Positive electrode for secondary battery, and secondary battery

The positive electrode for secondary batteries, featuring a carbon-based conductive agent with a controlled half-value width, addresses the issue of insufficient battery characteristics by ensuring uniform dispersibility and distribution, leading to improved performance and durability.

WO2024204282A1PCT designated stage expired Publication Date: 2024-10-03MURATA MFG CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012118
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-03-26
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Secondary batteries exhibit insufficient battery characteristics despite various studies on their configuration, necessitating the development of a positive electrode that can enhance performance.

Method used

A positive electrode with a carbon-based conductive agent, where the half-value width of the Raman peak is 0.50 or less, achieved by optimizing the dispersibility and distribution of the conductive agent within the active material layer using specific Raman spectroscopy analysis and manufacturing processes.

Benefits of technology

This configuration results in improved electrical resistance and physical strength uniformity, enabling efficient lithium intercalation and release, reducing material deterioration and enhancing battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012118_03102024_PF_FP_ABST
    Figure JP2024012118_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a secondary battery with which it is possible to obtain excellent battery characteristics. The secondary battery comprises: a positive electrode including a positive electrode active material layer; a negative electrode; and an electrolytic solution. The positive electrode active material layer contains a positive electrode active material and a positive electrode electroconductive agent, and the positive electrode electroconductive agent contains a carbon material. The half-value width of a peak identified through the procedures (1) to (3) on the basis of an analysis result of the surface of the positive electrode active material layer using Raman spectroscopy is 0.50 or less. (1) Obtain a Raman mapping of D / G ratios by analyzing the surface of the positive electrode active material layer using Raman spectroscopy. (2) On the basis of the Raman mapping, acquire a histogram of a D / G ratio having a peak. (3) Calculate the half-value width of the peak on the basis of the histogram.
Need to check novelty before this filing date? Find Prior Art

Description

Positive electrode for secondary battery and secondary battery

[0001] The present technology relates to a positive electrode for a secondary battery and a secondary battery.

[0002] Due to the widespread use of various electronic devices such as mobile phones, secondary batteries have been developed as small, lightweight power sources that can provide high energy density. These secondary batteries contain a positive electrode (a positive electrode for the secondary battery), a negative electrode, and an electrolyte solution, and various studies have been conducted on the configuration of these secondary batteries.

[0003] Specifically, the positive electrode material layer contains a conductive material, and the Raman peak integrated intensity ratio for the positive electrode material layer is greater than 0.6 and less than or equal to 10 (see, for example, Patent Document 1). The positive electrode contains carbon black, non-fibrous graphite particles, and fibrous carbon (see, for example, Patent Document 2). The battery electrode contains carbon nanotubes and a non-fibrous conductive carbon material (see, for example, Patent Document 3). The positive electrode mixture layer contains carbon black, first carbon nanotubes with a small fiber length, and second carbon nanotubes with a large fiber length (see, for example, Patent Document 4).

[0004] JP 2015-084323 A JP 2000-058066 A International Publication No. 2012 / 114590 JP 2018-097961 A

[0005] Although various studies have been conducted on the configuration of secondary batteries, the battery characteristics of the secondary batteries are still insufficient and there is room for improvement.

[0006] There is a demand for a positive electrode for a secondary battery and a secondary battery that can provide excellent battery characteristics.

[0007] According to one embodiment of the present disclosure, a positive electrode for a secondary battery includes a positive electrode active material layer. The positive electrode active material layer includes a positive electrode active material and a positive electrode conductive agent, and the positive electrode conductive agent includes a carbon material. The surface of the positive electrode active material layer is analyzed using Raman spectroscopy according to the following steps (1) to (3). The half-width of a peak identified based on the analysis results is 0.50 or less.

[0008] (1) A Raman mapping of the D / G ratio is obtained by analyzing the surface of the positive electrode active material layer using Raman spectroscopy. (2) A histogram of the D / G ratio having a peak is obtained based on the Raman mapping. (3) The half-width of the peak is calculated based on the histogram.

[0009] A secondary battery according to an embodiment of the present technology includes a positive electrode, a negative electrode, and an electrolyte solution, and the positive electrode has a configuration similar to the configuration of the positive electrode for a secondary battery according to the embodiment of the present technology described above.

[0010] Here, the "D / G ratio" is the integrated intensity ratio of two types of peaks (D-band peak and G-band peak) detected when the surface of the positive electrode active material layer is analyzed using Raman spectroscopy. This D / G ratio is an index representing the crystalline state of the carbon material contained as a positive electrode conductive agent in the positive electrode active material layer, and is calculated based on the following formula: D / G ratio = integrated intensity (area) of D-band peak / integrated intensity (area) of G-band peak. The D-band peak has a Raman shift of approximately 1300 cm -1 ~1400cm -1 and the G-band peak has a Raman shift of about 1550 cm -1 ~1650cm -1 The peaks detected within the range are:

[0011] As described above, the "half width" is determined based on the analysis results (Raman mapping and histogram) of the surface of the positive electrode active material layer using Raman spectroscopy. This half width is the so-called full width at half maximum (FWHM). Details of the procedure for determining the half width will be described later.

[0012] According to the positive electrode for a secondary battery or the secondary battery of an embodiment of the present technology, the positive electrode active material layer contains a positive electrode active material and a positive electrode conductive agent, the positive electrode conductive agent contains a carbon material, and the half width of a peak identified based on the analysis results of the surface of the positive electrode active material layer using Raman spectroscopy is 0.50 or less, so that excellent battery characteristics can be obtained.

[0013] Note that the effects of the present technology are not necessarily limited to the effects described here, but may be any of a series of effects related to the present technology described below.

[0014] Fig. 1 is a cross-sectional view showing a configuration of a positive electrode for a secondary battery according to an embodiment of the present technology. Fig. 2 is a diagram showing an example of a histogram acquired based on Raman mapping. Fig. 3 is a perspective view showing a configuration of a secondary battery according to an embodiment of the present technology. Fig. 4 is a cross-sectional view showing a configuration of the battery element shown in Fig. 3. Fig. 5 is a block diagram showing a configuration of an application example of a secondary battery. Fig. 6 is a cross-sectional view showing a configuration of a test secondary battery.

[0015] Hereinafter, an embodiment of the present technology will be described in detail with reference to the drawings. The description will be made in the following order: 1. Positive electrode for secondary battery 1-1. Configuration 1-2. Physical properties 1-3. Operation 1-4. Manufacturing method 1-5. Action and effect 2. Secondary battery 2-1. Configuration 2-2. Operation 2-3. Manufacturing method 2-4. Action and effect 3. Modified example 4. Use of secondary battery

[0016] 1. Positive Electrode for Secondary Battery First, a positive electrode for a secondary battery (hereinafter simply referred to as "positive electrode") according to an embodiment of the present technology will be described.

[0017] The positive electrode described here is used in a secondary battery, which is an electrochemical device. However, the positive electrode may also be used in electrochemical devices other than secondary batteries. Specific examples of other electrochemical devices include primary batteries and capacitors.

[0018] The positive electrode absorbs and releases an electrode reactant during operation of the electrochemical device (during electrode reaction). The type of electrode reactant is not particularly limited, but specifically includes light metals such as alkali metals and alkaline earth metals. Specific examples of alkali metals include lithium, sodium, and potassium, and specific examples of alkaline earth metals include beryllium, magnesium, and calcium.

[0019] In the following, an example will be given in which the electrode reactant is lithium, whereby lithium is absorbed and released in an ionic state at the positive electrode during the electrode reaction.

[0020] 1-1. Structure FIG. 1 shows a cross-sectional structure of a positive electrode 100, which is a specific example of a positive electrode.

[0021] The positive electrode 100 includes a positive electrode active material layer 100B. Here, the positive electrode 100 further includes a positive electrode current collector 100A that supports the positive electrode active material layer 100B.

[0022] [Positive Electrode Current Collector] The positive electrode current collector 100A is a conductive support that supports the positive electrode active material layer 100B, and has a pair of surfaces (upper and lower surfaces) on which the positive electrode active material layer 100B is provided. The positive electrode current collector 100A contains a conductive material such as a metal material, and a specific example of the conductive material is aluminum.

[0023] [Positive Electrode Active Material Layer] The positive electrode active material layer 100B is a layer that absorbs and releases lithium, and is provided on one surface (upper or lower surface) of the positive electrode current collector 100A. However, the positive electrode active material layer 100B may be provided on both surfaces (upper and lower surfaces) of the positive electrode current collector 100A. This positive electrode active material layer 100B contains a positive electrode active material and a positive electrode conductive agent.

