Isolation film and secondary battery and electric apparatus related thereto
By using a porous base film and a coating containing particles such as molybdenum disulfide in the isolation membrane of a secondary battery, the risk of metal dendrite puncture is reduced, the reliability and energy density of the battery are improved, and the isolation membrane's Heat resistance.
Patent Information
- Application Number
- PCT/CN2023/087329
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-10
- Publication Date
- 2024-10-17
AI Technical Summary
During the charging and discharging process of existing secondary batteries, metal dendrites easily penetrate the isolation film, causing the positive and negative electrodes to be short-circuited, reducing the reliability of the battery.
An isolation membrane composed of a first porous base film, a second porous base film and a coating is used. The coating contains particles such as molybdenum disulfide, silicon oxide or transition metal oxide, which reduces dendrite puncture through redox reactions. risk and improve the heat resistance of the isolation film.
It effectively isolates the positive electrode piece and the negative electrode piece, reduces the risk of dendrite puncture, improves the reliability and energy density of secondary batteries, and improves the heat resistance of the isolation film.
Smart Images

Figure CN2023087329_17102024_PF_FP_ABST
Abstract
Description
Separator and related secondary battery and electrical device Technical Field
[0001] The present application relates to the field of batteries, and in particular to an isolation membrane and related secondary batteries and electrical devices. Background Art
[0002] Secondary batteries have the characteristics of high capacity and long life, and are therefore widely used in electronic devices such as mobile phones, laptops, electric vehicles, electric airplanes, electric boats, electric toy cars, electric toy boats, electric toy airplanes, and power tools, etc.
[0003] As battery applications become increasingly widespread, the requirements for secondary battery performance, especially safety, are becoming increasingly stringent. Further improving the reliability of batteries during use remains a topic that professionals in this field need to continuously explore.
[0004] Summary of the Invention
[0005] The present application is made in view of the above-mentioned problems, and its purpose is to provide a separator and its related secondary battery and electric device.
[0006] The first aspect of the present application provides an isolation membrane, which includes a first porous base membrane, a second porous base membrane and a coating; the coating is arranged between the first porous base membrane and the second porous base membrane, and the coating includes first particles, and the first particles include at least one of molybdenum disulfide, silicon oxide, transition metal oxide or conductive carbon particles.
[0007] Therefore, the isolation membrane of the embodiment of the present application sets the coating between the first porous base membrane and the second porous base membrane. When the secondary battery is charged and discharged normally, the isolation membrane can effectively isolate the positive electrode plate and the negative electrode plate; when the growth of metal dendrites in the secondary battery increases, the coating in the isolation membrane can undergo redox reaction with the metal dendrites, reducing the risk of dendrites piercing the isolation membrane and causing direct contact between the positive electrode plate and the negative electrode plate, thereby effectively improving the reliability of the secondary battery.
[0008] In some embodiments, the first particles include at least one of molybdenum disulfide or a transition metal oxide.
[0009] In some embodiments, the silicon oxide includes at least one of silicon monoxide or silicon dioxide.
[0010] In some embodiments, the transition metal oxide includes one or more of manganese dioxide, cobalt oxide, iron oxide, or nickel oxide.
[0011] In some embodiments, the conductive carbon particles include one or more of conductive carbon black, carbon nanotubes, graphite, or graphene.
[0012] In some embodiments, the first particles comprise greater than or equal to 20%, and optionally comprise between 30% and 60%, based on the total weight of the coating. When the first particles comprise within this range, the first particles can fully react with the alkali metal and / or alkaline earth metal, thereby reducing the risk of metal dendrites piercing the separator, thereby further improving the reliability of the secondary battery.
[0013] In some embodiments, the average particle size of the first particles is less than or equal to 3 μm; optionally, it is 0.01 μm to 1 μm.
[0014] When the average particle size of the first particles is within the above range, the first particles will not be too large and are easy to distribute evenly, and the contact area between the first particles and the alkali metal and / or alkaline earth metal is relatively large, which is beneficial to promoting the redox reaction; and because the particle size of the first particles is small, it is beneficial to the thin coating of the coating, reducing the overall thickness of the isolation membrane, thereby increasing the space occupied by the positive electrode and / or negative electrode, and improving the energy density of the secondary battery.
[0015] In some embodiments, the coating further comprises second particles, which do not undergo oxidation and reduction reactions within the operating voltage range of the secondary battery. The second particles have good heat resistance and can improve the heat resistance of the entire separator.
[0016] In some embodiments, the second particles include at least one of inorganic particles or organic particles.
[0017] In some embodiments, the inorganic particles include one or more of boehmite γ-AlOOH, aluminum oxide Al2O3, aluminum hydroxide Al(OH)3, barium sulfate BaSO4, magnesium oxide MgO, magnesium hydroxide Mg(OH)2, calcium oxide CaO, cerium oxide CeO2, zirconium titanate SrTiO3, barium titanate BaTiO3, and magnesium fluoride MgF2.
[0018] In some embodiments, the organic particles include at least one of polystyrene, polyethylene, polyimide, melamine resin, phenolic resin, polypropylene, polyester (e.g., polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate), polyphenylene sulfide, polyaramid, polyamideimide, polyimide, copolymer of butyl acrylate and ethyl methacrylate, and mixtures thereof.
[0019] In some embodiments, based on the total weight of the coating, the ratio of the second particles to the first particles is less than or equal to 1, and can be selected from 0.35 to 0.85. A ratio of the second particles to the first particles within this range can both improve the heat resistance of the isolation membrane and reduce the risk of the isolation membrane being pierced by metal dendrites.
[0020] In some embodiments, the coating includes at least two sub-coatings, and the first and second particles are disposed in different sub-coatings. Placing the first and second particles in different layers reduces the likelihood of the second particles interfering with the first particles, thereby facilitating the first particles' ability to mitigate further dendrite growth.
[0021] In some embodiments, the coating includes a binder; optionally, the binder includes one or more of polyacrylate, acrylic acid, carboxymethyl cellulose, polyvinylidene fluoride-co-trichloroethylene copolymer, polymethyl methacrylate, polyvinyl pyrrolidone, polyvinyl acetate, polyethylene-co-vinyl acetate copolymer, polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, polyvinylidene fluoride, polyacrylonitrile, polyvinyl alcohol, starch, hydroxypropyl cellulose, regenerated cellulose, tetrafluoroethylene, polyethylene, polypropylene, and cyanoethyl pullulan.
[0022] In some embodiments, the first porous base membrane and the second porous base membrane have different melting points.
[0023] In some embodiments, the melting point of the first porous base membrane is denoted as T m1 The melting point of the second porous base film is recorded as T m2 , then the isolation film satisfies: 1.05≤T m1 / T m2 ≤2.50.
[0024] In some embodiments, 160°C ≤ T m1 ≤350℃; optionally, 180℃≤T m1 ≤320℃.
[0025] In some embodiments, 120°C ≤ T m2 ≤160℃; optionally, 135℃≤T m2 ≤150℃.
[0026] In some embodiments, the coating includes a first sub-coating and a second sub-coating, the first sub-coating includes the first particles, the second sub-coating includes the second particles, and the first sub-coating is disposed between the first porous base membrane and the second sub-coating, or the first sub-coating is disposed between the second porous base membrane and the second sub-coating.
[0027] In some embodiments, the thickness of the first porous base membrane is W1, and the unit is μm; the thickness of the second porous base membrane is W2, and the unit is μm, W1 / W2≥1.02; optionally, 1.2≤W1 / W2≤5.0.
[0028] In some embodiments, 1≤W1≤12; optionally, 3≤W1≤6.
[0029] In some embodiments, 2≤W2≤12; optionally, 3≤W2≤5.
