Lithium metal battery and manufacturing method therefor

The introduction of a protective layer with boric acid or boron oxide on the negative electrode current collector in lithium metal batteries addresses the issue of lithium dendrite growth, enhancing the battery's high-rate capabilities and lifespan by preventing material deterioration and side reactions.

WO2024205093A1PCT designated stage expired Publication Date: 2024-10-03SAMSUNG SDI CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/003362
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-23
Filing Date
2024-03-18
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Lithium metal batteries with carbon-based anode active materials have limited capacity and are prone to lithium dendrite growth due to side reactions with the electrolyte, leading to reduced lifespan and safety issues.

Method used

A lithium metal battery design featuring a negative electrode with a protective layer containing boric acid or boron oxide, which inhibits lithium dendrite growth and improves lithium ion transfer, comprising a negative electrode current collector with a protective layer and an optional lithium electrodeposition induction layer, and using a suitable electrolyte.

Benefits of technology

The solution enhances the high-rate characteristics and lifespan of lithium metal batteries by preventing deterioration of the negative electrode active material layer and minimizing side reactions, thereby maintaining capacity and improving stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024003362_03102024_PF_FP_ABST
    Figure KR2024003362_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided are a negative electrode for a lithium metal battery, a lithium metal battery comprising same, and a method for producing the same, wherein the negative electrode comprises: a current collector; and a protective layer formed on the current collector and includes or is free of an active material layer disposed between the current collector and the protective layer, the protective layer comprising a hydroxyl group-containing first polymer, a hydrate of i) boric acid (H3BO3) or ii) boron oxide (B2O3) and water, or a combination thereof.
Need to check novelty before this filing date? Find Prior Art

Description

Lithium metal battery and manufacturing method thereof

[0001] It relates to a lithium metal battery and a method for manufacturing the same.

[0002] Lithium metal batteries currently on the market primarily use carbon-based anode materials, such as graphite. Carbon-based anode materials exhibit no volume change during charge / discharge, enhancing the stability of lithium metal batteries. However, their low capacity necessitates the use of higher-capacity anode materials.

[0003] Lithium metal, which has a much larger theoretical electric capacity than carbon-based negative electrode materials, can be used as a negative electrode material.

[0004] When lithium metal is charged and discharged, dendrites are formed on the surface of the lithium metal due to a side reaction with the electrolyte, and the growth of the dendrites can cause a short circuit between the positive and negative electrodes, which can reduce the life characteristics of a lithium metal battery containing lithium metal.

[0005] A method for improving the life characteristics of a lithium metal battery containing lithium metal is required.

[0006] One aspect is to provide a new structure of cathode for lithium metal batteries.

[0007] Another aspect is to provide a lithium metal battery comprising a cathode of a novel structure.

[0008] Another aspect is to provide a method for manufacturing a negative electrode for a lithium metal battery of a new structure.

[0009] According to one embodiment, a negative current collector; and

[0010] It includes a protective layer formed on the negative electrode current collector,

[0011] It includes a negative electrode active material layer disposed between the negative electrode current collector and the protective layer, or the negative electrode active material layer is absent (free),

[0012] The above protective layer comprises a first polymer containing a hydroxyl group,

[0013] i) boric acid (H3BO3); or ii) a hydrate of boron oxide (B2O3) and water; or a combination thereof,

[0014] A cathode for a lithium metal battery is provided.

[0015] Bipolar according to other aspects;

[0016] The above-mentioned cathode; and

[0017] A lithium metal battery is provided including an electrolyte disposed between the positive electrode and the negative electrode.

[0018] The electrolyte is a liquid electrolyte, a solid electrolyte, a gel polymer electrolyte, or a combination thereof. The solid electrolyte includes an oxide-based solid electrolyte, a sulfide-based solid electrolyte, a polymer solid electrolyte, or a combination thereof, and the gel electrolyte includes a polymer gel electrolyte.

[0019] Another aspect is the step of preparing a cathode current collector;

[0020] A step of preparing a composition for forming a protective layer comprising a first polymer containing a hydroxyl group and i) a hydrate of boric acid (H3BO3), ii) boron oxide (B2O3) and water or a combination thereof, and then coating and drying the composition on a negative electrode current collector to form a protective layer;

[0021] Steps for preparing electrolyte;

[0022] Steps for preparing the anode; and

[0023] A method for manufacturing a lithium metal battery is provided, including a step of preparing an assembly by laminating a negative electrode current collector, a separator, and a positive electrode.

[0024] According to one aspect, by adopting a negative electrode for a lithium metal battery having a new structure, deterioration of the negative electrode active material layer is prevented, and a lithium metal battery with improved high-rate characteristics and lifespan characteristics is provided.

[0025] Figure 1a is for explaining the effect of boric acid in the protective layer of a negative electrode for a lithium metal battery according to an embodiment.

[0026] Figure 1b is for explaining the effect of improving Li ion transfer by BOB bonding in the protective layer of a negative electrode for a lithium metal battery according to an embodiment.

[0027] Figure 2 is a drawing for explaining the laminated structure of a lithium metal battery according to an embodiment.

[0028] Figure 3 shows the change in capacity retention rate according to the number of cycles in the lithium metal batteries of Example 1 and Comparative Example 1.

[0029] Figure 4 shows the change in capacity according to the number of cycles in the lithium metal batteries of Example 1 and Comparative Example 1.

[0030] Figure 5 is an SEM photograph showing a state in which a protective layer is laminated on top of the negative electrode current collector in the lithium metal battery manufactured in Example 1.

[0031] Figure 6a is a scanning electron microscope (SEM) photograph showing the state of the negative electrode in a diagonal direction after charging to 100% SOC (state of charge) in the lithium metal battery of Example 1.

[0032] Figure 6b is a cross-sectional SEM photograph showing the state of the negative electrode after charging to 100% SOC in the lithium metal battery of Example 1.

[0033] Figure 6c is a cross-sectional SEM photograph showing the state of the negative electrode after charging to 100% SOC in the lithium metal battery of Example 1.

[0034] Figure 7 is a schematic diagram of a lithium metal battery according to an embodiment.

[0035] Figure 8 is a schematic diagram of a lithium metal battery according to another embodiment.

[0036] Figure 9 is a schematic diagram of a lithium metal battery according to another embodiment.

[0037] <Brief explanation of drawing symbols>

[0038] 1 Lithium metal battery 2, 20 cathode

[0039] 3, 10 anode 4 separator

[0040] 5 Battery case 6 Cap assembly

[0041] 7 Battery structure 8 Electrode tab

[0042] The present inventive concept described below is capable of various modifications and embodiments. Specific embodiments are illustrated in the drawings and described in detail. However, this is not intended to limit the present inventive concept to specific embodiments, but rather to encompass all modifications, equivalents, or alternatives within the technical scope of the present inventive concept.

[0043] The terminology used below is only used to describe specific embodiments and is not intended to limit the present invention. The singular expression includes the plural expression unless the context clearly indicates otherwise. Hereinafter, the terms "comprises" or "has" and the like are intended to indicate the presence of a feature, number, step, operation, component, part, ingredient, material, or combination thereof described in the specification, but should be understood to not preclude the possibility of the presence or addition of one or more other features, numbers, steps, operations, components, parts, ingredients, materials, or combinations thereof. The " / " used below may be interpreted as "and" or "or" depending on the context.

[0044] In order to clearly express various layers and regions in the drawings, the thickness is shown enlarged or reduced. Similar parts are designated by the same drawing reference numerals throughout the specification. When a part such as a layer, film, region, or plate is said to be "on" or "above" another part throughout the specification, this includes not only cases where it is directly above the other part, but also cases where there is another part in between. Terms such as first, second, etc. may be used throughout the specification to describe various components, but the components should not be limited by the terms. The terms are used only for the purpose of distinguishing one component from another. In this specification and the drawings, components having substantially the same functional configuration are referred to by the same reference numerals, and redundant descriptions are omitted.

[0045] In the present disclosure, the "particle diameter" of a particle refers to the average diameter when the particle is spherical, and refers to the average major axis length when the particle is non-spherical. The particle diameter of a particle can be measured using a particle size analyzer (PSA). The "particle diameter" of a particle is, for example, the average particle diameter. The average particle diameter is, for example, the median particle diameter (D50). The median particle diameter (D50) is the size of a particle corresponding to 50% of the cumulative volume, calculated from the side of particles having a small particle size in a size distribution of particles measured by, for example, laser diffraction. The average particle diameter and average major axis length of a particle can be measured using a scanning electron microscope. When the particle size is measured using a scanning electron microscope, it is determined as the average value of 30 or more randomly selected particles having a size of 1 μm or more, excluding fine particles.

[0046] In this disclosure, “metal” includes both metals and metalloids such as silicon and germanium, in their elemental or ionic states.

[0047] In this disclosure, “alloy” means a mixture of two or more metals.

[0048] In the present disclosure, “positive electrode material” means a positive electrode material capable of undergoing lithiation and delithiation.

[0049] In the present disclosure, “negative electrode active material” means a negative electrode material capable of undergoing lithiation and delithiation.

[0050] In the present disclosure, “lithiation” and “lithiating” mean a process of adding lithium to a positive electrode active material or a negative electrode active material.

[0051] In the present disclosure, “delithiation” and “delithiate” mean a process of removing lithium from a positive electrode active material or a negative electrode active material.

[0052] In this disclosure, “charging” and “charging” mean a process of providing electrochemical energy to a battery.

[0053] In this disclosure, “discharging” and “discharging” mean the process of removing electrochemical energy from a battery.

[0054] In the present disclosure, “positive electrode” and “cathode” mean an electrode at which electrochemical reduction and lithiation occur during a discharge process.

[0055] In the present disclosure, “cathode” and “anode” mean electrodes where electrochemical oxidation and delithiation occur during a discharge process.

[0056]

[0057] Hereinafter, a negative electrode for a lithium metal battery, a lithium metal battery including the same, and a method for manufacturing the negative electrode for a lithium metal battery according to exemplary embodiments are described in more detail.

[0058] A non-cathode lithium metal battery is a battery that uses only a cathode current collector without a cathode active material layer. When charging, lithium ions transferred from the cathode are deposited on the surface of the cathode current collector, and when discharging, the lithium deposited on the cathode current collector is eluted again and inserted into the cathode, thereby operating the battery.

[0059] Non-cathode lithium metal batteries offer the advantage of maximizing energy density per volume / weight of the battery by omitting lithium metal as the anode active material. However, lithium metal precipitates during operation, and the uneven current concentration during oxidation / reduction causes lithium dendrites to grow. These dendrites not only cause lithium anode loss, reducing battery capacity and lifespan, but can also cause short-circuiting between the anode and cathode, posing safety concerns.

[0060] To solve the above-mentioned problem, a method was proposed to introduce a protective layer on top of the negative electrode current collector in a way that minimizes contact between lithium and electrolyte, thereby reducing side reactions, thereby minimizing exposure of the electrolyte on the electrode surface and creating a uniform flow of lithium ions throughout the electrode, thereby suppressing lithium dendrite growth.

[0061] A lithium metal battery according to an embodiment comprises: a negative electrode current collector; and on the negative electrode current collector;

[0062] A negative electrode for a lithium metal battery is provided, which includes a disposed protective layer, and includes a negative electrode active material layer disposed between the negative electrode current collector and the protective layer, or the negative electrode active material layer is absent (free), and the protective layer includes a first polymer containing a hydroxyl group, and i) boric acid (H3BO3); or ii) a hydrate of boron oxide (B2O3) and water; or a combination thereof.

[0063] A lithium electrodeposition induction layer may be further included between the negative electrode current collector and the protective layer.

[0064] there is.

[0065] A protective layer comprising a first polymer containing a hydroxyl group and i) boric acid (H3BO3); or ii) a hydrate of boron oxide (B2O3) and water; or a combination thereof is densely packed, thereby increasing density and strength, allowing free movement of lithium ions and enhancing lithium ion transport, thereby improving lithium electrodeposition characteristics. As a result, ion conductivity is improved, thereby improving the high-rate characteristics of a lithium metal battery. In addition, by disposing the above-described protective layer on the negative electrode active material layer, side reactions between the negative electrode active material layer and the electrolyte can be effectively blocked and suppressed.

[0066] Referring to Fig. 1a, when forming a protective layer, a hydrogen bond is formed between the first polymer containing a hydroxyl group and an additive including i) a hydrate of boric acid (H3BO3), ii) boron oxide (B2O3) and water, or a combination thereof.

[0067] When a general cross-linking agent is added to the protective layer, the cross-linking reaction product provides a protective layer with improved physical properties, but lithium ion movement may be partially hindered, which may reduce the ionic conductivity of the protective layer.

[0068] However, in the protective layer according to the present invention, the physical properties of the protective layer are effectively improved without reducing the ionic conductivity of the protective layer as the first polymer containing a hydroxyl group and the second polymer are crosslinked.

[0069] When the protective layer is formed by crosslinking the first polymer containing a hydroxyl group and the second polymer to form a crosslinked polymer, some of the first polymer containing a hydroxyl group remains, and the hydroxyl groups of the first polymer form hydrogen bonds with an additive such as boric acid. The mixing ratio of the first polymer and the second polymer can be adjusted so that some of the first polymer containing a hydroxyl group can remain. The mixing weight ratio of the first polymer containing a hydroxyl group and the second polymer is adjusted to be in the range of 50:50 to 99:1, 50:50 to 90:10, or 60:40 to 90:10.

[0070] As shown in Fig. 1b, when a boric acid-containing protective layer is laminated on a copper foil, which is a negative electrode collector, the lithium ion transfer capability can be improved.