[0024] (Positive Electrode Active Material) The positive electrode active material is one or more of materials that absorb and release lithium. The type of positive electrode active material is not particularly limited, but specifically, it is a lithium-containing compound, etc. This is because a high voltage can be obtained.

[0025] This lithium-containing compound is a compound containing lithium and one or more transition metal elements as constituent elements, and may further contain one or more other elements (excluding lithium and transition metal elements) as constituent elements. The type of other elements is not particularly limited, but specifically, they are elements belonging to groups 2 to 15 of the long period periodic table. The type of lithium-containing compound is not particularly limited, but specifically, they include oxides, phosphate compounds, silicate compounds, and borate compounds.

[0026] A specific example of the oxide is LiNiO 2  , LiCoO 2  , LiCo 0.98 Al 0.01 Mg 0.01 O 2  , LiNi 0.5  Co 0.2  Mn 0.3  O 2  and LiMn 2  O 4  Specific examples of phosphate compounds include LiFePO 4  , LiMnPO 4  and LiFe 0.5  Mn 0.5  P.O. 4  And so on.

[0027] (Positive Electrode Conductive Agent) The positive electrode conductive agent is a material that improves the conductivity of the positive electrode active material layer 100B, and contains one or more types of carbon materials that are conductive materials.

[0028] The type of carbon material is not particularly limited, but specifically, it is one or both of a particulate carbon material and a fibrous carbon material. That is, the positive electrode conductive agent may contain only a particulate carbon material, may contain only a fibrous carbon material, or may contain both a particulate carbon material and a fibrous carbon material. The type of particulate carbon material may be one type or two or more types. Similarly, the type of fibrous carbon material may be one type or two or more types.

[0029] Specific examples of particulate carbon materials include graphite, carbon black, acetylene black, and ketjen black. Specific examples of fibrous carbon materials include carbon nanotubes, carbon fibers, and carbon nanofibers.

[0030] In particular, the carbon material preferably contains both particulate carbon material and fibrous carbon material, because this further improves the conductivity of the positive electrode active material layer 100B.

[0031] Specifically, when the carbon material contains both particulate carbon material and fibrous carbon material, the particulate carbon material is more likely to be arranged on the surface of the positive electrode active material, and the fibrous carbon material is more likely to be arranged across multiple positive electrode active materials using the particulate carbon material as binding points. This makes it easier to form a conductive network using the positive electrode active material, the particulate carbon material, and the fibrous carbon material in the positive electrode active material layer 100B. In contrast, when the carbon material contains only either the particulate carbon material or the fibrous carbon material, the conductive network described above is less likely to be formed.

[0032] In this positive electrode 100, the physical properties of the positive electrode active material layer 100B containing a carbon material as a positive electrode conductive agent are optimized, thereby improving the dispersibility of the positive electrode conductive agent inside the positive electrode active material layer 100B. Details of the physical properties of the positive electrode active material layer 100B described here will be described later.

[0033] The positive electrode conductive agent may further contain one or more of other conductive materials such as metal materials and conductive polymer compounds.

[0034] (Positive Electrode Binder) The positive electrode active material layer 100B may further contain a positive electrode binder. This positive electrode binder is a material that binds the positive electrode active material and the positive electrode conductive agent together, and contains one or more types of materials such as synthetic rubber and polymer compounds. Specific examples of synthetic rubber include styrene-butadiene rubber, fluorine-containing rubber, and ethylene propylene diene. Specific examples of polymer compounds include polyvinylidene fluoride, polyimide, and carboxymethyl cellulose.

[0035] 2 shows an example of a histogram obtained based on Raman mapping, in which the horizontal axis represents the D / G ratio and the vertical axis represents the frequency.

[0036] As described above, in this positive electrode 100, the physical properties of the positive electrode active material layer 100B containing a carbon material as a positive electrode conductive agent are optimized. Specifically, the half-width HW of the peak P identified based on the results of an analysis of the surface of the positive electrode active material layer 100B using Raman spectroscopy according to the procedures (1) to (3) below is 0.50 or less. The value of the half-width HW is rounded to two decimal places.

[0037] (1) A Raman mapping of the D / G ratio is obtained by analyzing the surface of the positive electrode active material layer 100B using Raman spectroscopy. (2) A histogram of the D / G ratio having the peak P is obtained based on the Raman mapping obtained in (1) above. (3) The half-width HW of the peak P is calculated based on the histogram obtained in (2) above.

[0038] Here, as described above, the "D / G ratio" is the integrated intensity ratio of two types of peaks (D-band peak and G-band peak) detected when the surface of the positive electrode active material layer 100B is analyzed using Raman spectroscopy. This D / G ratio is an index representing the crystalline state of the carbon material contained as a positive electrode conductive agent in the positive electrode active material layer 100B, and is calculated based on the following formula: D / G ratio = integrated intensity (area) of the D-band peak / integrated intensity (area) of the G-band peak.

[0039] The D-band peak has a Raman shift of about 1300 cm -1 ~1400cm -1 and the G-band peak has a Raman shift of about 1550 cm -1 ~1650cm -1 The peaks detected within the range are:

[0040] As described above, the "half width HW" is determined based on the analysis results (Raman mapping and histogram) of the surface of the positive electrode active material layer 100B using Raman spectroscopy. This half width is the so-called full width at half maximum (FWHM).

[0041] The detailed procedure for determining the half-value width HW is as follows: The procedure for determining the half-value width HW will be described below for each of the steps (1) to (3).

[0042] (1) Obtaining Raman Mapping To determine the half-width HW, first, a Raman mapping of the D / G ratio is obtained by analyzing the surface of the positive electrode active material layer 100B using Raman spectroscopy. In this case, a laser Raman microscope such as RAMANforce manufactured by Nanophoton Inc. can be used as the Raman spectroscopic analyzer. The analysis conditions are an analysis range of 100 μm × 100 μm and an excitation wavelength of 532 nm.

[0043] This Raman mapping is the result of calculating the D / G ratio by analyzing the surface of the positive electrode active material layer 100B using Raman spectroscopy, and then displaying (mapping) the D / G ratio two-dimensionally. In other words, the Raman mapping is the result of visualizing the distribution of the crystalline state of the carbon material identified based on the D / G ratio.

[0044] (2) Obtaining a Histogram Next, based on the Raman mapping obtained in (1), a histogram of the D / G ratio is obtained as shown in Fig. 2. In this case, the Raman mapping is converted into a histogram by utilizing a function (arithmetic processing) provided in the Raman spectroscopic analyzer.

[0045] This histogram is the result of graphing Raman mapping to continuously display the change in the frequency of the D / G ratio. In this histogram, the frequency of the D / G ratio increases and then decreases, resulting in the detection of a peak P.

[0046] (3) Calculation of Half-Width HW Finally, based on the histogram acquired in (2), the half-width HW of peak P is calculated. As is clear from Fig. 2, this half-width HW is the width of peak P at the position where the maximum frequency F1 of peak P is half (F2 = F1 / 2), based on the maximum frequency F1 of peak P, and more specifically, is the value obtained by subtracting the D / G ratio value (R2) corresponding to point T2 from the D / G ratio value (R1) corresponding to point T1 (HW = R1 - R2).

[0047] When calculating the half-value width HW, the surface of the positive electrode active material layer 100B is analyzed at 10 different locations using Raman spectroscopy, and 10 half-value widths are calculated based on the analysis results of the 10 locations (10 Raman mappings and 10 histograms), and the average value of the 10 half-value widths is taken as the half-value width HW.

[0048] The reason why the half-width HW is 0.5 or less is that the dispersibility of the positive electrode conductive agent within the positive electrode active material layer 100B is improved, resulting in a uniform distribution of the D / G ratio within the positive electrode active material layer 100B. In this case, the electrical resistance and physical strength within the positive electrode active material layer 100B are uniform. This facilitates uniform occlusion and desorption of lithium within the positive electrode active material layer 100B when a secondary battery using the positive electrode 100 is charged and discharged, and facilitates uniform expansion and contraction of the positive electrode active material layer 100B. Therefore, the positive electrode active material layer 100B is less likely to deteriorate or break, even when the secondary battery is repeatedly charged and discharged.

