Binder composition for non-aqueous secondary battery electrode, slurry composition for non-aqueous secondary battery electrode, electrode for non-aqueous secondary battery, and non-aqueous secondary battery
The binder composition for non-aqueous secondary battery electrodes, featuring a polymer blend with specific units, addresses flexibility and performance issues by forming a film with targeted mechanical properties, enhancing electrode flexibility and battery characteristics.
Patent Information
- Application Number
- PCT/JP2024/011987
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-03
AI Technical Summary
Non-aqueous secondary battery electrodes face challenges in achieving both flexibility and improved battery characteristics, particularly when increased thickness leads to reduced flexibility and potential cracking, and higher binder content deteriorates battery performance.
A binder composition for non-aqueous secondary battery electrodes containing a polymer blend with specific nitrile group-containing and alkylene structural units, which forms a film with a predetermined breaking stress and strain, enhancing electrode flexibility and battery performance.
The binder composition improves the flexibility and battery characteristics of non-aqueous secondary battery electrodes, preventing cracking and maintaining performance even at increased thickness, while optimizing IV, rate, and cycle characteristics.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002
Abstract
Description
Binder composition for non-aqueous secondary battery electrodes, slurry composition for non-aqueous secondary battery electrodes, electrodes for non-aqueous secondary batteries, and non-aqueous secondary batteries
[0001] The present invention relates to a binder composition for a non-aqueous secondary battery electrode, a slurry composition for a non-aqueous secondary battery electrode, an electrode for a non-aqueous secondary battery, and a non-aqueous secondary battery.
[0002] Non-aqueous secondary batteries such as lithium ion secondary batteries (hereinafter sometimes abbreviated as "secondary batteries") are small, lightweight, have high energy density, and are capable of repeated charge and discharge, and are therefore used in a wide range of applications. Therefore, in recent years, improvements to battery components such as electrodes have been investigated with the aim of further improving the performance of non-aqueous secondary batteries.
[0003] Here, an electrode used in a secondary battery such as a lithium-ion secondary battery typically includes a current collector and an electrode mixture layer (positive electrode mixture layer or negative electrode mixture layer) formed on the current collector. The electrode mixture layer is formed, for example, by applying a slurry composition containing an electrode active material and a binder composition containing a binding agent onto the current collector and then drying the applied slurry composition.
[0004] In recent years, attempts have been made to improve the electrode mixture layer in order to achieve further improvements in the performance of secondary batteries. For example, Patent Document 1 discloses that in a positive electrode active material layer (electrode mixture layer) containing a positive electrode active material, a conductive material, and a binder (binding material), the binder contains a first polymer that is a predetermined fluorine-containing polymer, and a second polymer that contains polymerization units having nitrile groups, polymerization units having hydrophilic groups, (meth)acrylic acid ester polymerization units, and linear alkylene polymerization units having 4 or more carbon atoms, each in a predetermined proportion.
[0005] JP 2017-143075 A
[0006] In recent years, thicker electrode films have been investigated to improve the energy density of secondary batteries. However, thicker electrodes reduce the electrode's flexibility, and in wound secondary batteries in particular, cracks can occur in the electrode when the innermost electrode is wound. Furthermore, increasing the binder content to improve electrode flexibility can degrade the secondary battery's battery characteristics, such as IV characteristics, cycle characteristics, and rate characteristics.
[0007] Therefore, an object of the present invention is to provide a binder composition for non-aqueous secondary battery electrodes that can be suitably used to produce electrodes with excellent flexibility and that can improve the battery characteristics of secondary batteries equipped with the resulting electrodes. Another object of the present invention is to provide a slurry composition for non-aqueous secondary battery electrodes that can form electrodes with excellent flexibility and can improve the battery characteristics of secondary batteries equipped with the resulting electrodes. A further object of the present invention is to provide a non-aqueous secondary battery electrode that can improve the battery characteristics of non-aqueous secondary batteries, and a non-aqueous secondary battery that has excellent battery characteristics.
[0008] The present inventors have conducted extensive research to solve the above problems, and have newly discovered that by using a binder composition for a non-aqueous secondary battery electrode containing a specific polymer that, when formed into a film, satisfies a specific relationship between the breaking stress [MPa] and the breaking strain [-] in a tensile test of the film, an electrode with excellent flexibility can be produced and the battery characteristics of the secondary battery can be improved, thereby completing the present invention.
[0009] The present invention aims to advantageously solve the above-mentioned problems. The present invention provides a binder composition for a non-aqueous secondary battery electrode, comprising: [1] a polymer A; wherein, when the binder composition for a non-aqueous secondary battery electrode is formed into a film X, the breaking stress [MPa] and breaking strain [-] of the film X in a tensile test satisfy the relationship: 0.010≦breaking stress [MPa] / breaking strain [-]≦1.000. Thus, if the breaking stress and breaking strain values of the binder composition for a non-aqueous secondary battery electrode formed into a film and subjected to a tensile test satisfy the above-mentioned relationship, the flexibility of an electrode formed using the binder composition for a non-aqueous secondary battery electrode can be improved, and the battery characteristics of a secondary battery using the electrode can be improved. In the present invention, the breaking stress and breaking strain of a film X of the binder composition for a non-aqueous secondary battery electrode in a tensile test can be measured by the method described in the Examples.
[0010] [2] In the binder composition for a non-aqueous secondary battery electrode according to [1] above, the breaking strain when the film X is subjected to a tensile test is preferably 6.0 or more. In this way, when the breaking strain in the tensile test of the film X of the binder composition for a non-aqueous secondary battery electrode is equal to or more than the above lower limit, the flexibility of the obtained electrode can be further improved.
[0011] [3] In the binder composition for a non-aqueous secondary battery electrode according to the above [1] or [2], it is preferable that the polymer A contains two or more types of polymers. In this way, if the polymer A contains two or more types of polymers, the flexibility of the obtained electrode can be further improved, and the battery characteristics of a secondary battery using the electrode can be further improved.
[0012] [4] In the binder composition for a non-aqueous secondary battery electrode according to any one of [1] to [3] above, the polymer A preferably comprises a polymer A1 such that, when formed into a film Y, the film Y has a breaking stress of 0.3 MPa or more and a breaking strain of 6.0 or more and less than 25.0, as determined by a tensile test. Thus, if the polymer A comprises a polymer A1 whose breaking stress and breaking strain when formed into a film are within the above-mentioned ranges, the electrode mixture layer can be maintained, and the cycle characteristics of a secondary battery using the electrode can be further improved. In the present invention, the breaking stress and breaking strain measured when a polymer film Y is subjected to a tensile test can be measured by the method described in the Examples.
[0013] [5] In the binder composition for a non-aqueous secondary battery electrode according to [4] above, it is preferable that the polymer A further contains a polymer A2 such that, when formed into a film Y, the film Y has a breaking stress of 0.3 MPa or more and a breaking strain of 25.0 or more in a tensile test. In this way, if the polymer A further contains a polymer A2 whose breaking stress and breaking strain when formed into a film are each within the above-mentioned predetermined ranges, the flexibility of the obtained electrode can be further improved, and the IV characteristics can be maintained even in a wound secondary battery using the electrode.
[0014] [6] In the binder composition for a non-aqueous secondary battery electrode according to the above item [5], the mass ratio of the polymer A1 to the polymer A2 (polymer A1:polymer A2) is preferably 9: 1 or more and 1: 9 or less. As described above, when the mass ratio of the polymer A1 to the polymer A2 is within the above-mentioned range, the flexibility of the obtained electrode can be further improved, and the battery characteristics of a secondary battery using the electrode can be further improved.
[0015] [7] In the binder composition for a non-aqueous secondary battery electrode according to any one of [4] to [6] above, the polymer A1 preferably contains a nitrile group-containing monomer unit and an alkylene structural unit. Thus, if the polymer A1 contains a nitrile group-containing monomer unit and an alkylene structural unit, the flexibility of the resulting electrode can be further improved, and the IV characteristics of a wound secondary battery using the electrode can be further improved. In the present invention, the "monomer unit" of a polymer means "a repeating unit derived from the monomer contained in a polymer obtained using the monomer." Whether or not a polymer contains a predetermined structural unit or monomer unit can be determined by the following: 1 This can be determined using nuclear magnetic resonance (NMR) techniques such as H-NMR.
[0016] [8] In the binder composition for a non-aqueous secondary battery electrode according to any one of [5] to [7] above, the polymer A2 preferably contains a (meth)acrylic acid ester monomer unit. When the polymer A2 contains a (meth)acrylic acid ester monomer unit, the flexibility of the electrode can be further improved, and the battery characteristics of a secondary battery using the electrode can be further improved. In the present invention, "(meth)acrylic" means acrylic and / or methacrylic.
[0017] Another object of the present invention is to advantageously solve the above-mentioned problems, and the present invention provides a slurry composition for a non-aqueous secondary battery electrode, comprising [9] an electrode active material and any one of the binder compositions for a non-aqueous secondary battery electrode described above in [1] to [8]. In this way, by blending the binder composition for a non-aqueous secondary battery electrode described above with an electrode active material, a slurry composition for a non-aqueous secondary battery electrode can be easily obtained, which makes it possible to produce an electrode having excellent flexibility and can improve the battery characteristics of a secondary battery equipped with the obtained electrode.
[0018] Another object of the present invention is to advantageously solve the above-mentioned problems, and the present invention provides
[10] a non-aqueous secondary battery electrode including an electrode mixture layer formed using the non-aqueous secondary battery electrode slurry composition according to [9]. In this way, by using the above-mentioned non-aqueous secondary battery electrode slurry composition, a non-aqueous secondary battery electrode having excellent flexibility can be successfully produced, and the battery characteristics of a secondary battery using the non-aqueous secondary battery electrode can be improved.
[0019] Another object of the present invention is to advantageously solve the above-mentioned problems, and the present invention provides
[11] a nonaqueous secondary battery including the electrode for a nonaqueous secondary battery according to
[10] . In this way, the use of the electrode for a nonaqueous secondary battery described above can improve the battery characteristics of the secondary battery.
[0020] According to the present invention, there is provided a binder composition for a non-aqueous secondary battery electrode that can be suitably used to produce an electrode with excellent flexibility and that can improve the battery characteristics of a secondary battery including the resulting electrode. Furthermore, according to the present invention, there is provided a slurry composition for a non-aqueous secondary battery electrode that can form an electrode with excellent flexibility and can improve the battery characteristics of a secondary battery including the resulting electrode. Furthermore, according to the present invention, there is provided a non-aqueous secondary battery electrode that can improve the battery characteristics of a non-aqueous secondary battery, and a non-aqueous secondary battery with excellent battery characteristics.
