Method for preparing complex cathode material for lithium sulfur battery, and lithium sulfur battery comprising complex cathode material prepared thereby
The composite cathode material for lithium-sulfur batteries, featuring a multi-walled carbon nanotube-sulfur complex and oxygen-functionalized single-walled carbon nanotubes, addresses conductivity issues and polysulfide leakage, enhancing battery performance and stability by forming a network structure that binds lithium polysulfide, thus improving charge/discharge efficiency and lifespan.
Patent Information
- Application Number
- PCT/KR2024/001264
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-03
- Filing Date
- 2024-01-26
- Publication Date
- 2024-10-10
AI Technical Summary
Lithium-sulfur batteries face challenges with poor electron transfer and sulfur leakage due to low conductivity of sulfur-based positive electrode active materials, leading to reduced battery performance and lifespan due to the 'Shuttle reaction' where lithium polysulfide dissolves and reacts with the lithium metal anode.
A composite cathode material is manufactured by creating a multi-walled carbon nanotube-sulfur complex and dispersing single-walled carbon nanotubes with oxygen-containing functional groups to form a network structure that binds lithium polysulfide, preventing its elution and improving charge/discharge efficiency.
The composite cathode material suppresses lithium polysulfide elution, maintains electrode stability after repeated cycles, and enhances the charge/discharge efficiency of lithium-sulfur batteries by preventing polysulfide penetration and diffusion, thereby improving battery performance and lifespan.
Smart Images

Figure KR2024001264_10102024_PF_FP_ABST
Abstract
Description
Method for manufacturing composite cathode material for lithium sulfur battery and lithium sulfur battery including composite cathode material manufactured thereby
[0001] The present invention relates to a method for manufacturing a composite cathode material for a lithium sulfur battery and a lithium sulfur battery including a composite cathode material manufactured thereby.
[0002] The commercialization of lithium secondary batteries has significantly contributed to the development of portable devices and electric vehicles, being applied in various fields. Currently, metal oxides such as cobalt, nickel, and manganese are widely used as essential cathode materials for lithium-ion batteries used in representative IT devices, small home appliances, and electric vehicles. However, lithium-ion batteries composed of these metal oxides (anode) and graphite (cathode) have limited theoretical capacity during charge / discharge, limiting their performance as high-energy-density, long-term batteries.
[0003] To address these issues, active research is being conducted on lithium secondary battery systems utilizing sulfur (S), sodium (Na), and oxygen (O), which are readily available on Earth. Research is underway using various materials based on the fundamental mechanism of electron movement due to the difference in electromotive force between the positive and negative electrodes. Among these, lithium-sulfur batteries are batteries based on the serial electrochemical redox reaction of lithium and sulfur.
[0004] In a lithium-sulfur battery, an oxidation reaction of lithium occurs at the negative electrode during a discharge reaction, and a reduction reaction of sulfur occurs at the positive electrode. Before discharge, sulfur has a cyclic S8 structure, and during a reduction reaction (discharge), the S-S bond is broken, the oxidation number of S decreases, and during an oxidation reaction (charge), the S-S bond is re-formed, the oxidation number of S increases. This oxidation-reduction reaction is used to store and generate electrical energy. During this reaction, sulfur is reduced from the cyclic S8 to form lithium polysulfide (Li2S) with a linear structure. x , x = 8, 6, 4, 2, 1) and eventually, when these lithium polysulfides are completely reduced, lithium sulfide (Li2S) is ultimately generated. The discharge behavior of a lithium-sulfur battery is characterized by showing a discharge voltage in steps, unlike a lithium ion battery, due to the process of reducing each lithium polysulfide.
[0005] However, in the case of lithium-sulfur secondary batteries, there was a problem that it was difficult to secure high performance due to poor electron transfer during charge and discharge due to sulfur-based cathode active materials with high theoretical capacity but low conductivity. In addition, when sulfur is used as a cathode active material, sulfur is released into the electrolyte during the oxidation-reduction reaction, which not only reduces the battery life, but also causes lithium polysulfide, a reduced substance of sulfur, to be eluted, resulting in a phenomenon known as the "shuttle reaction." The shuttle reaction is a reaction in which Li2S, one of the polysulfide species, which is a reaction intermediate generated during the discharge process of a lithium-sulfur battery, is eluted. x(1≤x≤8) is highly soluble in ether-based electrolytes, and the dissolved polysulfide diffuses from the positive electrode through the separator to the lithium metal negative electrode, causing a chemical side reaction with the lithium metal negative electrode. This phenomenon causes serious problems such as loss of active material in the positive electrode and deterioration of the surface condition of the lithium metal negative electrode, which ultimately worsens the life characteristics of lithium-sulfur secondary batteries.
[0006] To address this, research is underway to minimize this phenomenon using various materials. Korean Patent Publication No. 10-2002-39823 proposes a lithium-sulfur battery positive electrode obtained by coating a slurry of a positive electrode active material for a lithium-sulfur battery on a porous current collector made of carbon fiber, and Korean Patent Publication No. 10-2011-40565 proposes a method of incorporating a sulfur electrode active material into a fiber conductor by spraying a solution containing carbon nanotubes onto a fiber conductor using carbon felt.
[0007] However, although the above conventional technologies have made some progress in improving charge / discharge efficiency and capacity by suggesting technologies for including active materials in porous collectors, supports, or conductors in battery electrodes, the performance of active materials has not yet been sufficiently maximized, and in particular, there have been problems in that active materials leak out of the support or conductor and are lost, or in that stability in terms of conductivity is reduced.
[0008] Meanwhile, attempts to utilize carbon materials such as carbon nanotubes as battery materials to improve conductivity are ongoing. However, although carbon nanotubes are attracting attention as a conductive material due to their unique electrical, thermal, and physicochemical properties, they have the disadvantage of being difficult to secure dispersion stability due to the aggregation into bundle shapes caused by entanglement.
