Lithium secondary battery electrode plate and lithium secondary battery comprising same
By using high binder content particles in specific areas to create a 'core-shell' structure within the electrode mixture layer, the edge detachment issue in lithium secondary battery electrode plates is resolved, improving energy density and process efficiency in the dry electrode process.
Patent Information
- Application Number
- PCT/KR2024/004095
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-03-28
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-03
AI Technical Summary
The dry electrode process for manufacturing lithium secondary battery electrode plates faces issues with detachment at the edge portion due to weak electrode mixture coating, which affects the energy density and requires a solution to enhance bonding strength and prevent detachment.
Incorporating particles with high binder content in specific areas of the electrode mixture layer, particularly in the edge regions, to create a 'core-shell' structure where the binder is concentrated near the surface, improving adhesion and preventing detachment during the dry electrode process.
This approach enhances the bonding strength at the edge portions, prevents detachment, and increases the energy density of the electrode plates, making the dry electrode process more viable and cost-effective by eliminating the need for organic solvent drying steps.
Smart Images

Figure KR2024004095_03102024_PF_FP_ABST
Abstract
Description
Electrode plate for lithium secondary battery and lithium secondary battery including same
[0001] This application claims the benefit of priority to Republic of Korea Patent Application No. 10-2023-0040898, dated March 29, 2023, and Republic of Korea Patent Application No. 10-2024-0042597, dated March 28, 2024, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to a lithium secondary battery electrode plate and a lithium secondary battery including the same.
[0003] Key trends in recent electronics industry development can be summarized as the shift toward wireless and mobile devices and the transition from analog to digital. Representative examples include the rapid proliferation of mobile devices and laptops, and the transition from analog to digital cameras.
[0004] In line with this trend, research and development on secondary batteries as the operating power source for devices is actively underway. Among these, lithium secondary batteries, which utilize lithium transition metal oxides or lithium composite oxides as the cathode active material and boast high power and capacity relative to their weight, are attracting significant attention. Lithium secondary batteries consist of an electrode assembly consisting of a cathode / separator / anode, housed together with an electrolyte in a sealed container.
[0005] Meanwhile, the electrode generates current through the exchange of ions, and the positive and negative electrodes that make up the electrode are structured in such a way that an electrode active material is applied to an electrode current collector made of metal.
[0006] In general, the positive electrode has a structure in which an active material such as LiCoO2, LiMnO2, or LiNiO2 is coated on an electrode plate made of aluminum, etc., and the negative electrode has a structure in which a carbon-based active material is coated on an electrode plate made of copper or aluminum, etc.
[0007] In order to manufacture a positive or negative electrode plate, an electrode mixture containing an electrode active material is applied at regular intervals to an electrode current collector made of a long metal sheet in one direction, and then a process is performed to process the electrode into a set electrode shape.
[0008] The method of applying electrode mixture to the electrode plate can be broadly divided into wet electrode process and dry electrode process.
[0009] The wet electrode process is characterized by the process of preparing an electrode mixture to be applied to a current collector, in which the main components of the electrode mixture, such as an electrode active material, a conductive material, and a binder, are mixed using an organic solvent such as N-methyl-2-pyrrolidone (NMP) to produce an electrode mixture slurry, and applying the slurry to the electrode current collector.
[0010] The above wet electrode process must go through a step of removing an organic solvent such as NMP that was separately added to manufacture an electrode mixture slurry to ultimately manufacture an electrode. In this process, some of the binder dissolved in the organic solvent may fall out, which may reduce the bonding strength between the electrode active material / conductive material and the current collector. In addition, there is a disadvantage in that a large amount of power and cost are consumed in the drying process to remove the organic solvent.
[0011] To address the shortcomings of these wet electrode processes, a dry electrode process has recently emerged, which manufactures electrodes by directly applying the electrode mixture to the current collector without adding a separate organic solvent during the electrode mixture manufacturing process. When manufacturing electrodes for lithium secondary batteries using the dry electrode process, it is environmentally friendly because no separate solvent is used in the process of preparing the electrode mixture, and there is no need for a separate solvent drying step, which simplifies the process and reduces costs. In addition, since the electrode mixture can be applied onto the current collector through the rolling process, it can reduce the electrode thickness and improve the energy density of the electrode, and is therefore evaluated as a suitable method for manufacturing high-nickel or all-solid-state batteries.
[0012] However, in the case of the above dry electrode process, since a step of preparing an electrode mixture slurry using a separate organic solvent is not performed during the electrode mixture production, the electrode mixture coating at the edge of the electrode is relatively weak compared to the wet electrode process, and there is a problem that the electrode mixture may be detached from the edge, and a solution to this problem is urgently needed.
[0013] [Prior Art Literature]
[0014] [Patent Document]
[0015] (Patent Document 1) Japanese Patent Application Publication No. 2022-075282 (May 18, 2022)
[0016] The purpose of the present invention is to provide a lithium secondary battery electrode plate that includes an electrode mixture layer, and by disposing particles having a high binder content or a high surface binder content in a specific area formed from the edge of the electrode mixture layer, thereby preventing detachment from the edge of the electrode plate and increasing the energy density of the electrode plate even when the electrode plate is manufactured by a dry electrode process.
[0017] Another object of the present invention is to provide a lithium secondary battery including the above-described electrode plate for a lithium secondary battery.
[0018] One embodiment of the present invention provides a lithium secondary battery electrode plate, comprising a current collector layer and an electrode mixture layer formed on one or both sides of the current collector layer, wherein the electrode mixture layer includes a first region formed from one edge of the electrode mixture layer in the direction of the other edge based on a transverse direction (TD) cross-section of the electrode mixture layer, and a second region excluding the first region, wherein the electrode mixture layer includes first particles and second particles each including an electrode active material, a conductive material, and a binder, wherein the first particle has a higher binder content than the second particle, or a binder is included in a region that is 20% or less of a length from the outermost surface of the particle to the center of the particle, in an amount of 30% or more of the total binder content contained in the particle.
[0019] The first particle may be included in the first region, and the second particle may be included in the second region.
[0020] The first and second particles may be in the form of granules.