[0071] When a protective layer according to an embodiment of the present invention is present on the surface of a negative electrode active material layer including lithium metal, the generation and / or growth of lithium dendrites on the negative electrode current collector can be effectively prevented. In addition, the cycle characteristics and stability of a negative electrode including the above-described protective layer and a lithium metal battery employing the same are improved.

[0072] The above hydroxyl group-containing first polymer is carboxymethyl cellulose (CMC); polyvinyl alcohol (PVA); Vinyl acetate, butyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 2-hydroxyethylene glycol (meth)acrylate, 2-hydroxypropylene glycol (meth)acrylate, acrylic acid, methacrylic acid, 2-(meth)acryloyloxy acetic acid, 3-(meth)acryloyloxy propyl acid, 4-(meth)acryloyloxy butyric acid, itaconic acid, maleic acid, 2-isocyanatoethyl (meth)acrylate, 3-isocyanatopropyl (meth)acrylate, A polymerization reaction product of one or more monomers selected from among 4-isocyanatobutyl (meth)acrylate, (meth)acrylamide, ethylene di(meth)acrylate, diethylene glycol (meth)acrylate, triethylene glycol di(meth)acrylate, trimethylene propane tri(meth)acrylate, trimethylene propane triacrylate, 1,3-butanediol (meth)acrylate, 1,6-hexanediol di(meth)acrylate, allyl acrylate, and N-vinyl caprolactam, a hydrolyzate thereof, or a combination thereof may be mentioned.

[0073] The first polymer may be polyvinyl alcohol (PVA). For example, polyvinyl alcohol may be a hydrolyzate obtained by hydrolyzing polyvinyl acetate with an alkali.

[0074] The degree of saponification of polyvinyl alcohol is 60 to 99%, 70 to 95%, 75 to 90% or 80

[0075] The degree of saponification of polyvinyl alcohol can be 85 to 90%. For example, the degree of saponification of polyvinyl alcohol can be 85 to 90%.

[0076] There is. The properties can be further improved by the protective layer within the above saponification range.

[0077] The weight average molecular weight of the first polymer may be 10,000 to 500,000 Dalton, 10,000 to 500,000 Dalton, 10,000 to 400,000 Dalton, 10,000 to 300,000 Dalton, 10,000 to 200,000 Dalton, 50,000 to 150,000 Dalton, 70,000 to 100,000 Dalton, or 80,000 to 100,000 Dalton. The physical properties of the protective layer may be further improved within the weight average molecular weight range of the first polymer.

[0078] The protective layer may further include a second polymer having a functional group capable of crosslinking with the first polymer containing a hydroxyl group. In this case, the protective layer further includes a crosslinked polymer of the first polymer and the second polymer.

[0079] In the above protective layer, the additives i) boric acid (H3BO3) or ii) boron oxide (B2O3) and

[0080] The content of water hydrate is 5 wt% or less, 0.1 to 5 wt%, 0.1 to 3 wt%, or 0.1 to 2 wt% based on 100 wt% of the total weight of the protective layer. When the content of the additive is within the above range, the physical properties of the protective film, such as the elastic modulus, increase by 20% or more. If the content of the additive exceeds 5 wt%, crosslinking progresses too quickly, making it difficult to apply practically.

[0081] The second polymer includes at least one selected from a fluorinated polyamic acid having a carboxyl group and a fluorinated polyimide having a carboxyl group.

[0082] The above fluorinated polyamic acid may be, for example, a polymer represented by the following chemical formula 1 or 2, and the above fluorinated polyimide may be a polymer represented by the following chemical formula 3 or 4.

[0083] [Chemical Formula 1]

[0084]

[0085] [Chemical Formula 2]

[0086]

[0087] [Chemical Formula 3]

[0088]

[0089] [Chemical Formula 4]

[0090]

[0091] In the above formulas, M is an alkali metal,

[0092] Ar1 and Ar3 are independently an aromatic ring group selected from a substituted or unsubstituted tetravalent arylene group having 6 to 24 carbon atoms or a substituted or unsubstituted tetravalent heteroarylene group having 4 to 24 carbon atoms, wherein the aromatic ring group is one aromatic ring, a fused ring of two or more aromatic rings, or a ring of two or more aromatic rings connected by a single bond, -O-, -S-, -C(=O)-, -S(=O)2-, -Si(Ra)(Rb)- (Ra and Rb are each independently an alkyl group having 1 to 10 carbon atoms), a substituted or unsubstituted alkylene group having 1 to 10 carbon atoms, or -C(=O)-NH-.

[0093] Ar2 and Ar4 are independently an aromatic ring group selected from a substituted or unsubstituted divalent arylene group having 6 to 24 carbon atoms or a substituted or unsubstituted divalent heteroarylene group having 4 to 24 carbon atoms, wherein the aromatic ring group is a ring connected by one aromatic ring, a fused ring of two or more aromatic rings, a single bond, -O-, -S-, -C(=O)-, -S(=O)2-, -Si(Ra)(Rb)- (Ra and Rb are independently an alkyl group having 1 to 10 carbon atoms), a substituted or unsubstituted alkylene group having 1 to 10 carbon atoms, or -C(=O)-NH-.

[0094] At least one of Ar1 to Ar4 is substituted with a halogen group,

[0095] X1 is the first functional group, which is -COOH, -OH, -CO-NH2, or -COH,

[0096] n and m are the mole fractions within the repeating unit, respectively, and 0 <n≤1, 0≤m<1, n+m=1이다.

[0097] The halogen group may be a fluorine group, a chlorine group, a bromine group, or an iodine group. For example, the halogen group may be a fluorine group.

[0098] Here, Ar1 and Ar3 are independently selected from the following chemical formulae 1a and 1b, and Ar2 and Ar4 can be independently selected from the following chemical formulae 1c to 1e.

[0099] there is.

[0100] [Chemical Formula 1a]

[0101]

[0102] [Chemical Formula 1b]

[0103]

[0104] [Chemical Formula 1c]

[0105]

[0106] [Chemical Formula 1d]

[0107]

[0108] [Chemical Formula 1e]

[0109]

[0110] In the above formulas, R1, R2, R3, R4, R5, R6, R7, R8, R9, R 10 , R 11 , R 12 , R 13 , R 14 , R 15 and R 16 are each independently hydrogen, halogen, -COOH, -OH, -CO-NH2, -COH, a halogen-substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, a halogen-substituted or unsubstituted aryl group having 6 to 20 carbon atoms, or a halogen-substituted or unsubstituted heteroaryl group having 2 to 20 carbon atoms; provided that R1 to R 16At least one of the groups is a halogen group or a group substituted with a halogen group, and the group substituted with a halogen is, for example, a C1-C10 alkyl group substituted with a halogen, or a C6-C20 aryl group; A1, A2 and A3 are each independently a single bond, -O-, -C(=O)-, -S-, -S(=O)2-, -Si(Ra)(Rb)- (Ra and Rb are each independently an alkyl group having 1 to 10 carbon atoms), an alkylene group having 1 to 10 carbon atoms substituted or unsubstituted with a halogen, or -C(=O)-NH-; provided that the above chemical formulas 1c to 1e, which become Ar2, are R5 to R 16 At least one of the first functional groups is -COOH, -OH, -CO-NH2, or -COH.

[0111] For example, in the above chemical formulas 1a to 1e, R1 to R 16 are each independently a hydrogen atom, a halogen atom, a hydroxyl group, -CH3, or -CF3, provided that the above chemical formulas 1c to 1e, which become Ar2, are R5 to R 16 At least one of the first functional groups is -COOH, -OH, -CO-NH2, or -COH; A2 and A3 can each independently be a single bond, -O-, -CO-, -S-, -SO2-, -C(CH3)2-, -CONH-, -C(CF3)2-, -CH2-, or -CF2-.

[0112] The above polyamic acid may be, for example, a polymer represented by the following chemical formula 5 or 6, and the above polyimide may be a polymer represented by the following chemical formula 7 or 8.

[0113] [Chemical Formula 5]

[0114]

[0115] [Chemical Formula 6]

[0116]

[0117] [Chemical Formula 7]

[0118]

[0119] [Chemical Formula 8]

[0120]

[0121] In the above formulas, M is lithium or sodium,

[0122] R1, R2, R3, R4, R5, R6, R7, R8, R9, R 10 , R 11 , and R 12 are independently hydrogen, halogen, -COOH, -OH, -CO-NH2, -COH, an alkyl group having 1 to 10 carbon atoms substituted or unsubstituted with a halogen, an aryl group having 6 to 20 carbon atoms substituted or unsubstituted with a halogen, or a heteroaryl group having 2 to 20 carbon atoms substituted or unsubstituted with a halogen, provided that R1 to R 12 At least one of which is a halogen group or a group substituted with a halogen group,

[0123] A1 and A2 are each independently a single bond, -O-, -S-, -C(=O)-, -S(=O)2-, -Si(Ra)(Rb)- (Ra and Rb are each independently an alkyl group having 1 to 10 carbon atoms), an alkylene group having 1 to 10 carbon atoms which is unsubstituted or substituted with halogen, or -C(=O)-NH-;

[0124] However, at least one of R5, R6, R7, and R8 is -COOH, -OH, -CO-NH2, or -COH, and n and m are each a mole fraction within the repeating unit, 0 <n≤1, 0≤m<1, n+m=1이다.

[0125] The halogen group may be a fluorine group, a chlorine group, a bromine group, or an iodine group. For example, the halogen group may be a fluorine group. Here, Ar1 and Ar3 may be independently selected from the chemical formulae 1a and 1b, and Ar2 and Ar4 may be independently selected from the chemical formulae 1c to 1e.

[0126] The above polyamic acid is represented by the following chemical formula 9 or 10, and the above polyimide is a polymer represented by the following chemical formula 11 or 12.

[0127] [Chemical Formula 9]

[0128]

[0129] [Chemical Formula 10]

[0130]

[0131] [Chemical Formula 11]

[0132]

[0133] [Chemical Formula 12]

[0134]

[0135] In the above equations, n and m are the mole fractions within the repeating unit, respectively, and 0 <n≤1, 0≤m<1,

[0136] n+m=1.

[0137] For example, in the second polymer, a repeating unit including a crosslinking group and a crosslinking group

[0138] The mole fraction of repeating units that do not contain each other is 0 <n≤0.5, 0.5≤m<1 및 n+m=1일 수 있다. 예를 들어, 상기 제2 고분자에서 가교기를 포함하는 반복단위와 가교기를 포함하지 않는 반복단위의 몰분율이 각각 0.1≤n≤0.4, 0.6≤m≤0.9 및 n+m=1일 수 있다. 예를 들어, 상기 제2 고분자에서 가교기를 포함하는 반복단위와 가교기를 포함하지 않는 반복단위의 몰분율이 각각 0.15≤n≤0.35, 0.65≤m≤0.85 및 n+m=1일 수 있다. 예를 들어, 상기 제2 고분자에서 가교기를 포함하는 반복단위와 가교기를 포함하지 않는 반복단위의 몰분율이 각각 0.2≤n≤0.3, 0.7≤m≤0.8 및 n+m=1일 수 있다. 상기 몰분율 범위에서 더욱 향상된 물성을 제공할 수 있다.

[0139] For example, the second polymer may be a random copolymer. For example, the above

[0140] The second polymer may be a block copolymer.

[0141] The weight average molecular weight of the second polymer may be 10,000 to 1,200,000 Dalton, 10,000 to 1,100,000 Dalton, 10,000 to 1,000,000 Dalton, 10,000 to 500,000 Dalton, 100,000 to 500,000 Dalton, 100,000 to 400,000 Dalton, for example, 100,000 to 300,000 Dalton. The physical properties of the protective layer may be further improved within the weight average molecular weight range of the first polymer.

[0142] In the above protective layer, the weight ratio of the first polymer and the second polymer containing a hydroxyl group included in the third polymer may be 99:1 to 50:50, 95:5 to 55:45, 95:5 to 60:40, 95:5 to 65:35, or 90:10 to 70:30. In the above range of the weight ratio of the first polymer to the second polymer, the physical properties of the protective layer may be further improved.

[0143] The hydroxyl groups of the first polymer and the carboxyl groups of the second polymer react with each other to form an ester bond, thereby forming a third polymer crosslinked with the first and second polymers. The formation of the third polymer enhances the stability of the protective layer, and in the case of halogen groups such as fluorine functional groups, it can improve interfacial stability by reducing the formation of irreversible lithium inclusions.

[0144] The protective layer according to an embodiment includes a crosslinked polymer of polyvinyl alcohol and polyamic acid. The polyamic acid is, for example, a polymer represented by the chemical formula 9 or 10 described above.

[0145] In another embodiment, the crosslinked polymer of the protective layer is a crosslinked polymer of polyvinyl alcohol and fluorinated polyimide (PVA / PI-f). The fluorinated polyimide is a polymer represented by the chemical formula 11 or 12 described above.

[0146] The protective layer may further include a lithium salt. The lithium salt may include one or more of materials such as LiSCN, LiN(CN)2, LiClO4, LiBF4, LiAsF6, LiPF6, LiCF3SO3, LiC(CF3SO2)3, LiC(FSO2)3, LiN(SO2C2F5)2, LiN(SO2CF3)2, LiN(SO2F)2, LiSbF6, LiPF3(CF2CF3)3, LiPF3(CF3)3, and LiB(C2O4)2.

[0147] In the negative electrode according to an embodiment, the negative electrode active material layer includes lithium metal foil, lithium metal powder, lithium alloy foil, lithium alloy powder, or a combination thereof, wherein the lithium alloy contains lithium and a first metal.