[0009] Single-walled carbon nanotubes, with diameters of only about 1 nm, cannot exist alone and tend to aggregate into bundles due to van der Waals forces. Multi-walled carbon nanotubes, due to their larger diameters, may also aggregate, but their properties are more similar to the entanglement of polymer chains. Some double-walled carbon nanotubes, with smaller diameters, exhibit properties similar to single-walled carbon nanotubes, while others, with larger diameters, exhibit properties similar to multi-walled carbon nanotubes.
[0010] Due to these characteristics, the aggregation of carbon nanotubes has been difficult to physically address. Therefore, a method for pretreating carbon nanotubes is needed to ensure stable dispersion without bundling, aggregation, or precipitation in the solvent.
[0011] Accordingly, the present inventors have developed a method for manufacturing a composite cathode material for a lithium-sulfur battery, which includes a highly concentrated carbon nanotube dispersion and a multi-walled carbon nanotube-sulfur composite (MWCNT-S complex) in which oxygen-containing functional groups are introduced through pretreatment to suppress the dissolution of lithium polysulfide and improve charge-discharge efficiency, thereby providing excellent battery performance, and a lithium-sulfur battery including the composite cathode material manufactured thereby, and have completed the present invention.
[0012] The present invention provides a method for manufacturing a composite cathode material for a lithium sulfur battery and a lithium sulfur battery including a composite cathode material manufactured thereby as a technical problem.
[0013] To achieve the above technical task,
[0014] A method for manufacturing a cathode material for a lithium sulfur battery capable of suppressing the dissolution of lithium polysulfide,
[0015] (1) A step of manufacturing a multi-walled carbon nanotube-sulfur composite (MWCNT-S complex) by ball milling, mixing, and heat-treating multi-walled carbon nanotubes (MWCNT) and sulfur precursors;
[0016] (2) A step of manufacturing a carbon nanotube dispersion (CNT solution) in which carbon nanotubes having oxygen-containing functional groups are highly dispersed;
[0017] (3) Step of preparing single-walled carbon nanotubes (SWCNT); and
[0018] (4) A step of manufacturing a composite cathode material by mixing and dispersing the multi-walled carbon nanotube-sulfur composite, the carbon nanotube dispersion, and the single-walled carbon nanotube (SWCNT); including,
[0019] The above composite cathode material is a carbon nanotube having an oxygen-containing functional group, and forms a network structure with the multi-walled carbon nanotube-sulfur composite or the single-walled carbon nanotube,
[0020] The oxygen-containing functional group is characterized in that it can bind to lithium polysulfide and suppress the dissolution of lithium polysulfide by the network structure.
[0021] A method for manufacturing a composite cathode material for a lithium sulfur battery is provided.
[0022] In order to achieve the above other technical tasks, a lithium sulfur battery including a composite cathode material manufactured according to the above manufacturing method is provided.
[0023] The composite cathode material for a lithium sulfur battery manufactured according to the present invention includes the multi-walled carbon nanotube-sulfur composite (MWCNT-S complex), single-walled carbon nanotube (SWCNT), and pretreated carbon nanotube dispersion (CNT solution), thereby suppressing the dissolution of lithium polysulfide and maintaining the cathode material even after repeated cycles, thereby increasing the charge-discharge efficiency.
[0024] The lithium sulfur battery of the present invention can increase charge / discharge efficiency by including the composite cathode material to suppress the elution of lithium polysulfide from the cathode and maintain the cathode material even after repeated cycles, and by combining with a phosphorus-doped separator to enhance the effect of suppressing the penetration and diffusion of lithium polysulfide into the cathode, thereby improving the performance and lifespan stability of the lithium-sulfur battery.
[0025] Figure 1 is a schematic diagram showing a method for manufacturing a positive electrode active material according to an embodiment of the present invention.
[0026] Figure 2 shows the results of thermogravimetric analysis of Pristine, Low Ox-SWCNT, and High Ox-SWCNT samples according to examples and comparative examples of the present invention.
[0027] Figures 3 and 4 are charge-discharge graphs of a lithium-sulfur battery according to one embodiment of the present invention.
[0028] Figures 5 and 6 are graphs showing changes in capacity and coolant efficiency according to the number of charge / discharge cycles of a lithium-sulfur battery according to one embodiment of the present invention.
[0029] Figures 7 and 8 are graphs of capacity according to the number of charge / discharge cycles of a lithium-sulfur battery according to one embodiment of the present invention.
[0030] The present invention is susceptible to various modifications and embodiments. Specific embodiments are illustrated and described in detail in the drawings. However, this is not intended to limit the present invention to specific embodiments, but rather to encompass all modifications, equivalents, and alternatives falling within the spirit and technical scope of the present invention. Throughout the description of each drawing, similar reference numerals have been used to designate similar components.
[0031] The terminology used herein is merely for the purpose of describing specific embodiments and is not intended to limit the present invention. The singular expression includes the plural expression unless the context clearly indicates otherwise. In the present invention, it should be understood that the terms "comprise" or "have" indicate the presence of a feature, number, step, reaction, component, or combination thereof described in the specification, but do not preclude the possibility of the presence or addition of one or more other features, numbers, steps, reactions, components, or combinations thereof.
[0032] Unless otherwise defined, all terms used herein, including technical or scientific terms, have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. Terms defined in commonly used dictionaries should be interpreted as having a meaning consistent with their meaning in the context of the relevant technology, and shall not be interpreted in an idealized or overly formal sense unless explicitly defined herein.
[0033]
[0034] According to one aspect of the present invention, there is provided a method for manufacturing a cathode material for a lithium sulfur battery capable of suppressing the dissolution of lithium polysulfide, comprising: (1) a step of ball milling and mixing multi-walled carbon nanotubes (MWCNTs) and a sulfur precursor, and heat-treating the mixture to manufacture a multi-walled carbon nanotube-sulfur composite (MWCNT-S complex); (2) a step of manufacturing a carbon nanotube dispersion (CNT solution) in which carbon nanotubes having oxygen-containing functional groups are highly dispersed; (3) a step of preparing single-walled carbon nanotubes (SWCNTs); And (4) a step of mixing and dispersing the multi-walled carbon nanotube-sulfur composite, the carbon nanotube dispersion, and the single-walled carbon nanotube (SWCNT) to produce a composite cathode material; wherein the composite cathode material is characterized in that the carbon nanotube having the oxygen-containing functional group forms a network structure with the multi-walled carbon nanotube-sulfur composite or the single-walled carbon nanotube, and the oxygen-containing functional group binds to lithium polysulfide to suppress the elution of lithium polysulfide by the network structure.