[0021] The average particle diameters of the first and second particles may each be 30 to 100 μm.
[0022] The above first region may be formed at an area ratio of 1% to 20% based on the total area of the electrode mixture layer.
[0023] The binder content ratio of the first particle and the binder content ratio of the second particle may be 1.2:1 to 3.0:1.
[0024] The binder included in the first and second particles may be at least one selected from the group consisting of polytetrafluoroethylene (PTFE), polyvinylidene difluoride (PVDF), polyethylene (PE), high molecular weight polyethylene (HMWPE), ultra-high molecular weight polyethylene (UHMWPE), polypropylene (PP), carboxymethyl cellulose (CMC), polyvinylphenol, polyvinylpyrrolidine, polyvinyl acetate, polyvinyl alcohol, and polyacetylene.
[0025] The first particle may include 3.6 to 9 wt% of a binder based on the total weight of the first particle, and the second particle may include 1 to 5 wt% of a binder based on the total weight of the second particle.
[0026] The first particle and the second particle may each independently further include a sulfide-based solid electrolyte represented by the following chemical formula 1.
[0027] [Chemical Formula 1]
[0028] Li k M 2 l S m X 2 n
[0029] In the above chemical formula 1, M 2 is Sn, Mg, Ba, B, Al, Ga, In, Si, Ge, Pb, N, P, As, Sb, Bi, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Hf, Ta, W, or La, 2 is F, Cl, Br, I, Se, Te, or O, and 0 <k≤6, 0<l≤6, 0<m≤6 및 0≤n≤6이다.
[0030] One embodiment of the present invention provides a lithium secondary battery including the above-described electrode plate for a lithium secondary battery.
[0031] According to the present invention, a lithium secondary battery electrode plate includes an electrode mixture layer, and particles having a high binder content or a high surface binder content are arranged in a specific area formed from an edge portion of the electrode mixture layer, thereby preventing detachment from the edge portion of the electrode plate and increasing the energy density of the electrode plate even when the electrode plate is manufactured by a dry electrode process. In addition, since a wet electrode process is not applied in manufacturing a lithium secondary battery electrode plate, a drying step of an organic solvent in an electrode mixture slurry can be omitted, making it an environmentally friendly process and economical because the production cost can be lowered.
[0032] Figures 1 and 2 are schematic diagrams showing the structure of a lithium secondary battery electrode plate according to one embodiment of the present invention.
[0033] Figure 3 shows an image of an electrode mixture layer including particles according to a manufacturing example of the present invention and a comparative manufacturing example formed on a current collector.
[0034] Figures 4 and 5 show scanning electron microscope (SEM) images of particles according to a manufacturing example of the present invention and the results of measuring the average particle diameter of the particles using a particle size analyzer.
[0035] Figures 6 to 8 illustrate images of a lithium secondary battery electrode plate according to one embodiment of the present invention.
[0036] Figure 9 shows a scanning electron microscope (SEM) image of a lithium secondary battery electrode plate according to one embodiment of the present invention.
[0037] Figure 10 shows a carbon EDS mapping image of a lithium secondary battery electrode plate according to one embodiment of the present invention.
[0038] Hereinafter, embodiments of the present invention will be described in detail. Prior to this, terms and words used in this specification and claims should not be interpreted as limited to their conventional or dictionary meanings. Rather, they should be interpreted with meanings and concepts consistent with the technical concept of the present invention, based on the principle that the inventor can appropriately define the concept of a term to best explain his or her invention. Accordingly, the configurations described in the embodiments described in this specification are merely the most preferred embodiments of the present invention and do not represent all of the technical concept of the present invention. Therefore, it should be understood that various equivalents and modified examples may exist as of the time of this application.
[0039] Throughout this specification, whenever a part is said to 'include' a component, this does not mean that it excludes other components, but rather that it may include other components, unless otherwise specifically stated.
[0040] Additionally, the description that concretizes or adds components can be applied to all inventions unless there are special limitations, and is not limited to a specific invention.
[0041] Additionally, throughout the description and claims of the invention herein, the singular includes the plural unless otherwise stated.
[0042] Additionally, throughout the description and claims of the present invention, the term "or" includes "and" unless otherwise stated. Therefore, "comprising A or B" means all three cases of including A, including B, or including A and B.
[0043] Additionally, all numerical ranges include the extreme values and all intermediate values between them, unless explicitly stated otherwise.
[0044] Throughout this specification, the average particle diameter of the particles may be, for example, the median diameter (D50) measured using a laser particle size distribution meter.
[0045] Hereinafter, a composite sulfide-based solid electrolyte according to one embodiment of the present invention will be described.
[0046] The present invention relates to a lithium secondary battery electrode plate capable of preventing detachment of an edge portion of a plate and improving the energy density of the plate when manufacturing an electrode for a lithium secondary battery using a dry electrode process, and to a lithium secondary battery including the same.
[0047] Figure 1 is a schematic diagram showing a lithium secondary battery electrode plate according to one embodiment of the present invention. Referring to FIG. 1, a lithium secondary battery electrode plate (100) according to one embodiment of the present invention includes a current collector layer (not shown) and an electrode mixture layer formed on one or both sides of the current collector layer, wherein the electrode mixture layer includes a first region (10) formed from one edge portion (50) of the electrode mixture layer in the direction of the other edge portion based on a transverse direction (TD) cross-section of the electrode mixture layer, and a second region (20) excluding the first region, wherein the electrode mixture layer includes first particles (30) and second particles (40) each including an electrode active material, a conductive material, and a binder, wherein the first particle (30) has a higher binder content than the second particle (40), or includes a binder in an area that is 20% or less of the length from the outermost surface portion of the particle to the center of the particle, in an amount of 30% or more of the total binder content contained in the particle.
