
[0085] In the heat treatment step, stretching at a specific stretch ratio or higher tends to result in a good trunk height. The heat stretch ratio in the heat treatment step is preferably 160% or higher, more preferably 170% or higher, and even more preferably 180% or higher. This is because, at a specific stretch ratio or lower, pores with a large area average pore diameter are preferentially formed, whereas at a high heat stretch ratio, a structural change occurs that results in a decrease in trunk height after sufficient pore formation. This tends to result in a good withstand voltage.
[0086] When polypropylene and polyethylene are used as the materials for the microporous layer in a co-extrusion process, it is difficult to form all layers of the laminated separator under optimal temperature and cooling conditions. When formed under conditions suitable for polypropylene, a larger stem height is easily obtained in all layers than when polypropylene is used as the main component, and it is preferable to perform the heat treatment step at a higher heat stretch ratio. When polyethylene is used, the heat treatment step preferably has a heat stretch ratio of 180% or more, more preferably 190% or more, and even more preferably 200% or more.
[0087] The obtained separator substrate can be used as it is as a separator for an electricity storage device. Optionally, one or both sides of the separator substrate may be provided with an additional layer such as a coating layer, and if necessary, may be subjected to a surface treatment such as a corona treatment.
[0088] The power storage device of the present disclosure includes the separator for a power storage device of the present disclosure. The power storage device of the present disclosure preferably has a positive electrode and a negative electrode, and the separator for a power storage device of the present disclosure is disposed between the positive electrode and the negative electrode.
[0089] Examples of the power storage device include, but are not limited to, lithium secondary batteries (including all-solid-state lithium batteries, lithium-sulfur batteries, and lithium-air batteries), lithium ion secondary batteries, sodium secondary batteries, sodium ion secondary batteries, magnesium secondary batteries, magnesium ion secondary batteries, calcium secondary batteries, calcium ion secondary batteries, aluminum secondary batteries, aluminum ion secondary batteries, nickel-metal hydride batteries, nickel-cadmium batteries, electric double layer capacitors, lithium ion capacitors, redox flow batteries, and zinc-air batteries. Among these, from the viewpoints of high energy density, low cost, and durability, lithium secondary batteries, lithium ion secondary batteries, and lithium ion capacitors are preferred, and lithium ion secondary batteries are more preferred.
[0090] The electricity storage device can be produced, for example, by stacking a positive electrode and a negative electrode with the separator described above interposed therebetween and winding them as necessary to form a stacked electrode body or a wound electrode body, which is then loaded into an outer casing, connecting the positive and negative electrodes to the positive and negative electrode terminals of the outer casing via lead bodies or the like, and further injecting a non-aqueous electrolyte solution containing a non-aqueous solvent such as a chain or cyclic carbonate and an electrolyte such as a lithium salt into the outer casing, and then sealing the outer casing.
[0091] The present electricity storage device is more preferably a lithium ion secondary battery, and preferred embodiments of the lithium ion secondary battery will now be described.
[0092] The positive electrode is not particularly limited as long as it functions as a positive electrode of a lithium ion secondary battery, and known positive electrodes can be used. The positive electrode preferably contains, as a positive electrode active material, one or more materials selected from the group consisting of materials capable of absorbing and releasing lithium ions. From the viewpoints of battery capacity and safety, the positive electrode is preferably LiCoO 2 Lithium cobalt oxide, represented by Li 2 Mn2 O 4 Spinel-based lithium manganese oxides, such as Li 2 Mn 1.5 Ni 0.5 O 4 Spinel-based lithium nickel manganese oxides, such as LiNiO 2 Lithium nickel oxide, LiMO 2 (M represents two or more elements selected from the group consisting of Ni, Mn, Co, Al, and Mg), a lithium-containing composite metal oxide represented by LiFePO 4 Among these, from the viewpoint of high safety and long-term stability, LiCoO 2 Lithium cobalt oxide, represented by LiNiO 2 Lithium nickel oxide, LiMO 2 (M represents two or more elements selected from the group consisting of Ni, Mn, Co, Al, and Mg), a lithium-containing composite metal oxide represented by LiFePO 4 Particularly preferred is a lithium iron phosphate compound represented by LiFePO 4 It is a lithium iron phosphate compound represented by the formula:
[0093] The negative electrode is not particularly limited as long as it functions as a negative electrode for a lithium-ion secondary battery, and may be any known material. The negative electrode preferably contains, as the negative electrode active material, one or more materials selected from the group consisting of materials capable of absorbing and releasing lithium ions and metallic lithium. That is, the negative electrode preferably contains, as the negative electrode active material, one or more materials selected from the group consisting of metallic lithium, carbon materials, materials containing elements capable of forming an alloy with lithium, and lithium-containing compounds. Examples of such materials include metallic lithium, as well as carbon materials such as hard carbon, soft carbon, artificial graphite, natural graphite, graphite, pyrolytic carbon, coke, glassy carbon, fired bodies of organic polymer compounds, mesocarbon microbeads, carbon fibers, activated carbon, carbon colloids, and carbon black.