[0148] The above negative active material layer is a carbon-based compound; a carbon-based material; and a first metal.

[0149] A composition comprising one or more selected mixtures; one or more composites selected from a carbonaceous material and a first metal; or a combination thereof, wherein the carbonaceous material comprises amorphous carbon, and the average particle size of the amorphous carbon is from 10 nm to 100 nm. The carbonaceous material comprises carbon black, carbon nanotubes, carbon nanofibers, fullerenes, activated carbon, carbon fibers, or a combination thereof.

[0150] The first metal is indium (In), silicon (Si), gallium (Ga), tin (Sn), aluminum (Al), titanium (Ti), zirconium (Zr), niobium (Nb), germanium (Ge), antimony (Sb), bismuth (Bi), gold (Au), platinum (Pt), palladium (Pd), magnesium (Mg), silver (Ag), zinc (Zn), nickel, iron, cobalt, chromium, cesium, sodium, potassium, calcium, yttrium, bismuth, tantalum, hafnium, barium, vanadium, strontium, lanthanum, or a combination thereof.

[0151] A lithium metal layer (e.g., a first lithium metal layer) may be further disposed between the negative electrode current collector and one surface of the protective layer. A lithium metal layer (e.g., a second lithium metal layer) may be further disposed on the other surface of the protective layer opposite to the one surface of the protective layer (i.e., the opposite surface of the protective layer). That is, the lithium metal layer may be a surface of the protective layer that is not adjacent to the negative electrode active material layer.

[0152] The thickness of the protective layer is 1 to 10 μm, 2 to 8 μm, or 3 to 5 μm.

[0153] When the thickness of the protective layer is within the above range, the internal resistance increases, and the energy density of the lithium battery is improved without decreasing, and the high-rate characteristics and life characteristics are improved.

[0154] According to another aspect, the positive electrode; the negative electrode according to an embodiment; and the positive electrode and the negative electrode

[0155] A lithium metal battery including an electrolyte disposed therebetween is provided.

[0156] The electrolyte may be a liquid electrolyte, a solid electrolyte, a gel electrolyte, or a combination thereof. The electrolyte may be, for example, an organic electrolyte. An organic electrolyte is prepared, for example, by dissolving a lithium salt in an organic solvent.

[0157] The above solid electrolyte includes an oxide-based solid electrolyte, a sulfide-based solid electrolyte, a polymer solid electrolyte, or a combination thereof. A gel electrolyte may have a gel state, for example, without including a polymer.

[0158] The above gel electrolyte comprises a polymer gel electrolyte. The positive electrode comprises a positive electrode current collector and a positive electrode active material layer, and at least one of the positive electrode current collector and the negative electrode current collector comprises a base film and a metal layer disposed on one or both sides of the base film, and the base film comprises a polymer, and the polymer comprises polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof.

[0159] The above metal layer includes indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof.

[0160] Referring to FIG. 2, a lithium metal battery (1) has a negative electrode (20) including a negative electrode current collector (21), and the negative electrode active material layer is absent.

[0161] A protective layer (22) is formed between the negative electrode current collector (21) and the electrolyte (30).

[0162] A positive electrode (10) is sequentially arranged on top of the above electrolyte (30). The positive electrode (10) contains a positive electrode active material layer (12) and a positive electrode current collector (11).

[0163] A negative electrode active material layer may be further disposed between the negative electrode current collector (21) and the protective layer (22). The negative electrode active material layer may include lithium metal or a lithium alloy.

[0164] The lithium metal may include, for example, a lithium metal foil, a lithium alloy foil, or a combination thereof. The lithium metal may be in powder form (or particle form). The lithium powder (or lithium particle) may include a lithium metal powder, a lithium alloy powder, or a combination thereof. A lithium alloy is an alloy of lithium and another metal that can be alloyed with lithium, such as a lithium-silver alloy, a lithium-zinc alloy, a lithium-magnesium alloy, or a lithium-tin alloy. The negative electrode active material layer including a lithium metal foil may be, for example, a lithium metal layer. The negative electrode active material layer including a lithium alloy foil may be, for example, a lithium alloy layer. The negative electrode active material layer including a lithium metal powder and / or a lithium alloy powder may be introduced by coating a slurry including lithium powder and a binder onto a negative electrode current collector. The binder may be, for example, a fluorine-based binder such as polyvinylidene fluoride (PVDF). The negative electrode active material layer may not include a carbon-based negative electrode active material. Therefore, the negative electrode active material layer can be made of a metal-based negative electrode active material.

[0165] The thickness of the lithium metal may be, for example, 1 μm to 50 μm, 1 μm to 30 μm, or 10 μm to 30 μm, or 10 μm to 80 μm. When the lithium metal has a thickness in this range, the life characteristics of the lithium battery including the protective layer can be further improved. The particle size of the lithium powder may be, for example, 0.1 μm to 3 μm, 0.1 μm to 2 μm, or 0.1 μm to 2 μm. When the lithium powder has a thickness in this range, the life characteristics of the lithium battery including the protective layer can be further improved.

[0166] The thickness of the negative electrode active material layer is, for example, 0.1 ㎛ to 500 ㎛, 1 ㎛ to 500 ㎛, or 10 ㎛ to 500 ㎛, but is not necessarily limited to this range and can be adjusted according to the shape, capacity, etc. of the required lithium metal battery. When the thickness of the negative electrode active material layer is within the above range, the cycle characteristics are improved without lowering the energy density of the lithium metal battery.

[0167] A lithium metal battery according to one embodiment does not include a negative electrode active material layer disposed between a negative electrode current collector (21) and a protective layer (22). An anode not including a negative electrode active material layer may include a negative electrode active material layer by plating lithium metal between a negative electrode current collector (21) and a protective layer (22) upon charging after being introduced into a lithium battery together with a positive electrode and an electrolyte. The negative electrode active material layer may be a lithium plating layer (plated lithium layer).

[0168] Lithium metal batteries may further include a separator.

[0169] The pore diameter of the separator is generally 0.01 to 10 μm, and the thickness can generally be 5 to 20 μm. Examples of such separators include sheets or non-woven fabrics made of olefin-based polymers such as polypropylene, glass fiber, or polyethylene. When a solid polymer electrolyte is used as the electrolyte, the solid polymer electrolyte may also function as the separator.

[0170] Among the above separation membranes, specific examples of olefin-based polymers include polyethylene, polypropylene, or a multilayer membrane of two or more layers thereof, and mixed multilayer membranes such as a polyethylene / polypropylene two-layer separation membrane, a polyethylene / polypropylene / polyethylene three-layer separation membrane, and a polypropylene / polyethylene / polypropylene three-layer separation membrane may be used.

[0171] In a lithium metal battery according to an embodiment, the liquid electrolyte contains a lithium salt and an organic solvent.

[0172] As the organic solvent, for example, an aprotic organic solvent such as N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma-butyrolactone, 1,2-dimethoxyethane, tetrahydroxy franc, 2-methyl tetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, triester phosphate, trimethoxy methane, dioxolane derivatives, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl pyrropionate, ethyl propionate, etc. can be used. Carbonate solvents such as propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, and diethyl carbonate can be used.

[0173] The above lithium salt can be any one that is commonly used in lithium secondary batteries, and as a material that is easily dissolved in the non-aqueous solvent, for example, one or more of the following materials can be used: LiSCN, LiN(CN)2, LiClO4, LiBF4, LiAsF6, LiPF6, LiCF3SO3, LiC(CF3SO2)3, LiC(FSO2)3, LiN(SO2C2F5)2, LiN(SO2CF3)2, LiN(SO2F)2, LiSbF6, LiPF3(CF2CF3)3, LiPF3(CF3)3, and LiB(C2O4)2.

[0174] The concentration of the lithium salt may be, for example, 1 to 5 M, for example, 1 to 2.5 M, in the liquid electrolyte. In the above range, a sufficient amount of lithium ions required for charging and discharging a lithium metal battery can be generated.

[0175] When a gel-type polymer electrolyte exists in the pores of a porous substrate, the interfacial resistance between the positive electrode, negative electrode, and separator is minimized, and lithium movement becomes easier.

[0176] According to one embodiment, the negative electrode active material layer may be disposed during the assembly of the lithium metal battery. According to another embodiment, the negative electrode active material layer may include a negative electrode active material layer by plating lithium metal after charging. The negative electrode active material layer may be a plated lithium layer.

[0177] The above negative electrode active material layer includes lithium metal or a lithium alloy.

[0178] When the negative electrode active material layer is placed at the time of assembly, it may include only a carbon-based material, a carbon-based material, and at least one selected from metals and metalloids.

[0179] The carbon-based material includes amorphous carbon, and the average particle diameter of the amorphous carbon is 10 nm to 100 nm, and the carbon-based material includes carbon black (CB), acetylene black (AB), furnace black (FB), ketjen black (KB), graphene, or a combination thereof.

[0180] The above negative active material layer includes a lithium metal foil, a lithium metal powder, a lithium alloy foil, a lithium alloy powder, or a combination thereof, wherein the lithium alloy contains lithium and a first metal.

[0181] The first metal is indium (In), silicon (Si), gallium (Ga), tin (Sn), aluminum (Al), titanium (Ti), zirconium (Zr), niobium (Nb), germanium (Ge), antimony (Sb), bismuth (Bi), gold (Au), platinum (Pt), palladium (Pd), magnesium (Mg), silver (Ag), zinc (Zn), nickel, iron, cobalt, chromium, cesium, sodium, potassium, calcium, yttrium, bismuth, tantalum, hafnium, barium, vanadium, strontium, lanthanum, or a combination thereof.

[0182] The negative electrode active material layer (22) may include, for example, lithium foil, lithium powder, or a combination thereof. The lithium foil may include, for example, lithium metal foil, lithium alloy foil, or a combination thereof. The lithium powder may include lithium metal powder, lithium alloy powder, or a combination thereof. A lithium alloy is an alloy of lithium and another metal that can be alloyed with lithium, such as a lithium-silver alloy, a lithium-zinc alloy, a lithium-magnesium alloy, or a lithium-tin alloy. The negative electrode active material layer including a lithium metal foil may be, for example, a lithium metal layer. The negative electrode active material layer including a lithium alloy foil may be, for example, a lithium alloy layer. The negative electrode active material layer including a lithium metal powder and / or a lithium alloy powder may be introduced by coating a slurry including lithium powder and a binder, etc., on a negative electrode current collector. The binder may be, for example, a fluorine-based binder such as polyvinylidene fluoride (PVDF). The negative electrode active material layer may not include a carbon-based negative electrode active material. Therefore, the negative electrode active material layer can be made of a metal-based negative electrode active material.

[0183] The negative electrode current collector is composed of a material that does not react with lithium, i.e., does not form an alloy or compound. The material constituting the negative electrode current collector includes, but is not limited to, copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), and nickel (Ni), and any material that is used as an electrode current collector in the relevant technical field may be used. The negative electrode current collector may be composed of one of the above-mentioned metals, or may be composed of an alloy or a coating material of two or more metals. The negative electrode current collector is, for example, in the form of a plate or foil.

[0184] In one embodiment of the present invention, the positive electrode collector uses a plate or foil made of, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. The thickness of the positive electrode collector is, for example, 1 µm to 100 µm, 1 µm to 50 µm, 5 µm to 25 µm, or 10 µm to 20 µm.

[0185] The negative electrode active material layer may contain a negative electrode active material and a binder.

[0186] The negative active material has, for example, a particle form. The average particle diameter of the negative active material having a particle form is, for example, 10 nm to 4 ㎛, 10 nm to 1 ㎛, 10 nm to 500 nm, 10 nm to 100 nm, or 20 nm to 80 nm. When the negative active material has an average particle diameter in this range, reversible plating and / or dissolution of lithium can be facilitated during charge and discharge. The average particle diameter of the negative active material is, for example, a median diameter (D50) measured using a laser particle size distribution analyzer.

[0187] The negative electrode active material may include, for example, at least one selected from a carbon-based negative electrode active material and a metal or metalloid negative electrode active material. The carbon-based negative electrode active material may be, for example, amorphous carbon. Examples of the carbon-based negative electrode active material include, but are not limited to, carbon black (CB), acetylene black (AB), furnace black (FB), ketjen black (KB), graphene, etc., and any material classified as amorphous carbon in the relevant technical field may be used. Amorphous carbon is carbon that has no crystallinity or very low crystallinity, and is distinguished from crystalline carbon or graphite-based carbon. The metal or metalloid negative electrode active material includes, but is not limited to, one or more selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn), and any metal or metalloid negative electrode active material that forms an alloy or compound with lithium in the relevant technical field may be used. For example, nickel (Ni) does not form an alloy with lithium, and therefore is not a metal negative electrode active material in the present specification. The negative electrode active material layer includes a type of negative electrode active material among these negative electrode active materials, or includes a mixture of a plurality of different negative electrode active materials. For example, the negative electrode active material layer may include a mixture of amorphous carbon and one or more selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). The mixing ratio of the mixture may be, for example, 10:1 to 1:2, 10:1 to 1:1, 7:1 to 1:1, 5:1 to 1:1, or 4:1 to 2:1 by weight.The negative electrode active material included in the negative electrode active material layer may include a mixture of first particles made of, for example, amorphous carbon and second particles made of a metal or a metalloid. The metal includes, for example, gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). The content of the second particles is 8 to 60 wt%, 10 to 50 wt%, 15 to 40 wt%, or 20 to 30 wt% based on the total weight of the mixture. When the second particles have a content in this range, the cycle characteristics of, for example, a lithium metal battery are further improved.

