Composite solid electrolyte, thermal battery comprising same, and manufacturing method therefor

The composite solid electrolyte with a molten salt-coated core-shell structure addresses the leakage issues in thermal batteries by enhancing ionic conductivity and stability, improving thermocell performance and longevity.

WO2024205113A1PCT designated stage expired Publication Date: 2024-10-03AGENCY FOR DEFENSE DEV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/003476
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-19
Filing Date
2024-03-20
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional thermal batteries face issues with electrolyte leakage when molten salt melts, leading to increased internal resistance and short-circuits, due to the high melting point of eutectic salts used as electrolytes.

Method used

A composite solid electrolyte is developed by mixing a precursor mixture with molten salt, calcining the mixture to form a molten salt-coated solid electrolyte, and then pelletizing the resulting powder to create a thermocell with a core-shell structure, where the molten salt acts as an insulating layer at room temperature and enhances ionic conductivity at high temperatures.

Benefits of technology

This approach reduces the risk of leakage, improves ionic conductivity, and extends the storage life of thermocells, while simplifying the manufacturing process and reducing costs by omitting the washing step.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024003476_03102024_PF_FP_ABST
    Figure KR2024003476_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a composite solid electrolyte, a thermal battery comprising same, and a manufacturing method therefor. An embodiment of the present invention provides a manufacturing method for a composite solid electrolyte, the method comprising the steps of: mixing a precursor mixture and a molten salt to form a molten salt-precursor mixture; calcining the molten salt-precursor mixture to form a molten salt-coated solid electrolyte mixture; and pulverizing the molten salt-coated solid electrolyte mixture to obtain a composite solid electrolyte powder.
Need to check novelty before this filing date? Find Prior Art

Description

Composite solid electrolyte, thermal battery including same, and method for manufacturing same

[0001] The present invention relates to a composite solid electrolyte, a thermal battery including the same, and a method for manufacturing the same.

[0002] A thermal battery is a non-rechargeable battery that is activated when an electrically insulating solid-state molten salt melts at high temperatures and transforms into an ionically conductive liquid electrolyte. Eutectic salts, such as LiF-LiCl-LiBr and LiCl-KCl, which are most commonly used as electrolytes in thermal batteries, have high ion conductivity but a high melting point of 300 to 450°C. Eutectic salts are insulating in their solid state, but can be conductive when melted into a liquid state. Thermal batteries can be stored in an inactive state at room temperature and activated at about 500°C, when the solid-state eutectic salt melts and transforms into a liquid electrolyte. The activated thermal battery can then be slowly cooled, and operation can be halted when the liquid electrolyte transforms back into a solid state.

[0003] The molten salt may be provided in a form impregnated in a binder including sand, porous materials, metal foam, etc. (U.S. Patent Publication No. 2016-0072153, Japanese Patent Publication No. 6592030, Korean Patent Publication No. 10-1750203, U.S. Patent Publication No. 10,998,583, Korean Patent Publication No. 10-2143173).

[0004] Conventional thermoelectric cells have problems in that when the molten salt melts and becomes a liquid electrolyte, the electrolyte leaks, increasing internal resistance or causing a short circuit. The present invention aims to solve these and other problems, and provides a composite solid electrolyte with high ionic conductivity, a thermoelectric cell including the same, and a method for manufacturing the same. However, these tasks are exemplary and should not be construed as limiting the scope of the present invention.

[0005] According to one aspect of the present invention, a method for producing a composite solid electrolyte is provided, comprising the steps of mixing a precursor mixture and a molten salt to form a molten salt-precursor mixture, calcining the molten salt-precursor mixture to form a solid electrolyte mixture coated with molten salt, and pulverizing the molten salt-coated solid electrolyte mixture to obtain a composite solid electrolyte powder.

[0006] In one embodiment, the molten salt may be LiF-LiCl-LiBr, LiCl-KCl, LiF-LiBr-KBr, LiBr-KBr-RbCl, or mixtures thereof.

[0007] In one embodiment, the precursor mixture may include a raw material composition containing lithium elements, lanthanum elements, and zirconium elements.

[0008] In one embodiment, the precursor mixture further comprises an additive, wherein the additive may comprise one or more of tantalum oxide and strontium carbonate.

