Lithium metal battery, and method for manufacturing lithium metal battery anode included therein
The integration of a porous layer with a specific structure into the negative electrode of lithium metal batteries addresses dendrite formation and electrolyte consumption issues, enhancing the battery's cycle characteristics and lifespan.
Patent Information
- Application Number
- PCT/KR2024/003731
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-12-27
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-03
AI Technical Summary
Lithium metal batteries using lithium as a negative electrode face issues with dendrite formation and electrolyte consumption, leading to short circuits and rapid deterioration of cycle characteristics due to side reactions and impurity accumulation on the electrode surface.
Incorporating a porous layer with a specific structure into the negative electrode active material layer, where one region is exposed and another is inserted, to create a spaced configuration between the current collector and the active material, preventing dendrite growth and reducing electrolyte consumption.
This configuration enhances the cycling characteristics and lifespan of lithium metal batteries by suppressing dendrite formation and minimizing electrolyte consumption, thereby improving the battery's stability and performance.
Smart Images

Figure KR2024003731_03102024_PF_FP_ABST
Abstract
Description
Method for manufacturing a lithium metal battery and a negative electrode for a lithium metal battery included therein
[0001] It relates to a method for manufacturing a lithium metal battery and a negative electrode for a lithium metal battery included therein.
[0002] Lithium metal batteries currently on the market primarily use carbon-based anode materials, such as graphite. Carbon-based anode materials exhibit no volume change during charge and discharge, contributing to the stability of lithium metal batteries. Graphite's theoretical capacity is relatively small, at around 372 mAh / g.
[0003] Lithium metal can be used as an anode active material. Lithium metal has a very high theoretical electrical capacity of approximately 3860 mAh / g. During charge / discharge, lithium metal can form dendrites on its surface due to side reactions with the electrolyte. These dendrites can then grow and cause short circuits between the anode and cathode. Consequently, the lifespan of lithium metal batteries containing lithium metal deteriorates.
[0004] A method for improving the life characteristics of a lithium metal battery containing lithium metal is required.
[0005] One aspect is to provide a lithium metal battery comprising a negative electrode for a lithium metal battery of a novel structure.
[0006] Another aspect is to provide a method for manufacturing a negative electrode for a lithium metal battery included in a lithium metal battery.
[0007] According to the implementation example
[0008] A positive electrode; a negative electrode; and an electrolyte disposed between the positive electrode and the negative electrode,
[0009] The above negative electrode is a negative electrode current collector;
[0010] A negative electrode active material layer disposed on the negative electrode current collector; and
[0011] A porous layer including a porous structure,
[0012] The porous layer includes a first region exposed on the negative electrode active material layer and a second region inserted into the negative electrode active material layer,
[0013] A lithium metal battery is provided, wherein the negative electrode active material layer includes a second region in which the porous layer is inserted and a third region in which the porous layer is not inserted.
[0014] According to another implementation example,
[0015] As a method for manufacturing the above cathode,
[0016] A step of preparing a negative electrode structure including a negative electrode current collector, a negative electrode active material layer disposed on the negative electrode current collector, and a porous layer disposed on the negative electrode active material layer; and
[0017] A method for manufacturing a negative electrode for a lithium metal battery is provided, including a step of rolling the negative electrode structure using a roll press and inserting at least a portion of the porous layer into the negative electrode active material layer.
[0018] According to one aspect, it is possible to provide a lithium metal battery with improved cycle characteristics by employing a cathode including a porous layer.
[0019] Figure 1 is a cross-sectional view of a lithium metal battery according to an exemplary embodiment.
[0020] Figure 2 is a cross-sectional view of a cathode according to an exemplary embodiment.
[0021] Figure 3 is a cross-sectional view of a cathode according to another exemplary embodiment.
[0022] Figure 4 is a schematic diagram of a lithium metal battery according to an exemplary embodiment.
[0023] Figure 5 is a schematic diagram of a lithium metal battery according to an exemplary embodiment.
[0024] Figure 6 is a schematic diagram of a lithium metal battery according to an exemplary embodiment.
[0025] During the charge and discharge process of a lithium metal battery using lithium metal as the anode active material, a lithium-containing metal layer is precipitated and dissolved between the anode current collector and the electrolyte layer. As the lithium metal battery is repeatedly charged and discharged, the anode active material layer contains impurities remaining in the electrode and decomposition products of the electrolyte. Consequently, the inclusion of these impurities causes the surface of the anode active material layer to become rough and hard. Lithium dendrites are precipitated on the lithium-containing metal layer with this rough surface. These lithium dendrites continuously grow during the charge and discharge process, which can cause a short circuit between the positive and negative electrodes. Furthermore, as the charge and discharge of the lithium metal battery is repeated, the electrolyte is continuously consumed due to side reactions, which can rapidly deteriorate the cycle characteristics of the lithium metal battery.
[0026] A lithium metal battery according to one aspect includes a porous layer, and a negative electrode active material layer is disposed between the porous layer and the negative electrode current collector, so that the porous layer and the negative electrode current collector have a negative electrode spaced apart from each other, thereby suppressing lithium dendrite formation in the negative electrode active material layer and suppressing consumption of electrolyte, thereby improving the cycle characteristics of a lithium metal battery employing such a negative electrode.
[0027]
[0028] The present inventive concept described below is capable of various modifications and embodiments. Specific embodiments are illustrated in the drawings and described in detail. However, this is not intended to limit the present inventive concept to specific embodiments, but rather to encompass all modifications, equivalents, or alternatives within the technical scope of the present inventive concept.
[0029] The terminology used below is only used to describe specific embodiments and is not intended to limit the present invention. The singular expression includes the plural expression unless the context clearly indicates otherwise. Hereinafter, the terms "comprises" or "has" and the like are intended to indicate the presence of a feature, number, step, operation, component, part, ingredient, material, or combination thereof described in the specification, but should be understood to not preclude the possibility of the presence or addition of one or more other features, numbers, steps, operations, components, parts, ingredients, materials, or combinations thereof. The " / " used below may be interpreted as "and" or "or" depending on the context.
[0030] In order to clearly express various layers and regions in the drawings, the thickness is shown enlarged or reduced. Similar parts are designated by the same drawing reference numerals throughout the specification. When a part such as a layer, film, region, or plate is said to be "on" or "above" another part throughout the specification, this includes not only cases where it is directly above the other part, but also cases where there is another part in between. Terms such as first, second, etc. may be used throughout the specification to describe various components, but the components should not be limited by the terms. The terms are used only for the purpose of distinguishing one component from another. In this specification and the drawings, components having substantially the same functional configuration are referred to by the same reference numerals, and redundant descriptions are omitted.
[0031] In the present disclosure, the "size" of a particle refers to, for example, the "particle diameter" of the particle. The "particle diameter" of a particle refers to the average diameter when the particle is spherical, and refers to the average major axis length when the particle is non-spherical. The particle diameter of a particle can be measured using a particle size analyzer (PSA). The "particle diameter" of a particle refers to, for example, the average particle diameter. The average particle diameter is, for example, the median particle diameter (D50). The median particle diameter (D50) is the size of a particle corresponding to 50% of the cumulative volume, calculated from the side of particles having a small particle size in a size distribution of particles measured by, for example, laser diffraction.
[0032] In this disclosure, “metal” includes both metals and metalloids such as silicon and germanium, in their elemental or ionic states.
[0033] In this disclosure, “alloy” means a mixture of two or more metals.
[0034] In the present disclosure, “positive electrode material” means a positive electrode material capable of undergoing lithiation and delithiation.
[0035] In the present disclosure, “negative electrode active material” means a negative electrode material capable of undergoing lithiation and delithiation.
[0036] In the present disclosure, “lithiation” and “lithiating” mean a process of adding lithium to a positive electrode active material or a negative electrode active material.
[0037] In the present disclosure, “delithiation” and “delithiate” mean a process of removing lithium from a positive electrode active material or a negative electrode active material.
[0038] In this disclosure, “charging” and “charging” mean a process of providing electrochemical energy to a battery.
[0039] In this disclosure, “discharging” and “discharging” mean the process of removing electrochemical energy from a battery.
[0040] In the present disclosure, “positive electrode” and “cathode” mean an electrode at which electrochemical reduction and lithiation occur during a discharge process.
[0041] In the present disclosure, “cathode” and “anode” mean electrodes where electrochemical oxidation and delithiation occur during a discharge process.
[0042]
[0043] Fig. 1 is a cross-sectional view of a lithium metal battery according to an exemplary embodiment. Fig. 2 is a cross-sectional view of a negative electrode according to an exemplary embodiment. Fig. 3 is a cross-sectional view of a negative electrode according to another exemplary embodiment.
[0044] Hereinafter, with reference to the drawings, a lithium metal battery including a negative electrode for a lithium metal battery and a method for manufacturing a negative electrode for a lithium metal battery according to exemplary embodiments are described in more detail.