[0188] The binder included in the negative electrode active material layer may be, for example, styrene-butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, vinylidene fluoride / hexafluoropropylene copolymer, polyacrylonitrile, polymethyl methacrylate, etc., but is not necessarily limited thereto, and any binder used in the relevant technical field may be used. The binder may be composed of a single binder or a plurality of different binders. When the negative electrode active material layer does not include a binder, the negative electrode active material layer can be easily separated from the ceramic coating layer (21) or the negative electrode current collector (21). The content of the binder included in the negative electrode active material layer may be, for example, 1 to 20 wt% based on the total weight of the negative electrode active material layer.

[0189] The thickness of the negative electrode active material layer may be, for example, 0.1 ㎛ to 500 ㎛, or 100 ㎛ to 50 ㎛. The thickness of the negative electrode active material layer may be, for example, 1% to 50%, 1% to 30%, 1% to 10%, or 1% to 5% of the thickness of the positive electrode active material layer. If the thickness of the negative electrode active material layer is too thin, lithium dendrites formed between the negative electrode active material layer and the negative electrode current collector may collapse the negative electrode active material layer, making it difficult to improve the cycle characteristics of the lithium metal battery. If the thickness of the negative electrode active material layer increases excessively, the energy density of the lithium metal battery employing the negative electrode (20) may decrease, and it may be difficult to improve the cycle characteristics.

[0190] When the thickness of the negative electrode active material layer decreases, the charge capacity of the negative electrode active material layer also decreases, for example. The charge capacity of the negative electrode active material layer may be, for example, 0.1% to 50%, 1% to 30%, 1% to 10%, 1% to 5%, or 1% to 2% of the charge capacity. If the charge capacity of the negative electrode active material layer is too small, lithium dendrites formed between the negative electrode active material layer and the negative electrode current collector may collapse the negative electrode active material layer, making it difficult to improve the cycle characteristics of the lithium metal battery. If the charge capacity of the negative electrode active material layer increases excessively, the energy density of the lithium metal battery using the negative electrode (20) may decrease, and it may be difficult to improve the cycle characteristics. The charge capacity of the positive electrode active material layer is obtained by multiplying the charge capacity density (mAh / g) of the positive electrode active material by the mass of the positive electrode active material in the positive electrode active material layer. When multiple types of positive electrode active materials are used, the charge capacity density × mass value is calculated for each positive electrode active material, and the sum of these values ​​is the charge capacity of the positive electrode active material layer. The charge capacity of the negative electrode active material layer is also calculated in the same way. That is, the charge capacity of the negative electrode active material layer is obtained by multiplying the charge capacity density (mAh / g) of the negative electrode active material by the mass of the negative electrode active material in the negative electrode active material layer. When multiple types of negative electrode active materials are used, the charge capacity density × mass value is calculated for each negative electrode active material, and the sum of these values ​​is the capacity of the negative electrode active material layer. Here, the charge capacity density of the positive electrode active material and the negative electrode active material is the estimated capacity using an all-solid-state half-cell using lithium metal as a counter electrode. The charge capacity of the positive electrode active material layer and the negative electrode active material layer are directly measured by measuring the charge capacity using an all-solid-state half-cell. The charge capacity density is obtained by dividing the measured charge capacity by the mass of each active material. Alternatively, the charge capacity of the positive electrode active material layer and the negative electrode active material layer may be the initial charge capacity measured at the first charge cycle.

[0191] [Lithium metal battery]

[0192] According to one embodiment, a lithium metal battery includes a positive electrode; a negative electrode; and an electrolyte disposed between the positive electrode and the negative electrode. The lithium metal battery may further include a separator. Such a lithium metal battery can simultaneously provide excellent lifespan characteristics. The lithium metal battery may be, but is not limited to, a lithium primary battery, a lithium secondary battery, a lithium-sulfur battery, a lithium-air battery, etc., and any lithium metal battery used in the art may be used.

[0193] Lithium metal batteries are manufactured by, for example, the following exemplary methods, but are not necessarily limited to these methods and are adjusted according to required conditions.

[0194] (anode)

[0195] First, a positive electrode active material composition is prepared by mixing a positive electrode active material, a conductive agent, a binder, and a solvent. The prepared positive electrode active material composition is directly coated and dried on an aluminum current collector to produce a positive electrode plate having a positive electrode active material layer formed thereon. Alternatively, the positive electrode active material composition is cast on a separate support, and then the film obtained by peeling from the support is laminated on the aluminum current collector to produce a positive electrode plate having a positive electrode active material layer formed thereon.

[0196] The cathode active material is a lithium-containing metal oxide, and any one commonly used in the art can be used without limitation. For example, one or more types of composite oxides of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof can be used, and specific examples thereof include Li a A 1-b B b D2 (in the above formula, 0.90 ≤ a ≤ 1, and 0 ≤ b ≤ 0.5); Li a E 1-b B b O 2-c D c (In the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); LiE 2-b Bb O 4-c D c (In the above formula, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); Li a Ni 1-b-c Co b B c D α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Co b B c O 2-α F α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Co b B c O 2-α F2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B c D α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Mn b B c O 2-α F α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B c O 2-α F2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni b E c G dO2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0.001 ≤ d ≤ 0.1); Li a Ni b Co c Mn d GeO2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0 ≤ d ≤ 0.5, 0.001 ≤ e ≤ 0.1); Li a NiG b O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); Li a CoG b O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤

[0197] 0.1); Li a MnG b O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); Li a Mn2G b O4 (wherein 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiIO2; LiNiVO4; Li (3-f) J2(PO4)3(0 ≤ f ≤ 2); Li (3-f) A compound represented by any one of the chemical formulas Fe2(PO4)3(0 ≤ f ≤ 2); LiFePO4 can be used.

[0198] In the chemical formula representing the above-described compound, A is Ni, Co, Mn, or a combination thereof; B is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element, or a combination thereof; D is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; F is F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; Q is Ti, Mo, Mn, or a combination thereof; I is Cr, V, Fe, Sc, Y, or a combination thereof; J is V, Cr, Mn, Co, Ni, Cu, or a combination thereof. It is also possible to use a compound having a coating layer added to the surface of the above-described compound, or it is also possible to use a mixture of the above-described compound and the compound having a coating layer added. The coating layer added to the surface of the above-mentioned compound includes a coating element compound of, for example, an oxide, a hydroxide, an oxyhydroxide of the coating element, an oxycarbonate of the coating element, or a hydroxycarbonate of the coating element of the coating element. The compound forming the coating layer is amorphous or crystalline. The coating elements included in the coating layer are Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a mixture thereof. The method for forming the coating layer is selected within a range that does not adversely affect the physical properties of the positive electrode active material. The coating method includes, for example, spray coating and dipping. Since the specific coating method is well understood by those working in the relevant field, a detailed description thereof will be omitted.

[0199] The cathode active material is, for example, Li a Ni x Co y M z O 2-b A b(1.0≤a≤1.2, 0≤b≤0.2, 0.8≤x<1, 0 <y≤0.3, 0<z≤0.3, 및 x+y+z=1이고, M은 망간(Mn), 니오븀(Nb), 바나듐(V), 마그네슘(Mg), 갈륨(Ga), 실리콘(Si), 텅스텐(W), 몰리브덴(Mo), 철(Fe), 크롬(Cr), 구리(Cu), 아연(Zn), 티타늄(Ti), 알루미늄(Al), 보론(B) 또는 이들의 조합이고, A는 F, S, Cl, Br 또는 이들의 조합), LiNi x Co y Mn z O2(0.8≤x≤0.95, 0≤y≤0.2, 0 <z≤0.2 및 x+y+z=1), LiNi x Co y Al z O2(0.8≤x≤0.95, 0≤y≤0.2, 0 <z≤0.2 및 x+y+z=1), LiNi x Co y Mn z Al w O2(0.8≤x≤0.95, 0≤y≤0.2, 0 <z≤0.2, 0<w≤0.2, 및 x+y+z+w=1), Li a Co x M y O 2-b A b (1.0≤a≤1.2, 0≤b≤0.2, 0.9≤x≤1, 0≤y≤0.1, and x+y=1, M is manganese (Mn), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B) or a combination thereof, and A is F, S, Cl, Br or a combination thereof), Li a Ni x Mn y M' z O 2-b A b(1.0≤a≤1.2, 0≤b≤0.2, 0 <x≤0.3, 0.5≤y<1, 0<z≤0.3, 및 x+y+z=1이고, M'는 코발트(Co), 니오븀(Nb), 바나듐(V), 마그네슘(Mg), 갈륨(Ga), 실리콘(Si), 텅스텐(W), 몰리브덴(Mo), 철(Fe), 크롬(Cr), 구리(Cu), 아연(Zn), 티타늄(Ti), 알루미늄(Al), 보론(B) 또는 이들의 조합이고, A는 F, S, Cl, Br 또는 이들의 조합), Li a M1 x M2 y PO 4-b X b (Here, 0.90≤a≤1.1, 0≤x≤0.9, 0≤y≤0.5, 0.9 <x+y<1.1, 0≤b≤2 이며, M1이 크롬(Cr), 망간(Mn), 철(Fe), 코발트(Co), 니켈(Ni), 구리(Cu), 지르코늄(Zr) 또는 이들의 조합이며, M2가 마그네슘(Mg), 칼슘(Ca), 스트론튬(Sr), 바륨(Ba), 티탄(Ti), 아연(Zn), 보론(B), 니오븀(Nb), 갈륨(Ga), 인듐(In), 몰리브덴(Mo), 텅스텐(W), 알루미늄(Al), 실리콘(Si), 크롬(Cr), 바나듐(V), 스칸듐(Sc), 이트륨(Y) 또는 이들의 조합이며, X가 O, F, S, P 또는 이들의 조합), Li a M3 z PO4 (0.90≤a≤1.1, 0.9≤z≤1.1, and M3 is chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zirconium (Zr), or a combination thereof).

[0200] The conductive material may include, but is not limited to, carbon black, graphite particles, natural graphite, artificial graphite, acetylene black, Ketjen black, carbon fibers; carbon nanotubes; metal powders or metal fibers or metal tubes such as copper, nickel, aluminum, and silver; and conductive polymers such as polyphenylene derivatives. Any conductive material used in the relevant technical field may be used. Alternatively, the anode may not include a separate conductive material, for example.

[0201] As the binder, vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene (PTFE), mixtures of the above polymers, styrene butadiene rubber polymer, etc. are used, and as the solvent, N-methylpyrrolidone (NMP), acetone, water, etc. are used, but are not necessarily limited to these, and any solvent used in the relevant technical field may be used.

[0202] It is also possible to form pores inside the electrode plate by further adding a plasticizer or a pore forming agent to the positive electrode active material composition.

[0203] The contents of the cathode active material, conductive agent, binder, and solvent used in the cathode are at levels typically used in lithium batteries. Depending on the intended use and configuration of the lithium metal battery, one or more of the conductive agent, binder, and solvent may be omitted.

[0204] The binder content included in the positive electrode may be 0.1 wt% to 10 wt% or 0.1 wt% to 5 wt% of the total weight of the positive electrode active material layer. The positive electrode active material content included in the positive electrode may be 80 wt% to 99 wt%, 90 wt% to 99 wt% or 95 wt% to 99 wt% of the total weight of the positive electrode active material layer.

[0205] The positive electrode collector uses a plate or foil made of, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. The thickness of the positive electrode collector is, for example, 1 ㎛ to 100 ㎛, 1 ㎛ to 50 ㎛, 5 ㎛ to 25 ㎛, or 10 ㎛ to 20 ㎛.

[0206] The cathode current collector may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The base film may include, for example, a polymer. The polymer may be, for example, a thermoplastic polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. The base film may be, for example, an insulator. Since the base film includes an insulating thermoplastic polymer, when a short circuit occurs, the base film may soften or liquefy, thereby blocking battery operation and suppressing a sudden increase in current. The metal layer may include, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), or an alloy thereof. The metal layer can act as an electrochemical fuse and cut off in case of overcurrent to prevent short circuits. The limit current and maximum current can be controlled by adjusting the thickness of the metal layer. The metal layer can be plated or deposited on the base film. As the thickness of the metal layer decreases, the limit current and / or maximum current of the positive electrode current collector decreases, thereby improving the stability of the lithium battery in case of a short circuit. A lead tab can be added to the metal layer for external connection. The lead tab can be welded to the metal layer or the metal layer / base film laminate by ultrasonic welding, laser welding, spot welding, etc. During welding, the base film and / or the metal layer melt, so that the metal layer can be electrically connected to the lead tab. To strengthen the welding between the metal layer and the lead tab, a metal chip can be added between the metal layer and the lead tab.The metal piece may be a thin piece of the same material as the metal of the metal layer. The metal piece may be, for example, a metal foil, a metal mesh, etc. The metal piece may be, for example, aluminum foil, copper foil, SUS foil, etc. After the metal piece is placed on the metal layer, the lead tab may be welded to the metal piece / metal layer laminate or the metal piece / metal layer / base film laminate. During welding, the base film, the metal layer, and / or the metal piece may melt, so that the metal layer or the metal layer / metal piece laminate may be electrically connected to the lead tab. A metal chip and / or a lead tab may be added to a portion of the metal layer. The base film may have a thickness of, for example, 1 to 50 μm, 1.5 to 50 μm, 1.5 to 40 μm, or 1 to 30 μm. When the base film has a thickness in this range, the weight of the electrode assembly can be more effectively reduced. The melting point of the base film may be, for example, 100 to 300°C, 100 to 250°C or less, or 100 to 200°C. Since the base film has a melting point within this range, the base film can be melted and easily bonded to the lead tab during the welding process of the lead tab. To improve the adhesion between the base film and the metal layer, a surface treatment such as corona treatment may be performed on the base film. The thickness of the metal layer may be, for example, 0.01 to 3 μm, 0.1 to 3 μm, 0.1 to 2 μm, or 0.1 to μm. Since the metal layer has a thickness within this range, conductivity can be maintained while ensuring the stability of the electrode assembly. The thickness of the metal piece may be, for example, 2 to 10 μm, 2 to 7 μm, or 4 to 6 μm. Since the metal piece has a thickness within this range, the connection between the metal layer and the lead tab can be performed more easily. By having this structure as the cathode current collector, the weight of the cathode can be reduced, and as a result, the energy density of the cathode and lithium battery can be improved. (Electrolyte)

[0207] Next, an electrolyte is prepared. The electrolyte can be, for example, a liquid electrolyte, a solid electrolyte, a gel electrolyte, or a combination thereof. The electrolyte is, for example, an organic electrolyte. An organic electrolyte is prepared by dissolving a lithium salt in an organic solvent.