[0048] The electrode plate for a lithium secondary battery according to the present invention includes particles having a specific structure in which the binder content is high in a region formed in a certain range based on the transverse direction (TD) cross-section of the electrode mixture layer with respect to the edge of the electrode mixture layer as the reference, or the binder content is concentrated in a specific region in the length from the outermost surface of the particle to the center of the particle, so that even when the electrode plate for manufacturing a lithium secondary battery, particularly the electrode plate for manufacturing an electrode mixture, is manufactured through a so-called 'dry electrode process' that does not use a separate solvent such as an organic solvent, the edge of the electrode plate can be prevented from being detached, by imparting improved bonding strength to the edge of the electrode plate, and since the electrode plate for a lithium secondary battery can be more easily applied to the dry electrode process, the energy density of the electrode plate can also be improved compared to the electrode plate manufactured through the wet electrode process.
[0049] In the present invention, the electrode plate for a lithium secondary battery may mean a structure in which an electrode mixture including an electrode active material is applied to an electrode current collector including a metal sheet formed long in one direction.
[0050] In the present invention, the electrode mixture may refer to a mixture applied to a plate for a lithium secondary battery, and may be, for example, a composition in which an electrode active material, a conductive material, a binder, and other components are mixed, and each component will be described later.
[0051] In one embodiment of the present invention, the first particle (30) and the second particle (40) may be in the form of granules formed by mixing and agglomerating constituent particles of the electrode active material, conductive material, binder, and other components contained in each particle. For example, the first particle (30) and the second particle (40) may be in the form of granules formed by uniformly mixing and distributing constituent particles of the electrode active material, conductive material, binder, and other components, or may have the form of granules formed such that one constituent component is concentrated in a specific region.
[0052] In one embodiment of the present invention, the average particle diameter of the first particle (30) may be 30 to 100 μm, for example, 35 to 95 μm, 40 to 90 μm, and preferably 50 to 80 μm.
[0053] In one embodiment of the present invention, the average particle diameter of the second particles (40) may be 30 to 100 μm, for example, 35 to 95 μm, 40 to 90 μm, and preferably 50 to 80 μm.
[0054] In one embodiment of the present invention, the first particle (30) may include 3.6 to 9 wt% of binder based on the total weight of the first particle including the electrode active material, the conductive material, and the binder, for example, 3.6 to 8.0 wt%, 3.8 to 7.0 wt%, and preferably 4.0 to 6.0 wt% of binder.
[0055] If the binder content of the first particle is less than 3.6 wt%, there is a problem that the adhesion of the electrode plate of the primary particle applied to the edge of the electrode plate for a lithium secondary battery may decrease, and if it exceeds 9 wt%, there may be a problem that the resistance of the electrode plate may increase due to the first particle, so it is appropriately adjusted within the above range.
[0056] In one embodiment of the present invention, the second particle (40) may include 1 to 5 wt% of binder relative to the total weight of the second particle including the electrode active material, the conductive material, and the binder, for example, 1.5 to 4.5 wt%, 2 to 4.0 wt%, and preferably 2.5 to 3.5 wt% of binder.
[0057] If the binder content of the second particle is less than 1 wt%, there is a problem that the manufacturing yield of the second particle may decrease, and if it exceeds 5 wt%, there may be a problem that the resistance of the electrode plate may increase due to the second particle, so it is appropriately adjusted within the above range.
[0058] Additionally, in one embodiment of the present invention, the binder content ratio of the first particle (30) and the binder content ratio of the second particle (40) may be 1.2:1 to 3.0:1, for example, 1.3:1 to 2.9:1, 1.4:1 to 2.8:1, or 1.5:1 to 2.7:1.
[0059] If the binder content ratio of the second particles compared to the binder content ratio of the first particles is less than the above range, there is a problem that the adhesive strength improvement effect of the electrode plate for a lithium secondary battery by the first and second particles may be reduced, and if it exceeds the above range, there may be a problem that the resistance of the electrode plate may increase. Therefore, in order to prevent detachment of the edge of the electrode plate that may occur when manufacturing the electrode plate for a lithium secondary battery according to the present invention using a dry electrode process, it is preferable that the binder content in the first particles (30) and second particles (40) included in the electrode mixture layer satisfies the above range.
[0060] In the case of the first particle (30) included in the electrode mixture layer of the electrode plate for a lithium secondary battery according to the present invention, the binder content within the particle may be higher than that of the second particle (40), or the binder content may be distributed such that 30% or more of the binder content within the particle is included in a region that is 20% or less of the length from the outermost surface of the particle to the center of the particle.
[0061] For example, the first particle (30) may have a 'core-shell structure' in which the shell portion of the first particle (30) is formed in an area corresponding to 20% of the length from the outermost surface portion of the particle to the center of the particle, and the remaining area up to the center is formed as a 'core'. At this time, the shell portion of the first particle (30) may have a form in which 30% or more of the binder content included in the first particle is distributed. That is, the first particle (30) includes an electrode active material, a conductive material, and a binder, and in particular, has a characteristic in which the binder is distributed so as to be biased toward the relatively outer portion of the first particle, thereby increasing the bonding strength with other adjacent first particles or a current collector layer, thereby preventing detachment from the edge portion of a lithium secondary battery electrode plate.
[0062] When the first particle (30) is formed into a 'core-shell structure' as described above, the region where the binder is positioned to be biased may be a region that is 20% of the length from the outermost surface of the particle to the center of the particle, or a region that is 1% to 20% of the length from the outermost surface of the particle to the center of the particle.
[0063] When the first particle (30) is formed into a 'core-shell structure' as described above, a binder of 30% or more of the total binder content contained in the first particle may be included in a region that is 20% or less of the length from the outermost surface of the particle to the center of the particle.
[0064] In one embodiment of the present invention, the binder included in the first particle (30) and the second particle (40) may be at least one selected from the group consisting of polytetrafluoroethylene (PTFE), polyvinylidene difluoride (PVDF), polyethylene (PE), high molecular weight polyethylene (HMWPE), ultra-high molecular weight polyethylene (UHMWPE), polypropylene (PP), carboxymethyl cellulose (CMC), polyvinylphenol, polyvinylpyrrolidine, polyvinyl acetate, polyvinyl alcohol, and polyacetylene, and preferably, polytetrafluoroethylene (PTFE) may be used.
