Separator, battery, and electrical apparatus

By using a multi-layer base film structure and a solid particle adhesive layer in the lithium-ion battery isolation film, the problem of insufficient mechanical properties of the isolation film is solved, and the safety performance and ion conductivity of the battery are improved.

WO2024212583A1PCT designated stage expired Publication Date: 2024-10-17CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/141016
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-14
Filing Date
2023-12-22
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Existing lithium-ion battery isolation membranes have poor mechanical properties and are easily punctured, causing safety hazards.

Method used

Use at least three laminated base films, and set a solid particle adhesive layer between the two base films to improve the mechanical properties and ion permeability of the isolation film and reduce the risk of puncture.

Benefits of technology

The puncture resistance of the isolation film and the safety performance of the battery are significantly improved, while maintaining good ion conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023141016_17102024_PF_FP_ABST
    Figure CN2023141016_17102024_PF_FP_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of batteries. Disclosed are a separator, a battery, and an electrical apparatus. The separator comprises at least three layers of stacked base film, with at least two neighboring base film layers having disposed between same and bonded thereto a first bonding layer. Providing the separator as comprising at least three layers of stacked base film, with a first bonding layer being disposed between at least two of the layers of base film, and using the first bonding layer to bond the base film located on the two sides thereof, with the bonded base film layers supporting one another, increases the difficulty of puncturing a single-layer base film, thereby decreasing the risk of the separator being punctured and improving the safety performance of a battery utilizing said separator.
Need to check novelty before this filing date? Find Prior Art

Description

Isolation film, battery and electrical device

[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on April 14, 2023, with application number 202320838552.4 and application name "Isolation membrane, battery and electrical device". Technical Field

[0002] The present application relates to the field of battery technology, and in particular to an isolation membrane, a battery, and an electrical device. Background Art

[0003] Secondary batteries can reversibly convert chemical energy into electrical energy, making them an ideal carrier for human energy utilization and storage. Lithium-ion batteries are widely used in a variety of fields, including 3C electronics, electric vehicles, and energy storage power stations, due to their high energy density, good cycle performance, and environmental friendliness. Lithium-ion batteries typically include a positive electrode, a negative electrode, a separator, and an electrolyte. The separator's primary function is to separate the positive and negative electrodes, preventing contact and short circuits. Furthermore, the separator allows ions in the electrolyte to pass through. The performance of the separator determines the battery's interface structure, internal resistance, and other characteristics, directly affecting the battery's cycle life and safety.

[0004] Currently, commercial separators are primarily based on single-layer polyolefin-based films, such as polyethylene (PE) and polypropylene (PP). Single-layer films typically have poor mechanical properties. Due to the manufacturing process, the surface of the battery's electrode plates may be uneven. When the separator is sandwiched between the positive and negative electrodes, it can be easily punctured, posing a safety hazard.

[0005] Summary of the Invention

[0006] In view of the above problems, the embodiments of the present application provide an isolation membrane, a battery, and an electrical device, aiming to solve the problem of insufficient puncture resistance of the isolation membrane.

[0007] In a first aspect, an embodiment of the present application provides an isolation film comprising at least three stacked base films, wherein a first adhesive layer bonding at least two adjacent base films is provided between the two layers.

[0008] The isolation membrane provided in the embodiment of the present application includes at least three layers of stacked base membranes, and a first adhesive layer is provided between at least two layers of base membranes. The first adhesive layer is utilized to bond the base membranes on both sides of the first adhesive layer. The bonded base membranes provide support to each other, thereby improving the mechanical properties of the isolation membrane and increasing the difficulty of puncturing the single-layer base membrane, thereby further reducing the risk of puncturing the isolation membrane, thereby improving the safety performance of the battery using the isolation membrane.

[0009] In some embodiments, at least two adjacent layers of the base films are laminated together.

[0010] By arranging at least two layers of laminated base films on at least one side of the first adhesive layer, the performance of the isolation film can be adjusted through the combination of the base films, and the range of material selection for the base films can be expanded.

[0011] In some embodiments, the first adhesive layer is disposed between adjacent base films. By configuring the separator to include at least three base film layers, with each base film connected by the first adhesive layer, the overall puncture resistance of the separator is improved, making the separator suitable for use in battery types requiring high puncture resistance. In some embodiments, the first adhesive layer is a solid particle adhesive layer containing dispersed solid particles.

[0012] In the embodiments of the present application, a solid particle adhesive layer is sandwiched between two base films, the solid particle adhesive layer is bonded to the base films, and the base films are used to support and protect the solid particle adhesive layer, thereby preventing displacement of the solid particle adhesive layer and improving the structural stability of the isolation membrane. More importantly, in the embodiments of the present application, since the first adhesive layer is sandwiched between the two base films, by configuring the first adhesive layer as a solid particle adhesive layer, the solid particles dispersed in the solid particle adhesive layer are used to improve the air permeability of the solid particle adhesive layer, thereby improving the ion permeability of the isolation membrane. In particular, when a solid particle adhesive layer is provided between two adjacent base films, the solid particle adhesive layer is used to improve the strength of the isolation membrane while effectively ensuring the ion permeability of the isolation membrane.

[0013] In some embodiments, the solid particles are inorganic particles, and the solid particle bonding layer is an inorganic particle bonding layer.

[0014] Generally, inorganic particles have a certain hardness and heat resistance. By setting the solid particle bonding layer as the inorganic particle bonding layer, the mechanical strength and heat resistance of the isolation membrane can be improved. At the same time, the elastic modulus of the inorganic particles is relatively high, so that the air permeability of the inorganic particle bonding layer is guaranteed.

[0015] In some embodiments, the inorganic particles have a Dv50 of 0.2 μm to 0.8 μm.

[0016] Generally, the larger the particle size of the inorganic particles, the better the air permeability of the inorganic particle bonding layer, and the higher the ion conductivity of the separator. However, the larger the particle size of the inorganic particles, the easier it is for the base membrane to be punctured by the inorganic particles. At the same time, the particle size of the inorganic particles also affects the thickness of the inorganic particle bonding layer. The appropriate average particle size of the inorganic particles can be selected based on the thickness of the inorganic particle bonding layer, the content of the binder, the number of inorganic particle bonding layers in the separator, etc. For example, when the thickness of the inorganic particle bonding layer is relatively small, inorganic particles with a smaller average particle size can be selected. For the isolation membrane provided in the embodiment of the present application, since the number of base membrane layers in the isolation membrane is multi-layer, in order to ensure the ion permeability of the isolation membrane, the thickness of the base membrane is usually relatively thin, and since the inorganic particle bonding layer is sandwiched between the base membranes, relying on the support of the base membrane, by setting the average particle size Dv50 of the inorganic particles to 0.2μm~0.8μm, on the one hand, the inorganic particle bonding layer can be made thinner, further improving the ion conductivity of the isolation membrane, and on the other hand, the risk of the base membrane being punctured can be reduced, thereby improving the structural stability of the isolation membrane.

[0017] In some embodiments, the specific surface area of ​​the solid particles is 1.05 m 2 / g~1.8m 2 / g.

[0018] Generally, the specific surface area of ​​solid particles will affect the wetting effect of the solid particle bonding layer in the electrolyte. The larger the specific surface area of ​​the solid particles, the better the wetting effect of the solid particle bonding layer. By setting the specific surface area of ​​the solid particles to 1.05m 2 / g~1.8m 2 / g, which increases the wetting rate of the isolation membrane in the electrolyte and further improves the ion conductivity of the isolation membrane.

[0019] In some embodiments, the thickness of the first adhesive layer is 0.5 μm to 2 μm.