[0049] The reason why the half-width HW is 0.5 or less is that, as will be described later, when preparing the cathode composite slurry in the manufacturing process of the cathode 100, the cathode conductive agent is added to a solvent containing the cathode active material at different times while stirring the solvent. That is, the cathode active material and the cathode conductive agent are not added to the solvent together, but the cathode active material is added to the solvent and then the cathode conductive agent is added to the solvent separately. In this case, the half-width HW can be controlled to a desired value by adjusting the stirring conditions, such as the stirring speed and stirring time.

[0050] The same applies to the positive electrode binder as described above. Specifically, when the positive electrode active material layer 100B contains a positive electrode binder, in order to set the half-width HW to 0.5 or less, in the manufacturing process of the positive electrode 100 (when preparing the positive electrode mixture slurry), the positive electrode conductive agent and the positive electrode binder are added to a solvent containing the positive electrode active material with a time lag while stirring the solvent. That is, instead of adding the positive electrode active material, the positive electrode conductive agent, and the positive electrode binder together to the solvent, only one of the positive electrode conductive agent and the positive electrode binder is added to the solvent containing the positive electrode active material, and then the other of the positive electrode conductive agent and the positive electrode binder is added separately.

[0051] The method for producing the positive electrode 100 (the procedure for preparing the positive electrode mixture slurry) will be described in detail later.

[0052] <1-3. Operation> In this positive electrode 100, during the electrode reaction, lithium is released in an ionic state from the positive electrode active material layer 100B, and lithium is absorbed in an ionic state into the positive electrode active material layer 100B.

[0053] <1-4. Manufacturing Method> When manufacturing the positive electrode 100, a positive electrode mixture slurry is prepared according to the procedure described below as an example, and then the positive electrode 100 is fabricated using the positive electrode mixture slurry.

[0054] In the following, a case will be described in which the positive electrode active material layer 100B is formed using a positive electrode mixture slurry containing a positive electrode binder in addition to a positive electrode active material and a positive electrode conductive agent.

[0055] [Preparation of Positive Electrode Mixture Slurry] When preparing the positive electrode mixture slurry, as described below, a first dispersion liquid and a second dispersion liquid are prepared in this order, and then the positive electrode mixture slurry is prepared using the second dispersion liquid.

[0056] (Preparation of First Dispersion) First, the positive electrode active material is added to a solvent, and the solvent is then stirred. As a result, the positive electrode active material is dispersed in the solvent, and a first dispersion is prepared.

[0057] The type of solvent is not particularly limited, and may be an aqueous solvent or a non-aqueous solvent (organic solvent). In this case, a stirrer such as a planetary mixer, a homogenizer, or a ball mill may be used to stir the solvent. Stirring conditions such as the stirring speed (rotation speed of the stirrer (rpm)) and the stirring time (minutes) can be set as desired.

[0058] (Preparation of Second Dispersion) Subsequently, while stirring the first dispersion, either one of the positive electrode conductive agent or the positive electrode binder is added to the first dispersion, and the first dispersion is then stirred. In this case, the above-described stirrer may be used.

[0059] As a result, when a positive electrode conductive agent is added to the first dispersion, the positive electrode conductive agent is dispersed in the first dispersion, thereby preparing a second dispersion, whereas when a positive electrode binder is added to the first dispersion, the positive electrode binder is dissolved in the first dispersion, thereby preparing a second dispersion.

[0060] (Preparation of Positive Electrode Mixture Slurry) Finally, while stirring the second dispersion, the other of the positive electrode conductive agent and the positive electrode binder is added to the second dispersion, and then the second dispersion is stirred. This "other" refers to the positive electrode binder when the positive electrode conductive agent is added to the first dispersion, and also refers to the positive electrode conductive agent when the positive electrode binder is added to the first dispersion. In this case, the above-mentioned stirrer may be used.

[0061] As a result, when a positive electrode conductive agent is added to the second dispersion, the positive electrode conductive agent is dispersed in the second dispersion, thereby preparing a positive electrode mixture slurry, and when a positive electrode binder is added to the second dispersion, the positive electrode binder is dissolved in the second dispersion, thereby preparing a positive electrode mixture slurry.

[0062] Here, the reason why the positive electrode conductive agent and the positive electrode binder are added with a time lag to prepare the positive electrode mixture slurry is that the dispersibility of the positive electrode conductive agent in the positive electrode mixture slurry is improved, and the half width HW falls within the above-mentioned range.

[0063] In particular, by adding only the positive electrode conductive agent to the first dispersion liquid separately from the positive electrode binder, the dispersibility of the positive electrode conductive agent in the first dispersion liquid is improved compared to when both the positive electrode conductive agent and the positive electrode binder are added to the first dispersion liquid together, which makes it easier for the positive electrode conductive agent to be uniformly dispersed in the first dispersion liquid.

[0064] The advantages of the positive electrode conductive agent described here are also obtained for the positive electrode binder. That is, by adding only the positive electrode binder to the first dispersion liquid separately from the positive electrode conductive agent, the dispersibility of the positive electrode binder in the first dispersion liquid is improved compared to when both the positive electrode binder and the positive electrode conductive agent are added to the first dispersion liquid together. This makes it easier for the positive electrode binder to be dissolved uniformly in the first dispersion liquid.

[0065] Therefore, the dispersibility of the positive electrode conductive agent is improved inside the positive electrode active material layer 100B formed using the positive electrode mixture slurry in a later step, and the D / G ratio is more likely to be uniformly distributed, so that the half width HW falls within the above-mentioned range.

[0066] The advantages of preparing the first dispersion described here are similarly obtained when preparing the second dispersion. That is, by adding only the positive electrode conductive agent to the second dispersion separately from the positive electrode binder, the dispersibility of the positive electrode conductive agent in the second dispersion is improved, making it easier for the positive electrode conductive agent to be uniformly dispersed in the second dispersion. Furthermore, by adding only the positive electrode binder to the second dispersion separately from the positive electrode conductive agent, the solubility of the positive electrode binder in the second dispersion is improved, making it easier for the positive electrode binder to be uniformly dissolved in the second dispersion.

[0067] When adding a positive electrode conductive agent to the first dispersion, instead of adding the positive electrode conductive agent directly to the first dispersion, a dispersion in which the positive electrode conductive agent is dispersed in a solvent in advance may be added to the first dispersion. This is because the dispersibility of the positive electrode conductive agent in the first dispersion is improved. Details regarding the solvent are as described above.

[0068] Of course, when adding a positive electrode conductive agent to the second dispersion, a dispersion in which the positive electrode conductive agent is dispersed in a solvent in advance may be added to the second dispersion in the same manner.

[0069] Furthermore, when adding a positive electrode binder to the first dispersion, instead of adding the positive electrode binder directly to the first dispersion, a solution in which the positive electrode binder is dissolved in a solvent in advance may be added to the first dispersion. This is because the dispersibility of the positive electrode binder in the first dispersion is improved. Details regarding the solvent are as described above.

[0070] Of course, when adding a positive electrode binder to the second dispersion, a dispersion in which the positive electrode conductive agent is dispersed in a solvent in advance may be added to the second dispersion in the same manner.

[0071] Furthermore, when two or more types of positive electrode conductive agents are used to prepare the positive electrode mixture slurry, it is preferable to add the two or more types of positive electrode conductive agents at different times, because this improves the dispersibility of each positive electrode conductive agent in the positive electrode mixture slurry for the reasons described above.

[0072] For example, when two types of positive electrode conductive agents are used, the order of adding the positive electrode binder and the two types of positive electrode conductive agents may be any of the orders described below.

[0073] First, (1) a positive electrode binder may be added, (2) a first type of positive electrode conductive agent may be added, and (3) a second type of positive electrode conductive agent may be added.

[0074] Secondly, (1) a positive electrode binder may be added, (2) a second type of positive electrode conductive agent may be added, and (3) a first type of positive electrode conductive agent may be added.

[0075] Third, (1) a first type of positive electrode conductive agent may be added, (2) a positive electrode binder may be added, and (3) a second type of positive electrode conductive agent may be added.

[0076] Fourth, (1) a first type of positive electrode conductive agent may be added, (2) a second type of positive electrode conductive agent may be added, and (3) a positive electrode binder may be added.

[0077] Fifth, (1) a second type of positive electrode conductive agent may be added, (2) a positive electrode binder may be added, and (3) a first type of positive electrode conductive agent may be added.

