Coating-layer-provided positive electrode active material for lithium ion secondary batteries, coating-layer forming solution, method for producing coating-layer-provided positive electrode active material for lithium ion secondary batteries, and all-solid-state lithium ion secondary battery
A lithium metal composite oxide with a coating layer containing lithium, phosphorus, and a pentavalent transition metal element addresses capacity degradation issues in lithium ion secondary batteries by stabilizing the interface with sulfide-based solid electrolytes, ensuring efficient battery performance.
Patent Information
- Application Number
- PCT/JP2024/012911
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-06
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional lithium ion secondary batteries face capacity degradation due to the formation of high-resistance layers at the interface between sulfide-based solid electrolytes and oxide positive electrode active materials during charging and discharging, which is not adequately prevented by existing coating layers like lithium niobate.
A coating layer containing lithium, phosphorus, and a pentavalent transition metal element, such as niobium, is applied to a lithium metal composite oxide positive electrode active material with a layered rock salt structure, ensuring a coverage rate of 60% or more to suppress interfacial reactions and maintain battery capacity.
The proposed coating layer effectively prevents capacity degradation by stabilizing the interface and maintaining high discharge capacity and output characteristics in all-solid-state lithium ion secondary batteries.
Smart Images

Figure JP2024012911_03102024_PF_FP_ABST
Abstract
Description
Positive electrode active material for lithium ion secondary battery with coating layer, solution for forming coating layer, method for producing positive electrode active material for lithium ion secondary battery with coating layer, and all-solid-state lithium ion secondary battery
[0001] The present invention relates to a positive electrode active material for a lithium ion secondary battery with a coating layer, a solution for forming a coating layer, a method for producing a positive electrode active material for a lithium ion secondary battery with a coating layer, and an all-solid-state lithium ion secondary battery.
[0002] With the recent widespread use of electric vehicles, there has been a strong demand for the development of small, lightweight secondary batteries with high energy density, such as lithium-ion secondary batteries.
[0003] Currently, in general lithium ion secondary batteries, the positive electrode active material for lithium ion secondary batteries (hereinafter also referred to as "positive electrode active material") is LiCoO 2 , LiNiO 2 , LiMn 2 O 4 Lithium metal, lithium alloys, metal oxides, carbon, etc. are used as negative electrode active materials for lithium ion secondary batteries. In addition, LiClO in an organic solvent such as ethylene carbonate, dimethyl carbonate, or ethyl methyl carbonate is used as an electrolyte. 4 , LiPF 6 An electrolyte solution in which a Li salt such as the above is dissolved as a supporting salt is used.
[0004] Among the components of lithium-ion secondary batteries, the electrolyte in particular is a factor that limits battery performance, such as fast charging and lifespan, due to its chemical properties such as heat resistance and potential window. Therefore, research and development is currently being actively conducted on all-solid-state lithium-ion secondary batteries, which improve battery performance by using a solid electrolyte instead of the electrolyte.
[0005] As research and development of all-solid-state lithium ion secondary batteries progresses, it has been proposed, for example, in Patent Document 1 that sulfide-based solid electrolytes have high lithium ion conductivity and are therefore preferable for use in all-solid-state lithium ion secondary batteries.
[0006] However, as disclosed in Non-Patent Document 1, when a sulfide-based solid electrolyte comes into contact with an oxide positive electrode active material, a reaction occurs at the interface between the solid electrolyte and the positive electrode active material during charging and discharging, forming a high-resistance layer that inhibits battery operation, resulting in a decrease in battery capacity after repeated charging and discharging.
[0007] In order to suppress the formation of this high resistance layer, it has been proposed in Non-Patent Document 1 and elsewhere to provide a coating layer made of lithium niobate on the surface of the positive electrode active material. However, lithium niobate has a low potential of 4.6 V (vs. Li / Li + ) or higher, it decomposes, releasing oxygen and interdiffusing with the sulfur in the solid electrolyte layer, producing by-products that act as resistors. This may not be sufficient to prevent the formation of a resistive layer. Furthermore, mixing is likely to occur at the interface between the positive electrode active material and the coating layer, which is not sufficient to prevent resistance increases. Therefore, even when a coating layer made of lithium niobate is provided, the battery capacity decreases with repeated charging and discharging.
[0008] As a compound that has the effect of suppressing the mixing that occurs between the above-mentioned positive electrode active material and the coating layer, a compound containing phosphoric acid is effective, and it has been proposed in Non-Patent Document 2 and elsewhere that it is extremely stable compared to lithium niobate and the like.
[0009] However, compounds containing phosphoric acid have problems such as difficulty in existing in basic conditions, corroding the surface of the positive electrode active material when used in an acidic solution, and difficulty in controlling the composition when used in an organic solution due to the tendency of P (phosphorus) to disappear upon heating, making it difficult to control the composition. For these reasons, it has been difficult to form a coating layer on the surface of the positive electrode active material using compounds containing phosphoric acid.
[0010] Japanese Patent Application Publication No. 2014-56661
[0011] Narumi Ohta et al. , "LiNbO3-coated LiCoO2 as cathode material for all solid-state lithium secondary batteries", Electrochemistry Communications 9 (2007) 1486-1490William D. et al. , "Interface Stability in Solid-State Batteries", Chem. Mater. 2016, 28, 266-273
[0012] In view of the problems associated with the above-described conventional techniques, one aspect of the present invention aims to provide a positive electrode active material for a lithium ion secondary battery with a coating layer, which is applicable to an all-solid-state lithium ion secondary battery using a solid electrolyte and can suppress a decrease in battery capacity when repeatedly charged and discharged.
[0013] In order to solve the above-mentioned problems, one aspect of the present invention provides a positive electrode active material for a lithium ion secondary battery with a coating layer, comprising: a lithium metal composite oxide; and a coating layer that coats at least a portion of the surface of the lithium metal composite oxide and has a coverage of 60% or more, wherein the lithium metal composite oxide has a layered rock salt structure and contains lithium (Li), nickel (Ni), and an M element (M) in a substance amount ratio of Li:Ni:M=a:1-x:x, where a and x satisfy the relationships 0.98≦a≦1.20 and 0≦x≦1.0, and the M element is one or more elements excluding lithium, nickel, and oxygen, and the coating layer contains lithium, phosphorus, and a Z element, and the Z element is at least one pentavalent transition metal element.
[0014] According to one aspect of the present invention, it is possible to provide a coating layer-provided positive electrode active material for a lithium ion secondary battery, which is applicable to an all-solid-state lithium ion secondary battery using a solid electrolyte and can suppress a decrease in battery capacity during repeated charge and discharge.