[0021] Hereinafter, embodiments of the present invention will be described in detail. Herein, the binder composition for a non-aqueous secondary battery electrode of the present invention (hereinafter also simply referred to as the "binder composition") can be suitably used, for example, when preparing the slurry composition for a non-aqueous secondary battery electrode of the present invention (hereinafter also simply referred to as the "slurry composition"). Furthermore, the slurry composition for a non-aqueous secondary battery electrode of the present invention can be suitably used, for example, when manufacturing the electrode for a non-aqueous secondary battery of the present invention. Furthermore, the non-aqueous secondary battery of the present invention is characterized by using a non-aqueous secondary battery electrode formed using the slurry composition for a non-aqueous secondary battery electrode of the present invention. The binder composition for a non-aqueous secondary battery electrode and the slurry composition for a non-aqueous secondary battery electrode of the present invention can be particularly suitably used when forming a positive electrode for a non-aqueous secondary battery.
[0022] (Binder Composition for Nonaqueous Secondary Battery Electrodes) The binder composition of the present invention contains polymer A and, optionally, further contains at least one selected from a solvent and other components. The binder composition of the present invention is characterized in that, when formed into film X, the breaking stress [MPa] and breaking strain [-] of film X in a tensile test satisfy the relational expression 0.010≦breaking stress [MPa] / breaking strain [-]≦1.000. Therefore, when an electrode is manufactured by forming an electrode mixture layer on a current collector using a slurry composition prepared using the binder composition, the electrode can be imparted with a certain level of strength to function as an electrode while also being imparted with sufficient flexibility. As a result, the occurrence of cracks when the electrode is wound, etc., can be suppressed, and the battery characteristics of a secondary battery including the electrode can be improved.
[0023] <Polymer A> In an electrode produced by forming an electrode mixture layer on a current collector using a slurry composition prepared using a binder composition, polymer A is a component that has the function of imparting flexibility to the electrode while retaining components such as an electrode active material contained in the electrode mixture layer so that they do not detach from the electrode mixture layer.
[0024] <<Composition>> The polymer constituting polymer A is not particularly limited as long as it can exhibit the above-mentioned functions, and a polymer of any composition can be used. Polymer A may be composed of one type or two or more types of polymers. In the following, when polymer A is composed of two or more types of polymers, the content of structural units and / or monomer units in polymer A refers to the total content of structural units and / or monomer units in all polymers constituting polymer A. Examples of polymers suitable for use as polymer A include polymers containing at least one structural unit and / or monomer unit selected from the group consisting of nitrile group-containing monomer units, alkylene structural units, (meth)acrylic acid ester monomer units, hydrophilic group-containing monomer units, and aromatic vinyl monomers. Among these, from the viewpoint of further improving the flexibility of the obtained electrode and further improving the battery characteristics of the secondary battery, polymer A is preferably a polymer containing at least a nitrile group-containing monomer unit and an alkylene structural unit, more preferably a polymer containing a nitrile group-containing monomer unit, an alkylene structural unit, and at least one monomer unit selected from the group consisting of a (meth)acrylic acid ester monomer unit, a hydrophilic group-containing monomer unit, and an aromatic vinyl monomer unit, and even more preferably a polymer containing all of a nitrile group-containing monomer unit, an alkylene structural unit, and a (meth)acrylic acid ester monomer unit. Note that polymer A preferably does not contain a fluorine-containing monomer unit.
[0025] [Nitrile Group-Containing Monomer Unit] The nitrile group-containing monomer unit is a repeating unit derived from a nitrile group-containing monomer unit. Examples of nitrile group-containing monomers that can form the nitrile group-containing monomer unit include α,β-ethylenically unsaturated nitrile monomers. The α,β-ethylenically unsaturated nitrile monomer is not particularly limited as long as it is an α,β-ethylenically unsaturated compound having a nitrile group, and examples include acrylonitrile; α-halogenoacrylonitriles such as α-chloroacrylonitrile and α-bromoacrylonitrile; and α-alkylacrylonitriles such as methacrylonitrile and α-ethylacrylonitrile. Among these, acrylonitrile and methacrylonitrile are preferred as the nitrile group-containing monomer, with acrylonitrile being more preferred. These may be used alone or in combination of two or more.
[0026] The content of the nitrile group-containing monomer units in polymer A is preferably 5% by mass or more, more preferably 10% by mass or more, and preferably 40% by mass or less, and more preferably 30% by mass or less, when the total repeating units in polymer A (the sum of structural units and monomer units) is taken as 100% by mass. If the content of the nitrile group-containing monomer units in polymer A exceeds the above upper limit, flexibility may decrease and a coating may form on the conductive material, deteriorating IV characteristics. If the content of the nitrile group-containing monomer units in polymer A is less than the above lower limit, the solubility of polymer A may decrease during preparation of the slurry composition, deteriorating electrode formability. If the content of the nitrile group-containing monomer units is within the above specified range, the flexibility of the resulting electrode can be further improved, and the suitability for the secondary battery production process and battery characteristics can be further improved.
[0027] [Alkylene structural unit] The alkylene structural unit is represented by the general formula: -C n H 2n- [where n is an integer of 2 or greater]. When polymer A contains an alkylene structural unit, the flexibility of the resulting electrode can be further improved, and the battery characteristics of the secondary battery can be further improved.
[0028] The alkylene structural unit may be linear or branched, but from the viewpoint of further improving the flexibility of the resulting electrode, the alkylene structural unit is preferably linear, i.e., a linear alkylene structural unit. The alkylene structural unit has 4 or more carbon atoms (i.e., the alkylene structural unit represented by the above-mentioned general formula -C n H 2n -n is an integer of 4 or more).
[0029] The method for introducing alkylene structural units into polymer A is not particularly limited, and examples thereof include the following methods (1) and (2): (1) a method of preparing a polymer from a monomer composition containing a conjugated diene monomer and hydrogenating (adding hydrogen) the polymer to convert the conjugated diene monomer units into alkylene structural units; and (2) a method of preparing a polymer from a monomer composition containing a 1-olefin monomer. Among these, method (1) is preferred because it allows for easy production of the polymer.
[0030] That is, the alkylene structural unit is preferably a structural unit (conjugated diene hydride unit) obtained by hydrogenating (hydrogenating) a conjugated diene monomer unit, more preferably a structural unit (isoprene hydride unit) obtained by hydrogenating an isoprene unit or a structural unit (1,3-butadiene hydride unit) obtained by hydrogenating a 1,3-butadiene unit, and even more preferably a structural unit (1,3-butadiene hydride unit) obtained by hydrogenating a 1,3-butadiene unit. Here, hydrogenation can be carried out using a known method as described below. Furthermore, examples of 1-olefin monomers include 1-butene and 1-hexene. These conjugated diene monomers and 1-olefin monomers can be used alone or in combination of two or more.
[0031] Examples of the conjugated diene monomer that can be used in the above method (1) include conjugated diene compounds such as 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, etc. Among these, isoprene and 1,3-butadiene are preferred, and 1,3-butadiene is more preferred.
[0032] When an alkylene structural unit is introduced into polymer A via the above method (1), if the conjugated diene monomer unit is not completely hydrogenated, the conjugated diene monomer unit may remain in polymer A. In other words, polymer A may optionally contain a conjugated diene monomer unit as a repeating unit.
[0033] The total content of alkylene structural units and conjugated diene monomer units in polymer A is preferably 20% by mass or more, more preferably 25% by mass or more, and even more preferably 30% by mass or more, and preferably 70% by mass or less, more preferably 65% by mass or less, and even more preferably 60% by mass or less, when the total repeating units in polymer A (the sum of structural units and monomer units) is taken as 100% by mass. If the total content of alkylene structural units and conjugated diene monomer units in polymer A exceeds the upper limit, the solubility of polymer A during preparation of a slurry composition may be reduced, and electrode formability may be impaired. If the total content of alkylene structural units and conjugated diene monomer units in polymer A is less than the lower limit, it may be difficult to form a carbon conductive path, resulting in poor IV characteristics. In addition, the flexibility of the electrode may be impaired. When the total content ratio of the alkylene structural unit and the conjugated diene monomer unit is within the above-mentioned range, the flexibility of the obtained electrode can be further improved, and the battery characteristics of the secondary battery can be further improved.
[0034] In addition, when polymer A does not contain conjugated diene monomer units, for example, when the conjugated diene monomer units are completely hydrogenated by the above method (1), or when polymer A is produced by the above method (2), the content of alkylene structural units in polymer A is preferably 20% by mass or more, more preferably 25% by mass or more, and even more preferably 30% by mass or more, and preferably 70% by mass or less, more preferably 65% by mass or less, and even more preferably 60% by mass or less, when the total repeating units in polymer A (the sum of structural units and monomer units) is taken as 100% by mass. If the content of alkylene structural units in polymer A exceeds the above upper limit, the solubility of polymer A during preparation of a slurry composition may be reduced, and electrode formability may be impaired. On the other hand, if the content of alkylene structural units in polymer A is less than the above lower limit, it may be difficult to form a carbon conductive path, resulting in poor IV characteristics. Furthermore, there is a risk of electrode flexibility being impaired. If the content ratio of the alkylene structural unit is within the above-mentioned range, the flexibility of the obtained electrode can be further improved, and the battery characteristics of the secondary battery can be further improved.
[0035] -(Meth)acrylic acid ester monomer unit- The (meth)acrylic acid ester monomer unit is a repeating unit derived from a (meth)acrylic acid ester monomer.
[0036] Examples of the (meth)acrylic acid ester monomer include alkyl acrylates such as methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, t-butyl acrylate, isobutyl acrylate, n-pentyl acrylate, isopentyl acrylate, hexyl acrylate, heptyl acrylate, octyl acrylate, 2-ethylhexyl acrylate, nonyl acrylate, decyl acrylate, lauryl acrylate, n-tetradecyl acrylate, stearyl acrylate, and cyclohexyl acrylate; methacrylate alkyl esters such as methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, t-butyl methacrylate, isobutyl methacrylate, n-pentyl methacrylate, isopentyl methacrylate, hexyl methacrylate, heptyl methacrylate, octyl methacrylate, 2-ethylhexyl methacrylate, nonyl methacrylate, decyl methacrylate, lauryl methacrylate, n-tetradecyl methacrylate, stearyl methacrylate, and cyclohexyl methacrylate. Among these, n-butyl acrylate or ethyl acrylate is preferred, and ethyl acrylate is more preferred.
[0037] The content of the (meth)acrylic acid ester monomer units in polymer A is preferably 20% by mass or more, more preferably 30% by mass or more, and preferably 60% by mass or less, more preferably 50% by mass or less, and even more preferably 40% by mass or less, when the total repeating units in polymer A (the sum of structural units and monomer units) is taken as 100% by mass. If the content of the (meth)acrylic acid ester monomer units in polymer A exceeds the above upper limit, the degree of swelling in the electrolyte may increase, and the IV characteristics may deteriorate. If the content of the (meth)acrylic acid ester monomer units in polymer A is less than the above lower limit, the flexibility of the electrode may deteriorate. If the content of the (meth)acrylic acid ester monomer units is within the above specified range, the flexibility of the obtained electrode can be further improved, and the battery characteristics of the secondary battery can be further improved.