[0065] In one embodiment of the present invention, the first particle (30) may be included in the first region (10) of the electrode mixture layer, and the second particle (40) may be included in the second region (20) of the electrode mixture layer.
[0066] The above first region (10) means a portion formed as a certain region in the direction of the other edge portion based on the transverse direction (TD) cross-section of the electrode mixture layer from one edge portion (50) of the electrode mixture layer, and may be formed on only one side based on the edge portions of both sides of the electrode mixture layer, or may be formed on both sides, and in order to prevent detachment of the edge portion of the electrode plate for a lithium secondary battery, it may be preferably formed on both sides based on the positive electrode edge portion.
[0067] Referring to FIG. 2, in the electrode plate (200) for a lithium secondary battery according to the present invention, if necessary, the first region may be formed on both sides based on the first edge portion (60) and the second edge portion (70) of the electrode combination layer, thereby forming first regions (11, 13) having different areas.
[0068] In one embodiment of the present invention, the first region (10, 11, 13) may be formed at an area ratio of 1% to 20% based on the total area of the electrode mixture layer, for example, at an area ratio of 2% to 19%, 3% to 18%, and preferably 5% to 15%.
[0069] If the area ratio of the first region is less than 1% based on the total area of the electrode mixture layer, there may be a problem that the adhesive strength of the edge of the electrode plate for a lithium secondary battery may decrease, and if it exceeds 20%, there may be a problem that the resistance of the electrode plate may increase, so it is appropriately adjusted within the above range.
[0070] Another embodiment of the present invention provides a lithium secondary battery including the above-described electrode plate for a lithium secondary battery.
[0071] The above lithium secondary battery may be a battery having a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, or may be an all-solid-state battery having a solid electrolyte interposed between the positive electrode and the negative electrode without using a separate separator.
[0072] The electrode plate for the lithium secondary battery according to the present invention may be a positive electrode or a negative electrode.
[0073] The above positive electrode may have a structure in which a positive electrode composite layer is laminated on one or both sides of a positive electrode current collector.
[0074] For example, the positive electrode composite layer may include a positive electrode active material, a conductive material, and a binder, and may further include a positive electrode additive commonly used in the art, if necessary.
[0075] The above-mentioned positive electrode active material is not particularly limited in type as long as it is a material capable of reversible absorption and release of lithium ions, and may include, for example, one or more of a complex compound of metals such as cobalt, manganese, nickel, iron, or a combination thereof; and lithium.
[0076] For a more specific example, as the positive electrode active material, a compound represented by any one of the following chemical formulas may be used. Li a A 1-b R b D2 (in the above formula, 0.90 ≤ a ≤ 1.8 and 0 ≤ b ≤ 0.5); Li a E 1-b R b O 2-c D c (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, and 0 ≤ c ≤ 0.05); LiE 2-b R b O 4-c D c (In the above formula, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); Li a Ni 1-b-c Co b R c Dα (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05 and 0 < α ≤ 2); Li a Ni 1-b-c Co b R c O 2-α Z α (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05 and 0 < α < 2); Li a Ni 1-b-c Co b R c O 2-α Z2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05 and 0 < α < 2); Li a Ni 1-b-c Mn b R c D α (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05 and 0 < α ≤ 2); Li a Ni 1-b-c Mn b R c O 2-α Z α (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05 and 0 < α < 2); Li a Ni 1-b-c Mn b R c O 2-α Z2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05 and 0 < α < 2); Li a Ni b E c G d O2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5 and 0.001 ≤ d ≤ 0.1); Li a Ni b Co c Mn dG e O2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0 ≤ d ≤ 0.5, and 0 ≤ e ≤ 0.1); Li a NiG b O2 (in the above formula, 0.90 ≤ a ≤ 1.8 and 0.001 ≤ b ≤ 0.1); Li a CoG b O2 (in the above formula, 0.90 ≤ a ≤ 1.8 and 0.001 ≤ b ≤ 0.1); Li a MnG b O2 (in the above formula, 0.90 ≤ a ≤ 1.8 and 0.001 ≤ b ≤ 0.1); Li a Mn2G b O4 (wherein 0.90 ≤ a ≤ 1.8 and 0.001 ≤ b ≤ 0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiTO2; LiNiVO4; Li (3-f) J2(PO4)3(0 ≤ f ≤ 2); Li (3-f) Fe2(PO4)3(0 ≤ f ≤ 2); and LiFePO4.
[0077] In the above chemical formula, A is Ni, Co, Mn or a combination thereof; R is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element or a combination thereof; D is O, F, S, P or a combination thereof; E is Co, Mn or a combination thereof; Z is F, S, P or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V or a combination thereof; Q is Ti, Mo, Mn or a combination thereof; T is Cr, V, Fe, Sc, Y or a combination thereof; J is V, Cr, Mn, Co, Ni, Cu or a combination thereof.
[0078] The conductive material is not particularly limited as long as it is conductive and does not cause a chemical change in the battery, and examples thereof include graphite such as natural graphite or artificial graphite; carbon black such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, and summer black; conductive fibers such as carbon fiber or metal fiber; metal powders such as fluorinated carbon, aluminum, and nickel powder; conductive whiskey such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives. The conductive material may be included in an amount of about 0.01 to 10 parts by weight, or 0.01 to 5 parts by weight, or 0.01 to 3 parts by weight, based on 100 parts by weight of the total positive electrode mixture layer.
[0079] The above binder is a component added in consideration of the binding properties of the positive electrode active material, conductive material, and other components of the positive electrode mixture layer, and since the binder included in the electrode mixture layer according to the present invention is as described above, further description is omitted below.
[0080] When the lithium secondary battery according to the present invention is an all-solid-state battery including a solid electrolyte layer between the positive electrode and the negative electrode, the positive electrode may further include a solid electrolyte.
[0081] The above solid electrolyte can be broadly divided into a polymer-based solid electrolyte, an oxide-based solid electrolyte, or a sulfide-based solid electrolyte. For example, when a sulfide-based solid electrolyte is included in the positive electrode, the sulfide-based solid electrolyte may be represented by the following chemical formula 1.