[0015] Fig. 1 is a cross-sectional schematic diagram of a coating layer-attached positive electrode active material for a lithium ion secondary battery according to an embodiment of the present disclosure. Fig. 2 is a cross-sectional schematic diagram of a lithium ion secondary battery. Fig. 3 is an explanatory diagram of the cross-sectional configuration of a test battery used to evaluate battery characteristics.
[0016] Hereinafter, embodiments for carrying out the present invention will be described with reference to the drawings. However, the present invention is not limited to the following embodiments, and various modifications and substitutions can be made to the following embodiments without departing from the scope of the present invention.
[0017] A coating layer-formed positive electrode active material for a lithium ion secondary battery, a coating layer-forming solution, a method for producing a coating layer-formed positive electrode active material for a lithium ion secondary battery, and an all-solid-state lithium ion secondary battery according to one embodiment of the present invention will be described in the following order.
[0018] 1. Cathode active material for coated lithium-ion secondary battery 1-1. Lithium metal composite oxide 1-2. Coating layer 1-3. Other characteristics of the cathode active material for coated lithium-ion secondary battery 2. Coating layer-forming solution and method for producing the cathode active material for coated lithium-ion secondary battery 3. All-solid-state lithium-ion secondary battery 3-1. Positive electrode 3-2. Negative electrode 3-3. Solid electrolyte layer 3-4. Shape and configuration of secondary battery 3-5. Battery evaluation of secondary battery <1. Cathode active material for coated lithium-ion secondary battery> The inventors of the present invention have investigated a cathode active material for coated lithium-ion secondary battery that can be applied to an all-solid-state lithium-ion secondary battery (hereinafter also referred to as "secondary battery") that uses a solid electrolyte, and that can suppress a decrease in battery capacity during repeated charge and discharge. Specifically, the present inventors conducted extensive research into a coated cathode active material for lithium-ion secondary batteries (hereinafter also referred to as a "coated cathode active material") having a coating layer capable of suppressing interfacial reactions between the solid electrolyte and the cathode active material. As a result, they discovered that by coating a coating layer containing lithium, phosphorus, and the Z element on the surface of a lithium metal composite oxide, which is a cathode active material, in a certain amount or more so as to achieve a predetermined coverage, the coating layer can be applied to a secondary battery and the decrease in battery capacity during repeated charge and discharge can be suppressed, thereby completing the present invention.
[0019] As shown in the cross-sectional schematic diagram of Figure 1, the coating layer-equipped positive electrode active material 10 for a lithium ion secondary battery of this embodiment can have a lithium metal composite oxide 11, which is a positive electrode active material, and a coating layer 12 that coats at least a portion of the surface of the lithium metal composite oxide 11. Note that Figure 1 is a schematic cross-sectional diagram in which the lithium metal composite oxide 11 is shown as a circle, but the cross-sectional shape does not have to be circular and can have any shape. As will be described later, the coating layer 12 only needs to coat at least a portion of the surface of the lithium metal composite oxide 11, and does not need to coat the entire surface of the lithium metal composite oxide 11, nor does it need to have a uniform thickness.
[0020] Hereinafter, each component contained in the coating layer-equipped positive electrode active material for lithium-ion secondary batteries of this embodiment will be described. <1-1. Lithium Metal Composite Oxide> The lithium metal composite oxide, which is the positive electrode active material contained in the coating layer-equipped positive electrode active material of this embodiment, has a layered rock salt structure and can contain lithium (Li), nickel (Ni), and an M element (M) in a substance amount ratio of Li:Ni:M=a:1-x:x. In the above formula, Ni is nickel, and the M element is one or more elements excluding lithium, nickel, and oxygen.
[0021] The value of a in the above formula, which indicates the lithium content, can be 0.98 or more and 1.20 or less. That is, 0.98≦a≦1.20 can be satisfied. The value of a is more preferably 1.00 or more and 1.10 or less.
[0022] By setting the value of a to 0.98 or more, the internal resistance of a secondary battery using a coating layer-equipped positive electrode active material containing a lithium metal composite oxide can be suppressed, and the output characteristics can be improved. Furthermore, by setting the value of a to 1.20 or less, the initial discharge capacity of a secondary battery using a coating layer-equipped positive electrode active material containing the lithium metal composite oxide can be maintained high. In other words, by setting the value of a to the above-mentioned range, the output characteristics and capacity characteristics of a secondary battery using a coating layer-equipped positive electrode active material containing the lithium metal composite oxide can be improved.
[0023] Nickel (Ni) in the lithium metal composite oxide described above is an element that contributes to increasing the capacity of a secondary battery using a positive electrode active material containing the lithium metal composite oxide. In the lithium metal composite oxide, part or all of the nickel can be substituted with the M element. Therefore, the value of x, which represents the amount of nickel substituted, can be 0≦x≦1.0. However, since nickel (Ni) is an element that contributes to increasing the capacity of a secondary battery using a positive electrode active material containing the lithium metal composite oxide, as described above, it is preferable that the lithium metal composite oxide contains nickel, and x is preferably 0≦x≦0.7. It is particularly preferable that x is 0≦x≦0.65.
[0024] The M element is one or more elements excluding lithium, nickel, and oxygen, and can replace part or all of the nickel. The M element can contain at least one element selected from, for example, Al (aluminum), Ti (titanium), V (vanadium), Mn (manganese), Fe (iron), Co (cobalt), Cu (copper), Zr (zirconium), Nb (niobium), Mo (molybdenum), Ta (tantalum), and W (tungsten). The M element may be at least one element selected from the above element group.
[0025] It is particularly preferable that the M element contains at least cobalt. When the lithium metal composite oxide contains cobalt, the structure of the lithium metal composite oxide is more likely to be stabilized during charge and discharge, and therefore deterioration of the lithium metal composite oxide during high-voltage use of the secondary battery can be suppressed.
[0026] The structure of the lithium metal composite oxide can be identified by analytical techniques such as X-ray diffraction, electron beam diffraction, etc. The ratio of the amounts of elements contained in the lithium metal composite oxide and the coating layer-attached positive electrode active material can be determined by analytical techniques such as X-ray fluorescence analysis, ICP emission spectroscopy, etc.
[0027] The volume-average particle diameter of the lithium metal composite oxide particles, as measured with a laser diffraction / scattering particle size distribution analyzer, is preferably 1 μm or more and 10 μm or less, more preferably 2 μm or more and 7 μm or less, and even more preferably 3 μm or more and 5 μm or less. This is because, when the volume-average particle diameter of the lithium metal composite oxide particles is 1 μm or more and 10 μm or less, a secondary battery using a positive electrode active material with a coating layer containing the lithium metal composite oxide particles as a positive electrode can have a sufficiently large battery capacity per volume. <1-2. Coating Layer> The coating layer can contain lithium, phosphorus, and the element Z.