[0009] In one embodiment, the precursor mixture may include a raw material composition containing lithium element, phosphorus element, and sulfur element.

[0010] In one embodiment, the weight ratio of the molten salt to the molten salt-precursor mixture may be from 10 wt% to 80 wt%, and the weight ratio of the precursor mixture may be from 20 wt% to 90 wt%.

[0011] In one embodiment, the weight ratio of the molten salt to the molten salt-precursor mixture may be 30 wt% to 80 wt%, and the weight ratio of the precursor mixture may be 20 wt% to 70 wt%.

[0012] In one embodiment, the calcination temperature of the molten salt-precursor mixture may be from 550° C. to 1,150° C.

[0013] In one embodiment, the step of forming the solid electrolyte mixture coated with the molten salt may include the step of calcining the molten salt-precursor mixture to form a mixture of a liquid molten salt and a solid electrolyte, and the step of solidifying the mixture to separate an upper salt including the molten salt and a lower salt including the solid electrolyte mixture coated with the molten salt.

[0014] According to another aspect of the present invention, a composite solid electrolyte manufactured according to any one of the above-described methods for manufacturing a composite solid electrolyte is provided.

[0015] According to another aspect of the present invention, a thermal battery is provided, comprising: a negative electrode current collector; a negative electrode layer disposed on an upper portion of the negative electrode current collector; a composite solid electrolyte layer disposed on an upper portion of the negative electrode layer; a positive electrode layer disposed on an upper portion of the solid electrolyte layer; and a heat source disposed on an upper portion of the positive electrode layer, wherein the composite solid electrolyte layer is formed by mixing a precursor mixture and a molten salt to form a molten salt-precursor mixture, calcining the molten salt-precursor mixture to form a solid electrolyte mixture coated with the molten salt, and pelletizing a composite solid electrolyte powder obtained by pulverizing the solid electrolyte mixture coated with the molten salt.

[0016] Other aspects, features and advantages other than those described above will become apparent from the following drawings, claims and detailed description of the invention.

[0017] According to one embodiment of the present invention, as described above, a composite solid electrolyte coated with a molten salt and having high ionic conductivity, and a thermal battery including the same, can be realized. Furthermore, the method for manufacturing a composite solid electrolyte according to one embodiment of the present invention simplifies the process by omitting the washing step in the solid electrolyte synthesis step, thereby obtaining a high-quality composite solid electrolyte at a low cost. Of course, the scope of the present invention is not limited by these effects.

[0018] FIG. 1 is a schematic diagram illustrating a unit cell of a thermoelectric cell including a composite solid electrolyte according to one embodiment of the present invention.

[0019] FIG. 2 is a block diagram schematically illustrating a method for manufacturing a composite solid electrolyte according to one embodiment of the present invention.

[0020] Figure 3 is a schematic drawing illustrating a molten salt-precursor mixture, and Figure 4 is a schematic drawing illustrating a solid electrolyte mixture coated with molten salt.

[0021] FIG. 5 is a drawing for explaining a composite solid electrolyte layer obtained by uniaxially pressing and molding the solid electrolyte mixture coated with the molten salt obtained in FIG. 4.

[0022] Figure 6 is a drawing for explaining a precipitation separation method of a solid electrolyte mixture coated with a molten salt.

[0023] Fig. 7a is a graph showing the results of X-ray diffraction analysis of a composite solid electrolyte manufactured using a LiBr-LiCl-LiF eutectic salt, and Fig. 7b is a graph showing the results of X-ray diffraction analysis of a composite solid electrolyte manufactured using a LiCl-KCl eutectic salt.

[0024] The present invention is capable of various modifications and embodiments. Specific embodiments are illustrated in the drawings and described in detail in the detailed description. The effects and features of the present invention, as well as the methods for achieving them, will become clearer with reference to the embodiments described in detail below, along with the drawings. However, the present invention is not limited to the embodiments disclosed below and can be implemented in various forms.

[0025] Hereinafter, embodiments of the present invention will be described in detail with reference to the attached drawings. When describing with reference to the drawings, identical or corresponding components are given the same reference numerals and redundant descriptions thereof will be omitted.