[0035] Accordingly, the manufacturing method of the present invention includes sulfur as an active material and a conductive material, and is specifically characterized by manufacturing a composite cathode material including a multi-walled carbon nanotube-sulfur complex (MWCNT-S complex), a single-walled carbon nanotube (SWCNT), and a carbon nanotube dispersion in which carbon nanotubes having oxygen-containing functional groups are dispersed at a high concentration through pretreatment.
[0036] First, the steps for manufacturing a multi-walled carbon nanotube-sulfur composite are described.
[0037] In the present invention, a multi-walled carbon nanotube-sulfur composite is manufactured by mixing, milling, and heat-treating multi-walled carbon nanotubes and a sulfur compound or a sulfur precursor and multi-walled carbon nanotube powder to coat the sulfur compound on the surface of the multi-walled carbon nanotube powder.
[0038] The sulfur precursor may include not only elemental sulfur but also various kinds of sulfur compounds or mixtures thereof, examples of which include disulfides, poly(disulfides), polysulfides, thiols and their modified products. Specifically, Li2Sn(n≥1), organosulfur compounds or carbon-sulfur polymers ((C2S x )n, x=2.5∼50, n=2), etc., and also includes the use of mono- and / or di-sulfides.
[0039] Carbon nanotubes are giant molecules with unique physical properties depending on their size and shape, consisting of hexagonal honeycomb graphite sheets, each carbon atom bonded to three other carbon atoms, rolled into a nanoscale diameter. Because they are hollow, they are lightweight, have electrical conductivity comparable to copper, thermal conductivity comparable to diamond, and tensile strength comparable to steel. Depending on their rolled shape, they are classified as single-walled carbon nanotubes (SWCNTs), multi-walled carbon nanotubes (MWCNTs), and rope carbon nanotubes.
[0040] The multi-walled carbon nanotube used in the present invention is a tube-shaped tube with multiple layers of walls composed of carbon atoms, and the single-walled carbon nanotube is a tube-shaped tube with a single wall composed of carbon atoms.
[0041] The above multi-walled carbon nanotubes (MWCNTs) (diameter = 9.5 nm, Nanocyl (Belgium)) and sulfur powder (Sulfur) may be mixed in a ratio of MWCNT : S = 2~4 : 6~8. If the ratio of sulfur is less than 6, it may be difficult to exhibit high-loading electrodes and high energy density of the electrodes, and if it exceeds 8, the conductivity of sulfur, which is an insulator, may not be sufficiently secured, so that sufficient discharge capacity may not be derived and it may be difficult to operate the battery at the expected C-rate.
[0042] Next, a step for producing a carbon nanotube dispersion containing carbon nanotubes having oxygen-containing functional groups is described.
[0043] In the present invention, the step of preparing a carbon nanotube dispersion includes (2-1) a step of mixing a composite powder containing at least one of a sulfate and a phosphate mixed with bundle-shaped carbon nanotubes, an acid solution, and an alkali metal-containing oxidizing agent while applying shear stress, so that at least one of the sulfate and the phosphate co-intercalates between adjacent layers of the carbon nanotubes to prepare debundled carbon nanotubes; (2-2) a step of heating the debundled carbon nanotubes at 30 to 50°C, so as to prepare carbon nanotubes to which an oxygen-containing functional group is introduced by at least one of the sulfate and the phosphate and the acid solution; (2-3) a step of washing and filtering the carbon nanotubes to which the oxygen-containing functional group is introduced, so as to prepare pretreated carbon nanotubes; and (2-4) a step of dispersing the pretreated carbon nanotubes in a solvent to prepare a carbon nanotube dispersion.
[0044] Oxygen-containing functional groups are introduced into carbon nanotubes through pretreatment, and specifically, carbon nanotubes having oxygen-containing functional groups can be manufactured by modifying carbon nanotubes with a salt solution of at least one of sulfate and phosphate and an acid solution.
[0045] In the present invention, the carbon nanotubes that can be pretreated may be at least one of a single-walled carbon nanotube (SWCNT), a double-walled carbon nanotube (DWCNT), and a multi-walled carbon nanotube (MWCNT). Among these, single-walled carbon nanotubes have a diameter of only about 1 nm, and therefore cannot exist alone, but have the characteristic of aggregating into a bundle shape due to van der Waals attraction. Multi-walled carbon nanotubes may aggregation due to their large diameter, but rather exhibit characteristics similar to the entanglement of polymer chains. In the case of double-walled carbon nanotubes, some with small diameters have characteristics similar to single-walled carbon nanotubes, and some with large diameters have characteristics similar to multi-walled carbon nanotubes.
[0046] Carbon nanotubes, possessing the above characteristics, are attracting attention as conductive materials due to their unique electrical, thermal, and physicochemical properties. However, they suffer from the disadvantage of bundle-like aggregation caused by entanglement, making it difficult to ensure dispersion stability. In particular, the aggregation of carbon nanotubes has been difficult to physically address.
[0047] Accordingly, a method for pretreating carbon nanotubes is required to disperse the carbon nanotubes in a stable state without bundling, agglomeration, or precipitation in a solvent. Therefore, in the present invention, the carbon nanotubes are mixed in a solid state with at least one of sulfate and phosphate to prepare a composite powder, and then the composite powder, an acid solution, and an alkali metal-containing oxidizing agent are added and mixed to prepare debundled carbon nanotubes.