[0028] For example, the coating layer may contain a compound or mixture containing one or more elements selected from lithium, phosphorus, a Z element, and oxygen. Examples of the mixture include a mixture of compounds containing one or more elements selected from lithium, phosphorus, a Z element, and oxygen, and the coating layer may contain, for example, two or more of a Li-P-O compound, a Li-P-Z-O compound, and a Li-Z-O compound.
[0029] The element Z is at least one pentavalent transition metal element, and is preferably Nb (niobium).
[0030] By disposing a coating layer on the surface of the lithium metal composite oxide particles, an increase in the interfacial resistance between the lithium metal composite oxide and the solid electrolyte can be suppressed in a secondary battery equipped with a positive electrode containing the positive electrode active material with a coating layer of this embodiment. (Coverage Ratio) The coating layer is preferably disposed so that the coverage of the surface of the lithium metal composite oxide particles is a predetermined value or more.
[0031] The coverage rate of the coating layer, specifically the extent of the coverage area of the lithium metal composite oxide particles, can be calculated using the results of semi-quantitative analysis by X-ray photoelectron spectroscopy (XPS). Specifically, it can be determined from the ratio of the sum of the amounts of substance of phosphorus and Z element present on the surface to the sum of the amounts of substance of phosphorus, Z element, nickel, and M element, which are known from the results of semi-quantitative analysis by XPS on the positive electrode active material with a coating layer. The coverage rate of the coating layer can be calculated, for example, by the following formula (1). In the following formula (1), P, Z, Ni, and M correspond to the amounts of substance of phosphorus, Z element, nickel, and M element, respectively, measured by XPS.
[0032] (Coverage of coating layer (%)) = (P + Z) / (P + Z + Ni + M) × 100 ... (1) Due to its characteristics, XPS can selectively obtain information from a thickness of 1 nm to 5 nm of the surface of the object being measured. Therefore, the composition ratio of the surface layer of the material can be determined from the XPS measurement results. The coverage of the coating layer is preferably 60% or more, more preferably 65% or more, and even more preferably 70% or more. A coverage of 60% or more is effective in preventing both the interfacial reaction between the lithium metal composite oxide and the solid electrolyte and the interfacial mixing between the lithium metal composite oxide and the coating layer, thereby suppressing deterioration during cycling. Furthermore, the coating layer contains lithium, phosphorus, and Z elements, which improves stability even during high-voltage charging.
[0033] The upper limit of the coverage is not particularly limited, but can be, for example, 100% or less, preferably 90% or less. (Ratio of the amount of substance of Z element to phosphorus) The ratio of the amount of substance of Z element (Z) to the amount of phosphorus (P) contained in the coating layer, Z / P, preferably satisfies 0.5≦Z / P≦3.0. By setting Z / P within the above range, the effect of preventing both the interfacial reaction between the lithium metal composite oxide and the solid electrolyte and the interfacial mixing between the lithium metal composite oxide and the coating layer can be particularly enhanced. The amount of substance of phosphorus and the amount of substance of Z element in the above formula can also be measured and calculated using XPS. (Thickness of the coating layer) There is no need for a clear boundary between the coating layer and the lithium metal composite oxide particles. Therefore, the coating layer refers to a region or area on the surface side of the coated cathode active material of this embodiment where the concentrations of phosphorus and Z element are higher than those of the lithium metal composite oxide particles, i.e., the central region. The coating layer may partially form a solid solution with the lithium metal composite oxide.
[0034] The content of the coating layer is not particularly limited, but it is preferable to adjust the content, specifically the calculated thickness of the coating layer, depending on the specific surface area of the lithium metal composite oxide particles to be coated. Specifically, the thickness of the coating layer at the time of formation, calculated from the specific surface area of the lithium metal composite oxide particles forming the coating layer and the amount of coating layer-forming solution to be applied, is preferably 5 nm or more and 15 nm or less. By making the coating layer thickness 5 nm or more, the coverage rate can be easily made 60% or more, and the coating layer can be formed stably. Furthermore, by making the coating layer thickness 5 nm or more, the reaction between the lithium metal composite oxide and the solid electrolyte can be particularly suppressed.
[0035] Furthermore, by setting the thickness of the coating layer to 15 nm or less, it is possible to particularly suppress the influence on the movement of lithium ions between the lithium metal composite oxide and the solid electrolyte. <1-3. Other characteristics of the positive electrode active material for lithium ion secondary battery with coating layer> So far, the lithium metal composite oxide and the coating layer have been described, but it is preferable that the positive electrode active material with coating layer of this embodiment has the following characteristics.
[0036] The coating layer-attached positive electrode active material of this embodiment is preferably composed only of the above-described lithium metal composite oxide particles and the coating layer, but impurities may be mixed in during production. In particular, moisture is an impurity that may be mixed in when the coating layer is formed. Since moisture may cause hydrolysis and deterioration of the solid electrolyte and affect the initial discharge capacity, it is preferable that the moisture content be controlled within a predetermined range.
[0037] The coating layer-attached cathode active material of this embodiment preferably has a water content of 0.08% by mass or less, which can more reliably suppress the hydrolysis reaction of the solid electrolyte in a secondary battery using the coating layer-attached cathode active material.
[0038] As described above, it is preferable to set the moisture content of the coating layer-provided cathode active material of this embodiment to 0.08% by mass or less, because this more reliably suppresses the hydrolysis reaction of the solid electrolyte. The moisture content of the coating layer-provided cathode active material of this embodiment can be evaluated, for example, by the Karl Fischer method at a heating temperature of 300°C.
[0039] The lower limit of the water content of the coating layer-equipped cathode active material of this embodiment can be 0% by mass or more. 2. Method for producing coating layer-forming solution and coating layer-equipped cathode active material for lithium-ion secondary battery> (Method for producing coating layer-equipped cathode active material) An example of the coating layer-forming solution and method for producing coating layer-equipped cathode active material according to this embodiment will be described. According to the method for producing a coating layer-equipped cathode active material of this embodiment, the previously described coating layer-equipped cathode active material can be produced, so some of the details already described will be omitted. Note that the method for producing a coating layer-equipped cathode active material of this embodiment is just one example of a production method, and the previously described method for producing a coating layer-equipped cathode active material is not limited to the production method below.
[0040] The method for producing a coating layer-attached positive electrode active material of this embodiment can include a precursor formation step and a heat treatment step, which will be described below.
[0041] Each step will be described below: (Precursor Forming Step) In the precursor forming step, a solution for forming a coating layer is applied to the surface of particles of lithium metal composite oxide, followed by drying, to form a precursor.