[0045] According to one embodiment, a positive electrode (10); a negative electrode (20); and an electrolyte (30) disposed between the positive electrode (10) and the negative electrode (20), wherein the negative electrode (20) comprises a negative electrode current collector (210); a negative electrode active material layer (220) disposed on the negative electrode current collector (210); and a porous layer (230) having a porous structure, wherein the porous layer (230) comprises a first region (A1) exposed on the negative electrode active material layer and a second region (A2) inserted into the negative electrode active material layer, and the negative electrode active material layer (220) comprises a second region (A2) into which the porous layer (230) is inserted and a third region (A3) into which the porous layer (230) is not inserted. For example, the negative electrode (20) included in the lithium metal battery (1) may include a third region (A3) in which the porous layer (230) is not inserted among the negative electrode active material layers (220), so that the porous layer (230) and the negative electrode current collector (210) may be spaced apart from each other. In this case, cracks or damage that may occur within the negative electrode (20) during the process of inserting the porous layer (230) into the negative electrode active material layer (220) may be prevented. Accordingly, the cycle characteristics of the lithium metal battery (1) including the negative electrode (20) may be improved.
[0046] In addition, the first region (A1) exposed on the negative electrode active material layer among the porous layer (230) functions as a lithium host when the lithium metal battery (1) is charged, thereby effectively preventing lithium dendrites from forming on the negative electrode active material layer (220). In addition, the second region (A2) where the porous layer (230) and the negative electrode active material layer (220) overlap functions as a lithium supply source, thereby further improving the cycle characteristics of the lithium metal battery (1) including the porous layer (230).
[0047]
[0048] [cathode]
[0049] Referring to FIGS. 2 and 3, a negative electrode (20) for a lithium metal battery according to one embodiment includes a negative electrode current collector (210); a negative electrode active material layer (220) disposed on the negative electrode current collector; and a porous layer (230) having a porous structure, wherein the porous layer (230) includes a first region (A1) exposed on the negative electrode active material layer and a second region (A2) inserted into the negative electrode active material layer, and the negative electrode active material layer (220) may include a second region (A2) into which the porous layer (230) is inserted and a third region (A3) into which the porous layer is not inserted.
[0050] According to one embodiment, the thickness of the first region (A1) can satisfy 100 to 130% of Equation 1 below.
[0051] <Formula 1>
[0052] Anode current density (mAh / cm 2 ) * 4.89㎛ / (mAh / cm 2 ) * (1 / porosity of the first region)
[0053] For example, the above equation 1 means the minimum height (㎛) that can fill the first region (A1) of the porous layer (230) with lithium ions moving from the positive electrode (10) to the negative electrode (20). For example, the above 4.89 ㎛ / (mAh / cm 2 ) is the anode current density 1 mAh / cm 2 The height at which lithium is filled refers to the height at which lithium is filled. For example, when the thickness of the first region (A1) satisfies 100 to 130% of the value of the above formula 1, lithium ions moving from the positive electrode (10) to the negative electrode (20) are deposited within the first region (A1) of the porous layer (230), thereby effectively preventing lithium dendrite from being formed during the charging process.
[0054] According to one embodiment, when the lithium metal battery (1) is charged, a lithium precipitation layer (240) is formed on the negative electrode active material layer (220), and the thickness of the lithium precipitation layer (240) may be 130% or less of the thickness of the first region. For example, the thickness of the lithium precipitation layer (240) may be 100% to 130% of the thickness of the first region (A1). For example, the thickness of the lithium precipitation layer (240) may be the same as the thickness of the first region (A1).
[0055] For example, at least a portion of the lithium precipitation layer (240) may be positioned within the porous layer (230). For example, the lithium precipitation layer (240) may be positioned within the porous layer (230). In this case, since at least a portion of the lithium precipitation layer (240) is formed within the porous layer (230), uneven growth of the lithium precipitation layer (240) is prevented, and lithium dendrite formation can be effectively prevented.
[0056] According to one embodiment, the porosity of the porous structure included in the first region (A1) of the porous layer (230) may be 1 to 99%. For example, the porosity of the porous structure included in the first region (A1) of the porous layer (230) before charging may be 1 to 99%, 50 to 99%, or 50 to 90%.
[0057] According to one embodiment, the porosity of the porous structure included in the second region (A2) of the porous layer (230) may be smaller than the porosity of the porous structure included in the first region (A1). For example, the porosity of the porous structure included in the porous layer (230) may decrease as one moves from the first region (A1) to the second region (A2). For example, the porosity of the pre-filled porous structure included in the second region (A2) may be 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, 5% or less, 1% or less, or 0%.
[0058] According to one embodiment, the size of the pores included in the first region of the porous layer (230) may be 1 nm to 10 μm. For example, the size of the pores included in the first region of the porous layer (230) may be 1 nm to 5 μm, 1 nm to 3 μm, 10 nm to 10 μm, 0.1 μm to 10 μm, 0.2 μm to 10 μm, 0.5 μm to 10 μm, 1 μm to 10 μm, or 1 μm to 3 μm.
[0059] According to one embodiment, the thickness of the first region (A1) of the porous layer (230) may be 1 µm to 100 µm, and the thickness of the second region (A2) of the porous layer (230) may be 1 µm to 50 µm. For example, the thickness of the first region (A1) of the porous layer (230) may be 1 µm to 100 µm, 5 µm to 100 µm, 10 µm to 100 µm, 15 µm to 100 µm, 20 µm to 100 µm, 25 µm to 100 µm, 1 µm to 90 µm, 1 µm to 80 µm, 1 µm to 70 µm, or 25 µm to 70 µm. For example, for example, the thickness of the second region (A1) of the porous layer (230) may be 1 µm to 50 µm, 5 µm to 50 µm, 10 µm to 50 µm, 1 µm to 40 µm, 1 µm to 30 µm, 1 µm to 25 µm, or 10 µm to 25 µm.
[0060] According to one embodiment, the thickness of the second region (A2) may be 70% or less of the thickness of the negative electrode active material layer (220). According to one embodiment, the thickness of the second region (A2) may be 50% or less, 10 to 50%, or 20 to 50% of the thickness of the negative electrode active material layer (220). For example, when the thickness of the second region (A2) satisfies 70% or less of the thickness of the negative electrode active material layer (220), damage to the negative electrode (20) that may occur during the process of inserting the porous layer (230) into the negative electrode active material layer (220) can be effectively prevented. Accordingly, the life characteristics of the lithium metal battery (1) including the negative electrode (20) can be improved.
[0061] According to one embodiment, the hardness of the porous layer (230) may be greater than the hardness of the negative electrode active material layer (220). For example, hardness refers to the degree of hardness of an object and can be measured using a Brinell hardness tester, etc. For example, when the hardness of the porous layer (230) is greater than the hardness of the negative electrode active material layer (220), the porous layer (230) can be inserted more easily into the negative electrode active material layer (220), and cracks that may occur in the negative electrode (20) during the insertion process can be more effectively prevented.
[0062] According to one embodiment, the porous layer (230) includes a metal or carbon-based material, and the metal may include copper (Cu), nickel (Ni), stainless steel (SUS), iron (Fe), or cobalt (Co). For example, the metal may include copper (Cu), nickel (Ni), stainless steel (SUS), or iron (Fe). For example, the carbon-based material may include carbon steel.
[0063] According to one embodiment, the porous structure included in the porous layer (230) may include a foam structure or a mesh structure. For example, the porous structure may include a foam structure. For example, when the porous structure includes a foam structure, lithium ions can move more easily through the three-dimensional passages included in the foam structure, thereby reducing internal resistance. Accordingly, the charge / discharge efficiency of the lithium metal battery (1) can be further improved.
[0064] According to one embodiment, the porous structure included in the porous layer (230) may be acid-treated. For example, the porous structure may be acid-treated with hydrochloric acid, nitric acid, or sulfuric acid. For example, when the porous structure is acid-treated, the oxide present on the surface of the porous structure is removed, thereby increasing the proportion of metal atoms on the surface of the porous structure. Accordingly, lithium ions may be more easily oxidized and reduced within the porous structure, thereby improving the cycle characteristics and charge / discharge characteristics of the lithium metal battery (1) including the same.
[0065] According to one embodiment, the acid-treated porous structure may have a ratio of oxide peaks to metal peaks of from 50:1 to 1:1 when analyzed by X-ray photoelectron spectroscopy (XPS). For example, the acid-treated porous structure may have a ratio of oxide peaks to metal peaks of from 40:1 to 1:1, 30:1 to 1:1, 20:1 to 1:1, 50:1 to 2:1, 50:1 to 3:1, 30:1 to 2:1, or 20:1 to 3:1 when analyzed by X-ray photoelectron spectroscopy (XPS).
[0066] According to one embodiment, the porous structure may further include a coating layer formed on the surface. For example, the coating layer may include a lithium-affinity material. For example, the coating layer may include gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), or zinc (Zn). For example, the coating layer formed on the surface of the porous structure may increase reactivity with lithium ions, thereby further improving the charge / discharge efficiency of a lithium metal battery (1) including the same.
[0067]
[0068] [Cathode: Cathode active material layer]
[0069] According to one embodiment, the negative electrode active material layer (220) may include, for example, lithium foil, lithium powder, plated lithium, a carbon-based material, or a combination thereof. The negative electrode active material layer including lithium foil may be, for example, a lithium metal layer. The negative electrode active material layer including lithium powder may be introduced by coating a slurry including lithium powder and a binder, etc., on a negative electrode current collector. The binder may be, for example, a fluorine-based binder such as polyvinylidene fluoride (PVDF). The negative electrode active material layer may not include a carbon-based negative electrode active material. Therefore, the negative electrode active material layer may be formed of a metal-based negative electrode active material.