[0094] <<Measurement and Evaluation Methods>> [Measurement of Melt Flow Rate (MFR)] The melt flow rate (MFR) of the microporous layer was measured in accordance with JIS K 7210 at a temperature of 230°C and a load of 2.16 kg, or at a temperature of 190°C and a load of 2.16 kg (unit: g / 10 min). The MFR of polypropylene was measured in accordance with JIS K 7210 at a temperature of 230°C and a load of 2.16 kg. The melt flow rate (MFR) of polyethylene was measured in accordance with JIS K 7210 at a temperature of 190°C and a load of 2.16 kg.
[0095] [Measurement of Mw and Mn by GPC (Gel Permeation Chromatography)] Using an Agilent PL-GPC220, standard polystyrene was measured under the following conditions to create a calibration curve. Chromatography was also performed on the sample polymer under the same conditions, and based on the calibration curve, the weight average molecular weight (Mw), number average molecular weight (Mn), and MWD (Mw / Mn), calculated by dividing the weight average molecular weight (Mw) by the number average molecular weight (Mn) in terms of polystyrene, were calculated under the following conditions. Column: TSKgel GMHHR-H(20) HT (7.8 mm I.D. x 30 cm), 2 columns Mobile phase: 1,2,4-trichlorobenzene Detector: RI Column temperature: 160°C Sample concentration: 1 mg / ml Calibration curve: polystyrene
[0096] [Melt Tension Measurement] The melt tension (mN) of the microporous membrane or microporous layer was measured using a Capillograph manufactured by Toyo Seiki Seisakusho under the following conditions: Capillary: diameter 1.0 mm, length 20 mm Cylinder extrusion speed: 2 mm / min Take-up speed: 60 m / min Temperature: 240°C
[0097] [Mean Flow Pore Diameter] The mean flow pore diameter of the microporous layer was measured using a perm porometer (Porous Materials, Inc.: CFP-1500AE) in accordance with the bubble point method (ASTM F316-86, JIS K 3832). The immersion liquid used was a perfluoropolyester manufactured by the same company (trade name "Galwick", surface tension γ = 15.6 dyn / cm). The applied pressure and air permeation rate were measured for the dry curve and the wet curve, and the mean flow diameter dHD (μm) was calculated from the pressure PHD (Pa) at which the obtained half curve of the dry curve intersects with the wet curve using the following formula: dHD = 2860 × γ / PHD
[0098] [Measurement of Pentad Fraction] The pentad fraction of polypropylene was assigned based on the description in the Polymer Analysis Handbook (edited by the Japan Society for Analytical Chemistry). 13 Calculation was performed from the C-NMR spectrum using the peak height method. 13 The C-NMR spectrum was measured using a JEOL-ECZ500 by dissolving polypropylene pellets in o-dichlorobenzene-d at a measurement temperature of 145°C and accumulating 25,000 times.
[0099] [Measurement of Thickness (μm)] The thickness (μm) of the separator substrate was measured using a Mitutoyo Digimatic Indicator IDC112 at room temperature of 23±2° C. The thickness of each microporous layer was calculated from cross-sectional SEM image data obtained by the method for evaluating the area average long pore diameter described below.
[0100] [Measurement of Porosity (%)] A sample having a size of 10 cm x 10 cm was cut from the separator or the microporous layer, and its volume (cm 3 ) and mass (g), and calculate the density (g / cm 3 ) and the porosity was calculated using the following formula: Porosity (%) = (volume - mass / density) / volume x 100
[0101] [Air permeability (sec / 100cm) 3 ) )] The air permeability resistance (sec / 100 cm) of the separator substrate was measured using a Gurley air permeability meter conforming to JIS P-8117. 3 The air resistance (sec / 100 cm) was also measured. 3) by the separator thickness (μm) and multiplying by 10 μm to obtain the air permeation resistance (sec / (100 cm)) when the thickness of the separator substrate is converted to 10 μm. 3 ・10 μm) was obtained.