[0048] The sulfate may be at least one selected from the group consisting of sodium sulfate (Na2SO4), potassium sulfate (K2SO4), sodium hydrogen sulfate (NaHSO4), potassium hydrogen sulfate (KHSO4), potassium peroxymonosulfate (KHSO5), and ammonium persulfate ((NH4)2S2O8), and the phosphate may be at least one selected from the group consisting of dipotassium phosphate (K2HPO4) and potassium phosphate (KH2PO4).
[0049] The acid solution may be selected from the group consisting of sulfuric acid (H2SO4), nitric acid (HNO3), phosphoric acid (H3PO4), hydrogen peroxide (H2O2), and hydrochloric acid (HCl). However, the acid solution is not limited to the types described above, and various substances that can be included in a liquid acid solution may be used.
[0050] If only sulfate or phosphate is used, the oxidation efficiency of carbon nanotubes may be somewhat low, so it is recommended to use an oxidizing agent containing an alkali metal together. In the case of an oxidizing agent containing an alkali metal, one or more of potassium permanganate (KMnO4), sodium chlorate (NaClO3), sodium perchlorate (NaClO4), potassium chlorate (KClO3), potassium perchlorate (KClO4), and potassium peroxymonosulfate (KHSO5) can be used. If a general oxidizing agent (e.g., sulfuric acid or nitric acid) is used instead of an alkali metal-containing oxidizing agent, oxidation proceeds only when the temperature is raised to a high temperature of approximately 70°C or higher, which is not recommended.
[0051] It is desirable to minimize the amount of sulfate or phosphate in the composite powder so that the debundled carbon nanotubes form a liquid crystal phase. Usually, when using nitrate instead of sulfate or phosphate, it is used in an amount exceeding 10 times the amount of carbon nanotubes. However, in the present invention, it is desirable to form a liquid crystal phase using shear stress, and accordingly, it is sufficient to mix at least one of sulfate and phosphate in a weight ratio of 0.1 to 10 per 1 weight of carbon nanotubes.
[0052] The above debundled carbon nanotubes are heated at 30 to 50°C to produce carbon nanotubes having oxygen-containing functional groups introduced by at least one of sulfate and phosphate and an acid solution. When heat treatment is performed, at least one of sulfate and phosphate, which were positioned in a solvated state by the acid solution between adjacent layers of the carbon nanotubes, and oxygen-containing functional groups such as carboxyl groups and hydroxyl groups can be introduced to the interior, surface, or terminal of the carbon nanotubes by the acid solution.
[0053] The heat treatment can be carried out at a temperature close to room temperature of 30 to 50°C, preferably in the range of 30 to 45°C. The heat treatment can be carried out for 30 minutes to 24 hours, preferably for 1 to 10 hours.
[0054] The use of sulfate or phosphate allows the heating temperature to be lowered to at least 30°C, which has the advantage of enabling stable heat treatment without raising the temperature to near 100°C. Heating the debundled carbon nanotubes in the liquid crystal phase at temperatures below 30°C or for less than 1 hour takes a long time for oxygen-containing functional groups to form in the carbon nanotubes, so it is preferable that the temperature be at least 30°C or higher. If the temperature exceeds 50°C or for more than 24 hours, there is a disadvantage that the electrical conductivity may be reduced due to the formation of a defect structure caused by the excessive introduction of oxygen-containing functional groups into the carbon nanotubes.
[0055] Carbon nanotubes that have been pretreated in this manner and have dispersibility can be dispersed in one or more solvents selected from water (H2O), alcohol, dimethylformamide (DMF), N-methylformamide (NMF), and N-methyl-2-pyrrolidone (NMP) to produce a carbon nanotube dispersion. Preferably, a water-dispersible carbon nanotube dispersion can be produced by dispersing it in water.
[0056] In the present invention, the carbon nanotube dispersion is characterized in that the content of oxygen-containing functional groups introduced into the carbon nanotubes through pretreatment is 0.5 to 20 wt.%. If the content of oxygen-containing functional groups is less than 0.5 wt.%, the lithium polysulfide adsorption ability is reduced, which is undesirable, and if it exceeds 20 wt.%, the electrical conductivity increases excessively, which is undesirable.
[0057] In the present invention, the carbon nanotube dispersion is characterized in that the content of the carbon nanotube solid dispersed in the solvent is 0.5 to 6.3 wt.% by introducing oxygen-containing functional groups into the carbon nanotubes through pretreatment. Preferably, it may be a water-dispersible solution in which carbon nanotubes having oxygen-containing functional groups are dispersed. In the present invention, the carbon nanotube dispersion can be applied as a water-dispersible solution in which oxygen-containing functional groups are introduced into the carbon nanotubes and thus they are uniformly dispersed without a separate dispersant. Preferably, it is characterized in that the content is 4.5 to 6.3 wt.%.
[0058] Next, single-walled carbon nanotubes are prepared.
[0059] In the present invention, the single-walled carbon nanotube (SWCNT) is not limited to a product of a specific manufacturer, but may be a commonly used single-walled carbon nanotube (CNT) powder.
[0060] Finally, a composite cathode material is manufactured by mixing and dispersing a multi-walled carbon nanotube-sulfur composite, a carbon nanotube dispersion, and a single-walled carbon nanotube.
[0061] At this time, the multi-walled carbon nanotube-sulfur complex (MWCNT-S complex), single-walled carbon nanotube (SWCNT), and carbon nanotube dispersion (CNT solution) can be mixed in a weight ratio of 70 to 80: 20 to 30: 1 to 10. Preferably, it can be 75: 22: 3.
[0062] The composite cathode material for a lithium-sulfur battery manufactured according to the present invention comprises carbon nanotubes having the oxygen-containing functional group, which form a network structure with the multi-walled carbon nanotube-sulfur composite or the single-walled carbon nanotube, and the oxygen-containing functional group can bind to lithium polysulfide to suppress the dissolution of lithium polysulfide by the network structure. By suppressing the dissolution of lithium polysulfide, the cathode material is maintained continuously even after repeated cycles, thereby improving electrochemical properties such as increasing the charge / discharge efficiency of a lithium-sulfur battery.