[0030] In some embodiments, the isolation film satisfies at least one of conditions (1) to (6):
[0031] (1) The longitudinal thermal shrinkage of the isolation film at 250°C for 1 hour is less than or equal to 1.0%;
[0032] (2) The transverse heat shrinkage of the isolation film at 250°C for 1 hour is less than or equal to 1.0%;
[0033] (3) The air permeability of the isolation membrane is less than or equal to 500s / 100cc; it can be selected from 150s / 100cc to 400s / 100cc;
[0034] (4) The longitudinal tensile strength of the separator is greater than or equal to 600 kg / cm 2 ; Optional 800kg / cm 2 -2000kg / cm 2 ;
[0035] (5) The transverse tensile strength of the separator is greater than or equal to 1000 kg / cm 2 ; Optional 1200kg / cm 2 -2500kg / cm 2 ;
[0036] (6) The ion conductivity of the isolation membrane is 0.5mS / cm-2.0mS / cm; optionally 0.8mS / cm-1.5mS / cm.
[0037] The second aspect of the present application provides a secondary battery, comprising an isolation membrane according to any embodiment of the first aspect of the present application or an isolation membrane prepared by the preparation method according to any embodiment of the second aspect of the present application.
[0038] In some embodiments, the secondary battery includes a positive electrode sheet and a negative electrode sheet, the separator is disposed between the positive electrode sheet and the negative electrode sheet; and the second porous base film of the separator faces the negative electrode sheet.
[0039] A third aspect of the present application provides an electrical device comprising the secondary battery according to the second aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following is a brief introduction to the drawings required for use in the embodiments of the present application. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the drawings without creative work.
[0041] FIG1 is a schematic diagram of an embodiment of a secondary battery of the present application.
[0042] FIG. 2 is an exploded schematic diagram of an embodiment of the secondary battery of FIG. 1 .
[0043] FIG3 is a schematic diagram of an embodiment of a battery module of the present application.
[0044] FIG4 is a schematic diagram of an embodiment of a battery pack of the present application.
[0045] FIG. 5 is an exploded schematic diagram of the embodiment of the battery pack shown in FIG. 4 .
[0046] FIG6 is a schematic diagram of an embodiment of an electric device including the secondary battery of the present application as a power source.
[0047] The drawings are not necessarily drawn to scale.
[0048] The reference numerals are as follows: 1. battery pack; 2. upper case; 3. lower case; 4. battery module; 5. secondary battery; 51. housing; 52. electrode assembly; 53. cover plate; 6. electrical device. DETAILED DESCRIPTION
[0049] The following detailed description specifically discloses embodiments of the separator of the present application, and its related secondary batteries and electrical devices. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repeated descriptions of substantially identical structures may be omitted. This is to avoid unnecessary length in the following description and to facilitate understanding by those skilled in the art. In addition, the drawings and the following description are provided to enable those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0050] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0051] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution. Unless otherwise specified, all technical features and optional technical features of the present application can be combined with each other to form a new technical solution.
[0052] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, a method includes steps (a) and (b), which indicates that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, a method may further include step (c), which indicates that step (c) may be added to the method in any order, for example, the method may include steps (a), (b), and (c), or may include steps (a), (c), and (b), or may include steps (c), (a), and (b), etc.
[0053] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may indicate that other components not listed may also be included or that only the listed components are included.
[0054] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0055] In this application, the terms "first", "second", etc. are used for descriptive purposes only and should not be understood as indicating or implying relative importance.
[0056] In this application, the terms "plurality" and "multiple" refer to two or more.
[0057] Unless otherwise specified, the terms used in this application have the common meanings that are commonly understood by those skilled in the art.
[0058] Unless otherwise stated, the numerical values of the parameters mentioned in this application can be measured using various test methods commonly used in the art, for example, they can be measured according to the test methods given in the examples of this application.
[0059] A secondary battery consists of a positive electrode, a negative electrode, a separator, and an electrolyte. The separator is placed between the positive and negative electrodes to prevent short circuits between them while allowing active ions to pass freely through the electrolyte.
[0060] With the application and promotion of secondary batteries, people have higher and higher requirements for the performance (such as safety) of secondary batteries. The separator is an important component of secondary batteries. The reliability of secondary batteries can be improved by improving the performance of the separator.
[0061] During the charging process of a secondary battery, metal ions migrate from the positive electrode to the negative electrode, gaining electrons on the surface of the negative electrode before being embedded or deposited. As the number of charges increases, incomplete metal embedding or deposition leads to the formation of dendrites. These dendrites can pierce the separator, short-circuiting the positive and negative electrodes and causing reliability issues for the secondary battery. To improve the reliability of secondary batteries, related technologies coat active materials on the surface of polymer separators. However, because these active materials are exposed at the negative electrode interface, they undergo a redox reaction with the negative electrode and are consumed before acting on the dendrites, preventing them from interacting with the dendrites. This results in no improvement in the reliability of the secondary battery.
[0062] In view of the above problems, the isolation membrane of the embodiment of the present application includes a first porous base membrane and a second porous base membrane. The first porous base membrane and the second porous base membrane can give the isolation membrane excellent mechanical properties; a coating is provided between the first porous base membrane and the second porous base membrane. During the normal charge and discharge process of the secondary battery, the isolation membrane can effectively isolate the positive electrode plate and the negative electrode plate, playing an insulating role; and the coating is not easy to contact with the electrolyte, the negative electrode plate, etc. to produce side reactions. As the number of dendrites deposited on the negative electrode plate increases, the dendrites may pierce one of the base membranes outside the coating, such as the second porous base membrane, and directly contact the coating. The first particles in the coating can undergo redox reactions with active ions such as lithium ions near the dendrite tip, thereby reducing the risk of dendrites further piercing another base membrane, such as the first porous base membrane, resulting in a short circuit between the positive electrode plate and the negative electrode plate, thereby improving the reliability of the secondary battery. The technical solution of the embodiment of the present application is described in detail below.
[0063] Isolation film
[0064] In a first aspect, the present application provides a separator, which is applied to a secondary battery.
[0065] The isolation membrane includes a first porous base membrane, a second porous base membrane and a coating, wherein the coating is arranged between the first porous base membrane and the second porous base membrane, and the coating includes first particles, which include at least one of molybdenum disulfide, silicon oxide, transition metal oxide or conductive carbon particles.
[0066] The isolation membrane includes a first porous base membrane and a second porous base membrane. The first porous base membrane and the second porous base membrane can give the isolation membrane excellent mechanical properties, can effectively isolate the positive electrode and the negative electrode of the secondary battery, and reduce the risk of short circuit between the positive electrode and the negative electrode.
[0067] A coating is provided between the first porous base membrane and the second porous base membrane. Due to the protection of the first porous base membrane and the second porous base membrane, the coating is basically not in direct contact with the negative electrode active material, thereby reducing the risk of the coating failing due to premature redox reaction and being consumed. During the normal charge and discharge process of the secondary battery, metal ions (such as alkali metal ions and / or alkaline earth metal ions) migrate to the surface of the negative electrode active material of the secondary battery to obtain electrons for embedding or deposition. As the number of cycles increases, metal dendrites are gradually formed. Since the base membrane has a certain mechanical strength, when the amount of metal dendrite deposition is small, the base membrane can alleviate the risk of metal dendrites piercing the base membrane to a certain extent. As the amount of metal dendrite deposition increases, the metal dendrites may pierce the base membrane (such as the second porous base membrane) and contact the first particles in the coating. The first particles undergo redox reaction with the lithium ions near the metal dendrites, passivating the growth of the dendrite tips, thereby reducing the risk of dendrites further piercing another base membrane (such as the first porous base membrane) to cause a short circuit between the positive electrode and the negative electrode, thereby improving the reliability of the secondary battery.
[0068] The isolation membrane of the embodiment of the present application sets the coating between the first porous base membrane and the second porous base membrane. When the secondary battery is normally charged and discharged, the isolation membrane can effectively isolate the positive electrode plate and the negative electrode plate; when the growth of metal dendrites in the secondary battery increases, the coating in the isolation membrane can undergo redox reaction with the metal dendrites, reducing the risk of dendrites piercing the isolation membrane and causing direct contact between the positive electrode plate and the negative electrode plate, thereby effectively improving the reliability of the secondary battery.