[0020] The thickness of the first adhesive layer affects the puncture resistance and ion conductivity of the isolation membrane. A thicker thickness improves puncture resistance but reduces ion conductivity. In conjunction with the isolation membrane structure provided in the embodiments of this application, the first adhesive layer is disposed between the base films, and the thickness of the first adhesive layer is set to 0.5 μm to 2 μm. Within this range, the puncture resistance and ion conductivity of the isolation membrane can be balanced, resulting in a strong puncture resistance and excellent ion conductivity.

[0021] In some embodiments, the base film has a thickness of 1 μm to 8 μm.

[0022] The thickness of the base film can affect the puncture resistance and ion conductivity of the base film. The thinner the base film, the lower the internal resistance and the higher the ion conductivity. However, its mechanical strength will decrease and the puncture strength will be worse. In combination with the isolation membrane structure provided in the embodiments of the present application, the number of base film layers is set to multiple layers, and the thickness of each base film layer is controlled to 1μm to 8μm. The base film is made as thin as possible while ensuring sufficient mechanical strength. This balances the puncture resistance and ion conductivity of the isolation membrane, making the isolation membrane have strong puncture resistance while also having excellent ion conductivity.

[0023] In some embodiments, the average pore size of the base film is 100 nm to 800 nm.

[0024] The average pore size of the basement membrane can affect its tensile strength and ionic conductivity. A larger average pore size results in lower internal resistance and higher ionic conductivity, but this also reduces tensile strength. In combination with the isolation membrane structure provided in the embodiments of this application, the number of basement membrane layers is set to multiple layers, and the average pore size of each layer is controlled to 100nm to 800nm. This balances the tensile strength and ionic conductivity of the isolation membrane, resulting in a membrane with both high tensile strength and excellent ionic conductivity.

[0025] In some embodiments, the porosity of the base film is 30% to 70%.

[0026] The porosity of the basement membrane can affect its tensile strength and ionic conductivity. A higher porosity results in lower internal resistance and higher ionic conductivity, but at the expense of decreased tensile strength. In combination with the separator structure provided in the embodiments of this application, controlling the basement membrane porosity to 30% to 70% balances the separator's tensile strength and ionic conductivity, resulting in a separator with both high tensile strength and excellent ionic conductivity.

[0027] In some embodiments, the surface density of the base film is 2 g / m 2 ~10g / m 2 .

[0028] Since there are a large number of micropores on the base film, as the number of micropores increases, the surface density of the base film decreases. By setting the surface density of the base film to 2g / m 2 ~10g / m 2 , which makes the porosity and air permeability of the base membrane moderate, and is conducive to balancing the tensile strength and ion conductivity of the isolation membrane.

[0029] In some embodiments, the air permeability of the isolation membrane is 300s / 100cc to 500s / 100cc.

[0030] By setting the air permeability of the separator to 300s / 100cc to 500s / 100cc, the battery has better electrochemical performance when the separator is used in the battery.

[0031] In some embodiments, the isolation membrane has a porosity of 25% to 65%.

[0032] By setting the porosity of the separator to 25% to 65%, the battery has better electrochemical performance when the separator is used in the battery.

[0033] In some embodiments, the transverse tensile strength of the isolation film is greater than 1000 kg / cm 2 .

[0034] The above-mentioned separator has good mechanical properties.

[0035] In some embodiments, the longitudinal tensile strength of the isolation film is greater than 1200 kg / cm 2 .

[0036] The above-mentioned separator has good mechanical properties.

[0037] In some embodiments, the isolation film has a thickness of 3 μm to 14 μm.

[0038] The thickness of the isolation membrane affects the mechanical properties and ion conductivity of the isolation membrane. Increasing the thickness of the isolation membrane will enhance the mechanical properties of the isolation membrane, but reduce the ion conductivity. Within the above thickness range, the isolation membrane has good mechanical properties and ion conductivity.

[0039] In some embodiments, the isolation film also includes a second adhesive layer located on the side of the base film away from the first adhesive layer, the second adhesive layer forms the outermost layer of the isolation film, the first adhesive layer is a ceramic adhesive layer, and the second adhesive layer is a polymer adhesive layer.

[0040] By arranging a ceramic bonding layer and a polymer bonding layer in the isolation membrane, the ceramic bonding layer and the polymer bonding layer are not located on the same side of the base membrane, wherein the ceramic bonding layer is located between the base membranes, that is, located inside the isolation membrane, and the polymer bonding layer is formed as the outermost layer of the isolation membrane. By arranging the ceramic bonding layer, the mechanical properties of the isolation membrane (including puncture resistance and tensile strength) are improved, and the base membrane is used to support and protect the ceramic bonding layer, thereby improving the structural stability of the isolation membrane. When using the isolation membrane, the polymer bonding layer can be bonded to the electrode plate of the battery, thereby improving the contact interface between the isolation membrane and the electrode plate and improving the consistency of the battery.

[0041] In a second aspect, an embodiment of the present application provides a battery, comprising a positive electrode sheet, a negative electrode sheet, and the above-mentioned isolation film that separates the positive electrode sheet from the negative electrode sheet.

[0042] In a third aspect, an embodiment of the present application provides an electrical device comprising the above-mentioned battery.

[0043] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Various other advantages and benefits will become apparent to those skilled in the art upon reading the detailed description of the optional embodiments below. The accompanying drawings are for illustration purposes only and are not to be considered as limiting the present application. The same reference numerals are used throughout the accompanying drawings to represent the same components. In the accompanying drawings:

[0045] FIG1 is a schematic structural diagram of a vehicle according to some embodiments of the present application;

[0046] FIG2 is a schematic diagram of an exploded structure of a battery according to some embodiments of the present application;

[0047] FIG3 is a schematic diagram of an exploded structure of a battery cell according to some embodiments of the present application;

[0048] FIG4 is a schematic structural diagram of an electrode assembly according to some embodiments of the present application;

[0049] FIG5 is a first structural diagram of an isolation membrane according to some embodiments of the present application;

[0050] FIG6 is a second structural schematic diagram of an isolation membrane according to some embodiments of the present application;

[0051] FIG. 7 is a third structural schematic diagram of an isolation membrane according to some embodiments of the present application.

[0052] The figure numbers in the specific implementation manner are as follows: 10, pole piece; 20, electrode assembly; 101, negative pole piece; 102, positive pole piece; 201, negative pole tab; 202, positive pole tab; 203, isolation film; 2031, base film; 2032, first adhesive layer; 2033, second adhesive layer; 30, battery cell; 301, shell; 302, end cover; 303, negative electrode adapter; 304, positive electrode adapter; 305, insulating part; 40, battery; 401, box body; 4011, box body; 4012, box cover; 50, electrical device; 501, controller; 502, motor. DETAILED DESCRIPTION

[0053] The following embodiments of the technical solution of the present application will be described in detail with reference to the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application and are therefore only examples and are not intended to limit the scope of protection of the present application.

[0054] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in the specification and claims of this application and the above-mentioned figure descriptions are intended to cover non-exclusive inclusions.

[0055] In the description of the embodiments of this application, the technical terms "first" and "second" are used only to distinguish different objects and should not be understood to indicate or imply relative importance or implicitly specify the quantity, specific order, or primary and secondary relationship of the indicated technical features. In the description of the embodiments of this application, the meaning of "plurality" is more than two, unless otherwise clearly and specifically defined.

[0056] References herein to "embodiments" mean that a particular feature, structure, or characteristic described in connection with the embodiments may be included in at least one embodiment of the present application. The appearance of this phrase in various places in the specification does not necessarily refer to the same embodiment, nor does it constitute an independent or alternative embodiment that is mutually exclusive of other embodiments. It is understood, both explicitly and implicitly, by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0057] In the description of the embodiments of this application, the term "and / or" is simply a description of the association relationship between associated objects, indicating that three relationships can exist. For example, A and / or B can represent the following three situations: A exists alone, A and B exist simultaneously, and B exists alone. In addition, the character " / " in this document generally indicates that the associated objects are in an "or" relationship.