[0082] [Chemical Formula 1]
[0083] Li k M 2 l S m X 2 n
[0084] In the above chemical formula 1, M 2is Sn, Mg, Ba, B, Al, Ga, In, Si, Ge, Pb, N, P, As, Sb, Bi, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Hf, Ta, W, or La, 2 is F, Cl, Br, I, Se, Te, or O, and 0 <k≤6, 0<l≤6, 0<m≤6 및 0≤n≤6이다.
[0085] For example, in the above chemical formula 1, M 2 can be B, Si, Ge, P or N.
[0086] For example, in the above chemical formula 1, X 2 can be F, Cl, Br, I or O.
[0087] For example, the sulfide-based solid electrolyte represented by the above chemical formula 1 is Li2S-P2S5, Li2S-P2S5-LiX, X is a halogen element, Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-Z m S n , m, n are positive numbers, Z is one of Ge, Zn or Ga, Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li p MO q , p, q are positive numbers, M is one of P, Si, Ge, B, Al, Ga In, Li 7-x PS 6-x Cl x , 0≤x≤2, Li 7-x PS 6-x Br x , 0≤x≤2, and Li 7-x PS 6-x I x, may be one or more selected from 0≤x≤2.
[0088] In addition, preferably, the sulfide-based solid electrolyte may be an argyrodite-type solid electrolyte including at least one selected from among Li6PS5Cl, Li6PS5Br, and Li6PS5I.
[0089] The above positive electrode can be manufactured according to a method widely known in the art, and is not limited to a specific manufacturing method, but for example, the positive electrode active material, sulfide-based solid electrolyte, conductive material, and binder can be mixed to make a positive electrode composite paste, and the paste can be spray-dried to granulate the paste, and then applied to a positive electrode current collector.
[0090] The above-described positive electrode current collector is generally made with a thickness of 3 to 500 ㎛. The positive electrode current collector is not particularly limited as long as it has high conductivity and does not cause chemical changes in the battery. For example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. can be used. The current collector can also form fine irregularities on its surface to increase the adhesiveness of the positive electrode active material, and various forms such as a film, sheet, foil, net, porous body, foam, or non-woven fabric can be used.
[0091] In addition to the above-described positive electrode active material, conductive agent, and binder, the positive electrode may further include additives such as fillers, coating agents, dispersants, and ion-conducting aids. The fillers, coating agents, dispersants, and ion-conducting aids may be any known materials commonly used in electrodes of all-solid-state secondary batteries.
[0092] The thickness of the above anode may be, for example, 70 to 150 μm.
[0093] The above negative electrode may include a negative electrode current collector and a negative electrode composite layer.
[0094] The thickness of the negative electrode composite layer is, for example, 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, or 5% or less of the thickness of the positive electrode composite layer. The thickness of the negative electrode active material layer is, for example, 1 μm to 20 μm, 2 μm to 10 μm, or 3 μm to 7 μm.
[0095] The negative electrode composite layer includes, for example, a negative electrode active material that forms an alloy or compound with lithium.
[0096] The negative electrode active material included in the negative electrode composite layer has, for example, a particle form. The average particle diameter of the negative electrode active material having a particle form is, for example, 4 μm or less, 3 μm or less, 2 μm or less, 1 μm or less, or 900 nm or less. The average particle diameter of the negative electrode active material having a particle form is, for example, 10 nm to 4 μm or less, 10 nm to 3 μm or less, 10 nm to 2 μm or less, 10 nm to 1 μm or less, or 10 nm to 900 nm or less.
[0097] The negative electrode active material included in the negative electrode composite layer includes, for example, at least one selected from a carbon-based negative electrode active material and a metal or metalloid negative electrode active material.
[0098] The carbon-based negative electrode active material is, in particular, amorphous carbon. Amorphous carbon includes, but is not limited to, carbon black (CB), acetylene black (AB), furnace black (FB), ketjen black (KB), and graphene, and any material classified as amorphous carbon in the relevant technical field is acceptable. Amorphous carbon is carbon that has no crystallinity or very low crystallinity, and is distinguished from crystalline carbon or graphite-based carbon.
[0099] The metal or metalloid negative electrode active material includes, but is not limited to, one or more selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn), and any metal or metalloid negative electrode active material that forms an alloy or compound with lithium in the relevant technical field may be used. For example, nickel (Ni) does not form an alloy with lithium and therefore is not a metal negative electrode active material.
[0100] The negative electrode composite layer includes a type of negative electrode active material among these negative electrode active materials, or includes a mixture of a plurality of different negative electrode active materials. For example, the negative electrode composite layer includes only amorphous carbon, or includes at least one selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). Alternatively, the negative electrode active material layer includes a mixture of amorphous carbon and at least one selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). The mixing ratio of amorphous carbon and silver (Ag) etc. may be, for example, 10:1 to 1:2, 5:1 to 1:1, or 4:1 to 2:1 by weight, but may not necessarily be limited to this range.
[0101] The negative active material included in the negative electrode composite layer includes a mixture of first particles made of, for example, amorphous carbon and second particles made of a metal or a metalloid. The metal or metalloid includes, for example, gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). The metalloid is alternatively a semiconductor. The content of the second particles may be 8 to 60 wt%, 10 to 50 wt%, 15 to 40 wt%, or 20 to 30 wt% based on the total weight of the mixture.
[0102] The cathode composite layer may further include a conductive material and a binder, similar to the anode composite layer, and the conductive material and binder are the same as those described above.
[0103] The negative electrode current collector is composed of a material that does not react with lithium, i.e., does not form an alloy or compound. The material constituting the negative electrode current collector includes, but is not limited to, copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), and nickel (Ni), and any material that can be used as an electrode current collector in the relevant technical field may be used. The negative electrode current collector may be composed of one of the above-mentioned metals, or may be composed of an alloy or a coating material of two or more metals. The negative electrode current collector is, for example, in the form of a plate or foil.
[0104] The negative electrode composite layer may further include additives used in conventional lithium secondary batteries, such as fillers and dispersants.