[0069] In the embodiments of the present application, the first particles substantially do not generate gas during the redox reaction with the alkali metal and / or alkaline earth metal, thereby maintaining a relatively stable gas pressure within the secondary battery. Furthermore, the first particles exhibit good stability in the electrolyte and are less likely to undergo side reactions with the electrolyte. Optionally, the first particles comprise at least one of molybdenum disulfide and a transition metal oxide.
[0070] In the embodiments of this application, the operating voltage of a secondary battery refers to the voltage exhibited by the secondary battery during normal operation, also referred to as the operating voltage; this voltage can be measured using a multimeter. For example, the operating voltage of a lithium-ion battery can be 3.6V. The first particles can undergo a redox reaction with the alkali metal and / or alkaline earth metal at the operating voltage of the secondary battery.
[0071] In some embodiments, the alkali metal includes one or more of lithium metal, sodium metal, potassium metal, rubidium metal, cesium metal, or francium metal.
[0072] In some embodiments, the alkaline earth metal includes one or more of magnesium metal, calcium metal, strontium metal, or barium metal.
[0073] The alkali metal and / or alkaline earth metal as a metal element has strong reducing properties and can undergo redox reaction with the first particles in the coating.
[0074] Alkali metal ions and / or alkaline earth metal ions can act as metal ions of secondary batteries, migrating between the positive electrode and the negative electrode, thereby realizing the charging and discharging of the secondary battery; and alkali metals and / or alkaline earth metals, as metal elements, have certain reducing properties, and can undergo redox reactions with the first particles in the coating, passivate dendrites, and reduce the risk of metal dendrites piercing the isolation membrane, thereby further improving the reliability of the secondary battery.
[0075] The first particles are conductive or highly reactive substances that can undergo redox reactions with alkali metals and / or alkaline earth metals. The first particles are disposed between the two layers of base films, which can effectively reduce the risk of the first particles reacting prematurely with the negative electrode active material, resulting in the first particles being consumed and failing.
[0076] Illustratively, the conductive carbon particles include one or more of conductive carbon black, carbon nanotubes, graphite or graphene.
[0077] Exemplarily, the transition metal oxide includes one or more of manganese dioxide MnO2, cobalt oxide, iron oxide, or nickel oxide. Specifically, the cobalt oxide includes cobalt trioxide Co3O4 and / or cobalt oxide CoO. The iron oxide includes one or more of ferric oxide Fe2O3, iron oxide FeO, or ferric oxide Fe3O4. The nickel oxide includes nickel oxide NiO and / or nickel trioxide Ni2O3.
[0078] Exemplarily, the silicon oxide includes silicon dioxide SiO2 and / or silicon monoxide.
[0079] In some embodiments, the average particle size of the first particles is less than or equal to 3.0 μm; optionally 0.001 μm to 3.0 μm; optionally 0.01 μm to 1 μm. When the volume average particle size of the first particles is within the above range, the first particles will not be too large and are easy to distribute evenly, and the contact area between the first particles and the alkali metal and / or alkaline earth metal is relatively large, which is conducive to promoting the redox reaction; and because the particle size of the first particles is small, it is conducive to the light coating of the coating, reducing the overall thickness of the separator, thereby increasing the space occupied by the positive electrode and / or negative electrode sheet, and improving the energy density of the secondary battery. For example, the average particle size of the first particles can be 0.001 μm, 0.01 μm, 0.1 μm, 0.2 μm, 0.5 μm, 1 μm, 1.2 μm, 1.5 μm, 1.8 μm, 2.0 μm, 2.5 μm, 3.0 μm, or a range consisting of any two of the above values.
[0080] In this application, the average particle size of a material can be determined by measuring Dv50, which represents the particle size at which the cumulative volume distribution percentage of the material reaches 50%. This can be determined using instruments and methods known in the art. For example, the particle size distribution can be measured using a laser particle size analyzer (e.g., Master Size 3000) in accordance with GB / T 19077-2016, Laser Diffraction Method.
[0081] In some embodiments, based on the total weight of the coating, the content of the first particles in the coating is greater than or equal to 20%, optionally 30% to 60%. When the content of the first particles is within the above range, the first particles can fully react with the alkali metal and / or alkaline earth metal, thereby reducing the risk of metal dendrites piercing the isolation membrane, thereby further improving the reliability of the secondary battery. Exemplarily, the content of the first particles can be 20%, 25%, 30%, 35%, 40%, 45%, 50%, 60%, 70%, 80%, 90%, 95% or a range consisting of any two of the above values.
[0082] To improve the heat resistance of the separator, in some embodiments, the coating further includes second particles. These second particles exhibit superior heat resistance, improving the overall heat resistance of the separator. Within the operating voltage range of the secondary battery, the second particles substantially avoid oxidation and reduction reactions with metal dendrites. In other words, the second particles are configured to avoid oxidation and reduction reactions with alkali metals and / or alkaline earth metals at the nominal voltage of the secondary battery.
[0083] Illustratively, the second particles include at least one of inorganic particles or organic particles.
[0084] In some embodiments, the inorganic particles include one or more of boehmite γ-AlOOH, aluminum oxide Al2O3, aluminum hydroxide Al(OH)3, barium sulfate BaSO4, magnesium oxide MgO, magnesium hydroxide Mg(OH)2, calcium oxide CaO, cerium oxide CeO2, zirconium titanate SrTiO3, barium titanate BaTiO3, and magnesium fluoride MgF2.
[0085] In some embodiments, the organic particles include at least one of polystyrene, polyethylene, polyimide, melamine resin, phenolic resin, polypropylene, polyester (e.g., polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate), polyphenylene sulfide, polyaramid, polyamideimide, polyimide, copolymer of butyl acrylate and ethyl methacrylate, and mixtures thereof.
[0086] In some embodiments, the volume average particle size Dv50 of the second particles is less than or equal to 3 μm; it can be optionally 0.01 μm to 1 μm. When the volume average particle size of the second particles is within the above range, the second particles will not be too large and are easy to distribute evenly. Moreover, since the particle size of the second particles is small, it is conducive to the light and thin coating of the coating, reducing the overall thickness of the separator, thereby increasing the space occupied by the positive electrode and / or negative electrode, and improving the energy density of the secondary battery. For example, the volume average particle size Dv50 of the second particles can be 0.01 μm, 0.05 μm, 0.1 μm, 0.2 μm, 0.5 μm, 1 μm, 1.2 μm, 1.5 μm, 1.8 μm, 2.0 μm, 2.5 μm, 3.0 μm, or a range consisting of any two of the above values.
[0087] In some embodiments, based on the total weight of the coating, the ratio of the content of the second particles to the content of the first particles is less than or equal to 1, and can be optionally 0.35 to 0.85. The ratio of the content of the second particles to the content of the first particles is within the above range, which can take into account both improving the heat resistance of the isolation membrane and reducing the risk of the isolation membrane being pierced by metal dendrites. Exemplarily, the content ratio of the second particles to the first particles can be 0.35, 0.40, 0.45, 0.50, 0.55, 0.60, 0.65, 0.70, 0.75, 0.80, 0.85, 0.90, 1 or a range consisting of any two of the above values.
[0088] Illustratively, the content of the second particles in the coating is greater than 0%, and may be 30% to 60%. Of course, the content of the second particles in the coating may also be 0, i.e., no second particles are added to the coating. Illustratively, the content of the second particles may be 1%, 5%, 8%, 10%, 12%, 15%, 18%, 20%, 23%, 25%, 28%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, or a range consisting of any two of the foregoing values.
[0089] In some embodiments, the coating includes a binder; optionally, the binder includes one or more of polyacrylate, acrylic acid, carboxymethyl cellulose, polyvinylidene fluoride-co-trichloroethylene copolymer, polymethyl methacrylate, polyvinyl pyrrolidone, polyvinyl acetate, polyethylene-co-vinyl acetate copolymer, polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, polyvinylidene fluoride, polyacrylonitrile, polyvinyl alcohol, starch, hydroxypropyl cellulose, regenerated cellulose, tetrafluoroethylene, polyethylene, polypropylene, and cyanoethyl pullulan.