[0102] [Air permeability after high-temperature treatment (sec / 100 cm 3 The separator substrate was cut into a square of 100 mm in each of the MD and TD directions, and the obtained sample was placed in a hot air dryer (manufactured by Yamato Scientific Co., Ltd., DF1032) and subjected to heat treatment at 140°C for 30 minutes in the air at normal pressure. The sample was removed from the hot air dryer and allowed to cool at 25°C for 10 minutes. Thereafter, the air permeability resistance (sec / 100 cm) of the separator substrate was measured using a Gurley air permeability meter conforming to JIS P-8117. 3 ) was measured.
[0103] [TD Heat Shrinkage Rate (%)] The separator substrate was cut into a 50 mm square in each of the MD and TD directions, and the resulting sample was placed on a sheet of copy paper in a hot air dryer (manufactured by Yamato Scientific Co., Ltd., DF1032) and subjected to heat treatment at 105°C for 1 hour in the atmosphere at normal pressure. The sample was removed from the hot air dryer and allowed to cool at 25°C for 10 minutes, after which the TD dimensional shrinkage rate was determined. Heat shrinkage rate (%): (dimension before heating (mm) - dimension after heating (mm)) / (dimension before heating (mm)) x 100
[0104] [Puncture Strength] A needle with a hemispherical tip and a radius of 0.5 mm was prepared, and a separator was sandwiched between two plates with openings of 11 mm diameter (dia.), and the needle, separator, and plates were set in place. A puncture test was performed using an "MX2-50N" made by Imada Co., Ltd., under the conditions of a needle tip curvature radius of 0.5 mm, an opening diameter of 11 mm in the separator holding plate, and a puncture speed of 25 mm / min. The needle and separator were brought into contact, and the maximum puncture load (i.e., puncture strength (gf)) was measured. The puncture strength (gf) was divided by the separator thickness (μm) and multiplied by 10 μm to determine the puncture strength (gf / 10 μm) when the thickness of the separator substrate was converted to 10 μm.
[0105] [Tensile Strength] The tensile strength of the separator was measured using a tensile tester (TG-1kN type manufactured by Minebea Co., Ltd.) by setting the sample length before the test to 35 mm and pulling the sample at a speed of 100 mm / min. The tensile strength was determined as the strength (tensile load value) when the sample yielded, or, if the sample broke (fractured) before yielding, the strength (tensile load value) at break by the cross-sectional area of the test piece. The tensile strength was measured in the MD direction of the separator.
[0106] [Area-average pore diameter (nm)] The area-average pore diameter was measured by image analysis of cross-sectional SEM observation. As a pretreatment, the separator was stained with ruthenium, and a cross-sectional sample was prepared by freeze-fracturing. The cross-section was the MD-ND plane. The cross-sectional sample was fixed to a SEM sample stage for cross-sectional observation with a conductive adhesive (carbon-based) and dried. After that, an osmium coating was performed as a conductive treatment using an osmium coater (HPC-30W, manufactured by Vacuum Device Co., Ltd.) under conditions of an applied voltage adjustment knob setting of 4.5 and a discharge time of 0.5 seconds, and a microscopic specimen was prepared. Next, using a scanning electron microscope (S-4800 manufactured by Hitachi High-Technologies Corporation), eight random points on the cross section of each microporous layer of the microporous membrane were observed under conditions of an acceleration voltage of 1 kV, a detection signal LA10, a working distance of 5 mm, and a magnification of 30,000x.
[0107] The observed image was trimmed using a function of OpenCV, an image analysis library, in a programming language Python environment so that only the cross section of one microporous layer was included, and the surface, outer layer, and other microporous layers were removed. The image was then binarized using the Otsu method to separate the resin portion from the pore portion, and the average major axis of the pores was calculated. At this time, the area of the pores existing across the photographed range and outside the photographed range was 0.001 nm 2 The following pores were excluded from the measurement: The average diameter was calculated by averaging the area of each pore.