[0058] In the description of the embodiments of the present application, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).

[0059] In the description of the embodiments of the present application, the technical terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc., indicating the orientation or position relationship, are based on the orientation or position relationship shown in the accompanying drawings, and are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the embodiments of the present application.

[0060] In the description of the embodiments of the present application, unless otherwise expressly specified or limited, technical terms such as "installed," "connected," "connected," and "fixed" should be understood in a broad sense. For example, they can refer to fixed connections, detachable connections, or integration; mechanical connections or electrical connections; direct connections or indirect connections through an intermediate medium; internal connections between two components or interactions between two components. Those skilled in the art can understand the specific meanings of the above terms in the embodiments of the present application based on specific circumstances.

[0061] Secondary batteries can reversibly convert chemical energy into electrical energy, making them an ideal carrier for human energy utilization and storage. Lithium-ion batteries are widely used in a variety of fields, including 3C electronics, electric vehicles, and energy storage power stations, due to their high energy density, good cycle performance, and environmental friendliness. Lithium-ion batteries typically include a positive electrode, a negative electrode, a separator, and an electrolyte. The separator's primary function is to separate the positive and negative electrodes, preventing contact and short circuits. Furthermore, the separator allows ions in the electrolyte to pass through. The performance of the separator determines the battery's interface structure, internal resistance, and other characteristics, directly affecting the battery's cycle life and safety.

[0062] Currently, commercial separators are primarily based on single-layer polyolefin-based films, such as polyethylene (PE) and polypropylene (PP). Single-layer films typically have poor mechanical properties. Due to the manufacturing process, the surface of the battery's electrode plates may be uneven. When the separator is sandwiched between the positive and negative electrodes, it can be easily punctured, posing a safety hazard.

[0063] Based on this, an embodiment of the present application proposes a new type of isolation membrane, which includes a plurality of base films. By stacking the plurality of base films, the isolation membrane will be punctured only when all the base films are punctured, thereby reducing the risk of the isolation membrane being punctured; further, a first adhesive layer is provided between at least two base films, and the first adhesive layer is utilized to bond the base films on both sides of the first adhesive layer. The base films bonded together provide support to each other, thereby increasing the difficulty of puncturing the single-layer base film, further reducing the risk of the isolation membrane being punctured, and thus improving the safety performance of the battery using the isolation membrane.

[0064] The batteries disclosed in some embodiments of the present application may be used, but are not limited to, in electrical devices such as vehicles, ships, or aircraft. The power supply system of the electrical device may be composed of the batteries disclosed in some embodiments of the present application.

[0065] Some embodiments of the present application provide an electrical device using a battery as a power source, which may be, but is not limited to, a vehicle, a mobile phone, a portable device, a laptop computer, a ship, a spacecraft, an electric toy, an electric tool, etc. Vehicles may be, but are not limited to, fuel-powered vehicles, gas-powered vehicles, or new energy vehicles; new energy vehicles may be, but are not limited to, pure electric vehicles, hybrid vehicles, or extended-range vehicles; spacecraft include, but are not limited to, airplanes, rockets, space shuttles, and spacecraft; electric toys include fixed or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys; and electric tools include metal cutting power tools, grinding power tools, assembly power tools, and railway power tools, such as electric drills, electric grinders, electric wrenches, electric screwdrivers, electric hammers, impact drills, concrete vibrators, and electric planers.

[0066] For the convenience of description, the following embodiments are described by taking a vehicle 50 as an example of an electrical device according to an embodiment of the present application.

[0067] Please refer to Figure 1, which is a schematic structural diagram of a vehicle 50 provided in some embodiments of the present application. A battery 40 is provided inside the vehicle 50, and the battery 40 can be provided at the bottom, head, or tail of the vehicle 50. The battery 40 can be used to power the vehicle 50. For example, the battery 40 can serve as an operating power source for the vehicle 50. The vehicle 50 may further include a controller 501 and a motor 502. The controller 501 is electrically connected to the motor 502 and the battery 40, respectively. The controller 501 is used to control the battery 40 to power the motor 502, for example, for starting, navigating, and meeting the power requirements of the vehicle 50 during operation.

[0068] In some embodiments of the present application, the battery 40 can serve not only as an operating power source for the vehicle 50 , but also as a driving power source for the vehicle 50 , replacing or partially replacing fuel or natural gas to provide driving power for the vehicle 50 .

[0069] In some embodiments of the present application, the battery 40 is a secondary battery, which has various forms, including but not limited to battery cells, battery modules, and battery packs. A secondary battery here refers to a battery that can be recharged to activate the active material after discharge and continue to be used.

[0070] Please refer to Figure 2, which is an exploded view of a battery 40 provided in some embodiments of the present application. Battery 40 includes a housing 401 and battery cells 30, with battery cells 30 housed within housing 401. Housing 401 is a component used to provide accommodation for battery cells 30 and can adopt a variety of structures.

[0071] In some embodiments, the box body 401 may include a box body 4011 and a box cover 4012, which cover each other and together define a storage space for accommodating the battery cells 30. Alternatively, the box body 4011 may be a hollow structure with one end open, and the box cover 4012 may be a plate-like structure that covers the open side of the box body 4011.

[0072] In the battery 40, there can be multiple battery cells 30, and the multiple battery cells 30 can be connected in series, in parallel, or in a mixed connection. Mixed connection means that the multiple battery cells 30 are both connected in series and in parallel. The multiple battery cells 30 can be directly connected in series, in parallel, or in a mixed connection, and then the whole formed by the multiple battery cells 30 is accommodated in the box 401; of course, the battery 40 can also be a battery module formed by first connecting multiple battery cells 30 in series, in parallel, or in a mixed connection, and the multiple battery modules are then connected in series, in parallel, or in a mixed connection to form a whole, and accommodated in the box 401. The battery 40 may also include other structures, such as a busbar component (not shown), for achieving electrical connection between the multiple battery cells 30.

[0073] The battery cell 30 may be cylindrical, flat, rectangular, or in other shapes.

[0074] Please refer to Figure 3, which shows an exploded view of a battery cell 30 in some embodiments of the present application. A battery cell 30 is the basic unit that enables the conversion of chemical energy into electrical energy and is the smallest unit in a battery. As shown in Figure 3, a battery cell 30 includes a housing 301, an end cap 302, an electrode assembly 20, an electrolyte (not shown), and other functional components.

[0075] The shell 301 is a hollow structure with one end open. The shell 301 is used to cooperate with the end cap 302 to form an internal environment for accommodating the electrode assembly 20, the electrolyte and other functional components. The shell 301 can be of various shapes and sizes, such as a rectangular parallelepiped, a cylindrical shape, a hexagonal prism, etc. Specifically, the shape of the shell 301 can be determined according to the specific shape and size of the electrode assembly 20. The material of the shell 301 can be, but is not limited to, copper, iron, aluminum, stainless steel, aluminum alloy, plastic, etc., and is not limited here.

[0076] The end cap 302 refers to a component that covers the opening of the shell 301 to isolate the internal environment of the battery cell 30 from the external environment. Optionally, the shape of the end cap 302 can be adapted to the shape of the shell 301 to match the shell 301. Optionally, the end cap 302 can be made of a material with a certain hardness and strength (such as aluminum alloy). In this way, the end cap 302 is not easily deformed when squeezed or collided, so that the battery cell 30 can have a higher structural strength and improved safety performance. The material of the end cap 302 can be, but is not limited to, copper, iron, aluminum, stainless steel, aluminum alloy, plastic, etc., and is not limited here.