[0042] The lithium metal composite oxide supplied to the precursor formation step is the same as the lithium metal composite oxide already described for the coating layer-attached positive electrode active material. That is, the lithium metal composite oxide has a layered rock salt structure and can contain lithium (Li), nickel (Ni), and an M element (M) in a ratio of Li:Ni:M = a:1-x:x in terms of the amount of substance. a and x satisfy the relationships 0.98≦a≦1.20 and 0≦x≦1.0, and the M element can be one or more elements excluding lithium, nickel, and oxygen. Since more preferred forms of the lithium metal composite oxide have already been described, further description will be omitted.
[0043] The coating layer-forming solution is a solution in which lithium, phosphorus, and a Z element are all dissolved, and the Z element is at least one pentavalent transition metal element. Since a preferred form of the Z element has already been described, a description thereof will be omitted. The coating layer-forming solution is a solution used to form the coating layer of the above-described coating layer-attached positive electrode active material.
[0044] The coating layer forming solution can be prepared, for example, by mixing a solution containing Li-Z-O and a solution containing Li-P-O while adjusting the pH. Alternatively, the coating layer forming solution may be prepared by adding and mixing components such as lithium, phosphorus, and compounds that serve as sources of Z element to a solvent such as water. The solvent used in the coating layer forming solution is not limited to water; for example, one or more solvents selected from water and alcohols such as ethanol can be used. The coating layer forming solution can be formed by adjusting the content ratio of each element so that the coating layer to be formed has the desired composition. The resulting solution is preferably a transparent, dissolved solution rather than a sol solution in which nanoparticles are dispersed. In other words, the resulting coating layer forming solution is preferably a solution in which lithium, phosphorus, and Z element are all dissolved.
[0045] The term "completely dissolved solution" means a solution in which the added components are dissolved and no precipitate is visually confirmed, and can be, for example, a transparent solution as described above.
[0046] Z / P, which is the ratio of the amount of substance of the Z element (Z) to the phosphorus (P) contained in the coating layer-forming solution, preferably satisfies, for example, 0<Z / P≦3.0, and more preferably satisfies 0.5≦Z / P≦3.0. By setting Z / P within the above range for the coating layer-forming solution, the ratio of the amount of substance of the Z element (Z) to the contained phosphorus (P) can be easily set within a predetermined range for the coating layer of the coating layer-formed positive electrode active material produced using the coating layer-forming solution.
[0047] In the precursor formation step, the coating layer forming solution can be applied to the lithium metal composite oxide particles and dried. The coating and drying device used here can be any method that can coat the lithium metal composite oxide particles thinly and uniformly, and a method in which the coating layer forming solution is sprayed while stirring and fluidizing the lithium metal composite oxide powder is preferred. An apparatus that is less susceptible to particle crushing or damage from impact during stirring and fluidization can be suitably used, such as a tumbling fluidizer. A tumbling fluidizer is also preferred because it can simultaneously dry the particles by heating them from the outside or adjusting the temperature of the gas (air, etc.) introduced into the apparatus. The drying temperature should be equal to or higher than the temperature at which the solvent in the coating layer forming solution evaporates. (Heat Treatment Step) In the heat treatment step, the precursor can be heat-treated.
[0048] The heat treatment step can be carried out on the precursor formed in the precursor formation step, in which the dried product of the coating layer forming solution is disposed on the surface of the lithium metal composite oxide particles, in order to completely evaporate the solvent.
[0049] The atmosphere for the heat treatment step may be an air atmosphere, but more preferably, air from which carbon dioxide has been removed or an oxygen atmosphere can be used. The heat treatment temperature is preferably 300°C or higher, at which the solvent reliably evaporates. Furthermore, if it is necessary to increase the crystallinity of the coating layer, it is preferable to perform the heat treatment at a temperature of 600°C or lower. By performing the heat treatment at 600°C or lower, it is possible to reliably prevent mixing of the lithium metal composite oxide and the coating layer. The heat treatment time depends on the thickness of the coating layer, but is preferably 1 hour or more and 10 hours or less. By performing the heat treatment for 1 hour or more, the solvent in the coating layer can be sufficiently reduced and removed. Furthermore, by setting the heat treatment time to 10 hours or less, productivity can be increased.
[0050] Therefore, in the heat treatment step, it is preferable to heat treat the precursor in dry air or an oxygen atmosphere at a heat treatment temperature of 300°C or higher and 600°C or lower for 1 hour or longer and 10 hours or shorter, and it is more preferable that the atmosphere is an oxygen atmosphere.
[0051] The coated cathode active material obtained after the heat treatment step can have a lithium metal composite oxide and a coating layer that coats at least a portion of the surface of the lithium metal composite oxide. The coating layer preferably has a coverage of 60% or more, as described for the coated cathode active material. The method for determining the coverage and the preferred range of the coverage have already been described, and therefore further explanation is omitted. 3. All-Solid-State Lithium-Ion Secondary Battery Next, an example configuration of the all-solid-state lithium-ion secondary battery of this embodiment will be described. For example, as shown in FIG. 2 , an all-solid-state lithium-ion secondary battery 20 of this embodiment can have a cathode 21, an anode 23, and a solid electrolyte layer 22, each of which includes the coated cathode active material. These components can be sealed within a container 24. The cathode 21 and the anode 23 can be provided with a cathode terminal 211 and an anode terminal 231, respectively, so that they can be connected to components outside the container 24.
[0052] Each component of the secondary battery of this embodiment will be described below. Note that the embodiment described below is merely illustrative, and the all-solid-state lithium-ion secondary battery of the present invention can be implemented in various forms with various modifications and improvements based on the knowledge of those skilled in the art based on the embodiments described herein. Furthermore, the all-solid-state lithium-ion secondary battery of this embodiment is not particularly limited in its use. <3-1. Positive Electrode> The positive electrode can be formed by molding a positive electrode mixture. Note that the positive electrode is processed appropriately according to the battery to be used. For example, pressure compression treatment using a press or the like can be performed to increase the electrode density.
[0053] The above-mentioned positive electrode mixture can be formed by mixing, for example, the above-mentioned powdered positive electrode active material with a coating layer and a solid electrolyte.
[0054] The solid electrolyte is added to the electrode to provide it with suitable ionic conductivity.
[0055] The material of the solid electrolyte is not particularly limited, but for example, Li 3 P.S. 4 , Li 7 P 3 S 11 , Li 10 GeP 2 S 12 Sulfide-based solid electrolytes such as Li 7 La 3 Zr 2 O 12 , Li 0.34 La 0.51 TiO 2.94 An oxide-based solid electrolyte such as SiO 2 or a polymer-based electrolyte such as PEO can be used.