[0070] The thickness of the negative electrode active material layer (220) may be, for example, 0.1 ㎛ to 100 ㎛, 0.1 ㎛ to 80 ㎛, 1 ㎛ to 80 ㎛, or 10 ㎛ to 80 ㎛, but is not necessarily limited to this range and may be adjusted according to the required shape, capacity, etc. of the lithium metal battery. If the thickness of the negative electrode active material layer (23) increases excessively, the structural stability of the lithium metal battery may deteriorate and side reactions may increase. If the thickness of the negative electrode active material layer (220) is excessively small, the energy density of the lithium metal battery may decrease. The thickness of the lithium foil may be, for example, 1 ㎛ to 50 ㎛, 1 ㎛ to 30 ㎛, or 10 ㎛ to 30 ㎛, or 10 ㎛ to 80 ㎛. When the lithium foil has a thickness in this range, the life characteristics of the lithium metal battery can be further improved. The particle size of the lithium powder may be, for example, 0.1 ㎛ to 3 ㎛, 0.1 ㎛ to 2 ㎛, or 0.1 ㎛ to 2 ㎛. When the lithium powder has a thickness in this range, the life characteristics of the lithium metal battery can be further improved.
[0071] For example, the negative electrode active material layer (220) may include a second region (A2) in which the porous layer (230) is inserted and a third region (A3) in which the porous layer (230) is not inserted. For example, since the negative electrode active material layer (220) includes the third region (A3), the negative electrode current collector (210) and the porous layer (230) may be spaced apart from each other. Accordingly, damage to the negative electrode (20) that may occur during the process of inserting the porous layer (230) into the negative electrode active material layer (220) is effectively prevented, and since the active material included in the third region (A3) is used in the charge and discharge process, the life characteristics of the lithium metal battery may be further improved.
[0072] According to one embodiment, the thickness of the second region (A2) of the negative electrode active material layer (220) may be 70% or less of the total thickness of the negative electrode active material layer.
[0073] According to one embodiment, the thickness of the third region (A3) of the negative electrode active material layer (220) may be 30% or more of the total thickness of the negative electrode active material layer. According to one embodiment, the thickness of the third region (A3) of the negative electrode active material layer (220) may be 0.3 to 50 μm.
[0074] [Cathode: Negative current collector]
[0075] For example, the material constituting the negative electrode current collector (210) can be any material that does not react with lithium, that is, any material that does not form an alloy or compound with lithium and has conductivity. The metal substrate is, for example, a metal or an alloy. The metal substrate can be made of, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. The electrode current collector (200) can have a shape selected from, for example, a sheet, a foil, a film, a plate, a porous body, a mesoporous body, a body containing through-holes, a polygonal ring body, a mesh body, a foam body, and a non-woven body, but is not necessarily limited to these shapes, and any shape used in the relevant technical field can be used.
[0076] For example, the negative electrode current collector (210) may have a reduced thickness compared to the negative electrode current collector included in a conventional negative electrode. Therefore, the negative electrode according to the present disclosure is distinguished from a conventional electrode including a thick film current collector, for example, by including a thin film current collector. Since the electrode according to one embodiment employs a thin film current collector having a reduced thickness, the thickness of the negative electrode active material layer in the negative electrode including the thin film current collector is relatively increased. As a result, the energy density of a lithium metal battery employing such an electrode is increased. The thickness of the negative electrode current collector (210) including a metal substrate and an intermediate layer may be, for example, less than 15 um, 14.5 um or less, or 14 um or less. The thickness of the negative electrode current collector (210) may be, for example, 0.1 um to less than 15 um, 1 um to 14.5 um, 2 um to 14 um, 3 um to 14 um, 5 um to 14 um, or 10 um to 14 um.
[0077] The material constituting the negative electrode current collector (210) may be any material that does not react with lithium, i.e., does not form an alloy or compound with lithium, and has conductivity. The negative electrode current collector (210) is, for example, a metal or an alloy. The negative electrode current collector (210) may be made of, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof.
[0078] The negative electrode current collector (210) may have a form selected from, for example, a sheet, a foil, a film, a plate, a porous body, a mesoporous body, a body containing through holes, a polygonal ring body, a mesh body, a foam body, and a non-woven body, but is not necessarily limited to these forms, and any form used in the relevant technical field is possible.
[0079] The negative electrode current collector (210) may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The negative electrode current collector (210) includes a substrate, and the substrate may have a structure including, for example, a base film and a metal layer disposed on one or both sides of the base film. The above-described intermediate layer may be additionally disposed on the metal layer. The base film may include, for example, a polymer. The polymer may be, for example, a thermoplastic polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. Since the base film includes a thermoplastic polymer, the base film may melt when a short circuit occurs, thereby suppressing a rapid increase in current. The base film may be, for example, an insulator. The metal layer may include, for example, copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), or an alloy thereof. The metal layer may act as an electrochemical fuse and may be cut off in the event of an overcurrent to prevent a short circuit. The limit current and the maximum current may be controlled by adjusting the thickness of the metal layer. The metal layer may be plated or deposited on the base film. As the thickness of the metal layer decreases, the limit current and / or the maximum current of the negative electrode current collector (210) may decrease, thereby improving the stability of the lithium metal battery in the event of a short circuit. A lead tab may be added on the metal layer for connection to the outside. The lead tab may be welded to the metal layer or the metal layer / base film laminate by ultrasonic welding, laser welding, spot welding, or the like. When welding, the base film and / or the metal layer may be melted, so that the metal layer may be electrically connected to the lead tab.In order to strengthen the welding between the metal layer and the lead tab, a metal chip may be added between the metal layer and the lead tab. The metal chip may be a thin piece of the same material as the metal of the metal layer. The metal chip may be, for example, a metal foil, a metal mesh, etc. The metal chip may be, for example, aluminum foil, copper foil, SUS foil, etc. By placing the metal chip on the metal layer and then welding it with the lead tab, the lead tab may be welded to the metal chip / metal layer laminate or the metal chip / metal layer / base film laminate. During welding, the base film, the metal layer, and / or the metal chip may melt, so that the metal layer or the metal layer / metal chip laminate may be electrically connected to the lead tab. The metal chip and / or the lead tab may be added to a portion of the metal layer. The thickness of the base film may be, for example, 1 to 50 ㎛, 1.5 to 50 ㎛, 1.5 to 40 ㎛, or 1 to 30 ㎛. By having a thickness of the base film in this range, the weight of the negative electrode assembly can be more effectively reduced. The melting point of the base film can be, for example, 100 to 300°C, 100 to 250°C, or 100 to 200°C. By having a melting point in this range, the base film can be melted during the process of welding the lead tab and easily bonded to the lead tab. A surface treatment, such as corona treatment, can be performed on the base film to improve the adhesion between the base film and the metal layer. The thickness of the metal layer can be, for example, 0.01 to 3 μm, 0.1 to 3 μm, 0.1 to 2 μm, or 0.1 to μm. By having a thickness of the metal layer in this range, the stability of the negative electrode assembly can be secured while maintaining conductivity. The thickness of the metal piece can be, for example, 2 to 10 μm, 2 to 7 μm, or 4 to 6 μm. By having the metal piece in this range of thickness, the connection between the metal layer and the lead tab can be performed more easily.By having this structure, the negative electrode collector (210) can reduce the weight of the electrode and consequently improve the energy density.
[0080] According to one embodiment, the negative electrode (20) may further include an interlayer disposed between the negative electrode current collector (210) and the negative electrode active material layer (220).
[0081] According to one embodiment, the interlayer may be directly disposed on, for example, one or both surfaces of the negative electrode collector (210). Accordingly, no other layer may be disposed between the negative electrode collector (210) and the interlayer. By directly disposing the interlayer on one or both surfaces of the negative electrode collector (210), the bonding force between the negative electrode collector (210) and the negative electrode active material layer (220) may be further enhanced.
[0082] The thickness of the intermediate layer (not shown) is, for example, 30% or less of the thickness of the negative electrode current collector (210). The thickness of the intermediate layer (not shown) is, for example, 0.01 to 30%, 0.1 to 30%, 0.5 to 30%, 1 to 25%, 1 to 20%, 1 to 15%, 1 to 10%, 1 to 5%, or 1 to 3% of the thickness of the negative electrode current collector (210). The thickness of the intermediate layer (not shown) is, for example, 10 nm to 5 ㎛, 50 nm to 5 ㎛, 200 nm to 4 ㎛, 500 nm to 3 ㎛, 500 nm to 2 ㎛, 500 nm to 1.5 ㎛, or 700 nm to 1.3 ㎛. By having the above intermediate layer (not shown) with a thickness within this range, the bonding force between the negative electrode current collector (210) and the negative electrode active material layer (220) can be further improved, and an increase in interface resistance can be suppressed.
[0083] For example, the intermediate layer may include a binder. By including the binder in the intermediate layer, the bonding strength between the negative electrode current collector (210) and the negative electrode active material layer (220) may be further enhanced. The binder included in the intermediate layer (not shown) may be, for example, a conductive binder or a non-conductive binder.
[0084] The conductive binder may be, for example, an ion-conducting binder and / or an electron-conducting binder. A binder having both ion-conducting and electron-conducting properties may be classified as either an ion-conducting binder or an electron-conducting binder.