[0105] If the lithium secondary battery according to the present invention is an all-solid-state battery, it may further include a solid electrolyte layer between the positive electrode and the negative electrode, and for example, the solid electrolyte layer may include a sulfide-based solid electrolyte. The sulfide-based solid electrolyte may be the same as or different from the sulfide-based solid electrolyte included in the positive electrode.
[0106] For specific details on the sulfide-based solid electrolyte, refer to the positive electrode section described above.
[0107] The elastic modulus of the solid electrolyte layer, i.e., Young's modulus, is, for example, 35 GPa or less, 30 GPa or less, 27 GPa or less, 25 GPa or less, or 23 GPa or less. The elastic modulus of the solid electrolyte layer, i.e., Young's modulus, is, for example, 10 to 35 GPa, 15 to 35 GPa, 15 to 30 GPa, or 15 to 25 GPa. When the solid electrolyte layer has an elastic modulus in this range, pressurization and / or sintering of the solid electrolyte is more easily performed.
[0108] The solid electrolyte layer further includes, for example, a binder. The binder included in the solid electrolyte layer includes, but is not limited to, styrene butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, and the like, and any binder used in the relevant technical field may be used. The binder of the solid electrolyte layer may be the same as or different from the binders of the positive electrode mixture layer and the negative electrode mixture layer.
[0109] A lithium secondary battery according to the present invention can be manufactured, for example, by manufacturing a positive electrode, a negative electrode, and a solid electrolyte layer, respectively, and then laminating these layers.
[0110] The lithium secondary battery according to the present invention can be implemented as a battery module including the lithium secondary battery as a unit battery, a battery pack including the battery module, and a device including the battery pack as a power source.
[0111] At this time, specific examples of the device include, but are not limited to, a power tool that is powered by an electric motor; an electric vehicle including an electric vehicle (EV), a hybrid electric vehicle (HEV), a plug-in hybrid electric vehicle (PHEV), etc.; an electric two-wheeled vehicle including an electric bicycle (E-bike) and an electric scooter (E-scooter); an electric golf cart; and a power storage system.
[0112] Below, specific embodiments of the present invention are presented. However, the embodiments described below are intended solely to specifically illustrate or explain the present invention and are not intended to limit the scope of the invention. Furthermore, any details not described herein are technically feasible to those skilled in the art and thus are omitted.
[0113]
[0114] Manufacturing Example 1: Manufacturing of electrode composite layer particles
[0115] (1) 94 wt% of a cathode active material containing nickel, cobalt, and manganese in a weight ratio of 8:1:1, 1 wt% of a carbon black conductive agent, and 5 wt% of a polytetrafluoroethylene (PTFE) binder were mixed with water as a dispersion medium to prepare a slurry having a viscosity of approximately 1,000 cPs through a homogenizer. At this time, the solid content in the slurry was 30 wt%.
[0116] (2) The slurry manufactured above was introduced into a spray dryer together with hot air at a pressure range of -40 mmH2O and dried to manufacture granule-shaped electrode mixture layer particles. At this time, the conditions of the spray dryer were controlled as follows: inlet temperature 180 ℃, outlet temperature 90 ℃, and rotation speed 18,000 rpm. The average particle diameter (D50) of the obtained granule-shaped particles was measured using a particle size analyzer, and the shape was measured using a scanning electron microscope (SEM), and the results are shown in Fig. 4.
[0117]
[0118] Manufacturing Examples 2 to 6: Manufacturing of electrode mixture layer particles
[0119] In the above Manufacturing Example 1, granule-shaped electrode mixture layer particles were manufactured in the same manner as Manufacturing Example 1, except that the contents of the positive electrode active material, conductive agent, and binder and the spray drying time were as shown in Table 1 below. The average particle diameter (D50) of the electrode mixture layer particles according to Manufacturing Example 2 was measured using a particle size analyzer, and the shape was measured through a scanning electron microscope (SEM), and the results are shown in Fig. 5. The average (D50) of the particles according to Manufacturing Examples 3 to 6 was also measured using the same method and is shown in Table 1 below.
[0120] Manufacturing Example Positive electrode active material (weight%) Conductive material (weight%) Binder (weight%) Average particle size (D50) (㎛) Drying relative speed 194155012941530139415301.5494153025944250169442301
[0121]
[0122] Example 1: Manufacturing of a plate for a lithium secondary battery
[0123] A thickness adjustment bar is used on one side of the current collector layer formed of aluminum foil to adjust the current collector to 25 cm. 2The granular electrode mixture layer particles manufactured in Manufacturing Examples 1 and 5 above in an amount of 400 mg were applied to different areas on a current collector, and a lithium secondary battery electrode plate was manufactured by applying pressure of 0.7 ton per cm and 60°C at a speed of 2 m per minute using a roll-to-roll hot rolling forming device, and the results are shown in Fig. 6.
[0124] Specifically, the electrode mixture layer particles manufactured in Manufacturing Example 1 were applied to one edge portion of the electrode mixture layer produced above and the other edge portion formed on the other side based on the transverse cross-section of the electrode mixture layer, and the electrode mixture layer particles manufactured in Manufacturing Example 5 were applied to an area of the electrode mixture layer excluding the two edge portions, so that granule-shaped particles with a high binder content could be positioned at the edge portion of the electrode mixture layer. The two edge portions were formed to have an area of 30% of the total area of the electrode mixture layer.
[0125] Referring to Fig. 6, it can be seen that the aluminum foil is somewhat crumpled due to increased stress at the edge of the electrode mixture layer, but since electrode mixture layer particles with a high binder content are positioned at the edge of the electrode mixture layer, it can be seen that the electrode mixture layer is not detached from the current collector and stable sheeting of the electrode mixture layer is possible.
[0126]
[0127] Example 2: Manufacturing of a plate for a lithium secondary battery
[0128] In the above Example 1, a lithium secondary battery electrode plate was manufactured in the same manner as in the above Example 1, except that the electrode mixture layer particles manufactured in the above Manufacturing Example 2 were applied to the two edges of the electrode mixture layer, and the results are shown in Fig. 7.
[0129] Referring to Fig. 7, it can be seen that by placing high-binder particles having a smaller average particle diameter compared to Example 1, the stress at the edge of the electrode mixture layer is reduced, and the phenomenon of aluminum foil being crumpled is relatively reduced.