[0056] A binder and a conductive agent (conductive assistant) may also be added to the positive electrode mixture.
[0057] The conductive agent is added to the electrode to provide it with appropriate conductivity. The material of the conductive agent is not particularly limited, but examples thereof include graphite such as natural graphite, artificial graphite, and expanded graphite, as well as acetylene black, Ketjen Black (registered trademark), carbon nanotubes, and fibrous graphite.
[0058] The binder serves to bind the positive electrode active material with the coating layer, but does not need to be added if not necessary. The binder used in the positive electrode mixture is not particularly limited, and may be one or more selected from, for example, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), fluororubber, ethylene propylene diene rubber, styrene-based thermoplastic elastomer, hydrogenated styrene-based thermoplastic elastomer, cellulose-based resin, polyacrylic acid, etc.
[0059] The mixing ratio of each material in the positive electrode mixture is not particularly limited. For example, the content of the coating layer-attached positive electrode active material in the positive electrode mixture can be 50 parts by mass or more and 90 parts by mass or less, and the content of the solid electrolyte can be 10 parts by mass or more and 50 parts by mass or less.
[0060] However, the method for producing the positive electrode is not limited to the above-mentioned examples, and other methods may be used. <3-2. Negative Electrode> The negative electrode can be formed by molding a metal (lithium metal, indium metal, lithium-indium alloy, lithium-aluminum alloy, Si or an alloy containing Si, etc.) or a negative electrode mixture.
[0061] Although the components constituting the negative electrode mixture and their blending are different, the negative electrode mixture can be formed in substantially the same manner as the positive electrode described above, and various treatments are carried out as necessary in the same manner as the positive electrode.
[0062] The negative electrode mixture can be prepared by mixing a negative electrode active material with a solid electrolyte. The negative electrode active material can be, for example, an occlusion material capable of occluding and desorbing lithium ions.
[0063] The storage material is not particularly limited, and may be one or more selected from, for example, natural graphite, artificial graphite, sintered organic compounds such as phenolic resin, and powdered carbon materials such as coke. When such a storage material is used as the negative electrode active material, a solid electrolyte containing Li, 3 P.S. 4<3-3. Solid Electrolyte Layer> As the solid electrolyte contained in the solid electrolyte layer, for example, an inorganic solid electrolyte can be used, and as the inorganic solid electrolyte, an oxide-based solid electrolyte, a sulfide-based solid electrolyte, etc. can be used.
[0064] The oxide-based solid electrolyte is not particularly limited, and any oxide-based solid electrolyte containing oxygen (O) and having lithium ion conductivity and electronic insulation can be used. Examples of the oxide-based solid electrolyte include lithium phosphate (Li 3 P.O. 4 ), Li 3 P.O. 4 N X , LiBO 2 N X , LiNbO 3 , LiTaO 3 , Li 2 SiO 3 , Li 4 SiO 4 -Li 3 P.O. 4 , Li 4 SiO 4 -Li 3 VO 4 , Li 2 Alumni 2 O 3 -P 2 O 5 , Li 2 O—SiO 2 , Li 2 Alumni 2 O 3 -ZnO, Li 1+X Al X Ti 2-X (P.O. 4 ) 3 (0≦X≦1), Li 1+X Al X Ge 2-X (P.O. 4 ) 3 (0≦X≦1), LiTi 2 (P.O. 4 ) 3 , Li 3X La 2/3-X TiO 3 (0≦X≦2 / 3), Li 5 La 3Ta 2 O 12 , Li 7 La 3 Zr 2 O 12 , Li 6 BaLa 2 Ta 2 O 12 , Li 3.6 Si 0.6 P 0.4 O 4 etc.
[0065] The sulfide-based solid electrolyte is not particularly limited, and any sulfide-based solid electrolyte containing sulfur (S) and having lithium ion conductivity and electronic insulation can be used. 2 S-P 2 S 5 , Li 2 S-SiS 2 , LiI-Li 2 S-SiS 2 , LiI-Li 2 S-P 2 S 5 , LiI-Li 2 S-B 2 S 3 , Li 3 P.O. 4 -Li 2 S-Si 2 S., Li. 3 P.O. 4 -Li 2 S-SiS 2 , LiPO 4 -Li 2 S-SiS, LiI-Li 2 S-P 2 O 5 , LiI-Li 3 P.O. 4 -P 2 S 5 , Li 6 P.S. 5 Cl, Li 6 P.S. 5 Br, Li 10 GeP 2 S 12 , Li 9.54 Si 1.74 P 1.44 S11.7 Cl 0.3 etc.
[0066] In addition, inorganic solid electrolytes other than those mentioned above may be used. For example, Li 3 N, LiI, Li 3 N-LiI-LiOH, etc. may also be used. <3-4. Shape and Structure of Secondary Battery> Next, an example of the arrangement and structure of the components of the secondary battery of this embodiment will be described.
[0067] The secondary battery of this embodiment, which has the positive electrode, negative electrode, and solid electrolyte layer described above, can be formed into various shapes, such as a coin shape or a stacked shape, as long as a certain pressure can be applied. Regardless of the shape, the positive electrode and negative electrode can be stacked with the solid electrolyte interposed therebetween, as described with reference to FIG. 2 . The positive electrode current collector and a positive electrode terminal connected to the outside, and the negative electrode current collector and a negative electrode terminal connected to the outside, can then be connected using current collecting leads or the like, and the battery can be sealed in a battery case to form a secondary battery.
[0068] The secondary battery of this embodiment using the above-described positive electrode active material with a coating layer can be an all-solid-state lithium ion secondary battery having a charge / discharge capacity equivalent to that of a lithium ion battery using an electrolyte solution. <3-5. Battery Evaluation of Secondary Battery> The secondary battery of this embodiment using the above-described positive electrode active material with a coating layer can be evaluated, for example, under the following conditions.
[0069] Specifically, the positive electrode active material with a coating layer of this embodiment was used for the positive electrode to form a test battery 30 shown in FIG. 3, and the current density was 0.5 mA / cm 2 As a result, the cutoff voltage is 4.8 V (vs. Li / Li + ) and after a 1-hour rest, the cut-off voltage is 3.0 V (vs. Li / Li + ) for 50 cycles, and the capacity retention rate is compared with that of a battery having no coating layer or a battery having a different coating layer, thereby enabling evaluation of effectiveness.
[0070] The use of the secondary battery of this embodiment is not particularly limited, and it can be suitably used for various applications requiring a power source. In addition, since the secondary battery of this embodiment has a charge / discharge capacity equivalent to that of a lithium-ion secondary battery using an electrolyte solution and can be miniaturized, it is also suitable as a power source for electric vehicles, which are limited in installation space.