[0108] [Trunk height (nm)] The trunk height was measured by image analysis of cross-sectional SEM observation. As in the calculation of the area average pore diameter, cross-sectional samples and microscopic samples were prepared, and then three arbitrary points on the cross section of the microporous membrane were observed under conditions of an accelerating voltage of 1 kV, a detection signal LA10, a working distance of 5 mm, and a magnification of 5000x.
[0109] The observed image was binarized using the Otsu method in a Python programming language environment, using functions from the OpenCV image analysis library to separate the resin portion from the pore portion. Furthermore, a blurring process was repeatedly performed only in the ND direction to remove the fibril portion. The fibril removal process was performed 100 times using a Gaussian filter in a rod-shaped processing range of 3 pixels in the ND direction and 1 pixel in the MD direction. After the blurring process, an opening process and a closing process were sequentially performed in an elliptical processing range of 7 pixels in the ND direction and 3 pixels in the MD direction to remove noise, and a fibril-removed image was obtained.
[0110] The stem height was calculated from the fibril-removed image. The fibril-removed image was cut out at 1 pixel in the MD direction, and the entire length of the resin portion in the ND direction was detected. This was repeated so as to include the entire MD direction, and the length of the resin portion in the ND direction over the entire range of the fibril-removed image was detected. A weighted average was calculated for the obtained values of the resin portion length in the ND direction, with the length of the resin portion in the ND direction as the weight, and the obtained value was taken as the stem height. If the length of the resin portion in the ND direction is L, the stem height H can be calculated using the following formula: By using a weighted average of n lengths L, the trunk height H becomes a value that is more highly correlated with the withstand voltage.
[0111] [Measurement of withstand voltage (kV)] The separator substrate sandwiched between aluminum foils was set on the sample stage of a withstand voltage tester (grade) manufactured by Kikusui Electronics Co., Ltd., and an electrode indenter was placed thereon. The voltage was increased at a starting voltage of 0 kV and a voltage increase rate of 0.025 kV / sec, and the voltage value when a current of 0.2 mA flowed between the electrodes was taken as the withstand voltage value. The withstand voltage value (kV) was also divided by the separator thickness (μm) and multiplied by 10 μm to determine the withstand voltage (kV / 10 μm) when the thickness of the separator substrate was converted to 10 μm.
[0112] [Battery Performance (Dendrite Short-Circuit Evaluation)] As an electrolyte, ethylene carbonate and ethyl methyl carbonate were mixed in a volume ratio of 1:2, and LiPF 6 was added as a lithium salt. 6 An electrolyte solution containing 1 mol / L of
[0113] The positive electrode active material is a lithium-nickel-manganese-cobalt mixed oxide (LiNi 0.5 Co 0.2 Mn 0.3 O 2 ), carbon black powder (manufactured by Timcal, product name: SuperP Li) as a conductive additive, and PVDF as a binder were mixed in a mass ratio of mixed oxide:conductive additive:binder=100:3.5:3, and the mixture was applied to both sides of an aluminum foil serving as a positive electrode current collector with a thickness of 15 μm, dried, and then pressed with a roll press to prepare a double-sided coated positive electrode.
[0114] Graphite powder (manufactured by Hitachi Chemical Co., Ltd., product name: MAG) having a particle diameter of 22 μm (D50) as the negative electrode active material, a binder (manufactured by Zeon Corporation, product name: BM400B), and carboxymethyl cellulose (manufactured by Daicel Corporation, product name: #2200) as a thickener were mixed in a mass ratio of graphite powder:binder:thickener = 100:1.5:1.1, and the mixture was applied to one side and both sides of copper foil as a negative electrode current collector having a thickness of 10 μm. The solvent was then dried and removed, and the coated copper foil was then pressed with a roll press to produce a single-side-coated negative electrode and a double-side-coated negative electrode, respectively.
[0115] The obtained positive electrode and negative electrode were stacked on the opposing surfaces of the active materials, with the separator prepared below sandwiched between them, in the order of single-sided coated negative electrode / double-sided coated positive electrode / double-sided coated negative electrode / double-sided coated positive electrode / single-sided coated negative electrode. The microporous layer (A) was arranged facing the negative electrode. The obtained laminate was then inserted into a bag (battery exterior) made of a laminate film in which both sides of aluminum foil (thickness 40 μm) were coated with a resin layer, with the positive and negative electrode terminals protruding. Then, 0.8 mL of the electrolyte prepared as described above was poured into the bag, and the bag was vacuum-sealed to produce a sheet-shaped lithium ion secondary battery.