[0085] The ion-conducting binder is, for example, polystyrene sulfonate (PSS), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP, polyvinylidene fluoride-hexafluoropropylene), polyvinyl fluoride (PVF, polyvinylidene fluoride), polymethyl methacrylate (PMMA, poly(methylmethacrylate), polyethylene oxide (PEO, polyethylene oxide), polyethylene glycol (PEG), polyacrylonitrile (PAN), polytetrafluoroethylene (PTFE), polyethylenedioxythiophene (PEDOT), polypyrrole (PPY), polyacrylonitrile (PAN), polyaniline, and polyacetylene. The ion-conducting binder may include a polar functional group. Examples of the ion-conducting binder including a polar functional group include Nafion, Aquibion, etc. (Aquivion), Flemion, Gore, Aciplex, Morgane ADP, sulfonated poly(ether ether ketone) (SPEEK), sulfonated poly(arylene ether ketone ketone sulfone) (SPAEKKS), sulfonated poly(aryl ether ketone) (SPAEK), poly[bis(benzimidazobenzisoquinolinones)] (SPBIBI), poly(styrene sulfonate) (PSS), lithium 9,10-diphenylatlacene-2-sulfonate 9,10-diphenylanthracene-2-sulfonate, DPASLi +) etc. The electronically conductive binder is, for example, polyacetylene, polythiophene, polypyrrole, poly(p-phenylene), poly(phenylenevinylene), poly(phenylenesulfide), polyaniline, etc. The intermediate layer can be, for example, a conductive layer comprising a conductive polymer.
[0086] The binder included in the intermediate layer may be, for example, a fluorinated binder. The fluorinated binder included in the intermediate layer may be, for example, polyvinylidene fluoride (PVDF). The intermediate layer may be disposed on the negative electrode current collector (210) in a dry or wet manner, for example. The intermediate layer may be, for example, a binding layer including a binder.
[0087] The intermediate layer may additionally include, for example, a carbon-based conductive material. By including the carbon-based conductive material, the intermediate layer may be, for example, a conductive layer. The intermediate layer may be, for example, a conductive layer including a binder and a carbon-based conductive material.
[0088] The intermediate layer may be disposed on the negative electrode current collector (210) in a dry manner, for example, by deposition such as CVD or PVD. The intermediate layer may be disposed on the negative electrode current collector (210) in a wet manner, for example, by spin coating, dip coating, or the like. The intermediate layer may be disposed on the negative electrode current collector (210) by, for example, depositing a carbon-based conductive material on the negative electrode current collector (210) by deposition. The dry-coated intermediate layer may be made of a carbon-based conductive material and may not include a binder. Alternatively, the intermediate layer may be disposed on the negative electrode current collector by, for example, coating a composition including a carbon-based conductive material, a binder, and a solvent on the surface of the negative electrode current collector and drying it. The intermediate layer may have a single-layer structure or a multi-layer structure including a plurality of layers.
[0089]
[0090] [Lithium metal battery]
[0091] A lithium metal battery (1) according to one embodiment includes a positive electrode (10); the above-described negative electrode (20); and an electrolyte (30) disposed between the positive electrode and the negative electrode. By including the above-described negative electrode, the lithium metal battery can simultaneously provide improved capacity and excellent lifespan characteristics.
[0092] For example, a lithium metal battery (1) may include a liquid electrolyte, a semi-solid gel electrolyte, a solid electrolyte, or a combination thereof as the electrolyte.
[0093] Lithium metal battery (1) is manufactured by, for example, the following exemplary method, but is not necessarily limited to this method and is adjusted according to required conditions.
[0094] (cathode)
[0095] Prepare the cathode described above.
[0096] (anode)
[0097] First, a positive electrode active material composition is prepared by mixing a positive electrode active material, a conductive agent, a binder, and a solvent. The prepared positive electrode active material composition is directly coated and dried on an aluminum current collector to produce a positive electrode plate having a positive electrode active material layer (12) formed thereon. Alternatively, the positive electrode active material composition is cast on a separate support, and then the film obtained by peeling from the support is laminated on the aluminum current collector to produce a positive electrode (10) having a positive electrode active material layer (12) formed thereon.
[0098] The cathode active material is a lithium-containing metal oxide, and any one commonly used in the art can be used without limitation. For example, one or more types of composite oxides of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof can be used, and specific examples thereof include Li a A 1-b B b D2 (in the above formula, 0.90 ≤ a ≤ 1, and 0 ≤ b ≤ 0.5); Li a E 1-b B b O 2-c D c (In the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); LiE 2-b B b O 4-c D c (In the above formula, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); Li a Ni 1-b-c Co b B c D α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Co b B c O 2-α F α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Lia Ni 1-b-c Co b B c O 2-α F2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B c D α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Mn b B c O 2-α F α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B c O 2-α F2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni b E c G d O2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0.001 ≤ d ≤ 0.1); Li a Ni b Co c Mn d GeO2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0 ≤ d ≤ 0.5, 0.001 ≤ e ≤ 0.1); Li a NiG b O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); Li a CoG b O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); Lia MnG b O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); Li a Mn2G b O4 (wherein 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiIO2; LiNiVO4; Li (3-f) J2(PO4)3(0 ≤ f ≤ 2); Li (3-f) A compound represented by any one of the chemical formulas Fe2(PO4)3(0 ≤ f ≤ 2); LiFePO4 can be used.
[0099] In the chemical formula representing the above-described compound, A is Ni, Co, Mn, or a combination thereof; B is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element, or a combination thereof; D is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; F is F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; Q is Ti, Mo, Mn, or a combination thereof; I is Cr, V, Fe, Sc, Y, or a combination thereof; J is V, Cr, Mn, Co, Ni, Cu, or a combination thereof. It is also possible to use a compound having a coating layer added to the surface of the above-described compound, or it is also possible to use a mixture of the above-described compound and the compound having a coating layer added. The coating layer added to the surface of the above-mentioned compound includes a coating element compound of, for example, an oxide, a hydroxide, an oxyhydroxide of the coating element, an oxycarbonate of the coating element, or a hydroxycarbonate of the coating element of the coating element. The compound forming the coating layer is amorphous or crystalline. The coating elements included in the coating layer are Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a mixture thereof. The method for forming the coating layer is selected within a range that does not adversely affect the physical properties of the positive electrode active material. The coating method includes, for example, spray coating and dipping. Since the specific coating method is well understood by those working in the relevant field, a detailed description thereof will be omitted.
[0100] The cathode active material is, for example, Li a Ni x Co y M z O 2-b A b(1.0≤a≤1.2, 0≤b≤0.2, 0.8≤x<1, 0 <y≤0.3, 0<z≤0.3, 및 x+y+z=1이고, M은 망간(Mn), 니오븀(Nb), 바나듐(V), 마그네슘(Mg), 갈륨(Ga), 실리콘(Si), 텅스텐(W), 몰리브덴(Mo), 철(Fe), 크롬(Cr), 구리(Cu), 아연(Zn), 티타늄(Ti), 알루미늄(Al), 보론(B) 또는 이들의 조합이고, A는 F, S, Cl, Br 또는 이들의 조합), LiNi x Co y Mn z O2(0.8≤x≤0.95, 0≤y≤0.2, 0 <z≤0.2 및 x+y+z=1), LiNi x Co y Al z O2(0.8≤x≤0.95, 0≤y≤0.2, 0 <z≤0.2 및 x+y+z=1), LiNi x Co y Mn z Al w O2(0.8≤x≤0.95, 0≤y≤0.2, 0 <z≤0.2, 0<w≤0.2, 및 x+y+z+w=1), Li a Co x M y O 2-b A b (1.0≤a≤1.2, 0≤b≤0.2, 0.9≤x≤1, 0≤y≤0.1, and x+y=1, M is manganese (Mn), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B) or a combination thereof, and A is F, S, Cl, Br or a combination thereof), Li a Ni x Mn y M' z O 2-b A b(1.0≤a≤1.2, 0≤b≤0.2, 0 <x≤0.3, 0.5≤y<1, 0<z≤0.3, 및 x+y+z=1이고, M'는 코발트(Co), 니오븀(Nb), 바나듐(V), 마그네슘(Mg), 갈륨(Ga), 실리콘(Si), 텅스텐(W), 몰리브덴(Mo), 철(Fe), 크롬(Cr), 구리(Cu), 아연(Zn), 티타늄(Ti), 알루미늄(Al), 보론(B) 또는 이들의 조합이고, A는 F, S, Cl, Br 또는 이들의 조합), Li a M1 x M2 y PO 4-b X b (In the above chemical formula 7, 0.90≤a≤1.1, 0≤x≤0.9, 0≤y≤0.5, 0.9 <x+y<1.1, 0≤b≤2 이며, M1이 크롬(Cr), 망간(Mn), 철(Fe), 코발트(Co), 니켈(Ni), 구리(Cu), 지르코늄(Zr) 또는 이들의 조합이며, M2가 마그네슘(Mg), 칼슘(Ca), 스트론튬(Sr), 바륨(Ba), 티탄(Ti), 아연(Zn), 보론(B), 니오븀(Nb), 갈륨(Ga), 인듐(In), 몰리브덴(Mo), 텅스텐(W), 알루미늄(Al), 실리콘(Si), 크롬(Cr), 바나듐(V), 스칸듐(Sc), 이트륨(Y) 또는 이들의 조합이며, X가 O, F, S, P 또는 이들의 조합), Li a M3 z PO4 (0.90≤a≤1.1, 0.9≤z≤1.1, and M3 is chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zirconium (Zr), or a combination thereof).