[0208] Any organic solvent used in the relevant technical field may be used. Examples of the organic solvent include propylene carbonate, ethylene carbonate, fluoroethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, dibutyl carbonate, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, dimethylacetamide, dimethyl sulfoxide, dioxane, 1,2-dimethoxyethane, sulfolane, dichloroethane, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether, or mixtures thereof.

[0209] Lithium salts are all possible if they are used as lithium salts in the relevant technical field. Lithium salts include, for example, LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2)(1≤x≤20, 1≤y≤20), LiCl, LiI or a mixture thereof. The concentration of the lithium salt is, for example, 0.1 M to 5.0 M.

[0210] The solid electrolyte is, for example, an oxide-based solid electrolyte, a sulfide-based solid electrolyte, a polymer solid electrolyte, or a combination thereof.

[0211] Solid electrolytes are, for example, oxide-based solid electrolytes. Oxide-based solid electrolytes are Li 1+x+yAl x Ti 2-x Si y P 3-y O 12 (0 <x<2, 0≤y<3), BaTiO3, Pb(Zr,Ti)O3(PZT), Pb 1-x La x Zr 1-y Ti y O3(PLZT)(O≤x<1, O≤y<1), PB(Mg3Nb 2 / 3 )O3-PbTiO3(PMN-PT), HfO2, SrTiO3, SnO2, CeO2, Na2O, MgO, NiO, CaO, BaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiO2, Li3PO4, Li x Ti y (PO4)3(0 <x<2, 0<y<3), Li x Al y Ti z (PO4)3(0 <x<2, 0<y<1, 0<z<3), Li 1+x+y (Al, Ga) x (Ti, Ge) 2-x Si y P 3-y O 12 (0≤x≤1 0≤y≤1), Li x La y TiO3(0 <x<2, 0<y<3), Li2O, LiOH, Li2CO3, LiAlO2, Li2O-Al2O3-SiO2-P2O5-TiO2-GeO2, Li 3+x La3M2O 12 (M = Te, Nb, or Zr, x is an integer from 1 to 10) is one or more selected from. The solid electrolyte is manufactured by a sintering method, etc. For example, the oxide-based solid electrolyte is Li7La3Zr2O 12 (LLZO) and Li 3+x La3Zr 2-a M a O 12 A garnet-type solid electrolyte selected from (M doped LLZO, M=Ga, W, Nb, Ta, or Al, x is an integer from 1 to 10).

[0212] The sulfide-based solid electrolyte may include, for example, lithium sulfide, silicon sulfide, phosphorus sulfide, boron sulfide, or a combination thereof. The sulfide-based solid electrolyte particles may include Li2S, P2S5, SiS2, GeS2, B2S3, or a combination thereof. The sulfide-based solid electrolyte particles may be Li2S or P2S5. Sulfide-based solid electrolyte particles are known to have high lithium ion conductivity compared to other inorganic compounds. For example, the sulfide-based solid electrolyte includes Li2S and P2S5. When the sulfide solid electrolyte material constituting the sulfide-based solid electrolyte includes Li2S-P2S5, the mixing molar ratio of Li2S to P2S5 may be, for example, in a range of about 50:50 to about 90:10. In addition, Li3PO4, halogen, halogen compound, Li 2+2x Zn 1-x GeO4("LISICON", 0≤x<1), Li 3+y PO 4-x N x( "LIPON", 0 <x<4, 0<y<3), Li 3.25 Ge 0.25 P 0.75 S4("ThioLISICON"), Li2O-Al2O3-TiO2-P2O 5( An inorganic solid electrolyte prepared by adding "LATP") etc. to an inorganic solid electrolyte of Li2S-P2S5, SiS2, GeS2, B2S3, or a combination thereof can be used as a sulfide solid electrolyte. Non-limiting examples of sulfide solid electrolyte materials include Li2S-P2S5; Li2S-P2S5-LiX (X=halogen element); Li2S-P2S5-Li2O; Li2S-P2S5-Li2O-LiI; Li2S-SiS2; Li2S-SiS2-LiI; Li2S-SiS2-LiBr; Li2S-SiS2-LiCl; Li2S-SiS2-B2S3-LiI; Li2S-SiS2-P2S5-LiI; Li2S-B2S3; Li2S -P2S5-Z m S n(0 <m<10, 0<n<10, Z=Ge, Zn 또는 Ga); Li2S-GeS2; Li2S-SiS2-Li3PO4; 및 Li2S-SiS2-Li p FOR q (0 <p<10, 0<q<10, M=P, Si, Ge, B, Al, Ga 또는 In)을 포함한다. 이와 관련하여, 황화물계 고체전해질 재료는 황화물계 고체전해질 물질의 원료 시작 물질(예를 들면, Li2S, P2S5, 등)을 용융 담금질법(melt quenching method), 기계적 밀링법 등에 의해 처리함으로써 제조될 수 있다. 또한, 소성(calcinations) 공정이 상기 처리 후에 수행될 수 있다. 황화물계 고체전해질은 비정질이거나, 결정질이거나, 이들이 혼합된 상태일 수 있다.

[0213] The polymer solid electrolyte may, for example, comprise a mixture of a lithium salt and a polymer, or a polymer having ion-conducting functional groups. The polymer solid electrolyte may be, for example, a polymer electrolyte that is solid at 25°C and 1 atm. The polymer solid electrolyte may not, for example, comprise a liquid.The polymer solid electrolyte comprises a polymer, and the polymer is, for example, polyethylene oxide (PEO), polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene (PVDF-HFP), polyethylene oxide (PEO), poly(styrene-b-ethylene oxide) block copolymer (PS-PEO), poly(styrene-butadiene), poly(styrene-isoprene-styrene), poly(styrene-b-divinylbenzene) block copolymer, poly(styrene-ethylene oxide-styrene) block copolymer, polystyrene sulfonate (PSS), polyvinyl fluoride (PVF), polymethyl methacrylate (PMMA, poly(methylmethacrylate), polyethylene glycol (PEG), polyacrylonitrile (PAN), polytetrafluoroethylene (PTFE), polyethylenedioxythiophene (PEDOT), polypyrrole (PPY), Polyacrylonitrile (PAN), polyaniline, polyacetylene, Nafion, Aquivion, Flemion, Gore, Aciplex, Morgane ADP, sulfonated poly(ether ether ketone) (SPEEK), sulfonated poly(arylene ether ketone ketone sulfone) (SPAEKKS), sulfonated poly(aryl ether ketone) (SPAEK), poly[bis(benzimidazobenzisoquinolinones)] (SPBIBI), poly(styrene sulfonate) (PSS), lithium 9,10-Diphenylanthracene-2-sulfonate (lithium 9,10-diphenylanthracene-2-sulfonate, DPASLi. +) or a combination thereof, but is not limited thereto, and any lithium salt that can be used in polymer electrolytes in the relevant technical field is possible. The lithium salt can be any lithium salt that can be used in the relevant technical field. The lithium salt is, for example, LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2) (x and y are each 1 to 20), LiCl, LiI or a mixture thereof, etc. The polymer included in the polymer solid electrolyte may be, for example, a compound including 10 or more, 20 or more, 50 or more or 100 or more repeating units. The weight average molecular weight of the polymer included in the polymer solid electrolyte may be, for example, 1000 Dalton or more, 10,000 Dalton or more, 100,000 Dalton or more or 1,000,000 Dalton or more.

[0214] A gel electrolyte is, for example, a polymer gel electrolyte. A gel electrolyte can have a gel state without containing a polymer, for example.

[0215] A polymer gel electrolyte may include, for example, a liquid electrolyte and a polymer, or an organic solvent and a polymer having an ion-conducting functional group. The polymer gel electrolyte may be, for example, a polymer electrolyte that is in a gel state at 25°C and 1 atm. The polymer gel electrolyte may, for example, have a gel state without containing a liquid. The liquid electrolyte used in the polymer gel electrolyte may be, for example, an ionic liquid, a mixture of a lithium salt and an organic solvent; a mixture of a lithium salt and an organic solvent; a mixture of an ionic liquid and an organic solvent; or a mixture of a lithium salt, an ionic liquid, and an organic solvent. The polymer used in the polymer gel electrolyte may be selected from among the polymers used in solid polymer electrolytes. The organic solvent may be selected from among the organic solvents used in liquid electrolytes. The lithium salt may be selected from among the lithium salts used in solid polymer electrolytes. An ionic liquid refers to a salt that has a melting point below room temperature, is composed solely of ions, and is liquid at room temperature or a molten salt at room temperature. The ionic liquid may include, for example, one or more cations selected from among a) ammonium compounds, pyrrolidinium compounds, pyridinium compounds, pyrimidinium compounds, imidazolium compounds, piperidinium compounds, pyrazolium compounds, oxazolium compounds, pyridazinium compounds, phosphonium compounds, sulfonium compounds, triazolium compounds, and mixtures thereof, and b) one or more anions selected from among BF4-, PF6-, AsF6-, SbF6-, AlCl4-, HSO4-, ClO4-, CH3SO3-, CF3CO2-, Cl-, Br-, I-, SO4-, CF3SO3-, (FSO2)2N-, (C2F5SO2)2N-, (C2F5SO2)(CF3SO2)N-, and (CF3SO2)2N-. A polymer solid electrolyte can form a polymer gel electrolyte, for example, by being impregnated into a liquid electrolyte in a secondary battery. The polymer gel electrolyte may further include inorganic particles. The polymer included in the polymer gel electrolyte may be, for example, a compound containing 10 or more, 20 or more, 50 or more, or 100 or more repeating units.The weight average molecular weight of the polymer included in the polymer gel electrolyte may be, for example, 500 Dalton or more, 1000 Dalton or more, 10,000 Dalton or more, 100,000 Dalton or more, or 1,000,000 Dalton or more.

[0216] (cathode)

[0217] The cathode contains a cathode current collector.

[0218] Although not shown in the drawing, the negative electrode current collector (21) may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The base film may include, for example, a polymer. The polymer may be, for example, a thermoplastic polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. The polymer may be an insulating polymer. Since the base film includes an insulating thermoplastic polymer, when a short circuit occurs, the base film may soften or liquefy, thereby blocking battery operation and suppressing a rapid increase in current. The metal layer may include, for example, copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), or an alloy thereof. The metal layer may correspond to, for example, the first metal substrate. The metal layer may additionally include a coating layer including a second metal. The negative electrode current collector (21) may additionally include a metal piece and / or a lead tab. For more specific details on the base film, metal layer, metal chip, and lead tab of the negative electrode current collector (21), refer to the positive electrode current collector. By having such a structure, the negative electrode current collector (21) can reduce the weight of the negative electrode, thereby improving the energy density of the negative electrode and the lithium battery.

[0219] A negative electrode active material layer may be formed on the negative electrode current collector. The negative electrode active material layer may be formed as a lithium deposition layer after charging. Alternatively, the negative electrode active material layer may be formed using a negative electrode active material during battery assembly.

[0220] The method of forming a negative electrode active material layer using a negative electrode active material can be manufactured in the same manner as described above, except that the negative electrode active material is used instead of the positive electrode active material when forming the positive electrode active material layer.

[0221] A lithium metal battery may further include, for example, a thin film comprising an element capable of forming an alloy with lithium on one surface of an anode current collector. The thin film is disposed between the anode current collector and the anode active material layer. The thin film includes, for example, an element capable of forming an alloy with lithium. The element capable of forming an alloy with lithium includes, but is not limited to, gold, silver, zinc, tin, indium, silicon, aluminum, bismuth, etc., and any element capable of forming an alloy with lithium in the art may be used. The thin film may be composed of one of these metals or an alloy of several types of metals. By disposing the thin film on one surface of the anode current collector, for example, the deposition shape of the first anode active material layer deposited between the thin film and the anode active material layer becomes flatter, and the cycle characteristics of the lithium metal battery may be further improved.

[0222] (Separator)

[0223] A separator may be further placed between the anode and cathode.

[0224] Any separator commonly used in lithium metal batteries can be used. For example, a separator with low resistance to ion transport and excellent electrolyte absorption capacity is used. The separator may be selected from glass fiber, polyester, Teflon, polyethylene, polypropylene, polytetrafluoroethylene (PTFE), or combinations thereof, and may be in nonwoven or woven form. For lithium-ion batteries, rollable separators, such as polyethylene or polypropylene, are used, while for lithium-ion polymer batteries, separators with excellent organic electrolyte absorption capacity are used.

[0225] The membrane is manufactured by the following exemplary method, but is not limited to this method and may be adjusted according to required conditions.