[0077] In some embodiments, the battery cell 30 further includes functional components such as a negative electrode adapter 303 and a positive electrode adapter 304. The negative electrode adapter 303 is used to electrically connect to the negative electrode tab on the electrode assembly 20, and the positive electrode adapter 304 is used to electrically connect to the positive electrode tab on the electrode assembly 20 to output or input electrical energy to the battery cell 30. It is understood that the negative electrode adapter 303 is made of a conductive material, and the material of the negative electrode adapter 303 can be, but is not limited to, copper, iron, aluminum, etc. The positive electrode adapter 304 is made of a conductive material, and the material of the positive electrode adapter 304 can be, but is not limited to, copper, iron, aluminum, etc.

[0078] In some embodiments, the battery cell 30 further includes an insulating member 305 located inside the housing 301 to isolate the housing 301 from the electrode assembly 20 and reduce the risk of short circuits. For example, the insulating member 305 may be made of plastic, rubber, or the like.

[0079] One or more electrode assemblies 20 may be contained within the housing 301 .

[0080] Please refer to Figure 4, which is a schematic diagram of the structure of the electrode assembly 20 in some embodiments of the present application. The electrode assembly 20 is the component in the battery cell 30 where the electrochemical reaction occurs. The electrode assembly 20 is primarily formed by winding or stacking a negative electrode sheet 101 and a positive electrode sheet 102 into an integrated structure, and a separator 203 is typically provided between adjacent negative electrode sheets 101 and positive electrode sheets 102.

[0081] The negative electrode sheet 101 includes a negative electrode current collector and a negative electrode material layer, which is coated on the surface of the negative electrode current collector. Taking a lithium-ion battery as an example, the negative electrode current collector can be made of copper, and the negative electrode material layer includes a negative electrode material, which can be a silicon-based material.

[0082] The positive electrode sheet 102 includes a positive electrode current collector and a positive electrode material layer, which is coated on the surface of the positive electrode current collector. Taking a lithium-ion battery as an example, the positive electrode current collector can be made of aluminum, and the positive electrode material layer includes a positive electrode material, which can be lithium cobalt oxide, lithium iron phosphate, ternary lithium, or lithium manganese oxide.

[0083] The isolation membrane 203 is a porous plastic film that allows lithium ions in the electrolyte to pass freely, but isolates the negative electrode plate 101 and the positive electrode plate 102, so that electrons inside the battery cannot pass freely.

[0084] The negative electrode current collector and the positive electrode current collector also have portions that are not coated with the active material layer. These portions without the active material layer are provided with connecting tabs. Specifically, the negative electrode current collector is connected to the negative electrode tab 201, and the positive electrode current collector is connected to the positive electrode tab 202. During the charge and discharge process of the battery, the positive electrode material layer and the negative electrode material layer react with the electrolyte, the negative electrode tab 201 is connected to the negative electrode adapter 303, and the positive electrode tab 202 is connected to the positive electrode adapter 304 to form a current loop. Of course, in some embodiments, the portions of the negative electrode current collector and the positive electrode current collector that are not coated with the active material layer each constitute a tab.

[0085] 5 to 7 , some embodiments of the present application provide an isolation film 203 , which includes at least three stacked base films 2031 , and a first adhesive layer 2032 bonded to at least two adjacent base films 2031 .

[0086] The isolation membrane 203 includes a base membrane 2031, which may include but is not limited to at least one of a porous membrane and a porous nonwoven web. Optionally, the porous membrane includes a microporous membrane, which refers to a porous membrane with a pore size between 5.0 nm and 1.0 mm. The base membrane 2031 is made of an organic polymer. The organic polymer here includes but is not limited to a composite material of one or more of polyolefins, polyethers, polyetheretherketones, polyimides, polytetrafluoroethylene, polyvinyl fluoride, polyvinylidene fluoride, polyvinylidene chloride, polyethylene-propylene copolymers, copolymers containing C-F bonds, etc. The number of layers of the base membrane 2031 is at least three, and here at least three layers means three or more layers. The materials of each base membrane 2031 may be the same or different.

[0087] At least three layers of base films 2031 are stacked, which means that the base films 2031 are stacked one on top of the other. The stacked base films 2031 may be in direct contact or indirect contact with each other.

[0088] The isolation film 203 also includes a first adhesive layer 2032, which refers to a film layer used to bond two adjacent base films 2031 together. It is understood that the first adhesive layer 2032 is disposed between the two base films 2031. The first adhesive layer 2032 may be disposed between each adjacent base film 2031, or between some adjacent base films 2031. That is, the number of first adhesive layers 2032 in the isolation film 203 is one or more. The first adhesive layer 2032 contains a binder, which refers to a medium material that tightly connects materials together. The binder includes, but is not limited to, at least one of polyacrylate, acrylic acid, carboxymethyl cellulose, polypropylene alcohol, polyurethane, polystyrene, vinyl acetate resin, acrylic resin, and chlorinated rubber.

[0089] The isolation film 203 provided in the embodiment of the present application includes at least three layers of base film 2031. By superimposing at least three layers of base film 2031, and providing a first adhesive layer 2032 between at least two layers of base film 2031, the first adhesive layer 2032 is utilized to bond the base films 2031 on both sides of the first adhesive layer 2032, and the base films 2031 bonded together provide support to each other, thereby improving the mechanical properties of the isolation film 203 and increasing the difficulty of puncturing the single-layer base film 2031, further reducing the risk of puncturing the isolation film 203, and thus improving the safety performance of the battery using the isolation film 203.

[0090] In some embodiments, at least two adjacent layers of base films 2031 are laminated together.

[0091] Here, the term "laminated arrangement" refers to the fact that no other structure is provided between two adjacent base films 2031, and the two are in direct contact. It is understood that at least two layers of laminated base films 2031 are provided on at least one side of the first adhesive layer 2032. By adjusting the material, porosity, pore size, and surface density of each laminated base film 2031, a combination of different base films 2031 can be achieved, thereby adjusting the properties of the isolation film 203 and expanding the range of materials for the base film 2031. As an example, at least one side of the first adhesive layer 2032 is provided with two layers of laminated base films 2031. By laminating the two layers of base films 2031, a double-layer composite film layer is obtained. Compared with a single-layer base film 2031, the porosity of the double-layer composite film layer is reduced. Therefore, when preparing the isolation film 203, base films 2031 with porosities that do not meet the requirements can be selected and combined together to make the porosity of the resulting composite film layer meet the requirements, thereby expanding the range of materials for the base film 2031.

[0092] Optionally, the two layers of base film 2031 bonded together are heat-pressed. Heat-pressing at least two adjacent layers of base film 2031 means that the at least two adjacent layers of base film 2031 are laminated together using a heat-pressing process. It is understood that at least two layers of heat-pressed base film 2031 are disposed on at least one side of the first adhesive layer 2032. Compared to other lamination methods, heat-pressing bonding is simpler and more reliable.

[0093] As an example, referring to FIG. 5 , the isolation film 203 includes three base films 2031 and a first adhesive layer 2032 , and the structure of the isolation film 2033 is: base film 2031 - base film 2031 - first adhesive layer 2032 - base film 2031 .

[0094] As an example, the isolation film 203 includes four layers of base film 2031 and a first adhesive layer 2032. The structure of the isolation film 203 can be set to: base film 2031-base film 2031-first adhesive layer 2032-base film 2031-base film 2031, where the two adjacent layers of base film 2031 are combined together by hot pressing; the structure of the isolation film 203 can also be set to: base film 2031-first adhesive layer 2032-base film 2031-base film 2031-base film 2031, where the three adjacent layers of base film 2031 are combined together by hot pressing.