[0090] The coating in the embodiments of the present application can be a single-layer structure or a multi-layer structure. In some embodiments, the coating includes at least two sub-coatings, and the first particles and the second particles are disposed in different sub-coatings. Disposing the first particles and the second particles in different layers reduces the possibility of the second particles interfering with the first particles, which helps the first particles to mitigate the continued growth of dendrites.
[0091] As some examples, the at least two sub-coating layers include a first sub-coating layer and a second sub-coating layer, wherein the first particles are disposed in the first sub-coating layer and the second particles are disposed in the second sub-coating layer. The first sub-coating layer may be disposed between the first porous base membrane and the second sub-coating layer, or the first sub-coating layer may be disposed between the second porous base membrane and the second sub-coating layer.
[0092] The first particles in the first sub-coating layer mitigate dendrite growth, while the second sub-coating layer exhibits excellent heat resistance. Compared to the second sub-coating layer, the first sub-coating layer can be positioned closer to the negative electrode plate, further facilitating the first sub-coating layer's ability to mitigate dendrite growth and thus improving the battery's reliability. Furthermore, the first sub-coating layer can also be positioned closer to the positive electrode plate than the second sub-coating layer.
[0093] In other embodiments, the coating includes at least two sub-coatings, each of which includes first particles and second particles. This arrangement can enhance the heat resistance of each sub-coating and alleviate the continued growth of dendrites.
[0094] In some embodiments, the thickness of the coating may be greater than or equal to 0.3 μm, and may be 0.5 μm to 5 μm. This helps to improve the energy density of the secondary battery. For example, the thickness of the coating may be 0.3 μm, 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 5 μm, or a range consisting of any two of the above values.
[0095] In some embodiments, the first porous base membrane and the second porous base membrane have different melting points. The first porous base membrane and the second porous base membrane have different melting points, i.e., different melting points, and different mechanical properties. The relative position of the base membrane and the negative electrode plate can be set according to production requirements.
[0096] Optionally, the melting point of the first porous base membrane is denoted as T m1 , whose unit is ℃, the melting point of the second porous base membrane is recorded as T m2 , the unit is ℃, then the isolation film satisfies: 1.05≤T m1 / T m2 ≤2.50. For example, T m1 / T m2It can be 1.05, 1.20, 1.50, 1.80, 2.00, 2.20, 2.30, 2.50 or a range consisting of any two of the above values.
[0097] For example, 160°C≤T m1 ≤350℃; optionally, 180℃≤T m1 ≤320° C. Specifically, the melting point of the first porous base membrane may be 160° C., 170° C., 180° C., 200° C., 220° C., 250° C., 280° C., 300° C., 320° C., 350° C., or a range consisting of any two of the above values.
[0098] For example, 120°C≤T m2 ≤160℃; optionally, 135℃≤T m2 ≤150° C. Specifically, the melting point of the second porous base membrane may be 120° C., 130° C., 135° C., 140° C., 150° C., or a range consisting of any two of the above values.
[0099] In some embodiments, the thickness of the first porous base membrane is W1, and its unit is μm; the thickness of the second porous base membrane is W2, and its unit is μm, W1 / W2 ≥ 1.02; optionally, 1.2 ≤ W1 / W2 ≤ 5.0. The thickness of the first porous base membrane and the second porous base membrane has the above difference, and their mechanical properties are different. The mechanical strength of the first porous base membrane is greater, which is more conducive to alleviating the risk of dendrites piercing the first porous base membrane. The first porous base membrane can be preferably arranged close to the negative electrode plate, which is conducive to improving the reliability of the secondary battery. For example, W1 / W2 can be 1.02, 1.05, 1.20, 1.50, 1.80, 2.00, 2.20, 2.30, 2.50, 3.00, 3.50, 4.00, 4.50, 5.00 or a range consisting of any two of the above values.
[0100] For example, 1≤W1≤12; optionally, 3≤W1≤6. Specifically, the thickness of the first porous base membrane may be 1 μm, 2 μm, 3 μm, 5 μm, 6 μm, 8 μm, 10 μm, 11 μm, 12 μm, or a range consisting of any two of the above values.
[0101] For example, 2≤W2≤12; optionally, 3≤W2≤5. Specifically, the thickness of the second porous base membrane can be 2 μm, 2.5 μm, 3 μm, 4 μm, 5 μm, 6 μm, 8 μm, 10 μm, 11 μm, 12 μm, or a range consisting of any two of the above values.
[0102] In some embodiments, the porosity of at least one of the first porous base membrane and the second porous base membrane is greater than or equal to 25%, and can optionally be between 28% and 41%. When the porosity is within this range, the air permeability of the base membrane is guaranteed to be conducive to the migration of active ions. The moderate porosity also ensures the mechanical properties of the base membrane, providing good support for the coating.
[0103] The embodiments of the present application have no particular restrictions on the material of the base membrane. Any known base membrane with good chemical and mechanical stability can be selected. For example, the base membrane may include at least one of a porous polyolefin-based resin membrane (e.g., at least one of polyethylene, polypropylene, and polyvinylidene fluoride), a porous glass fiber, a porous non-woven fabric, and a polyimide, or a polysulfone-based resin membrane (e.g., at least one of bisphenol A-type polysulfone, polyarylsulfone, and polyethersulfone). The base membrane may be a single-layer film or a multi-layer composite film. When the base membrane is a multi-layer composite film, the materials of each layer may be the same or different.
[0104] In some embodiments, the separator may further include an adhesive layer disposed between the coating and the base film (e.g., between the coating and the first porous base film, and / or between the coating and the second porous base film), wherein the adhesive layer includes a first binder. The adhesive layer not only prevents the coating from falling off, thereby improving the adhesion between the coating and the base film and the safety performance of the secondary battery, but also improves the interface between the separator and the electrode, thereby enhancing the cycle performance of the secondary battery.
[0105] Optionally, the first binder includes at least one of an acrylate monomer homopolymer or copolymer, an acrylic acid monomer homopolymer or copolymer, and a fluorine-containing olefin monomer homopolymer or copolymer. The comonomer includes, but is not limited to, at least one of the following: an acrylate monomer, an acrylic acid monomer, an olefin monomer, a halogen-containing olefin monomer, a fluoroether monomer, and the like.
[0106] Alternatively, the first binder includes a vinylidene fluoride based polymer, such as a homopolymer of vinylidene fluoride monomer (VDF) and / or a copolymer of vinylidene fluoride monomer and a comonomer. The comonomer may be at least one of an olefin monomer, a fluorine-containing olefin monomer, a chlorine-containing olefin monomer, an acrylate monomer, an acrylic monomer, and a fluoroether monomer. Alternatively, the comonomer may include at least one of trifluoroethylene (VF3), chlorotrifluoroethylene (CTFE), 1,2-difluoroethylene, tetrafluoroethylene (TFE), hexafluoropropylene (HFP), perfluoro (alkyl vinyl) ether (such as perfluoro (methyl vinyl) ether PMVE, perfluoro (ethyl vinyl) ether PEVE, perfluoro (propyl vinyl) ether PPVE), perfluoro (1,3-dioxole) and perfluoro (2,2-dimethyl-1,3-dioxole) (PDD).
[0107] In some embodiments, the longitudinal thermal shrinkage of the isolation film at 250° C. for 1 hour is less than or equal to 1.0%.
[0108] In some embodiments, the isolation film has a transverse thermal shrinkage of less than or equal to 1.0% at 250° C. for 1 hour.
[0109] The separator according to the embodiment of the present application has a low thermal shrinkage rate in both the transverse and longitudinal directions at a high temperature of 250° C., thereby improving the safety performance of the secondary battery.
[0110] In some embodiments, the air permeability of the isolation membrane is less than or equal to 500s / 100cc; optionally, it can be 150s / 100cc-400s / 100cc.
[0111] In some embodiments, the longitudinal tensile strength of the separator is greater than or equal to 600 kg / cm 2 ; Optional 800kg / cm 2 -2000kg / cm 2 .
[0112] In some embodiments, the transverse tensile strength of the separator is greater than or equal to 1000 kg / cm 2 ; Optional 1200kg / cm 2 -2500kg / cm 2 .