[0063]
[0064] According to another aspect of the present invention, the present invention can provide a lithium-sulfur battery comprising a composite cathode material manufactured according to the above method. In the present invention, the lithium-sulfur battery means a battery comprising the composite cathode material as a cathode material and using lithium metal as an anode material. In the lithium-sulfur battery, an oxidation reaction of lithium can occur at the cathode during discharge, and a reduction reaction of sulfur can occur at the anode.
[0065] In the lithium-sulfur battery of the present invention, the separator may use a generally applied PE, or a separator coated with carbon powder having phosphorus (P) deposited on at least one side or at least a part of one side may be used. Preferably, a separator coated with carbon powder having phosphorus (P) deposited on it may be used. This P-deposited carbon powder layer is formed by chemically bonding phosphorus (P) deposited on the surface of a carbon material to form lithium polysulfide (Li2S). x ) is adsorbed. This capturing by chemical bonding is achieved by PS bonding and P-Li bonding, and the diffusion of lithium polysulfide can be suppressed.
[0066] The above carbon powder may include at least one selected from the group consisting of SWCNT, MWCNT, DWCNT, CB (carbon black), DB (Denka black), SPB (Super P black), KB (Ketjen black), AB (acetylene black), and activated carbon.
[0067] The above P source may include at least one compound selected from the group consisting of NaPO2H2, Li3PO4, Red phosphate, KH2PO4, AlPO4, Al(H2PO4)3, and (NH4)2HPO4.
[0068] In the present invention, the content of P coated on the carbon powder may preferably be 4 to 40 wt%, 4 to 30 wt%, 4 to 20 wt%, or 4 to 10 wt% with respect to the total weight of the carbon.
[0069] The deposition of phosphorus may utilize a reactor comprising a first chamber and a second chamber, but is not limited thereto, and the reactor may also be composed of one chamber.
[0070] The first chamber is equipped with a P source sample, and the P source sample can be a liquid or solid source containing phosphorus. The first chamber supplies the P source to the second chamber for phosphorus (P) deposition. The supplied P source is preferably a gaseous source, for example, PO x (x=0~4) can be included. An inert gas such as Ar can be used as a carrier gas for inducing a P source from the first chamber to the second chamber.
[0071] In the present invention, for heating the source, the first chamber may be provided with a heating means for vaporizing the liquid or solid source. The interior of the first chamber may be heated to a temperature suitable for vaporizing the source by the heating means.
[0072] A P source of gaseous phase supplied from the first chamber is introduced into the second chamber through an induction pipe. The second chamber is equipped with carbon powder, and the introduced gaseous phase source reacts with the carbon powder to coat the surface of the carbon particles.
[0073] The ratio of the above P source specimen (S1) and carbon powder specimen (S2) can be loaded at a preset ratio. For example, the weight ratio of S1:S2 is preferably in the range of 5:1 to 10:1.
[0074] In the present invention, the content of P coated on the carbon powder may preferably be 4 to 40 wt%, 4 to 30 wt%, 4 to 20 wt%, or 4 to 10 wt% relative to the total weight of the carbon. The content of P coated may be controlled by the temperature of the second chamber. For example, as the temperature of the second chamber increases, the content of P coated may decrease.
[0075] P in the above carbon powder layer is phosphorus (P) on the surface of carbon particles, phosphorus atom or phosphorus compound, (PO4) 3-It can exist in an ionic state such as Li and can react with Li to produce a compound such as Li3PO4. The reaction layer containing Li3PO4 can increase the ionic conductivity of the membrane.
[0076] Although the present invention describes chemical adsorption of lithium polysulfide, the carbon powder layer can physically adsorb lithium polysulfide, and the aforementioned chemical reaction can occur following the physical adsorption. To facilitate physical adsorption of the carbon powder layer, carbon powder with a high specific surface area can be used. For example, a carbon material with a high porosity, such as activated carbon, can be used.
[0077] After forming a phosphorus-containing deposition layer on the surface of carbon powder particles, the carbon powder is dispersed in a solvent to produce a carbon powder solution. Subsequently, a binder such as PVDF is dissolved in the solvent and mixed with the carbon powder solution, and the mixed solution is applied to one or both sides of a separator to produce a separator.
[0078] Through the mechanism described above, the separator having the P-deposited carbon powder layer can suppress the penetration and diffusion of lithium polysulfide into the negative electrode, thereby contributing to improving the performance and lifespan stability of a lithium-sulfur battery.
[0079] In the present invention, the lithium negative electrode is a material capable of absorbing and releasing lithium ions, and is not limited to any material containing lithium. For example, it may be metallic lithium, a lithium alloy, a metal oxide, a metal sulfide, etc.
[0080] The electrolyte used in the lithium-sulfur battery of the present invention may be composed of conventional materials that can be used in lithium-sulfur batteries. The electrolyte is a medium that transfers ions, and both solid and liquid electrolytes may be used as the electrolyte of the present invention. However, the use of a liquid electrolyte is preferred because it facilitates the implementation of improved battery performance.
[0081] As described above, the lithium-sulfur battery of the present invention uses a composite cathode material including a multi-walled carbon nanotube-sulfur complex (MWCNT-S complex), a single-walled carbon nanotube (SWCNT), and a carbon nanotube dispersion (CNT solution) in which carbon nanotubes having oxygen-containing functional groups are dispersed, thereby suppressing the elution of lithium polysulfide from the cathode and maintaining the cathode material even after repeated cycles, thereby increasing the charge-discharge efficiency.
[0082] Furthermore, when combined with a doped separator, it has excellent technical characteristics in that it improves the performance and lifespan stability of lithium-sulfur batteries by enhancing the effect of inhibiting the penetration and diffusion of lithium polysulfide into the negative electrode.
[0083]
[0084] Hereinafter, embodiments of the present invention will be described in more detail. However, the following embodiments are provided merely to aid understanding of the present invention, and the scope of the present invention is not limited thereby.