[0101] Conductive materials include, but are not limited to, carbon black, graphite particles, natural graphite, artificial graphite, acetylene black, Ketjen black, carbon fibers; carbon nanotubes; metal powders or metal fibers or metal tubes such as copper, nickel, aluminum, and silver; and conductive polymers such as polyphenylene derivatives. Any conductive material used in the relevant technical field may be used. Alternatively, the anode may not include a separate conductive material, for example.
[0102] As the binder, vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene (PTFE), mixtures of the above polymers, styrene butadiene rubber polymer, etc. are used, and as the solvent, N-methylpyrrolidone (NMP), acetone, water, etc. are used, but are not necessarily limited to these, and any solvent used in the relevant technical field may be used.
[0103] It is also possible to form pores inside the electrode plate by further adding a plasticizer or a pore forming agent to the positive electrode active material composition.
[0104] The contents of the positive electrode active material, conductive agent, binder, and solvent used in the positive electrode (10) are at levels typically used in lithium batteries. Depending on the purpose and configuration of the lithium metal battery, one or more of the conductive agent, binder, and solvent may be omitted.
[0105] The binder content included in the positive electrode (10) may be 0.1 wt% to 10 wt% or 0.1 wt% to 5 wt% of the total weight of the positive electrode active material layer (12). The positive electrode active material content included in the positive electrode (10) may be 80 wt% to 99 wt%, 90 wt% to 99 wt% or 95 wt% to 99 wt% of the total weight of the positive electrode active material layer (12).
[0106] According to one embodiment, when the lithium metal battery (1) includes a solid electrolyte as an electrolyte, the positive electrode active material layer (12) may further include a solid electrolyte in addition to the positive electrode active material. The solid electrolyte included in the positive electrode (10) may be the same as or different from the solid electrolyte included in the subsequent electrolyte layer (30). For details on the solid electrolyte included in the positive electrode (10), refer to the electrolyte layer (30) section.
[0107] The solid electrolyte used in the positive electrode active material layer (12) may have a smaller D50 average particle size than the solid electrolyte used in the electrolyte layer (30). For example, the D50 average particle size of the solid electrolyte used in the positive electrode active material layer (12) may be 90% or less, 80% or less, 70% or less, 60% or less, 50% or less, 40% or less, 30% or less, or 20% or less of the D50 average particle size of the solid electrolyte used in the electrolyte layer (30). The D50 average particle size of the solid electrolyte used in the positive electrode active material layer (12) may be, for example, 0.1 ㎛ to 2 ㎛, 0.2 ㎛ to 1.5 ㎛, or 0.3 ㎛ to 1.0 ㎛.
[0108] For example, the content of the solid electrolyte included in the positive electrode active material layer (12) may be 1 to 15 wt%, 5 to 15 wt%, or 8.0 to 12.0 wt% of the total weight of the positive electrode active material layer (12).
[0109] For example, when the lithium metal battery (1) includes a solid electrolyte, the positive electrode active material layer (12) included in the lithium metal battery (1) may include a binder. The binder is, for example, styrene butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, etc., but is not necessarily limited thereto, and any binder that can be used in the relevant technical field may be used. The content of the binder included in the positive electrode active material layer (12) may be, for example, 0.1 to 5 wt%, 0.5 to 3 wt%, or 1.0 to 2.0 wt% of the total weight of the positive electrode active material layer (12).
[0110] When the lithium metal battery (1) includes a solid electrolyte, the cathode active material layer (12) included in the lithium metal battery (1) may include a conductive material. The conductive material may be, for example, a carbon-based conductive material or a metal-based conductive material. The conductive material is not necessarily limited to graphite, carbon black, acetylene black, Ketjen black, carbon fiber, carbon tube, metal powder, etc., and any conductive material that can be used as a conductive material in the relevant technical field may be used. The content of the conductive material included in the cathode active material layer (12) may be, for example, 0.1 to 10 wt%, 0.5 to 5 wt%, or 1.0 to 4.0 wt% of the total weight of the cathode active material layer (12). In addition to the above-described cathode active material, solid electrolyte, binder, and conductive material, the cathode active material layer (12) may further include additives such as fillers, coating agents, dispersants, and ion conductive aids.
[0111] The positive electrode current collector (11) may be, for example, a plate or foil made of aluminum (Al), indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), germanium (Ge), lithium (Li), or an alloy thereof. The positive electrode current collector may be omitted. The positive electrode current collector (11) may further include a carbon layer disposed on one or both sides of the metal substrate. By additionally disposing the carbon layer on the metal substrate, the metal of the metal substrate is prevented from being corroded by the solid electrolyte included in the positive electrode layer, and the interface resistance between the positive electrode active material layer (12) and the positive electrode current collector (11) can be reduced. The thickness of the carbon layer may be, for example, 1 ㎛ to 5 ㎛, 1 ㎛ to 4 ㎛, or 1 ㎛ to 3 ㎛. If the thickness of the carbon layer is too thin, it may be difficult to completely block contact between the metal substrate and the solid electrolyte. If the carbon layer is too thick, the energy density of the all-solid-state secondary battery may decrease. The carbon layer may include amorphous carbon, crystalline carbon, etc. The thickness of the cathode current collector (11) including the metal substrate and optionally the carbon layer may be, for example, 10 ㎛ to 50 ㎛, 10 ㎛ to 40 ㎛, or 10 ㎛ to 30 ㎛, but is not necessarily limited to these ranges and may be selected depending on the characteristics of the all-solid-state lithium metal battery required.
[0112] According to one embodiment, the positive electrode (10) may further include a positive electrode current collector (11), a positive electrode active material layer (12) disposed on the positive electrode current collector (11), and an inactive member disposed on one side of the positive electrode active material layer (12). The area of the positive electrode active material layer (12) may be smaller than the area of the electrolyte layer (30) in contact with the positive electrode active material layer (12). The inactive member may be disposed to surround the side of the positive electrode active material layer (12) to correct an area error between the positive electrode active material layer (12) and the electrolyte layer (30). The inactive member is a member that does not include an electrochemically active material, for example, an electrode active material. The electrode active material may be a material that absorbs / releases lithium. The inactive member may be a member made of a material other than the electrode active material and used in the relevant technical field. The above-described inert member surrounds the side surface of the positive electrode active material layer (12) and can be in contact with the electrolyte layer (30). By surrounding the side surface of the positive electrode active material layer (12) and making contact with the electrolyte layer (30), cracks in the electrolyte layer (30) that occur due to a pressure difference during the pressing process in the electrolyte layer (30) that does not contact the positive electrode active material layer (12) can be effectively suppressed. By compensating for the difference between the area of the positive electrode active material layer (12) and the area of the electrolyte layer (30), cracks in the electrolyte layer (30) that occur due to a pressure difference during the pressing process can be effectively suppressed. The above-described inert member can be disposed between the positive electrode current collector (11) and the electrolyte layer (30) that face each other. The above-described inert member can serve as a filler that fills the space between the positive electrode current collector (11) and the electrolyte layer (30) that face each other. The above inert member may include at least one selected from a lithium ion insulator and a lithium ion conductor. The above inert member may be an electronic insulator.That is, the inert member may not be an electronic conductor. The inert member may be an organic material, an inorganic material, or an organic-inorganic composite material. The organic material may be, for example, a polymer. The inorganic material may be, for example, a ceramic such as a metal oxide. The organic-inorganic composite material may be a composite of a polymer and a metal oxide. The inert member may include, for example, at least one selected from among an insulating polymer, an ion-conducting polymer, an insulating inorganic material, an oxide-based solid electrolyte, and a sulfide-based solid electrolyte. The inert member may be, for example, an olefin-based polymer such as polypropylene (PP) or polyethylene (PE). The inert member may be, for example, a gasket. The thickness of the inert member may be the same as or similar to the thickness of the positive electrode active material layer (12).
[0113] According to one implementation example, the current density of the anode (10) is 1 mAh / cm 2 20 mAh / cm 2 It can be. For example, the current density of the anode (10) is 1.5 mAh / cm 2 20 mAh / cm 2 , 2mAh / cm 2 20 mAh / cm 2 , 1mAh / cm 2 18 mAh / cm 2 , 1mAh / cm 2 16 mAh / cm 2 , 1mAh / cm 2 14 mAh / cm 2 , 1mAh / cm 2 12 mAh / cm 2 , 1mAh / cm 2 10 mAh / cm 2 or 2mAh / cm 2 10 mAh / cm 2 It could be.
[0114]
[0115] (Separator)
[0116] Next, a separator to be inserted between the positive electrode (10) and negative electrode (20) is prepared.
[0117] Any separator commonly used in lithium batteries can be used. For example, a separator with low resistance to ion migration and excellent electrolyte absorption capacity is used. The separator may be selected from glass fiber, polyester, Teflon, polyethylene, polypropylene, polytetrafluoroethylene (PTFE), or combinations thereof, and may be in the form of a nonwoven or woven fabric. For lithium-ion batteries, a rollable separator, such as polyethylene or polypropylene, is used, while for lithium-ion polymer batteries, a separator with excellent organic electrolyte absorption capacity is used.
[0118] The separator is manufactured by the following exemplary methods, but is not limited to these methods and may be adjusted according to required conditions.
[0119] First, a separator composition is prepared by mixing a polymer resin, a filler, and a solvent. The separator composition is directly coated and dried on the electrode to form a separator. Alternatively, the separator composition is cast on a support and dried, and then a separator film peeled from the support is laminated on the electrode to form a separator.