[0113] The separator according to the embodiment of the present application has high tensile strength in both the transverse and longitudinal directions. Therefore, when the secondary battery expands, the separator is less likely to be damaged, thereby improving the safety performance of the secondary battery.
[0114] In some embodiments, the ion conductivity of the isolation membrane is 0.5 mS / cm-2.0 mS / cm; optionally 0.8 mS / cm-1.5 mS / cm.
[0115] The separator according to the embodiment of the present application has good air permeability, thereby improving ion conductivity and secondary battery capacity performance.
[0116] In the embodiments of the present application, the thermal shrinkage, tensile strength, and air permeability of the separator have well-known meanings in the art and can be measured using methods known in the art. For example, they can be tested in accordance with standard GB / T 36363-2018.
[0117] Preparation method
[0118] In a second aspect, the present application provides a method for preparing an isolation membrane, which can be used to prepare the isolation membrane described in any embodiment of the first aspect of the present application.
[0119] The method comprises the following steps:
[0120] providing a first porous base membrane;
[0121] providing a coating layer containing first particles on a surface of the first porous base membrane, wherein the first particles are configured to undergo an oxidation-reduction reaction with an alkali metal and / or an alkaline earth metal at a nominal voltage of the secondary battery;
[0122] A second porous base membrane is disposed on the surface of the coating layer that is away from the first porous base membrane to prepare a separator.
[0123] In some embodiments, the coating layer may be formed by applying a coating slurry on the surface of the first porous base membrane and curing the coating slurry. The coating slurry may include a solvent, and the solvent may be water, such as deionized water.
[0124] In some embodiments, the coating slurry may further include other components, for example, a dispersant, a wetting agent, a binder, etc.
[0125] In some embodiments, the coating is performed using a coating machine. The present embodiments do not specifically limit the type of coating machine; for example, a commercially available coating machine may be used. The coating machine includes a gravure roller for transferring the slurry onto the base film.
[0126] In some embodiments, the coating method may be transfer coating, spin spray coating, dip coating, etc.
[0127] Some parameters such as raw materials and their contents used in the preparation method of the isolation membrane of the present application can refer to the isolation membrane of the first aspect of the embodiment of the present application, and will not be repeated here.
[0128] Unless otherwise specified, all raw materials used in the method for preparing the separator of the present application can be obtained commercially.
[0129] secondary batteries
[0130] In a third aspect, the present application also provides a secondary battery.
[0131] Secondary batteries, also known as rechargeable batteries or storage batteries, are batteries that can be recharged after discharge to reactivate their active materials for continued use. Typically, a secondary battery comprises an electrode assembly and an electrolyte. The electrode assembly includes a positive electrode sheet, a negative electrode sheet, and a separator. The separator is positioned between the positive and negative electrodes to prevent short circuits between the positive and negative electrodes while allowing active ions to pass through.
[0132] The present application has no particular limitation on the type of secondary battery. For example, the secondary battery may be a lithium-ion battery, a sodium-ion battery, etc. In particular, the secondary battery may be a lithium-ion secondary battery.
[0133] The secondary battery described in the present application includes the separator of the first aspect of the present application or the separator prepared by the method of the second aspect of the embodiment of the present application, and the separator is arranged between the positive electrode sheet and the negative electrode sheet.
[0134] In some embodiments, the coating includes a first sub-coating and a second sub-coating, wherein the first sub-coating includes the first particles and is located on the surface of the first porous base membrane facing the second porous base membrane; the second sub-coating includes second particles, and the second particles are configured to not undergo a redox reaction with alkali metals and / or alkaline earth metals at the nominal voltage of the secondary battery, that is, they have good electrochemical stability at the nominal voltage of the secondary battery and are not susceptible to redox reactions with alkali metals and / or alkaline earth metals. The second sub-coating is located on the surface of the first sub-coating facing the second porous base membrane, wherein the first sub-coating is located on the side of the second sub-coating closer to the negative electrode plate. The first sub-coating is closer to the negative electrode plate, which can better mitigate the continued growth of metal dendrites and further improve the reliability of the secondary battery.
[0135] [Positive electrode]
[0136] In some embodiments, the positive electrode sheet includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector and comprising a positive electrode active material. For example, the positive electrode current collector has two surfaces that oppose each other in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposing surfaces of the positive electrode current collector.
[0137] When the secondary battery of the present application is a lithium-ion battery, the positive electrode active material may include, but is not limited to, at least one of a lithium-containing transition metal oxide, a lithium-containing phosphate, and their respective modified compounds. Examples of the lithium transition metal oxide may include, but are not limited to, at least one of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and their respective modified compounds. Examples of the lithium-containing phosphate may include, but are not limited to, at least one of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, a composite material of lithium iron manganese phosphate and carbon, and their respective modified compounds.
[0138] In some embodiments, in order to further improve the energy density of the secondary battery, the positive electrode active material for the lithium ion battery may include a general formula of Lia Ni b Co c M d O e A f At least one of a lithium transition metal oxide and a modified compound thereof. 0.8≤a≤1.2, 0.5≤b<1, 0<c<1, 0<d<1, 1≤e≤2, 0≤f≤1, M includes at least one of Mn, Al, Zr, Zn, Cu, Cr, Mg, Fe, V, Ti and B, and A includes at least one of N, F, S and Cl.
[0139] As an example, the positive active material for lithium ion batteries may include LiCoO2, LiNiO2, LiMnO2, LiMn2O4, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2(NCM333),LiNi 0.5 Co 0.2 Mn 0.3 O2(NCM523),LiNi 0.6 Co 0.2 Mn 0.2 O2(NCM622),LiNi 0.8 Co 0.1 Mn 0.1 O2(NCM811), LiNi 0.85 Co 0.15 Al 0.05 At least one of O2, LiFePO4, and LiMnPO4.
[0140] When the secondary battery of the present application is a sodium ion battery, the positive electrode active material may include but is not limited to at least one of sodium-containing transition metal oxides, polyanion materials (such as phosphates, fluorophosphates, pyrophosphates, sulfates, etc.), and Prussian blue materials.
[0141] As an example, the positive active material for sodium ion batteries may include NaFeO2, NaCoO2, NaCrO2, NaMnO2, NaNiO2, NaNi 1 / 2 Ti 1 / 2 O2、NaNi 1 / 2 Mn 1 / 2 O2、Na 2 / 3 Fe 1 / 3 Mn 2 / 3 O2、NaNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, NaFePO4, NaMnPO4, NaCoPO4, Prussian blue materials, general formula X p M'q (PO4) r O x Y 3-x At least one of the materials. p M' q (PO4) r O x Y 3-x , 0<p≤4, 0<q≤2, 1≤r≤3, 0≤x≤2, X includes H + 、Li + 、Na + , K + and NH4 + At least one of , M' is a transition metal cation, optionally at least one of V, Ti, Mn, Fe, Co, Ni, Cu and Zn, and Y is a halogen anion, optionally at least one of F, Cl and Br.
[0142] In the present application, the modified compounds of the above-mentioned positive electrode active materials may be the ones subjected to doping modification and / or surface coating modification on the positive electrode active materials.
[0143] In some embodiments, the positive electrode film layer may further optionally include a positive electrode conductive agent. The present application does not particularly limit the type of the positive electrode conductive agent. By way of example, the positive electrode conductive agent may include at least one of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. In some embodiments, the mass percentage of the positive electrode conductive agent is ≤5% based on the total weight of the positive electrode film layer.
[0144] In some embodiments, the positive electrode film layer may further optionally include a positive electrode binder. This application does not particularly limit the type of the positive electrode binder. As an example, the positive electrode binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylic resin. In some embodiments, based on the total weight of the positive electrode film layer, the mass percentage of the positive electrode binder is ≤5%.
[0145] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, aluminum foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include at least one of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. As an example, the polymer material base layer may include at least one of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).