[0078] Sixth, (1) a second type of positive electrode conductive agent may be added, (2) a first type of positive electrode conductive agent may be added, and (3) a positive electrode binder may be added.

[0079] [Fabrication of Positive Electrode] When fabricating the positive electrode 100 using the positive electrode mixture slurry, the positive electrode mixture slurry is applied to one surface of the positive electrode current collector 100A to form the positive electrode active material layer 100B. The positive electrode active material layer 100B may then be compression-molded using a molding machine such as a roll press. In this case, the positive electrode active material layer 100B may be heated, or the compression molding may be repeated multiple times.

[0080] As a result, the positive electrode active material layer 100B is formed on one surface of the positive electrode current collector 100A, and thus the positive electrode 100 is completed.

[0081] <1-5. Actions and Effects> According to this positive electrode 100, the positive electrode active material layer 100B contains a positive electrode active material and a positive electrode conductive agent, the positive electrode conductive agent contains a carbon material, and the half width HW of the peak P identified based on the results of an analysis of the surface of the positive electrode active material layer 100B using Raman spectroscopy is 0.5 or less.

[0082] In this case, as described above, the dispersibility of the positive electrode conductive agent inside the positive electrode active material layer 100B is improved, and the D / G ratio tends to be uniformly distributed. This results in a uniform electrical resistance and a uniform physical strength inside the positive electrode active material layer 100B. Therefore, when a secondary battery using the positive electrode 100 is charged and discharged, lithium tends to be uniformly absorbed and desorbed inside the positive electrode active material layer 100B, and the positive electrode active material layer 100B tends to expand and contract uniformly.

[0083] For these reasons, the positive electrode active material layer 100B is less likely to deteriorate or be damaged even when the secondary battery is repeatedly charged and discharged, and therefore a secondary battery having excellent battery characteristics can be realized by using the positive electrode 100.

[0084] In particular, when the carbon material contains a particulate carbon material and a fibrous carbon material, a conductive network using the positive electrode active material, the particulate carbon material, and the fibrous carbon material is easily formed in the positive electrode active material layer 100B, thereby further improving the conductivity of the positive electrode active material layer 100B and achieving a greater effect.

[0085] Furthermore, if the positive electrode active material layer 100B further contains a positive electrode binder, the half-value width HW is controlled to be within the above-described range, and the binding property of the positive electrode active material and the positive electrode conductive agent is improved, thereby obtaining a higher effect.

[0086] 2. Secondary Battery Next, a secondary battery according to an embodiment of the present technology to which the positive electrode 100 is applied will be described.

[0087] The secondary battery described here is a secondary battery that obtains battery capacity by absorbing and releasing an electrode reactant, and includes a positive electrode, a negative electrode, and an electrolyte. Hereinafter, as described above, the case where the electrode reactant is lithium will be taken as an example. A secondary battery that obtains battery capacity by absorbing and releasing lithium is a so-called lithium-ion secondary battery. In this lithium-ion secondary battery, lithium is absorbed and released in an ionic state.

[0088] The charge capacity of the negative electrode is preferably larger than the discharge capacity of the positive electrode. That is, the electrochemical capacity per unit area of ​​the negative electrode is preferably larger than the electrochemical capacity per unit area of ​​the positive electrode. This is to prevent lithium from being deposited on the surface of the negative electrode during charging.

[0089] <2-1. Configuration> Fig. 3 shows a perspective view of the secondary battery, and Fig. 4 shows an enlarged cross-sectional configuration of the battery element 20 shown in Fig. 3. However, Fig. 3 shows a state in which the exterior film 10 and the battery element 20 are separated from each other, and the cross section of the battery element 20 along the XZ plane is shown by a dashed line. Also, Fig. 4 shows only a portion of the battery element 20.

[0090] This secondary battery includes an exterior film 10, a battery element 20, a positive electrode lead 31, a negative electrode lead 32, and sealing films 41 and 42. The secondary battery described here is a laminate film type secondary battery that uses a flexible or pliable exterior film 10 as an exterior member for housing the battery element 20.

[0091] [Exterior Film] The exterior film 10 has a bag-like structure that is sealed with the battery element 20 housed therein. As a result, the exterior film 10 houses an electrolyte solution together with a positive electrode 21 and a negative electrode 22, which will be described later.

[0092] Here, the exterior film 10 is a single film-like member that is folded in a folding direction F. The exterior film 10 is provided with a recessed portion 10U (a so-called deep drawn portion) for accommodating the battery element 20.

[0093] Specifically, the exterior film 10 is a three-layer laminate film in which a fusion layer, a metal layer, and a surface protection layer are laminated in this order from the inside out, and when the exterior film 10 is folded, the outer peripheral edges of the opposing fusion layers are fused to each other. The fusion layer contains a polymer compound such as polypropylene. The metal layer contains a metal material such as aluminum. The surface protection layer contains a polymer compound such as nylon.

[0094] However, the configuration (number of layers) of the exterior film 10, which is a laminate film, is not particularly limited, and may be one layer, two layers, or four or more layers.

[0095] [Battery Element] The battery element 20 is a power generating element including a positive electrode 21 , a negative electrode 22 , a separator 23 , and an electrolyte (not shown), and is housed inside the exterior film 10 .

[0096] This battery element 20 is a so-called wound electrode body, and therefore the positive electrode 21 and the negative electrode 22 are wound around a winding axis P while facing each other with a separator 23 interposed therebetween. This winding axis P is an imaginary axis extending in the Y-axis direction.

[0097] The three-dimensional shape of battery element 20 is not particularly limited. Here, battery element 20 is flat, and therefore the shape of a cross section (cross section along the XZ plane) of battery element 20 intersecting winding axis P is a flat shape defined by a major axis J1 and a minor axis J2. This major axis J1 is an imaginary axis that extends in the X-axis direction and has a length greater than that of minor axis J2, and minor axis J2 is an imaginary axis that extends in the Z-axis direction intersecting with the X-axis direction and has a length smaller than that of major axis J1. Here, the three-dimensional shape of battery element 20 is a flat cylindrical shape, and therefore the shape of the cross section of battery element 20 is a flat, approximately elliptical shape.

[0098] (Positive Electrode) The positive electrode 21 has the same configuration as the positive electrode 100 .

[0099] Specifically, the positive electrode 21 includes a positive electrode current collector 21A and a positive electrode active material layer 21B. The configuration of the positive electrode current collector 21A is similar to the configuration of the positive electrode current collector 100A, and the configuration of the positive electrode active material layer 21B is similar to the configuration of the positive electrode active material layer 100B. Here, the positive electrode active material layer 21B is provided on both sides of the positive electrode current collector 21A.

[0100] (Negative Electrode) The negative electrode 22 includes a negative electrode current collector 22A and a negative electrode active material layer 22B.

[0101] The negative electrode current collector 22A has a pair of surfaces on which the negative electrode active material layer 22B is provided. The negative electrode current collector 22A contains a conductive material such as a metal material, and a specific example of the conductive material is copper.

[0102] The negative electrode active material layer 22B includes one or more types of negative electrode active materials that absorb and release lithium. However, the negative electrode active material layer 22B may further include one or more types of other materials, such as a negative electrode binder and a negative electrode conductive agent. The method for forming the negative electrode active material layer 22B is not particularly limited, and specifically includes one or more types of a coating method, a vapor phase method, a liquid phase method, a thermal spraying method, and a firing method (sintering method).

[0103] Here, the anode active material layer 22B is provided on both sides of the anode current collector 22A. However, the anode active material layer 22B may be provided on only one side of the anode current collector 22A on the side where the anode 22 faces the cathode 21.

[0104] The type of negative electrode active material is not particularly limited, but specific examples include carbon materials and metal-based materials, because high energy density can be obtained.

[0105] Specific examples of carbon materials include graphitizable carbon, non-graphitizable carbon, and graphite (natural graphite and artificial graphite).

[0106] The metal-based material is a material containing, as a constituent element, one or more of metal elements and metalloid elements that can form an alloy with lithium, and specific examples of the metal elements and metalloid elements include silicon and tin. This metal-based material may be a simple substance, an alloy, a compound, a mixture of two or more of these, or a material containing two or more of these phases. However, since the simple substance may contain any amount of impurities, the purity of the simple substance is not necessarily limited to 100%. A specific example of the metal-based material is TiSi 2  and SiO x  (0<x≦2, or 0.2<x<1.4), etc.