[0116] The resulting sheet-shaped lithium ion secondary battery was placed in a thermostatic chamber (manufactured by Futaba Scientific Co., Ltd., product name: PLM-73S) set at 25°C, connected to a charge / discharge device (manufactured by Asuka Electronics Co., Ltd., product name: ACD-01), and left to stand for 16 hours. The battery was then charged at a constant current of 0.05 C, and after the voltage reached 4.35 V, it was charged at a constant voltage of 4.35 V for 2 hours, and then discharged at a constant current of 0.2 C to 3.0 V. This charge / discharge cycle was repeated three times to perform initial charge / discharge of the battery. 1 C refers to the current value when the battery's full capacity is discharged in 1 hour.
[0117] After the initial charge and discharge, the battery was placed in a thermostatic chamber set at 10°C, and the battery was charged at a constant current of 1 C. After the voltage reached 4.50 V, the battery was charged at a constant voltage of 4.50 V for one hour, then left to stand in an open-circuit state for one hour, and then discharged at a constant current of 1 C to 3.0 V. This charge and discharge cycle was repeated 10 times, and the presence or absence of dendritic short-circuiting during this period was confirmed using 10 sheet-like lithium-ion secondary batteries. The pass rate (%) was calculated from the number of sheet-like lithium-ion secondary batteries that did not develop a short circuit. The presence or absence of dendritic short-circuiting was determined to be present if the voltage dropped by 0.3 V or more while left to stand in an open-circuit state after charging, or if the battery could not be charged to 4.5 V within two hours during constant-current charging at 1 C.
[0118] Example 1 Preparation of Microporous Layer A high molecular weight polypropylene resin (MFR (230°C) = 0.31 g / 10 min, density = 0.91 g / cm) was used as the resin for the microporous layer (A). 3 ) was melted in a 2.5-inch extruder and fed to both outer layers of a two-kind, three-layer coextrusion blown film die using a gear pump. Furthermore, a high-molecular-weight polypropylene resin (MFR (230°C) = 0.51 g / 10 min, density = 0.91 g / cm) was used as the resin for the microporous layer (B). 3A resin material was obtained by dry blending 92% by weight of styrene-ethylene propylene-styrene block copolymer (referred to as "SEPS" in the table) with 8% by weight of styrene-ethylene propylene-styrene block copolymer (referred to as "SEPS" in the table). The resulting resin material was melted in a 2.5-inch extruder and fed to the inner layer of the two-component, three-layer coextrusion blown film die using a gear pump. The blown film die temperature was set to 245°C, and the molten polymer was extruded from the blown film die. The extruded resin was cooled by blown air while being wound on a roll, yielding a precursor sheet with an A / B / A layer structure approximately 14 μm thick. The lip clearance of the blown film die was set to 1.8 mm, and extrusion was performed at a discharge rate of 9 kg / h.
[0119] The resulting precursor was then placed in a dryer and annealed at 150°C for 180 minutes. The annealed precursor was then cold stretched 30% at room temperature, and the stretched film was placed in a 140°C oven without shrinkage and hot stretched to 180%, followed by relaxation by 50% to obtain a separator substrate having a three-layer structure consisting of A / B / A layers. The structure and physical properties of the resulting separator substrate are shown in Table 1.
[0120] Example 2 A microporous membrane was obtained in the same manner as in Example 1, except that the membrane was placed in an oven at 150°C for hot stretching and relaxation, and the obtained microporous membrane was evaluated as a separator.
[0121] Examples 3, 6, 7, and 8 Microporous membranes were obtained in the same manner as in Example 1, except that raw materials were changed as shown in Table 1, the membrane was cold stretched by 40%, and the membrane was hot stretched by 220% in an oven at 135°C and relaxed by 30%. The resulting microporous membranes were evaluated as separators.
[0122] Example 4 A microporous membrane was obtained in the same manner as in Example 1, except that the raw materials were changed as shown in Table 1, the membrane was cold stretched by 20%, and the membrane was hot stretched by 190% in an oven at 135°C and relaxed by 30%. The obtained microporous membrane was evaluated as a separator.
[0123] Example 5 A microporous membrane was obtained in the same manner as in Example 1, except that 16% cold stretching and 195% hot stretching were performed, and the obtained microporous membrane was evaluated as a separator.
