Method for producing recycled polybutylene terephthalate and method for producing polybutylene terephthalate composite material
The method of dissolving PBT composite materials in a phenolic solvent and precipitating with an insoluble solvent addresses the challenges of recycling PBT composite materials by maintaining mechanical properties and reducing environmental impact, enabling the production of high-quality recycled PBT for composite materials.
Patent Information
- Application Number
- PCT/JP2024/013205
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-11-30
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-03
AI Technical Summary
Current recycling methods for polybutylene terephthalate (PBT) composite materials face challenges in removing impurities and maintaining mechanical strength due to the difficulty in separating PBT from composite materials containing various fillers and resins, leading to decreased molecular weight and strength upon repeated recycling.
A method involving dissolving PBT composite materials in a phenolic solvent to remove insoluble matter, followed by precipitation using an insoluble solvent, allowing for the recovery of recycled PBT without chemical decomposition and thermal energy, thereby maintaining mechanical properties.
This method enables the production of recycled PBT with acceptable quality and properties, suitable for practical use without environmental impact, and allows for the manufacturing of PBT composite materials using the obtained recycled PBT.
Smart Images

Figure JPOXMLDOC01-APPB-M000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Method for producing recycled polybutylene terephthalate and method for producing polybutylene terephthalate composite material
[0001] The present invention relates to a method for producing recycled polybutylene terephthalate and a method for producing a polybutylene terephthalate composite material.
[0002] Polybutylene terephthalate (hereinafter sometimes referred to as "PBT") has excellent mechanical properties, heat resistance, chemical resistance, and electrical properties, and is also easily colorable, easy to mold, and inexpensive. As a result, it is used as a material in the electrical and electronic fields, automotive fields, and high-performance films, and demand for it is growing.
[0003] On the other hand, in recent years, the use of plastics has been shunned from the perspective of environmental protection, and there is an urgent need to establish recycling technologies, but the recycling of PBT has not progressed. This is because, rather than using PBT alone, it is often compounded with glass fiber, which dramatically improves strength and heat resistance when combined with various fillers, or with AS resin, ABS resin, PS resin, PC resin, PET resin, etc., to form polybutylene terephthalate composite materials (PBT composite materials) in order to improve warpage, dimensional accuracy, paintability, and impact resistance.
[0004] Japanese Patent Application Laid-Open No. 2023-75033
[0005] When attempting to recycle PBT composite materials, it is difficult to remove various fillers, additives, and other resins from the PBT composite material, making it difficult to obtain pure recycled PBT without impurities. Furthermore, re-kneading the PBT obtained through material recycling can result in cracking of the mixed fillers, potentially reducing strength. Furthermore, repeated recycling can also lead to a decrease in the molecular weight of the PBT, resulting in a decrease in mechanical strength.
[0006] Chemical recycling has also been proposed as a method for recycling PBT (Patent Document 1). While this recycling method is well-established, this document focuses on PBT alone, such as process waste, and does not mention PBT composite materials containing other resins. Furthermore, chemical recycling involves many processes and requires a large amount of thermal energy for depolymerization, which breaks down the material down to the monomer, and for repolymerization, which poses challenges such as a heavy environmental burden and high production costs. Therefore, it is currently believed that obtaining recycled PBT from PBT composite materials through chemical recycling is difficult.
[0007] Under these circumstances, there is a demand for recovering only PBT from PBT composite materials containing PBT. The present invention has been made in consideration of the above circumstances, and aims to provide a method for producing recycled PBT that can produce recycled PBT of practically acceptable quality using a method with little environmental impact, without requiring the extensive steps of depolymerization and repolymerization or thermal energy required in chemical recycling. Another aim is to provide a method for producing a PBT composite material using the recycled PBT obtained.
[0008] As a result of intensive research into solving the above-mentioned problems, the present inventors have discovered that by dissolving PBT in a solvent (solvent (S)) containing a phenolic solvent, removing impurities such as fibers, resins, and metal impurities other than PBT by filtration, and then contacting the solution with a solvent (solvent (P)) in which PBT is insoluble to precipitate PBT, it is possible to recover recycled PBT of a quality that is acceptable for practical use without decomposing it down to the monomer, and have thus completed the invention of the following method for producing recycled PBT.
[0009] That is, the present invention relates to the following inventions. <1> A method for producing recycled polybutylene terephthalate from a polybutylene terephthalate composite material, comprising the following steps (A) to (D): step (A): dissolving a polybutylene terephthalate composite material in a solvent (S) containing a phenolic solvent to obtain a solution in which polybutylene terephthalate is dissolved; step (B): removing insoluble matter from the solution in which polybutylene terephthalate is dissolved to obtain a liquid component (L) in which polybutylene terephthalate is dissolved; step (C): mixing the liquid component (L) with a solvent (P) that can precipitate polybutylene terephthalate when mixed with the liquid component (L), thereby precipitating polybutylene terephthalate to obtain a slurry, and then subjecting the slurry to solid-liquid separation to obtain solid polybutylene terephthalate; and step (D): drying the solid polybutylene terephthalate to obtain recycled polybutylene terephthalate. <2> A method for producing recycled polybutylene terephthalate according to <1>, comprising, before step (B), a step (X1) of contacting the solution in which the polybutylene terephthalate has been dissolved with a flocculant. <3> A method for producing recycled polybutylene terephthalate according to <1> or <2>, comprising, before step (B), a step (X2) of contacting the solution in which the polybutylene terephthalate has been dissolved with a filter aid. <4> A method for producing recycled polybutylene terephthalate according to any one of <1> to <3>, wherein the temperature of the solvent (S) in step (A) is 45°C or higher and 150°C or lower. <5> A method for producing recycled polybutylene terephthalate according to any one of <1> to <4>, wherein, in step (C), the slurry is obtained at a temperature of 0°C or higher and 80°C or lower. <6> The method for producing recycled polybutylene terephthalate according to any one of <1> to <5>, wherein the solvent (P) in the step (C) is one or more selected from the group consisting of aromatic hydrocarbon solvents, aliphatic hydrocarbon solvents, ketone solvents, aldehyde solvents, alcohol solvents, ether solvents, and water.<7> The method for producing recycled polybutylene terephthalate according to <6>, wherein the solvent (P) in step (C) is one or more selected from the group consisting of acetone, toluene, methanol, ethanol, isopropyl alcohol, and water. <8> The method for producing recycled polybutylene terephthalate according to <2>, wherein the flocculant in step (X1) is one or more selected from the group consisting of inorganic salts other than alkali metals and alkaline earth metals and polymer compounds. <9> The method for producing recycled polybutylene terephthalate according to <2>, wherein the flocculant in step (X1) is an inorganic salt other than alkali metals and alkaline earth metals. <10> The method for producing recycled polybutylene terephthalate according to <8> or <9>, wherein the inorganic salt other than alkali metals and alkaline earth metals is one or more selected from the group consisting of iron(III) chloride, iron(II) sulfate, iron(III) sulfate, aluminum sulfate, and aluminum chloride. <11> The method for producing recycled polybutylene terephthalate according to <8>, wherein a solution containing dissolved polybutylene terephthalate is contacted with the flocculant composed of an inorganic salt other than the alkali metal and alkaline earth metal, and then contacted with the flocculant composed of the polymer compound. <12> The method for producing recycled polybutylene terephthalate according to <8>, wherein the polymer compound is one or more selected from the group consisting of polyacrylamide and polyethylene oxide. <13> The method for producing recycled polybutylene terephthalate according to <3>, wherein the filter aid in step (X2) is one or more selected from the group consisting of activated carbon, activated clay, celite, silica gel, synthetic adsorbents, bentonite, alumina, and zeolite. <14> The method for producing recycled polybutylene terephthalate according to any one of <1> to <13>, wherein the solvent (S) contains an aromatic hydrocarbon solvent and / or an aliphatic hydrocarbon solvent. <15> The method for producing recycled polybutylene terephthalate according to <14>, wherein the total content of the aromatic hydrocarbon solvent and the aliphatic hydrocarbon solvent in the solvent (S) is 20 mass% or more.<16> The method for producing recycled polybutylene terephthalate according to any one of <1> to <15>, wherein the polybutylene terephthalate content in the polybutylene terephthalate composite is 10% by mass or more. <17> The method for producing recycled polybutylene terephthalate according to any one of <1> to <16>, wherein the polybutylene terephthalate composite contains other components besides polybutylene terephthalate, and the other components include one or more selected from the group consisting of inorganic compounds, organic low-molecular-weight compounds, fibers other than polybutylene terephthalate, and resins other than polybutylene terephthalate. <18> The method for producing recycled polybutylene terephthalate according to any one of <1> to <17>, wherein the polybutylene terephthalate composite is an injection-molded article containing polybutylene terephthalate. <19> The method for producing recycled polybutylene terephthalate according to any one of <1> to <18>, wherein the recycled polybutylene terephthalate has an intrinsic viscosity of 0.6 dL / g or more and 1.5 dL / g or less. <20> Material recycled polybutylene terephthalate having an intrinsic viscosity of 0.6 dL / g or more and 1.5 dL / g or less. <21> A method for producing a polybutylene terephthalate composite material, comprising: a step of producing recycled polybutylene terephthalate by the method for producing recycled polybutylene terephthalate according to any one of <1> to <19>, and a step of producing a polybutylene terephthalate composite material using the recycled polybutylene terephthalate obtained.