[0107] The negative electrode binder contains one or more of materials such as synthetic rubber and polymer compounds. Specific examples of synthetic rubber include styrene-butadiene rubber, fluorine-containing rubber, and ethylene-propylene-diene. Specific examples of polymer compounds include polyvinylidene fluoride, polyimide, and carboxymethyl cellulose.

[0108] The negative electrode conductive agent contains one or more conductive materials such as a carbon material, a metal material, and a conductive polymer compound, and specific examples of the carbon material include graphite, carbon black, acetylene black, and ketjen black.

[0109] (Separator) The separator 23 is an insulating porous film interposed between the positive electrode 21 and the negative electrode 22, and allows lithium ions to pass through while preventing a short circuit caused by contact between the positive electrode 21 and the negative electrode 22. The separator 23 contains a polymer compound such as polyethylene.

[0110] (Electrolyte) The electrolyte is a liquid electrolyte that is impregnated into each of the positive electrode 21, the negative electrode 22, and the separator 23, and contains a solvent and an electrolyte salt.

[0111] Here, the solvent contains one or more types of non-aqueous solvents (organic solvents), and the electrolyte solution containing the non-aqueous solvent is a so-called non-aqueous electrolyte solution. The non-aqueous solvents include esters and ethers, more specifically, carbonate ester compounds, carboxylic acid ester compounds, and lactone compounds. This is because the dissociation of the electrolyte salt is improved and the mobility of ions is also improved.

[0112] The carbonate ester compounds include cyclic carbonate esters and chain carbonate esters. Specific examples of the cyclic carbonate esters include ethylene carbonate and propylene carbonate, and specific examples of the chain carbonate esters include dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate.

[0113] The carboxylic acid ester compound is a chain carboxylic acid ester, and specific examples of the chain carboxylic acid ester include ethyl acetate, ethyl propionate, propyl propionate, and ethyl trimethylacetate. The lactone compound is a lactone, and specific examples of the lactone include γ-butyrolactone and γ-valerolactone. The ether may be 1,2-dimethoxyethane, tetrahydrofuran, 1,3-dioxolane, or 1,4-dioxane.

[0114] The electrolyte salt contains one or more light metal salts such as lithium salts. Specific examples of lithium salts include lithium hexafluorophosphate (LiPF 6  ), lithium tetrafluoroborate (LiBF 4 ), lithium trifluoromethanesulfonate (LiCF 3  SO 3  ), lithium bis(fluorosulfonyl)imide (LiN(FSO 2  ) 2  ), lithium bis(trifluoromethanesulfonyl)imide (LiN(CF 3  SO 2  ) 2  ), lithium tris(trifluoromethanesulfonyl)methide (LiC(CF 3  SO 2  ) 3  ), lithium bis(oxalato)borate (LiB(C 2  O 4  ) 2  ), lithium monofluorophosphate (Li 2  PFO 3  ) and lithium difluorophosphate (LiPF 2  O 2  ) etc. This is because a high battery capacity can be obtained.

[0115] The content of the electrolyte salt is not particularly limited, but specifically, it is 0.3 mol / kg to 3.0 mol / kg relative to the solvent, because high ionic conductivity can be obtained.

[0116] The electrolyte may further contain one or more additives, which improves the electrochemical stability of the electrolyte. The additives are not particularly limited, but specific examples include unsaturated cyclic carbonates, fluorinated cyclic carbonates, sulfonates, phosphates, acid anhydrides, nitrile compounds, and isocyanate compounds.

[0117] Specific examples of unsaturated cyclic carbonates include vinylene carbonate, vinylethylene carbonate, and methyleneethylene carbonate. Specific examples of fluorinated cyclic carbonates include monofluoroethylene carbonate and difluoroethylene carbonate. Specific examples of sulfonic acid esters include propane sultone and propene sultone. Specific examples of phosphate esters include trimethyl phosphate and triethyl phosphate. Specific examples of acid anhydrides include succinic anhydride, 1,2-ethanedisulfonic anhydride, and 2-sulfobenzoic anhydride. Specific examples of nitrile compounds include succinonitrile. Specific examples of isocyanate compounds include hexamethylene diisocyanate.

[0118] [Positive Electrode Lead and Negative Electrode Lead] The positive electrode lead 31 is a positive electrode terminal connected to the positive electrode current collector 21A and is led out of the exterior film 10. The positive electrode lead 31 contains a conductive material such as a metal material, and a specific example of the conductive material is aluminum. The shape of the positive electrode lead 31 is not particularly limited, but is specifically either a thin plate shape or a mesh shape.

[0119] The negative electrode lead 32 is a negative electrode terminal connected to the negative electrode current collector 22A, and is led out of the exterior film 10. The negative electrode lead 32 contains a conductive material such as a metal material, and a specific example of the conductive material is copper. Here, the details regarding the lead-out direction and shape of the negative electrode lead 32 are the same as the details regarding the lead-out direction and shape of the positive electrode lead 31.

[0120] [Sealing Film] The sealing film 41 is inserted between the exterior film 10 and the positive electrode lead 31, and the sealing film 42 is inserted between the exterior film 10 and the negative electrode lead 32. However, one or both of the sealing films 41 and 42 may be omitted.

[0121] The sealing film 41 is a sealing member that prevents outside air and the like from entering the interior of the exterior film 10. Specifically, the sealing film 41 contains a polymer compound such as polyolefin that has adhesiveness to the positive electrode lead 31, and a specific example of the polyolefin is polypropylene.

[0122] The configuration of the sealing film 42 is the same as the configuration of the sealing film 41, except that the sealing film 42 is a sealing member that has adhesion to the negative electrode lead 32. That is, the sealing film 42 contains a polymer compound such as polyolefin that has adhesion to the negative electrode lead 32.

[0123] <2-2. Operation> The secondary battery operates as follows during charging and discharging.

[0124] During charging, lithium is released from the positive electrode 21 of the battery element 20 and is absorbed into the negative electrode 22 via the electrolyte. During discharging, lithium is released from the negative electrode 22 of the battery element 20 and is absorbed into the positive electrode 21 via the electrolyte. During charging and discharging, lithium is absorbed and released in an ionic state.

[0125] <2-3. Manufacturing Method> When manufacturing a secondary battery, the positive electrode 21 and the negative electrode 22 are each produced and an electrolytic solution is prepared according to the procedure described below as an example. Thereafter, the positive electrode 21, the negative electrode 22, and the electrolytic solution are used to assemble a secondary battery, and a stabilization process is performed on the assembled secondary battery.

[0126] [Fabrication of Positive Electrode] The positive electrode 21 is fabricated by forming the positive electrode active material layers 21B on both sides of the positive electrode current collector 21A using the same procedure as that for fabricating the positive electrode 100 described above.

[0127] [Fabrication of Negative Electrode] First, a paste-like negative electrode mixture slurry is prepared by adding a mixture (negative electrode mixture) of a negative electrode active material, a negative electrode binder, and a negative electrode conductive agent to a solvent. This solvent may be an aqueous solvent or a non-aqueous solvent (organic solvent). Next, the negative electrode mixture slurry is applied to both surfaces of the negative electrode current collector 22A to form the negative electrode active material layer 22B. The negative electrode active material layer 22B may then be compression-molded. As a result, the negative electrode active material layer 22B is formed on both surfaces of the negative electrode current collector 22A, and the negative electrode 22 is fabricated.

[0128] [Preparation of Electrolyte Solution] An electrolyte salt is added to a solvent, whereby the electrolyte salt is dispersed or dissolved in the solvent, thereby preparing an electrolyte solution.

[0129] [Assembly of Secondary Battery] First, the positive electrode lead 31 is connected to the positive electrode current collector 21A by a joining method such as welding, and the negative electrode lead 32 is connected to the negative electrode current collector 22A by a joining method such as welding.

[0130] Next, the positive electrode 21 and the negative electrode 22 are stacked together with the separator 23 interposed therebetween, and then the positive electrode 21, the negative electrode 22, and the separator 23 are wound together to produce a wound body (not shown). Next, the wound body is pressed using a press or the like to form a flat shape. The wound body after this formation has the same configuration as the battery element 20, except that the positive electrode 21, the negative electrode 22, and the separator 23 are not impregnated with an electrolyte solution.

[0131] Next, after the roll is housed inside the recess 10U, the exterior film 10 (adhesive layer / metal layer / surface protection layer) is folded to face each other. Next, the outer peripheral edges of two sides of the opposing adhesive layers are joined together using an adhesive method such as heat fusion, thereby housing the roll inside the bag-shaped exterior film 10.