[0120] The polymer used in separator manufacturing is not particularly limited; any polymer used as a binder for electrode plates can be used. Examples include vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, or mixtures thereof.
[0121] (electrolyte)
[0122] Next, the electrolyte is prepared.
[0123] The electrolyte layer (30) may include, for example, a liquid electrolyte, a semi-solid gel electrolyte, a solid electrolyte, or a combination thereof.
[0124] The electrolyte is, for example, an organic electrolyte. An organic electrolyte is prepared by dissolving a lithium salt in an organic solvent, for example.
[0125] Any organic solvent used in the relevant technical field may be used. Examples of the organic solvent include propylene carbonate, ethylene carbonate, fluoroethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, dibutyl carbonate, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, dimethylacetamide, dimethyl sulfoxide, dioxane, 1,2-dimethoxyethane, sulfolane, dichloroethane, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether, or mixtures thereof.
[0126] Lithium salts are all possible if they are used as lithium salts in the relevant technical field. Lithium salts include, for example, LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2)(1≤x≤20, 1≤y≤20), LiCl, LiI or a mixture thereof. The concentration of the lithium salt is, for example, 0.1 M to 5.0 M.
[0127] For example, a semi-solid gel electrolyte may have a gel or semi-solid form. When a semi-solid gel electrolyte has a gel or semi-solid form, it can overcome the disadvantages of conventional lithium metal batteries described above because at least one selected from lithium metal and lithium alloy can freely expand during charge and discharge compared to when it is in a completely solid form.
[0128] For example, a semi-solid gel electrolyte may include one or more selected from lithium metal and lithium alloys and a liquid electrolyte. For example, a semi-solid gel electrolyte may be prepared by supplying a composition for forming a semi-solid gel electrolyte and drying it.
[0129] For example, a composition for forming a semi-solid gel electrolyte is prepared by mixing at least one selected from lithium metal and a lithium alloy with a liquid electrolyte. The composition for forming a semi-solid gel electrolyte has a gel or semi-solid form. The viscosity of the composition for forming a semi-solid gel electrolyte is not particularly limited, but is, for example, 5 cP or less at 25°C, for example, 2.5 to 4.0 cP.
[0130] The solid electrolyte is, for example, an oxide-based solid electrolyte, a sulfide-based solid electrolyte, or a combination thereof.
[0131] Solid electrolytes are, for example, oxide-based solid electrolytes. Oxide-based solid electrolytes are Li 1+x+y Al x Ti 2-x Si y P 3-y O 12 (0 <x<2, 0≤y<3), BaTiO3, Pb(Zr,Ti)O3(PZT), Pb 1-x La x Zr 1-y Ti y O3(PLZT)(O≤x<1, O≤y<1), PB(Mg3Nb 2 / 3)O3-PbTiO3(PMN-PT), HfO2, SrTiO3, SnO2, CeO2, Na2O, MgO, NiO, CaO, BaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiO2, Li3PO4, Li x Ti y (PO4)3(0 <x<2, 0<y<3), Li x Al y Ti z (PO4)3(0 <x<2, 0<y<1, 0<z<3), Li 1+x+y (Al, Ga) x (Ti, Ge) 2-x Si y P 3-y O 12 (0≤x≤1 0≤y≤1), Li x La y TiO3(0 <x<2, 0<y<3), Li2O, LiOH, Li2CO3, LiAlO2, Li2O-Al2O3-SiO2-P2O5-TiO2-GeO2, Li 3+x La3M2O 12 (M = Te, Nb, or Zr, x is an integer from 1 to 10) is one or more selected from. The solid electrolyte is manufactured by a sintering method, etc. For example, the oxide-based solid electrolyte is Li7La3Zr2O 12 (LLZO) and Li 3+x La3Zr 2-a M a O 12 (M doped LLZO, M=Ga, W, Nb, Ta, or Al, x is an integer from 1 to 10, 0 <a<2) 중에서 선택된 가넷계(Garnet-type) 고체전해질이다.
[0132] The sulfide-based solid electrolyte may include, for example, lithium sulfide, silicon sulfide, phosphorus sulfide, boron sulfide, or a combination thereof. The sulfide-based solid electrolyte particles may include Li2S, P2S5, SiS2, GeS2, B2S3, or a combination thereof. The sulfide-based solid electrolyte particles may be Li2S or P2S5. Sulfide-based solid electrolyte particles are known to have high lithium ion conductivity compared to other inorganic compounds. For example, the sulfide-based solid electrolyte includes Li2S and P2S5. When the sulfide solid electrolyte material constituting the sulfide-based solid electrolyte includes Li2S-P2S5, the mixing molar ratio of Li2S to P2S5 may be, for example, in a range of about 50:50 to about 90:10. In addition, Li3PO4, halogen, halogen compound, Li 2+2x Zn 1-x GeO4("LISICON" 0≤x<1), Li 3+y PO 4-x N x( "LIPON" 0 <x<4, 0<y<3), Li 3.25 Ge 0.25 P 0.75 S4("Thio-LISICON"), Li2O-Al2O3-TiO2-P2O 5( An inorganic solid electrolyte prepared by adding "LATP") etc. to an inorganic solid electrolyte of Li2S-P2S5, SiS2, GeS2, B2S3, or a combination thereof can be used as a sulfide solid electrolyte.
[0133] Sulfide-based solid electrolytes include, for example, Li2S-P2S5, Li2S-P2S5-LiX, where X is a halogen element, Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-Z m S n, m, n are positive numbers, Z is one of Ge, Zn or Ga, Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li p MO q , p, q are positive numbers, M is one of P, Si, Ge, B, Al, Ga In, Li 7-x PS 6-x Cl x , 0≤x≤2, Li 7-x PS 6-x Br x , 0≤x≤2, and Li 7-x PS 6-x I x , may include at least one selected from 0≤x≤2. The sulfide-based solid electrolyte is manufactured by treating starting materials such as Li2S and P2S5 by a melting rapid cooling method or a mechanical milling method. In addition, heat treatment may be performed after the treatment. The solid electrolyte may be amorphous, crystalline, or a mixture thereof. In addition, the solid electrolyte may be, for example, one containing sulfur (S), phosphorus (P), and lithium (Li) as constituent elements among the above-described sulfide-based solid electrolyte materials. For example, the solid electrolyte may be a material containing Li2S-P2S5. When using a sulfide-based solid electrolyte material containing Li2S-P2S5 to form the solid electrolyte, the mixing molar ratio of Li2S and P2S5 is, for example, in the range of Li2S: P2S5= 50:50 to 90:10.
[0134] The sulfide-based solid electrolyte may include, for example, an argyrodite type solid electrolyte represented by the following chemical formula 1:
[0135] <Chemical Formula 1>
[0136] Li + 12-n-x A n+ X 2- 6-x Y -x
[0137] In the above formula, A is P, As, Ge, Ga, Sb, Si, Sn, Al, In, Ti, V, Nb or Ta, X is S, Se or Te, Y is Cl, Br, I, F, CN, OCN, SCN or N3, and 1≤n≤5, 0≤x≤2. The sulfide-based solid electrolyte is, for example, Li 7-x PS 6-x Cl x , 0≤x≤2, Li 7-x PS 6-x Br x , 0≤x≤2, and Li 7-x PS 6-x I x , may be an argyrodite-type compound including at least one selected from 0≤x≤2. The sulfide-based solid electrolyte may be, for example, an argyrodite-type compound including at least one selected from Li6PS5Cl, Li6PS5Br, and Li6PS5I.
[0138] The density of the argyrodite-type solid electrolyte may be 1.5 to 2.0 g / cc. Since the argyrodite-type solid electrolyte has a density of 1.5 g / cc or more, the internal resistance of the all-solid-state secondary battery is reduced, and penetration of the solid electrolyte layer by Li can be effectively suppressed.
[0139] The elastic modulus, i.e., Young's modulus, of the sulfide-based solid electrolyte may be, for example, 35 GPa or less, 30 GPa or less, 27 GPa or less, 25 GPa or less, or 23 GPa or less. The elastic modulus, i.e., Young's modulus, of the sulfide-based solid electrolyte may be, for example, 10 to 35 GPa, 10 to 30 GPa, 10 to 27 GPa, 10 to 25 GPa, or 10 to 23 GPa. Since the sulfide-based solid electrolyte has an elastic modulus in this range, the temperature and / or pressure required for sintering, etc. is reduced, and thus sintering of the solid electrolyte can be performed more easily.
[0140] The average D50 particle size of the solid electrolyte used in the electrolyte layer (30) may be, for example, 1 μm to 10 μm, 1.5 μm to 7 μm, or 2 μm to 5 uμm.
[0141] The content of the sulfide-based solid electrolyte included in the electrolyte layer (30) may be, for example, 97 to 100 wt%, 98 to 99.9 wt%, or 98.5 to 99.0 wt% of the total weight of the electrolyte layer (30).
[0142] The electrolyte layer (30) may further include, for example, a binder. The binder included in the electrolyte layer (30) may be, for example, styrene butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, etc., but is not limited thereto, and any binder used in the relevant technical field may be used. The binder of the electrolyte layer (30) may be the same as or different from the binders included in the positive electrode active material layer (12) and the negative electrode active material layer (220).
[0143] The content of the binder included in the electrolyte layer (30) may be, for example, 0.1 to 3 wt%, 0.5 to 2 wt%, or 1.0 to 2.0 wt% of the total weight of the electrolyte layer (30).