[0085]
[0086] <Example>
[0087] Figure 1 is a schematic diagram illustrating a method for manufacturing a positive electrode active material according to an embodiment of the present invention. Hereinafter, the specific manufacturing method will be described with reference to Figure 1.
[0088]
[0089] Pretreated carbon nanotube dispersion
[0090] A composite powder was prepared by mixing 5 g of bundle-shaped single-walled carbon nanotubes (SWCNTs) and 5 g of sodium sulfate (Na2SO4) in a powder state. The prepared composite powder was added to 500 ml of a sulfuric acid solution and mixed while stirring at 1,000 rpm for 10 minutes using a paste mixer capable of rotation and revolution, thereby preparing a debundled carbon nanotube liquid crystal phase.
[0091] The content of oxygen functional groups introduced into carbon nanotubes is affected by the amount of oxidizing agent added, temperature, and time. In this example, in order to produce carbon nanotubes with high and low oxygen functional group contents, 20 g and 10 g of potassium peroxymonosulfate, which are oxidizing agents, were added respectively, and stirred for an additional 10 minutes to produce a carbon nanotube liquid crystal phase in which the oxidizing agent and intercalant were evenly mixed in a sulfuric acid solution. This was heated at 60°C for 20 hours to introduce hydroxyl and carboxyl groups into the carbon nanotubes. Afterwards, an excess of distilled water was added, and the pretreated carbon nanotubes were obtained by repeatedly centrifuging and filtering to wash and remove moisture.
[0092] The obtained carbon nanotubes were dispersed in water to prepare a carbon nanotube dispersion. Each sample was named as Pristine, Low Ox-SWCNT, and High Ox-SWCNT according to the oxygen functional group content as shown in Table 1 below.
[0093] Name Type Pristine Original SWCNT in water (oxygen functional group 0 wt.%) Low Ox-SWCNTOx-SWCNT in water (oxygen functional group 4 wt.%) High Ox-SWCNTOx-SWCNT in water (oxygen functional group 11 wt.%)
[0094] FIG. 2 shows the thermogravimetric analysis results of Pristine, Low Ox-SWCNT, and High Ox-SWCNT samples according to an embodiment of the present invention. It was confirmed that Pristine SWCNT has 0 wt.% of oxygen functional groups removed around 200 degrees Celsius, and Low Ox-SWCNT and High Ox-SWCNT have approximately 4 wt.% and 11 wt.% of oxygen functional groups introduced, respectively. Pristine has a content of carbon nanotube solids dispersed in a solvent of only 0.4 wt.%, whereas Low Ox-SWCNT and High Ox-SWCNT with oxygen-containing functional groups introduced have 4.5 wt.% and 6.3 wt.% of carbon nanotube solids dispersed in water, respectively.
[0095]
[0096] Fabrication of multi-walled carbon nanotube-sulfur composites
[0097] Multi-walled carbon nanotubes (MWCNT) (diameter = 9.5 nm, Nanocyl (Belgium)) and sulfur powder (Sulfur) are added to ethanol at a ratio of MWCNT:S = 3:7, ball milled (450 rpm, 30 min, 10 cycles), and MWCNT and sulfur powder are filtered by vacuum filtration. The remaining solvent is then dried in a vacuum oven at 60°C for 24 hours.
[0098] Afterwards, the dried MWCNT and sulfur powder were ground and placed in a sealed flask, followed by heat treatment at 155°C for 2 hours to produce a multi-walled carbon nanotube-sulfur composite (MWCNT-S complex).
[0099]
[0100] Manufacturing of anodes
[0101] The multi-walled carbon nanotube-sulfur composite (MWCNT-S complex) and single-walled carbon nanotube (SWCNT) (Meijo SWCNT), and pretreated carbon nanotube dispersion (CNT solution) produced above were added to H2O at a weight ratio of MWCNT-S complex: Meijo SWCNT: CNT solution = 75:22:3 and dispersed using a ball mill for 10 minutes to manufacture a cathode composite.
[0102] Afterwards, the remaining H2O was removed through vacuum filtration, and the obtained electrode was dried in a vacuum oven at 60°C for 24 h to manufacture a multi-walled carbon nanotube-sulfur composite and a single-walled carbon nanotube electrode.
[0103]
[0104] Fabrication of phosphorus-doped separator membranes
[0105] Phosphorus (P) was deposited on a mixture of activated carbon (trade name: YP-80F) and Super Phosphate Black (SPB) powder. Sodium phosphate hydrate processed into pellet form was used as the P source in the first chamber, and the deposition process was performed for 2 hours at 300°C in the first chamber and 600°C in the second chamber. The ratio of activated carbon, SPB, and P source was 4:1:1 to 8:2:1 by weight, and Ar was used as the carrier gas.
[0106] Next, the P-deposited activated carbon powder was dispersed in NMP to prepare a dispersion solution. Meanwhile, PVDF was dissolved as a binder in NMP solvent to prepare a binder solution. The prepared dispersion solution and binder solution were mixed and then applied to one side of a PE membrane to produce a separator. At this time, the weight ratio of activated carbon (YP): Super P Black (SPB): PVDF among the prepared P-deposited carbon powders was maintained in the range of 8:1:1 to 7:2:1.
[0107]
[0108] Manufacturing of lithium-sulfur batteries
[0109] A battery was configured with the following cell configuration.
[0110] - Anode: Sulfur@MWCNT : SWCNT : CNT(solution) = 75 : 22 : 3
[0111] - Cathode: Li-metal 100μm
[0112] - Electrolyte: 1M LiTFSI in DOL / DME (1 / 1=v / v) + 1wt.% LiNO3
[0113] - Cut-off: 1.8V - 2.8V
[0114] - C-rate: 0.1C
[0115] - Working temperature: 25℃
[0116] In the case of the separator, a battery was manufactured by applying a generally used PE separator or a P-doped separator (YP@SPB@P coated separator) according to the present invention.