[0132] Finally, after injecting an electrolyte solution into the bag-shaped exterior film 10, the outer peripheral edges of the remaining sides of the opposing fusion layers are joined together using an adhesive method such as heat fusion. In this case, a sealing film 41 is inserted between the exterior film 10 and the positive electrode lead 31, and a sealing film 42 is inserted between the exterior film 10 and the negative electrode lead 32.

[0133] As a result, the wound body is impregnated with the electrolyte, producing the battery element 20 which is a wound electrode body, and the battery element 20 is sealed inside the bag-shaped exterior film 10, thereby assembling a secondary battery.

[0134] [Stabilization Treatment of Assembled Secondary Battery] The assembled secondary battery is charged and discharged. Various conditions, such as the ambient temperature, the number of charge / discharge cycles (number of cycles), and the charge / discharge conditions, can be set as desired. This forms a coating on the surface of each of the positive electrode 21 and the negative electrode 22, electrochemically stabilizing the state of the battery element 20. This completes the secondary battery.

[0135] <2-4. Actions and Effects> In this secondary battery, the positive electrode 21 has a configuration similar to that of the positive electrode 100, and therefore, for the reasons described above, the positive electrode active material layer 21B is less likely to deteriorate or be damaged even with repeated charge and discharge. Therefore, the discharge capacity is less likely to decrease even with repeated charge and discharge, and excellent battery characteristics can be obtained.

[0136] In particular, if the secondary battery is a lithium ion secondary battery, a sufficient battery capacity can be stably obtained by utilizing the absorption and release of lithium, and therefore a greater effect can be obtained.

[0137] Other functions and effects of the secondary battery are the same as those of the positive electrode 100 .

[0138] 3. Modifications The configuration of the secondary battery described above can be modified as appropriate, as described below. However, the series of modifications described below may be combined with each other.

[0139] [Modification 1] A porous film separator 23 is used. However, although not specifically shown here, a laminated separator including a polymer compound layer may also be used.

[0140] Specifically, the laminated separator includes a porous membrane having a pair of surfaces and a polymer compound layer provided on one or both surfaces of the porous membrane. This is because the separator improves adhesion to the positive electrode 21 and the negative electrode 22, respectively, thereby suppressing misalignment of the battery element 20 (misalignment of the positive electrode 21, the negative electrode 22, and the separator 23). This suppresses swelling of the secondary battery even if a decomposition reaction of the electrolyte occurs. The polymer compound layer includes a polymer compound such as polyvinylidene fluoride. Polyvinylidene fluoride is excellent in physical strength and is electrochemically stable.

[0141] One or both of the porous film and the polymer compound layer may contain a plurality of insulating particles. This is because the plurality of insulating particles promotes heat dissipation when the secondary battery generates heat, thereby improving the safety (heat resistance) of the secondary battery. The plurality of insulating particles contain one or more insulating materials, such as inorganic materials and resin materials. Specific examples of inorganic materials include aluminum oxide, aluminum nitride, boehmite, silicon oxide, titanium oxide, magnesium oxide, and zirconium oxide. Specific examples of resin materials include acrylic resin and styrene resin.

[0142] When a laminated separator is produced, a precursor solution containing a polymer compound and a solvent is prepared, and then the precursor solution is applied to one or both sides of a porous film. In this case, multiple insulating particles may be added to the precursor solution as needed.

[0143] Even when this laminated separator is used, the same effect can be obtained because lithium becomes movable between the positive electrode 21 and the negative electrode 22. In this case, as described above, the safety of the secondary battery is particularly improved, and therefore, a greater effect can be obtained.

[0144] [Modification 2] An electrolytic solution that is a liquid electrolyte is used. However, although not specifically shown here, an electrolyte layer that is a gel electrolyte may also be used.

[0145] In the battery element 20 using the electrolyte layer, the positive electrode 21 and the negative electrode 22 are wound facing each other with the separator 23 and the electrolyte layer interposed therebetween. The electrolyte layer is interposed between the positive electrode 21 and the separator 23, and also between the negative electrode 22 and the separator 23.

[0146] Specifically, the electrolyte layer contains a polymer compound together with an electrolytic solution, and the electrolytic solution is held by the polymer compound. This is because leakage of the electrolytic solution is prevented. The composition of the electrolytic solution is as described above. The polymer compound contains polyvinylidene fluoride, etc. When forming the electrolyte layer, a precursor solution containing the electrolytic solution, the polymer compound, a solvent, etc. is prepared, and then the precursor solution is applied to one or both surfaces of each of the positive electrode 21 and the negative electrode 22.

[0147] Even when this electrolyte layer is used, the same effect can be obtained because lithium can move between the positive electrode 21 and the negative electrode 22 via the electrolyte layer. In this case, particularly, as described above, leakage of the electrolyte solution is prevented, so that a greater effect can be obtained.

[0148] 4. Uses of Secondary Batteries There are no particular limitations on the uses (application examples) of secondary batteries. Secondary batteries used as power sources may be the main power source or auxiliary power source in electronic devices, electric vehicles, and the like. The main power source is a power source that is used preferentially regardless of the presence or absence of other power sources. The auxiliary power source may be a power source used in place of the main power source or a power source that can be switched from the main power source.

[0149] Specific examples of uses for secondary batteries are as follows: Electronic devices such as video cameras, digital still cameras, mobile phones, laptop computers, headphone stereos, portable radios, and portable information terminals. Storage devices such as backup power supplies and memory cards. Power tools such as power drills and power saws. Battery packs installed in electronic devices. Medical electronic devices such as pacemakers and hearing aids. Electric vehicles such as electric cars (including hybrid cars). Power storage systems such as home or industrial battery systems that store power in preparation for emergencies. In these uses, one secondary battery may be used, or multiple secondary batteries may be used.

[0150] The battery pack may use a single cell or a battery pack. The electric vehicle is a vehicle that runs on a secondary battery as a driving power source, and may be a hybrid vehicle that also has a driving source other than the secondary battery. In a home power storage system, power stored in a secondary battery, which is a power storage source, can be used to power home electrical appliances, etc.

[0151] Here, an example of an application of the secondary battery will be specifically described. The configuration of the application described below is merely an example and can be modified as appropriate.

[0152] Fig. 5 shows the block configuration of a battery pack. The battery pack described here is a battery pack (a so-called soft pack) that uses one secondary battery, and is installed in electronic devices such as smartphones.

[0153] 5, the battery pack includes a power supply 51 and a circuit board 52. The circuit board 52 is connected to the power supply 51 and includes a positive terminal 53, a negative terminal 54, and a temperature detection terminal 55.

[0154] The power source 51 includes one secondary battery. The positive electrode lead of this secondary battery is connected to a positive electrode terminal 53, and the negative electrode lead is connected to a negative electrode terminal 54. The power source 51 can be connected to the outside via the positive electrode terminal 53 and the negative electrode terminal 54, and is therefore capable of charging and discharging. The circuit board 52 includes a control unit 56, a switch 57, a PTC element 58, and a temperature detection unit 59. However, the PTC element 58 may be omitted.

[0155] The control unit 56 includes a central processing unit (CPU) and memory, and controls the operation of the entire battery pack. The control unit 56 detects and controls the usage state of the power source 51 as necessary.

[0156] When the voltage of the power supply 51 (secondary battery) reaches the overcharge detection voltage or the overdischarge detection voltage, the control unit 56 turns off the switch 57 to prevent the charging current from flowing through the current path of the power supply 51. The overcharge detection voltage is not particularly limited, but specifically, it is 4.20 V±0.05 V. The overdischarge detection voltage is not particularly limited, but specifically, it is 2.40 V±0.1 V.

[0157] Switch 57 includes a charge control switch, a discharge control switch, a charge diode, a discharge diode, etc., and switches between the connection and disconnection of power supply 51 and an external device in response to instructions from control unit 56. Switch 57 includes a metal oxide semiconductor field effect transistor (MOSFET), etc., and the charge / discharge current is detected based on the ON resistance of switch 57.

[0158] Temperature detection unit 59 includes a temperature detection element such as a thermistor. Temperature detection unit 59 measures the temperature of power supply 51 using temperature detection terminal 55 and outputs the temperature measurement result to control unit 56. The temperature measurement result measured by temperature detection unit 59 is used when control unit 56 performs charge / discharge control in the event of abnormal heat generation and when control unit 56 performs correction processing when calculating the remaining capacity.