[0010] The present invention provides a method for producing recycled PBT that can produce recycled PBT of practically acceptable quality using an environmentally friendly method without chemical decomposition, without requiring a large number of steps or thermal energy, and also provides a method for producing a PBT composite material using the recycled PBT obtained.
[0011] The following describes in detail an embodiment of the present invention, but the following description of the constituent elements is one example (typical example) of an embodiment of the present invention, and the present invention is not limited to the following content unless the gist of the present invention is changed. Note that when the expression "~" is used in this specification, it is used as an expression including the numerical values or physical property values before and after it.
[0012] <Method for producing recycled polybutylene terephthalate (PBT)> The present invention is a method for producing recycled PBT from a PBT composite material, comprising the following steps (A) to (D): step (A): dissolving a PBT composite material in a solvent (S) containing a phenolic solvent to obtain a solution in which PBT is dissolved (hereinafter, may be referred to as a "PBT solution"); step (B): removing insoluble matter from the solution in which PBT is dissolved to obtain a liquid component (L) in which PBT is dissolved; step (C): mixing the liquid component (L) with a solvent (P) that can precipitate polybutylene terephthalate when mixed with the liquid component (L), precipitating PBT to obtain a slurry, and then subjecting the slurry to solid-liquid separation to obtain solid PBT; step (D): drying the solid PBT to obtain recycled PBT. The present invention relates to a method for producing recycled polybutylene terephthalate (hereinafter, sometimes referred to as "a method for producing recycled PBT of the present invention"), which includes the steps of:
[0013] The method for producing recycled PBT of the present invention produces recycled PBT by material recycling. That is, in the method for producing recycled PBT of the present invention, the PBT composite material is not chemically decomposed, but resins other than PBT, fillers, and additives are removed, and then the PBT is regenerated again as PBT.
[0014] One feature of the method for producing recycled PBT of the present invention is that in step (A), a solvent (S) containing a phenolic solvent is selected as the solvent for dissolving PBT, PBT is dissolved in this solvent (S) to obtain a PBT solution, and then in step (B), insoluble matters such as resins other than PBT, fillers, and additives are removed. Finally, in step (C), the PBT is reprecipitated to obtain a PBT precipitate. The inventors have found that by using a solvent (S) containing a phenolic solvent, PBT in a PBT composite material can be dissolved under mild conditions, while resins other than PBT, fillers, additives, and the like are not dissolved, thereby allowing the removal of most of the components other than PBT. This method makes it possible to obtain recycled PBT that is practically acceptable even when the PBT composite material is used as a recycled raw material.
[0015] Each step will be described below.
[0016] [Step (A)] Step (A) is a step of dissolving a PBT composite material in a solvent (S) containing a phenolic solvent to obtain a solution in which PBT is dissolved (PBT solution).
[0017] <PBT Composite Material> The PBT composite material used in the present invention is a material containing PBT and components other than PBT, and is a post-consumer material and / or pre-consumer material of a PBT resin composition. Post-consumer materials are generally used PBT resin compositions after they have been incorporated into products as molded articles or used by consumers as exterior materials indoors or outdoors. Specific examples include automobile parts, aircraft parts, electrical and electronic components, and household appliances. Pre-consumer materials also include purged resins generated during polymerization or compounding, as well as PBT resins and compositions thereof that do not meet the quality standards for finished products.
[0018] Products containing PBT are manufactured by, for example, injection molding, and injection-molded articles containing PBT can be used as PBT composite materials.
[0019] (Components other than PBT) Components other than PBT contained in the PBT composite material are impurities that are removed in any step of the method for producing recycled PBT of the present invention.
[0020] The other components other than PBT include compounds used as additives in various products and resins other than PBT. For example, a PBT composite material can be a composite material containing PBT and one or more other components selected from the group consisting of low-molecular-weight organic compounds, inorganic compounds, fibers other than PBT, and resins other than PBT. The method for producing recycled PBT of the present invention allows for the removal of other components, resulting in PBT from which the other components have been removed. Examples of low-molecular-weight organic compounds include compounds used as colorants, antistatic agents, flame retardants, surfactants, antioxidants, and light stabilizers, and typically have a molecular weight of 2000 or less. Examples of inorganic compounds include glass beads, mica, talc, calcium carbonate, titanium oxide, and carbon black, which are added to prevent warpage or as colorants. Examples of fibers other than PBT include glass fiber and carbon fiber, which are added to improve the strength, thermal conductivity, linear expansion coefficient, and electrical properties of PBT. Examples of resins other than PBT include ABS resin, AS resin, polystyrene resin (PS), polyphenylene oxide (PPO), polycarbonate (PC), and polyethylene terephthalate (PET).
[0021] The content of PBT in the PBT composite material is not particularly limited, but a material containing 10 mass % or more of PBT in the PBT composite material is preferred, a material containing 30 mass % or more is more preferred, and a material containing 50 mass % or more is even more preferred. Furthermore, as the PBT composite material, one type of material or two or more types of materials may be used.
[0022] The method for producing recycled PBT of the present invention can efficiently remove resins other than PBT contained in PBT composite materials, so it is more effective to apply the method for producing recycled PBT of the present invention to materials containing other resins.
[0023] The PBT composite material used in step (A) may be used in the form of a resin composition as a post-consumer material or a pre-consumer material, or may be divided into appropriate sizes by cutting, crushing, pulverization, or the like. The division method, such as cutting, crushing, or pulverization, is not particularly limited, and may include cutting using a cutting tool; fusion cutting using gas, plasma, laser, or the like; splitting; shredding using a shredder; coarse crushing using a jaw crusher or a rotary crusher to crush to 20 cm or less; medium crushing using a rotary crusher, cone crusher, or mill to crush to 1 cm or less; and pulverization using a mill to crush to 1 mm or less. These methods may be used alone or in combination.
[0024] If the PBT composite material is too large, the dissolution time will be undesirably long. Therefore, it is preferable to use the pulverized PBT composite material obtained by pulverizing the PBT composite material as a raw material. The pulverized PBT composite material preferably has a size of 50 mm or less, more preferably 30 mm or less, and even more preferably 10 mm or less. On the other hand, if the size is too small, there is a risk of it becoming airborne as dust when fed into the equipment, so a size of 3 mm or more is preferable, and 5 mm or more is more preferable. Note that "50 mm or less" means passing through a sieve with a nominal mesh size of 50 mm as specified in JIS-Z-8801-1 (2019), "30 mm or less" means passing through a sieve with a nominal mesh size of 30 mm, and "10 mm or less" means passing through a sieve with a nominal mesh size of 10 mm. Furthermore, "3 mm or more" means not passing through a sieve with a nominal mesh size of 3 mm, and "5 mm or more" means not passing through a sieve with a nominal mesh size of 5 mm.
[0025] (Solvent (S)) The solvent (S) used to dissolve the PBT composite material in step (A) is not particularly limited as long as it can dissolve PBT and includes a phenolic solvent. Examples of phenolic solvents include phenol, cresol, xylenol, ethylphenol, propylphenol, butylphenol, methoxyphenol, ethoxyphenol, propoxyphenol, butoxyphenol, benzylphenol, phenylphenol, chlorophenol, dichlorophenol, and chloromethylphenol. One or more of these solvents may be selected. The ratio of the phenolic solvent in the solvent (S) may be any ratio as long as it dissolves PBT. However, it is preferable that the total amount of the phenolic solvents contained in the solvent (S) is 30% by mass or more, more preferably 35% by mass or more, and even more preferably 40% by mass or more.
[0026] The solvent (S) may contain a solvent other than a phenol-based solvent, and specific examples thereof include aromatic hydrocarbon solvents such as toluene and xylene, aliphatic hydrocarbon solvents such as hexane, heptane, hexene, and cyclohexane, tetrahydrofuran (THF), acetonitrile, dimethyl carbonate, hexafluoroisopropyl alcohol, water, etc. The solvent (S) can be used in appropriate combination of these solvents so that PBT dissolves at the dissolution temperature.