[0038] [Hydrophilic Group-Containing Monomer Unit] The hydrophilic group-containing monomer unit is a repeating unit derived from a hydrophilic group-containing monomer. Examples of the hydrophilic group-containing monomer that can form the hydrophilic group-containing monomer unit include a monomer having a carboxylic acid group, a monomer having a sulfonic acid group, a monomer having a phosphoric acid group, and a monomer having a hydroxyl group.
[0039] Examples of monomers having a carboxylic acid group include monocarboxylic acids and their derivatives, dicarboxylic acids and their acid anhydrides, and their derivatives. Examples of monocarboxylic acids include acrylic acid, methacrylic acid, and crotonic acid. Examples of monocarboxylic acid derivatives include 2-ethylacrylic acid, isocrotonic acid, α-acetoxyacrylic acid, β-trans-aryloxyacrylic acid, α-chloro-β-E-methoxyacrylic acid, and β-diaminoacrylic acid. Examples of dicarboxylic acids include maleic acid, fumaric acid, and itaconic acid. Examples of dicarboxylic acid derivatives include methylmaleic acid, dimethylmaleic acid, phenylmaleic acid, chloromaleic acid, dichloromaleic acid, fluoromaleic acid, and maleic acid esters such as methylallyl maleate, diphenyl maleate, nonyl maleate, decyl maleate, dodecyl maleate, octadecyl maleate, and fluoroalkyl maleates. Examples of dicarboxylic acid anhydrides include maleic anhydride, acrylic anhydride, methylmaleic anhydride, and dimethylmaleic anhydride. Further, as the monomer having a carboxylic acid group, an acid anhydride that generates a carboxyl group upon hydrolysis can also be used.Other examples include monoesters and diesters of α,β-ethylenically unsaturated polycarboxylic acids such as monoethyl maleate, diethyl maleate, monobutyl maleate, dibutyl maleate, monoethyl fumarate, diethyl fumarate, monobutyl fumarate, dibutyl fumarate, monocyclohexyl fumarate, dicyclohexyl fumarate, monoethyl itaconate, diethyl itaconate, monobutyl itaconate, and dibutyl itaconate.
[0040] Examples of the monomer having a sulfonic acid group include vinyl sulfonic acid, methyl vinyl sulfonic acid, (meth)allyl sulfonic acid, styrene sulfonic acid, (meth)acrylic acid-2-ethyl sulfonate, 2-acrylamido-2-methylpropanesulfonic acid, 3-allyloxy-2-hydroxypropanesulfonic acid, etc. In the present invention, "(meth)allyl" means allyl and / or methallyl.
[0041] Examples of the monomer having a phosphate group include 2-(meth)acryloyloxyethyl phosphate, methyl-2-(meth)acryloyloxyethyl phosphate, ethyl-(meth)acryloyloxyethyl phosphate, vinylphosphonic acid, dimethyl vinylphosphonate, etc. In the present invention, "(meth)acryloyl" means acryloyl and / or methacryloyl.
[0042] Examples of the monomer having a hydroxyl group include ethylenically unsaturated alcohols such as (meth)allyl alcohol, 3-butene-1-ol, and 5-hexene-1-ol; alkanol esters of ethylenically unsaturated carboxylic acids such as 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, di-2-hydroxyethyl maleate, di-4-hydroxybutyl maleate, and di-2-hydroxypropyl itaconate; and compounds of the general formula: CH 2 =CR 1 -COO-(C n H 2n O) m-H (wherein m is an integer of 2 to 9, n is an integer of 2 to 4, and R1 represents hydrogen or a methyl group), and esters of (meth)acrylic acid; mono(meth)acrylic acid esters of dihydroxy esters of dicarboxylic acids such as 2-hydroxyethyl-2'-(meth)acryloyloxyphthalate and 2-hydroxyethyl-2'-(meth)acryloyloxysuccinate; vinyl ethers such as 2-hydroxyethyl vinyl ether and 2-hydroxypropyl vinyl ether; (meth)allyl-2-hydroxyethyl ether, (meth)allyl-2-hydroxypropyl ether, (meth)allyl-3-hydroxypropyl ether, (meth)allyl-2-hydroxybutyl ether, (meth)allyl-3-hydroxybutyl ether, (meth)allyl-4-hydroxybutyl ether, (meth)allyl-6-hydroxyethyl ether, mono(meth)allyl ethers of alkylene glycols such as diethylene glycol mono(meth)allyl ether and dipropylene glycol mono(meth)allyl ether; mono(meth)allyl ethers of halogen- and hydroxy-substituted (poly)alkylene glycols such as glycerin mono(meth)allyl ether, (meth)allyl-2-chloro-3-hydroxypropyl ether and (meth)allyl-2-hydroxy-3-chloropropyl ether; mono(meth)allyl ethers of polyhydric phenols such as eugenol and isoeugenol, and halogen-substituted products thereof; (meth)allyl thioethers of alkylene glycols such as (meth)allyl-2-hydroxyethyl thioether and (meth)allyl-2-hydroxypropyl thioether; and the like.
[0043] The content of the hydrophilic group-containing monomer units in polymer A is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and preferably 5% by mass or less, and more preferably 3% by mass or less, when the total repeating units (the total of structural units and monomer units) in polymer A is taken as 100% by mass. If the content of the hydrophilic group-containing monomer units in polymer A is within the above range, the manufacturability of polymer A can be improved, and by suppressing coating of the active material, the rate characteristics of the secondary battery can be improved.
[0044] -Aromatic vinyl monomer unit- The aromatic vinyl monomer unit is a repeating unit derived from an aromatic vinyl monomer. Examples of aromatic vinyl monomers that can form the aromatic vinyl monomer unit include styrene, α-methylstyrene, vinyltoluene, and divinylbenzene. These can be used alone or in combination of two or more.
[0045] The content of aromatic vinyl monomer units in polymer A is preferably 1% by mass or more, more preferably 3% by mass or more, and preferably 30% by mass or less, and more preferably 20% by mass or less, when the total repeating units (the sum of structural units and monomer units) in polymer A is taken as 100% by mass. Within the above ranges, the electrochemical stability of polymer A can be increased, and coating of the conductive material can be suppressed, thereby improving the rate characteristics of the secondary battery.
[0046] <<Properties>> [Break Stress] When polymer A is formed into film Y, the break stress of film Y in a tensile test (hereinafter sometimes simply referred to as "break stress") is preferably 0.3 MPa or more, preferably 0.5 MPa or more, more preferably 1.0 MPa or more, and preferably 20 MPa or less, more preferably 15 MPa or less, and even more preferably 10 MPa or less. If the break stress exceeds the upper limit, the rigidity may be too high and the flexibility of the electrode may be reduced. On the other hand, if the break stress is below the lower limit, it may be difficult to maintain the electrode mixture layer, which may deteriorate the cycle characteristics of the secondary battery. If the break stress is within the above range, the strength and flexibility of the obtained electrode can be well combined, and the battery characteristics of the secondary battery can be further improved. The break stress of polymer A can be controlled, for example, by changing the composition, molecular weight, polymer chain branching, and monomer sequence of polymer A.
[0047] [Break Strain] When polymer A is formed into film Y, the break strain of film Y in a tensile test (hereinafter sometimes simply referred to as "break strain") is preferably 6.0 or more, more preferably 8.0 or more, more preferably 10.0 or more, and preferably 80 or less, more preferably 70 or less, and even more preferably 60 or less. If the break strain exceeds the upper limit, it may be difficult to maintain the electrode mixture layer, which may deteriorate the cycle characteristics of the secondary battery. If the break strain is below the lower limit, the flexibility of the electrode may deteriorate. If the break strain is within the above range, the strength and flexibility of the obtained electrode can be satisfactorily achieved, while the battery characteristics of the secondary battery can be further improved. The break strain of polymer A can be controlled, for example, by changing the composition, molecular weight distribution, and entanglement density of polymer A.
[0048] [Iodine Value] The iodine value of polymer A is preferably 5 mg / 100 mg or more, more preferably 10 mg / 100 mg or more, preferably 30 mg / 100 mg or less, more preferably 25 mg / 100 mg or less, and even more preferably 20 mg / 100 mg or less. When the iodine value is within the above range, the electrochemical stability of polymer A is improved, and the cycle characteristics of the secondary battery can be improved. The iodine value of polymer A can be measured by the method described in the Examples. The iodine value of polymer A can be controlled, for example, based on the amount of hydrogenation catalyst used when hydrogenating the polymer in the preparation of polymer A and / or the hydrogenation conditions (pressure and time).
[0049] <<Combination of Types of Polymer A>> From the viewpoint of further improving the flexibility of the resulting electrode and further improving the battery characteristics of the secondary battery, it is preferable that the polymer A contains two or more types of polymers. Specifically, it is preferable that the polymer A contains two or more types of polymers that differ in at least one property selected from the group consisting of composition, breaking stress, breaking strain, iodine value, molecular weight, and glass transition temperature. In particular, the polymer A preferably contains two types of polymers A1 and A2 that differ in at least one property selected from the group consisting of composition, breaking stress, breaking strain, iodine value, molecular weight, and glass transition temperature, more preferably two types of polymers A1 and A2 that differ in composition and / or breaking strain, even more preferably two types of polymers A1 and A2 that differ in at least one property selected from the group consisting of composition, breaking stress, breaking strain, iodine value, molecular weight, and glass transition temperature, and particularly preferably two types of polymers A1 and A2 that differ in composition and / or breaking strain.
[0050] A preferred example of a combination of polymers A1 and A2 having different compositions is a combination of, for example, a polymer containing a nitrile group-containing monomer unit and an alkylene structural unit as polymer A1; and a polymer containing at least one structural unit and / or monomer unit selected from the group consisting of a nitrile group-containing monomer unit, an alkylene structural unit, a (meth)acrylic acid ester monomer unit, a hydrophilic group-containing monomer unit, and an aromatic vinyl monomer unit as polymer A2. Among these, a more preferred combination is a polymer containing a nitrile group-containing monomer unit and an alkylene structural unit as polymer A1; and a polymer containing a (meth)acrylic acid ester monomer unit as polymer A2.
[0051] Specifically, polymer A1 is preferably a polymer containing a nitrile group-containing monomer unit and an alkylene structural unit, and more preferably a polymer consisting of a nitrile group-containing monomer unit and an alkylene structural unit.