[0124] Example 9 A high molecular weight polypropylene resin (MFR (230°C) = 0.91 g / 10 min, density = 0.91 g / cm) was used as the resin for the microporous layer (A). 3 ) was melted in a 2.5-inch extruder and fed to a single-layer inflation die using a gear pump. The temperature of the inflation die was set to 225°C, and the molten polymer was extruded from the inflation die. The extruded resin was cooled by blown air while being wound around a roll, yielding a single-layer precursor sheet consisting of a microporous layer (A) approximately 12 μm thick. The lip clearance of the inflation die was set to 1.8 mm, and extrusion was performed at a discharge rate of 9 kg / h.
[0125] The resulting precursor sheet was then placed in a dryer and annealed at 150°C for 180 minutes. The annealed precursor was then cold stretched by 30% at room temperature, and the stretched film was placed in an oven at 135°C without shrinkage and hot stretched to 240%, followed by relaxation by 50% to obtain a separator substrate having a single-layer structure consisting of a microporous layer (A). The resulting separator substrate was evaluated.
[0126] Example 13 A high molecular weight polypropylene resin (MFR (230°C) = 0.25 g / 10 min, density = 0.91 g / cm) was used as the resin for the microporous layer (A). 3 ) was melted in a 2.5-inch extruder and fed to the inner layer of a two-kind, three-layer coextrusion blown film die at a discharge rate of 7 kg / h using a gear pump. Furthermore, a high-molecular-weight polypropylene resin (MFR (230°C) = 0.91 g / 10 min, density = 0.91 g / cm) was used as the resin for the microporous layer (B). 3) 100 wt.% was melted in a 2.5-inch extruder and fed to both outer layers of the two-kind, three-layer coextrusion blown film die at a discharge rate of 2 kg / h using a gear pump. The temperature of the blown film die was set to 225°C, and after the molten polymer was extruded from the blown film die, the extruded resin was cooled by blown air while being wound on a roll, yielding a precursor sheet with a B / A / B layer structure approximately 12 μm thick. Here, the lip distance (lip clearance) of the blown film die was set to 1.8 mm, and extrusion was performed at a total discharge rate of 9 kg / h.
[0127] The resulting precursor sheet was then placed in a dryer and annealed at 130°C for 180 minutes. The annealed precursor was then cold stretched by 30% at room temperature, and the stretched film was placed in an oven at 140°C without shrinkage and hot stretched to 180%, followed by relaxation by 50% to obtain a separator substrate having a three-layer structure consisting of B / A / B layers. The resulting separator was evaluated.
[0128] Examples 10, 11, and 15, Comparative Example 4 Separator substrates having a single-layer structure composed of a microporous layer (A) were obtained in the same manner as in Example 9, except that the resin raw materials and production conditions were changed as shown in Table 1. The obtained separator substrates were evaluated.
[0129] Example 12 The resin of the microporous layer (A) was changed as shown in Table 1, and a polyethylene resin (MFR (190°C) = 0.32 g / 10 min, density = 0.96 g / cm) was used as the resin of the microporous layer (B). 3 A microporous membrane was obtained in the same manner as in Example 1, except that the amount of cellulose acetate copolymer (C10) in the cellulose acetate film was changed to 100 wt %, the inflation die temperature was set to 225°C, and the membrane was cold stretched by 30%, hot stretched to 200% in a 120°C oven, and relaxed by 40%, and the resulting separator was evaluated.
[0130] Example 14 A microporous membrane was obtained in the same manner as in Example 4, except that the membrane was cold stretched by 12%, hot stretched to 170%, and relaxed by 40%, and the resulting separator was evaluated.
[0131] Comparative Example 1 A microporous membrane was obtained in the same manner as in Example 13, except that annealing was performed at 150°C for 180 minutes, cold stretching was performed by 10%, hot stretching was performed to 150%, and relaxation was performed by 40%, and the resulting separator was evaluated.
[0132] Comparative Example 2 A separator substrate having a three-layer structure consisting of B / A / B layers was obtained in the same manner as in Example 13, except that the resin raw materials and manufacturing conditions were changed as shown in Table 1. The obtained separator was evaluated.
[0133] Comparative Example 3 A separator substrate having a three-layer structure consisting of A / B / A layers was obtained in the same manner as in Example 12, except that the resin raw materials and manufacturing conditions were changed as shown in Table 1. The obtained separator was evaluated.