[0071] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. [Example 1] (1) Physical Properties of Lithium Metal Composite Oxide Particles (1-1) Chemical Composition The chemical composition of the lithium metal composite oxide was confirmed to be Li:Ni:Co:Al=1.02:0.80:0.15:0.05, as determined by quantitative analysis using an ICP optical emission spectrometer (VARIAN, 725ES). (1-2) Crystal Structure The crystal structure of the lithium metal composite oxide was measured using XRD (PANALYTICAL, X'Pert, PROMRD), and was found to be a layered rock salt structure attributed to the R-3m structure. (1-3) Specific Surface Area The BET specific surface area of the lithium metal composite oxide was measured using a fully automatic BET specific surface area measuring device (Macsorb, manufactured by Mountec Co., Ltd.). The result was 0.58 m 2 (1-4) Volume Average Particle Diameter The volume average particle diameter of the lithium metal composite oxide was measured using a laser diffraction scattering particle size distribution measuring device (Microtrac HRA, manufactured by Nikkiso Co., Ltd.) and was found to be 5.8 μm.
[0072] (2) Production of a Positive Electrode Active Material with a Coating Layer (2-1) Preparation of a Solution for Forming a Coating Layer The solution for forming a coating layer was prepared by dissolving hydrogen peroxide, niobium hydroxide, ammonia water, lithium hydroxide, and LiH in ion-exchanged water. 2 P.O. 4 were added in order in a predetermined order and mixed to prepare an aqueous solution in which all of the components were dissolved. The resulting coating layer forming solution was mixed so that the molar ratio (Nb / P) of niobium (Nb) to phosphorus (P) contained therein was 1.0. The Nb / P value in the coating layer forming solution is shown in the "Nb / P in coating layer forming solution" column in Table 1.
[0073] (2-2) Formation of coating layer Li 1.02 Ni 0.80 Co 0.15 Al 0.05 O 2 The lithium metal composite oxide powder was subjected to the following precursor formation step and heat treatment step to produce a positive electrode active material with a coating layer.
[0074] (Precursor Formation Step) The total surface area (m 2 ) is the specific surface area (m 2 / g) relative to the total surface area. 3 The density of the crystal (2.46 g / cm 3 ), LiNbO 3 The density of the crystal (4.65 g / cm 3 ), and the amount of the coating layer-forming solution was calculated so that the target coating layer thickness would be 7 nm, and adjusted accordingly. The target coating layer thickness is shown in the "Coating Layer Thickness (Target Value)" column in Table 1. Next, 500 g of lithium metal composite oxide powder was weighed and fluidized in a tumbling fluidized granulation coating device (MP-01, manufactured by Powrex Corporation), and the coating layer-forming solution was sprayed into the fluidization tank. During this process, the temperature of the air supplied into the fluidization tank was controlled to 120°C, and a coating process was carried out slowly over a period of 4 hours to form a precursor.
[0075] (Heat Treatment Step) The precursor, which is the powder obtained in the precursor formation step, was recovered, and the precursor was subjected to heat treatment in an oxygen atmosphere at a heat treatment temperature of 300°C for 2 hours to produce a coated cathode active material having a coating layer containing Li, P, and Nb, from which the water solvent had been completely removed. Composition analysis of the cross section of the obtained coated cathode active material was performed using EDX, and it was confirmed that the coating layer was disposed on the surface of the lithium metal composite oxide. It was also confirmed that the other examples below had similar structures. (3) Evaluation of the coated cathode active material The following evaluations were performed on the coated cathode active material obtained in this manner.
[0076] (3-1) Surface Analysis The positive electrode active material with the coating layer was measured by XPS (Versa Probe II, manufactured by ULVAC-PHI). 3/2 Spectrum, Co=2p 3/2 spectrum, Al=2p spectrum, P=2p spectrum, Nb=3d 5/2 The amount of each element (at%) on the surface of the coated positive electrode active material was determined from the semi-quantitative values calculated from the area of each peak in the spectrum. The coverage, which is the ratio of the sum of the amounts of P and Nb present on the surface to the sum of the amounts of P, Nb, Ni, Co, and Al, was (P + Nb) / (P + Nb + Ni + Co + Al) × 100 = 86%. The evaluation results are shown in the "Coverage" column of Table 1.
[0077] The ratio of the amount of Nb to the amount of P was calculated to be 0.96 (Nb / P). The evaluation results are shown in the "Nb / P" column of Table 1.
[0078] (3-2) Moisture Content The moisture content of the coating layer-attached positive electrode active material was measured using a Karl Fischer moisture meter (manufactured by Kyoto Electronics Manufacturing Co., Ltd., model: MKC210) at a heating temperature of 300° C., and was found to be 0.045% by mass.
[0079] (4) Fabrication of Secondary Battery For battery evaluation of the positive electrode active material with a coating layer, an all-solid-state lithium ion secondary battery (hereinafter referred to as "test battery") having the structure shown in Fig. 3 was used. The test battery 30 was composed of a case and a powder compact cell 31 housed in the case.
[0080] The case has a hollow negative electrode can 32 with one end open, and a positive electrode can 33 that is placed in the opening of the negative electrode can 32. The case is configured so that when the positive electrode can 33 is placed in the opening of the negative electrode can 32, a space is formed between the positive electrode can 33 and the negative electrode can 32 to accommodate the powder compact cell 31. The positive electrode can 33 is fixed to the negative electrode can 32 with a thumbscrew 34 and a nut 35.
[0081] The negative electrode can 32 has a negative terminal, and the positive electrode can 33 has a positive terminal. The case is provided with an insulating sleeve 36, which fixes the negative electrode can 32 and the positive electrode can 33 so that they are kept out of contact with each other.
[0082] A pressure screw 37 is provided at the closed end of the negative electrode can 32, and after the positive electrode can 33 is fixed to the negative electrode can 32, the pressure screw 37 is tightened toward the compact cell storage space, thereby maintaining the compact cell 31 in a pressurized state through a hemispherical washer 38. A screw-type plug 39 is provided at the end of the negative electrode can 32 where the pressure screw 37 is located. O-rings 40 are provided between the negative electrode can 32 and the positive electrode can 33 and between the negative electrode can 32 and the plug 39, which seal the gap between the negative electrode can 32 and the positive electrode can 33 and maintain an airtight seal inside the case.