[0027] Among these, the solvent (S) preferably contains an aromatic hydrocarbon solvent and / or an aliphatic hydrocarbon solvent. The total content of the aromatic hydrocarbon solvent and the aliphatic hydrocarbon solvent in the solvent (S) is preferably 20% by mass or more, more preferably 30% by mass or more. By including a total of 20% by mass or more of the aromatic hydrocarbon solvent and the aliphatic hydrocarbon solvent in the solvent (S), it is possible to reduce the amount of the phenolic solvent remaining in the resulting recycled PBT. If a large amount of the phenolic solvent remains in the recycled PBT, the phenolic solvent is oxidized by heat during the drying process, producing colored components. As a result, the crystals become yellowish, and molded products using the phenolic solvent also become yellowish. Furthermore, the phenolic solvent may evaporate during molding, causing molding defects.
[0028] The amount of solvent (S) is preferably 200% by mass or more, more preferably 300% by mass or more, and even more preferably 500% by mass or more, relative to the mass of the PBT composite material. If the ratio of solvent (S) is low, the viscosity of the solution becomes extremely high, making stirring and dissolution difficult, and the filtration rate during filtration may decrease or the filtrate may adhere to the filter medium, resulting in a decrease in yield. Furthermore, the amount of solvent (S) is preferably 5000% by mass or less, more preferably 4000% by mass or less, and even more preferably 3000% by mass or less, relative to the mass of the PBT composite material. If the ratio of solvent (S) is high, the solubility of PBT increases, and even when solvent (P) is added in step (C), a large amount of PBT remains dissolved and does not precipitate, which may result in a decrease in yield. For example, the amount of the solvent (S) can be 200% by mass to 5000% by mass, 300% by mass to 4000% by mass, or 500% by mass to 3000% by mass relative to the mass of the PBT composite material.
[0029] (Dissolution Temperature) When dissolving the PBT composite material in the solvent (S), it is preferable to control the temperature (the temperature of the solution in the dissolution tank). If the temperature is not controlled, the dissolution time will be uneven, and undissolved components may be generated when the solution is sent to the next process. The temperature is preferably equal to or lower than the boiling point of the solvent (S). If the temperature is higher than the boiling point of the solvent (S), a condenser will be required in the dissolution tank, complicating the process. A specific temperature of the solvent (S) (the temperature of the solution in the dissolution tank) is preferably 45°C or higher, more preferably 50°C or higher, and even more preferably 55°C or higher. If the temperature is too low, the solubility of PBT will decrease, and dissolution will take a long time. Furthermore, when the solution is sent to the next process, it may take a long time to send the solution, or a large load may be placed on the filtration. The upper limit is preferably 150°C or lower, more preferably 140°C or lower, more preferably 130°C or lower, and even more preferably 120°C or lower. If the temperature is too high, there is a risk of PBT being thermally deteriorated. For example, the dissolution temperature can be 45°C to 150°C, 45°C to 150°C, 50°C to 130°C, or 55°C to 120°C.
[0030] (Dissolution Time) The dissolution time is preferably 20 minutes or more, more preferably 40 minutes or more, and even more preferably 1 hour or more. Also, it is preferably 5 hours or less, more preferably 4 hours or less, and even more preferably 3 hours or less. If the dissolution time is too short, the amount of undissolved material will increase, which may result in a decrease in yield or blockage in the process. If the dissolution time is too long, it may cause decomposition or discoloration of the polymer. For example, the dissolution time may be 20 minutes to 5 hours, 40 minutes to 4 hours, or 1 hour to 3 hours.
[0031] Alternatively, as long as PBT does not precipitate, a PBT solution may be prepared by dissolving PBT in solvent (S) and then mixing with additional solvents. To improve the filterability of the PBT solution, a solvent other than a phenol-based solvent may be mixed after dissolving PBT. For example, PBT may be dissolved in a phenol-based solvent and then mixed with a solvent other than a phenol-based solvent, such as an aromatic hydrocarbon solvent. The amount of solvent added after dissolving PBT is sufficient as long as it does not cause PBT to precipitate, and is preferably 10% by mass or more, more preferably 20% by mass or more, relative to the mass of the PBT composite material. However, depending on the type of solvent added, if the amount of solvent added is too large, PBT may precipitate. Therefore, the amount of solvent added is preferably 2000% by mass or less, more preferably 1500% by mass or less, relative to the mass of the PBT composite material. For example, the amount of the added solvent can be 10% by mass to 2000% by mass, or 20% by mass to 1500% by mass, based on the mass of the PBT composite material.
[0032] [Step (X)] Some PBT composite materials are colored with pigments such as carbon black. While colorant removal is not essential for materials used inside equipment and not visible to the user, when recycled PBT is used in the manufacture of products where design is important, removing colorants is preferable for the production of recycled products. However, it is difficult to sufficiently remove colorants simply by performing steps (A) to (D). This is because the particle size of coloring components such as pigments is small, making it difficult to capture impurities by filtration or other methods in step (B). Therefore, to improve the removal efficiency of colorants such as pigments, it is preferable to perform step (X) before step (B), in which the PBT solution is contacted with a flocculant and / or filter aid. Prior to step (B), the PBT solution is contacted with a filter aid and / or flocculant to adsorb or aggregate coloring components such as pigments, making them more easily captured by filtration or other methods.
[0033] Step (X) is a step of carrying out at least one of step (X1) of contacting the PBT solution with a flocculant before step (B) and step (X2) of contacting the PBT solution with a filter aid before step (B), and it is preferable to carry out step (X1) and step (X2).
[0034] The method for contacting the PBT solution with the flocculant and / or filter aid is not particularly limited as long as the flocculant and / or filter aid contacts the PBT solution, but examples include a method in which the PBT solution is prepared in step (A) and then the filter aid and / or flocculant is added and mixed into a reactor containing the PBT solution, a method in which the filter aid is packed into a column and the PBT solution is passed through it, and a method in which the filter aid and / or flocculant is added and mixed during the preparation of the PBT solution in step (A). These methods may also be combined.
[0035] Examples of filter aids include activated carbon, activated clay, bentonite, celite, alumina, silica gel, zeolite, and synthetic adsorbents. If the amount of filter aid added when mixing in a reactor is small, adsorption of pigments and the like does not proceed sufficiently. Therefore, it is preferable to add 5% by mass or more of the filter aid relative to the mass of the PBT composite material, more preferably 15% by mass or more, and even more preferably 25% by mass or more. If the amount added is small, adsorption does not proceed sufficiently. On the other hand, if the amount of filter aid added is large, for example, when filtering in step (B), the filter aid may leak through the mesh. Therefore, the amount of filter aid added relative to the mass of the PBT composite material is preferably 500% by mass or less, more preferably 250% by mass or less. For example, the amount of filter aid relative to the PBT composite material can be 5% by mass to 500% by mass, 15% by mass to 500% by mass, or 25% by mass to 250% by mass.
[0036] When using a flocculant, the lower limit of the amount added is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, relative to the mass of the PBT composite material, because a small amount is sufficient to achieve the desired effect. On the other hand, if too much flocculant is added, impurities derived from the flocculant may remain in the PBT solution, potentially deteriorating the color tone and mechanical strength of the final recycled PBT. Therefore, the amount of flocculant added is preferably 20% by mass or less, more preferably 10% by mass or less, relative to the mass of the PBT composite material. For example, the amount of flocculant relative to the PBT composite material can be 0.1% by mass to 20% by mass or 0.5% by mass to 10% by mass.
[0037] The flocculant neutralizes the charge of impurities, such as pigments, dispersed in the PBT solution, promoting adsorption and aggregation of the impurities and increasing the particle size to a size that can be captured in step (B). Usable flocculants include one or more selected from the group consisting of inorganic salts other than alkali metal salts and alkaline earth metal salts that decompose PBT, and polymer compounds. For example, inorganic salts other than alkali metal salts and alkaline earth metal salts include iron (III) chloride, iron (II) sulfate, iron (III) sulfate, aluminum chloride, aluminum sulfate, titanium oxide, copper (I) sulfate, copper (II) sulfate, copper (I) chloride, copper (II) chloride, and zinc sulfate. One or more selected from the group consisting of iron (III) chloride, iron (II) sulfate, iron (III) sulfate, aluminum sulfate, and aluminum chloride are preferred. Alternatively, a mixture of commercially available inorganic salts may be used as the flocculant. In particular, when promoting adsorption and aggregation of pigments, such as carbon black, with small particle sizes, using inorganic salts with relatively similar molecular sizes is more likely to promote adsorption and aggregation.