[0117]
[0118] Results and Evaluation
[0119] Charge and discharge characteristics
[0120] Figures 3 and 4 are charge-discharge graphs of a lithium-sulfur battery according to one embodiment of the present invention.
[0121] Figure 3 shows a case in which a positive electrode according to the present invention is applied with a PE separator, and Figure 4 shows a case in which a phosphorus-doped separator is applied together with the positive electrode according to the present invention. These are the results of a battery performance test conducted at a rate of 0.1C with a cut-off voltage set to 1.8 to 2.8 V at 25°C.
[0122] The data of Fig. 3 are shown in Table 2 below, and the data of Fig. 4 are shown in Table 3 below.
[0123] PristineLow Ox-SWCNTHigh Ox-SWCNTDischargecapacity[mAh / g]Chargecapacity[mAh / g]Dischargecapacity[mAh / g]Chargecapacity[mAh / g]Dischargecapacity[mAh / g]Chargecapacity[mAh / g]1st936.6264997.38571077.4821130.379973.0673957.08642nd 797.6662874.7786957.7647993.9576856.5657861.60143rd780.9881835.793927.1381954.9865831.046839.39334t h769.8681819.0844913.2214935.4885811.0706820.52275th761.538813.5072907.6361929.9085797.7624807.2002
[0124] PristineLow Ox-SWCNTHigh Ox-SWCNTDischargecapacity[mAh / g]Chargecapacity[mAh / g]Dischargecapacity[mAh / g]Chargecapacity[mAh / g]Dischargecapacity[mAh / g]Chargecapacity[mAh / g]1st1164.4711217.4351063.1521066.7061040.1071060.9182nd 1046.1631136.282929.0591991.8906934.2339989.1553rd990.1281064.482891.6653935.7162909.3175948.5924th 983.88311039.509888.5333923.1944909.3127942.33785th980.77351030.144885.4208916.9835906.1977936.1305
[0125] Referring to FIG. 3 and Table 2, it can be confirmed that the electrodes (Low Ox-SWCNT, High Ox-SWCNT) manufactured according to the examples show superior initial capacities at similar loading values than the case where the carbon nanotube solution without pretreatment (Pristine) is included, as they contain a carbon nanotube solution in which oxygen-containing functional groups are introduced through pretreatment. In addition, referring to FIG. 4 and Table 3, it can be confirmed that the use of a phosphorus-doped separator shows superior initial capacities than the use of a general separator (PE).
[0126]
[0127] Capacity and Coulombic efficiency over cycles
[0128] Figures 5 and 6 are graphs showing changes in capacity and coulombic efficiency according to the number of charge / discharge cycles of a lithium-sulfur battery according to an embodiment of the present invention. Figure 5 shows a battery using a positive electrode according to the present invention with a PE separator, and Figure 6 shows a battery using a phosphorus-doped separator together with the positive electrode according to the present invention. A battery performance test was conducted at a rate of 0.1C with a cut-off voltage set to 1.8 to 2.8 V at 25°C.
[0129] The data of Fig. 5 are shown in Table 4 below, and the data of Fig. 6 are shown in Table 5 below.
[0130] PristineLow Ox-SWCNTHigh Ox-SWCNT1st Capacity[mAh / g]936.62641077.482973.067350th Capacity[mAh / g]503.0537927.1089792.2011100th Capacity[mAh / g]22.23492520.6185670.1222100th Afterlife Maintenance Rate[%]2.3748.3268.87
[0131] PristineLow Ox-SWCNTHigh Ox-SWCNT1st Capacity[mAh / g]1164.4711063.1521040.10750th Capacity[mAh / g]881.183832.4371825.2322100th Capacity[mAh / g]93.41331782.5204784.7337100th Afterlife Maintenance Rate[%]8.0273.6075.45
[0132] Referring to Fig. 5 and Table 4, in the case of the electrodes (Low Ox-SWCNT, High Ox-SWCNT) manufactured according to the examples, since they contain a carbon nanotube solution in which oxygen-containing functional groups are introduced through pretreatment, they show a high capacity retention rate based on 50 cycles and excellent changes in Coulombic efficiency can be confirmed. On the other hand, when a carbon nanotube solution that has not been pretreated is included (Pristine), it shows a low lifespan retention rate and charge / discharge efficiency, which seems to be due to the shuttle effect caused by polysulfide elution. Referring to Fig. 6 and Table 5, in the case of using a phosphorus-doped separator, it was confirmed that the capacity retention rate and Coulombic efficiency changes were better than those of using a general separator (PE).
[0133] In addition, Figures 7 and 8 are capacity graphs according to the number of charge / discharge cycles of a lithium-sulfur battery according to an embodiment of the present invention. Figure 7 shows a battery using a positive electrode according to the present invention with a PE separator, and Figure 8 shows a battery using a phosphorus-doped separator together with the positive electrode according to the present invention. At 25°C, the cut-off voltage was set to 1.8 to 2.8 V, and a battery performance test was conducted at a rate of 0.1C to 2C.
[0134] PristineLow Ox-SWCNTHigh Ox-SWCNT0.1C1st Capacity[mAh / g]953.78171011.266988.31440.5C6th Capacity[mAh / g]409.5278563.0275649.48581C11th Capacity[mAh / g]132.7083167.957402C16th Capacity[mAh / g]46.64877000.1C21th Capacity[mAh / g]736.7942800.2232832.5963
[0135] PristineLow Ox-SWCNTHigh Ox-SWCNT0.1C1st Capacity[mAh / g]975.5294911.2226955.12390.5C6th Capacity[mAh / g]652.5303443.8786654.2611C11th Capacity[mAh / g]111.1809194.4443194.99382C16th Capacity[mAh / g]0000.1C21th Capacity[mAh / g]867.1168763.982813.1914
[0136] Referring to Fig. 7 and Table 6, it can be seen that in the case of an electrode (Low Ox-SWCNT, High Ox-SWCNT) including a carbon nanotube solution into which oxygen-containing functional groups are introduced through pretreatment according to an embodiment, a high capacity retention rate is maintained even after 50 cycles, and the discharge capacity is recovered again when reduced from 2C to a low output of 0.1C. Similarly, in Fig. 8, it can be seen that in the case of an electrode (Low Ox-SWCNT, High Ox-SWCNT) including a carbon nanotube solution into which oxygen-containing functional groups are introduced through pretreatment, a high capacity is maintained even after 50 cycles.