[0134] Table 1 shows that by strictly controlling the composition of each layer and the film-forming conditions, it is possible to control the area average pore diameter of the microporous layer (A) arranged in the outermost layer and the stem height of the separator substrate to be small, even though each layer uses a polypropylene resin. Furthermore, such a separator configuration can simultaneously achieve high permeability required for a separator for a lithium ion secondary battery, as well as high puncture strength and high voltage resistance to achieve high safety.
[0135]
[0136]
[0137] Example 16 [Preparation of Microporous Layer] As the resin for the microporous layer (A), a high molecular weight polypropylene resin (MFR (230°C) = 0.30 g / 10 min, density = 0.91 g / cm 3 ) was melted in a 2.5-inch extruder and fed to both outer layers of a two-kind, three-layer coextrusion blown film die using a gear pump. Furthermore, a high-molecular-weight polypropylene resin (MFR (230°C) = 0.51 g / 10 min, density = 0.91 g / cm) was used as the resin for the microporous layer (B). 3) was melted in a 2.5-inch extruder and fed to the inner layer of the two-kind, three-layer coextrusion blown film die using a gear pump. The temperature of the blown film die was set to 245°C, and the molten polymer was extruded from the blown film die. The extruded resin was cooled by blown air while being wound on a roll, yielding a precursor sheet with an A / B / A layer structure approximately 14 μm thick. Here, the lip distance (lip clearance) of the blown film die was set to 1.8 mm, and extrusion was performed at a discharge rate of 9 kg / h.
[0138] The resulting precursor was then placed in a dryer and annealed at 150°C for 180 minutes. The annealed precursor was then cold stretched 30% at room temperature, and the stretched film was placed in a 140°C oven without shrinkage and hot stretched to 180%, followed by relaxation by 50% to obtain a separator substrate having a three-layer structure consisting of A / B / A layers. The structure, physical properties, and battery performance evaluation results of the resulting separator substrate are shown in Table 2.
[0139] Examples 17 to 19 and Examples 22 to 24 Microporous membranes were obtained in the same manner as in Example 16, except that the raw materials were changed as shown in Table 2, and the resulting separators were evaluated.
[0140] Examples 20 and 21 As the resin for the microporous layer (B), a high molecular weight polypropylene resin (MFR (230°C) = 0.51 g / 10 min, density = 0.91 g / cm 3 A resin material was obtained by dry blending 92% by weight of styrene-ethylene propylene-styrene block copolymer (referred to as "SEPS" in the table) with 8% by weight of styrene-ethylene propylene-styrene block copolymer (referred to as "SEPS" in the table). The obtained resin material was melted in a 2.5-inch extruder and fed to the inner layer of a two-kind, three-layer coextrusion blown film die using a gear pump. Furthermore, a high-molecular-weight polypropylene resin (MFR (230°C) = 0.30 g / 10 min in Example 20, MFR (230°C) = 0.50 g / 10 min in Example 21, density = 0.91 g / cm in Examples 20 and 21) was used as the resin for the microporous layer (A). 3) was melted in a 2.5-inch extruder and fed to both outer layers of the two-kind, three-layer coextrusion blown film die using a gear pump. The temperature of the blown film die was set to 245°C, and the molten polymer was extruded from the blown film die. The extruded resin was cooled by blown air while being wound up on a roll, yielding a precursor sheet with an A / B / A layer structure approximately 14 μm thick. Here, the lip distance (lip clearance) of the blown film die was set to 1.8 mm, and extrusion was performed at a discharge rate of 9 kg / h.
[0141] Example 25 As shown in Table 2, a precursor sheet was obtained using the same raw materials and manufacturing method as in Example 16.
[0142] The resulting precursor sheet was then placed in a dryer and annealed at 150°C for 180 minutes. The annealed precursor was then cold stretched 40% at room temperature, and the stretched film was placed in a 140°C oven without shrinkage and hot stretched to 180%, followed by relaxation by 50% to obtain a separator substrate with a three-layer structure consisting of A / B / A layers. The structure, physical properties, and battery performance evaluation results of the resulting separator substrate are shown in Table 2.