[0083] The compact cell 31 is a pellet made of a positive electrode layer, a solid electrolyte layer, and a negative electrode layer, stacked in this order. The compact cell 31 is housed in a case such that the positive electrode layer contacts the inner surface of the positive electrode can 33 through the lower current collector 41, and the negative electrode layer contacts the inner surface of the negative electrode can 32 through the upper current collector 42, washer 38, and pressure screw 37. The lower current collector 41, compact cell 31, and upper current collector 42 are protected by a sleeve 43 to prevent electrical contact between the positive electrode layer and the negative electrode layer.
[0084] Such a test battery 30 was fabricated as follows.
[0085] First, 60 mg of the coating layer-attached positive electrode active material and Li 3 P.S. 4 A positive electrode mixture was prepared by mixing 40 mg of a solid electrolyte (aluminum oxide) in a mortar. Next, a molding die capable of producing pellets with a diameter of 10 mm was prepared, and 60 mg of the solid electrolyte was placed in the mold and pressed at 10 MPa. Next, 15 mg of the positive electrode mixture was added, and the mixture was pressed at 360 MPa to obtain a two-layer pellet consisting of a firmly bonded positive electrode layer and a solid electrolyte layer.
[0086] The lower electrode, a pellet with the positive electrode layer facing downward, indium foil serving as the negative electrode layer, and the upper electrode were stacked in this order from the bottom up, and the electrodes were sealed in a case. The pressure screws 37 were then tightened with a torque of 6 to 7 N·m to apply a restraining force. The test battery 30 was fabricated in a glove box with an Ar atmosphere and a dew point controlled at -80°C. (5) Evaluation of the secondary battery The cycle characteristics of the test battery were evaluated under the following conditions.
[0087] A rest period of 1 hour was provided until the open circuit voltage (OCV) became approximately stable. After that, a constant current density of 0.5 mA / cm was applied. 2 The cutoff voltage is 4.8V (vs. Li / Li + After one hour of rest, the cut-off voltage was 3.0 V (vs. Li / Li + ) at a current density of 0.5 mA / cm 2 This operation from charge to discharge was defined as "one cycle," and 50 cycles were performed in total, and the capacity retention rate (%) was calculated by dividing the discharge capacity (mAh / g) at the 50th cycle by the discharge capacity (mAh / g) at the 2nd cycle.
[0088] The capacity of a battery varies depending on the battery materials, configuration, and measurement conditions. Therefore, the capacity retention rate is calculated based on the LiNbO 3 Table 1 shows the relative ratios when the capacity retention rate of the lithium metal composite oxide coating is set to 1. A relative ratio exceeding 1 means that the capacity retention rate is high, that is, deterioration is suppressed, and when applied to an all-solid-state lithium ion secondary battery using a solid electrolyte, it is possible to suppress a decrease in battery capacity when repeatedly charged and discharged. In Example 1, the capacity retention rate, which is a relative ratio, was 1.44. The evaluation results are shown in the column of "Capacity retention rate (relative ratio)" in Table 1.
[0089] [Example 2] In Example 2, Li was used as the lithium metal composite oxide. 1.1 Ni 0.38 Co 0.32 Mn 0.30 O 2 (Layered rock salt structure, specific surface area = 0.68 m 2 / g, volume average particle diameter=4.7 μm) was used. A positive electrode active material with a coating layer was produced under the same conditions as in Example 1 except for the above points, and was evaluated.
[0090] The coverage after the heat treatment was calculated by (P + Nb) / (P + Nb + Ni + Co + Mn) × 100. Mn in the above formula was determined by measuring the positive electrode active material with a coating layer by XPS, and was calculated as Mn = 2p 3/2The amount of Mn (at %) was determined from a semi-quantitative value calculated from the peak area of the spectrum.
[0091] After the heat treatment, the coverage was 88%, and the Nb / P ratio was 0.96. The capacity retention rate, which is a relative ratio in the battery evaluation, was 1.39.
[0092] [Example 3] When preparing a solution for forming a coating layer, the Nb / P ratio in the solution for forming a coating layer was set to 0.5. A positive electrode active material with a coating layer was prepared and evaluated under the same conditions as in Example 1 except for the above points. The coverage after heat treatment was 85%, and the Nb / P ratio was 0.52. The capacity retention rate, which is a relative ratio in battery evaluation, was 1.30.
[0093] [Example 4] When preparing a solution for forming a coating layer, the Nb / P ratio in the solution for forming a coating layer was set to 3.0. A positive electrode active material with a coating layer was prepared and evaluated under the same conditions as in Example 1 except for the above points. The coverage after heat treatment was 82%, and the Nb / P ratio was 2.9. The capacity retention rate, which is a relative ratio in battery evaluation, was 1.28.
[0094] [Example 5] In the precursor formation step, the amount of the coating layer forming solution was calculated so that the target coating layer thickness would be 5 nm, and adjusted accordingly. A positive electrode active material with a coating layer was produced and evaluated under the same conditions as in Example 1 except for the above points. The coverage after heat treatment was 68%, and Nb / P was 1.1. The capacity retention rate, which is a relative ratio in battery evaluation, was 1.32. [Example 6] For the coating layer forming solution, a niobium oxide-based inorganic coating solution "Bailar Nb-G6000" manufactured by Taki Chemical Co., Ltd. was added with lithium hydroxide and LiH dissolved in ion-exchanged water. 2 P.O. 4 The aqueous solutions were added sequentially in a predetermined order and mixed to prepare an aqueous solution in which all of the components were dissolved. The resulting coating layer forming solution was mixed so that the molar ratio of niobium (Nb) to phosphorus (P) contained therein (Nb / P) was 1.0.
[0095] A coating layer-attached positive electrode active material was produced and evaluated under the same conditions as in Example 1 except for the above points. The coverage after heat treatment was 88%, and Nb / P was 1.0. The capacity retention rate, which is a relative ratio in battery evaluation, was 1.36. [Example 7] A coating layer-forming solution was produced by mixing two solutions: a Li-Nb solution in which lithium ethoxide and niobium ethoxide were dissolved in ethanol, and a Li-P solution in which lithium ethoxide and triethyl phosphate were dissolved in ethanol.
[0096] The coating layer forming solution was mixed so that the substance ratios of Li:Nb and Li:P were 1:1 and 1:30, respectively, and triethyl phosphate was added in excess. That is, the resulting coating layer forming solution was mixed so that the substance ratio (Nb / P) of niobium (Nb) to phosphorus (P) contained therein was 1 / 30.
[0097] A coating layer-attached positive electrode active material was prepared and evaluated under the same conditions as in Example 1 except for the above points. After the heat treatment, the coating rate was 86%, and the Nb / P ratio was 0.95. The capacity retention rate, which is a relative ratio in battery evaluation, was 1.33.