[0095] By placing at least two layers of laminated base films on at least one side of the first adhesive layer 2032, the performance of the isolation film can be adjusted through the combination of base films, while also expanding the range of base film material selection. In some embodiments, the first adhesive layer 2032 is placed between two adjacent base films 2031.

[0096] As an example, referring to FIG. 6 , the isolation film 203 includes three base films 2031 and two first adhesive layers 2032 , and the structure of the isolation film 2033 is: base film 2031 - first adhesive layer 2032 - base film 2031 - first adhesive layer 2032 - base film 2031 .

[0097] As an example, the isolation film 203 includes four base films 2031 and three first adhesive layers 2032 , and the structure of the isolation film 2033 is set as: base film 2031 - first adhesive layer 2032 - base film 2031 - first adhesive layer 2032 - base film 2031 - first adhesive layer 2032 - base film 2031 .

[0098] By setting the isolation membrane 203 to include at least three layers of base membranes 2031, and connecting two base membranes 2031 by sandwiching a first adhesive layer 2032, the overall puncture resistance of the isolation membrane 203 is improved, making the isolation membrane 203 suitable for use in some battery types that have high requirements for the puncture resistance of the isolation membrane 203.

[0099] In some embodiments, the first bonding layer 2032 is a solid particle bonding layer in which solid particles are dispersed.

[0100] Solid particles refer to geometric solids with specific shapes ranging from millimeters to nanometers. The solid particle bonding layer comprises a mixture of solid particles and a binder. The solid particles may include at least one of organic particles and inorganic particles. Optionally, based on the weight of the first bonding layer 2032, the weight content of the solid particles is 30%-50%; the weight content of the binder is 10%-20%.

[0101] There are also some isolation membranes in the related technology that contain a solid particle bonding layer, but the solid particle bonding layer is usually attached to the outside of the base membrane. When the isolation membrane is used, the isolation membrane is in direct contact with the electrolyte in the battery. As the battery is used, the solid particle bonding layer will usually be displaced, loosened, or even fall off, which will reduce the overall performance of the isolation membrane.

[0102] In the embodiment of the present application, a solid particle adhesive layer is sandwiched between two base films 2031, the solid particle adhesive layer being bonded to the base films 2031. The base films 2031 are then used to support and protect the solid particle adhesive layer, preventing displacement of the solid particle adhesive layer and improving the structural stability of the isolation membrane 203. More importantly, in the embodiment of the present application, since the first adhesive layer 2032 is sandwiched between the two base films 2031, by providing the first adhesive layer 2032 as a solid particle adhesive layer, the solid particles are used to enhance the air permeability of the solid particle adhesive layer, thereby improving the ion permeability of the isolation membrane 203. In particular, when a solid particle adhesive layer is provided between two adjacent base films 2031, the solid particle adhesive layer enhances the strength of the isolation membrane 203 while effectively ensuring the ion permeability of the isolation membrane 203.

[0103] In some embodiments, the solid particles are inorganic particles, and the solid particle bonding layer is an inorganic particle bonding layer.

[0104] Inorganic particles refer to solid particles made of inorganic materials. Inorganic particles include, but are not limited to, at least one of boehmite (γ-AlOOH), aluminum oxide (Al2O3), barium sulfate (BaSO4), magnesium oxide (MgO), magnesium hydroxide (Mg(OH)2), silicon dioxide (SiO2), tin dioxide (SnO2), titanium oxide (TiO2), calcium oxide (CaO), zinc oxide (ZnO), zirconium oxide (ZrO2), yttrium oxide (Y2O3), nickel oxide (NiO), cerium oxide (CeO2), zirconium titanate (SrTiO3), barium titanate (BaTiO3), and magnesium fluoride (MgF2).

[0105] Generally, inorganic particles have a certain hardness and heat resistance. By setting the solid particle bonding layer as the inorganic particle bonding layer, the mechanical strength and heat resistance of the isolation membrane 203 can be improved. At the same time, the elastic modulus of the inorganic particles is relatively high, so that the air permeability of the inorganic particle bonding layer is guaranteed.

[0106] In some embodiments, the inorganic particles have a Dv50 of 0.2 μm to 0.8 μm.

[0107] The average particle size is generally expressed as Dv50, which means that the powder particles larger than and smaller than this particle size each account for 50%. As an example, the average particle size Dv50 of the inorganic particles can be 0.2μm, 0.3μm, 0.4μm, 0.5μm, 0.6μm, 0.7μm or 0.8μm.

[0108] Generally, the larger the particle size of the inorganic particles, the better the air permeability of the inorganic particle bonding layer, and the higher the ionic conductivity of the isolation membrane 203. However, the larger the particle size of the inorganic particles, the easier it is for the inorganic particles to puncture the base film 2031. The particle size of the inorganic particles also affects the thickness of the inorganic particle bonding layer. An appropriate average particle size of the inorganic particles can be selected based on the thickness of the inorganic particle bonding layer, the binder content, the number of inorganic particle bonding layers in the isolation membrane 203, and other factors. For example, when the inorganic particle bonding layer is thin, inorganic particles with a smaller average particle size can be selected. For the isolation membrane 203 provided in the embodiment of the present application, since the number of layers of the base membrane 2031 in the isolation membrane 203 is multiple, in order to ensure the ion permeability of the isolation membrane 203, the thickness of the base membrane 2031 is usually relatively thin, and since the inorganic particle bonding layer is sandwiched between the base membranes 2031, relying on the support of the base membrane 2031, by setting the average particle size Dv50 of the inorganic particles to 0.2μm~0.8μm, on the one hand, the inorganic particle bonding layer can be made thinner, further improving the ion conductivity of the isolation membrane 203, and on the other hand, the risk of the base membrane 2031 being punctured can be reduced, thereby improving the structural stability of the isolation membrane 203.

[0109] In some embodiments, the specific surface area of ​​the solid particles is 1.05 m 2 / g~1.8m 2 / g.

[0110] Specific surface area refers to the total area per unit mass of material, and its unit is m 2 / g. As an example, the specific surface area of ​​a solid particle is 1.05m 2 / g, 1.1m 2 / g, 1.2m 2 / g, 1.3m 2 / g, 1.4m 2 / g, 1.5m 2 / g, 1.6m 2 / g, 1.7m 2 / g or 1.8m 2 / g.

[0111] Generally, the specific surface area of ​​solid particles will affect the wetting effect of the solid particle bonding layer in the electrolyte. The larger the specific surface area of ​​the solid particles, the better the wetting effect of the solid particle bonding layer. By setting the specific surface area of ​​the solid particles to 1.05m 2 / g~1.8m 2 / g, thereby increasing the wetting rate of the isolation membrane 203 in the electrolyte and further increasing the ion conductivity of the isolation membrane 203.

[0112] In some embodiments, the thickness of the first adhesive layer 2032 is 0.5 μm to 2 μm.

[0113] As an example, the thickness of the first adhesive layer 2032 may be 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1.0 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm, 1.5 μm, 1.6 μm, 1.7 μm, 1.8 μm, 1.9 μm, or 2 μm.

[0114] The thickness of the first adhesive layer 2032 affects the puncture resistance and ion conductivity of the isolation membrane 203. A thicker layer improves puncture resistance but reduces ion conductivity. In conjunction with the isolation membrane 203 structure provided in the embodiments of the present application, the first adhesive layer 2032 is disposed between the base film 2031, and the thickness of the first adhesive layer 2032 is set to 0.5 μm to 2 μm. Within this range, the puncture resistance and ion conductivity of the isolation membrane 203 are balanced, resulting in the isolation membrane 203 having strong puncture resistance while also having excellent ion conductivity.

[0115] In some embodiments, the base film 2031 has a thickness of 1 μm to 8 μm.

[0116] As an example, the thickness of the base film 2031 may be 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, 7.5 μm, or 8 μm.