[0026] In this specification, the terms first, second, etc. are not used in a limiting sense, but are used for the purpose of distinguishing one component from another.

[0027] In this specification, singular expressions include plural expressions unless the context clearly indicates otherwise.

[0028] In this specification, terms such as “include” or “have” mean that a feature or component described in the specification exists, and do not preclude the possibility that one or more other features or components may be added.

[0029] As used herein, the terms "about" or "approximately" include the stated value and may indicate an acceptable range of deviation, determined by taking into account errors associated with the manufacturing or measurement method, relative to the stated value. For example, as used herein, the term "about" may mean within ±20%, ±10%, or ±5% of the stated value.

[0030] In some embodiments of this specification, where implementations are otherwise feasible, specific process sequences may be performed in a different order than described. For example, two processes described in succession may be performed substantially simultaneously, or in a reverse order from the described order.

[0031] FIG. 1 is a schematic diagram illustrating a unit cell of a thermoelectric cell including a composite solid electrolyte according to one embodiment of the present invention.

[0032] Referring to FIG. 1, a unit cell (100) of a thermal battery including a composite solid electrolyte according to one embodiment of the present invention may include a negative current collector (110), a negative electrode (120), a composite solid electrolyte layer (130), a positive electrode (140), and a heat source (150).

[0033] Each of the negative electrode current collector (110), negative electrode (120), composite solid electrolyte layer (130), positive electrode (140), and heat source (150) is provided in the form of pellets and can be sequentially stacked.

[0034] The negative electrode collector (110) may include a metal material. For example, the negative electrode collector (110) may include stainless steel or nickel (Ni).

[0035] The negative electrode (120) may be disposed on the negative electrode current collector (110). The negative electrode (120) may include a lithium-silicon alloy or pure lithium. In one embodiment, the negative electrode (120) may be manufactured in a pellet shape by mixing iron powder into pure lithium. In another embodiment, the negative electrode (120) may be manufactured by impregnating pure lithium into a metal foam having a plurality of pores.

[0036] A composite solid electrolyte layer (130) may be disposed on the cathode (120). The composite solid electrolyte layer (130) may be formed by mixing a precursor mixture and a molten salt to form a molten salt-precursor mixture, calcining the formed molten salt-precursor mixture at a temperature range of about 550°C to about 1,150°C to form a solid electrolyte mixture coated with a molten salt, and pelletizing the obtained composite solid electrolyte powder by pulverizing the molten salt-coated solid electrolyte mixture.

[0037] In one embodiment, the precursor mixture may include a raw material composition containing lithium elements, lanthanum elements, and zirconium elements. In another embodiment, the precursor mixture may include a raw material composition containing lithium elements, phosphorus elements, and sulfur elements.

[0038] The molten salt may be a eutectic salt such as LiF-LiCl-LiBr, LiCl-KCl, LiF-LiBr-KBr, LiBr-KBr-RbCl or a mixture thereof.

[0039] An anode (140) may be placed on the composite solid electrolyte layer (130). The anode (140) may include iron sulfide (FeS2), cobalt sulfide (CoS2), nickel sulfide (NiS2), iron fluoride (FeF3), or a combination thereof.

[0040] A heat source (150) may be placed on the anode (140). In this regard, FIG. 1 illustrates that the heat source (150) is placed on the anode (140), but the placement of the heat source (150) may be changed to effectively activate the thermoelectric cell.

[0041] A thermoelectric cell may include one or more unit cells (100). For example, one thermoelectric cell may have a structure in which a plurality of unit cells (100) are stacked and connected in series.

[0042] FIG. 2 is a block diagram schematically illustrating a method for manufacturing a composite solid electrolyte according to one embodiment of the present invention.

[0043] Referring to FIG. 2, a method for manufacturing a composite solid electrolyte according to one embodiment of the present invention may include a step of forming a molten salt-precursor mixture (S10), a step of forming a solid electrolyte mixture coated with molten salt (S20), and a step of obtaining a composite solid electrolyte powder (S30).

[0044] The step of forming a molten salt-precursor mixture (S10) may be a step of mixing the precursor mixture and the molten salt.