[0098] [Comparative Example 1] A solution prepared by weighing out lithium ethoxide and niobium ethoxide so that the ratio of Li:Nb was 1:1 (amount of material) and dissolving them in ethanol was used as the coating layer forming solution. A positive electrode active material with a coating layer was prepared and evaluated under the same conditions as in Example 1, except for the above points. The coverage rate after heat treatment was 81%. The capacity retention rate, which is a relative ratio in battery evaluation, was set to the reference value of 1.00.
[0099] Comparative Example 2: A solution prepared by mixing a Li—Nb solution, which was a solution prepared by dissolving lithium ethoxide and niobium ethoxide in ethanol, with a Li—P solution, which was a solution prepared by dissolving lithium ethoxide and triethyl phosphate in ethanol, was used as the coating layer forming solution. When mixing the Li—Nb solution and the Li—P solution, the ratios of Li:Nb and Li:P were adjusted and mixed to a mass ratio of 1:1. A positive electrode active material with a coating layer was prepared and evaluated under the same conditions as in Example 1, except for the above points. The coverage after heat treatment was 32%, and the Nb / P ratio was 28. The capacity retention rate, which is a relative ratio in battery evaluation, was 1.02.
[0100] [Comparative Example 3] When preparing a solution for forming a coating layer, the Nb / P ratio in the solution for forming a coating layer was set to 0.3. A positive electrode active material with a coating layer was prepared under the same conditions as in Example 1 except for the above points, and was evaluated. After the heat treatment, the coverage was 83%, and the Nb / P ratio was 0.26. The capacity retention rate, which is a relative ratio in battery evaluation, was 0.94.
[0101] [Comparative Example 4] When preparing a solution for forming a coating layer, the Nb / P ratio in the solution for forming a coating layer was set to 3.6. A positive electrode active material with a coating layer was prepared and evaluated under the same conditions as in Example 1 except for the above points. The coverage after heat treatment was 80%, and the Nb / P ratio was 3.7. The capacity retention rate, which is a relative ratio in battery evaluation, was 1.05.
[0102] [Comparative Example 5] In the precursor formation step, the amount of the coating layer forming solution was calculated so that the target coating layer thickness would be 2.4 nm, and adjusted accordingly. A positive electrode active material with a coating layer was prepared and evaluated under the same conditions as in Example 1, except for the above points. The coverage after heat treatment was 53%, and the Nb / P ratio was 1.0. The capacity retention rate, which is a relative ratio in battery evaluation, was 1.10.
[0103] This application claims priority based on Japanese Patent Application No. 2023-059405 filed with the Japan Patent Office on March 31, 2023, and Japanese Patent Application No. 2023-093516 filed with the Japan Patent Office on June 6, 2023. The entire contents of Japanese Patent Application No. 2023-059405 and Japanese Patent Application No. 2023-093516 are incorporated by reference into this international application.
[0104] REFERENCE SIGNS LIST 10 Positive electrode active material for lithium ion secondary battery with coating layer 11 Lithium metal composite oxide 12 Coating layer 20 All-solid-state lithium ion secondary battery 21 Positive electrode 211 Positive electrode terminal 22 Solid electrolyte layer 23 Negative electrode 231 Negative electrode terminal 24 Container 30 Test battery 31 Compacted powder cell 32 Negative electrode can 33 Positive electrode can 34 Thumb screw 35 Nut 36 Insulating sleeve 37 Pressure screw 38 Washer 39 Plug 40 O-ring 41 Lower current collector 42 Upper current collector 43 Sleeve
Claims
1. A positive electrode active material for a lithium ion secondary battery with a coating layer, comprising: a lithium metal composite oxide; and a coating layer that covers at least a portion of the surface of the lithium metal composite oxide and has a coverage rate of 60% or more, the lithium metal composite oxide has a layered rock salt structure and contains lithium (Li), nickel (Ni), and an M element (M) in a substance amount ratio of Li:Ni:M=a:1-x:x, where a and x satisfy the relationships 0.98≦a≦1.20 and 0≦x≦1.0, and the M element is one or more elements excluding lithium, nickel, and oxygen, and the coating layer contains lithium, phosphorus, and a Z element, and the Z element is at least one pentavalent transition metal element.
2. The positive electrode active material for a lithium ion secondary battery with a coating layer according to claim 1, wherein the M element is at least one selected from the group consisting of Al, Ti, V, Mn, Fe, Co, Cu, Zr, Nb, Mo, Ta and W.
3. The positive electrode active material for a lithium ion secondary battery with a coating layer according to claim 1 or 2, wherein Z / P, which is the ratio of the amount of substance of the Z element (Z) to phosphorus (P) contained in the coating layer, satisfies 0.5≦Z / P≦3.
0.
4. The positive electrode active material for a lithium ion secondary battery with a coating layer according to claim 1 or 2, wherein the Z element is niobium.
5. A coating layer forming solution used to form the coating layer of the positive electrode active material for a lithium ion secondary battery with a coating layer according to claim 1 or 2, the coating layer forming solution being a solution in which lithium, phosphorus and the Z element are all dissolved.
6. A method for producing a positive electrode active material for a lithium ion secondary battery with a coating layer, comprising: a precursor formation step of applying a coating layer forming solution to the surface of a lithium metal composite oxide particle, drying the solution to form a precursor; and a heat treatment step of heat treating the precursor, wherein the lithium metal composite oxide has a layered rock salt structure and contains lithium (Li), nickel (Ni), and an M element (M) in a substance amount ratio of Li:Ni:M=a:1-x:x, where a and x satisfy the relationships 0.98≦a≦1.20 and 0≦x≦1.0, and the M element is one or more elements excluding lithium, nickel, and oxygen, the coating layer forming solution is a solution in which lithium, phosphorus, and a Z element are all dissolved, and the Z element is at least one pentavalent transition metal element.
7. A method for producing a positive electrode active material for a lithium ion secondary battery with a coating layer as described in claim 6, wherein in the heat treatment step, the precursor is heat treated in an oxygen atmosphere at a heat treatment temperature of 300°C or more and 600°C or less for 1 hour or more and 10 hours or less.
8. An all-solid-state lithium ion secondary battery having a positive electrode, a negative electrode, and a solid electrolyte layer, wherein the positive electrode contains the positive electrode active material for a lithium ion secondary battery with a coating layer according to claim 1 or 2.
Citation Information
Patent Citations
Sulfide solid electrolyte
JP2014056661A
UV-reflective composition and method for producing the same
JP2023059405A
Transport of sampled signals on multiple electromagnetic paths
JP2023093516A
Lithium titanium niobium phosphate coated ternary positive electrode material and preparation method thereof
CN116504978A
Positive electrode composite material and sulfide all-solid battery arranged by use thereof
JP2016039062A