[0159] An embodiment of the present technology will be described.

[0160] Examples 1 to 4 and Comparative Examples 1 to 5 As will be explained below, secondary batteries were manufactured, and then the battery characteristics of the secondary batteries were evaluated.

[0161] [Manufacturing of Secondary Battery] FIG. 6 shows a cross-sectional structure of a test secondary battery, which is a so-called coin-type secondary battery (lithium ion secondary battery).

[0162] This secondary battery includes a test electrode 61, a counter electrode 62, a separator 63, an exterior cup 64, an exterior can 65, a gasket 66, and an electrolyte (not shown).

[0163] The test electrode 61 is housed in an exterior cup 64, and the counter electrode 62 is housed in an exterior can 65. The test electrode 61 and the counter electrode 62 are stacked together with a separator 63 interposed therebetween, and the test electrode 61, the counter electrode 62, and the separator 63 are impregnated with an electrolyte. The exterior cup 64 and the exterior can 65 are crimped together with a gasket 66, so that the test electrode 61, the counter electrode 62, and the separator 63 are sealed by the exterior cup 64 and the exterior can 65.

[0164] The secondary battery shown in FIG. 6 was fabricated according to the procedure described below.

[0165] (Preparation of Test Electrode) First, a powder of a positive electrode active material (LiCoO , a lithium-containing compound (oxide)) was dissolved in a solvent (N-methyl-2-pyrrolidone, an organic solvent). 2  After adding the above ingredients, the solvent was stirred using a stirrer (homogenizer) equipped with a stirrer, to prepare a first dispersion. The stirring conditions were a stirring speed (number of rotations) of the stirrer of 3000 rpm and a stirring time of 15 minutes.

[0166] Subsequently, while the first dispersion was being stirred, two types of powdered positive electrode conductive agents (carbon materials) and a pellet-shaped positive electrode binder were added to the first dispersion with a time lag, thereby preparing a positive electrode mixture slurry.

[0167] The two types of positive electrode conductive agents were carbon black (CB, median diameter of primary particles = 23 nm) as the first type of positive electrode conductive agent (particulate carbon material) and carbon nanotubes (CNT, average fiber diameter = 15 μm, average fiber length = 150 μm) as the second type of positive electrode conductive agent (fibrous carbon material).Polyvinylidene fluoride (PVDF) was used as the positive electrode binder.

[0168] In particular, a positive electrode conductive agent solution in which a second type of positive electrode conductive agent (carbon nanotubes) was dispersed in advance in a solvent (N-methyl-2-pyrrolidone) was used, and a positive electrode binder solution in which a positive electrode binder (polyvinylidene fluoride) was dissolved in advance in a solvent (N-methyl-2-pyrrolidone) was used.

[0169] When preparing the positive electrode mixture slurry, as shown in Table 1, in three steps (first step, second step, and third step), two types of positive electrode conductive agents and a positive electrode binder were added at different times, and then the mixture was stirred using a stirrer.

[0170] The "Material" column in Table 1 shows the type of material added in each process. "PVDF" is the positive electrode binder (polyvinylidene fluoride), "CB" is the first type of positive electrode conductive agent (carbon black), and "CNT" is the second type of positive electrode conductive agent (carbon nanotubes). The stirring conditions (stirring speed (rpm) and stirring time (minutes)) in each process are as shown in Table 1.

[0171] As an example, the procedure for preparing the positive electrode mixture slurry in Example 1 is as follows.

[0172] First, a first dispersion containing a positive electrode active material was prepared according to the procedure described above. Subsequently, a first type of positive electrode conductive agent (carbon black) was added to the first dispersion while stirring the first dispersion, and the first dispersion was then stirred to prepare a second dispersion (first step). Subsequently, a positive electrode binder (polyvinylidene fluoride) was added to the second dispersion while stirring the second dispersion, and the second dispersion was then stirred to prepare a third dispersion (second step). Finally, a second type of positive electrode conductive agent (carbon nanotubes) was added to the third dispersion while stirring the third dispersion, and the third dispersion was then stirred to prepare a positive electrode mixture slurry (third step).

[0173] After preparing the positive electrode mixture slurry, the positive electrode mixture slurry was used to fabricate the positive electrode 100. Specifically, the positive electrode mixture slurry was applied to one surface of a positive electrode current collector (aluminum foil having a thickness of 12 μm) using a coating device, and then the positive electrode mixture slurry was dried to form a positive electrode active material layer.

[0174] Finally, the positive electrode current collector on which the positive electrode active material layer was formed was punched out into a disk shape (diameter = 16.5 mm), thereby producing a test electrode 61 (Examples 1 to 3 and Comparative Examples 1 to 4).

[0175] When producing this test electrode 61, the half-value width HW was changed by changing the order of addition of a series of materials (two types of positive electrode conductors and a positive electrode binder) and the stirring conditions (stirring speed and stirring time) in each step in the step of preparing the positive electrode mixture slurry, as shown in Table 1. The procedure for specifying the half-value width HW was as described above.

[0176] For comparison, a test electrode 61 was produced using the same procedure as in Comparative Example 5, except that in the step of preparing the positive electrode mixture slurry, instead of adding the series of materials (two types of positive electrode conductive agents and a positive electrode binder) separately at different times, the series of materials were added together.

[0177] (Fabrication of Counter Electrode) A lithium metal plate was punched out into a disk shape (diameter = 17 mm), thereby obtaining a counter electrode 62.

[0178] (Preparation of Electrolyte Solution) A solvent (ethylene carbonate, which is a cyclic carbonate ester, and diethyl carbonate, which is a chain carbonate ester) was dissolved in an electrolyte salt (lithium hexafluorophosphate (LiPF 6  )) was added, and the solvent was stirred. In this case, the mixing ratio (weight ratio) of the solvents was ethylene carbonate:diethyl carbonate=30:70, and the content of the electrolyte salt in the electrolytic solution was 1 mol / kg relative to the solvent. In this way, the electrolytic solution was prepared.

[0179] (Assembly of Secondary Battery) First, the test electrode 61 was placed in the exterior cup 64, and the counter electrode 62 was placed in the exterior can 65. Next, the test electrode 61 placed in the exterior cup 64 and the counter electrode 62 placed in the exterior can 65 were stacked together with a separator 63 (a microporous polyethylene film with a thickness of 20 μm) impregnated with an electrolyte interposed therebetween. In this case, the test electrode 61 was arranged so that the positive electrode active material layer and the counter electrode 62 faced each other with the separator 63 interposed therebetween. Next, with the test electrode 61 and the counter electrode 62 stacked together with the separator 63 interposed therebetween, the exterior cup 64 and the exterior can 65 were crimped together with the gasket 66. As a result, the test electrode 61 and the counter electrode 62 were sealed inside the exterior cup 64 and the exterior can 65, and a secondary battery was assembled.

[0180] (Stabilization Treatment of Assembled Secondary Battery) The secondary battery was subjected to one cycle of charge and discharge in a room temperature environment (temperature = 23°C). During charging, the battery was charged at a constant current of 0.1 C until the voltage reached 4.2 V, and then charged at a constant voltage of 0.025 C at the same voltage of 4.2 V. During discharging, the battery was discharged at a constant current of 0.1 C until the voltage reached 3.0 V. 0.1 C is the current value at which the battery capacity (theoretical capacity) is fully discharged in 10 hours, and 0.025 C is the current value at which the battery capacity is fully discharged in 40 hours.

[0181] As a result, the test electrode 61 and the counter electrode 62 were electrochemically stabilized, and the secondary battery was completed.

[0182] [Evaluation of Battery Characteristics] When the cycle characteristics were evaluated as the battery characteristics, the results shown in Table 1 were obtained.

[0183] When evaluating the cycle test, first, the discharge capacity (discharge capacity at the first cycle) was measured by charging and discharging the secondary battery in a room temperature environment (temperature = 23°C). Next, the discharge capacity (discharge capacity at the 100th cycle) was measured by repeatedly charging and discharging the secondary battery in the same environment until the number of cycles reached 100. Finally, the capacity retention rate, which is an index for evaluating cycle characteristics, was calculated based on the formula: capacity retention rate (%) = (discharge capacity at the 100th cycle / discharge capacity at the first cycle) × 100. The charge and discharge conditions were the same as those used during the stabilization treatment of the assembled secondary battery.