[0052] Here, the content of nitrile group-containing monomer units in polymer A1 is preferably 20% by mass or more, more preferably 25% by mass or more, and preferably 50% by mass or less, and more preferably 40% by mass or less, when all repeating units in polymer A1 (the sum of structural units and monomer units) are taken as 100% by mass. The content of alkylene structural units in polymer A1 is preferably 50% by mass or more, more preferably 60% by mass or more, and preferably 80% by mass or less, and more preferably 75% by mass or less, when all repeating units in polymer A1 (the sum of structural units and monomer units) are taken as 100% by mass. Furthermore, the total content of alkylene structural units and conjugated diene monomer units in polymer A1 is preferably 50% by mass or more, more preferably 60% by mass or more, and preferably 80% by mass or less, and more preferably 75% by mass or less, when all repeating units in polymer A1 (the sum of structural units and monomer units) are taken as 100% by mass.
[0053] When polymer A1 is formed into film Y, the breaking strain is preferably 6.0 or more, more preferably 10.0 or more, and preferably less than 25.0, more preferably 20.0 or less. When polymer A1 is formed into film Y, the breaking stress is preferably 0.3 MPa or more, more preferably 0.5 MPa or more, and preferably 3.0 MPa or less, more preferably 2.0 MPa or less.
[0054] As polymer A2, a polymer containing at least one structural unit and / or monomer unit selected from the group consisting of a nitrile group-containing monomer unit, an alkylene structural unit, a (meth)acrylic acid ester monomer unit, a hydrophilic group-containing monomer unit, and an aromatic vinyl monomer unit is preferred, and a polymer containing a (meth)acrylic acid ester monomer unit is more preferred.
[0055] Here, the content of nitrile group-containing monomer units in polymer A2 is preferably 10% by mass or more, more preferably 15% by mass or more, and preferably 30% by mass or less, and more preferably 25% by mass or less, when all repeating units in polymer A2 (the sum of structural units and monomer units) are taken as 100% by mass. The content of alkylene structural units in polymer A2 is preferably 20% by mass or more, more preferably 30% by mass or more, and preferably 60% by mass or less, and more preferably 50% by mass or less, when all repeating units in polymer A2 (the sum of structural units and monomer units) are taken as 100% by mass. Furthermore, the total content of alkylene structural units and conjugated diene monomer units in polymer A2 is preferably 20% by mass or more, more preferably 30% by mass or more, and preferably 60% by mass or less, and more preferably 50% by mass or less, when all repeating units in polymer A2 (the sum of structural units and monomer units) are taken as 100% by mass. The content of (meth)acrylic acid ester monomer units in polymer A2 is preferably 20% by mass or more, more preferably 30% by mass or more, and is preferably 60% by mass or less, more preferably 50% by mass or less, when the total amount of repeating units in polymer A2 (the total amount of structural units and monomer units) is taken as 100% by mass.
[0056] When polymer A2 is formed into film Y, the breaking strain is preferably 20.0 or more, more preferably 25 or more, and preferably 80 or less, more preferably 75 or less. When polymer A2 is formed into film Y, the breaking stress is preferably 0.3 MPa or more, more preferably 0.5 MPa or more, and preferably 3.0 MPa or less, more preferably 2.0 MPa or less.
[0057] From the viewpoint of further improving the flexibility of the obtained electrode and further improving the battery characteristics of the secondary battery, the mass ratio of polymer A1 to polymer A2 (polymer A1:polymer A2) is preferably 9:1 or more and 1:9 or less, and more preferably 2:8 or more and 8:2 or less.
[0058] For example, the mass ratio (polymer A1:polymer A2) of polymer A1 having a breaking strain of 6.0 or more and less than 25.0 to polymer A2 having a breaking strain of 25.0 or more is preferably 9:1 or more and 1:9 or less, and more preferably 2:8 or more and 8:2 or less.
[0059] When polymer A contains a polymer other than polymers A1 and A2, the content of the polymer other than polymers A1 and A2 in polymer A is usually preferably 15 mass% or less. The polymer other than polymers A1 and A2 is not particularly limited as long as it does not inhibit the manifestation of the desired effects of the present invention.
[0060] <<Method for Preparing Polymer A>> The method for producing the above-mentioned polymer A is not particularly limited, and any method such as solution polymerization, suspension polymerization, bulk polymerization, or emulsion polymerization can be used. Furthermore, addition polymerization such as ionic polymerization, radical polymerization, or living radical polymerization can be used as the polymerization initiator. Furthermore, known polymerization initiators can be used as the polymerization initiator.
[0061] In the polymerization, it is preferable to use a molecular weight modifier having a sulfur-containing group such as a mercapto group. Examples of the compound having a mercapto group as a molecular weight regulator include compounds having a mercapto group having 8 to 12 carbon atoms, such as octyl mercaptan, 2,2,4,6,6-pentamethyl-4-heptanethiol, 2,4,4,6,6-pentamethyl-2-heptanethiol, 2,3,4,6,6-pentamethyl-2-heptanethiol, 2,3,4,6,6-pentamethyl-3-heptanethiol, t-dodecyl mercaptan, and n-dodecyl mercaptan; and compounds having a mercapto group, such as 2,2,4,6,6-pentamethyl-4-octanethiol, 2,2,4,6,6,8,8-heptamethyl-4-nonanethiol, bis(2-mercaptoethyl)sulfide, methyl 3-mercaptopropionate, and 1-butanethiol. Among these, compounds having a mercapto group and having 8 to 12 carbon atoms are preferred, and t-dodecyl mercaptan is more preferred. The amount of the compound having a mercapto group used as a molecular weight regulator can be adjusted as appropriate.
[0062] Furthermore, when the above-mentioned polymer is produced by the above-mentioned method (1), it is preferable to use radical polymerization using a redox polymerization initiator containing an iron-based compound as the polymerization method for the polymer to be hydrogenated. The redox polymerization initiator is not particularly limited, and for example, a combination of cumene hydroperoxide, ethylenediaminetetraacetic acid monosodium iron, sodium hydroxymethanesulfinate, and ethylenediaminetetraacetic acid tetrasodium salt (EDTA.4Na) can be used.
[0063] When the above-mentioned polymer A is produced by the above-mentioned method (1), after emulsion polymerization, a coagulant may be added to the obtained aqueous dispersion of the polymer before hydrogenation (i.e., the precursor of polymer A) to coagulate it, and the pre-hydrogenation polymer may be recovered, and the recovered polymer may be hydrogenated (optionally after carrying out the "metathesis reaction" described below).
[0064] The hydrogenation can be carried out by a known hydrogenation method such as an oil phase hydrogenation method or an aqueous phase hydrogenation method. The catalyst used for the hydrogenation can be any known selective hydrogenation catalyst, and can include palladium-based catalysts and rhodium-based catalysts. Two or more of these catalysts can be used in combination.
[0065] The hydrogenation of the polymer may be carried out, for example, using the method described in Japanese Patent No. 4509792. Specifically, the hydrogenation of the polymer may be carried out after carrying out a metathesis reaction of the polymer in the presence of a catalyst and a co-olefin. Here, known ruthenium-based catalysts can be used as the catalyst for the metathesis reaction. Among them, it is preferable to use a Grubbs catalyst such as bis(tricyclohexylphosphine)benzylidene ruthenium dichloride or 1,3-bis(2,4,6-trimethylphenyl)-2-(imidazolidinylidene)(dichlorophenylmethylene)(tricyclohexylphosphine)ruthenium as the catalyst for the metathesis reaction. Furthermore, olefins having 2 to 16 carbon atoms such as ethylene, isobutane, and 1-hexane can be used as the co-olefin. Furthermore, the hydrogenation catalyst used in hydrogenation after the metathesis reaction can be, for example, a Wilkinson catalyst (PPh 3 ) 3 Known homogeneous hydrogenation catalysts such as RhCl can be used.
[0066] <Solvent> The solvent contained in the binder composition is not particularly limited, and either water or an organic solvent can be used. Examples of organic solvents include N-methylpyrrolidone (hereinafter also simply referred to as "NMP"), N,N-dimethylformamide, and acetone. From the viewpoint of improving the stability of the binder composition and the electrode manufacturability, it is preferable to use N-methylpyrrolidone as the organic solvent. Note that one type of solvent may be used alone, or two or more types may be mixed in any ratio.
[0067] <Other Components> Examples of other components that may be optionally contained in the binder composition of the present invention include dispersants, reinforcing materials, leveling agents, viscosity modifiers, electrolyte additives, etc. These are not particularly limited as long as they do not affect the battery reaction, and known components, such as those described in WO 2012 / 115096, can be used. Furthermore, these components may be used alone or in combination of two or more types in any ratio.
[0068] <Physical Properties of Binder Composition> [Break Stress [MPa] / Break Strain [-]] As described above, when the binder composition of the present invention is formed into film X, the break stress [MPa] and break strain [-] of film X measured in a tensile test must satisfy the relational expression 0.010≦break stress [MPa] / break strain [-]≦1.000. If the value of break stress [MPa] / break strain [-] is less than 0.001, the battery characteristics (particularly cycle characteristics) of the resulting secondary battery will deteriorate. On the other hand, if the value of break stress [MPa] / break strain [-] is more than 1.000, the resulting electrode will not be imparted with sufficient flexibility, and cracking of the electrode will not be sufficiently suppressed, resulting in deterioration of the battery characteristics of the secondary battery. From the viewpoint of further improving the flexibility of the obtained electrode and further improving the battery characteristics of the obtained secondary battery, the binder composition of the present invention, when formed into film X, preferably has a value of the breaking stress [MPa] / breaking strain [−] of 0.050 or more, more preferably 0.267 or more, and preferably 0.800 or less, more preferably 0.769 or less.
[0069] [Breaking Stress] From the viewpoint of further improving the flexibility of the obtained electrode and further improving the battery characteristics of the obtained secondary battery, when the binder composition of the present invention is formed into film X, the breaking stress of the film X in a tensile test is preferably 0.3 MPa or more, more preferably 0.5 MPa or more, and preferably 10 MPa or less. The breaking stress of the binder composition can be controlled, for example, by changing the composition of polymer A, the mass ratio of polymer A1 to polymer A2, or the solvent.
[0070] [Break Strain] From the viewpoint of further improving the flexibility of the obtained electrode and further improving the battery characteristics of the obtained secondary battery, when the binder composition of the present invention is formed into film X, the break strain of the film X in a tensile test is preferably 6.0 or more, more preferably 8.0 or more, and even more preferably 13.5 or more, and is preferably 80 or less, more preferably 70 or less, and even more preferably 35 or less. The break strain of the binder composition can be controlled, for example, by changing the composition of polymer A, the mass ratio of polymer A1 to polymer A2, or the solvent.
[0071] <Preparation of Binder Composition> When the binder composition of the present invention contains a solvent, it can be prepared by dissolving or dispersing the above-mentioned polymer A and any other components described above in the solvent. Specifically, the binder composition can be prepared by mixing the above-mentioned components and the solvent using a mixer such as a ball mill, sand mill, bead mill, pigment disperser, crusher, ultrasonic disperser, homogenizer, planetary mixer, or Filmix. When the polymer A is prepared in the form of an aqueous dispersion, the aqueous dispersion may be used as the binder composition as is, or the binder composition may be obtained by mixing the aqueous dispersion of the polymer A with an organic solvent and then removing the water.