[0117] The thickness of the base film 2031 can affect the puncture resistance and ion conductivity of the base film 2031. The thinner the base film 2031, the lower the internal resistance and the higher the ion conductivity. However, its mechanical strength decreases and the puncture strength decreases. In combination with the structure of the isolation film 203 provided in the embodiment of the present application, the number of layers of the base film 2031 is set to multiple layers, and the thickness of each layer of the base film 2031 is controlled to be 1μm to 8μm. The base film 2031 is made as thin as possible while ensuring sufficient mechanical strength. This balances the puncture resistance and ion conductivity of the isolation film 203, ensuring that the isolation film 203 has strong puncture resistance while also having excellent ion conductivity.

[0118] In some embodiments, the average pore size of the base film 2031 is 100 nm to 800 nm.

[0119] Typically, a large number of micropores are formed on the base film 2031, and the average pore size of the micropores is 100 nm to 800 nm. For example, the average pore size of the micropores can be 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm, 500 nm, 550 nm, 600 nm, 650 nm, 700 nm, 750 nm, or 800 nm.

[0120] The average pore size of the base membrane 2031 can affect the tensile strength and ionic conductivity of the base membrane 2031. A larger average pore size of the base membrane 2031 results in lower internal resistance and higher ionic conductivity, but its tensile strength decreases. In combination with the structure of the isolation membrane 203 provided in the embodiments of the present application, the number of base membrane 2031 layers is set to multiple layers, and the average pore size of each base membrane 2031 layer is controlled to be between 100 nm and 800 nm. This balances the tensile strength and ionic conductivity of the isolation membrane 203, resulting in the isolation membrane 203 having both high tensile strength and excellent ionic conductivity.

[0121] In some embodiments, the porosity of the base film 2031 is 30% to 70%.

[0122] As an example, the porosity of the base film 2031 is 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65% or 70%.

[0123] The porosity of the base membrane 2031 can affect its tensile strength and ionic conductivity. A higher porosity results in lower internal resistance and higher ionic conductivity, but also lower tensile strength. In conjunction with the structure of the isolation membrane 203 provided in the embodiments of this application, controlling the porosity of the base membrane 2031 to 30% to 70% balances the tensile strength and ionic conductivity of the isolation membrane 203, ensuring that the isolation membrane 203 has both high tensile strength and excellent ionic conductivity.

[0124] In some embodiments, the surface density of the base film 2031 is 2 g / m 2 ~10g / m 2 .

[0125] Areal density refers to the mass per unit area of ​​a substance of a specified thickness, expressed in g / m 2 As an example, the surface density of the base film 2031 is 2g / m 2 , 3g / m 2 , 4g / m 2 , 5g / m 2 , 6g / m 2 , 7g / m 2 , 8g / m 2 , 9g / m 2 or 10g / m 2 .

[0126] Since there are a large number of micropores on the base film 2031, as the number of micropores increases, the surface density of the base film 2031 decreases. By setting the surface density of the base film 2031 to 2g / m 2 ~10g / m 2, so that the porosity and air permeability of the base film 2031 are moderate, which is conducive to balancing the tensile strength and ion conductivity of the isolation film 203.

[0127] In some embodiments, the air permeability of the isolation film 203 is 300 s / 100 cc to 500 s / 100 cc.

[0128] The air permeability of the isolation membrane 203 refers to the degree to which the isolation membrane 203 allows gas to pass through it. The air permeability testing method for the isolation membrane 203 is as follows: The isolation membrane 203 is fixed, air pressure is applied to one side of the isolation membrane 203, and the pressure drop and the time taken are measured to test the air permeability of the isolation membrane 203. With the isolation membrane 203 fixed, a certain air pressure is applied to one side of the isolation membrane 203. Due to the micropores in the isolation membrane 203, the air pressure gradually decreases until it reaches atmospheric pressure. By comparing the time it takes for the pressure to drop from the initial pressure to the final pressure, the air permeability of the isolation membrane 203 can be determined. By comparing the pressure drop times of different isolation membranes 203, their air permeability performance can be compared. The shorter the pressure drop time, the better the air permeability.

[0129] As an example, the air permeability of the isolation film 203 is 300 s / 100 cc, 350 s / 100 cc, 400 s / 100 cc, 450 s / 100 cc, or 500 s / 100 cc.

[0130] By setting the air permeability of the separator 203 to 300s / 100cc to 500s / 100cc, the battery has better electrochemical performance when the separator 203 is used in the battery.

[0131] In some embodiments, the porosity of the isolation film 203 is 25% to 65%.

[0132] As an example, the porosity of the isolation film 203 is 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60% or 65%.

[0133] By setting the porosity of the separator 203 to 25% to 65%, the battery has better electrochemical performance when the separator 203 is used in the battery.

[0134] In some embodiments, the transverse tensile strength of the isolation film 203 is greater than 1000 kg / cm 2 .

[0135] Tensile strength is the maximum tensile force a material can withstand after undergoing tensile deformation. Specifically, tensile strength includes longitudinal tensile strength (machine direction, MD) and transverse tensile strength (transverse direction, TD), where the machine direction is the machine direction of stretching and the transverse direction is perpendicular to the machine direction of stretching.

[0136] As an example, the transverse tensile strength of the isolation film 203 may be, but is not limited to, 1000 kg / cm 2 、1050kg / cm 2 、1100kg / cm 2 , 1200kg / cm 2 、1300kg / cm 2 or 1400kg / cm 2 .

[0137] The isolation film 203 has good mechanical properties.

[0138] In some embodiments, the longitudinal tensile strength of the isolation film 203 is greater than 1200 kg / cm 2 .

[0139] As an example, the longitudinal tensile strength of the isolation film 203 may be, but is not limited to, 1200 kg / cm 2 、1250kg / cm 2 、1300kg / cm 2 、1400kg / cm 2 、1500kg / cm 2 or 1600kg / cm 2 .

[0140] The isolation film 203 has good mechanical properties.

[0141] In some embodiments, the isolation film 203 has a thickness of 3 μm to 14 μm.

[0142] As an example, the thickness of the isolation film 203 is 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, or 14 μm.

[0143] The thickness of the isolation membrane 203 affects the mechanical properties and ion conductivity of the isolation membrane 203. Increasing the thickness of the isolation membrane 203 will enhance the mechanical properties of the isolation membrane 203, but reduce the ion conductivity. Within the above thickness range, the isolation membrane 203 has good mechanical properties and ion conductivity.

[0144] In some embodiments, the isolation film 203 also includes a second adhesive layer 2033 located on the side of the base film 2031 facing away from the first adhesive layer 2032. The second adhesive layer 2033 is formed as the outermost layer of the isolation film 203. The first adhesive layer 2032 is a ceramic adhesive layer, and the second adhesive layer 2033 is a polymer adhesive layer.

[0145] It is understood that the first adhesive layer 2032 and the second adhesive layer 2033 are not located on the same side of the base film 2031. Alternatively, only the first adhesive layer 2032 is bonded to the base film 2031. Alternatively, only the second adhesive layer 2033 is bonded to the base film 2031. Alternatively, both the first adhesive layer 2032 and the second adhesive layer 2033 are provided on the base film 2031, with the first adhesive layer 2032 and the second adhesive layer 2033 being located on opposite sides of the base film 2031, respectively.

[0146] The second adhesive layer 2033 is formed as the outermost layer of the isolation film 203, that is, the second adhesive layer 2033 is used to directly contact the electrode when the isolation film 203 is used. It should be noted that the second adhesive layer 2033 can be one layer or two layers.

[0147] The first adhesive layer 2032 is a ceramic coated separator (CCS), that is, the solid particles contained in the first adhesive layer 2032 are ceramic particles. As inorganic particles, the ceramic particles can improve the mechanical strength and heat resistance of the isolation film 203 .