[0045] The precursor mixture may be a raw material composition capable of synthesizing a lithium-containing oxide-based solid electrolyte or a lithium-containing sulfide-based solid electrolyte when calcined with a molten salt.

[0046] In one embodiment, the precursor mixture may include a raw material composition for synthesizing an oxide-based solid electrolyte including lithium. For example, the precursor mixture may include a raw material composition containing lithium element, lanthanum element, and zirconium element. The oxide-based solid electrolyte including lithium may be Li 6.5 La3Zr 2-x Ta x O 12 (x=0.3~0.7)(hereinafter, LLZO). The LLZO solid electrolyte has excellent stability at high temperatures.

[0047] In another embodiment, the precursor mixture may include a raw material composition for synthesizing a lithium-containing sulfide-based solid electrolyte. For example, the precursor mixture may include a raw material composition containing lithium, phosphorus, and sulfur. The lithium-containing sulfide-based solid electrolyte may be argyrodite.

[0048] The precursor mixture may further include an additive for doping the solid electrolyte. For example, the additive may include one or more of tantalum oxide (Ta2O5) and strontium carbonate (SrCO3).

[0049] The molten salt may include a eutectic salt that melts above a certain temperature. The molten salt may be a material that does not react with the cathode and anode of the thermoelectric cell and melts at a temperature lower than the decomposition temperatures of the cathode and anode materials. In one embodiment, the molten salt may be LiF-LiCl-LiBr, LiCl-KCl, LiF-LiBr-KBr, LiBr-KBr-RbCl, or a mixture thereof.

[0050] The precursor mixture may be prepared in a solid powder form. In one embodiment, the molten salt may be prepared in a solid powder form and uniformly mixed with the precursor mixture through a ball milling process. In another embodiment, the molten salt may be heat treated at a temperature ranging from about 450°C to about 650°C so that it is at least partially molten and mixed with the precursor mixture.

[0051] In one embodiment, the molten salt may have a weight ratio of about 10 wt% to about 50 wt% relative to the molten salt-precursor mixture, and the precursor mixture may have a weight ratio of about 50 wt% to 90 wt% relative to the molten salt-precursor mixture. In such a case, the process of separating and removing excess molten salt after the calcination process may be omitted.

[0052] In another embodiment, the molten salt precursor mixture may include an excess of molten salt. The molten salt may have a weight ratio of about 30 wt % to about 80 wt % relative to the molten salt precursor mixture, and the precursor mixture may have a weight ratio of about 20 wt % to 70 wt % relative to the molten salt-precursor mixture.

[0053] In another embodiment, the molten salt can have a weight ratio of about 10 wt % to about 80 wt % with respect to the molten salt precursor mixture, and the precursor mixture can have a weight ratio of about 20 wt % to 90 wt % with respect to the molten salt-precursor mixture.

[0054] The step (S20) of forming a solid electrolyte mixture coated with a molten salt may be a step of forming a solid electrolyte mixture coated with a molten salt by calcining a molten salt-precursor mixture.

[0055] The molten salt-precursor mixture can be calcined at a temperature in the range of about 550° C. to about 1,150° C. to grow solid electrolyte crystals. In one embodiment, the calcination of the molten salt-precursor mixture can be performed at a lower temperature in the range of about 800° C. to about 1,000° C.

[0056] When synthesizing a solid electrolyte using a conventional solid-state synthesis method, a high-temperature heat treatment process of 1,100°C or higher is required, which causes problems such as deviation from the stoichiometric composition of the solid electrolyte due to volatilization of lithium, or formation of secondary phases. On the other hand, the method for manufacturing a composite solid electrolyte according to embodiments of the present invention grows solid electrolyte crystals with only one heat treatment at a relatively low temperature, thereby enabling the synthesis of a high-quality solid electrolyte at low cost.

[0057] An additive for doping a solid electrolyte can increase the concentration of lithium ion conducting channels and lithium vacancies in the solid electrolyte through chemical substitution of elements during the growth of the solid electrolyte crystal. For example, when the solid electrolyte is LLZO, the strontium element in the additive can be substituted with a lanthanum element, and the tantalum element in the additive can be substituted with a zirconium element.