[0072] (Slurry Composition for Non-Aqueous Secondary Battery Electrode) The slurry composition of the present invention contains the binder composition of the present invention described above and an electrode active material, and optionally further contains at least one selected from a conductive material, a solvent, and other components. Since the slurry composition of the present invention contains the binder composition of the present invention described above, an electrode with excellent flexibility can be produced. Furthermore, the slurry composition of the present invention can enable a secondary battery to exhibit excellent battery characteristics. Hereinafter, a case where the slurry composition for a non-aqueous secondary battery electrode is a slurry composition for a lithium-ion secondary battery positive electrode will be described as an example, but the present invention is not limited to the following example.
[0073] The binder composition is the binder composition for a non-aqueous secondary battery electrode of the present invention. The content of the binder composition in the slurry composition of the present invention (solid content equivalent) can be, for example, 0.1 mass % to 5 mass % relative to the total solid content of the slurry composition (100 mass %).
[0074] <Electrode Active Material> An electrode active material is a material that transfers electrons at an electrode of a secondary battery. As a positive electrode active material for a lithium ion secondary battery, a material that can absorb and release lithium is usually used.
[0075] Specifically, the positive electrode active material for a lithium ion secondary battery is not particularly limited, and may be a lithium-containing cobalt oxide (LiCoO 2 ), lithium manganese oxide (LiMn 2 O 4 ), lithium-containing nickel oxide (LiNiO 2 ), Co—Ni—Mn lithium-containing composite oxide (Li(Co, Mn, Ni)O 2 ), lithium-containing composite oxide of Ni-Mn-Al, lithium-containing composite oxide of Ni-Co-Al, olivine-type lithium iron phosphate (LiFePO 4 ), olivine-type lithium manganese phosphate (LiMnPO 4 ), Li 2 MnO 3 -LiNiO 2 system solid solution, Li 1+x Mn 2-x O 4 (0<X<2) Lithium-excess spinel compound represented by Li[Ni 0.17 Li 0.2 Co 0.07 Mn 0.56 ]O 2 , LiNi 0.5 Mn 1.5 O 4 , LiNi 0.5 Mn 0.3 Co 0.2 O 2Examples of known positive electrode active materials include the above. The particle size of the positive electrode active material is not particularly limited and can be the same as that of conventionally used positive electrode active materials. The content of the positive electrode active material in the slurry composition can be, for example, 90% by mass or more and 99% by mass or less, where the total solid content in the slurry composition is 100% by mass.
[0076] <Conductive Material> The conductive material that may be contained in the slurry composition of the present invention is intended to ensure electrical contact between electrode active materials. Examples of conductive materials that can be used include carbon black (e.g., acetylene black, Ketjen Black (registered trademark), furnace black, etc.), single-walled or multi-walled carbon nanotubes (multi-walled carbon nanotubes include cup-stacked types), carbon nanohorns, vapor-grown carbon fibers, milled carbon fibers obtained by calcining and then crushing polymer fibers, single-walled or multi-walled graphene, and carbon nonwoven fabric sheets obtained by calcining nonwoven fabrics made of polymer fibers; and various metal fibers or foils. Among these, acetylene black is preferred. These materials can be used alone or in combination of two or more. The particle size of the conductive material is not particularly limited and can be the same as that of conventionally used conductive materials. The content of the conductive material in the slurry composition can be, for example, 0.1% by mass or more to 3% by mass or less, based on 100% by mass of the total solids content of the slurry composition.
[0077] <Other Components> Other components that can be incorporated into the slurry composition are not particularly limited, and examples thereof include the same components as those that can be incorporated into the binder composition of the present invention. Furthermore, one type of other component may be used alone, or two or more types may be used in combination at any ratio. In particular, when the slurry composition is a slurry composition for a lithium-ion secondary battery positive electrode, it is preferable to use, in addition to the above-mentioned polymer A, a binder other than polymer A (for example, a fluorine-containing polymer such as polyvinylidene fluoride (PVdF) or polytetrafluoroethylene (PTFE)). When the slurry composition contains one or more binders in addition to the above-mentioned polymer A, the proportion of the above-mentioned polymer A can be 10 parts by mass or more and 90 parts by mass or less, assuming that the total content of such one or more binders is 100 parts by mass. When the content of the above-mentioned polymer A in the slurry composition is equal to or greater than the above-mentioned lower limit, the flexibility of the electrode can be improved, and the battery characteristics of the resulting secondary battery can be improved. Furthermore, when the content of the polymer A is equal to or less than the upper limit, the adhesiveness of the electrode mixture layer (positive electrode mixture layer) can be improved.
[0078] <Preparation of Slurry Composition> The method for preparing the slurry composition is not particularly limited. The slurry composition of the present invention can be prepared, for example, by mixing the binder composition of the present invention described above, an electrode active material, and optionally, a conductive material and / or other components in the presence of a solvent. The solvent can be the same as the solvent described above in the binder composition section. The solvent can be the same as the solvent contained in the binder composition, or it can be a newly added solvent. The mixing method used to prepare the slurry composition is not particularly limited, and mixers such as a ball mill, sand mill, bead mill, pigment disperser, crusher, ultrasonic disperser, homogenizer, planetary mixer, and Filmix can be used.
[0079] (Electrode for Non-Aqueous Secondary Battery) The electrode for a non-aqueous secondary battery of the present invention comprises a current collector and an electrode mixture layer formed on the current collector, the electrode mixture layer being formed using the above-described slurry composition of the present invention. That is, the electrode mixture layer is a dried product of the above-described slurry composition of the present invention, and contains at least polymer A and an electrode active material, and optionally further contains at least one selected from the group consisting of a conductive material and other components. Note that the components contained in the electrode mixture layer are those contained in the above-described slurry composition, and the preferred abundance ratio of each component is the same as the preferred abundance ratio of each component in the slurry composition. Note that the above-described polymer A may be in a particle form or another form in the electrode mixture layer. Furthermore, the electrode for a non-aqueous secondary battery of the present invention is formed using a slurry composition containing the binder composition of the present invention, and therefore has excellent flexibility. Furthermore, use of this electrode can result in a secondary battery with excellent battery characteristics.
[0080] <Method for manufacturing electrode> The electrode for a non-aqueous secondary battery of the present invention is manufactured, for example, through a step of applying the above-described slurry composition onto a current collector (application step) and a step of drying the slurry composition applied onto the current collector to form an electrode mixture layer on the current collector (drying step).
[0081] [Coating Step] The method for applying the slurry composition to the current collector is not particularly limited, and known methods can be used. Specifically, examples of the coating method include a doctor blade method, a dipping method, a reverse roll method, a direct roll method, a gravure method, an extrusion method, and a brush coating method. In this case, the slurry composition may be applied to only one side of the current collector, or may be applied to both sides. The thickness of the slurry film on the current collector after application and before drying can be appropriately set depending on the thickness of the electrode mixture layer obtained by drying.
[0082] Here, the current collector to which the slurry composition is applied is made of a material that is electrically conductive and electrochemically durable. Specifically, the current collector may be made of, for example, iron, copper, aluminum, nickel, stainless steel, titanium, tantalum, gold, platinum, etc. Note that one of the above materials may be used alone, or two or more may be used in combination in any ratio.
[0083] [Drying Step] The method for drying the slurry composition on the current collector is not particularly limited and any known method can be used, for example, drying with warm air, hot air, or low-humidity air, vacuum drying, or drying by irradiation with infrared rays or electron beams, etc. By drying the slurry composition on the current collector in this manner, an electrode mixture layer can be formed on the current collector, and a secondary battery electrode including the current collector and the electrode mixture layer can be obtained.
[0084] After the drying step, the electrode mixture layer may be subjected to a pressure treatment using a mold press, a roll press, or the like. The pressure treatment can improve the adhesion between the electrode mixture layer and the current collector. Furthermore, when the electrode mixture layer contains a curable polymer, it is preferable to cure the polymer after the electrode mixture layer is formed.
[0085] (Nonaqueous secondary battery) The nonaqueous secondary battery of the present invention includes the nonaqueous secondary battery electrode of the present invention. More specifically, the nonaqueous secondary battery of the present invention includes a positive electrode, a negative electrode, an electrolyte, and a separator, and uses the nonaqueous secondary battery electrode of the present invention as at least one of the positive electrode and the negative electrode. The nonaqueous secondary battery of the present invention has excellent battery characteristics because it includes the nonaqueous secondary battery electrode of the present invention. Note that the nonaqueous secondary battery of the present invention preferably uses the nonaqueous secondary battery electrode of the present invention as the positive electrode. In addition, the following description will be given of a case where the secondary battery is a lithium ion secondary battery as an example, but the present invention is not limited to the following example.
[0086] <Electrode> Electrodes other than the above-described electrodes for non-aqueous secondary batteries that can be used in the non-aqueous secondary battery of the present invention are not particularly limited, and known electrodes used in the manufacture of non-aqueous secondary batteries can be used. Specifically, electrodes other than the above-described electrodes for non-aqueous secondary batteries can be electrodes formed by forming an electrode mixture layer on a current collector using a known manufacturing method.
[0087] <Electrolyte> As the electrolyte, an organic electrolyte solution in which a supporting electrolyte is dissolved in an organic solvent is usually used. As the supporting electrolyte of a lithium ion secondary battery, for example, a lithium salt is used. As the lithium salt, for example, LiPF 6 , LiAsF 6 , LiBF 4 , LiSbF 6 , LiAlCl 4 , LiClO 4 , C.F. 3 SO 3 Li, C 4 F 9 SO 3 Li, CF 3 COOLi, (CF 3 CO) 2 NLi, (CF 3 SO 2 ) 2 NLi, (C 2 F 5 SO 2 Among them, LiPF is particularly preferred because it is easily soluble in solvents and shows a high degree of dissociation. 6 , LiClO 4 , C.F. 3 SO 3 Li is preferred, and LiPF 6 is particularly preferred. Note that one type of electrolyte may be used alone, or two or more types may be used in combination in any ratio. Generally, the lithium ion conductivity tends to increase as the supporting electrolyte with a higher degree of dissociation is used, so the lithium ion conductivity can be adjusted by the type of supporting electrolyte.
[0088] The organic solvent used in the electrolyte is not particularly limited as long as it can dissolve the supporting electrolyte. For example, carbonates such as dimethyl carbonate (DMC), ethylene carbonate (EC), diethyl carbonate (DEC), propylene carbonate (PC), butylene carbonate (BC), and ethyl methyl carbonate (EMC) are suitable. Other suitable solvents include esters such as γ-butyrolactone and methyl formate, ethers such as 1,2-dimethoxyethane and tetrahydrofuran, and sulfur-containing compounds such as sulfolane and dimethyl sulfoxide. Mixtures of these solvents may also be used. Among these, carbonates are preferred because of their high dielectric constant and wide stable potential range, and a mixture of ethylene carbonate and diethyl carbonate is even more preferred. The concentration of the electrolyte in the electrolyte can be adjusted as appropriate. Known additives, such as vinylene carbonate, can also be added to the electrolyte.