[0148] The second adhesive layer 2033 is a polymer adhesive layer (PCS), that is, the second adhesive layer 2033 contains an organic polymer, which can improve the adhesion between the isolation film 203 and the electrode.

[0149] As an example, referring to FIG7 , the isolation film 203 includes three layers of base film 2031 , one first adhesive layer 2032 and two second adhesive layers 2033 , and the structure of the isolation film 203 is set as: second adhesive layer 2033 - base film 2031 - base film 2031 - first adhesive layer 2032 - base film 2031 - second adhesive layer 2033 .

[0150] As an example, the isolation film 203 includes three layers of base film 2031, two layers of first adhesive layer 2032 and two layers of second adhesive layer 2033. The structure of the isolation film 203 can be set to: second adhesive layer 2033-base film 2031-first adhesive layer 2032-base film 2031-first adhesive layer 2032-base film 2031-second adhesive layer 2033.

[0151] By setting a ceramic bonding layer and a polymer bonding layer in the isolation membrane 203, the ceramic bonding layer and the polymer bonding layer are not located on the same side of the base film 2031, wherein the ceramic bonding layer is located between the base films 2031, that is, located inside the isolation membrane 203, and the polymer bonding layer is formed as the outermost layer of the isolation membrane 203. By setting the ceramic bonding layer, the mechanical properties (including puncture resistance and tensile strength) of the isolation membrane 203 are improved, and the base film 2031 is used to support and protect the ceramic bonding layer, thereby improving the structural stability of the isolation membrane 203. When the isolation membrane 203 is used, the polymer bonding layer can be bonded to the electrode plate of the battery, thereby improving the contact interface between the isolation membrane 203 and the electrode plate and improving the consistency of the battery.

[0152] To facilitate understanding of the structure of the isolation film 203, the following is an example of the manufacturing process of the isolation film 203: providing a base film 2031, applying a slurry coating comprising inorganic particles, a solvent, and a binder to the base film 2031, covering the slurry coating with another base film 2031, drying, and hot pressing to obtain the isolation film 203. The slurry coating has a solid content of 35 wt% to 50 wt%, a coating speed of >50 m / min, and a slurry viscosity of 250 mPa.s to 380 mPa.s.

[0153] The following describes the details in conjunction with specific embodiments.

[0154] Example 1

[0155] S1: Prepare polyethylene (PE) based film (thickness 3 μm, average pore size 100 nm, surface density 2.2 g / m) by melt extrusion equipment and hot stretching equipment. 2 ), polypropylene (PP) based membrane (thickness 3 μm, average pore size 100 nm, surface density 2.4 g / m 2 ), PE-based membrane and PP-based membrane are both microporous membranes;

[0156] S2: Boehmite, polyacrylate, and carboxymethyl cellulose are mixed uniformly in a ratio of 4:1:1 in an appropriate amount of deionized water to prepare a coating slurry. The coating slurry is used to prepare the CCS layer.

[0157] S3: The coating slurry is coated onto a PE base film through a coating machine. Another unwinding roller is a PP / PE double-layer base film, which is laminated to the coating slurry surface. The oven temperature is controlled at 35°C, dried for 5 seconds, and pressed under a pressure of 10N to obtain a composite film, in which the thickness of the CCS layer is 0.5μm;

[0158] S4: Place the composite film on the PCS coating machine and perform double-sided PCS coating. At this time, CCS and PCS are located on both sides of the base film respectively to obtain an isolation film. The structure of the isolation film is PCS / PE / CCS / PP / PE / PCS.

[0159] Example 2

[0160] Same as Example 1, except that in step S3 the thickness of the CCS layer is controlled to be 1.2 μm.

[0161] Example 3

[0162] Same as Example 1, except that in step S3 the thickness of the CCS layer is controlled to be 2 μm.

[0163] Example 4

[0164] Same as Example 1, except that in step S1 , the thickness of the PE base film and the PP base film is 5 μm.

[0165] Example 5

[0166] Same as Example 1, except that in step S1 , the thickness of the PE base film and the PP base film is 6 μm.

[0167] Example 6

[0168] Same as Example 1, except that in step S1 , the pore size of the PE-based film and the PP-based film is 300 nm.

[0169] Example 7

[0170] Same as Example 1, except that in step S1 , the pore size of the PE-based film and the PP-based film is 600 nm.

[0171] Example 8

[0172] Same as Example 1, except that in step S1 , the pore size of the PE-based film and the PP-based film is 800 nm.

[0173] Comparative Example 1

[0174] S1: The polyethylene raw material was melt-extruded and hot-stretched to prepare the following two membranes: polyethylene (PE) based membrane (thickness 3 μm, average pore size 100 nm, surface density 2.2 g / m 2 ) and polyethylene (PE) based membrane (thickness 6 μm, average pore size 100 nm, surface density 2.2 g / m 2 );

[0175] S2: Boehmite, polyacrylate, and carboxymethyl cellulose are mixed uniformly in a ratio of 4:1:1 in an appropriate amount of deionized water to prepare a coating slurry. The coating slurry is used to prepare the CCS layer.

[0176] S3: The coating slurry is coated onto a PE base film through a coating machine. Another unwinding roller is used to laminate another PE base film with the coating slurry surface. The oven temperature is controlled at 35°C, dried for 5 seconds, and pressed under a pressure of 10N to obtain a composite film, wherein the thickness of the CCS layer is 0.5μm.

[0177] S4: Place the composite film on the PCS coating machine and perform double-sided PCS coating. At this time, CCS and PCS are located on both sides of the base film respectively to obtain an isolation film. The structure of the isolation film is PCS / PE / CCS / PE / PCS.

[0178] In order to verify the progress of the examples of the present application, the samples prepared in Examples 1 to 8 and Comparative Example 1 were tested as follows:

[0179] Test method:

[0180] 1. Destruction resistance test:

[0181] S1. Sample preparation: Cut a sample with a diameter greater than 65 mm and lay it flat on the testing machine;

[0182] S2. Test: Install a puncture fixture on the tensile testing machine with a needle diameter of 1mm. Click the test button until the isolation membrane is punctured. Test at least three parallel samples each time. The tensile testing machine display shows the test value, and the average value is taken.

[0183] 2. Thermal shrinkage test:

[0184] S1. Sample preparation: Use a punch to cut 5-10 samples with a width of 50 mm and a length of 100 mm. Place the samples on a glass plate and secure them with paper clips on all four sides.

[0185] S2. Test: Set the temperature of the forced-air oven to a specified temperature, for example, 250°C. After the temperature reaches the set temperature and stabilizes for 60 minutes, place the glass plate in the oven. Measure the length and width of the isolation film for 1 hour. Mark the values ​​as a and b, respectively.

[0186] S3. Calculation:

[0187] Lengthwise shrinkage A = (100-a) / 100 × 100%;

[0188] Width direction shrinkage B = (50-b) / 50 × 100%;

[0189] Record the values ​​of A and B separately and take the average of the five values.

[0190] 3. Ionic conductivity test:

[0191] S1. Sample Preparation: Punch the separator into sample pieces of a certain size (45.3mm x 33.7mm). Alternately stack the lithium sheets and separators to prepare test samples 1-4. Test sample 1 contains two lithium sheets and one separator layer; test sample 2 contains three lithium sheets and two separator layers; test sample 3 contains four lithium sheets and three separator layers; and test sample 4 contains five lithium sheets and four separator layers. Place the test samples in outer packaging and inject electrolyte to obtain symmetrical batteries.

[0192] S2. Test: A Bio-logic electrochemical workstation was used to perform constant voltage AC impedance spectroscopy on isolation membranes with different numbers of layers to obtain ionic conductivity.