[0058] In one embodiment, when calcining the molten salt-precursor mixture, an excess of molten salt may be added. For example, molten salt may be added in an amount of about 30 wt% to 100 wt% based on the molten salt-precursor mixture. Adding more molten salt can compensate for lithium element volatilization during the heat treatment process, thereby improving the synthesis rate of the solid electrolyte.

[0059] Calcination of the molten salt-precursor mixture can be performed within a time range of about 2 to about 10 hours. If the calcination process time is less than 2 hours, individual grains may not grow smoothly. If the calcination process time exceeds 10 hours, grain coarsening may deteriorate properties such as ionic conductivity.

[0060] In one embodiment, the step (S20) of forming a solid electrolyte mixture coated with molten salt may include a step of calcining a molten salt-precursor mixture to form a mixture of a liquid molten salt and a solid electrolyte, and a step of solidifying the mixture to separate an upper salt including the molten salt and a lower salt including a solid electrolyte mixture coated with the molten salt.

[0061] When the solid electrolyte is LLZO, the density of the solid electrolyte (5.26 g / cm 3 ) is the density of LiCl-KCl (2.02 g / cm 3 ) and LiF-LiCl-LiBr (2.92 g / cm 3 ) may be larger. Therefore, when the mixture is slowly cooled, a solid electrolyte with a high density may precipitate, and only the remaining molten salt used in the synthesis may be located at the upper portion of the mixture. Therefore, by removing the solidified upper salt, a solid electrolyte mixture coated with molten salt may be obtained. Here, the position of the cutting line separating the upper salt and the lower salt may be adjusted according to the amount of molten salt contained in the final composite solid electrolyte powder.

[0062] The step (S30) of obtaining a composite solid electrolyte powder may be a step of obtaining a composite solid electrolyte powder by pulverizing a solid electrolyte mixture coated with a molten salt.

[0063] The finally obtained composite solid electrolyte powder may have a core-shell structure in which a molten salt is coated on the surface of the solid electrolyte particles.

[0064] Although not shown in FIG. 2, the method for manufacturing a composite solid electrolyte according to one embodiment of the present invention may further include a step of pelletizing the composite solid electrolyte powder.

[0065] In the step of pelletizing the composite solid electrolyte powder, the composite solid electrolyte powder is filled into a mold, heat-treated at about 150° C. to about 300° C., and pressurized to produce a pelletized composite solid electrolyte layer (130, see Fig. 1). The molten salt coated on the surface of the solid electrolyte particles can combine with each other in the pelletizing step to form a high-density and high-strength structure.

[0066] Fig. 3 is a schematic diagram illustrating a molten salt-precursor mixture, and Fig. 4 is a schematic diagram illustrating a solid electrolyte mixture coated with molten salt. Fig. 3 schematically illustrates a molten salt-precursor mixture (M1) formed in a step of forming a molten salt-precursor mixture (S10, see Fig. 2), and Fig. 4 schematically illustrates a solid electrolyte mixture (M2) coated with molten salt formed in a step of forming a solid electrolyte mixture (S20, see Fig. 2).

[0067] Referring to FIG. 3, the molten salt-precursor mixture (M1) may include solid precursor mixtures (PC) and molten salts (ES).

[0068] The precursor mixture (PC) may be a raw material composition containing lithium elements, lanthanum elements, and zirconium elements. For example, the precursor mixture (PC) may include lithium carbonate (Li2CO3), lanthanum oxide (La2O3), and zirconium oxide (ZrO2). In one embodiment, lithium carbonate, which has high volatility characteristics, may be added in excess to ensure that the composition of the ultimately formed solid electrolyte crystal does not deviate from the desired composition.

[0069] Alternatively, the precursor mixtures (PCs) may be raw material compositions containing lithium elements, phosphorus elements, and sulfur elements. In one embodiment, argyrodite (Li6PS5Cl) may be synthesized using a molten salt synthesis method. In this case, the precursor mixtures (PCs) together with the molten salt may further include an additive. In this case, the additive may include one or more of lithium sulfide (Li2S), phosphorus sulfide (P2S5), lithium chloride (LiCl), and the like.

[0070] The molten salts (ES) may be prepared in a solid powder form and mixed with the precursor mixture (PC). Alternatively, the molten salts (ES) may be heat treated at a temperature in the range of about 450°C to about 650°C so as to be mixed with the precursor mixture in a state in which at least a portion of the ES is molten.