[0089] <Separator> The separator is not particularly limited, and for example, those described in JP 2012-204303 A can be used. Among these, a microporous film made of a polyolefin resin (polyethylene, polypropylene, polybutene, polyvinyl chloride) is preferred because it allows the thickness of the entire separator to be thin, thereby increasing the proportion of electrode active material in the secondary battery and increasing the capacity per volume.
[0090] <Method for Manufacturing Non-Aqueous Secondary Battery> The non-aqueous secondary battery of the present invention can be manufactured, for example, by stacking a positive electrode and a negative electrode with a separator interposed therebetween, rolling or folding the resulting assembly as needed according to the battery shape, placing it in a battery container, injecting an electrolyte into the battery container, and sealing it. To prevent internal pressure increases, overcharging and overdischarging, and the like, a fuse, an overcurrent protection element such as a PTC element, an expanded metal, a lead plate, or the like may be provided as needed. The shape of the secondary battery may be, for example, any of a coin type, a button type, a sheet type, a cylindrical type, a rectangular type, a flat type, and the like.
[0091] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the following description, the terms "%" and "parts" used to represent amounts are based on mass unless otherwise specified. In a polymer produced by copolymerizing multiple types of monomers, the proportion of a monomer unit formed by polymerizing a certain monomer in the polymer usually corresponds to the proportion (feed ratio) of the certain monomer relative to all monomers used in the polymerization of the polymer, unless otherwise specified. In a polymer produced by hydrogenating a polymer containing conjugated diene monomer units, the total content of unhydrogenated conjugated diene monomer units and alkylene structural units as hydrogenated conjugated diene monomer units in the hydrogenated polymer corresponds to the proportion (feed ratio) of the conjugated diene monomer relative to all monomers used in the polymerization of the polymer. In the examples and comparative examples, various measurements and evaluations were carried out using the following methods.
[0092] <Break stress [MPa] / break strain value> An 8% by mass NMP solution of the binder composition prepared in the Examples and Comparative Examples, or the polymer prepared in the Synthesis Examples, was cast into a Teflon (registered trademark) Petri dish and dried in an oven at 150°C for 10 hours to produce a 500 μm thick film. According to JIS K-6251, the film was punched into a dumbbell shape and stretched at a speed of 100 mm / min using a tensile tester, and the break strain [-] and break stress [MPa] at that time were recorded. The break stress [MPa] / break strain [-] value was then determined. <Iodine value> The iodine value of the polymer prepared in the Synthesis Examples was measured according to JIS K6235;2006. <Electrode flexibility> An aluminum foil with a thickness of 15 μm was prepared as a current collector, and the positive electrode slurry composition prepared in the Examples and Comparative Examples was coated on the aluminum foil using a comma coater to a weight per unit area of 30 mg / cm after drying. 2 The positive electrode blank was rolled by a roll press to a density of 3.7 g / cm. 3A positive electrode was fabricated, consisting of a positive electrode active material layer and aluminum foil. The fabricated positive electrodes were subjected to a bending test in accordance with JIS K5600-5-1. Specifically, a positive electrode cut to a width of 10 mm was attached to a mandrel tester, and the positive electrode was bent with the positive electrode active material layer facing outward. The positive electrode active material layer was observed under a microscope in the bent state to determine whether or not there were cracks in the positive electrode. The mandrel diameter was then gradually increased until no cracks were found in the positive electrode, and the mandrel diameter at which the positive electrode did not crack was recorded. A smaller mandrel diameter indicates better flexibility (windability) of the positive electrode. A: No cracks at a diameter of 5 mm B: No cracks at a diameter of 8 mm C: No cracks at a diameter of 10 mm <IV characteristics> The lithium-ion secondary batteries fabricated in the examples and comparative examples were allowed to stand at a temperature of 25°C for 5 hours after injection of the electrolyte. Next, the battery was charged to a cell voltage of 3.65 V at a constant current of 0.2 C at 25 °C, and then aged for 12 hours at 60 °C. The battery was charged to a cell voltage of 4.2 V at a constant current of 0.2 C and discharged to a cell voltage of 3.0 V three times, and the initial capacity was measured. After charging to a depth of charge (SOC) of 50%, the battery was charged for 20 seconds and discharged for 20 seconds at 0.5 C, 1.0 C, 1.5 C, and 2.0 C, centered around 50% SOC. The battery voltage after 20 seconds in each case (charge side and discharge side) was plotted against the current value, and the slope was calculated as the IV resistance (Ω) (IV resistance during charge and discharge). The obtained IV resistance values (Ω) were evaluated according to the following criteria. The smaller the IV resistance value, the lower the internal resistance and the better the IV characteristics. A: IV resistance value less than 2.3Ω B: IV resistance value 2.3Ω or more but less than 2.5Ω C: IV resistance value 2.5Ω or more <Rate characteristics> The lithium ion secondary batteries produced in the examples and comparative examples were left to stand at a temperature of 25°C for 5 hours after electrolyte injection. Next, they were charged at a temperature of 25°C and a constant current of 0.2C to a cell voltage of 3.65V, and then aged at a temperature of 60°C for 12 hours. Then, they were discharged at a temperature of 25°C and a constant current of 0.2C to a cell voltage of 3.0V. Then, they were subjected to CC-CV charging at a constant current of 0.2C (upper limit cell voltage 4.20V), and CC discharging at a constant current of 0.2C to a cell voltage of 3.00V.This charge / discharge cycle at 0.2 C was repeated three times. Next, in an environment at a temperature of 25°C, constant current charge / discharge of 0.2 C was performed between cell voltages of 3.00 and 4.20 V, and the discharge capacity at this time was defined as C0. Thereafter, similarly, CC-CV charging was performed at a constant current of 0.2 C, and CC discharging was performed to 3.00 V at a constant current of 3.0 C in an environment at a temperature of 25°C, and the discharge capacity at this time was defined as C1. Then, as the rate characteristics, the ratio (percentage, capacity retention) of the discharge capacity at 3.0 C (C1) to the discharge capacity at 0.2 C (C0), expressed as (C1 / C0) x 100 (%), was calculated and evaluated according to the following criteria. A larger value of this capacity retention ratio indicates less decrease in discharge capacity at high current and lower internal resistance (i.e., excellent rate characteristics). A: Capacity retention rate 65% or more B: Capacity retention rate 55% or more but less than 65% C: Capacity retention rate less than 55% <Cycle characteristics> The lithium ion secondary batteries produced in the examples and comparative examples were charged to 4.2 V at a constant current of 1.0 C in an atmosphere of 45°C and discharged to 3.0 V, and 200 charge-discharge cycles were repeated. The cycle capacity retention rate, expressed as the ratio of the electric capacity at the end of 200 cycles to the initial electric capacity (= [electric capacity at the end of cycles] / [initial electric capacity] × 100 (%)), was then determined and evaluated according to the following criteria. A higher cycle capacity retention rate indicates better cycle characteristics. A: Cycle capacity retention rate 90% or more B: Cycle capacity retention rate 80% or more but less than 90% C: Cycle capacity retention rate less than 80%.
[0093] Synthesis Example 1 [Production of Polymer 1] A reactor was charged with 200 parts of ion-exchanged water and 0.2 parts of sodium carbonate. After dissolving the sodium carbonate, 2.25 parts of fatty acid potassium soap (potassium salt of fatty acid) was added to prepare an aqueous soap solution. Then, 30 parts of acrylonitrile and 0.4 parts of t-dodecyl mercaptan were charged to the obtained aqueous soap solution, in this order. The internal gas was replaced with nitrogen three times, and then 70 parts of 1,3-butadiene was charged. Next, the reactor was kept at 10°C, and 0.1 parts of cumene hydroperoxide, 0.01 parts of ethylenediaminetetraacetic acid monosodium iron hydrate, 0.03 parts of sodium hydroxymethanesulfinate dihydrate, and EDTA.4Na.4H were added. 2 A redox polymerization initiator consisting of a combination of 0.02 parts of ethanol and 0.02 parts of methyl methyl acrylate was added to initiate the polymerization reaction. When the polymerization conversion reached 85%, 0.1 parts of a 10% aqueous solution of hydroquinone (polymerization terminator) was added to terminate the polymerization reaction. Residual monomers were removed using a rotary evaporator at a water temperature of 60°C to obtain a nitrile rubber latex. Next, a portion of the obtained latex was added to an aqueous solution of magnesium sulfate as a coagulant in an amount of 1.0% by mass relative to the nitrile rubber content, and the mixture was stirred to coagulate the latex. The coagulated latex was then filtered while washing with water, and the obtained coagulated material was vacuum dried at 60°C for 12 hours to obtain nitrile rubber as a polymer precursor. The obtained nitrile rubber was dissolved in acetone to a concentration of 12%, placed in an autoclave, and a palladium-silica catalyst was added in an amount of 500 ppm by mass relative to the nitrile rubber. A hydrogenation reaction was carried out at a hydrogen pressure of 3.0 MPa. After completion of the hydrogenation reaction, the mixture was poured into a large amount of water to coagulate, and then filtered and dried to obtain hydrogenated nitrile-butadiene rubber as polymer 1. The iodine value of polymer 1, as well as the breaking stress and breaking strain when polymer 1 was formed into a film, were measured. The results are shown in Table 1.
[0094] Synthesis Example 2 [Production of Polymer 2] A reactor was charged with 200 parts of ion-exchanged water and 0.2 parts of sodium carbonate. After dissolving the sodium carbonate, 2.25 parts of fatty acid potassium soap (potassium salt of fatty acid) was added to prepare an aqueous soap solution. 20 parts of acrylonitrile, 40 parts of ethyl acrylate, and 0.4 parts of t-dodecyl mercaptan were then charged to the resulting aqueous soap solution, in this order. The internal gas was replaced with nitrogen three times, and then 40 parts of 1,3-butadiene was added. Next, the reactor was kept at 10°C, and 0.1 parts of cumene hydroperoxide, 0.01 parts of ethylenediaminetetraacetic acid monosodium iron hydrate, 0.03 parts of sodium hydroxymethanesulfinate dihydrate, and EDTA.4Na.4H were added. 2 A redox polymerization initiator consisting of a combination of 0.02 parts of ethanol and 0.02 parts of ethanol was added to initiate the polymerization reaction. When the polymerization conversion rate reached 85%, 0.1 parts of a 10% aqueous solution of hydroquinone (polymerization terminator) was added to terminate the polymerization reaction, and residual monomers were removed using a rotary evaporator at a water temperature of 60°C to obtain a nitrile rubber latex. Next, a portion of the obtained latex was added to an aqueous solution of magnesium sulfate as a coagulant in an amount of 1.0% by mass relative to the nitrile rubber content, and the mixture was stirred to coagulate the latex. The mixture was then filtered while washing with water, and the obtained coagulated material was vacuum dried at 60°C for 12 hours to obtain nitrile rubber as a polymer precursor. The obtained nitrile rubber was dissolved in acetone to a concentration of 12%, placed in an autoclave, and a palladium-silica catalyst was added in an amount of 500 ppm by mass relative to the nitrile rubber, followed by a hydrogenation reaction at a hydrogen pressure of 3.0 MPa. After the hydrogenation reaction was completed, the mixture was poured into a large amount of water to be coagulated, and then filtered and dried to obtain hydrogenated nitrile-butadiene rubber as polymer 2. The iodine value of polymer 2, as well as the breaking stress and breaking strain when polymer 2 was formed into a film, were measured. The results are shown in Table 1.