[0038] Inorganic salts can neutralize electric charges, but if the particle size of the aggregated particles is small, it is advisable to add a polymer compound such as an anionic polymer compound, a cationic polymer compound, or a nonionic polymer compound. That is, it is preferable to contact the PBT solution with a flocculant consisting of an inorganic salt other than an alkali metal salt or an alkaline earth metal salt, and then with a flocculant consisting of a polymer compound. The particles dispersed in the PBT solution adhere to the polymer chains, allowing for an increase in particle size. For these reasons, when removing impurities with relatively small particle sizes, such as pigments, adding an inorganic salt first and then a polymer flocculant can effectively increase the particle size to a size that can be captured in step (B). Typical examples of polymer compounds include polyacrylamide and polyethylene oxide.
[0039] As described above, it is preferable to use a filter aid and a flocculant in combination. When used in combination, the filter aid may be treated first with a flocculant, or the flocculant may be treated first with a filter aid, or the filter aid and the flocculant may be used simultaneously. In addition, the contact method between the PBT solution and the filter aid and the contact method between the PBT solution and the flocculant may be different methods.
[0040] If the contact time is too short, adsorption and coagulation do not proceed sufficiently, so it is preferably 20 minutes or more, more preferably 30 minutes or more. On the other hand, if it is too long, impurities will be eluted from the added filter aid and coagulant, so it is preferably 180 minutes or less, more preferably 120 minutes or less. For example, the contact time can be 20 to 180 minutes or 30 to 120 minutes.
[0041] [Step (B)] Step (B) is a step of removing insoluble matter from the PBT solution to obtain a liquid component (L) in which PBT is dissolved. By filtering the PBT solution obtained in step (A) or step (X), much of the insoluble matter in the PBT solution can be removed. This impurity removal does not necessarily require complete removal of the insoluble matter, as long as it is within a range that does not cause problems in the use of the resulting recycled PBT. For example, as described above, when the recycled PBT is intended to be used as an internal component of an apparatus, coloration of the resulting recycled PBT is acceptable. Therefore, if the PBT solution contains a colorant, it is not a problem if the colorant cannot be completely removed, and some colorant may remain.
[0042] The method for removing insoluble matter from a PBT solution may be any of filter paper, centrifugation, cyclone filtration, glass filters, bag filters, candle filters, etc., or a combination of these. Furthermore, multiple stages of filtering and multiple methods may be used. The smallest mesh size of the filter medium is preferably 10 μm or less, more preferably 5 μm or less, and even more preferably 1 μm or less. If the mesh size is too large, removal of foreign matter tends to be insufficient, while if it is too small, filterability tends to be poor. Furthermore, the temperature during filtration is preferably in the range of 10°C to 120°C. If the temperature is too low, the viscosity of the solution increases, placing a heavy load on the filtration, and if the temperature is too high, there is a risk of PBT deterioration.
[0043] [Step (C)] Step (C) is a step of mixing a liquid component (L) with a solvent (P) that can precipitate polybutylene terephthalate when mixed with the liquid component (L), precipitating PBT to obtain a slurry, and then subjecting the slurry to solid-liquid separation to obtain solid PBT.
[0044] (Solvent (P)) The solvent (P) that can be used to precipitate PBT is not particularly limited as long as it can precipitate PBT by mixing with the liquid component (L), but is preferably at least one selected from the group consisting of aromatic hydrocarbon solvents, aliphatic hydrocarbon solvents, ketone solvents, aldehyde solvents, alcohol solvents, ether solvents, and water. Examples of the solvent (P) include aromatic hydrocarbon solvents such as toluene; aliphatic hydrocarbon solvents such as hexane, heptane, octane, hexene, heptene, octene, cyclopentane, cyclohexane, cycloheptane, cyclohexene, and cycloheptene; ketone solvents such as acetone, methyl ethyl ketone, pentanone, hexanone, diethyl ketone, methyl isobutyl ketone, 3-penten-2-one, cyclopropanone, cyclobutanone, and dimethylacetophenone; propionaldehyde, butyraldehyde, pentanal, hexanal, and the like. Examples of suitable solvents include aldehyde solvents such as methyl methyl ether, vinyl aldehyde, glyoxal, isobutyl aldehyde, and succinaldehyde; alcohol solvents such as methanol, ethanol, propanol, isopropanol, isobutyl alcohol, and tert-butyl alcohol; ether solvents such as diethyl ether, 1,4-dioxane, tetrahydrofuran, isopropyl methyl ether, methyl propyl ether, furan, cyclopentyl methyl ether, ethyl isopropyl ether, and tert-butyl propyl ether; and water. These solvents may be used alone or in combination of two or more. Among these, it is preferable to use one or more solvents selected from the group consisting of acetone, toluene, methanol, ethanol, isopropyl alcohol, and water as the solvent (P).
[0045] The amount of solvent (P) used may be any amount sufficient to precipitate PBT, but is preferably 200% by mass or more, more preferably 300% by mass or more, and even more preferably 400% by mass or more, relative to the mass of the PBT composite material. If the proportion of solvent (P) is low, precipitation may not occur sufficiently, or fluidity may be reduced during subsequent solid-liquid separation. Furthermore, the amount of solvent (P) used is preferably 5000% by mass or less, more preferably 4000% by mass or less, and even more preferably 3000% by mass or less, relative to the mass of the PBT composite material. If the proportion of solvent (P) is high, PBT may also dissolve in the solvent (P) depending on the conditions, resulting in a decrease in yield. For example, the amount of solvent (P) used may be 200% by mass to 5000% by mass, 300% by mass to 3000% by mass, or 400% by mass to 4000% by mass, relative to the mass of the PBT composite material.
[0046] In step (C), the operation for obtaining a slurry (precipitation operation) is preferably carried out while controlling the temperature (the temperature of the mixed liquid of the liquid component (L) and the solvent (P)). If the temperature is not controlled, the precipitation time will be non-uniform, and when the liquid is sent to the next step, precipitation may be insufficient, resulting in a poor yield. The temperature during the precipitation operation is preferably equal to or lower than the boiling points of the solvents (S) and (P). If the temperature exceeds the boiling points of the solvents (S) and (P), the solubility of PBT increases, making it difficult to recover a sufficient amount of PBT. The specific temperature during the precipitation operation is preferably 0°C or higher, more preferably 5°C or higher, and even more preferably 10°C or higher. If the temperature is too low, the liquid may take a long time to be sent to the next step, or a large load may be placed on the filtration during filtration. The upper limit is preferably 80°C or lower, more preferably 60°C or lower, and even more preferably 50°C or lower. If the temperature is too high, there is a risk that the PBT may be deteriorated by heat. For example, the specific temperature during the precipitation operation can be 0°C to 80°C, 5°C to 60°C, or 10°C to 50°C.
[0047] In step (C), the liquid component (L) and the solvent (P) are usually mixed, and then the mixture is stirred for a predetermined time to sufficiently precipitate PBT and obtain a slurry. The precipitated PBT is usually PBT crystals having at least a crystalline structure in part. The method for mixing the liquid component (L) and the solvent (P) is not particularly limited, and the solvent (P) may be supplied to the liquid component (L), or the liquid component (L) may be supplied to the solvent (P). From the viewpoint of being able to slowly precipitate PBT and making it difficult for impurities to be incorporated into the PBT, a method of supplying the solvent (P) to the liquid component (L) is preferred, and a method of supplying the solvent (P) dropwise to the liquid component (L) is more preferred. When two or more types of solvents (P) are supplied to the liquid component (L), two or more types of solvents (P) may be mixed and supplied, or supplied separately.
[0048] As PBT precipitates, the ratio of solid (PBT) to liquid increases, and therefore the stirring efficiency tends to decrease. In order to suppress the decrease in stirring efficiency that accompanies this PBT precipitation, it is preferable to mix the liquid component (L) and the solvent (P) while controlling the temperature so that the PBT is gradually precipitated and the PBT does not form clumps, and it is more preferable to mix by dropwise supply while controlling the temperature.
[0049] The operation of precipitating PBT may be carried out at a constant temperature, but it is preferable to mix the liquid component (L) and the solvent (P) and then cool the mixture to a temperature lower than the mixing temperature to further precipitate PBT. In this case, in order to gradually precipitate PBT, the liquid component (L) and the solvent (P) are preferably mixed at a temperature of more than 20°C and less than 80°C in the reaction vessel in step (C). When the liquid component (L) is supplied to the solvent (P), the temperature of the solvent (P) is preferably more than 20°C, more preferably 30°C or higher, depending on the boiling points of the solvent (P) and the liquid component (L). Furthermore, when the solvent (P) is supplied to the liquid component (L), the temperature of the liquid component (L) is preferably more than 20°C and less than 80°C, more preferably 30°C or higher and less than 60°C, depending on the boiling points of the solvent (P) and the liquid component (L).