[0071] Referring to FIG. 4, the molten salt-coated solid electrolyte mixture (M2) may include molten salts (ES) and molten salt-coated solid electrolyte powder (EP). The molten salt-coated solid electrolyte powder (EP) may have a core-shell structure in which a core (C), which is a solid electrolyte particle, is coated with molten salt to form a molten salt shell (SH).

[0072] The core (C) may include solid electrolyte particles having uniform crystallinity. As described above, the solid electrolyte particles may be an oxide-based solid electrolyte containing lithium or a sulfide-based solid electrolyte containing lithium. For example, the core (C) may include Li 7-x La3Zr 2-xTa x O 12 (x=0.3~0.7) or may include argyrodite (Li6PS5Cl) crystals.

[0073] The solid electrolyte particles can prevent or reduce leakage of the molten salt even when the thermoelectric cell is in operation and the molten salt is melted.

[0074] Conventional solid electrolyte synthesis methods required a primary heat treatment performed at about 900°C and a secondary heat treatment performed at about 1130°C. In contrast, embodiments of the present invention utilize a molten salt, thereby enabling the synthesis of solid electrolyte particles having excellent crystallinity with only a single heat treatment at a low temperature of about 550°C to about 1,150°C.

[0075] The molten salt shell (SH) is an insulating layer that prevents self-discharge of solid electrolyte particles at room temperature, thereby increasing the storage life of the thermoelectric cell to more than 10 years. Furthermore, the molten salt shell (SH) melts at the operating temperature of the thermoelectric cell and exhibits high ionic conductivity, thereby improving the output characteristics of the thermoelectric cell.

[0076] The molten salt-coated solid electrolyte mixture (M2) may further include molten salt (ES) particles that are not coated on the solid electrolyte particles.

[0077] In one embodiment, a solid electrolyte mixture (M2) coated with a molten salt can be used as an electrolyte for a thermoelectric cell without a subsequent processing step such as sintering. Therefore, the manufacturing cost of the thermoelectric cell can be reduced.

[0078] FIG. 5 is a drawing for explaining a composite solid electrolyte layer obtained by uniaxially pressing and molding the solid electrolyte mixture coated with the molten salt obtained in FIG. 4.

[0079] As described above, the molten salt-coated solid electrolyte mixture (M2) may have a core-shell structure in which the molten salt coats the core (C), which is a solid electrolyte particle, to form a molten salt shell (SH).

[0080] Referring to Fig. 5, when a solid electrolyte mixture (M2) coated with molten salt is pressurized in a single-axis press, a composite solid electrolyte layer (130) with high density can be manufactured as shown in Fig. 5. The molten salt and the molten salt shell (SH) of each of the molten salt and molten salt-coated solid electrolyte powders (EP) forming the composite solid electrolyte layer (130) can be combined with each other to form a high-density and high-strength structure.

[0081] Figure 6 is a drawing for explaining a precipitation separation method of a solid electrolyte mixture coated with a molten salt.

[0082] Referring to FIG. 6, the molten salt-coated solid electrolyte mixture (M2) may further include molten salt (ES) and molten salt-coated solid electrolyte powder (EP).

[0083] In general, since the density of solid electrolyte particles is greater than the density of molten salt, when the mixture is slowly cooled, solid electrolyte powder coated with molten salt may be precipitated at the bottom of the mixture, as illustrated in Fig. 6. The solid electrolyte mixture (M2) coated with molten salt may be solidified and separated into an upper salt (S1) containing only molten salt (ES) and a lower salt (S2) containing molten salt (ES) and solid electrolyte powder coated with molten salt (EP).

[0084] Depending on the amount of molten salt to be contained in the composite solid electrolyte powder to be formed, the position of the cutting line (CL) for separating the upper salt (S1) and the lower salt (S2) can be adjusted. By removing the upper salt (S1) on the cutting line (CL), unnecessary molten salt (ES) can be removed.

[0085] Therefore, not only can solid electrolyte particles having excellent crystal phases be grown at low temperatures using molten salt, but unnecessary molten salt can be removed, leaving only an appropriate amount of molten salt without a complex washing process.