[0095] Synthesis Example 3 [Production of Polymer 3] A reactor was charged with 200 parts of ion-exchanged water and 0.2 parts of sodium carbonate. After dissolving the sodium carbonate, 2.25 parts of fatty acid potassium soap (potassium salt of fatty acid) was added to prepare an aqueous soap solution. Then, 18 parts of acrylonitrile and 0.3 parts of t-dodecyl mercaptan were charged to the obtained aqueous soap solution, in this order. The internal gas was replaced with nitrogen three times, and then 42 parts of 1,3-butadiene was charged. Next, the reactor was kept at 10°C, and 0.1 parts of cumene hydroperoxide, 0.01 parts of ethylenediaminetetraacetic acid monosodium iron hydrate, 0.03 parts of sodium hydroxymethanesulfinate dihydrate, and EDTA.4Na.4H were added. 2 A redox polymerization initiator consisting of a combination of 0.02 parts of acrylonitrile and 28 parts of 1,3-butadiene was added to initiate the polymerization reaction. When the polymerization conversion rate reached 60%, 12 parts of acrylonitrile and 28 parts of 1,3-butadiene were added, and the polymerization reaction was further carried out. When the polymerization conversion rate reached 90%, 0.1 parts of a 10% aqueous solution of hydroquinone (polymerization terminator) was added to terminate the polymerization reaction, and residual monomers were removed using a rotary evaporator at a water temperature of 60°C to obtain a nitrile rubber latex. Next, a portion of the obtained latex was added to an aqueous solution of magnesium sulfate as a coagulant in an amount of 1.0% by mass relative to the nitrile rubber content, and the mixture was stirred to coagulate the latex. The resulting mixture was then washed with water and filtered, and the resulting coagulated material was vacuum dried at 60°C for 12 hours to obtain a nitrile rubber as a polymer precursor. The resulting nitrile rubber was dissolved in acetone to a concentration of 12%, and the solution was placed in an autoclave. A palladium-silica catalyst was added in an amount of 500 ppm by mass relative to the nitrile rubber, and a hydrogenation reaction was carried out at a hydrogen pressure of 3.0 MPa. After completion of the hydrogenation reaction, the mixture was poured into a large amount of water to coagulate, and then filtered and dried to obtain hydrogenated nitrile-butadiene rubber as polymer 3. The iodine value of polymer 3, as well as the breaking stress and breaking strain when polymer 3 was formed into a film, were measured. The results are shown in Table 1.
[0096] Synthesis Example 4 [Production of Polymer 4] A reactor was charged with 200 parts of ion-exchanged water and 0.2 parts of sodium carbonate. After dissolving the sodium carbonate, 2.25 parts of fatty acid potassium soap (potassium salt of fatty acid) was added to prepare an aqueous soap solution. Then, 30 parts of acrylonitrile and 1.0 part of t-dodecyl mercaptan were charged to the obtained aqueous soap solution, in this order. The gas inside was replaced with nitrogen three times, and then 70 parts of 1,3-butadiene was charged. Next, the reactor was kept at 10°C, and 0.1 parts of cumene hydroperoxide, 0.01 parts of ethylenediaminetetraacetic acid monosodium iron hydrate, 0.03 parts of sodium hydroxymethanesulfinate dihydrate, and EDTA.4Na.4H were added. 2 A redox polymerization initiator consisting of a combination of 0.02 parts of ethanol and 0.02 parts of methyl methyl acrylate was added to initiate the polymerization reaction. When the polymerization conversion rate reached 80%, 0.1 parts of a 10% aqueous solution of hydroquinone (polymerization terminator) was added to terminate the polymerization reaction, and residual monomers were removed using a rotary evaporator at a water temperature of 60°C to obtain a nitrile rubber latex. Next, a portion of the obtained latex was added to an aqueous solution of magnesium sulfate as a coagulant in an amount of 1.0% by mass relative to the nitrile rubber content, and the mixture was stirred to coagulate the latex. The mixture was then filtered while washing with water, and the obtained coagulated material was vacuum dried at 60°C for 12 hours to obtain nitrile rubber as a polymer precursor. The obtained nitrile rubber was dissolved in acetone to a concentration of 12%, placed in an autoclave, and a palladium-silica catalyst was added in an amount of 500 ppm by mass relative to the nitrile rubber, followed by a hydrogenation reaction at a hydrogen pressure of 3.0 MPa. After the hydrogenation reaction was completed, the mixture was poured into a large amount of water to be coagulated, and then filtered and dried to obtain hydrogenated nitrile-butadiene rubber as polymer 4. The iodine value of polymer 4, as well as the breaking stress and breaking strain when polymer 4 was formed into a film, were measured. The results are shown in Table 1.
[0097] Synthesis Example 5 [Production of Polymer 5] A reactor was charged with 200 parts of ion-exchanged water and 0.2 parts of sodium carbonate. After dissolving the sodium carbonate, 2.25 parts of fatty acid potassium soap (potassium salt of fatty acid) was added to prepare an aqueous soap solution. Then, 50 parts of acrylonitrile and 1.0 part of t-dodecyl mercaptan were charged to the obtained aqueous soap solution, in this order. The internal gas was replaced with nitrogen three times, and then 20 parts of 1,3-butadiene was charged. Next, the reactor was kept at 10°C, and 0.1 parts of cumene hydroperoxide, 0.01 parts of ethylenediaminetetraacetic acid monosodium iron hydrate, 0.03 parts of sodium hydroxymethanesulfinate dihydrate, and EDTA.4Na.4H were added. 2 A redox polymerization initiator consisting of a combination of 0.02 parts of acetic acid and 0.02 parts of acetic acid was added to initiate the polymerization reaction. When the polymerization conversion reached 50%, 30 parts of acrylonitrile was added, and the polymerization reaction was further carried out. When the polymerization conversion reached 70%, 0.1 parts of a 10% aqueous solution of hydroquinone (polymerization terminator) was added to terminate the polymerization reaction. Residual monomers were removed using a rotary evaporator at a water temperature of 60°C to obtain a nitrile rubber latex. Next, a portion of the obtained latex was added to an aqueous solution of magnesium sulfate as a coagulant in an amount of 1.0% by mass relative to the nitrile rubber content, and the mixture was stirred to coagulate the latex. The mixture was then filtered while washing with water, and the obtained coagulated material was vacuum dried at 60°C for 12 hours to obtain nitrile rubber as a polymer precursor. The obtained nitrile rubber was dissolved in acetone to a concentration of 12%, placed in an autoclave, and a palladium-silica catalyst was added at 1,000 ppm by mass relative to the nitrile rubber. A hydrogenation reaction was carried out at a hydrogen pressure of 3.0 MPa. After completion of the hydrogenation reaction, the mixture was poured into a large amount of water to coagulate, and then filtered and dried to obtain hydrogenated nitrile-butadiene rubber as polymer 5. The iodine value of polymer 5, as well as the breaking stress and breaking strain when polymer 5 was formed into a film, were measured. The results are shown in Table 1.
[0098] Synthesis Example 6 [Production of Polymer 6] A reactor was charged with 200 parts of ion-exchanged water and 0.2 parts of sodium carbonate. After dissolving the sodium carbonate, 2.25 parts of fatty acid potassium soap (potassium salt of fatty acid) was added to prepare an aqueous soap solution. Then, 17 parts of acrylonitrile, 50 parts of ethyl acrylate, and 0.4 parts of t-dodecyl mercaptan were charged to the obtained aqueous soap solution, in this order. The internal gas was replaced with nitrogen three times, and then 33 parts of 1,3-butadiene was charged. Next, the reactor was kept at 10°C, and 0.1 parts of cumene hydroperoxide, 0.01 parts of ethylenediaminetetraacetic acid monosodium iron hydrate, 0.03 parts of sodium hydroxymethanesulfinate dihydrate, and EDTA.4Na.4H were added. 2 A redox polymerization initiator consisting of a combination of 0.02 parts of ethanol and 0.02 parts of methyl methyl acrylate was added to initiate the polymerization reaction. When the polymerization conversion rate reached 85%, 0.1 parts of a 10% aqueous solution of hydroquinone (polymerization terminator) was added to terminate the polymerization reaction, and residual monomers were removed using a rotary evaporator at a water temperature of 60°C to obtain a nitrile rubber latex. Next, a portion of the obtained latex was added to an aqueous solution of magnesium sulfate as a coagulant in an amount of 1.0% by mass relative to the nitrile rubber content, and the mixture was stirred to coagulate the latex. The mixture was then filtered while washing with water, and the obtained coagulated material was vacuum dried at 60°C for 12 hours to obtain nitrile rubber as a polymer precursor. The obtained nitrile rubber was dissolved in acetone to a concentration of 12%, placed in an autoclave, and a palladium-silica catalyst was added in an amount of 1500 ppm by mass relative to the nitrile rubber, followed by a hydrogenation reaction at a hydrogen pressure of 3.0 MPa. After the hydrogenation reaction was completed, the mixture was poured into a large amount of water to be coagulated, and then filtered and dried to obtain hydrogenated nitrile-butadiene rubber as polymer 6. The iodine value of polymer 6, as well as the breaking stress and breaking strain when polymer 6 was formed into a film, were measured. The results are shown in Table 1.
[0099] Example 1 Preparation of Binder Composition Polymer A was prepared by stirring polymer 1 (0.25 parts) prepared in Synthesis Example 1 and polymer 2 (0.25 parts) prepared in Synthesis Example 2 in the presence of NMP using a disperser to prepare a binder composition (solid content concentration: 8% by mass). This binder composition was formed into a film and subjected to a tensile test to measure the breaking strain and breaking stress. The value of breaking stress [MPa] / breaking strain was then calculated. The results are shown in Table 2.