[0226] First, a separator composition is prepared by mixing a polymer resin, a filler, and a solvent. The separator composition is directly coated and dried on the electrode to form a separator. Alternatively, the separator composition is cast onto a support and dried, and then a separator film peeled from the support is laminated onto the electrode to form a separator.

[0227] The polymer used in membrane manufacturing is not particularly limited; any polymer used as a binder for electrode plates can be used. Examples include vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, or mixtures thereof.

[0228] The separator may contain a liquid electrolyte, which is prepared, for example, by dissolving a lithium salt in an organic solvent.

[0229] Any organic solvent used in the relevant technical field may be used. Examples of the organic solvent include propylene carbonate, ethylene carbonate, fluoroethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, dibutyl carbonate, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, dimethylacetamide, dimethyl sulfoxide, dioxane, 1,2-dimethoxyethane, sulfolane, dichloroethane, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether, or mixtures thereof.

[0230] Lithium salts are all possible if they are used as lithium salts in the relevant technical field. Lithium salts include, for example, LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2)(1≤x≤20, 1≤y≤20), LiCl, LiI or a mixture thereof. The concentration of the lithium salt is, for example, 0.1 M to 5.0 M.

[0231] A lithium metal battery according to one embodiment may further include a solid electrolyte. The solid electrolyte is, for example, an oxide-based solid electrolyte, a sulfide-based solid electrolyte, or a combination thereof.

[0232] Solid electrolytes are, for example, oxide-based solid electrolytes. Oxide-based solid electrolytes are Li 1+x+y Al x Ti 2-x Si y P 3-y O 12 (0 <x<2, 0≤y<3), Li3PO4, Li x Ti y(PO4)3(0 <x<2, 0<y<3), Li x Al y Ti z (PO4)3(0 <x<2, 0<y<1, 0<z<3), Li 1+x+y (Al, Ga) x (Ti, Ge) 2-x Si y P 3-y O 12 (0≤x≤1 0≤y≤1), Li x La y TiO3(0 <x<2, 0<y<3), Li2O, LiOH, Li2CO3, LiAlO2, Li2O-Al2O3-SiO2-P2O5-TiO2-GeO2, Li 3+x La3M2O 12 (M = Te, Nb, or Zr, x is an integer from 1 to 10) is one or more selected from. The solid electrolyte is manufactured by a sintering method, etc. For example, the oxide-based solid electrolyte is Li7La3Zr2O 12 (LLZO) and Li 3+x La3Zr 2-a M a O 12 A garnet-type solid electrolyte selected from (M doped LLZO, M=Ga, W, Nb, Ta, or Al, x is an integer from 1 to 10).

[0233] The sulfide-based solid electrolyte may include, for example, lithium sulfide, silicon sulfide, phosphorus sulfide, boron sulfide, or a combination thereof. The sulfide-based solid electrolyte particles may include Li2S, P2S5, SiS2, GeS2, B2S3, or a combination thereof. The sulfide-based solid electrolyte particles may be Li2S or P2S5. Sulfide-based solid electrolyte particles are known to have high lithium ion conductivity compared to other inorganic compounds. For example, the sulfide-based solid electrolyte includes Li2S and P2S5. When the sulfide solid electrolyte material constituting the sulfide-based solid electrolyte includes Li2S-P2S5, the mixing molar ratio of Li2S to P2S5 may be, for example, in a range of about 50:50 to about 90:10. In addition, Li3PO4, halogen, halogen compound, Li 2+2x Zn 1??x GeO4("LISICON", 0≤x<1), Li 3+y PO 4-x N x( "LIPON", 0 <x<4, 0<y<3), Li 3.25 Ge 0.25 P 0.75 S4("ThioLISICON"), Li2O-Al2O3-TiO2-P2O 5( An inorganic solid electrolyte prepared by adding "LATP") etc. to an inorganic solid electrolyte of Li2S-P2S5, SiS2, GeS2, B2S3, or a combination thereof can be used as a sulfide solid electrolyte. Non-limiting examples of sulfide solid electrolyte materials include Li2S-P2S5; Li2S-P2S5-LiX (X=halogen element); Li2S-P2S5-Li2O; Li2S-P2S5-Li2O-LiI; Li2S-SiS2; Li2S-SiS2-LiI; Li2S-SiS2-LiBr; Li2S-SiS2-LiCl; Li2S-SiS2-B2S3-LiI; Li2S-SiS2-P2S5-LiI; Li2S-B2S3; Li2S -P2S5-Z m S n(0 <m<10, 0<n<10, Z=Ge, Zn 또는 Ga); Li2S-GeS2; Li2S-SiS2-Li3PO4; 및 Li2S-SiS2-Li p MO q (0 <p<10, 0<q<10, M=P, Si, Ge, B, Al, Ga 또는 In)을 포함한다. 이와 관련하여, 황화물계 고체전해질 재료는 황화물계 고체전해질 물질의 원료 시작 물질(예를 들면, Li2S, P2S5, 등)을 용융 담금질법(melt quenching method), 기계적 밀링법 등에 의해 처리함으로써 제조될 수 있다. 또한, 소성(calcinations) 공정이 상기 처리 후에 수행될 수 있다. 황화물계 고체전해질은 비정질이거나, 결정질이거나, 이들이 혼합된 상태일 수 있다.

[0234] (lithium metal battery)

[0235] Referring to FIG. 6, a lithium metal battery (1) according to one embodiment includes a positive electrode (3), the above-described negative electrode (2), and an electrolyte (4). A gel-type polymer electrolyte (not shown) may be disposed between the electrolyte and the positive electrode. The positive electrode (3), the negative electrode (2), and the electrolyte (4) are wound or folded to form a battery structure (7). The formed battery structure (7) is accommodated in a battery case (5). An organic electrolyte is injected into the battery case (5) and sealed with a cap assembly (6), thereby completing the lithium metal battery (1). The battery case (5) is cylindrical, but is not necessarily limited to this shape, and may be, for example, square, thin-film, etc.

[0236] Referring to FIG. 6, a lithium metal battery (1) according to one embodiment includes a positive electrode (3), a negative electrode (2), and an electrolyte (4). An electrolyte (4) is disposed between the positive electrode (3) and the negative electrode (2), and the positive electrode (3), the negative electrode (2), and the separator (4) are wound or folded to form a battery structure (7). The formed battery structure (7) is accommodated in a battery case (5). An electrode tab (8) that serves as an electrical path for guiding the current formed in the battery structure (7) to the outside may be included. An organic electrolyte is injected into the battery case (5) and sealed to complete the lithium metal battery (1). The battery case (5) is not necessarily limited to a square shape, and may be, for example, a cylindrical shape, a thin film shape, etc.

[0237] Referring to FIG. 7, a lithium metal battery (1) according to one embodiment includes a positive electrode (3), a negative electrode (2) according to one embodiment, and an electrolyte (4). An electrolyte (4) is disposed between the positive electrode (3) and the negative electrode (2), thereby forming a battery structure. A gel-type polymer electrolyte between the separator and the positive electrode is not shown. The battery structure (7) is stacked in a bi-cell structure and then accommodated in a battery case (5). An electrode tab (8) that serves as an electrical path for guiding the current formed in the battery structure (7) to the outside may be included. An organic electrolyte is injected into the battery case (5) and sealed, thereby completing the lithium metal battery (1). The battery case (5) is not necessarily limited to a square shape, and may be, for example, a cylindrical shape, a thin-film shape, etc.

[0238] A pouch-type lithium metal battery corresponds to the lithium metal batteries of FIGS. 7 and 8, each of which uses a pouch as a battery case. The pouch-type lithium metal battery includes one or more battery structures. An electrolyte is disposed between a positive electrode and a negative electrode, or an electrolyte and a separator are disposed to form a battery structure. The battery structures are laminated in a bi-cell structure, then impregnated with a liquid electrolyte, and accommodated and sealed in a pouch, thereby completing a pouch-type lithium metal battery. For example, although not shown in the drawings, the above-described positive electrode, negative electrode, and separator may be simply laminated and accommodated in a pouch in the form of an electrode assembly, or may be wound or folded into a jellyroll-shaped electrode assembly and then accommodated in a pouch. Subsequently, an organic electrolyte is injected into the pouch and sealed, thereby completing a lithium metal battery.

[0239] The lithium metal battery of the present disclosure has excellent discharge capacity and cycle life characteristics, as well as high energy density, and is therefore used in, for example, electric vehicles (EVs). For example, it is used in hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs). It is also used in applications requiring large amounts of power storage, such as electric bicycles and power tools.

[0240] Lithium metal batteries are stacked in multiple layers to form a battery module, and the multiple battery modules form a battery pack. Such a battery pack can be used in any device requiring high capacity and high output. For example, it can be used in laptops, smartphones, electric vehicles, etc. The battery module includes, for example, multiple batteries and a frame that holds them. The battery pack includes, for example, multiple battery modules and a bus bar that connects them. The battery module and / or the battery pack may further include a cooling device. The multiple battery packs are controlled by a battery management system. The battery management system includes a battery pack and a battery control device connected to the battery pack.

[0241] [Method for manufacturing lithium metal batteries]

[0242] A lithium metal battery according to an embodiment includes a step of preparing a negative electrode current collector; a step of forming a protective layer by coating and drying a composition for forming a protective layer on the negative electrode current collector; a step of preparing an electrolyte; a step of preparing a positive electrode; and a step of preparing an assembly by laminating a negative electrode current collector, an electrolyte, and a positive electrode.

[0243] The composition for forming the protective layer contains the first polymer containing a hydroxyl group and i) boric acid (H3BO3); or ii) a hydrate of boron oxide (B2O3) and water; or iii) a combination thereof. The composition for forming the protective layer may further contain a second polymer having a crosslinkable functional group. The protective layer formed from the composition for forming the protective layer further contains a crosslinked polymer of the first polymer and the second polymer. Here, the mixing weight ratio of the first polymer containing a hydroxyl group and the second polymer is adjusted to be in the range of 50:50 to 99:1, 50:50 to 99:1, or 60:40 to 90:10.

[0244] The above second polymer is at least one selected from among fluorinated polyamic acid and fluorinated polyimide having a carboxyl group.

[0245] When the second polymer is a fluorinated polyamic acid having a carboxyl group, a composition for forming a protective layer containing the same may be coated on a negative electrode current collector, dried, and then further heat-treated to cause a crosslinking reaction between the first polymer and the second polymer, thereby forming a protective layer containing a crosslinked polymer. The heat-treatment may vary depending on the composition of the first polymer and the second polymer, but may be performed at, for example, 80 to 200°C, 100 to 200°C, 150 to 200°C, or 150 to 190°C. When the heat-treatment temperature is within the above range, the protective layer formed on the electrode surface can minimize or reduce exposure of the electrolyte at the electrode surface and create a uniform lithium ion flow throughout the electrode, thereby effectively suppressing lithium dendrite growth.

[0246] The composition for forming the above protective layer may further include a lithium salt.

[0247] The above lithium metal battery may further include a separator. The separator may further include a liquid electrolyte and / or a gel-type polymer electrolyte.

[0248] The present invention is explained in more detail through the following examples and comparative examples. However, the examples are intended to illustrate the present invention and are not intended to limit the scope of the present invention.

[0249] Manufacturing Example 1: Manufacturing of a polymer solution containing polyvinyl alcohol and a fluorinated polyamic acid of the following chemical formula 10.

[0250] Polyvinyl alcohol was purchased from Sigma-Aldrich. The synthesis process of fluorinated polyamic acid of chemical formula 10 is as follows.

[0251] First, after filling a round-bottomed flask with nitrogen, 4.9411 g (0.00154 mol) of 2,2'-bis(trifluoromethyl)benzidine (TFDB) and 0.7825 g (0.00051 mol) of diaminobenzoic acid (DABA) were added, followed by adding 131 g of N-methylpyrrolidone (NMP) and completely dissolving using a mechanical stirrer. Next, 9.2764 g (0.0209 mol) of 4,4'-(hexafluoroisopropylidene) (6FDA) was added and stirred at room temperature for 24 hours, thereby producing a polyamic acid represented by the following chemical formula 9. The polyamic acid is a random copolymer. The molar ratio of 6FDA:TFDB:DABA was 4:3:1.

[0252] In chemical formula 9, the molar ratio of n:m was 1:3.

[0253] 10g of LiOH aqueous solution having 0.5 equivalents in carboxylic acid equivalent ratio was added to polyamic acid (6FDA:TFDB:DABA, acid equivalent 210g / eq) represented by the following chemical formula 9, and 0.5 equivalents of COOH in the polyamic acid was converted to COO-Li+ A water-soluble polyamic acid represented by the chemical formula 10 substituted with was prepared.

[0254] [Chemical Formula 9]

[0255]

[0256] In the above equation, n is 0.25, m is 0.75, and the sum of n and m is 1.

[0257] A water-soluble polyamic acid represented by the following chemical formula 10 and polyvinyl alcohol (weight average molecular weight, Mw = 89,000, hydrolysis +99%) were mixed at a weight ratio of 20:80 to prepare a polymer solution having a solid content of 10 wt%.

[0258] [Chemical Formula 10]

[0259]

[0260] In the above equation, n is 0.25, m is 0.75, and the sum of n and m is 1.

[0261] Example 1: Protective layer: 0.5% boric acid + PVA / PI-F

[0262] A water-soluble polyamic acid represented by chemical formula 10 obtained according to Manufacturing Example 1, and

[0263] Polyvinyl alcohol was mixed in a weight ratio of 20:80 to prepare a polymer solution having a solid content of 10 wt% and boric acid (H3BO3), and then mixed with NMP as a solvent to prepare a composition for forming a protective layer. At this time, the content of boric acid was 0.5 wt% based on 100 wt parts of the composition for forming a protective layer, and the content of the solvent was 99.5 wt parts based on 100 wt parts of the composition for forming a protective layer.