[0050] The supply rate can be appropriately set depending on the size of the reaction vessel, the amount of liquid, etc., as long as it does not exceed the above-mentioned temperature, but it is preferable to set it to a rate that allows the entire amount to be supplied within 4 hours. Furthermore, if the supply rate is too fast, crystal growth will proceed rapidly and impurities will be more likely to be incorporated, so it is preferable to set it to a rate that allows the entire amount to be supplied in 0.25 hours or more. That is, the supply time is preferably 0.25 to 3 hours, more preferably 0.5 to 1.5 hours. The supply time refers to the time required to supply the entire amount of liquid component (L) when supplying liquid component (L) to solvent (P), and the time required to supply the entire amount of solvent (P) when supplying solvent (P) to liquid component (L).
[0051] In step (C), after mixing the liquid component (L) and the solvent (P), it is preferable to cool the mixture to a predetermined aging temperature of 20°C or less, and then maintain the aging temperature to precipitate PBT. The aging temperature is preferably 20°C or less, more preferably 15°C or less. The lower limit is preferably 0°C or more, more preferably 5°C or more. The cooling rate is preferably 5°C / min or less, preferably 3°C / min or less, and even more preferably 1°C / min or less. If the aging temperature is maintained for too short a time (aging time), PBT may not precipitate sufficiently, which may reduce the yield of recycled PBT. Therefore, the time for maintaining the aging temperature (aging time) is preferably 0.5 hours or more, more preferably 1.5 hours or more. Furthermore, since the increase in the amount of precipitated PBT is small beyond a certain time, the upper limit of the aging time is usually 3 hours or less.
[0052] (Separation of PBT) In step (C), after obtaining a slurry in which PBT has precipitated, the slurry is subjected to solid-liquid separation to recover solid PBT. Solid-liquid separation of the slurry can be performed by known methods such as filtration or centrifugation, but filtration is preferred. Filtration may be performed using any of filter paper, centrifugal filtration, cyclone filtration, glass filters, bag filters, candle filters, etc. In addition, multiple stages and multiple methods may be used for filtering. If the mesh size of the filter medium is too large, removal of foreign matter tends to be insufficient, and if it is too small, filtering performance tends to be poor. Therefore, the smallest mesh size of the filter medium is preferably 15 μm or less, more preferably 10 μm or less, and even more preferably 5 μm or less. In addition, the smallest mesh size of the filter medium is preferably 1 μm or more, more preferably 3 μm or more.
[0053] (Washing of PBT) The solid PBT recovered by solid-liquid separation may be dried as is in step (D). However, since impurities may be attached to the surface of the PBT, it is preferable to further wash the PBT and then dry it in step (D). Therefore, after step (C), a step of further washing the solid PBT may be performed. Specifically, the solid PBT recovered by solid-liquid separation is mixed with a post-washing solvent, stirred, and then the post-washing solvent is removed. This removes impurities attached to the surface of the PBT.
[0054] The solvent for post-washing can be any solvent that can be used as the solvent (P) in step (C), and it is preferable to use one or more selected from the group consisting of acetone, toluene, methanol, ethanol, isopropyl alcohol, and water. The solvent for post-washing and the solvent (P) in step (C) may be the same or different. To facilitate solvent removal in step (D), the solvent for post-washing preferably has a boiling point of 100°C or less, more preferably 60°C or less. The temperature of the solvent during post-washing can be appropriately set depending on the boiling point of the solvent used, but is preferably 25 to 80°C. The amount of solvent used for post-washing is preferably 200% by mass or more, more preferably 500% by mass or more, relative to the mass of the precipitated PBT. Washing may also be performed multiple times. When performing multiple washes, the type of solvent used, temperature, amount of solvent, and other conditions may be the same or different for each wash.
[0055] <Step (D)> Step (D) is a step of drying the solid PBT to obtain recycled PBT. The drying method is not particularly limited, and a known method can be used, and drying under reduced pressure or atmospheric pressure can be used. The drying temperature can be determined appropriately, and for example, drying can be performed at 50 to 120°C for 2 to 15 hours.
[0056] <Recycling of Solvent> When producing recycled PBT on an industrial scale, the solvents used in each step may be separated from impurities by distillation, recovered, and reused. For example, the liquid separated from PBT by solid-liquid separation in step (C) contains solvent (S) and solvent (P), and these may be recovered by distillation and reused in step (A) and step (C).
[0057] <Recycled PBT> The recycled PBT obtained by the recycled PBT manufacturing method of the present invention is polybutylene terephthalate regenerated from a PBT composite material by material recycling. The recycled PBT has physical properties such as intrinsic viscosity and MFR value that are satisfactory for practical use, making it possible to use the recycled PBT for molding processing.
[0058] [Intrinsic Viscosity] Measurement of intrinsic viscosity can confirm that the recycled PBT production method of the present invention does not cause a decrease in intrinsic viscosity due to PBT decomposition or an increase in viscosity due to the inclusion of impurities. Generally, the intrinsic viscosity of PBT is preferably 0.5 to 2 dL / g, and it is known that, from the standpoint of moldability and mechanical properties, an intrinsic viscosity in the range of 0.6 to 1.5 dL / g is more preferable. If the recycled PBT obtained by the recycled PBT production method of the present invention can be kept within this range, it can be used practically without problems during molding. The recycled PBT production method of the present invention can produce material recycled PBT with an intrinsic viscosity of 0.6 to 1.5 dL / g.
[0059] [Melt flow rate (MFR)] The melt flow rate (MFR) is a numerical value that indicates the fluidity of a thermoplastic resin when melted. This value is an index of fluidity and molecular weight, and the larger the value, the higher the fluidity and the lower the molecular weight. Generally, at 250°C and 50 kgf / cm 2 The MFR of the PBT resin at 250°C and 50 kgf / cm is preferably 10 to 100 g / 10 min, and from the viewpoint of moldability and mechanical properties, 10 to 90 g / 10 min is preferable. 2 It is possible to obtain recycled PBT with an MFR of 10 to 90 g / 10 min.
[0060] [L Value] When it is desired to dye the obtained recycled PBT to a desired color, the L value of the recycled PBT is preferably 80 or more, more preferably 85 or more, and even more preferably 90 or more.
[0061] [Ash content] The amount of inorganic matter remaining in the recycled PBT can be calculated by incinerating the recycled PBT and then calculating the amount of inorganic matter (ash content) remaining in the recycled PBT from the amount of the remaining inorganic matter. The amount of ash remaining in the recycled PBT is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 1% by mass or less.
[0062] <Method for producing PBT composite material> The present invention also relates to a method for producing a PBT composite material (hereinafter, sometimes referred to as "method for producing a PBT composite material of the present invention"), which includes a step of producing recycled PBT by the method for producing recycled PBT of the present invention, and a step of producing a PBT composite material using the obtained recycled PBT.
[0063] The process for producing recycled PBT is as described above. The process for producing a PBT composite material can be carried out by a known production method, except that recycled PBT is used as the raw material PBT. Examples of methods for producing a PBT composite material include injection molding, ultra-high speed injection molding, injection compression molding, two-color molding, gas-assisted or other blow molding, molding using an insulated mold, molding using a rapidly heated mold, insert molding, IMC (in-mold coating) molding, extrusion molding, and sheet molding. This allows for the production of injection-molded products, extrusion-molded products, sheets, pipes, various films, and the like. Furthermore, these may be molded products containing glass fiber or other resins, rather than PBT alone.
[0064] In the process for producing a PBT composite material, the raw material PBT may contain recycled PBT, and recycled PBT alone may be used, or recycled PBT and virgin PBT may be used in combination.
[0065] The form of the PBT composite material to be produced is not particularly limited, and PBT-containing molded articles, PBT-containing laminated articles, etc. can be produced by the method for producing a PBT composite material of the present invention.
[0066] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as the gist of the present invention is not changed.
[0067] <Analysis Method> = Intrinsic Viscosity Measurement = 0.5 g of the recycled PBT obtained was dissolved in 30 mL of a mixed solvent of phenol / 1,1,2,2-tetrachloroethane (mass ratio 1 / 1). Using an Ubbelohde viscometer, the number of seconds it took for the polymer solution of the dissolved sample and the mixed solvent alone to fall at 30°C was measured, and the intrinsic viscosity was calculated using the following formula.
[0068]
[0069] where η sp = η / η0-1, where η is the number of seconds it takes for the polymer solution to fall, and η0 is the number of seconds it takes for the mixed solvent alone to fall. C is the concentration of the polymer solution [g / dL]. K H is the Hangis multiplier, and K H was set to 0.33.
[0070] =Measurement of Melt Flow Rate (MFR)= The obtained recycled PBT was measured at 250°C and 50 kgf / cm using a high-temperature flow tester. 2 The MFR was measured under the following conditions.