[0144] For example, a lithium metal battery (1) includes an electrolyte layer (30), a positive electrode (10) disposed on one surface of the electrolyte layer (30), and a negative electrode (20) disposed on the other surface of the electrolyte layer (30). The positive electrode (30) includes a positive electrode active material layer (12) in contact with the electrolyte layer (30) and a positive electrode current collector (11) in contact with the positive electrode active material layer (12), and the negative electrode (20) includes a negative electrode active material layer (22) in contact with the electrolyte layer (30) and a negative electrode current collector (21) in contact with the negative electrode active material layer (22). For example, an all-solid-state lithium metal battery (1) is completed by arranging a positive electrode active material layer (12) and a negative electrode active material layer (22) on both sides of an electrolyte layer (30), and arranging a positive electrode current collector (11) and a negative electrode current collector (21) on the positive electrode active material layer (12) and the negative electrode active material layer (22), respectively, to form an all-solid-state lithium metal battery (30). Alternatively, an all-solid-state lithium metal battery (40) is completed by sequentially stacking a negative electrode active material layer (22), an electrolyte layer (30), a positive electrode active material layer (12), and a positive electrode current collector (11) on the negative electrode current collector (21).
[0145]
[0146] (lithium metal battery)
[0147] Referring to FIG. 4, a lithium metal battery (1) according to one embodiment includes a positive electrode (3), the aforementioned negative electrode (2), and a separator (4). The positive electrode (3), the negative electrode (2), and the separator (4) are wound or folded to form a battery structure (7). The formed battery structure (7) is accommodated in a battery case (5). An organic electrolyte is injected into the battery case (5) and sealed with a cap assembly (6), thereby completing the lithium metal battery (1). The battery case (5) is cylindrical, but is not necessarily limited to this shape, and may be, for example, square, thin-film, etc.
[0148] Referring to FIG. 5, a lithium metal battery (1) according to one embodiment includes a positive electrode (3), the aforementioned negative electrode (2), and a separator (4). A separator (4) is disposed between the positive electrode (3) and the negative electrode (2), and the positive electrode (3), the negative electrode (2), and the separator (4) are wound or folded to form a battery structure (7). The formed battery structure (7) is accommodated in a battery case (5). An electrode tab (8) that serves as an electrical path for guiding the current formed in the battery structure (7) to the outside may be included. An organic electrolyte is injected into the battery case (5) and sealed to complete the lithium metal battery (1). The battery case (5) is not necessarily limited to a square shape, but may be, for example, a cylindrical shape, a thin film shape, etc.
[0149] Referring to FIG. 6, a lithium metal battery (1) according to one embodiment includes a positive electrode (3), the aforementioned negative electrode (2), and a separator (4). A separator (4) is disposed between the positive electrode (3) and the negative electrode (2) to form a battery structure. A battery structure (7) is stacked in a bi-cell structure and then accommodated in a battery case (5). An electrode tab (8) that serves as an electrical path for guiding a current formed in the battery structure (7) to the outside may be included. An organic electrolyte is injected into the battery case (5) and sealed to complete the lithium metal battery (1). The battery case (5) is not necessarily limited to a square shape, but may be, for example, a cylindrical shape, a thin film shape, etc.
[0150] A pouch-type lithium metal battery corresponds to the lithium metal batteries of FIGS. 4 to 6, each of which uses a pouch as a battery case. The pouch-type lithium metal battery includes one or more battery structures. A separator is disposed between a positive electrode and a negative electrode to form a battery structure. The battery structures are laminated in a bi-cell structure, then impregnated with an organic electrolyte, and accommodated and sealed in a pouch to complete the pouch-type lithium metal battery. For example, although not shown in the drawings, the above-described positive electrode, negative electrode, and separator may be simply laminated and accommodated in a pouch in the form of an electrode assembly, or may be wound or folded into a jelly-roll-shaped electrode assembly and then accommodated in a pouch. Subsequently, an organic electrolyte is injected into the pouch and sealed to complete the lithium metal battery.
[0151] Lithium metal batteries have excellent cycle life and high-rate characteristics, making them suitable for use in electric vehicles (EVs). Examples include plug-in hybrid electric vehicles (PHEVs). They are also used in applications requiring large amounts of power storage, such as electric bicycles and power tools.
[0152] Lithium metal batteries are stacked in multiple layers to form a battery module, and the multiple battery modules form a battery pack. Such a battery pack can be used in any device requiring high capacity and high output. For example, it can be used in laptops, smartphones, electric vehicles, etc. The battery module includes, for example, multiple batteries and a frame that holds them. The battery pack includes, for example, multiple battery modules and a bus bar that connects them. The battery module and / or the battery pack may further include a cooling device. The multiple battery packs are controlled by a battery management system. The battery management system includes a battery pack and a battery control device connected to the battery pack.
[0153]
[0154] [Cathode manufacturing method]
[0155] According to one embodiment, a negative electrode (20) may be manufactured by a method including: preparing a negative electrode structure including a negative electrode current collector (210), a negative electrode active material layer (220) disposed on the negative electrode current collector (210), and a porous layer (230) disposed on the negative electrode active material layer (220); and rolling the negative electrode structure using a roll press to insert at least a portion of the porous layer (230) into the negative electrode active material layer (220).
[0156] For example, the step of preparing the negative electrode structure may include a step of preparing a negative electrode current collector, a step of preparing a negative electrode active material layer (220) on the negative electrode current collector (210), and a step of preparing a porous layer (230) on the negative electrode active material layer (220).
[0157] For example, the description of the negative electrode current collector (210), the negative electrode active material layer (220), and the porous layer (230) may refer to the above-described description.
[0158] For example, the negative electrode structure may be rolled using a roll press to insert at least a portion of the porous layer (230) into the negative electrode active material layer (220). For example, the roll press may include a plurality of rollers, and the porous layer may be inserted into the negative electrode active material layer by inserting the negative electrode structure between the plurality of rollers. For example, the degree to which the porous layer (230) is inserted into the negative electrode active material layer (220) may be controlled by adjusting the gap between the plurality of rollers. For example, the degree to which the porous layer (230) is inserted into the negative electrode active material layer (220) may be controlled by adjusting the pressure applied to the negative electrode structure.
[0159]
[0160] The present invention is explained in more detail through the following examples and comparative examples. However, the examples are intended to illustrate the present invention and are not intended to limit the scope of the present invention.
[0161]
[0162] (Lithium metal battery manufacturing)
[0163] Example 1: Cu substrate / Li foil / Cu foam (80% porosity), H = 100%
[0164] (Manufacturing of positive electrode)
[0165] LiNi as a cathode active material 0.8 Mn 0.1 Co 0.1 A mixture of O2, carbon conductive agent (Denka Black), and polyvinylidene fluoride (PVdF) in a weight ratio of 96:2:2 was mixed with N-methylpyrrolidone (NMP) in an agate mortar to prepare a slurry.
[0166] The slurry was applied at 8.5 mg / cm on a 15 μm thick aluminum collector. 2 By loading, bar coating, drying at room temperature, drying again under vacuum at 120℃, rolling and punching, a positive electrode plate having a thickness of 21㎛ and an electrode density of 4.1g / cc was manufactured.
[0167] The current density of the anode is 6 mAh / cm 2 It was.
[0168]
[0169] (Cathode manufacturing)
[0170] A lithium foil having a thickness of 20 μm was attached on a copper (Cu) current collector having a thickness of 10 μm. A copper foam having a thickness of 50 μm and a porosity of 80% was prepared and placed on the lithium foil to manufacture a negative electrode structure. When the copper foam was analyzed on the surface by X-ray photoelectron spectroscopy (XPS), the ratio of oxide peaks to metal peaks was 4:1.
[0171] The above-described cathode structure was inserted into a roll press, so that 70% of the total thickness of the copper foam was inserted into the lithium foil. In this case, the value of Equation 1 below was 36.7 μm, and the thickness (H) of the copper foam (first region) not inserted into the lithium foil was 100% of that of Equation 1 below.
[0172] <Formula 1> Anode current density (mAh / cm 2 ) * 4.89㎛ / (mAh / cm 2 ) * (1 / porosity of the first region)
[0173]
[0174] (Manufacturing of lithium metal batteries)
[0175] A lithium metal battery was manufactured using the positive and negative electrodes manufactured above, a PTFE separator, and a solution containing 1.3 M LiPF6 dissolved in EC (ethylene carbonate) + EP (ethyl propionate) + PP (propyl propionate) (25:30:45 volume ratio) as an electrolyte.
[0176]
[0177] Example 2: Cu substrate / Li foil / Cu foam (80% porosity), H = 130%
[0178] A lithium metal battery was manufactured in the same manner as in Example 1, except that the thickness (H) of the copper foam (first region) not inserted into the lithium foil was changed to 130% of the value in Equation 1.
[0179]
[0180] Example 3: Cu substrate / Li foil / Cu foam (80% porosity), H = 50%
[0181] A lithium metal battery was manufactured in the same manner as in Example 1, except that the thickness of the copper foam not inserted into the lithium foil was changed to 80% of the value in Equation 1.
[0182] Example 4: Cu substrate / Li foil / Cu foam (80% porosity), H = 160%
[0183] A lithium metal battery was manufactured in the same manner as in Example 1, except that the thickness of the copper foam not inserted into the lithium foil was changed to 80% of the value in Equation 1.