[0130]
[0131] Example 3: Manufacturing of a plate for a lithium secondary battery
[0132] In the above Example 1, a lithium secondary battery electrode plate was manufactured in the same manner as in the above Example 1, except that the electrode mixture layer particles manufactured in the above Manufacturing Example 4 were applied to the two edges of the electrode mixture layer, and the results are shown in Fig. 8.
[0133] Referring to Fig. 8, when using particles manufactured by increasing the drying speed for manufacturing granule-shaped particles compared to the high-binder particles used in Example 2, it can be seen that the phenomenon of aluminum foil wrinkling is significantly reduced and the adhesion between the current collector and the electrode mixture layer is also further improved. This can be understood as a result of improving the adhesive performance of the particles as the binder component within the particles migrates to the surface of the particles along with the evaporation of the dispersion medium as a result of increasing the drying speed compared to Manufacturing Example 1 or 2 when manufacturing granule-shaped particles.
[0134] FIG. 9 shows a scanning electron microscope (SEM) image of a lithium secondary battery electrode plate according to Example 3, and FIG. 10 shows a carbon EDS mapping image of a lithium secondary battery electrode plate according to Example 3.
[0135] Referring to FIGS. 9 and 10, in the case of the lithium secondary battery electrode plate according to the above-described Example 3, it can be seen through the carbon EDS mapping image of the lithium secondary battery electrode plate that granule-shaped particles in which the binder migrates to the surface of the particles are applied to the edge of the electrode mixture layer.
[0136]
[0137] Comparative Example 1: Manufacturing of a plate for a lithium secondary battery
[0138] A thickness adjustment bar is used on one side of the current collector layer formed of aluminum foil to adjust the current collector to 25 cm. 2 The granular electrode mixture layer particles manufactured in the above Manufacturing Example 1 were applied on a current collector in an amount of 400 mg, and pressurized at a speed of 2 m per minute under the conditions of a pressure of 0.7 ton per cm and 60°C using a roll-to-roll hot rolling forming device to manufacture a lithium secondary battery electrode plate formed on the electrode mixture layer on the current collector layer, and the results are shown in Fig. 3 B).
[0139] Referring to Fig. 3 B), when an electrode mixture layer was formed using a single particle manufactured in Manufacturing Example 1, the adhesion between the current collector and the electrode mixture layer was good, but it was confirmed that the aluminum foil was crumpled as a result of increased stress at the edge of the electrode mixture layer.
[0140]
[0141] Comparative Example 2: Manufacturing of a plate for a lithium secondary battery
[0142] In the above Comparative Example 1, a lithium secondary battery electrode plate was manufactured in the same manner as in Comparative Example 1, except that the particles manufactured in Manufacturing Example 2 were applied instead of the particles manufactured in Manufacturing Example 1, and the results are shown in Fig. 3 C).
[0143] Referring to FIG. 3 C), as a result of forming an electrode mixture layer using a single particle manufactured in Manufacturing Example 2, the average particle diameter of the particles was relatively small compared to the particles manufactured in Manufacturing Example 1, so the content of the binder located on the surface of the particles was reduced, resulting in a decrease in adhesive strength, and it was confirmed that the packing of the electrode mixture layer was not performed smoothly.
[0144]
[0145] Comparative Example 3: Manufacturing of a plate for a lithium secondary battery
[0146] In the above Comparative Example 1, a lithium secondary battery electrode plate was manufactured in the same manner as in Comparative Example 1, except that the particles manufactured in Manufacturing Example 4 were applied instead of the particles manufactured in Manufacturing Example 1, and the results are shown in Fig. 3 D).
[0147] Referring to FIG. 3 D), as a result of forming an electrode mixture layer using a single particle manufactured in Manufacturing Example 4, it was confirmed that the adhesive strength between the current collector layer and the electrode mixture layer increased somewhat compared to the electrode plate according to Comparative Example 2, but the packing of the electrode mixture layer was still not performed smoothly.
[0148]
[0149] Comparative Example 4: Manufacturing of a plate for a lithium secondary battery
[0150] In the above Comparative Example 1, a lithium secondary battery electrode plate was manufactured in the same manner as in Comparative Example 1, except that the particles manufactured in Manufacturing Example 5 were applied instead of the particles manufactured in Manufacturing Example 1, and the results are shown in Fig. 3 A).
[0151] Referring to Fig. 3 A), as a result of forming an electrode mixture layer using a single particle manufactured in Manufacturing Example 5, it was confirmed that the content of binder in the particle was greatly reduced compared to the content of the particle manufactured in Manufacturing Example 1, and thus the adhesive force between the current collector and the electrode mixture layer was greatly reduced.
[0152]
[0153] Experimental Example: Evaluation of Initial Discharge Capacity, High-Rate Discharge Characteristics, and Lifetime Characteristics of Lithium Secondary Batteries
[0154] The initial discharge capacity, high-rate discharge characteristics, and life characteristics of all-solid-state batteries including the electrode plates according to Examples 1 to 3, Comparative Examples 1, and Comparative Examples 4 were evaluated.
[0155] The above all-solid-state battery was manufactured by the following method.
[0156] After loading 150 mg of Li6PS5Cl as a solid electrolyte into a mold cell, it is pelletized at a pressure of 70 MPa. The electrode plates according to the manufactured Examples 1 to 3, Comparative Examples 1 and 4 are loaded as a cathode on one side of the solid electrolyte pellet, and Li is loaded on the other side. 0.5 An all-solid-state half-cell was fabricated by loading 100 mg of a composite cathode containing In and a solid electrolyte in a weight ratio of 8:2 and pressurizing at a pressure of 370 MPa. The fastening strength of the bolts of the jig was tightened so that an operating pressure of 70 MPa was applied. To evaluate the all-solid-state half-cell, the cell was sealed to prevent atmospheric infiltration and then transferred to a constant-temperature chamber to conduct the following electrochemical evaluation.