[0071] Measurement of Melting Point (Tm) Using a DSC ("DSC200" manufactured by Hitachi High-Tech Science Corporation), 8 mg of the recycled PBT sample was heated from 30°C to 300°C at a rate of 10°C / min to measure the melting point (Tm) of the recycled PBT. Furthermore, to confirm the absence of PBT decomposition and the presence of other resins using the method of the present invention, it was confirmed that the PBT melting point peak was not split into two, was not broadened, and that no other peaks were present. When no abnormalities were observed in the peak, the result was evaluated as "absent," and when an abnormality was observed in the peak, the result was evaluated as "present."
[0072] = Measurement of Ash Content = Sulfuric acid was added to the recycled PBT, and the mixture was subjected to a white smoke treatment on a hot plate, followed by dry ashing in an electric furnace ("Muffle Furnace FP410" manufactured by Yamato Co., Ltd.) at 650° C. The weight of the mixture was measured, and the weight before and after treatment was compared to calculate the ash content.
[0073] =Confirmation of presence or absence of other resins= Raw material B, which will be described later, contains AS resin, and raw material C contains HIPS (high impact polystyrene) resin. 20 mg of the obtained recycled PBT sample was dissolved in 1 mL of 1,1,1,3,3,3-hexafluoro-2-propanol (HFIP). Since the HIPS contained in raw material C does not dissolve in HFIP, filtration was carried out and the residual rate was confirmed from the weight of the residue. Since the AS resin contained in raw material B dissolves in HFIP, after dissolution and filtration, 1 mL of deuterated chloroform was added and the remaining AS resin was confirmed by 1H-NMR, and each was evaluated as follows: None: residual rate is 0.1% or less (below the lower limit of quantification) Slightly remaining: residual rate is 0.5% or less Present: residual rate is 1% or more
[0074] =Measurement of Color Tone= The L value of the recycled PBT was measured using a color difference meter ("ZE-6000" manufactured by Nippon Denshoku Industries Co., Ltd.).
[0075] =Measurement of Residual Amount of Phenol= The obtained recycled PBT was immersed in acetonitrile for 24 hours to extract phenol into the acetonitrile, and then the amount of phenol was quantified by high performance liquid chromatography (Waters "Waters e2695" manufactured by Waters).
[0076] <PBT composite material (raw materials)> The following raw materials A to C were used. Raw material A: Polybutylene terephthalate resin containing 30% glass fiber (GF) (containing carbon black (CB)) (process waste) Raw material B: Polybutylene terephthalate containing 30% GF / AS resin (process waste from spool runner) Raw material C: Polybutylene terephthalate containing 30% GF / HIPS resin (process waste from spool runner)
[0077] The raw material was previously cut into particles of 0.5 cm x 0.5 cm size using a cutter.
[0078] [Example 1] (Step (A)) In a 500 mL flask, 100 g of phenol (1000% by mass relative to raw material A) was added as a solvent (S), and 10 g of crushed raw material A was added. The mixture was heated at 80°C for 1 hour while stirring under a nitrogen atmosphere to obtain a PBT solution.
[0079] (Step (B)) The PBT solution obtained in step (A) was filtered using filter paper with a pore size of 0.5 μm to remove impurities, and a filtrate (liquid component (L)) in which PBT was dissolved was obtained.
[0080] (Step (C)) While the filtrate obtained in step (B) was kept at 50°C, 100 g of acetone (1000% by mass relative to raw material A) was gradually added dropwise to the filtrate as a solvent (P) so that the temperature did not exceed the controlled temperature of 50°C, thereby precipitating PBT. After the entire amount of acetone was added, the temperature was lowered to 20°C over 30 minutes, and then the mixture was stirred at 20°C for 1 hour. The mixture was filtered using filter paper with a pore size of 7 μm, and the filtrate (PBT) was recovered.
[0081] (Step (D)) The filtered product (wet cake) obtained in step (C) was dried at 80° C. under reduced pressure using an evaporator to obtain recycled PBT.
[0082] The recycled PBT obtained was subjected to the evaluations according to the above procedures. The evaluation results are shown in Table 1.
[0083] Example 2 The same procedure as in Example 1 was carried out, except that the solvent (P) in step (C) was changed to isopropyl alcohol. Table 1 shows the evaluation results.
[0084] Example 3 The same procedure as in Example 1 was carried out, except that the solvent (P) in step (C) was changed to water. Table 1 shows the evaluation results.
[0085] Example 4 The procedure of Example 1 was repeated except that the solvent (P) in step (C) was changed to methanol. Table 1 shows the evaluation results.
[0086] Example 5 The same procedure as in Example 1 was carried out, except that the solvent (S) in step (A) was changed from phenol to cresol. Table 1 shows the evaluation results.
[0087] [Example 6] (Step (A)) 300 g (1000 mass % based on raw material A) of a mixed solvent of phenol:toluene = 1:1 (mass ratio) was added as solvent (S) to a 1 L separable flask, 30 g of cut raw material A was added, and the mixture was heated at 80°C for 1 hour while stirring under a nitrogen atmosphere to obtain a PBT solution.
[0088] (Step (B)) The PBT solution obtained in step (A) was filtered using filter paper with a pore size of 0.5 μm to remove impurities, and a filtrate (liquid component (L)) in which PBT was dissolved was obtained.
[0089] (Step (C)) While the filtrate obtained in step (B) was kept at 50°C, 300 g of acetone (1000% by mass relative to raw material A) was gradually added dropwise to the filtrate as solvent (P) so that the temperature did not exceed the controlled temperature of 50°C, thereby precipitating PBT. After the entire amount of acetone was added, the temperature was lowered to 20°C over 30 minutes, and then the mixture was stirred for 1 hour at 10°C. The mixture was filtered using filter paper with a pore size of 7 μm, and the filtrate (PBT) was recovered.
[0090] (Step (D)) The filtered product obtained in step (C) was dried at 80° C. under reduced pressure using an evaporator to obtain recycled PBT. Table 1 shows the evaluation results.
[0091] Example 7 The same procedure as in Example 1 was repeated, except that the PBT composite material was changed to raw material B. Table 2 shows the evaluation results.
[0092] Example 8 The same procedure as in Example 1 was repeated, except that the PBT composite material was changed to raw material C. Table 2 shows the evaluation results.
[0093] Example 9 The same procedure as in Example 1 was repeated, except that the PBT composite material was changed to raw material B and the solvent (S) in step (A) was changed to phenol:toluene = 4:6 (mass ratio). Table 2 shows the evaluation results.
[0094] [Example 10] (Step (A)) In a 500 mL flask, 100 g of phenol (1000% by mass relative to raw material A) was added as a solvent (S), and 10 g of crushed raw material A was added. The mixture was heated at 80°C for 1 hour while stirring under a nitrogen atmosphere to obtain a PBT solution.
[0095] (Step (X)) 2.5 g of activated carbon (powder, sawdust) was added to the PBT solution obtained in step (A), and the mixture was stirred for 30 minutes.
[0096] (Step (B)) The PBT solution after step (X) was filtered using filter paper with a pore size of 0.5 μm to remove impurities, and a clear filtrate (liquid component (L)) in which PBT was dissolved was obtained.
[0097] (Step (C)) While the filtrate obtained in step (B) was kept at 50°C, 100 g of acetone (1000% by mass relative to raw material A) was gradually added dropwise to the filtrate as a solvent (P) so that the temperature did not exceed the controlled temperature of 50°C, thereby precipitating PBT. After the entire amount of acetone was added, the temperature was lowered to 20°C over 30 minutes, and then the mixture was stirred at 20°C for 1 hour. The mixture was filtered using filter paper with a pore size of 7 μm, and the filtrate (PBT) was recovered.
[0098] (Step (D)) The filtered product obtained in step (C) was dried at 80° C. under reduced pressure using an evaporator to obtain recycled PBT. Table 3 shows the evaluation results.
[0099] [Example 11] (Step (A)) In a 500 mL flask, 100 g of phenol (1000% by mass relative to raw material A) was added as a solvent (S), and 10 g of crushed raw material A was added. The mixture was heated at 80°C for 1 hour while stirring under a nitrogen atmosphere to obtain a PBT solution.
[0100] (Step (X) and Step (B)) 2.5 g of activated carbon (powder, sawdust) was added to the PBT solution obtained in Step (A) and stirred for 30 minutes. Next, the PBT solution was filtered through 2.5 g of Celite placed on a filter paper with a pore size of 0.5 μm to remove impurities, and a clear filtrate (liquid component (L)) in which the PBT was dissolved was obtained.