[0086] Conventional solid electrolyte layers have a temperature of about 10 -4 S / cm to about 10 -3 It has an ionic conductivity in the range of S / cm and a conductivity of about 10 at high temperatures above 300 ℃. -5 S / cm to about 10 -2 It has an ionic conductivity in the range of S / cm.

[0087] The composite solid electrolyte layer (130) according to the embodiment of the present invention has a temperature of about 10 -4 It can reduce self-discharge of the thermal battery by having a low ionic conductivity of S / cm. In addition, the composite solid electrolyte layer (130) melts the molten salt on the surface at a high temperature of 300°C or higher, and the temperature is about 10 -2 It has a high ionic conductivity of S / cm, which can greatly improve the output characteristics of the thermoelectric cell.

[0088] In addition, the latent heat of fusion of the molten salt included in the composite solid electrolyte layer (130) can reduce the rapid thermal shock at the initial stage of operation of the thermal battery, thereby improving the thermal stability of the thermal battery.

[0089] Fig. 7a is a graph showing the results of X-ray diffraction analysis of a composite solid electrolyte manufactured using LiBr-LiCl-LiF molten salt, and Fig. 7b is a graph showing the results of X-ray diffraction analysis of a composite solid electrolyte manufactured using LiCl-KCl molten salt.

[0090] Comparative Example 1 (C1) of Fig. 7a is a mixture simply mixed with LiF-LiCl-LiBr molten salt powder and LLZO solid electrolyte powder. Example 1 (E1) is a composite solid electrolyte powder obtained by calcining LiF-LiCl-LiBr molten salt powder and a precursor mixture at 1,000°C, Example 2 (E2) is a composite solid electrolyte powder obtained by calcining LiF-LiCl-LiBr molten salt powder and a precursor mixture at 950°C, and Example 3 (E3) is a composite solid electrolyte powder obtained by calcining LiF-LiCl-LiBr molten salt powder and a precursor mixture at 900°C. Here, the precursor mixture was prepared by stoichiometrically balancing lithium carbonate, lanthanum oxide, zirconium oxide, and an additive. The additive includes tantalum oxide and strontium carbonate. Each molten salt was melted and heat-treated at 550°C and then mixed with the precursor mixture.

[0091] Comparative Example 2 (C2) of Fig. 7b is a mixture simply mixed with LiCl-KCl molten salt powder and LLZO solid electrolyte powder. Example 4 (E4) is a composite solid electrolyte powder obtained by calcining LiCl-KCl molten salt powder and a precursor mixture at 1,000°C, Example 5 (E5) is a composite solid electrolyte powder obtained by calcining LiCl-KCl molten salt powder and a precursor mixture at 950°C, and Example 6 (E7) is a composite solid electrolyte powder obtained by calcining LiCl-KCl molten salt powder and a precursor mixture at 900°C.

[0092] Referring to FIGS. 7a and 7b, it was confirmed that the composite solid electrolyte manufactured according to the embodiments of the present invention had well-grown LLZO solid electrolyte crystals and that there was no formation of a second phase depending on the calcination temperature.

[0093] ClassificationLiCl-KClLiF-LiCl-LiBrComparative Example 3Example 7Comparative Example 4Example 8Strength (gf)31592543

[0094] Table 1 shows the results of measuring the mechanical strength of composite solid electrolyte layers manufactured according to comparative examples and examples. The composite solid electrolyte layer was formed into a disk shape with a diameter of 56.2 mm and a thickness of 0.43 mm, and the mechanical strength was measured in a push-pull gauge by dividing it into four parts. In Comparative Example 3, a composite solid electrolyte layer was formed by simply mixing LiCl-KCl molten salt powder and solid electrolyte powder and then pelletizing them, and in Example 7, a LiCl-KCl molten salt-precursor mixture was calcined to form a solid electrolyte mixture coated with molten salt, and then the resulting composite solid electrolyte powder was pelletized to form a composite solid electrolyte layer. In Comparative Example 4, a composite solid electrolyte layer was formed by simply mixing LiF-LiCl-LiBr molten salt powder and solid electrolyte powder and then pelletizing them, and in Example 8, a LiF-LiCl-LiBr molten salt-precursor mixture was calcined to form a solid electrolyte mixture coated with molten salt, and then the resulting composite solid electrolyte powder was pelletized to form a composite solid electrolyte layer. In the present invention It was confirmed that the composite solid electrolyte layer manufactured according to the examples had a higher strength than the composite solid electrolyte layer manufactured according to the comparative examples, as the molten salt on the surface of the solid electrolyte was bonded to each other during the pelletization process as described above.