[0264] The composition for forming the protective layer was coated on top of a copper foil having a thickness of 10 μm, which is a negative electrode current collector, and dried in a vacuum oven at 80°C for 30 minutes, followed by heat treatment at 180°C for 30 minutes to prepare a negative electrode. The negative electrode had a structure in which a 10 μm thick protective layer was coated on a lithium metal thin film disposed on a copper current collector.

[0265] The heat treatment above causes the carboxyl group of the polyamic acid of the above chemical formula 10 to react with the hydroxyl group of the polyvinyl alcohol to form an ester linker, thereby forming a crosslinked polymer (PVA / PI-F) of the polyimide of the following chemical formula 12 and the polyvinyl alcohol. The crosslinked polymer has a three-dimensional network structure in which the polyimide of the following chemical formula 12 and the polyvinyl alcohol are crosslinked at multiple points.

[0266] [Chemical Formula 12]

[0267]

[0268] In the above formula, n is 1, m is 3, and the weight average molecular weight of the polyimide of chemical formula 12 is approximately 2,000,000.

[0269] A polyethylene single film with a thickness of 20 μm was laminated as a separator, and a positive electrode was laminated on the other side of the separator to manufacture a laminate. A liquid electrolyte was injected into the prepared laminate to manufacture a lithium metal battery.

[0270] The lithium metal battery had a structure of a cathode / gel polymer electrolyte (separator) / protective layer / negative current collector. The liquid electrolyte was a 2:1 volume ratio mixed solvent of diethyl carbonate (DEC) and fluoroethylene carbonate (FEC), with 0.6 M LiBF4 and 0.6 M LiDFOB (lithium difluoro(oxalate)borate).

[0271] The above anode was manufactured according to the following method.

[0272] Li 1.04 Ni 0.88 Co 0.1 Al 0.02 O2 powder and carbon conductive material (Super-P; Timcal Ltd.) were uniformly mixed at a weight ratio of 90:5, and then a PVDF (polyvinylidene fluoride) binder solution was added to prepare a positive electrode active material slurry with a weight ratio of active material:carbon conductive material:binder = 90:5:5.

[0273] The manufactured slurry was coated on a 15 ㎛ thick aluminum substrate using a doctor blade, dried under reduced pressure at 120°C, and rolled using a roll press to form a sheet to manufacture a positive electrode.

[0274] Example 2: Protective layer: 1% boric acid + PVA / PI-F

[0275] A protective layer and a lithium metal battery having the same were manufactured in the same manner as in Example 1, except that the content of boric acid was changed to 1 wt% based on 100 wt% of the composition for forming a protective layer.

[0276] Example 3: Protective layer: 2% boric acid + PVA / PI-F

[0277] A protective layer and a lithium metal battery having the same were manufactured in the same manner as in Example 1, except that the content of boric acid was changed to 2 wt% based on 100 wt% of the composition for forming a protective layer.

[0278] Example 4: Protective layer: 5% boric acid + PVA / PI-F

[0279] A protective layer and a lithium metal battery having the same were manufactured in the same manner as in Example 1, except that the content of boric acid was changed to 5 wt% based on 100 wt% of the composition for forming a protective layer.

[0280] Example 5: Protective layer: 0.5% boric acid + CMC

[0281] The content of boric acid is 0.5 based on 100 parts by weight of the composition for forming a protective layer.

[0282] A protective layer and a lithium metal battery having the same were manufactured in the same manner as in Example 1, except that the weight % was changed and carboxymethylcellulose (CMC) was used instead of the polymer solution obtained according to Manufacturing Example 1.

[0283] Example 6

[0284] A protective layer and a lithium metal battery having the same were manufactured in the same manner as in Example 1, except that hydroxyethyl methacrylate was used instead of the water-soluble polyamic acid represented by the chemical formula 10 when manufacturing a polymer solution having a solid content of 10 wt%.

[0285] Example 7

[0286] A protective layer and a lithium metal battery having the same were manufactured according to the same method as Example 1, except that hydroxypropyl acrylate was used instead of the water-soluble polyamic acid represented by Chemical Formula 10 when manufacturing a polymer solution having a solid content of 10 wt%.

[0287] Comparative Example 1

[0288] A protective layer and a lithium metal battery having the same were manufactured in the same manner as in Example 1, except that boric acid (H3BO3) was not added when manufacturing the composition for forming a protective layer.

[0289] Comparative Example 2

[0290] A composition for forming a protective layer was prepared by mixing polyethylene oxide (MV: 4,000,000) and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI, ((CF3SO2)2NLi) in an acetonitrile solvent at a ratio of EO:Li=9:1 (repeating unit of EO:PEO).

[0291] A protective layer and a lithium metal battery having the same were manufactured in the same manner as in Example 1, except that the protective layer-forming composition was used instead of the protective layer-forming composition of Example 1.

[0292] Evaluation Example 1: Lifespan at room temperature (25℃)

[0293] The charge / discharge characteristics of the lithium metal batteries of Example 1-7 and Comparative Example 1-2 were evaluated under the following conditions.

[0294] The battery was charged at a constant current of 0.1 C rate at 25°C until the voltage reached 4.3 V (vs. Li), and then cut-off at a current of 0.05 C rate while maintaining 4.3 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.1 C rate until the voltage reached 3.6 V (vs. Li) (formation cycle).

[0295] The lithium metal battery, which had undergone a Mars cycle, was charged at a constant current of 0.2 C rate at 25°C until the voltage reached 4.3 V (vs. Li), and then cut-off at a current of 0.05 C rate while maintaining 4.3 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.5 C rate until the voltage reached 3.6 V (vs. Li) (1 st cycle). These cycles are 100 th The cycle was repeated under the same conditions.

[0296] In all charge / discharge cycles, a 10-minute pause was provided after each charge / discharge cycle. Some of the results of the room-temperature charge / discharge experiments are shown in Table 1 below. The capacity retention rate is defined by Equation 1 below.

[0297] <Formula 1>

[0298] Capacity retention rate [%] = [100 th Discharge capacity in cycles / 1 st Discharge capacity in cycle] × 100

[0299] Capacity retention rate (%) Example 168.4 Example 273.1 Example 367.9 Example 464.3 Example 561.1 Comparative example 155.7 Comparative example 243.2

[0300] As shown in Table 1, the lithium metal battery of Comparative Example 1 had a reduced capacity retention rate due to lithium and electrolyte side reactions resulting from dendrite growth due to the absence of a protective layer, and the lithium metal battery of Comparative Example 2 had a structure in which a polyethylene oxide protective layer was formed on the negative electrode current collector, but the protective layer did not have a sufficient effect of suppressing the growth of negative electrode dendrites, so that in the cases of Examples 1 to 5, the protective layer was formed on the negative electrode current collector, and when the protective layer was formed, the physical properties of the protective layer increased without reducing ionic conductivity, resulting in a reduced capacity retention rate characteristic of the lithium metal battery.

[0301] The capacity retention rate of the lithium metal battery of Examples 6 and 7 was similar to that of the lithium metal battery of Example 1.

[0302] Evaluation Example 2: High Temperature (45℃) Lifespan

[0303] The charge / discharge characteristics of the lithium metal batteries of Example 1-5 and Comparative Example 1-2 were evaluated under the following conditions.

[0304] The battery was charged at a constant current of 0.1 C rate at 45°C until the voltage reached 4.3 V (vs. Li), and then cut-off at a current of 0.05 C rate while maintaining 4.3 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.1 C rate until the voltage reached 3.6 V (vs. Li) during discharge (formation cycle).

[0305] The lithium metal battery, which had undergone a Mars cycle, was charged at a constant current of 0.2 C rate at 25°C until the voltage reached 4.3 V (vs. Li), and then cut-off at a current of 0.05 C rate while maintaining 4.3 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.5 C rate until the voltage reached 3.6 V (vs. Li) (1 st cycle). These cycles are 100 th The cycle was repeated under the same conditions.

[0306] In all charge / discharge cycles, a 10-minute pause was observed after each charge / discharge cycle. Some of the results of the room-temperature charge / discharge experiments are shown in Table 2 below. The capacity retention rate is defined by Equation 2 below.

[0307] <Formula 2>

[0308] Capacity retention rate [%] = [100 th Discharge capacity in cycles / 1 st Discharge capacity in cycle] × 100

[0309] Capacity retention rate (%) Example 184.5 Example 285.1 Example 383.7 Example 480.9 Example 575.7 Comparative example 174.1 Comparative example 265.3

[0310] As shown in Table 2, the lithium metal battery of Comparative Example 1 showed a decrease in high-temperature capacity retention rate due to lithium and electrolyte side reactions resulting from dendrite growth due to the absence of a protective layer, and the lithium metal battery of Comparative Example 2 had a structure in which a polyethylene oxide protective layer was formed on the negative electrode current collector, but the protective layer did not have a sufficient effect in suppressing negative electrode dendrite growth, resulting in a decrease in high-temperature capacity retention rate characteristics compared to Examples 1 to 5.

[0311] Evaluation Example 3: High-rate characteristics

[0312] The lithium metal batteries manufactured in Example 1-5 and Comparative Example 1-2 were charged at a constant current of 0.1 C rate at 25°C until the voltage reached 4.3 V (vs. Li), and then cut-off at a current of 0.05 C rate while maintaining 4.3 V in constant voltage mode. Subsequently, the batteries were discharged at a constant current of 0.1 C rate until the voltage reached 3.6 V (vs. Li) during discharge (formation cycle).

[0313] The lithium metal battery, which had undergone a Mars cycle, was charged at a constant current of 0.2 C rate at 25°C until the voltage reached 4.3 V (vs. Li), and then cut-off at a current of 0.05 C rate while maintaining 4.3 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.5 C rate until the voltage reached 3.6 V (vs. Li) (1 st cycle).

[0314] 1 st The cycled lithium battery was charged at a constant current of 0.2 C at 25°C until the voltage reached 4.3 V (vs. Li), and then cut off at a current of 0.05 C while maintaining 4.3 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.2 C until the voltage reached 2.8 V (vs. Li) (2 nd cycle).

[0315] 2 nd Cycle 7 th The cycle was repeated under the same conditions.

[0316] 7 thThe cycled lithium battery was charged at a constant current of 0.33 C at 25°C until the voltage reached 4.35 V (vs. Li), and then cut off at a current of 0.05 C while maintaining 4.35 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.5 C until the voltage reached 2.8 V (vs. Li) (8 rd cycle).

[0317] 8th cycle 17 th The cycle was repeated under the same conditions.

[0318] 17 th The cycled lithium battery was charged at a constant current of 0.33 C at 25°C until the voltage reached 4.35 V (vs. Li), and then cut off at a current of 0.05 C while maintaining 4.35 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 1 C until the voltage reached 2.8 V (vs. Li) (18 th cycle).

[0319] 18 th Cycle 25 th The cycle was repeated under the same conditions.

[0320] 25 st The cycled lithium battery was charged at a constant current of 0.33 C at 25°C until the voltage reached 4.35 V (vs. Li), and then cut off at a current of 0.05 C while maintaining 4.35 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 2 C until the voltage reached 2.8 V (vs. Li) (26 th cycle).

[0321] 26th cycle 35 th The cycle was repeated under the same conditions.

[0322] 35 stThe cycled lithium battery was charged at a constant current of 0.33 C at 25°C until the voltage reached 4.35 V (vs. Li), and then cut off at a current of 0.05 C while maintaining 4.35 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 3 C until the voltage reached 2.8 V (vs. Li) (36 th cycle).

[0323] 36 th The cycled lithium battery was charged at a constant current of 0.33 C at 25°C until the voltage reached 4.35 V (vs. Li), and then cut off at a current of 0.05 C while maintaining 4.35 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.2 C until the voltage reached 2.8 V (vs. Li) (46 th cycle), these cycles are 100 th The cycle was repeated under the same conditions.

[0324] In all the above charge / discharge cycles, a pause of 10 minutes was allowed after each charge / discharge cycle.

[0325] Some of the results of the above charge-discharge experiment are shown in Table 3 below. In addition, the capacity retention rate and capacity characteristic changes according to the number of cycles in the lithium metal batteries of Example 1 and Comparative Example 1 are shown in FIGS. 3 and 4, respectively.

[0326] The high-rate characteristic is defined by Equation 3 below.

[0327] <Formula 3>

[0328] High rate characteristic [%] = [25 st Discharge capacity in cycles (1C rate) / 2 nd Discharge capacity in cycle (0.2C rate)] × 100

[0329] Characteristics of the composition ratio of the protective layer (%) Example 1 Boric acid 0.5% + PVA / PI-F 8 4.3 Example 2 Boric acid 1% + PVA / PI-F 8 4.1 Example 3 Boric acid 2% + PVA / PI-F 8 3.3 Example 4 Boric acid 5% + PVA / PI-F 8 1.0 Example 5 Boric acid 0.5% + CMC 7 3.5 Comparative Example 1 PVA / PI-F 7 2.1 Comparative Example 2 PEO / LiTFSi (9:1) 65.3

[0330] Referring to Table 3, Examples 1 to 4 had a protective layer formed on the negative electrode current collector containing boric acid, which improved lithium ion transfer and thus the ionic conductivity characteristics, thereby significantly increasing the high-rate characteristics compared to the lithium metal battery of Comparative Example 1 that did not have a protective layer. The lithium metal battery of Comparative Example 2 had a polyethylene oxide protective layer, which resulted in a decrease in the high-rate characteristics compared to Comparative Example 1, and showed lower high-rate characteristics compared to Examples 1 to 4 having a protective layer containing PVA / PI-f and boric acid and Example 5 having a protective layer containing CMC and boric acid. From this, it was found that the physical strength of the protective layer of Examples 1 to 5 increased, which further increased stability, and thus the high-rate characteristics were improved due to the improvement in ionic conductivity.