[0143] Table 2 shows that by strictly controlling the composition of each layer and the film-forming conditions, it is possible to control the area average pore diameter of microporous layer (A) arranged in the outermost layer to be smaller than the area average pore diameter of microporous layer (B), even though each layer uses a polypropylene resin. Furthermore, such a separator configuration effectively suppresses dendrite short-circuiting in a lithium ion secondary battery and further provides excellent voltage resistance characteristics and permeability.
[0144]
[0145]
[0146] Examples 26 to 29 Separator substrates having a three-layer structure consisting of B / A / B layers were obtained in the same manner as in Example 13, except that the resin raw materials and manufacturing conditions were changed as shown in Table 3. The obtained separators were evaluated.
[0147] Table 3 shows that by strictly controlling the membrane formation conditions, it is possible to control the area average pore diameter of the microporous layer surface to be large and the mean flow pore diameter to be small, even though each layer uses a polypropylene resin. Furthermore, it is also shown that a separator having such a configuration has the high permeability required for a separator for a lithium ion secondary battery, and can simultaneously achieve high voltage resistance and high strength to ensure high safety.
[0148]
[0149] The separator for an electricity storage device according to the present disclosure can be suitably used as a separator for an electricity storage device, such as a lithium ion secondary battery.
Claims
1. A separator for an electricity storage device, comprising a microporous layer (A) containing polypropylene as a main component and a microporous layer (B) containing polypropylene as a main component laminated together, or comprising a microporous membrane containing at least one of the microporous layer (A) and the microporous layer (B), wherein the stem height calculated from analysis of an SEM image of an MD-ND cross section of the microporous membrane is 500 nm or more and 1000 nm or less.
2. The separator for an electricity storage device according to claim 1, wherein the area average long pore diameter of the microporous layer (A) calculated by analysis of a SEM image of an MD-ND cross section of the microporous membrane is 100 nm or more and 280 nm or less.
3. The separator for an electricity storage device according to claim 1 or 2, wherein the area average long pore diameter of the microporous layer (A) is smaller than the area average long pore diameter of the microporous layer (B).
4. Melt tension Mt of the microporous layer (A) at 240°C A The separator for an electricity storage device according to claim 1 or 2, wherein the compressive strength is 10 mN or more and 35 mN or less.
5. The separator for an electricity storage device according to claim 1 or 2, wherein the thickness of the microporous film is 8 μm or more and 20 μm or less.
6. The separator for an electricity storage device according to claim 1 or 2, wherein the thickness of the microporous layer (A) is 5 μm or less.
7. The separator for an electric storage device according to claim 1 or 2, wherein the molecular weight distribution (Mw / Mn), which is the value obtained by dividing the weight average molecular weight (Mw) by the number average molecular weight (Mn) of the polypropylene of the microporous layer (A), is 6.0 or more and 14 or less.
8. The separator for an electric storage device according to claim 1 or 2, wherein the proportion of components having a molecular weight of 80,000 or less contained in the polypropylene of the microporous layer (A) is 10% or more and 20% or less, and the proportion of components having a molecular weight of 1,500,000 or more is 10% or more and 20% or less.
9. The separator for an electricity storage device according to claim 1 or 2, wherein the microporous layer (B) has a mean flow pore size of 20 nm or more and 25 nm or less.
10. The separator for an electricity storage device according to claim 1 or 2, wherein the area average long pore diameter of the surface of the microporous layer (B) is 140 nm or more and 300 nm or less.
11. The separator for an electricity storage device according to claim 1 or 2, wherein the microporous membrane has a TD heat shrinkage rate of 5% or less at 105° C. for 1 hour.
12. The separator for an electricity storage device according to claim 1 or 2, wherein the porosity of the microporous film is 40% or more and 54% or less.
13. In the microporous membrane, the melt tension Mt of the microporous layer (A) at 240°C A and the melt tension Mt of the microporous layer (B). B The separator for an electricity storage device according to claim 1 or 2, wherein 14. The microporous membrane has an MD tensile strength of 1500 kgf / cm 2 The separator for an electricity storage device according to claim 1 or 2.
Citation Information
Patent Citations
Separator for electrolytic capacitor, and electrolytic capacitor
WO2013069146A1
Improved microlayer membranes, improved battery separators, and related methods
WO2018089748A1
Separator for power storage device
WO2020196120A1
Separator for power storage device
JP2022051521A
Separator for power storage device and power storage device
JP2022142698A
Cited By
Multilayer microporous membranes and uses thereof