[0137]
[0138] Thus, it can be confirmed that the composite cathode material for a lithium-sulfur battery manufactured according to the present invention contains a multi-walled carbon nanotube-sulfur composite (MWCNT-S complex), a single-walled carbon nanotube (SWCNT), and a pretreated carbon nanotube dispersion (CNT solution), thereby suppressing the dissolution of lithium polysulfide and maintaining the cathode material even after repeated cycles, thereby increasing the charge-discharge efficiency. The lithium-sulfur battery manufactured including the above cathode active material has a technical feature in that it can increase the charge-discharge efficiency by suppressing the dissolution of lithium polysulfide from the cathode and maintaining the cathode material even after repeated cycles, and can improve the performance and lifespan stability of a lithium-sulfur battery by combining with a phosphorus-doped separator to enhance the effect of suppressing the penetration and diffusion of lithium polysulfide into the cathode.
[0139]
[0140] The above description is merely an illustrative description of the technical idea of the present invention, and those skilled in the art will appreciate that various modifications and variations can be made without departing from the essential characteristics of the present invention. Therefore, the embodiments disclosed in the present invention are not intended to limit the technical idea of the present invention, but rather to illustrate it, and the scope of the technical idea of the present invention is not limited by these embodiments. The scope of protection of the present invention should be interpreted by the claims, and all technical ideas within a scope equivalent thereto should be interpreted as being included in the scope of the rights of the present invention.
Claims
1. A method for manufacturing a cathode material for a lithium sulfur battery capable of suppressing the dissolution of lithium polysulfide, (1) A step of manufacturing a multi-walled carbon nanotube-sulfur composite (MWCNT-S complex) by ball milling, mixing, and heat-treating multi-walled carbon nanotubes (MWCNT) and sulfur precursors; (2) A step of manufacturing a carbon nanotube dispersion (CNT solution) in which carbon nanotubes having oxygen-containing functional groups are highly dispersed; (3) Step of preparing single-walled carbon nanotubes (SWCNT); and (4) A step of manufacturing a composite cathode material by mixing and dispersing the multi-walled carbon nanotube-sulfur composite, the carbon nanotube dispersion, and the single-walled carbon nanotube (SWCNT); including, The above composite cathode material is a carbon nanotube having an oxygen-containing functional group, and forms a network structure with the multi-walled carbon nanotube-sulfur composite or the single-walled carbon nanotube, The oxygen-containing functional group is characterized in that it binds to lithium polysulfide and suppresses the dissolution of lithium polysulfide by the network structure. Method for manufacturing composite cathode materials for lithium sulfur batteries.
2. In paragraph 1, The step of manufacturing the above (2) carbon nanotube dispersion (CNT solution) is: (2-1) A step of producing a debundled carbon nanotube by mixing a composite powder containing at least one of sulfate and phosphate in a bundle-shaped carbon nanotube, an acid solution, and an alkali metal-containing oxidizing agent while applying shear stress, so that at least one of the sulfate and phosphate is co-intercalated between adjacent layers of the carbon nanotube; (2-2) A step of heating the debundled carbon nanotube at 30 to 50°C to produce a carbon nanotube into which an oxygen-containing functional group is introduced by at least one of the sulfate and phosphate and the acid solution; (2-3) A step of manufacturing a pretreated carbon nanotube by washing and filtering the carbon nanotube into which the oxygen-containing functional group has been introduced; and (2-4) A step of preparing a carbon nanotube dispersion by dispersing the above-mentioned pretreated carbon nanotubes in a solvent, The above carbon nanotube dispersion is characterized in that the content of oxygen-containing functional groups introduced into the carbon nanotubes is 0.5 to 20 wt.%. Method for manufacturing composite cathode materials for lithium sulfur batteries.
3. In paragraph 1, A method for manufacturing a composite cathode material for a lithium sulfur battery, characterized in that the multi-walled carbon nanotube-sulfur composite, single-walled carbon nanotube, and carbon nanotube dispersion are mixed in a weight ratio of 70 to 80: 20 to 30: 1 to 10.
4. In paragraph 1, A method for manufacturing a composite cathode material for a lithium sulfur battery, characterized in that the oxygen-containing functional group is a carboxyl group or a hydroxyl group.
5. In a lithium sulfur battery including a positive electrode, a negative electrode, a separator, and an electrolyte, A lithium sulfur battery, characterized in that the positive electrode comprises a composite positive electrode material manufactured according to any one of claims 1 to 4.
6. In paragraph 5, The above separator is coated with phosphorus-deposited carbon powder on one or both sides, A lithium sulfur battery, characterized in that the carbon powder is at least one material selected from the group consisting of activated carbon, carbon black, graphene, and CNT.
Citation Information
Patent Citations
Sulfur-carbon complex, preaparation method thereof, and lithium-sulfur battery comprising the same
KR1020180017796A
Electron transport material for solar cell comprising nickel-graphite core-shell nanoparticles, bulk heterojunction solar cell comprising same, and method for manufacturing same
KR1020210049406A
Support device, test system, and method of controlling support device
KR1020230053513A
KR20210057489A
Cited By
Battery positive electrode material, battery and preparation method thereof
CN119920839A
A battery cathode material, a battery and a preparation method thereof
CN119920839B
Composite positive electrode conductive paste and preparation method thereof
CN120914257A
Composite positive electrode for solid-state lithium-sulfur battery and preparation method of composite positive electrode
CN120955081A
Modified carbon nanotube material as well as preparation method and application thereof
CN121192171A