[0184] The values ​​of the capacity retention rate shown in Table 1 are normalized values ​​with the value of the capacity retention rate in Example 1 set to 100.

[0185]

[0186] [Discussion] As shown in Table 1, the capacity retention rate varied depending on the physical property (half width HW) of the test electrode 61 .

[0187] Specifically, when a series of materials were added at different times in the preparation process of the positive electrode mixture slurry (Examples 1 to 4 and Comparative Examples 1 to 4), the capacity retention rate changed depending on the half-value width HW. That is, when the half-value width HW was greater than 0.50 (Comparative Examples 1 to 4), the capacity retention rate decreased. In contrast, when the half-value width HW was 0.50 or less (Examples 1 to 4), the capacity retention rate increased.

[0188] When the series of materials were not added with a time lag in the preparation process of the positive electrode mixture slurry (Comparative Example 5), the half width HW was greater than 0.50, similar to the cases when the series of materials were added with a time lag in the preparation process of the positive electrode mixture slurry but the half width HW was greater than 0.50 (Comparative Examples 1 to 4), and therefore the capacity retention rate decreased.

[0189] Example 5 and Comparative Examples 6 and 7 Secondary batteries were fabricated in the same manner as in Example 1 and Comparative Examples 1 and 5, except that the type of positive electrode active material was changed as shown in Table 2. The battery characteristics of the secondary batteries were then evaluated. Here, LiCoO 2  Instead of LiNi 0.82 Co 0.14 Al 0.04 O 2  was used.

[0190]

[0191] As shown in Table 2, even when the type of positive electrode active material was changed, the same results as those in Table 1 were obtained. That is, when the half-value width HW was greater than 0.50 (Comparative Examples 6 and 7), the capacity retention ratio decreased. In contrast, when the half-value width HW was 0.50 or less (Example 5), the capacity retention ratio increased.

[0192] Example 6 and Comparative Example 8 Secondary batteries were fabricated in the same manner as in Example 1 and Comparative Example 5, except that the type of positive electrode conductive agent was changed as shown in Table 3. The battery characteristics of the secondary batteries were then evaluated. Here, one type of positive electrode conductive agent (carbon black) was used instead of two types of positive electrode conductive agents (carbon black (CB) and carbon nanotubes (CNT)).

[0193] The positive electrode mixture slurry was prepared using a two-stage process (first and second processes) as shown in Table 3. The "Materials" column in Table 3 indicates the type of material (positive electrode conductive agent and positive electrode binder) added in each process. The stirring conditions (stirring speed (rpm) and stirring time (minutes)) for each process are as shown in Table 3.

[0194]

[0195] As shown in Table 3, even when the type of positive electrode conductive agent was changed, the same results as those in Table 1 were obtained. That is, when the half width HW was greater than 0.50 (Comparative Example 8), the capacity retention rate decreased. In contrast, when the half width HW was 0.50 or less (Example 6), the capacity retention rate increased.

[0196] [Summary] From the results shown in Tables 1 to 3, when the positive electrode active material layer contained a positive electrode active material and a positive electrode conductive agent, the positive electrode conductive agent contained a carbon material, and the half width HW of the peak P identified based on the results of analysis of the surface of the positive electrode active material layer using Raman spectroscopy was 0.5 or less, the capacity retention rate increased. Therefore, the cycle characteristics were improved, and excellent battery characteristics were obtained in the secondary battery.

[0197] The present technology has been described above with reference to an embodiment and examples. However, the configuration of the present technology is not limited to the configuration described in the embodiment and examples, and can be modified in various ways.

[0198] Specifically, the battery structure of the secondary battery has been described as being of a laminate film type and a coin type. However, the battery structure of the secondary battery is not particularly limited, and may be of a cylindrical type, a square type, a button type, or the like.

[0199] The battery element has been described as having a wound structure. However, the structure of the battery element is not particularly limited, and may be a stacked structure or a zigzag structure. In the stacked structure, the positive and negative electrodes are stacked on top of each other, and in the zigzag structure, the positive and negative electrodes are folded in a zigzag pattern.

[0200] Furthermore, although the electrode reactant is lithium in the above description, the electrode reactant is not particularly limited. Specifically, as described above, the electrode reactant may be other alkali metals such as sodium and potassium, or alkaline earth metals such as beryllium, magnesium, and calcium. In addition, the electrode reactant may be other light metals such as aluminum.

[0201] The effects described in this specification are merely examples, and the effects of the present technology are not limited to the effects described in this specification. Therefore, other effects may be obtained with respect to the present technology.

[0202] The present technology may also be configured as follows. <1> A secondary battery comprising: a positive electrode including a positive electrode active material layer; a negative electrode; and an electrolyte; wherein the positive electrode active material layer includes a positive electrode active material and a positive electrode conductive agent; and the positive electrode conductive agent includes a carbon material; and wherein the half-width of a peak identified based on the results of an analysis of the surface of the positive electrode active material layer using Raman spectroscopy according to the following steps (1) to (3) is 0.50 or less. (1) A Raman mapping of a D / G ratio is obtained by analyzing the surface of the positive electrode active material layer using the Raman spectroscopy. (2) A histogram of the D / G ratio having the peak is obtained based on the Raman mapping. (3) The half-width of the peak is calculated based on the histogram. <2> The secondary battery according to <1>, wherein the carbon material includes a particulate carbon material and a fibrous carbon material. <3> The secondary battery according to <1> or <2>, wherein the positive electrode active material layer further includes a positive electrode binder. <4> The secondary battery according to any one of <1> to <3>, which is a lithium-ion secondary battery. <5> A positive electrode for a secondary battery, comprising a positive electrode active material layer, wherein the positive electrode active material layer contains a positive electrode active material and a positive electrode conductive agent, and the positive electrode conductive agent contains a carbon material, and wherein the half-width of a peak identified based on the results of an analysis of the surface of the positive electrode active material layer using Raman spectroscopy according to the steps (1) to (3) below is 0.50 or less. (1) A Raman mapping of the D / G ratio is obtained by analyzing the surface of the positive electrode active material layer using the Raman spectroscopy. (2) A histogram of the D / G ratio having the peak is obtained based on the Raman mapping. (3) The half-width of the peak is calculated based on the histogram.

[0203] 21... Positive electrode, 21B... Positive electrode active material layer, 22... Negative electrode

Claims

1. A secondary battery comprising: a positive electrode including a positive electrode active material layer; a negative electrode; and an electrolyte; wherein the positive electrode active material layer includes a positive electrode active material and a positive electrode conductive agent, and the positive electrode conductive agent includes a carbon material; and wherein the half-width of a peak identified based on the results of an analysis of the surface of the positive electrode active material layer using Raman spectroscopy according to the steps (1) to (3) below is 0.50 or less. (1) A Raman mapping of a D / G ratio is obtained by analyzing the surface of the positive electrode active material layer using the Raman spectroscopy. (2) A histogram of the D / G ratio having the peak is obtained based on the Raman mapping. (3) The half-width of the peak is calculated based on the histogram.

2. The secondary battery according to claim 1, wherein the carbon material includes a particulate carbon material and a fibrous carbon material.

3. The secondary battery according to claim 1 or 2, wherein the positive electrode active material layer further contains a positive electrode binder.

4. The secondary battery according to any one of claims 1 to 3, which is a lithium ion secondary battery.

5. A positive electrode for a secondary battery, comprising a positive electrode active material layer, the positive electrode active material layer containing a positive electrode active material and a positive electrode conductive agent, the positive electrode conductive agent containing a carbon material, and a half-width of a peak identified based on an analysis result of the surface of the positive electrode active material layer using Raman spectroscopy according to the steps (1) to (3) below is 0.50 or less. (1) A Raman mapping of a D / G ratio is obtained by analyzing the surface of the positive electrode active material layer using the Raman spectroscopy. (2) A histogram of the D / G ratio having the peak is obtained based on the Raman mapping. (3) The half-width of the peak is calculated based on the histogram.

Citation Information

Patent Citations

  • Positive electrode material for lithium ion secondary battery, positive electrode for lithium ion secondary battery, and lithium ion secondary battery

    JP2021158083A

  • Positive electrode for lithium secondary battery and lithium secondary battery including the same

    JP2022137007A

  • Binder composition for electromechanical element positive electrode, conductive material dispersion for electromechanical element positive electrode, slurry composition for electromechanical element positive electrode, positive electrode for electromechanical element, and electromechanical element