[0331] Evaluation Example 4: SEM Analysis I

[0332] The laminated structure of the negative electrode current collector / protective layer of the lithium metal battery of Example 1 was investigated using FE-SEM, and the results are shown in Fig. 5.

[0333] Referring to Figure 5, it was confirmed that the protective layer was formed with a thickness of approximately 1.5 um.

[0334] Evaluation Example 5: SEM Analysis II

[0335] After charging the lithium metal battery of Example 1 to 100% SOC at 25°C, the cell was disassembled and the cross-section and thickness of the lithium under-deposition and uniform protective layer were measured using SEM. The analysis results are shown in Figures 6a to 6c.

[0336] Figure 6a is an SEM photograph showing a state in which a protective layer is formed on the negative electrode current collector in the lithium metal battery of Example 1. Figures 6b and 6c are SEM photographs showing a structure in which a lithium metal layer is deposited on the negative electrode current collector and a protective layer is arranged on top of it.

[0337] Referring to Fig. 6a, it can be confirmed that a protective layer was formed on top of the negative electrode current collector. In addition, from Figs. 6b and 6c, it can be confirmed that when boric acid was added, the thickness of the lithium precipitation layer was relatively low, indicating that it was formed in a dense lithium layer.

[0338] Evaluation Example 6: Ionic Conductivity

[0339] The ionic conductivity of the lithium metal battery of Example 1-5 was investigated and is shown in Table 4 below.

[0340] Composition of protective layer Ionic conductivity (mS / cm) Example 1 Boric acid 0.5% + PVA / PI-F 0.53 Example 2 Boric acid 1% + PVA / PI-F 0.57 Example 3 Boric acid 2% + PVA / PI-F 0.71 Example 4 Boric acid 5% + PVA / PI-F 0.68 Example 5 Boric acid 0.5% + CMC 0.40

[0341] As shown in Table 4, the lithium metal batteries of Examples 1-5 were found to have excellent ionic conductivity.

[0342] While exemplary embodiments have been described in detail with reference to the attached drawings, the present invention is not limited to these examples. It is self-evident that those skilled in the art to which the present invention pertains can devise various modifications or variations within the scope of the technical concepts described in the patent claims, and these also naturally fall within the technical scope of the present invention.

Claims

1. Negative current collector; and It includes a protective layer formed on the negative electrode current collector, It includes a negative electrode active material layer disposed between the negative electrode current collector and the protective layer, or the negative electrode active material layer is absent (free), The above protective layer comprises a first polymer containing a hydroxyl group, A negative electrode for a lithium metal battery comprising i) boric acid (H3BO3); or ii) a hydrate of boron oxide (B2O3) and water; or a combination thereof.

2. In the first paragraph, the first polymer containing a hydroxyl group is carboxymethyl cellulose (CMC); polyvinyl alcohol (PVA); Vinyl acetate, butyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 2-hydroxyethylene glycol (meth)acrylate, 2-hydroxypropylene glycol (meth)acrylate, acrylic acid, methacrylic acid, 2-(meth)acryloyloxy acetic acid, 3-(meth)acryloyloxy propyl acid, 4-(meth)acryloyloxy butyric acid, itaconic acid, maleic acid, 2-isocyanatoethyl (meth)acrylate, 3-isocyanatopropyl (meth)acrylate, A negative electrode for a lithium metal battery, wherein the negative electrode is at least one selected from the group consisting of a polymerization reaction product of one or more monomers selected from 4-isocyanatobutyl (meth)acrylate, (meth)acrylamide, ethylene di(meth)acrylate, diethylene glycol (meth)acrylate, triethylene glycol di(meth)acrylate, trimethylene propane tri(meth)acrylate, trimethylene propane triacrylate, 1,3-butanediol (meth)acrylate, 1,6-hexanediol di(meth)acrylate, allyl acrylate, and N-vinyl caprolactam, or a hydrolyzate thereof; 3. In the first paragraph, the protective layer further includes a second polymer having a functional group capable of crosslinking with the first polymer containing a hydroxyl group, A negative electrode for a lithium metal battery, wherein the protective layer further comprises a crosslinked polymer of a first polymer and a second polymer.

4. A negative electrode for a lithium metal battery, wherein the second polymer is at least one selected from among fluorinated polyamic acid and fluorinated polyimide having a carboxyl group in the third paragraph.

5. A negative electrode for a lithium metal battery, wherein in the first paragraph, the content of i) boric acid (H3BO3) or ii) boron oxide (B2O3) and water hydrate in the protective layer is 5 wt% or less based on 100 wt% of the total weight of the protective layer.

6. In paragraph 4, the fluorinated polyamic acid is a polymer represented by the following chemical formula 1 or 2, A negative electrode for a lithium metal battery, wherein the above fluorinated polyimide is a polymer represented by the following chemical formula 3 or 4: [Chemical Formula 1] [Chemical Formula 2] [Chemical Formula 3] [Chemical Formula 4] In the above formulas, M is an alkali metal, Ar1 and Ar3 are independently an aromatic ring group selected from a substituted or unsubstituted tetravalent arylene group having 6 to 24 carbon atoms or a substituted or unsubstituted tetravalent heteroarylene group having 4 to 24 carbon atoms, wherein the aromatic ring group is one aromatic ring, a fused ring of two or more aromatic rings, or a ring of two or more aromatic rings connected by a single bond, -O-, -S-, -C(=O)-, -S(=O)2-, -Si(Ra)(Rb)- (Ra and Rb are each independently an alkyl group having 1 to 10 carbon atoms), a substituted or unsubstituted alkylene group having 1 to 10 carbon atoms, or -C(=O)-NH-. Ar2 and Ar4 are independently an aromatic ring group selected from a substituted or unsubstituted divalent arylene group having 6 to 24 carbon atoms or a substituted or unsubstituted divalent heteroarylene group having 4 to 24 carbon atoms, wherein the aromatic ring group is a ring connected by one aromatic ring, a fused ring of two or more aromatic rings, a single bond, -O-, -S-, -C(=O)-, -S(=O)2-, -Si(Ra)(Rb)- (Ra and Rb are independently an alkyl group having 1 to 10 carbon atoms), a substituted or unsubstituted alkylene group having 1 to 10 carbon atoms, or -C(=O)-NH-. At least one of Ar1 to Ar4 is substituted with a halogen group, X1 is the first functional group, which is -COOH, -OH, -CO-NH2, or -COH, n and m are the mole fractions within the repeating unit, respectively, and 0 <n≤1, 0≤m<1, n+m=1이다.

7. In paragraph 6, the polyamic acid is a polymer represented by the following chemical formula 5 or 6, A negative electrode for a lithium metal battery, wherein the polyimide is a polymer represented by the following chemical formula 7 or 8: [Chemical Formula 5] [Chemical Formula 6] [Chemical Formula 7] [Chemical Formula 8] In the above formulas, M is lithium or sodium, and R1, R2, R3, R4, R5, R6, R7, R8, R9, R 10 , R 11 , and R 12 are independently hydrogen, halogen, -COOH, -OH, -CO-NH2, -COH, an alkyl group having 1 to 10 carbon atoms substituted or unsubstituted with a halogen, an aryl group having 6 to 20 carbon atoms substituted or unsubstituted with a halogen, or a heteroaryl group having 2 to 20 carbon atoms substituted or unsubstituted with a halogen, provided that R1 to R 12 At least one of which is a halogen group or a group substituted with a halogen group, A1 and A2 are each independently a single bond, -O-, -S-, -C(=O)-, -S(=O)2-, -Si(Ra)(Rb)- (Ra and Rb are each independently an alkyl group having 1 to 10 carbon atoms), an alkylene group having 1 to 10 carbon atoms substituted or unsubstituted with a halogen, or -C(=O)-NH-; provided that at least one of R5, R6, R7, and R8 is -COOH, -OH, -CO-NH2, or -COH, and n and m are each a mole fraction within the repeating unit, 0 <n≤1, 0≤m<1, n+m=1이다.

8. In the first paragraph, the polyamic acid is represented by the following chemical formula 9 or 10, A negative electrode for a lithium metal battery, wherein the polyimide is a polymer represented by the following chemical formula 11 or 12: [Chemical Formula 9] [Chemical Formula 10] [Chemical Formula 11] [Chemical Formula 12] In the above equations, n and m are the mole fractions within the repeating unit, respectively, and 0 <n≤1, 0≤m<1, n+m=1이다.

9. A negative electrode for a lithium metal battery, wherein the weight ratio of the first polymer and the second polymer in the third paragraph is 50:50 to 99:

1.

10. In the first paragraph, the protective layer is a negative electrode for a lithium metal battery comprising a cross-linked polymer of polyvinyl alcohol and polyamic acid of the following chemical formula 9 or 10: [Chemical Formula 9] [Chemical Formula 10] In the above equations, n and m are the mole fractions within the repeating unit, respectively, and 0 <n≤1, 0≤m<1, n+m=1이다.

11. In the first paragraph, the protective layer further includes a lithium salt, A negative electrode for a lithium metal battery, wherein the thickness of the protective layer is 1 to 10㎛.

12. In the first paragraph, the negative active material layer includes lithium metal foil, lithium metal powder, lithium alloy foil, lithium alloy powder, or a combination thereof, The above lithium alloy contains lithium and a first metal, A lithium metal battery wherein the first metal is indium (In), silicon (Si), gallium (Ga), tin (Sn), aluminum (Al), titanium (Ti), zirconium (Zr), niobium (Nb), germanium (Ge), antimony (Sb), bismuth (Bi), gold (Au), platinum (Pt), palladium (Pd), magnesium (Mg), silver (Ag), zinc (Zn), nickel, iron, cobalt, chromium, cesium, sodium, potassium, calcium, yttrium, bismuth, tantalum, hafnium, barium, vanadium, strontium, lanthanum, or a combination thereof.

13. In the first paragraph, the negative electrode active material layer contains a carbon-based compound; a mixture of at least one selected from a carbon-based material and a first metal; a composite of at least one selected from a carbon-based material and a first metal; or a combination thereof. The above carbon-based material includes amorphous carbon, The average particle diameter of the above amorphous carbon is 10 nm to 100 nm, The above carbon-based material includes carbon black, carbon nanotubes, carbon nanofibers, fullerenes, activated carbon, carbon fibers, or a combination thereof, A negative electrode for a lithium metal battery, wherein the first metal is indium (In), silicon (Si), gallium (Ga), tin (Sn), aluminum (Al), titanium (Ti), zirconium (Zr), niobium (Nb), germanium (Ge), antimony (Sb), bismuth (Bi), gold (Au), platinum (Pt), palladium (Pd), magnesium (Mg), silver (Ag), zinc (Zn), nickel, iron, cobalt, chromium, cesium, sodium, potassium, calcium, yttrium, bismuth, tantalum, hafnium, barium, vanadium, strontium, lanthanum or a combination thereof.

14. In the first paragraph, the negative electrode has a structure in which a negative electrode current collector, a negative electrode active material layer, and a protective layer are sequentially arranged, A negative electrode for a lithium metal battery, further comprising a lithium metal layer disposed on the upper surface of the protective layer that is not adjacent to the negative electrode active material layer.

15. Bipolar; A cathode according to any one of the above clauses 1 to 14; and A lithium metal battery comprising an electrolyte disposed between the positive electrode and the negative electrode.

16. In paragraph 15, the electrolyte is a liquid electrolyte, a solid electrolyte, a gel electrolyte, or a combination thereof, The above solid electrolyte includes an oxide-based solid electrolyte, a sulfide-based solid electrolyte, a polymer solid electrolyte, or a combination thereof, A lithium metal battery, wherein the gel electrolyte comprises a polymer gel electrolyte.

17. A lithium metal battery according to claim 15, wherein the lithium metal battery further comprises a separator.

18. In the 15th paragraph, the positive electrode includes a positive electrode current collector and a positive electrode active material layer, At least one of the positive electrode current collector and the negative electrode current collector includes a base film and a metal layer disposed on one or both sides of the base film, The above base film comprises a polymer, and the polymer comprises polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI) or a combination thereof, A lithium metal battery, wherein the metal layer comprises indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof.

19. Step of preparing the negative electrode collector; A step of preparing a composition for forming a protective layer comprising a first polymer containing a hydroxyl group and i) a hydrate of boric acid (H3BO3), ii) boron oxide (B2O3) and water or a combination thereof, and then coating and drying the composition on a negative electrode current collector to form a protective layer; Steps for preparing electrolyte; Steps for preparing the anode; and A method for manufacturing a lithium metal battery, comprising the step of preparing an assembly by laminating a negative electrode current collector, an electrolyte, and a positive electrode; 20. A method for manufacturing a lithium metal battery in claim 19, wherein the composition for forming the protective layer further includes a second polymer having a functional group capable of crosslinking with the first polymer containing a hydroxyl group.

Citation Information

Patent Citations

  • Negative electrode for lithium metal battery and lithium metal battery including the same

    KR1020170001069A

  • Apparatus for cleaning glasses

    KR1020200095812A

  • Memory controller and operating method thereof

    KR1020200114149A

  • Apparatus and method of flux cleaning of semiconductor package

    KR1020220101328A

  • Electrode for lithium-ion secondary battery

    US20190148734A1