[0146] The positive electrode film layer is typically formed by coating a positive electrode slurry onto a positive electrode current collector, drying, and cold pressing. The positive electrode slurry is typically formed by dispersing the positive electrode active material, an optional conductive agent, an optional binder, and any other components in a solvent and stirring them uniformly. The solvent may be, but is not limited to, N-methylpyrrolidone (NMP).
[0147] [Negative electrode]
[0148] In some embodiments, the negative electrode sheet includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector and comprising a negative electrode active material. For example, the negative electrode current collector has two opposing surfaces in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposing surfaces of the negative electrode current collector.
[0149] The negative electrode active material may be any negative electrode active material known in the art for use in secondary batteries. For example, the negative electrode active material may include, but is not limited to, at least one of natural graphite, artificial graphite, soft carbon, hard carbon, silicon-based film materials, tin-based film materials, and lithium titanate. The silicon-based film material may include at least one of elemental silicon, silicon oxide, a silicon-carbon composite, a silicon-nitrogen composite, and a silicon alloy. The tin-based film material may include at least one of elemental tin, tin oxide, and a tin alloy.
[0150] In some embodiments, the negative electrode film layer may further optionally include a negative electrode conductive agent. The present application does not particularly limit the type of the negative electrode conductive agent. By way of example, the negative electrode conductive agent may include at least one of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. In some embodiments, the mass percentage of the negative electrode conductive agent is ≤5% based on the total weight of the negative electrode film layer.
[0151] In some embodiments, the negative electrode film layer may further optionally include a negative electrode binder. The present application does not particularly limit the type of the negative electrode binder. As an example, the negative electrode binder may include at least one of styrene-butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, water-based acrylic resin (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), and carboxymethyl chitosan (CMCS). In some embodiments, the mass percentage of the negative electrode binder based on the total weight of the negative electrode film layer is ≤5%.
[0152] In some embodiments, the negative electrode film layer may optionally include other additives. For example, the other additives may include thickeners, such as sodium carboxymethyl cellulose (CMC), PTC thermistor materials, and the like. In some embodiments, the weight percentage of the other additives is ≤ 2% based on the total weight of the negative electrode film layer.
[0153] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, copper foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include at least one of copper, a copper alloy, nickel, a nickel alloy, titanium, a titanium alloy, silver, and a silver alloy. As an example, the polymer material base layer may include at least one of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).
[0154] The negative electrode film layer is typically formed by coating a negative electrode slurry onto a negative electrode current collector, drying, and cold pressing. The negative electrode slurry is typically formed by dispersing the negative electrode active material, an optional conductive agent, an optional binder, and other optional additives in a solvent and stirring until uniformly mixed. The solvent may be, but is not limited to, N-methylpyrrolidone (NMP) or deionized water.
[0155] The negative electrode plate does not exclude other additional functional layers in addition to the negative electrode film layer. For example, in some embodiments, the negative electrode plate described herein further includes a conductive primer layer (e.g., composed of a conductive agent and a binder) sandwiched between the negative electrode current collector and the negative electrode film layer and disposed on the surface of the negative electrode current collector. In other embodiments, the negative electrode plate described herein further includes a protective layer covering the surface of the negative electrode film layer.
[0156] [Electrolyte]
[0157] During the charge and discharge process of a secondary battery, active ions are embedded and released back and forth between the positive and negative electrodes, and the electrolyte conducts the active ions between the positive and negative electrodes. This application does not specifically limit the type of electrolyte, and the electrolyte can be selected according to actual needs.
[0158] The electrolyte solution includes an electrolyte salt and a solvent. The types of the electrolyte salt and the solvent are not particularly limited and can be selected according to actual needs.
[0159] When the secondary battery of the present application is a lithium ion battery, as an example, the electrolyte salt may include but is not limited to at least one of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bisfluorosulfonyl imide (LiFSI), lithium bistrifluoromethanesulfonyl imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium dioxalatoborate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobisoxalatophosphate (LiDFOP) and lithium tetrafluorooxalatophosphate (LiTFOP).
[0160] When the secondary battery of the present application is a sodium ion battery, as an example, the electrolyte salt may include but is not limited to at least one of sodium hexafluorophosphate (NaPF6), sodium tetrafluoroborate (NaBF4), sodium perchlorate (NaClO4), sodium hexafluoroarsenate (NaAsF6), sodium bis(fluorosulfonyl)imide (NaFSI), sodium bis(trifluoromethanesulfonyl)imide (NaTFSI), sodium trifluoromethanesulfonate (NaTFS), sodium difluorooxalatoborate (NaDFOB), sodium dioxalatoborate (NaBOB), sodium difluorophosphate (NaPO2F2), sodium difluorobis(oxalatophosphate) (NaDFOP) and sodium tetrafluorooxalatophosphate (NaTFOP).
[0161] As an example, the solvent may include, but is not limited to, at least one of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS) and diethyl sulfone (ESE).
[0162] In some embodiments, the electrolyte may optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, or additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high-temperature performance, and additives that improve battery low-temperature power performance.
[0163] In some embodiments, the positive electrode sheet, the separator, and the negative electrode sheet may be formed into an electrode assembly through a winding process and / or a lamination process.
[0164] In some embodiments, the secondary battery may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.
[0165] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery can also be a soft package, such as a bag-type soft package. The material of the soft package can be plastic, such as at least one of polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS).
[0166] The present application has no particular limitation on the shape of the secondary battery, which can be cylindrical, square, or any other shape. FIG1 shows a secondary battery 5 with a square structure as an example.
[0167] In some embodiments, as shown in FIG2 , the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 is used to cover the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation film can be formed into an electrode assembly 52 through a winding process and / or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is impregnated in the electrode assembly 52. The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, which can be adjusted according to demand.
[0168] The method for preparing the secondary battery of the present application is well known. In some embodiments, a positive electrode sheet, a separator, a negative electrode sheet, and an electrolyte can be assembled to form a secondary battery. As an example, the positive electrode sheet, separator, and negative electrode sheet can be formed into an electrode assembly through a winding process and / or a lamination process. The electrode assembly is placed in an outer packaging, dried, and then injected with electrolyte. The secondary battery is obtained through vacuum packaging, static standing, formation, and shaping processes.
[0169] In some embodiments of the present application, the secondary batteries according to the present application can be assembled into a battery module. The battery module can contain multiple secondary batteries, and the specific number can be adjusted according to the application and capacity of the battery module.
[0170] Figure 3 is a schematic diagram of an exemplary battery module 4. As shown in Figure 3 , within the battery module 4, multiple secondary batteries 5 may be arranged sequentially along the length of the battery module 4. Of course, any other arrangement is also possible. Furthermore, the multiple secondary batteries 5 may be secured using fasteners.
[0171] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.
[0172] In some embodiments, the battery modules described above may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.
[0173] Figures 4 and 5 are schematic diagrams of an exemplary battery pack 1. As shown in Figures 4 and 5, the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 covers the lower case 3 and forms an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.
[0174] Electrical devices
[0175] The fourth aspect of the embodiment of the present application provides an electric device, which includes at least one of the secondary battery, battery module or battery pack of the present application. The secondary battery, battery module or battery pack can be used as a power source for the electric device, and can also be used as an energy storage unit for the electric device. The electric device can be, but is not limited to, a mobile device (such as a mobile phone, a laptop computer, etc.), an electric vehicle (such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship and a satellite, an energy storage system, etc.
[0176] The electrical device may select a secondary battery, a battery module or a battery pack according to its usage requirements.
[0177] Figure 6 is a schematic diagram of an exemplary electric device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of this device, a battery pack or battery module may be used.
[0178] As another example, the electric device may be a mobile phone, a tablet computer, a laptop computer, etc. Such an electric device is usually required to be lightweight and thin, and may use a secondary battery as a power source.
[0179] Example
[0180] The following examples describe the present disclosure in more detail. These examples are intended to be illustrative only, as various modifications and variations within the scope of the present disclosure will be apparent to those skilled in the art. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are by mass, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing. The instruments used in the examples are commercially available.
[0181] Example 1
[0182] Preparation of isolation membrane
[0183] Provide PP base film: thickness 6μm, porosity 40%, ion conductivity 1.20mS / cm.