[0100] [Preparation of Slurry Composition] NMC532 (LiNi) having a layered structure was used as the positive electrode active material. 0.5 Mn 0.3 Co 0.2 O 2 To 96.8 parts of acetylene black (Li435, manufactured by Denka Co., Ltd.) as a conductive material, 0.5 parts of PVdF and 0.5 parts of the binder composition (corresponding to the solid content) were added. A carbon paste prepared by mixing 2.0 parts of acetylene black (Li435, manufactured by Denka Co., Ltd.) as a conductive material and 0.2 parts of hydrogenated nitrile butadiene rubber (H-NBR) as a dispersant was added, and an appropriate amount of NMP was added. The resulting mixture was stirred with a planetary mixer to prepare a slurry composition (slurry composition for a positive electrode).
[0101] [Production of Positive Electrode] An aluminum foil having a thickness of 15 μm was prepared as a current collector. The above slurry composition was applied to both sides of the aluminum foil using a comma coater in a coating amount of 23 mg / cm after drying. 2 The positive electrode was rolled using a roll press to a density of 3.7 g / cm. 3 A positive electrode was fabricated, which consisted of a positive electrode active material layer and aluminum foil.
[0102] [Production of negative electrode] A planetary mixer with a disperser was used to mix a negative electrode active material with a specific surface area of 4 m 2100 parts of 1 / g artificial graphite and 1 part (solids equivalent) of a 1% aqueous solution of carboxymethyl cellulose ("BSH-12" manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) as a dispersant were added, and the solids concentration was adjusted to 55% with ion-exchanged water, followed by mixing at 25°C for 60 minutes. Next, the solids concentration was adjusted to 52% with ion-exchanged water. Mixing was then continued for an additional 15 minutes to obtain a mixed solution. To the above mixed solution, 1.0 part (solids equivalent) of a 40% aqueous solution containing a styrene-butadiene copolymer and ion-exchanged water were added, and the final solids concentration was adjusted to 50%, followed by mixing for an additional 10 minutes. This was degassed to obtain a negative electrode slurry composition with good fluidity. The above negative electrode slurry composition was coated on both sides of a 20 μm-thick copper foil current collector using a comma coater, resulting in a coating weight of 13 mg / cm after drying. 2 and dried at 60° C. Thereafter, a heat treatment was performed at 120° C. for 2 minutes to obtain a negative electrode blank. This negative electrode blank was rolled using a roll press to obtain a negative electrode having a negative electrode active material layer with a thickness of 80 μm.
[0103] [Separator] A single-layer polypropylene separator (thickness: 25 μm, porosity: 55%) was used.
[0104] [Manufacturing of Lithium-ion Secondary Battery] An aluminum packaging material was prepared as the battery exterior. The positive electrode obtained above was cut into a width of 25.0 mm and a length of 60 cm, and the negative electrode obtained above was cut into a width of 35.0 mm and a length of 70 cm to form a sheet. The prepared positive electrode for lithium-ion secondary battery and negative electrode for lithium-ion secondary battery were wound around a core with a diameter of 20 mm, with the separator interposed, so that the electrode mixture layers faced each other, to obtain a wound body. The obtained wound body was then pressed at a speed of 10 mm / sec to form a flat body, which was then wrapped in the aluminum packaging material as the battery exterior. A 1.0 M LiPF 6 electrolyte was added. 6 A solution (solvent: a mixed solvent of ethylene carbonate (EC) / diethyl carbonate (DEC) = 3 / 7 (volume ratio), additive: containing 2 volume% vinylene carbonate (solvent ratio)) was poured into the battery so that no air remained. The opening of the aluminum packaging was then heat-sealed at a temperature of 150°C to close the opening, and a wound-type lithium-ion secondary battery with a capacity of 620 mAh was fabricated. The IV characteristics, rate characteristics, and cycle characteristics were evaluated. The results are shown in Table 2.
[0105] (Example 2) A binder composition, a slurry composition, a positive electrode, a negative electrode, and a lithium ion secondary battery were prepared or manufactured in the same manner as in Example 1, except that in the preparation of the binder composition in Example 1, polymer 2 (0.1 part) and polymer 3 (0.4 parts) prepared in Synthesis Example 3 were used instead of polymer 1 (0.25 parts) and polymer 2 (0.25 parts). Then, various operations and measurements were performed in the same manner as in Example 1. The results are shown in Tables 1 and 2.
[0106] (Example 3) A binder composition, a slurry composition, a positive electrode, a negative electrode, and a lithium ion secondary battery were prepared or manufactured in the same manner as in Example 1, except that in the preparation of the binder composition in Example 1, the blending amount of Polymer 1 was changed from 0.25 parts to 0.05 parts, and the blending amount of Polymer 2 was changed from 0.25 parts to 0.45 parts. Then, various operations and measurements were performed in the same manner as in Example 1. The results are shown in Tables 1 and 2.
[0107] (Example 4) A binder composition, a slurry composition, a positive electrode, a negative electrode, and a lithium ion secondary battery were prepared or manufactured in the same manner as in Example 1, except that in the preparation of the binder composition in Example 1, only Polymer 3 (0.5 parts) prepared in Synthesis Example 3 was used instead of Polymer 1 (0.25 parts) and Polymer 2 (0.25 parts). Various operations and measurements were then performed in the same manner as in Example 1. The results are shown in Tables 1 and 2.
[0108] Example 5 A binder composition, a slurry composition, a positive electrode, a negative electrode, and a lithium ion secondary battery were prepared or manufactured in the same manner as in Example 1, except that in the preparation of the binder composition of Example 1, only Polymer 4 (0.5 parts) prepared in Synthesis Example 4 was used instead of Polymer 1 (0.25 parts) and Polymer 2 (0.25 parts). Various operations and measurements were then performed in the same manner as in Example 1. The results are shown in Tables 1 and 2.
[0109] Example 6 A binder composition, a slurry composition, a positive electrode, a negative electrode, and a lithium ion secondary battery were prepared or manufactured in the same manner as in Example 1, except that in the preparation of the slurry composition of Example 1, the blending amounts of Polymer 1 and Polymer 2 were changed from 0.25 parts to 0.50 parts, and PVdF was not blended as a binder. Then, various operations and measurements were performed in the same manner as in Example 1. The results are shown in Tables 1 and 2.
[0110] Comparative Example 1 A binder composition, a slurry composition, a positive electrode, a negative electrode, and a lithium ion secondary battery were prepared or manufactured in the same manner as in Example 1, except that in the preparation of the binder composition in Example 1, only Polymer 5 (0.5 parts) prepared in Synthesis Example 5 was used instead of Polymer 1 (0.25 parts) and Polymer 2 (0.25 parts). Various operations and measurements were then performed in the same manner as in Example 1. The results are shown in Tables 1 and 2.
[0111] Comparative Example 2 A binder composition, a slurry composition, a positive electrode, a negative electrode, and a lithium ion secondary battery were prepared or manufactured in the same manner as in Example 1, except that in the preparation of the binder composition in Example 1, only Polymer 6 (0.5 parts) prepared in Synthesis Example 6 was used instead of Polymer 1 (0.25 parts) and Polymer 2 (0.25 parts). Various operations and measurements were then performed in the same manner as in Example 1. The results are shown in Tables 1 and 2. In Table 1, AN represents acrylonitrile, BD represents 1,3-butadiene, and EA represents ethyl acrylate. In Table 2, PVdF represents polyvinylidene fluoride.
[0112] The results in Table 2 show that in Examples 1 to 6, in which the binder compositions for nonaqueous secondary battery electrodes were used such that, when formed into films, the breaking stress [MPa] and breaking strain [−] of the films in a tensile test satisfied the relational expression 0.010≦breaking stress [MPa] / breaking strain [−]≦1.000, the resulting electrodes were excellent in flexibility and the resulting secondary batteries had excellent battery properties.
[0113] According to the present invention, there is provided a binder composition for a non-aqueous secondary battery electrode that can be suitably used to produce an electrode with excellent flexibility and that can improve the battery characteristics of a secondary battery including the resulting electrode. Furthermore, according to the present invention, there is provided a slurry composition for a non-aqueous secondary battery electrode that can form an electrode with excellent flexibility and can improve the battery characteristics of a secondary battery including the resulting electrode. Furthermore, according to the present invention, there is provided a non-aqueous secondary battery electrode that can improve the battery characteristics of a non-aqueous secondary battery, and a non-aqueous secondary battery with excellent battery characteristics.
Claims
1. A binder composition for a non-aqueous secondary battery electrode, comprising a polymer A, wherein when the binder composition for a non-aqueous secondary battery electrode is formed into a film X, the breaking stress [MPa] and breaking strain [-] of the film X in a tensile test satisfy the following relationship: 0.010≦breaking stress [MPa] / breaking strain [-]≦1.
000.
2. The binder composition for a non-aqueous secondary battery electrode according to claim 1, wherein the breaking strain of the film X in a tensile test is 6.0 or more.
3. The binder composition for a non-aqueous secondary battery electrode according to claim 1 or 2, wherein the polymer A contains two or more kinds of polymers.
4. The binder composition for a non-aqueous secondary battery electrode according to any one of claims 1 to 3, wherein the polymer A comprises a polymer A1 such that, when made into a film Y, the film Y has a breaking stress of 0.3 MPa or more and a breaking strain of 6.0 or more and less than 25.0 as determined by a tensile test.
5. The binder composition for a non-aqueous secondary battery electrode according to claim 4, wherein the polymer A further contains a polymer A2 such that, when the polymer A is made into a film Y, the film Y has a breaking stress of 0.3 MPa or more and a breaking strain of 25.0 or more in a tensile test.
6. The binder composition for a non-aqueous secondary battery electrode according to claim 5, wherein the mass ratio of the polymer A1 to the polymer A2 (polymer A1:polymer A2) is 9:1 or more and 1:9 or less.
7. The binder composition for a non-aqueous secondary battery electrode according to any one of claims 4 to 6, wherein the polymer A1 contains a nitrile group-containing monomer unit and an alkylene structural unit.
8. The binder composition for a non-aqueous secondary battery electrode according to any one of claims 5 to 7, wherein the polymer A2 contains a (meth)acrylic acid ester monomer unit.
9. A slurry composition for a non-aqueous secondary battery electrode, comprising an electrode active material and the binder composition for a non-aqueous secondary battery electrode according to any one of claims 1 to 8.
10. A non-aqueous secondary battery electrode comprising an electrode mixture layer formed using the slurry composition for a non-aqueous secondary battery electrode according to claim 9.
11. A non-aqueous secondary battery comprising the electrode for a non-aqueous secondary battery according to claim 10.
Citation Information
Patent Citations
Electrode for secondary battery, binder for secondary battery electrode, manufacturing method and secondary battery
JP2012204303A
Positive electrode for secondary battery, and secondary battery
JP2017143075A
Low molecular weight nitrocellulose containing composite materials
JP4509792B2
Secondary cell negative electrode, secondary cell, slurry composition for negative electrode, and method of producing secondary cell negative electrode
WO2012115096A1
Lithium-ion battery anode sizing agent based on waterborne polyurethane bonder
CN105161720A