[0101] (Step (C)) While the filtrate obtained in step (B) was kept at 50°C, 100 g of acetone (1000% by mass relative to raw material A) was gradually added dropwise to the filtrate as a solvent (P) so that the temperature did not exceed the controlled temperature of 50°C, thereby precipitating PBT. After the entire amount of acetone was added, the temperature was lowered to 20°C over 30 minutes, and then the mixture was stirred at 20°C for 1 hour. The mixture was filtered using filter paper with a pore size of 7 μm, and the filtrate (PBT) was recovered.
[0102] (Step (D)) The filtered product obtained in step (C) was dried at 80° C. under reduced pressure using an evaporator to obtain recycled PBT. Table 3 shows the evaluation results.
[0103] [Example 12] (Step (A)) In a 500 mL flask, 100 g of phenol (1000% by mass relative to raw material A) was added as a solvent (S), and 10 g of crushed raw material A was added. The mixture was heated at 80°C for 1 hour while stirring under a nitrogen atmosphere to obtain a PBT solution.
[0104] (Step (X)) 0.5 g of iron (II) sulfate was added to the PBT solution obtained in step (A), and the mixture was stirred for 60 minutes.
[0105] (Step (B)) The PBT solution after step (X) was filtered using filter paper with a pore size of 0.5 μm to remove impurities, and a clear filtrate (liquid component (L)) in which PBT was dissolved was obtained.
[0106] (Step (C)) While the filtrate obtained in step (B) was kept at 50°C, 100 g of acetone (1000% by mass relative to raw material A) was gradually added dropwise to the filtrate as a solvent (P) so that the temperature did not exceed the controlled temperature of 50°C, thereby precipitating PBT. After the entire amount of acetone was added, the temperature was lowered to 20°C over 30 minutes, and then the mixture was stirred at 20°C for 1 hour. The mixture was filtered using filter paper with a pore size of 7 μm, and the filtrate (PBT) was recovered.
[0107] (Step (D)) The filtered product obtained in step (C) was dried at 80° C. under reduced pressure using an evaporator to obtain recycled PBT. Table 3 shows the evaluation results.
[0108] [Example 13] (Step (A)) In a 500 mL flask, 100 g of phenol (1000% by mass relative to raw material A) was added as a solvent (S), and 10 g of chopped raw material A was added. The mixture was heated at 80°C for 1 hour while stirring under a nitrogen atmosphere to obtain a PBT solution.
[0109] (Step (X)) 0.1 g of iron(III) chloride was added to the PBT solution obtained in step (A), and the mixture was stirred for 60 minutes.
[0110] (Step (B)) The PBT solution after step (X) was filtered using filter paper with a pore size of 0.5 μm to remove impurities, and a clear filtrate (liquid component (L)) in which PBT was dissolved was obtained.
[0111] (Step (C)) While the filtrate obtained in step (B) was kept at 50°C, 100 g of acetone (1000% by mass relative to raw material A) was gradually added dropwise to the filtrate as a solvent (P) so that the temperature did not exceed the controlled temperature of 50°C, thereby precipitating PBT. After the entire amount of acetone was added, the temperature was lowered to 20°C over 30 minutes, and then the mixture was stirred at 20°C for 1 hour. The mixture was filtered using filter paper with a pore size of 7 μm, and the filtrate (PBT) was recovered.
[0112] (Step (D)) The filtered product obtained in step (C) was dried at 80° C. under reduced pressure using an evaporator to obtain recycled PBT. Table 3 shows the evaluation results.
[0113] Example 14 (Step (A)) To a 500 mL flask, 100 g of phenol (1000% by mass relative to raw material A) was added as a solvent (S), and 10 g of crushed raw material A was added. The mixture was heated at 80°C for 1 hour while stirring under a nitrogen atmosphere to obtain a PBT solution.
[0114] (Step (X)) 1 g of aluminum sulfate was added to the PBT solution obtained in step (A), and the mixture was stirred for 60 minutes.
[0115] (Step (B)) The PBT solution after step (X) was filtered using a filter paper with a pore size of 0.5 μm to remove impurities, thereby obtaining a clear filtrate in which PBT was dissolved.
[0116] (Step (C)) While the filtrate obtained in step (B) was kept at 50°C, 100 g of acetone (1000% by mass relative to raw material A) was gradually added dropwise to the filtrate as a solvent (P) so that the temperature did not exceed the controlled temperature of 50°C, thereby precipitating PBT. After the entire amount of acetone was added, the temperature was lowered to 20°C over 30 minutes, and then the mixture was stirred at 20°C for 1 hour. The mixture was filtered using filter paper with a pore size of 7 μm, and the filtrate (PBT) was recovered.
[0117] (Step (D)) The filtered product obtained in step (C) was dried at 80° C. under reduced pressure using an evaporator to obtain recycled PBT. Table 3 shows the evaluation results.
[0118] [Example 15] (Step (A)) In a 500 mL flask, 100 g of phenol (1000% by mass relative to raw material A) was added as a solvent (S), and 10 g of crushed raw material A was added. The mixture was heated at 80°C for 1 hour while stirring under a nitrogen atmosphere to obtain a PBT solution.
[0119] (Step (X)) 0.3 g of activated carbon (powder, sawdust) was added to the PBT solution obtained in step (A) and stirred for 30 minutes, after which 0.3 g of iron (III) sulfate was added and stirred for 60 minutes.
[0120] (Step (B)) The PBT solution after step (X) was filtered using filter paper with a pore size of 0.5 μm to remove impurities, and a clear filtrate (liquid component (L)) in which PBT was dissolved was obtained.
[0121] (Step (C)) While the filtrate obtained in step (B) was kept at 50°C, 100 g of acetone (1000% by mass relative to raw material A) was gradually added dropwise to the filtrate as a solvent (P) so that the temperature did not exceed the controlled temperature of 50°C, thereby precipitating PBT. After the entire amount of acetone was added, the temperature was lowered to 20°C over 30 minutes, and then the mixture was stirred at 20°C for 1 hour. The mixture was filtered using filter paper with a pore size of 7 μm, and the filtrate (PBT) was recovered.
[0122] (Step (D)) The filtered product obtained in step (C) was dried at 80° C. under reduced pressure using an evaporator to obtain recycled PBT. Table 3 shows the evaluation results.
[0123] Example 16 (Step (A)) In a 500 mL flask, 100 g (1000 mass % based on raw material A) of a mixed solvent of phenol:toluene = 1:1 (mass ratio) was placed as solvent (S), and 10 g of chopped raw material A was added. The mixture was heated at 80°C for 1 hour with stirring under a nitrogen atmosphere to obtain a PBT solution.
[0124] (Step (X)) 0.1 g of activated carbon (powder, sawdust) was added to the PBT solution obtained in step (A) and stirred for 30 minutes, after which 0.1 g of iron (II) sulfate was added and stirred for 60 minutes.
[0125] (Step (B)) The PBT solution after step (X) was filtered using filter paper with a pore size of 0.5 μm to remove impurities, and a clear filtrate (liquid component (L)) in which PBT was dissolved was obtained.
[0126] (Step (C)) While the filtrate obtained in step (B) was kept at 50°C, 100 g of acetone (1000% by mass relative to raw material A) was gradually added dropwise to the filtrate as a solvent (P) so that the temperature did not exceed the controlled temperature of 50°C, thereby precipitating PBT. After the entire amount of acetone was added, the temperature was lowered to 20°C over 30 minutes, and then the mixture was stirred at 20°C for 1 hour. The mixture was filtered using filter paper with a pore size of 7 μm, and the filtrate (PBT) was recovered.
[0127] (Step (D)) The filtered product obtained in step (C) was dried at 80° C. under reduced pressure using an evaporator to obtain recycled PBT. Table 3 shows the evaluation results.
[0128] [Reference Example] The intrinsic viscosity, MFR, and Tm were measured using "NovaDuran (registered trademark) 5020" manufactured by Mitsubishi Chemical Corporation. The results are shown in Tables 1 and 2.
[0129] Comparative Example 1: 100 g of phenol (1000% by mass relative to raw material A) was added to a 500 mL flask, and 10 g of crushed raw material A was added. The mixture was heated at 80°C for 1 hour with stirring under a nitrogen atmosphere to obtain a PBT solution. The phenol was gradually distilled off from the obtained PBT solution under reduced pressure at 120°C, and the solution was dried. The results are shown in Table 4.
[0130] Comparative Example 2 The same procedure as in Comparative Example 1 was carried out, except that the raw material was changed to raw material B. The results are shown in Table 4.
[0131] Comparative Example 3 The same procedure as in Comparative Example 1 was carried out, except that the raw material was changed to raw material C. The results are shown in Table 4.