[0095] While the present invention has been described with reference to the embodiments illustrated in the drawings, these are merely exemplary, and those skilled in the art will understand that various modifications and equivalent alternative embodiments are possible. Therefore, the true technical protection scope of the present invention should be determined by the technical spirit of the appended claims.

Claims

1. A step of forming a molten salt-precursor mixture by mixing a precursor mixture and a molten salt; A step of calcining the molten salt-precursor mixture to form a solid electrolyte mixture coated with molten salt; and A method for producing a composite solid electrolyte, comprising the step of pulverizing a solid electrolyte mixture coated with the molten salt to obtain a composite solid electrolyte powder.

2. In paragraph 1, A method for producing a composite solid electrolyte, wherein the molten salt is LiF-LiCl-LiBr, LiCl-KCl, LiF-LiBr-KBr, LiBr-KBr-RbCl or a mixture thereof.

3. In paragraph 1, A method for producing a composite solid electrolyte, wherein the precursor mixture comprises a raw material composition containing lithium elements, lanthanum elements, and zirconium elements.

4. In paragraph 1, The above precursor mixture further comprises an additive. A method for producing a composite solid electrolyte, wherein the additive comprises at least one of tantalum oxide and strontium carbonate.

5. In paragraph 1, A method for producing a composite solid electrolyte, wherein the precursor mixture comprises a raw material composition containing lithium element, phosphorus element, and sulfur element.

6. In paragraph 1, A method for producing a composite solid electrolyte, wherein the weight ratio of the molten salt to the molten salt-precursor mixture is 10 wt% to 80 wt%, and the weight ratio of the precursor mixture is 20 wt% to 90 wt%.

7. In paragraph 6, A method for producing a composite solid electrolyte, wherein the weight ratio of the molten salt to the molten salt-precursor mixture is 30 wt% to 80 wt%, and the weight ratio of the precursor mixture is 20 wt% to 70 wt%.

8. In paragraph 1, A method for producing a composite solid electrolyte, wherein the calcination temperature of the molten salt-precursor mixture is 550°C to 1,150°C.

9. In paragraph 1, The step of forming the solid electrolyte mixture coated with the molten salt is as follows: A step of calcining the above molten salt-precursor mixture to form a mixture of a liquid molten salt and a solid electrolyte; and A method for producing a composite solid electrolyte, comprising: a step of solidifying the above mixture to separate an upper salt containing the molten salt and a lower salt containing a solid electrolyte mixture coated with the molten salt.

10. A composite solid electrolyte manufactured according to any one of claims 1 to 9.

11. Negative current collector; A cathode layer disposed on top of the above cathode current collector; A composite solid electrolyte layer disposed on top of the cathode layer; A cathode layer disposed on top of the solid electrolyte layer; and Including a heat source placed on the upper part of the above anode layer, A thermal battery in which the composite solid electrolyte layer is formed by mixing a precursor mixture and a molten salt to form a molten salt-precursor mixture, calcining the molten salt-precursor mixture to form a solid electrolyte mixture coated with the molten salt, and pelletizing the obtained composite solid electrolyte powder by pulverizing the molten salt-coated solid electrolyte mixture.

Citation Information

Patent Citations

  • Method for preparing garnet type solid electrolyte Li7La3Zr2O12 block by molten salt method

    CN108695551A

  • A thermal batteries using a eutectic salt coated solid-electrolyte and a manufacturing method therefor

    KR101739803B1

  • Composite solid electrolyte without self-discharge, battery unit cell having the same, and Method for manufacturing the same

    KR102143173B1

  • Electric rotating machine and manufacturing method thereof

    KR102191727B1

  • nano-cellulose materials for 3d bioprinting, Method for preparing nano-cellulose and applications thereof

    KR102471982B1