[0184] Provide PE base film: thickness 5μm, porosity 35%, ion conductivity 1.0mS / cm.
[0185] Prepare the first coating slurry: Molybdenum disulfide and binder aqueous solution type polyacrylic acid are mixed uniformly in a suitable amount of deionized water as a solvent at a mass ratio of 95:5 to obtain the first coating slurry. The volume average particle size Dv50 of the molybdenum disulfide is 0.10 μm.
[0186] Prepare the second coating slurry: Aluminum oxide and binder aqueous solution type polyacrylic acid are mixed uniformly in a suitable amount of deionized water as a solvent at a mass ratio of 95:5 to obtain the second coating slurry. The volume average particle size Dv50 of the aluminum oxide is 0.10 μm.
[0187] Preparation of isolation film:
[0188] The prepared first coating slurry is coated on one surface of the PE base film by a coating machine, and a first sub-coating layer is obtained through a drying process.
[0189] The prepared second coating slurry was applied to the surface of the first sub-coating layer using a coating machine to form a second sub-coating layer. The PP and PE base films were then heat-pressed to form a separator film. The first and second sub-coating layers were positioned between the PP and PE base films, with the first sub-coating layer being closer to the PE base film and the second sub-coating layer being closer to the PP base film. The coating layer had a molybdenum disulfide content (A) of 47.5% and an aluminum oxide content (B) of 47.5%, with a B / A ratio of 1.00.
[0190] Preparation of positive electrode
[0191] Aluminum foil with a thickness of 12 μm was used as the positive electrode current collector.
[0192] The positive electrode active material LiNi 0.8 Co0.1 Mn 0.1 O2 (NCM811), conductive agent carbon black (Super P), and binder polyvinylidene fluoride (PVDF) are mixed evenly in an appropriate amount of solvent N-methylpyrrolidone (NMP) in a mass ratio of 96.2:2.7:1.1 to obtain a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector aluminum foil, and the positive electrode sheet is made through processes such as drying, cold pressing, slitting, and cutting.
[0193] Preparation of negative electrode sheet
[0194] A copper foil with a thickness of 8 μm was used as the negative electrode current collector.
[0195] Artificial graphite (the negative electrode active material), conductive agent Super P, thickener CMC, and binder styrene-butadiene rubber (SBR) are mixed evenly in deionized water to create a negative electrode slurry. The mass ratio of artificial graphite, Super P, CMC, and SBR in the solids of the negative electrode slurry is 96.4:0.7:1.8:1.1. The negative electrode slurry is coated onto the negative electrode current collector copper foil and then dried, cold pressed, trimmed, cut, and slit to form the negative electrode sheet.
[0196] Preparation of electrolyte
[0197] In an environment with a water content of less than 10 ppm, non-aqueous organic solvents ethylene carbonate EC and diethyl carbonate DMC are mixed in a volume ratio of 1:1 to obtain an electrolyte solvent, and then lithium salt lithium hexafluorophosphate and the mixed solvent are mixed to prepare an electrolyte with a lithium salt concentration of 1 mol / L.
[0198] Preparation of secondary batteries
[0199] The positive electrode sheet, separator, and negative electrode sheet are stacked and wound in sequence to obtain an electrode assembly; the electrode assembly is placed in an outer package, dried, and then injected with electrolyte. After vacuum packaging, standing, formation, shaping and other processes, a secondary battery is obtained.
[0200] Example 2-1 to Example 2-6
[0201] The secondary battery was prepared using a method similar to that of Example 1, except that the material of at least one of the first particles and the second particles was changed.
[0202] Example 3-1 to Example 3-4
[0203] The secondary battery was prepared by a method similar to that of Example 1, except that the volume average particle size of the first particles was adjusted.
[0204] Example 4-1 to Example 4-4
[0205] The secondary battery was prepared by a method similar to that of Example 1, except that the contents of the first particles and the second particles were adjusted.
[0206] Example 5
[0207] Preparation of isolation membrane
[0208] Provide PP base film: thickness 6μm, porosity 40%, ion conductivity 1.20mS / cm.
[0209] Provide PE base film: thickness 5μm, porosity 35%, ion conductivity 1.0mS / cm.
[0210] Preparation of coating slurry: Molybdenum disulfide and binder aqueous solution type polyacrylic acid are uniformly mixed in an appropriate amount of solvent deionized water at a mass ratio of 95.0:5.0 to obtain coating slurry.
[0211] Preparation of isolation film:
[0212] The prepared coating slurry was applied to one surface of a PE base film using a coating machine to form a coating layer. The PP and PE base films were then heat-pressed to form a separator film, wherein the coating layer was located between the PP base film and the PE base film. The molybdenum disulfide content in the coating layer was 95.0%.
[0213] Example 6
[0214] Preparation of isolation membrane
[0215] Provide PP base film: thickness 6μm, porosity 40%, ion conductivity 1.20mS / cm.
[0216] Provide PE base film: thickness 5μm, porosity 35%, ion conductivity 1.0mS / cm.
[0217] Preparation of coating slurry: Molybdenum disulfide, aluminum oxide, and binder aqueous solution type polyacrylic acid are uniformly mixed in an appropriate amount of solvent deionized water at a mass ratio of 47.5:47.5:5 to obtain coating slurry.
[0218] Preparation of isolation film:
[0219] The prepared coating slurry was applied to one surface of a PE base film using a coater to form a coating. The PP and PE base films were then heat-pressed to form a separator film, with the coating located between the PP and PE base films. The coating contained 47.5% molybdenum disulfide (A) and 47.5% aluminum oxide (B), with a B / A ratio of 1:1.
[0220] Comparative Example 1
[0221] The secondary battery was prepared using a method similar to that of Example 1, except that the steps for preparing the separator were as follows:
[0222] Provide PE base film: thickness 5μm, porosity 35%, ion conductivity 1.0mS / cm.
[0223] Prepare the first coating slurry: mix molybdenum disulfide and binder aqueous solution type polyacrylic acid in a mass ratio of 95:5 in an appropriate amount of solvent deionized water to obtain the first coating slurry.
[0224] Coating:
[0225] The prepared first coating slurry is coated on one surface of the PE base film by a coating machine, and a first sub-coating layer is obtained through a drying process, and then the isolation film is prepared through slitting.
[0226] Comparative Example 2
[0227] The secondary battery was prepared using a method similar to that of Example 1, except that the steps for preparing the separator were as follows:
[0228] Provide PP base film: thickness 6μm, porosity 40%, ion conductivity 1.20mS / cm.
[0229] Provide PE base film: thickness 5μm, porosity 35%, ion conductivity 1.0mS / cm.
[0230] Preparation of coating slurry: Alumina particles and binder aqueous solution type polyacrylic acid are uniformly mixed in an appropriate amount of solvent deionized water at a mass ratio of 95:5 to obtain coating slurry.
[0231] Preparation of a release film: The prepared coating slurry is applied on one surface of a PE base film using a coating machine to form a coating layer, and the PP and PE base films are hot-pressed so that the coating layer is between the PP base film and the PE base film to prepare a release film.
[0232] The relevant parameters of the comparative examples and embodiments are shown in Table 1.
[0233] The test results are shown in Table 1.
[0234] Test section
[0235] 1. Thermal shrinkage test of isolation film
[0236] Sample preparation: The isolation films prepared in the above embodiments and comparative examples were punched out along the TD and MD directions into samples with a width of 50 mm and a length of 100 mm using a punching machine. Five parallel samples were placed on A4 paper, and then the A4 paper containing the samples was placed on corrugated paper with a thickness of 1 mm to 5 mm.
[0237] Sample test: Set the temperature of the blast oven to 150°C. After the temperature reaches the set temperature and stabilizes for 30 minutes, place the A4 paper placed on the corrugated paper into the blast oven, start timing, and after the set time (1 hour in this application) is reached, measure the length and width of the isolation film, and mark the values as a and b respectively.