[0132] Comparative Example 4 100 g of 1,4-butanediol (1000% by mass based on raw material A) was placed in a 500 mL flask, and 10 g of chopped raw material A was added. The mixture was heated to 120° C. with stirring under a nitrogen atmosphere, but did not dissolve.
[0133] Comparative Example 5: To a 500 mL flask, 100 g of 1,4-butanediol (1000% by mass relative to raw material A) was added, 10 g of chopped raw material A was added, and 0.1 g of sodium hydroxide was further added. The mixture was heated to 80°C with stirring under a nitrogen atmosphere, resulting in dissolution. Next, the mixture was filtered using filter paper with a pore size of 0.5 μm to obtain a filtrate. When 100 g of acetone (1000% by mass relative to raw material A) was added dropwise to the obtained filtrate, no crystals were precipitated. It is believed that the addition of sodium hydroxide caused the PBT to decompose.
[0134] Comparative Example 6: Using a 15 mm vent-type twin-screw extruder (manufactured by Technovel Co., Ltd., twin-screw extruder "KZW") equipped with a 50-mesh screen mesh on the breaker plate, raw material A was melt-extruded at a barrel temperature of 260°C to remove impurities such as glass fibers. The screen mesh became clogged, and the extruder was frequently stopped and the screen mesh was replaced, resulting in the production of PBT. The results are shown in Table 4.
[0135] Table 1 shows the results of Examples 1 to 6, in which various solvents were used to study raw material A. It can be seen that by dissolving PBT in a solvent (S) containing a phenolic solvent and then contacting it with a solvent (P) in which PBT is insoluble, recycled PBT of a quality that is acceptable for practical use can be obtained without decomposing the PBT.
[0136]
[0137] Table 2 shows the results of Examples 7 to 9, which used raw materials contaminated with other resins. It can be seen that even in samples contaminated with other resins, recycled PBT of a quality that is acceptable for practical use can be obtained without decomposing the PBT and without containing any resins other than PBT.
[0138]
[0139] Table 3 shows the results of Examples 10 to 16. It can be seen that the addition of a filter aid or a flocculant can improve the color tone of recycled PBT obtained from black-colored PBT resin.
[0140]
[0141] The results of the comparative examples are shown in Table 4. It can be seen that when recovering PBT by distillation of the solvent (S), inorganic substances such as reinforcing agents such as glass fiber cannot be removed, it does not dissolve in solvents generally used in chemical recycling, and it decomposes when alkali is added, and when material recycling by melt extrusion is performed, not only are impurities not sufficiently removed, but the physical properties deteriorate due to thermal degradation.
[0142]
[0143] As described above, the method for producing recycled PBT of the present invention makes it possible to obtain recycled PBT of a quality that is acceptable for practical use, and to produce PBT composite materials from the obtained recycled PBT.
Claims
1. A method for producing recycled polybutylene terephthalate from a polybutylene terephthalate composite material, comprising the following steps (A) to (D); step (A): dissolving a polybutylene terephthalate composite material in a solvent (S) containing a phenol-based solvent to obtain a solution in which polybutylene terephthalate is dissolved; step (B): removing insoluble matter from the solution in which polybutylene terephthalate is dissolved to obtain a liquid component (L) in which polybutylene terephthalate is dissolved; step (C): mixing the liquid component (L) with a solvent (P) capable of precipitating polybutylene terephthalate when mixed with the liquid component (L), precipitating polybutylene terephthalate to obtain a slurry, and then subjecting the slurry to solid-liquid separation to obtain solid polybutylene terephthalate; step (D): drying the solid polybutylene terephthalate to obtain recycled polybutylene terephthalate; A method for producing recycled polybutylene terephthalate, comprising:
2. A method for producing recycled polybutylene terephthalate as described in claim 1, comprising a step (X1) of contacting the solution in which the polybutylene terephthalate is dissolved with a coagulant prior to the step (B).
3. The method for producing recycled polybutylene terephthalate according to claim 1 or 2, comprising a step (X2) of contacting the solution in which the polybutylene terephthalate is dissolved with a filter aid prior to the step (B).
4. A method for producing recycled polybutylene terephthalate according to claim 1 or 2, wherein the temperature of the solvent (S) in step (A) is 45°C or higher and 150°C or lower.
5. A method for producing recycled polybutylene terephthalate according to claim 1 or 2, wherein in step (C), the slurry is obtained at a temperature of 0°C or higher and 80°C or lower.
6. A method for producing recycled polybutylene terephthalate as described in claim 1 or 2, wherein the solvent (P) in step (C) is one or more selected from the group consisting of aromatic hydrocarbon solvents, aliphatic hydrocarbon solvents, ketone solvents, aldehyde solvents, alcohol solvents, ether solvents and water.
7. The method for producing recycled polybutylene terephthalate according to claim 6, wherein the solvent (P) in step (C) is one or more selected from the group consisting of acetone, toluene, methanol, ethanol, isopropyl alcohol and water.
8. The method for producing recycled polybutylene terephthalate described in claim 2, wherein the coagulant in step (X1) is one or more selected from the group consisting of inorganic salts other than alkali metals and alkaline earth metals and polymer compounds.
9. The method for producing recycled polybutylene terephthalate according to claim 2, wherein the coagulant in step (X1) comprises an inorganic salt other than an alkali metal or an alkaline earth metal.
10. A method for producing recycled polybutylene terephthalate according to claim 8 or 9, wherein the inorganic salt other than alkali metals and alkaline earth metals is one or more selected from the group consisting of iron (III) chloride, iron (II) sulfate, iron (III) sulfate, aluminum sulfate and aluminum chloride.
11. A method for producing recycled polybutylene terephthalate as described in claim 8, wherein a solution in which the polybutylene terephthalate is dissolved is contacted with the coagulant consisting of an inorganic salt other than the alkali metal and alkaline earth metal, and then contacted with the coagulant consisting of the polymer compound.
12. The method for producing recycled polybutylene terephthalate described in claim 8, wherein the polymer compound is one or more selected from the group consisting of polyacrylamide and polyethylene oxide.
13. The method for producing recycled polybutylene terephthalate described in claim 3, wherein the filter aid in step (X2) is one or more selected from the group consisting of activated carbon, activated clay, celite, silica gel, synthetic adsorbents, bentonite, alumina and zeolite.
14. The method for producing recycled polybutylene terephthalate according to claim 1 or 2, wherein the solvent (S) contains an aromatic hydrocarbon solvent and / or an aliphatic hydrocarbon solvent.
15. A method for producing recycled polybutylene terephthalate as described in claim 14, wherein the total content of aromatic hydrocarbon solvents and aliphatic hydrocarbon solvents in the solvent (S) is 20 mass% or more.
16. A method for producing recycled polybutylene terephthalate as described in claim 1 or 2, wherein the polybutylene terephthalate content in the polybutylene terephthalate composite material is 10 mass% or more.
17. A method for producing recycled polybutylene terephthalate as described in claim 1 or 2, wherein the polybutylene terephthalate composite material contains other components other than polybutylene terephthalate, and the other components include one or more selected from the group consisting of inorganic compounds, organic low molecular weight compounds, fibers other than polybutylene terephthalate, and resins other than polybutylene terephthalate.
18. The method for producing recycled polybutylene terephthalate according to claim 1 or 2, wherein the polybutylene terephthalate composite material is an injection-molded article containing polybutylene terephthalate.
19. A method for producing recycled polybutylene terephthalate according to claim 1 or 2, wherein the intrinsic viscosity of the recycled polybutylene terephthalate is 0.6 dL / g or more and 1.5 dL / g or less.
20. Material recycled polybutylene terephthalate having an intrinsic viscosity of 0.6 dL / g or more and 1.5 dL / g or less.
21. A method for producing a polybutylene terephthalate composite material, comprising the steps of: producing recycled polybutylene terephthalate by the method for producing recycled polybutylene terephthalate according to claim 1 or 2; and producing a polybutylene terephthalate composite material using the recycled polybutylene terephthalate obtained.
Citation Information
Patent Citations
Method for producing polybutylene telephthalate
JP2023075033A
Aromatic polycarbonate resin composition and resin molded product
JP2007176969A
Method for removing inorganic particle in liquid
JP2009112901A
Solvent based approach to post-consumer recycling of polyethylene terephthalate
US20220332914A1
Removal of color from polymeric materials
WO2022040119A1
Cited By
Method for producing recycled polybutylene terephthalate resin, method for separating polybutylene terephthalate resin from recycled materials, and method for recovering a solution containing at least polybutylene terephthalate.
JP2026111837A
Method for producing recycled polybutylene terephthalate resin, method for separating polybutylene terephthalate resin from material for recycling, and method for recovering solution that includes at least polybutylene terephthalate
WO2026141066A1