[0157] For the all-solid-state batteries including the electrode plates according to Examples 1 to 3, Comparative Examples 1 and 4, the initial discharge capacity was evaluated by the following test method. The batteries were charged at a rate (C-rate) of 0.1 C until the voltage reached 4.3 V (vs. Li), and then cut-off at 4.3 V (vs. Li). Subsequently, the batteries were discharged at a rate (C-rate) of 0.1 C until the voltage reached 3.0 V (vs. Li) (1 st cycle). The results are shown in Table 2 below.
[0158] For the all-solid-state batteries including the electrode plates according to Examples 1 to 3 and Comparative Examples 1 and 4, the high-rate discharge characteristics were evaluated by the following test method. After charging under constant current (0.1 C) and constant voltage (1.0 V, 0.01 C cut-off) conditions, the batteries were rested for 10 minutes and discharged under constant current (3.0 C) conditions until the voltage reached 2.5 V. The high-rate discharge characteristics at this time are shown in Table 2 below.
[0159] In Table 2 below, the high-rate discharge characteristics can be calculated by the following mathematical equation 1.
[0160] [Mathematical Formula 1]
[0161] High-rate discharge characteristics (%) = (discharge capacity when discharging the cell at 3.0C) / (discharge capacity when discharging the cell at 0.1C) * 100
[0162] For the all-solid-state batteries including the electrode plates according to Examples 1 to 3 and Comparative Examples 1 and 4, the life characteristics were evaluated by the following test method. 100 charge and discharge cycles were performed under the conditions of constant current (1C) and constant voltage (1.0 V, 0.01 C cut-off) charging, 10-minute rest, and constant current (1C, room temperature (20°C), 2.5 V cut-off) discharge, and the discharge capacity after 100 cycles was measured compared to the initial discharge capacity, thereby measuring the life characteristics. The life characteristics at this time are shown in Table 2 below.
[0163]
[0164] Initial discharge capacity (mAh / g) High-rate discharge characteristics (3.0C / 0.1C) (%) Life characteristics (100 cycles, %) Example 1 185.05 883.0 Example 2 188.07 390.0 Example 3 189.08 592.0 Comparative example 1 Electrode detachment prevents evaluation experiment Comparative example 4 Electrode stress (tension) increases, deteriorating battery assembly.
[0165]
[0166] Referring to Table 2 above, it can be seen that the initial discharge capacity, high-rate discharge characteristics, and life characteristics of the all-solid-state battery including the electrode mixture layer according to Example 3, which uses particles having a relatively small average particle diameter and a fast drying speed for particle production, when applying high-binder particles to the electrode mixture layer, are the best.
[0167] [Explanation of symbols]
[0168] 10, 11, 13: Area 1
[0169] 20: Second Area
[0170] 30: First particle
[0171] 40: Second particle
[0172] 50: Edge of the electrode mixture layer
[0173] 60: First edge of the electrode mixture layer
[0174] 70: Second edge of the electrode mixture layer
[0175] 100, 200: Electrode plates for lithium secondary batteries
Claims
1. Current collector layer; and Including an electrode composite layer formed on one or both sides of the current collector layer, The electrode mixture layer includes a first region formed in the direction of the other edge from one edge of the electrode mixture layer based on the transverse direction (TD) cross-section of the electrode mixture layer, and a second region excluding the first region. The above electrode composite layer includes first particles and second particles each including an electrode active material, a conductive material, and a binder, The first particle has a higher binder content than the second particle, or contains 30% or more of the total binder content contained in the particle in a region that is 20% or less of the length from the outermost surface of the particle to the center of the particle. Electrode plates for lithium secondary batteries.
2. In paragraph 1, The first particle is included in the first region, The second particle is included in the second region, Electrode plates for lithium secondary batteries.
3. In paragraph 1, The first and second particles are in the form of granules, Electrode plates for lithium secondary batteries.
4. In paragraph 1, The average particle diameters of the first and second particles are each 30 to 100 μm, Electrode plates for lithium secondary batteries.
5. In paragraph 1, The above first region is formed at an area ratio of 1% to 20% based on the total area of the electrode mixture layer. Electrode plates for lithium secondary batteries.
6. In paragraph 1, The binder content ratio of the first particle and the binder content ratio of the second particle is 1.2:1 to 3.0:
1. Electrode plates for lithium secondary batteries.
7. In paragraph 1, The binder included in the first and second particles is at least one selected from the group consisting of polytetrafluoroethylene (PTFE), polyvinylidene difluoride (PVDF), polyethylene (PE), high molecular weight polyethylene (HMWPE), ultra-high molecular weight polyethylene (UHMWPE), polypropylene (PP), carboxymethyl cellulose (CMC), polyvinylphenol, polyvinylpyrrolidine, polyvinyl acetate, polyvinyl alcohol, and polyacetylene. Electrode plates for lithium secondary batteries.
8. In paragraph 1, The first particle comprises 3.6 to 9 wt% of a binder based on the total weight of the first particle, The second particle contains a binder in an amount of 1 to 5 wt% based on the total weight of the second particle. Electrode plate for lithium secondary battery.
9. In paragraph 1, The first particle and the second particle each independently further include a sulfide-based solid electrolyte represented by the following chemical formula 1. Electrode plates for lithium secondary batteries: [Chemical Formula 1] Li k M 2 l S m X 2 n In the above chemical formula 1, M 2 is Sn, Mg, Ba, B, Al, Ga, In, Si, Ge, Pb, N, P, As, Sb, Bi, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Hf, Ta, W, or La, 2 is F, Cl, Br, I, Se, Te, or O, and 0 <k≤6, 0<l≤6, 0<m≤6 및 0≤n≤6이다.
10. A lithium secondary battery comprising a lithium secondary battery electrode plate according to Article 1.
Citation Information
Patent Citations
Method of manufacturing electrode for lithium ion secondary battery
JP2016122631A
Lithium ion secondary battery
JP2018073602A
Electrodes for lithium-ion secondary batteries and methods for manufacturing the same
JP5403153B2
Linker apparatus for controling tension of distribution line
KR102331395B1
Estimation system of concrete strength by impact hammer test
KR102579510B1