[0238] Calculation of thermal shrinkage: longitudinal (MD) thermal shrinkage = [(100-a) / 100] × 100%, transverse (TD) thermal shrinkage = [(50-b) / 50] × 100%, and the average value of 5 parallel samples is taken as the test result.
[0239] 2. Cycle performance of secondary batteries
[0240] At 25°C, the secondary batteries prepared in the above examples and comparative examples were charged at a constant current of 0.5C to a voltage of 3.65V. They were then charged at a constant voltage of 3.65V to a current of ≤0.05C. The batteries were then discharged at a constant current of 0.5C to a voltage of 2.5V. This constituted one charge-discharge cycle, and the discharge capacity at this point was recorded as the discharge capacity of the battery's first cycle. This charge and discharge cycle was repeated, and the number of cycles required for the capacity to drop to 80% was recorded.
[0241] Test results
[0242] The test results are shown in Table 1.
[0243] Table 1
[0244] As can be seen from Table 1, the embodiments of the present application provide a coating comprising a specific material between the two base films. This prevents the coating from coming into contact with the electrolyte, the negative electrode, and other components, causing side reactions, during the normal charge and discharge process of the secondary battery. As the number of dendrites deposited on the negative electrode increases, they may pierce one of the base films outside the coating and come into direct contact with the coating. The first particles in the coating can then undergo a redox reaction with the dendrite tips, thereby reducing the risk of the dendrites further piercing the other base film and causing a short circuit between the positive and negative electrode sheets, thereby improving the reliability of the secondary battery.
[0245] The surface of the base film of the isolation membrane of Comparative Example 1 is provided with a coating containing molybdenum disulfide. During the cycle of the lithium-ion battery, the first particles of molybdenum disulfide in the coating come into contact with the negative electrode plate, so that the molybdenum disulfide may be consumed prematurely.
[0246] Although Comparative Example 2 is provided with two base films and a coating layer is provided between the two base films, the particles in the coating layer cannot undergo redox reaction with the dendrites and have little effect on alleviating the dendrites.
[0247] Compared to Example 1, Examples 3-1 and 3-4 adjust the particle size of the first particles to a certain extent, thereby improving the reliability of the secondary battery. Compared to Example 1, the amount of first particles used in Examples 4-1 and 4-4 was adjusted. When the content of first particles was greater than that of second particles, the effect of passivating dendrite growth was better, which could further improve the reliability of the secondary battery. The coatings in Examples 5 and 6 are single-layer structures, which still allow the first particles to play a good role in passivating dendrites.
[0248] Although the present application has been described with reference to preferred embodiments, various modifications may be made thereto and components may be substituted with equivalents without departing from the scope of the present application. In particular, the various technical features described in the various embodiments may be combined in any manner as long as there are no structural conflicts. The present application is not limited to the specific embodiments disclosed herein, but encompasses all technical solutions within the scope of the claims.
Claims
1. A separation film, comprising: a first porous base membrane and a second porous base membrane; as well as A coating layer is disposed between the first porous base membrane and the second porous base membrane, wherein the coating layer comprises first particles, wherein the first particles comprise at least one of molybdenum disulfide, silicon oxide, transition metal oxide or conductive carbon particles.
2. The isolation film according to claim 1, wherein: The first particles include at least one of molybdenum disulfide or a transition metal oxide.
3. The isolation film according to claim 1 or 2, wherein: The silicon oxide comprises at least one of silicon monoxide or silicon dioxide; and / or, The transition metal oxide comprises one or more of manganese dioxide, cobalt oxide, iron oxide or nickel oxide; and / or, The conductive carbon particles include one or more of conductive carbon black, carbon nanotubes, graphite or graphene.
4. The separator according to any one of claims 1 to 3, wherein: Based on the total weight of the coating, the content of the first particles is greater than or equal to 20%, and can be optionally 30% to 60%.
5. The separator according to any one of claims 1 to 4, wherein: The average particle size of the first particles is less than or equal to 3 μm, and can be optionally 0.01 μm to 1 μm.
6. The separator according to any one of claims 1 to 5, wherein: The coating further includes second particles, which do not undergo oxidation and reduction reactions within the operating voltage range of the secondary battery; Optionally, the second particles include at least one of inorganic particles or organic particles.
7. The isolation film according to claim 6, wherein: Based on the total weight of the coating, a ratio of the content of the second particles to the content of the first particles is less than or equal to 1, and can be selected from 0.35 to 0.
85.
8. The separator according to any one of claims 1 to 7, wherein: The coating includes at least two sub-coatings, and the first particles and the second particles are disposed in different sub-coatings.
9. The separator according to any one of claims 1 to 8, wherein: The coating also includes a binder; optionally, the binder includes one or more of polyacrylate, acrylic acid, carboxymethyl cellulose, polyvinylidene fluoride-co-trichloroethylene copolymer, polymethyl methacrylate, polyvinyl pyrrolidone, polyvinyl acetate, polyethylene-co-vinyl acetate copolymer, polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, polyvinylidene fluoride, polyacrylonitrile, polyvinyl alcohol, starch, hydroxypropyl cellulose, regenerated cellulose, tetrafluoroethylene, polyethylene, polypropylene or cyanoethyl pullulan.
10. The separator according to any one of claims 1 to 9, wherein: The first porous base membrane and the second porous base membrane have different melting points.
11. The separator according to any one of claims 1 to 10, wherein: The melting point of the first porous base film is denoted as T m1 The melting point of the second porous substrate is denoted as T m2 , then the isolation film satisfies: 1.05≤T m1 / T m2 ≤2.50; Optionally, 160℃≤T m1 ≤350℃; and / or Optionally, 120℃≤T m2 ≤180℃.
12. The isolation film according to claim 10 or 11, wherein: The coating comprises a first sub-coating and a second sub-coating, the first sub-coating comprises the first particles, the second sub-coating comprises the second particles, The first sub-coating layer is disposed between the first porous base membrane and the second sub-coating layer, or The first sub-coating layer is disposed between the second porous base membrane and the second sub-coating layer.
13. The separator according to any one of claims 1 to 12, wherein: The thickness of the first porous base film is W1, and its unit is μm; The thickness of the second porous base film is W2, in μm. W1 / W2≥1.02; optionally, 1.2≤W1 / W2≤5.0; 14. The isolation film according to claim 13, wherein: 1≤W1≤12; optionally, 3≤W1≤6; and / or 2≤W2≤12; optionally, 3≤W2≤5.
15. The separator according to any one of claims 1 to 14, wherein: The isolation film satisfies at least one of conditions (1) to (6): (1) The longitudinal heat shrinkage of the isolation film at 250°C for 1 hour is less than or equal to 1.0%; (2) The transverse heat shrinkage of the isolation film at 250° C. for 1 hour is less than or equal to 1.0%; (3) The air permeability of the isolation film is less than or equal to 500s / 100cc; it can be 150s / 100cc-400s / 100cc; (4) The longitudinal tensile strength of the isolation film is greater than or equal to 600 kg / cm 2 ; Optional 800kg / cm 2 -2000kg / cm 2 ; (5) The transverse tensile strength of the separator is greater than or equal to 1000 kg / cm 2 ; Optional 1200kg / cm 2 -2500kg / cm 2 ; (6) The ion conductivity of the isolation membrane is 0.5 mS / cm-2.0 mS / cm; optionally 0.8 mS / cm-1.5 mS / cm. 16 . A secondary battery comprising the separator according to claim 1 .
17. The secondary battery according to claim 16, comprising a positive electrode sheet and a negative electrode sheet, wherein the separator is disposed between the positive electrode sheet and the negative electrode sheet; The second porous base film of the separator faces the negative electrode plate.
18. An electrical device comprising the secondary battery according to claim 16 or 17.
Citation Information
Patent Citations
Safety layer and lithium secondary battery
CN108448160A
Isolating membrane and electrochemical device
CN109980164A
Isolating membrane and electrochemical device
CN110364662A
All-solid-state lithium ion battery
CN111710904A
Lithium secondary battery
CN112840494A
Cited By
Composite diaphragm capable of eliminating lithium dendrites, preparation method and lithium battery
CN121076409A