[0184] Example 5: Cu substrate / Li foil / acid-treated Cu foam (80% porosity), H = 100%
[0185] A lithium metal battery was manufactured in the same manner as in Example 1, except that copper foam treated with hydrochloric acid was used. The ratio of oxide peaks to metal peaks in the surface analysis of the copper foam treated with hydrochloric acid by X-ray photoelectron spectroscopy (XPS) was 5:1.
[0186]
[0187] Example 6: Cu substrate / Li foil / Cu foam (50% porosity), H = 100%
[0188] A lithium metal battery was manufactured in the same manner as in Example 1, except that a copper foam with a porosity of 50% was used.
[0189]
[0190] Comparative Example 1: Cu substrate / Li foil / Cu foam (80% porosity)
[0191] A lithium metal battery was manufactured in the same manner as in Example 1, except that, instead of attaching lithium foil on the negative electrode collector, copper foam was directly attached to the negative electrode collector.
[0192]
[0193] Comparative Example 2: Cu substrate / Li foil / Cu foam (80% porosity)
[0194] A lithium metal battery was manufactured in the same manner as in Example 1, except that copper foam was not inserted into the negative electrode active material layer.
[0195]
[0196] Evaluation Example 1: Evaluation of room-temperature charge-discharge characteristics
[0197] The lithium batteries manufactured in Examples 1 to 6 and Comparative Examples 1 to 2 were charged at a constant current of 0.1 C at 25°C until the voltage reached 4.55 V (vs. Li), and then cut-off at a current of 0.05 C while maintaining 4.55 V in constant voltage mode. Subsequently, the batteries were discharged at a constant current of 0.1 C until the voltage reached 3.0 V (vs. Li) during discharge (formation cycle).
[0198] The lithium battery that had undergone the Mars cycle was charged at a constant current of 0.2C at 25℃ until the voltage reached 4.55 V (vs. Li), and then cut-off at a current of 0.05C while maintaining 4.55 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.2C until the voltage reached 3.0 V (vs. Li) (1st cycle). At this time, the voltage drop (V) was measured while flowing a current of 1C for 1 second at SOC 10 (a state of charge of 100% of the total charge capacity of the battery, which means a state of discharge of 90%), and the DC internal resistance (DC-IR) was calculated.
[0199] The lithium battery that had gone through the 1st cycle was charged at a constant current of 1C rate at 25℃ until the voltage reached 4.55 V (vs. Li), and then cut-off was made at a current of 0.05 C rate while maintaining 4.55 V in constant voltage mode. Then, the battery was discharged at a constant current of 1C rate until the voltage reached 3.0 V (vs. Li) (2nd cycle), and this cycle was repeated (repeated 200 times) under the same conditions until the 200th cycle. At this time, 200 th The capacity retention rate for each cycle was calculated.
[0200] In every charge / discharge cycle, a 10-minute pause was provided after each charge / discharge cycle.
[0201] The initial efficiency (0.2C, %) and the number of cycles at which the capacity retention rate reached 80% among the results of the room temperature charge-discharge experiment are shown in Table 1 below. The capacity retention rate (%) in each cycle is defined by the following mathematical equation 1.
[0202] <Mathematical Formula 1>
[0203] Capacity retention rate [%] = [Discharge capacity in each cycle / 1] st Discharge capacity in cycles] Х 100
[0204] Porous layer initial efficiency (0.2C, %) cycle number (@80%) first region (H) thickness ratio (%) porosity (%) XPS ratio Example 1 100 804:195.7 126 Example 2 130 804:195.8 141 Example 3 50 804:195.174 Example 4 160 804:194.382 Example 5 100 801 1:196.1 137 Example 6 100 504:194.3 111 Comparative example 1-804:192.2 10 Comparative example 2-804:194.965
[0205] As shown in Table 1, the lithium metal batteries of Examples 1 to 6 had lower DC-IR and improved life characteristics compared to the lithium metal batteries of Comparative Examples 1 to 2.
[0206]
[0207] While exemplary embodiments have been described in detail with reference to the attached drawings, the present invention is not limited to these examples. It is self-evident that those skilled in the art to which the present invention pertains can devise various modifications or variations within the scope of the technical concepts described in the patent claims, and these also naturally fall within the technical scope of the present invention.
[0208]
[0209] [Explanation of symbols]
[0210] 1 Lithium metal battery 2, 20 cathode
[0211] 3, 10 positive electrode 4 separator
[0212] 5 Battery case 6 Cap assembly
[0213] 7 Battery structure 8 Electrode tab
[0214] 11. Cathode current collector 12. Cathode active material layer
[0215] 20 cathode 30 electrolyte layer
[0216] 210 negative electrode current collector 220 negative electrode active material layer
[0217] 230 porous layer 240 lithium precipitation layer
[0218] A1 Area 1 A2 Area 2
[0219] A3 Area 3
Claims
1. Contains an anode; a cathode; and an electrolyte disposed between the anode and the cathode, The above negative electrode is a negative electrode current collector; A negative electrode active material layer disposed on the negative electrode current collector; and A porous layer including a porous structure, The porous layer includes a first region exposed on the negative electrode active material layer and a second region inserted into the negative electrode active material layer, A lithium metal battery, wherein the negative electrode active material layer includes a second region in which the porous layer is inserted and a third region in which the porous layer is not inserted.
2. In paragraph 1, A lithium metal battery having a thickness of the first region satisfying 100 to 130% of the following equation 1: <Formula 1> Anode current density (mAh / cm 2 ) * 4.89㎛ / (mAh / cm 2 ) * (1 / 1st area porosity) 3. In paragraph 1, As the above lithium metal battery is charged, a lithium precipitation layer is formed on the negative electrode active material layer, The thickness of the above lithium precipitation layer is 130% or less of the thickness of the first region, lithium metal battery.
4. In paragraph 1, A lithium metal battery, wherein the porosity of the porous structure included in the first region of the porous layer is 1 to 99%.
5. In paragraph 1, A lithium metal battery, wherein the size of the pores included in the first region of the porous layer is 1 nm to 10 μm.
6. In paragraph 1, The thickness of the first region of the above porous layer is 1 ㎛ to 100 ㎛, The thickness of the second region of the above porous layer is 1 µm to 50 µm, lithium metal battery.
7. In paragraph 1, A lithium metal battery, wherein the thickness of the second region is 70% or less of the thickness of the negative electrode active material layer.
8. In paragraph 1, A lithium metal battery, wherein the hardness of the porous layer is greater than the hardness of the negative electrode active material layer.
9. In paragraph 1, The above porous layer includes a metal or carbon-based material, A lithium metal battery, wherein the metal comprises copper (Cu), nickel (Ni), stainless steel (SUS), iron (Fe), or cobalt (Co).
10. In paragraph 1, A lithium metal battery, wherein the porous structure includes a foam structure or a mesh structure.
11. In paragraph 1, The above porous structure is an acid-treated lithium metal battery.
12. In paragraph 1, A lithium metal battery having the above-mentioned acid-treated porous structure, wherein the ratio of oxide peaks to metal peaks is 50:1 to 1:1 when analyzed by X-ray photoelectron spectroscopy (XPS).
13. In paragraph 1, A lithium metal battery, wherein the porous structure further includes a coating layer formed on the surface.
14. In paragraph 1, A lithium metal battery, wherein the negative electrode active material layer comprises lithium metal or a lithium alloy.
15. In paragraph 1, A lithium metal battery, wherein the thickness of the third region among the negative electrode active material layers is 0.1 to 10 μm.
16. In paragraph 1, A lithium metal battery, wherein the negative electrode collector has a form selected from among a sheet, a foil, a film, a plate, a porous body, a mesoporous body, a body containing through holes, a polygonal ring body, a mesh body, a foam body, and a non-woven body.
17. In paragraph 1, The above negative electrode collector includes a base film and a metal layer disposed on one or both sides of the base film, The above base film comprises a polymer, and the polymer comprises polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI) or a combination thereof, A lithium metal battery, wherein the metal layer comprises indium (In), copper (Cu), magnesium (Mg), titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof.
18. In paragraph 1, The current density of the above anode is 1 mAh / cm 2 Up to 20mAh / cm 2 In, lithium metal battery.
19. In paragraph 1, A lithium metal battery, wherein the electrolyte comprises a liquid electrolyte, a semi-solid gel electrolyte, a solid electrolyte, or a combination thereof.
20. A method for manufacturing a cathode according to Article 1, A step of preparing a negative electrode structure including a negative electrode current collector, a negative electrode active material layer disposed on the negative electrode current collector, and a porous layer disposed on the negative electrode active material layer; and A method for manufacturing a negative electrode for a lithium metal battery, comprising the step of rolling the negative electrode structure using a roll press and inserting at least a portion of the porous layer into the negative electrode active material layer.
Citation Information
Patent Citations
Rechargeable lithium battery with ultra-high volumetric energy density and required manufacturing method
JP2018525795A
Porous silicon based negative electrode active material, manufacturing method thereof and lithium secondary battery including same
KR1020150000069A
Anode with buffer layer made by conductive textile, lithium secondary battery containing the same
KR1020180036564A
Watch
KR1020210007428A
A fuel cell solenoid valve having an elastic controlling part, and a fuel supply device including the same
KR102298125B1
Cited By
Battery pole piece and preparation method thereof
CN121641844A