[0193] 4. Battery performance test:

[0194] S1. Sample preparation: Preparation of ternary 8-series batteries;

[0195] S2. Testing: At 25°C, the prepared lithium-ion battery was subjected to a cycle test according to the following procedure: fully charged at a 1C rate and fully discharged until the capacity of the lithium-ion battery was less than 80% of the initial capacity, and the number of cycles was recorded.

[0196] The test results are shown in Table 1:

[0197] Table 1

[0198] As can be seen from Table 1, in Examples 1 to 3, the thickness of the CCS layer is 0.5 μm, 1.2 μm, and 2 μm, respectively. As the thickness of the CCS layer increases, the thickness of the separator increases, so that the ion conductivity of the separator decreases. The CCS layer contains inorganic particles boehmite with good mechanical strength and heat resistance. As the thickness of the CCS layer increases, the puncture resistance of the separator is improved, and the thermal shrinkage rate is reduced, which ultimately improves the cycle performance of the battery using the separator. This is because as the puncture resistance and thermal stability of the separator are improved, the separator is not easily punctured by lithium dendrites, resulting in a short circuit between the anode and cathode of the battery, thereby increasing the number of cycles of the battery.

[0199] As can be seen from Table 1, in Examples 1, 4 and 5, the thickness of the base film is 3 μm, 5 μm and 6 μm, respectively. As the thickness of the base film increases, the thickness of the separator increases, the ion conductivity of the separator decreases, and the puncture resistance improves, but the thermal shrinkage rate increases slightly. Generally, the improvement of the puncture resistance of the separator can improve the cycle performance of the battery, but the increase in the thermal shrinkage rate will have a negative impact on the cycle performance of the battery, which ultimately leads to the overall similar cycle performance of the batteries provided in Examples 1, 4 and 5.

[0200] As can be seen from Table 1, in Examples 1 and 6 to 8, the pore sizes of the base membranes are 100 nm, 300 nm, 600 nm, and 800 nm, respectively. As the pore thickness increases, the ion conductivity of the separator increases, the puncture resistance decreases, and the thermal shrinkage rate increases, ultimately leading to reduced cycle performance of the battery. This is because the puncture resistance of the separator decreases and the thermal shrinkage rate increases, both of which increase the risk of short-circuiting the anode and cathode of the battery, thereby reducing the number of battery cycles.

[0201] As can be seen from Table 1, compared with Comparative Example 1, the isolation membrane provided by Example 1 is superior to that of Comparative Example 1 in terms of ion conductivity, puncture resistance and thermal stability. This is because the performance of the double-layer membrane formed by the composite of the 3μm PP base film and the 3μm PE base film in Example 1 is better than that of the single-layer 6μm PE base film, thereby improving the performance of the final isolation membrane.

[0202] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some or all of the technical features therein. These modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.

Claims

1. A separation film, wherein: The invention comprises at least three layers of stacked base films, wherein a first adhesive layer bonding at least two adjacent base films is arranged between the two layers.

2. The isolation film according to claim 1, wherein: At least two adjacent base films are arranged in a laminated manner.

3. The isolation film according to claim 1, wherein: The first adhesive layer is disposed between the base films that are adjacent to each other; or, the first adhesive layer is disposed between two partially adjacent base films.

4. The isolation film according to any one of claims 1 to 3, wherein: The first bonding layer is a solid particle bonding layer, in which solid particles are dispersed.

5. The isolation film according to claim 4, wherein: The solid particles are inorganic particles and / or organic particles, and the solid particle bonding layer is an inorganic particle bonding layer and / or an organic particle bonding layer.

6. The isolation film according to claim 5, wherein: When the solid particles are inorganic particles, Dv50 of the inorganic particles is 0.2 μm to 0.8 μm.

7. The isolation film according to any one of claims 4 to 6, wherein: The specific surface area of ​​the solid particles is 1.05 m 2 / g~1.8m 2 / g.

8. The isolation film according to any one of claims 1 to 7, wherein: The thickness of the first adhesive layer is 0.5 μm to 2 μm.

9. The isolation film according to any one of claims 1 to 7, wherein: The thickness of the base film is 1 μm to 8 μm; and / or the average pore size of the base film is 100 nm to 800 nm; and / or the porosity of the base film is 30% to 70%; and / or the surface density of the base film is 2 g / m 2 ~10g / m 2 .

10. The isolation film according to any one of claims 1 to 7, wherein: The air permeability of the isolation membrane is 300s / 100cc to 500s / 100cc; and / or, the porosity of the isolation membrane is 25% to 65%; and / or, the transverse tensile strength of the isolation membrane is greater than 1000kg / cm 2 ; and / or, the longitudinal tensile strength of the isolation film is greater than 1200kg / cm 2 ; and / or, the thickness of the isolation film is 3μm to 14μm.

11. The isolation film according to any one of claims 1 to 7, wherein: The isolation film also includes a second adhesive layer located on the side of the base film away from the first adhesive layer, the second adhesive layer forms the outermost layer of the isolation film, the first adhesive layer is a ceramic adhesive layer, and the second adhesive layer is a polymer adhesive layer.

12. The isolation film according to claim 1, wherein Two layers of the base film bonded together are arranged on at least one side of the first adhesive layer.

13. The isolation film according to claim 1, wherein: The structure of the isolation film is as follows: The base film-the base film-the first adhesive layer-the base film; Alternatively, the base film-the first adhesive layer-the base film-the first adhesive layer-the base film; Alternatively, the base film-the first adhesive layer-the base film-the first adhesive layer-the base film-the first adhesive layer-the base film.

14. The isolation film according to any one of claims 1 to 7, wherein: The base film includes at least one of a porous film and a porous nonwoven web.

15. The isolation film according to any one of claims 1 to 7, wherein: The base film includes an organic high molecular polymer, and the organic high molecular polymer includes one or more of polyolefin, polyether, polyetheretherketone, polyimide, polytetrafluoroethylene, polyvinyl fluoride, polyvinylidene fluoride, polyvinylidene chloride, polyethylene-propylene copolymer, and copolymer containing CF bond. and / or, The first adhesive layer contains a binder, and the binder includes at least one of polyacrylate, acrylic acid, carboxymethyl cellulose, polypropylene alcohol, polyurethane, polystyrene, vinyl acetate resin, acrylic resin and chlorinated rubber; and / or, When the solid particles are inorganic particles, the inorganic particles include but are not limited to at least one of boehmite, aluminum oxide, barium sulfate, magnesium oxide, magnesium hydroxide, silicon dioxide, tin dioxide, titanium oxide, calcium oxide, zinc oxide, zirconium oxide, yttrium oxide, nickel oxide, cerium oxide, zirconium titanate, barium titanate, and magnesium fluoride.

16. The isolation film according to claim 11, wherein The structure of the isolation film is as follows: The second adhesive layer-the base film-the base film-the first adhesive layer-the base film-the second adhesive layer; Alternatively, the second adhesive layer-the base film-the first adhesive layer-the base film-the first adhesive layer-the base film-the second adhesive layer.

17. The isolation film according to claim 16, wherein: The second adhesive layer is a polymer adhesive layer.

18. A battery, wherein: It comprises a positive electrode sheet, a negative electrode sheet and a separator according to any one of claims 1 to 17 for separating the positive electrode sheet and the negative electrode sheet.

19. An electrical device, wherein: Comprising a battery according to claim 18.

Citation Information

Patent Citations

  • Lithium ion battery and membrane thereof

    CN102569701A

  • Isolating membrane and electrochemical device

    CN109980164A

  • Isolating membrane as well as preparation method and application thereof

    CN113708008A

  • Separator and battery including the same

    CN115714235A

  • Isolating membrane and preparation method thereof, secondary battery and electric device

    CN115832623A